Inkjet ink composition and recording method

The aqueous inkjet ink composition with a phosphorus-containing self-dispersing pigment, water-soluble resin, and betaine addresses ink permeation and clogging issues, achieving superior color development and quick image fixation.

JP2024135611APending Publication Date: 2024-10-04SEIKO EPSON CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023046391
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Inkjet prints on plain paper suffer from inferior color development due to ink permeation into the medium and resin particles forming a film upon drying, leading to clogging issues in the recording device.

Method used

An aqueous inkjet ink composition comprising a self-dispersing pigment with a phosphorus-containing group, a water-soluble resin with an acid value of 250-600 mgKOH/g, and betaine, with specific mass ratios and content percentages to enhance image fixation and prevent clogging.

Benefits of technology

The composition ensures excellent color development, quick image fixation, and reduces clogging by suppressing resin drying and solidification, maintaining print quality and device reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135611000001
    Figure 2024135611000001
  • Figure 2024135611000002
    Figure 2024135611000002
  • Figure 2024135611000003
    Figure 2024135611000003
Patent Text Reader

Abstract

To provide an inkjet ink composition which has good color development property and good fastness of an obtained image, and prevents clogging in a nozzle.SOLUTION: An aqueous inkjet ink composition contains a self-dispersible pigment, a water-soluble resin, and betaine, wherein the self-dispersible pigment is a self-dispersible pigment to which a phosphorus-containing group is introduced, the water-soluble resin has an acid value of 250 mgKOH / g or more and 600 mgKOH / g or less, a content of the self-dispersible pigment is 3.5 mass% or more and 8.5 mass% or less with respect to the total mass of an ink composition, a mass ratio (self-dispersible pigment / water-soluble resin) of the self-dispersible pigment to the water-soluble resin is 2.8 or more and less than 30, and a content of the betaine is 2.5 mass% or more and 9.5 mass% or less with respect to the total mass of the ink composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ink-jet ink composition and a recording method. [Background technology]

[0002] Inkjet printing is used in a wide range of fields. It is widely used for both home and business purposes. Furthermore, with the increase in remote work and SOHO, printing at home is also on the rise.

[0003] For example, Patent Document 1 discloses an ink composition that contains a pigment, a resin, and an organic solvent and is injected into an ink container having an ink chamber that can be refilled with the ink composition and an ink inlet that can be opened and closed, the ink chamber being capable of communicating with the outside air. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-061896 A Summary of the Invention [Problem to be solved by the invention]

[0005] In comparison with printing methods such as electrophotography, inkjet prints are inferior in color development on plain paper. One of the reasons for this is that, due to the liquid nature of the inkjet ink composition, the coloring material penetrates into the recording medium together with the ink and does not remain on the surface. In addition, when a dispersion resin (resin particles) is used to improve the scratch resistance of an image on a recording medium, the resin particles dry and form a film when the inkjet ink composition dries, and solidify, which may worsen the recovery ability of the recording device when it becomes clogged. [Means for solving the problem]

[0006] One embodiment of the ink-jet ink composition according to the present invention is a water-based ink-jet ink composition, Contains a self-dispersing pigment, a water-soluble resin, and a betaine, the self-dispersion pigment is a self-dispersion pigment having a phosphorus-containing group introduced therein; The water-soluble resin has an acid value of 250 mgKOH / g or more and 600 mgKOH / g or less, the content of the self-dispersion pigment is 3.5% by mass or more and 8.5% by mass or less with respect to the total mass of the ink composition; a mass ratio of the self-dispersion pigment to the water-soluble resin (self-dispersion pigment / water-soluble resin) is 2.8 or more and less than 30; The content of the betaine is 2.5% by mass or more and 9.5% by mass or less with respect to the total mass of the ink composition.

[0007] One aspect of the recording method according to the present invention is to This is carried out using an inkjet recording device having an inkjet head, ejecting an ink-jet ink composition from the ink-jet head and depositing the ink-jet ink composition on a recording medium; The ink-jet ink composition is the ink-jet ink composition described above. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic diagram of an example of an inkjet recording apparatus. [Diagram 2] FIG. 1 is a block diagram of an example of an inkjet recording apparatus. [Diagram 3] Table 1 shows the composition of the compositions of the examples. [Figure 4] Table 2 shows the composition formulations of the examples and comparative examples. [Diagram 5] Table 3 shows the compositional formulations of comparative examples and reference examples. [Figure 6] Table 4 shows the evaluation results of the compositions of the examples. [Figure 7] Table 5 shows the evaluation results of the compositions of the examples and comparative examples. [Figure 8] Table 6 shows the evaluation results of the compositions of comparative examples and reference examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The following describes an embodiment of the present invention. The embodiment described below is an example of the present invention. The present invention is not limited to the following embodiment, and includes various modified forms that are implemented within the scope of the present invention. Note that not all of the configurations described below are necessarily essential configurations of the present invention.

[0010] 1. Inkjet ink composition The inkjet ink composition of this embodiment is a water-based composition that contains a self-dispersing pigment, a water-soluble resin, and betaine.

[0011] 1.1. Self-dispersing pigments The inkjet ink composition of this embodiment contains a self-dispersing pigment in which a phosphorus-containing group has been introduced. A self-dispersing pigment is a pigment that can be dispersed and / or dissolved in an aqueous medium without a dispersant such as a resin or a surfactant. Here, "dispersed and / or dissolved in an aqueous medium without a dispersant" refers to a state in which the pigment is stably present in the aqueous medium due to hydrophilic groups on the surface, even without using a dispersant to disperse the pigment.

[0012] An inkjet ink composition containing a self-dispersing pigment does not need to contain a dispersant for dispersing the pigment, and is easy to have excellent ejection stability because it is almost free of bubbles caused by the dispersant and the defoaming property is hardly deteriorated. In addition, the ejection reliability is also excellent because the generation of foreign matter due to drying at the gas-liquid interface caused by the dispersant is suppressed. In addition, since a significant increase in viscosity caused by the dispersant is suppressed, it is possible to contain a larger amount of pigment, and the print density may be increased.

[0013] Furthermore, when the recording medium contains calcium, the self-dispersing pigment reacts with calcium to easily form an image with excellent color development. The self-dispersing pigment of the present embodiment is a self-dispersing pigment having a phosphorus-containing group bonded to its surface, and therefore such color development is easily obtained. This tendency is particularly strong in the self-dispersing pigment having a phosphonic acid group bonded to its surface.

[0014] Self-dispersed pigments tend to have slightly inferior image fixation properties compared to pigments in which an anionic resin is physically adsorbed onto the surface of the pigment particles, or resin-dispersed pigments in which the pigment is encapsulated and dispersed in an anionic resin. However, the inkjet ink composition of the present embodiment can achieve excellent image fixation properties by using a water-soluble resin described below.

[0015] The self-dispersing pigment having a phosphorus-containing group introduced therein includes pigments in which the phosphorus-containing group is bonded to the pigment surface directly or via another atomic group.

[0016] Examples of phosphorus-containing groups present on the surface of the self-dispersing pigment include phosphate groups, phosphonate groups, -PO3HM, and -PO3M2. Among these, phosphate groups are more preferred. In the formula, M represents a hydrogen atom, an alkali metal, ammonium, or an organic amine, and R represents an alkyl group having 1 to 12 carbon atoms or a naphthyl group which may have a substituent.

[0017] Examples of other atomic groups include linear or branched alkylene groups having from 1 to 12 carbon atoms, phenylene groups, naphthylene groups, amide groups, sulfonyl groups, amino groups, carbonyl groups, ester groups, ether groups, and combinations of these groups.

[0018] These self-dispersing pigments include those in which a phosphorus-containing group is bonded to the surface of a pigment particle by a known method, and those in which a functional group containing a phosphorus-containing group, such as diazo coupling, is bonded to the surface of a pigment particle, and either of these can be suitably used. A self-dispersing pigment in which an anionic resin is bonded to the surface of a pigment particle may also be used, and the hydrophilic unit is a resin having at least a unit having a phosphorus-containing group, which is bonded to the surface of a pigment particle directly or via another atomic group.

[0019] The pigment that can be made self-dispersible is not particularly limited, and examples of the pigment that can be used include inorganic pigments such as carbon black, calcium carbonate, and titanium oxide, and organic pigments such as azo pigments, isoindolinone pigments, diketopyrrolopyrrole pigments, phthalocyanine pigments, quinacridone pigments, and anthraquinone pigments.

[0020] Examples of black pigments include No. 2300, No. 900, MCF88, No. 33, No. 40, No. 45, No. 52, MA7, MA8, MA100, No. 2200B, etc. (all manufactured by Mitsubishi Chemical Corporation), Raven 5750, Raven 5250, Raven 5000, Raven 3500, Raven 1255, Raven 700, etc. (all manufactured by Columbia Carbon Co., Ltd.), Rega1 400R, Rega1 330R, Rega1 660R, Mogul L, Monarch 700, Monarch 800, Monarch 880, Monarch 900, Monarch 1000, Monarch 1100, Monarch 1300, Monarch 1400, etc. (all manufactured by Cabot Corporation), Color Black FW1, Color Black FW2, Color Black Examples of such inks include FW2V, Color Black FW18, Color Black FW200, Color Black S150, Color Black S160, Color Black S170, Printex 35, Printex U, Printex V, Printex 140U, Special Black 6, Special Black 5, Special Black 4A, and Special Black 4 (all manufactured by Degussa).

[0021] White pigments include CI Pigment White 1 (basic lead carbonate), 4 (zinc oxide), 5 (mixture of zinc sulfide and barium sulfate), 6 (titanium dioxide), 6:1 (titanium dioxide with other metal oxides), 7 (zinc sulfide), 18 (calcium carbonate), 19 (clay), 20 (titanium mica), 21 (barium sulfate), 22 (natural barium sulfate), 23 (gloss white), 24 (alumina white), 25 (gypsum), 26 (magnesium oxide-silicon oxide), 27 (silica), and 28 (anhydrous calcium silicate).

