Diamond electrode and manufacturing method for diamond electrode
The diamond electrode with a niobium carbide layer and porous structure enhances adhesion and durability by alleviating thermal expansion, addressing peeling issues and maintaining performance in acidic environments.
Patent Information
- Application Number
- JP2023046377
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-23
AI Technical Summary
Existing diamond electrodes face issues with peeling of the conductive diamond film and inadequate durability, particularly when used in strongly acidic environments.
A diamond electrode is designed with a niobium substrate that includes a niobium carbide layer with a porous portion containing voids, where a carbon source is embedded and reacted to form a continuous niobium carbide layer, upon which a conductive diamond film is deposited, alleviating thermal expansion coefficient differences and enhancing adhesion.
The design effectively suppresses peeling of the conductive diamond film and improves the durability of the electrode, maintaining performance even in strongly acidic conditions.
Smart Images

Figure 2024135599000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a diamond electrode and a method for manufacturing a diamond electrode. [Background technology]
[0002] Conductive diamond has a wide potential window in both aqueous and non-aqueous systems and a small background current, making it known as an electrode material capable of highly sensitive electrochemical detection over a wide potential range.
[0003] For example, Patent Document 1 discloses a method for producing a conductive diamond electrode, which comprises plastically processing at least the surface of an electrode substrate comprising a material selected from a valve metal selected from the group consisting of niobium, tantalum, titanium, and zirconium, and a metal-based alloy thereof, and then heat-treating the electrode substrate in a vacuum or in an inert atmosphere, and forming a conductive diamond film on the heat-treated surface of the electrode substrate. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 4456378 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a technique capable of suppressing peeling of a conductive diamond film and improving the durability of a diamond electrode. [Means for solving the problem]
[0006] According to one aspect of the present invention, A substrate made of metal niobium; a niobium carbide layer formed on at least one major surface of the substrate; a conductive diamond film formed on the niobium carbide layer; A diamond electrode is provided, wherein the niobium carbide layer comprises a porous portion having voids.
[0007] According to another aspect of the present invention, A step of forming a porous portion having voids inside at least one main surface of a substrate made of metal niobium; embedding a carbon source made of a solid carbon or carbon compound inside the main surface; a step of subjecting the substrate to a heat treatment to react the niobium metal and the carbon source to form a niobium carbide layer continuously covering the main surface; and depositing a conductive diamond film on the niobium carbide layer. Effect of the Invention
[0008] According to the present invention, a technique can be provided that can suppress peeling of the conductive diamond film and improve the durability of the diamond electrode. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1(a) is a schematic diagram showing a cross section of a diamond electrode 10 according to an embodiment of the present invention, and FIG. 1(b) is an enlarged schematic diagram of the vicinity of the boundary between a niobium carbide layer 30 and a conductive diamond film 40 in FIG. 1(a). [Diagram 2] FIG. 2 is a schematic diagram showing a detailed cross section of the diamond electrode 10 according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a flowchart showing an example of a method for manufacturing the diamond electrode 10 according to the embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram illustrating the porous portion forming step S102 according to the embodiment of the present invention. [Diagram 5] FIG. 5 is a flow chart showing an example of a method for manufacturing a diamond electrode 10 according to another embodiment of the present invention. [Figure 6]FIG. 6 is a cross-sectional photograph of Sample 1 according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] <Inventor's findings> First, the findings of the inventors will be described.
[0011] Diamond electrodes that are made conductive by including boron or the like can be used to generate oxidizing agents such as ozone. Durability is a major issue for such diamond electrodes. Although the technology described in Patent Document 1 and the like has improved the adhesion and peel strength between the substrate and the diamond film, it has been found that it is difficult to obtain a practical level of durability.
[0012] For example, paragraph 0009 of Patent Document 1 states that "if the intermediate layer is made of carbide derived from the substrate, it is expected that the adhesion of the diamond film will be improved due to the relationship between the substrate, the carbide growing from the substrate, and the diamond that generates using the carbide as a nucleus. However, in reality, carbides are often inferior in corrosion resistance to oxides when a potential is applied as an anode in strong acidity. Carbide is likely to form in a substrate that comes into contact with hydrocarbon radicals or diamond at high temperatures, so care must be taken when using it as an anode." From the perspective of improving durability, it was thought that it was preferable to prevent carbide from forming as much as possible in the intermediate layer between the substrate and the diamond film.
[0013] The inventor of the present application has conducted extensive research into the above-mentioned carbide layer. As a result, it has been found that the carbide layer only inhibits the durability of the diamond electrode when a strongly acidic liquid comes into contact with the carbide layer, and that the essence of the problem is the presence of pinholes on the surface of the diamond film that reach the substrate or the carbide layer. It has also been found that the occurrence of the above-mentioned pinholes can be suppressed by forming a continuous carbide layer as an intermediate layer.
[0014] Furthermore, as a result of further intensive research by the inventors of the present application, it has been found that by forming a porous portion having voids in the above-mentioned carbide layer, the difference in thermal expansion coefficient between the substrate and the diamond film can be alleviated, and the peeling of the diamond film can be suppressed. This makes it possible to further improve the durability of the diamond electrode.
[0015] [Details of the embodiment of the present invention] Next, an embodiment of the present invention will be described below with reference to the drawings. Note that the present invention is not limited to these examples, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.
[0016] <Embodiments of the present invention> (1) Structure of diamond electrode 10 First, the configuration of the diamond electrode 10 of this embodiment will be described. The diamond electrode 10 of this embodiment can be used, for example, as a diamond electrode 10 for electrochemical reactions (for example, for ozone generation). In this case, it is possible to suppress the deterioration of the diamond electrode 10 due to electrical conduction and improve its durability. In addition, it is possible to suppress the peeling of the conductive diamond film 40 and improve the durability of the diamond electrode 10.
[0017] Fig. 1(a) is a schematic diagram showing a cross section of a diamond electrode 10 of this embodiment. As shown in Fig. 1(a), the diamond electrode 10 has, for example, a substrate 20, a niobium carbide layer 30, and a conductive diamond film 40.
[0018] The substrate 20 is, for example, a flat niobium metal plate material for depositing the conductive diamond film 40 and for supporting the conductive diamond film 40. The size and thickness of the main surface of the substrate 20 are not particularly limited, but for example, the main surface has a rectangular shape with one side measuring 20 mm or more and 500 mm or less, and the thickness is 0.5 mm or more and 5 mm or less.
[0019] The niobium carbide layer 30 is formed, for example, on at least one of the main surfaces of the substrate 20, and is a layer formed by reacting a part of the metal niobium of the substrate 20 with a carbon source 22 described later. The niobium carbide layer 30 functions, for example, as an intermediate layer for increasing the nucleation density of diamond crystals. The main component of the niobium carbide layer 30 is preferably niobium carbide of the chemical formula NbC or Nb2C. This makes it possible to efficiently increase the nucleation density of diamond crystals for forming the conductive diamond film 40.
