Phenoxy resin, method for producing the same, resin composition and cured product

The use of a carboxylic acid salt of a quaternary phosphonium salt as a catalyst in the production of phenoxy resin addresses storage stability issues, ensuring high reaction rates and stability when blended with curing agents, thereby improving the resin's performance in thermosetting applications.

JP2024135604APending Publication Date: 2024-10-04NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
JP2023046383
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing methods for producing phenoxy resins using onium salt compounds and alkaline compounds as catalysts result in insufficient storage stability when mixed with other materials, and triphenylphosphine catalysts have low reaction activity in two-step processes.

Method used

Using a carboxylic acid salt of a quaternary phosphonium salt as a catalyst for the reaction between a bifunctional epoxy resin and a bifunctional compound with phenolic hydroxyl or active ester groups, achieving a weight average molecular weight of 10,000 to 150,000, and incorporating 0.001 to 5% by mass of the catalyst in the phenoxy resin.

Benefits of technology

The method ensures sufficient reaction rate, low epoxy equivalent weight, and excellent storage stability of the phenoxy resin when mixed with curing components, reducing the need to remove residual catalysts and enhancing the resin's suitability for thermosetting applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135604000001
    Figure 2024135604000001
  • Figure 2024135604000002
    Figure 2024135604000002
  • Figure 2024135604000003
    Figure 2024135604000003
Patent Text Reader

Abstract

To provide a method for producing a phenoxy resin which sufficiently proceeds reaction, when reacting a bifunctional epoxy resin with a bifunctional compound having two phenolic hydroxyl groups and / or active ester groups as functional groups in one molecule by a two-stage method, and is excellent in storage stability when the obtained phenoxy resin is blended with other material, and a phenoxy resin obtained by the production method, a phenoxy resin composition, and a cured product.SOLUTION: A method for producing a phenoxy resin reacts a bifunctional epoxy resin with a bifunctional compound having two phenolic hydroxyl groups and / or active ester groups as functional groups in one molecule in the presence of a carboxylate of a quaternary phosphonium salt represented by the following formula (1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a phenoxy resin having excellent reactivity and excellent storage stability when the resulting phenoxy resin is mixed with other components, particularly with a curing component, and to a phenoxy resin obtained by the method. The present invention also relates to a resin composition and a cured product obtained by using the phenoxy resin. [Background technology]

[0002] Epoxy resins are widely used in the fields of paints, civil engineering, adhesion, electrical materials, etc., because of their excellent heat resistance, adhesiveness, chemical resistance, water resistance, mechanical strength, and electrical properties. Film-forming properties are imparted by increasing the molecular weight in various ways. Such highly molecular epoxy resins are called phenoxy resins. In particular, bisphenol A-type phenoxy resins are mainly used as base resins for paint varnishes and base resins for film molding, and are added to epoxy resin varnishes to adjust the flowability and improve the toughness and adhesiveness of the cured product. In addition, those having phosphorus atoms or bromine atoms in the skeleton are used as flame retardants to be blended with epoxy resin compositions and thermoplastic resins.

[0003] Generally, known methods for producing phenoxy resin include the "one-step method" in which a bifunctional phenolic compound is reacted with epihalohydrin in the presence of an alkali, and the "two-step method" in which a bifunctional epoxy resin is reacted with a bifunctional phenolic compound in the presence of a catalyst. The two-step method is known to be suitable for producing phenoxy resin, which is difficult to purify after synthesis, because it produces almost no by-products such as salt compared to the one-step method. Non-Patent Document 1 describes that onium salt compounds, alkaline compounds, etc. are generally used as catalysts when producing phenoxy resin by the two-step method.

[0004] When phenoxy resin is used in the fields of paint, civil engineering, adhesives, electrical materials, etc., as described above, it is mainly used as a base resin, and is generally used as a mixture with multiple materials including epoxy resins and curing agents. According to detailed studies by the present inventors, when produced by the two-stage method, phenoxy resins using onium salt compounds and alkaline compounds as catalysts as described in Non-Patent Document 1 above may have insufficient storage stability when mixed with other materials. In addition, Non-Patent Document 1 also describes the use of triphenylphosphine as a catalyst as a phosphorus compound, but triphenylphosphine has insufficient activity as a catalyst for the two-stage method. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] General Review of Epoxy Resins, Vol. 1, Basics I, Epoxy Resin Technology Association (2003) Summary of the Invention [Problem to be solved by the invention]

[0006] The object of the present invention is to provide a method for producing a phenoxy resin, which allows the reaction to proceed sufficiently when a bifunctional epoxy resin is reacted with a bifunctional compound having two phenolic hydroxyl groups and / or active ester groups as functional groups in one molecule in a two-stage process, and which provides a phenoxy resin having excellent storage stability when blended with other materials. Another object of the present invention is to provide a phenoxy resin obtained by this production method, and a phenoxy resin composition and cured product containing the same. [Means for solving the problem]

[0007] As a result of intensive investigations aimed at solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by using a specific quaternary phosphonium carboxylate as a catalyst when a phenoxy resin is obtained from a bifunctional epoxy resin and a bifunctional compound having two phenolic hydroxyl groups and / or active ester groups as functional groups in one molecule as raw materials, and have thus completed the present invention.

[0008] That is, the present invention is a method for producing a phenoxy resin having a weight average molecular weight (Mw) of 10,000 to 150,000 by reacting a bifunctional epoxy resin with a bifunctional compound having two phenolic hydroxyl groups and / or active ester groups as functional groups in one molecule in the presence of a catalyst, wherein the catalyst is a carboxylate of a quaternary phosphonium salt represented by the following formula (1). [ka] In the formula, R 1 ~R 4 each independently represents an alkyl group, an aryl group, or an aralkyl group, and may be the same or different groups. X is a residue obtained by removing two carboxy groups from a polycarboxylic acid.

[0009] The above X is preferably any one of the divalent groups represented by the following formulas (2a) to (2d). [ka] In the formula, R 5 ~R 8 R each independently represents a hydrogen atom, an alkyl group, a hydroxyl group, an amino group, a carboxyl group, or a carboxyalkyl group. 10 is a methylene group or an ethylene group, R 11 ~R 18 R is each independently a hydrogen atom, an alkyl group, or a carboxy group. 19 ~R 22 each independently represents a hydrogen atom, an alkyl group, a hydroxyl group, an amino group, or an alkoxy group.

[0010] It is preferable to use 0.95 to 1.05 mol of the bifunctional compound per 1.0 mol of the bifunctional epoxy resin, and the amount of the quaternary phosphonium carboxylate used is preferably 0.001 to 5 mass % of the total amount of the bifunctional epoxy resin and the bifunctional compound used.

[0011] It is preferable that a part or all of the above-mentioned bifunctional epoxy resin, a part or all of the above-mentioned bifunctional compound, or both are phosphorus-containing compounds containing phosphorus in the molecule, and the phosphorus content of the obtained phenoxy resin is preferably 1 to 6 mass%. The epoxy equivalent of the resulting phenoxy resin is preferably 4,000 to 200,000 g / eq. The present invention also relates to a phenoxy resin obtained by the above production method.

[0012] The present invention also relates to a phenoxy resin having an Mw of 10,000 to 150,000, characterized in that the phenoxy resin contains 0.001 to 5 mass % of a carboxylate of a quaternary phosphonium salt represented by the above formula (1).

[0013] The present invention also relates to a resin composition comprising the above-mentioned phenoxy resin and a curing component. The curing component is preferably at least one selected from epoxy resins, acrylic ester resins, melamine resins, urea resins, phenolic resins, acid anhydride compounds, amine compounds, imidazole compounds, amide compounds, cationic polymerization initiators, organic phosphines, polyisocyanate compounds, and blocked isocyanate compounds. The resin composition preferably further contains a filler.

[0014] The present invention also relates to a cured product obtained by curing the above resin composition, and to a laminate for electric / electronic circuits obtained by using the above resin composition. Effect of the Invention

[0015] The method for producing the phenoxy resin of the present invention has a sufficient reaction rate. In addition, the phenoxy resin of the present invention has a relatively low epoxy equivalent and many remaining epoxy groups, so the phenoxy resin itself can participate in curing. It also has excellent storage stability when other components, especially curing components, are mixed. In addition, when solidifying the phenoxy resin, unnecessary polymerization, etc. may occur due to the heat history applied during reaction solvent recovery, so it is common to remove or inactivate the remaining catalyst. However, in the production method of the present invention, such reactions such as polymerization caused by the remaining catalyst hardly occur, so there is no need to remove the remaining catalyst, which is also advantageous in terms of cost. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will be described in detail below based on preferred embodiments thereof. The method for producing the phenoxy resin of the present invention involves reacting a bifunctional epoxy resin with a compound having two phenolic hydroxyl groups and / or active ester groups (acyloxy groups) as functional groups in one molecule in the presence of a carboxylate of a quaternary phosphonium salt represented by the above formula (1) (a salt of a phosphonium cation and an anion residue of a polycarboxylic acid). In this specification, the method for producing the phenoxy resin of the present invention may be referred to as the "production method of the present invention." The phenoxy resin obtained by the production method of the present invention may be referred to as the phenoxy resin of the present invention. A bifunctional compound having two phenolic hydroxyl groups and / or active ester groups (acyloxy groups) as functional groups in one molecule may be simply referred to as a "bifunctional compound." In addition, in this specification, the term "anionic residue of a polycarboxylic acid" refers to a monovalent or divalent or higher (typically monovalent) carboxyl anion resulting from the removal of a hydrogen atom from one or more (typically one) carboxyl groups of a polycarboxylic acid.

[0017] The bifunctional epoxy resin used in the method for producing the phenoxy resin of the present invention may be an epoxy resin having two epoxy groups in the molecule. If the purity of the bifunctional epoxy resin is high, it may contain a positional isomer or an oligomer. These bifunctional epoxy resins may be used alone or in combination.

[0018] Examples of bifunctional epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol E type epoxy resins, bisphenol Z type epoxy resins, bisphenol S type epoxy resins, bisphenol AD ​​type epoxy resins, bisphenol acetophenone type epoxy resins, bisphenol trimethylcyclohexane type epoxy resins, bisphenol fluorene type epoxy resins (e.g., ZX-1201 (manufactured by Nippon Steel Chemical & Material Co., Ltd.) and the like), biscresol fluorene type epoxy resins (e.g., OGSOL bisphenol type epoxy resins such as tetramethylbisphenol A type epoxy resins, tetramethylbisphenol F type epoxy resins (e.g., YSLV-80XY (manufactured by Nippon Steel Chemical & Material Co., Ltd.)), tetra-t-butylbisphenol A type epoxy resins, tetramethylbisphenol S type epoxy resins, dihydroxydiphenyl ether type epoxy resins, thiodiphenol type epoxy resins, tetra-t-butylbisphenol A type epoxy resins, and tetrabromobisphenol A type epoxy resins; biphenol type epoxy resins, tetramethylbiphenol type epoxy resins (e.g., YX4000 (manufactured by Mitsubishi Chemical Co., Ltd.)); Examples of the epoxy resin include biphenol-type epoxy resins such as tetra-t-butylbiphenol-type epoxy resins, hydroquinone-type epoxy resins, methylhydroquinone-type epoxy resins, di-t-butylhydroquinone-type epoxy resins (for example, YDC-1312 (manufactured by Nippon Steel Chemical & Material Co., Ltd.)), benzenediol-type epoxy resins such as resorcin-type epoxy resins, methylresorcin-type epoxy resins, and catechol-type epoxy resins, dihydroxyanthracene-type epoxy resins, hydroanthrahydroquinone-type epoxy resins, dihydroxynaphthalene-type epoxy resins, bisnaphtholfluorene-type epoxy resins, and diphenyldicyclopentadiene-type epoxy resins.