[0022] Examples of yellow pigments include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 16, 17, 24, 34, 35, 37, 53, 55, 65, 73, 74, 75, 81, 83, 93, 94, 95, 97, 98, 99, 108, 109, 110, 113, 114, 117, 120, 124, 128, 129, 133, 138, 139, 147, 151, 153, 154, 167, 172, and 180.

[0023] Magenta pigments include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 40, 41, 42, 48(Ca), 48(Mn), 57(Ca), 57:1, 88, 112, 114, 122, 123, 144, 146, 149, 150, 166, 168, 170, 171, 175, 176, 177, 178, 179, 184, 185, 187, 202, 209, 219, 224, 245, and CI Pigment Violet 19, 23, 32, 33, 36, 38, 43, 50.

[0024] Cyan pigments include CI Pigment Blue 1, 2, 3, 15, 15:1, 15:2, 15:3, 15:34, 15:4, 16, 18, 22, 25, 60, 65, 66, and CI Vat Blue 4 and 60.

[0025] Examples of pigments other than black, white, yellow, magenta, and cyan include CI Pigment Green 7, 10, CI Pigment Brown 3, 5, 25, 26, and CI Pigment Orange 1, 2, 5, 7, 13, 14, 15, 16, 24, 34, 36, 38, 40, 43, 63, and the like.

[0026] Examples of color pigments include pigments such as Pigment Yellow, Pigment Red, Pigment Violet, and Pigment Blue listed in the Color Index, as well as phthalocyanine, azo, anthraquinone, azomethine, and condensed ring pigments. Other examples include organic pigments such as Yellow No. 4, No. 5, No. 205, and No. 401; Orange No. 228 and No. 405; and Blue No. 1 and No. 404; and inorganic pigments such as titanium oxide, zinc oxide, zirconium oxide, iron oxide, ultramarine, Prussian blue, and chromium oxide.

[0027] The above-exemplified pigments may be pigments in which a phosphorus-containing group is bonded to the particle surface directly or via another atomic group.

[0028] On the other hand, examples of self-dispersing pigments other than carbon black include those in which a phosphorus-containing group is bonded to the pigment surface via a phenyl group. As a surface treatment method for bonding the functional group or a salt thereof, which is a phosphorus-containing group, to the pigment surface via a phenyl group, various known surface treatment methods can be applied.

[0029] The content of the self-dispersed pigment (solid content) is 3.5% by mass or more and 8.5% by mass or less with respect to the total mass of the inkjet ink composition. The content of the self-dispersed pigment (solid content) is preferably 4% by mass or more, more preferably 4.5% by mass or more with respect to the total mass of the inkjet ink composition. The content of the self-dispersed pigment (solid content) is preferably 8% by mass or less, more preferably 7.5% by mass or less, and particularly preferably 7% by mass or less with respect to the total mass of the inkjet ink composition. When the content of the self-dispersed pigment is within the above range, the color development and clogging recovery properties may be more excellent.

[0030] In the inkjet ink composition of this embodiment, the amounts of the self-dispersing pigment and the water-soluble resin are set so that the mass ratio of the self-dispersing pigment to the water-soluble resin (self-dispersing pigment / water-soluble resin) is 2.8 or more and less than 30. In addition, this mass ratio is preferably 3.0 or more and less than 28, and more preferably 3.2 or more and less than 25.

[0031] If the amount of the water-soluble resin is small relative to the self-dispersing pigment, the abrasion resistance of the image may be poor, whereas if the amount of the water-soluble resin is large relative to the self-dispersing pigment, clogging may occur.

[0032] The self-dispersing pigment having a phosphorus-containing group may contain an anionic group other than the phosphorus-containing group. Furthermore, the inkjet ink composition of this embodiment may contain a self-dispersing pigment that does not have a phosphorus-containing group.

[0033] 1.2.Water-soluble resin The inkjet ink composition of this embodiment contains a water-soluble resin having an acid value of 250 mgKOH / g or more and 600 mgKOH / g or less. The content of the water-soluble resin is such that the mass ratio of the self-dispersing pigment to the water-soluble resin (self-dispersing pigment / water-soluble resin) is 2.8 or more and less than 30.

[0034] The water-soluble resin mainly contributes to the fixability of the image. Unlike resin particles, the water-soluble resin is less likely to become a foreign body at the gas-liquid interface. However, when the water-soluble resin dries at the gas-liquid interface, the dried and solidified components may cause clogging. Since the water-soluble resin is highly hydrophilic, when the water dries and the environment becomes hydrophobic, the resin may become a foreign body and become difficult to re-dissolve. In particular, it is presumed that the water-soluble resin and the hydrophilized self-dispersing pigment become a composite foreign body and become difficult to re-dissolve when the water dries and the environment becomes hydrophobic. In the inkjet ink composition of the present embodiment, it is believed that the betaine described below is contained, and thus the betaine takes in (absorbs) the water-soluble resin, which is believed to suppress the water-soluble resin from becoming foreign matter, and even if the water-soluble resin does become foreign matter, it is believed that the water-soluble resin can be re-dissolved, which is believed to result in good clogging resistance.

[0035] In addition, the water-soluble resin may generate foreign matter when mixed with other components such as the self-dispersing pigment in the inkjet ink composition, but the inkjet ink composition of the present embodiment contains betaine, which is described below, and is considered to form a state in which the betaine incorporates (absorbs) foreign matter including the water-soluble resin, thereby suppressing the formation of foreign matter, and even if foreign matter does form, it is presumed that re-solubility is obtained, which is considered to result in good clogging resistance.

[0036] Water-soluble resins can also improve the robustness of images. The mechanism by which water-soluble resins improve the robustness of images is different from the mechanism by which dispersion particles improve the robustness of images. Water-soluble resins are thought to have the effect of fixing images to recording media by reacting with Ca (calcium) contained in the recording media. On the other hand, the main mechanism for resin particles is that the resin is fixed by evaporation of water, and fixing the resin takes a relatively long time. Therefore, no significant difference is observed after a certain amount of time has passed since printing, but when compared immediately after printing, water-soluble resins can exhibit superior robustness at an earlier stage. Water-soluble resins also have superior color development because they quickly fix the ink components on the recording media by reacting with Ca in the recording media.

[0037] In this specification, the water-soluble resin is different from a resin for dispersing a pigment (pigment dispersion resin) used to disperse a pigment, and refers to a resin that is not attached to the pigment by adsorption or the like, but is dissolved in the ink. In this specification, "water-soluble" refers to a property that allows the resin to dissolve in ion-exchanged water at 20°C at 3% by mass or more, preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 25% by mass or more.

[0038] "Soluble" means that after mixing and stirring the resin with water, there is no sign of residual dissolution, cloudiness, or layer separation. Also, the resin is not dispersed in water (resin particles), but rather dissolved in water.

[0039] The characteristics of the water-soluble resin include anionic resin, nonionic resin, and cationic resin. In the inkjet ink composition of this embodiment, it is preferable to use an anionic resin. The water-soluble resin preferably has an acidic group in its structure and has an acid value. The acidic group may be in the form of a salt. Examples of the acidic group include a carboxy group, a sulfonyl group, and a phosphate group, and the carboxy group is more preferable.

[0040] The acid value of the water-soluble resin used in this embodiment is 250 [KOHmg / g] or more and 600 [KOHmg / g] or less, preferably 300 [KOHmg / g] or more and 500 [KOHmg / g] or less, more preferably 350 [KOHmg / g] or more and 450 [KOHmg / g] or less, and even more preferably 400 [KOHmg / g] or more and 450 [KOHmg / g] or less.

[0041] The acid value is measured by titration, for example, by the method described in JIS K 0070:1992 (potentiometric titration method).

[0042] When the acid value of the water-soluble resin is within the above range, the balance between the hydrophobic group and the hydrophilic group is good, so that an image having excellent solubility in water and excellent water resistance can be obtained.

[0043] On the other hand, if the acid value of the water-soluble resin is less than the above range, the solubility of the water-soluble resin in water may decrease, and foreign matter may easily be generated. If the acid value of the water-soluble resin exceeds the above range, the solubility of the water-soluble resin in water may become too high, and the water resistance of the image may decrease. The "acid value" refers to the amount of KOH (mg) required to neutralize 1 g of the water-soluble resin.

[0044] Preferred types of water-soluble resins include, for example, acrylic resins, maleic acid resins, urethane resins, and polyester resins.

[0045] The acrylic resin is a resin obtained by polymerizing at least an acrylic monomer.

[0046] The maleic acid resin is a resin polymerized using at least maleic acid or a maleic acid derivative. More specifically, it includes an acrylic resin, a styrene-acrylic resin, a styrene-maleic acid resin, an acrylonitrile-acrylic resin, a vinyl acetate-acrylic resin, a polyurethane resin, and a polyester resin. The water-soluble resin is preferably selected from an acrylic resin or a maleic acid resin.

[0047] Furthermore, a maleic acid-based resin obtained by polymerization using at least maleic acid or a maleic acid derivative, such as a styrene-maleic acid-based resin, is more preferable. In other words, a maleic acid-based resin is a polymer compound having a structure derived from maleic acids.

[0048] A resin obtained by polymerizing at least an acrylic monomer and maleic acid or a maleic acid derivative is called a maleic acid-based resin.

[0049] Examples of maleic acids include compounds having a structure in which one carboxyl group is bonded to each of adjacent carbon atoms bonded to ethylene through a carbon-carbon double bond, and compounds that are derivatives of this.

[0050] Specific examples of maleic acids include maleic acid, maleic anhydride, fumaric acid, citraconic acid, citraconic anhydride, and mesaconic acid. The maleic acids may be those in which the carboxyl groups bonded to the adjacent carbon atoms are dehydrated and cyclized or esterified. Carboxyl groups that form salts are also included in the carboxyl group.