[0020] The thickness of the niobium carbide layer 30 is preferably, for example, 0.5 μm or more and 10 μm or less (more preferably, 0.8 μm or more and 2.5 μm or less). In other words, it is preferable that the minimum thickness and the maximum thickness of the niobium carbide layer 30 are within the range of 0.5 μm or more and 10 μm or less (more preferably, 0.8 μm or more and 2.5 μm or less). If the thickness of the niobium carbide layer 30 is less than 0.5 μm, it may be difficult to form a continuous niobium carbide layer 30. On the other hand, by making the thickness of the niobium carbide layer 30 0.5 μm or more, it is easy to form a continuous niobium carbide layer 30. On the other hand, if the thickness of the niobium carbide layer 30 exceeds 10 μm, the internal stress increases and the diamond electrode 10 may be warped. On the other hand, by making the thickness of the niobium carbide layer 30 10 μm or less, the internal stress can be reduced and the warping of the diamond electrode 10 can be reduced.
[0021] The conductive diamond film 40 is, for example, a polycrystalline film having conductivity formed on the niobium carbide layer 30. The conductive diamond film 40 may be either a polycrystalline diamond film or a diamond-like carbon (DLC) film. The conductive diamond film 40 may be, for example, a film having 1×10 19 cm -3 More than 1×10 22 cm -3 It is preferable that it is contained at the following concentration: The thickness of the conductive diamond film 40 is, for example, 0.5 μm or more and 10 μm or less, and from the viewpoint of maintaining a balance between durability and cost, it is preferably 1 μm or more and 5 μm or less.
[0022] When the surface of the conductive diamond film 40 is observed, for example, using a scanning electron microscope (for example, magnification 5000 times), it is preferable that there are no pinholes reaching the substrate 20 or the niobium carbide layer 30 within a field of view of 20 μm×20 μm. This reduces the risk that the strongly acidic liquid contacts the niobium carbide layer 30 even if the diamond electrode 10 is used in a strongly acidic liquid, so that it is possible to improve the durability of the diamond electrode 10. From the viewpoint of further improving the durability of the diamond electrode 10, it is more preferable that there are no pinholes reaching the substrate 20 or the niobium carbide layer 30 within a field of view of 1 mm×1 mm, and it is particularly preferable that there are no pinholes on the entire surface of the conductive diamond film 40.
[0023] In addition, even when the cross section (longitudinal or transverse section) of the conductive diamond film 40 is observed, for example, using a scanning electron microscope (for example, magnification 5000 times), it is preferable that there are no pinholes reaching the substrate 20 or the niobium carbide layer 30 within a field of view of 20 μm×20 μm. In other words, the conductive diamond film 40 has reduced pinholes not only observed from the surface, but also internal pinholes. This makes it possible to further improve the durability of the diamond electrode 10. It is more preferable that there are no pinholes reaching the substrate 20 or the niobium carbide layer 30 within a field of view of 1 mm×1 mm in the cross section (longitudinal or transverse section) of the conductive diamond film 40, and it is particularly preferable that there are no pinholes across the entire cross section of the conductive diamond film 40.
[0024] Fig. 1(b) is an enlarged schematic diagram of the vicinity of the boundary between the niobium carbide layer 30 and the conductive diamond film 40. As shown in Fig. 1(b), the niobium carbide layer 30 has a porous portion 33 having a large number of voids. This reduces the difference in thermal expansion coefficient between niobium and the conductive diamond film 40, and suppresses peeling of the conductive diamond film 40. In other words, it is possible to further improve the durability of the diamond electrode 10.
[0025] As shown in Fig. 1(b), the porous portion 33 is preferably present in the vicinity of the boundary between the niobium carbide layer 30 and the conductive diamond film 40. This can further enhance the effect of reducing the thermal expansion coefficient difference between niobium and the conductive diamond film 40. In this specification, the vicinity of the boundary between the niobium carbide layer 30 and the conductive diamond film 40 means, for example, a region from the boundary between the niobium carbide layer 30 and the conductive diamond film 40 to a depth of 1 µm toward the niobium carbide layer 30.
[0026] The porosity of the porous portion 33 is preferably, for example, 20% or more and 80% or less. If the porosity of the porous portion 33 is less than 20%, it may be difficult to obtain the effect of reducing the thermal expansion coefficient difference. On the other hand, by making the porosity of the porous portion 33 20% or more, it is possible to obtain a sufficient effect of reducing the thermal expansion coefficient difference. On the other hand, if the porosity of the porous portion 33 exceeds 80%, the strength of the diamond electrode 10 may decrease. On the other hand, by making the porosity 80% or less, it is possible to maintain the strength of the diamond electrode 10. In addition, when measuring the porosity of the porous portion 33, for example, the cross section of the porous portion 33 is observed by a scanning electron microscope, and the total area Sv of voids present in any observation field in the porous portion 33 is calculated by image analysis, and the ratio of the total area Sv of voids to the area S of the observation field is taken as the porosity of the porous portion 33.
[0027] When the cross section of the diamond electrode 10 is observed, for example, using a scanning electron microscope (for example, magnification 5000 times), it is preferable that a continuous niobium carbide layer 30 having a thickness of 0.5 μm or more is formed over a width of 20 μm or more (length in the direction parallel to the main surface of the substrate 20). This sufficiently increases the nucleation density of diamond crystals for forming the conductive diamond film 40, and can suppress the occurrence of pinholes. From the viewpoint of further suppressing the occurrence of pinholes, it is more preferable that a continuous niobium carbide layer 30 having a thickness of 0.5 μm or more is formed over a width of 1 mm or more, and it is particularly preferable that a continuous niobium carbide layer 30 having a thickness of 0.5 μm or more is formed over the entire main surface of the substrate 20.
[0028] 2 is a schematic diagram showing the cross-sectional details of the diamond electrode 10 of this embodiment. As shown in FIG. 2, the niobium carbide layer 30 has a two-layer structure, that is, an upper layer 31 and a lower layer 32.
[0029] The main component of the upper portion 31 of the niobium carbide layer 30 is niobium carbide of the chemical formula NbC, and the lower portion 32 of the niobium carbide layer 30 preferably contains niobium carbide of the chemical formula Nb2C (or the main component of the lower portion 32 is niobium carbide of the chemical formula Nb2C). Since the niobium carbide layer 30 is carbonized from the surface side, Nb2C with a high Nb component is likely to be formed in the lower portion 32 where the carbon source 22 diffused from the surface side is small. Thus, even if the lower portion 32 of the niobium carbide layer 30 contains Nb2C, the continuous niobium carbide layer 30 is formed, so that the nucleation density of diamond crystals for forming the conductive diamond film 40 can be sufficiently increased and the occurrence of pinholes can be suppressed, thereby improving the durability of the diamond electrode 10.
[0030] The porous portion 33 (not shown in FIG. 2) is preferably present in the upper portion 31 of the niobium carbide layer 30 (particularly, in the vicinity of the boundary with the conductive diamond film 40 inside the niobium carbide layer 30). This reduces the difference in thermal expansion coefficient between niobium and the conductive diamond film 40, and suppresses peeling of the conductive diamond film 40. In other words, it becomes possible to further improve the durability of the diamond electrode 10.
