Semiconductor device and manufacturing method for the same

By chamfering the edges of element formation regions in semiconductor devices using DHF and HPM cleaning, the method addresses uneven film thickness and enhances performance by reducing steps and electrolytic concentration.

JP2024135307AInactive Publication Date: 2024-10-04LAPIS SEMICON CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023045930
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing semiconductor manufacturing methods result in uneven film thickness and reduced performance due to steps formed at the edges of element isolation regions, leading to potential breakdown voltage failures.

Method used

A method involving multiple cleaning steps with DHF and HPM cleaning solutions is used to chamfer the edges of element formation regions, forming a gently curved surface to ensure uniform oxide film thickness and reduce steps.

Benefits of technology

This approach reduces variations in oxide film thickness and minimizes electrolytic concentration, improving breakdown voltage characteristics and film formation properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135307000001_ABST
    Figure 2024135307000001_ABST
Patent Text Reader

Abstract

To provide a semiconductor device and a manufacturing method for the same, in which the variation in thickness of an oxide film to be formed can be reduced without deteriorating the film formation property of the oxide film at an end part of an element formation region that is adjacent to an element separation region.SOLUTION: A semiconductor device includes a semiconductor substrate, an element formation region formed on the semiconductor substrate and having a semiconductor element formed therein, an element separation region formed on the semiconductor substrate and separating the element formation region for each semiconductor element, and an oxide film covering the element formation region and the element separation region. An end part of the element formation region that is adjacent to the element separation region includes a flat part that is parallel to a main surface of the semiconductor substrate, and a chamfered part obtained by chamfering a step difference between a surface of the element formation region and a surface of the element separation region. The chamfered part has a shape whose height increases and radius of curvature increases from a border between the element formation region and the element separation region toward the flat part at a cross section along a width direction of the element separation region.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor device and a manufacturing method thereof. [Background technology]

[0002] 5, a semiconductor device manufactured using STI (Shallow Trench Isolation) technology includes, on a silicon substrate 110, an isolation trench 154 and an element formation region 114 isolated by the isolation trench 154. Silicon oxide 112 is buried in the element isolation trench 154. A MOS transistor 116 including a gate electrode 120, a channel region 122, a source region 124, and a drain region 126 is formed in a well 118 of the element formation region 114.

[0003] As shown in Fig. 6, a step may occur between the surface of the end 114E of the element formation region 114 and the surface of the silicon oxide 112 embedded in the element isolation trench 154. The step occurs when the silicon oxide 112 is excessively etched back in the manufacturing process. Such a step affects the film formation properties of the oxide film 130 such as the gate insulating film 128 formed thereon, and ultimately causes a decrease in the performance of the semiconductor device. For example, as shown by the arrow, the oxide film becomes thin at the sharp corners of the edge of the step, which causes electric field concentration and causes a breakdown voltage failure.

[0004] To solve this problem, the method for manufacturing a semiconductor device described in Patent Document 1 includes a step of forming a rounded upper end of the trench by wet etching. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2000-21970 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the method described in Patent Document 1, only the edges are etched away and rounded, and the steps are not completely removed. As a result, the problem of the deterioration of the oxide film formability still remains.

[0007] The present invention has been made in view of the above problems, and an object of the present invention is to provide a semiconductor device and a manufacturing method thereof that can reduce the variation in thickness of an oxide film formed at an end of an element formation region adjacent to an element isolation region without impairing the film formability of the oxide film. [Means for solving the problem]

[0008] One aspect of the present invention relates to a semiconductor device comprising: a semiconductor substrate; an element formation region formed on the semiconductor substrate in which semiconductor elements are formed; an element isolation region formed on the semiconductor substrate for isolating the element formation region into individual semiconductor elements; and an oxide film covering the element formation region and the element isolation region, wherein an end of the element formation region adjacent to the element isolation region comprises a flat portion parallel to a main surface of the semiconductor substrate and a chamfered portion that chamfers a step between a surface of the element formation region and a surface of the element isolation region, and the chamfered portion has a shape that, in a cross section taken along the width direction of the element isolation region, increases in height and has an increasing radius of curvature from the boundary between the element formation region and the element isolation region toward the flat portion.

