Electrode, secondary battery, battery pack, and vehicle
By using inorganic particles with a larger diameter and a thin inorganic particle-containing layer to trap hydrofluoric acid, the electrode structure addresses the deterioration issue of niobium titanium oxide, enhancing the cycle and output performance of non-aqueous electrolyte batteries.
Patent Information
- Application Number
- JP2023045822
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-22
AI Technical Summary
Non-aqueous electrolyte batteries, such as lithium ion secondary batteries, experience a decrease in discharge capacity due to the deterioration of niobium titanium oxide electrodes caused by hydrofluoric acid produced from side reactions, leading to degraded cycle and output performance.
Incorporating inorganic particles with an inorganic particle-containing layer on the surface of niobium titanium oxide particles, where the average particle diameter of the inorganic particles is larger than the thickness of the layer, to trap hydrofluoric acid and prevent contact with the niobium titanium oxide, thereby suppressing deterioration and improving cycle and output performance.
The described electrode structure enhances the cycle and output performance of the battery by effectively capturing hydrofluoric acid, preventing niobium titanium oxide deterioration, and maintaining high ionic and electronic conductivity.
Smart Images

Figure 2024135237000001_ABST
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention relates to an electrode, a secondary battery, a battery pack, and a vehicle. [Background technology]
[0002] 2. Description of the Related Art In non-aqueous electrolyte batteries such as lithium ion secondary batteries, there is a problem that the discharge capacity of the electrodes decreases with the increase in charge / discharge cycles. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-11929 A [Patent Document 2] JP 2012-209064 A [Patent Document 3] Patent Publication No. 2021-44221 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the embodiments is to provide an electrode having excellent cycle performance and output performance, a secondary battery including the electrode, a battery pack including the secondary battery, and a vehicle including the battery pack. [Means for solving the problem]
[0005] According to an embodiment, an electrode is provided. The electrode includes inorganic particles, niobium titanium oxide particles, and an inorganic particle-containing layer that covers at least a portion of the surface of the niobium titanium oxide particles. The average particle size of the inorganic particles is greater than the thickness of the inorganic particle-containing layer.
[0006] According to another embodiment, a secondary battery including the electrode of the embodiment is provided.
[0007] According to another embodiment, a battery pack including the secondary battery of the embodiment is provided.
[0008] According to another embodiment, a vehicle including a battery pack of the embodiment is provided. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a cross-sectional view illustrating an example of an electrode according to an embodiment. [Diagram 2] FIG. 4 is an enlarged view showing the vicinity of an active material particle in an example of an electrode according to the embodiment. [Diagram 3] FIG. 11 is a cross-sectional view illustrating an example of an electrode according to a reference example. [Figure 4] FIG. 2 is a schematic diagram showing a HAADF-STEM image of a first particle. [Diagram 5] FIG. 1 is a cross-sectional view illustrating an example of a secondary battery according to an embodiment. [Figure 6] 6 is an enlarged cross-sectional view of a portion A of the secondary battery shown in FIG. 5. [Figure 7] FIG. 4 is a partially cutaway perspective view illustrating a schematic diagram of another example of a secondary battery according to an embodiment. [Figure 8] 8 is an enlarged cross-sectional view of a portion B of the secondary battery shown in FIG. 7. [Figure 9] FIG. 1 is a perspective view illustrating an example of a battery pack according to an embodiment. [Figure 10] FIG. 1 is an exploded perspective view illustrating an example of a battery pack according to an embodiment. [Figure 11] FIG. 11 is a block diagram showing an example of an electric circuit of the battery pack shown in FIG. [Figure 12] 1 is a partially see-through view illustrating an example of a vehicle according to an embodiment. [Figure 13] 1 is a diagram illustrating an example of a control system for an electrical system in a vehicle according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiments will be described with reference to the drawings as appropriate. Note that the same reference numerals are used to designate common components throughout the embodiments, and duplicated descriptions will be omitted. Also, each figure is a schematic diagram for explaining the embodiments and for facilitating understanding thereof, and the shapes, dimensions, ratios, etc. may differ from those of the actual device, but these can be appropriately modified in design by taking into consideration the following explanation and known techniques.
[0011] (First embodiment) One of the factors that cause the cycle performance and output performance of the electrode to decrease is the deterioration of the niobium titanium oxide in the electrode, which can occur, for example, when hydrofluoric acid produced by a side reaction comes into contact with the niobium titanium oxide.
[0012] As a result of intensive research, the present inventors have found that inorganic particles can capture (trap) hydrofluoric acid. However, when the electrode contains inorganic particles alone, if hydrofluoric acid approaches the niobium titanium oxide without being captured by the inorganic particles, the niobium titanium oxide is inevitably deteriorated.
[0013] Based on this result, the inventors conducted further research and achieved the electrode according to the first embodiment.
[0014] According to a first embodiment, an electrode is provided. The electrode according to the first embodiment includes inorganic particles, niobium titanium oxide particles, and an inorganic particle-containing layer that covers at least a part of the surface of the niobium titanium oxide particles. The average particle size of the inorganic particles is larger than the thickness of the inorganic particle-containing layer.
[0015] Both the inorganic particles and the inorganic particle-containing layer can capture (trap) hydrofluoric acid.
[0016] Therefore, the inorganic particles can suppress the approach of hydrofluoric acid to the niobium titanium oxide particles. Also, even if hydrofluoric acid approaches the niobium titanium oxide particles without being captured by the inorganic particles, the inorganic particle-containing layer can capture the hydrofluoric acid. Therefore, according to this electrode, the contact of hydrofluoric acid with the niobium titanium oxide particles can be suppressed, and as a result, the deterioration of the niobium titanium oxide can be suppressed. Therefore, it contributes to improving cycle performance and output performance.
[0017] Furthermore, in the electrode, the average particle size of the inorganic particles is larger than the thickness of the inorganic particle-containing layer. Therefore, the average particle size of the inorganic particles is not too small, so that the inorganic particles are less likely to aggregate with each other during the manufacturing process of the electrode. Therefore, the inorganic particles can be uniformly present in the electrode, so that hydrofluoric acid can be efficiently captured. As a result, the deterioration of the niobium titanium oxide can be suppressed. Therefore, it contributes to improving cycle performance and output performance.
[0018] In addition, the thickness of the inorganic particle-containing layer is smaller than the average particle diameter of the inorganic particles, so that the decrease in ion conductivity caused by the inorganic particle-containing layer being too thick can be suppressed, and as a result, the output performance can be improved.
[0019] When the inorganic particle-containing layer is thick, the hydrofluoric acid trapping ability tends to be greater, but the electronic conductivity of the active material particles may be lower than when the inorganic particle-containing layer is thin.
[0020] On the other hand, the larger the average particle diameter of the inorganic particles, the more the inorganic particles can be inhibited from aggregating with each other, and therefore the inorganic particles tend to be uniformly dispersed in the electrode. The electrode may further contain a conductive agent. By inhibiting the aggregation of the inorganic particles, the conductive agent is less likely to be adsorbed to the inorganic particles, and the dispersibility of the conductive agent can be improved. This contributes to improving the output performance. Therefore, even when the thickness of the inorganic particle-containing layer is thick, the output performance of the electrode can be kept high by combining it with inorganic particles having a large average particle diameter.
[0021] In such an electrode, the average particle size of the inorganic particles is larger than the thickness of the inorganic particle-containing layer, and therefore the high dispersibility of the inorganic particles and the conductive agent has a large effect of improving output performance against the decrease in electronic conductivity that accompanies an increase in the thickness of the inorganic particle-containing layer, thereby making it possible to maintain high output performance.
[0022] In addition, when the thickness of the inorganic particle-containing layer is thin, the electronic conductivity of the active material particles can be kept high. Therefore, as long as the thickness is larger than that of the inorganic particle-containing layer, even when combined with inorganic particles having a relatively small average particle size, the effect of improving electronic conductivity due to the thin inorganic particle-containing layer against the decrease in output performance caused by the small average particle size of the inorganic particles can be increased. Therefore, the output performance as an electrode can be kept high.
[0023] Hereinafter, electrodes according to embodiments will be described in detail with reference to the drawings.
[0024] The electrode may be, for example, for a nonaqueous electrolyte battery. The nonaqueous electrolyte battery may be, for example, a nonaqueous electrolyte battery with an alkali metal ion as a carrier ion. For example, it may be a lithium battery (lithium ion battery). The electrode may be, for example, for a secondary battery.
[0025] In the manufacturing process of a non-aqueous electrolyte battery, water is likely to be mixed in as an inevitable impurity. When a non-aqueous electrolyte containing fluorine atoms is used as the non-aqueous electrolyte to be combined with an electrode, a side reaction occurs between water and the non-aqueous electrolyte, and hydrofluoric acid (hydrogen fluoride, HF) may be generated as a decomposition product of the non-aqueous electrolyte. Details of the non-aqueous electrolyte will be described later.
[0026] When hydrofluoric acid comes into contact with a material contained in an electrode, it may dissolve, for example, a transition metal. The dissolved transition metal may be deposited, for example, on the electrode. In addition, when an electrode is combined with an electrolyte, hydrofluoric acid may react with the electrolyte to form lithium fluoride. The lithium fluoride may be deposited, for example, on the electrode. These substances deposited on the electrode may be a cause of an increase in resistance.
[0027] The electrode includes inorganic particles and an inorganic particle-containing layer, which can suppress the elution of transition metals and the formation of lithium fluoride, thereby improving the output performance of the electrode.
[0028] Fig. 1 is a cross-sectional view showing an example of an electrode. Fig. 2 is an enlarged view showing the vicinity of active material particles in the example of the electrode. For convenience, the conductive agent and binder that may be contained in the active material-containing layer are omitted in Figs. 1 and 2.
[0029] The electrode 3 includes a current collector 3a and an active material-containing layer 3b formed on the current collector 3a. The active material-containing layer 3b includes first particles 10 and inorganic particles 13. The first particles 10 include niobium titanium oxide particles 11 and an inorganic particle-containing layer 12 that covers at least a portion of the surface of the niobium titanium oxide particles 11.
[0030] As shown in FIG. 2, the first particle 10 may include an exposed portion 14. The exposed portion 14 is a portion of the surface of the niobium titanium oxide particle 11 that is not covered with the inorganic particle-containing layer 12. In other words, the exposed portion 14 is a portion of the surface of the first particle 10 where the surface of the niobium titanium oxide particle 11 is exposed. Although the first particle 10 shown in FIG. 2 includes the exposed portion 14, the first particle 10 may not include an exposed portion. In other words, the entire surface of the niobium titanium oxide particle 11 may be covered with the inorganic particle-containing layer 12.
[0031] If the first particle 10 includes the exposed portion 14, the ion conductivity can be kept high and the output performance can be improved, which is preferable.
[0032] When the first particle 10 includes the exposed portion 14, at least a part of the surface of the niobium titanium oxide particle 11 may be exposed on the surface of the electrode 3. The surface of the electrode 3 may be, of the main surfaces of the active material-containing layer 3b, a main surface on the side not in contact with the current collector 3a.
[0033] An electrode according to a reference example will be described with reference to FIG.
[0034] FIG. 3 is a cross-sectional view showing an example of an electrode according to a reference example. For convenience, the conductive agent and binder that may be contained in the active material-containing layer are omitted in FIG. 3. The electrode 30 according to the reference example includes a current collector 3a and an active material-containing layer 30b formed on the current collector 3a. The active material-containing layer 30b includes niobium titanium oxide particles 11 and inorganic particles 13.
[0035] As shown in Fig. 3, in the electrode 30 according to the reference example, no inorganic particle-containing layer is present on the surface of the niobium titanium oxide particle 11. Therefore, the entire surface of the niobium titanium oxide particle 11 is exposed. Therefore, when hydrofluoric acid that has not been captured by the inorganic particles 13 approaches the niobium titanium oxide particle 11, the hydrofluoric acid may come into contact with the surface of the niobium titanium oxide particle 11. As a result, the niobium titanium oxide particle may be deteriorated.
[0036] The electrodes according to the embodiments will be described in further detail below.
[0037] The electrode according to the embodiment may include a current collector and an active material-containing layer. The active material-containing layer may be formed on one or both sides of the current collector. The active material-containing layer includes first particles and inorganic particles. The first particles include niobium titanium oxide particles, and an inorganic particle-containing layer that covers at least a portion of the surface of the niobium titanium oxide particles.
[0038] The niobium titanium oxide can function as an active material. The first particles can be active material particles because they contain niobium titanium oxide particles. The active material-containing layer can contain the first particles alone as an active material, or a mixture of the first particles and one or more other active materials.