[0031] The ratio of the thickness of the upper portion 31 and the lower portion 32 of the niobium carbide layer 30 is not particularly limited, but for example, the thickness of the lower portion 32 of the niobium carbide layer 30 is 1.5 to 10 times the thickness of the upper portion 31.
[0032] The crystallite diameter of the niobium carbide contained in the upper portion 31 of the niobium carbide layer 30 is smaller than that of the niobium carbide contained in the lower portion 32. Specifically, for example, the crystallite diameter of the niobium carbide contained in the upper portion 31 is 1 nm or more and 100 nm or less, and the crystallite diameter of the niobium carbide contained in the lower portion 32 is, for example, 10 nm or more and 2000 nm or less. The crystallite diameter of the main component of the niobium carbide layer 30 can be measured, for example, by the Scherrer method of XRD. When the upper portion 31 of the niobium carbide layer 30 is measured by XRD, peaks such as NbC(111), NbC(200), NbC(222), and NbC(400) are observed, but the peak of NbC(200) is the strongest, so in this specification, unless otherwise specified, the crystallite diameter of NbC is calculated from the peak of NbC(200). Similarly, the crystallite size of the niobium carbide contained in the lower portion 32 was calculated from the peak of Nb2C(211) in XRD.
[0033] The crystallite diameter of niobium carbide (NbC) contained in the upper portion 31 of the niobium carbide layer 30 is, for example, preferably 1 nm or more and 100 nm or less, more preferably 5 nm or more and 60 nm or less. If the crystallite diameter is outside the above range, it may be difficult to form a continuous niobium carbide layer 30 having a thickness of 0.5 μm or more. In contrast, by setting the crystallite diameter within the above range, it becomes easier to form a continuous niobium carbide layer 30 having a thickness of 0.5 μm or more, and as a result, it becomes easier to suppress the occurrence of pinholes. Moreover, the crystallite size of niobium carbide (Nb2C) contained in the lower portion 32 of the niobium carbide layer 30 is, for example, preferably 10 nm or more and 2000 nm or less, and more preferably 20 nm or more and 1000 nm or less.
[0034] (2) Manufacturing method of diamond electrode 10 Next, a description will be given of a manufacturing method of the diamond electrode 10 of this embodiment. As described above, the diamond electrode 10 of this embodiment can be used as a diamond electrode 10 for electrochemical reactions (for example, for generating ozone).
[0035] Fig. 3 is a flow chart showing an example of the manufacturing method of the diamond electrode 10 of this embodiment. As shown in Fig. 3, the manufacturing method of the diamond electrode 10 of this embodiment has, for example, a porous part forming step S102, a carbon source embedding step S103, a niobium carbide layer forming step S105, and a diamond film depositing step S106. In this embodiment, the case of manufacturing the diamond electrode 10 from a substrate 20 made of metal niobium will be described.
[0036] (Porous part formation step S102) Fig. 4 is a schematic diagram illustrating the porous portion forming step S102. As shown in Fig. 4, the porous portion forming step S102 is, for example, a step of forming a porous portion 33 having a large number of voids inside at least one of the main surfaces of the substrate 20. By forming the porous portion 33, the voids in the porous portion 33 relieve distortion caused by the difference in thermal expansion coefficient between niobium and the conductive diamond film 40, so that peeling of the conductive diamond film 40 can be suppressed.
[0037] In the porous portion forming step S102, for example, the main surface of the substrate 20 is subjected to plastic deformation (for example, rough surface pressing) to a depth of 1 μm or more, and then the substrate 20 is heat-treated in a hydrogen atmosphere to form the porous portion 33. The purpose of the plastic deformation is to increase the contact area between the niobium surface and hydrogen, and to promote the diffusion of hydrogen by introducing processing strain into the niobium surface. When the substrate 20 is heat-treated in a hydrogen atmosphere, the metal niobium in the region subjected to the plastic deformation becomes embrittled, and then, in the process of cooling to room temperature, microcracks occur in the embrittled metal niobium, and the microcracks progress to become voids. The number and size of the microcracks (or voids) that occur can be controlled by the heat treatment conditions (temperature, time, cooling rate, etc.). From the viewpoint of efficiently forming a large number of voids in the porous portion 33, the substrate 20 may be further subjected to mechanical processing such as pressing after the heat treatment and cooling. The heat treatment conditions in the porous portion forming step S102 are exemplified as follows. Heat treatment temperature (substrate temperature): 600 to 800 degrees Heat treatment time: 30 to 90 minutes Cooling rate: 10~200 degrees / min In addition, the hydrogen that has bonded to metallic niobium by the above-mentioned embrittlement treatment is removed in the niobium carbide layer formation process S105 described below, so that it does not ultimately remain in large quantities in the substrate 20 and does not adversely affect the strength, etc. of the diamond electrode 10.
[0038] In the porous portion forming step S102, it is preferable to form the porous portion 33 so that the porosity of the porous portion 33 is, for example, 20% or more and 80% or less. If the porosity of the porous portion 33 is less than 20%, it may be difficult to obtain the effect of reducing the thermal expansion coefficient difference. In contrast, by setting the porosity of the porous portion 33 to 20% or more, the effect of reducing the thermal expansion coefficient difference can be sufficiently obtained. On the other hand, if the porosity of the porous portion 33 exceeds 80%, the strength of the diamond electrode 10 may decrease. In contrast, by setting the porosity to 80% or less, the strength of the diamond electrode 10 can be maintained.
[0039] (Carbon source embedding step S103) The carbon source embedding step S103 is a step of embedding a carbon source 22 made of a solid of carbon or a carbon compound inside the main surface of the substrate 20. Specifically, for example, the carbon source 22 is sprinkled on the surface of the substrate 20 on which the porous portion 33 has been formed by plastic deformation processing, and the surface is rubbed against a substrate 20 of the same size, etc., to embed the carbon source 22 in the surface of the substrate 20 while crushing the carbon source 22 until it has a size similar to the voids of the porous portion 33 (for example, an average particle size of 200 nm or less). Since the carbon source 22 is a solid, it is possible to introduce carbon atoms into the main surface of the substrate 20 at a higher concentration than a hydrocarbon gas or the like. This makes it easier for carbon atoms to diffuse into the metal niobium, making it easier to form a continuous niobium carbide layer 30.
[0040] As the carbon source 22, for example, graphite, boron carbide, diamond powder, etc. can be used. When diamond powder is used as the carbon source 22, at least the outer periphery of the diamond powder is preferably an amorphous layer (sp 2It is preferable to use diamond powder covered with carbon (carbon). From the viewpoints of increasing the reactivity with metal niobium and reducing costs, it is preferable to use graphite as the carbon source 22.
[0041] The average particle size of the carbon source 22 is preferably 200 nm or less. This makes it easier to embed the carbon source 22 inside the substrate 20. In addition, the surface area of the carbon source 22 is increased, and the reactivity with metal niobium can be improved. The lower limit of the average particle size of the carbon source 22 is not particularly limited, but is, for example, 5 nm or more.