[0019] Further, bifunctional epoxy resins in which hydrogen has been added to the aromatic rings of the above-mentioned bifunctional epoxy resins, glycidyl ester type epoxy resins produced from various dicarboxylic acids such as adipic acid, succinic acid, phthalic acid, tetrahydrophthalic acid, methylhexahydrophthalic acid, terephthalic acid, isophthalic acid, orthophthalic acid, biphenyldicarboxylic acid, and dimer acid, and epihalohydrin, glycidyl amine type epoxy resins produced from an amine compound such as aniline, and epihalohydrin, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, polytetramethylene glycol diglycidyl ether, 1,5-pentanediol diglycidyl ether, polypentamethylene glycol diglycidyl ether, Examples of the epoxy resin include (poly)alkylene glycol type epoxy resins consisting only of a chain structure, such as 1,4-cyclohexanedimethanol diglycidyl ether, 1,6-hexanediol diglycidyl ether, polyhexamethylene glycol diglycidyl ether, 1,7-heptanediol diglycidyl ether, polyheptamethylene glycol diglycidyl ether, 1,8-octanediol diglycidyl ether, 1,10-decanediol diglycidyl ether, and 2,2-dimethyl-1,3-propanediol diglycidyl ether; alkylene glycol type epoxy resins having a cyclic structure, such as 1,4-cyclohexanedimethanol diglycidyl ether; aliphatic cyclic epoxy resins; and phosphorus-containing bifunctional epoxy resins (for example, FX-305 (manufactured by Nippon Steel Chemical & Material Co., Ltd.), diphenylphosphinylhydroquinone diglycidyl ether, etc.).

[0020] In order to improve the heat resistance of the phenoxy resin, dihydroxynaphthalene type epoxy resins, bisphenol fluorene type epoxy resins, biscresol fluorene type epoxy resins, and bisnaphthol fluorene type epoxy resins are preferred, and bifunctional epoxy resins having a fluorene ring structure such as bisphenol fluorene type epoxy resins, biscresol fluorene type epoxy resins, and bisnaphthol fluorene type epoxy resins are more preferred. In order to impart flame retardancy, tetrabromobisphenol A epoxy resins and phosphorus-containing difunctional epoxy resins are preferred, with phosphorus-containing difunctional epoxy resins being more preferred.

[0021] The bifunctional compound used in the production method of the present invention may be any one of a diphenol compound (B1) having two hydroxyl groups bonded to an aromatic ring, a diester compound (B2) having two acyloxy groups bonded to an aromatic ring, and a monoester compound (B3) having one hydroxyl group and one acyloxy group bonded to an aromatic ring. The diester compound (B2) and the monoester compound (B3) may be referred to as "ester compounds" without distinction. If the purity of the bifunctional compound is high, positional isomers may be included. These bifunctional compounds may be used alone or in combination. The acyloxy group is represented by R-CO-O-, where R is a hydrocarbon group having 1 to 19 carbon atoms. As the hydrocarbon group having 1 to 19 carbon atoms, an alkyl group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 13 carbon atoms is preferable.

[0022] The alkyl group having 1 to 12 carbon atoms may be linear, branched, or cyclic, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a t-butyl group, an n-pentyl group, an isopentyl group, a neopentyl group, a t-pentyl group, a cyclopentyl group, an n-hexyl group, an isohexyl group, a cyclohexyl group, an n-heptyl group, a cycloheptyl group, a methylcyclohexyl group, an n-octyl group, a cyclooctyl group, an n-nonyl group, a 3,3,5-trimethylcyclohexyl group, an n-decyl group, a cyclodecyl group, an n-undecyl group, an n-dodecyl group, and a cyclododecyl group. Examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a tolyl group, an ethylphenyl group, a xylyl group, an n-propylphenyl group, an isopropylphenyl group, a mesityl group, a naphthyl group, and a methylnaphthyl group.

[0023] Examples of the aralkyl group having 7 to 13 carbon atoms include a benzyl group, a methylbenzyl group, a dimethylbenzyl group, a trimethylbenzyl group, a phenethyl group, a 2-phenylisopropyl group, and a naphthylmethyl group.

[0024] The acyloxy group is preferably an acyloxy group having a hydrocarbon group having 1 to 7 carbon atoms, more preferably an acetyloxy group, a propanoyloxy group, a butanoyloxy group, a benzoyloxy group, or a methylbenzoyloxy group, still more preferably an acetyloxy group or a benzoyloxy group, and particularly preferably an acetyloxy group.

[0025] Examples of the diphenol compound (B1) include bisphenol compounds such as bisphenol A, bisphenol F, bisphenol E, bisphenol Z, bisphenol S, bisphenol AD, bisphenol AF, bisphenol B, bisphenol BP, bisphenol C, bisphenol G, bisphenol M, bisphenol P, bisphenol PH, bisphenolacetophenone, bisphenol trimethylcyclohexane, bisphenol fluorene, biscresol fluorene, tetramethyl bisphenol A, tetramethyl bisphenol F, tetra-t-butyl bisphenol A, tetramethyl bisphenol S, dihydroxydiphenyl ether, dihydroxydiphenylmethane, bis(hydroxyphenoxy)benzene, thiodiphenol, and dihydroxystilbene; biphenol compounds such as biphenol, tetramethyl biphenol, dimethyl biphenol, and tetra-t-butyl biphenol; benzenediol compounds such as hydroquinone, methyl hydroquinone, dibutyl hydroquinone, resorcin, and methyl resorcin; and dihydroxy anthraquinone. 10-(2,5-dihydroxyphenyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO-HQ), 10-(2,7-dihydroxynaphthyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO-NQ), 10-(1,4-dihydroxy-2-naphthyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, 10-(2,5-dihydroxyphenyl) and phosphorus-containing phenol compounds such as 8-benzyl-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-(2,7-dihydroxy-1-naphthyl)-8-benzyl-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, diphenylphosphinylhydroquinone, diphenylphosphinyl-1,4-dioxynaphthalene, 1,4-cyclooctylenephosphinyl-1,4-phenyldiol, and 1,5-cyclooctylenephosphinyl-1,4-phenyldiol.

[0026] In order to improve the heat resistance of the phenoxy resin, dihydroxynaphthalene, bisphenol fluorene, and biscresol fluorene are preferred, and bisphenol fluorene and biscresol fluorene are more preferred. In addition, a phosphorus-containing phenol compound may be used for the purpose of imparting flame retardancy.

[0027] The diester compound (B2) and the monoester compound (B3) include compounds in which two or one hydroxyl group of the diphenol compound (B1) is replaced with an acyloxy group (active ester). The diester compound (B2) is obtained by acylation of the diphenol compound (B1) with an acylating agent such as an acid anhydride of an organic acid, an organic acid halide, or an organic acid by condensation reaction. The monoester compound (B3) is also obtained by isolating from a mixture of the monoester compound (B3), the diester compound (B2), and the diphenol compound (B1), which is obtained by adjusting the molar ratio of the acylating agent during the acylation of the diphenol compound (B1).

[0028] Examples of the acid component used in the acylation include organic acids such as acetic acid, propionic acid, butyric acid, isobutyric acid, pentanoic acid, octanoic acid, caprylic acid, lauric acid, stearic acid, oleic acid, benzoic acid, t-butylbenzoic acid, hexahydrobenzoic acid, phenoxyacetic acid, acrylic acid, and methacrylic acid, as well as acid anhydrides of organic acids, halides of organic acids, and esters of organic acids.

[0029] Examples of the acid anhydrides of organic acids include acetic anhydride, benzoic anhydride, and phenoxyacetic anhydride.

[0030] Examples of the esters of organic acids include methyl acetate, ethyl acetate, butyl acetate, methyl benzoate, ethyl benzoate, etc. Examples of the halides of organic acids include acetate chloride, benzoate chloride, phenoxyacetate chloride, etc.

[0031] As these acylating agents, preferred are organic acid halides such as acetic acid chloride, benzoic acid chloride, and phenoxyacetic acid chloride, acid halides such as acetic anhydride, benzoic acid anhydride, and phenoxyacetic acid anhydride, and acid anhydrides of organic acids. In order to eliminate the need for washing with water after esterification and to avoid contamination with halogens, which are undesirable in electrical material applications, acid anhydrides such as acetic anhydride and benzoic acid anhydride are more preferred, and acetic anhydride is even more preferred.

[0032] In the method for producing the phenoxy resin of the present invention, the amount of the bifunctional compound used is preferably 0.9 to 1.1 mol, more preferably 0.95 to 1.05 mol, even more preferably 0.96 to 1.00 mol, and particularly preferably 0.97 to 0.99 mol, relative to 1.00 mol of the bifunctional epoxy resin. If the amount of the bifunctional compound is within this range, the molecular weight of the obtained phenoxy resin is sufficiently extended, which is preferable. In addition, from the viewpoint of reactivity, it is desirable to have many epoxy groups in the terminal groups, so that the amount of the bifunctional compound is preferably less than 1.00 mol. If the bifunctional epoxy resin is in excess, the epoxy group terminal tends to be formed, and if the bifunctional compound is in excess, the phenol group terminal or acyloxy group terminal tends to be formed.

[0033] In order to impart heat resistance, it is preferable to use a bifunctional epoxy resin having a fluorene ring structure as part or all of the bifunctional epoxy resin, or a bifunctional phenol compound having a fluorene ring structure as part or all of the bifunctional compound.

