Epoxy resin, curable resin composition, and cured product of the same
A novel epoxy resin with controlled alkyl groups and a curable resin composition addresses the need for low water absorption and low dielectric loss tangent, enhancing semiconductor encapsulation and composite materials with improved mechanical and electrical properties.
Patent Information
- Application Number
- JP2023046178
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-23
AI Technical Summary
Existing epoxy resins do not adequately address the need for low water absorption, high heat resistance, and low dielectric loss tangent, which are crucial for advanced semiconductor encapsulation and substrates with thinner layers and complex structures.
A novel epoxy resin represented by specific chemical formulas with controlled alkyl groups and epoxidation methods, combined with a curable resin composition and curing agents, to achieve low water absorption and low dielectric loss tangent properties.
The resulting cured product exhibits excellent low water absorption, high heat resistance, and low dielectric loss tangent, making it suitable for high-reliability semiconductor sealing materials and composite materials with improved mechanical and electrical properties.
Smart Images

Figure 2024135479000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an epoxy resin, a curable resin composition, and a cured product thereof. [Background technology]
[0002] Epoxy resins have excellent electrical, mechanical, adhesive and thermal properties and are therefore widely used in the electrical and electronic fields, including in cast products, laminates and IC encapsulation materials, as well as in structural materials, adhesives and paints.
[0003] In recent years, in the electrical and electronic fields, there has been a demand for further improvements in various properties of resin compositions, such as improved flame retardancy, moisture resistance, adhesion, and dielectric properties, high purity, low viscosity for high filling of fillers (inorganic or organic fillers), and improved reactivity for shortening molding cycles (Patent Document 1). In addition, as structural materials, lightweight materials with excellent mechanical properties are required for aerospace materials, leisure and sports equipment applications, etc. In particular, in the semiconductor encapsulation field and substrates (the substrates themselves, or their peripheral materials), semiconductors have become more complex, becoming thinner, stacked, systemized, and three-dimensional, with the evolution of the semiconductors, and properties such as extremely high levels of heat resistance, low water absorption, and low dielectric loss tangent are required. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-147854 A Summary of the Invention [Problem to be solved by the invention]
[0005] In view of the above problems, an object of the present invention is to provide an epoxy resin which provides a cured product having low water absorption, high heat resistance and a low dielectric tangent, and a curable resin composition containing the same. [Means for solving the problem]
[0006] That is, the present invention relates to the following [1] to [5]. Note that in this application, "(Numerical value 1) to (Numerical value 2)" indicates that the upper and lower limits are included. [1] An epoxy resin represented by the following formula (1).
[0007] [ka]
[0008] (In formula (1), each of the multiple R's independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. Each of the multiple p's independently represents an integer of 0 to 4. q represents an integer of 0 to 9.) [2] An epoxy resin represented by the following formula (2).
[0009] [ka]
[0010] [3] A curable resin composition comprising the epoxy resin according to the above item [1] or [2]. [4] The curable resin composition according to the above item [3], further comprising a curing agent or a curing accelerator. [5] A cured product obtained by curing the curable resin composition described in the above item [3]. Effect of the Invention
[0011] According to the present invention, it is possible to provide an epoxy resin whose cured product has low water absorption, high heat resistance, and low dielectric tangent, and a curable resin composition containing the same. Therefore, the epoxy resin of the present invention is useful for insulating materials for electric and electronic components (highly reliable semiconductor encapsulation materials, etc.), laminates (printed wiring boards, build-up boards, etc.), various composite materials including CFRP, adhesives, paints, etc. [Brief description of the drawings]
[0012] [Figure 1] 1 shows a GC-MS chart of Example 1. [Diagram 2] 1 shows a 1H-NMR chart of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The epoxy resin of the present embodiment is represented by the following formula (1).
[0014] [ka]
[0015] (In formula (1), each of the multiple R's independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. Each of the multiple p's independently represents an integer of 0 to 4. q represents an integer of 0 to 9.)
[0016] In formula (1), R represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, still more preferably a hydrogen atom or a methyl group, and particularly preferably a hydrogen atom. p represents an integer of 0 to 4, more preferably an integer of 0 to 2, and still more preferably 0. q represents an integer of 0 to 9, more preferably an integer of 0 to 7, still more preferably an integer of 0 to 5, and particularly preferably 0. When q is 9, this indicates that all hydrogen atoms in the fluorene ring are substituted.
[0017] The epoxy resin represented by the formula (1) can be in the form of a semi-solid to solid resin at room temperature. In this case, the softening point is preferably 120° C. or less, and more preferably 100° C. or less. If the softening point is higher than 120° C., the viscosity is high and the fiber impregnation property is reduced during the preparation of the prepreg.
[0018] The epoxy equivalent of the epoxy resin represented by the formula (1) is preferably 200 to 1000 g / eq, more preferably 220 to 800 g / eq, particularly preferably 240 to 700 g / eq, and most preferably 245 to 600 g / eq.
[0019] The ICI viscosity of the epoxy resin represented by the formula (1) at 150° C. is preferably 0.01 to 1.2 Pa s, more preferably 0.01 to 1.0 Pa s, and even more preferably 0.01 to 0.8 Pa s. If it is within the above range, it is possible to ensure appropriate fluidity as an encapsulant when it is made into an encapsulant composition.
[0020] An example of a preferred structure of the epoxy resin represented by the above formula (1) is an epoxy resin represented by the following formula (2).
[0021] [ka]
[0022] The method for producing the epoxy resin of the present embodiment is not particularly limited, but for example, the epoxy resin can be obtained by subjecting a phenolic resin represented by the following formula (3) to an addition or ring-closing reaction with epihalohydrin in the presence of a solvent and a catalyst. The amount of epihalohydrin used is preferably 1.0 to 20.0 mol, more preferably 1.5 to 10.0 mol, per mol of phenolic hydroxyl group of the phenolic resin.