[0042] In the carbon source embedding step S103, when graphite (average particle size 5 to 200 nm) is embedded inside the main surface of the substrate 20 as the carbon source 22, a niobium plate 1 cm 2 It is preferable that the amount of graphite (carbon source 22) used per cm is, for example, 200 μg or more and 1000 μg or less. 2 If the amount of the carbon source 22 is less than 200 μg / cm 3 , the carbonization of the metal niobium becomes insufficient, and it may be difficult to form a continuous niobium carbide layer 30. 2 If the amount of carbon source 22 used is less than 200 μg / cm, the hydrogen atoms bonded to the metal niobium in the porous portion forming step S102 cannot be completely released, and embrittlement regions may remain, making the diamond film more susceptible to peeling. 2 By using the carbon source 22 in an amount of 1000 μg / cm or more, the niobium metal is sufficiently carbonized to easily form a continuous niobium carbide layer 30, and the hydrogen atoms bonded to the niobium metal are removed to eliminate embrittled regions of the niobium metal. 2 If the amount of carbon source 22 used exceeds 1000 μg / cm 2 , a large amount of carbon source 22 will remain after the formation of the niobium carbide layer 30, which may adversely affect the deposition of the conductive diamond film 40. 2or less, it is possible to reduce the amount of residual carbon source 22. Moreover, from the viewpoint of reducing the energy (cost) required for embedding the carbon source 22, it is preferable to embed the carbon source 22 to a depth of 1 μm or less. When checking the carbon source 22 inside the main surface of the substrate 20, for example, a cross-section of the substrate 20 (for example, at a depth of about 1 μm) may be observed using a transmission electron microscope.
[0043] (Niobium carbide layer formation step S105) The niobium carbide layer forming step S105 is a step of forming a niobium carbide layer 30 that continuously covers the main surface of the substrate 20 by subjecting the substrate 20 to a heat treatment and reacting the niobium metal with the carbon source 22. This makes it possible to suppress the occurrence of pinholes on the surface of the conductive diamond film 40. In addition, since the niobium carbide layer 30 has a porous portion 33, peeling of the conductive diamond film 40 can be suppressed.
[0044] The niobium carbide layer forming step S105 also has the effect of removing hydrogen that has been bonded to metallic niobium by the embrittlement treatment in the porous portion forming step S102 from the substrate 20. In addition, the voids formed in the porous portion forming step S102 can be transformed into a rounded shape by this heat treatment.
[0045] In the niobium carbide layer forming step S105, the niobium carbide layer 30 can be formed, for example, by using a hot filament CVD apparatus described later as a heating furnace for heat treatment.
[0046] The heat treatment conditions in the niobium carbide layer forming step S105 are exemplified as follows. Heat treatment temperature (substrate temperature): 550 to 850 degrees Pressure: 10~50 Torr Heat treatment time: 30 to 120 minutes
[0047] In the niobium carbide layer forming step S105, for example, it is preferable to form a niobium carbide layer 30 mainly composed of niobium carbide of the chemical formula NbC near the surface of metal niobium. This makes it possible to increase the nucleation density of diamond crystals for forming the conductive diamond film 40.
[0048] In the niobium carbide layer forming step S105, it is preferable to form the niobium carbide layer 30 so that the crystallite size of niobium carbide (NbC) contained in the upper portion 31 of the niobium carbide layer 30 is 1 nm or more and 100 nm or less, more preferably 5 nm or more and 60 nm or less. This makes it easier to suppress the occurrence of pinholes.
[0049] In the niobium carbide layer forming step S105, it is desirable to form the niobium carbide layer 30 so that the main component of the upper portion 31 is niobium carbide of the chemical formula NbC. Since the smaller the crystallite size of metallic niobium, the easier it is to carbonize and the easier it is to form NbC, when forming the niobium carbide layer 30, it is effective to previously apply plastic deformation processing to the metallic niobium in the region that will become the upper portion 31 in the porous portion forming step S102 to reduce the crystallite size of the metallic niobium.
[0050] (Diamond film deposition step S106) The diamond film deposition step S106 is, for example, a step of depositing a conductive diamond film 40 on the niobium carbide layer 30. In this embodiment, since the continuous niobium carbide layer 30 is formed in the above-mentioned niobium carbide layer formation step S105, the occurrence of pinholes on the surface of the conductive diamond film 40 can be suppressed. In the diamond film deposition step S106, for example, the conductive diamond film 40 can be deposited using a hot filament CVD apparatus. The hot filament CVD apparatus is configured to be able to supply various gases such as hydrogen gas, carbon-containing gas, and boron-containing gas to the growth chamber. As the carbon-containing gas, methane gas or ethane gas can be used. As the boron-containing gas, trimethylboron (TMB) gas, trimethylborate gas, triethylborate gas, or diborane gas can be used. In addition, the hot filament CVD apparatus has a temperature sensor, a tungsten filament, an electrode (for example, a molybdenum electrode), and the like in an airtight container configured inside the growth chamber.
[0051] The diamond crystal growth conditions in the diamond film deposition step S106 are exemplified as follows. Heat treatment temperature (substrate temperature): 700 to 1000 degrees Pressure: 5~50 Torr Heat treatment time: 1 to 10 hours
[0052] The above steps make it possible to manufacture the diamond electrode 10. Furthermore, a plurality of diamond electrodes 10 may be combined to manufacture a diamond electrode 10 unit.
[0053] (3) Effects of this embodiment According to this embodiment, one or more of the following advantages are achieved.
[0054] (a) In the diamond electrode 10 of this embodiment, the niobium carbide layer 30 has a porous portion 33 having a large number of voids. This reduces the difference in thermal expansion coefficient between niobium and the conductive diamond film 40, and suppresses peeling of the conductive diamond film 40. In other words, it is possible to further improve the durability of the diamond electrode 10.
[0055] (b) In the diamond electrode 10 of this embodiment, the porous portion 33 is preferably present in the vicinity of the boundary between the conductive diamond film 40 and the niobium carbide layer 30. This can further enhance the effect of reducing the difference in thermal expansion coefficient between niobium and the conductive diamond film 40.
[0056] (c) In the diamond electrode 10 of this embodiment, the porosity of the porous portion 33 is preferably, for example, 20% or more and 80% or less. If the porosity of the porous portion 33 is less than 20%, it may be difficult to obtain the effect of reducing the thermal expansion coefficient difference. In contrast, by setting the porosity of the porous portion 33 to 20% or more, the effect of reducing the thermal expansion coefficient difference can be sufficiently obtained. On the other hand, if the porosity of the porous portion 33 exceeds 80%, the strength of the diamond electrode 10 may decrease. In contrast, by setting the porosity to 80% or less, the strength of the diamond electrode 10 can be maintained.
