Polishing composition, polishing method, and method for producing semiconductor substrate

The polishing composition with abrasive grains and a polyalkylene oxide compound at a pH of less than 7 addresses the challenge of high-speed silicon nitride polishing while reducing polycrystalline silicon polishing, improving manufacturing efficiency in semiconductor processes.

JP2024135558AActive Publication Date: 2024-10-04FUJIMI INCORPORATED
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023046310
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04
Estimated Expiration
2043-03-23

AI Technical Summary

Technical Problem

Existing polishing compositions fail to achieve high-speed polishing of silicon nitride films while simultaneously suppressing the polishing rate of polycrystalline silicon films, which is necessary for efficient semiconductor manufacturing.

Method used

A polishing composition containing abrasive grains with a negative zeta potential and a polyalkylene oxide compound at a pH of less than 7, which enhances the polishing rate of silicon nitride films while reducing the polishing rate of polycrystalline silicon films.

Benefits of technology

The composition enables high-speed polishing of silicon nitride films with improved selectivity, achieving a higher polishing rate ratio of silicon nitride to polycrystalline silicon, thereby enhancing manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135558000001
    Figure 2024135558000001
  • Figure 2024135558000002
    Figure 2024135558000002
  • Figure 2024135558000003
    Figure 2024135558000003
Patent Text Reader

Abstract

To provide a polishing composition that enables high-speed polishing of a silicon nitride film while reducing the polishing rate for a polycrystalline silicon film.SOLUTION: A polishing composition contains abrasive grains and a polyalkylene oxide compound, and has a pH less than 7. The abrasive grains have a negative zeta potential in the polishing composition. The polyalkylene oxide compound is represented by formula (1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing composition, a polishing method, and a method for producing a semiconductor substrate. [Background technology]

[0002] 2. Description of the Related Art In recent years, with the trend toward multi-layer wiring on the surface of a semiconductor substrate, a technique known as chemical mechanical polishing (CMP), in which a semiconductor substrate is polished and planarized, is used in the manufacture of devices.

[0003] The CMP has been applied to each process in semiconductor manufacturing, and one aspect of the CMP is its application to the gate formation process in transistor manufacturing. When manufacturing a transistor, materials such as metal, silicon, silicon oxide, polycrystalline silicon, and silicon nitride may be polished, and there is a demand for polishing each material at high speed in order to improve productivity. For example, there is a demand for polishing silicon nitride, which has poor chemical reactivity, at high speed. In order to meet such a demand, for example, Patent Document 1 discloses that silicon nitride can be polished at a high polishing rate by using a polishing composition containing colloidal silica with sulfonic acid fixed thereto and having a pH of 6 or less. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-040671 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present inventor, while examining the application of CMP to each process in semiconductor manufacturing, has found that in some cases, it is preferable in terms of manufacturing to polish a silicon nitride film at high speed in the presence of a polycrystalline silicon film. On the other hand, it has been found that in some cases, it is preferable in terms of manufacturing to reduce the polishing rate of a polycrystalline silicon film as much as possible. However, there is still no polishing composition that can polish a silicon nitride film at high speed and suppress the polishing rate of a polycrystalline silicon film.

[0006] Therefore, an object of the present invention is to provide a polishing composition which is capable of polishing a silicon nitride film at high speed while suppressing the polishing rate of a polycrystalline silicon film. [Means for solving the problem]

[0007] In order to solve the above problems, the present inventors have conducted extensive research. As a result, a polishing composition containing abrasive grains and a polyalkylene oxide compound and having a pH of less than 7, wherein the abrasive grains have a negative zeta potential in the polishing composition, and the polyalkylene oxide compound is represented by the following formula (1):

[0008] [ka]

[0009] [In formula (1), R 1 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms; R 2 represents an alkylene group having 4 carbon atoms; n represents an alkyleneoxy group (OR 2 ) is the average number of moles added, and is a number between 3 and 100. It has been found that the above problems can be solved by a polishing composition represented by the formula (I), and thus the present invention has been completed. Effect of the Invention

[0010] According to the present invention, there is provided a polishing composition which can polish a silicon nitride film at a high speed while suppressing the polishing rate of a polycrystalline silicon film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiments for carrying out the present invention will be described in detail. The embodiments shown here are merely examples for embodying the technical idea of ​​the present invention, and do not limit the present invention. Therefore, all other possible embodiments, methods of use, and operating techniques that can be conceived by those skilled in the art without departing from the gist of the present invention are included in the scope and gist of the present invention, and are included in the scope of the invention described in the claims and its equivalents. The embodiments described in this specification can be combined in any manner to form other embodiments. In addition, unless otherwise specified in this specification, the operation and measurement of physical properties are performed under the conditions of room temperature (20°C to 25°C) / relative humidity of 40% RH to 60% RH.

[0012] The present invention relates to a polishing composition comprising an abrasive grain and a polyalkylene oxide compound, and having a pH of less than 7, wherein the abrasive grain has a negative zeta potential in the polishing composition, and the polyalkylene oxide compound has a repeating unit of an oxyalkylene group having 4 carbon atoms. Such a polishing composition can polish a silicon nitride film at high speed and suppress the polishing rate of a polycrystalline silicon film. The present inventors speculate that the mechanism by which such an effect is obtained by the present invention is as follows. However, the following mechanism is merely speculation, and the scope of the present invention is not limited thereby.

[0013] In the present invention, the object to be polished preferably includes at least a silicon nitride film and a polycrystalline silicon film. According to the polishing composition of the present invention, among the objects to be polished, the silicon nitride film is polished at a high speed, and the polishing rate of the polycrystalline silicon film is suppressed. In a polishing composition having a pH of less than 7, abrasive grains having a negative zeta potential are easily adsorbed to the silicon nitride film and the polycrystalline silicon film, and thus the number of abrasive grains present on the surfaces of the silicon nitride film and the polycrystalline silicon film during polishing increases. However, if the polishing rate of the polycrystalline silicon film is increased, the ratio of the polishing rate of the silicon nitride film to the polishing rate of the polycrystalline silicon film (polishing rate of the silicon nitride film / polishing rate of the polycrystalline silicon film) (hereinafter also referred to as "polishing selectivity of silicon nitride") decreases. The inventors have found that the polishing composition of the present invention contains a specific polyalkylene oxide compound in an environment of less than pH 7, thereby suppressing the polishing rate of the polycrystalline silicon film while improving or maintaining the polishing rate of the silicon nitride film. That is, it is considered that the specific polyalkylene oxide compound is a hydrophobic compound and therefore easily adsorbs to the polycrystalline silicon film, which is a hydrophobic film, due to hydrophobic interaction. It is considered that the specific polyalkylene oxide compound adsorbs to the polycrystalline silicon film, reducing the contact between the abrasive grains and the polycrystalline silicon film, thereby suppressing the polishing speed of the polycrystalline silicon film. On the other hand, the specific polyalkylene oxide compound is difficult to adsorb to the silicon nitride film, which is a hydrophilic film. It is considered that the polishing composition of the present invention can polish the silicon nitride film at a high speed and suppress the polishing speed of the polycrystalline silicon film.

