Semiconductor device, power conversion device and method for manufacturing semiconductor device

By designing semiconductor devices with a first Ni-containing metal layer having higher surface roughness than a second layer and applying a noble metal film, the issue of uneven appearance is addressed, enhancing yield and bonding performance.

JP2024134749AInactive Publication Date: 2024-10-04MITSUBISHI ELECTRIC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023045097
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The uneven appearance of thick Ni-containing metal layers in semiconductor devices leads to reduced yield in subsequent processes due to appearance unevenness in the electrodes.

Method used

A semiconductor device design where the surface roughness of a first Ni-containing metal layer is greater than that of a second Ni-containing metal layer, formed through electroless plating with controlled stirring speeds of the plating solution, and a noble metal film is applied to enhance bonding properties.

Benefits of technology

Reduces appearance unevenness in the Ni-containing metal layer, improving yield by minimizing inspection errors and delays, while maintaining excellent bonding performance with external objects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134749000001_ABST
    Figure 2024134749000001_ABST
Patent Text Reader

Abstract

To provide a semiconductor device that reduces appearance irregularities in a metal layer on an electrode.SOLUTION: A semiconductor device 101 has a semiconductor substrate 1, a surface electrode 2, a first metal layer 3 and a second metal layer 4. The surface electrode 2 includes Al. The surface electrode 2 is provided on the surface of the semiconductor substrate 1. The first metal layer 3 includes Ni. The first metal layer 3 is provided on the surface electrode 2. The second metal layer 4 includes Ni. The second metal layer 4 is provided on the first metal layer 3. The surface roughness of the first metal layer 3 is greater than that of the second metal layer 4.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a semiconductor device, a power conversion device, and a method for manufacturing a semiconductor device. [Background technology]

[0002] The electrodes of a semiconductor device are bonded to various objects to be bonded, such as metal wires, circuit patterns, and metal plates, depending on the specifications of the semiconductor device. In order to achieve an excellent bond between the electrodes and the objects to be bonded, for example, a Ni / Au layer that is excellent for solder bonding is used. Since the Ni layer is consumed by the solder during solder bonding and reduced, it is necessary that a thick Ni-containing metal layer is formed on the electrodes of the semiconductor device. Such a thick Ni-containing metal layer is generally formed by a plating method. Patent Document 1 discloses an electrolytic plating method for forming a Ni layer in a power storage device, although the technical field is different from that of semiconductor devices. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2019 / 111556 Summary of the Invention [Problem to be solved by the invention]

[0004] The surface condition of the thick-film Ni-containing metal layer to which Patent Document 1 is applied may have an uneven appearance. If the thick-film electrode has an uneven appearance in the process of forming an electrode of a semiconductor device, the yield in the subsequent process may be reduced.

[0005] In order to solve the above problems, the present disclosure has an object to provide a semiconductor device in which unevenness in appearance of a Ni-containing metal layer on an electrode is reduced. [Means for solving the problem]

[0006] A semiconductor device according to the present disclosure includes a semiconductor substrate, a surface electrode, a first metal layer, and a second metal layer. The surface electrode includes Al. The surface electrode is provided on a surface of the semiconductor substrate. The first metal layer includes Ni. The first metal layer is provided on the surface electrode. The second metal layer includes Ni. The second metal layer is provided on the first metal layer. The surface roughness of the first metal layer is greater than the surface roughness of the second metal layer. Effect of the Invention

[0007] According to the present disclosure, a semiconductor device is provided in which unevenness in appearance of a Ni-containing metal layer on an electrode is reduced.

[0008] The objects, features, aspects, and advantages of the present disclosure will become more apparent from the following detailed description and the accompanying drawings. [Brief description of the drawings]

[0009] [Figure 1] 1 is a cross-sectional view showing a configuration of a semiconductor device in a first embodiment. [Diagram 2] 1 is an enlarged cross-sectional view showing a configuration of a semiconductor device; [Diagram 3] 3 is a flowchart showing a method for manufacturing the semiconductor device in the first embodiment. [Figure 4] 1 is a cross-sectional view showing a configuration of a semiconductor device in a manufacturing process according to a first embodiment. [Diagram 5] 1 is a cross-sectional view showing a configuration of a semiconductor device in a manufacturing process according to a first embodiment. [Figure 6] 1 is a cross-sectional view showing a configuration of a semiconductor device in a manufacturing process according to a first embodiment. [Figure 7] 1 is a cross-sectional view showing a configuration of a semiconductor device in a manufacturing process according to a first embodiment. [Figure 8] FIG. 2 is a diagram showing a detailed process recipe in a manufacturing method of a semiconductor device. [Figure 9] FIG. 11 is a cross-sectional view showing a configuration of a semiconductor device in a second embodiment. [Figure 10] 1 is an enlarged cross-sectional view showing a configuration of a semiconductor device; [Figure 11] 11 is a flowchart showing a method for manufacturing a semiconductor device in a second embodiment. [Figure 12] 11 is a cross-sectional view showing the configuration of a semiconductor device in a manufacturing process according to the second embodiment. [Figure 13] 11 is a cross-sectional view showing the configuration of a semiconductor device in a manufacturing process according to the second embodiment. [Figure 14] 11 is a cross-sectional view showing the configuration of a semiconductor device in a manufacturing process according to the second embodiment. [Figure 15] 11 is a cross-sectional view showing the configuration of a semiconductor device in a manufacturing process according to the second embodiment. [Figure 16] FIG. 2 is a diagram showing a detailed process recipe in a manufacturing method of a semiconductor device. [Figure 17] FIG. 11 is a functional block diagram showing a configuration of a power conversion system according to a third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] <Embodiment 1> Fig. 1 is a cross-sectional view showing the configuration of a semiconductor device 101 in embodiment 1. Fig. 2 is an enlarged cross-sectional view showing the configuration of the semiconductor device 101. The semiconductor device 101 includes a semiconductor substrate 1, a front surface electrode 2, a first metal layer 3, a second metal layer 4, a front surface-side precious metal film 5, a protective film 6, and a back surface electrode 7.

