Electrode for electrochemical degradation of biomass wastewater, and preparation method therefor and use thereof

Through the surface oxidation pretreatment, hydrothermal reaction and high-temperature etching of boron-doped diamond electrodes, porous boron-doped diamond electrodes were prepared, which solved the problem of insufficient active area of ​​the electrode and achieved the effect of efficiently degrading biomass wastewater.

WO2024221647A1PCT designated stage expired Publication Date: 2024-10-31NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/112478
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2023-08-11
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The existing boron-doped diamond electrode has a smooth surface and limited active area, resulting in low anodization efficiency and inability to effectively degrade biomass chemical wastewater.

Method used

Through surface oxidation pretreatment, hydrothermal reaction growth of metal layer, high-temperature hydrogen etching and strong acid immersion, porous boron-doped diamond electrodes were prepared to increase the active area and conductive properties of the electrode.

Benefits of technology

It significantly improves the anodizing efficiency, can efficiently degrade biomass chemical wastewater, while reducing energy consumption, and has good industrial promotion prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023112478_31102024_PF_FP_ABST
    Figure CN2023112478_31102024_PF_FP_ABST
Patent Text Reader

Abstract

An electrode for the electrochemical degradation of biomass wastewater, and a preparation method therefor and the use thereof. The preparation method for the electrode comprises the following steps: subjecting a planar boron-doped diamond electrode to a surface oxidation pretreatment; adding a mixed solution of the pretreated boron-doped diamond electrode, a metal salt and a precipitant to a reaction kettle to perform a hydrothermal reaction, and uniformly growing a metal layer on the surface of the electrode; placing the metal / boron-doped diamond electrode into a tubular furnace, introducing hydrogen thereto to perform high-temperature etching under the catalytic action of the metal, and cooling same to obtain a metal / porous boron-doped diamond electrode; and soaking the metal / porous boron-doped diamond electrode in a strong acid to obtain a porous boron-doped diamond electrode. By means of the method, the active area of the electrode is effectively increased, the anodic oxidation efficiency is improved, and biomass wastewater from the chemical industry can be efficiently degraded.
Need to check novelty before this filing date? Find Prior Art

Description

[Corrected 22.08.2023 according to Rule 26] Electrode for electrochemical degradation of biomass wastewater and its preparation method and application Technical Field

[0001] The present invention relates to the technical field of electrocatalytic biomass, and in particular to an electrode for electrochemically degrading biomass wastewater, and a manufacturing method and application thereof. Background Art

[0002] With the increasing demand for green environmental protection, new biomass materials have gradually attracted people's attention, and the biomass chemical industry has developed rapidly. Biomass resources can be converted into a variety of high-value-added biomass compounds, such as 5-hydroxymethylfurfural (HMF) and 2,5-furandicarboxylic acid (FDCA), through catalytic conversion processes such as hydrolysis and isomerization. However, the rapid rise of the industry and the expansion of industrial production lines have also led to the emergence of environmental problems. Biomass products are usually extracted during the production process, but the extraction rate cannot reach 100%. Some biomass chemicals are still dissolved in the wastewater. These organic substances in the chemical wastewater enter the aquatic system, causing serious water pollution and ultimately endangering human life and safety. Therefore, research on the effective degradation of biomass chemical wastewater is of great significance.

[0003] Anodic oxidation, a clean, effective, and environmentally friendly water treatment method within electrochemical oxidation technology, can completely convert organic matter into substances such as CO2 and H2O under the action of an electric current. The efficiency and selectivity of anodic oxidation are largely influenced by the properties of the anode material. Boron-doped diamond (BDD) electrodes are ideal anode materials due to their excellent mechanical properties, high oxygen evolution potential, wide potential window, extremely low background current, good stability, corrosion resistance, and lack of metal contamination. However, existing BDD electrodes are mostly smooth and planar, resulting in a limited active area, which also limits the efficiency of anodic oxidation.

[0004] Summary of the Invention

[0005] In view of the shortcomings of the prior art, the technical problem to be solved by the present invention is how to increase the active area of ​​the boron-doped diamond electrode and improve the anodic oxidation efficiency.