[0023] [ka]
[0024] In formula (3), the values and preferred ranges of R, p, and q are the same as those in formula (1) above.
[0025] Examples of alkali metal hydroxides that can be used in the epoxidation reaction include sodium hydroxide and potassium hydroxide. The alkali metal hydroxide may be a solid or an aqueous solution thereof. When an aqueous solution is used, the aqueous solution of the alkali metal hydroxide may be continuously added to the reaction system, and water and epihalohydrin may be continuously distilled under reduced pressure or normal pressure, and water may be removed by liquid separation, and epihalohydrin may be continuously returned to the reaction system. The amount of the alkali metal hydroxide used is preferably 0.9 to 2.5 moles, more preferably 0.95 to 1.5 moles, per mole of the phenolic hydroxyl group of the phenolic resin. If the amount of the alkali metal hydroxide used is small, the reaction does not proceed sufficiently. On the other hand, excessive use of the alkali metal hydroxide exceeding 2.5 moles per mole of the phenolic hydroxyl group of the phenolic resin leads to unnecessary by-production of waste.
[0026] In order to promote the above reaction, a quaternary ammonium salt such as tetramethylammonium chloride, tetramethylammonium bromide, or trimethylbenzylammonium chloride may be added as a catalyst. The amount of the quaternary ammonium salt used is usually 0.1 to 15 g, and preferably 0.2 to 10 g, per mole of the phenolic hydroxyl group of the phenolic resin. If the amount used is too small, a sufficient reaction promotion effect cannot be obtained, and if the amount used is too large, the amount of the quaternary ammonium salt remaining in the epoxy resin increases, which may cause deterioration of electrical reliability.
[0027] In the epoxidation reaction, it is preferable to add alcohols such as methanol, ethanol, and isopropyl alcohol, and aprotic polar solvents such as dimethyl sulfone, dimethyl sulfoxide, tetrahydrofuran, and dioxane to proceed with the reaction. When using alcohols, the amount of alcohol used is preferably 2 to 50% by weight, more preferably 4 to 20% by weight, based on the amount of epihalohydrin used. When using aprotic polar solvents, the amount of alcohol used is preferably 5 to 100% by weight, more preferably 10 to 80% by weight, based on the amount of epihalohydrin used. The reaction temperature is preferably 30 to 90°C, more preferably 35 to 80°C. The reaction time is preferably 0.5 to 100 hours, more preferably 1 to 30 hours. After the reaction is completed, the reaction product is washed with water or heated under reduced pressure to remove epihalohydrin and solvent. In order to obtain an epoxy resin with a smaller amount of hydrolyzable halogen, the recovered epoxy resin can be dissolved in a solvent such as toluene or methyl isobutyl ketone, and an aqueous solution of an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide is added to the epoxy resin to ensure ring closure. In this case, the amount of the alkali metal hydroxide used is preferably 0.01 to 0.3 mol, more preferably 0.05 to 0.2 mol, per mol of the phenolic hydroxyl group of the phenolic resin used for glycidylation. The reaction temperature is preferably 50 to 120° C., and the reaction time is preferably 0.5 to 24 hours. After the reaction is completed, the salt formed is removed by filtration, washing with water, etc., and the solvent is further distilled off under reduced pressure with heating to obtain the epoxy resin of this embodiment.
[0028] Next, a method for producing the phenolic resin represented by the formula (3) will be described. The method for producing the phenolic resin represented by the formula (3) is not particularly limited, but for example, the phenolic resin can be obtained by reacting an acetylfluorene compound with a phenolic compound under an acid catalyst such as hydrochloric acid. In this case, the substituent of the phenolic compound is preferably unsubstituted or has an alkyl group having 1 to 5 carbon atoms, and from the viewpoint of improving heat resistance, it is more preferable that the substituent is unsubstituted or has an alkyl group having 1 to 3 carbon atoms. In the synthesis, as an acid catalyst, hydrochloric acid, phosphoric acid, sulfuric acid, formic acid, p-toluenesulfonic acid, methanesulfonic acid, Lewis acids such as aluminum chloride and zinc chloride, activated clay, acidic clay, white carbon, zeolite, silica alumina, solid acids, acidic ion exchange resins, etc. can be used. These may be used alone or in combination of two or more. The amount of the catalyst used is preferably 1 to 200% by weight, more preferably 50% by weight, based on the total weight of the fluorene compound and the phenolic compound as the reaction substrates. If the amount of catalyst used is too large, there is a risk of unnecessary waste increasing, and if the amount is too small, there is a risk of the reaction proceeding slowly. The reaction may be carried out using an organic solvent such as toluene or xylene as necessary, or may be carried out without a solvent. Examples of the solvent used include, but are not limited to, non-water-soluble solvents such as aromatic solvents such as toluene or xylene, aliphatic solvents such as cyclohexane or n-hexane, ethers such as diethyl ether or diisopropyl ether, ester solvents such as ethyl acetate or butyl acetate, and ketone solvents such as methyl isobutyl ketone or cyclopentanone, and two or more types may be used in combination. In addition to the non-water-soluble solvent, an aprotic polar solvent may also be used in combination. Examples include dimethyl sulfone, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, 1,3-dimethyl-2-imidazolidinone, and N-methylpyrrolidone, and two or more types may be used in combination. When an aprotic polar solvent is used, it is preferable to use one with a higher boiling point than the non-water-soluble solvent used in combination. The reaction temperature is preferably from 20 to 120°C, more preferably from 30 to 110°C, and further preferably from 40 to 100°C.After the reaction is complete, the acid catalyst is neutralized with an alkaline aqueous solution or the like, and then a non-water-soluble organic solvent is added to the oil layer and the wastewater is repeatedly washed with water until it becomes neutral, after which the solvent is removed under heating and reduced pressure. When activated clay or ion exchange resin is used, the reaction liquid is filtered after the reaction is complete to remove the catalyst.
