Polyamide porous membrane, filtration membrane module, and oil-water separation method

A polyamide porous membrane with a 0.45 MPa initial bubble point effectively separates oil and water from mixed liquids, including emulsions, addressing the limitations of conventional membranes by achieving high separation efficiency and compact design.

JP2024134979APending Publication Date: 2024-10-04UNITIKA LTD

Patent Information

Application Number
JP2023045451
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Conventional polyamide separation membranes are ineffective in separating oil and water from mixed liquids, particularly emulsions, due to their inability to handle small water droplets, limiting their application in oil-water separation processes.

Method used

Development of a polyamide porous membrane with an initial bubble point of 0.45 MPa or more, capable of effectively separating oil and water from mixed liquids, including emulsions, by utilizing a polyamide resin with specific properties and optional fillers to enhance durability and separation efficiency.

Benefits of technology

The membrane achieves high separation efficiency with an 80% or more removal rate of water droplets in water-in-oil emulsions, even with very small droplet sizes, at low cost and energy consumption, and in a compact design.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134979000002
    Figure 2024134979000002
  • Figure 2024134979000003
    Figure 2024134979000003
  • Figure 2024134979000001
    Figure 2024134979000001
Patent Text Reader

Abstract

To provide a polyamide porous membrane for oil-water separating a mixed liquid containing water and oil, a filtration membrane module using the polyamide porous membrane, and an oil-water separation method using the filtration membrane module.SOLUTION: A polyamide porous membrane is a polyamide porous membrane for oil-water separation of a mixed liquid containing water and oil, wherein the polyamide porous membrane is formed of a polyamide resin, and has an initial bubble point in a bubble point test added with a pneumatic pressure in 2-propanol at 20°C of 0.45 MPa or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyamide porous membrane for oil-water separation of a mixed liquid containing water and oil. [Background technology]

[0002] Examples of oils used in machining processes such as metal cutting and polishing, and oils discharged from various machines and devices include cutting oil, cleaning oil, lubricating oil, machine oil, compressor oil, etc. Water may become mixed into these oils during use, and it is necessary to remove the water from these oils that contain water (hereinafter also referred to as "water-containing oils") in order to reuse them.

[0003] Furthermore, from the viewpoint of environmental conservation, etc., it is common for oil-water mixtures containing oil and turbidity (hereinafter also referred to as "produced water") generated during the extraction of crude oil, bitumen, natural gas, etc., to be discharged after the oil and turbidity content is reduced to a certain value or less before being re-injected into oil fields, gas fields, aquifers, etc. In particular, in areas with water shortages, where it is not possible to secure a sufficient amount of water for use in water flooding, there are an increasing number of cases where treated water from which oil and turbidity have been removed from produced water is reused as injection water.

[0004] Methods for removing water from water-containing oil and oil from produced water usually involve heating and using a coalescer to separate oil and water by coarsening droplets and using the difference in specific gravity, but the heating method has the disadvantage of high separation costs and the coalescer requires a large amount of space due to the large size of the device. Therefore, there is a need for a technology that can separate oil and water at a high level with low cost, low energy consumption, and space saving.

[0005] On the other hand, membrane separation technology can be applied to separate chemical species with various molecular weights in liquid and gas phases, and can perform separation processing at low cost, with low energy consumption, and in a small space; therefore, it is widely used in separation processes in various industrial fields.

[0006] The separation membranes used in membrane separation processing technology are mainly polymer membranes because they are relatively easy to mold, an inexpensive mass production process can be easily established, and they are lightweight, flexible, and easy to handle. In particular, polyamide separation membranes, which have excellent resistance to organic solvents, are preferably used.

[0007] For example, Patent Document 1 discloses a composite hollow fiber membrane that can perform separation suitably using a semipermeable membrane layer and has excellent durability, the composite hollow fiber membrane comprising a semipermeable membrane layer containing a crosslinked polyamide, a hollow fiber-shaped porous support layer, and an intermediate layer interposed between the semipermeable membrane layer and the support layer.

[0008] Patent Document 2 discloses a hollow fiber membrane having high water permeability or high moisture permeability and high selectivity, which contains 70% by weight or more of at least one aliphatic polyamide selected from the group consisting of polyamide 4, polyamide 6, polyamide 11, polyamide 12, polyamide 46, polyamide 66, and polyamide 610.

[0009] Furthermore, Patent Document 3 discloses an asymmetric semipermeable membrane that is a separation membrane capable of realizing high water permeability and rejection rate and contains a polyamide having a specific chemical structure. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] International Publication No. 2020 / 175205 [Patent Document 2] JP 2015-198999 A [Patent Document 3] JP 2014-144438 A Summary of the Invention [Problem to be solved by the invention]

[0011] However, these conventional polyamide separation membranes are generally used for the removal of bacteria and viruses in water purification, the separation or concentration of heat-sensitive substances such as proteins and enzymes in the industrial field, the removal of viruses and proteins in artificial dialysis and the production of pharmaceuticals and medical water in the medical field, the production of ultrapure water, the recovery of electrodeposition paint, wastewater treatment in silk and pulp factories, treatment of building wastewater, clarification of fruit juice, the production of unpasteurized sake, the concentration and desalination of cheese whey, the production of concentrated milk, the concentration of egg whites, and the like, and due to the characteristics of the separation membranes, they have not been used for oil-water separation of mixed liquids containing water and oil, such as the above-mentioned water-containing oil and the above-mentioned associated water.

[0012] In particular, when a mixed liquid containing water and oil, such as the water-containing oil or the associated water, is an emulsion, it was thought that it was impossible for conventional polyamide separation membranes to separate and remove water droplets or oil droplets in the emulsion, due to the characteristics of the separation membrane.

[0013] The present invention aims to solve the above-mentioned problems in the prior art, and has as its main object to provide a polyamide porous membrane for oil-water separation of a mixed liquid containing water and oil, and a filtration membrane module using the polyamide porous membrane. Another object of the present invention is to provide an oil-water separation method using the filtration membrane module. [Means for solving the problem]

[0014] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that a polyamide porous membrane having an initial bubble point of 0.45 MPa or more in a bubble point test in which air pressure is applied in 2-propanol at 20°C can achieve high oil-water separation of a mixture containing water and oil. The present invention has been completed through further research based on this knowledge.

[0015] That is, the present invention provides the following aspects. Item 1. A polyamide porous membrane for oil-water separation of a mixed liquid containing water and oil, The polyamide porous membrane is formed of a polyamide resin, and A polyamide porous membrane having an initial bubble point of 0.45 MPa or more in a bubble point test in which air pressure is applied in 2-propanol at 20°C. Item 2. The polyamide porous membrane according to Item 1, which has a burst bubble point of 0.50 to 0.90 MPa in the bubble point test. Item 3. The polyamide porous membrane according to Item 1 or 2, wherein the oil is a hydrocarbon oil. Item 4. The polyamide porous membrane according to any one of Items 1 to 3, wherein the mixed liquid is an emulsion. Item 5. The polyamide porous membrane according to Item 4, wherein the emulsion is a water-in-oil emulsion. Item 6. The polyamide porous membrane according to Item 5, wherein the water droplets in the water-in-oil emulsion have an average droplet diameter of 0.5 to 5 μm. Item 7. For separating oil and water from water-in-oil emulsions. Item 7. The polyamide porous membrane according to any one of Items 1 to 6, wherein the polyamide porous membrane has a water-in-oil emulsion containing 94% by weight of isoparaffin oil, 1% by weight of water, and 5% by weight of a surfactant having an HLB value of 7, and has a water droplet removal rate of 80% or more when filtering a water-in-oil emulsion having an average water droplet diameter of 1.2 μm. Item 8. For separating oil and water from water-in-oil emulsions. Item 8. The polyamide porous membrane according to any one of Items 1 to 7, wherein the polyamide porous membrane has a water-in-oil emulsion containing 85% by weight of isoparaffin oil, 10% by weight of water, and 5% by weight of a surfactant having an HLB value of 7, and has a water droplet removal rate of 80% or more when filtering a water-in-oil emulsion having an average water droplet diameter of 2.3 μm. Item 9. For separating oil and water from water-in-oil emulsions. Item 9. The polyamide porous membrane according to any one of Items 1 to 8, wherein the polyamide porous membrane has a water-in-oil emulsion containing 94% by weight of paraffin oil, 1% by weight of water, and 5% by weight of a surfactant having an HLB value of 7, and having an average water droplet diameter of 1.3 μm, when filtered, has a water droplet removal rate of 80% or more. Item 10. For separating oil and water from water-in-oil emulsions. Item 10. The polyamide porous membrane according to any one of Items 1 to 9, wherein the polyamide porous membrane has a water-in-oil emulsion containing 85% by weight of paraffin oil, 10% by weight of water, and 5% by weight of a surfactant having an HLB value of 7, and having an average water droplet diameter of 2.4 μm, has a water droplet removal rate of 80% or more when the water-in-oil emulsion is filtered. Item 11. The polyamide porous membrane according to any one of Items 1 to 10, wherein the polyamide porous membrane is a polyamide hollow fiber membrane. Item 12. The polyamide porous film according to any one of Items 1 to 11, wherein the polyamide resin is polyamide 6. Item 13. A filtration membrane module comprising a module case and the polyamide porous membrane according to any one of Items 1 to 12 housed therein. Item 14. An oil-water separation method, comprising separating a mixed liquid containing water and oil into oil and water using the filtration membrane module according to item 13. Effect of the Invention

[0016] The polyamide porous membrane of the present invention has an initial bubble point of 0.45 MPa or more in a bubble point test in which air pressure is applied in 2-propanol at 20°C, and therefore can perform high-level oil-water separation of a mixed liquid containing water and oil. Therefore, by using the polyamide porous membrane of the present invention, the water-containing oil and the associated water can be separated into oil and water at low cost, with low energy, and in a small space. Furthermore, by using the polyamide porous membrane of the present invention, high-level oil-water separation can be performed even when the water-containing oil and the associated water are an emulsion, and even when the emulsion has very small droplets. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic diagram of an apparatus used for measuring bubble point. [Diagram 2] FIG. 1 is a schematic diagram of an apparatus used for measuring the removal rate of water droplets in a water-in-oil emulsion and the permeation flow rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] 1.Polyamide porous membrane The polyamide porous membrane of the present invention is a polyamide porous membrane formed from a polyamide resin, and is characterized in that the initial bubble point is 0.45 MPa or more in a bubble point test in which air pressure is applied in 2-propanol at 20° C. The polyamide porous membrane of the present invention will be described in detail below.