[0051] The above-mentioned derivatives include those in which the carboxyl group is derivatized as described above, and those in which the ethylene skeleton further has a substituent.

[0052] Among maleic acids, it is preferable to use maleic acid or a maleic acid derivative having a carboxyl group.

[0053] The maleic acid resin may be a resin in which a carboxyl group derived from maleic acid is dehydrated and cyclized or esterified. A carboxyl group that forms a salt is also included in the carboxyl group.

[0054] The polymer compound having a structure derived from a maleic acid compound may be a polymer compound obtained by polymerization or copolymerization using at least a maleic acid compound.

[0055] The maleic acid resin may be a polymer of maleic acid or a copolymer of maleic acid and other monomers, such as vinyl monomers, styrene, vinyl naphthalene, vinyl acetate, etc., and acrylic monomers, such as (meth)acrylic acid, esters of (meth)acrylic acid, etc.

[0056] Maleic acid resins have a structure derived from maleic acids, and have carboxyl groups or structures derived from carboxyl groups on adjacent carbon atoms. Here, for example, when a polymer of acrylic acid is polymerized by a generally known method, it is polymerized in a so-called head-to-tail manner, so it is statistically rare for carboxyl groups to be located on adjacent carbons. Therefore, in the case of a polymer of acrylic acids, compared to the case of polymerizing maleic acids, it is rare for carboxyl groups to be located adjacent to each other in the carbon chain of the main chain in the polymer. This makes it possible to confirm whether adjacent carboxyl groups are derived from maleic acids, for example, by NMR (nuclear magnetic resonance) or the like.

[0057] The carboxyl group of the maleic acid resin may be esterified. For example, it may be esterified with a compound having a hydroxyl group. The two carboxyl groups in the structure derived from maleic acid may not be esterified, one may be esterified, or both may be esterified.

[0058] In addition, when the carboxyl group of the structure derived from maleic acids is not esterified, it may be present as a carboxylic acid in the aqueous ink-jet ink composition, or may be partially or completely neutralized with ammonia, an alkanolamine or an alkylamine.

[0059] Maleic acid-based resins are water-soluble because they contain many structures derived from the carboxyl groups of maleic acids. Therefore, in a water-based inkjet ink composition, the molecular chains of the maleic acid-based resin are spread out. This increases the probability that the maleic acid-based resin will encounter the aggregating agent when the inkjet ink composition is mixed with the aggregating agent. Therefore, the maleic acid-based resin has good aggregating properties, which can improve the image quality of the image obtained by using the ink set.

[0060] When one of the two carboxyl groups in the structure derived from maleic acids of the maleic acid resin is esterified, the water resistance of the resulting image tends to improve. In addition, when the two carboxyl groups in the structure derived from maleic acids are not esterified, the water resistance of the resulting image tends to decrease. Depending on the degree of esterification, the balance between the hydrophilicity and hydrophobicity of the maleic acid resin can be adjusted, which can improve the storage stability of the inkjet ink composition and further improve the water resistance of the resulting image. For example, styrene maleic anhydride half ester copolymer salt is preferable in terms of the balance between hydrophilicity and hydrophobicity. This is presumably because the esterified carboxyl group is highly hydrophobic and promotes insolubilization and solid-liquid separation during the reaction.

[0061] When the maleic acid-based resin contains a structure derived from maleic anhydride, it is believed that in water, the anhydride is converted into a carboxyl group by addition of water.

[0062] The maleic acid-based resin is a water-soluble resin, and unlike a pigment dispersant, it does not adsorb to the pigment in the inkjet ink composition, and exists as a solution dissolved in water, which is the solvent component of the ink. When the ink contains a pigment dispersed with a pigment dispersant, the maleic acid-based resin described in this section is contained in the ink separately from the pigment dispersant.

[0063] Maleic acid-based resins exhibit coagulability due to the action of a coagulant such as calcium propionate, which will be described later, depending on the skeleton of the resin constituting the particles, the number of functional groups, and the properties thereof.

[0064] The maleic acid resin preferably has an acidic group such as a carboxyl group, a sulfonic acid group, or a phosphoric acid group. That is, even if the carboxyl group derived from maleic acids is present in the form of an acid or a salt, or even if all of the carboxyl groups derived from maleic acids are esterified, the skeleton or ester group preferably has an acidic group such as a carboxyl group, a sulfonic acid group, or a phosphoric acid group in the form of an acid or a salt. In addition, the acidic group may be partially or completely neutralized with ammonia, an alkanolamine, or an alkylamine.

[0065] Commercially available maleic acid resins include, for example, SN Dispersant 5027 and 5029 (manufactured by San Nopco Ltd.), Sunspearl PS-8 (manufactured by Sanyo Chemical Industries Ltd.), Marialim HKM-50A, 150A, AKM-0531, SC-0505K, and Polystar OMA (manufactured by NOF Corp.), Demol P, EP, ST, Boys 520 and 521 (manufactured by Kao Corp.), and Polity A550 (manufactured by Lion Corp.). Examples of such compounds include Arakawa Chemical Industries Co., Ltd.), Alastar 703S, Polymaron 1318, 351T, 385, 372, 375CB, 482, 482S, and 1329 (all manufactured by Arakawa Chemical Industries Co., Ltd.), XIRAN 1440H, 2625H, 1000H, 2000H, and 3000H (all manufactured by Polyscope Co., Ltd.), Isoban-104 (manufactured by Kuraray Co., Ltd.), FLOWLEN G-700AMP, and G-700DMEA (all manufactured by Kyoeisha Chemical Co., Ltd.).

[0066] In the anionic water-soluble resin, the composition ratio of the water-soluble monomer in its molecular structure is preferably 70% by mass or less, preferably less than 60% by mass, and more preferably 50% by mass or less, when the total monomers of the water-soluble resin are taken as 100% by mass. In addition, the composition ratio of the water-soluble monomer in the molecular structure of the anionic water-soluble resin is preferably 25% by mass or more, more preferably 30% by mass or more, when the total monomers of the water-soluble resin are taken as 100% by mass. Furthermore, it is preferably 40% by mass or more.

[0067] If the composition ratio of the water-soluble monomer in the molecular structure of the anionic water-soluble resin is smaller than the above range, sufficient water solubility is not obtained, and the resin cannot be regarded as a water-soluble polymer, but rather appears as a dispersed resin (resin particles).On the other hand, if the composition ratio is larger than the above range, the water-soluble resin is likely to precipitate when the water evaporates, i.e., when the ink-jet ink composition becomes hydrophobic, and clogging may worsen.

[0068] The water-soluble urethane resin means a water-soluble urethane resin having a polar group in the molecular structure. The polar group may be in a salt state. In addition, the polar group is preferably an acidic group. Examples of the acidic group include phosphorus-containing groups such as a carboxyl group, a sulfonic acid group, and a phosphoric acid group.

[0069] The water-soluble urethane resin has repeating units derived from polyisocyanate and polyol, and among them, those having repeating units derived from polyol having an acid group are preferred, and resins having repeating units derived from polyisocyanate, polyol having no acid group, and polyol having an acid group are preferred. The water-soluble urethane resin may further have repeating units derived from polyamine.

[0070] The water-soluble polyester resin may be any resin having a polyester structure. Other examples of the water-soluble resin include nonionic water-soluble resins such as polyethylene oxide, carboxymethyl cellulose, hydroxyethyl cellulose, polyvinylpyrrolidone, hydroxypropyl methyl cellulose, cellulose acetate, polyvinyl alcohol, and salts thereof.

[0071] The weight average molecular weight Mw of the water-soluble resin is preferably 5,000 or more and 150,000 or less, more preferably 10,000 or more and 100,000 or less, even more preferably 15,000 or more and 50,000 or less, even more preferably 20,000 or more and 30,000 or less, and especially preferably 20,000 or more and 23,000 or less.

[0072] By setting the molecular weight range to the lower limit or more, the viscosity of the ink-jet ink composition can be made suitable, and for example, good color development can be obtained. By setting the molecular weight range to the upper limit or less, the viscosity of the ink-jet ink composition can be made more suitable for the ink-jet method.

[0073] In this specification, the molecular weight of the water-soluble resin refers to a molecular weight measured by a GPC method and is the molecular weight of a standard sample. The molecular weight may be measured for the water-soluble resin alone or for the inkjet ink composition. In this case, it is preferable that the components contained in the inkjet ink composition are specified.

[0074] The content of the water-soluble resin is preferably 0.1% by mass or more and 10.0% by mass or less, more preferably 0.2% by mass or more and 5.0% by mass or less, more preferably 0.3% by mass or more and 2% by mass or less, and even more preferably 0.4% by mass or more and 1.8% by mass or less, based on the total mass of the inkjet ink composition. If the content is within such a range, sufficient image fixation can be obtained. Furthermore, if the content is within such a range, the viscosity of the inkjet ink composition can be easily adjusted to a more appropriate range. Furthermore, clogging resistance is also more excellent.

[0075] In the inkjet ink composition of this embodiment, the amounts of the self-dispersing pigment and the water-soluble resin are set so that the mass ratio of the self-dispersing pigment to the water-soluble resin (self-dispersing pigment / water-soluble resin) is 2.8 or more and less than 30. Moreover, this mass ratio is preferably 3.0 or more and 28 or less, and more preferably 3.2 or more and 25 or less. It is further preferably 3.5 to 20, more preferably 4.0 to 10.0, more preferably 5.0 to 8.0, and even more preferably 5.5 to 7.0.

[0076] If the amount of the water-soluble resin is small relative to the self-dispersing pigment, the abrasion resistance of the image may be poor, whereas if the amount of the water-soluble resin is large relative to the self-dispersing pigment, clogging may occur.