[0039] The active material-containing layer can contain an active material including first particles, inorganic particles, and optionally a conductive agent and a binder.
[0040] The average particle size of the first particles including the niobium titanium oxide particles and the inorganic particle-containing layer is preferably in the range of 0.5 μm to 2.0 μm. When the average particle size of the first particles is 0.5 μm or more, the surface energy of the first particles can be reduced, so that, for example, aggregation during the dispersion step in preparing the slurry can be suppressed. When the average particle size of the first particles is 2.0 μm or less, the Li + This increases the diffusion rate within the solid. + Diffusion within a solid can be increased.
[0041] An example of the niobium titanium oxide contained in the niobium titanium oxide particles is monoclinic niobium titanium oxide.
[0042] As an example of the monoclinic niobium titanium oxide, Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δ Here, M1 is at least one selected from the group consisting of Zr, Si, and Sn. M2 is at least one selected from the group consisting of V, Ta, and Bi. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3. Specific examples of monoclinic niobium titanium oxide include Li x Examples include Nb2TiO7 (0≦x≦5).
[0043] Another example of monoclinic niobium titanium oxide is Li x Ti 1-y M3 y+z Nb 2-z O 7-δ Here, M3 is at least one selected from Mg, Fe, Ni, Co, W, Ta, and Mo. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3.
[0044] The form of the inorganic particle-containing layer is not particularly limited, but may be, for example, a form in which particles containing an inorganic material are aggregated on the surface of a niobium titanium oxide particle to cover at least a part of the surface of the niobium titanium oxide particle. The particles containing an inorganic material may be primary particles, or may be in the form of secondary particles formed by aggregation of primary particles.
[0045] The inorganic particle-containing layer may cover a part of the surface of the niobium titanium oxide particle, or may cover the entire surface of the niobium titanium oxide particle. When the inorganic particle-containing layer does not cover the entire surface of the niobium titanium oxide particle, the surface of the niobium titanium oxide particle may include a part that is not covered by the inorganic particle-containing layer. When the surface of the niobium titanium oxide includes a part that is not covered by the inorganic particle-containing layer, at least a part of the part that is not covered by the inorganic particle-containing layer may be exposed on the surface of the electrode.
[0046] The thickness of the inorganic particle-containing layer can be in the range of 0.0005 μm or more and 0.7 μm or less. The thickness of the inorganic particle-containing layer is preferably in the range of 0.001 μm or more and 0.4 μm or less. When the thickness of the inorganic particle-containing layer is 0.001 μm or more, the durability against hydrofluoric acid can be increased. Specifically, since the amount of hydrofluoric acid that the inorganic particle-containing layer can capture increases, it is possible to suppress contact of hydrofluoric acid that exceeds the amount of hydrofluoric acid that the inorganic particle-containing layer can capture with the niobium titanium oxide particles. When the thickness of the inorganic particle-containing layer is 0.4 μm or less, it is possible to suppress an increase in resistance. The lower limit of the thickness of the inorganic particle-containing layer can be, for example, 0.0010 μm.
[0047] The thickness of the inorganic particle-containing layer is more preferably in the range of 0.01 μm to 0.35 μm, and even more preferably in the range of 0.05 μm to 0.3 μm.
[0048] The mass of the inorganic particle-containing layer is preferably in the range of 1% by mass to 20% by mass relative to the mass of the niobium titanium oxide particles. When it is 1% by mass or more, hydrogen fluoride can be prevented from coming into contact with the niobium titanium oxide particles. When it is 20% by mass or less, an increase in interface resistance can be prevented.
[0049] The particles containing an inorganic material preferably include at least one selected from the group consisting of particles containing a metal oxide containing at least one element selected from the group consisting of Al, Ti, Si, Zr, and Mg, and solid electrolyte-containing particles.
[0050] The inorganic particle-containing layer may contain only metal oxide-containing particles, may contain only solid electrolyte-containing particles, or may contain both metal oxide-containing particles and solid electrolyte-containing particles. The type of metal oxide-containing particles may be one or more types. The type of solid electrolyte-containing particles may be one or more types.
[0051] The particles containing a metal oxide may further include a solid electrolyte.The particles containing a solid electrolyte may further include a metal oxide.
[0052] Examples of metal oxides include Al2O3, TiO2, SiO2, ZrO2, and MgO. The type of metal oxide may be one or more.
[0053] A solid electrolyte is a solid substance that has Li-ion conductivity. Here, Li-ion conductivity is defined as a Li-ion conductivity of 1×10 -6 It means that the solid electrolyte has a lithium ion conductivity of 10 ...
[0054] As the oxide-based solid electrolyte, a lithium phosphate solid electrolyte having a NASICON (Sodium (Na) Super Ionic Conductor) type structure can be used. For example, lithium phosphate solid electrolyte represented by the general formula Li 1+x It is preferable to use a lithium phosphate solid electrolyte represented by Mα2(PO4)3. Mα in the above general formula is, for example, one or more selected from the group consisting of titanium (Ti), germanium (Ge), strontium (Sr), zirconium (Zr), tin (Sn), aluminum (Al), and calcium (Ca). The subscript x is in the range of 0 ≦ x ≦ 2.
[0055] As another example of the lithium phosphate solid electrolyte having a NASICON type structure, Li 1+x Al x Ti 2-x (PO4)3 represented LATP compound where 0.1 ≦ x ≦ 0.5; Li 1+x Al y Mβ 2-y (PO4)3 represented where Mβ is one or more selected from the group consisting of Ti, Ge, Sr, Zr, Sn, and Ca and 0 ≦ x ≦ 1 and 0 ≦ y ≦ 1; Li 1+x Al x Ge 2-x (PO4)3 represented compound where 0 ≦ x ≦ 2; and, Li 1+x Al x Zr 2-x (PO4)3 represented compound where 0 ≦ x ≦ 2; Li 1+x+y Al x Mγ 2-x Si y P 3-y O 12 represented compound where Mγ is one or more selected from the group consisting of Ti and Ge and 0 < x ≦ 2, 0 ≦ y < 3; Li 1+2x Zr 1-x Ca x (PO4)3 represented compound where 0 ≦ x < 1 can be mentioned.
[0056] In addition, as an example of the oxide-based solid electrolyte, in addition to the above lithium phosphate solid electrolyte, Li x PO y Nz and 2.6≦x≦3.5, 1.9≦y≦3.8, and 0.1≦z≦1.3. 2.9 PO 3.3 N 0.46 ); Garnet-type structure La 5+x A x La 3-x MδO 12 A is 1 or more selected from the group consisting of Ca, Sr, and Ba, Mδ is 1 or more selected from the group consisting of Nb and Ta, and 0≦x≦0.5; Li3Mδ 2-x L2O 12 wherein Mδ is at least one selected from the group consisting of Nb and Ta, and L may contain Zr, and 0≦x≦0.5; Li 7-3x Al x La3Zr3O 12 and 0≦x≦0.5; Li 5+x La3Mδ 2-x Zr x O 12 where Mδ is at least one selected from the group consisting of Nb and Ta, and 0≦x≦2. LLZ compounds (e.g., Li7La3Zr2O 12 ); and La 2 / 3-x Li x Examples of such compounds include those represented by TiO3, where x is 0.3≦x≦0.7.
[0057] One or more of the above compounds can be used as the solid electrolyte. Two or more of the above solid electrolytes can also be used.
[0058] The inorganic particle-containing layer preferably contains solid electrolyte-containing particles. The inorganic particle-containing layer containing the solid electrolyte-containing particles can have high ion conductivity. Therefore, the output performance can be improved.
[0059] When the electrode according to the embodiment includes, for example, the first particles as a negative electrode active material, examples of the other active materials include lithium titanate having a ramsdellite structure (e.g., Li 2+yTi3O7, 0≦y≦3), lithium titanates with spinel structure (e.g., Li 4+x Ti5O 12 , 0≦x≦3), titanium dioxide (TiO2), anatase type titanium dioxide, rutile type titanium dioxide, niobium pentoxide (Nb2O5), hollandite type titanium composite oxide, orthorhombic titanium composite oxide, and monoclinic type niobium titanium oxide. As the monoclinic type niobium titanium oxide, for example, the same ones as those described above can be used.
[0060] As an example of the above-mentioned orthorhombic titanium-containing composite oxide, Li 2+a M I 2-b Ti 6-c M II d O 14+σ In this case, the compound represented by M I is at least one selected from the group consisting of Sr, Ba, Ca, Mg, Na, Cs, Rb and K. II is at least one selected from the group consisting of Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni, and Al. The subscripts in the composition formula are 0≦a≦6, 0≦b<2, 0≦c<6, 0≦d<6, and -0.5≦σ≦0.5. Specific examples of orthorhombic titanium-containing composite oxides include Li 2+a Na2Ti6O 14 (0≦a≦6).
[0061] The average particle diameter of the inorganic particles can be in the range of 0.3 μm to 2.0 μm. The average particle diameter of the inorganic particles is preferably in the range of 0.4 μm to 1.0 μm. When the average particle diameter of the inorganic particles is 0.4 μm or more, the amount of hydrofluoric acid that can be captured per inorganic particle can be increased. Furthermore, in the manufacturing process of the electrode, the inorganic particles can be prevented from agglomerating with each other, so that the inorganic particles can be uniformly dispersed in the electrode. When the average particle diameter of the inorganic particles is 1.0 μm or less, the number of inorganic particles per mass can be increased. In addition, the inorganic particles can be uniformly distributed in the fine gaps in the electrode. Therefore, inorganic particles with an average particle diameter in the range of 0.4 μm to 1.0 μm can efficiently capture hydrofluoric acid.
[0062] The average particle size of the inorganic particles is more preferably in the range of 0.4 μm to 0.9 μm, and even more preferably in the range of 0.4 μm to 0.8 μm.
[0063] The inorganic particles may be primary particles, secondary particles formed by aggregation of primary particles, or a mixture of primary particles and secondary particles.
[0064] The inorganic particles preferably contain at least one selected from the group consisting of a metal oxide containing at least one element selected from the group consisting of Al, Ti, Si, Zr, and Mg, and a solid electrolyte. Of the above, the inorganic particles may contain only a metal oxide, may contain only a solid electrolyte, or may contain both a metal oxide and a solid electrolyte.
[0065] The metal oxide and solid electrolyte may be of the types described above.
[0066] The inorganic particles preferably contain a solid electrolyte. The inorganic particles containing a solid electrolyte can have high ionic conductivity, and therefore can improve the output performance of the electrode.
[0067] The inorganic particles and the inorganic particle-containing layer may be made of the same material or may contain different materials. It is preferred that the inorganic particles contain a solid electrolyte and the inorganic particle-containing layer contains solid electrolyte-containing particles.
[0068] The conductive agent is blended to improve the current collecting performance and to reduce the contact resistance between the active material and the current collector. Examples of the conductive agent include carbonaceous materials such as vapor grown carbon fiber (VGCF), carbon black such as acetylene black, graphite, carbon nanotubes, and carbon nanofibers. One of these may be used as the conductive agent, or two or more may be used in combination as the conductive agent. Alternatively, instead of using a conductive agent, a carbon coating or an electronically conductive inorganic material coating may be applied to the surface of the active material particles.
[0069] The binder is blended to fill the gaps between the dispersed active materials and to bind the active materials and the current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene-butadiene rubber (SBR), polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.
[0070] The mixing ratio of the active material, inorganic particles, conductive agent and binder in the active material-containing layer can be appropriately changed depending on the application of the electrode. For example, when the electrode is used as a negative electrode of a secondary battery, it is preferable to mix the active material (negative electrode active material), inorganic particles, conductive agent and binder at a ratio of 68% by mass or more and 96% by mass or less, 1% by mass or more and 10% by mass or less, 2% by mass or more and 30% by mass or less, and 2% by mass or more and 30% by mass or less, respectively. By making the amount of inorganic particles 1% by mass or more, the hydrofluoric acid trapping effect can be ensured. By making the amount of conductive agent 2% by mass or more, the current collecting performance of the active material-containing layer can be improved. In addition, by making the amount of binder 2% by mass or more, the binding property between the active material-containing layer and the current collector becomes sufficient, and excellent cycle performance can be expected. On the other hand, it is preferable to make the amount of inorganic particles 10% by mass or less in terms of ensuring electronic conductivity. It is preferable to make the amount of conductive agent and binder 30% by mass or less each in terms of achieving high capacity.
[0071] The proportion of the first particles in the active material is preferably 80% by mass or more, and can be 100% by mass.
