Method for producing silicon carbide fibrous material
A sealed container process using silicon oxide, hydrogen/hydrocarbon-generating, and carbonaceous substances with a transition metal catalyst produces silicon carbide fibers efficiently, addressing cost and length limitations in existing methods.
Patent Information
- Application Number
- JP2023045246
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Existing methods for producing silicon carbide materials require the external supply of hydrogen gas, which increases manufacturing costs and limits the ability to produce materials with longer fiber lengths.
A method involving a sealed container where silicon oxide-generating, hydrogen/hydrocarbon-generating, and carbonaceous substances react to form silicon carbide fibers, utilizing a transition metal catalyst within the container to promote reactions without external hydrogen supply.
This method efficiently produces silicon carbide fibers with lengths of 1 mm or more, reducing manufacturing costs by eliminating the need for external hydrogen gas and enhancing fiber length, while maintaining reaction efficiency.
Smart Images

Figure 2024134842000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing silicon carbide fibrous material. [Background technology]
[0002] In recent years, there has been a demand for silicon carbide materials with high aspect ratios as peripheral components for electronic devices.
[0003] As a method for producing silicon carbide whiskers, for example, Patent Document 1 discloses a method in which a powdered silicon oxide raw material and a powdered carbon raw material are mixed and heated while passing hydrogen gas through the mixture. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 61-295299 Summary of the Invention [Problem to be solved by the invention]
[0005] However, with the method described in Patent Document 1, it has been desired to further reduce the production cost of silicon carbide material and to produce silicon carbide material having a longer fiber length.
[0006] The present invention has been made to solve the above-mentioned problems, and has an object to provide a manufacturing method that does not require the supply of hydrogen gas from an outside source and that can produce silicon carbide material with long fiber length. [Means for solving the problem]
[0007] The method for producing silicon carbide fibrous material of the present invention is characterized by heating a substance (A) that generates silicon oxide gas, a substance (B) that decomposes thermally to generate hydrogen or hydrocarbons, a carbonaceous substance (C), and a substance containing a transition metal (D) in a sealed container (E) containing silicon carbide on its surface.
[0008] In the method for producing a silicon carbide fibrous material of the present invention, a substance (A) that generates silicon oxide gas, a substance (B) that generates hydrogen or hydrocarbons by thermal decomposition, a carbonaceous substance (C), and a substance (D) containing a transition metal are heated in a sealed container (E). At this time, hydrogen or hydrocarbons are generated from the substance (B) by thermal decomposition in the container (E), and the generated hydrogen reacts with the substance (C) as shown in reaction formulas (1) and (2) to become hydrocarbons. The substance (A) generates silicon oxide gas by heating, and reacts with the substance (B) and / or the hydrocarbons generated from the substances (B) and (C) as shown in reaction formulas (3) and (4), to produce a silicon carbide fibrous material. The substance (D) functions as a catalyst to promote reaction formulas (3) and (4). In addition, the hydrogen produced in reactions (3) and (4), like the hydrogen produced by thermal decomposition of substance (B), reacts with substance (C) to form hydrocarbons, which are then used to react with silicon oxide gas. 2C(s)+4H2=2CH4(g) (1) 2C(s)+H2(g)=C2H2(g) (2) SiO(g)+2CH4(g)=SiC(s)+CO(g)+4H2(g) (3) SiO(g)+C2H2(g)=SiC(s)+CO(g)+H2(g) (4)
[0009] At this time, since the container (E) is sealed, there is no need to continuously supply raw material gases such as silicon oxide gas and hydrogen gas from outside the system, and the reaction proceeds continuously. Therefore, there is no need to supply hydrogen gas. In addition, since the container (E) has silicon carbide on its surface, the silicon oxide gas generated from the material (A) does not react with the container (E), so the silicon oxide gas is not consumed and it can be used efficiently to produce silicon carbide fibrous material.
[0010] In the method for producing a silicon carbide fibrous material of the present invention, the material (A) is preferably a mixture containing silicon carbide and silicon dioxide. When the substance (A) is a mixture containing silicon carbide and silicon dioxide, silicon oxide gas can be efficiently generated within the container (E).