[0057] (d) In the diamond electrode 10 of this embodiment, when the cross section of the diamond electrode 10 is observed using, for example, a scanning electron microscope, it is preferable that a continuous niobium carbide layer 30 having a thickness of 0.5 μm or more is formed over a width of 20 μm or more. This sufficiently increases the nucleation density of diamond crystals for forming the conductive diamond film 40, and can suppress the occurrence of pinholes. In addition, from the viewpoint of further suppressing the occurrence of pinholes, it is more preferable that a continuous niobium carbide layer 30 having a thickness of 0.5 μm or more is formed over a width of 1 mm or more, and it is particularly preferable that a continuous niobium carbide layer 30 having a thickness of 0.5 μm or more is formed over the entire main surface of the substrate 20.
[0058] (e) In the diamond electrode 10 of this embodiment, the thickness of the niobium carbide layer 30 is preferably, for example, 0.5 μm or more and 10 μm or less (more preferably, 0.8 μm or more and 2.5 μm or less). In other words, it is preferable that the minimum thickness and the maximum thickness of the niobium carbide layer 30 are within the range of 0.5 μm or more and 10 μm or less (more preferably, 0.8 μm or more and 2.5 μm or less). If the thickness of the niobium carbide layer 30 is less than 0.5 μm, it may be difficult to form a continuous niobium carbide layer 30. On the other hand, by making the thickness of the niobium carbide layer 30 0.5 μm or more, it is easy to form a continuous niobium carbide layer 30. On the other hand, if the thickness of the niobium carbide layer 30 exceeds 10 μm, the internal stress increases and the diamond electrode 10 may be warped. On the other hand, by making the thickness of the niobium carbide layer 30 10 μm or less, the internal stress can be reduced and the warpage of the diamond electrode 10 can be reduced.
[0059] (f) In the diamond electrode 10 of this embodiment, the main component of the niobium carbide layer 30 is preferably, for example, niobium carbide of the chemical formula NbC or Nb2C. This can efficiently increase the nucleation density of diamond crystals for forming the conductive diamond film 40.
[0060] (g) In the diamond electrode 10 of this embodiment, the main component of the upper portion 31 of the niobium carbide layer 30 is niobium carbide of the chemical formula NbC, and the lower portion 32 of the niobium carbide layer 30 preferably contains niobium carbide of the chemical formula Nb2C (or the main component of the lower portion 32 is niobium carbide of the chemical formula Nb2C). Since the niobium carbide layer 30 is carbonized from the surface side, Nb2C with a high Nb component is likely to be formed in the lower portion 32 where the carbon source 22 diffused from the surface side is small. In this way, even if the lower portion 32 of the niobium carbide layer 30 contains Nb2C, the continuous niobium carbide layer 30 is formed, so that the nucleation density of diamond crystals for forming the conductive diamond film 40 can be sufficiently increased and the occurrence of pinholes can be suppressed, thereby improving the durability of the diamond electrode 10.
[0061] (h) In the diamond electrode 10 of this embodiment, the crystallite diameter of the niobium carbide (NbC) contained in the upper portion 31 of the niobium carbide layer 30 is, for example, preferably 1 nm or more and 100 nm or less, more preferably 5 nm or more and 60 nm or less. If the crystallite diameter is outside the above range, it may be difficult to form a continuous niobium carbide layer 30 with a thickness of 0.5 μm or more. On the other hand, by setting the crystallite diameter within the above range, it becomes easier to form a continuous niobium carbide layer 30 with a thickness of 0.5 μm or more, and as a result, it becomes easier to suppress the occurrence of pinholes.
[0062] (i) In the diamond electrode 10 of this embodiment, when the surface of the conductive diamond film 40 is observed using, for example, a scanning electron microscope, it is preferable that there are no pinholes reaching the substrate 20 or the niobium carbide layer 30 within a field of view of 20 μm×20 μm. This makes it possible to improve the durability of the diamond electrode 10, since it is possible to reduce the risk that the strongly acidic liquid contacts the niobium carbide layer 30, even if the diamond electrode 10 is used in, for example, a strongly acidic liquid. In addition, from the viewpoint of further improving the durability of the diamond electrode 10, it is more preferable that there are no pinholes reaching the substrate 20 or the niobium carbide layer 30 within a field of view of 1 mm×1 mm, and it is particularly preferable that there are no pinholes on the entire surface of the conductive diamond film 40.
[0063] Specifically, for example, when the diamond electrode 10 of the present embodiment is used as the diamond electrode 10 for generating ozone water, it is possible to suppress the deterioration of the diamond electrode 10 due to electrical current and prevent the peeling of the conductive diamond film 40. That is, it is possible to improve the durability of the diamond electrode 10.
[0064] (j) The manufacturing method of the diamond electrode 10 of this embodiment includes, for example, a porous portion forming step S102, a carbon source embedding step S103, a niobium carbide layer forming step S105, and a diamond film depositing step S106. This allows the niobium carbide layer 30 that continuously covers the main surface of the substrate 20 and has a porous portion 33 to be formed, making it possible to suppress the occurrence of pinholes on the surface of the conductive diamond film 40. In addition, the difference in thermal expansion coefficient between niobium and the conductive diamond film 40 can be alleviated, and peeling of the conductive diamond film 40 can be suppressed.
[0065] <Other embodiments of the present invention> Although the embodiment of the present invention has been specifically described above, the present invention is not limited to the above-mentioned embodiment, and various modifications can be made without departing from the gist of the present invention.
[0066] Fig. 5 is a flow chart showing an example of a method for manufacturing a diamond electrode 10 according to another embodiment of the present invention. In the above-mentioned embodiment, each step of the method for manufacturing a diamond electrode 10 has been described, but for example, as shown in the flow chart of Fig. 5, the unevenness forming step S101 may be performed before the porous portion forming step S102, and the seeding step S104 may be performed before the niobium carbide layer forming step S105. In this case, as in the above-mentioned embodiment, a continuous niobium carbide layer 30 may be formed, and pinholes in the conductive diamond film 40 may be suppressed. Hereinafter, the unevenness forming step S101 and the seeding step S104 will be described.
[0067] (Irregularity forming step S101) The unevenness forming step S101 is, for example, a step of processing at least one of the main surfaces of the substrate 20 to form uneven undulations. This can suppress peeling caused by the difference in thermal expansion coefficient between the substrate 20 and the conductive diamond film 40. In other words, the peel strength of the diamond electrode 10 can be further improved. In the unevenness forming step S101, it is preferable to form unevenness so that the arithmetic mean roughness Ra (see JIS B0601-2001) of the main surface is 0.5 μm or more and 10 μm or less. For the processing to form unevenness, for example, known methods such as grinding, blasting, wet etching, dry etching, etc. can be used.
[0068] The unevenness forming step S101 is preferably performed, for example, before the porous portion forming step S102. If a process for forming unevenness is performed on the surface on which the porous portion 33 is formed, there is a possibility that the porous portion 33 will be removed. In contrast, by performing the unevenness forming step S101 before the porous portion forming step S102, the subsequent steps can be performed in a state in which the porous portion 33 remains.
