Standing pouch and manufacturing method of the same

The standing pouch with a weak and strong seal configuration and two-step sealing process addresses the issue of weak drop impact resistance in all-polyolefin materials, reducing bag breakage and leakage by allowing the weak seal to peel off first, enhancing impact resistance.

JP2024134847AInactive Publication Date: 2024-10-04TOPPAN HOLDINGS INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023045252
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Standing pouches made of all-polyolefin materials face challenges with weak drop impact resistance, particularly at the intersection of the ridgeline of the bottom film and the side seal portion, leading to bag breakage and content leakage.

Method used

The standing pouch design incorporates a weak seal part and a strong seal part at the bottom seal, with a specific angle and curvature configuration, and a two-step sealing process to form these seals, ensuring the weak seal part peels off first under impact, reducing stress concentration and preventing bag breakage.

Benefits of technology

The design enhances drop impact resistance, minimizing bag breakage and content leakage by allowing the weak seal to peel off first, maintaining the pouch's integrity during falls.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134847000001_ABST
    Figure 2024134847000001_ABST
Patent Text Reader

Abstract

To provide an all-polyolefin standing pouch which has an excellent anti-drop impact property, and in which breakage is reduced in an intersection part between a ridge line of a ridge of a bottom film and a side seal part, and to provide a manufacturing method of the same.SOLUTION: A standing pouch comprises a surface side body film, a rear surface side body film, and a bottom film folded to a bottom surface, each of which has a base material layer and a sealant layer, respectively. The sealant layers of the surface side body film and the rear surface side body film are made to oppose to each other, the bottom film is inserted between these by being two-folded so that the sealant layer becomes the outside, and the opposing sealant layers are sealed with each other. A surface side bottom seal part and a rear surface side bottom seal part are divided into a weak seal part region and a strong seal part region, and they are continuously formed from a weak seal part to a strong seal part in this order toward an outer edge of the bottom film.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a standing pouch which reduces the occurrence of breakage of the pouch due to impact when dropped, even when a film having a relatively low rigidity such as a mono-material film is used, and to a method for producing the same. [Background technology]

[0002] Conventionally, a standing pouch has been generally known as a self-supporting packaging bag for accommodating contents such as liquids, powders, etc. For example, standing pouches for accommodating liquids and flowable substances such as beverages, shampoos, and seasonings are widely used.

[0003] This standing pouch is usually constructed by folding a bottom film and inserting it under a main film, then heat-bonding it to form a bottom seal and heat-bonding both sides of the main film to form side seals. The space formed by the main film and bottom film is filled with contents, and then the top of the standing pouch is heat-bonded to seal it. The bottom film is expanded during filling to form a self-supporting packaging bag. Many of them also have a pouring outlet formed in the upper corner.

[0004] In recent years, the weight of stand-up pouches has increased due to an increase in the volume of contents, and when a stand-up pouch is dropped, the impact of the drop causes the sealed portion of the bottom film to break, causing the contents to scatter and contaminate the surrounding area, and bag breakage when dropped has become a problem. Therefore, there is a demand for pouches that are strong enough not to break when dropped and cause liquid leakage, and to meet this demand, laminates combining highly rigid materials such as polyester film, nylon film, and polyolefin film have been used (see Patent Documents 1 and 2).

[0005] In recent years, however, there has been a demand for more efficient sorting and recovery of plastic materials and recycling due to growing environmental awareness triggered by the problem of marine plastic waste, etc. In other words, even in laminates for packaging, which have traditionally been made high-performance by combining various different materials, there is now a demand for mono-materialization, in which the laminates constituting the packaging material are made of materials of the same type and the packaging material is reused as an integrated material.

[0006] Polyolefin films such as polyethylene films are widely used as packaging materials, and there are high expectations for the mono-materialization of polyolefin films. In particular, in the case of materials made of all polyolefins, thorough recycling is effective in terms of sorting and recovery.

