Nickel-metal hydride battery

By limiting Mn to 15 at% or less and adding Al, the nickel-metal hydride battery addresses the issue of capacity loss due to Mn elution, resulting in improved cycle life and capacity retention.

JP2024135138AActive Publication Date: 2024-10-04TOYOTA JIDOSHA KK

Patent Information

Application Number
JP2023045675
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

Conventional hydrogen storage alloys used in nickel-metal hydride secondary batteries exhibit poor cycle life characteristics due to the elution of manganese (Mn), which reduces battery capacity over charge/discharge cycles.

Method used

A nickel-metal hydride battery design that incorporates a negative electrode active material with a specific composition, where the proportion of Mn is limited to 15 at% or less, and optionally includes aluminum (Al) to enhance alkali resistance, thereby suppressing Mn elution and maintaining battery capacity.

Benefits of technology

The proposed battery design significantly improves capacity retention by reducing Mn elution, leading to enhanced cycle life and sustained performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135138000005
    Figure 2024135138000005
  • Figure 2024135138000006
    Figure 2024135138000006
  • Figure 2024135138000007
    Figure 2024135138000007
Patent Text Reader

Abstract

To provide a novel nickel-metal hydride battery which has improved capacity retention.SOLUTION: A nickel-metal hydride battery of the present disclosure includes a positive electrode active material layer, a negative electrode active material layer, and an aqueous electrolyte. A negative electrode active material contained in the negative electrode active material layer is a hydrogen storage alloy having an AB2 main phase, and the A site includes Ti, Zr, or a combination thereof and the B site includes Mn, Cr, Ni, Fe, or a combination thereof. In a first aspect, among all metal atoms in the hydrogen storage alloy, a proportion of Mn is 15 at% or less, a proportion of Cr is 10 at% to 80 at%, a proportion of Ni is 10 at% to 80 at%, and a proportion of Fe is 50 at% or less. In a second aspect, the hydrogen storage alloy contains Al.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to nickel-metal hydride batteries. [Background technology]

[0002] In recent years, hydrogen storage alloys have been attracting attention as negative electrodes for alkaline storage batteries, and their development as electrode materials with large discharge capacity is underway. The characteristics and performance of these hydrogen storage alloys for electrodes are highly dependent on their composition, crystal structure, and manufacturing method, so these various aspects are being examined from various angles when developing new alloys.

[0003] Although various ideas and improvements have been proposed so far, the usual method is to melt the constituent elements of various hydrogen storage alloys at high temperatures, cool them, and then crush and mold the alloy block, or mix the powder with a conductive agent and a resin binder and bind it to a current collector to use as an active material. However, while most of the hydrogen storage alloys to date have a large discharge capacity as active materials, most of them have poor cycle life characteristics when used in nickel-hydrogen secondary batteries.

[0004] As a solution to these problems, in terms of the alloy composition or crystal structure, it has been proposed that the alloy phase has a Laves phase of an intermetallic compound, and the crystal structure is a cubic C15 type or C14 type. Specifically, Patent Document 1 discloses a hydrogen storage alloy in which the crystal structure of the intermetallic compound as the alloy phase is a cubic C15 type or a hexagonal C14 type belonging to the Laves phase, and the constituent elements Zr, Ti, Nb, V, Ni, Mn, Cr, Co, Fe, Si, Mo, and B are expressed in the following atomic ratio ranges:

[0005] In Patent Document 2, Zr 1-a Mm a Ni b V c Mn d M eThis document discloses a hydrogen storage alloy with excellent friability and a negative electrode for a nickel-hydrogen secondary battery that uses this hydrogen storage alloy as an active material, the alloy having a composition represented by the formula: where M is one or more elements selected from the group consisting of Cr, Fe, Mo, and Nb, and 0.03≦a<0.5, 1.0≦b≦1.50, 0.1≦c≦0.5, 0.2≦d≦0.7, 0.05≦e≦0.30, and 1.8≦b+c+d+e≦2.3. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 10-36930 [Patent Document 2] Japanese Patent Application Publication No. 8-73970 Summary of the Invention [Problem to be solved by the invention]

[0007] The present disclosure provides a novel nickel-metal hydride battery with improved capacity retention. [Means for solving the problem]