[0077] 1.3. Betaine Betaine means a compound that has a positive charge and a negative charge at non-adjacent positions in the same molecule, has no dissociable hydrogen bonded to the positively charged atom, can form an intramolecular salt, and has no charge as a whole molecule. In this embodiment, the betaine is preferably one in which the positively charged site is a quaternary ammonium cation.

[0078] By including betaine in the inkjet ink composition, it is possible to suppress the deflection of the inkjet ink composition or non-ejection caused by the inkjet ink composition drying in the nozzle of the inkjet head, and to improve the clogging resistance. As already mentioned, it is considered that the betaine takes in (absorbs) the above-mentioned water-soluble resin, and this can be assumed to suppress the water-soluble resin from becoming a foreign body, and even if it becomes a foreign body, it can be assumed that re-dissolving is obtained. This is considered to result in good clogging resistance.

[0079] The betaine is not particularly limited, and examples thereof include trialkylglycines such as trimethylglycine and triethylglycine, γ-butyrobetaine, homarine, trigonelline, carnitine, homoserine betaine, valine betaine, lysine betaine, ornithine betaine, alanine betaine, stachydrine, and glutamic acid betaine. Among them, the glycine contained in the inkjet ink composition is preferably selected from trialkylglycines, and more preferably contains trimethylglycine. Trialkylglycine is a compound in which three alkyl groups are substituted on the nitrogen atom of glycine. This tends to improve clogging properties. Note that one type of betaine may be used alone, or two or more types may be used in combination.

[0080] The number of carbon atoms constituting the betaine is preferably 4 or more and 12 or less, more preferably 4 or more and 7 or less, and even more preferably 4 or more and 6 or less. When the number of carbon atoms in the betaine is within the above range, the above-mentioned effect tends to be more remarkable.

[0081] The content of betaine is 2.5% by mass or more and 9.5% by mass or less, based on the total mass of the inkjet ink composition. The content of betaine is preferably 3% by mass or more and 8% by mass or less, more preferably 4% by mass or more and 8% by mass or less, based on the total mass of the inkjet ink composition. By having the content of betaine within the above range, it is possible to suppress the formation of foreign matter in the water-soluble resin. If the content of betaine is less than the above range, the suppression of drying and solidifying of the water-soluble resin tends to be insufficient, and clogging properties may be poor. If the content of betaine is more than the above range, the drying and solidifying of the betaine when the betaine itself dries tends to increase, and clogging properties may be deteriorated.

[0082] 1.4.Water The inkjet ink composition of the present embodiment is an aqueous composition containing water. An "aqueous" composition is a composition in which water is one of the main solvents. Examples of water include pure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, and distilled water, as well as ultrapure water with reduced ionic impurities. In addition, if water sterilized by ultraviolet irradiation or the addition of hydrogen peroxide is used, the growth of bacteria and fungi can be suppressed when the inkjet ink composition is stored for a long period of time.

[0083] The water content is 30% by mass or more, preferably 40% by mass or more, more preferably 45% by mass or more, and even more preferably 50% by mass or more, based on the total amount (100% by mass) of the ink-jet ink composition. The upper limit of the water content is preferably 97% by mass or less, even more preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less, based on the total amount (100% by mass) of the ink composition.

[0084] 1.5.Other Ingredients The inkjet ink composition of this embodiment may contain the following components in addition to the above components.

[0085] 1.5.1. Organic Solvents The inkjet ink composition of this embodiment may contain an organic solvent. Examples of the organic solvent include alkyl polyols, glycol ethers, and nitrogen-containing solvents.

[0086] 1.5.1.1. Alkyl polyols The inkjet ink composition of this embodiment may contain an alkyl polyol. An alkyl polyol is a compound having a skeleton and having two or more hydroxyl groups (substituted with two or more hydroxyl groups). Examples of the skeleton include an alkyl chain and a polyalkyleneoxy chain. The number of hydroxyl groups in the molecule is 2 or more, preferably 2 to 4, and more preferably 2 or 3. The number of carbon atoms in the molecule is preferably 2 to 10.

[0087] The alkyl polyol conceptually includes polyhydric alcohol, and when it contains an alkyl polyol, it is possible to enhance the moisture retention of the ink-jet ink composition, to provide excellent ejection stability by the ink-jet method, and to effectively suppress evaporation of water from the recording head when left unused for a long period of time. This also makes it possible to better maintain recovery after being left unused and continuous ejection stability, even when a coloring material that is prone to clogging the nozzle is used.

[0088] Specific examples of alkyl polyols include 1,2-butanediol, 1,2-pentanediol, 1,2-hexanediol, 1,2-heptanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-ethyl-2-methyl-1,3-propanediol, 2-methyl-2-propyl-1,3-propanediol, 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 3-methyl-1,3-butanediol, 2-ethyl-1,3-hexanediol, 3-methyl-1,5-pentanediol, 2-methylpentane-2,4-diol, diethylene glycol, propylene glycol, dipropylene glycol, glycerin, triethylene glycol, and tetraethylene glycol. These alkyl polyols may be used alone or in combination of two or more.

[0089] The inkjet ink composition more preferably contains, among the alkyl polyols, an alkanediol having a carbon number of 3 to 6. Examples of the alkanediol having a carbon number of 3 to 6 include 1,2-butanediol, 1,2-pentanediol, 1,2-hexanediol, 1,2-heptanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-ethyl-2-methyl-1,3-propanediol, 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 3-methyl-1,3-butanediol, 3-methyl-1,5-pentanediol, and 2-methylpentane-2,4-diol.

[0090] When the inkjet ink composition contains an alkanediol having 3 to 6 carbon atoms, the viscosity may be further suppressed and the ejection stability (reliability of continuous ejection) may be improved. In addition, the solubility and dispersibility of the coloring material may be improved, and good clogging recovery may be obtained.

[0091] When the inkjet ink composition contains an alkyl polyol, it more preferably contains a polyol having a normal boiling point of more than 280° C. Examples of polyols having a normal boiling point of more than 280° C. include glycerin and triethylene glycol. By containing such a polyol, the drying speed of the inkjet ink composition can be suppressed, and clogging resistance and ejection stability can be improved in some cases.

[0092] When an alkyl polyol is contained, the content thereof is preferably from 2 to 30% by mass, more preferably from 5 to 20% by mass, and even more preferably from 8 to 15% by mass, based on the total amount of the inkjet ink composition.

[0093] 1.5.1.2. Glycol ethers The inkjet ink composition of this embodiment may contain a glycol ether. Examples of the glycol ether include monoalkyl ethers or dialkyl ethers of glycols selected from ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, and polyoxyethylene polyoxypropylene glycol. More specifically, examples of the glycol ether include methyl triglycol (triethylene glycol monomethyl ether), butyl triglycol (triethylene glycol monobutyl ether), butyl diglycol (diethylene glycol monobutyl ether), and dipropylene glycol monopropyl ether, and a typical example is diethylene glycol monobutyl ether.

[0094] It is more preferable that the inkjet ink composition contains, among the glycol ethers, one or more selected from the glycol ethers represented by the following formula (1). R 1 -O-(CH2-CH2-O) n -R 2 (1) (In formula (1), R 1 represents H or an alkyl group having 1 to 4 carbon atoms, R 2 represents an alkyl group having 1 to 4 carbon atoms, and n represents an integer of 2 to 3.

[0095] Examples of glycol ethers represented by formula (1) include methyl triglycol (triethylene glycol monomethyl ether), butyl triglycol (triethylene glycol monobutyl ether), butyl diglycol (diethylene glycol monobutyl ether), triethylene glycol dimethyl ether, triethylene glycol dibutyl ether, and diethylene glycol dibutyl ether.

[0096] A mixture of two or more glycol ethers may be used. When glycol ethers are used, the total amount of glycol ethers is from 0.5% by mass to 30% by mass, preferably from 1.0% by mass to 20% by mass, more preferably from 3.0% by mass to 10.0% by mass, based on the total amount of the inkjet ink composition, from the viewpoints of adjusting the viscosity of the inkjet ink composition and suppressing clogging due to the moisturizing effect.

[0097] 1.5.1.3.Nitrogen-containing substances The inkjet ink composition of this embodiment may contain a nitrogen-containing compound. The nitrogen-containing compound is preferably, for example, an amide. The amide may be a cyclic amide or a non-cyclic amide. The nitrogen-containing compound is expected to have the effect of suppressing solidification or drying of the inkjet ink composition.

[0098] Examples of the cyclic amide include compounds having a ring structure containing an amide group. Examples of such compounds include γ-lactams such as 2-pyrrolidone, 1-methyl-2-pyrrolidone (N-methyl-2-pyrrolidone), 1-ethyl-2-pyrrolidone (N-ethyl-2-pyrrolidone), 1-propyl-2-pyrrolidone, 1-butyl-2-pyrrolidone, and N-vinyl-2-pyrrolidone (NVP), β-lactams, δ-lactams, and ε-lactams such as ε-caprolactam. These cyclic amides may be used alone or in combination of two or more.

[0099] 1.5.1.4. Other organic solvents The inkjet ink composition of this embodiment may contain other organic solvents, such as lactones such as γ-butyrolactone, and betaine compounds.

[0100] The content of the organic solvent is preferably from 2 to 30% by mass, more preferably from 5 to 20% by mass, and even more preferably from 8 to 15% by mass, based on the total amount of the inkjet ink composition.

[0101] 1.5.2.Resin particles The inkjet ink composition may contain resin particles. The resin particles are also called dispersion resin. Since the resin particles tend to cause a decrease in clogging properties, the content of the resin particles is preferably 1% by mass or less, more preferably 0.5% by mass or less, even more preferably 0.3% by mass or less, more preferably 0.1% by mass or less, and particularly preferably less than 0.1% by mass, based on the total mass of the inkjet ink composition, whether or not the resin particles are contained. For the same reason, it is more preferable that the inkjet ink composition does not contain resin particles.