[0029] An example of a preferred structure of the phenol resin represented by the above formula (3) is a phenol resin represented by the following formula (4).
[0030] [ka]
[0031] The curable resin composition of the present embodiment will be described below. In the curable resin composition of the present embodiment, the epoxy resin represented by the formula (1) can be used alone or in combination with other epoxy resins. When used in combination, the ratio of the epoxy resin represented by the formula (1) to the total epoxy resin is preferably 10 to 98% by weight, more preferably 20 to 95% by weight, and even more preferably 30 to 95% by weight. By making the amount added 10% or more, it is possible to achieve low dielectric tangent, high heat resistance, low water absorption, high elastic modulus, and high fluidity.
[0032] Specific examples of other epoxy resins that can be used in combination with the epoxy resin of the present embodiment include polycondensates of bisphenols (bisphenol A, bisphenol F, bisphenol S, biphenol, bisphenol AD, etc.) or phenols (phenol, alkyl-substituted phenol, aromatic-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) with various aldehydes (formaldehyde, acetaldehyde, alkyl aldehyde, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.); polycondensates of the phenols and various diene compounds (dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinylnorbornene, tetrahydroindene, divinylbenzene, divinylbiphenyl, disopropene, etc.); Examples of the epoxy resins include polymers of the phenols and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzophenone, etc.); polycondensates of the phenols and aromatic dimethanols (benzene dimethanol, biphenyl dimethanol, etc.); polycondensates of the phenols and aromatic dichloromethyls (α,α'-dichloroxylene, bischloromethyl biphenyl, etc.); polycondensates of the phenols and aromatic bisalkoxymethyls (bismethoxymethylbenzene, bismethoxymethyl biphenyl, bisphenoxymethyl biphenyl, etc.); polycondensates of the bisphenols and various aldehydes or glycidyl alcohols, glycidyl ether epoxy resins, alicyclic epoxy resins, glycidyl amine epoxy resins, glycidyl ester epoxy resins, etc., but are not limited to these, so long as they are commonly used epoxy resins. These may be used alone or in combination of two or more.
[0033] Curing agents that can be used in the curable resin composition of the present embodiment include amine-based curing agents, acid anhydride-based curing agents, amide-based curing agents, phenol-based curing agents, etc. Specific examples of curing agents that can be used include o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenylsulfone, 3,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, 2,2'-diaminodiphenylsulfone, diethyltoluenediamine, dimethylthiotoluenediamine, diaminodiphenylmethane, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, ... ,4'-Diamino-3,3'-diethyl-5,5'-dimethyldiphenylmethane, 4,4'-Diamino-3,3',5,5'-tetramethyldiphenylmethane, 4,4'-Diamino-3,3',5,5'-tetraethyldiphenylmethane, 4,4'-Diamino-3,3',5,5'-tetraisopropyldiphenylmethane, 4,4'-Methylenebis(N-methylaniline), Bis(aminophenyl)fluorene, 3,4'-Diaminodiphenyl ether, 4,4'-Diaminodiphenyl ether, 2,2'-Bis [4-(4-aminophenoxy)phenyl]propane, bis[4-(4-aminophenoxy)phenyl]sulfone, 1,3'-bis(4-aminophenoxy)benzene, 1,4'-bis(4-aminophenoxy)benzene, 1,4'-bis(4-aminophenoxy)biphenyl, 4,4'-(1,3-phenylenediisopropylidene)bisaniline, 4,4'-(1,4-phenylenediisopropylidene)bisaniline, naphthalenediamine, benzidine, dimethylbenzidine, WO 2017 / 170551 Examples of the aromatic amine compounds include the aromatic amine compounds described in Synthesis Examples 1 and 2, and aliphatic amines such as 1,3-bis(aminomethyl)cyclohexane, isophoronediamine, 4,4'-methylenebis(cyclohexylamine), norbornanediamine, ethylenediamine, propanediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, dimer diamine, and triethylenetetramine, but are not limited to these. These can be suitably used depending on the properties that are desired to be imparted to the composition.To ensure pot life, it is preferable to use aromatic amines, and to impart quick curing properties, it is preferable to use aliphatic amines. By using an amine compound containing a bifunctional component as the main component as a curing agent, a highly linear network can be constructed during the curing reaction, and particularly excellent toughness can be expressed.Further, amide compounds such as dicyandiamide and polyamide resins synthesized from a dimer of linolenic acid and ethylenediamine; acid anhydride compounds such as phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, and methylhexahydrophthalic anhydride; bisphenols (bisphenol A, bisphenol F, bisphenol S, biphenol, bisphenol AD, etc.) or phenols (phenols) Polycondensates of phenols, alkyl-substituted phenols, aromatic substituted phenols, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) and various aldehydes (formaldehyde, acetaldehyde, alkyl aldehyde, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.), or polycondensates of the above phenols and various dienes Polymers of the phenols and compounds (dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinylnorbornene, tetrahydroindene, divinylbenzene, divinylbiphenyl, disopropenylbiphenyl, butadiene, isoprene, etc.), or polycondensates of the phenols and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzophenone, etc.), or polycondensates of the phenols and aromatic dimethanols (benzene dimethanol, biphenyl dimethanol, etc.), Alternatively, polycondensates of the phenols and aromatic dichloromethyls (α,α'-dichloroxylene, bischloromethylbiphenyl, etc.), polycondensates of the phenols and aromatic bisalkoxymethyls (bismethoxymethylbenzene, bismethoxymethylbiphenyl, bisphenoxymethylbiphenyl, etc.), polycondensates of the bisphenols and various aldehydes, and phenolic compounds such as modified products thereof; trifluoroborane-amine complexes, guanidine derivatives, etc. may be mentioned, but are not limited to these. In addition, the phenolic resin represented by the formula (3) and the phenolic resin represented by the formula (4) may also be used as a curing agent.