[0011] The semiconductor substrate 1 is also called a semiconductor wafer. A semiconductor element (not shown) is formed on the semiconductor substrate 1. The semiconductor element includes a front surface element region 1A and a back surface diffusion region 1B. The front surface element region 1A is formed in a surface layer on the front surface side of the semiconductor substrate 1. The back surface diffusion region 1B is formed in a surface layer on the back surface side of the semiconductor substrate 1. The semiconductor element in the first embodiment is a vertical type semiconductor element in which a current flows between the front surface element region 1A and the back surface diffusion region 1B.

[0012] The semiconductor element is made of a semiconductor such as Si, or a semiconductor such as SiC, GaN, Ga 2 O 3The semiconductor element is formed of a so-called wide band gap semiconductor such as diamond. The semiconductor element is a power semiconductor element, an element included in a control IC (Integrated Circuit) for controlling the power semiconductor element, etc. The semiconductor element is, for example, an IGBT (Insulated Gate Bipolar Transistor), a MOSFET (Metal Oxide Semiconductor Field Effect Transistor), a Schottky barrier diode, etc. Alternatively, the semiconductor element may be an RC-IGBT (Reverse-Conducting IGBT) in which an IGBT and a free wheel diode are formed in one semiconductor substrate 1.

[0013] The front electrode 2 is provided on the front element region 1A, that is, on the front surface of the semiconductor substrate 1. The front electrode 2 contains Al. The front electrode 2 is, for example, an Al alloy layer containing AlSi, AlCu, AlSiCu, or the like.

[0014] The first metal layer 3 is provided on the front surface electrode 2. The first metal layer 3 contains Ni. The first metal layer 3 is formed by, for example, an electroless plating method. The first metal layer 3 in the first embodiment is an electroless Ni plating layer.

[0015] The second metal layer 4 is provided on the first metal layer 3. The second metal layer 4 contains Ni. The second metal layer 4 is formed by, for example, an electroless plating method. The second metal layer 4 in the first embodiment is an electroless Ni plating layer.

[0016] The surface roughness of the first metal layer 3 is greater than the surface roughness of the second metal layer 4. The surface roughness is measured, for example, by a contact or non-contact measuring instrument. The surface roughness is measured, for example, by an AFM (Atomic Force Microscope), a SEM (Scanning Electron Microscope), an optical interferometer, or the like.

[0017] The front-side precious metal film 5 is provided on the second metal layer 4. The front-side precious metal film 5 contains a metal more noble than the second metal layer 4. The front-side precious metal film 5 in the first embodiment contains Au. The thickness of the front-side precious metal film 5 is thinner than the thicknesses of the first metal layer 3 and the second metal layer 4, for example. The front-side precious metal film 5 prevents oxidation of the second metal layer 4. As described later, the front-side precious metal film 5 is formed by, for example, an electroless plating method. The front-side precious metal film 5 in the first embodiment is an electroless Au plating film.

[0018] The protective film 6 is provided so as to cover the edge of the surface electrode 2. The protective film 6 is made of, for example, polyimide.

[0019] The back electrode 7 is provided on the back diffusion region 1B, that is, on the back surface of the semiconductor substrate 1. The back electrode 7 in the first embodiment has a structure in which an Al alloy layer, a Ti layer, a Ni layer, and an Au layer are laminated in this order. The Al alloy layer includes AlSi, AlCu, AlSiCu, etc. The Al alloy layer improves the bonding between the back electrode 7 and the semiconductor substrate 1. The Ti layer functions as a barrier metal. The Ni layer and the Au layer are provided to obtain good bonding with wiring (not shown) connected to the semiconductor device 101 or a bonding material (not shown) for the wiring. The bonding material is, for example, solder.

[0020] Fig. 3 is a flowchart showing a method for manufacturing the semiconductor device 101 in the first embodiment. Fig. 4 to Fig. 7 are cross-sectional views showing the configuration of the semiconductor device 101 in the manufacturing process of the first embodiment.

[0021] In step S11, the surface element region 1A is formed in a surface layer on the surface side of the semiconductor substrate 1, as shown in FIG.

[0022] In step S12, a front surface electrode 2 is formed on the front surface of the semiconductor substrate 1. As shown in Fig. 4, the front surface electrode 2 is formed in a predetermined region on the front surface element region 1A. The front surface electrode 2 is formed by a sputtering method. The front surface electrode 2 in the first embodiment is an Al alloy layer.

[0023] In step S13, the protective film 6 is formed. As shown in Fig. 5, the protective film 6 is formed so as to cover the edges of the surface electrode 2. The protective film 6 is made of polyimide.

[0024] In step S14, the rear surface of the semiconductor substrate 1 is mechanically ground to thin the semiconductor substrate 1. The mechanical grinding generates a defect layer on the rear surface of the semiconductor substrate 1. In order to remove the defect layer, the semiconductor layer on the rear surface of the semiconductor substrate 1, which has a thickness of 5 to 20 μm, is wet etched. The semiconductor substrate 1 is thinned to a predetermined thickness.

[0025] In step S15, the back surface diffusion region 1B is formed in the surface layer on the back surface side of the semiconductor substrate 1, as shown in FIG.

[0026] In step S16, the back electrode 7 is formed. As shown in Fig. 6, the back electrode 7 is formed on the back diffusion region 1B, that is, on the back surface of the semiconductor substrate 1. The back electrode 7 is formed by a sputtering method. Here, an Al alloy layer, a Ti layer, a Ni layer, and an Au layer are deposited in this order as the back electrode 7.