[0072] The current collector is made of a material that is electrochemically stable at the potential at which lithium (Li) is inserted and removed from the active material. For example, when the active material is used as a negative electrode active material, the current collector is preferably made of copper, nickel, stainless steel, or aluminum, or an aluminum alloy containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si. The thickness of the current collector is preferably 5 μm or more and 20 μm or less. A current collector having such a thickness can balance the strength and weight of the electrode.
[0073] The current collector may also include a portion on the surface of which no active material-containing layer is formed, and this portion can function as a current collecting tab.
[0074] <How to make electrodes> The electrodes can be prepared, for example, by the following method.
[0075] First, a first particle containing niobium titanium oxide particles and an inorganic particle-containing layer is prepared. Then, an active material containing the first particle, inorganic particles, a conductive agent, and a binder are suspended in a solvent to prepare a slurry. For example, water or N-methylpyrrolidone (NMP) can be used as the solvent for the slurry. This slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate of the active material-containing layer and the current collector. Then, the laminate is pressed. In this manner, an electrode is prepared.
[0076] During suspension in the preparation of the slurry, stirring may be performed using a bead mill. When forming exposed portions in the production of the first particles described below, the stirring conditions for suspension are preferably glass bead diameter of about 2 mm, packing rate of about 50%, stirring speed of about 3000 rpm, and stirring time of about 1 hour. By using the above conditions, the stirring intensity is not too strong, so that the thickness of the inorganic particle-containing layer can be prevented from becoming too thin due to excessive scraping of the first particles.
[0077] Alternatively, the electrode may be prepared by the following method. First, the active material including the first particles, inorganic particles, a conductive agent, and a binder are mixed to obtain a mixture. Then, the mixture is formed into pellets. Then, the pellets are placed on a current collector to obtain an electrode.
[0078] (Method of producing first particles) The first particles can be produced, for example, as follows.
[0079] First, an inorganic particle-containing layer precursor is dissolved or dispersed in a solvent to prepare an inorganic particle-containing layer precursor solution.
[0080] As the solvent, for example, water can be used. Nitric acid and polyvinyl alcohol (PVA) may be further added to the solvent. By adding nitric acid, the metal elements contained in the inorganic particle-containing layer precursor can be easily dissolved in the solvent. By adding PVA, dispersibility can be maintained. The concentrations of nitric acid and PVA can be within the ranges of 0.01% by mass to 0.05% by mass and 0.1% by mass to 20% by mass, respectively.
[0081] As the inorganic particle-containing layer precursor, a material containing an element contained in the desired inorganic particle-containing layer can be used. For example, an alkoxide or nitrate containing a metal element contained in the desired inorganic particle-containing layer can be used. In addition, when the desired inorganic particle-containing layer contains phosphorus (P) in its composition, for example, ammonium dihydrogen phosphate can be used as the phosphorus (P) source. These materials are mixed in a molar ratio that results in the composition of the desired inorganic particle-containing layer, and dissolved or dispersed in a solvent to obtain an inorganic particle-containing layer precursor solution.
[0082] Niobium titanium oxide particles are added to an inorganic particle-containing layer precursor solution and stirred to prepare a dispersion liquid. The solvent is removed from the stirred dispersion liquid to obtain a dry powder. The dry powder is fired to produce first particles having an inorganic particle-containing layer formed on the surface of the niobium titanium oxide particles.
[0083] The mixing ratio of the inorganic particle-containing layer precursor solution and the niobium titanium oxide particles can be, for example, such that the mass of the inorganic particle-containing layer obtained after firing is 1% by mass or more and 20% by mass or less relative to the mass of the niobium titanium oxide particles. When it is 1% by mass or more, the inorganic particle-containing layer can be easily formed after firing. When it is 20% by mass or less, the formation of an excessive inorganic particle-containing layer can be suppressed.
[0084] The firing conditions are not particularly limited, but the firing temperature is preferably 600° C. or more and 1000° C. or less. The firing time is preferably 5 hours or more and 10 hours or less. The firing time can be changed depending on the firing temperature.
[0085] (Formation of exposed area) The exposed portion may be formed on the first particles obtained as described above. The exposed portion can be formed, for example, by subjecting the first particles to a bead mill. As the bead mill, for example, a wet bead mill can be used.
[0086] The bead mill for forming the exposed portion can be performed under the following conditions, for example. The diameter of the glass beads used in the bead mill is preferably within a range of 2 mm to 10 mm. When the diameter of the glass beads is 2 mm or more, the crushing force can be ensured. When the diameter of the glass beads is 10 mm or less, the crushing efficiency can be increased. The filling rate of the glass beads in the bead mill is preferably within a range of 50% to 80%. When the filling rate of the glass beads is 50% or more, the crushing efficiency can be increased. When the filling rate of the glass beads is 80% or less, the movement efficiency of the beads is high, and as a result, the crushing efficiency can be increased. The bead mill is preferably performed at 1000 rpm to 3000 rpm. When it is 1000 rpm or more, the crushing efficiency can be increased. When it is 3000 rpm or less, the first particles can be prevented from being excessively crushed. The stirring time is preferably 30 minutes to 60 minutes. When it is 30 minutes or more, the exposed portion can be easily formed. When it is 60 minutes or less, the first particles can be prevented from being excessively crushed.
[0087] The primary particles on which the exposed portions have been formed in advance can be used for preparing the above-mentioned slurry, or the exposed portions can be formed simultaneously with the preparation of the slurry as described below.
[0088] First, the first particles not having an exposed portion formed thereon and inorganic particles are added to a solvent, and a first bead mill is performed. The first bead mill conditions are set to the above-mentioned conditions for forming the exposed portion, thereby forming the exposed portion on the first particles. Next, a conductive agent and CMC as a binder are added, and a second bead mill is performed. The second bead mill conditions are set to the stirring conditions for suspension described above. Finally, a binder other than CMC is further added and stirred to prepare a slurry. Alternatively, the slurry can be prepared by adding an active material including the first particles not having an exposed portion formed thereon, inorganic particles, a conductive agent, and a binder to a solvent, and performing a bead mill under conditions for forming the exposed portion. In this manner, a slurry containing primary particles including an exposed portion can be prepared.
[0089] <Various measurement methods for active materials> Next, a method for measuring the composition and structure of the active material will be described.
[0090] When measuring the active material contained in an electrode incorporated in a battery, the electrode is removed from the battery as described below, and then the active material is removed from the electrode and subjected to the measurement.
[0091] (Extraction of electrodes) First, the lithium ions are completely released from the niobium titanium oxide contained in the electrode. For example, when measuring the negative electrode, the battery is completely discharged. However, even in a completely discharged battery, a small amount of lithium ions may remain in the niobium titanium oxide particles in the negative electrode.
[0092] Next, the battery is disassembled in a glove box filled with argon, and the electrodes containing the active material to be measured are taken out. The electrodes are then washed with an appropriate solvent. If the battery is a non-aqueous electrolyte battery, it is preferable to use an organic solvent contained in the non-aqueous electrolyte, such as ethyl methyl carbonate.
[0093] (Removal of active material) The removed electrode is appropriately cut, immersed in a solvent, and ultrasonicated. As the solvent, an organic solvent such as alcohol or NMP is preferably used. This allows the active material-containing layer to be peeled off from the current collector foil. Next, the peeled active material-containing layer is dispersed in a solvent to obtain a dispersion liquid, which is then subjected to centrifugation. This allows the active material to be separated from the powder of the active material-containing layer containing a conductive agent such as carbon.
[0094] (Identification of the first particle) The presence of particles containing niobium titanium oxide in the separated active material can be identified by inductively coupled plasma (ICP) emission spectroscopy. Specifically, ICP analysis can be performed as follows. The active material separated by the above-mentioned method is dissolved in acid to prepare a measurement sample. The prepared measurement sample is analyzed by ICP emission spectroscopy to measure the concentration of each element per unit weight in the measurement sample. An example of an ICP analysis device is SPS-3520UV manufactured by SII Nano Technology Co., Ltd. or a device having equivalent functions. From the measurement results, the composition ratio of the metal elements contained in the active material can be calculated. From this composition ratio, it can be identified that the active material contains particles containing niobium titanium oxide.
[0095] The fact that the particles containing niobium titanium oxide further contain an inorganic particle-containing layer can be identified as follows: The active material separated by the above-mentioned method is observed with a transmission electron microscope (TEM) and element mapping is performed by energy dispersive X-ray spectroscopy (EDX) measurement, whereby the particles containing niobium titanium oxide that further contain an inorganic particle-containing layer can be identified.
[0096] Among the particles containing niobium titanium oxide, the particles further containing an inorganic particle-containing layer can be identified as the first particles.
[0097] (Distinguishing between niobium titanium oxide particles and inorganic particle-containing layer) The niobium titanium oxide particles and the inorganic particle-containing layer can be distinguished by observing the first particles in the active material with a transmission electron microscope (TEM).
[0098] For TEM observation, it is preferable to use a high-angle annular dark field scanning transmission electron microscope (HAADF-STEM) image. HAADF-STEM is a method of detecting and observing transmitted electrons scattered at high angles, and can obtain a contrast proportional to the atomic weight. In the first particle, the niobium titanium oxide particles containing the niobium titanium composite oxide may contain more Nb elements than the inorganic particle-containing layer. Therefore, in the HAADF-STEM image of the first particle, the niobium titanium oxide particles can be observed as dark compared to the inorganic particle-containing layer. This allows the inorganic particle-containing layer and the niobium titanium oxide particles to be clearly distinguished from each other based on the difference in contrast.
[0099] (Method of measuring the thickness of an inorganic particle-containing layer) A method for measuring the thickness of the inorganic particle-containing layer will be described with reference to Fig. 4. Fig. 4 is a diagram that illustrates a schematic HAADF-STEM image of the first particle.
[0100] First, an arbitrary first particle 10 is selected from the TEM observation image. Next, HAADF-STEM observation is performed on the selected first particle 10. In the obtained HAADF-STEM image, the niobium titanium oxide particle 11 and the inorganic particle-containing layer 12 can be distinguished from each other based on the contrast.
[0101] In the HAADF-STEM image of the first particle 10, a point on the surface of the niobium titanium oxide particle 11 is set as point R. Point R may be located at the innermost part of the inorganic particle-containing layer 12. Next, a tangent r is drawn to point R on the niobium titanium oxide particle 11. A line s perpendicular to the tangent r to point R is drawn. The point where the line s intersects with the outermost part of the first particle 10 is set as point S. Point S may be located at the outermost part of the inorganic particle-containing layer 12. The same operation is performed on the same first particle 10, and the longest distance RS on the first particle 10 is defined as the thickness of the inorganic particle-containing layer 12 of the first particle. The same operation is performed on 10 first particles, and the average value is defined as the thickness of the inorganic particle-containing layer 12.
[0102] On the surface of the niobium titanium oxide particle 11, a portion where the inorganic particle-containing layer 12 is not formed can be an exposed portion .
[0103] (FE-TEM) Whether the first particles include the exposed portion can be determined by observing the first particles with a field-emission transmission electron microscope (FE-TEM).
[0104] The surface of the first particle is observed by FE-TEM at a high magnification of about 1 million times. In the first particle, a portion on the surface of the niobium titanium oxide particle where no compound of other composition is present can be defined as an exposed portion.
[0105] <Measurement of the average particle size of inorganic particles> The average particle size of the inorganic particles can be measured by TEM observation of a cross section of the electrode.
[0106] When measuring an electrode incorporated in a battery, the electrode is removed from the battery and subjected to measurement in the same manner as described above.
[0107] The cross section of the electrode is observed by TEM at a magnification of 1500 times. Among the particles in the observation field, the particles containing the elements contained in the solid electrolyte described above can be identified as solid electrolyte-containing particles. For example, when the particles contain Al, Ti, and P, the particles can be identified as containing the LATP compound, which is a lithium phosphate solid electrolyte. In addition, among the particles in the observation field, the particles containing the elements contained in the metal oxide described above can be identified as metal oxide-containing particles. For example, the particles containing Al can be identified as Al2O3-containing particles, the particles containing Si can be identified as SiO2-containing particles, the particles containing Ti can be identified as TiO2-containing particles, the particles containing Zr can be identified as ZrO2-containing particles, and the particles containing Mg can be identified as MgO-containing particles. Furthermore, by identifying that the particles do not contain any metal elements other than the metal elements contained in the metal oxide described above by TEM-EDX measurement, the type of metal oxide contained in the particles to be measured can be identified. For example, if the particles to be measured do not contain any metal elements other than Ti, the particles can be identified as containing TiO2. The above solid electrolyte-containing particles and particles containing metal oxides can be identified as inorganic particles. The particle sizes of five inorganic particles within the observation field are measured, and the average value is regarded as the average particle size.