[0011] In the method for producing a silicon carbide fibrous material of the present invention, the material (A) is preferably a molded product containing silicon carbide and silicon dioxide. When the substance (A) is a molded body containing silicon carbide and silicon dioxide, silicon oxide gas can be gradually released from the surface of the molded body, and therefore the silicon oxide gas concentration in the vessel (E) can be easily adjusted by controlling the reaction conditions. In addition, by arranging the molded body containing silicon carbide and silicon dioxide so as to surround the vicinity of the above substances (B), (C), and (D), the generated silicon oxide gas will remain in the vicinity of the above substances (B), (C), and (D), and the reaction can proceed efficiently.
[0012] In the method for producing a silicon carbide fibrous material of the present invention, the above material (C) is preferably graphite. When the substance (C) is graphite, the reactions of the above reaction formulas (1) and (2) tend to proceed easily.
[0013] In the method for producing a silicon carbide fibrous material of the present invention, the material (C) is preferably a graphite molded body. When the material (C) is a graphite molded body, the silicon carbide fibrous material formed on the graphite can be easily collected, and the material (B) and the material (D) can be uniformly coated on the graphite molded body.
[0014] In the method for producing a silicon carbide fibrous material of the present invention, the substance (B) is preferably a phenol resin. When the substance (B) is a phenol resin, hydrocarbons can be efficiently generated by thermal decomposition.
[0015] In the method for producing a silicon carbide fibrous material of the present invention, the above-mentioned substance (D) is preferably iron oxide. Iron oxide is suitable as substance (D) because it acts as a catalyst for the reactions of reaction equations (3) and (4) above.
[0016] In the method for producing silicon carbide fibrous material of the present invention, it is preferable that the substance (B) is a phenolic resin, the substance (D) is iron oxide, and the phenolic resin and the iron oxide are formed as a coating layer on the surface of the substance (C). When the phenolic resin and iron oxide are formed as a coating layer on the surface of the substance (C), the hydrocarbon gas generated from the phenolic resin and the substance (C) is likely to be present near the catalyst, and the reactions of the above reaction formulas (3) and (4) are likely to proceed. In addition, the hydrogen generated in the reaction formulas (3) and (4) is likely to react with the substance (C), so the reactions of the above reaction formulas (1) to (4) proceed continuously.
[0017] In the method for producing silicon carbide fibrous material of the present invention, it is preferable to heat the above-mentioned materials (A), (B), (C) and (D) in the sealed container (E) under an inert atmosphere at a temperature of 1500 to 1700°C. When the materials (A), (B), (C) and (D) are heated in a sealed container (E) under the above-mentioned conditions, a silicon carbide fibrous material can be efficiently produced.
[0018] In the method for producing a silicon carbide fibrous material of the present invention, it is preferable that the silicon carbide fibrous material obtained has an average length of 1 mm or more. By using the method for producing a silicon carbide fibrous material of the present invention, it is possible to obtain a silicon carbide fibrous material having a length of 1 mm or more. [Brief description of the drawings]
[0019] [Figure 1] Figure 1 is a cross-sectional view showing a schematic diagram of a container (E) used in the method for producing silicon carbide fibrous material of the present invention, and an example of material (A), material (B), material (C) and material (D) placed in the container (E). [Diagram 2]FIG. 2 is a schematic diagram showing the reaction that occurs when the container (E) shown in FIG. 1 is heated. [Diagram 3] FIG. 3 is a schematic diagram showing how silicon carbide fibrous material is produced by heating. [Figure 4] FIG. 4 is a photograph showing the appearance of the silicon carbide fibrous material obtained in Example 1. [Diagram 5] FIG. 5 is a partially enlarged view of the silicon carbide fibrous material shown in FIG. [Figure 6] FIG. 6 is a partially enlarged view of the silicon carbide fibrous material shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, the embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope of the present invention.