[0102] When ink contains resin particles, the surfactant (dispersant) used to disperse the resin makes the ink prone to foaming and air bubbles are likely to form. Air bubbles are particularly likely to form when ink is injected into an ink container through an ink inlet. Furthermore, the resin particles themselves are likely to become foreign matter at the air-liquid interface inside the ink container.

[0103] In addition, when air bubbles are generated, the number of gas-liquid interfaces increases, and foreign matter is more likely to be generated at the gas-liquid interface. In addition, since resin particles are not soluble in water, there is concern about environmental problems caused by microplastics when the ink is released into the natural environment. Examples of resin dispersions include dispersion resins dispersed with a surfactant and soapless dispersion resins dispersed without using a surfactant.

[0104] Surfactants The inkjet ink composition according to this embodiment may contain a surfactant. The surfactant can be used to reduce the surface tension of the inkjet ink composition and adjust and improve the wettability with a recording medium, for example, the permeability into fabrics and the like. As the surfactant, any of nonionic surfactants, anionic surfactants, cationic surfactants, and amphoteric surfactants can be used, and these may be used in combination. Among the surfactants, acetylene glycol surfactants, silicone surfactants, and fluorine-based surfactants can be more preferably used.

[0105] The acetylene glycol surfactant is not particularly limited, but examples thereof include Surfynol 104, 104E, 104H, 104A, 104BC, 104DPM, 104PA, 104PG-50, 104S, 420, 440, 465, 485, SE, SE-F, 504, 61, DF37, CT111, CT121, CT131, CT136, TG, GA, DF110D (product name, manufactured by Air Products and Chemicals Inc.), Olfine B, Y, P, A, STG, SPC, E1004, E1010, PD-001, PD-002W, PD-003, PD-004, PD-005, and EXP. 4001, EXP.4036, EXP.4051, EXP.4123, EXP.4200, EXP.4300, D-10PG, AF-103, AF-104, AK-02, SK-14, AE-3 (trade names, manufactured by Nissin Chemical Industry Co., Ltd.), Acetylenol E00, E00P, E40, E100 (trade names, manufactured by Kawaken Fine Chemical Co., Ltd.).

[0106] The silicone surfactant is not particularly limited, but a polysiloxane compound is preferred. The polysiloxane compound is not particularly limited, but for example, a polyether-modified organosiloxane is exemplified. Examples of commercially available polyether-modified organosiloxanes include BYK-306, BYK-307, BYK-333, BYK-341, BYK-345, BYK-346, BYK-348 (trade names, manufactured by BYK Co.), KF-351A, KF-352A, KF-353, KF-354L, KF-355A, KF-615A, KF-945, KF-640, KF-642, KF-643, KF-6020, X-22-4515, KF-6011, KF-6012, KF-6015, and KF-6017 (trade names, manufactured by Shin-Etsu Chemical Co., Ltd.).

[0107] As the fluorosurfactant, it is preferable to use a fluorine-modified polymer, and an example thereof is BYK-340 (trade name, manufactured by BYK-Chemie Japan KK).

[0108] When a surfactant is added to the inkjet ink composition, the total amount of the surfactant is preferably 0.01% by mass or more and 3% by mass or less, more preferably 0.05% by mass or more and 2% by mass or less, even more preferably 0.1% by mass or more and 1.5% by mass or less, and particularly preferably 0.2% by mass or more and 1% by mass or less, based on the entire inkjet ink composition.

[0109] When a surfactant is added to the inkjet ink composition, it is more preferable to select a surfactant having defoaming properties. By including a surfactant in the inkjet ink composition, the stability of the ink when ejected from the head tends to increase.

[0110] 1.5.4 Chelating Agents The ink-jet ink composition of the present embodiment may use a chelating agent, which is capable of removing certain ions in the ink-jet ink composition.

[0111] Examples of the chelating agent include ethylenediaminetetraacetic acid and its salts such as EDTA, EDTA-2Na (ethylenediaminetetraacetic acid dihydrogen disodium salt), EDTA-3Na (ethylenediaminetetraacetic acid monohydrogen trisodium salt), EDTA-4Na (ethylenediaminetetraacetic acid tetrasodium salt), and EDTA-3K (ethylenediaminetetraacetic acid monohydrogen tripotassium salt); diethylenetriaminepentaacetic acid such as DTPA, DTPA-2Na (diethylenetriaminepentaacetic acid disodium salt), and DTPA-5Na (diethylenetriaminepentaacetic acid pentasodium salt); Examples of such acids include acetic acid and its salts, nitrilotriacetic acid and its salts such as NTA, NTA-2Na (nitrilotriacetic acid disodium salt), and NTA-3Na (nitrilotriacetic acid trisodium salt), ethylenediamine-N,N'-disuccinic acid and its salts, 3-hydroxy-2,2'-iminodisuccinic acid and its salts, L-aspartic acid-N,N'-diacetic acid and its salts, L-glutamic acid diacetic acid and its salts, N-(1-carboxylatomethyl)iminodiacetic acid and its salts, and N-(2-hydroxyethyl)iminodiacetic acid and its salts.

[0112] Examples of chelating agents other than acetate analogs include ethylenediaminetetramethylenephosphonic acid and its salts, ethylenediaminetetrametaphosphoric acid and its salts, ethylenediaminepyrophosphoric acid and its salts, and ethylenediaminemetaphosphoric acid and its salts.

[0113] When a chelating agent is contained in the inkjet ink composition of this embodiment, one or more types selected from the above examples can be used.

[0114] 1.5.5. pH Adjusters A pH adjuster may be added to the inkjet ink composition of this embodiment. The pH adjuster is not particularly limited, and may be an appropriate combination of an acid, a base, a weak acid, or a weak base. Examples of acids and bases used in such combinations include inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid, inorganic bases such as lithium hydroxide, sodium hydroxide, potassium hydroxide, potassium dihydrogen phosphate, disodium hydrogen phosphate, potassium carbonate, sodium carbonate, sodium bicarbonate, and ammonia, organic bases such as triethanolamine, tripropanolamine, diethanolamine, monoethanolamine, triisopropanolamine, diisopropanolamine, and trishydroxymethylaminomethane (THAM), and organic acids such as adipic acid, citric acid, succinic acid, lactic acid, and N,N-bis(2-hydroxyethyl)-2-amine. Good's buffers such as benzyl ether (BES), 4-(2-hydroxyethyl)-1-piperazineethanesulfonic acid (HEPES), morpholinoethanesulfonic acid (MES), morpholinopropanesulfonic acid (MOPS), carbamoylmethyliminobisacetic acid (ADA), piperazine-1,4-bis(2-ethanesulfonic acid) (PIPES), N-(2-acetamido)-2-aminoethanesulfonic acid (ACES), cholamine hydrochloride, N-tris(hydroxymethyl)methyl-2-aminoethanesulfonic acid (TES), acetamidoglycine, tricine, glycineamide, and bicine, phosphate buffer, citrate buffer, Tris buffer, and the like may also be used. Furthermore, among these, it is preferable that the pH adjuster contains, as part or all of a tertiary amine such as triethanolamine or triisopropanolamine, or a carboxyl group-containing organic acid such as adipic acid, citric acid, succinic acid, or lactic acid, since this makes it possible to obtain a more stable pH buffering effect.

[0115] 1.5.6.Ureas Ureas may be used as a moisturizer for the inkjet ink composition or as a dyeing assistant for improving the dyeing property of the dye. Specific examples of ureas include urea, ethylene urea, tetramethyl urea, thiourea, 1,3-dimethyl-2-imidazolidinone, etc. When ureas are contained, the content thereof may be 1% by mass or more and 10% by mass or less with respect to the total mass of the inkjet ink composition.

[0116] 1.5.7. Antiseptics, mildew inhibitors, and rust inhibitors The inkjet ink composition may contain a preservative or an antifungal agent. Examples of the preservative or antifungal agent include sodium benzoate, sodium pentachlorophenol, sodium 2-pyridinethiol-1-oxide, sodium sorbate, sodium dehydroacetate, 1,2-dibenzisothiazolin-3-one (Proxel CRL, Proxel BDN, Proxel GXL, Proxel XL-2, Proxel TN, Proxel LV, both from Zeneca), and 4-chloro-3-methylphenol (Preventol CMK, etc., from Bayer). Examples of the rust inhibitor include benzotriazole.

[0117] Sugars The inkjet ink composition may contain sugars. Specific examples of sugars include glucose, mannose, fructose, ribose, xylose, arabinose, galactose, aldonic acid, glucitol (sorbitol), maltose, cellobiose, lactose, sucrose, trehalose, and maltotriose.

[0118] Other In addition to the above, other components include, for example, antioxidants, ultraviolet absorbers, oxygen absorbers, dissolving agents, etc. The ink-jet ink composition may contain additives such as auxiliaries that can be normally used in ink-jet ink compositions.

[0119] 1.6. Manufacturing and Properties The inkjet ink composition of the present embodiment can be obtained by mixing the above-mentioned components in any order, and removing impurities by filtering or the like as necessary. As a mixing method, a method in which materials are added sequentially to a container equipped with a stirring device such as a mechanical stirrer or a magnetic stirrer and stirred and mixed is preferably used. As a filtering method, for example, centrifugal filtering or filter filtering can be performed as necessary.

[0120] From the viewpoint of reliability as an inkjet ink, the inkjet ink composition of this embodiment preferably has a surface tension at 20° C. of 20 mN / m or more and 40 mN / m or less, and more preferably 22 mN / m or more and 35 mN / m or less. From the same viewpoint, the viscosity of the ink at 20° C. is preferably 1.5 mPa·s or more and 10 mPa·s or less, and more preferably 2 mPa·s or more and 8 mPa·s or less. One method for adjusting the surface tension and viscosity to be within the above ranges is to adjust the types of the water-soluble resin, organic solvent, and surfactant, and the amounts of these and water added, etc.