[0006] To solve the above technical problems, the first aspect of the present invention provides a method for preparing an electrode for electrochemical degradation of biomass wastewater, comprising the following steps:

[0007] S1, performing surface oxidation pretreatment on the planar boron-doped diamond electrode;

[0008] S2, adding the pretreated boron-doped diamond electrode and a mixed solution of metal salt and precipitant into a reactor for hydrothermal reaction to uniformly grow a metal layer on the electrode surface;

[0009] S3, placing the metal / boron-doped diamond electrode in a tube furnace, introducing hydrogen gas for high-temperature etching, and cooling to obtain a metal / porous boron-doped diamond electrode;

[0010] S4. Immersing the metal / porous boron-doped diamond electrode in a strong acid to prepare a porous boron-doped diamond electrode.

[0011] The present invention takes a planar boron-doped diamond electrode as the basis, uses a hydrothermal method to grow a metal layer on the surface of the boron-doped diamond electrode, and then uses high-temperature hydrogen etching technology to prepare a porous boron-doped diamond electrode with excellent performance, effectively increasing the active area of ​​the electrode, improving the anodic oxidation efficiency, and can efficiently degrade biomass chemical wastewater.

[0012] In a preferred or optional embodiment, in step S2, the heating temperature is 90-140° C. and the heating time is 8-16 hours. By limiting the temperature and time of the hydrothermal reaction, a metal layer with small and uniform grain size can be obtained, which facilitates subsequent etching.

[0013] In a preferred or optional embodiment, in step S2, the metal salt and precipitant mixed solution has a metal salt concentration of 10 to 40 mM, a precipitant concentration of 10 to 40 mM, and a metal salt to precipitant concentration ratio of 1:1 to 2. The precipitant functions to promote the formation of a complex formed by metal ions and precipitated on the electrode surface, after which the complex is hydrothermally converted to a metal hydroxide or oxide. Typically, the ratio of metal ions to organic ligands to form a complex is 1:1, so the precipitant concentration is in excess or equal to that of the metal salt.

[0014] In a preferred or optional embodiment, the metal salt is selected from one or more of ferric nitrate, ferric sulfate, ferric chloride, ferric acetate, cobalt nitrate, cobalt sulfate, cobalt chloride, cobalt acetate, nickel nitrate, nickel sulfate, nickel chloride, and nickel acetate, and the precipitant is selected from one or more of hexamethylenetetramine, urea, and ethylenediaminetetraacetic acid.

[0015] In a preferred or optional embodiment, the step S3 specifically includes: placing the metal / boron-doped diamond electrode in a tube furnace, introducing an inert gas and heating it to 850-950°C at a heating rate of 5-15°C / min, keeping it warm for 10-60 minutes, introducing a hydrogen flow at the beginning of the insulation, and keeping the inert gas flow rate constant. After the insulation is completed, the hydrogen flow is cut off and the electrode is cooled naturally. In the case of pure inert gas, an etching reaction will also occur, although the reaction is very slow. If the heating rate is too slow, the heating time will be too long, which may increase the degree of etching and cause damage to the electrode surface. The insulation temperature and insulation time are important conditions for the etching reaction. If the temperature is too low, etching cannot be carried out, and if the temperature is too high, etching will be excessive. If the insulation time is too short, the degree of etching is shallow, and the performance improvement is small. If the insulation time is long, the degree of etching is deep, the surface is severely damaged, and the performance is seriously affected.

[0016] In a preferred or optional embodiment, in step S3, the inert gas flow rate is 20 to 60 mL min -1 , hydrogen flow rate is 20~60mL·min -1 The flow rate ratio of inert gas to hydrogen is 1 to 2:1. Hydrogen is a reactant in the diamond etching reaction. Surface metal hydroxides or oxides are reduced by hydrogen to form metal particles, which catalyze hydrogen etching of the electrode surface. The gas flow rate can control the sufficient amount of hydrogen in the reaction. The inert gas mainly assists in etching and isolates oxygen, and its flow rate is coordinated with the hydrogen.

[0017] In a preferred or optional embodiment, in step S4, the strong acid is selected from one or more of concentrated hydrochloric acid, concentrated sulfuric acid, and concentrated nitric acid, and the soaking time is 12 to 24 hours. The soaking time is limited to ensure that the metal is completely reacted with the strong acid.

[0018] In a preferred or optional embodiment, step S1 specifically includes:

[0019] S11, the planar boron-doped diamond electrode was subjected to constant current oxidation in the electrolyte for 20 to 60 minutes at a current of 50 to 70 mA;

[0020] S12, ultrasonically cleaning the oxidized electrode sheet with water and ethanol in sequence;

[0021] S13. Soak the cleaned electrode sheets in concentrated nitric acid for 20 to 40 minutes.