[0021] The method for producing silicon carbide fibrous material of the present invention is characterized by heating a substance (A) that generates silicon oxide gas, a substance (B) that decomposes thermally to generate hydrogen or hydrocarbons, a carbonaceous substance (C), and a substance containing a transition metal (D) in a sealed container (E) containing silicon carbide on its surface.
[0022] An example of a method for producing a silicon carbide fibrous material of the present invention will be described with reference to FIG. Figure 1 is a cross-sectional view showing a schematic diagram of a container (E) used in the method for producing silicon carbide fibrous material of the present invention, and an example of material (A), material (B), material (C) and material (D) placed in the container (E).
[0023] In FIG. 1, a molded body 10 and a graphite block 30 having a surface coated with a phenol resin 20 are arranged separately in a container 50 consisting of a container body 50a and a lid 50b. A transition metal powder 40 is disposed on the surface of the phenol resin 20 .
[0024] The molded body 10 is a substance (A) that generates silicon oxide gas.
[0025] The phenol resin 20 is a substance (B) that undergoes thermal decomposition to generate hydrogen or hydrocarbons.
[0026] The graphite block 30 is a carbonaceous material (C).
[0027] The transition metal powder 40 is a substance (D) containing a transition metal. 1, the transition metal powder 40 is drawn to have a size that can be seen with the naked eye, but it is not necessary for the powder to have a size that can be seen with the naked eye. The transition metal powder 40 may be embedded in the phenol resin 20.
[0028] Silicon carbide layers 51a and 51b containing silicon carbide are formed on the inner portions of the surface of container 50, that is, the inner wall surface of container body 50a and the surface of lid portion 50b facing container body 50a, respectively. The container 50 is a container (E) containing silicon oxide on its surface.
[0029] The upper surface (opening) of the container body 50a is closed by a lid 50b, and the compact 10, the phenolic resin 20, the graphite block 30 and the transition metal powder 40 are sealed inside the container 50.
[0030] In this specification, "sealed" refers to a state in which the free movement of gas between the inside and outside of a container is prevented, and is not intended to mean that the movement of gas between the inside and outside of a container is strictly blocked. For example, in the container 50 shown in FIG. 1, the container body 50a and the lid portion 50b are simply in contact with each other, so gas transfer occurs between the inside and outside of the container 50 through the gap at the contact portion between the container body 50a and the lid portion 50b. That is, when a sealed container is placed in a reduced pressure environment, the atmosphere inside the container also becomes a reduced pressure environment. When the reduced pressure environment is switched to an argon atmosphere, the atmosphere inside the sealed container also becomes an argon atmosphere. However, since the upper part of the container body 50a is covered with the lid 50b, even if the atmospheric gas flows in one direction outside the container, the flow of the atmospheric gas does not affect the inside of the container. Furthermore, the gas generated inside the container does not easily leak out to the outside.
[0031] A molded body 10 as the substance (A), a phenolic resin 20 as the substance (B), a graphite block 30 as the substance (C), and a transition metal powder 40 as the substance (D) are heated in a sealed state in a container 50. The reaction that occurs upon heating is explained with reference to FIG.
[0032] FIG. 2 is a schematic diagram showing the reaction that occurs when the container (E) shown in FIG. 1 is heated. As shown in FIG. 2, by heating the container 50, silicon oxide gas [SiO(g)] is generated from the molded body 10, which is the substance (A). Additionally, hydrocarbon gas [CH4(g) / C2H2(g)] is generated from the phenol resin 20, which is the substance (B).
[0033] When the substance (B) is a substance that generates hydrogen gas, the generated hydrogen gas [H2(g)] reacts with the graphite block 30, which is the substance (C), to generate a hydrocarbon gas [CH4(g) / C2H2(g)]. The reaction at this time is represented, for example, by the following reaction formulas (1) and (2). 2C(s)+4H2=2CH4(g) (1) 2C(s)+H2(g)=C2H2(g) (2)
[0034] FIG. 3 is a schematic diagram showing how silicon carbide fibrous material is produced by heating. 3, silicon oxide gas and hydrocarbon gas produced by heating the container 50 react with each other due to the catalytic action of the transition metal powder 40, which is the substance (D), to produce silicon carbide fibrous material 60. The reaction formula at this time is shown, for example, in the following (3) and (4). SiO(g)+2CH4(g)=SiC(s)+CO(g)+4H2(g) (3) SiO(g)+C2H2(g)=SiC(s)+CO(g)+H2(g) (4)
[0035] As shown in the above reaction formulas (3) and (4), silicon oxide gas reacts with hydrocarbon to produce silicon carbide (silicon carbide fibrous material) and generate hydrogen gas.