[0034] In the curable resin composition of the present embodiment, the amount of the curing agent used is preferably 0.5 to 1.5 equivalents, and particularly preferably 0.6 to 1.2 equivalents, relative to 1 equivalent of the epoxy group of the epoxy resin. By using 0.5 to 1.5 equivalents, good curing properties can be obtained.
[0035] When the curing reaction is carried out using the above curing agent, a curing accelerator may be used in combination. Examples of the curing accelerator that can be used include imidazoles such as 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, and 2-ethyl-4-methylimidazole, tertiary amines such as 2-(dimethylaminomethyl)phenol, triethylenediamine, triethanolamine, and 1,8-diazabicyclo(5,4,0)undecene-7, phosphines such as triphenylphosphine, tri(tolyl)phosphine, tetraphenylphosphonium bromide, and tetraphenylphosphonium tetraphenylborate, and phosphonic acids such as phosphines and phosphines. Examples of the curing accelerator include tetraphenylboron salts such as tetraphenylboron salts, tetraphenylboron salts, and carboxylic acid compounds such as benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, naphthoic acid, and salicylic acid. Carboxylic acid compounds such as salicylic acid are preferred from the viewpoint of promoting the curing reaction between the amine compound and the epoxy resin. The curing accelerator is used in an amount of 0.01 to 15 parts by weight per 100 parts by weight of the epoxy resin, as required.
[0036] Furthermore, an inorganic filler can be added to the curable resin composition of the present embodiment as necessary. Examples of inorganic fillers include, but are not limited to, powders such as crystalline silica, fused silica, alumina, zircon, calcium silicate, calcium carbonate, silicon carbide, silicon nitride, boron nitride, zirconia, fosterite, steatite, spinel, titania, and talc, or beads obtained by sphering these. These may be used alone or in combination. The amount of these inorganic fillers varies depending on the application, but when used as a semiconductor sealant, it is preferable to use them in a proportion of 20% by weight or more in the curable resin composition from the standpoint of heat resistance, moisture resistance, mechanical properties, and flame retardancy of the cured product of the curable resin composition, more preferably 30% by weight or more, and even more preferably 70 to 95% by weight in order to improve the linear expansion coefficient with the lead frame.
[0037] The curable resin composition of the present embodiment may contain a mold release agent to improve release from the mold during molding. Any of the conventionally known mold release agents may be used, including, for example, ester waxes such as carnauba wax and montan wax, fatty acids such as stearic acid and palmitic acid and their metal salts, and polyolefin waxes such as oxidized polyethylene and non-oxidized polyethylene. These may be used alone or in combination of two or more. The amount of these mold release agents is preferably 0.5 to 3% by weight based on the total organic components. If the amount is less than this, release from the mold is poor, and if the amount is too much, adhesion to a lead frame or the like is poor.
[0038] The curable resin composition of the present embodiment can be blended with a coupling agent to enhance the adhesion between the inorganic filler and the resin component. Any of the conventionally known coupling agents can be used, including, for example, various alkoxysilane compounds such as vinylalkoxysilane, epoxyalkoxysilane, styrylalkoxysilane, methacryloxyalkoxysilane, acryloxyalkoxysilane, aminoalkoxysilane, mercaptoalkoxysilane, and isocyanatoalkoxysilane, alkoxytitanium compounds, and aluminum chelates. These may be used alone or in combination of two or more. The method of adding the coupling agent may involve treating the inorganic filler surface with the coupling agent in advance and then kneading it with the resin, or mixing the coupling agent with the resin and then kneading the inorganic filler.
[0039] Furthermore, the curable resin composition of the present embodiment may contain known additives as necessary.Specific examples of additives that can be used include polybutadiene and its modified products, modified products of acrylonitrile copolymers, polyphenylene ether, polystyrene, polyethylene, polyimide, fluororesin, maleimide-based compounds, cyanate ester-based compounds, silicone gel, silicone oil, and colorants such as carbon black, phthalocyanine blue, and phthalocyanine green.Specific examples of preferred compounds are listed below, but are not limited to these.
[0040] Polyphenylene ether compound: Any known polyphenylene ether compound may be used, but from the viewpoint of heat resistance and electrical properties, it is preferable to use a polyphenylene ether compound having an ethylenically unsaturated double bond, and more preferable to use a polyphenylene ether compound having an acrylic group, a methacrylic group, or a styrene structure. Commercially available products include SA-9000-111 (manufactured by SABIC, a polyphenylene ether compound having a methacrylic group) and OPE-2St 1200 (manufactured by Mitsubishi Gas Chemical, a polyphenylene ether compound having a styrene structure). The number average molecular weight (Mn) of the polyphenylene ether compound is preferably 500 to 5000, more preferably 2000 to 5000, and more preferably 2000 to 4000. If the molecular weight is less than 500, the heat resistance of the cured product tends to be insufficient. If the molecular weight is more than 5000, the melt viscosity increases and sufficient fluidity cannot be obtained, which tends to lead to molding defects. In addition, the reactivity decreases, the curing reaction takes a long time, and the amount of unreacted material that is not incorporated into the curing system increases, which decreases the glass transition temperature of the cured product and tends to decrease the heat resistance of the cured product. If the number average molecular weight of the polyphenylene ether compound is 500 to 5000, it is possible to exhibit excellent heat resistance, moldability, etc. while maintaining excellent dielectric properties. The number average molecular weight here can be specifically measured using gel permeation chromatography, etc.