[0034] Specific examples of bifunctional phenol compounds having a fluorene ring structure include 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-2-methylphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-hydroxy-3-ethylphenyl)fluorene, 9,9-bis(3-hydroxy-6-methylphenyl)fluorene, 9,9-bis(2-hydroxy-4-methylphenyl)fluorene, 9,9-bis(4-hydroxy-3-t-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3,5-dimethylphenyl)fluorene, 9,9-bis(4-hydroxy-2,6-dimethylphenyl)fluorene, 9,9-bis(4-hydroxy-3,5-di-t-butylphenyl)fluorene, and 9,9-bis(4-hydroxy-3-cyclohexylphenyl)fluorene. Examples of the fluorene ring structure-containing bifunctional phenol compound include 9,9-bis(hydroxyphenyl)fluorenes such as 9,9-bis(4-hydroxy-3-phenylphenyl)fluorene, and 9,9-bis(hydroxynaphthyl)fluorenes such as 9,9-bis(2-hydroxy-6-naphthyl)fluorene and 9,9-bis(1-hydroxy-5-naphthyl)fluorene. These fluorene ring structure-containing bifunctional phenol compounds may be used alone or in combination.

[0035] The bifunctional epoxy resin having a fluorene ring structure may be a diglycidyl compound obtained by reacting the bifunctional phenol compound having the fluorene ring structure with 5 to 20 times the molar amount of epihalohydrin such as epichlorohydrin using an alkali catalyst such as sodium hydroxide or potassium hydroxide. Specific examples of the bifunctional epoxy resin include bisphenolfluorene type epoxy resin, biscresolfluorene type epoxy resin, and bisnaphtholfluorene type epoxy resin.

[0036] In order to impart flame retardancy, a bifunctional halogenated phenol compound to which a halogen has been added (e.g., tetrabromobisphenol A, etc.) or a bifunctional phosphorus-containing phenol compound may be used as part or all of the bifunctional compound, and from an environmental standpoint, a bifunctional phosphorus-containing phenol compound is preferred.

[0037] Examples of bifunctional phosphorus-containing phenolic compounds include 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, 10-(2,7-dihydroxy-1-naphthyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, 10-(1,4-dihydroxy-2-naphthyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, and 10-(2,5-dihydroxyphenyl)-8-benzyl-9,1 Examples of the phosphorus-containing phenol compounds include 0-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-(2,7-dihydroxy-1-naphthyl)-8-benzyl-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, diphenylphosphinyl hydroquinone, diphenylphosphenyl-1,4-dioxynaphthalene, 1,4-cyclooctylenephosphinyl-1,4-phenyldiol, 1,5-cyclooctylenephosphinyl-1,4-phenyldiol, etc. These phosphorus-containing phenol compounds may be used alone or in combination of two or more.

[0038] In order to impart flame retardancy, it is preferable to use a phosphorus-containing compound as part or all of the difunctional epoxy resin.

[0039] The phosphorus-containing compound as the bifunctional epoxy resin may be a diglycidyl compound obtained by reacting the above phosphorus-containing phenolic compound with 5 to 20 times the molar amount of epihalohydrin using an alkali catalyst. Specific examples include the above epoxy resin, FX-305, diphenylphosphinyl hydroquinone diglycidyl ether, etc.

[0040] The phosphorus content of the phenoxy resin obtained by using the difunctional phosphorus-containing compound may be appropriately adjusted depending on the purpose of use, but is preferably 1 to 6 mass%, more preferably 2 to 5 mass%, and even more preferably 3 to 4.5 mass%.

[0041] The carboxylate of a quaternary phosphonium salt used in the method for producing a phenoxy resin of the present invention acts as a catalyst for the reaction between a difunctional epoxy resin and a difunctional compound.

[0042] In the production method of the present invention, the carboxylate of a quaternary phosphonium salt used as a catalyst is represented by the following formula (1): That is, it is a salt of a phosphonium cation and an anion residue of a polycarboxylic acid. [ka]

[0043] In formula (1), the phosphonium cation is represented by the following formula (1a), and the anion portion is represented by the following formula (1b). [ka]

[0044] In formulas (1) and (1a), R 1 ~R 4 are each independently an alkyl group, an aryl group, or an aralkyl group, and may be the same group or different groups. The alkyl group may be either linear or branched, and preferably has 1 to 12 carbon atoms, more preferably has 1 to 4 carbon atoms, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, a sec-butyl group, an iso-butyl group, and a t-butyl group. The aryl group preferably has 6 to 10 carbon atoms, and examples thereof include a phenyl group and a p-tolyl group, and may have a substituent. The aralkyl group preferably has 7 to 12 carbon atoms, and examples thereof include a benzyl group. Among these, an ethyl group, a butyl group, a phenyl group, and a benzyl group are preferable, and particularly R 1 ~R 4 More preferably, all of are butyl groups or phenyl groups.

[0045] Examples of the phosphonium cation represented by formula (1a) include the following formulae (4a) to (4f). [ka]

[0046] In the anions of polycarboxylic acids represented by the formulae (1) and (1b), X is a structure in which two carboxy groups have been removed from a polycarboxylic acid, and is preferably any one of the groups of the following formulae (2a) to (2d). [ka]

[0047] Formula (2a) is a group derived from an aliphatic polycarboxylic acid represented by the following formula (3a), formula (2b) or (2c) is a group derived from an alicyclic polycarboxylic acid represented by the following formula (3b) or (3c), and formula (2d) is a group derived from an aromatic polycarboxylic acid represented by the following formula (3d). [ka] In the formula, R 5 ~R 8 is R in formula (2a) 5 ~R 8 is synonymous with R 10 ~R 14 is R in formula (2b). 10 ~R 14 is synonymous with R 15 ~R 18 is R in formula (2c) 15 ~R 18 is synonymous with R 19 ~R 22 is R in formula (2d). 19 ~R 22 is synonymous with.

[0048] The anionic moiety represented by formula (1b), for example, in the case of formula (2a), indicates an anionic residue (monovalent anionic residue) of an aliphatic polycarboxylic acid represented by formula (3a), and strictly speaking, is an anionic residue in which, among multiple carboxyl groups or carboxyl anions, carboxyl groups and carboxyl anions present separated by ethylene chains are coordinated to a phosphonium cation.

[0049] It is believed that the coordination of the anion residue to the phosphonium cation causes a time lag before activity appears in the initial stage of heating, which is the cause of the low viscosity (latency) in the initial stage of heating. In this case, ethylene chains are optimal from the viewpoint of the balance between latency and coordination power.

[0050] For this reason, preferred aliphatic polycarboxylic acids of formula (3a) include those having R 5 ~R 8 Succinic acid, where R is all hydrogen atoms 5 ~R 7 is a hydrogen atom and R 8 is malic acid, R is hydroxyl group 5 , R 6 is a hydrogen atom, and R 7 is a hydroxyl group, R 8 Citric acid and R 5 , R 7 is a hydrogen atom and R 6 , R 8 butane-1,2,3,4-tetracarboxylic acid, etc., in which the carboxyl group is present, is preferred. These aliphatic polycarboxylic acids may be used alone or in combination of two or more.

[0051] The carboxylate of a quaternary phosphonium salt used in the method for producing a phenoxy resin of the present invention can be easily produced by a known method, for example, the method described in JP-A-63-190893.

[0052] For example, a method can be mentioned in which a solution of a tetra-substituted phosphonium halide (solvent: water, methanol, etc.) is converted into a solution of a tetra-substituted phosphonium hydroxide (solvent: water, methanol, etc.) by ion exchange, and the solution is neutralized with 0.5 to 5 moles, more preferably 0.5 to 2 moles, of an aliphatic polycarboxylic acid represented by formula (3a) per mole of the tetra-substituted phosphonium hydroxide to form a salt. The solvent is removed from the reaction mixture containing the obtained salt by a suitable method, for example, distillation under reduced pressure, to separate the target salt. Note that, as the above-mentioned tetra-substituted phosphonium hydroxide, commercially available products may be used.

[0053] The aliphatic polycarboxylic acid represented by formula (3a) may contain water of hydration, water of crystallization, water of adsorption, etc., and may be used alone or in combination of two or more kinds. Furthermore, instead of the aliphatic polycarboxylic acids, the corresponding aliphatic polycarboxylic anhydrides may be used, respectively.

[0054] The salt obtained by the above method is usually mainly a 1:1 salt of 1 mole of a phosphonium cation and 1 mole of an anion residue of at least one kind of aliphatic polycarboxylic acid.

[0055] The carboxylate of the quaternary phosphonium salt in which X is represented by formula (2b) or (2c) in formula (1) can be obtained by using an alicyclic polycarboxylic acid represented by formula (3b) or (3c) as the polycarboxylic acid. Furthermore, instead of the alicyclic polycarboxylic acid represented by formula (3b) or formula (3c), a corresponding alicyclic polycarboxylic anhydride may be used.

[0056] In the reaction product obtained by the above-mentioned method, in addition to the 1:1 salt, a small amount of other types of salts (salts of phosphonium cations and at least one anion residue of an alicyclic polycarboxylic acid) may be present, and such reaction products can be used as they are.

[0057] The alicyclic polycarboxylic acid represented by formula (3b) which is easily available industrially is usually a mixture containing two or more acids represented by formula (3b). Therefore, a salt of a mixed anion residue derived from a mixture containing two or more alicyclic polycarboxylic acids represented by formula (3b) and a phosphonium cation may be used, and excellent effects are also shown in this case.

[0058] In addition, in the case of the carboxylic acid salt of the quaternary phosphonium salt in which X is the formula (2c) in the formula (1), the alicyclic polycarboxylic acid represented by the formula (3c) is often available industrially as a single product. Usually, it is advantageous to use a salt obtained by using one kind of alicyclic polycarboxylic acid represented by the formula (3c) from the viewpoint of industrial availability. Therefore, when the alicyclic polycarboxylic acid represented by the formula (3c) is used as a raw material, it is typically a 1:1 salt.

[0059] As regards the alicyclic polycarboxylic acids of the formula (3b) and the formula (3c), the following can be given as preferred examples.

[0060] In formula (3b), R 10 is a methylene group, and R 11 ~R 14 is an alicyclic polycarboxylic acid consisting entirely of hydrogen atoms, R 10 is a methylene group, and R 11 ~R 14 wherein one of the groups is a methyl group and the remaining three are hydrogen atoms, or a mixture thereof.

[0061] In formula (3c), R 15 ~R 18 alicyclic polycarboxylic acid in which R is all hydrogen atom; 15 ~R 18 Alicyclic polycarboxylic acid in which one of the groups is a methyl group and the remaining three are hydrogen atoms, R 15 ~R 18 Two of them (especially R 16 and R 17 ) is a carboxyl group and the remaining two are hydrogen atoms, and R 15 ~R 18 alicyclic polycarboxylic acid in which R is all hydrogen atom; 15 ~R 18 Two of them (especially R 16 and R 17 ) is a carboxyl group and the remaining two are hydrogen atoms.

[0062] In the alicyclic polycarboxylic acids represented by formulae (3b) and (3c), there exist isomers in which the two carboxyl groups bonded to adjacent carbon atoms are in a cis configuration, and isomers in which the two carboxyl groups are in a trans configuration. The cis configuration refers to a case in which the two carboxyl groups are present on the same side of the single bond between the two carbon atoms to which the two carboxyl groups are bonded. In addition, the trans configuration refers to a case in which one of the two carboxyl groups is present on a different side from the other with respect to the single bond between the two carbon atoms to which the two carboxyl groups are bonded.