[0027] In step S17, the rear electrode 7 is covered with a protective material (not shown). The protective material is, for example, a PET (polyethylene terephthalate) film. The first metal layer 3, the second metal layer 4, and the front-side precious metal film 5 in the first embodiment are formed by an electroless plating method, as described below. The protective material protects the rear electrode 7 from chemicals such as a plating solution used in the electroless plating method.

[0028] In step S18, the surface of the front electrode 2 is cleaned with oxygen plasma. This oxygen plasma cleaning process oxidizes and decomposes organic residues attached to the front electrode 2. Even stubborn residues that cannot be removed by pretreatment for the electroless plating method described below are removed. By cleaning the entire front electrode 2, the wettability of the front electrode 2 with the plating solution is improved, and a uniform substitution reaction is promoted. As a result, it is possible to form a first metal layer 3 that has good adhesion to the front electrode 2.

[0029] In step S19, a first metal layer 3 and a second metal layer 4 are formed. As shown in FIG. 7, the first metal layer 3 is formed on the front electrode 2, and the second metal layer 4 is formed on the first metal layer 3. The first metal layer 3 and the second metal layer 4 are formed by electroless plating. The first metal layer 3 and the second metal layer 4 are electroless Ni plating layers containing Ni, and are formed by a zincate method. In the zincate method, Al in the surface layer of the front electrode 2 is replaced with Zn, and Zn precipitates on the surface layer. Furthermore, a plating layer containing Ni is formed starting from the Zn. The procedure of the zincate method will be described below.

[0030] The semiconductor substrate 1 placed on the carrier is immersed in an alkaline degreasing solution, which removes oils and organic matter adhering to the front electrode 2.

[0031] Acid cleaning is performed. The acid cleaning removes oxides formed on the surface layer of the front electrode 2 and roughens the surface of the front electrode 2. This increases the reactivity in the zincate treatment performed after the acid cleaning, and thus improves the adhesion between the front electrode 2 and the first metal layer 3.

[0032] The semiconductor substrate 1 is immersed in an alkaline zincate treatment solution. Since the standard oxidation-reduction potential of Zn is more noble than that of Al, Al in the surface layer of the front electrode 2 is replaced by Zn, and Zn is precipitated on the surface layer. The semiconductor substrate 1 is then immersed in nitric acid. The Zn precipitated on the front electrode 2 is removed by the nitric acid. The semiconductor substrate 1 is then immersed again in an alkaline zincate treatment solution. Al in the surface layer of the front electrode 2 is replaced by Zn, and Zn is precipitated on the surface layer. By repeating the zincate treatment, a dense Zn film is formed on the surface of the front electrode 2. Such a dense Zn film improves the adhesion between the Ni plating film formed starting from Zn and the front electrode 2. The number of times this zincate treatment is repeated is preferably two or more, but is preferably at most three times in consideration of productivity.

[0033] To form the first metal layer 3, the semiconductor substrate 1 is immersed in an acidic electroless Ni plating solution. The circulation flow rate of the electroless Ni plating solution during the formation of the first metal layer 3 is 50 L / min. First, Zn on the surface layer of the front electrode 2 is replaced with Ni, and Ni precipitates on the surface layer. Thereafter, Ni is continuously precipitated by the reducing agent contained in the electroless Ni plating solution, and the thickness of the Ni layer increases. In this way, the first metal layer 3 is formed. The thickness of the first metal layer 3 is preferably 0.5 μm or more and 2 μm or less.

[0034] The second metal layer 4 is formed by the same process as the first metal layer 3, but the stirring speed of the electroless Ni plating solution is different from that during the formation of the first metal layer 3. The circulation flow rate of the electroless Ni plating solution during the formation of the second metal layer 4 is 25 L / min. Ni is continuously precipitated by the reducing agent contained in the electroless Ni plating solution, forming the second metal layer 4. The thickness of the second metal layer 4 is preferably 1.5 μm or more and 8 μm or less.

[0035] As described above, the stirring speed of the plating solution in the step of forming the first metal layer 3 is faster than the stirring speed of the plating solution in the step of forming the second metal layer 4.

[0036] Taking into consideration the film stress applied to the semiconductor substrate 1, the total thickness of the first metal layer 3 and the second metal layer 4 is preferably 2 μm or more and 10 μm or less. After the formation of the first metal layer 3 and the second metal layer 4, the semiconductor substrate 1 is washed with water.

[0037] In step S20, the front-side precious metal film 5 is formed. As shown in FIG. 7, the front-side precious metal film 5 is formed on the second metal layer 4. The front-side precious metal film 5 is formed by electroless plating. The front-side precious metal film 5 is an electroless Au plating film containing Au. In this step S20, the semiconductor substrate 1 is immersed in an electroless Au plating solution. As a result, Au is continuously deposited on the second metal layer 4, and the front-side precious metal film 5 is formed. The thickness of the front-side precious metal film 5 is 20 nm or more and 100 nm or less. After the front-side precious metal film 5 is formed, the semiconductor substrate 1 is washed with water.

[0038] In step S21, the protective material covering the back surface electrode 7 is peeled off. The above steps S11 to S21 constitute the method for manufacturing the semiconductor device 101 in the first embodiment.

[0039] In this manufacturing method, as described above, the stirring speed of the plating solution in the step of forming the first metal layer 3 is faster than the stirring speed of the plating solution in the step of forming the second metal layer 4. Through such a process, a first metal layer 3 having a surface roughness larger than the surface roughness of the second metal layer 4 is formed.