[0036] The hydrogen generated by the above reactions (3) and (4) also plays a role in reacting with the substance (C) by the above reactions (1) and (2) to generate a hydrocarbon gas. In addition, since the container 50 is sealed, the generated hydrogen gas is unlikely to leak out of the container 50.
[0037] Furthermore, since gas is not circulated from the outside into the container 50, gas convection is unlikely to occur within the container 50. Therefore, it is believed that damage to the produced silicon carbide fibrous material due to gas convection is suppressed, and a silicon carbide fibrous material having a long fiber length can be obtained.
[0038] In addition, since silicon carbide layers 51a, 51b are formed on the surfaces of container 50 (the inner wall surface of container body 50a and the lower surface of lid portion 50b), silicon oxide gas [SiO(g)] generated in container 50 is also inhibited from reacting with container 50.
[0039] As described above, the reactions represented by the above reaction formulas (3) and (4) proceed efficiently inside the container 50, making it possible to obtain silicon carbide material having long fiber length without the need to supply hydrogen gas from the outside.
[0040] In the above description, methane (CH4) and acetylene (C2H2) are used as examples of the hydrocarbon gas generated by the substance (B) or substance (C), but in the method for producing a silicon carbide fibrous material of the present invention, the hydrocarbon gas is not limited to the above gases. For example, the hydrocarbon gas may be ethane (C2H6) or ethylene (C2H4).
[0041] The temperature to which the substances (A), (B), (C) and (D) sealed in the container (E) are heated is not particularly limited, but is preferably 1500 to 1700°C.
[0042] The means for heating the substances (A), (B), (C) and (D) sealed in the container (E) is not particularly limited, and for example, the container (E) may be heated from the outside with an electric heating wire or the like, or the container (E) itself may be heated. Methods for heating the container (E) itself include, for example, resistance heating and induction heating.
[0043] The atmosphere in which the substances (A), (B), (C) and (D) sealed in the container (E) are heated is preferably an inert atmosphere. Inert atmospheres include non-oxidizing atmospheres and reducing atmospheres.
[0044] The time for heating the substances (A), (B), (C) and (D) sealed in the container (E) can be appropriately adjusted depending on the amount of silicon carbide fibrous material to be obtained, and can be, for example, 1 to 5 hours.
[0045] In the method for producing a silicon carbide fibrous material of the present invention, the silicon carbide fibrous material obtained preferably has an average fiber length of 1 mm or more.
[0046] In the method for producing a silicon carbide fibrous material of the present invention, the silicon carbide fibrous material obtained preferably has an average fiber diameter of 0.5 to 10 μm.
[0047] In the method for producing a silicon carbide fibrous material of the present invention, the aspect ratio of the resulting silicon carbide fibrous material is preferably 1,000-50,000.
[0048] The material (A), material (B), material (C), material (D) and container (E) used in the method for producing a silicon carbide fibrous material of the present invention will be described below.
[0049] [Substance (A)] The substance (A) is a substance that generates silicon oxide gas when heated. Examples of the substance (A) include silicon dioxide, a mixture of silicon dioxide and carbon, and a mixture containing silicon carbide and silicon dioxide.
[0050] The material (A) is preferably a mixture containing silicon carbide and silicon dioxide. The mixing ratio of silicon carbide to silicon dioxide in the above mixture is preferably 10:1 to 1:2 (molar ratio).
[0051] When the substance (A) is a mixture containing silicon carbide and silicon dioxide, silicon oxide gas can be efficiently generated in a sealed container (E).