[0008] As a result of intensive research, the present inventors have found that the above problems can be solved by the following means, and have completed the nickel-metal hydride battery of the present disclosure. Aspect 1: A nickel-metal hydride battery, A positive electrode active material layer, a negative electrode active material layer, and an aqueous electrolyte solution, The negative electrode active material contained in the negative electrode active material layer is a hydrogen storage alloy having an AB2 type main phase, The A site has Ti, Zr, or a combination thereof; The B site contains Mn, Cr, Ni, Fe, or a combination thereof; and In the total metal atoms of the hydrogen storage alloy, the ratio of Mn is 15 at% or less, the ratio of Cr is 10 at% to 80 at%, the ratio of Ni is 10 at% to 80 at%, and the ratio of Fe is 50 at% or less. Nickel-metal hydride battery. Aspect 2: The nickel-metal hydride battery according to aspect 1, wherein the atomic ratio of Mn to Cr in the B site of the negative electrode active material is 0.8 or less. Aspect 3: A nickel-metal hydride battery, A positive electrode active material layer, a negative electrode active material layer, and an aqueous electrolyte solution, The negative electrode active material contained in the negative electrode active material layer is a hydrogen storage alloy having an AB2 type main phase, The A site has Ti, Zr, or a combination thereof; The B site contains Mn, Cr, Ni, Fe, or a combination thereof; and The hydrogen storage alloy contains Al. Nickel-metal hydride battery. Aspect 4: The nickel-metal hydride battery according to aspect 3, wherein the hydrogen storage alloy contains Al in an amount of 10 at % or less based on the total metal atoms of the hydrogen storage alloy. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a novel nickel-metal hydride battery having an improved capacity retention rate. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic diagram of a nickel-metal hydride battery of the present disclosure. [Diagram 2] FIG. 2 is a graph showing the changes in discharge capacity and capacity retention rate over time in Comparative Example 1 and Examples 1 to 4. [Diagram 3] FIG. 3 is a graph showing the changes in discharge capacity and capacity retention rate over time in Comparative Example 1 and Examples 5 to 8. [Figure 4] FIG. 4 is a graph showing the changes in discharge capacity and capacity retention rate over time in Comparative Example 1 and Examples 9 to 12. [Diagram 5] FIG. 5 is a graph showing the changes in discharge capacity and capacity retention rate over time in Comparative Example 1 and Examples 13 and 14. [Figure 6] FIG. 6 is a graph showing the changes in discharge capacity and capacity retention rate in Comparative Examples 1 to 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Nickel-metal hydride battery The nickel-metal hydride battery of the present disclosure is A positive electrode active material layer, a negative electrode active material layer, and an aqueous electrolyte solution, The negative electrode active material contained in the negative electrode active material layer is a hydrogen storage alloy having an AB2 type main phase, The A site has Ti, Zr, or a combination thereof; The B site contains Mn, Cr, Ni, Fe, or a combination thereof.

[0012] In a first embodiment, in all metal atoms of the hydrogen storage alloy, the proportion of Mn is 15 at% or less, the proportion of Cr is 10 at% to 80 at%, the proportion of Ni is 10 at% to 80 at%, and the proportion of Fe is 50 at% or less.

[0013] In a second embodiment, the hydrogen storage alloy contains Al. Al may be present in the B site or in the grain boundary phase.

[0014] The present inventors have discovered that Mn, an element with a relatively low oxidation potential among the metal elements constituting the negative electrode active material of a nickel-metal hydride battery, dissolves from the negative electrode active material during charge-discharge cycles due to its low resistance to leaching in electrolytes, which are generally strongly alkaline, and this causes a decrease in capacity due to the charge-discharge cycles.

[0015] In response to this, the present inventors have found that the above two aspects can suppress the elution of Mn, and as a result, the decrease in capacity due to charge-discharge cycles can be suppressed.

[0016] More specifically, in the first embodiment, by reducing the amount of Mn, the amount of eluted Mn is reduced, and thus the reduction in battery capacity can be suppressed.

[0017] In the second embodiment, the addition of Al enhances the alkali resistance of the hydrogen storage alloy, thereby making it possible to suppress the elution of Mn.