[0063] In the present invention, the anion residue may be either one derived from an alicyclic polycarboxylic acid with a cis configuration or one derived from an alicyclic polycarboxylic acid with a trans configuration, or may be a mixture of both. When the alicyclic polycarboxylic acid used as the raw material is a trans-cis mixture and two carboxyl groups bonded to adjacent carbon atoms are a pair, the anion residue derived from the alicyclic polycarboxylic acid with a cis configuration is preferably 80% or more (area basis by GC (gas chromatography) analysis). Basically, the configuration of the raw material alicyclic polycarboxylic acid is also preserved in the reaction for forming a phosphonium salt, and the cis content of the raw material alicyclic polycarboxylic acid is considered to be almost the same as the cis content of the salt of the resulting phosphonium and alicyclic polycarboxylic acid anion residue.

[0064] In formula (1), the carboxylate of a quaternary phosphonium salt in which X is formula (2d) can be obtained by using an aromatic polycarboxylic acid represented by formula (3d) as the polycarboxylic acid. Note that an aromatic polycarboxylic acid other than the aromatic polycarboxylic acid represented by formula (3d) may be used as the aromatic polycarboxylic acid.

[0065] Examples of the compound represented by formula (3d) include phthalic acid, 4-methylphthalic acid, 4-hydroxyphthalic acid, 4-aminophthalic acid, and 4-methoxyphthalic acid.

[0066] The salt of the phosphonium cation and the anion residue of phthalic acid is known or can be easily produced by a known method. For example, a method of forming a salt by reacting a solution of a tetra-substituted phosphonium halide and an alkali metal salt of phthalic acid in a solvent (solvent is water, methanol, etc.) can be mentioned. In this case, the above salt may be formed by using the tetra-substituted phosphonium halide and the alkali metal salt of phthalic acid alone or two or more kinds. When mixing two or more kinds, two or more kinds of tetra-substituted phosphonium halides and alkali metal salts of phthalic acid may be mixed together first, and then the phosphonium phthalate may be formed, or two or more kinds of phosphonium phthalate may be mixed. The salt obtained by the above method is usually a 1:1 salt of 1 mole of phosphonium cation and 1 mole of anion residue of phthalic acid. The anion portion represents the anion residue of phthalic acid represented by formula (3d) (monovalent anion residue), and the carboxyl group and the carboxyl anion are actually equivalent.

[0067] Examples of the carboxylate of a quaternary phosphonium salt in which X is represented by formula (2d) include tetraphenylphosphonium phthalate, tetraphenylphosphonium 4-methylphthalate, tetraphenylphosphonium 4-hydroxyphthalate, tetraphenylphosphonium 4-aminophthalate, tetraphenylphosphonium 4-methoxyphthalate, (4-methylphenyl)triphenylphosphonium phthalate, (4-methylphenyl)triphenylphosphonium 4-methylphthalate, (4-methylphenyl)triphenylphosphonium 4-hydroxyphthalate, (4-methylphenyl)triphenylphosphonium 4-aminophthalate, and (4-methylphenyl)triphenylphosphonium 4-methoxyphthalate.

[0068] In the method for producing the phenoxy resin of the present invention, the amount of the carboxylate of the quaternary phosphonium salt used is preferably 0.001 to 5 parts by mass, more preferably 0.005 to 2 parts by mass, even more preferably 0.01 to 1 part by mass, and particularly preferably 0.01 to 0.5 parts by mass, relative to 100 parts by mass of the total amount of the bifunctional epoxy resin and the bifunctional compound. If the amount of the carboxylate of the quaternary phosphonium salt used is small, the molecular weight of the phenoxy resin may not be sufficiently large. In addition, if the amount is large, the storage stability is likely to deteriorate, and it is necessary to remove it after the reaction, which is not preferable. If the amount of the carboxylate of the quaternary phosphonium salt used is within the range, the molecular weight of the phenoxy resin is likely to be sufficiently large during the reaction, and the storage stability is also likely to be good, which is preferable. In addition, these catalysts may be charged all at once at the start of the reaction, or may be charged in portions at appropriate times according to the course of the reaction.

[0069] The carboxylic acid salt of the quaternary phosphonium salt can be used after diluting with an organic solvent or water. Any organic solvent can be used as long as it dissolves the raw material. Specifically, the same organic solvent as that usable during the reaction of the phenoxy resin of the present invention described later can be used.

[0070] The reaction between the bifunctional epoxy resin and the bifunctional compound can be carried out under normal pressure, pressurized, or reduced pressure. The reaction is carried out in a temperature range in which the catalyst used does not decompose. If the reaction temperature is too high, the phenoxy resin produced may deteriorate, and if it is too low, the reaction may not proceed and the target molecular weight may not be obtained. Therefore, the reaction temperature is preferably 50 to 240°C, more preferably 80 to 230°C, even more preferably 100 to 220°C, and particularly preferably 120 to 200°C. The reaction time is not particularly limited, but is preferably 0.5 to 24 hours, more preferably 1 to 20 hours, even more preferably 2 to 12 hours, and particularly preferably 3 to 10 hours. If the reaction time is within the preferred range, it is preferable in terms of improving production efficiency and reducing unreacted components. In addition, when a low-boiling point solvent such as acetone or methyl ethyl ketone is used, the reaction temperature can be ensured by carrying out the reaction under high pressure using an autoclave. When it is necessary to remove the heat of reaction, this is usually achieved by evaporation, condensation and reflux of the solvent using the heat of reaction, indirect cooling, or a combination of these.

[0071] In the method for producing the phenoxy resin of the present invention, a solvent may be used during the reaction. Any solvent may be used as long as it dissolves the raw materials and the reaction product (phenoxy resin) and does not adversely affect the reaction, but it is usually an organic solvent. Examples of the organic solvent include aromatic solvents, ketone solvents, ester solvents, ether solvents, amide solvents, and glycol ether solvents. These solvents may be used alone or in combination of two or more. The amount of the solvent used may be appropriately selected depending on the reaction conditions, but a solid content concentration of 35 to 95 mass% is preferable. In addition, if a highly viscous product is produced during the reaction, the reaction may be continued by adding more solvent during the reaction.

[0072] Examples of aromatic solvents include benzene, toluene, and xylene.

[0073] Examples of ketone solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, 2-heptanone, 4-heptanone, 2-octanone, cyclopentanone, cyclohexanone, and acetylacetone.

[0074] Examples of ester solvents include methyl acetate, ethyl acetate, propyl acetate, butyl acetate, benzyl acetate, ethyl propionate, ethyl butyrate, butyl butyrate, valerolactone, butyrolactone, etc. Examples of ether solvents include diethyl ether, dibutyl ether, t-butyl methyl ether, tetrahydrofuran (THF), dioxane, etc.

[0075] Examples of amide solvents include formamide, N-methylformamide, N,N-dimethylformamide (DMF), acetamide, N-methylacetamide, N,N-dimethylacetamide, 2-pyrrolidone, and N-methylpyrrolidone.

[0076] Examples of glycol ether solvents include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol dimethyl ether, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol dimethyl ether, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether, propylene glycol mono-n-butyl ether, propylene glycol dimethyl ether, propylene glycol monomethyl ether acetate, and dipropylene glycol dimethyl ether.

[0077] After the reaction is completed, the solvent may be removed by distillation or the like as necessary, or may be added to adjust the solid content concentration. The solvent may be any solvent that dissolves the phenoxy resin, but is usually an organic solvent. Examples of the organic solvent include the same organic solvents as those described above.

[0078] In the method for producing the phenoxy resin of the present invention, other catalysts may be used in combination with the carboxylate of the quaternary phosphonium salt, as long as the storage stability is not deteriorated during the reaction. The other catalysts are not particularly limited as long as they are usually used as catalysts in the two-stage process. For example, alkali metal compounds, organic phosphorus compounds other than the carboxylate of the quaternary phosphonium salt, tertiary amine compounds, quaternary ammonium salts, cyclic amine compounds, imidazole compounds, etc. may be mentioned. These other catalysts may be used alone or in combination of two or more. From the viewpoint of storage stability, it is preferable that the resin composition is stored without other catalysts or in a smaller amount than the carboxylate of the quaternary phosphonium salt.

[0079] Examples of the alkali metal compound include alkali metal hydroxides such as sodium hydroxide, lithium hydroxide, and potassium hydroxide; alkali metal salts such as sodium carbonate, sodium bicarbonate, sodium chloride, lithium chloride, and potassium chloride; alkali metal alkoxides such as sodium methoxide and sodium ethoxide; alkali metal phenoxides, alkali metal hydrides such as sodium hydride and lithium hydride; and alkali metal salts of organic acids such as sodium acetate and sodium stearate.

[0080] Examples of organic phosphorus compounds other than the carboxylate of the quaternary phosphonium salt include tetramethylphosphonium bromide, tetramethylphosphonium iodide, tetramethylphosphonium hydroxide, trimethylcyclohexylphosphonium chloride, trimethylcyclohexylphosphonium bromide, trimethylbenzylphosphonium chloride, trimethylbenzylphosphonium bromide, tetraphenylphosphonium bromide, triphenylmethylphosphonium bromide, triphenylmethylphosphonium iodide, triphenylethylphosphonium chloride, triphenylethylphosphonium bromide, triphenylethylphosphonium iodide, triphenylbenzylphosphonium chloride, triphenylbenzylphosphonium bromide, etc. In addition, since phosphines other than the carboxylate of the quaternary phosphonium salt represented by the above formula (1) may remain in the phenoxy resin, which is the reaction product, it is not desirable to use them in combination when the phenoxy resin is to be free of phosphines.

[0081] Examples of the tertiary amine compounds include triethylamine, tri-n-propylamine, tri-n-butylamine, triethanolamine, and benzyldimethylamine.

[0082] Examples of quaternary ammonium salts include tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium hydroxide, triethylmethylammonium chloride, tetraethylammonium chloride, tetraethylammonium bromide, tetraethylammonium iodide, tetrapropylammonium bromide, tetrapropylammonium hydroxide, tetrabutylammonium chloride, tetrabutylammonium bromide, tetrabutylammonium iodide, benzyltrimethylammonium chloride, benzyltrimethylammonium bromide, benzyltrimethylammonium hydroxide, benzyltributylammonium chloride, and phenyltrimethylammonium chloride.

[0083] Examples of the cyclic amine compounds include 1,8-diazabicyclo(5,4,0)-7-undecene and 1,5-diazabicyclo(4,3,0)-5-nonene.

[0084] Examples of the imidazole compounds include 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, 2-undecylimidazole, 2-ethyl-4-methylimidazole, and 1-cyanoethyl-2-methylimidazole.