[0009] Another aspect of the present invention relates to a method for manufacturing a semiconductor device, the method including the steps of forming an isolation trench in an isolation region on a semiconductor substrate, filling the isolation trench with a semiconductor oxide, etching the semiconductor oxide filled in the isolation trench, and cleaning a surface of the element formation region and the isolation region on the semiconductor substrate, the cleaning step being performed by a first cleaning step of removing a native oxide film formed on the surface of the element formation region with a first cleaning liquid, and a second cleaning step performed after the first cleaning step of scraping off the surface of the semiconductor substrate in the element formation region with a second cleaning liquid, and if a step occurs between the surface of the element formation region and the surface of the element isolation region, the second cleaning step is performed by spraying the second cleaning liquid obliquely from above onto the step to chamfer the step. Effect of the Invention

[0010] According to the present invention, it is possible to reduce the variation in thickness of the oxide film formed at the end of the element formation region adjacent to the element isolation region without impairing the film formability of the oxide film. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view showing an example of a configuration of a semiconductor device according to an embodiment of the present invention. [Diagram 2] 2A and 2B are enlarged views showing an example of a detailed configuration of region A in FIG. [Diagram 3] 5(A) to 5(G) are cross-sectional views showing an example of a step of forming an isolation trench in a semiconductor device. [Figure 4] 4(A) to 4(F) are schematic diagrams showing an example of a procedure of a cleaning step in the element isolation trench forming step shown in FIG. [Diagram 5] FIG. 1 is a cross-sectional view showing an example of the configuration of a conventional semiconductor device. [Figure 6] 6 is an enlarged view showing an example of a detailed configuration of an area B in FIG. 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] An embodiment of the present invention will now be described in detail with reference to the drawings.

[0013] <Semiconductor device> First, the configuration of a semiconductor device according to an embodiment of the present invention will be described with reference to FIG. 1, the semiconductor device 1 according to this embodiment includes, on a silicon substrate 10, which is an example of a semiconductor substrate, an element isolation trench 54, which is an example of an element isolation region, and an element formation region 14, which is isolated by the element isolation trench 54. Silicon oxide 12, which is an example of a semiconductor oxide, is buried in a well 18 of the element formation region 14. A MOS transistor 16, which is an example of a semiconductor element, is formed in a well 18 of the element formation region 14.

[0014] The MOS transistor 16 includes a gate electrode 20 formed on the surface of the well 18 via a gate insulating film 28, a channel region 22 located below the gate electrode 20, and a source region 24 and a drain region 26 arranged on either side of the channel region 22. The element formation region 14 and the element isolation region in which the element isolation trench 54 is formed are each covered with an insulating oxide film 30 made of silicon oxide.

[0015] (Structure of the edge of the element formation region) 2(A) and 2(B) are enlarged views showing the structure of the end portion of the element formation region 14 shown as region A in Fig. 1. As will be described later, steps that occur at the end portion of the element formation region 14 during the manufacturing process are removed by repeating a cleaning process that combines DHF cleaning and HPM cleaning multiple times (see Figs. 3(F) and (G)). The more times the cleaning process is repeated, the more the step portion is removed.

[0016] 2A shows a structure in the case where the cleaning process is repeated a number of times less than the threshold value. In this case, the end 14E of the element formation region 14 is composed of a flat portion 14T in the center of the element formation region 14 and a chamfered portion 14R continuing from the flat portion 14T. The chamfered portion 14R has a gently curved surface. When viewed in a cross section along the width direction of the element isolation trench 54, the chamfered portion 14R has a shape in which the radius of curvature increases from the boundary between the element formation region 14 and the element isolation trench 54 (i.e., the silicon oxide 12) toward the flat portion 14T.