[0041] The polyphenylene ether compound may be one obtained by a polymerization reaction, or one obtained by a redistribution reaction of a high molecular weight polyphenylene ether compound having a number average molecular weight of about 10,000 to 30,000. In addition, these may be used as raw materials and reacted with a compound having an ethylenically unsaturated double bond, such as methacryl chloride, acrylic chloride, or chloromethylstyrene, to impart radical polymerizability. The polyphenylene ether compound obtained by the redistribution reaction is obtained, for example, by heating a high molecular weight polyphenylene ether compound in a solvent such as toluene in the presence of a phenolic compound and a radical initiator to cause a redistribution reaction. The polyphenylene ether compound obtained by the redistribution reaction in this way has hydroxyl groups derived from a phenolic compound that contributes to curing at both ends of the molecular chain, and is therefore preferable in that it can maintain even higher heat resistance, and that functional groups can be introduced at both ends of the molecular chain even after modification with a compound having an ethylenically unsaturated double bond. In addition, the polyphenylene ether compound obtained by the polymerization reaction is preferable in that it exhibits excellent fluidity.
[0042] The molecular weight of the polyphenylene ether compound can be adjusted by adjusting the polymerization conditions, etc., in the case of a polyphenylene ether compound obtained by a polymerization reaction. In addition, in the case of a polyphenylene ether compound obtained by a redistribution reaction, the molecular weight of the obtained polyphenylene ether compound can be adjusted by adjusting the conditions of the redistribution reaction, etc. More specifically, it is possible to adjust the amount of the phenolic compound used in the redistribution reaction. That is, the greater the amount of the phenolic compound, the lower the molecular weight of the obtained polyphenylene ether compound. In this case, poly(2,6-dimethyl-1,4-phenylene ether) and the like can be used as the high molecular weight polyphenylene ether compound that undergoes the redistribution reaction. In addition, the phenolic compound used in the redistribution reaction is not particularly limited, but for example, a multifunctional phenolic compound having two or more phenolic hydroxyl groups in the molecule, such as bisphenol A, phenol novolac, cresol novolac, etc., is preferably used. These may be used alone or in combination of two or more.
[0043] The content of the polyphenylene ether compound is not particularly limited, but is preferably 10 to 90% by weight, more preferably 20 to 80% by weight, based on the total weight of the curable resin components. A polyphenylene ether compound content of 10 to 90% by weight is preferable in that a cured product is obtained that is not only excellent in heat resistance, but also fully exhibits the excellent dielectric properties of the polyphenylene ether compound.
[0044] Active alkene-containing resin: a polycondensate of the above-mentioned phenol resin and an active alkene-containing halogen-based compound (chloromethylstyrene, allyl chloride, methallyl chloride, acrylic acid chloride, allyl chloride, etc.), a polycondensate of an active alkene-containing phenol (2-allylphenol, 2-propenylphenol, 4-allylphenol, 4-propenylphenol, eugenol, isoeugenol, etc.) and a halogen-based compound (4,4'-bis(methoxymethyl)-1,1'-biphenyl, 1,4-bis(chloromethyl)benzene, 4,4'-difluorobenzophenone, 4,4'-dichlorobenzophenone, 4,4'-dibromobenzophenone, cyanuric chloride, etc.), an epoxy resin or an alcohol Polycondensates of substituted or unsubstituted acrylates (acrylates, methacrylates, etc.), maleimide resins (4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, m-phenylene bismaleimide, 2,2'-bis[4-(4-maleimidophenoxy)phenyl]propane, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 4,4'-diphenylether bismaleimide, 4,4'-diphenylsulfone bismaleimide, 1,3-bis(3-maleimidophenoxy)benzene, 1,3-bis(4-maleimidophenoxy)benzene), Xylox type maleimide resins (anilix Maleimide, manufactured by Mitsui Chemicals Fine Co., Ltd.) Biphenylaralkyl-type maleimide resin (solidified by distilling off the solvent from a resin solution containing the maleimide resin (M2) described in Example 4 of JP 2009-001783 A under reduced pressure) Bisaminocumylbenzene-type maleimide (maleimide resin described in WO 2020 / 054601 A).
[0045] Isocyanate resins: aromatic diisocyanates such as p-phenylene diisocyanate, m-phenylene diisocyanate, p-xylylene diisocyanate, m-xylylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and naphthalene diisocyanate; aliphatic or alicyclic diisocyanates such as isophorone diisocyanate, hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, hydrogenated xylene diisocyanate, norbornene diisocyanate, and lysine diisocyanate; polyisocyanates such as one or more biuret forms of isocyanate monomers or isocyanate forms obtained by trimerizing the above diisocyanate compounds; and polyisocyanates obtained by a urethanization reaction between the above isocyanate compounds and polyol compounds.
[0046] Polyamide resins: amino acids (6-aminocaproic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, p-aminomethylbenzoic acid, etc.), lactams (ε-caprolactam, ω-undecanelactam, ω-laurolactam), and aliphatic diamines such as diamines (ethylenediamine, trimethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decanediamine, undecanediamine, dodecanediamine, tridecanediamine, tetradecanediamine, pentadecanediamine, hexadecanediamine, heptadecanediamine, octadecanediamine, nonadecanediamine, eicosanediamine, 2-methyl-1,5-diaminopentane, 2-methyl-1,8-diaminooctane, etc. Polymers made primarily from one or more of the following: alicyclic diamines such as cyclohexanediamine, bis-(4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)methane; aromatic diamines such as xylylenediamine; and mixtures of dicarboxylic acids (aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, and dodecanedioic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodiumsulfoisophthalic acid, hexahydroterephthalic acid, and hexahydroisophthalic acid; alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid; dialkyl esters of these dicarboxylic acids, and dichlorides).