[0022] The surface of commercial boron-doped diamond electrodes usually has an attached carbon deposit layer, which is removed by constant current oxidation; water and ethanol cleaning removes residual inorganic and organic pollutants on the surface; concentrated nitric acid treatment can change the hydrophobicity of the electrode surface, making the electrode surface hydrophilic, which facilitates better growth of the metal layer.

[0023] A second aspect of the present invention provides an electrode for electrochemical degradation of biomass wastewater, produced by the aforementioned preparation method. The electrode surface is provided with a plurality of pores, each 50 to 500 nm in size. The method of the present invention forms a large number of pores on the surface of the boron-doped diamond electrode, thereby increasing the active area of ​​the electrode and significantly improving its electrical conductivity while retaining its other excellent properties.

[0024] A second aspect of the present invention provides the use of the aforementioned electrode to degrade biomass wastewater containing furanic compounds under the oxidative action of the electrode, mineralizing the organic matter into carbon dioxide. The electrode prepared by the present invention can be used for electrochemical degradation of biomass wastewater, thereby improving degradation efficiency and reducing energy consumption.

[0025] In summary, compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) The present invention uses a hydrothermal method combined with a thermal etching method to process a planar boron-doped diamond electrode. The operation is simple and repeatable. The metal particle size and pore size are controllable, and a porous boron-doped diamond electrode with a large number of nano-scale pores distributed on the surface can be prepared.

[0027] (2) The preparation method of the present invention etches only the surface of the boron-doped diamond electrode, thereby increasing the active area of ​​the electrode and retaining the excellent performance of the boron-doped diamond electrode.

[0028] (3) The electrical conductivity of porous boron-doped diamond electrodes has been significantly improved, which can improve the degradation efficiency of biomass wastewater while reducing energy consumption, and has good prospects for industrial promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] FIG1 is a microscopic morphology of a planar boron-doped diamond electrode in Example 1 of the present invention.

[0030] FIG2 is a microscopic morphology of the nickel / boron-doped diamond electrode in Example 1 of the present invention.

[0031] FIG3 is a microscopic morphology of the nickel / porous boron-doped diamond electrode in Example 1 of the present invention.

[0032] FIG4 is a microscopic morphology of the porous boron-doped diamond electrode in Example 1 of the present invention.

[0033] FIG5 is a graph showing the LSV curves of the electrodes of Example 1 and Comparative Example 1 in Example 4 of the present invention.

[0034] FIG6 is a statistical curve diagram of substrate removal rate and chemical oxygen demand removal rate during electrolysis using the electrode prepared in Example 1 as the anode in Example 5 of the present invention.

[0035] FIG7 is a statistical curve diagram of the chemical oxygen demand removal rate in the electrolysis process using the electrodes of Example 1 and Comparative Example 1 as anodes in Example 6 of the present invention.

[0036] FIG8 is a statistical curve diagram of the chemical oxygen demand removal rate in the electrolysis process using the electrode of Example 2 as the anode in Example 7 of the present invention. DETAILED DESCRIPTION

[0037] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0038] It should be understood that the terms described herein are intended only to describe particular embodiments and are not intended to limit the present invention. In addition, for numerical ranges herein, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Each smaller range between any intermediate value within a stated value or stated range and any other stated value or intermediate value within the stated range is also encompassed by the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded within the scope.

[0039] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments described herein without departing from the scope or spirit of the invention. Other embodiments will be apparent to those skilled in the art from the description of the invention. The present description and examples are intended to be illustrative only.

[0040] A specific embodiment of the present invention provides an electrode for electrochemical degradation of biomass wastewater, which is prepared by the following method:

[0041] S1. Pre-treating the surface of the planar boron-doped diamond electrode by surface oxidation.

[0042] The specific steps of pretreatment include: constant current oxidation of the planar boron-doped diamond electrode in an electrolyte with a current of 50 to 70 mA for 20 to 60 minutes, and the electrolyte is sulfuric acid and / or sodium sulfate, and the carbon deposit layer attached to the surface of the boron-doped diamond electrode is removed by constant current oxidation; the oxidized electrode sheet is ultrasonically cleaned with water and ethanol in turn to remove inorganic and organic pollutants remaining on the surface; the cleaned electrode sheet is soaked in concentrated nitric acid for 20 to 40 minutes. The concentrated nitric acid treatment can change the hydrophobicity of the electrode surface, making the electrode surface hydrophilic, which facilitates the subsequent better growth of the metal layer.