[0108] The electrode according to the first embodiment includes inorganic particles, niobium titanium oxide particles, and an inorganic particle-containing layer that covers at least a part of the surface of the niobium titanium oxide particles. The average particle diameter of the inorganic particles is larger than the thickness of the inorganic particle-containing layer. Therefore, the electrode can improve cycle performance and output performance.
[0109] Second Embodiment According to the second embodiment, a secondary battery including a negative electrode, a positive electrode, and an electrolyte is provided. At least one of the positive electrode and the negative electrode is the electrode according to the first embodiment. That is, the secondary battery includes the electrode according to the first embodiment.
[0110] The secondary battery may further include a separator disposed between the positive electrode and the negative electrode. The negative electrode, the positive electrode, and the separator may constitute an electrode group. The electrolyte may be held in the electrode group.
[0111] Moreover, such a secondary battery can further include an exterior member that houses the electrode group and the electrolyte.
[0112] Furthermore, such a secondary battery may further include a negative electrode terminal electrically connected to the negative electrode and a positive electrode terminal electrically connected to the positive electrode.
[0113] Such a secondary battery may be, for example, a lithium secondary battery. The secondary battery also includes a non-aqueous electrolyte secondary battery that contains a non-aqueous electrolyte.
[0114] The negative electrode, the positive electrode, the electrolyte, the separator, the exterior member, the negative electrode terminal, and the positive electrode terminal will be described in detail below.
[0115] 1) Negative electrode The negative electrode may include a negative electrode current collector and a negative electrode active material-containing layer. The negative electrode current collector and the negative electrode active material-containing layer may be the current collector and the active material-containing layer that the electrode according to the first embodiment may include, respectively. The negative electrode active material-containing layer may include, as a negative electrode active material, first particles that include niobium titanium oxide particles and an inorganic particle-containing layer.
[0116] Among the details of the negative electrode, those parts that overlap with the details explained in the first embodiment will be omitted.
[0117] The density of the negative electrode active material-containing layer (excluding the current collector) is 1.8 g / cm 3 More than 2.8g / cm 3 A negative electrode having a density of the negative electrode active material-containing layer within this range is excellent in energy density and electrolyte retention. The density of the negative electrode active material-containing layer is preferably 2.1 g / cm or less. 3 More than 2.6g / cm 3 It is more preferable that:
[0118] The negative electrode can be produced, for example, by the same method as that for the electrode according to the first embodiment.
[0119] 2) Positive electrode The positive electrode can include a positive electrode current collector and a positive electrode active material-containing layer. The positive electrode active material-containing layer can be formed on one or both sides of the positive electrode current collector. The positive electrode active material-containing layer can include a positive electrode active material, and optionally a conductive agent and a binder.
[0120] As the positive electrode active material, for example, an oxide or a sulfide can be used. The positive electrode may contain one type of compound alone as the positive electrode active material, or may contain a combination of two or more types of compounds. Examples of the oxide and the sulfide can include compounds into which Li or Li ions can be inserted and desorbed.
[0121] Examples of such compounds include, for example, manganese dioxide (MnO2), iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide (e.g., Li x Mn2O4 or Li x MnO2; 0 < x ≦ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≦ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≦ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≦ 1, 0 < y < 1), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≦ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≦ 1, 0 < y < 2), lithium phosphate having an olivine structure (e.g., Li x FePO4; 0 < x ≦ 1, Li x Fe 1-y Mn y PO4; 0 < x ≦ 1, 0 < y ≦ 1, Li x CoPO4; 0 < x ≦ 1), iron sulfate (Fe2(SO4)3), vanadium oxide (e.g., V2O5), and lithium nickel cobalt manganese composite oxide (Li x Ni1-y-z Co y Mn z O2; where 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, and y + z < 1 is included.
[0122] Among the above, examples of more preferable compounds as the positive electrode active material include lithium manganese composite oxides having a spinel structure (e.g., Li x Mn2O4; 0 < x ≤ 1), lithium nickel composite oxides (e.g., Li x NiO2; 0 < x ≤ 1), lithium cobalt composite oxides (e.g., Li x CoO2; 0 < x ≤ 1), lithium nickel cobalt composite oxides (e.g., Li x Ni 1-y Co y O2; 0 < x ≤ 1, 0 < y < 1), lithium manganese nickel composite oxides having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≤ 1, 0 < y < 2), lithium manganese cobalt composite oxides (e.g., Li x Mn y Co 1-y O2; 0 < x ≤ 1, 0 < y < 1), lithium iron phosphate (e.g., Li x FePO4; 0 < x ≤ 1), and lithium nickel cobalt manganese composite oxides (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, and y + z < 1) are included. When these compounds are used as the positive electrode active material, the positive electrode potential can be increased.
[0123] When a room temperature molten salt is used as the electrolyte of the battery, it is preferable to use a positive electrode active material containing lithium iron phosphate, Li x VPO4F (0 ≤ x ≤ 1), a lithium manganese composite oxide, a lithium nickel composite oxide, a lithium nickel cobalt composite oxide, or a mixture thereof. Since these compounds have low reactivity with the room temperature molten salt, the cycle life can be improved. Details of the room temperature molten salt will be described later.
[0124] The primary particle size of the positive electrode active material is preferably 100 nm or more and 1 μm or less. A positive electrode active material with a primary particle size of 100 nm or more is easy to handle in industrial production. A positive electrode active material with a primary particle size of 1 μm or less allows lithium ions to diffuse smoothly within the solid.
[0125] The specific surface area of the positive electrode active material is 0.1 m 2 / g or more 10m 2 / g or less. 2 A positive electrode active material having a specific surface area of 10m / g or more can secure sufficient sites for absorbing and releasing Li ions. 2 A positive electrode active material having a specific surface area of 100 / g or less is easy to handle in industrial production and can ensure good charge-discharge cycle performance.
[0126] The binder is blended to fill the gaps between the dispersed positive electrode active material and to bind the positive electrode active material and the positive electrode current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.
[0127] The conductive agent is blended to improve current collection performance and reduce contact resistance between the positive electrode active material and the positive electrode current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, and carbonaceous materials such as graphite. One of these may be used as the conductive agent, or two or more may be combined and used as the conductive agent. The conductive agent may also be omitted.
[0128] In the positive electrode active material-containing layer, the positive electrode active material and the binder are preferably mixed in an amount of 80% by mass to 98% by mass and 2% by mass to 20% by mass, respectively.
[0129] By making the amount of binder 2% by mass or more, sufficient electrode strength can be obtained. In addition, the binder can function as an insulator. Therefore, by making the amount of binder 20% by mass or less, the amount of insulator contained in the electrode is reduced, and the internal resistance can be reduced.
[0130] When a conductive agent is added, the positive electrode active material, the binder, and the conductive agent are preferably mixed in proportions of 77% by mass or more and 95% by mass or less, 2% by mass or more and 20% by mass or less, and 3% by mass or more and 15% by mass or less, respectively.
[0131] By making the amount of the conductive agent 3% by mass or more, the above-mentioned effects can be achieved. Also, by making the amount of the conductive agent 15% by mass or less, the ratio of the conductive agent in contact with the electrolyte can be reduced. If this ratio is low, decomposition of the electrolyte during high-temperature storage can be reduced.
[0132] The positive electrode current collector is preferably an aluminum foil or an aluminum alloy foil containing one or more elements selected from Mg, Ti, Zn, Ni, Cr, Mn, Fe, Cu, and Si.
[0133] The thickness of the aluminum foil or aluminum alloy foil is preferably 5 μm or more and 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99 mass% or more. The content of transition metals such as iron, copper, nickel, and chromium contained in the aluminum foil or aluminum alloy foil is preferably 1 mass% or less.
[0134] The positive electrode current collector may also include a portion on the surface of which the positive electrode active material-containing layer is not formed, and this portion can function as a positive electrode current collecting tab.
[0135] The positive electrode can be produced, for example, by the following method. First, a positive electrode active material, a conductive agent, and a binder are suspended in a solvent to prepare a slurry. This slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate of an active material-containing layer and a current collector. Then, the laminate is pressed. In this manner, an electrode is produced.
[0136] Alternatively, the electrode may be prepared by the following method. First, the active material including the first particles, inorganic particles, a conductive agent, and a binder are mixed to obtain a mixture. Then, the mixture is formed into pellets. Then, the pellets are placed on a current collector to obtain an electrode.
[0137] The positive electrode can be prepared, for example, by the same method as the electrode according to the first embodiment. When the positive electrode is the electrode according to the first embodiment, the niobium titanium oxide contained in the first particle can function as a positive electrode active material. The negative electrode to be combined with the positive electrode does not have to be the electrode according to the first embodiment. For example, it can be combined with the inorganic particle-containing layer or the negative electrode that does not contain inorganic particles described in the first embodiment.
[0138] 3) Electrolytes As the electrolyte, for example, a non-aqueous electrolyte can be used. As the non-aqueous electrolyte, for example, a liquid non-aqueous electrolyte, a gel non-aqueous electrolyte, or a polymer solid electrolyte can be used. The liquid non-aqueous electrolyte is prepared by dissolving an electrolyte salt as a solute in an organic solvent. The gel non-aqueous electrolyte is prepared by compounding a liquid non-aqueous electrolyte with a polymer material. The polymer solid electrolyte is prepared by dissolving an electrolyte salt in a polymer material and solidifying it. The type of non-aqueous electrolyte can be one or more types.
[0139] The concentration of the electrolyte salt is preferably 0.5 mol / L or more and 2.5 mol / L or less.
[0140] The non-aqueous electrolyte may contain fluorine atoms. Examples of the non-aqueous electrolyte containing fluorine atoms include non-aqueous electrolytes containing an electrolyte salt containing fluorine atoms.
[0141] Examples of electrolyte salts that may be included in the non-aqueous electrolyte include lithium salts such as lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), and lithium bistrifluoromethylsulfonylimide (LiN(CF3SO2)2), and mixtures thereof. The electrolyte salt is preferably one that is difficult to oxidize even at high potential, and LiPF6 is the most preferable. Among the above, examples of electrolyte salts containing fluorine atoms include lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), and lithium bistrifluoromethylsulfonylimide (LiN(CF3SO2)2). The type of electrolyte salt may be one or more types.
[0142] Examples of organic solvents include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyl tetrahydrofuran (2MeTHF), and dioxolane (DOX); chain ethers such as dimethoxyethane (DME) and diethoxyethane (DEE); γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These organic solvents can be used alone or as a mixed solvent.
[0143] Examples of polymer materials contained in the gel-like non-aqueous electrolyte include polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyethylene oxide (PEO), or a mixture thereof.
[0144] Alternatively, the non-aqueous electrolyte may be a room temperature molten salt (ionic melt) containing lithium ions or an inorganic solid electrolyte, in addition to a liquid non-aqueous electrolyte, a gel non-aqueous electrolyte, or a polymer solid electrolyte. The non-aqueous electrolyte may contain one of the above alone, or may contain two or more of them. Among the above non-aqueous electrolytes, the room temperature molten salt or the inorganic solid electrolyte may be mixed with the liquid non-aqueous electrolyte, the gel non-aqueous electrolyte, or the polymer solid electrolyte.
[0145] Room temperature molten salts (ionic melts) refer to organic salts consisting of a combination of organic cations and anions that can exist as a liquid at room temperature (15°C or higher and 25°C or lower). Room temperature molten salts include room temperature molten salts that exist as a liquid by themselves, room temperature molten salts that become liquid when mixed with an electrolyte salt, room temperature molten salts that become liquid when dissolved in an organic solvent, and mixtures of these. In general, the melting point of room temperature molten salts used in secondary batteries is 25°C or lower. In addition, organic cations generally have a quaternary ammonium skeleton.
[0146] The inorganic solid electrolyte is a solid substance that has Li-ion conductivity. Here, Li-ion conductivity is defined as a Li-ion conductivity of 1×10 -6 It means that the inorganic solid electrolyte has a lithium ion conductivity of 10 ...
[0147] The oxide-based solid electrolyte has a NASICON (Sodium (Na) Super Ionic Conductor) type structure and is represented by the general formula Li 1+x It is preferable to use a lithium phosphate solid electrolyte represented by Mα2(PO4)3. In the above general formula, Mα is, for example, one or more selected from the group consisting of titanium (Ti), germanium (Ge), strontium (Sr), zirconium (Zr), tin (Sn), aluminum (Al), and calcium (Ca). The subscript x is within the range of 0≦x≦2.