[0007] As mentioned above, conventional packaging materials have improved required physical properties such as impact resistance by combining various different materials. However, when the material is made of all-polyolefin, there is a problem that the resistance to drop impact is weak and the bag is prone to tearing at certain parts. In particular, the part that is prone to tearing is the part where the ridge of the bottom film folded in half intersects with the side seal part. This part is also the intersection where three seal parts intersect: the front side bottom seal part that seals the main film on the front side to the bottom film, the back side bottom seal part that seals the main film on the back side to the bottom film, and the side seal part.

[0008] When a self-supporting packaging bag is dropped vertically, the bottom film is pulled vertically downward, and the greatest impact is applied to the intersection 6 (shown in Figure 1) where the bottom seal and side seal meet, and this is the part where the film tends to break.

[0009] In Patent Document 3, the folding line of the bottom film is positioned within the bottom seal portion, thereby alleviating stress concentration at the seal intersection portion and aiming to improve strength. However, this standing pouch has two main films, the front and back, fused at the top end of the bottom film, so the starting point of the bottom film is fixed in a closed state, and there is a problem that the bottom is difficult to open. If the bottom is difficult to open, the self-supporting ability is also reduced, making the standing pouch very difficult to use.

[0010] In addition, it has been considered to improve the tensile strength and impact resistance of the bottom film by using a two-layer or three-layer structure, etc. However, increasing the number of layers leads to an increase in production costs, and while efforts are being made to reduce costs by making the film in the layer structure thinner, this reduces drop impact resistance.

[0011] Therefore, there is a demand for a standing pouch that has excellent drop impact resistance and reduces breakage even if it is made of a material with a relatively low rigidity, such as all-polyolefin. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] Japanese Patent Application Publication No. 7-237281 [Patent Document 2] Japanese Patent Application Publication No. 7-241967 [Patent Document 3] JP 2015-214352 A Summary of the Invention [Problem to be solved by the invention]

[0013] In view of the problems in the background art as described above, an object of the present invention is to provide an all-polyolefin standing pouch that has excellent resistance to drop impact and reduces bag breakage at the intersection between the ridgeline of the bottom film and the side seal portion, and a method for producing the same. [Means for solving the problem]

[0014] As a means for solving the above problems, the first aspect of the present invention is The package includes a front side main film, a back side main film, and a bottom film that is folded onto the bottom surface, each of which has a base layer and a sealant layer; A standing pouch is formed by placing the sealant layers of the front side main body film and the back side main body film opposite each other, folding the bottom film in half so that the sealant layer is on the outside and inserting it between them, and sealing the opposing sealant layers, a front-side bottom seal portion that seals the front-side main body film and the bottom film, a back-side bottom seal portion that seals the back-side main body film and the bottom film, and a side seal portion that seals the opposing sides of the front-side main body film and the back-side main body film, all intersect at one intersection; This standing pouch is characterized in that the front side bottom seal portion and the back side bottom seal portion are divided into a weak seal area and a strong seal area, and the weak seal area and the strong seal area are formed continuously in that order toward the outer edge of the bottom film.

[0015] By forming a weak seal portion in the boat-shaped bottom seal portion, the impact of a drop on the base material is mitigated by the peeling of the weak seal portion, thereby reducing the risk of the standing pouch breaking.

[0016] In addition, the second aspect is When the boundary between the weakly sealed portion and the unsealed portion is defined as a bottom seal line A, and the boundary between the strongly sealed portion and the weakly sealed portion is defined as a bottom seal line B, The bottom seal line A is a downward convex curve, and the bottom seal line B is a downward convex curve. and the curve is curved more gently than the bottom seal line A, the peaks of the two curves coincide, and both ends intersect with the intersection portion. The area surrounded by the bottom seal line A and the bottom seal line B is a weak seal portion, An angle θ between the ridge line of the bottom film extending from the intersection portion and the bottom seal line A may be 25 degrees or more and 35 degrees or less.