[0047] Polyimide resin: the above diamine and tetracarboxylic dianhydride (4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-cyclohexene-1,2 dicarboxylic anhydride, pyromellitic dianhydride, 1,2,3,4-benzenetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4, 4'-Diphenylsulfonetetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, methylene-4,4'-diphthalic dianhydride, 1,1-ethylidene-4,4'-diphthalic dianhydride, 2,2'-propylidene-4,4'-diphthalic dianhydride, 1,2-ethylene-4,4'-diphthalic dianhydride, 1,3-trimethylene-4,4'-diphthalic dianhydride, 1,4-tetramethylene-4,4'-diphthalic dianhydride, 1,5-pentamethylene-4,4'-diphthalic dianhydride, 4,4'-oxydiphthalic dianhydride , thio-4,4'-diphthalic dianhydride, sulfonyl-4,4'-diphthalic dianhydride, 1,3-bis(3,4-dicarboxyphenyl)benzene dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,3-bis[2-(3,4-dicarboxyphenyl)-2-propyl]benzene dianhydride, 1,4-bis[2-(3,4-dicarboxyphenyl)-2-propyl]benzene dianhydride, bis[3-(3,4-dicarboxyphenoxy)phenyl]methane dianhydride , bis[4-(3,4-dicarboxyphenoxy)phenyl]methane dianhydride, 2,2-bis[3-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, bis(3,4-dicarboxyphenoxy)dimethylsilane dianhydride, 1,3-bis(3,4-dicarboxyphenyl)-1,1,3,3-tetramethyldisiloxane dianhydride, 2,3,6,7-naphthalenetetracarboxylic acid dianhydride, 1,4,5,8-naphthalenetetracarboxylic acid dianhydride, 1,2,5,6-Naphthalenetetracarboxylic dianhydride, 3,4,9,10-Perylenetetracarboxylic dianhydride, 2,3,6,7-Anthracenetetracarboxylic dianhydride, 1,2,7,8-Phenanthrenetetracarboxylic dianhydride, Ethylenetetracarboxylic dianhydride, 1,2,3,4-Butanetetracarboxylic dianhydride, 1,2,3,4-Cyclobutanetetracarboxylic dianhydride, Cyclopentanetetracarboxylic dianhydride, Cyclohexane-1,2,3,4-tetracarboxylic dianhydride , cyclohexane-1,2,4,5-tetracarboxylic dianhydride, 3,3',4,4'-bicyclohexyltetracarboxylic dianhydride, carbonyl-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, methylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, 1,2-ethylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, 1,1-ethylidene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, 2,2-Propylidene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, oxy-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, thio-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, sulfonyl-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, bicyclo[2,2,2]oct-7-ene-2,3,5,6-tetracarboxylic acid dianhydride, rel-[1S,5R,6R]-3-oxabicyclo[3 ,2,1]Octane-2,4-dione-6-spiro-3'-(tetrahydrofuran-2',5'-dione), 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride, ethylene glycol-bis-(3,4-dicarboxylic anhydride phenyl) ether, 4,4'-biphenyl bis(trimellitic acid monoester acid anhydride), 9,9'-bis(3,4-dicarboxyphenyl)fluorene dianhydride) polycondensate.
[0048] Cyanate ester resin: A cyanate ester compound obtained by reacting a phenolic resin with a cyanogen halide. Specific examples include, but are not limited to, dicyanatobenzene, tricyanatobenzene, dicyanatonaphthalene, dicyanatobiphenyl, 2,2'-bis(4-cyanatophenyl)propane, bis(4-cyanatophenyl)methane, bis(3,5-dimethyl-4-cyanatophenyl)methane, 2,2'-bis(3,5-dimethyl-4-cyanatophenyl)propane, 2,2'-bis(4-cyanatophenyl)ethane, 2,2'-bis(4-cyanatophenyl)hexafluoropropane, bis(4-cyanatophenyl)sulfone, bis(4-cyanatophenyl)thioether, phenol novolac cyanate, and phenol-dicyclopentadiene co-condensates in which the hydroxyl groups have been converted to cyanate groups. Furthermore, the cyanate ester compound, the synthesis method of which is described in JP-A-2005-264154, is particularly preferred as the cyanate ester compound since it has excellent low moisture absorption, flame retardancy, and low dielectric properties. The cyanate ester resin may contain a catalyst such as zinc naphthenate, cobalt naphthenate, copper naphthenate, lead naphthenate, zinc octoate, tin octoate, lead acetylacetonate, dibutyltin maleate, etc., to trimerize the cyanate group and form a sym-triazine ring, if necessary. The catalyst is usually used in an amount of 0.0001 to 0.10 parts by weight, preferably 0.00015 to 0.0015 parts by weight, per 100 parts by weight of the total weight of the curable resin composition.
[0049] Active ester resin: A compound having one or more active ester groups in one molecule can be used as a curing agent for the curable resin composition of this embodiment, if necessary. As the active ester resin, a compound having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, is preferred. The active ester resin is preferably one obtained by a condensation reaction between at least one compound of a carboxylic acid compound and a thiocarboxylic acid compound and at least one compound of a hydroxy compound and a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester resin obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester resin obtained from a carboxylic acid compound and at least one compound of a phenol compound and a naphthol compound is preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol. Preferred specific examples of the active ester resin include active ester resins containing a dicyclopentadiene-type diphenol structure, active ester resins containing a naphthalene structure, active ester resins containing an acetylated product of phenol novolac, and active ester resins containing a benzoylated product of phenol novolac. Among them, active ester resins containing a naphthalene structure and active ester resins containing a dicyclopentadiene-type diphenol structure are more preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentylene-phenylene. Commercially available active ester resins include, for example, active ester resins containing a dicyclopentadiene-type diphenol structure, such as "EXB9451", "EXB9460", "EXB9460S", "HPC-8000-65T", "HPC-8000H-65TM", "EXB-8000L-65TM", and "EXB-8150-65T" (manufactured by DIC Corporation); active ester resins containing a naphthalene structure, such as "EXB9416-70BK" (manufactured by DIC Corporation); and phenol Examples of active ester resins containing acetylated novolac include "DC808" (manufactured by Mitsubishi Chemical Corporation); active ester resins containing benzoylated phenol novolac include "YLH1026", "YLH1030", and "YLH1048" (manufactured by Mitsubishi Chemical Corporation); active ester resins which are acetylated phenol novolac include "DC808" (manufactured by Mitsubishi Chemical Corporation); and an active ester resin containing phosphorus atoms is "EXB-9050L-62M" (manufactured by DIC Corporation).