[0069] As in the above embodiment, the unevenness forming step S101 may be omitted. Even if the unevenness forming step S101 is omitted, the niobium carbide layer 30 having the porous portion 33 can be formed in the niobium carbide layer forming step S105 by performing the porous portion forming step S102, and this porous portion 33 produces the effect of reducing the thermal expansion coefficient difference between niobium and the conductive diamond film 40, so that the peeling of the conductive diamond film 40 can be suppressed.
[0070] (Seeding process S104) The seeding step S104 is, for example, a step of seeding diamond particles on the main surface of the substrate 20 (the main surface on which the porous portion 33 is formed). In a typical seeding step S104, diamond particles are attached (seeded) to the surface of the substrate 20 on which the niobium carbide layer 30 is formed by a method such as rubbing, immersion, or blasting immediately before the diamond film deposition step S106. By thus interposing diamond particles at the interface between the niobium carbide layer 30 and the conductive diamond film 40, the energy barrier required for initial nucleation to form the conductive diamond film 40 can be lowered.
[0071] The seeding step S104 can be carried out, for example, before forming the niobium carbide layer 30 (i.e., before the niobium carbide layer forming step S105). That is, the seeding step S104 and the above-mentioned carbon source embedding step S103 can be carried out simultaneously. This is made possible by using the same diamond particles as the carbon source 22 used in the carbon source embedding step S103 and the diamond particles used in the seeding step S104. As described above, the carbon source 22 can be sp 2 It is preferable that the diamond structure (sp 3 The core of the structure is surrounded by an amorphous layer (sp 2 The diamond particles (e.g., nano-diamond particles obtained by detonation) covered with niobium carbide (carbon) are sp 2 Carbon is exhausted and sp 3 The core of the structure can be left as seeded diamond particles, which allows the niobium carbide layer formation step S105 and the diamond film deposition step S106 to be carried out consecutively in the same apparatus.
[0072] As in the above embodiment, the seeding step S104 may be omitted. Even if the seeding step S104 is omitted, by performing the above carbon source embedding step S103, the main surface of the substrate 20 is continuously covered with the niobium carbide layer 30 in the niobium carbide layer forming step S105, which promotes nucleation when depositing the diamond film, and therefore the occurrence of pinholes in the conductive diamond film 40 can be suppressed.
[0073] In the above embodiment, the carbon source 22 is embedded in the main surface of the substrate 20 in the carbon source embedding step S103, but the carbon source 22 does not necessarily have to be embedded in the main surface of the substrate 20. For example, by making the crystallite diameter of the metal niobium in the main surface of the substrate 20 sufficiently small (for example, 20 nm or less), a large number of grain boundaries in which crystal defects are densely assembled and arranged can be formed. This ensures a sufficient diffusion path for the carbon source 22 and a sufficiently large surface area of the metal niobium that contributes to the carbonization reaction. Therefore, even if the carbon source 22 is not embedded in the main surface of the substrate 20 and is introduced so as to be in contact with the surface of the substrate 20, it is possible to form the niobium carbide layer 30. Even if the carbon source 22 is not embedded in the main surface of the substrate 20, it diffuses from the grain boundaries of the metal niobium to the inside, and therefore it is possible to obtain the niobium carbide layer 30 having a thickness according to the diffusion length. However, from the viewpoint of facilitating the formation of a continuous niobium carbide layer 30 of sufficient thickness (eg, 0.5 μm or more), it is preferable to embed the carbon source 22 inside the main surface of the substrate 20 as in the above embodiment.
[0074] In the above embodiment, the conductive diamond film 40 has a single layer structure, but the conductive diamond film 40 may have a multilayer structure in which a plurality of conductive diamond layers are stacked. However, according to the present invention, even when the conductive diamond film 40 has a single layer structure as in the above embodiment, it is possible to suppress the occurrence of pinholes. EXAMPLES
[0075] Next, examples of the present invention will be described. These examples are merely examples of the present invention, and the present invention is not limited to these examples.
[0076] (1) Manufacturing of diamond electrode 10 (Sample 1) First, the diamond electrode 10 of Sample 1 was manufactured by the following procedure.
[0077] A substrate 20 made of metal niobium with a size of 50 mm×50 mm and a thickness of 1 mm was prepared, and a main surface was subjected to plastic deformation processing by pressing. Specifically, a cemented carbide die with a rough surface (Ra of about 1 μm) was used, and the surface of the substrate 20 was subjected to plastic deformation processing by pressing at a pressure of 60 t.
[0078] After the plastic deformation process, the substrate 20 was subjected to a heat treatment in a hydrogen atmosphere at 600 degrees for 60 minutes, and then cooled to room temperature to form the porous portion 33. When the porous portion 33 was observed with a scanning electron microscope, the porosity of the porous portion 33 was found to be 70%.
[0079] Graphite (particle size: 1 to 2 μm) was applied as the carbon source 22 at a concentration of approximately 1 mg / cm on the main surface of the substrate 20 on which the porous portion 33 was formed. 2 The amount of graphite embedded in the main surface of the substrate 20 was calculated from the amount of carbon source 22 recovered after the rubbing operation, and the inside of the main surface of the substrate 20 was found to be about 300 μg / cm 2 It was confirmed that graphite (grain size 5 to 70 nm) was embedded in the sintered material.
[0080] In the present examples, the crystallite sizes were calculated from the results of wide-angle X-ray diffraction measurements using an X-ray diffractometer (RINT2500HLB) manufactured by Rigaku Corporation. The measurement conditions were as follows: Measurement wavelength: CuKα (0.15418nm) X-ray output: 50kV-250mA Optical system: Parallel beam with monochromator Divergence slit (DS): 0.5°+10mmH Scattering slit (SS): 0.5° Receiving slit (RS): 0.15 mm Scanning axis: 2θ / θ Scanning method: Continuous scanning Scanning range: 5°≦2θ≦100° Scanning speed: 0.5° / min Sampling: 0.01°
[0081] The substrate 20 with the graphite embedded therein was placed in a hot filament CVD apparatus, and the formation of the niobium carbide layer 30 and the deposition of the conductive diamond film 40 were carried out successively. Specifically, hydrogen gas, methane gas, and TMB gas were introduced, and the pressure was set to 20 to 50 Torr. Then, a voltage (120 to 150 V) was applied to the 40 cm filament, and the filament was carbonized and held until the resistance became constant. Furthermore, the filament voltage was increased to 175 V, and the filament temperature was held at 2200 to 2400°C and the substrate temperature was held at 700 to 800°C for 180 minutes.
[0082] The diamond electrode 10 was removed from the hot filament CVD apparatus, and it was confirmed that a conductive diamond film 40 with a thickness of 3.21 μm had been deposited. In addition, when the diamond electrode 10 was measured by XRD from the conductive diamond film 40 side, the crystallite diameter of niobium carbide (NbC) was 12.8 nm.
[0083] (Sample 2) Moreover, the diamond electrode 10 of Sample 2 was manufactured by the following procedure.
[0084] A substrate 20 made of metal niobium was prepared, and similarly to sample 1, a main surface was subjected to plastic deformation processing by pressing.