[0017] FIG. 2(B) shows a structure in the case where the cleaning process is repeated a number of times less than the threshold value. In this case, the end 14E of the element formation region 14 is composed of a flat portion 14T in the center of the element formation region 14 and a chamfered portion 14R continuing from the flat portion 14T. The chamfered portion 14R includes a gentle slope. When viewed in a cross section along the width direction of the element isolation trench 54, the chamfered portion 14R has a shape in which the radius of curvature increases from the boundary between the element formation region 14 and the element isolation trench 54 toward the flat portion 14T. In the sloped portion, the radius of curvature becomes infinite. Also, compared to FIG. 2(A), the flat portion (flat portion 14T) has decreased, and the sloped portion (chamfered portion 14R) has increased.

[0018] As shown in Figures 2(A) and 2(B), at the end 14E of the element formation region 14, the corners of the steps are scraped off to make the surface approximately flat, so that when the oxide film 30 is formed on the surfaces of the element formation region 14 and the silicon oxide 12, the oxide film 30 is formed with an approximately uniform thickness. In either structure, the surface of the element formation region 14 is covered with a chemical oxide film 32. Therefore, on the element formation region 14, the oxide film has a two-layer structure of the chemical oxide film 32 and the insulating oxide film 30. Here, the "chemical oxide film" is an oxide film formed by carrying out a chemical oxidation treatment such as a cleaning agent treatment, and is an example of the "natural oxide film" described in the claims.

[0019] <Semiconductor device manufacturing process> Next, a manufacturing process of the semiconductor device shown in FIG. 1 will be described with reference to FIG. Here, the process of forming the MOS transistor 16 will be omitted, and the process of forming the element isolation trench 54 filled with the silicon oxide 12 will be mainly described. The MOS transistor 16 can be formed by a conventionally known method.

[0020] First, a pad oxide film 50 is formed on the surface of the silicon substrate 10, and then a silicon nitride film 52 is formed by using a CVD method (FIG. 3(A)).

[0021] Next, a resist film (not shown) is applied onto the silicon nitride film 52, and then a resist pattern having an opening corresponding to the element isolation trench 54 is formed by photolithography. Then, using the resist pattern as a mask, the silicon nitride film 52 and the pad oxide film 50 are sequentially etched. Then, using the silicon nitride film 52 and the pad oxide film 50 that remain unetched as a mask, the silicon substrate 10 is etched to form the element isolation trench 54 (FIG. 3(B)).

[0022] Next, the side and bottom surfaces of the element isolation trench 54 are oxidized by thermal oxidation to form a thermal oxide film (not shown). Subsequently, silicon oxide 12 is deposited on the silicon nitride film 52 and in the element isolation trench 54 by high density plasma CVD to fill the element isolation trench 54 with the silicon oxide 12 (FIG. 3(C)).

[0023] Next, the surface of the silicon oxide 12 is planarized by chemical mechanical polishing (CMP) (FIG. 3(D)). Then, the silicon nitride film 52 is removed by wet etching using hot phosphoric acid to expose the pad oxide film 50. Then, after removing the pad oxide film 50 by wet etching using hydrofluoric acid, a sacrificial oxide film 56 is formed on the exposed surface of the silicon substrate 10.

[0024] Next, the silicon oxide 12 in the element isolation trench 54 is etched back to the height of the surface of the silicon substrate 10 by wet etching using hydrofluoric acid. Here, the surface of the silicon oxide 12 that is not covered with the sacrificial oxide film 56 is excessively etched back and becomes lower than the surface of the silicon substrate 10, forming a step. Next, the sacrificial oxide film 56 is removed to expose the surface of the silicon substrate 10 (FIG. 3(F)).

[0025] Next, a cleaning step, which will be described later, is repeated multiple times to clean the surface of the silicon substrate 10 and the surface of the silicon oxide 12. This cleaning removes steps by grinding the corners of the element formation region 14 of the silicon substrate 10. After completion of the cleaning step, a chemical oxide film 32 is formed on the surface of the silicon substrate 10. Finally, an insulating oxide film 30 is formed to a predetermined thickness on the surfaces of the silicon substrate 10 and the silicon oxide 12 (FIG. 3(G)).