[0085] The weight average molecular weight (Mw) of the phenoxy resin obtained by the production method of the present invention is preferably 10,000 to 150,000, more preferably 20,000 to 100,000, further preferably 25,000 to 80,000, and particularly preferably 30,000 to 60,000. If Mw is low, the film formability and extensibility are poor, and if Mw is too high, the handling of the resin is significantly deteriorated. Here, Mw is determined by GPC measurement, and the GPC measurement method is according to the conditions described in the examples.

[0086] The epoxy equivalent (g / eq.) of this phenoxy resin is preferably 4,000 to 200,000, more preferably 5,000 to 100,000, even more preferably 6,000 to 50,000, and particularly preferably 8,000 to 30,000. This also includes cases where both ends are not necessarily epoxy groups, in which case the epoxy equivalent may increase the average molecular weight. If the epoxy equivalent is within the preferred range, the molecular weight of the phenoxy resin is sufficiently large, which is preferable from the viewpoint of flexibility.

[0087] The phenoxy resin of the present invention is advantageously a phenoxy resin obtained by the production method of the present invention. Advantageously, it contains 0.001 to 5 mass% of a carboxylate of a quaternary phosphonium salt. The preferred Mw and epoxy equivalent of the phenoxy resin of the present invention are the same as those of the phenoxy resin obtained by the production method of the present invention.

[0088] The amount of the carboxylate of the quaternary phosphonium salt present in the phenoxy resin of the present invention is preferably 0.01 to 2 mass%, more preferably 0.05 to 1 mass%. If the amount of the carboxylate of the quaternary phosphonium salt is too large, the storage stability may deteriorate when mixed with a curing agent. If the amount is less than 0.001 mass%, a burden is placed on the removal of impurities such as reaction or unreacted materials in the production of the phenoxy resin. The amount of the carboxylate of the quaternary phosphonium salt can be quantified by high performance liquid chromatography (HPLC). The measurement method follows the conditions described in the Examples.

[0089] The phenoxy resin of the present invention is a flexible thermoplastic resin in itself and can be used alone, but can also be mixed with a curing component to form a thermosetting resin composition.

[0090] The curing component may be a thermosetting resin that can be cured by itself, a resin or curing agent that can be cured by reacting with the hydroxyl group or epoxy group of the phenoxy resin, or a resin that can be cured by being used together with a curing agent.

[0091] Examples of the curing component include epoxy resin, acrylic ester resin, phenol resin, melamine resin, urea resin, unsaturated polyester resin, alkyd resin, thermosetting polyimide resin, acid anhydride compound, polyisocyanate compound, blocked isocyanate compound, amine compound, imidazole compound, amide compound, cationic polymerization initiator, organic phosphine, etc. These curing components may be used alone or in combination of two or more. In addition, it is preferable to use a curing agent for epoxy resin in the case of epoxy resin, and a radical polymerization initiator in the case of acrylic ester resin.

[0092] The blending amount of the curing component is preferably 1 / 99 to 99 / 1, more preferably 10 / 90 to 90 / 10, and even more preferably 25 / 75 to 75 / 25, as a phenoxy resin / curing component (mass ratio). By blending the curing component, a material with even better heat resistance can be obtained.

[0093] When the curing component is an epoxy resin, conventionally known epoxy resins can be used. The epoxy resin refers to an epoxy resin having at least one epoxy group, but an epoxy resin having two or more epoxy groups is preferable, and an epoxy resin having three or more epoxy groups is more preferable. Specifically, polyglycidyl ether compounds, polyglycidyl amine compounds, polyglycidyl ester compounds, alicyclic epoxy resins, other modified epoxy resins, etc. can be mentioned. These epoxy resins may be used alone, or two or more kinds of the same type of epoxy resin may be used in combination, or different types of epoxy resins may be used in combination.

[0094] Examples of the polyglycidyl ether compound include the above-mentioned bifunctional epoxy resins that can be used as a raw material for phenoxy resins, polyfunctional novolac epoxy resins such as phenol novolac epoxy resins, cresol novolac epoxy resins, alkyl novolac epoxy resins, styrenated phenol novolac epoxy resins, bisphenol novolac epoxy resins, naphthol novolac epoxy resins, β-naphthol aralkyl epoxy resins, naphthalenediol aralkyl epoxy resins, α-naphthol aralkyl epoxy resins, biphenyl aralkyl phenol epoxy resins, trihydroxyphenylmethane epoxy resins, tetrahydroxyphenylethane epoxy resins, and dicyclopentadiene epoxy resins, alkylene glycol epoxy resins, and aliphatic cyclic epoxy resins.

[0095] Examples of polyglycidylamine compounds include diaminodiphenylmethane type epoxy resins, metaxylenediamine type epoxy resins, 1,3-bisaminomethylcyclohexane type epoxy resins, isocyanurate type epoxy resins, aniline type epoxy resins, hydantoin type epoxy resins, and aminophenol type epoxy resins.

[0096] Examples of the polyglycidyl ester compound include dimer acid type epoxy resins, hexahydrophthalic acid type epoxy resins, and trimellitic acid type epoxy resins. Examples of alicyclic epoxy resins include alicyclic epoxy resins such as CELLOXIDE 2021 (manufactured by Daicel Chemical Industries, Ltd.).

[0097] Other modified epoxy resins include, for example, urethane-modified epoxy resins, oxazolidone ring-containing epoxy resins, epoxy-modified polybutadiene rubber derivatives, carboxyl-terminated butadiene nitrile rubber (CTBN)-modified epoxy resins, and polyvinylarene polyoxides (e.g., divinylbenzene dioxide, trivinylnaphthalene trioxide, etc.).

[0098] When an epoxy resin is blended, it is preferable to also include a curing agent. The curing agent is a substance that contributes to the crosslinking reaction and / or the chain extension reaction between the epoxy groups of the epoxy resin. The blending amount of the curing agent is 0.1 to 100 parts by mass based on 100 parts by mass of the epoxy resin as required, preferably 1 to 80 parts by mass, more preferably 5 to 60 parts by mass, and further preferably 10 to 60 parts by mass.

[0099] The curing agent is not particularly limited, and any agent generally known as a curing agent for epoxy resins can be used. From the viewpoint of increasing heat resistance, preferred examples include phenol-based curing agents, amide-based curing agents, and imidazole-based compounds. From the viewpoint of decreasing water absorption, preferred examples include active ester-based curing agents. Other examples include amine-based curing agents, acid anhydride-based curing agents, organic phosphines, phosphonium salts, benzo compounds, tetraphenyl boron salts, organic acid dihydrazides, boron halide amine complexes, polymercaptan-based curing agents, isocyanate-based curing agents, and blocked isocyanate-based curing agents. These curing agents may be used alone, or two or more of the same type may be used in combination, or other types may be used in combination.

[0100] Examples of the phenol-based curing agent include the above-mentioned bifunctional phenol compounds that can be used as raw materials for phenoxy resins, phenol novolac, bisphenol A novolac, cresol novolac, xylenol novolac, trishydroxyphenylmethane novolac, dicyclopentadiene phenol, naphthol novolac, styrenated phenol novolac, terpene phenol, heavy oil modified phenol, phenol aralkyl, naphthol aralkyl, polyhydroxystyrene, fluoroglycinol, pyrogallol, t-butylpyrogallol, benzenetriol, trihydroxynaphthalene, trihydroxybenzophenone, and trihydroxyacetophenone, and the above-mentioned phosphorus-containing phenol compounds. These phenol compounds may be reacted with indene or styrene to be used as the curing agent. The phenol-based curing agent is preferably used in a molar ratio of active hydroxyl groups in the curing agent to epoxy groups in the epoxy resin in the range of 0.8 to 1.5.

[0101] Examples of the amide-based curing agent include dicyandiamide and its derivatives, polyamide resins, etc. The amide-based curing agent is preferably used in an amount of 0.1 to 25 parts by mass relative to 100 parts by mass of the total epoxy resin component.

[0102] The imidazole compound is not particularly limited as long as it has an imidazole skeleton. For example, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyano-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethylenediamine, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate ... Examples of the imidazole-based compound include ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and an adduct of an epoxy resin and the above imidazole-based compound. The imidazole-based compound is preferably used in the range of 0.1 to 25 parts by mass relative to 100 parts by mass of the total epoxy resin component. In addition, since the imidazole-based compound has catalytic ability, it is generally classified as a curing accelerator, which will be described later.

[0103] As the active ester-based curing agent, compounds having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, are preferred, and among them, phenol esters obtained by reacting a polyfunctional phenol compound with an aromatic carboxylic acid, as described in Japanese Patent No. 5152445, are more preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of the aromatic compound having a phenolic hydroxyl group include catechol, dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadienyldiphenol, and phenol novolac. Commercially available products include, but are not limited to, Epicron HPC-8000-65T (manufactured by DIC Corporation). The active ester curing agent is preferably used in such a manner that the molar ratio of the active ester groups in the curing agent to the epoxy groups in the resin composition falls within the range of 0.2 to 2.0.

[0104] Examples of the amine-based curing agent include amine-based compounds such as diethylenetriamine, triethylenetetramine, metaxylenediamine, isophoronediamine, diaminodiphenylmethane, diaminodiphenylsulfone, diaminodiphenylether, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, dicyandiamide, and polyamidoamines which are condensates of acids such as dimer acid and polyamines. The amine-based curing agent is preferably used in a molar ratio of active hydrogen groups in the curing agent to epoxy groups in the resin composition in the range of 0.5 to 1.5.

[0105] Examples of acid anhydride curing agents include methyltetrahydrophthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, pyromellitic anhydride, phthalic anhydride, trimellitic anhydride, methylnadic anhydride, maleic anhydride, etc. The acid anhydride curing agent is preferably used in a molar ratio of the acid anhydride group in the curing agent to the epoxy group in the resin composition in the range of 0.5 to 1.5.

[0106] The active hydrogen group refers to a functional group having active hydrogen reactive with an epoxy group (including a functional group having latent active hydrogen that generates active hydrogen by hydrolysis, etc., and a functional group that shows an equivalent curing action). Specific examples include an acid anhydride group, a carboxyl group, an amino group, and a phenolic hydroxyl group. Regarding active hydrogen groups, a carboxyl group (-COOH) or a phenolic hydroxyl group (-OH) is calculated as 1 mole, and an amino group (-NH2) is calculated as 2 moles. If the active hydrogen group is not clear, the active hydrogen equivalent can be determined by measurement. For example, the active hydrogen equivalent of the curing agent used can be determined by reacting a monoepoxy resin with a known epoxy equivalent, such as phenyl glycidyl ether, with a curing agent with an unknown active hydrogen equivalent, and measuring the amount of monoepoxy resin consumed.