[0019] [Forming material] The type of polyamide resin forming the polyamide porous membrane of the present invention is not particularly limited, and examples thereof include polyamide homopolymers, polyamide copolymers, and mixtures thereof. Specific examples of polyamide homopolymers include polyamide 6, polyamide 66, polyamide 46, polyamide 610, polyamide 612, polyamide 11, polyamide 12, polyamide MXD6, polyamide 4T, polyamide 6T, polyamide 9T, and polyamide 10T. Specific examples of polyamide copolymers include copolymers of polyamide and polyethers such as polytetramethylene glycol or polyethylene glycol. The ratio of the polyamide component in the polyamide copolymer is not particularly limited, and examples of the ratio of the polyamide component are preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and particularly preferably 95 mol% or more. By satisfying the above range of the ratio of the polyamide component in the polyamide copolymer, it is possible to provide excellent durability. The polyamide resin may be used alone or in combination of two or more kinds.

[0020] Among these polyamide resins, polyamide 6 is preferably used as a resin for forming the polyamide porous membrane of the present invention, since it is easy to produce a polyamide porous membrane having an initial bubble point of 0.45 MPa or more as specified in the present invention, and it is easy to improve the liquid permeability.

[0021] The polyamide resin may be crosslinked or not, but from the viewpoint of reducing production costs, a non-crosslinked polyamide resin is preferred.

[0022] The relative viscosity of the polyamide resin is not particularly limited, but may be, for example, 2.0 to 7.0, preferably 3.0 to 6.0, and more preferably 2.0 to 4.0. By providing such a relative viscosity, the moldability and controllability of phase separation during the production of the polyamide porous membrane are improved, and it is possible to provide the polyamide porous membrane with excellent shape stability. Here, the relative viscosity refers to a value measured by an Ubbelohde viscometer at 25°C using a solution in which 1 g of polyamide resin is dissolved in 100 mL of 96% sulfuric acid.

[0023] In addition to the polyamide resin, the polyamide porous membrane of the present invention may contain a filler as necessary within a range that does not impair the effects of the present invention. By containing a filler, the strength, elongation, and elastic modulus of the polyamide porous membrane can be improved. In particular, by containing a filler, the polyamide porous membrane is less likely to deform even when high pressure is applied during filtration. The type of filler to be added is not particularly limited, and examples thereof include fibrous fillers such as glass fiber, carbon fiber, potassium titanate whisker, zinc oxide whisker, calcium carbonate whisker, wollastonite whisker, aluminum borate whisker, aramid fiber, alumina fiber, silicon carbide fiber, ceramic fiber, asbestos fiber, gypsum fiber, and metal fiber; talc, hydrotalcite, wollastonite, zeolite, sericite, mica, kaolin, clay, pyrophyllite, bentonite, asbestos, and the like. Examples of the filler include silicates such as sulphur oxide and alumina silicate; metal compounds such as silicon oxide, magnesium oxide, alumina, zirconium oxide, titanium oxide, and iron oxide; carbonates such as calcium carbonate, magnesium carbonate, and dolomite; sulfates such as calcium sulfate and barium sulfate; metal hydroxides such as calcium hydroxide, magnesium hydroxide, and aluminum hydroxide; and inorganic materials such as non-fibrous fillers such as glass beads, glass flakes, glass powder, ceramic beads, boron nitride, silicon carbide, carbon black, silica, and graphite. These fillers may be used alone or in combination of two or more. Among these fillers, preferred are talc, hydrotalcite, silica, clay, and titanium oxide, and more preferred are talc and clay. The content of the filler is not particularly limited, but may be, for example, 5 to 100 parts by weight, preferably 10 to 75 parts by weight, and more preferably 25 to 50 parts by weight of the filler per 100 parts by weight of the polyamide resin. By including the filler in such a content, the strength, elongation, and elastic modulus of the polyamide porous film can be improved.

[0024] The polyamide porous membrane of the present invention may contain additives such as thickeners, antioxidants, surface modifiers, lubricants, and surfactants, as necessary, for the purpose of pore size control and improvement of membrane performance.

[0025] [shape] The shape of the polyamide porous membrane of the present invention is not particularly limited and can be selected from any shape such as a hollow fiber membrane or a flat membrane. A hollow fiber membrane is preferred in the present invention because it has a large filtration area per unit volume of the module and enables efficient filtration processing.

[0026] When the polyamide porous membrane of the present invention is a hollow fiber membrane, its outer diameter is appropriately set according to the water or oil permeability to be provided, but in consideration of the relationship between the effective membrane area when filled in a module, the membrane strength, the pressure loss of the fluid flowing through the hollow part, and the buckling pressure, the outer diameter of the porous membrane is 400 μm or more, preferably 450 to 4000 μm, and more preferably 500 to 3500 μm. Furthermore, when the polyamide porous membrane of the present invention is a hollow fiber membrane, its inner diameter is not particularly limited, but for example, 100 to 3000 μm, preferably 200 to 2500 μm, more preferably 300 to 2000 μm, and even more preferably 300 to 1500 μm. In the present invention, the outer diameter and inner diameter of the porous membrane are values ​​obtained by observing five porous membranes with an optical microscope at a magnification of 200 times, measuring the outer diameter and inner diameter of each porous membrane (both at the point where the diameter is maximum), and calculating the average value of each.

[0027] The thickness of the polyamide porous membrane of the present invention is appropriately set depending on the shape, liquid permeability, etc. of the polyamide porous membrane, and is, for example, 50 to 600 μm, preferably 100 to 350 μm. When the polyamide porous membrane of the present invention is a hollow fiber membrane, the thickness is a value calculated by subtracting the inner diameter from the outer diameter and dividing the value by 2.

[0028] [Bubble Point] The polyamide porous membrane of the present invention has an initial bubble point of 0.45 MPa or more in a bubble point test in which air pressure is applied in 2-propanol at 20°C. The polyamide porous membrane of the present invention having an initial bubble point of 0.45 MPa or more can separate a mixture containing water and oil into oil and water to a high degree. In addition, the polyamide porous membrane of the present invention having an initial bubble point of 0.45 MPa or more can separate oil and water to a high degree even if the mixture containing water and oil is an emulsion, or even if the mixture is an emulsion containing very small droplets with an average droplet diameter of 0.5 to 5 μm. From the viewpoint of more highly separating oil and water from a mixture containing water and oil, particularly an emulsion, the polyamide porous membrane of the present invention has an initial bubble point of preferably 0.50 to 0.80 MPa, more preferably 0.55 to 0.80 MPa, even more preferably 0.60 to 0.80 MPa, and even more preferably 0.70 to 0.80 MPa.

[0029] Furthermore, in the bubble point test, the polyamide porous membrane of the present invention has a burst bubble point of preferably 0.50 to 0.90 MPa, more preferably 0.55 to 0.85 MPa, even more preferably 0.60 to 0.85 MPa, still more preferably 0.70 to 0.85 MPa or less, and particularly preferably 0.70 to 0.80 MPa, from the viewpoint of achieving a higher degree of oil-water separation in a mixed liquid containing water and oil, particularly an emulsion, and from the viewpoint of suppressing clogging of pores.

[0030] The polyamide porous membrane of the present invention having the above-mentioned initial bubble point and burst bubble point can be produced by the method for producing a polyamide porous membrane described below.

[0031] In the present invention, the bubble point test is a measurement method generally used to determine the maximum pore size, and is widely used to estimate pore size because the measurement is simple and can be performed quickly. The principle and method of the bubble point test are described in JIS standard K3832.

[0032] When the polyamide porous membrane of the present invention is a hollow fiber membrane, the initial bubble point and burst bubble point are values ​​measured by the following procedure using the device shown in the schematic diagram of FIG. 1. First, a hollow fiber membrane mini-module 6 for measuring the initial bubble point and burst bubble point is prepared. Specifically, 10 hollow fiber membranes are cut to a length of 20 cm, bundled together, and bent into a U-shape, and the end of about 1 cm on the side of the opening of the hollow fiber membrane is heat-sealed to block the hollow part, and a hollow fiber membrane bundle is prepared. Next, a 5 cm long soft nylon tube for air piping (outer diameter 8 mm, inner diameter 6 mm) is prepared, and one of the openings is blocked with a silicone plug to plug it. Next, the end of the nylon tube with the silicone plug attached is placed down, and a potting agent (polyurethane resin) is introduced into the nylon tube to a height of about 4 cm. Then, the hollow fiber membrane bundle is inserted into a nylon tube from the heat-sealed end, and a part of the hollow fiber membrane bundle is immersed in the potting agent and left to stand until the potting agent hardens. After hardening, the hollow fiber membrane bundle is cut above the heat-sealed portion to open the hollow part of the hollow fiber membrane. At this time, it is visually confirmed whether the potting agent has penetrated into the hollow part and whether the potting agent is filled between the hollow fiber membranes. After confirming that the hollow is maintained without any problems, the initial bubble point and burst bubble point are measured. Next, the initial bubble point and burst bubble point of the hollow fiber membrane are measured using the device shown in the schematic diagram of Figure 1. Specifically, 2-propanol is introduced into a glass container 7, the hollow fiber membrane mini-module 6 prepared above is immersed therein, and the pressure is reduced for several seconds to fill the holes with the liquid. After that, the hollow fiber membrane mini-module 6 immersed in 2-propanol is set as shown in Figure 1, and air is pumped into the hollow fiber membrane at 0.4 MPa / min to increase the pressure. The pressure is measured when bubbles first appear in the hollow fiber membrane, and this is taken as the initial bubble point. The pressure is then continued to be increased, and the pressure is measured when bubbles appear throughout almost the entire hollow fiber membrane, and this is taken as the burst bubble point.

[0033] In addition, when the polyamide porous membrane of the present invention is a flat membrane, the initial bubble point and burst bubble point are values ​​measured by the following procedure. A flat membrane cut into a circle with a diameter of 40 mm or more is immersed in 2-propanol, and the pressure is reduced for several seconds to fill the holes with liquid. Next, the flat membrane is taken out, and while wet with 2-propanol, both sides of the flat membrane are sandwiched between an O-ring and a mesh with a diameter of 40 mm, and these are fixed with a resin jig. Then, an air pressure pipe is connected to one side of the jig, and air is sent to the inside of the flat membrane at 0.4 MPa / min through the air pressure pipe while the flat membrane and the jig are immersed in the test liquid to increase the pressure. The pressure when bubbles first appear from the flat membrane is confirmed, and this is taken as the initial bubble point. The pressure is continued to be increased, and the pressure when bubbles appear from the entire flat membrane is confirmed, and this is taken as the burst bubble point.