[0026] (Cleaning process) Next, the cleaning process will be described with reference to FIGS. 4(A) to 4(F) are enlarged views of the periphery of end 14E of element formation region 14, and show how the corners of end 14E are removed in the cleaning process to form chamfered portion 14R.

[0027] The cleaning process is performed by combining DHF cleaning and HPM cleaning. DHF cleaning is a process that uses dilute hydrofluoric acid (HF / H2O) as a cleaning solution to remove the chemical oxide film on the silicon surface. HPM cleaning is a process that removes metals using a cleaning solution composed of hydrochloric acid, hydrogen peroxide, and pure water in a volumetric ratio of 1:1 to 2:5 to 7. DHF cleaning and HPM cleaning after DHF cleaning constitute one set of cleaning processes, and one set of cleaning processes is performed multiple times.

[0028] Fig. 4(A) shows the state of the boundary between end 14E of element formation region 14 and silicon oxide 12 filling element isolation trench 54 after sacrificial oxide film 56 has been removed in Fig. 3(F). The surface of element formation region 14 is higher than the surface of silicon oxide 12, and a step is formed between element formation region 14 and silicon oxide 12. The surface of element formation region 14 is covered with chemical oxide film 32. In this state, the entire surface of end 14E is flat portion 14T, and the edge of end 14E has a sharp corner due to the step.

[0029] In the first cleaning step, DHF cleaning is first performed. As shown in Fig. 4(B), the DHF cleaning removes the chemical oxide film 32 and also scrapes off the silicon oxide 12, causing the surface of the silicon oxide 12 to recede. The height of the surface of the silicon oxide 12 before the DHF cleaning is indicated by a dotted line. As the surface of the silicon oxide 12 recedes, the exposed portion of the side surface of the element formation region 14 (the wall surface of the element isolation trench 54) increases.

[0030] Next, HPM cleaning is performed. HPM cleaning is usually performed by immersion processing, but in this embodiment, as shown by the arrows in Fig. 4(B), the HPM cleaning solution is sprayed from above toward the surface of the element formation region 14 to clean the surface of the element formation region 14. For the end portion 14E of the element formation region 14, the HPM cleaning solution is sprayed diagonally from above toward the corner.

[0031] The spray angle of the HPM cleaning solution is determined according to the desired inclination of the chamfered portion 14R. For example, if it is desired to incline the slope of the chamfered portion 14R at 45 degrees with respect to the main surface of the substrate, the HPM cleaning solution is sprayed at an angle of 45 degrees with respect to the main surface.

[0032] As a result of this HPM cleaning, as shown in Fig. 4(C), the metallic silicon surface is scraped off, and the surface of the element formation region 14 recedes. In Fig. 4(B), the height of the surface of the silicon oxide 12 in the element formation region 14 after the HPM cleaning is indicated by a dashed line. At the end 14E of the element formation region 14, the corners are scraped off and chamfered to form a curved chamfered portion 14R. In addition, a chemical oxide film 32 is formed on the exposed surface of the element formation region 14. Once the chemical oxide film 32 is formed, it no longer reacts with the HPM cleaning solution.

[0033] The reason why the DHF cleaning and the HPM cleaning are performed as a set is that the silicon of the element formation region 14 does not react with the HPM cleaning solution until the chemical oxide film 32 formed on the surface of the element formation region 14 is removed by the DHF cleaning to expose the silicon surface of the element formation region 14. The HPM cleaning is performed after the DHF cleaning for the same reason.