[0121] 1.7. Effects, etc. According to the inkjet ink composition of this embodiment, the self-dispersing pigment has a phosphorus-containing group on the pigment surface, so that the color development of the obtained image is excellent. Furthermore, by including a water-soluble resin, the image is quickly fixed and the pigment is likely to remain on the surface of the recording medium, so that the color development is excellent. Furthermore, even with a self-dispersing pigment that tends to have insufficient fixability, the water-soluble resin can provide sufficient fixability of the image. Furthermore, by including betaine, drying and solidification of the water-soluble resin in the nozzle and ink supply path is suppressed, so that clogging is less likely to occur.

[0122] 2. Recording method The recording method of the present embodiment is carried out using an inkjet recording apparatus having an inkjet head, and includes a step of ejecting an inkjet ink composition from the inkjet head and depositing the inkjet ink composition onto a recording medium. The inkjet ink composition is the inkjet ink composition described above.

[0123] An example of an inkjet recording device that can be used in the recording method of this embodiment will be described with reference to the drawings. Fig. 1 is a schematic perspective view showing an inkjet recording device. As shown in Fig. 1, the inkjet recording device 1 includes a recording head 2, a carriage 9, a platen 11, a carriage moving mechanism 13, a transport means 14, and a control unit CONT. The control unit CONT shown in Fig. 1 controls the operation of the entire inkjet recording device 1.

[0124] The recording head 2 is configured to perform recording on the recording medium M by ejecting and depositing ink from the nozzles of the recording head 2. The recording head 2 shown in FIG. 1 is a serial type recording head that scans multiple times in the main scanning direction relative to the recording medium M to deposit ink on the recording medium M. The recording head 2 is mounted on a carriage 9 shown in FIG. 1. The recording head 2 is scanned multiple times in the main scanning direction relative to the recording medium M by the operation of a carriage movement mechanism 13 that moves the carriage 9 in the medium width direction of the recording medium M. The medium width direction is the main scanning direction of the recording head 2. Scanning in the main scanning direction is also called main scanning.

[0125] Here, the main scanning direction is the direction in which the carriage 9 carrying the recording head 2 moves. In Fig. 1, the width direction of the recording medium M, that is, the direction represented by S1-S2, is the main scanning direction MS, and the direction represented by T1→T2 is the sub-scanning direction SS. Note that scanning is performed in one main scanning direction, that is, in the direction of either the arrow S1 or the arrow S2, in one scan. Then, recording is performed on the recording medium M by repeating the main scanning of the recording head 2 and the sub-scanning, which is the transport of the recording medium M, multiple times.

[0126] The cartridge 12 that supplies ink to the recording head 2 includes a plurality of independent cartridges. The cartridge 12 is detachably mounted on a carriage 9 on which the recording head 2 is mounted. Each of the plurality of cartridges can be filled with a different type of ink, and ink is supplied from the cartridge 12 to each nozzle. Note that, although an example in which the cartridge 12 is mounted on the carriage 9 is shown in Figs. 1 and 2, the cartridge 12 is not limited to this, and may be provided at a location other than the carriage 9, and ink may be supplied to each nozzle by a supply pipe (not shown).

[0127] A conventionally known method can be used for ejecting ink from the recording head 2. In this embodiment, a method for ejecting ink droplets using the vibration of a piezoelectric element, that is, an ejection method for forming ink droplets by mechanical deformation of an electrostrictive element, is used.

[0128] Below the carriage 9, there are provided a platen 11 that supports the recording medium M, a carriage movement mechanism 13 that moves the carriage 9 relatively to the recording medium M, and a transport means 14 that is a roller that transports the recording medium M in the sub-scanning direction. The operations of the carriage movement mechanism 13 and the transport means 14 are controlled by a control unit CONT.

[0129] <Electrical control> FIG. 2 is a functional block diagram of the inkjet recording apparatus 1. The control unit CONT is a control unit for controlling the inkjet recording apparatus 1. The interface unit 101 (I / F) is for transmitting and receiving data between the computer 130 (COMP) and the inkjet recording apparatus 1. The CPU 102 is an arithmetic processing device for controlling the entire inkjet recording apparatus 1. The memory 103 (MEM) is for securing an area for storing programs for the CPU 102, a working area, and the like. The CPU 102 controls each unit by a unit control circuit 104 (UCTRL). The situation inside the inkjet recording apparatus 1 is monitored by a detector group 121 (DS), and the control unit CONT controls each unit based on the detection results.

[0130] The transport unit 111 (CONVU) controls the sub-scanning (transport) of inkjet recording, specifically, controls the transport direction and transport speed of the recording medium M. More specifically, it controls the transport direction and transport speed of the recording medium M by controlling the rotation direction and rotation speed of a transport roller driven by a motor.

[0131] The carriage unit 112 (CARU) controls the main scan (pass) of inkjet recording, and specifically, moves the recording head 2 back and forth in the main scanning direction. The carriage unit 112 includes a carriage 9 on which the recording head 2 is mounted, and a carriage movement mechanism 13 for moving the carriage 9 back and forth.

[0132] The head unit 113 (HU) controls the amount of ink ejected from the nozzles of the recording head 2. For example, if the nozzles of the recording head 2 are driven by piezoelectric elements, the head unit 113 controls the operation of the piezoelectric elements in each nozzle. The head unit 113 controls the timing of deposition of each ink droplet, the size of the ink dots, etc. Also, the amount of ink deposited per scan is controlled by a combination of the controls of the carriage unit 112 and the head unit 113.

[0133] The inkjet recording device 1 alternately repeats an operation of moving the carriage 9 carrying the recording head 2 in the main scanning direction and a transport operation (sub-scanning). At this time, when performing each pass, the control unit CONT controls the carriage unit 112 to move the recording head 2 in the main scanning direction, and controls the head unit 113 to eject ink droplets from predetermined nozzle holes of the recording head 2 and deposit the ink droplets on the recording medium M. In addition, the control unit CONT controls the transport unit 111 to transport the recording medium M in the transport direction by a predetermined transport amount (feed amount) during the transport operation.

[0134] In the inkjet recording device 1, the recording area to which multiple droplets have been attached is gradually transported by repeating main scanning (passes) and sub-scanning (transport operation). The droplets attached to the recording medium M are dried to complete the image. The completed recorded matter may then be wound into a roll by a winding mechanism or transported by a flatbed mechanism. Alternatively, the recording medium may be discharged to a paper output tray. When printing continuously, the recording media may be discharged to a paper output tray and stacked.

[0135] The step of depositing the inkjet ink composition on a recording medium can be carried out using the inkjet recording apparatus described above. That is, the inkjet ink composition is filled into an inkjet head so that it can be ejected from a predetermined nozzle, and then ejected in that state onto a recording medium at a predetermined timing, thereby carrying out the step of depositing the inkjet ink composition on a recording medium.

[0136] The recording method of the present embodiment may also include a step of heating the recording medium as appropriate. The step of heating the recording medium can be performed, for example, by using the drying means described above when an inkjet recording device is used. The step can also be performed by any suitable drying means, not limited to an inkjet recording device. This dries the resulting image, making it possible to suppress bleeding of the image and fix it more efficiently.

[0137] The recording method of the present embodiment may further include other steps as appropriate, for example, a step of applying another composition, a washing step, etc. According to the recording method of the present embodiment, since the above-mentioned inkjet ink composition is used, an image having good color development and abrasion resistance of the inkjet ink composition can be formed.

[0138] The printing method of this embodiment may be a printing method performed by a serial type printing apparatus as in the above example, or may be a printing method performed by a line type printing apparatus.

[0139] The recording medium is not particularly limited, and may be one having a recording surface that absorbs liquid, or one that does not have a recording surface that absorbs liquid. Therefore, the recording medium is not particularly limited, and for example, paper, film, cloth, metal, glass, polymer, etc. can be used. In addition, transfer paper for performing sublimation transfer onto the recording medium can also be a recording medium. In addition, the size and length of the recording medium are not limited.

[0140] It is more preferable that the recording medium on which the recording is performed by the recording method of this embodiment is a liquid-absorbent recording medium. 1 / 2 Water absorption up to 10mL / m 2 The Bristow method is the most widely used method for measuring the amount of liquid absorbed in a short period of time, and is also used by the Japan Pulp and Paper Technical Association (JAPAN TAPPI). Details of the test method are described in Standard No. 51 "Paper and paperboard - Liquid absorbency test method - Bristow method" of the "JAPAN TAPPI Paper and Pulp Test Method 2000 Edition."

[0141] The liquid-absorbent recording medium may be one in which a liquid-absorbing receiving layer is provided on the surface of the recording medium, making it a liquid-absorbent recording medium. For example, inkjet paper (paper exclusively for inkjet printing) may be mentioned. The liquid-absorbent receiving layer may be a layer made of a liquid-absorbent resin, liquid-absorbent inorganic fine particles, etc.

[0142] The liquid-absorbent recording medium may be a recording medium in which the substrate itself is liquid-absorbent. For example, it may be a fabric made of fiber, or a paper made of pulp. The paper may be plain paper, cardboard, or liner paper. The liner paper may be made of kraft pulp, recycled paper, or other paper.

[0143] Using the inkjet recording apparatus described above, the inkjet ink composition of this embodiment can be ejected from an inkjet head and adhered to a recording medium. This allows an image with excellent color development to be formed. In addition, the image has excellent fixability and is also excellent in terms of nozzle clogging recovery. Furthermore, the water-soluble resin is prevented from drying and solidifying in the nozzle and ink supply path. In addition, since the image is quickly fixed by the water-soluble resin, when recording is performed on a liquid-absorbent recording medium, sinking of the ink components is prevented, and an image with better color development can be obtained.