[0034] [Water droplet removal rate] As described above, the polyamide porous membrane of the present invention has an initial bubble point of 0.45 MPa or more, and is therefore characterized in that it can separate and remove water droplets to a high degree even from water-in-oil emulsions containing very small water droplets with an average droplet diameter of 0.5 to 5 μm, or even 0.5 to 3 μm.

[0035] In one embodiment of the polyamide porous membrane of the present invention, the polyamide porous membrane of the present invention has a water droplet removal rate of 80% or more, and may further be 85% or more, 90% or more, or 95% or more when filtering a water-in-oil emulsion (A) containing 94% by weight of isoparaffin oil, 1% by weight of water, and 5% by weight of a surfactant having an HLB value of 7 and containing water droplets with an average water droplet diameter of 1.2 μm. Examples of the isoparaffin oil include ISOPAR G manufactured by Standard Corporation.

[0036] In one embodiment of the polyamide porous membrane of the present invention, the polyamide porous membrane of the present invention has a water droplet removal rate of 80% or more, or even 85% or more, or 90% or more, when filtering a water-in-oil emulsion (B) containing 85% by weight of isoparaffin oil, 10% by weight of water, and 5% by weight of a surfactant having an HLB value of 7 and containing water droplets with an average water droplet diameter of 2.3 μm. Examples of the isoparaffin oil include those exemplified above.

[0037] In one embodiment of the polyamide porous membrane of the present invention, the polyamide porous membrane of the present invention has a water droplet removal rate of 80% or more, and may further be 85% or more, 90% or more, or 95% or more when filtering a water-in-oil emulsion (C) containing 94% by weight of paraffin oil, 1% by weight of water, and 5% by weight of a surfactant having an HLB value of 7 and containing water droplets with an average water droplet diameter of 1.3 μm. Examples of the paraffin oil include NORPAR12 manufactured by Standard Corporation.

[0038] In one embodiment of the polyamide porous membrane of the present invention, the polyamide porous membrane of the present invention has a water droplet removal rate of 80% or more, or even 85% or more, or 90% or more when filtering a water-in-oil emulsion (D) containing 85% by weight of paraffin oil, 10% by weight of water, and 5% by weight of a surfactant having an HLB value of 7 and containing water droplets with an average water droplet diameter of 2.4 μm. Examples of the paraffin oil include those exemplified above.

[0039] The water-in-oil emulsions (A) to (D) have a very small average water droplet diameter compared to common water-in-oil emulsions, and when a conventional polyamide porous membrane is used, the water droplets are hardly separated and removed. However, the polyamide porous membrane of the present invention has an initial bubble point of 0.45 MPa or more as described above, so that even water-in-oil emulsions containing water droplets with a very small average water droplet diameter can be separated and removed to a high degree.

[0040] In the water-in-oil emulsions (A) to (D), the maximum diameter of the droplets is not particularly limited, but may be, for example, about 0.1 to 200 μm, and may be, for example, about 1 to 100 μm, 1 to 50 μm, 1 to 20 μm, 1 to 10 μm, 1 to 5 μm, 2 to 5 μm, 3 to 5 μm, or 4 to 5 μm. In addition, in the water-in-oil emulsions (A) to (D), the minimum diameter of the droplets is not particularly limited, but may be, for example, about 0.01 to 10 μm, and may be, for example, about 0.05 to 5 μm, 0.1 to 3 μm, 0.1 to 2 μm, 0.1 to 1 μm, or 0.1 to 0.5 μm.

[0041] The water-in-oil emulsions (A) to (D) were prepared by subjecting a mixture of isoparaffin oil or paraffin oil, a surfactant having an HLB value of 7, and pure water to ultrasonic treatment for 30 minutes.

[0042] The surfactant having an HLB value of 7 is a mixture of two types of surfactants, a surfactant (E) having an HLB value of 4.3 and a surfactant (F) having an HLB value of 15, whose HLB value was adjusted to 7 based on the following formula: N HLB = N 1 HLB ×W 1 +N 2 HLB ×W 2 (N HLB : HLB value of the mixture, N 1 HLB : HLB value of surfactant (E), W 1 : weight fraction of surfactant (E), N 2 HLB : HLB value of surfactant (F), W 2 : weight fraction of surfactant (F) The HLB (hydrophilic-lipophilic balance) value is a value indicating the affinity of a surfactant to water and oil, and is a value calculated by the Griffin method using the following formula: In the following formula, examples of the "hydrophilic group contained in the surfactant" include a hydroxyl group and an ethyleneoxy group. HLB value = 20 x [(total formula weight of hydrophilic groups contained in surfactant) / (molecular weight of surfactant)]

[0043] When the polyamide porous membrane of the present invention is a hollow fiber membrane, the water droplet removal rate is a value measured by internal pressure filtration, and is calculated by passing a water-in-oil emulsion through a cross-flow module at a pressure of 1 bar to obtain a permeate that has permeated the hollow fiber membrane, using the water content in the permeate and the water content in the water-in-oil emulsion according to the following formula. Water droplet removal rate (%) = 100 - (water content in permeate / water content in water-in-oil emulsion) x 100

[0044] When the polyamide porous membrane of the present invention is a hollow fiber membrane, the water droplet removal rate is specifically a value measured by the following procedure. First, 20 hollow fiber membranes are cut to a length of 30 cm, and bundled together. Next, a polybutylene terephthalate (PBT) tube with an outer diameter of 12.7 mm, an inner diameter of 9.5 mm, and a length of 53 mm is prepared, and a silicone tube with an inner diameter of 12 mm and a length of about 50 mm is inserted about 15 mm into one end opening of the tube to connect it, and a rubber plug with a length of about 20 mm is inserted on the side of the silicone tube opposite to the side inserted into the PBT tube to plug the one end opening. Next, a two-liquid mixed epoxy resin is injected from the opening on the opposite side of the connecting tube from the side where the rubber plug is inserted, and the space inside the tube is filled with the epoxy resin. Then, one end of the bundle of hollow fiber membranes prepared above is heat sealed to prevent the epoxy resin from penetrating into the hollow portion, and the end is inserted into the tube filled with the epoxy resin until the tip of the end touches the rubber stopper, and the epoxy resin is cured in this state. Next, the region of the cured epoxy resin on the rubber stopper side is cut together with the tube to open the hollow portion. The same operation is performed on the other end to prepare a crossflow module with open hollow portions at both ends of the hollow fiber membrane. Next, the prepared cross-flow module 10 is connected to the internal pressure separation processing line shown in FIG. 2, and the water-in-oil emulsion is continuously passed through the cross-flow module 10 by the liquid supply circulation pump 11. In the module, the pressure of the primary pressure gauge 14 and the pressure of the secondary pressure gauge 15 are adjusted by the regulator 12 so that the arithmetic mean value of the pressure of the primary pressure gauge 14 and the pressure of the secondary pressure gauge 15 is 1 bar. Of the water-in-oil emulsion passing through the module, that which has permeated the hollow fiber membrane is collected as a permeate separated from the water-in-oil emulsion, and the remainder is circulated again to the separation processing line. The permeate that flows out of the cross-flow module between 2 hours and 4 hours after the start of circulation is collected in a receiver 16. The water content in the obtained permeate is calculated from the water content in the sample (permeate) obtained by measurement using a Karl Fischer moisture meter and the sample amount. The water content in the water-in-oil emulsion is also calculated in the same manner as above using a Karl Fischer moisture meter. Then, the water droplet removal rate is calculated using the following formula. Water droplet removal rate (%) = 100 - (water content in permeate / water content in water-in-oil emulsion) x 100

[0045] When the polyamide porous membrane of the present invention is a flat membrane, the water droplet removal rate is a value measured by dead-end filtration, and is a value measured by the following procedure. A flat membrane cross-flow tester (e.g., Sepa-CF flat membrane test cell manufactured by GE Water Technologies) connected to a high-pressure pump is used to cut a flat membrane-shaped polyamide porous membrane to a predetermined size and fix it in the cell, and the water-in-oil emulsion prepared at 25°C is passed through it to collect the permeated liquid at a predetermined pressure. The water content in the obtained permeated liquid and the water content in the water-in-oil emulsion are calculated in the same manner as above, and the water droplet removal rate is calculated from the above formula.

[0046] [Permeation flow rate] As described above, the polyamide porous membrane of the present invention has an initial bubble point of 0.45 MPa or more, and therefore has the characteristic of a high water droplet removal rate. In addition, the membrane has the characteristic of excellent oil permeability, and the oil permeability is unlikely to decrease during the filtration operation.

[0047] In one embodiment of the polyamide porous membrane of the present invention, when the water-in-oil emulsion (A) is filtered through the polyamide porous membrane of the present invention, the permeation flow rate 5 minutes after the start of filtration is, for example, 200 L / (m 2 ·bar·h) or more, and even more than 250 L / (m 2 ·bar·h) or more, or 300L / (m 2 ·bar·h) or more. The upper limit of the permeation flow rate after 5 minutes from the start of filtration is usually 350 L / (m 2 ·bar·h).

[0048] In one embodiment of the polyamide porous membrane of the present invention, when the water-in-oil emulsion (A) is filtered through the polyamide porous membrane of the present invention, the permeation flow rate after 60 minutes from the start of filtration is, for example, 200 L / (m 2 ·bar·h) or more, and even more than 230L / (m 2 ·bar·h) or more, or 250L / (m 2 ·bar·h) or more. The upper limit of the permeation flow rate after 60 minutes from the start of filtration is usually 300 L / (m 2 ·bar·h).

[0049] In one embodiment of the polyamide porous membrane of the present invention, the polyamide porous membrane of the present invention has a permeability during a filtration operation of the water-in-oil emulsion (A), and the retention of the permeation flow rate 60 minutes after the start of filtration relative to the permeation flow rate 5 minutes after the start of filtration, calculated by the following formula, can be, for example, 85% or more, or even 90% or more. Retention rate (%) = 100 - [(Permeation flow rate 5 minutes after the start of filtration - Permeation flow rate 60 minutes after the start of filtration) / Permeation flow rate 5 minutes after the start of filtration] x 100

[0050] In one embodiment of the polyamide porous membrane of the present invention, when the water-in-oil emulsion (B) is filtered through the polyamide porous membrane of the present invention, the permeation flow rate 5 minutes after the start of filtration is, for example, 200 L / (m 2 ·bar·h) or more, and even more than 250 L / (m 2 ·bar·h) or more, or 300L / (m 2 ·bar·h) or more. The upper limit of the permeation flow rate after 5 minutes from the start of filtration is usually 350 L / (m 2 ·bar·h).