[0018] FIG. 1 is a schematic diagram showing a configuration of a nickel-metal hydride battery 100 according to a first embodiment of the present disclosure. As shown in FIG. 1, the nickel-metal hydride battery 100 may include a positive electrode 10, a separator 20, and a negative electrode 30. The positive electrode 10 may include a positive electrode active material layer 11 and a positive electrode current collector 12, and the negative electrode 30 may include a negative electrode active material layer 31 and a negative electrode current collector 32. In this case, the negative electrode active material layer 31 may contain the above-mentioned negative electrode active material. Although not shown, the above-mentioned aqueous electrolyte may be contained in the positive electrode active material layer 11 and the negative electrode active material layer 31.

[0019] Each component of the present disclosure will be described below.

[0020] <Negative electrode current collector layer> The negative electrode current collector layer may be made of a known metal that can be used as a negative electrode current collector for a nickel-metal hydride battery. Examples of such metals include metal materials containing at least one element selected from the group consisting of Cu, Ni, Al, V, Au, Pt, Mg, Fe, Ti, Pb, Co, Cr, Zn, Ge, In, Sn, and Zr. In particular, when considering stability in an aqueous electrolyte, the negative electrode current collector may contain at least one element selected from the group consisting of Al, Ti, Pb, Zn, Sn, Mg, Zr, and In, may contain at least one element selected from the group consisting of Ti, Pb, Zn, Sn, Mg, Zr, and In, or may contain Ti. All of Al, Ti, Pb, Zn, Sn, Mg, Zr, and In have low work functions, and it is considered that electrolysis of the aqueous electrolyte is unlikely to occur even if they come into contact with the aqueous electrolyte.

[0021] <Negative electrode active material layer> The negative electrode active material layer contains a negative electrode active material. The negative electrode active material layer may contain a conductive assistant and a binder in addition to the negative electrode active material. The thickness of the negative electrode active material layer is not particularly limited, but may be, for example, 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.

[0022] (Negative electrode active material) The negative electrode active material contains a hydrogen storage alloy having an AB2 type main phase.

[0023] The content of the negative electrode active material is not particularly limited and may be, for example, 20 mass% or more, 30 mass% or more, 40 mass% or more, or 45 mass% or more, relative to the mass of the negative electrode active material layer, and may be 99 mass% or less, 97 mass% or less, 95 mass% or less, 29 mass% or less, 90 mass% or less, 88 mass% or less, 85 mass% or less, 83 mass% or less, 80 mass% or less, 75 mass% or less, 70 mass% or less, 65 mass% or less, 60 mass% or less, 55 mass% or less, or 50 mass% or less.

[0024] (Negative electrode active material: hydrogen storage alloy) The hydrogen storage alloy has an AB2 type main phase, where the atom with the larger atomic radius is referred to as "A" and the atom with the smaller atomic radius is referred to as "B" among two types of atoms with different sizes.

[0025] The A site comprises Ti, Zr, or a combination thereof.

[0026] The B site contains Mn, Cr, Ni, Fe, or a combination thereof.

[0027] The hydrogen storage alloy of the present disclosure can be obtained by mixing and melting the metals that make it up. Melting can be performed, for example, by an arc melting method.

[0028] (Hydrogen Storage Alloy: First Aspect) In a first aspect of the hydrogen storage alloy of the present disclosure, the Mn content may be 15 at% or less, 14 at% or less, 13 at% or less, 12 at% or less, 11 at% or less, 10 at% or less, 9 at% or less, 8 at% or less, 7 at% or less, 6 at% or less, 5 at% or less, 4 at% or less, 3 at% or less, 2 at% or less, 1 at% or less, or 0 at% relative to the total metal atoms of the hydrogen storage alloy.

[0029] In a first aspect of the hydrogen storage alloy of the present disclosure, the Cr content may be 10 at% or more, 12 at% or more, 15 at% or more, or 18 at% or more, and may be 80 at% or less, 75 at% or less, 70 at% or less, 65 at% or less, 60 at% or less, 55 at% or less, 50 at% or less, 45 at% or less, 40 at% or less, or 38 at% or less, relative to the total metal atoms of the hydrogen storage alloy.

[0030] In a first aspect of the hydrogen storage alloy of the present disclosure, the Ni content may be 10 at% or more, 12 at% or more, 15 at% or more, or 18 at% or more, and may be 80 at% or less, 75 at% or less, 70 at% or less, 65 at% or less, 60 at% or less, 55 at% or less, 50 at% or less, 45 at% or less, 40 at% or less, 38 at% or less, 35 at% or less, or 32 at% or less, relative to the total metal atoms of the hydrogen storage alloy.