[0050] The curable resin composition of the present embodiment can also be improved in curability by using a curing accelerator (curing catalyst) in combination. As a specific example of a curing accelerator that can be used, it is preferable to use a radical polymerization initiator for the purpose of promoting self-polymerization of a radically polymerizable curable resin such as an olefin compound or a maleimide compound, or radical polymerization with other components. Examples of the radical polymerization initiator that can be used include ketone peroxides such as methyl ethyl ketone peroxide and acetylacetone peroxide, diacyl peroxides such as benzoyl peroxide, dialkyl peroxides such as dicumyl peroxide and 1,3-bis-(t-butylperoxyisopropyl)-benzene, peroxyketals such as t-butyl peroxybenzoate and 1,1-di-t-butylperoxycyclohexane, α-cumyl peroxyneodecanoate, t-butyl peroxyneodecanoate, t-butyl peroxypivalate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, t-amylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-amylperoxy-3,5,5-trimethylhexanoate, and the like. Examples of known curing accelerators include alkyl peresters such as di-2-ethylhexyl peroxydicarbonate, bis(4-t-butylcyclohexyl)peroxydicarbonate, t-butylperoxyisopropyl carbonate, 1,6-bis(t-butylperoxycarbonyloxy)hexane, organic peroxides such as t-butyl hydroperoxide, cumene hydroperoxide, t-butyl peroxyoctoate, lauroyl peroxide, and azo compounds such as azobisisobutyronitrile, 4,4'-azobis(4-cyanovaleric acid), and 2,2'-azobis(2,4-dimethylvaleronitrile), but are not particularly limited thereto. Ketone peroxides, diacyl peroxides, hydroperoxides, dialkyl peroxides, peroxyketals, alkyl peresters, percarbonates, etc. are preferred, and dialkyl peroxides are more preferred.The amount of the radical polymerization initiator added is preferably 0.01 to 5 parts by weight, particularly preferably 0.01 to 3 parts by weight, per 100 parts by weight of the curable resin composition. If the amount of the radical polymerization initiator used is too large, the molecular weight does not sufficiently extend during the polymerization reaction.
[0051] The curable resin composition of this embodiment is obtained by uniformly mixing the above components. The curable resin composition of this embodiment can be easily made into a cured product by the same method as the conventionally known method. For example, the epoxy resin and the curing agent, and if necessary, the curing accelerator, inorganic filler, release agent, silane coupling agent and additives are mixed sufficiently until they are uniform using an extruder, kneader, roll, etc., to obtain the curable resin composition of this embodiment, which is molded by a melt casting method, transfer molding method, injection molding method, compression molding method, etc., and further heated at 80 to 200 ° C. for 2 to 10 hours to obtain a cured product.
[0052] The curable resin composition of the present embodiment may contain a solvent as necessary. The solvent-containing curable resin composition (varnish) is impregnated into a fibrous material (substrate) such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, alumina fiber, or paper, and the prepreg obtained by heating and drying is then hot-press molded to obtain a cured product of the curable resin composition of the present embodiment. The solvent content of this curable resin composition is usually about 10 to 70% by weight, preferably about 15 to 70% by weight, based on the total weight. Examples of the solvent include amide-based solvents such as γ-butyrolactones, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and N,N-dimethylimidazolidinone; sulfones such as tetramethylene sulfone; ether-based solvents such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether monoacetate, and propylene glycol monobutyl ether, preferably mono- or di-lower (1-3 carbon atoms) alkyl ethers of lower (1-3 carbon atoms) alkylene glycols; ketone-based solvents such as methyl ethyl ketone and methyl isobutyl ketone, preferably in which the two alkyl groups are the same or different; di-lower (1-3 carbon atoms) alkyl ketones; and aromatic solvents such as toluene and xylene. These may be used alone or in a mixture of two or more.
[0053] In addition, a sheet-like adhesive (also simply called a sheet) can be obtained by applying the epoxy resin varnish onto a release film, removing the solvent under heating, and carrying out B-stage formation. This sheet-like adhesive can be used as an interlayer insulating layer in a multilayer substrate or the like.
[0054] The cured product obtained in this embodiment can be used for various applications, specifically, general applications in which thermosetting resins such as epoxy resins are used, such as adhesives, paints, coating agents, molding materials (including sheets, films, FRP, etc.), insulating materials (including printed circuit boards, electric wire coatings, etc.), sealants, and additives for other resins, etc.
[0055] Examples of adhesives include adhesives for civil engineering, construction, automobiles, general office use, and medical use, as well as adhesives for electronic materials. Among these, adhesives for electronic materials include interlayer adhesives for multilayer boards such as build-up boards, die bonding agents, semiconductor adhesives such as underfills, underfills for reinforcing BGAs, and mounting adhesives such as anisotropic conductive films (ACFs) and anisotropic conductive pastes (ACPs).
[0056] Examples of the sealing agent include potting, dipping and transfer mold sealing for capacitors, transistors, diodes, light-emitting diodes, ICs and LSIs, potting sealing for COB, COF, TAB and the like of ICs and LSIs, underfill for flip chips, and sealing (including reinforcing underfill) when mounting IC packages such as QFP, BGA and CSP. EXAMPLES
[0057] The present invention will now be described in more detail with reference to examples, in which parts are by weight unless otherwise specified. The present invention is not limited to these examples. In the examples, the epoxy equivalent was measured according to JIS K-7236, and the softening point was measured according to JIS K-7234. The softening point was measured using a METLER TOLEDO softening point tester FP90.