[0051] In one embodiment of the polyamide porous membrane of the present invention, when the water-in-oil emulsion (B) is filtered, the polyamide porous membrane of the present invention has a permeation flow rate of, for example, 170 L / (m 2 ·bar·h) or more, and even more than 180L / (m 2 ·bar·h) or more, or 190L / (m 2 ·bar·h) or more. The upper limit of the permeation flow rate after 60 minutes from the start of filtration is usually 250 L / (m 2 ·bar·h).

[0052] In one embodiment of the polyamide porous membrane of the present invention, regarding the permeability during the filtration operation of the water-in-oil emulsion (B), the retention of the permeation flow rate 60 minutes after the start of filtration relative to the permeation flow rate 5 minutes after the start of filtration calculated by the above formula may be, for example, 55% or more, or further 65% or more, or 80% or more.

[0053] In one embodiment of the polyamide porous membrane of the present invention, when the water-in-oil emulsion (C) is filtered through the polyamide porous membrane of the present invention, the permeation flow rate 5 minutes after the start of filtration is, for example, 200 L / (m 2 ·bar·h) or more, and even more than 250 L / (m 2 ·bar·h) or more, or 300L / (m 2 ·bar·h) or more. The upper limit of the permeation flow rate after 5 minutes from the start of filtration is usually 350 L / (m 2 ·bar·h).

[0054] In one embodiment of the polyamide porous membrane of the present invention, when the water-in-oil emulsion (C) is filtered through the polyamide porous membrane of the present invention, the permeation flow rate after 60 minutes from the start of filtration is, for example, 190 L / (m 2 ·bar·h) or more, and even 200 L / (m 2 ·bar·h) or more, or 240L / (m 2 ·bar·h) or more. The upper limit of the permeation flow rate after 60 minutes from the start of filtration is usually 300 L / (m 2 ·bar·h).

[0055] In one embodiment of the polyamide porous membrane of the present invention, regarding the permeability during the filtration operation of the water-in-oil emulsion (C), the retention of the permeation flow rate 60 minutes after the start of filtration relative to the permeation flow rate 5 minutes after the start of filtration calculated by the above formula may be, for example, 70% or more, or even 75% or more, or 80% or more.

[0056] In one embodiment of the polyamide porous membrane of the present invention, when the water-in-oil emulsion (D) is filtered through the polyamide porous membrane of the present invention, the permeation flow rate 5 minutes after the start of filtration is, for example, 200 L / (m 2 ·bar·h) or more, and even more than 250 L / (m 2 ·bar·h) or more, or 280L / (m 2 ·bar·h) or more. The upper limit of the permeation flow rate after 5 minutes from the start of filtration is usually 300 L / (m 2 ·bar·h).

[0057] In one embodiment of the polyamide porous membrane of the present invention, when the water-in-oil emulsion (D) is filtered, the polyamide porous membrane of the present invention has a permeation flow rate of, for example, 180 L / (m 2 ·bar·h) or more, and even more than 190 L / (m 2 ·bar·h) or more, or 200L / (m 2 ·bar·h) or more. The upper limit of the permeation flow rate after 60 minutes from the start of filtration is usually 250 L / (m 2·bar·h).

[0058] In one embodiment of the polyamide porous membrane of the present invention, regarding the permeability during the filtration operation of the water-in-oil emulsion (D), the retention of the permeation flow rate 60 minutes after the start of filtration relative to the permeation flow rate 5 minutes after the start of filtration calculated by the above formula can be, for example, 70% or more, or even 75% or more, or 80% or more.

[0059] When the polyamide porous membrane of the present invention is a hollow fiber membrane, the permeation flow rate is a value measured by internal pressure filtration, and is a value measured by the same measurement procedure as the measurement procedure for the water droplet removal rate. The permeation flow rate 5 minutes after the start of filtration is calculated by collecting the permeated liquid that has flowed out of the crossflow module within 5 to 6 minutes after the start of circulation, measuring the weight of the permeated liquid obtained, and calculating the permeation flow rate (L / (m)) from the following formula: 2 The permeation flow rate 60 minutes after the start of filtration was calculated by collecting the permeate that had flowed out of the crossflow module within 60 to 61 minutes after the start of circulation, measuring the weight of the permeate, and calculating the permeation flow rate (L / (m 2 Calculate the value of 1.5 bar h). Permeation flow rate = weight of permeate (g) / [inner diameter of hollow fiber membrane (m) x 3.14 x effective filtration length of hollow fiber membrane (m) x number of hollow fiber membranes (units) x (pressure (bar) x time (h) x specific gravity of permeate (g / L)] Effective filtration length of hollow fiber membrane: This is the length of the part of the outer surface of the hollow fiber membrane that is not covered with epoxy resin in the crossflow module. The specific gravity of the permeate is measured based on the "Method of measuring density and specific gravity using a pycnometer" in JIS Z 8804:2012 (Method of measuring density and specific gravity of liquids).

[0060] When the polyamide porous membrane of the present invention is a flat membrane, the permeation flow rate is a value measured by dead-end filtration, and is a value measured by the same measurement procedure as the measurement procedure for the water droplet removal rate. The permeation flow rate 5 minutes after the start of filtration is calculated by collecting the permeated liquid that has permeated within 5 to 6 minutes after the start of filtration, measuring the volume (L), and calculating the permeation flow rate (L / (m)) according to the following formula: 2 The permeation flow rate 60 minutes after the start of filtration was calculated by collecting the permeated liquid that had passed through within 60 to 61 minutes after the start of filtration, measuring the volume (L), and calculating the permeation flow rate (L / (m 2 Calculate the value of 1.5 bar h). Permeation flow rate = Volume of permeate that permeates the flat membrane (L) / [Flat membrane area (m 2 ) × {(pressure (bar)} × time (h)]

[0061] [Application] The polyamide porous membrane of the present invention is used for separating a mixture containing water and oil into oil and water. Conventional polyamide porous membranes cannot separate a mixture containing water and oil into oil and water, but the polyamide porous membrane of the present invention has an initial bubble point of 0.45 MPa or more as described above, and therefore can separate a mixture containing water and oil into oil and water to a high degree.

[0062] The mixed liquid is not particularly limited as long as it contains at least water and oil, and may contain other components other than water and oil. Examples of other components include oils used in machining such as metal cutting and polishing, and oils discharged from various machines and devices, such as various additives (e.g., surfactants) contained in cutting oils, cleaning oils, lubricating oils, machine oils, and compressor oils; and turbidity (e.g., minerals and metal salts) contained in produced water generated when extracting crude oil, bitumen, and natural gas.

[0063] The oil in the mixed liquid is not particularly limited, and examples thereof include oils used in machining such as metal cutting and polishing, and oils discharged from various machines and devices, specifically, cutting oils, cleaning oils, lubricating oils, machine oils, compressor oils, oils contained in the produced water, edible oils, etc., but are preferably hydrocarbon oils, and are preferably (liquid) hydrocarbon oils having a carbon number of about 15 to 35. Examples of the hydrocarbon oils include paraffin-based hydrocarbons, olefin-based hydrocarbons, naphthenic hydrocarbons, and aromatic hydrocarbons. The hydrocarbon oil may be a synthetic oil, and may be derived from petroleum, plants, or animals. These hydrocarbon oils may be contained alone or in combination.

[0064] When the mixed liquid mainly contains oil, the oil content is, for example, about 70 to 99 wt %, preferably 80 to 99 wt %, and more preferably 85 to 95 wt %, and the water content is the amount that is the remainder excluding the oil and other components.

[0065] When the mixed liquid mainly contains water, the water content is, for example, about 70 to 99 wt %, preferably 80 to 99 wt %, and more preferably 85 to 95 wt %, and the oil content is the amount that is the remainder excluding water and other components.

[0066] The mixed liquid may be an emulsion. As described above, the polyamide porous membrane of the present invention has an initial bubble point of 0.45 MPa or more, so that even if the mixed liquid is an emulsion, water droplets or oil droplets can be separated and removed from the emulsion to a high degree, and the emulsion can be subjected to oil-water separation treatment in a short time.

[0067] The emulsion contains at least water, oil, and a surfactant, and may be a water-in-oil (W / O) emulsion or an oil-in-water (O / W) emulsion, but is preferably a water-in-oil emulsion.

[0068] Examples of the water-in-oil emulsion include those obtained by mixing oil used in machining such as metal cutting and polishing with cleaning water containing a surfactant for cleaning metal, and specifically, emulsified water-containing oil discharged from automobile parts factories, machine part manufacturing factories, building hardware manufacturing factories, and the like.

[0069] The average droplet size of the droplets in the emulsion is not particularly limited, but is, for example, about 0.05 to 100 μm, preferably 0.5 to 50 μm, more preferably 0.5 to 30 μm, even more preferably 0.5 to 10 μm, and even more preferably 0.5 to 5 μm. The maximum diameter of the droplets in the emulsion is not particularly limited, but is, for example, about 0.1 to 200 μm, preferably 1 to 100 μm, more preferably 1 to 50 μm, even more preferably 1 to 20 μm, and even more preferably 1 to 10 μm. The minimum diameter of the droplets in the emulsion is not particularly limited, but is, for example, about 0.01 to 10 μm, preferably 0.05 to 5 μm, more preferably 0.1 to 1 μm, and even more preferably 0.1 to 0.5 μm. As described above, the polyamide porous membrane of the present invention has an initial bubble point of 0.45 MPa or more, and therefore can separate and remove droplets from an emulsion to a high degree even when the average droplet diameter of the droplets in the emulsion is extremely small.

[0070] In the present invention, the average droplet size, the minimum diameter, and the maximum diameter of droplets in an emulsion are values ​​that are determined from a particle size distribution chart obtained by measuring the particle size distribution using a particle size measuring device. Specifically, these values ​​are measured by the following procedure. First, the water and oil in the emulsion are separated by distillation, and the refractive index of the separated oil is measured with a refractometer. The refractive index of water is set to 1.33. Then, using a particle size measuring device, in the case of a water-in-oil emulsion, the background is measured using the separated oil, and in the case of an oil-in-water emulsion, the background is measured using water. Next, the inside of the cell is washed with the water-in-oil emulsion or oil-in-water emulsion used for the measurement. Then, the refractive index of the separated oil and the refractive index of the water are input into the measuring device, and the shape of the droplets is set to non-spherical particles and input into the measuring device, and the temperature inside the cell is adjusted to 25°C. The measurement time is 120 seconds, and a particle size distribution chart is obtained by the measurement. The above operation is repeated at 30-minute intervals until the particle size distribution range of the droplet diameter does not change in the obtained particle size distribution chart (until the values ​​of the minimum diameter and maximum diameter on the particle size distribution do not change). The average droplet diameter (median diameter D50), minimum diameter, and maximum diameter in the particle size distribution chart when the particle size distribution range of the droplet diameter does not change are taken as the average droplet diameter, minimum diameter, and maximum diameter of the droplets present in the emulsion.