[0017] In addition, the third aspect is The peel strength of the strong seal part and the weak seal part may be 10:8 to 10:10. When the peel strength ratio of the strong seal part to the weak seal part is within this range, the shape is maintained without peeling even at the weak seal part during a filling process, etc., and when a strong impact is applied, such as when the pouch is dropped, the weak seal part partially peels off, preventing the standing pouch from breaking.

[0018] In addition, the fourth aspect is Peeling may start at the sealant layer of the main film and the bottom film at the weak seal portion. When the film is dropped, peeling starts from the sealant layer of the weak seal portion, so that the original breaking strength of the main film and the bottom film is maintained, and breakage of the film edge or the occurrence of pinholes can be suppressed.

[0019] In addition, the fifth aspect is The bottom seal portion forming line includes a first bottom seal process for sealing the bottom seal portion with a first bottom seal bar that matches the shape of the bottom seal line A, and a second bottom seal process for sealing with a second bottom seal bar that matches the shape of the bottom seal line B, This is a method for manufacturing a standing pouch, characterized in that a weak seal part is formed by the first bottom sealing process at the bottom seal position where two main body films and a bottom film folded in half are sealed, and then a strong seal part is overlapped and formed at the bottom seal position by the second bottom sealing process. This makes it possible to easily form a pouch by overlapping and sealing a seal bar having a seal shape of the weak seal part and a seal bar having a seal shape of the strong seal part, without requiring additional sealing in the bag making process. Effect of the Invention

[0020] According to the present invention, it is possible to provide an all-polyolefin standing pouch that has excellent resistance to drop impact and reduces bag breakage at the intersection between the ridgeline of the bottom film and the side seal portion, and a method for manufacturing the same. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a front view showing one embodiment of a standing pouch according to the present invention. [Diagram 2] FIG. 2 is an exploded perspective view showing an example of a film configuration of a standing pouch according to the present invention. [Diagram 3] FIG. 2 is an enlarged explanatory view of a portion in the vicinity of an intersection in FIG. [Figure 4] FIG. 2 is a schematic cross-sectional view showing an example of the layer structure of a main film and a bottom film. [Diagram 5] FIG. 2 is a diagram showing a bottom seal forming process in a bag making line. [Figure 6] 13 is a diagram showing the heating portions (protrusions) of the first bottom seal bar and the second bottom seal bar. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, an example of an embodiment of a standing pouch according to the present invention will be described with reference to the drawings.

[0023] Fig. 1 is a front view showing one embodiment of a standing pouch according to the present invention, Fig. 2 is an exploded perspective view showing an example of a film configuration of the standing pouch according to the present invention.

[0024] As shown in Figure 2, the standing pouch 1 is made up of two main films 2 and 3, one on the front and one on the back, and a bottom film 4. The main films 2 and 3 and the bottom film 4 are flexible films. The bottom film 4 is shown being inserted between the lower parts of the main films 2 and 3 while being folded.

[0025] As can be seen by referring to Figures 1 and 2, the folded bottom film 4 is inserted between the lower parts of the two main films 2, 3, and the main films 2, 3 and the bottom film 4 are sealed to form the front and back bottom seal parts 13, 14. Next, the side edges of the two main films 2, 3 are sealed to form the left and right side seal parts 11, 12. The bottom films 4 are sealed together at predetermined positions in the parts corresponding to the side seal parts 11, 12 of the front and back bottom seal parts 13, 14. In other words, the front and back main films are bonded together, giving the film self-supporting properties. When the contents are filled, the bottom film 4 is expanded by the pressure exerted on it by the weight of the contents.

[0026] After the contents are filled into the space formed by the front side main body film 2, the back side main body film 3, and the bottom film 4, the container is sealed by forming a top seal portion 15 by joining the upper edges of the front side main body film 2 and the back side main body film 3. The bottom film 4 expands when the contents are filled, thereby providing a three-dimensional shape as a container.