[0052] The substance (A) may be in the form of a powder or a lump.
[0053] In the mixture containing silicon carbide and silicon dioxide, the silicon carbide and silicon dioxide are preferably in a powdered state and uniformly mixed together, although the mixture may be in either powder or lump form.
[0054] The mixture containing silicon carbide and silicon dioxide is preferably in the form of a molded body.
[0055] [Substance (B)] Substance (B) is a substance that undergoes thermal decomposition to generate hydrogen or hydrocarbons. The substance (B) may be a phenol resin, a water-soluble alcohol, a polysaccharide, etc. Among these, the phenol resin is preferred. When the substance (B) is a phenol resin, hydrocarbons can be efficiently generated by thermal decomposition.
[0056] The substance (B) may be in the form of a powder or a lump.
[0057] The substance (B) may or may not be in contact with the substance (A) that generates silicon oxide gas.
[0058] [Substance (C)] The substance (C) is a carbonaceous substance. Examples of the substance (C) include graphite and amorphous carbon.
[0059] The material (C) is preferably graphite. If the substance (C) is graphite, it is likely to generate hydrocarbon gases by reacting with hydrogen gas.
[0060] The material (C) is preferably a graphite molded body. When the material (C) is a graphite molded body, the silicon carbide fibrous material formed on the graphite can be easily collected, and the material (B) and the material (D) can be uniformly coated on the graphite molded body.
[0061] The substance (C) does not have to be in contact with the substance (B), but it is preferable that the substance (C) is in contact with the substance (B). When substance (C) is in contact with substance (B), the hydrogen gas generated from substance (B) tends to react with substance (C) and be converted into hydrocarbon gas.
[0062] [Substance (D)] The substance (D) is a substance containing a transition metal. Examples of the transition metal contained in the substance (D) include iron, nickel, and cobalt. As the substance (D), it is preferable to use an oxide of the above transition metal. As the substance (D), two or more of the oxides of the above transition metals may be used in combination.
[0063] As the material (D), iron oxide and nickel oxide are preferred, and iron oxide is more preferred. Examples of iron oxide include FeO, Fe2O3, and Fe3O4, with Fe3O4 being preferred.
[0064] The substance (D) functions as a catalyst for the reaction in which silicon oxide gas and hydrocarbon gas undergo a gas-phase reaction to form a silicon carbide fibrous material. Therefore, it is preferred that substance (D) is in contact with either substance (A) which is a silicon oxide gas source, substance (B) which is a hydrogen or hydrocarbon gas source, or substance (C) which is a hydrocarbon gas source.
[0065] The substance (D) is preferably in powder form. When the substance (D) is in powder form, its surface area is increased and it is easy for it to act as a catalyst.
[0066] In the method for producing a silicon carbide fibrous material of the present invention, it is preferable that substance (B) is a phenolic resin, substance (D) is iron oxide, and the phenolic resin and iron oxide are formed as a coating layer on the surface of substance (C). When the phenolic resin and iron oxide are formed as a coating layer on the surface of the substance (C), the hydrocarbon gas generated from the phenolic resin and the substance (C) is likely to be present near the catalyst, and the reactions of the above reaction formulas (3) and (4) are likely to proceed. In addition, the hydrogen generated in the reaction formulas (3) and (4) is likely to react with the substance (C), so the reactions of the above reaction formulas (1) to (4) proceed continuously.
[0067] In this case, it is preferable that the iron oxide, which is the substance (D), is uniformly dispersed in the coating layer of the phenol resin, which is the substance (B).
[0068] [Container (E)] The container (E) is a container containing silicon carbide on its surface. The container (E) is preferably a container made of a carbon base material.
[0069] The shape and size of the container (E) can be appropriately determined depending on the amounts and arrangement of the substances (A), (B), (C) and (D) contained therein.
[0070] The container (E) may be made up of multiple parts. For example, the container (E) may include a container body that contains the substance (A), the substance (B), the substance (C) and the substance (D) and a lid that covers the upper part of the container body.