[0148] A specific example of a lithium phosphate solid electrolyte having a NASICON structure is Li 1+x Al x Ti 2-x LATP compound represented by (PO4)3, where 0.1≦x≦0.5; Li 1+x Al y Mβ 2-y A compound represented by the formula (PO4)3, in which Mβ is one or more selected from the group consisting of Ti, Ge, Sr, Zr, Sn, and Ca, and 0≦x≦1 and 0≦y≦1; Li 1+x Alx Ge 2-x (PO4)3 represented compound where 0 ≦ x ≦ 2; and, Li 1+x Al x Zr 2-x (PO4)3 represented compound where 0 ≦ x ≦ 2; Li 1+x+y Al x Mγ 2-x Si y P 3-y O 12 represented compound where Mγ is one or more selected from the group consisting of Ti and Ge, 0 < x ≦ 2, 0 ≦ y < 3; Li 1+2x Zr 1-x Ca x compounds represented by (PO4)3 where 0 ≦ x < 1 can be mentioned.
[0149] Also, as the oxide solid electrolyte, in addition to the above lithium phosphate solid electrolyte, Li x PO y N z represented amorphous LIPON compound where 2.6 ≦ x ≦ 3.5, 1.9 ≦ y ≦ 3.8, and 0.1 ≦ z ≦ 1.3 (for example, Li 2.9 PO 3.3 N 0.46 ); Garnet-type structure La 5+x A x La 3-x Mδ2O 12 represented compound where A is one or more selected from the group consisting of Ca, Sr, and Ba, Mδ is one or more selected from the group consisting of Nb and Ta, and 0 ≦ x ≦ 0.5; Li3Mδ 2-x L2O 12 represented compound where Mδ is one or more selected from the group consisting of Nb and Ta, L may contain Zr, and 0 ≦ x ≦ 0.5; Li 7-3x Al x La3Zr3O 12 represented compound where 0 ≦ x ≦ 0.5; Li 5+x La3Mδ 2-x Zr x O 12 represented compound where Mδ is one or more selected from the group consisting of Nb and Ta, and 0 ≦ x ≦ 2, LLZ compound (for example, Li7La3Zr2O 12); and La 2 / 3-x Li x Examples of such compounds include those represented by TiO3, where x is 0.3≦x≦0.7.
[0150] One or more of the above compounds can be used as the solid electrolyte. Two or more of the above solid electrolytes can also be used.
[0151] 4) Separator The separator is formed, for example, from a porous film containing polyethylene (PE), polypropylene (PP), cellulose, or polyvinylidene fluoride (PVdF), or a synthetic resin nonwoven fabric. From the viewpoint of safety, it is preferable to use a porous film formed from polyethylene or polypropylene. This is because these porous films melt at a certain temperature and are capable of cutting off electric current.
[0152] 5) Exterior materials As the exterior member, for example, a container made of a laminate film or a metal container can be used.
[0153] The thickness of the laminate film is, for example, 0.5 mm or less, preferably 0.2 mm or less.
[0154] The laminate film is a multi-layer film including a plurality of resin layers and a metal layer interposed between the resin layers. The resin layers include polymeric materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably made of aluminum foil or aluminum alloy foil for weight reduction. The laminate film can be molded into the shape of the exterior member by sealing it by heat fusion.
[0155] The thickness of the wall of the metal container is, for example, 1 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less.
[0156] The metal container is made of, for example, aluminum or an aluminum alloy. The aluminum alloy preferably contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains transition metals such as iron, copper, nickel, and chromium, the content of the transition metals is preferably 100 ppm by mass or less.
[0157] The shape of the exterior member is not particularly limited. The shape of the exterior member may be, for example, flat (thin), rectangular, cylindrical, coin, or button. The exterior member can be appropriately selected depending on the battery dimensions and the application of the battery.
[0158] 6) Negative terminal The negative electrode terminal has a potential range of 1V to 3V with respect to the redox potential of lithium (vs. Li / Li + ) and can be formed from a material that is electrically stable and conductive. Specifically, the material of the negative electrode terminal can be copper, nickel, stainless steel, aluminum, or an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The material of the negative electrode terminal is preferably aluminum or an aluminum alloy. The negative electrode terminal is preferably made of the same material as the negative electrode current collector in order to reduce the contact resistance with the negative electrode current collector.
[0159] 7) Positive terminal The positive electrode terminal has a potential range of 3V to 4.5V with respect to the redox potential of lithium (vs. Li / Li +) and can be formed from a material that is electrically stable and conductive. Examples of the material for the positive electrode terminal include aluminum and an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The positive electrode terminal is preferably formed from the same material as the positive electrode current collector in order to reduce the contact resistance with the positive electrode current collector.
[0160] Next, the secondary battery according to the embodiment will be described more specifically with reference to the drawings.
[0161] Fig. 5 is a cross-sectional view showing an example of a secondary battery, and Fig. 6 is an enlarged cross-sectional view of part A of the secondary battery shown in Fig. 5.
[0162] The secondary battery 100 shown in Figures 5 and 6 includes a bag-shaped exterior member 2 shown in Figure 5, an electrode group 1 shown in Figures 5 and 6, and an electrolyte (not shown). The electrode group 1 and the electrolyte are stored in the bag-shaped exterior member 2. The electrolyte (not shown) is held in the electrode group 1.
[0163] The bag-shaped exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0164] As shown in Fig. 5, the electrode group 1 is a flat wound-type electrode group. As shown in Fig. 6, the flat wound-type electrode group 1 includes a negative electrode 3, a separator 4, and a positive electrode 5. The separator 4 is interposed between the negative electrode 3 and the positive electrode 5.
[0165] The negative electrode 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b. In the negative electrode 3, in a portion located at the outermost shell of the wound-type electrode group 1, the negative electrode active material-containing layer 3b is formed only on the inner surface side of the negative electrode current collector 3a as shown in Fig. 6. In the other portions of the negative electrode 3, the negative electrode active material-containing layer 3b is formed on both sides of the negative electrode current collector 3a.
[0166] The positive electrode 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b formed on both sides of the positive electrode current collector 5a.
[0167] As shown in FIG. 5, the negative electrode terminal 6 and the positive electrode terminal 7 are located near the outer peripheral end of the wound electrode group 1. The negative electrode terminal 6 is connected to a portion located at the outermost shell of the negative electrode current collector 3a. The positive electrode terminal 7 is connected to a portion located at the outermost shell of the positive electrode current collector 5a. The negative electrode terminal 6 and the positive electrode terminal 7 extend to the outside from an opening of the bag-shaped exterior member 2. A thermoplastic resin layer is provided on the inner surface of the bag-shaped exterior member 2, and the opening is closed by heat sealing.
[0168] The secondary battery according to the embodiment is not limited to the secondary battery having the configuration shown in FIGS. 5 and 6, but may be a battery having the configuration shown in FIGS.
[0169] Fig. 7 is a partially cutaway perspective view showing a schematic diagram of another example of the secondary battery, and Fig. 8 is an enlarged cross-sectional view of part B of the secondary battery shown in Fig. 7.
[0170] The secondary battery 100 shown in Figures 7 and 8 includes an electrode group 1 shown in Figures 7 and 8, an exterior member 2 shown in Figure 7, and an electrolyte (not shown). The electrode group 1 and the electrolyte are housed in the exterior member 2. The electrolyte is held in the electrode group 1.
[0171] The exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0172] The electrode group 1 is a laminated type electrode group, as shown in Fig. 8. The laminated type electrode group 1 has a structure in which negative electrodes 3 and positive electrodes 5 are alternately laminated with separators 4 interposed therebetween.
[0173] The electrode group 1 includes a plurality of negative electrodes 3. Each of the plurality of negative electrodes 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b supported on both sides of the negative electrode current collector 3a. The electrode group 1 also includes a plurality of positive electrodes 5. Each of the plurality of positive electrodes 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b supported on both sides of the positive electrode current collector 5a.
[0174] The negative electrode current collector 3a of each negative electrode 3 includes a portion on one side where the negative electrode active material-containing layer 3b is not supported on any surface. This portion serves as a negative electrode current collector tab 3c. As shown in FIG. 8, the negative electrode current collector tab 3c does not overlap with the positive electrode 5. The negative electrode current collector tabs 3c are electrically connected to a belt-shaped negative electrode terminal 6. The tip of the belt-shaped negative electrode terminal 6 is pulled out to the outside of the exterior member 2.
[0175] Although not shown, the positive electrode current collector 5a of each positive electrode 5 includes a portion on one side where the positive electrode active material-containing layer 5b is not supported on any surface. This portion serves as a positive electrode current collector tab. Just as the negative electrode current collector tab 3c does not overlap with the positive electrode 5, the positive electrode current collector tab does not overlap with the negative electrode 3. The positive electrode current collector tab is located on the opposite side of the electrode group 1 to the negative electrode current collector tab 3c. The positive electrode current collector tab is electrically connected to a strip-shaped positive electrode terminal 7. The tip of the strip-shaped positive electrode terminal 7 is located on the opposite side to the negative electrode terminal 6 and is drawn out to the outside of the exterior member 2.
[0176] The secondary battery according to the second embodiment includes the electrode according to the first embodiment, and therefore, according to this embodiment, it is possible to provide a secondary battery with improved cycle performance and output performance.
[0177] (Third embodiment) According to a third embodiment, there is provided a battery pack including a plurality of secondary batteries according to the second embodiment.
[0178] In such a battery pack, the individual cells may be electrically connected in series or parallel, or may be arranged in a combination of series and parallel connections.
[0179] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.
[0180] Fig. 9 is a perspective view showing an example of a battery pack. The battery pack 200 shown in Fig. 9 includes five cells 100a to 100e, four bus bars 21, a positive electrode lead 22, and a negative electrode lead 23. Each of the five cells 100a to 100e is a secondary battery according to the second embodiment.
[0181] The bus bar 21 connects, for example, the negative electrode terminal 6 of one cell 100a and the positive electrode terminal 7 of the adjacent cell 100b. In this way, the five cells 100 are connected in series by the four bus bars 21. That is, the battery pack 200 in FIG. 9 is a five-series battery pack. Although no example is shown, in a battery pack including a plurality of cells electrically connected in parallel, for example, the plurality of negative electrode terminals are connected to each other by a bus bar and the plurality of positive electrode terminals are connected to each other by a bus bar, thereby electrically connecting the plurality of cells.
[0182] The positive electrode terminal 7 of at least one of the five cells 100a to 100e is electrically connected to a positive electrode lead 22 for external connection. Also, the negative electrode terminal 6 of at least one of the five cells 100a to 100e is electrically connected to a negative electrode lead 23 for external connection.
[0183] The battery pack according to the third embodiment includes the secondary battery according to the second embodiment, and therefore can achieve excellent cycle performance and output performance.
[0184] (Fourth embodiment) According to a fourth embodiment, there is provided a battery pack. The battery pack includes the battery assembly according to the third embodiment. The battery pack may include a single secondary battery according to the second embodiment, instead of the battery assembly according to the third embodiment.
[0185] Such a battery pack may further include a protection circuit. The protection circuit has a function of controlling charging and discharging of the secondary battery. Alternatively, a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source may be used as the protection circuit for the battery pack.
[0186] The battery pack may further include an external terminal for current flow. The external terminal for current flow is for outputting current from the secondary battery to the outside and / or inputting current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, current is supplied to the outside through the external terminal for current flow. When the battery pack is charged, a charging current (including regenerative energy from the power of an automobile or the like) is supplied to the battery pack through the external terminal for current flow.
[0187] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.
[0188] Fig. 10 is an exploded perspective view showing an example of a battery pack, and Fig. 11 is a block diagram showing an example of an electric circuit of the battery pack shown in Fig. 10.
[0189] The battery pack 300 shown in Figs. 10 and 11 includes a container 31, a lid 32, a protective sheet 33, a battery pack 200, a printed wiring board 34, wiring 35, and an insulating plate (not shown).
[0190] 10 is a bottomed, square container having a rectangular bottom. The container 31 is configured to be able to accommodate a protective sheet 33, a battery pack 200, a printed wiring board 34, and wiring 35. The lid 32 has a rectangular shape. The lid 32 covers the container 31 to accommodate the battery pack 200 and the like. Although not shown, the container 31 and the lid 32 are provided with openings or connection terminals for connection to an external device or the like.