[0014] As described above, the present inventor has discovered that a polishing composition having a pH of less than 7, which contains abrasive grains having a negative zeta potential and a specific polyalkylene oxide compound, can polish a silicon nitride film at high speed while suppressing the polishing rate for a polycrystalline silicon film, thereby solving the problem.

[0015] It should be noted that the above mechanism is based on speculation, and the present invention is not limited to the above mechanism in any way.

[0016] [Polished object] The object to be polished according to the present invention preferably includes a silicon nitride (Si3N4) film and a polycrystalline silicon (polysilicon) film. That is, the polishing composition according to a preferred embodiment of the present invention is used for polishing an object to be polished that includes a silicon nitride film and a polycrystalline silicon film.

[0017] According to one embodiment of the present invention, the use of the object to be polished is not limited, and examples of the object include semiconductor substrates, solar cell substrates, TFTs of liquid crystal displays (LCDs), etc. Also, the present invention is suitable for test wafers, monitor wafers, transport check wafers, dummy wafers, etc.

[0018] The object to be polished according to the present invention may contain other materials in addition to the silicon nitride film and the polycrystalline silicon film. Examples of other materials include silicon oxide, silicon carbonitride (Si x C y N z ), doped polycrystalline silicon (doped polysilicon), undoped amorphous silicon, metal, SiGe, etc.

[0019] Examples of films containing silicon oxide include TEOS (Tetraethyl Orthosilicate) type silicon oxide films (hereinafter simply referred to as "TEOS films") produced using tetraethyl orthosilicate as a precursor, HDP (High Density Plasma) films, USG (Undoped Silicate Glass) films, PSG (Phosphorus Silicate Glass) films, BPSG (Boron-Phospho Silicate Glass) films, and RTO (Rapid Thermal Oxidation) films.

[0020] Examples of films containing metals include tungsten (W) films, titanium nitride (TiN) films, ruthenium (Ru) films, platinum (Pt) films, silver (Ag) films, gold (Au) films, hafnium (Hf) films, cobalt (Co) films, palladium (Pd), iridium (Ir), osmium (Os), nickel (Ni) films, copper (Cu) films, aluminum (Al) films, and tantalum (Ta) films.

[0021] Furthermore, the shape of the object to be polished is not particularly limited. In one embodiment of the present invention, the polishing composition can be preferably applied to polishing an object to be polished having a flat surface, such as a plate-like or polyhedral shape.

[0022] [Abrasive grain] The polishing composition according to the present invention contains abrasive grains. The abrasive grains contained in the polishing composition according to the present invention have a negative zeta potential. When the zeta potential of the abrasive grains is 0 mV or positive at a pH of less than 7, the polishing rate of the silicon nitride film is reduced, and as a result, the polishing rate of the silicon nitride film is lower than the polishing rate of the polycrystalline silicon film (the polishing selectivity of silicon nitride is reduced). The abrasive grains are preferably anion-modified silica (silica having an anionic group), and more preferably anion-modified colloidal silica (colloidal silica having an anionic group). The abrasive grains may be used alone or in combination of two or more kinds. In addition, the abrasive grains may be commercially available products or synthetic products.

[0023] The polishing composition according to the present invention preferably contains anion-modified colloidal silica as an abrasive. The anion-modified colloidal silica is colloidal silica whose surface is modified with an anionic group, and in the polishing composition, has the effect of mechanically polishing an object to be polished.

[0024] Preferred examples of anion-modified colloidal silica include colloidal silica having an anionic group fixed to the surface, such as a carboxy group, a sulfonic acid group, a phosphonic acid group, an aluminic acid group, etc. The method for producing colloidal silica having such an anionic group is not particularly limited, and examples thereof include a method of reacting a silane coupling agent having an anionic group at the end with colloidal silica.

[0025] As a specific example, sulfonic acid groups can be fixed to colloidal silica by the method described in, for example, "Sulfonic acid-functionalized silica through quantitative oxidation of thiol groups", Chem. Commun. 246-247 (2003). Specifically, a silane coupling agent having a thiol group, such as 3-mercaptopropyltrimethoxysilane, is coupled to colloidal silica, and then the thiol group is oxidized with hydrogen peroxide to obtain colloidal silica having sulfonic acid groups fixed to the surface (sulfonic acid-modified colloidal silica).

[0026] Carboxy groups can be fixed to colloidal silica by, for example, the method described in "Novel Silane Coupling Agents Containing a Photolabile 2-Nitrobenzyl Ester for Introduction of a Carboxy Group on the Surface of Silica Gel", Chemistry Letters, 3, 228-229 (2000). Specifically, a silane coupling agent containing a photoreactive 2-nitrobenzyl ester is coupled to colloidal silica, followed by light irradiation to obtain colloidal silica with carboxy groups fixed to the surface (carboxylic acid-modified colloidal silica).

[0027] The lower limit of the zeta potential of the abrasive grain in the polishing composition is preferably -65mV or more, more preferably -60mV or more, even more preferably -55mV or more, particularly preferably -50mV or more, and most preferably -45mV or more.The upper limit of the zeta potential of the abrasive grain in the polishing composition is preferably -5mV or less, more preferably -10mV or less, even more preferably -15mV or less, particularly preferably -20mV or less, and most preferably -25mV or less.That is, the zeta potential of the abrasive grain in the polishing composition is preferably -65mV or more and -5mV or less, more preferably -60mV or more and -10mV or less, even more preferably -55mV or more and -15mV or less, particularly preferably -50mV or more and -20mV or less, and most preferably -45mV or more and -25mV or less.