[0027] The films may be joined together by a known method such as heat fusion, pressure bonding, ultrasonic welding, or the like.

[0028] Figure 3 is a partially enlarged view of the vicinity of the intersection 6 between the ridge line 5 of the bottom film 4 and the side seal portion 11. The bottom seal portion 13 in Figure 3 is divided into a weakly sealed portion region (16) and a strongly sealed portion region (17), and if the boundary between the weakly sealed portion region (16) and the unsealed portion is defined as bottom seal line A, and the boundary between the strongly sealed portion region (17) and the weakly sealed portion region (16) is defined as bottom seal line B, bottom seal line A is a downward convex curve, and bottom seal line B is a downward convex curve that is more gently curved than bottom seal line A, the peaks C of the two curves coincide, and both ends intersect with intersection 6, and the area surrounded by bottom seal line A and bottom seal line B is the weakly sealed portion region (16).

[0029] In the case of an all-polyolefin material configuration, the bag has poor resistance to drop impact and is prone to tearing at certain locations. The location that is particularly prone to tearing is the intersection 6 where the ridge 5 of the bottom film 4, which is folded in half, intersects with the side seal portion 11. The intersection 6 in Figure 3 is also the part where three seal portions intersect together: the front side bottom seal portion 13, which seals the front side main film 2 and the bottom film 4, the back side bottom seal portion 14, which seals the back side main film 3 and the bottom film 4, and the side seal portion 11.

[0030] When the standing pouch 1 is dropped vertically, the bottom film 4 is pulled vertically downward and the greatest impact is applied to the intersection 6 where the bottom seal portions 13, 14 and the side seal portions 11, 12 are sealed and meet, and the film tends to break from this portion. This is thought to be because this portion is where the seal portions of the front side main film 2 and the back side main film 3, the front side main film 2 and the bottom film 4, and the back side main film 3 and the bottom film 4 come into contact, and pressure is likely to concentrate there.

[0031] As a result of various studies on the seal structure of the intersection 6, it was found that in the current bottom shape, the angle θ between the ridge 5 of the bottom film 4 and the bottom seal line A at the intersection 6 where the ridge 5 of the mountain of the bottom film 4 and the side seal portion 11 intersect is as steep as 47°. It was found that by specifying this angle to be between 25 degrees and 35 degrees, the probability of bag breakage at the intersection 6 between the ridge line 5 of the bottom film 4 and the side seal portion 11 is reduced.

[0032] The reason that this angle reduces the probability of bag breakage is that, normally, at an angle of 47°, the bottom seal line A is curved at a steep angle relative to the ridge line 5 of the bottom film 4, resulting in high tensile stress in the width direction. With a shape specified at an angle of 25° or more and 35° or less, the curve is gentler and the tensile stress in the width direction is smaller, making it harder for peeling to occur at the intersection 6 and preventing bag breakage.

[0033] Furthermore, the standing pouch 1 of the present invention has the front side bottom seal portion 13 and the back side bottom seal portion 14 divided into a weak seal portion area (16) and a strong seal portion area (17). Therefore, even if the bottom film 4 is pulled vertically downward when dropped and the bottom seal portions 13, 14 peel off due to the tensile stress, peeling will first begin at the sealant surface of the weak seal portion area (16), which relieves the force tending to peel off in the width direction. As a result, even if the pouch peels off, it will not reach the edge of the strong seal portion, and tearing of the bag at the intersection 6 is prevented.

[0034] Furthermore, by combining the specification of the shape of the bottom seal portion of the bottom film with the formation of the weak seal portion as described above, it is possible to further suppress the occurrence of tearing of the sealant layer of the bottom film at the intersections.