[0191] The battery pack 200 includes a plurality of cells 100, a positive electrode lead 22, a negative electrode lead 23, and an adhesive tape 24.
[0192] At least one of the plurality of unit cells 100 is a secondary battery according to the second embodiment. Each of the plurality of unit cells 100 is electrically connected in series as shown in FIG. 11. The plurality of unit cells 100 may be electrically connected in parallel, or may be connected in a combination of series and parallel connections. When the plurality of unit cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.
[0193] The adhesive tape 24 fastens the plurality of unit cells 100. The plurality of unit cells 100 may be fixed using heat shrink tape instead of the adhesive tape 24. In this case, the protective sheets 33 are disposed on both side surfaces of the battery pack 200, the heat shrink tape is wrapped around the battery pack 200, and the heat shrink tape is then thermally shrunk to bind the plurality of unit cells 100 together.
[0194] One end of the positive electrode lead 22 is connected to the battery pack 200. One end of the positive electrode lead 22 is electrically connected to the positive electrode of one or more cells 100. One end of the negative electrode lead 23 is connected to the battery pack 200. One end of the negative electrode lead 23 is electrically connected to the negative electrode of one or more cells 100.
[0195] The printed wiring board 34 is disposed along one of the short side surfaces of the inner surface of the container 31. The printed wiring board 34 includes a positive connector 342, a negative connector 343, a thermistor 345, a protection circuit 346, wiring 342a and 343a, an external terminal 350 for supplying electricity, a positive wiring (positive wiring) 348a, and a negative wiring (negative wiring) 348b. One main surface of the printed wiring board 34 faces one side of the battery pack 200. An insulating plate (not shown) is interposed between the printed wiring board 34 and the battery pack 200.
[0196] The other end 22a of the positive electrode lead 22 is electrically connected to the positive electrode connector 342. The other end 23a of the negative electrode lead 23 is electrically connected to the negative electrode connector 343.
[0197] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each of the cells 100, and transmits a detection signal to the protection circuit 346.
[0198] The external terminal 350 for current supply is fixed to the other main surface of the printed wiring board 34. The external terminal 350 for current supply is electrically connected to a device present outside the battery pack 300. The external terminal 350 for current supply includes a positive terminal 352 and a negative terminal 353.
[0199] The protection circuit 346 is fixed to the other main surface of the printed wiring board 34. The protection circuit 346 is connected to the positive terminal 352 via a positive wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via a negative wiring 348b. The protection circuit 346 is also electrically connected to the positive electrode connector 342 via a wiring 342a. The protection circuit 346 is electrically connected to the negative electrode connector 343 via a wiring 343a. Furthermore, the protection circuit 346 is electrically connected to each of the plurality of single cells 100 via the wiring 35.
[0200] The protective sheet 33 is disposed on both inner surfaces in the long side direction of the container 31 and on the inner surface in the short side direction that faces the printed wiring board 34 via the battery pack 200. The protective sheet 33 is made of, for example, resin or rubber.
[0201] The protection circuit 346 controls charging and discharging of the multiple cells 100. In addition, the protection circuit 346 cuts off electrical connection between the protection circuit 346 and external terminals 350 (positive terminal 352, negative terminal 353) for supplying electricity to an external device, based on a detection signal transmitted from the thermistor 345, or a detection signal transmitted from each of the cells 100 or the battery pack 200.
[0202] An example of the detection signal transmitted from the thermistor 345 is a signal that detects that the temperature of the cell 100 is equal to or higher than a predetermined temperature. An example of the detection signal transmitted from each cell 100 or the battery pack 200 is a signal that detects overcharging, overdischarging, and overcurrent of the cell 100. When detecting overcharging or the like for each cell 100, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 100.
[0203] The protection circuit 346 may be a circuit included in a device (such as an electronic device or an automobile) that uses the battery pack 300 as a power source.
[0204] As described above, the battery pack 300 includes the external terminal 350 for current supply. Therefore, the battery pack 300 can output a current from the assembled battery 200 to an external device and input a current from the external device to the assembled battery 200 via the external terminal 350 for current supply. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 is supplied to the external device through the external terminal 350 for current supply. When the battery pack 300 is charged, a charging current from the external device is supplied to the battery pack 300 through the external terminal 350 for current supply. When the battery pack 300 is used as an in-vehicle battery, regenerative energy of the vehicle's power can be used as the charging current from the external device.
[0205] The battery pack 300 may include a plurality of assembled batteries 200. In this case, the assembled batteries 200 may be connected in series, in parallel, or in a combination of series and parallel connections. The printed wiring board 34 and the wiring 35 may be omitted. In this case, the positive electrode lead 22 and the negative electrode lead 23 may be used as a positive terminal 352 and a negative terminal 353, respectively, of the external terminal 350 for current supply.
[0206] Such a battery pack is used in applications that require excellent cycle performance, for example, when a large current is drawn. Specifically, the battery pack is used, for example, as a power source for electronic devices, a stationary battery, or an on-board battery for various vehicles. An example of the electronic device is a digital camera. The battery pack is particularly suitable for use as an on-board battery.
[0207] The battery pack according to the fourth embodiment includes the secondary battery according to the second embodiment or the battery pack according to the third embodiment, and therefore the battery pack can achieve excellent cycle performance and output performance.
[0208] Fifth embodiment According to a fifth embodiment, a vehicle is provided. The vehicle is equipped with the battery pack according to the fourth embodiment.
[0209] In such a vehicle, the battery pack, for example, recovers regenerative energy of the vehicle's motive power. The vehicle may include a mechanism (regenerator) that converts the kinetic energy of the vehicle into regenerative energy.
[0210] Examples of vehicles include, for example, two to four wheel hybrid electric vehicles, two to four wheel electric vehicles, power assisted bicycles, and rail vehicles.
[0211] The mounting position of the battery pack in the vehicle is not particularly limited. For example, when the battery pack is mounted in an automobile, the battery pack can be mounted in the engine compartment, the rear of the vehicle body, or under the seat of the vehicle.
[0212] The vehicle may be equipped with a plurality of battery packs. In this case, the batteries included in each battery pack may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. For example, when each battery pack includes a battery pack, the battery packs may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. Alternatively, when each battery pack includes a single battery, the batteries may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections.
[0213] Next, an example of a vehicle according to an embodiment will be described with reference to the drawings.
[0214] FIG. 12 is a partially see-through view that diagrammatically illustrates an example of a vehicle.
[0215] A vehicle 400 shown in Fig. 12 includes a vehicle body 40 and a battery pack 300 according to the fourth embodiment. In the example shown in Fig. 12, the vehicle 400 is a four-wheeled automobile.
[0216] The vehicle 400 may be equipped with a plurality of battery packs 300. In this case, the batteries (e.g., single cells or assembled batteries) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series and parallel connections.
[0217] 12 illustrates an example in which the battery pack 300 is mounted in an engine room located in the front of the vehicle body 40. As described above, the battery pack 300 may be mounted, for example, in the rear of the vehicle body 40 or under a seat. This battery pack 300 can be used as a power source for the vehicle 400. In addition, this battery pack 300 can recover regenerative energy for the motive power of the vehicle 400.
[0218] Next, an embodiment of the vehicle according to the embodiment will be described with reference to FIG.
[0219] Fig. 13 is a diagram illustrating an example of a control system for an electrical system in a vehicle. The vehicle 400 illustrated in Fig. 13 is an electric vehicle.
[0220] The vehicle 400 shown in FIG. 13 comprises a vehicle body 40, a vehicle power supply 41, a vehicle ECU (ECU: Electric Control Unit) 42 which is a higher-level control device of the vehicle power supply 41, an external terminal (terminal for connecting to an external power supply) 43, an inverter 44, and a drive motor 45.
[0221] The vehicle 400 has a vehicle power supply 41 mounted, for example, in an engine compartment, the rear of the vehicle body, or under a seat. Note that in the vehicle 400 shown in Fig. 13, the mounting location of the vehicle power supply 41 is shown diagrammatically.
[0222] The vehicle power supply 41 includes a plurality of (eg, three) battery packs 300a, 300b, and 300c, a battery management unit (BMU) 411, and a communication bus 412.
[0223] The battery pack 300a includes an assembled battery 200a and an assembled battery monitoring device 301a (for example, VTM: Voltage Temperature Monitoring). The battery pack 300b includes an assembled battery 200b and an assembled battery monitoring device 301b. The battery pack 300c includes an assembled battery 200c and an assembled battery monitoring device 301c. The battery packs 300a to 300c are battery packs similar to the above-mentioned battery pack 300, and the assembled batteries 200a to 200c are assembled batteries similar to the above-mentioned battery pack 200. The assembled batteries 200a to 200c are electrically connected in series. The battery packs 300a, 300b, and 300c can be removed independently and replaced with another battery pack 300.
[0224] Each of the assembled batteries 200a to 200c includes a plurality of unit cells connected in series. At least one of the plurality of unit cells is the secondary battery according to the second embodiment. Each of the assembled batteries 200a to 200c is charged and discharged via a positive terminal 413 and a negative terminal 414.
[0225] The battery management device 411 communicates with the assembled battery monitoring devices 301a to 301c, and collects information on the voltage, temperature, and the like of each of the cells 100 included in the assembled batteries 200a to 200c included in the vehicle power supply 41. In this way, the battery management device 411 collects information on the maintenance of the vehicle power supply 41.
[0226] The battery management unit 411 and the assembled battery monitoring units 301a to 301c are connected via a communication bus 412. In the communication bus 412, one set of communication lines is shared by a plurality of nodes (the battery management unit 411 and one or more assembled battery monitoring units 301a to 301c). The communication bus 412 is a communication bus configured based on, for example, the CAN (Control Area Network) standard.
[0227] The battery pack monitoring devices 301a to 301c measure the voltage and temperature of each of the cells constituting the battery packs 200a to 200c based on commands communicated from the battery management device 411. However, the temperature can be measured at only a few points per battery pack, and it is not necessary to measure the temperatures of all the cells.
[0228] The vehicle power supply 41 may also have an electromagnetic contactor (for example, a switch device 415 shown in FIG. 13) that switches between the presence and absence of an electrical connection between the positive terminal 413 and the negative terminal 414. The switch device 415 includes a pre-charge switch (not shown) that is turned on when the assembled batteries 200a to 200c are charged, and a main switch (not shown) that is turned on when the output from the assembled batteries 200a to 200c is supplied to a load. Each of the pre-charge switch and the main switch includes a relay circuit (not shown) that is switched on or off by a signal supplied to a coil disposed near the switch element. The electromagnetic contactor such as the switch device 415 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 that controls the operation of the entire vehicle 400.
[0229] The inverter 44 converts the input DC voltage into a three-phase alternating current (AC) high voltage for driving the motor. The three-phase output terminals of the inverter 44 are connected to the three-phase input terminals of the drive motor 45. The inverter 44 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 for controlling the operation of the entire vehicle. By controlling the inverter 44, the output voltage from the inverter 44 is adjusted.
[0230] The drive motor 45 rotates by electric power supplied from the inverter 44. A driving force generated by the rotation of the drive motor 45 is transmitted to the axles and drive wheels W via, for example, a differential gear unit.
[0231] Although not shown, the vehicle 400 is also equipped with a regenerative braking mechanism (regenerator). The regenerative braking mechanism rotates the drive motor 45 when the vehicle 400 is braked, and converts kinetic energy into regenerative energy as electrical energy. The regenerative energy recovered by the regenerative braking mechanism is input to the inverter 44 and converted into a direct current. The converted direct current is input to the vehicle power source 41.
[0232] One terminal of a connection line L1 is connected to the negative terminal 414 of the vehicle power supply 41. The other terminal of the connection line L1 is connected to a negative input terminal 417 of the inverter 44. A current detection unit (current detection circuit) 416 in the battery management device 411 is provided between the negative terminal 414 and the negative input terminal 417 on the connection line L1.
[0233] One terminal of a connection line L2 is connected to the positive electrode terminal 413 of the vehicle power supply 41. The other terminal of the connection line L2 is connected to a positive electrode input terminal 418 of the inverter 44. A switch device 415 is provided in the connection line L2 between the positive electrode terminal 413 and the positive electrode input terminal 418.
[0234] The external terminal 43 is connected to the battery management unit 411. The external terminal 43 can be connected to, for example, an external power source.