[0028] Abrasive grains having the above-mentioned zeta potential can polish a silicon nitride film at a higher polishing rate, and the polishing rate for the silicon nitride film is higher than the polishing rate for the polycrystalline silicon film (the polishing selectivity for silicon nitride is higher).

[0029] The average primary particle size of the abrasive grains is preferably 1 nm or more, more preferably 3 nm or more, and even more preferably 5 nm or more. As the average primary particle size of the abrasive grains increases, the polishing speed of the silicon nitride film increases. Also, the average primary particle size of the abrasive grains is preferably 100 nm or less, more preferably 50 nm or less, and even more preferably 30 nm or less. As the average primary particle size of the abrasive grains decreases, the polishing speed of the silicon nitride film becomes higher compared to the polishing speed of the polycrystalline silicon film (the polishing selectivity of silicon nitride becomes higher).

[0030] That is, the average primary particle size of the abrasive grains is preferably 1 nm or more and 100 nm or less, more preferably 3 nm or more and 50 nm or less, and even more preferably 5 nm or more and 30 nm or less. The average primary particle size of the abrasive grains can be calculated, for example, based on the specific surface area (SA) of the abrasive grains calculated by the BET method and the density of the abrasive grains.

[0031] In addition, the average secondary particle diameter of the abrasive grains is preferably 15 nm or more, more preferably 20 nm or more, and even more preferably 25 nm or more. As the average secondary particle diameter of the abrasive grains increases, the resistance during polishing decreases, and stable polishing of the silicon nitride film becomes possible. In addition, the average secondary particle diameter of the abrasive grains is preferably 200 nm or less, more preferably 150 nm or less, and even more preferably 100 nm or less. As the average secondary particle diameter of the abrasive grains decreases, the surface area per unit mass of the abrasive grains increases, the contact frequency with the polishing object increases, and the polishing speed of the silicon nitride film increases. That is, the average secondary particle diameter of the abrasive grains is preferably 15 nm or more and 200 nm or less, more preferably 20 nm or more and 150 nm or less, and even more preferably 25 nm or more and 100 nm or less. In one embodiment, the average secondary particle diameter of the abrasive grains is 20 nm or more and less than 70 nm. The average secondary particle size of the abrasive grains can be measured by, for example, a dynamic light scattering method such as a laser diffraction scattering method, and specifically, the value measured by the method described in the examples is used.

[0032] The ratio of the average secondary particle diameter to the average primary particle diameter of the abrasive grains (average secondary particle diameter / average primary particle diameter, hereinafter also referred to as "average degree of association") is preferably 1.2 or more, more preferably 1.5 or more, even more preferably 1.8 or more, particularly preferably 2.0 or more, and most preferably 2.2 or more. As the average degree of association of the abrasive grains increases, the polishing speed of the polycrystalline silicon film increases. In addition, the average degree of association of the abrasive grains is preferably 5.5 or less, more preferably 5.0 or less, even more preferably 4.5 or less, particularly preferably 4.0 or less, and most preferably 3.5 or less. As the average degree of association of the abrasive grains decreases, the polishing speed of the silicon nitride film becomes higher than the polishing speed of the polycrystalline silicon film (the polishing selectivity of silicon nitride becomes higher). That is, the average degree of association of the abrasive grains is preferably 1.2 or more and 5.5 or less, more preferably 1.5 or more and 5.0 or less, even more preferably 1.8 or more and 4.5 or less, particularly preferably 2.0 or more and 4.0 or less, and most preferably 2.2 or more and 3.5 or less.

[0033] The average degree of association of the abrasive grains is obtained by dividing the average secondary particle size of the abrasive grains by the average primary particle size of the abrasive grains.

[0034] The upper limit of the aspect ratio of the abrasive grains in the polishing composition is not particularly limited, but is preferably 3.5 or less, more preferably 3.0 or less, even more preferably 2.5 or less, particularly preferably 2.0 or less, and most preferably 1.5 or less. Within such a range, defects on the surface of the object to be polished can be further reduced. The aspect ratio is the average of the values ​​obtained by taking the smallest rectangle that circumscribes the image of the abrasive grains using a scanning electron microscope and dividing the length of the long side of the rectangle by the length of the short side of the same rectangle, and can be determined using general image analysis software. The lower limit of the aspect ratio of the abrasive grains in the polishing composition is not particularly limited, but is preferably 1.1 or more.

[0035] The shape of the abrasive grains is not particularly limited, and may be spherical or non-spherical. Specific examples of non-spherical shapes include polygonal prisms such as triangular prisms and square prisms, cylinders, bales in which the center of a cylinder is bulged out more than the ends, donuts in which the center of a disk is penetrated, plates, so-called cocoon shapes with a constriction in the center, so-called association-type spheres in which multiple particles are integrated, beads-shaped shapes in which multiple particles are connected in a line, so-called confetti-shaped shapes with multiple protrusions on the surface, rugby ball shapes, and needle-shaped shapes that are even thinner than the rugby ball shapes, and are not particularly limited.

[0036] The size of the abrasive grains (average primary particle size, average secondary particle size, aspect ratio, particle shape, etc.) can be appropriately controlled by selecting the manufacturing method of the abrasive grains, etc.

[0037] In this specification, the zeta potential of the abrasive grains is a value measured by the method described in the Examples. The zeta potential of the abrasive grains can be adjusted by the amount of anionic groups in the abrasive grains, the pH of the polishing composition, etc.

[0038] In the polishing composition according to the present invention, the abrasive grains may be used alone or in combination of two or more kinds. In addition, the abrasive grains to be used may be either commercially available products or synthetic products.

[0039] The content (concentration) of the abrasive grains in the polishing composition is not particularly limited, but is preferably 0.1 mass% or more, more preferably 0.2 mass% or more, even more preferably 0.5 mass% or more, and particularly preferably more than 0.5 mass% based on the total mass of the polishing composition. The upper limit of the content (concentration) of the abrasive grains in the polishing composition is preferably 10 mass% or less, more preferably 5 mass% or less, even more preferably 4 mass% or less, and particularly preferably less than 4 mass% based on the total mass of the polishing composition. That is, the content (concentration) of the abrasive grains in the polishing composition is preferably 0.1 mass% or more and 10 mass% or less, more preferably 0.2 mass% or more and 5 mass% or less, even more preferably 0.5 mass% or more and 4 mass% or less, and particularly preferably more than 0.5 mass% and less than 4 mass% based on the total mass of the polishing composition. In one embodiment, the content (concentration) of the abrasive grains in the polishing composition is 2 mass% or more and 10 mass% or less.