[0034] In the second cleaning step, DHF cleaning is performed again. As shown in Fig. 4(D), the DHF cleaning removes the chemical oxide film 32 formed in the HPM cleaning, and also scrapes off the silicon oxide 12, causing the surface of the silicon oxide 12 to recede. As the surface of the silicon oxide 12 recede, the exposed portion of the side surface of the element formation region 14 further increases. In addition, the second DHF cleaning removes the silicon chemically oxidized in the HPM cleaning, and thus indirectly scrapes off the silicon surface of the element formation region 14.

[0035] Next, HPM cleaning is performed. As shown in FIG. 4(E), the HPM cleaning removes the silicon surface of the element formation region 14, which is metal, and the surface of the element formation region 14 recedes. At the end 14E of the element formation region 14, the chamfered portion 14R is further rounded, and the flat portion 14T is obliquely removed, increasing the area of ​​the chamfered portion 14R. In addition, a chemical oxide film 32 is formed on the exposed surface of the element formation region 14.

[0036] 4(F), for example, after the fifth cleaning step, a chemical oxide film 32 is formed on the surface of the silicon substrate 10. Finally, an insulating oxide film 30 is formed to a predetermined thickness on the surfaces of the silicon substrate 10 and the silicon oxide 12.

[0037] In this embodiment, one set of cleaning steps is performed multiple times. The part of the element formation region 14 that is exposed from the beginning is scraped off according to the number of times it is subjected to HPM cleaning. By spraying the HPM cleaning liquid from diagonally above, the step part of the end 14E of the element formation region 14 is also scraped off. In addition, the newly exposed part of the side surface of the element formation region 14 is scraped off according to the number of times it is subjected to HPM cleaning after exposure. Therefore, when a cross section of the chamfered portion 14R is viewed along the width direction of the element isolation trench 54, the radius of curvature is small near the boundary between the element formation region 14 and the element isolation trench 54, and the radius of curvature becomes larger as it approaches the flat portion 14T.

[0038] Moreover, the step portion exposed from the beginning is subjected to HPM cleaning many times, and is gradually scraped away and becomes flat. For example, by repeating the cleaning process a number of times less than a threshold, the chamfered portion 14R becomes a gently curved surface as shown in Fig. 2(A), and by repeating the cleaning process a number of times equal to or greater than the threshold, the chamfered portion 14R becomes a gently sloping surface as shown in Fig. 2(B). The threshold is determined according to the cleaning conditions, and can be, for example, 3 to 8 times.

[0039] As described above, in this embodiment, the corners of the end 14E of the element formation region 14 can be chamfered to form a gently curved surface or a gently sloping surface, improving the film-forming properties of the oxide film formed thereon. That is, when an oxide film is formed on the end 14E including the chamfered portion 14R, the variation in thickness of the oxide film can be reduced compared to when an oxide film is formed on a corner. Furthermore, the uniform thickness of the oxide film makes it difficult for electric field concentration to occur, and improves the withstand voltage characteristics.

[0040] Furthermore, the surface of silicon oxide 12 is scraped off by DHF cleaning, and the silicon surface of element formation region 14 is scraped off by HPM cleaning. More specifically, in the second and subsequent DHF cleanings, silicon chemically oxidized in HPM cleaning is removed, and the silicon surface of element formation region 14 is indirectly scraped off. Although exaggerated in FIG. 3, the amount scraped off by cleaning is minute compared to etching. In addition, in HPM cleaning, the surface of element formation region 14 is passivated by the formation of chemical oxide film 32, and erosion by the HPM cleaning solution stops. The next HPM cleaning cannot be performed until chemical oxide film 32 is removed by DHF cleaning. Therefore, the amount scraped off can be adjusted by the number of times the cleaning process is performed.

[0041] Moreover, by performing HPM cleaning from obliquely above, it is possible to chamfer the end 14E of the element formation region 14. The inclination angle of the chamfered portion 14R can be determined by the spray angle of the HPM cleaning solution. Therefore, by setting the conditions for HPM cleaning, it is possible to give the end 14E of the element formation region 14 a desired shape.