[0043] S2. Adding the boron-doped diamond electrode pretreated in step S1 and a mixed solution of metal salt and precipitant into a reactor to carry out a hydrothermal reaction, thereby uniformly growing a metal layer on the surface of the electrode.

[0044] In a specific embodiment, in the mixed solution of metal salt and precipitant, the concentration of metal salt is 10-40 mM, the concentration of precipitant is 10-40 mM, and the concentration ratio of metal salt to precipitant is 1:1-2; the metal salt is ferric nitrate, ferric sulfate, ferric chloride, ferric acetate, cobalt nitrate, cobalt sulfate, cobalt chloride, cobalt acetate, nickel nitrate, nickel sulfate, nickel chloride, nickel acetate, etc., and the precipitant is hexamethylenetetramine, urea, ethylenediaminetetraacetic acid, etc. The precipitant can promote the metal ions to form a complex and precipitate on the electrode surface, and then the complex is converted into a metal hydroxide or oxide by hydrothermal conversion, and a metal layer is uniformly grown on the electrode surface.

[0045] In a specific embodiment, the heating temperature of the hydrothermal reaction is 90-140° C., and the heating time is 8-16 hours, so as to obtain a metal layer with small and uniformly distributed grains, which is convenient for subsequent etching.

[0046] S3. Place the metal / boron-doped diamond electrode prepared in step S2 into a tube furnace, introduce hydrogen gas for high-temperature etching, and cool to obtain a metal / porous boron-doped diamond electrode.

[0047] The high-temperature hydrogen etching step specifically includes: placing the metal / boron-doped diamond electrode in a tube furnace, introducing inert gas and heating it to 850-950°C at a heating rate of 5-15°C / min, keeping it warm for 10-60 minutes, introducing hydrogen flow at the beginning of the insulation, and keeping the inert gas flow rate unchanged. After the insulation is completed, the hydrogen flow is cut off and the furnace is cooled naturally.

[0048] In a specific embodiment, the inert gas flow rate is 20 to 60 mL min -1 , hydrogen flow rate is 20~60mL·min -1 The flow rate ratio of the inert gas flow and the hydrogen gas is 1 to 2:1, and the gas flow rate is controlled to ensure sufficient hydrogen in the reaction.

[0049] S4. Soaking the metal / porous boron-doped diamond electrode obtained in step S3 in a strong acid to obtain a porous boron-doped diamond electrode.

[0050] In a specific embodiment, the strong acid is selected from one or more of concentrated hydrochloric acid, concentrated sulfuric acid, and concentrated nitric acid, and the soaking time is 12 to 24 hours to ensure that the metal is completely reacted by the strong acid.

[0051] The above method is based on a planar boron-doped diamond electrode, and uses a hydrothermal method to grow a metal layer on the surface of the boron-doped diamond electrode. It then combines high-temperature hydrogen etching technology to prepare a porous boron-doped diamond electrode with excellent performance. There are multiple holes distributed on the surface of the porous boron-doped diamond electrode, and the size of the holes is 50 to 500 nm, which effectively increases the active area of ​​the electrode, improves the efficiency of anodization, and can efficiently degrade biomass chemical wastewater.

[0052] The above preparation method is simple to operate, highly repeatable, and the particle size of the metal particles and the pore size are controllable. While etching the electrode surface, the excellent performance of the boron-doped diamond electrode is retained.

[0053] Another embodiment of the present invention provides an application of the above-mentioned porous boron-doped diamond electrode, using biomass wastewater containing furan compounds as a solution and the porous boron-doped diamond electrode as a working electrode to carry out a constant voltage electrolysis reaction.

[0054] In a specific embodiment, the constant voltage electrolysis reaction conditions are as follows: the reaction voltage is 5 to 6 V, and the reaction time is 2.5 h to 7 h.

[0055] In a specific embodiment, the furan compound is selected from one or more of furan, furfural, 2,5-furan dimethanol, 5-hydroxymethylfurfural, 5-hydroxymethyl-2-furancarboxylic acid, 2,5-furandicarboxaldehyde, 5-formyl-2-furancarboxylic acid, and 2,5-furandicarboxylic acid.