[0085] After the plastic deformation process, the main surface of the substrate 20 was subjected to a heat treatment in a hydrogen atmosphere at 600 degrees for 60 minutes, and then cooled to room temperature to form the porous portion 33. When the porous portion 33 was observed with a scanning electron microscope, the porosity of the porous portion 33 was 68%.
[0086] In sample 2, the carbon source 22 was not embedded, and the surface of the substrate 20 on which the porous portion 33 was formed was seeded by applying a suspension containing fine diamond powder, and then sufficiently dried. Thereafter, the substrate 20 was placed in a hot filament CVD apparatus, and under the same conditions as in sample 1, the formation of the niobium carbide layer 30 and the deposition of the conductive diamond film 40 were successively carried out.
[0087] The diamond electrode 10 was removed from the hot filament CVD apparatus, and it was confirmed that a conductive diamond film 40 with a thickness of 2.72 μm had been deposited. In addition, when the diamond electrode 10 was measured by XRD from the conductive diamond film 40 side, the crystallite diameter of the niobium carbide was 5.1 nm.
[0088] (Sample 3) Moreover, the diamond electrode 10 of Sample 3 was manufactured by the following procedure.
[0089] A substrate 20 made of metal niobium was prepared, and similarly to sample 1, a main surface was subjected to plastic deformation processing by pressing.
[0090] In sample 3, the porous portion 33 was not formed, and graphite (grain size 1 to 2 μm) was applied as the carbon source 22 at a concentration of 1 mg / cm on the main surface of the substrate 20 that had been subjected to plastic deformation processing. 2 The amount of embedded graphite was measured before and after embedding, and the inside of the main surface of the substrate 20 contained 50 μg / cm 2 It was confirmed that graphite (grain size 5 to 70 nm) was embedded in the sintered material.
[0091] The substrate 20 after grinding was placed in a hot filament CVD apparatus, and under the same conditions as those for Sample 1, the formation of the niobium carbide layer 30 and the deposition of the conductive diamond film 40 were carried out successively.
[0092] The diamond electrode 10 was removed from the hot filament CVD apparatus, and it was confirmed that a conductive diamond film 40 with a thickness of 2.94 μm had been deposited. In addition, when the diamond electrode 10 was measured by XRD from the conductive diamond film 40 side, the crystallite diameter of the niobium carbide was 8.7 nm.
[0093] (2) Evaluation of diamond electrodes 10 The cross sections of Samples 1 to 3 were observed using a scanning electron microscope. In Sample 2, in which the carbon source 22 was not embedded, niobium carbide formed in islands was observed at the interface between the substrate 20 and the conductive diamond film 40, and a continuous niobium carbide layer 30 was not formed. In contrast, in Samples 1 and 3, in which the carbon source 22 was embedded inside the main surface of the substrate 20, it was confirmed that a continuous niobium carbide layer 30 was formed at the interface between the substrate 20 and the conductive diamond film 40. It was also confirmed that the niobium carbide layer 30 of Samples 1 and 2 had a porous portion 33 near the boundary with the conductive diamond film 40. A cross-sectional photograph of Sample 1 is shown in FIG. 6.
[0094] Furthermore, for Samples 1 to 3, the surface of the conductive diamond film 40 was observed using a scanning electron microscope. In Sample 2, in which the carbon source 22 was not embedded, pinholes were observed on the surface of the conductive diamond film 40. In contrast, in Samples 1 and 3, in which the carbon source 22 was embedded inside the main surface of the substrate 20, no pinholes were observed on the surface of the conductive diamond film 40.
[0095] From the above, it was confirmed that a continuous niobium carbide layer 30 can be formed by embedding the carbon source 22 inside the main surface of the substrate 20. It was also confirmed that the formation of a continuous niobium carbide layer 30 can suppress the occurrence of pinholes on the surface of the conductive diamond film 40.
[0096] (3) Durability test of diamond electrode 10 A durability test was conducted to generate ozone water using the diamond electrodes 10 of samples 1 to 3 as the anode and cathode, respectively. The durability test was conducted by using tap water (flow rate 200 mL / min) as the raw water, driving the anode and cathode fixed with a polymer electrolyte membrane between them at a low voltage of 8 V for 1 minute and then pausing for 4 minutes, and repeating this cycle 10,000 times. The polymer electrolyte membrane used was Nafion324 (manufactured by Du Pont). The current values and the generated ozone water concentrations before and after the above 10,000 cycles, and the area ratio of the conductive diamond film 40 peeled off after 10,000 cycles were confirmed, and the results are shown in Table 1.
[0097] [Table 1]
[0098] As shown in Table 1, in sample 2 in which the carbon source 22 was not embedded, the ozone water concentration at 10,000 cycles was significantly lower than that at the first cycle, and degradation due to electrical current was confirmed, and extensive peeling of the conductive diamond film 40 was confirmed. In addition, in sample 3 in which the porous portion 33 was not formed, a decrease in the ozone water concentration at 10,000 cycles was observed, and partial peeling of the conductive diamond film 40 was confirmed. In contrast, in sample 1 in which the porous portion 33 was formed and the carbon source 22 was embedded inside the main surface of the substrate 20, an ozone water concentration at the 10,000 cycles was similar to that at the first cycle (90% or more at the first cycle). In addition, peeling of the conductive diamond film 40 was not confirmed.
[0099] From the above, it was confirmed that by continuously covering the main surface of the substrate 20 and forming the niobium carbide layer 30 having the porous portion 33, it is possible to suppress the electrical deterioration and prevent the peeling of the conductive diamond film 40. In other words, it was confirmed that the durability of the diamond electrode 10 can be further improved.
[0100] <Preferred embodiment of the present invention> Preferred embodiments of the present invention will be described below.
[0101] (Appendix 1) According to one aspect of the present invention, A substrate made of metal niobium; a niobium carbide layer formed on at least one major surface of the substrate; a conductive diamond film formed on the niobium carbide layer; A diamond electrode is provided, wherein the niobium carbide layer comprises a porous portion having voids.
[0102] (Appendix 2) 2. The diamond electrode according to claim 1, The porous portion exists within the niobium carbide layer near the boundary with the conductive diamond film.
[0103] (Appendix 3) 2. The diamond electrode according to claim 1, The porosity of the porous portion is not less than 20% and not more than 80%.
[0104] (Appendix 4) 2. The diamond electrode according to claim 1, When the cross section of the diamond electrode was observed using a scanning electron microscope, a continuous niobium carbide layer having a thickness of 0.5 μm or more was formed over a width of 20 μm or more. More preferably, the niobium carbide layer is formed continuously and has a thickness of 0.5 μm or more over a width of 1 mm or more. Particularly preferably, the niobium carbide layer is formed continuously over the entire main surface and has a thickness of 0.5 μm or more.
[0105] (Appendix 5) 2. The diamond electrode according to claim 1, The niobium carbide layer has a thickness of 0.5 μm or more and 10 μm or less. More preferably, the thickness of the niobium carbide layer is not less than 0.8 μm and not more than 2.5 μm.
[0106] (Appendix 6) 2. The diamond electrode according to claim 1, The main component of the niobium carbide layer is niobium carbide having the chemical formula NbC or Nb2C.