[0040] If the content of the abrasive grains is within this range, the polishing speed of the silicon nitride film will be higher than that of the polycrystalline silicon film (the polishing selectivity of silicon nitride will be higher). When the polishing composition contains two or more types of abrasive grains, the content of the abrasive grains refers to the total amount of these.

[0041] The polishing composition of the present invention may further contain other abrasive grains other than anion-modified silica, as long as the abrasive grains have a negative zeta potential in the polishing composition, within a range that does not impair the effects of the present invention. Such other abrasive grains may be any of inorganic particles, organic particles, and organic-inorganic composite particles. Specific examples of inorganic particles include unmodified silica, particles made of metal oxides such as alumina, ceria, and titania, silicon nitride particles, silicon carbide particles, and boron nitride particles. Specific examples of organic particles include polymethylmethacrylate (PMMA) particles.

[0042] [Polyalkylene oxide compounds] The polishing composition of the present invention contains a polyalkylene oxide compound represented by the following formula (1).

[0043] [ka]

[0044] In formula (1), R 1 and R 3 each independently represents a hydrogen atom or an alkyl group having from 1 to 20 carbon atoms. The alkyl group having from 1 to 20 carbon atoms may be any of a linear alkyl group, a branched alkyl group, or a cyclic alkyl group having from 1 to 20 carbon atoms, although a linear alkyl group having from 1 to 20 carbon atoms is preferred.

[0045] Specific examples of alkyl groups having 1 to 20 carbon atoms include, for example, a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tet-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a 2-ethylhexyl group, a hexyl group, a heptyl group, an octyl group, a 3,7-dimethyloctyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group (a lauryl group), a tridecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, and an octadecyl group.

[0046] R 1 and R 3 From the viewpoint of the polishing rate of silicon nitride, it is preferable that at least one of the groups is a hydrogen atom, and it is preferable that both of the groups are hydrogen atoms.

[0047] In formula (1), R 2represents an alkylene group having 4 carbon atoms. Examples of the alkylene group having 4 carbon atoms include an n-butylene group (tetramethylene group, -CH2CH2CH2CH2- group), a 1-methyltrimethylene group (-CH(CH3)CH2CH2- group), a 2-methyltrimethylene group (-CH2CH(CH3)CH2- group), a 1-ethylethylene group (-C(C2H5)CH2), a 1,1-dimethylethylene group (-C(CH3)2CH2- group), an ethylmethylmethylene group (-C(CH3)(C2H5)- group), a propylmethylene group (-C(C3H7)- group), and the like. Among these, an n-butylene group (-CH2CH2CH2CH2- group) and a 1-methyltrimethylene group (-CH(CH3)CH2CH2- group) are preferred. The compound of formula (1) may, for example, be represented by R 2 If is an n-butylene group, "-(OR 2 ) n -" is a compound having a tetramethylene oxide chain, R 2 If is a 1-methyltrimethylene group, "-(OR 2 ) n -" is a compound having a polybutylene oxide chain (poly 1-methyltrimethylene oxide chain).

[0048] In formula (1), n ​​is an alkyleneoxy group (OR 2 ) and is a number of 3 or more and 100 or less. n is preferably 3 or more and 60 or less, more preferably 5 or more and 50 or less, even more preferably 5 or more and 30 or less, and particularly preferably 5 or more and 25 or less. When n is within the above range, the polishing rate for the silicon nitride film is higher than the polishing rate for the polycrystalline silicon film (the polishing selectivity of silicon nitride is higher).

[0049] The polyalkylene oxide compound represented by formula (1) preferably has a weight average molecular weight (Mw) of 100 or more and 6000 or less, more preferably 150 or more and 5000 or less, even more preferably 200 or more and 4000 or less, particularly preferably 250 or more and 3500 or less, and most preferably 300 or more and less than 3000. In one embodiment, the weight average molecular weight of the polyalkylene oxide compound is less than 3000. If the weight average molecular weight of the polyalkylene oxide compound is within the above range, the polishing speed of the silicon nitride film is higher than the polishing speed of the polycrystalline silicon film (the polishing selectivity of silicon nitride is higher). Here, the weight average molecular weight of the polyalkylene oxide compound is measured by gel permeation chromatography (GPC) using polystyrene as a standard substance.

[0050] Specific examples of the polyalkylene oxide compound include polytetramethylene oxide and polybutylene oxide (poly 1-methyltrimethylene oxide). Among these, the polyalkylene oxide compound is preferably polytetramethylene oxide from the viewpoint of the polishing selectivity of silicon nitride.

[0051] In the polishing composition according to the present invention, the polyalkylene oxide compound may be used alone or in combination of two or more kinds. In addition, the polyalkylene oxide compound may be a commercially available product or a synthetic product.

[0052] The content (concentration) of polyalkylene oxide compound in the polishing composition is not particularly limited, but is preferably 0.0001 mass% or more, more preferably 0.0005 mass% or more, even more preferably 0.001 mass% or more, particularly preferably 0.003 mass% or more, and most preferably 0.005 mass% or more, based on the total mass of the polishing composition.In addition, the upper limit of the content (concentration) of polyalkylene oxide compound in the polishing composition is preferably 5 mass% or less, more preferably 1 mass% or less, even more preferably 0.5 mass% or less, particularly preferably 0.2 mass% or less, and most preferably 0.1 mass% or less, based on the total mass of the polishing composition. That is, the content (concentration) of the polyalkylene oxide compound is preferably 0.0001 mass% or more and 5 mass% or less, more preferably 0.0005 mass% or more and 1 mass% or less, even more preferably 0.001 mass% or more and 0.5 mass% or less, particularly preferably 0.003 mass% or more and 0.2 mass% or less, and most preferably 0.005 mass% or more and 0.1 mass% or less, relative to the total mass of the polishing composition.