[0056] Compared with planar boron-doped diamond electrodes, porous boron-doped diamond electrodes have significantly improved conductivity, can improve the degradation efficiency of biomass wastewater, and reduce energy consumption at the same time, and have good prospects for industrial promotion.

[0057] The technical effects of the present invention are described below with reference to specific embodiments.

[0058] Example 1

[0059] (1) Using a planar boron-doped diamond electrode as raw material, its micromorphology is shown in Figure 1. The planar boron-doped diamond electrode was subjected to constant current oxidation in sulfuric acid at a current of 50 mA for 30 minutes, ultrasonically cleaned with water and ethanol for 10 minutes, then soaked in concentrated nitric acid for 40 minutes, rinsed with deionized water, and air-dried.

[0060] (2) Prepare 50 mL of a mixed solution of 20 mM nickel sulfate and 40 mM hexamethylenetetramine. Place the planar boron-doped diamond electrode and the solution in a 100 mL hydrothermal reactor. React at 120°C for 10 h. Remove the electrode, rinse it with ethanol and deionized water, and dry it naturally to obtain a nickel / boron-doped diamond electrode. The micromorphology of the nickel / boron-doped diamond electrode after hydrothermal treatment is shown in Figure 2. A nickel layer has grown uniformly on the electrode surface.

[0061] (3) Place the nickel / boron-doped diamond electrode in a tube furnace and adjust the nitrogen flow rate to 40 mL min -1 , and set the tube furnace at 10℃·min -1 The heating rate was raised to 850℃ and kept at this temperature for 0.5h. At the beginning of the heating, the flow rate was 40mL·min -1 The hydrogen and nitrogen flow rates were kept constant. After the heat preservation period, the hydrogen flow was cut off, and the electrode was allowed to cool naturally, yielding a nickel / porous boron-doped diamond electrode. The micromorphology of the nickel / porous boron-doped diamond electrode is shown in Figure 3, showing numerous pores on the electrode surface.

[0062] (4) The nickel / porous boron-doped diamond electrode was immersed in concentrated hydrochloric acid for 12 h, rinsed with ethanol and deionized water, and then dried to obtain a porous boron-doped diamond electrode. The micromorphology of the porous boron-doped diamond electrode is shown in FIG4 .

[0063] Example 2

[0064] (1) The planar boron-doped diamond electrode was subjected to constant current oxidation in sodium sulfate at a current of 50 mA for 60 min; ultrasonic cleaning was performed in water and ethanol for 10 min in sequence; then, it was soaked in concentrated nitric acid for 40 min, rinsed with deionized water, and air-dried.

[0065] (2) Prepare 50 mL of a mixed solution of 40 mM cobalt sulfate and 40 mM urea, place the planar boron-doped diamond electrode and the solution into a 100 mL hydrothermal reactor, and react at 90 °C for 8 h. Remove the electrode, rinse it with ethanol and deionized water, and dry it naturally to obtain a cobalt / boron-doped diamond electrode.

[0066] (3) Place the cobalt / boron-doped diamond electrode in a tube furnace and adjust the nitrogen flow rate to 20 mL min -1 , set the tube furnace at 10℃·min -1 The heating rate was raised to 900℃ and kept at this temperature for 1h. At the beginning of the heating, the flow rate was 20mL·min -1 The hydrogen and nitrogen flows remain unchanged, and after the heat preservation is completed, the hydrogen flow is cut off, and then the electrode is cooled naturally to obtain a cobalt / porous boron-doped diamond electrode;

[0067] (4) The cobalt / porous boron-doped diamond electrode was immersed in concentrated hydrochloric acid for 12 hours, rinsed with ethanol and deionized water, and then dried to obtain a porous boron-doped diamond electrode.

[0068] Example 3

[0069] (1) The planar boron-doped diamond electrode was subjected to constant current oxidation in sodium sulfate at a current of 70 mA for 20 min; ultrasonic cleaning was performed in water and ethanol for 10 min in sequence; then, it was soaked in concentrated nitric acid for 40 min, rinsed with deionized water, and air-dried.

[0070] (2) Prepare 50 mL of a mixed solution of 20 mM ferric sulfate and 20 mM ethylenediaminetetraacetic acid, place the planar boron-doped diamond electrode and the solution into a 100 mL hydrothermal reactor, and react at 140 ° C for 16 h. Take out the electrode, rinse it with ethanol and deionized water, and dry it naturally to obtain an iron / boron-doped diamond electrode.