[0040] 8 is a diagram showing a detailed process recipe for the manufacturing method of semiconductor device 101. As a result of manufacturing semiconductor device 101 using this process recipe, the surface roughness of first metal layer 3 was 86.2 nm, and the surface roughness of second metal layer 4 was 53.2 nm. In a visual inspection from above front-side precious metal film 5, it was confirmed that unevenness in appearance had been reduced.

[0041] In summary, the semiconductor device 101 in the first embodiment includes a semiconductor substrate 1, a surface electrode 2, a first metal layer 3, and a second metal layer 4. The surface electrode 2 contains Al. The surface electrode 2 is provided on the surface of the semiconductor substrate 1. The first metal layer 3 contains Ni. The first metal layer 3 is provided on the surface electrode 2. The second metal layer 4 contains Ni. The second metal layer 4 is provided on the first metal layer 3. The surface roughness of the first metal layer 3 is greater than the surface roughness of the second metal layer 4.

[0042] In such a semiconductor device 101, the unevenness of the appearance of the second metal layer 4 on the surface electrode 2 is reduced. This is because, for example, the influence of the orientation of the underlying surface electrode 2 or the influence of the grain size is mitigated. In the appearance inspection process after the plating process, the frequency of visibility defects and the associated inspection errors is reduced. As a result, delays in the construction period and reduced yields due to false defects are avoided.

[0043] Furthermore, the stirring speed of the plating solution in the step of forming the first metal layer 3 is faster than the stirring speed of the plating solution in the step of forming the second metal layer 4. This makes it possible to suppress surface irregularities of the second metal layer 4 relative to the first metal layer 3. It is preferable that the difference between the circulating flow rate of the plating solution when forming the first metal layer 3 and the circulating flow rate of the plating solution when forming the second metal layer 4 is at least one time. In particular, when the difference in the circulating flow rates is two times or more, the unevenness in appearance is significantly improved. The difference in the stirring speed of the plating solution is not limited to being controlled by the circulating flow rate of the plating solution, and may be controlled by, for example, the rocking speed of a carrier in which the semiconductor substrate 1 is stored.

[0044] Agitation refers to the circulating action of the plating solution in the plating tank by a pump, or the swinging action of a carrier that houses the semiconductor substrate 1. In the swinging action of the carrier, the carrier swings in a fixed direction, making it difficult to control the amplitude of the plating solution. On the other hand, the circulating action by a pump creates a flow in which the plating solution rotates in one direction in the plating tank. This makes it easy to control the plating solution, and the agitation speed is also easy to adjust. In other words, it is easier to adjust the agitation speed by controlling the flow of the plating solution by the circulating action of a pump than by controlling the flow of the plating solution by the swinging action of the carrier.

[0045] Furthermore, since the front side precious metal film 5 containing Au is provided on the second metal layer 4, excellent bonding to a bonding object can be obtained. The bonding object is a metal wire, a circuit pattern, a metal plate, etc. for passing a current from the outside to a semiconductor element.

[0046] In a vertical semiconductor device 101 in which a current flows between the front and back surfaces of a semiconductor substrate 1, a metal wire is bonded to the front electrode 2, and a circuit board is bonded to the back electrode 7 via a bonding material. In order to further reduce costs and improve heat dissipation, a configuration in which the front electrode 2 is also bonded to a metal plate or the like via a bonding material is being used. In such a configuration, a Ni / Au layer with excellent bonding properties is required as the front electrode 2. In addition, a thick Ni layer of 2 μm or more is required to achieve good bonding properties. Electroless plating is preferable for forming a Ni layer with a thickness of 2 μm or more. Electroless plating makes it possible to form a Ni layer at low cost and with easy patterning.

[0047] <Embodiment 2> Fig. 9 is a cross-sectional view showing the configuration of a semiconductor device 102 in embodiment 2. Fig. 10 is an enlarged cross-sectional view showing the configuration of the semiconductor device 102. The semiconductor device 102 includes a semiconductor substrate 1, a front surface electrode 2, a first metal layer 3, a second metal layer 4, a front surface-side precious metal film 5, a protective film 6, a rear surface electrode 8, a third metal layer 9, a fourth metal layer 10 and a rear surface-side precious metal film 11.

[0048] The semiconductor substrate 1, front electrode 2, first metal layer 3, second metal layer 4, front-side noble metal film 5 and protective film 6 in the second embodiment are configured the same as those in the first embodiment.

[0049] The back surface electrode 8 is provided on the back surface diffusion region 1B, that is, on the back surface of the semiconductor substrate 1. The back surface electrode 8 contains Al. The back surface electrode 8 in the second embodiment is an Al alloy layer containing AlSi, AlCu, AlSiCu, or the like.

[0050] The third metal layer 9 is provided on the back electrode 8. The third metal layer 9 contains Ni. The third metal layer 9 is formed by, for example, an electroless plating method. The third metal layer 9 in the second embodiment is an electroless Ni plating layer.

[0051] The fourth metal layer 10 is provided on the third metal layer 9. The fourth metal layer 10 contains Ni. The fourth metal layer 10 is formed by, for example, an electroless plating method. The fourth metal layer 10 in the second embodiment is an electroless Ni plating layer.

[0052] The surface roughness of the third metal layer 9 is greater than the surface roughness of the fourth metal layer 10. The composition of the third metal layer 9 is the same as the composition of the first metal layer 3, and the composition of the fourth metal layer 10 is the same as the composition of the second metal layer 4.

[0053] The back side precious metal film 11 is provided on the fourth metal layer 10. The back side precious metal film 11 contains a metal more noble than the fourth metal layer 10. The back side precious metal film 11 in the second embodiment contains Au. The thickness of the back side precious metal film 11 is thinner than the thicknesses of the third metal layer 9 and the fourth metal layer 10, for example. The back side precious metal film 11 prevents oxidation of the fourth metal layer 10. As described later, the back side precious metal film 11 is formed by, for example, an electroless plating method. The back side precious metal film 11 in the second embodiment is an electroless Au plating film.