[0071] The polyamide porous membrane of the present invention is preferably used by being incorporated into a filtration membrane module described below.

[0072] The polyamide porous membrane of the present invention may be provided as a free-standing membrane, or may be laminated on a support such as a microfiltration membrane or an ultrafiltration membrane. The material of such a support is preferably resistant to organic solvents, and specific examples thereof include polymeric materials such as polyamide, polyethylene, polypropylene, polytetrafluoroethylene, polyphenylene sulfide, and polyether ether ketone; inorganic materials such as sintered metal and ceramics.

[0073] 2. Manufacturing method of polyamide porous membrane The method for producing the polyamide porous membrane of the present invention is not particularly limited, but a suitable example includes a production method including the following steps 1 and 2. The production method including the following steps 1 and 2 is preferably adopted because it is easy to produce the polyamide porous membrane of the present invention having an initial bubble point of 0.45 MPa or more. First step: A membrane-forming solution is prepared by dissolving a polyamide resin in an organic solvent containing sulfolane and dimethyl sulfone, in which the weight ratio of dimethyl sulfone to sulfolane (dimethyl sulfone / sulfolane) is 0.8 to 3.0, at a temperature of 100° C. or higher. Second step: The film-forming solution is extruded in a predetermined shape into a coagulation bath at 100° C. or less to coagulate the polyamide resin into a film.

[0074] Hereinafter, the first and second steps will be described in detail.

[0075] [1st step] In the first step, a membrane-forming stock solution is prepared by dissolving a polyamide resin in an organic solvent containing sulfolane and dimethyl sulfone, with the weight ratio of dimethyl sulfone to sulfolane (dimethyl sulfone / sulfolane) being 0.8 to 3.0, at a temperature of 100° C. or higher. From the viewpoint of facilitating the production of a polyamide porous membrane having an initial bubble point of 0.45 MPa or higher, the weight ratio of dimethyl sulfone to sulfolane (dimethyl sulfone / sulfolane) is preferably 1.5 to 3.0, more preferably 2.0 to 3.0, and even more preferably 2.2 to 2.8.

[0076] Furthermore, the membrane-forming solution prepared in the first step may contain an organic solvent other than sulfolane and dimethylsulfone, if necessary, within a range that does not impair the effects of the present invention.

[0077] The concentration of the polyamide resin in the membrane-forming solution is not particularly limited, but is, for example, 15 to 40% by weight, and from the viewpoint of facilitating the production of a polyamide porous membrane having an initial bubble point of 0.45 MPa or more, it is preferably 25 to 35% by weight, more preferably 25 to 30% by weight, and even more preferably 27 to 30% by weight.

[0078] In the first step, when dissolving the polyamide resin in the organic solvent, it is necessary to set the temperature of the solvent to 100°C or higher. Specifically, it is desirable to dissolve the polyamide resin at a temperature 10 to 50°C higher than the phase separation temperature of the membrane-forming solution to be prepared, preferably at a temperature 20 to 40°C higher. The phase separation temperature of the membrane-forming solution refers to the temperature at which liquid-liquid phase separation or solid-liquid phase separation due to crystal precipitation occurs when a mixture of the polyamide resin and the organic solvent at a sufficiently high temperature is gradually cooled. The phase separation temperature can be measured using a microscope equipped with a hot stage or the like.

[0079] In the first step, the temperature condition when dissolving the polyamide resin in the organic solvent may be appropriately set in the temperature range of 100°C or higher according to the above-mentioned index depending on the type of polyamide resin and the type of organic solvent used, and is preferably 120 to 250°C, more preferably 140 to 220°C, and even more preferably 160 to 200°C.

[0080] Furthermore, additives such as fillers, thickeners, surfactants, crystal nucleating agents, lubricants, etc. may be added to the membrane-forming solution as necessary for controlling the pore size of the polyamide porous membrane and improving its performance.

[0081] The film-forming solution prepared in the first step is supplied to the second step while still at that temperature (ie, at 100° C. or higher).

[0082] [Second process] In the second step, the film-forming solution prepared in the first step is extruded in a predetermined shape into a coagulation bath at 100° C. or less to coagulate the polyamide resin into a film.

[0083] As the coagulation liquid, a conventionally known coagulation liquid can be used. For example, a coagulation liquid that is compatible with the organic solvent used in the film-forming solution and has a high affinity with the polyamide resin, or a coagulation liquid that is compatible with the organic solvent used in the film-forming solution and has a low affinity with the polyamide resin can be used.

[0084] A specific example of a coagulation liquid that is compatible with the organic solvent used in the film-forming solution and has a high affinity with the polyamide resin is a coagulation liquid containing a solvent that is compatible with the organic solvent used in the film-forming solution at a temperature of 25° C. or less and dissolves the polyamide resin at a temperature of the boiling point or less. More specific examples include glycerin, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol 200, propylene glycol, 1,3-butanediol, sulfolane, N-methyl-2-pyrrolidone, γ-butyrolactone, δ-valerolactone, and aqueous solutions containing 20% ​​by weight or more of these. Among these, preferred are at least one selected from the group consisting of glycerin, propylene glycol, diethylene glycol, and polyethylene glycol 200, and an aqueous solution containing at least one of these in a proportion of 25 to 75% by weight; more preferred are at least one selected from the group consisting of glycerin, diethylene glycol, tetraethylene glycol, and propylene glycol, and an aqueous solution containing at least one of these in a proportion of 40 to 80% by weight (preferably 40 to 60% by weight).

[0085] Examples of the coagulation liquid that is compatible with the organic solvent used in the film-forming solution but has low affinity with the polyamide resin include a solvent that is compatible with the organic solvent used in the film-forming solution at a temperature of 50° C. or less, but does not dissolve the polyamide resin at a temperature below the boiling point or below 200° C. More specifically, examples of the coagulation liquid include aqueous solvents such as water and aqueous solutions with a water content of 80% by weight or more; monohydric lower alcohols such as 1-propanol, 2-propanol, and isobutanol; glycol ethers such as polyethylene glycols with an average molecular weight of 300 or more, polypropylene glycols with an average molecular weight of 400 or more, diethylene glycol diethyl ether, triethylene glycol monomethyl ether, and propylene glycol monoethyl ether; and glycol acetates such as triacetin and propylene glycol monoethyl ether acetate. Among these, preferred are polyethylene glycols having an average molecular weight of 300 to 1000, polypropylene glycols having an average molecular weight of 400 to 1000, triacetin, and triethylene glycol monomethyl ether; more preferred are polyethylene glycols having an average molecular weight of 300 to 700; and even more preferred are polyethylene glycols having an average molecular weight of 400 to 600. These solvents may be used alone or in combination of two or more. In the present invention, the average molecular weights of polyethylene glycols and polypropylene glycols are number average molecular weights calculated based on the hydroxyl value measured in accordance with JIS K 1557-6:2009 "Plastics - Polyurethane raw material polyols test method - Part 6: Determination of hydroxyl value by near infrared (NIR) spectroscopy".

[0086] When a coagulation liquid that is compatible with the organic solvent used in the membrane-forming solution and has low affinity with the polyamide resin is used as the coagulation liquid, the pore size of the surface of the polyamide porous membrane that comes into contact with the solvent can be made relatively small. On the other hand, when a coagulation liquid that is compatible with the organic solvent used in the membrane-forming solution and has high affinity with the polyamide resin is used as the coagulation liquid, the pore size of the surface of the polyamide porous membrane that comes into contact with the solvent can be made relatively large.

[0087] In addition, the coagulating liquid having compatibility with the organic solvent used in the membrane-forming solution and low affinity with the polyamide resin may be mixed with a coagulating liquid having compatibility with the organic solvent used in the membrane-forming solution and high affinity with the polyamide resin. In this case, the content of the coagulating liquid having compatibility with the organic solvent used in the membrane-forming solution and high affinity with the polyamide resin is, for example, 20% by weight or less, preferably 10% by weight or less.

[0088] In the case of forming a hollow fiber membrane as a polyamide porous membrane, the second step may be performed by using a double-tube nozzle for hollow fiber production having a double-tube structure, discharging the membrane forming solution from the outer annular nozzle and discharging the internal coagulation liquid from the inner nozzle, and immersing the membrane forming solution in a coagulation bath. In this case, as the internal coagulation liquid and the coagulation bath, the above-mentioned coagulation liquid having compatibility with the organic solvent used in the membrane forming solution and high affinity with the polyamide resin, or the coagulation liquid having compatibility with the organic solvent used in the membrane forming solution and low affinity with the polyamide resin, may be used. As the internal coagulation liquid and the coagulation bath, only the coagulation liquid having compatibility with the organic solvent used in the membrane forming solution and high affinity with the polyamide resin, or only the coagulation liquid having compatibility with the organic solvent used in the membrane forming solution and low affinity with the polyamide resin may be used. In addition, one of the coagulating liquids compatible with the organic solvent used in the membrane-forming solution and having a high affinity with the polyamide resin, and the other of the coagulating liquids compatible with the organic solvent used in the membrane-forming solution and having a low affinity with the polyamide resin, may be used as the coagulating liquid for the inside, and the other may be used as the coagulating bath. In particular, it is preferable to use one of the coagulating liquids compatible with the organic solvent used in the membrane-forming solution and having a high affinity with the polyamide resin, and the other of the coagulating liquids compatible with the organic solvent used in the membrane-forming solution and having a low affinity with the polyamide resin, as the coagulating liquid for the inside, and the other as the coagulating bath. In particular, the coagulating liquid compatible with the organic solvent used in the membrane-forming solution and having a high affinity with the polyamide resin (preferably at least one selected from the group consisting of glycerin, diethylene glycol, tetraethylene glycol, and propylene glycol, and an aqueous solution containing at least one of these at a ratio of 40 to 80% by weight (preferably 40 to 60% by weight)) is used.) is used as a coagulation bath, and a coagulation liquid that is compatible with the organic solvent used in the membrane-forming solution but has low affinity for the polyamide resin (preferably at least one selected from the group consisting of polyethylene glycol having an average molecular weight of 200 to 1000 (preferably 200 to 600), polypropylene glycol having an average molecular weight of 400 to 1000, triacetin, and triethylene glycol monomethyl ether, or a mixed liquid containing 60 to 80% by weight of at least one of these and 20 to 40% by weight of at least one selected from the group consisting of glycerin, diethylene glycol, tetraethylene glycol, and propylene glycol) is used as an internal coagulation liquid, thereby obtaining a hollow fiber membrane having pores with a relatively small pore size on the inner surface and pores with a relatively large pore size on the outer surface. It also becomes easier to produce a polyamide hollow fiber membrane having an initial bubble point of 0.45 MPa or more, and a polyamide hollow fiber membrane having an initial bubble point of 0.45 MPa or more and a burst bubble point of 0.50 to 0.90 MPa.