[0071] (3) Place the iron / boron-doped diamond electrode in a tube furnace and adjust the nitrogen flow rate to 40 mL min -1 , set the tube furnace at 10℃·min -1 The heating rate was raised to 950℃ and kept at this temperature for 0.5h. At the beginning of the heating, the flow rate was 40mL·min -1 The hydrogen and nitrogen flows remain unchanged, and after the heat preservation is completed, the hydrogen flow is cut off, and then the electrode is cooled naturally to obtain an iron / porous boron-doped diamond electrode;

[0072] (4) The iron / porous boron-doped diamond electrode was immersed in concentrated hydrochloric acid for 12 hours, rinsed with ethanol and deionized water, and then dried to obtain a porous boron-doped diamond electrode.

[0073] Comparative Example 1

[0074] A planar boron-doped diamond electrode was used as a comparative example.

[0075] Example 4

[0076] (1) The porous boron-doped diamond electrode prepared in Example 1 and the planar boron-doped diamond electrode prepared in Comparative Example 1 were respectively installed on an electrochemical workstation as anodes. 20 mL of 0.1 M Na2SO4 solution was used as the electrolyte. A titanium sheet was used as the counter electrode, and a silver-silver chloride electrode was used as the reference electrode. The area of ​​the catalyst immersed in the electrolyte was 2 × 1 cm 2 and stirred with a magnetic stirrer at a speed of 200 rpm.

[0077] (2) The LSV curve was obtained using the linear scan method of the electrochemical workstation with a scan rate of 5 mV / s and a scan range of 1.0 to 3.0 V. The results are shown in Figure 5 , which shows that the conductive performance of the porous boron-doped diamond electrode is significantly improved compared with the planar boron-doped diamond electrode.

[0078] Example 5

[0079] (1) 5-HMF was added to 150 mL of 0.1 M Na2SO4 electrolyte as a model pollutant. The concentration of 5-HMF was 500 mg·L -1 .

[0080] (2) Take a piece of porous boron-doped diamond electrode prepared in Example 1 as the anode and a titanium sheet as the cathode, and assemble them into a two-electrode system without a diaphragm with the above electrolyte. The area of ​​the electrodes immersed in the electrolyte is 2×2 cm 2 , using magnetic stirring at a speed of 200 rpm.

[0081] (3) The working voltage was set to 6 V, and the electrolysis was performed for 2.5 h. The 5-HMF removal rate and the chemical oxygen demand removal rate during the electrolysis process were statistically analyzed. The results are shown in FIG6 . The final 5-HMF removal rate was 94.20%, and the chemical oxygen demand removal rate was 55.57%.

[0082] Example 6

[0083] (1) 5-HMF was added to 150 mL of 0.1 M Na2SO4 electrolyte as a model pollutant. The concentration of 5-HMF was 1000 mg·L -1 .

[0084] (2) Take a porous boron-doped diamond electrode prepared in Example 1 and a planar boron-doped diamond electrode prepared in Comparative Example 1 as the anode, and a titanium sheet as the cathode, and assemble them into a diaphragm-free double-electrode system with the above electrolyte. The area of ​​the electrodes immersed in the electrolyte is 2×2 cm 2 , using magnetic stirring at a speed of 200 rpm.

[0085] (3) The operating voltage was set to 6 V and electrolysis was performed for 4 h. During the process, the chemical oxygen demand removal rate curves of the two electrodes as anodic oxidation were calculated. The results are shown in FIG7 . The chemical oxygen demand removal rate corresponding to the electrode of Example 1 reached 68.43%, and the chemical oxygen demand removal rate corresponding to the electrode of Comparative Example 1 was 62.99%. It can be seen that the porous boron-doped diamond electrode has a higher biomass wastewater degradation efficiency.

[0086] Example 7

[0087] (1) 5-HMF was added to 150 mL of 0.1 M Na2SO4 electrolyte as a model pollutant. The concentration of 5-HMF was 500 mg·L -1 .

[0088] (2) A porous boron-doped diamond electrode prepared in Example 2 was used as the anode, and a titanium sheet was used as the cathode. The electrodes were assembled into a two-electrode system without a diaphragm and the electrolyte was prepared. The area of ​​the catalyst immersed in the electrolyte was 2 × 2 cm. 2 , using magnetic stirring at a speed of 200 rpm.

[0089] (3) The working voltage was set to 6 V and electrolysis was performed for 7 h. The chemical oxygen demand removal rate curve during the electrolysis process is shown in FIG8 , and reached 94.87% at the end of the electrolysis.