[0054] Fig. 11 is a flowchart showing a method for manufacturing the semiconductor device 102 in the second embodiment. Fig. 12 to Fig. 15 are cross-sectional views showing the configuration of the semiconductor device 102 in the manufacturing process of the second embodiment.

[0055] 12, the surface element region 1A is formed in a surface layer on the surface side of the semiconductor substrate 1.

[0056] In step S32, a front surface electrode 2 is formed on the front surface of the semiconductor substrate 1. As shown in Fig. 12, the front surface electrode 2 is formed in a predetermined region on the front surface element region 1A. The front surface electrode 2 is formed by a sputtering method. The front surface electrode 2 in the second embodiment is an Al alloy layer.

[0057] In step S33, the protective film 6 is formed. As shown in Fig. 13, the protective film 6 is formed so as to cover the edges of the surface electrodes 2. The protective film 6 is made of polyimide.

[0058] In step S34, the rear surface of the semiconductor substrate 1 is mechanically ground to thin the semiconductor substrate 1. The mechanical grinding generates a defect layer on the rear surface of the semiconductor substrate 1. In order to remove the defect layer, the semiconductor layer on the rear surface of the semiconductor substrate 1, which has a thickness of 5 to 20 μm, is wet etched. The semiconductor substrate 1 is thinned to a predetermined thickness.

[0059] In step S35, the back surface diffusion region 1B is formed in the surface layer on the back surface side of the semiconductor substrate 1, as shown in FIG.

[0060] In step S36, a back electrode 8 is formed. As shown in Fig. 14, the back electrode 8 is formed on the back diffusion region 1B, that is, on the back surface of the semiconductor substrate 1. The back electrode 8 is formed by a sputtering method. The back electrode 8 in the second embodiment is an Al alloy layer such as AlSi, AlCu, or AlSiCu.

[0061] In step S37, the surfaces of the front electrode 2 and the back electrode 8 are cleaned with oxygen plasma. This oxygen plasma cleaning process oxidizes and decomposes organic residues attached to the front electrode 2 and the back electrode 8. Even stubborn residues that cannot be removed by pretreatment for the electroless plating method described below are removed. By cleaning the entire front electrode 2 and the back electrode 8, the wettability between the front electrode 2 and the plating solution and the wettability between the back electrode 8 and the plating solution are improved, and a uniform substitution reaction is promoted. As a result, it is possible to form a first metal layer 3 that has good adhesion to the front electrode 2 and a third metal layer 9 that has good adhesion to the back electrode 8.

[0062] In step S38, a first metal layer 3, a second metal layer 4, a third metal layer 9, and a fourth metal layer 10 are formed. As shown in FIG. 15, the first metal layer 3 is formed on the front electrode 2, and the second metal layer 4 is formed on the first metal layer 3. The third metal layer 9 is formed on the back electrode 8, and the fourth metal layer 10 is formed on the third metal layer 9. The first metal layer 3, the second metal layer 4, the third metal layer 9, and the fourth metal layer 10 are formed by an electroless plating method. The first metal layer 3, the second metal layer 4, the third metal layer 9, and the fourth metal layer 10 are electroless Ni plating layers containing Ni, and are formed by a zincate method. The procedure of the zincate method will be described below.

[0063] The semiconductor substrate 1 placed on the carrier is immersed in an alkaline degreasing liquid, which removes oil and organic matter adhering to the front electrode 2 and the back electrode 8.

[0064] Acid cleaning is performed. The acid cleaning removes oxides formed on the surface layers of the front electrode 2 and the back electrode 8, and also roughens the surfaces of the front electrode 2 and the back electrode 8. This increases the reactivity in the zincate treatment performed after the acid cleaning, and thus improves the adhesion between the front electrode 2 and the first metal layer 3 and between the back electrode 8 and the third metal layer 9.

[0065] The semiconductor substrate 1 is immersed in an alkaline zincate treatment solution. The Al in the surface layers of the front electrode 2 and the back electrode 8 is replaced with Zn, and Zn is precipitated on the surface layers. The semiconductor substrate 1 is then immersed in nitric acid. The Zn precipitated on the front electrode 2 and the back electrode 8 is removed by the nitric acid. The semiconductor substrate 1 is then immersed again in an alkaline zincate treatment solution. The Al in the surface layers of the front electrode 2 and the back electrode 8 is replaced with Zn, and Zn is precipitated on the surface layers. By repeating the zincate treatment, a dense Zn film is formed on the surface of the front electrode 2 and the back electrode 8. Such a dense Zn film improves the adhesion between the Ni plating film formed from Zn and the front electrode 2 and between the Ni plating film and the back electrode 8. The number of times this zincate treatment is repeated is preferably two or more, but is preferably at most three times in consideration of productivity.

[0066] In order to form the first metal layer 3 and the third metal layer 9, the semiconductor substrate 1 is immersed in an acidic electroless Ni plating solution. The circulation flow rate of the electroless Ni plating solution during the formation of the first metal layer 3 and the third metal layer 9 is 50 L / min. First, Zn in the surface layers of the front electrode 2 and the back electrode 8 is replaced with Ni, and Ni is precipitated on the surface layers. Then, Ni is continuously precipitated by the reducing agent contained in the electroless Ni plating solution, and the thickness of the Ni layer increases. As a result, the first metal layer 3 and the third metal layer 9 are formed. In the second embodiment, the step of forming the third metal layer 9 is performed simultaneously with the step of forming the first metal layer 3. That is, the composition of the third metal layer 9 is the same as the composition of the first metal layer 3. The thickness of the first metal layer 3 and the third metal layer 9 is preferably 0.5 μm or more and 2 μm or less.