[0089] In addition, since the internal coagulation liquid used in forming the hollow fiber membrane passes through the double annular nozzle, it is preferable that it does not contain water whose boiling point is equal to or lower than the temperature of the double annular nozzle.

[0090] As the double tubular nozzle for producing hollow fibers, a spinneret having a double tubular structure such as that used for producing core-sheath type composite fibers in melt spinning can be used. The diameter of the outer annular nozzle and the diameter of the inner nozzle of the double tubular nozzle for producing hollow fibers may be appropriately set according to the inner and outer diameters of the hollow fiber membrane.

[0091] The flow rate of the membrane-forming stock solution discharged from the outer annular nozzle of the hollow fiber production double tubular nozzle is not particularly limited because it depends on the slit width, and may be, for example, 2 to 30 g / min, preferably 3 to 20 g / min, and more preferably 5 to 15 g / min. The flow rate of the internal coagulation liquid is appropriately set in consideration of the diameter of the inner nozzle of the hollow fiber production double tubular nozzle, the type of the internal liquid used, the flow rate of the membrane-forming stock solution, and the like, and may be 0.1 to 2 times, preferably 0.2 to 1 times, and more preferably 0.4 to 0.7 times, the flow rate of the membrane-forming stock solution.

[0092] In addition, in the case of forming a flat membrane as the polyamide porous membrane, the second step may be performed by extruding the membrane-forming stock solution in a predetermined shape and immersing it in the coagulating bath using either a coagulating liquid that is compatible with the organic solvent used in the membrane-forming stock solution and has a low affinity for polyamide resin, or a coagulating liquid that is compatible with the organic solvent used in the membrane-forming stock solution and has a high affinity for polyamide resin.

[0093] In the second step, the temperature of the coagulation bath may be 100°C or less, preferably -20 to 100°C, more preferably 0 to 60°C, even more preferably 2 to 20°C, and particularly preferably 2 to 10°C. The suitable temperature of the coagulation bath may vary depending on the organic solvent used in the membrane-forming solution, the composition of the coagulation solution, etc., but generally, a lower temperature tends to favor thermally induced phase separation, and a higher temperature tends to favor non-solvent phase separation. That is, in the case of producing a hollow fiber membrane having pores with a relatively small pore diameter on the inner surface, it is preferable to set the coagulation bath at a low temperature in order to increase the pore diameter on the inner surface, and it is preferable to set the coagulation bath at a high temperature in order to make the pore diameter on the inner surface denser and the internal structure coarser.

[0094] Furthermore, in the case of forming a hollow fiber membrane as the polyamide porous membrane, the temperature of the internal coagulation liquid may be about the set temperature of the double tubular nozzle, for example, 120 to 250°C, preferably 160 to 230°C, and more preferably 180 to 220°C.

[0095] By carrying out the second step in this manner, the membrane-forming solution is coagulated in the coagulation bath, and the polyamide porous membrane of the present invention is formed.

[0096] After the second step, a step of extracting and removing the coagulated liquid that has undergone phase separation in the polyamide porous membrane may be included. In order to extract and remove the coagulated liquid that has undergone phase separation in the polyamide porous membrane, the polyamide porous membrane formed in the second step may be immersed in an extraction solvent, or the polyamide porous membrane formed in the second step may be showered with the extraction solvent. The extraction solvent used for the extraction and removal is preferably one that is inexpensive, has a low boiling point, and can be easily separated after extraction due to the difference in boiling point, and examples thereof include water, glycerin, methanol, ethanol, isopropanol, acetone, diethyl ether, hexane, petroleum ether, toluene, and the like. Among these, preferred are water, methanol, ethanol, isopropanol, and acetone; more preferred are water, methanol, and isopropanol. In addition, isopropyl alcohol, petroleum ether, and the like can be suitably used when extracting water-insoluble organic solvents such as phthalic acid esters and fatty acids. When the coagulation liquid is extracted and removed by immersing the polyamide porous membrane in an extraction solvent, the time for immersing the polyamide porous membrane in the extraction solvent is not particularly limited, and may be, for example, 0.2 hours to 2 months, preferably 0.5 hours to 1 month, and more preferably 2 hours to 10 days. In order to effectively extract and remove the coagulation liquid remaining in the polyamide porous membrane, the extraction solvent may be replaced or stirred.

[0097] Furthermore, after the extraction and removal of the coagulation liquid, the method may include a step of drying and removing the extraction solvent. The drying and removal of the extraction solvent can be performed by a known drying process such as natural drying, hot air drying, reduced pressure drying, vacuum drying, etc.

[0098] 3. Filtration Membrane Module The polyamide porous membrane of the present invention is housed in a module case equipped with an inlet for a liquid to be treated, an outlet for a permeated liquid, etc., and used as a filtration membrane module.

[0099] When the polyamide porous membrane of the present invention has a hollow fiber shape, it is used as a hollow fiber membrane module.

[0100] Specifically, the hollow fiber membrane module may have a structure in which the hollow fiber polyamide porous membrane of the present invention is bundled and housed in a module case, and one or both ends of the hollow fiber polyamide porous membrane are sealed and fixed with a potting agent. The hollow fiber membrane module may have an opening connected to a flow path passing through the outer wall surface side of the hollow fiber polyamide porous membrane and an opening connected to the hollow part of the hollow fiber polyamide porous membrane, as an inlet for the liquid to be treated or an outlet for the filtrate.

[0101] The shape of the hollow fiber membrane module is not particularly limited, and it may be a dead-end type module or a cross-flow type module. Specifically, examples of such modules include a dead-end module in which a hollow fiber membrane bundle is folded into a U-shape and packed, and the ends of the hollow fiber polyamide porous membrane bundle are sealed and then cut to open; a dead-end module in which a hollow fiber polyamide porous membrane bundle is packed in a straight line, with the hollow opening at one end closed by heat sealing or the like, and the end of the open hollow fiber polyamide porous membrane bundle is sealed and then cut to open; a dead-end module in which a hollow fiber polyamide porous membrane bundle is packed in a straight line, both ends of the hollow fiber polyamide porous membrane bundle are sealed, and only one end is cut to expose the opening; and a cross-flow module in which a hollow fiber polyamide porous membrane bundle is packed in a straight line, both ends of the hollow fiber polyamide porous membrane bundle are sealed, and the sealed parts at both ends of the hollow fiber polyamide porous membrane bundle are cut to create two flow paths on the side of the filter case.

[0102] The filling rate of the hollow fiber polyamide porous membrane inserted into the module case is not particularly limited, but for example, the volume of the hollow fiber polyamide porous membrane including the volume of the hollow part relative to the volume inside the module case is 15 to 75 volume %, preferably 25 to 65 volume %, and more preferably 35 to 55 volume %. By satisfying such a filling rate, it is possible to easily fill the hollow fiber polyamide porous membrane into the module case while securing a sufficient filtration area, and to make it easier for the potting agent to flow between the hollow fiber polyamide porous membranes.

[0103] The potting agent used in the manufacture of the hollow fiber membrane module is not particularly limited, but when the hollow fiber membrane module is used for the treatment of an organic solvent, it is desirable that the potting agent has resistance to the organic solvent, and examples of such potting agents include polyamide, silicone resin, polyurethane resin, epoxy resin, melamine resin, polyethylene, polypropylene, phenolic resin, polyimide, polyurea resin, etc. Among these potting agents, those that shrink or swell little when cured and are not too hard are preferred, and suitable examples include polyamide, silicone resin, epoxy resin, and polyethylene. These potting agents may be used alone or in combination of two or more.

[0104] The material of the module case used in the hollow fiber membrane module is not particularly limited, and examples thereof include polyamide, polyester, polyethylene, polypropylene, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl chloride, polysulfone, polyethersulfone, polycarbonate, polyarylate, polyphenylene sulfide, etc. Among these, preferred are polyamide, polyethylene, polypropylene, polytetrafluoroethylene, polycarbonate, polysulfone, polyethersulfone, and more preferred are polyamide, polyethylene, polypropylene, and polytetrafluoroethylene.

[0105] When the polyamide porous membrane of the present invention has a flat membrane shape, it is used as a sheet type module such as a plate and frame type or a stack type, a spiral type module, a rotating flat membrane type module, a pleated type module, or the like.

[0106] 4. Oil-water separation method The oil-water separation method of the present invention is characterized in that a mixed liquid containing water and oil is separated into oil and water using the filtration membrane module. According to the oil-water separation method of the present invention, a mixed liquid containing water and oil can be separated into oil and water to a high degree. Furthermore, according to the oil-water separation method of the present invention, even if the mixed liquid is an emulsion, particularly an emulsion containing very small droplets having an average droplet diameter of 0.5 to 5 μm, or even 0.5 to 3 μm, the droplets can be separated and removed to a high degree. Furthermore, according to the oil-water separation method of the present invention, as described in the above [Water Droplet Removal Rate], for example, when a water-in-oil emulsion containing water droplets having an average droplet diameter of 0.5 to 3 μm is filtered, the water droplets can be removed at a removal rate of 80% or more, 85% or more, 90% or more, or even 95% or more. Furthermore, according to the oil-water separation method of the present invention, as described in the above section on [Permeation flow rate], for example, when a water-in-oil emulsion containing water droplets with an average water droplet diameter of 0.5 to 3 μm is filtered, the permeation flow rate is 200 L / (m 2 ·bar·h) or more, 250L / (m 2 ·bar·h) or more, even 300L / (m 2 The separation process can be carried out at a permeation flow rate of at least 70%, at least 75%, at least 80%, at least 85%, or even at least 90% of the permeation flow rate.

[0107] In addition to using the filtration membrane module, the oil-water separation method of the present invention can employ a known separation method using a filtration membrane module. For example, one or more of the filtration membrane modules are incorporated into a filtration device equipped with a tank, a liquid circulation pump, a liquid supply line, various pressure gauges, and various valves, and a mixed liquid containing water and oil is passed through the filtration membrane module. Of the mixed liquid passing through the filtration membrane module, the part that has permeated the polyamide porous membrane is collected as a permeate separated from the mixed liquid, and the remainder is circulated back to the liquid supply line. The pressure, liquid passing speed, and temperature of the mixed liquid in the separation operation may be appropriately adjusted depending on the type of the mixed liquid and the filtration membrane module to be passed.