[0053] If the content (concentration) of the polyalkylene oxide compound is within this range, the polishing speed of the silicon nitride film is higher than that of the polycrystalline silicon film (the polishing selectivity of silicon nitride is higher). When the polishing composition contains two or more polyalkylene oxide compounds, the content (concentration) of the polyalkylene oxide compound refers to the total amount of these.

[0054] [pH and pH adjusters] The pH of the polishing composition according to the present invention is less than 7. When the pH of the polishing composition is 7 or more, the polishing rate of the polycrystalline silicon film increases, and the polishing selectivity of silicon nitride decreases. In one embodiment, the pH of the polishing composition exceeds 1. Thus, in one embodiment, the pH of the polishing composition is more than 1 and less than 7. The pH of the polishing composition is preferably 1.5 or more, more preferably 2.0 or more, even more preferably 2.5 or more, particularly preferably 3.0 or more, and most preferably 3.5 or more. The pH of the polishing composition is preferably 6.5 or less, more preferably 6.0 or less, even more preferably 5.5 or less, particularly preferably 5.0 or less, and most preferably 4.5 or less. That is, the pH of the polishing composition is preferably 1.5 or more and 6.5 or less, more preferably 2.0 or more and 6.0 or less, even more preferably 2.5 or more and 5.5 or less, particularly preferably 3.0 or more and 5.0 or less, and most preferably 3.5 or more and 4.5 or less. In one embodiment, the pH of the polishing composition is from 2 to 5. When the pH of the polishing composition is within such a range, the polishing rate of the polycrystalline silicon film is higher than the polishing rate of the silicon nitride film or the silicon oxide film (the polishing selectivity of silicon nitride is higher).

[0055] The polishing composition of the present invention may contain a pH adjuster to adjust the pH to less than 7. Examples of pH adjusters include inorganic acids, organic acids, alkalis, etc. These may be used alone or in combination of two or more.

[0056] Specific examples of inorganic acids that can be used as pH adjuster include hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid and phosphoric acid.Among these, hydrochloric acid, sulfuric acid, nitric acid or phosphoric acid is preferred, and nitric acid is more preferred.By using nitric acid as pH adjuster, it can improve the polishing selectivity for silicon nitride film, and can suitably improve the polishing speed for silicon nitride film.

[0057] Specific examples of organic acids that can be used as pH adjusters include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, lactic acid, diglycolic acid, 2-furancarboxylic acid, 2,5-furandicarboxylic acid, 3-furancarboxylic acid, 2-tetrahydrofurancarboxylic acid, methoxyacetic acid, methoxyphenylacetic acid, phenoxyacetic acid, methanesulfonic acid, ethanesulfonic acid, 10-camphorsulfonic acid, and isethionic acid.

[0058] Instead of or in combination with an inorganic or organic acid, a salt such as an alkali metal salt of an inorganic or organic acid may be used as a pH adjuster. In the case of a combination of a weak acid and a strong base, a strong acid and a weak base, or a weak acid and a weak base, a pH buffering effect can be expected.

[0059] Specific examples of alkalis that can be used as pH adjusters include ammonia, hydroxides of Group 1 elements (e.g., sodium hydroxide, potassium hydroxide), hydroxides of Group 2 elements (e.g., barium hydroxide), quaternary ammonium hydroxides (e.g., tetramethylammonium hydroxide), or salts thereof, etc. Examples of salts include carbonates, hydrogen carbonates, sulfates, acetates, etc.

[0060] In one embodiment, the polishing composition of the present invention further contains one or more pH adjusters selected from organic acids and inorganic acids. That is, in one embodiment, the polishing composition of the present invention further contains an organic acid or an inorganic acid as a pH adjuster. By containing an organic acid or an inorganic acid as a pH adjuster, the polishing selectivity for silicon nitride film can be improved, and the polishing speed for silicon nitride film can be suitably improved.

[0061] The content of the pH adjuster can be appropriately adjusted within the range in which the effects of the present invention are achieved. The pH of the polishing composition can be measured, for example, by a pH meter (for example, a pH meter (model number: LAQUA) manufactured by Horiba, Ltd.).

[0062] [Dispersion medium] The polishing composition according to the present invention preferably contains a dispersion medium for dispersing each component. Examples of the dispersion medium include water; alcohols such as methanol, ethanol, and ethylene glycol; ketones such as acetone, and mixtures thereof. Of these, water is preferable as the dispersion medium. That is, according to a preferred embodiment of the present invention, the dispersion medium contains water. According to a more preferred embodiment of the present invention, the dispersion medium is substantially composed of water. Note that the above-mentioned "substantially" means that a dispersion medium other than water may be included as long as the effects of the present invention can be achieved. More specifically, the dispersion medium is preferably composed of 90% by mass or more and 100% by mass or less of water and 0% by mass or more and 10% by mass or less of a dispersion medium other than water, and more preferably composed of 99% by mass or more and 100% by mass or less of water and 0% by mass or more and 1% by mass or less of a dispersion medium other than water. Most preferably, the dispersion medium is water.

[0063] From the viewpoint of not inhibiting the action of the components contained in the polishing composition, the dispersion medium is preferably water containing as few impurities as possible. Specifically, pure water or ultrapure water from which impurity ions are removed by ion exchange resin and then foreign matter is removed through a filter, or distilled water is more preferable.

[0064] [Other ingredients] The polishing composition according to the present invention may further contain known additives that can be used in polishing compositions, such as complexing agents, preservatives, fungicides, oxidizing agents, surfactants other than the polyalkylene oxide compound represented by formula (1), water-soluble polymers other than the polyalkylene oxide compound represented by formula (1), and dissolution aids, within the range that does not inhibit the effects of the present invention. The polishing composition according to the present invention has a pH of less than 7. For this reason, it is more preferable that the polishing composition contains a fungicide. That is, in one embodiment of the present invention, the polishing composition is substantially composed of at least one selected from the group consisting of abrasive grains, a polyalkylene oxide compound, a dispersion medium, and a pH adjuster, a dissolution aid, and a fungicide. In one embodiment of the present invention, the polishing composition is substantially composed of at least one selected from the group consisting of abrasive grains, a polyalkylene oxide compound, a dispersion medium, and a pH adjuster, a dissolution aid, and a fungicide. Here, "the polishing composition is substantially composed of at least one selected from the group consisting of abrasive grains, a polyalkylene oxide compound, a dispersion medium, a pH adjuster, a dissolution aid, and an antifungal agent" means that the total content of the abrasive grains, the polyalkylene oxide compound, the dispersion medium, the pH adjuster, the dissolution aid, and the antifungal agent is more than 99% by mass (upper limit: 100% by mass) relative to the polishing composition. Preferably, the polishing composition is composed of at least one selected from the group consisting of abrasive grains, a polyalkylene oxide compound, a dispersion medium, a pH adjuster, a dissolution aid, and an antifungal agent (the total content = 100% by mass).