[0067] Next, the second metal layer 4 and the fourth metal layer 10 are formed. The stirring speed of the electroless Ni plating solution when the second metal layer 4 and the fourth metal layer 10 are formed is different from the stirring speed when the first metal layer 3 and the third metal layer 9 are formed. The circulation flow rate of the electroless Ni plating solution when the second metal layer 4 and the fourth metal layer 10 are formed is 25 L / min. Ni is continuously precipitated by the reducing agent contained in the electroless Ni plating solution, and the second metal layer 4 and the fourth metal layer 10 are formed. In the second embodiment, the step of forming the fourth metal layer 10 is performed simultaneously with the step of forming the second metal layer 4. That is, the composition of the fourth metal layer 10 is the same as the composition of the second metal layer 4. The thickness of the second metal layer 4 and the fourth metal layer 10 is preferably 1.5 μm or more and 8 μm or less.

[0068] As described above, the stirring speed of the plating solution in the steps of forming the first metal layer 3 and the third metal layer 9 is faster than the stirring speed of the plating solution in the steps of forming the second metal layer 4 and the fourth metal layer 10.

[0069] Taking into consideration the film stress applied to the semiconductor substrate 1, the total thickness of the first metal layer 3 and the second metal layer 4 is preferably 2 μm or more and 10 μm or less. Similarly, the total thickness of the third metal layer 9 and the fourth metal layer 10 is preferably 2 μm or more and 10 μm or less. After the formation of the first metal layer 3, the second metal layer 4, the third metal layer 9 and the fourth metal layer 10, the semiconductor substrate 1 is washed with water.

[0070] In step S39, the front side precious metal film 5 and the back side precious metal film 11 are formed. As shown in FIG. 15, the front side precious metal film 5 is formed on the second metal layer 4, and the back side precious metal film 11 is formed on the fourth metal layer 10. The front side precious metal film 5 and the back side precious metal film 11 are formed by electroless plating. The front side precious metal film 5 and the back side precious metal film 11 are electroless Au plating films containing Au. In this step S39, the semiconductor substrate 1 is immersed in an electroless Au plating solution. As a result, Au is continuously precipitated on the second metal layer 4 and the fourth metal layer 10, and the front side precious metal film 5 and the back side precious metal film 11 are formed. The thickness of the front side precious metal film 5 and the back side precious metal film 11 is 20 nm or more and 100 nm or less. After the front side precious metal film 5 and the back side precious metal film 11 are formed, the semiconductor substrate 1 is washed with water. The above steps S31 to S39 constitute the method for manufacturing the semiconductor device 102 according to the second embodiment.

[0071] In this manufacturing method, as described above, the stirring speed of the plating solution in the steps of forming the first metal layer 3 and the third metal layer 9 is faster than the stirring speed of the plating solution in the steps of forming the second metal layer 4 and the fourth metal layer 10. By such a process, the first metal layer 3 having a surface roughness greater than the surface roughness of the second metal layer 4 is formed. Similarly, the third metal layer 9 having a surface roughness greater than the surface roughness of the fourth metal layer 10 is formed.

[0072] 16 is a diagram showing a detailed process recipe in the manufacturing method of the semiconductor device 102. In appearance inspections from above of the front-side precious metal film 5 and the back-side precious metal film 11, it was confirmed that appearance unevenness was reduced.

[0073] In the second embodiment, the electroless Ni plating layer on the front side and the electroless Ni plating layer on the back side of the semiconductor substrate 1 are formed simultaneously, but they may be formed separately. For example, the first metal layer 3 and the second metal layer 4 may be formed on the front side of the semiconductor substrate 1, and then the third metal layer 9 and the fourth metal layer 10 may be formed on the back side. Alternatively, the first metal layer 3 and the second metal layer 4 may be formed on the front side after the third metal layer 9 and the fourth metal layer 10 are formed on the back side of the semiconductor substrate 1.

[0074] <Embodiment 3> FIG. 17 is a functional block diagram showing a configuration of a power conversion system according to the third embodiment.

[0075] The power conversion system includes a power source 100 , a power conversion device 200 , and a load 300 .

[0076] The power supply 100 is a DC power supply. The power supply 100 supplies DC power to the power conversion device 200. The power supply 100 is, for example, a DC system, a solar cell, a storage battery, or the like. The power supply 100 may be configured with a DC / DC converter that converts DC power output from a DC system into a predetermined power. The power supply 100 may also be a rectifier circuit connected to an AC system, an AC / DC converter, or the like.

[0077] The power conversion device 200 is connected between the power source 100 and the load 300. The power conversion device 200 in the third embodiment is a three-phase inverter. The power conversion device 200 converts DC power supplied from the power source 100 into AC power. The power conversion device 200 supplies the AC power to the load 300.

[0078] The load 300 is driven by AC power supplied from the power conversion device 200. The load 300 in the third embodiment is a three-phase motor. The three-phase motor is not limited to a specific application. The three-phase motor is mounted in various electric devices. The three-phase motor is mounted in, for example, hybrid cars, electric cars, railroad cars, elevators, and air conditioners.

[0079] The following describes in detail the power conversion device 200. The power conversion device 200 includes a main conversion circuit 201, a drive circuit 202, and a control circuit 203.

[0080] The main conversion circuit 201 includes a two-level three-phase full-bridge circuit (not shown). The three-phase full-bridge circuit includes six switching elements (not shown) and six freewheeling diodes (not shown).

[0081] At least one of the switching elements and the free wheel diode corresponds to the semiconductor element shown in embodiment 1 or 2. In other words, the main conversion circuit 201 includes the semiconductor device 101 shown in embodiment 1 or the semiconductor device 102 shown in embodiment 2.