[0108] According to the oil-water separation method of the present invention, water droplets or oil droplets can be separated and removed to a high degree from an emulsion containing droplets with an average droplet diameter of 0.5 to 5 μm, or even 0.5 to 3 μm, so that water-containing oil or associated water can be separated into oil and water to a high degree even in emulsions with very small droplets. EXAMPLES

[0109] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0110] 1.Measurement method [Outer and inner diameters of hollow fiber membrane] The five hollow fiber membranes were observed under an optical microscope at a magnification of 200 times, the outer diameter and inner diameter (both at the maximum diameter point) of each hollow fiber membrane were measured, and the average values ​​were calculated.

[0111] [Initial bubble point and burst bubble point of hollow fiber membrane] First, a porous membrane mini-module was prepared for measuring the initial bubble point and burst bubble point. Specifically, 10 hollow fiber membranes were cut to a length of 20 cm, bundled together, and bent into a U-shape. The end of the hollow fiber membrane on the opening side was heat-sealed to about 1 cm to block the hollow, and a hollow fiber membrane bundle was prepared. Next, a 5 cm long soft nylon tube for air piping (outer diameter 8 mm, inner diameter 6 mm) was prepared, and one of the openings was blocked with a silicone plug. Next, the end of the nylon tube with the silicone plug attached was placed down, and a potting agent (polyurethane resin) was introduced into the nylon tube to a height of about 4 cm. Then, the hollow fiber membrane bundle was inserted into the nylon tube from the heat-sealed end, and a part of the hollow fiber membrane bundle was immersed in the potting agent and left to stand until the potting agent hardened. After hardening, the hollow fiber membrane bundle was cut above the heat-sealed portion to open the hollow part of the hollow fiber membrane. At this time, it was visually confirmed whether the potting agent had entered the hollow portion and whether the potting agent had filled the spaces between the hollow fiber membranes. After it was confirmed that the hollow portion was maintained without any problems, the initial bubble point and burst bubble point were measured.

[0112] Next, the initial bubble point and burst bubble point of the hollow fiber membrane were measured using the device shown in the schematic diagram of FIG. 1. In the measurement of the bubble point, it is necessary to fill the pores of the hollow fiber membrane with liquid. Therefore, 2-propanol (surface tension 21 mN / m at 20°C) used in the test was placed in a glass container 7, and the porous membrane mini-module 6 prepared above was immersed therein, and the pressure was reduced for several seconds to fill the pores with liquid. Next, the porous membrane mini-module 6 immersed in the test liquid was set as shown in FIG. 1, and air was sent into the inside of the hollow fiber membrane at 0.4 MPa / min to increase the pressure. First, the pressure when bubbles were generated from the hollow fiber membrane was confirmed, and this was taken as the initial bubble point. The pressure was continued to be increased, and the pressure when bubbles were generated from almost the entire hollow fiber membrane was confirmed, and this was taken as the burst bubble point.

[0113] [Preparation of water-in-oil emulsion for measurement] Each water-in-oil emulsion used in the measurements was prepared by the following method. First, two types of surfactants, Span 80 [HLB value: 4.3 (catalog value)] and Tween 80 [HLB value: 15 (catalog value)] manufactured by Sigma-Aldrich, were used, and a solution was prepared using these two types of surfactants based on the following formula to obtain a surfactant with an HLB value of 7 (a mixture of two types). N HLB = N 1 HLB ×W 1 +N 2 HLB ×W 2 (N HLB : HLB value of the mixture, N 1 HLB : HLB value of Span80, W 1 : Weight fraction of Span 80, N 2 HLB : HLB value of Tween 80, W 2 (Weight fraction of Tween 80) Then, a mixture was obtained by mixing the hydrocarbon oil A, which is an isoparaffin oil (ISOPAR G, manufactured by Standard Chemical Industries, Ltd.) or the hydrocarbon oil B, which is a paraffin oil (NORPAR12, manufactured by Standard Chemical Industries, Ltd.), the prepared surfactant with an HLB value of 7, and pure water in the proportions shown in Table 1, and the resulting mixture was ultrasonically treated for 30 minutes to prepare four types of water-in-oil emulsions.

[0114] [Average droplet size, minimum size, and maximum size of droplets in a water-in-oil emulsion] Using a particle size measuring device (Nikkiso Co., Ltd., Nanotrac WaveII UZ152), The average water droplet diameter, minimum diameter, and maximum diameter of the water droplets in the four types of water-in-oil emulsions prepared were measured. First, the background was measured using the hydrocarbon oil A or B used. Then, the inside of the cell was washed with each of the prepared water-in-oil emulsions. Using a refractometer (Anton Paar Japan, multi-wavelength refractometer), the refractive indexes of the hydrocarbon oils A and B were measured at a measurement temperature of 20°C and a measurement wavelength of 589 nm (D line: refractive index range 1.3000 to 1.7100), and both were 1.48. The refractive index of water was set to 1.33. The refractive index of water and the refractive index of the hydrocarbon oils A and B were input into the measurement device, and the shape of the water droplets was set to non-spherical particles and input into the measurement device, and the temperature in the cell was adjusted to 25°C. The measurement time was 120 seconds, and a particle size distribution chart was obtained by the measurement. The above operation was repeated after 30 minutes, and it was confirmed that the particle size distribution range of the water droplet diameter had not changed (the minimum and maximum diameter values ​​in the particle size distribution had not changed). The average water droplet diameter (median diameter D50), minimum diameter, and maximum diameter in the obtained particle size distribution chart were taken as the average water droplet diameter, minimum diameter, and maximum diameter of the water droplets in the water-in-oil emulsion. The measurement results are shown in Table 1.

[0115] [Removal rate of water droplets from water-in-oil emulsion] 20 hollow fiber membranes were cut to a length of 30 cm, and bundled together to prepare a bundle. Next, a polybutylene terephthalate (PBT) tube with an outer diameter of 12.7 mm, an inner diameter of 9.5 mm, and a length of 53 mm was prepared, and a silicone tube with an inner diameter of 12 mm and a length of about 50 mm was inserted about 15 mm into one end opening of the tube to connect it, and a rubber stopper with a length of about 20 mm was inserted into the side of the silicone tube opposite to the side inserted into the PBT tube to plug the one end opening. Next, a two-liquid mixed epoxy resin was injected from the opening of the connecting tube opposite to the side with the rubber stopper, and the space inside the tube was filled with the epoxy resin. Then, one end of the bundle of hollow fiber membranes prepared as above was heat sealed to prevent the epoxy resin from penetrating into the hollow part, and the end tip was inserted into the tube filled with the epoxy resin until it touched the rubber stopper, and the epoxy resin was cured in this state. Next, the region of the cured epoxy resin on the rubber plug side was cut together with the tube to open the hollow part. The same procedure was performed on the other end to prepare a cross-flow module with open hollow parts at both ends of the hollow fiber membrane. Next, the prepared cross-flow module 10 was connected to an internal pressure separation processing line shown in FIG. 2, and the prepared water-in-oil emulsion was continuously permeated through the cross-flow module 10 by a liquid circulation pump 11. In the module, the pressure of the primary pressure gauge 14 and the pressure of the secondary pressure gauge 15 were adjusted by a regulator 12 so that the arithmetic mean value of the pressure of the primary pressure gauge 14 and the pressure of the secondary pressure gauge 15 was 1 bar. Of the water-in-oil emulsion permeating through the module, that which permeated the hollow fiber membrane was collected as a permeate separated from the water-in-oil emulsion, and the remainder was circulated again to the separation processing line. The permeate that flowed out of the cross-flow module between 2 hours and 4 hours after the start of circulation was collected in a receiver 16. The water content in the obtained permeate was calculated from the water content in the sample (permeate) obtained by measurement using a hybrid Karl Fischer moisture meter (Kyoto Electronics Manufacturing Co., Ltd., MKH-700) and the sample amount. Specifically, the sample inlet was opened for 10 seconds before the measurement, a blank measurement was performed, and then an appropriate amount of sample was taken in a micropipette, weighed, and the balance was set to zero. Next, the sample in the micropipette was put into the titration cell through the sample inlet, and the weight of the micropipette was weighed again, and the weight (absolute value) displayed on the balance was taken as the amount of sample. The water content in the permeate was calculated from the amount of water in the sample and the amount of sample obtained by the measurement. The water content in the water-in-oil emulsion was also calculated in the same manner. The removal rate of water droplets in the water-in-oil emulsion was then calculated from the following formula. Removal rate of water droplets from water-in-oil emulsion (%) = 100 - (water content in permeate / water content in water-in-oil emulsion) x 100

[0116] [Permeation flow rate] The permeation flow rate of the water-in-oil emulsion was measured by the same procedure as that for measuring the water droplet removal rate. The permeation flow rate 5 minutes after the start of filtration was calculated by collecting the permeated liquid that had flowed out of the crossflow module within 5 to 6 minutes after the start of circulation in a receiver 16, measuring the weight of the permeated liquid, and calculating the permeation flow rate (L / (m 2The permeation flow rate 60 minutes after the start of filtration was calculated by collecting the permeated liquid that had flowed out of the cross-flow module in 60 to 61 minutes after the start of circulation in the receiver 16, measuring the weight of the permeated liquid, and calculating the permeation flow rate (L / (m 2 ·bar·h) was calculated. Permeation flow rate = weight of permeate (g) / [inner diameter of hollow fiber membrane (m) x 3.14 x effective filtration length of hollow fiber membrane (m) x 20 (pieces) x {(pressure (bar) x specific gravity of permeate (g / L)} x time (h)] Effective filtration length of hollow fiber membrane: The length of the outer surface of the hollow fiber membrane that is not covered with epoxy resin in the crossflow module. The specific gravity of the permeate was measured based on the "Method of measuring density and specific gravity using a pycnometer" in JIS Z 8804:2012 (Method of measuring density and specific gravity of liquids).