[0065] The antifungal agent (preservative) is not particularly limited and can be appropriately selected depending on the desired use and purpose.Specific examples include isothiazoline preservatives such as 1,2-benzoisothiazol-3(2H)-one (BIT), 2-methyl-4-isothiazolin-3-one, and 5-chloro-2-methyl-4-isothiazolin-3-one, and phenoxyethanol.

[0066] The dissolution aid is a substance that is present when the water-soluble polymer is dissolved in a dispersion medium (solvent) to improve the solubility of the water-soluble polymer. The polishing composition according to one embodiment of the present invention may further include a dissolution aid.

[0067] Examples of the dissolution aid include alcohol compounds such as methanol, ethanol, 1-propanol, 2-propanol, ethylene glycol, and propylene glycol; ether compounds such as diethylene glycol diethyl ether, 2-methoxyethanol, 2-ethoxyethanol, diethylene glycol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol, triethylene glycol monomethyl ether, tetraethylene glycol, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, tripropylene glycol monomethyl ether, diacetone alcohol, 2-methoxyethyl acetate, 2-ethoxyethyl acetate, and diethylene glycol monoethyl ether acetate; and ketone compounds such as acetone, methyl ethyl ketone, acetylacetone, and cyclohexanone. These dissolution aids can be used alone or in combination of two or more.

[0068] [Polishing method and semiconductor substrate manufacturing method] The polishing composition according to the present invention is preferably used for polishing an object to be polished, for example, containing silicon nitride and polycrystalline silicon. Therefore, the present invention provides a polishing method comprising polishing an object to be polished, containing silicon nitride and polycrystalline silicon, with the polishing composition according to the present invention. The present invention also provides a method for producing a semiconductor substrate, comprising polishing a semiconductor substrate containing silicon nitride and polycrystalline silicon with the polishing composition according to the present invention. The present invention also provides a method for producing a semiconductor substrate, comprising a step of polishing a semiconductor substrate containing silicon nitride and polycrystalline silicon by the polishing method according to the present invention.

[0069] As a polishing device, a general polishing device can be used which is equipped with a holder for holding a substrate or the like having an object to be polished, a motor whose rotation speed can be changed, and a polishing platen onto which a polishing pad (polishing cloth) can be attached.

[0070] The polishing pad may be made of any material, including, without particular limitation, a general nonwoven fabric, polyurethane, porous fluororesin, etc. The polishing pad is preferably provided with grooves for storing the polishing liquid.

[0071] Regarding the polishing conditions, for example, the rotation speed of the polishing platen and the carrier was 10 rpm (0.17 s -1 ) or more 500rpm (8.33s -1 The pressure (polishing pressure) applied to the substrate having the object to be polished is preferably 0.5 psi (3.4 kPa) or more and 10 psi (68.9 kPa).

[0072] The method of supplying the polishing composition to the polishing pad is not particularly limited, and for example, a method of continuously supplying the composition using a pump, etc. There is no limit to the amount of the composition supplied, but it is preferable that the surface of the polishing pad is always covered with the polishing composition according to the present invention.

[0073] After polishing, the substrate is washed with running water, and water droplets adhering to the substrate are removed by a spin dryer or the like, followed by drying to obtain a substrate having a metal-containing layer.

[0074] The polishing composition of the present invention may be a one-liquid type or a multi-liquid type such as a two-liquid type. The polishing composition of the present invention may be prepared by diluting the stock solution of the polishing composition, for example, 3 times or more (or, for example, 5 times or more) with a diluting liquid such as water.

[0075] [Polishing speed suppressor] The polishing composition according to the present invention selectively polishes silicon nitride and inhibits polishing of polycrystalline silicon when polishing a semiconductor substrate containing silicon nitride and polycrystalline silicon.

[0076] [ka]

[0077] [In formula (1), R 1 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms; R 2 represents an alkylene group having 4 carbon atoms; n represents an alkyleneoxy group (OR 2 ) is the average number of moles added, and is a number between 3 and 100. The present invention provides an agent for suppressing the polishing rate of a polycrystalline silicon film, comprising a polyalkylene oxide compound represented by the following formula:

[0078] [Polishing speed] When polishing with the polishing composition of the present invention, the polishing rate of the silicon nitride film is preferably 150 Å / min or more and 5000 Å / min or less, more preferably 200 Å / min or more and 2500 Å / min or less, even more preferably 220 Å / min or more and 2000 Å / min or less, and particularly preferably 250 Å / min or more and 1500 Å / min or less. When polishing with the polishing composition of the present invention, the polishing rate of the polycrystalline silicon film is preferably 100 Å / min or less, more preferably 50 Å / min or less, even more preferably 45 Å / min or less, and particularly preferably 40 Å / min or less. The lower limit of the polishing rate of the silicon nitride film and / or silicon oxide film is not particularly limited, but is practically 5 Å / min or more.

[0079] [Polishing selection ratio] When the polishing composition of the present invention is used for polishing an object containing silicon nitride and polycrystalline silicon, the ratio of the polishing rate of silicon nitride to the polishing rate of polycrystalline silicon (polishing rate of silicon nitride / polishing rate of polycrystalline silicon) is preferably 10 or more, more preferably 12 or more, even more preferably 15 or more, particularly preferably 20 or more, and most preferably 30 or more.

[0080] Although the embodiments of the present invention have been described in detail, it is apparent that the same are illustrative and exemplary, not restrictive, and the scope of the present invention should be interpreted by the appended claims.

[0081] The present invention encompasses the following aspects and configurations.