[0235] In response to operational inputs from the driver or the like, the vehicle ECU 42 coordinates with other management devices and control devices including the battery management device 411 to control the vehicle power supply 41, the switch device 415, the inverter 44, etc. Through the coordinated control of the vehicle ECU 42, etc., the output of power from the vehicle power supply 41 and the charging of the vehicle power supply 41 are controlled, and the entire vehicle 400 is managed. Data relating to the maintenance of the vehicle power supply 41, such as the remaining capacity of the vehicle power supply 41, is transferred between the battery management device 411 and the vehicle ECU 42 via a communication line.
[0236] The vehicle according to the fifth embodiment is equipped with the battery pack according to the fourth embodiment, and therefore the cycle performance and output performance of the battery pack of the vehicle are high, and therefore the reliability of the vehicle is high. EXAMPLES
[0237] Examples will be described below, but the embodiments are not limited to the examples described below.
[0238] Example 1 <Preparation of the first particle> The first particles were prepared by adding niobium titanium oxide particles to an inorganic particle-containing layer precursor solution and firing the solution, as described below.
[0239] <Preparation of the first solution> 1g of nitric acid and 10g of a 20% by weight solution of polyvinyl alcohol were added to 500mL of water and stirred with a stirrer for 10 minutes. 12g of titanium tetraisopropoxide was added thereto and stirred for 1 hour. Furthermore, 2.6g of lithium nitrate, 9g of ammonium dihydrogen phosphate, and 4g of aluminum nitrate nonahydrate were added and stirred for 30 minutes. Thus, a first solution was obtained.
[0240] <Formation of Inorganic Particle-Containing Layer> The first solution prepared above was prepared as the inorganic particle-containing layer precursor solution. Niobium titanium oxide particles were added to the first solution. At this time, the addition was made at a ratio such that the mass of the inorganic particle-containing layer obtained after firing was 3 mass% relative to the mass of the niobium titanium oxide particles. This dispersion was stirred for 1 hour. After stirring, it was heated to 200°C and evaporated to dryness to obtain a dry powder. The dry powder was transferred to an alumina crucible and fired in an electric furnace at 700°C for 8 hours. In this way, the first particles having an inorganic particle-containing layer formed on the surface of the niobium titanium oxide particles were obtained. The inorganic particle-containing layer contained solid electrolyte-containing particles. The solid electrolyte was Li 1.3 Al 0.3 Ti 1.7 The oxide-based solid electrolyte had a composition represented by (PO4)3. Thus, the first particles were obtained.
[0241] <Preparation of negative electrode> 88% by mass of the first particles as negative electrode active material particles, 4% by mass of acetylene black as a conductive agent, 2% by mass of carboxymethyl cellulose (CMC) and 2% by mass of styrene butadiene rubber (SBR) as binders, and 4% by mass of inorganic particles were added to pure water as a solvent and mixed. As the inorganic particles, particles having an average particle diameter of 0.5 μm and containing a solid electrolyte were used. The solid electrolyte was Li 1.3 Al 0.3 Ti 1.7The mixture was placed in a stirring vessel, and glass beads of φ2 mm were added to a filling rate of 60%, followed by stirring at 1500 rpm for 3 minutes to obtain a slurry. The stirred slurry was applied to one side of a current collector made of aluminum foil with a thickness of 12 μm, and dried on a hot plate at 100° C. The slurry was also applied to the other side, and dried on a hot plate at 100° C. Then, the mixture was pressed to obtain a negative electrode. The obtained negative electrode was a double-sided negative electrode in which a negative electrode active material-containing layer was formed on both sides of the current collector.
[0242] <Preparation of positive electrode> Lithium nickel cobalt manganese composite oxide (LiNi 0.8 Co 0.1 Mn 0.1 A slurry was prepared by adding and mixing 90% by mass of O2), 5% by mass of acetylene black as a conductive agent, and 5% by mass of polyvinylidene fluoride (PVdF) as a binder to N-methylpyrrolidone (NMP) as a solvent. The slurry was applied to one side of a current collector made of aluminum foil with a thickness of 12 μm and dried in a thermostatic chamber at 120° C. Then, the positive electrode was obtained by pressing. The obtained positive electrode was a single-sided positive electrode in which a positive electrode active material-containing layer was formed on one side of the current collector.
[0243] <Preparation of electrode groups> A single-sided positive electrode, a separator, a double-sided negative electrode, a separator, and a single-sided positive electrode were laminated in this order to obtain a laminate. The single-sided positive electrode was laminated so that the side on which the slurry was applied faced the separator. A 15 μm-thick polyethylene porous film was used as the separator. The laminate was hot-pressed at 80°C to produce a flat electrode group. The obtained electrode group was stored in a pack made of a 0.1 mm-thick laminate film having a three-layer structure of a nylon layer / aluminum layer / polyethylene layer, and dried in a vacuum at 120°C for 16 hours.
[0244] <Preparation of non-aqueous electrolyte and fabrication of secondary battery> A non-aqueous electrolyte was obtained by dissolving LiPF6 as an electrolyte at a concentration of 1 mol / L in a mixed solvent of propylene carbonate (PC) and diethyl carbonate (DEC) (volume ratio 1:2). The preparation of the non-aqueous electrolyte was carried out in an argon box.
[0245] A non-aqueous electrolyte was poured into the laminate film pack containing the electrode group, and the pack was then completely sealed by heat sealing to obtain a secondary battery with a capacity of 300 mAh.
[0246] Example 2 The ratio of niobium titanium oxide particles added to the first solution was adjusted so that the mass of the inorganic particle-containing layer obtained after firing was 10 mass% relative to the mass of the niobium titanium oxide particles. Also, the average particle diameter of the inorganic particles was changed to 1.0 μm. A secondary battery was produced in the same manner as in Example 1 except for the above.
[0247] Example 3 The ratio of niobium titanium oxide particles added to the first solution was adjusted so that the mass of the inorganic particle-containing layer obtained after firing was 0.5 mass% relative to the mass of the niobium titanium oxide particles. In addition, the average particle diameter of the inorganic particles was changed to 0.9 μm. A secondary battery was produced in the same manner as in Example 1 except for the above.
[0248] Example 4 The ratio of niobium titanium oxide particles added to the first solution was adjusted so that the mass of the inorganic particle-containing layer obtained after firing was 15 mass% relative to the mass of the niobium titanium oxide particles. Also, the average particle diameter of the inorganic particles was changed to 0.9 μm. A secondary battery was produced in the same manner as in Example 1 except for the above.
[0249] Example 5 The ratio of niobium titanium oxide particles added to the first solution was adjusted so that the mass of the inorganic particle-containing layer obtained after firing was 0.05 mass% relative to the mass of the niobium titanium oxide particles. In addition, the average particle diameter of the inorganic particles was changed to 0.8 μm. A secondary battery was produced in the same manner as in Example 1 except for the above.
[0250] Example 6 The average particle size of the inorganic particles was changed to 1.0 μm. A secondary battery was fabricated in the same manner as in Example 1 except for the above.
[0251] Example 7 The average particle size of the inorganic particles was changed to 0.4 μm. A secondary battery was fabricated in the same manner as in Example 1 except for the above.
[0252] Example 8 The average particle size of the inorganic particles was changed to 2.0 μm. A secondary battery was fabricated in the same manner as in Example 1 except for the above.
[0253] Example 9 The average particle size of the inorganic particles was changed to 0.3 μm. A secondary battery was fabricated in the same manner as in Example 1 except for the above.
[0254] Example 10 A secondary battery was produced in the same manner as in Example 2, except that in the production of the negative electrode, stirring was performed without adding glass beads.
[0255] Example 11 As the inorganic particle-containing layer precursor solution, a commercially available 98% aluminum isopropoxide solution was prepared instead of the first solution. In addition, the inorganic particles were changed to Al2O3 particles with an average particle diameter of 0.5 μm. A secondary battery was fabricated in the same manner as in Example 1 except for the above.
[0256] Example 12 As the inorganic particle-containing layer precursor solution, a commercially available 97% titanium tetraisopropoxide solution was prepared instead of the first solution. In addition, the inorganic particles were changed to TiO2 particles with an average particle diameter of 0.5 μm. A secondary battery was fabricated in the same manner as in Example 1 except for the above.
[0257] (Example 13) As the inorganic particle-containing layer precursor solution, a commercially available 70% zirconium propoxide solution was prepared instead of the first solution. In addition, the inorganic particles were changed to ZrO2 particles with an average particle diameter of 0.5 μm. A secondary battery was fabricated in the same manner as in Example 1 except for the above.
[0258] Example 14 As the inorganic particle-containing layer precursor solution, an aqueous magnesium sulfate solution was prepared instead of the first solution. The aqueous magnesium sulfate solution was prepared as follows. 20 g of magnesium sulfate heptahydrate was added to 100 g of water and stirred to obtain an aqueous magnesium sulfate solution. In addition, the inorganic particles were changed to MgO particles with an average particle diameter of 0.5 μm. A secondary battery was fabricated in the same manner as in Example 1 except for the above.
[0259] Comparative Example 1 The preparation of the first particles was omitted. In the preparation of the negative electrode, niobium titanium oxide particles were used as the negative electrode active material particles. A secondary battery was prepared in the same manner as in Example 1 except for the above.
[0260] Comparative Example 2 A secondary battery was produced in the same manner as in Example 1, except that the addition of inorganic particles was omitted in the production of the negative electrode.
[0261] Comparative Example 3 The ratio of niobium titanium oxide particles added to the first solution was adjusted so that the mass of the inorganic particle-containing layer obtained after firing was 15 mass% relative to the mass of the niobium titanium oxide particles. Also, the average particle diameter of the inorganic particles was changed to 0.5 μm. A secondary battery was produced in the same manner as in Example 1 except for the above.
[0262] Comparative Example 4 The preparation of the first particles was omitted. In preparing the negative electrode, niobium titanium oxide particles were used as the negative electrode active material particles. The average particle diameter of the inorganic particles was changed to 1.0 μm. Furthermore, 5 mass% of solid electrolyte-containing particles with an average particle diameter of 0.5 μm were added. The solid electrolyte was Li 1.3 Al 0.3 Ti1.7 The solid electrolyte was an oxide-based material represented by the formula (PO4)3.
[0263] The cycle performance and output performance of the produced secondary battery were evaluated by the following methods. <Cycle test> The obtained secondary battery was charged at a constant current of 1C rate at 25°C up to 3.0V. Then, it was discharged at a rate of 1C up to 1.5V. This charge / discharge was defined as one cycle. At the time of the discharge in the first cycle, the discharge capacity was measured. Next, the above charge / discharge was repeated for a total of 200 cycles. At the time of the discharge in the 200th cycle, the discharge capacity was measured. The value obtained by dividing the discharge capacity in the 200th cycle by the discharge capacity in the first cycle and multiplying the result by 100 was defined as the capacity retention rate (%). <0℃ discharge performance test> The battery was charged to 3.0 V at a constant current of 1 C at 25° C., and then discharged to 1.5 V at 1 C at 0° C. The discharge capacity was measured during discharge. The obtained discharge capacity was defined as the 0° C. discharge capacity (mAh).
[0264] The results of these measurements are shown in Table 1. The type and thickness of the inorganic particle-containing layer for the comparative example in which the preparation of the first particles was omitted, and the type and average particle size of the inorganic particles for the comparative example in which no inorganic particles were added are indicated by "-".
[0265] [Table 1]
[0266] The secondary batteries of the examples, which included an electrode containing inorganic particles and first particles, and in which the average particle diameter of the inorganic particles was larger than the thickness of the inorganic particle-containing layer, all had high capacity retention rates and 0° C. discharge capacities, i.e., excellent cycle performance and output performance.
[0267] In Comparative Example 1 and Comparative Example 4, in which the preparation of the first particles, i.e., the formation of an inorganic particle-containing layer on the surface of the niobium titanium oxide particles, was omitted, the capacity retention rate was low. This is considered to be because when the hydrofluoric acid that was not captured by the inorganic particles approaches the niobium titanium oxide particles, the hydrofluoric acid comes into contact with the surface of the niobium titanium oxide particles, and as a result, the niobium titanium oxide particles are deteriorated, resulting in a decrease in cycle performance.
[0268] Comparative Example 4 is an example in which the formation of the inorganic particle-containing layer is omitted and instead solid electrolyte-containing particles are further added, but the cycle performance was lower than that of the examples. From this, it is considered that when the solid electrolyte-containing particles are not formed in a layer on the surface of the niobium titanium oxide particles, that is, when they are present apart from the niobium titanium oxide particles, the effect of suppressing the contact of hydrofluoric acid with the niobium titanium oxide particles is low.