[0117] 2. Test Example [Examples 1, 4, 7, and 10] 290 g of polyamide 6 chips (A1030BRT manufactured by Unitika Co., Ltd., relative viscosity 3.53), 492 g of dimethyl sulfone (manufactured by Tokyo Chemical Industry Co., Ltd.), and 218 g of sulfolane (manufactured by Tokyo Chemical Industry Co., Ltd.) (DMS / SFL (weight ratio) = 2.3) were stirred and dissolved at 180 ° C for 1.5 hours, and the stirring speed was reduced and degassed for 1 hour to prepare a membrane-forming stock solution. The membrane-forming stock solution was sent to a spinneret kept at 200 ° C via a metering pump, and a mixture of polyethylene glycol 400 (PEG400) and glycerin (60 parts by weight of PEG400 and 40 parts by weight of glycerin) was poured as an internal coagulation liquid. The extruded membrane-forming stock solution was poured into a coagulation bath consisting of a 60 wt% propylene glycol (PG) aqueous solution at 5 ° C and cooled and solidified to form a polyamide porous membrane. The wound polyamide porous membrane was immersed in water for 24 hours to perform solvent extraction (washing), and then dried by passing through a hot air dryer (temperature inside: 130°C) without stretching to obtain a polyamide hollow fiber membrane. The outer diameter of the obtained polyamide hollow fiber membrane was 502 μm and the inner diameter was 274 μm. The initial bubble point, burst bubble point, removal rate of water droplets in a water-in-oil emulsion, and permeation flow rate were measured using the obtained polyamide hollow fiber membrane. The measurement results are shown in Table 1.

[0118] [Examples 2, 5, 8, and 11] In the preparation of the membrane forming solution, 275 g of polyamide 6 chips (A1030BRT manufactured by Unitika Co., Ltd., relative viscosity 3.53), 532 g of dimethyl sulfone (manufactured by Tokyo Chemical Industry Co., Ltd.), and 193 g of sulfolane (manufactured by Tokyo Chemical Industry Co., Ltd.) (DMS / SFL (weight ratio) = 2.8) were stirred and dissolved at 180 ° C. for 1.5 hours, and the stirring speed was reduced and degassed for 1 hour to prepare the membrane forming solution. The same procedure as in Example 1 was performed to obtain a polyamide hollow fiber membrane. The outer diameter of the obtained polyamide hollow fiber membrane was 532 μm and the inner diameter was 286 μm. The initial bubble point, burst bubble point, removal rate of water droplets in a water-in-oil emulsion, and permeation flow rate were measured using the obtained polyamide hollow fiber membrane. The measurement results are shown in Table 1.

[0119] [Examples 3, 6, 9, and 12] In preparing the film-forming solution, 275 g of polyamide 6 chips (A1030BRT manufactured by Unitika Co., Ltd., relative viscosity 3.53), 532 g of dimethyl sulfone (manufactured by Tokyo Chemical Industry Co., Ltd.), and 193 g of sulfolane (manufactured by Tokyo Chemical Industry Co., Ltd.) (DMS / SFL (weight ratio) = 2.8) were stirred and dissolved at 180 ° C for 1.5 hours, and the stirring speed was reduced and degassed for 1 hour to prepare the film-forming solution. The film-forming solution was sent to a spinneret kept at 200 ° C via a metering pump, and a mixture of polyethylene glycol 200 (PEG200) and glycerin (weight ratio of 75 parts by weight of PEG200 and 25 parts by weight of glycerin) was passed as an internal coagulation liquid. The extruded film-forming solution was poured into a coagulation bath consisting of a 60 wt% propylene glycol (PG) aqueous solution at 5 ° C and cooled and solidified to form a polyamide porous membrane. The wound polyamide porous membrane was immersed in water for 24 hours for solvent extraction (washing), and then dried by passing through a hot air dryer (temperature inside: 130°C) without stretching to obtain a polyamide hollow fiber membrane. The outer diameter of the obtained polyamide hollow fiber membrane was 529 μm and the inner diameter was 287 μm. The initial bubble point, burst bubble point, removal rate of water droplets in a water-in-oil emulsion, and permeation flow rate were measured using the obtained polyamide hollow fiber membrane. The measurement results are shown in Table 1.

[0120] [Comparative Examples 1 and 2] In the preparation of the membrane forming solution, 230 g of polyamide 6 chips (A1030BRT manufactured by Unitika Co., Ltd., relative viscosity 3.53), 565 g of dimethyl sulfone (manufactured by Tokyo Chemical Industry Co., Ltd.), and 205 g of sulfolane (manufactured by Tokyo Chemical Industry Co., Ltd.) (DMS / SFL (weight ratio) = 2.8) were stirred and dissolved at 180 ° C. for 1.5 hours, and the stirring speed was reduced and degassed for 1 hour to prepare the membrane forming solution. The same procedure as in Example 3 was performed to obtain a polyamide hollow fiber membrane. The outer diameter of the obtained polyamide hollow fiber membrane was 530 μm and the inner diameter was 282 μm. The initial bubble point, burst bubble point, removal rate of water droplets in a water-in-oil emulsion, and permeation flow rate were measured using the obtained polyamide hollow fiber membrane. The measurement results are shown in Table 1.

[0121] [Comparative Example 3] Using a polyvinylidene fluoride (PVDF) hollow fiber membrane with an outer diameter of 1069 μm and an inner diameter of 666 μm, the initial bubble point, burst bubble point, removal rate of water droplets in a water-in-oil emulsion, and permeation flow rate were measured. The measurement results are shown in Table 1.

[0122] [Comparative Example 4] Using a polytetrafluoroethylene (PTFE) hollow fiber membrane with an outer diameter of 1990 μm and an inner diameter of 988 μm, the initial bubble point, burst bubble point, removal rate of water droplets in a water-in-oil emulsion, and permeation flow rate were measured. The measurement results are shown in Table 1.

[0123] [Table 1]

[0124] From the results shown in Table 1, the polyamide hollow fiber membranes of Examples 1 to 12 have an initial bubble point of 0.45 MPa or more, and therefore the removal rate of water droplets is 80% or more when filtering a water-in-oil emulsion containing water droplets with an average water droplet diameter of 1.2 to 2.4 μm, and it is understood that even water-in-oil emulsions with very small water droplets can be separated into oil and water to a high degree. Moreover, from Examples 1 to 12, it is understood that the higher the burst bubble point of the polyamide hollow fiber membrane, the higher the removal rate of water droplets. On the other hand, the polyamide hollow fiber membranes of Comparative Examples 1 and 2 have an initial bubble point of 0.37 MPa, and therefore the removal rate of water droplets is about 30% when filtering a water-in-oil emulsion containing water droplets with an average water droplet diameter of 1.2 or 1.3 μm, and it is understood that water-in-oil emulsions with very small water droplets cannot be separated into oil and water to a high degree. In addition, the polyvinylidene fluoride (PVDF) hollow fiber membrane of Comparative Example 3 has an initial bubble point of 0.03 MPa, and the polytetrafluoroethylene (PTFE) hollow fiber membrane of Comparative Example 4 has an initial bubble point of 0.07 MPa. Therefore, the water droplet removal rate is very low when filtering a water-in-oil emulsion containing water droplets with an average diameter of 1.2 μm, and oil-water separation is not possible for water-in-oil emulsions with very small water droplets. [Explanation of symbols]

[0125] 1 Air inlet 2 Regulator 3. Booster tank 4 Speed ​​Controller 5. Pressure Sensor 6 Hollow fiber membrane mini module 7. Glass containers 8. 2-Propanol solution 9 Digital pressure indicator 10 Crossflow Module 11 Liquid delivery pump 12 Regulator 13 Fluid tank 14 Primary pressure gauge 15 Secondary pressure gauge 16 Saucer

Claims

1. A polyamide porous membrane for oil-water separation of a mixed liquid containing water and oil, The polyamide porous membrane is formed of a polyamide resin, and A polyamide porous membrane having an initial bubble point of 0.45 MPa or more in a bubble point test in which air pressure is applied in 2-propanol at 20°C.

2. The polyamide porous membrane according to claim 1, having a burst bubble point of 0.50 to 0.90 MPa in the bubble point test.

3. The polyamide porous membrane according to claim 1 , wherein the oil is a hydrocarbon oil.

4. The polyamide porous membrane according to claim 1 , wherein the mixed liquid is an emulsion.

5. The polyamide porous membrane according to claim 4 , wherein the emulsion is a water-in-oil emulsion.

6. The polyamide porous membrane according to claim 5, wherein the water droplets in the water-in-oil emulsion have an average droplet diameter of 0.5 to 5 μm.

7. For separating oil and water from water-in-oil emulsions.

2. The polyamide porous membrane according to claim 1, which has a water-in-oil emulsion containing 94% by weight of isoparaffin oil, 1% by weight of water, and 5% by weight of a surfactant having an HLB value of 7, and has an average water droplet diameter of 1.2 μm, and has a water droplet removal rate of 80% or more when the emulsion is filtered.

8. For separating oil and water from water-in-oil emulsions.

2. The polyamide porous membrane according to claim 1, which has a water-in-oil emulsion containing 85% by weight of isoparaffin oil, 10% by weight of water, and 5% by weight of a surfactant having an HLB value of 7, and has an average water droplet diameter of 2.3 μm, and has a water droplet removal rate of 80% or more when the emulsion is filtered.

9. For separating oil and water from water-in-oil emulsions.

2. The polyamide porous membrane according to claim 1, which has a water-in-oil emulsion containing 94% by weight of paraffin oil, 1% by weight of water, and 5% by weight of a surfactant having an HLB value of 7, and has an average water droplet diameter of 1.3 μm, and has a water droplet removal rate of 80% or more when the emulsion is filtered.

10. For separating oil and water from water-in-oil emulsions.

2. The polyamide porous membrane according to claim 1, which has a water-in-oil emulsion containing 85% by weight of paraffin oil, 10% by weight of water, and 5% by weight of a surfactant having an HLB value of 7, and has an average water droplet diameter of 2.4 μm, and has a water droplet removal rate of 80% or more when the emulsion is filtered.

11. The polyamide porous membrane according to claim 1 , wherein the polyamide porous membrane is a polyamide hollow fiber membrane.

12. The polyamide porous membrane according to claim 1 , wherein the polyamide resin is polyamide 6.

13. A filtration membrane module comprising a module case containing the polyamide porous membrane according to any one of claims 1 to 12.

14. An oil-water separation method, comprising separating a mixed liquid containing water and oil into oil and water using the filtration membrane module according to claim 13.

Citation Information

Patent Citations

  • Asymmetric semipermeable membrane, production method of the same and water production method using the same

    JP2014144438A

  • Hollow fiber membrane, method for manufacturing the same, and module using hollow fiber membrane

    JP2015198999A

  • Composite hollow fiber membrane and composite hollow fiber membrane manufacturing method

    WO2020175205A1

Cited By

  • C-PTFE / PVDF hollow fiber membrane for oil-water separation and preparation method thereof

    CN119838446A