[0031] In a first aspect of the hydrogen storage alloy of the present disclosure, the Fe content may be 50 at% or less, 45 at% or less, 40 at% or less, 35 at% or less, 30 at% or less, 25 at% or less, 20 at% or less, 15 at% or less, 10 at% or less, 5 at% or less, 3 at% or less, 2 at% or less, 1 at% or less, or 0 at% or less, relative to the total metal atoms of the hydrogen storage alloy.

[0032] In a first aspect of the hydrogen storage alloy of the present disclosure, the content of metal atoms belonging to the A site may be 20 at% or more, 25 at% or more, 28 at% or more, 30 at% or more, 33 at% or more, 35 at% or more, or 38 at% or more, and may be 60 at% or less, 55 at% or less, 53 at% or less, 50 at% or less, 48 ​​at% or less, or 45 at% or less, relative to the total metal atoms of the hydrogen storage alloy.

[0033] In a first aspect of the hydrogen storage alloy of the present disclosure, the content of metal atoms belonging to the B site may be 40 at% or more, 45 at% or more, 47 at% or more, 50 at% or more, 52 at% or more, or 55 at% or more, and may be 80 at% or less, 75 at% or less, 72 at% or less, 70 at% or less, 67 at% or less, 65 at% or less, or 62 at% or less, relative to the total metal atoms of the hydrogen storage alloy.

[0034] In the first embodiment of the hydrogen storage alloy of the present disclosure, the atomic ratio of Ni to Cr is preferably 1.5 or less, 1.4 or less, 1.3 or less, or 1.2 or less from the viewpoint of capacity retention rate. This atomic ratio may be 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, or 0.9 or more.

[0035] In a first aspect of the hydrogen storage alloy of the present disclosure, from the viewpoint of capacity retention, it is preferable that the atomic ratio of Mn to Cr is 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.3 or less, 0.2 or less, 0.1 or less, or 0. When all or a part of Mn in a conventional hydrogen storage alloy is replaced with Cr, which has a similar atomic radius and relatively high corrosion resistance, elution of components of the hydrogen storage alloy during charge / discharge cycles can be suppressed.

[0036] (Hydrogen storage alloy: second embodiment) In a second embodiment, the hydrogen storage alloy of the present disclosure contains Al.

[0037] In a second aspect of the hydrogen storage alloy of the present disclosure, the Al content may be 1 at% or more, 3 at% or more, 5 at% or more, or 7 at% or more, and may be 10 at% or less, or 9 at% or less, relative to the total metal atoms of the hydrogen storage alloy.

[0038] In a second aspect of the hydrogen storage alloy of the present disclosure, the Mn content, relative to the total metal atoms of the hydrogen storage alloy, may be 20 at% or less, 19 at% or less, 18 at% or less, 17 at% or less, 16 at% or less, 15 at% or less, 14 at% or less, 13 at% or less, 12 at% or less, 11 at% or less, 10 at% or less, 9 at% or less, 8 at% or less, 7 at% or less, 6 at% or less, 5 at% or less, 4 at% or less, 3 at% or less, 2 at% or less, 1 at% or less, or 0 at%.

[0039] In the second embodiment of the hydrogen storage alloy of the present disclosure, the contents of metal atoms other than Al and Mn can be referred to the description of the first embodiment.

[0040] (Conductive assistant) The conductive assistant optionally contained in the positive electrode active material layer may be any of those known as conductive assistants used in nickel-metal hydride batteries, such as metal powder, metal oxide, and carbon material. Metal powder may be, for example, Ni powder, specifically, Ketjen Black (KB), vapor grown carbon fiber (VGCF), acetylene black (AB), carbon nanotube (CNT), carbon nanofiber (CNF), carbon black, coke, graphite, and the like. Alternatively, it may be a metal material that can withstand the environment during use of the battery. Only one type of conductive assistant may be used alone, or two or more types may be used in combination. The conductive assistant may be in various shapes, such as powder and fiber.

[0041] The amount of the conductive assistant contained in the negative electrode active material layer is not particularly limited, and may be, for example, 1 mass% or more, 3 mass% or more, 5 mass% or more, 7 mass% or more, 10 mass% or more, 15 mass% or more, 20 mass% or more, 25 mass% or more, 30 mass% or more, 35 mass% or more, 40 mass% or more, or 45 mass% or more, relative to the mass of the negative electrode active material, and may be 70 mass% or less, 65 mass% or less, 60 mass% or less, 55 mass% or less, or 50 mass% or less.