[0042] <Modification> The configurations of the semiconductor device and the manufacturing method thereof described in the above embodiment are merely examples, and it goes without saying that the configurations may be changed without departing from the spirit of the present invention.

[0043] In the above embodiment, the structure in which the chamfered portion 14R has a slope with a predetermined inclination (see FIG. 2(B)) is exemplified, but the structure of the chamfered portion 14R is not limited to this. When the chamfered portion 14R has a slope, the chamfered portion 14R may have multiple slopes with different inclinations. In this case, the slopes of the multiple slopes are steep on the boundary side and become gentler as they approach the flat portion 14T.

[0044] In the above embodiment, the case where DHF cleaning and HPM cleaning are performed has been described. However, the first cleaning should be capable of removing a chemical oxide film formed on the surface of the element formation region, and the second cleaning should be capable of scraping off the surface of the semiconductor substrate in the element formation region, and the types of cleaning are not limited to DHF cleaning and HPM cleaning.

[0045] [Additional Notes] The following additional notes are provided in relation to the above-described embodiments. A first aspect of the present disclosure is a semiconductor device comprising: a semiconductor substrate; an element formation region formed on the semiconductor substrate in which semiconductor elements are formed; an element isolation region formed on the semiconductor substrate for isolating the element formation region into individual semiconductor elements; and an oxide film covering the element formation region and the element isolation region, wherein an end of the element formation region adjacent to the element isolation region comprises a flat portion parallel to a main surface of the semiconductor substrate and a chamfered portion that chamfers a step between a surface of the element formation region and a surface of the element isolation region, and the chamfered portion has a shape that, in a cross section taken along the width direction of the element isolation region, increases in height and has an increasing radius of curvature from the boundary between the element formation region and the element isolation region toward the flat portion. A second aspect of the present disclosure is the semiconductor device according to the first aspect, wherein the chamfered portion has a slope with the radius of curvature becoming infinite. A third aspect of the present disclosure is the semiconductor device according to the first or second aspect, wherein the oxide film formed on the element formation region has a two-layer structure of a native oxide film and an insulating oxide film. A fourth aspect of the present disclosure is a method for manufacturing a semiconductor device, comprising the steps of: forming an isolation trench in an isolation region on a semiconductor substrate; filling the isolation trench with a semiconductor oxide; etching the semiconductor oxide filled in the isolation trench; and cleaning a surface of the element formation region and the isolation region on the semiconductor substrate, wherein the cleaning step is performed by a first cleaning step of removing a native oxide film formed on the surface of the element formation region with a first cleaning liquid; and a second cleaning step performed after the first cleaning step of scraping off the surface of the semiconductor substrate in the element formation region with a second cleaning liquid, and when a step occurs between the surface of the element formation region and a surface of the isolation region, in the second cleaning step, the second cleaning step is sprayed from diagonally above onto the step to chamfer the step. A fifth aspect of the present disclosure is the method for producing a semiconductor device according to the fourth aspect, wherein the cleaning step is repeated multiple times. A sixth aspect of the present disclosure is a method for manufacturing a semiconductor device according to the fourth or fifth aspect, wherein the cleaning step is repeated multiple times until a chamfered portion formed by chamfering the step portion has a shape that, in a cross section along the width direction of the element isolation region, increases in height and has an increasing radius of curvature from the boundary with the element isolation region toward the center. A seventh aspect of the present disclosure is a method for manufacturing a semiconductor device according to the fourth or fifth aspect, wherein the cleaning step is repeated multiple times until a chamfered portion formed by chamfering the step portion has a shape including a slope whose height and radius of curvature become larger from the boundary with the element isolation region toward the center in a cross section along the width direction of the element isolation region, with the radius of curvature becoming infinite. An eighth aspect of the present disclosure is a method for manufacturing a semiconductor device according to any one of the fourth to seventh aspects, wherein the first cleaning is a DHF cleaning using dilute hydrofluoric acid as the first cleaning liquid, and the second cleaning is a HPM cleaning using a mixture of hydrochloric acid, hydrogen peroxide, and water as the second cleaning liquid. A ninth aspect of the present disclosure is a method for manufacturing a semiconductor device according to any one of the fourth to eighth aspects, further comprising, after completion of the cleaning step, a step of forming an insulating oxide film on the element isolation region and on the element formation region on which a native oxide film has been formed by the second cleaning. [Explanation of symbols]