[0035] FIG. 5 is a diagram showing the bottom seal forming process in a bag making line. This bag making line is a two-row line, and is equipped with a first bottom sealing process and a second bottom sealing process for standing pouches. In a continuous motion, two main body films 2, 3 are fed from the right side, and a bottom film 4 is fed while being folded, and while the bottom film 4 is inserted between the two main body films 2, 3, they are overlapped by a nip roll (not shown). The continuous motion is switched to an intermittent motion by a dancer roll (not shown), and the process proceeds to the first bottom sealing process. The direction of the intermittent motion is indicated by an arrow, and it is driven from right to left in the figure.

[0036] First, in the first bottom sealing process, the weakly sealed area (16) of the bottom seal parts 13, 14 is formed. To weakly seal the bottom film 4 and the main films 2, 3, a first bottom seal bar 31 whose shape matches the shape of the bottom seal line A is used for sealing. Specifically, a first bottom seal bar 31 capable of moving up and down is placed above the two main films 2, 3, on the front and back, and the first bottom seal bar 31 descends to heat and pressurize the main films 2, 3 and bottom film 4, which have been advancing with intermittent motion, to form a seal, and then the first bottom seal bar 31 rises, and the main films 2, 3 and bottom film 4 advance to the next process with intermittent motion.

[0037] Next, in the second bottom sealing process, the strong seal area (17) is formed. After the first bottom sealing process, the main body films 2, 3 and bottom film 4 are fed with an intermittent motion and aligned to the same position as when they were sealed in the first bottom sealing process, and are heat-sealed using the second bottom sealing bar 32 so that they overlap the weak seal area (16). The first and second bottom sealing processes are performed simultaneously, and the strong seal area (17) is formed overlapping the weak seal area (16) by the two sealing processes. Figure 6 shows the shapes of the protruding parts that heat the first bottom sealing bar 31 and the second bottom sealing bar 32. As shown in the figure, the shapes of the downwardly convex curved parts are different.

[0038] In order to vary the seal strength, it is sufficient to differentiate the seal conditions by varying the heating temperature or heating time. Specifically, the first bottom seal bar 31 is heated for a short time or at a low temperature to form the weak seal area (16), and the second bottom seal bar 32 is heated for a long time or at a high temperature to form the strong seal area (17). The seal strength of the strong seal area (17) may be equal to the side seal strength, and the seal strength ratio with the weak seal area (16) is preferably 10:8 to 10:10. When the peel strength ratio between the weak seal area and the strong seal area is within this range, the shape is maintained without peeling even in the weak seal area during the filling process, etc., and when a strong impact such as a drop is applied, the weak seal area partially peels off, and even if the weak seal area peels off, it does not reach the edge of the strong seal area, so that the impact mitigation effect can be maintained.

[0039] Fig. 4 is an explanatory diagram showing an example of the layer structure of the main body films 2, 3 and the bottom film 4. The main body films 2, 3 and the bottom film 4 are made of a flexible laminate 20. As shown in Fig. 4, the laminate 20 is made of a base material layer 21 and a sealant layer 22 laminated with an adhesive layer 23 interposed therebetween. The laminate 20 has a layer structure of base material layer 21 / adhesive layer 23 / sealant layer 22.

[0040] The standing pouch 1 according to the present invention is made entirely of polyolefin. The main body films 2 and 3 are a mono-material laminate 20 in which the base material layer 21 and the sealant layer 22 are all made of a polyethylene resin.

[0041] High density polyethylene can be used as the polyolefin resin for the base layer 21 of the main body films 2 and 3. Either stretched or unstretched may be used, but a biaxially stretched film is preferably used. By using a high density polyethylene resin for the base layer 21 of the main body films 2 and 3, the high rigidity of the high density polyethylene resin can provide sufficient strength for the standing pouch 1 to stand on its own. Taking processability into consideration, the thickness of the base layer 21 is preferably in the range of 10 to 50 μm.

[0042] The polyolefin resin for the sealant layer 22 of the main film 2, 3 may be a film made of low density polyethylene, linear low density polyethylene, medium density polyethylene, or high density polyethylene. The sealant layer 22 can be formed by forming a layer on the base layer 21 using a molten resin by using an extruder or the like. Alternatively, the sealant layer 22 can be formed on the surface of the base layer 21 by laminating a material that has already been formed into a film state with an adhesive.