[0042] (binder) The binder optionally contained in the negative electrode active material layer may be any binder known to be used in potassium ion secondary batteries. For example, styrene butadiene rubber (SBR)-based binders, carboxymethyl cellulose (CMC)-based binders, acrylonitrile butadiene rubber (ABR)-based binders, butadiene rubber (BR)-based binders, polyvinylidene fluoride (PVDF)-based binders, polytetrafluoroethylene (PTFE)-based binders, etc. Only one type of binder may be used alone, or two or more types may be used in combination.

[0043] The amount of binder contained in the negative electrode active material layer is not particularly limited, and may be, for example, 1 mass % or more, or 2 mass % or more, and may be 20 mass % or less, 18 mass % or less, 15 mass % or less, 12 mass % or less, 10 mass % or less, 7 mass % or less, 5 mass % or less, 4 mass % or less, or 3 mass % or less, relative to the mass of the negative electrode active material.

[0044] <Positive electrode current collector layer> The positive electrode current collector layer may be made of a known metal that can be used as a positive electrode current collector for a nickel-metal hydride battery. Examples of such metals include metal materials containing at least one element selected from the group consisting of Cu, Ni, Al, V, Au, Pt, Mg, Fe, Ti, Pb, Co, Cr, Zn, Ge, In, Sn, and Zr. The form of the positive electrode current collector is not particularly limited. It may take various forms such as a foil, a mesh, or a porous form. The above metal may be vapor-deposited or plated on the surface of a substrate.

[0045] <Cathode active material layer> The positive electrode active material layer contains a positive electrode active material. The positive electrode active material layer may further contain an optional conductive assistant, a binder, etc. The thickness of the positive electrode active material layer is not particularly limited, but may be, for example, 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.

[0046] The type of conductive assistant or binder optionally contained in the positive electrode active material layer is not particularly limited, and may be appropriately selected from, for example, those exemplified as the conductive assistant or binder optionally contained in the negative electrode active material layer. The amount of conductive assistant or binder contained in the positive electrode active material layer is not particularly limited, and the amount mentioned for the negative electrode active material layer may be referred to.

[0047] (Cathode active material) As the positive electrode active material, any nickel compound, particularly nickel hydroxide, that can be used to form a nickel-metal hydride battery in combination with an aqueous electrolyte and the negative electrode of the present disclosure can be used, such as nickel hydroxide (Ni(OH)2), nickel oxyhydroxide (NiO(OH)), etc.

[0048] The content of the positive electrode active material is not particularly limited, and may be, for example, 20 mass% or more, 30 mass% or more, 40 mass% or more, 50 mass% or more, 60 mass% or more, or 70 mass% or more, and may be 99 mass% or less, 97 mass% or less, 95 mass% or less, 29 mass% or less, 90 mass% or less, 88 mass% or less, 85 mass% or less, 83 mass% or less, or 80 mass% or less, relative to the mass of the positive electrode active material layer.

[0049] <Aqueous electrolyte> The aqueous electrolyte used in the nickel-metal hydride battery of the present disclosure contains an aqueous solvent and an alkali metal hydroxide dissolved in the aqueous solvent.

[0050] The pH of the aqueous electrolyte may be 10.0 or greater, 11.0 or greater, 11.5 or greater, 12.0 or greater, 12.5 or greater, 13.0 or greater, or 13.5 or greater.

[0051] (Water-based solvent) The aqueous solvent is a solvent containing water. The aqueous solvent may contain water as a main component. That is, based on the total amount of the aqueous solvent constituting the electrolytic solution (100 mol%), water may account for 50 mol% or more, 70 mol% or more, 90 mol% or more, or 95 mol% or more. The upper limit of the proportion of water in the aqueous solvent is not particularly limited, and the aqueous solvent may be 100 mol%, that is, the entire amount of the aqueous solvent may be water.

[0052] The aqueous solvent may consist of water alone, but may further contain other components, such as one or more organic solvents selected from ethers, carbonates, nitriles, alcohols, ketones, amines, amides, sulfur compounds, and hydrocarbons. The solvent other than water may account for 50 mol% or less, 30 mol% or less, 10 mol% or less, or 5 mol% or less based on the total amount of the aqueous solvent constituting the electrolyte (100 mol%).