[0082] The three-phase full-bridge circuit includes three upper arms and three lower arms. Each of the upper arms and the lower arms includes one switching element and one freewheeling diode connected in anti-parallel to the switching element. The switching element included in one upper arm is connected in series to the switching element included in one lower arm, and they form one set of upper and lower arms. The three sets of upper and lower arms correspond to the U phase, V phase, and W phase of the three-phase full-bridge circuit, respectively. The output terminals of the three sets of upper and lower arms, i.e., the three output terminals of the main conversion circuit 201, are connected to a load 300.

[0083] The main conversion circuit 201 converts the DC power supplied from the power source 100 into AC power by the switching operation of the switching element. The main conversion circuit 201 supplies the AC power to the load 300 via the output terminal.

[0084] The drive circuit 202 generates a drive signal for driving the switching element of the main conversion circuit 201 in accordance with a control signal output from the control circuit 203. The drive circuit 202 supplies the drive signal to a control electrode of the switching element of the main conversion circuit 201.

[0085] The drive signal is a signal for turning a switching element on or off. More specifically, when a switching element is maintained in an on state, the drive signal is a voltage signal (on signal) equal to or greater than the threshold voltage of the switching element. When a switching element is maintained in an off state, the drive signal is a voltage signal (off signal) smaller than the threshold voltage of the switching element.

[0086] The control circuit 203 outputs a control signal for controlling the drive circuit 202 to the drive circuit 202. At this time, the control circuit 203 calculates the time (ON time) during which each switching element of the main conversion circuit 201 should be in the ON state based on the power to be supplied to the load 300, and generates the control signal. In other words, the control circuit 203 generates a control signal so that the main conversion circuit 201 is PWM (Pulse Width Modulation) controlled. The control circuit 203 outputs a control signal to the drive circuit 202 so that the drive circuit 202 outputs an ON signal to a switching element that should be in the ON state, and an OFF signal to a switching element that should be in the OFF state. In this way, the control circuit 203 controls the switching elements of the main conversion circuit 201 so that a predetermined power is supplied to the load 300.

[0087] Since the semiconductor device 101 shown in the first embodiment or the semiconductor device 102 shown in the second embodiment is applied to the main conversion circuit 201 in the third embodiment, the reliability of the power conversion device 200 is improved.

[0088] In the third embodiment, an example has been shown in which the power conversion device 200 is a two-level three-phase inverter, but the configuration of the power conversion device 200 is not limited thereto. For example, the power conversion device 200 may be a multi-level power conversion device such as a three-level power conversion device. Alternatively, the power conversion device 200 may be a single-phase inverter for supplying power to a single-phase load. When the load 300 is a DC load, the power conversion device 200 may be a DC / DC converter or an AC / DC converter. When the load 300 is a solar power generation system, a power storage system, or the like, the power conversion device 200 may be a power conditioner.

[0089] In the third embodiment, the load 300 is a three-phase motor, but the configuration of the load 300 is not limited to this. For example, the load 300 may be an electric discharge machine, a laser processing machine, an induction heating cooker, or a non-contact power supply system.

[0090] In the present disclosure, each embodiment can be freely combined, and each embodiment can be modified or omitted as appropriate.

[0091] Various aspects of the present disclosure are summarized below as appendices.

[0092] (Appendix 1) A semiconductor substrate; a surface electrode including Al and provided on a surface of the semiconductor substrate; A first metal layer including Ni and provided on the front electrode; a second metal layer comprising Ni and disposed on the first metal layer; A semiconductor device, wherein the first metal layer has a surface roughness greater than a surface roughness of the second metal layer.

[0093] (Appendix 2) 2. The semiconductor device according to claim 1, further comprising a front-side noble metal film including a metal more noble than the second metal layer and provided on the second metal layer.

[0094] (Appendix 3) A back electrode including Al and provided on a back surface of the semiconductor substrate; a third metal layer including Ni and disposed on the back electrode; a fourth metal layer including Ni and disposed on the third metal layer; 3. The semiconductor device of claim 1, wherein the third metal layer has a surface roughness greater than a surface roughness of the fourth metal layer.

[0095] (Appendix 4) 4. The semiconductor device according to claim 3, further comprising a back-side noble metal film including a metal more noble than the fourth metal layer and provided on the fourth metal layer.

[0096] (Appendix 5) the composition of the third metal layer is the same as the composition of the first metal layer; 5. The semiconductor device of claim 3, wherein the fourth metal layer has a composition identical to that of the second metal layer.

[0097] (Appendix 6) A main conversion circuit including the semiconductor device according to any one of Supplementary Note 1 to Supplementary Note 5, which converts power input from a power source and outputs the power to a load; a drive circuit that outputs a drive signal for driving the semiconductor device to the semiconductor device; a control circuit that outputs a control signal for controlling the drive circuit to the drive circuit.

[0098] (Appendix 7) forming a surface electrode containing Al on a surface of a semiconductor substrate; forming a first metal layer containing Ni on the front electrode; forming a second metal layer containing Ni on the first metal layer; A method for manufacturing a semiconductor device, wherein the first metal layer has a surface roughness greater than a surface roughness of the second metal layer.

[0099] (Appendix 8) the first metal layer and the second metal layer are formed by an electroless plating method; 8. The method for manufacturing a semiconductor device according to claim 7, wherein a stirring speed of the plating solution in the step of forming the first metal layer is faster than a stirring speed of the plating solution in the step of forming the second metal layer.

[0100] (Appendix 9) 9. The method for manufacturing a semiconductor device according to claim 7, further comprising the step of forming a front-side noble metal film on the second metal layer, the front-side noble metal film including a metal more noble than the second metal layer.