[0269] Comparative Example 2, in which the addition of inorganic particles was omitted, had a low capacity retention rate. This is believed to be because the amount of hydrofluoric acid approaching the first particles in the electrode of Comparative Example 2 was greater than that of the electrode of the Example, since hydrofluoric acid was not captured by the inorganic particles. As a result, for example, the amount of hydrofluoric acid contacting the surface of the niobium titanium oxide particles from the exposed portion of the first particle is believed to have increased. In addition, it is believed that the amount of hydrofluoric acid contacting the niobium titanium oxide particles increased as the amount of hydrofluoric acid that exceeded the amount of hydrofluoric acid that the inorganic particle-containing layer could capture approached the first particle. As a result, it is believed that the cycle performance was reduced due to the deterioration of the niobium titanium oxide.
[0270] In Comparative Example 3, in which the thickness of the inorganic particle-containing layer was larger than the average particle diameter of the inorganic particles, the 0°C discharge capacity was lower than that of the Examples. That is, the output performance was lower than that of the Examples. In Comparative Example 3, the average particle diameter of the inorganic particles was relatively small compared to the thickness of the inorganic particle-containing layer, which is considered to have caused the dispersibility of the inorganic particles and the conductive agent in the electrode manufacturing process to decrease, thereby causing the uniformity of the inorganic particles and the conductive agent in the electrode to decrease. In addition, the active material particles of Comparative Example 3 have relatively low electronic conductivity due to the thickness of the inorganic particle-containing layer being larger than the average particle diameter of the inorganic particles. It is considered that the output performance of Comparative Example 3 was decreased due to these factors.
[0271] Comparing Examples 1 to 3 with Example 4 in which the thickness of the inorganic particle-containing layer was 0.7 μm, Examples 1 to 3 had particularly high 0° C. discharge capacity. This is believed to be because Examples 1 to 3 had a high effect of suppressing resistance increase due to the inorganic particle-containing layer having a thickness of 0.4 μm or less. Therefore, it was revealed that the electrode containing the first particles in which the inorganic particle-containing layer has a thickness of 0.4 μm or less is particularly excellent in output performance.
[0272] In addition, when Examples 1 to 3 are compared with Example 5 in which the thickness of the inorganic particle-containing layer is 0.0005 μm, Examples 1 to 3 have particularly high capacity retention rates. This is believed to be because Examples 1 to 3 have high durability against hydrofluoric acid due to the inorganic particle-containing layer having a thickness of 0.0010 μm or more. Therefore, it is clear that the electrode containing the first particles in which the inorganic particle-containing layer has a thickness of 0.0010 μm or more has particularly excellent cycle performance.
[0273] Comparing Examples 1, 6, and 7 with Example 8, in which the inorganic particles have an average particle size of 2.0 μm, and Example 9, in which the inorganic particles have an average particle size of 0.3 μm, Examples 1, 6, and 7 have particularly high capacity retention rates. From this result, it is considered that the inorganic particles having an average particle size of 0.4 μm or more and 1.0 μm or less contained in Examples 1, 6, and 7 are within the range of inorganic particle sizes suitable for exerting hydrofluoric acid trapping ability. Therefore, it has become clear that electrodes in which the inorganic particles have an average particle size in the range of 0.4 μm or more and 1.0 μm or less have particularly excellent cycle performance.
[0274] Example 10 is a secondary battery prepared in the same manner as Example 2, except that the anode was prepared by stirring without adding glass beads. It is considered that the first particles contained in Example 2, in which glass beads were added during stirring, had a part of the surface of the niobium titanium oxide particles exposed by scraping a part of the surface of the inorganic particle-containing layer. In other words, it is considered that the first particles had an exposed portion. Such Example 2 had a particularly high 0°C discharge capacity compared to Example 10, in which glass beads were not added during stirring. This revealed that the electrode containing the first particles having an exposed portion has particularly excellent output performance.
[0275] Example 11 is an electrode in which the inorganic particle-containing layer contains particles containing a metal oxide containing Al, and contains Al2O3 particles as the inorganic particles. Example 12 is an electrode in which the inorganic particle-containing layer contains particles containing a metal oxide containing Ti, and contains TiO2 particles as the inorganic particles. Example 13 is an electrode in which the inorganic particle-containing layer contains particles containing a metal oxide containing Zr, and contains ZrO2 particles as the inorganic particles. Example 14 is an electrode in which the inorganic particle-containing layer contains particles containing a metal oxide containing Mg, and contains MgO particles as the inorganic particles. In these Examples 11 to 14, both the capacity retention rate and the 0°C discharge capacity were high. That is, both the cycle performance and the output performance were excellent.
[0276] From this, it was revealed that the inorganic particle-containing layer can improve cycle performance and output performance even when it contains particles containing a metal oxide containing at least one element selected from the group consisting of Al, Ti, Zr, and Mg. It was also revealed that the inorganic particle-containing layer can improve cycle performance and output performance even when it contains a metal oxide containing at least one element selected from the group consisting of Al, Ti, Zr, and Mg as inorganic particles.
[0277] According to at least one embodiment described above, an electrode is provided. The electrode includes inorganic particles, niobium titanium oxide particles, and an inorganic particle-containing layer that covers at least a part of the surface of the niobium titanium oxide particles. The average particle diameter of the inorganic particles is larger than the thickness of the inorganic particle-containing layer. Therefore, the electrode can improve cycle performance and output performance.
[0278] The invention according to the embodiment will be described below.
[0279] <1> The present invention relates to a niobium titanium oxide particle having an inorganic particle-containing layer, the inorganic particle-containing layer comprising: an inorganic particle; a niobium titanium oxide particle; and an inorganic particle-containing layer covering at least a portion of the surface of the niobium titanium oxide particle. An electrode, wherein the average particle diameter of the inorganic particles is greater than a thickness of the inorganic particle-containing layer.
[0280] <2> The thickness of the inorganic particle-containing layer is in the range of 0.001 μm or more and 0.4 μm or less. <1> The electrode according to claim 1.
[0281] <3> The average particle size of the inorganic particles is in the range of 0.4 μm or more and 1 μm or less. <1> or <2> The electrode according to claim 1.
[0282] <4> The surfaces of the niobium titanium oxide particles include portions that are not covered by the inorganic particle-containing layer, and at least a portion of the portions that are not covered by the inorganic particle-containing layer are exposed on the surface of the electrode. <1> ~ <3> 13. The electrode according to any one of claims 1 to 12.
[0283] <5> The inorganic particles include at least one selected from the group consisting of metal oxides and solid electrolytes containing at least one element selected from the group consisting of Al, Ti, Si, Zr, and Mg. <1> ~ <4> 13. The electrode according to any one of claims 1 to 12.
[0284] <6> The inorganic particle-containing layer contains at least one selected from the group consisting of particles containing a metal oxide containing at least one element selected from the group consisting of Al, Ti, Si, Zr, and Mg, and solid electrolyte-containing particles. <1> ~ <5> 13. The electrode according to any one of claims 1 to 12.
[0285] <7> The inorganic particles contain a solid electrolyte, and the inorganic particle-containing layer contains solid electrolyte-containing particles. <1> ~ <6> 13. The electrode according to any one of claims 1 to 12.
[0286] <8> A positive electrode, a negative electrode, and a non-aqueous electrolyte, The non-aqueous electrolyte contains fluorine atoms, At least one of the positive electrode and the negative electrode is <1> ~ <7> 2. A secondary battery comprising the electrode according to claim 1.
[0287] <9> <8> A battery pack comprising the secondary battery according to claim 1.
[0288] <10> An external terminal for supplying electricity; Protection circuit and Further comprising <9> The battery pack according to claim 1 .
[0289] <11> A battery comprising a plurality of the secondary batteries, The secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel. <9> or <10> The battery pack according to claim 1 .
[0290] <12> <9> ~ <11> 2. A vehicle equipped with the battery pack according to claim 1.
[0291] <13> A mechanism for converting the kinetic energy of the vehicle into regenerative energy is included. <12> A vehicle as described in.
[0292] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0293] Reference Signs List 1...electrode group, 2...exterior member, 3...electrode (negative electrode), 3a...current collector (negative electrode current collector), 3b...active material-containing layer (negative electrode active material-containing layer), 3c...negative electrode current collector tab, 4...separator, 5...positive electrode, 5a...positive electrode current collector, 5b...positive electrode active material-containing layer, 6...negative electrode terminal, 7...positive electrode terminal, 10...first particle, 11...niobium titanium oxide particle, 12...inorganic particle-containing layer, 13...inorganic particle, 14...exposed portion, 21...busbar , 22...positive electrode lead, 22a...other end, 23...negative electrode lead, 23a...other end, 24...adhesive tape, 30...electrode, 30b...active material-containing layer, 31...container, 32...lid, 33...protective sheet, 34...printed wiring board, 35...wiring, 40...vehicle body, 41...vehicle power source, 42...electrical control device, 43...external terminal, 44...inverter, 45...driving motor, 100...secondary battery, 200...assembly Battery, 200a... battery pack, 200b... battery pack, 200c... battery pack, 300... battery pack, 300a... battery pack, 300b... battery pack, 300c... battery pack, 301a... battery pack monitoring device, 301b... battery pack monitoring device, 301c... battery pack monitoring device, 342... positive connector, 343... negative connector, 345... thermistor, 346... protection circuit, 342a... wiring, 343a... wiring Line, 350...external terminal for current flow, 352...positive terminal, 353...negative terminal, 348a...positive wiring, 348b...negative wiring, 400...vehicle, 411...battery management device, 412...communication bus, 413...positive terminal, 414...negative terminal, 415...switch device, 416...current detection unit, 417...negative input terminal, 418...positive input terminal, L1...connection line, L2...connection line, W...drive wheel.
Claims
1. The present invention relates to a niobium titanium oxide particle having an inorganic particle-containing layer, the inorganic particle-containing layer comprising: an inorganic particle; a niobium titanium oxide particle; and an inorganic particle-containing layer covering at least a portion of the surface of the niobium titanium oxide particle. An electrode, wherein the average particle diameter of the inorganic particles is greater than a thickness of the inorganic particle-containing layer.
2. The electrode according to claim 1 , wherein the inorganic particle-containing layer has a thickness in the range of 0.001 μm to 0.4 μm.
3. 2. The electrode according to claim 1, wherein the inorganic particles have an average particle size in the range of 0.4 μm or more and 1 μm or less.
4. 2. The electrode according to claim 1, wherein the surfaces of the niobium titanium oxide particles include portions that are not covered by the inorganic particle-containing layer, and at least a portion of the portions that are not covered by the inorganic particle-containing layer are exposed on the surface of the electrode.
5. 2. The electrode according to claim 1, wherein the inorganic particles comprise at least one selected from the group consisting of metal oxides and solid electrolytes containing at least one element selected from the group consisting of Al, Ti, Si, Zr, and Mg.
6. 2. The electrode according to claim 1, wherein the inorganic particle-containing layer contains at least one selected from the group consisting of particles containing a metal oxide containing at least one element selected from the group consisting of Al, Ti, Si, Zr, and Mg, and solid electrolyte-containing particles.
7. The electrode of claim 1 , wherein the inorganic particles comprise a solid electrolyte and the inorganic particle-containing layer comprises solid electrolyte-containing particles.
8. A positive electrode, a negative electrode, and a non-aqueous electrolyte, The non-aqueous electrolyte contains fluorine atoms, A secondary battery, wherein at least one of the positive electrode and the negative electrode is the electrode according to claim 1 .
9. A battery pack comprising the secondary battery according to claim 8.
10. An external terminal for supplying electricity; Protection circuit and The battery pack of claim 9 further comprising:
11. A battery comprising a plurality of the secondary batteries, The battery pack according to claim 9 , wherein the secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.
12. A vehicle equipped with the battery pack according to claim 9.
13. The vehicle of claim 12, further comprising a mechanism for converting kinetic energy of the vehicle into regenerative energy.
Citation Information
Patent Citations
Positive electrode mixture and nonaqueous electrolyte secondary battery
JP2014026819A
Electrode, nonaqueous electrolyte battery, battery pack and vehicle
JP2018049705A
Active material, electrode, secondary battery, battery pack, and vehicle
JP2022047864A
Cathode active material and secondary cell using the same
JP2012209064A
Power storage device
JP2015011929A
Cited By
Microscope for medical diagnosis and treatment
EP4697077A1
Inorganic oxide powder and lithium ion secondary battery including electrode containing the same
JP2026086982A
Lithium-ion secondary battery comprising inorganic oxide powder and electrodes containing the same
JP7932460B2
Inorganic oxide powder and lithium-ion secondary battery including electrode containing same
WO2026105417A1