[0144] In addition, in the recording method of the present embodiment, the inkjet ink composition described above is used, so that the image is quickly fixed by the water-soluble resin, and abrasion resistance is obtained early. Therefore, it is possible to perform recording at a higher speed. For example, if the recording medium is A4 size paper, even if the recording speed is set to 30 sheets / min or more, preferably 20 sheets / min or more, and more preferably 10 sheets / min or more, transfer between stacked recording media can be suppressed. In addition, in the case of double-sided printing, the ink is less likely to adhere to rollers or the like in the transport path of the recording medium after the inkjet ink composition is adhered thereto.

[0145] Such an effect can be obtained even when the recording medium is roll paper. For example, even when a line printer is used and the recording medium is rolled up after recording, offset of the ink-jet ink composition can be suppressed.

[0146] According to this recording method, the self-dispersing pigment has a phosphorus-containing group on the pigment surface, so that the color development of the obtained image is excellent. In addition, by including a water-soluble resin, the fixation of the image is excellent and the nozzle clogging recovery is also excellent. Furthermore, even if the self-dispersing pigment tends to have insufficient fixation, the water-soluble resin can provide sufficient fixation of the image. Furthermore, by including betaine, the drying and solidification of the water-soluble resin in the nozzle and the ink supply path is suppressed. This effect is achieved by the interaction of the specific combination of the self-dispersing pigment having a phosphorus-containing group, the water-soluble resin, and the betaine.

[0147] 3. Examples and Comparative Examples The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following, "parts" and "%" are based on mass unless otherwise specified. The evaluation was performed under an environment of a temperature of 25.0°C and a relative humidity of 40.0%, unless otherwise specified.

[0148] 4.1. Preparation of Inkjet Ink Composition The components were placed in a container so as to obtain the compositions shown in Tables 1 to 3, and mixed and stirred for 2 hours using a magnetic stirrer. The mixture was then filtered through a membrane filter having a pore size of 5 μm to obtain inkjet ink compositions according to the examples and comparative examples.

[0149] The substances in Tables 1 to 3 are as follows.

[0150] Phosphorus-containing base treated self-dispersing pigment: Produced as follows: 20.0 g of the pigment, 11.0 mmol of ((4-aminobenzoylamino)-methane-1,1-diyl)bisphosphonic acid monosodium salt, 20.0 mmol of nitric acid, and 200 mL of pure water were mixed. Carbon black (product name "Black Pearls 880", manufactured by Cabot) was used as the pigment. The mixture was mixed at room temperature at 6,000 rpm using a Silverson mixer. After 30 minutes, 20.0 mmol of sodium nitrite dissolved in a small amount of water was slowly added to the mixture. The temperature of the mixture reached 60°C by adding sodium nitrite. The mixture was allowed to react in this state for 1 hour. After that, the mixture was washed with water and then the pH of the mixture was adjusted to 10 using an aqueous solution of sodium hydroxide. The obtained pigment was a self-dispersing pigment having -C6H4-CONH-CH-(PO(OH)(ONa))(PO(OH)2) groups bonded to the surface of the pigment particles.

[0151] Non-phosphorus-containing base-treated self-dispersing pigment: CAB-O-JET (registered trademark) 300 (manufactured by Cabot Specialty Chemicals, Inc.)

[0152] Dispersion resin (resin particles): Resin particles produced as follows. In a reaction vessel equipped with a stirrer, reflux condenser, dropping device, and thermometer, 900g of ion-exchanged water and 1g of sodium lauryl sulfate were charged, and the temperature was raised to 70°C while stirring and replacing with nitrogen. The internal temperature was kept at 70°C, and 4g of potassium persulfate was added as a polymerization initiator. After dissolution, an emulsion was prepared by adding 20g of acrylamide, 365g of styrene, 545g of butyl acrylate, and 30g of methacrylic acid to 450g of ion-exchanged water and 3g of sodium lauryl sulfate under stirring, and then continuously dropped into the reaction solution over a period of 4 hours. After the dropping was completed, the mixture was aged for 3 hours. The obtained resin emulsion was cooled to room temperature, and then ion-exchanged water and hydroxide were added to the reaction solution. An aqueous sodium chloride solution was added to adjust the solid content to 40 mass % and the pH to 8. The glass transition temperature of the resin particles in the obtained aqueous emulsion was -6°C.

[0153] Water-soluble polymer 1: Prepared as follows: 93.4 parts of butanol was placed in a reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer, and replaced with nitrogen gas. After heating to 110°C, a mixture of 101.1 parts of styrene, 38.5 parts of acrylic acid, 60.0 parts of maleic acid, and 6 parts of a polymerization initiator (product name "V-601", Fujifilm Wako Pure Chemical Industries, Ltd.) was dropped over 2 hours to carry out a polymerization reaction. After reacting at 110°C for 3 hours, 0.6 parts of a polymerization initiator was further added, and the reaction was continued at 110°C for 1 hour to obtain a resin solution. After cooling to room temperature, 37.1 parts of dimethylaminoethanol were added to neutralize, and 100 parts of water were further added. Butanol was distilled off by heating to 100°C or higher to perform azeotropy with water, and the concentration was adjusted. As a result, a liquid containing water-soluble resin 1 with a resin content of 20.0% was obtained. The acid value of the water-soluble resin 1 was 440 mgKOH / g as determined by titration, the proportion of water-soluble monomer was 49 mass %, and the weight average molecular weight was 12,000.

[0154] Water-soluble polymer 2: prepared as follows: 93.4 parts of butanol was placed in a reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer, and replaced with nitrogen gas. After heating to 110°C, a mixture of 101.5 parts of styrene, 98.5 parts of acrylic acid, and 6 parts of a polymerization initiator (product name "V-601", Fujifilm Wako Pure Chemical Industries, Ltd.) was added dropwise over 2 hours to carry out a polymerization reaction. After reacting at 110°C for 3 hours, 0.6 parts of a polymerization initiator was further added, and the reaction was continued at 110°C for 1 hour to obtain a resin solution. After cooling to room temperature, 37.1 parts of dimethylaminoethanol were added to neutralize, and 100 parts of water were further added. Butanol was distilled off by heating to 100°C or higher to perform azeotropy with water, and the concentration was adjusted. As a result, a liquid containing water-soluble resin 2 with a content of water-soluble resin 2 of 20.0% was obtained. The acid value of the water-soluble resin 2 was 383 mgKOH / g as determined by titration, the water-soluble monomer ratio was 49 mass %, and the weight average molecular weight was 12,000.

[0155] Water-soluble polymer 3 (water-soluble monomer content: 60% or more): Produced as follows: 93.4 parts of butanol was placed in a reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer, and replaced with nitrogen gas. After heating to 110°C, a mixture of 101.5 parts of styrene, 38.5 parts of acrylic acid, 210.0 parts of maleic acid, and 6 parts of a polymerization initiator (product name "V-601", Fujifilm Wako Pure Chemical Industries, Ltd.) was dropped over 2 hours to carry out a polymerization reaction. After reacting at 110°C for 3 hours, 0.6 parts of a polymerization initiator was further added, and the reaction was continued at 110°C for 1 hour to obtain a resin solution. After cooling to room temperature, 37.1 parts of dimethylaminoethanol were added to neutralize, and 100 parts of water were further added. Butanol was distilled off by heating to 100°C or higher to perform azeotropy with water, and the concentration was adjusted. As a result, a liquid containing water-soluble resin 3 with a content of water-soluble resin 3 of 20.0% was obtained. The acid value of the water-soluble resin 3 was 664 mgKOH / g as determined by titration, the water-soluble monomer ratio was 71 mass %, and the weight average molecular weight was 12,000.

[0156] Water-soluble polymer 4 (less than 60% water-soluble monomer): prepared as follows. 93.4 parts of butanol was placed in a reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer, and replaced with nitrogen gas. After heating to 110°C, a mixture of 150.0 parts of styrene, 25.0 parts of acrylic acid, 30.0 parts of maleic acid, and 6 parts of a polymerization initiator (product name "V-601", Fujifilm Wako Pure Chemical Industries, Ltd.) was dropped over 2 hours to carry out a polymerization reaction. After reacting at 110°C for 3 hours, 0.6 parts of a polymerization initiator was further added, and the reaction was continued at 110°C for 1 hour to obtain a resin solution. After cooling to room temperature, 37.1 parts of dimethylaminoethanol were added to neutralize, and 100 parts of water were further added. Butanol was distilled off by heating to 100°C or higher to perform azeotropy with water, and the concentration was adjusted. As a result, a liquid containing water-soluble resin 4 with a content of water-soluble resin 4 of 20.0% was obtained. The acid value of the water-soluble resin 4 measured by titration was 236 mgKOH / g, the water-soluble monomer ratio was 27% by mass, and the weight average molecular weight was 12,000.

[0157] Olfin E1010: Nissin Chemical Industry Co., Ltd., acetylene glycol surfactant Olfin EXP4300: Acetylene glycol surfactant manufactured by Nissin Chemical Industry Co., Ltd. Olfin D-10PG: Manufactured by Nissin Chemical Industry Co., Ltd., an acetylene glycol surfactant

[0158] Evaluation method 4.2.1. Recording test A modified PX-S840 (cartridge type) manufactured by Seiko Epson Corporation was prepared. The recording medium used for the recording test was XeroxP (manufactured by Fuji Xerox Co., Ltd.). The amount of ink attached to the recording medium was 4 mg / inch. 2 As a result, monochrome 100% duty pattern 101 was recorded.