[0082] [1] A polishing composition comprising an abrasive grain and a polyalkylene oxide compound and having a pH of less than 7, wherein the abrasive grain has a negative zeta potential in the polishing composition, and the polyalkylene oxide compound is represented by the following formula (1):

[0083] [ka]

[0084] [In formula (1), R 1 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms; R 2 represents an alkylene group having 4 carbon atoms; n represents an alkyleneoxy group (OR 2 ) is the average number of moles added, and is a number between 3 and 100. The polishing composition represented by the formula:

[0085] [2] The polishing composition according to the above [1], wherein the polyalkylene oxide compound is polytetramethylene oxide.

[0086] [3] The polishing composition according to [1] or [2] above, wherein the polyalkylene oxide has a weight average molecular weight of less than 3,000.

[0087] [4] The polishing composition according to any one of the above [1] to [3], wherein the abrasive grains are contained in an amount of 2 mass % or more and 10 mass % or less.

[0088] [5] The polishing composition according to any one of the above [1] to [4], wherein the abrasive grains have an average secondary particle size of 20 nm or more and less than 70 nm.

[0089] [6] The polishing composition according to any one of the above [1] to [5], wherein the abrasive grains are anion-modified colloidal silica.

[0090] [7] The polishing composition according to any one of the above [1] to [6], which has a pH of 2 or more and 5 or less.

[0091] [8] The polishing composition according to any one of the above [1] to [7], further comprising an organic acid or an inorganic acid as a pH adjuster.

[0092] [9] The polishing composition according to any one of the above [1] to [8], which is used for polishing an object containing silicon nitride and polycrystalline silicon.

[0093]

[10] The polishing composition according to [9] above, wherein the ratio of the polishing rate of the silicon nitride to the polishing rate of the polycrystalline silicon (silicon nitride / polycrystalline silicon) is 20 or more.

[0094]

[11] A polishing method comprising the step of polishing an object containing silicon nitride and polycrystalline silicon with the polishing composition according to any one of the above [1] to

[10] . EXAMPLES

[0095] The present invention will be described in more detail with reference to the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. In addition, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.

[0096] <Average primary particle size of abrasive grains> The average primary particle size of the abrasive grains was calculated from the specific surface area of ​​the silica particles measured by the BET method using "Flow Sorb II 2300" manufactured by Micromeritics, and the density of the abrasive grains.

[0097] <Average secondary particle size of abrasive grains> The average secondary particle diameter of the abrasive grains was measured as the volume average particle diameter (arithmetic mean diameter based on volume; Mv) using a dynamic light scattering particle size / particle size distribution analyzer UPA-UTI151 (manufactured by Nikkiso Co., Ltd.).

[0098] <Average degree of association of abrasive grains> The average degree of association of the abrasive grains was calculated by dividing the value of the average secondary particle size of the abrasive grains by the value of the average primary particle size of the abrasive grains.

[0099] <Zeta potential of abrasive grains> The zeta potential of the abrasive grains in the polishing composition was measured by subjecting the polishing composition to a Zetasizer Nano manufactured by Malvern Panalytical and measuring it using the laser Doppler method (electrophoretic light scattering measurement method) at a measurement temperature of 25°C, and calculating the zeta potential by analyzing the obtained data using the Smoluchowski formula.

[0100] <pH of polishing composition> The pH of the polishing composition was measured using a glass electrode type hydrogen ion concentration indicator (Model number: F-23, manufactured by Horiba, Ltd.) and three-point calibration was performed using standard buffer solutions (phthalate pH buffer solution, pH: 4.01 (25°C), neutral phosphate pH buffer solution, pH: 6.86 (25°C), carbonate pH buffer solution, pH: 10.01 (25°C)).The glass electrode was then placed in the polishing composition and the pH value was recorded after stabilization for at least 2 minutes.

[0101] <Electrical Conductivity of Polishing Composition> The electrical conductivity (EC) of the polishing composition was measured with a tabletop electrical conductivity meter (manufactured by Horiba, Ltd., model number: DS-71 LAQUA (registered trademark)).

[0102] [Preparation of abrasive grains] Anion-modified colloidal silica, abrasive grains 1 to 3, were prepared by the method described in sulfonic acid-functionalized colloidal silica ("Sulfonic acid-functionalized silica through quantitative oxidation of thiol groups", Chem. Commun. 246-247 (2003). Two types of colloidal silica (abrasive grains) were used for the sulfonic acid modification (abrasive grains 1 and 2). Abrasive grains 3 and 4 described below are the same abrasive grains as abrasive grain 1, but differ in the silane coupling agent concentration (MPS modification amount) relative to the total mass of the silica solids: 0.24 mass%, 0.6 mass%, 0.96 mass%.

[0103] Abrasive grain 1: (MPS modification amount 0.6% by mass) Average primary particle size: 14 nm, average secondary particle size: 14 nm, average degree of association: 2.4 Abrasive grain 2: (MPS modification amount 0.6% by mass) Average primary particle size: 35 nm, average secondary particle size: 70 nm, average degree of association: 2.0 Abrasive grain 3: (MPS modification amount 0.24% by mass) Average primary particle size: 14 nm, average secondary particle size: 14 nm, average degree of association: 2.4 Abrasive grain 4: (MPS modification amount 0.96% by mass) Average primary particle size: 14 nm, average secondary particle size: 14 nm, average degree of association: 2.4 [Preparation of polishing composition] Example 1 The above-obtained abrasive grain 1 (anion-modified colloidal silica) was added to the pure water dispersion medium at room temperature (25° C.) to a final concentration of 3% by mass. Furthermore, 2-methyl-4-isothiazolin-3-one (manufactured by The Dow Chemical Company) was added as an antifungal agent to a final concentration of 0.014 mM to obtain a mixed solution.

[0104] Thereafter, polytetramethylene oxide (weight average molecular weight: 1000, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added as a polyalkylene oxide compound to a final concentration of 0.01 mass%, and nitric acid (HNO3) was added as a pH adjuster to a pH of 4, followed by stirring and mixing for 30 minutes at room temperature (25°C) to prepare the polishing composition of Example 1. The pH of the resulting polishing composition was measured to be 4, and the electrical conductivity was 1 mS / cm.