[0107] In addition, when an epoxy resin is blended, a curing accelerator can be used as necessary. Examples of the curing accelerator include imidazole compounds, tertiary amine compounds, phosphines, metal compounds, and amine complex salts. These curing accelerators may be used alone or in combination of two or more.

[0108] Examples of the imidazole-based compound, the tertiary amine-based compound, and the phosphines include the same as those described above as catalysts that can be used in the production method of the present invention.

[0109] An example of the metal compound is tin octoate.

[0110] Examples of the amine complex salt include boron trifluoride complexes such as boron trifluoride monoethylamine complex, boron trifluoride diethylamine complex, boron trifluoride isopropylamine complex, boron trifluoride chlorophenylamine complex, boron trifluoride benzylamine complex, boron trifluoride aniline complex, and mixtures thereof.

[0111] The amount of the curing accelerator may be appropriately selected depending on the purpose of use, but 0.01 to 15 parts by mass is used as necessary, preferably 0.01 to 10 parts by mass, more preferably 0.05 to 8 parts by mass, and even more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the epoxy resin component in the resin composition. By using the curing accelerator, the curing temperature can be lowered and the curing time can be shortened.

[0112] Resin compositions in which an acrylic ester resin as a curing component is cured with a radical polymerization initiator include thermosetting resin compositions and photocurable resin compositions of (meth)acrylate compounds. The (meth)acrylate compounds are acrylates having at least one (meth)acryloyl group in the molecule, which are used for viscosity adjustment or as a curing component. It is preferable that some of the (meth)acrylate compounds have two or more (meth)acryloyl groups. In this case, the resin composition contains a (meth)acrylate compound and a thermal polymerization initiator, a photopolymerization initiator, or both as essential components.

[0113] Examples of these (meth)acrylate compounds include monofunctional (meth)acrylic acid esters, polyfunctional (meth)acrylates, urethane (meth)acrylates, epoxy acrylates, etc. These (meth)acrylate compounds may be used alone or in combination of two or more kinds.

[0114] Examples of monofunctional (meth)acrylic acid esters include isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, acryloylmorpholine, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, cyclohexane-1,4-dimethanol mono(meth)acrylate, tetramethylphenyl ... Examples of the acrylates include hydrofurofuryl (meth)acrylate, phenoxyethyl (meth)acrylate, phenyl polyethoxy (meth)acrylate, 2-hydroxy-3-phenyloxypropyl (meth)acrylate, o-phenylphenol monoethoxy (meth)acrylate, o-phenylphenol polyethoxy (meth)acrylate, p-cumylphenoxyethyl (meth)acrylate, isobornyl (meth)acrylate, tribromophenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate.

[0115] Examples of polyfunctional (meth)acrylates include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, bisphenol A polyethoxy di(meth)acrylate, bisphenol A polypropoxy di(meth)acrylate, bisphenol F polyethoxy di(meth)acrylate, ethylene glycol di(meth)acrylate, trimethylolpropane trioxyethyl (meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and the like. acrylate, polyethylene glycol di(meth)acrylate, tris(acryloxyethyl)isocyanurate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, tripentaerythritol hexa(meth)acrylate, tripentaerythritol penta(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, cyclohexane dimethanol di(meth)acrylate, and dimethyloltricyclodecane di(meth)acrylate.

[0116] In addition, urethane (meth)acrylate can be obtained by reacting a polyol compound with a polyisocyanate compound and then reacting the resulting compound with a (meth)acrylate, while epoxy acrylate can be obtained by reacting an epoxy resin with a (meth)acrylate.

[0117] Compounds that can be used as polymerization initiators for (meth)acrylate compounds are not particularly limited as long as they generate radicals by means of heating, irradiation with active energy rays, or the like.

[0118] As the polymerization initiator, for example, in the case of curing by heating, any of those usable for normal radical thermal polymerization, such as azo-based initiators such as azobisisobutyronitrile and benzoyl peroxide, and peroxide-based initiators, can be used.

[0119] In addition, when the radical polymerization is carried out by photoradical polymerization, any of those that can be used in normal photoradical polymerization, such as benzoins, acetophenones, anthraquinones, thioxanthones, ketals, benzophenones, and phosphine oxides, can be used.

[0120] These polymerization photoinitiators may be used alone or in combination of two or more. Furthermore, the photoradical polymerization initiator may be used in combination with an accelerator such as a tertiary amine compound or N,N-dimethylaminobenzoic acid ethyl ester.

[0121] Examples of polyisocyanate compounds include tolylene diisocyanate, methylcyclohexane diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, dimer acid diisocyanate, trimethylhexamethylene diisocyanate, lysine triisocyanate, etc. Further examples include trimers to pentamers of these polyisocyanate compounds, and reaction products of these polyisocyanate compounds with compounds having at least two active hydrogen atoms such as amino groups, hydroxyl groups, carboxyl groups, water, etc.

[0122] Examples of the acid anhydride compound include phthalic anhydride, hexahydrophthalic anhydride, trimellitic anhydride, maleic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, pyromellitic anhydride, methylnadic anhydride, dodecenylsuccinic anhydride, chlorendic anhydride, benzenetetracarboxylic anhydride, benzophenonetetracarboxylic dianhydride, ethylenebis(trimellitic anhydride), methylcyclohexenyltetracarboxylic dianhydride, etc. Furthermore, condensates of these acid anhydride compounds and unsaturated compounds, etc. can be mentioned.

[0123] In addition, an organic solvent or a reactive diluent may be used in the resin composition of the present invention for adjusting the viscosity. These organic solvents or reactive diluents may be used alone or in combination of two or more kinds.

[0124] Examples of the organic solvent include the same organic solvents as those usable in the production method of the present invention, as well as alcohols such as methanol, ethanol, 1-methoxy-2-propanol, 2-ethyl-1-hexanol, benzyl alcohol, ethylene glycol, propylene glycol, butyl diglycol, and pine oil, sulfoxides such as dimethyl sulfoxide, and alkanes such as hexane and cyclohexane.

[0125] Examples of reactive diluents include monofunctional glycidyl ethers such as allyl glycidyl ether, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, phenyl glycidyl ether, and tolyl glycidyl ether; bifunctional glycidyl ethers such as resorcinol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, cyclohexanedimethanol diglycidyl ether, and propylene glycol diglycidyl ether; polyfunctional glycidyl ethers such as glycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, trimethylolethane polyglycidyl ether, and pentaerythritol polyglycidyl ether; glycidyl esters such as neodecanoic acid glycidyl ester; and glycidyl amine compounds such as phenyl diglycidyl amine and tolyl diglycidyl amine.

[0126] These organic solvents or reactive diluents are preferably used in an amount of 90% by mass or less as non-volatile matter, and the appropriate type and amount of use are appropriately selected depending on the application. For example, for printed wiring board applications, polar solvents with a boiling point of 160° C. or less, such as methyl ethyl ketone, acetone, and 1-methoxy-2-propanol, are preferred, and the amount of use is preferably 40 to 80% by mass as non-volatile matter. For adhesive film applications, for example, ketones, acetates, carbitols, aromatic hydrocarbons, dimethylformamide, dimethylacetamide, and N-methylpyrrolidone are preferred, and the amount of use is preferably 30 to 60% by mass as non-volatile matter.

[0127] In the resin composition of the present invention, known fillers can be used for the purpose of improving the physical properties such as impact resistance of the resulting cured product, within the range that does not decrease reliability.

[0128] Examples of fillers include fillers such as fused silica, crystalline silica, alumina, silicon nitride, boron nitride, aluminum nitride, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, boehmite, talc, mica, clay, calcium carbonate, magnesium carbonate, barium carbonate, zinc oxide, titanium oxide, magnesium oxide, magnesium silicate, calcium silicate, zirconium silicate, barium sulfate, and carbon; fibrous fillers such as carbon fiber, glass fiber, alumina fiber, silica alumina fiber, silicon carbide fiber, polyester fiber, cellulose fiber, aramid fiber, and ceramic fiber; and fine particle rubber.

[0129] Among these, those that are not decomposed or dissolved by oxidizing compounds such as aqueous solutions of permanganate used in the surface roughening treatment of the cured product are preferred, and fused silica and crystalline silica are particularly preferred because they are easy to obtain fine particles. In addition, it is preferable to use fused silica when the amount of filler to be blended is particularly large. Although fused silica can be used in either crushed or spherical form, it is more preferable to mainly use spherical silica in order to suppress an increase in the melt viscosity of the molding material while increasing the amount of fused silica blended. Furthermore, in order to increase the amount of spherical silica blended, it is preferable to appropriately adjust the particle size distribution of the spherical silica. The filler may be treated with a silane coupling agent or an organic acid such as stearic acid. The reasons for using a filler in general include the effect of improving the impact resistance of the cured product and the effect of reducing the linear expansion of the cured product.

[0130] When it acts as a flame retardant auxiliary to improve flame retardancy, metal hydroxides such as aluminum hydroxide, boehmite, and magnesium hydroxide are preferred. When it improves thermal conductivity, alumina, silicon nitride, boron nitride, aluminum nitride, fused silica, and crystalline silica are preferred, and alumina, boron nitride, fused silica, and crystalline silica are more preferred. When used in applications such as conductive paste, conductive fillers such as silver powder and copper powder can be used.

[0131] The amount of the filler is preferably high in consideration of the low linear expansion and flame retardancy of the cured product. The amount is preferably 1 to 98% by mass, more preferably 3 to 90% by mass, even more preferably 5 to 80% by mass, and particularly preferably 10 to 60% by mass, based on the total solid content in the resin composition. If the amount is high, the adhesiveness required for laminated plate applications may decrease, and the cured product may become brittle and sufficient mechanical properties may not be obtained. If the amount is low, the effect of the filler, such as improvement of the impact resistance of the cured product, may not be obtained.

[0132] Moreover, if the particle size of the filler is too large, voids tend to remain in the cured product, whereas if the particle size is too small, the filler tends to aggregate and become poorly dispersible. The average particle size (D50) is preferably 0.01 to 5 μm, more preferably 0.05 to 1.5 μm, and even more preferably 0.1 to 1 μm. If the average particle size of the filler is within this range, the flowability of the resin composition can be maintained good. The average particle size can be measured by a particle size distribution measuring device.

[0133] In addition, in the resin composition of the present invention, various known flame retardants can be used to improve the flame retardancy of the cured product obtained, as long as the reliability is not reduced. Examples of flame retardants that can be used include halogen-based flame retardants, phosphorus-based flame retardants, nitrogen-based flame retardants, silicone-based flame retardants, inorganic flame retardants, and organic metal salt-based flame retardants. From the viewpoint of the environment, flame retardants that do not contain halogens are preferred, and phosphorus-based flame retardants are particularly preferred. These flame retardants may be used alone, or two or more of the same type of flame retardants may be used in combination, or different types of flame retardants may be used in combination.