[0043] The bottom film 4 is also a mono-material laminate 20 in which the base layer 21 and the sealant layer 22 are all made of polyolefin resins, just like the main films 2 and 3. A multi-layered structure of polyethylene resins can be used. Examples of the polyethylene resins of the bottom film 4 include low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, high-density polyethylene, and ultra-high molecular weight polyethylene. The bottom film 4 can be formed by multi-layering using these resins. As a method for forming it into a sheet, a sheet can be formed by extrusion molding using an extruder or multi-layer extrusion molding using a co-extruder. The thickness of the bottom film 4 can be appropriately determined based on the thickness of the main films 2 and 3.

[0044] A non-solvent laminating adhesive or a dry laminating adhesive can be used as the adhesive layer 23. Examples of such adhesives include a two-component curing urethane adhesive, a polyester urethane adhesive, a polyether urethane adhesive, an acrylic adhesive, a polyester adhesive, a polyamide adhesive, and an epoxy adhesive. The laminating method can be a dry laminating method.

[0045] Furthermore, a printing layer can be provided on the base material layer 21 as necessary. This printing layer can be used to form characters, pictures, and the like. Examples of printing methods include offset printing, gravure printing, flexographic printing, silk screen printing, and inkjet printing. Any known printing method can be used.

[0046] Furthermore, if it is necessary to improve various physical properties of the laminate 20, an intermediate layer can be provided in the laminate 20. For example, an intermediate layer that can improve the oxygen gas barrier and water vapor barrier can be provided. To improve the oxygen gas barrier and water vapor barrier, aluminum foil, aluminum-deposited polyethylene terephthalate film, inorganic oxide-deposited polyethylene terephthalate film, etc. can be used. To laminate the intermediate layer, the layers can be bonded together by a dry lamination method via an adhesive layer 22.

[0047] Examples of inorganic oxides that can be used include metal oxides such as silicon oxide, aluminum oxide, magnesium oxide, calcium oxide, potassium oxide, tin oxide, sodium oxide, boron oxide, titanium oxide, lead oxide, zinc dioxide, and yttrium oxide. Among these, silicon oxide, aluminum oxide, and magnesium oxide are preferred in terms of productivity and cost.

[0048] Specific examples of the present invention will now be described. EXAMPLES

[0049] <Example 1> For the front side main body film 2, the back side main body film 3, and the bottom film 4, an all-polyethylene laminate having the following layer structure was used. High density polyethylene (12μm) / Dry lamination / Linear low density polyethylene (60μm) The above laminate was used to produce the standing pouch shown below. External dimensions: Width 145mm, height 220mm, bottom film fold 41mm, seal width 5mm. Bottom seal shape: Weak seal part R50mm, strong seal part R60mm. Here, R indicates the radius of the curved portion of the bottom seal. Seal strength: Weak seal area 32N / 15mm Peeling mode: Bottom film sealant layer surface-to-surface peeling. : Strong seal area 35N / 15mm Peeling mode: Bottom film substrate seal edge cut.

[0050] <Comparative Example 1> The bottom seal shape is the same as in Example 1, except that it is a strong seal part only and has a radius of 60 mm. (Seal incidence angle θ=38° for strong seal only) Here, θ indicates the angle (incidence angle) between the bottom tape fold and the bottom seal curve (normal) at the intersection of the main body and the base material.

[0051] <Comparative Example 2> The shape of the bottom seal is the same as in Example 1, except that the weak seal part has a radius of 50 mm and the strong seal part has a radius of 70 mm. (Strong seal θ=32°) Peeling mode: Bottom film substrate seal edge cut.