[0107] (Appendix 7) 2. The diamond electrode according to claim 1, The niobium carbide layer has a two-layer structure, an upper layer and a lower layer, and the main component of the upper layer is niobium carbide having the chemical formula NbC, and the lower layer of the niobium carbide layer contains niobium carbide having the chemical formula Nb2C. Preferably, the main component of the lower portion is niobium carbide of formula Nb2C.
[0108] (Appendix 8) 8. The diamond electrode according to claim 7, The crystallite size of niobium carbide (NbC) contained in the upper portion of the niobium carbide layer is 1 nm or more and 100 nm or less, and preferably 5 nm or more and 60 nm or less. Preferably, the crystallite size of niobium carbide (Nb2C) contained in the lower portion of the niobium carbide layer is 10 nm or more and 2000 nm or less, more preferably 20 nm or more and 1000 nm or less.
[0109] (Appendix 9) 9. A diamond electrode according to any one of claims 1 to 8, When the surface of the conductive diamond film is observed using a scanning electron microscope, there are no pinholes reaching the substrate or the niobium carbide layer within a field of view of 20 μm×20 μm. Preferably, there are no pinholes reaching down to the substrate or the niobium carbide layer within a 1 mm x 1 mm field of view. It is particularly preferable that no pinholes reaching the substrate or the niobium carbide layer exist over the entire surface of the conductive diamond film.
[0110] (Appendix 10) According to another aspect of the present invention, A step of forming a porous portion having voids inside at least one main surface of a substrate made of metal niobium; embedding a carbon source made of a solid carbon or carbon compound inside the main surface; a step of subjecting the substrate to a heat treatment to react the niobium metal and the carbon source to form a niobium carbide layer continuously covering the main surface; and depositing a conductive diamond film on the niobium carbide layer.
[0111] (Appendix 11) A method for producing a diamond electrode according to claim 10, comprising the steps of: In the step of forming the porous portion, the substrate is heat-treated in a hydrogen atmosphere, and then cooled, thereby forming the porous portion.
[0112] (Appendix 12) A method for producing a diamond electrode according to claim 10, comprising the steps of: In the step of forming the porous portion, the porous portion is formed so that the porosity of the porous portion is 20% or more and 80% or less.
[0113] (Appendix 13) A method for producing a diamond electrode according to claim 10, comprising the steps of: After the step of forming the porous portion, hydrogen atoms bonded to the niobium metal are removed from the substrate.
[0114] (Appendix 14) A method for producing a diamond electrode according to claim 10, comprising the steps of: The method further includes the step of seeding the main surface with diamond particles prior to forming the niobium carbide layer.
[0115] (Appendix 15) A method for producing a diamond electrode according to any one of claims 10 to 14, comprising: The method further includes a step of performing processing to form projections and recesses on the main surface before forming the porous portion.
[0116] (Appendix 16) A method for producing a diamond electrode according to claim 10, comprising the steps of: In the step of forming the niobium carbide layer, the niobium carbide layer is formed so that the main component of the upper part of the niobium carbide layer is niobium carbide having the chemical formula NbC, and the main component of the lower part of the niobium carbide layer is niobium carbide having the chemical formula NbC.
[0117] (Appendix 17) A method for producing a diamond electrode according to claim 10, comprising the steps of: In the step of forming the niobium carbide layer, the niobium carbide layer is formed so that the crystal grain size of niobium carbide (NbC) contained in the niobium carbide layer is 1 nm or more and 100 nm or less. [Explanation of symbols]
[0118] 10 Diamond electrode 20 Substrate 22 Carbon Source 30 Niobium carbide layer 31 Top 32 Lower 33 Porous part 40 Conductive diamond film S101 Irregularity forming process S102 Porous part formation process S103 Carbon source embedding process S104 Seeding process S105 Niobium carbide layer formation process S106 Diamond film deposition process
Claims
1. A substrate made of metal niobium; a niobium carbide layer formed on at least one major surface of the substrate; a conductive diamond film formed on the niobium carbide layer; A diamond electrode, wherein the niobium carbide layer has a porous portion having voids.
2. The diamond electrode according to claim 1 , wherein the porous portion is present inside the niobium carbide layer near the boundary with the conductive diamond film.
3. The diamond electrode according to claim 1 , wherein the porosity of the porous portion is 20% or more and 80% or less.
4. 2. The diamond electrode according to claim 1, wherein, when a cross section of the diamond electrode is observed using a scanning electron microscope, a continuous niobium carbide layer having a thickness of 0.5 μm or more is formed over a width of 20 μm or more.
5. The diamond electrode according to claim 1 , wherein the thickness of the niobium carbide layer is 0.5 μm or more and 10 μm or less.
6. The main component of the niobium carbide layer is represented by the chemical formula NbC or Nb 2 The diamond electrode according to claim 1, which is niobium carbide of C.
7. The main component of the upper part of the niobium carbide layer is niobium carbide having the chemical formula NbC, and the lower part of the niobium carbide layer is niobium carbide having the chemical formula Nb 2 2. The diamond electrode of claim 1 comprising niobium carbide of C.
8. The diamond electrode according to claim 7, wherein the crystallite diameter of the niobium carbide contained in the upper portion of the niobium carbide layer is 1 nm or more and 100 nm or less.
9. A diamond electrode described in any one of claims 1 to 8, wherein when the surface of the conductive diamond film is observed using a scanning electron microscope, there are no pinholes reaching the substrate or the niobium carbide layer within a field of view of 20 μm x 20 μm.
10. A step of forming a porous portion having voids inside at least one main surface of a substrate made of metal niobium; embedding a carbon source made of a solid carbon or carbon compound inside the main surface; a step of subjecting the substrate to a heat treatment to react the niobium metal and the carbon source to form a niobium carbide layer continuously covering the main surface; and depositing a conductive diamond film on the niobium carbide layer.
11. The method for manufacturing a diamond electrode according to claim 10, wherein in the step of forming the porous portion, the substrate is heat-treated in a hydrogen atmosphere and then cooled to form the porous portion.
12. The method for manufacturing a diamond electrode according to claim 10, wherein in the step of forming the porous portion, the porous portion is formed so that the porosity of the porous portion is 20% or more and 80% or less.
13. The method for producing a diamond electrode according to claim 10, further comprising removing hydrogen atoms bonded to the niobium metal from the substrate after the step of forming the porous portion.
14. The method for producing a diamond electrode according to claim 10, further comprising a step of seeding the main surface with diamond particles before forming the niobium carbide layer.
15. A method for producing a diamond electrode according to any one of claims 10 to 14, further comprising a step of processing the main surface to form irregularities before forming the porous portion.
Citation Information
Patent Citations
BDD membrane electrode material and preparation method thereof
CN108486546A
Boron doped diamond electrode and preparation method thereof
CN109750291A
Electrode for electrolysis and electrolytic cell using this electrode
JP1997268395A
Electrically conductive diamond electrode and its production method
JP2005240074A
Electroconductive diamond electrode and its producing method
JP2007039720A