[0134] In addition, the resin composition of the present invention may contain other additives as necessary within the range that does not impair the properties of the composition, such as thermoplastic resins, coupling agents, ultraviolet absorbers, antioxidants, release agents, defoamers, emulsifiers, thixotropy-imparting agents, smoothing agents, anti-cissing agents, plasticizers, pigments, pigment dispersants, etc.

[0135] Examples of thermoplastic resins include phenoxy resins other than those of the present invention, polyurethane resins, polyester resins, polyethylene resins, polypropylene resins, polystyrene resins, ABS resins, AS resins, vinyl chloride resins, polyvinyl acetate resins, polymethyl methacrylate resins, polycarbonate resins, polyacetal resins, cyclic polyolefin resins, polyamide resins, thermoplastic polyimide resins, polyamideimide resins, polytetrafluoroethylene resins, polyetherimide resins, polyphenylene ether resins, modified polyphenylene ether resins, polyethersulfone resins, polysulfone resins, polyetheretherketone resins, polyphenylene sulfide resins, polyvinyl formal resins, etc. In terms of compatibility, phenoxy resins other than those of the present invention are preferred, and in terms of low dielectric properties, polyphenylene ether resins and modified polyphenylene ether resins are preferred.

[0136] The resin composition of the present invention may contain a coupling agent. By adding a coupling agent, the adhesiveness to the substrate and the adhesiveness between the matrix resin and the inorganic filler can be improved. Examples of the coupling agent include a silane coupling agent and a titanate coupling agent. These coupling agents may be used alone or in combination of two or more types.

[0137] The amount of the coupling agent is preferably about 0.1 to 2.0% by mass based on the total solid content in the resin composition. If the amount of the coupling agent is too small, the effect of improving the adhesion between the matrix resin and the inorganic filler due to the incorporation of the coupling agent cannot be sufficiently obtained. On the other hand, if the amount of the coupling agent is too large, the coupling agent may bleed out from the obtained cured product.

[0138] Examples of the silane coupling agent include epoxy silane coupling agents such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino silane coupling agents such as γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, γ-aminopropyltrimethoxysilane, and γ-ureidopropyltriethoxysilane; mercapto silane coupling agents such as 3-mercaptopropyltrimethoxysilane; vinyl silane coupling agents such as p-styryltrimethoxysilane, vinyltrichlorosilane, vinyltris(β-methoxyethoxy)silane, vinyltrimethoxysilane, vinyltriethoxysilane, and γ-methacryloxypropyltrimethoxysilane; and further, epoxy-, amino-, and vinyl-based polymeric silanes.

[0139] Examples of titanate coupling agents include isopropyl triisostearoyl titanate, isopropyl tri(N-aminoethyl aminoethyl) titanate, diisopropyl bis(dioctyl phosphate) titanate, tetraisopropyl bis(dioctyl phosphite) titanate, tetraoctyl bis(ditridecyl phosphite) titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, bis(dioctyl pyrophosphate)oxyacetate titanate, and bis(dioctyl pyrophosphate)ethylene titanate.

[0140] Examples of the pigment include organic pigments such as quinacridone, azo, and phthalocyanine pigments, and inorganic pigments such as titanium oxide, metal foil pigments, and rust-preventive pigments. Examples of the ultraviolet absorber include hindered amine, benzotriazole, and benzophenone absorbers. Examples of the antioxidant include hindered phenol, phosphorus, sulfur, and hydrazide absorbers. Examples of the release agent include stearic acid, palmitic acid, zinc stearate, and calcium stearate. The amount of these other additives to be added is preferably in the range of 0.01 to 20% by mass based on the total solid content in the resin composition.

[0141] The resin composition of the present invention is obtained by uniformly mixing the above components. The resin composition containing the phenoxy resin, the curing component, and further various additives as necessary can be easily made into a cured product by the same method as the conventionally known method. Examples of the cured product include molded cured products such as laminates, cast products, molded products, adhesive layers, insulating layers, and films. The method for obtaining the cured product can be the same as that for known resin compositions, and methods such as casting, injection, potting, dipping, drip coating, transfer molding, compression molding, and the like, and laminating the resin in the form of a resin sheet, a copper foil with resin, a prepreg, etc., and curing the laminated plate by heating and pressing are preferably used. The curing method of the resin composition varies depending on the blending components and blending amounts in the resin composition, but the curing temperature is usually 80 to 300 ° C, and the curing time is 10 to 360 minutes. This heating is preferably performed in two stages, namely, a primary heating at 80 to 180 ° C for 10 to 90 minutes and a secondary heating at 120 to 200 ° C for 60 to 150 minutes. In addition, in a compounding system in which the glass transition temperature (Tg) exceeds the temperature of the secondary heating, it is preferable to further perform tertiary heating at 150 to 280°C for 60 to 120 minutes. By performing such secondary and tertiary heating, it is possible to reduce poor curing. When producing a semi-cured resin product such as a resin sheet, a copper foil with resin, or a prepreg, the curing reaction of the resin composition is usually advanced to a degree that the shape can be maintained by heating or the like. When the resin composition contains a solvent, most of the solvent is usually removed by a method such as heating, decompression, or air drying, but 5 mass% or less of the solvent may remain in the semi-cured resin product.

[0142] The phenoxy resin of the present invention or the resin composition of the present invention containing other components, particularly curing components, has excellent storage stability. Therefore, the resin composition of the present invention can be applied to various fields such as paints, electrical and electronic materials, sealing materials, casting materials, carbon fiber reinforced resins, conductive pastes, adhesives, and insulating materials, and is particularly useful as insulating casting, laminate materials, sealing materials, and the like in the electrical and electronic fields. Examples of applications include printed wiring boards, flexible wiring boards, laminates for electrical and electronic circuits such as capacitors, resin-attached metal foils, adhesives such as film-like adhesives and liquid adhesives, semiconductor sealing materials, underfill materials, interchip fills for 3D-LSI, insulating materials for circuit boards, insulating sheets, prepregs, heat dissipation substrates, and resist inks, but are not limited thereto. EXAMPLES

[0143] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to these as long as it does not deviate from the gist of the invention. Unless otherwise specified, "parts" refers to parts by mass, and "%" refers to mass%. Furthermore, the unit of all equivalents is "g / eq." The analytical and measurement methods are shown below.

[0144] (1) Epoxy equivalent: Measurements were performed in accordance with JIS K7236 and expressed in units of "g / eq.". Specifically, a potentiometric titrator was used, cyclohexanone was used as the solvent, tetraethylammonium bromide acetate solution was added, and a 0.1 mol / L perchloric acid-acetic acid solution was used. For the solvent-diluted product (resin varnish), the solid content was calculated from the non-volatile content.

[0145] (2) Non-volatile content (solid content): The measurements were made in accordance with JIS K7235. The drying temperature was 200°C and the drying time was 60 minutes.

[0146] (3.1) Weight average molecular weight (Mw): The results were obtained by GPC measurement. Specifically, the main body (Tosoh Corporation, HLC-8220GPC) was fitted with a column (Tosoh Corporation, TSKgel G4000H XL , TSKgelG3000H XL , TSKgelG2000H XL ) in series was used, and the column temperature was set to 40°C. THF was used as the eluent, the flow rate was set to 1mL / min, and a differential refractive index detector was used as the detector. 0.05g of solids was dissolved in 10mL of THF and filtered through a 0.45μm microfilter, and 50μL of the sample was used. Mw was calculated by converting from a calibration curve obtained from standard monodisperse polystyrene (Tosoh Corporation, A-500, A-1000, A-2500, A-5000, F-1, F-2, F-4, F-10, F-20, F-40, F-80, F-128). Data processing was performed using GPC-8020 Model II version 6.00 manufactured by Tosoh Corporation. In the case of phosphorus-containing phenoxy resin, the measurement method described below in (3.2) was used.

[0147] (3.2) Weight average molecular weight (Mw): It was determined by GPC measurement. Specifically, a column (TSKgel SuperH-H, SuperH2000, SuperHM-H, SuperHM-H, manufactured by Tosoh Corporation) was used in series in the main body (HLC-8320GPC, manufactured by Tosoh Corporation), and the column temperature was set to 40°C. The eluent was DMF (containing 20 mM lithium bromide), the flow rate was 0.3 mL / min, and the detector was a differential refractive index detector. The measurement sample was 20 μL of a solid content of 0.1 g dissolved in 10 mL of DMF and filtered through a 0.45 μm microfilter. Mw was calculated by conversion from a calibration curve obtained from standard polyethylene oxide (SE-2, SE-5, SE-8, SE-15, SE-30, SE-70, SE-150, manufactured by Tosoh Corporation). The data was processed using GPC-8020 model II version 6.00 manufactured by Tosoh Corporation.

[0148] (4)Gardner color number: Measurements were performed in accordance with JIS K0071-2 standard.

[0149] (5) Phosphorus content: Sulfuric acid, hydrochloric acid, and perchloric acid were added to the sample, which was then heated and wet-ashed to convert all phosphorus atoms into orthophosphate. Metavanadate and molybdate were reacted in the sulfuric acid acid solution, and the absorbance of the resulting phosphorus vanadomolybdate complex was measured at 420 nm. The phosphorus content (P / resin) was calculated in percentage from a calibration curve prepared in advance. For solvent-diluted products (resin varnish), the solid content was calculated from the non-volatile content.

[0150] (6)Reactivity: The phenoxy resin was evaluated according to the following criteria based on its Mw. ○: Mw in the range of 30,000 to 150,000 ×: Mw is less than 30,000 or more than 150,000

[0151] (7)Storage stability: The phenoxy resin was evaluated according to the following criteria based on its Mw. ○: Mw increase of 1000 or less after 30 days storage at 40℃ ×: Mw increase of 1000 or more after 30 days storage at 40℃

[0152] (8) Glass transition temperature (Tg): Measurements were performed in accordance with the IPC-TM-650 2.4.25.c standard. Specifically, the temperature was expressed as the extrapolated glass transition onset temperature (Tig) of the DSC chart obtained in the second cycle of differential scanning calorimetry. The differential scanning calorimetry device used was an EXSTAR6000 DSC6200 manufactured by SII NanoTechnology Co., Ltd. The measurement sample was prepared by punching a resin film, laminating it, and packing it in an aluminum capsule. The measurement was performed in two cycles from room temperature to 280°C at a heating rate of 10°C / min.

[0153] The abbreviations used in the examples and comparative examples are as follows.