[0159] 4.2.2. LM property immediately after printing (Line marker test immediately after recording) The image immediately after printing was rubbed once or twice with a line marker, and the results were visually observed and evaluated according to the following criteria. The evaluation results are shown in Tables 4 to 6. Since it was immediately after printing, a grade of B or higher is desirable, and a grade of A or higher is more desirable. A: Even after rubbing twice, the marks are not noticeable. B: After rubbing once, the rubbing is not noticeable. C: Scratches are noticeable after rubbing once

[0160] 4.2.3. LM property 5 minutes after printing (Line marker test 5 minutes after recording) After printing, the image was left for 5 minutes, then rubbed once or twice with a line marker, and the results were visually evaluated according to the following criteria. The evaluation results are shown in Tables 4 to 6. Since the image was left for 5 minutes after printing, it is desirable for it to be rated as A or higher. A: Even after rubbing twice, the marks are not noticeable. B: After rubbing once, the rubbing is not noticeable. C: Scratches are noticeable after rubbing once

[0161] 4.2.4.Clogging The cartridge of the recording device was filled with each ink of each example, and after the recording test, the cartridge was left uncapped in a 40°C, 20% RH environment for 7 days, and then the head was cleaned. The clogging recovery was evaluated according to the number of cleanings according to the following criteria, and the results are shown in Tables 4 to 6. A: Recovers within 6 times B: Recovers after 7 or 8 times C: No recovery after 8 times

[0162] 4.2.5.Optical Density (OD value) A monochrome 100% duty pattern 101 was measured with a colorimeter. The obtained OD value was evaluated according to the following criteria. The evaluation results are shown in Tables 4 to 6. A grade of B or higher is desirable. A:OD value 1.1 or more B: OD value 0.9 or more and less than 1.1 C:OD value less than 0.9

[0163] 4.2.6. Transferability evaluation Using the above recording device, recording was performed on plain XP paper, A4 size, at the recording speeds shown in Tables 4 to 6. Single-sided printing. The printing pattern was a 10 cm x 10 cm solid pattern (ink deposition amount 7 mg / inch 2 100 sheets were stacked on the paper output tray. After printing, the sheets were evaluated according to the following criteria. A: No ink transfer to the back side B: Some ink transfer is visible on the back C: There is a lot of transfer on the back side.

[0164] 4.2.7. Microplastics assessment It was determined whether or not the ink contained a water-insoluble resin. The results are shown in Tables 1 to 3. A is preferable. A: The ink does not contain water-insoluble resin. B: Ink contains water-insoluble resin

[0165] 4.3.Evaluation Results Looking at Tables 4 to 6, it was found that the inkjet ink compositions of each example, which contain a self-dispersing pigment having a phosphorus-containing group introduced into the pigment, a water-soluble resin, and betaine, wherein the acid value of the water-soluble resin is 250 mgKOH / g or more and 600 mgKOH / g or less, the content of the self-dispersing pigment is 3.5 mass% or more and 8.5 mass% or less relative to the total mass of the ink composition, the mass ratio of the self-dispersing pigment to the water-soluble resin (self-dispersing pigment / water-soluble resin) is 2.8 or more and less than 30, and the content of betaine is 2.5 mass% or more and 9.5 mass% or less relative to the total mass of the ink composition, have good clogging resistance, abrasion resistance, and color development.

[0166] The present invention includes configurations that are substantially the same as the configurations described in the embodiments, for example, configurations with the same functions, methods, and results, or configurations with the same purpose and effects. The present invention also includes configurations in which non-essential parts of the configurations described in the embodiments are replaced. The present invention also includes configurations that achieve the same effects as the configurations described in the embodiments, or configurations that can achieve the same purpose. The present invention also includes configurations in which publicly known technology is added to the configurations described in the embodiments.

[0167] The following can be derived from the above-described embodiment and modified examples.

[0168] The ink-jet ink composition is water-based, Contains a self-dispersing pigment, a water-soluble resin, and a betaine, the self-dispersion pigment is a self-dispersion pigment having a phosphorus-containing group introduced therein; The water-soluble resin has an acid value of 250 mgKOH / g or more and 600 mgKOH / g or less, the content of the self-dispersion pigment is 3.5% by mass or more and 8.5% by mass or less relative to the total mass of the ink composition; a mass ratio of the self-dispersion pigment to the water-soluble resin (self-dispersion pigment / water-soluble resin) is 2.8 or more and less than 30; The content of the betaine is 2.5% by mass or more and 9.5% by mass or less with respect to the total mass of the ink composition.

[0169] According to this inkjet ink composition, the self-dispersing pigment has a phosphorus-containing group on the pigment surface, so that the color development of the obtained image is excellent. In addition, by including a water-soluble resin, the image is quickly fixed and the pigment is likely to remain on the surface of the recording medium, so that the color development is excellent. Furthermore, even with a self-dispersing pigment that tends to have insufficient fixing ability, the water-soluble resin can provide sufficient fixing ability of the image. Furthermore, by including betaine, drying and solidification of the water-soluble resin in the nozzle and the ink supply path is suppressed, so that clogging is less likely to occur.

[0170] In the inkjet ink composition, The phosphorus-containing group may be a phosphonic acid group.

[0171] This ink-jet ink composition also provides good fixation of images.

[0172] In the inkjet ink composition, The content of the water-soluble resin may be 0.3% by mass or more and 2% by mass or less with respect to the total mass of the ink composition.

[0173] This ink-jet ink composition has more appropriate image fixation and better viscosity.

[0174] In the inkjet ink composition, The content of the resin particles may be less than 0.1% by mass relative to the total mass of the ink composition.

[0175] This ink-jet ink composition further suppresses the generation of foreign matter.

[0176] In the inkjet ink composition, The water-soluble resin may be selected from an acrylic resin or a maleic acid resin.

[0177] This ink-jet ink composition can provide images with even better quality.

[0178] In the inkjet ink composition, The composition ratio of the water-soluble monomer in the water-soluble resin may be 30% by mass or more and 60% by mass or less, when the total amount of all monomers in the water-soluble resin is taken as 100% by mass.

[0179] The ink-jet ink composition provides further reduction in clogging and more satisfactory water solubility.

[0180] In the inkjet ink composition, The betaine may be selected from trialkylglycines.

[0181] This ink-jet ink composition can make it possible to further reduce the occurrence of aggregation of the water-soluble resin.

[0182] In the inkjet ink composition, It may be used for recording on an absorbent recording medium.

[0183] This ink-jet ink composition makes it possible to form images with better color development even on an absorbent recording medium.

[0184] In the inkjet ink composition, Polyols having a normal boiling point of more than 280°C may be contained.

[0185] This ink-jet ink composition further facilitates suppression of clogging.

[0186] The recording method is carried out using an inkjet recording apparatus having an inkjet head, ejecting an ink-jet ink composition from the ink-jet head and depositing the ink-jet ink composition on a recording medium; The ink-jet ink composition is the ink-jet ink composition described above.

[0187] According to this recording method, the self-dispersing pigment has a phosphorus-containing group on the pigment surface, so that the color development of the obtained image is excellent. In addition, by including a water-soluble resin, the image is excellent in fixation and is fixed quickly, so that the color development and high-speed recording are also excellent. Furthermore, even if the self-dispersing pigment tends to have insufficient fixation, the water-soluble resin can provide sufficient fixation of the image. Furthermore, by including betaine, the water-soluble resin is prevented from drying and solidifying in the nozzle and the ink supply path. This effect is achieved by the interaction of the specific combination of the self-dispersing pigment having a phosphorus-containing group, the water-soluble resin, and the betaine.

[0188] In the inkjet ink composition, The printing speed may be 20 sheets / minute or more.

[0189] According to this recording method, the image is fixed quickly, so high speed recording is possible. [Explanation of symbols]

[0190] 1...inkjet recording device, 2...recording head, 9...carriage, 11...platen, 12...cartridge, 13...carriage moving mechanism, 14...transport means, 101...interface section, 102...CPU, 103...memory, 104...unit control circuit, 111...transport unit, 112...carriage unit, 113...head unit, 114...drying unit, 121...detector group, 130...computer, CONT...control section, MS...main scanning direction, SS...sub-scanning direction, M...recording medium

Claims

1. Contains a self-dispersing pigment, a water-soluble resin, and a betaine, the self-dispersion pigment is a self-dispersion pigment having a phosphorus-containing group introduced therein; The water-soluble resin has an acid value of 250 mgKOH / g or more and 600 mgKOH / g or less, the content of the self-dispersion pigment is 3.5% by mass or more and 8.5% by mass or less with respect to the total mass of the ink composition, a mass ratio of the self-dispersion pigment to the water-soluble resin (self-dispersion pigment / water-soluble resin) is 2.8 or more and less than 30; The content of the betaine is 2.5% by mass or more and 9.5% by mass or less based on the total mass of the ink composition.

2. In claim 1, The ink-jet ink composition, wherein the phosphorus-containing group is a phosphonic acid group.

3. In claim 1 or 2, The ink-jet ink composition has a content of the water-soluble resin of 0.3% by mass or more and 2% by mass or less relative to the total mass of the ink composition.

4. In claim 1 or 2, An ink-jet ink composition, comprising a resin particle content of less than 0.1% by mass based on the total mass of the ink composition.

5. In claim 1 or 2, The ink-jet ink composition, wherein the water-soluble resin is selected from an acrylic resin or a maleic acid resin.

6. In claim 1 or 2, an ink-jet ink composition, wherein a content of the water-soluble monomer in the water-soluble resin is 30% by mass or more and 60% by mass or less, when the total amount of the monomers in the water-soluble resin is taken as 100% by mass;

7. In claim 1 or 2, An ink-jet ink composition wherein the betaine is selected from trialkylglycines.

8. In claim 1 or 2, An ink-jet ink composition for use in recording on an absorbent recording medium.

9. In claim 1 or 2, An ink-jet ink composition comprising polyols having a normal boiling point of more than 280°C.

10. This is carried out using an inkjet recording device having an inkjet head, ejecting an ink-jet ink composition from the ink-jet head and depositing the ink-jet ink composition on a recording medium; The ink-jet ink composition is the ink-jet ink composition according to claim 1 or 2. Recording method.

11. In claim 10, A recording method in which the recording speed is 20 sheets / minute or more.

Citation Information

Patent Citations

  • Ink composition, set of ink composition and ink container, ink container, and recording device

    JP2015061896A