[0101] (Appendix 10) forming a back electrode containing Al on a back surface of the semiconductor substrate; forming a third metal layer containing Ni on the back electrode; forming a fourth metal layer containing Ni on the third metal layer; 10. The method for manufacturing a semiconductor device according to claim 7, wherein the third metal layer has a surface roughness greater than a surface roughness of the fourth metal layer.

[0102] (Appendix 11) the third metal layer and the fourth metal layer are formed by an electroless plating method; 11. The method for manufacturing a semiconductor device according to claim 10, wherein a stirring speed of the plating solution in the step of forming the third metal layer is faster than a stirring speed of the plating solution in the step of forming the fourth metal layer.

[0103] (Appendix 12) 12. The method for manufacturing a semiconductor device according to claim 10, further comprising the step of forming a back-side noble metal film on the fourth metal layer, the back-side noble metal film containing a metal more noble than the fourth metal layer.

[0104] (Appendix 13) the first metal layer, the second metal layer, the third metal layer, and the fourth metal layer are formed by an electroless plating method; the step of forming the third metal layer is performed simultaneously with the step of forming the first metal layer; the step of forming the fourth metal layer is performed simultaneously with the step of forming the second metal layer; 13. The method for manufacturing a semiconductor device according to any one of claims 10 to 12, wherein a stirring speed of the plating solution in the step of forming the first metal layer and the step of forming the third metal layer is faster than a stirring speed of the plating solution in the step of forming the second metal layer and the step of forming the fourth metal layer. [Explanation of symbols]

[0105] 1 semiconductor substrate, 1A front surface element region, 1B rear surface diffusion region, 2 front surface electrode, 3 first metal layer, 4 second metal layer, 5 front surface side precious metal film, 6 protective film, 7 rear surface electrode, 8 rear surface electrode, 9 third metal layer, 10 fourth metal layer, 11 rear surface side precious metal film, 100 power supply, 101 semiconductor device, 102 semiconductor device, 200 power conversion device, 201 main conversion circuit, 202 drive circuit, 203 control circuit, 300 load.

Claims

1. A semiconductor substrate; a surface electrode including Al and provided on a surface of the semiconductor substrate; a first metal layer including Ni and provided on the front electrode; a second metal layer including Ni and disposed on the first metal layer; A semiconductor device, wherein the first metal layer has a surface roughness greater than a surface roughness of the second metal layer.

2. The semiconductor device according to claim 1 , further comprising a front-side noble metal film including a metal more noble than the second metal layer and provided on the second metal layer.

3. a back electrode including Al and provided on a back surface of the semiconductor substrate; a third metal layer including Ni and disposed on the back electrode; a fourth metal layer including Ni and disposed on the third metal layer; The semiconductor device according to claim 1 , wherein a surface roughness of said third metal layer is greater than a surface roughness of said fourth metal layer.

4. The semiconductor device according to claim 3 , further comprising a back-side noble metal film including a metal more noble than said fourth metal layer and provided on said fourth metal layer.

5. the composition of the third metal layer is the same as the composition of the first metal layer; The semiconductor device according to claim 3 , wherein the fourth metal layer has a composition identical to that of the second metal layer.

6. a main conversion circuit including the semiconductor device according to claim 1, which converts power input from a power source and outputs the power to a load; a drive circuit that outputs a drive signal for driving the semiconductor device to the semiconductor device; a control circuit that outputs a control signal for controlling the drive circuit to the drive circuit.

7. forming a surface electrode containing Al on a surface of a semiconductor substrate; forming a first metal layer containing Ni on the front electrode; forming a second metal layer containing Ni on the first metal layer; A method for manufacturing a semiconductor device, wherein the first metal layer has a surface roughness greater than a surface roughness of the second metal layer.

8. the first metal layer and the second metal layer are formed by an electroless plating method; 8. The method for manufacturing a semiconductor device according to claim 7, wherein the plating solution is stirred at a faster rate in the step of forming the first metal layer than in the step of forming the second metal layer.

9. 8. The method for manufacturing a semiconductor device according to claim 7, further comprising the step of forming a front-side noble metal film containing a metal more noble than said second metal layer on said second metal layer.

10. forming a back electrode containing Al on a back surface of the semiconductor substrate; forming a third metal layer containing Ni on the back electrode; forming a fourth metal layer containing Ni on the third metal layer; The method for manufacturing a semiconductor device according to claim 7 , wherein the third metal layer has a surface roughness greater than a surface roughness of the fourth metal layer.

11. the third metal layer and the fourth metal layer are formed by an electroless plating method; The method for manufacturing a semiconductor device according to claim 10 , wherein an agitation speed of the plating solution in the step of forming the third metal layer is faster than an agitation speed of the plating solution in the step of forming the fourth metal layer.

12. The method for manufacturing a semiconductor device according to claim 10 , further comprising the step of forming a back surface side noble metal film on said fourth metal layer, said back surface side noble metal film containing a metal more noble than said fourth metal layer.

13. the first metal layer, the second metal layer, the third metal layer, and the fourth metal layer are formed by an electroless plating method; the step of forming the third metal layer is performed simultaneously with the step of forming the first metal layer; the step of forming the fourth metal layer is performed simultaneously with the step of forming the second metal layer; 11. The method for manufacturing a semiconductor device according to claim 10, wherein an agitation speed of the plating solution in the step of forming the first metal layer and the step of forming the third metal layer is faster than an agitation speed of the plating solution in the step of forming the second metal layer and the step of forming the fourth metal layer.

Citation Information

Patent Citations

  • Semiconductor device

    JP2005033130A

  • Semiconductor device

    JP2006114827A

  • Terminal, wiring connection structure, and method for manufacturing terminal

    WO2014129222A1

  • Metal member and production method therefor

    WO2020217787A1

  • Semiconductor element, electric power conversion device, and manufacturing method for semiconductor element

    WO2022186192A1