[0105] The zeta potential of the abrasive grains 1 (anion-modified colloidal silica) in the obtained polishing composition was measured according to the above-mentioned method and found to be -40 mV. Furthermore, the particle size of the abrasive grains 1 (anion-modified colloidal silica) in the polishing composition was similar to that of the abrasive grains 1 (anion-modified colloidal silica) used.

[0106] (Examples 2 to 10, Comparative Examples 1 to 4) The polishing compositions of Examples 2 to 10 and Comparative Examples 1 to 4 were prepared in the same manner as in Example 1, except that the type and concentration of each component, and the pH were changed as shown in Table 1 below. The composition of each polishing composition is shown in Table 1 below. Abrasive grain 1 was used in Examples 3, 6, 7, 9, 10 and Comparative Examples 1 to 4; abrasive grain 2 in Example 2; abrasive grain 3 in Example 4; and abrasive grain 4 in Examples 5 and 8. In Comparative Examples 2 and 3, polyethylene glycol (PEG) was used as the polyalkylene oxide compound (represented as "PEG200" and "PEG4000" in Table 1 below). "-" in Table 1 below indicates that the agent was not used. The pH of each polishing composition and the particle size of the abrasive grains in each polishing composition were measured, and the values ​​shown in Table 1 were obtained.

[0107] [evaluation] <Evaluation of Polishing Rate of Polishing Composition> The surfaces of the objects to be polished were polished with each of the polishing compositions under the following conditions: The objects to be polished were the following (1) and (2).

[0108] (1) Silicon nitride film (Si3N4 film): A silicon wafer (200 mm, blanket wafer) with a 2000 Å thick silicon nitride film formed on its surface. (2) Polycrystalline silicon film (poly-Si film): A silicon wafer with a 5,000 Å thick polycrystalline silicon film formed on its surface.

[0109] (Polishing equipment and polishing conditions) Polishing equipment: Applied Materials 200mm CMP single-sided polishing equipment Mirra Polishing pad: Nitta Haas IC1010 hard polyurethane pad Polishing pressure: 4.0psi (1psi=6894.76Pa) Polishing platen rotation speed: 47 rpm Head (carrier) rotation speed: 43 rpm Supply of polishing composition: free-flowing Polishing composition supply amount: 200mL / min Polishing time: 60 seconds.

[0110] (Calculation of polishing rate) The thickness of each polished object before and after polishing was measured using an optical film thickness measuring device (ASET-f5x: manufactured by KLA-Tencor Corporation). The film thickness was measured using an optical film thickness measuring device (ASET-f5x: manufactured by KLA-Tencor Corporation).

[0111] The polishing speed for each object to be polished was calculated by dividing the difference in film thickness before and after polishing [(thickness before polishing)-(thickness after polishing)] by the polishing time. For silicon nitride films, if the polishing speed is 150 Å / min or more, it is practical. For the polishing speed ratio between silicon nitride films and polycrystalline silicon films, if the polishing speed of silicon nitride / polishing speed of polycrystalline silicon (Si3N4 / poly-Si in Table 1) is 10 or more (preferably 20 or more), it is practical.

[0112] The above evaluation results are also shown in Table 1. In Table 1, the silicon nitride film is indicated as "Si3N4" and the polycrystalline silicon film is indicated as "poly-Si."

[0113] [Table 1]

[0114] As is clear from Table 1 above, the polishing compositions of the Examples have a high polishing rate for silicon nitride films and can suppress the polishing rate for polycrystalline silicon films, resulting in a high polishing rate ratio for silicon nitride films. On the other hand, the polishing compositions of the Comparative Examples have a low polishing rate for silicon nitride films and a too high polishing rate for polycrystalline silicon films, resulting in a failure to obtain a high polishing rate ratio for silicon nitride films.

[0115] Therefore, it is understood that the polishing composition of the present invention can polish a silicon nitride film at high speed, while suppressing the polishing rate of a polycrystalline silicon film.

[0116] The results shown in Table 1 were obtained by polishing a silicon nitride film and a polycrystalline silicon film separately. However, it is expected that the polishing speed and the polishing selectivity (polishing speed of silicon nitride / polishing speed of polycrystalline silicon) shown in Table 1 will be the same when polishing a silicon nitride film and a polycrystalline silicon film.

Claims

1. A polishing composition comprising an abrasive grain and a polyalkylene oxide compound, the composition having a pH of less than 7, The abrasive grains have a negative zeta potential in the polishing composition, The polyalkylene oxide compound is represented by the following formula (1): 【Chemistry 1】 [In formula (1), R 1 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms; R 2 represents an alkylene group having 4 carbon atoms; n represents an alkyleneoxy group (O-R 2 ) is the average number of moles added, and is a number of 3 to 100. The polishing composition represented by the formula:

2. The polishing composition according to claim 1 , wherein the polyalkylene oxide compound is polytetramethylene oxide.

3. The polishing composition according to claim 1 or 2, wherein the polyalkylene oxide has a weight average molecular weight of less than 3,000.

4. The polishing composition according to claim 1 or 2, wherein the abrasive grains are contained in an amount of 2 mass % or more and 10 mass % or less.

5. 3. The polishing composition according to claim 1, wherein the abrasive grains have an average secondary particle size of 20 nm or more and less than 70 nm.

6. 3. The polishing composition according to claim 1, wherein the abrasive grains are anion-modified colloidal silica.

7. The polishing composition according to claim 1 or 2, which has a pH of 2 or more and 5 or less.

8. The polishing composition according to claim 1 or 2, further comprising an organic acid or an inorganic acid as a pH adjuster.

9. 3. The polishing composition according to claim 1, which is used for polishing an object containing silicon nitride and polycrystalline silicon.

10. 10. The polishing composition according to claim 9, wherein the ratio of the polishing rate of said silicon nitride to the polishing rate of said polycrystalline silicon (polishing rate of silicon nitride / polishing rate of polycrystalline silicon) is 20 or more.

11. 13. A polishing method comprising the step of polishing an object containing silicon nitride and polycrystalline silicon with the polishing composition according to claim 1.

Citation Information

Patent Citations

  • Polishing method

    JP2007273641A

  • Polishing composition

    JP2019169687A

  • Polishing composition, polishing method, and method for manufacturing substrate

    JP2021080441A

  • Method of producing anionically modified colloidal silica

    JP2021188020A

  • Composition for polishing, polishing method, and manufacturing method of polished substrate