[0090] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A method for preparing an electrode for electrochemical degradation of biomass wastewater, It is characterized in that The following steps are involved: S1, performing surface oxidation pretreatment on the planar boron-doped diamond electrode; S2, adding the pretreated boron-doped diamond electrode and a mixed solution of a metal salt and a precipitant into a reactor for hydrothermal reaction to uniformly grow a metal layer on the surface of the electrode; S3, placing the metal / boron-doped diamond electrode into a tube furnace, introducing hydrogen gas for high-temperature etching, and cooling to obtain a metal / porous boron-doped diamond electrode; S4. Immerse the metal / porous boron-doped diamond electrode in a strong acid to obtain a porous boron-doped diamond electrode.

2. The method for preparing an electrode for electrochemical degradation of biomass wastewater according to claim 1, It is characterized in that In step S2, the heating temperature is 90-140° C. and the heating time is 8-16 hours.

3. The method for preparing an electrode for electrochemical degradation of biomass wastewater according to claim 2, It is characterized in that In the step S2, in the mixed solution of metal salt and precipitant, the concentration of metal salt is 10-40 mM, the concentration of precipitant is 10-40 mM, and the concentration ratio of metal salt to precipitant is 1:1-2.

4. The method for preparing an electrode for electrochemical degradation of biomass wastewater according to claim 3, It is characterized in that The metal salt is selected from one or more of ferric nitrate, ferric sulfate, ferric chloride, ferric acetate, cobalt nitrate, cobalt sulfate, cobalt chloride, cobalt acetate, nickel nitrate, nickel sulfate, nickel chloride, and nickel acetate; and the precipitant is selected from one or more of hexamethylenetetramine, urea, and ethylenediaminetetraacetic acid.

5. The method for preparing an electrode for electrochemical degradation of biomass wastewater according to claim 1, It is characterized in that The step S3 specifically comprises: placing the metal / boron-doped diamond electrode into a tubular furnace, introducing an inert gas and heating the temperature to 850-950° C. at a heating rate of 5-15° C. / min, keeping the temperature for 10-60 minutes, introducing a hydrogen flow at the beginning of the heat preservation, and keeping the flow rate of the inert gas unchanged, and cutting off the hydrogen flow after the heat preservation is completed, and cooling naturally.

6. The method for preparing an electrode for electrochemical degradation of biomass wastewater according to claim 5, It is characterized in that In step S3, the inert gas flow rate is 20 to 60 mL min -1 , hydrogen flow rate is 20~60mL·min -1 , the flow rate ratio of the inert gas flow and the hydrogen gas is 1 to 2:

1.

7. The method for preparing an electrode for electrochemical degradation of biomass wastewater according to claim 1, It is characterized in that In step S4, the strong acid is selected from one or more of concentrated hydrochloric acid, concentrated sulfuric acid, and concentrated nitric acid, and the soaking time is 12 to 24 hours.

8. The method for preparing an electrode for electrochemical degradation of biomass wastewater according to claim 1, It is characterized in that The step S1 specifically includes: S11, the planar boron-doped diamond electrode is subjected to constant current oxidation in an electrolyte for 20 to 60 min at a current of 50 to 70 mA; S12, ultrasonically cleaning the oxidized electrode sheet with water and ethanol in turn; S13. Soak the cleaned electrode in concentrated nitric acid for 20 to 40 minutes.

9. An electrode for electrochemical degradation of biomass wastewater, It is characterized in that The electrode is prepared by the preparation method according to any one of claims 1 to 8, wherein a plurality of holes are distributed on the surface of the electrode, and the size of the holes is 50 to 500 nm.

10. Use of the electrode as claimed in claim 9, It is characterized in that Biomass wastewater containing furan compounds is degraded under the oxidation action of the electrode, and organic matter is mineralized into carbon dioxide.

Citation Information

Patent Citations

  • Preparation method for graphene load flower-shaped porous nickel oxide composite materials

    CN103943379A

  • Ferrite-modified modified carbon fiber cloth electrode, preparation method and application thereof

    CN110156119A

  • Treatment method and treatment system for organic wastewater

    CN115180705A

  • Porous diamond layer, method for producing porous diamond particle and electrode for electrochemistry using them

    JP2006183102A

  • Boron doped diamond electrode and preparation method and applications thereof

    US20200048776A1