[0154] [Bifunctional epoxy resin] A1: 2,5-di-t-butylhydroquinone type epoxy resin (Nippon Steel Chemical & Material Co., Ltd., Epotohto YDC-1312, epoxy equivalent 154, m ≒ 0.05) [ka] A2: Bisphenol A type liquid epoxy resin (Nippon Steel Chemical & Material Co., Ltd., Epotohto YD-128, epoxy equivalent 186, m≒0.09) [ka]

[0155] [Diester compounds] B1: 4,4-diacetoxybiphenyl (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., active ester equivalent: 135) [ka] B2: Phosphorus-containing bifunctional acetylated compound obtained in Synthesis Example 1 (10-(2,5-diacetoxyphenyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, phosphorus content 7.6%, active equivalent 204) [ka]

[0156] [Bifunctional phenolic compounds] C1: 10-(2,5-dihydroxyphenyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (Sanko Chemical Co., Ltd., HCA-HQ, phosphorus content 9.5%, hydroxyl equivalent 162) [ka]

[0157] [Catalysts, curing accelerators] D1: Tetra(n-butyl)phosphonium-hydrogen-hexahydrophthalate (manufactured by Hokko Chemical Industry Co., Ltd., TBP-3S) [ka] D2: Tetraphenylphosphonium hydrogen phthalate (manufactured by Hokko Chemical Industry Co., Ltd., TPP-phthalic acid) [ka] D3: N,N'-Dimethylaminopyridine (Tokyo Chemical Industry Co., Ltd.) D4: 2-ethyl-4-methylimidazole (Curesol 2E4MZ, manufactured by Shikoku Chemical Industry Co., Ltd.) D5: (n-butyl)triphenylphosphonium bromide (Hokko Chemical Industry Co., Ltd., TPP-BB)

[0158] [Acid anhydride] E1: Acetic anhydride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)

[0159] [Solvents] S1: Cyclohexanone S2: Methyl ethyl ketone (MEK)

[0160] [Hardening agent] H1: Phenol novolac resin (Aica Kogyo Co., Ltd., Shounol BRG-557, hydroxyl equivalent 105)

[0161] Synthesis Example 1 In a glass reaction vessel equipped with a stirrer, a thermometer, a nitrogen gas introduction device, a cooling tube, and a dropping device, 100 parts of a bifunctional phenol compound (C1), 127 parts of acetic anhydride (E1), and 48 parts of pyridine were charged at room temperature, and the mixture was heated to 60°C while being stirred under nitrogen gas flow, and reacted for 2 hours. After that, the mixture was dried under reduced pressure at 150°C and 1.3 kPa (10 torr) for 2 hours, and 203 parts of a phosphorus-containing compound B2 was obtained.

[0162] Example 1 A glass reaction vessel equipped with a stirrer, a thermometer, a nitrogen gas inlet, a cooling tube, and a dropping device was charged with 100 parts of 2,5-di-t-butylhydroquinone type epoxy resin (A1) as a bifunctional epoxy resin, 85 parts of 4,4-diacetoxybiphenyl (B1) as a diester compound, and 46 parts of S1 as a reaction solvent at room temperature. The mixture was heated to 130 ° C. while stirring with nitrogen gas flowing, and 0.3 parts of tetra(n-butyl)phosphonium-hydrogen-hexahydrophthalate (D1) was added as a catalyst. The mixture was then heated to 145 ° C. and reacted at the same temperature for 7 hours. 46 parts of S1 and 185 parts of S2 were used as dilution solvents to dilute and mix, and a phenoxy resin varnish (R1) with a non-volatile content of 40% was obtained. The epoxy equivalent of the obtained phenoxy resin varnish (R1) was 10,000, Mw was 32,000, and the Gardner color score was 4. The reactivity was rated as good, and the storage stability was rated as good. The results are shown in Table 1.

[0163] Examples 2-3, Comparative Examples 1-2 A phenoxy resin varnish was obtained by the same operation as in Example 1, according to the charged amount (parts) of each raw material shown in Table 1. The obtained phenoxy resin varnish (R2 to R3 and RH1 to RH2) was subjected to the same measurements as in Example 1, and the measurement results are shown in Table 1. Furthermore, for R3, the phosphorus content was also measured, and the measurement results are shown in Table 1. In addition, the "molar ratio" in the table indicates the molar ratio of the difunctional epoxy resin to the diester compound.

[0164] [Table 1]

[0165] From Table 1, it can be seen that in the reaction between the epoxy group and the active ester group, the carboxylate of a specific quaternary phosphonium salt exhibits excellent reactivity, and the obtained phenoxy resin has excellent storage stability. In addition, it is possible to suppress side reactions and reduce the epoxy group equivalent weight at the same molecular weight. In addition, it also has the effect of reducing the Gardner color number.

[0166] Example 4 In the same apparatus as in Example 1, 100 parts of bisphenol A type liquid epoxy resin (A2) as a bifunctional epoxy resin, 85 parts of 10-(2,5-dihydroxyphenyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (C1) as a bifunctional phenolic compound, and 46 parts of S1 as a reaction solvent were charged at room temperature, and the mixture was heated to 150 ° C. while stirring with nitrogen gas flowing, and 0.1 parts of tetra(n-butyl)phosphonium-hydrogen-hexahydrophthalate (D1) was added as a catalyst, and then the mixture was heated to 160 ° C. and reacted at the same temperature for 5 hours. 46 parts of S1 and 185 parts of S2 were used as dilution solvents to dilute and mix, and a phenoxy resin varnish (R4) with a non-volatile content of 40% was obtained. The epoxy equivalent of the obtained phenoxy resin varnish (R4) was 9,000, Mw was 45,000, Gardner color number was 1, and phosphorus content was 4.4%. Reactivity was ◯, and storage stability was ◯. The results are shown in Table 2.

[0167] Comparative Examples 3 to 4 A phenoxy resin varnish was obtained by the same operation as in Example 4, according to the amount (parts) of each raw material shown in Table 2. The amount of catalyst D4 was adjusted in consideration of concerns about side reactions. The obtained phenoxy resin varnishes (RH3 to RH4) were subjected to the same measurements as in Example 4, and the measurement results are shown in Table 2. In addition, the "molar ratio" in the table indicates the molar ratio of the difunctional epoxy resin to the difunctional phenol compound.

[0168] [Table 2]

[0169] From Table 2, it can be seen that in the reaction of epoxy groups with phenolic hydroxyl groups, the carboxylates of certain quaternary phosphonium salts show excellent reactivity, and the resulting phenoxy resins have excellent storage stability. In addition, it is possible to suppress side reactions and reduce the epoxy equivalent weight at the same molecular weight.

[0170] Examples 5 and 6 and Comparative Example 5 A resin composition was obtained by mixing 30 parts (12 parts in solid content) of the phenoxy resin varnish (R1, R2, and RH1) obtained in Examples 1 and 2 and Comparative Example 1, 2 parts of the epoxy resin (A1), 2.5 parts of the curing agent (H1) in a 50% MEK solution, and 0.3 parts of the curing accelerator (D4) in a 20% MEK solution. These were then applied to an iron plate so that the film thickness after drying was 150 μm, and the mixture was dried at 150 ° C. for 1 hour using a dryer to obtain a polymer film-like cured product. The results of measuring Tg are shown in Table 3.

[0171] [Table 3]

[0172] As can be seen from Table 3, the resin composition containing the phenoxy resin obtained by using a specific quaternary phosphonium carboxylate as a catalyst suppresses side reactions compared to the catalyst (D3) used in the comparative example due to the quaternary phosphonium carboxylate remaining in the phenoxy resin varnish, and furthermore, due to the effect of reducing the epoxy equivalent at the same molecular weight, the functional groups contributing to the curing reaction increase, improving heat resistance. Therefore, the cured product made of the resin composition of the present invention has excellent heat resistance. [Industrial Applicability]

[0173] The phenoxy resin obtained by the production method of the present invention and a resin composition containing the same can be suitably used in the fields of paints, electric and electronic materials, adhesives, carbon fiber reinforced plastics (CFRP), and the like.

Claims

1. A method for producing a phenoxy resin by reacting a bifunctional epoxy resin with a bifunctional compound having two phenolic hydroxyl groups and / or active ester groups as functional groups in one molecule in the presence of a catalyst, wherein the catalyst is a carboxylate of a quaternary phosphonium salt represented by the following formula (1): 【Chemistry 1】 In the formula, R 1 ~R 4 each independently represents an alkyl group, an aryl group, or an aralkyl group, and may be the same or different groups. X represents a structure in which two carboxy groups have been removed from a polycarboxylic acid.

2. The method for producing a phenoxy resin according to claim 1, wherein X is any one of divalent groups represented by the following formulas (2a) to (2d): 【Chemistry 2】 In the formula, R 5 ~R 8 R each independently represents a hydrogen atom, an alkyl group, a hydroxyl group, an amino group, a carboxyl group, or a carboxyalkyl group. 10 is a methylene group or an ethylene group, R 11 ~R 18 R each independently represents a hydrogen atom, an alkyl group, or a carboxy group. 19 ~R 22 each independently represents a hydrogen atom, an alkyl group, a hydroxyl group, an amino group, or an alkoxy group.

3. The method for producing a phenoxy resin according to claim 1, wherein 0.95 to 1.05 moles of the difunctional compound are used per 1.0 mole of the difunctional epoxy resin.

4. The method for producing a phenoxy resin according to claim 1, wherein the amount of the quaternary phosphonium carboxylate used is 0.001 to 5 parts by mass per 100 parts by mass of the total amount of the bifunctional epoxy resin and the bifunctional compound.

5. 2. The method for producing a phenoxy resin according to claim 1, wherein a part or all of the difunctional epoxy resin and / or the difunctional compound is a phosphorus-containing compound.

6. The method for producing a phenoxy resin according to claim 5, wherein the phosphorus content of the obtained phenoxy resin is 1 to 6 mass %.

7. The method for producing a phenoxy resin according to claim 1, wherein the epoxy equivalent of the obtained phenoxy resin is 4,000 to 200,000 g / eq.

8. A phenoxy resin obtained by the method according to any one of claims 1 to 7.

9. The phenoxy resin has a weight average molecular weight of 10,000 to 150,000, and is characterized by containing 0.001 to 5 mass % of a carboxylate of a quaternary phosphonium salt represented by the following formula (1): 【Chemistry 3】 In the formula, R 1 ~R 4 each independently represents an alkyl group, an aryl group, or an aralkyl group, and may be the same or different groups. X represents a structure in which two carboxy groups have been removed from a polycarboxylic acid.

10. A resin composition comprising the phenoxy resin according to claim 9 and a curing component.

11. The resin composition according to claim 10, wherein the curing component is at least one selected from the group consisting of epoxy resins, acrylic ester resins, melamine resins, urea resins, phenolic resins, acid anhydride compounds, amine compounds, imidazole compounds, amide compounds, cationic polymerization initiators, organic phosphines, polyisocyanate compounds, and blocked isocyanate compounds.

12. The resin composition according to claim 10, further comprising a filler.

13. A cured product obtained by curing the resin composition according to any one of claims 10 to 12.

14. A laminate for electric / electronic circuits, comprising the resin composition according to any one of claims 10 to 12.

Citation Information

Cited By

  • Resin material, cured product, and multilayer printed wiring board

    WO2025206102A1