[0071] The surface of the container (E) contains silicon carbide. The surface of the container (E) is preferably provided with a silicon carbide layer containing silicon carbide. The thickness of the silicon carbide layer is not particularly limited, but is preferably 500 to 1500 μm.
[0072] The method for forming a silicon carbide layer on the surface of container (E) is not particularly limited, but examples thereof include a method of performing chemical vapor deposition using an organosilane gas, and a method of contacting a sheet-like material containing silicon carbide particles and silicon dioxide particles with the area where the silicon carbide layer is to be formed and heating it.
[0073] The surface of container (E) is the surface adjacent to the space containing substance (A), substance (B), substance (C) and substance (D). In other words, when substances (A), (B), (C) and (D) are contained inside container (E), the inner surface of container (E) must contain silicon carbide, but the outer surface of container (E) does not have to contain silicon carbide.
[0074] The present specification describes the following inventions:
[0075] The present disclosure (1) is a method for producing a silicon carbide fibrous material, characterized by heating a substance (A) that generates silicon oxide gas, a substance (B) that undergoes thermal decomposition to generate hydrogen or hydrocarbons, a carbonaceous substance (C), and a substance containing a transition metal (D) in a sealed container (E) containing silicon carbide on its surface.
[0076] The present disclosure (2) is a method for producing a silicon carbide fibrous material according to the present disclosure (1), wherein the material (A) is a mixture containing silicon carbide and silicon dioxide.
[0077] The present disclosure (3) is a method for producing a silicon carbide fibrous material according to the present disclosure (1) or (2), wherein the material (A) is a molded body containing silicon carbide and silicon dioxide.
[0078] The present disclosure (4) is a method for producing a silicon carbide fibrous material in any combination with any of the present disclosures (1) to (3), in which the material (C) is graphite.
[0079] The present disclosure (5) is a method for producing a silicon carbide fibrous material in any combination with any of the present disclosures (1) to (4), wherein the material (C) is a graphite molded body.
[0080] The present disclosure (6) is a method for producing a silicon carbide fibrous material in any combination with any of the present disclosures (1) to (5), in which the material (B) is a phenol resin.
[0081] The present disclosure (7) is a method for producing a silicon carbide fibrous material in any combination with any of the present disclosures (1) to (6), in which the material (D) is iron oxide.
[0082] The present disclosure (8) relates to a method for producing a phenolic resin, The substance (D) is iron oxide, The method for producing a silicon carbide fibrous material according to any combination of the present disclosure (1) to (7), wherein the phenol resin and the iron oxide are formed as a coating layer on the surface of the material (C).
[0083] The present disclosure (9) is a method for producing a silicon carbide fibrous material in any combination with any of the present disclosures (1) to (8), in which the material (A), the material (B), the material (C), and the material (D) are heated in the sealed container (E) under an inert atmosphere at a temperature of 1500 to 1700°C.
[0084] The present disclosure (10) is a method for producing a silicon carbide fibrous material in any combination with any of the present disclosures (1) to (9), in which the average length of the obtained silicon carbide fibrous material is 1 mm or more.
[0085] [Example] EXAMPLES Hereinafter, examples that more specifically disclose the present invention will be described, however, the present invention is not limited to these examples.
[0086] Example 1 A graphite crucible with inner dimensions of 170 mm length x 170 mm width x 43 mm height and 10 mm thickness was prepared, and a silicon carbide layer (600 μm thick) containing silicon carbide was formed on the inner surface by chemical vapor deposition using an organosilane gas to form the container body. Also, a silicon carbide layer (thickness 600 μm) containing silicon carbide was formed by chemical vapor deposition on one surface of a graphite flat plate measuring 190 mm in length × 190 mm in width × 10 mm in height (thickness) to serve as the lid of the container.