[0052] <Evaluation method> The standing pouches of Example 1 and Comparative Examples 1 and 2 were filled with 400 cc of cold water at 5°C. 20 pouches of each were made. The standing pouches were dropped 10 times from a height of 100 cm, and the presence or absence of breakage of the pouches was confirmed and the number of breakages was counted. The results of the frequency of sealant tears at the intersections are shown in Table 1.

[0053] [Table 1]

[0054] No breakage was observed in the standing pouch of Example 1. However, breakage was observed in the pouch of Comparative Example 1. Breaks were observed in 7 bags in Comparative Example 1 and 2 bags in Comparative Example 2. As can be seen from the above results, the drop test confirmed that the standing pouch of the present invention can reduce breakage at the intersection of the ridgeline of the bottom film and the bottom seal portion. [Explanation of symbols]

[0055] 1···Standing pouch 2. Surface side main body film 3 Back side body film 4. Bottom film 5. Bottom film ridge 6. The intersection of the ridge of the bottom film and the bottom seal 11 Side seal part (left side) 12 Side seal part (right side) 13 Bottom seal part (surface side) 14 Bottom seal part (reverse side) 15 Top seal part (16) Weak seal area (17) Strong seal area 20...Laminate 21...Base material layer 22...Sealant layer 23...Adhesive layer 30 Bottom seal forming line 31...First bottom seal bar 32...Second bottom seal bar θ: The angle between the ridge of the bottom film and the bottom seal line A A Bottom seal line A B Bottom seal line B C Peak of the two curves

Claims

1. The package includes a front side main film, a back side main film, and a bottom film that is folded onto the bottom surface, each of which has a base layer and a sealant layer; A standing pouch is formed by placing the sealant layers of the front side main body film and the back side main body film opposite each other, folding the bottom film in half so that the sealant layer is on the outside and inserting it between them, and sealing the opposing sealant layers, a front-side bottom seal portion that seals the front-side main body film and the bottom film, a back-side bottom seal portion that seals the back-side main body film and the bottom film, and a side seal portion that seals the opposing sides of the front-side main body film and the back-side main body film, all intersect at one intersection; A standing pouch characterized in that the front side bottom seal portion and the back side bottom seal portion are divided into a weak seal portion area and a strong seal portion area, and the weak seal portion and the strong seal portion are formed continuously in that order toward the outer edge of the bottom film.

2. When the boundary between the weakly sealed portion and the unsealed portion is defined as a bottom seal line A, and the boundary between the strongly sealed portion and the weakly sealed portion is defined as a bottom seal line B, The bottom seal line A is a downwardly convex arc curve, the bottom seal line B is a downwardly convex arc curve, and is curved more gently than the bottom seal line A, the peaks of the two curves coincide, and both ends intersect with the intersection point, The area surrounded by the bottom seal line A and the bottom seal line B is a weak seal portion, 2. The standing pouch according to claim 1, wherein an angle θ between the ridge line of the bottom film extending from the intersection portion and the bottom seal line A is 25 degrees or more and 35 degrees or less.

3. 2. The standing pouch according to claim 1, wherein the peel strength of the strong seal portion and the weak seal portion is 10:8 to 10:

10.

4. 2. The standing pouch according to claim 1, wherein peeling starts at the sealant layer between the main film and the bottom film at the weak seal portion.

5. A method for producing the standing pouch of claim 2, comprising the steps of: The bottom seal portion forming line includes a first bottom seal process for sealing the bottom seal portion with a first bottom seal bar that matches the shape of the bottom seal line A, and a second bottom seal process for sealing with a second bottom seal bar that matches the shape of the bottom seal line B, A method for manufacturing a standing pouch, comprising forming a weak seal portion by the first bottom sealing process at a bottom seal position where two main body films and a bottom film folded in half are sealed, and then forming a strong seal portion by the second bottom sealing process at the bottom seal position.

Citation Information

Patent Citations

  • Standing pouch

    JP1995237281A

  • Standing pouch

    JP1995241967A

  • Standing pouch and manufacturing method of the same

    JP2015214352A