[0053] (alkali metal hydroxides) Examples of alkali metal hydroxides that can be used include potassium hydroxide (KOH), sodium hydroxide (NaOH), and lithium hydroxide (LiOH).

[0054] The concentration of the alkali metal hydroxide may be 1 mol / L or more, 2 mol / L or more, 3 mol / L or more, 4 mol / L or more, or 5 mol / L or more, and may be 20 mol / L or less, 18 mol / L or less, 15 mol / L or less, 12 mol / L or less, 10 mol / L or less, 9 mol / L or less, 8 mol / L or less, or 7 mol / L or less.

[0055] <Other configurations> In addition to the above configuration, the nickel-metal hydride battery may also include obvious battery components such as terminals and a battery case.

[0056] A nickel-metal hydride battery having the above configuration can be manufactured, for example, by forming a positive electrode active material layer on the surface of a positive electrode current collector by a dry or wet process to obtain a positive electrode, forming a negative electrode active material layer on the surface of a negative electrode current collector by a dry or wet process to obtain a negative electrode, and disposing a separator between the positive electrode and the negative electrode and impregnating them with an aqueous electrolyte solution. EXAMPLES

[0057] The present disclosure will be specifically described with reference to examples and comparative examples, but the present disclosure is not limited thereto.

[0058] Using the reagents of each metal element in the atomic ratio shown in Table 1, 15g ingots were prepared by arc melting. The alloys were prepared by homogenizing the materials by melting three times. In the reagents used, the purity of Zr was 98%, and the purity of the other metal elements was 99.9%.

[0059] The obtained alloy was pulverized by a manual stamp mill (Tokyo Glass Equipment, DA-30) and classified into particles of 38 to 100 μm using a 38 μm sieve and a 100 μm sieve.

[0060] The alloy obtained was quantitatively analyzed by ICP.

[0061] For the first embodiment, the amounts of reagents added are shown in Table 1, and the measured ICP values ​​are shown in Table 2.

[0062] For the second embodiment, the amounts of reagents added are shown in Table 3, and the measured ICP values ​​are shown in Table 4.

[0063] [Table 1]

[0064] [Table 2]

[0065] [Table 3]

[0066] [Table 4]

[0067] <<Preparation of evaluation cell>> An evaluation cell was prepared as follows.

[0068] First, a negative electrode was prepared. More specifically, 49 parts by mass of the above alloy as a negative electrode active material, 49 parts by mass of Ni powder as a conductive assistant, and 2 parts by mass of carboxymethyl cellulose (CMC) as a binder were kneaded to prepare a paste-like composition. This paste-like composition was filled into a negative electrode current collector, and then vacuum dried at 80°C, and then roll pressed (clearance 300 μm) with pressure of about 8 kN to obtain a negative electrode. As the negative electrode current collector, porous Ni (Celmet #7, manufactured by Sumitomo Electrochemical Industries, Ltd., thickness 1.6 mm) with a Ni tab welded was used. The capacity was adjusted to aim for about 240 mAh.

[0069] Next, a positive electrode was prepared. More specifically, 88 parts by mass of nickel hydroxide (Ni(OH)2) as a positive electrode active material, 10 parts by mass of cobalt oxide (CoO) as a conductive assistant, and 1 part by mass of two types of binders (carboxymethyl cellulose (CMC) and polyvinyl alcohol (PVA)) were kneaded to prepare a paste-like composition. This paste-like composition was filled into the porous nickel, and then vacuum dried at 80°C, and roll pressed with a pressure of about 8kN to obtain a positive electrode. The capacity ratio of the negative electrode and the positive electrode was adjusted to negative electrode:positive electrode=1:4.5.

[0070] Next, an electrolyte solution was prepared. Pure water was added to KOH to adjust the concentration of KOH to 6 mol / L, and 90 ml of electrolyte solution was obtained. After that, the electrolyte solution and a separator (PE / PP nonwoven fabric, thickness 150 μm) were placed in a container, and further, a negative electrode (working electrode), a positive electrode (counter electrode), and a Hg / HgO electrode (reference electrode) were placed to obtain an evaluation cell.