[0087] Inside the container body, two molded bodies (34.3 mm long x 102.3 mm wide x 34.3 mm high) [corresponding to substance (A)] made of a mixture of silicon carbide particles (average particle diameter 11 μm) and silicon dioxide particles (average particle diameter 40 μm) in a weight ratio of 63.3:11.2 were placed, along with a 30 mm long x 40 mm wide x 7 mm high graphite block [corresponding to substance (C)] with a coating layer formed on its surface of a mixture of 1 g of phenol resin [corresponding to substance (B)] and 100 mg of iron oxide Fe3O4 particles [corresponding to substance (D)]. The opening of the container was covered with a lid with the surface with the silicon carbide layer facing the opening, thereby sealing the container.
[0088] The sealed container was placed in a firing furnace, the pressure inside the furnace was reduced and then replaced with argon gas to create an argon atmosphere inside the furnace and container. Argon gas was then circulated through the furnace at a rate of 15 L / min, and the material was heated at a rate of 300°C / hour to a maximum temperature of 1550°C for 4.5 hours. When the surface of the graphite block was observed after heating, it was confirmed that fibrous silicon carbide had been formed. The results are shown in Figure 4.
[0089] FIG. 4 is a photograph showing the appearance of the silicon carbide fibrous material obtained in Example 1. As shown in FIG. 4, it was confirmed that silicon carbide fibrous material 60 having a fiber length of about 2 mm can be obtained by using the method for producing a silicon carbide fibrous material of the present invention.
[0090] FIG. 5 is a partially enlarged view of the silicon carbide fibrous material shown in FIG. It was confirmed from FIG. 5 that the obtained silicon carbide fibrous material 60 had a high aspect ratio, and was formed in large amounts around the coating layer containing the transition metal-containing material [material (D)].
[0091] FIG. 6 is a partially enlarged view of the silicon carbide fibrous material shown in FIG. It was confirmed from FIG. 6 that the fiber diameter of the silicon carbide fibrous material 60 was about 1 μm, and the aspect ratio of the obtained silicon carbide fibrous material was about 2,000.
[0092] From the above, it was confirmed that by using the method for producing silicon carbide fibrous material of the present invention, it is possible to obtain silicon carbide material with long fiber length without requiring the supply of hydrogen gas from an outside source. [Explanation of symbols]
[0093] 10 Molded body 20 Phenolic Resin 30 Graphite Block 40 Transition metal powder 50 containers 50a Container body 50b Lid 51a, 51b silicon carbide layer 60 Silicon carbide fibrous material
Claims
1. A method for producing a silicon carbide fibrous material, comprising heating a substance (A) that generates silicon oxide gas, a substance (B) that decomposes thermally to generate hydrogen or hydrocarbons, a carbonaceous substance (C), and a substance (D) containing a transition metal in a sealed container (E) containing silicon carbide on the surface.
2. The method for producing a silicon carbide fibrous material according to claim 1, wherein the material (A) is a mixture containing silicon carbide and silicon dioxide.
3. 3. A method for producing a silicon carbide fibrous material according to claim 1 or 2, wherein the material (A) is a molded body containing silicon carbide and silicon dioxide.
4. A method for producing a silicon carbide fibrous material according to claim 1 or 2, wherein the material (C) is graphite.
5. A method for producing a silicon carbide fibrous material according to claim 1 or 2, wherein the material (C) is a graphite molded body.
6. A method for producing a silicon carbide fibrous material according to claim 1 or 2, wherein the material (B) is a phenolic resin.
7. A method for producing a silicon carbide fibrous material according to claim 1 or 2, wherein the material (D) is iron oxide.
8. The substance (B) is a phenolic resin, The substance (D) is iron oxide, A method for producing a silicon carbide fibrous material according to claim 1 or 2, wherein the phenolic resin and the iron oxide are formed as a coating layer on the surface of the material (C).
9. A method for producing a silicon carbide fibrous material as described in claim 1 or 2, wherein the material (A), the material (B), the material (C) and the material (D) are heated in the sealed container (E) under an inert atmosphere at a temperature of 1500 to 1700°C.
10. A method for producing a silicon carbide fibrous material according to claim 1 or 2, wherein the average length of the obtained silicon carbide fibrous material is 1 mm or more.
Citation Information
Patent Citations
Preparation of silicon carbide whisker
JP1986295299A