[0046] 10 Silicon substrate 12 Silicon oxide 14 Device formation area 14E End 14R chamfered part 14T flat part 16 Transistors 18 wells 20 Gate electrode 22 Channel Region 24 Source Region 26 Drain Region 28 Gate insulating film 30 Insulating oxide film (oxide film) 32 Chemical Oxide Film 50 Pad oxide film 52 Silicon nitride film 54 Isolation Groove 56 Sacrificial oxide film

Claims

1. A semiconductor substrate; an element formation region formed on the semiconductor substrate in which a semiconductor element is formed; an element isolation region formed on the semiconductor substrate, which isolates the element formation region for each semiconductor element; an oxide film covering the element formation region and the element isolation region; Equipped with an end portion of the element formation region adjacent to the element isolation region includes a flat portion parallel to a main surface of the semiconductor substrate and a chamfered portion that chamfers a step between a surface of the element formation region and a surface of the element isolation region; the chamfered portion has a shape in which, in a cross section along a width direction of the element isolation region, the height increases and the radius of curvature increases from a boundary between the element formation region and the element isolation region toward the flat portion. Semiconductor device.

2. The semiconductor device according to claim 1 , wherein said chamfered portion has a slope where said radius of curvature becomes infinite.

3. 3. The semiconductor device according to claim 1, wherein the oxide film formed on the element formation region has a two-layer structure consisting of a native oxide film and an insulating oxide film.

4. forming an isolation trench in an isolation region on a semiconductor substrate; filling the isolation trenches with a semiconductor oxide; Etching the semiconductor oxide filled in the isolation trench; cleaning surfaces of an element formation region and an element isolation region on the semiconductor substrate; Including, the cleaning step includes a first cleaning step of removing a native oxide film formed on the surface of the element formation region with a first cleaning solution, and a second cleaning step of scraping off the surface of the semiconductor substrate in the element formation region with a second cleaning solution and forming a native oxide film on the exposed surface of the semiconductor substrate in the element formation region, which is performed after the first cleaning step; When a step portion is formed between a surface of the element formation region and a surface of the element isolation region, the second cleaning includes spraying the second cleaning liquid obliquely from above onto the step portion to chamfer the step portion. A method for manufacturing a semiconductor device.

5. The washing step is repeated multiple times. The method for manufacturing a semiconductor device according to claim 4 .

6. repeating the cleaning step a number of times until a chamfered portion formed by chamfering the step portion has a shape in which the height increases and the radius of curvature increases from the boundary with the element isolation region toward the center in a cross section along the width direction of the element isolation region; The method for manufacturing a semiconductor device according to claim 4 .

7. repeating the cleaning step a number of times until a chamfered portion formed by chamfering the step portion has a shape including a slope whose height and radius of curvature become larger from the boundary with the element isolation region toward the center in a cross section along the width direction of the element isolation region, and whose radius of curvature becomes infinite; The method for manufacturing a semiconductor device according to claim 4 .

8. The first cleaning is a DHF cleaning using dilute hydrofluoric acid as the first cleaning liquid, The second cleaning is an HPM cleaning using a mixture of hydrochloric acid, hydrogen peroxide, and water as the second cleaning liquid. The method for manufacturing a semiconductor device according to any one of claims 4 to 7.

9. The method further includes, after the cleaning step is completed, a step of forming an insulating oxide film on the element isolation region and on the element formation region on which the native oxide film has been formed by the second cleaning. The method for manufacturing a semiconductor device according to claim 4 .

Citation Information

Patent Citations

  • Manufacture of semiconductor device

    JP2000021970A