[0058] ·GPC (gel permeation chromatography) analysis Columns: SHODEX GPC KF-601 (2 columns), KF-602, KF-602.5, KF-603 Flow rate: 1.5ml / min. Column temperature: 40℃ Solvent used: THF (tetrahydrofuran) Detector: RI (Differential Refraction Detector)
[0059] ·GC-MS (Gas Chromatography-Gravimetric Analysis) Equipment: JEOL JMS-Q1500GC Column: Agilent HP-5ms 30m x 0.25mm id (film thickness 0.25μm) Carrier: He 1.5mL / min Split 1 / 30 Injection temperature: 300℃ Oven temperature: 100℃ (2min) - 310℃ (37min) 10℃ / min temperature increase Ionization current: 70 eV Ionization: EI Sample injection: 1 μL
[0060] · 1 H-NMR (proton nuclear magnetic resonance) analysis Equipment: JNM-ECS400 Number of times: 8 Relaxation time: 5 seconds Solvent: CDCL3 Measurement temperature: room temperature
[0061] [Synthesis Example 1] With reference to JOURNAL OF POLYMER RESEARCH (2019) 26:17, a flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer was purged with nitrogen while adding 90.3 parts of phenol, 20.0 parts of 2-acetylfluorene, 2.0 parts of 3-mercaptopropionic acid, 80.0 parts of hydrochloric acid, and 40.0 parts of acetic acid, and the temperature was raised to 60 ° C. and reacted for 48 hours. As the reaction proceeded, a product precipitated. The precipitated product was dissolved in ethyl acetate, and the organic layer was washed with water until the waste liquid became neutral, and then concentrated to obtain a crude product. The crude product was purified by column chromatography and recrystallization to obtain 13.0 parts of phenolic resin (P1) as a white solid resin.
[0062] [Example 1] While purging with nitrogen into a flask equipped with a thermometer, a condenser, a fractionating tube, and a stirrer, 22.8 parts of the phenolic resin (P1) obtained in Synthesis Example 1, 55.6 parts of epichlorohydrin, 11.3 parts of dimethyl sulfoxide, and 1.4 parts of water were added, and the internal temperature was raised to 45°C. 5.2 parts of sodium hydroxide were added in portions over 1.5 hours, and the mixture was reacted at 45°C for 2 hours and at 70°C for 1 hour. Unreacted epichlorohydrin and the solvent were distilled off under heating and reduced pressure. 59 parts of MIBK were added, and the organic layer was washed once with 26 parts of water. The organic layer was returned to the reaction vessel, 1.6 parts of a 30 wt% aqueous sodium hydroxide solution was added, and the mixture was reacted at 75°C for 1 hour. After cooling, the organic layer was washed five times with 10 parts of water, and the solvent was distilled off under heating and reduced pressure, to obtain 27 parts of the target compound (E1) as a pale yellow solid resin. The epoxy equivalent was 262 g / eq, the ICI viscosity (150°C) was 0.17 Pa·s, and the softening point was 84.4°C. The GC-MS chart of the target compound is shown in Figure 1. 1 H-NMR is shown in Figure 2. GC-MS analysis and 1 H-NMR analysis confirmed that the target compound (a) was produced.
[0063] [ka]
[0064] [Example 2, Comparative Example 1] The epoxy resin (E1) obtained in Example 1, bisphenol A type epoxy resin (RE-310S, epoxy equivalent 184 g / eq, manufactured by Nippon Kayaku Co., Ltd.) and 2E4MZ (2-ethyl-4-methylimidazole, manufactured by Shikoku Kasei Co., Ltd.) as a curing accelerator were mixed in the ratios shown in Table 1, and the mixture was uniformly ground using an agate mortar to obtain a curable resin composition. This curable resin composition was press molded (220° C. for 120 minutes) to obtain a test piece for evaluation.
[0065] The evaluation test pieces were measured under the following conditions, and the results are shown in Table 1.
[0066] <Heat resistance test (Tg)> The glass transition temperature (the temperature at which tan δ is at its maximum value) was measured using a dynamic viscoelasticity tester. Dynamic viscoelasticity measuring instrument: TA-instruments DMA-2980 Heating rate: 2℃ / min Frequency: 10Hz
[0067] <Tensile modulus> The measurements were carried out using an autograph AGS-X500N manufactured by Shimadzu Corporation. ·Measurement temperature: Room temperature (25℃) Pulling speed: 0.5mm / min
[0068] <Water absorption rate> The weight change was calculated from a test piece measuring 2.5 mm wide x 100 mm long x 0.25 mm thick after immersing it in water at 100°C for 24 hours.
[0069] <Dielectric tangent test> The test was performed at 25° C. using a 10 GHz cavity resonator manufactured by AET Co., Ltd., using a cavity resonator perturbation method. The sample size was 2.5 mm wide x 100 mm long, and the thickness was 0.25 mm.
[0070] [Table 1]
[0071] From the results in Table 1, it was confirmed that Example 2 was excellent in high heat resistance, high elastic modulus, low water absorption, and low dielectric tangent. [Industrial Applicability]
[0072] The epoxy resin of the present invention is useful for applications such as insulating materials for electric and electronic components (highly reliable semiconductor encapsulating materials, etc.), laminates (printed wiring boards, BGA substrates, build-up substrates, etc.), adhesives (conductive adhesives, etc.), various composite materials such as CFRP, coating materials, etc., and is particularly useful for applications such as insulating materials for electric and electronic components (highly reliable semiconductor encapsulating materials, etc.) and laminates (printed wiring boards, BGA substrates, build-up substrates, etc.) that require tracking resistance.
Claims
1. An epoxy resin represented by the following formula (1): 【Chemistry 1】 (In formula (1), each of the multiple R's independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. Each of the multiple p's independently represents an integer of 0 to 4. q represents an integer of 0 to 9.)
2. An epoxy resin represented by the following formula (2): 【Chemistry 2】
3. A curable resin composition comprising the epoxy resin according to claim 1 or 2.
4. The curable resin composition according to claim 3 , further comprising a curing agent or a curing accelerator.
5. A cured product obtained by curing the curable resin composition according to claim 3 or 4.
Citation Information
Patent Citations
Modified epoxy resin, and curable resin composition
JP2015147854A