[0071] <Charge / discharge test (25℃)> The obtained evaluation cell was subjected to charge-discharge accelerating cycles until the negative electrode capacity was saturated. More specifically, the following charge-discharge cycles (1) to (4) were performed. (1) The battery was charged at 0.1 C for 14 hours and then discharged at 0.1 C until the negative electrode potential reached −0.6 V. (2) The battery was charged at 0.5 C for 2.2 hours and then discharged at 0.5 C until the negative electrode potential reached −0.6 V. (3) The battery was then charged at 0.1C for 14 hours and then discharged at 0.1C until the negative electrode potential reached -0.6V. (4) The above charge / discharge steps (1) to (3) were repeated until the 0.1 C discharge capacity was saturated, and the obtained electrode capacity was regarded as the initial capacity.

[0072] The intersections with the vertical axes of the graphs shown in FIGS. 2 to 6 correspond to this initial capacity.

[0073] After the charge-discharge adjustment, the evaluation cell was charged for 5 hours at 0.1 C. Next, while observing the amount of electricity, the cell was repeatedly charged and discharged at 0.5 C, with the potential corresponding to SOC 25% and the potential corresponding to SOC 75% going back and forth 20 times, to perform charge and discharge corresponding to SOC 1000%.

[0074] After this cycle, the battery was charged at 0.1 C for 14 hours, and then discharged at 0.1 C until the negative electrode potential reached −0.6 V, to confirm the capacity.

[0075] The above charge / discharge cycle and capacity confirmation were repeated every SOC 1000%, and the capacity transition was recorded for every SOC 1000%. This operation was repeated until charging / discharging equivalent to SOC 10000% was performed.

[0076] The evaluation results of the examples and comparative examples are shown in FIGS.

[0077] 2 to 5 and Tables 1 and 2, it can be seen that, compared to Comparative Example 1 (base composition), Examples 1 to 12, in which the Mn content was set to 15 at % or less by reducing the amount of Mn or substituting all or a part of Mn with Cr or Fe, had a good capacity retention rate.

[0078] Also, it can be seen from FIG. 6 and Tables 3 and 4 that in Examples 13 and 14 in which Al was added, the capacity retention rate was improved. [Explanation of symbols]

[0079] 10 positive electrode 11 Cathode active material layer 12 Positive electrode current collector 20 Separator 30 negative electrode 31 Negative electrode active material layer 32 Negative electrode current collector 100 Nickel Metal Hydride Battery

Claims

1. A nickel-metal hydride battery, A positive electrode active material layer, a negative electrode active material layer, and an aqueous electrolyte solution, The negative electrode active material contained in the negative electrode active material layer is 2 A hydrogen storage alloy having a main phase of the type: The A site has Ti, Zr, or a combination thereof; The B site contains Mn, Cr, Ni, Fe, or a combination thereof; and In the total metal atoms of the hydrogen storage alloy, the ratio of Mn is 15 at% or less, the ratio of Cr is 10 at% to 80 at%, the ratio of Ni is 10 at% to 80 at%, and the ratio of Fe is 50 at% or less. Nickel-metal hydride battery.

2. 2. The nickel-metal hydride battery in accordance with claim 1, wherein the atomic ratio of Mn to Cr in the B site of the negative electrode active material is 0.8 or less.

3. A nickel-metal hydride battery, A positive electrode active material layer, a negative electrode active material layer, and an aqueous electrolyte solution, The negative electrode active material contained in the negative electrode active material layer is 2 A hydrogen storage alloy having a main phase of the type: The A site has Ti, Zr, or a combination thereof; The B site contains Mn, Cr, Ni, Fe, or a combination thereof; and The hydrogen storage alloy contains Al. Nickel-metal hydride battery.

4. 4. The nickel-metal hydride battery in accordance with claim 3, wherein said hydrogen storage alloy contains Al at a ratio of 10 at % or less based on all metal atoms in said hydrogen storage alloy.

Citation Information

Patent Citations

  • Hydrogen-storing electrode

    JP1988284758A

  • Hydrogen storage alloy and hydrogen storage alloy electrode

    JP1995003365A

  • Hydrogen storage alloy and hydrogen storage alloy electrode

    JP1996319529A

  • High-power nickel-metal hydride battery and high-power alloy / electrode used therein

    JP2004506813A

  • Hydrogen storage alloy

    JP2018510965A

Cited By

  • Hydrogen storage alloy particles, nickel-metal hydride battery, and method for manufacturing hydrogen storage alloy particles

    JP2026156095A

  • Hydrogen storage alloy particles, nickel-metal hydride battery, and method for manufacturing hydrogen storage alloy particles

    JP2026161330A