Method for peeling cured material layer from substrate, method for producing substrate having patterned cured material layer, and peeling liquid
A peeling method using an acid-containing cleaning solution and a stripping solution with sodium metasilicate and sodium phosphate effectively removes cured photosensitive compositions from substrates, addressing the issue of metal damage and enabling reuse of substrates with intact metal surfaces.
Patent Information
- Application Number
- JP2023046565
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing methods for peeling organic films made of cured photosensitive compositions containing (meth)acrylic compounds from substrates often cause damage to metal surfaces, particularly when metal substrates or substrates with metal films are involved.
A peeling method involving contact with an acid-containing cleaning solution followed by a stripping solution composed of an inorganic basic compound, a water-soluble alkanolamine, and a solvent, specifically using sodium metasilicate and sodium phosphate, to denature and facilitate the removal of the cured material layer while minimizing metal damage.
The method effectively peels off the cured material layer without significant metal damage, allowing for the reuse of substrates with intact metal surfaces and enabling the formation of patterned cured material layers on the substrates.
Smart Images

Figure 2024135730000001 
Figure 2024135730000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a peeling method for peeling off a cured material layer formed on a substrate from the substrate, a manufacturing method for a substrate for forming a patterned cured material layer on the substrate from which the cured material layer has been peeled off by the above-mentioned method, and a peeling solution. [Background technology]
[0002] When various substrates are processed to manufacture various elements, an organic film, typically a resist film, is often formed on the substrate. However, defects often occur in the organic film formed on the substrate. In this case, the organic film is peeled off from the substrate in order to reuse the substrate. Typically, the organic film is peeled off from the substrate by contacting the organic film with a stripping solution. As such a stripping solution, for example, a stripping solution used for stripping an organic film baked with a positive resist composition containing a novolac resin has been proposed (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2018 / 061064 Summary of the Invention [Problem to be solved by the invention]
[0004] However, when various elements are manufactured, an organic film made of a cured product of a photosensitive composition containing a (meth)acrylic compound is often formed on a substrate. For this reason, there is a demand for a stripping solution that can effectively strip the organic film made of a cured product of a photosensitive composition containing a (meth)acrylic compound from a substrate. Depending on the type of element to be manufactured, a metal substrate may be used, or a substrate having a metal film or metal wiring on its surface may be used. In this case, the metal may be damaged when the organic film is peeled off from the substrate using a peeling solution. In view of the above, there is a need for a method capable of peeling off an organic film made of a cured product of a photosensitive composition containing a (meth)acrylic compound from a substrate while suppressing damage to the metal.
[0005] The present invention has been made in view of the above-mentioned problems, and has an object to provide a method for peeling a cured film, which is capable of peeling a cured layer made of a cured product of a photosensitive composition containing a (meth)acrylic compound from a substrate while suppressing damage to metal; a method for producing a substrate comprising a cured layer patterned by an imprint method on a substrate from which a cured layer has been peeled by the above-mentioned method; and a stripping solution that can be preferably used in the above-mentioned method. [Means for solving the problem]
[0006] The present inventors have found that the above-mentioned problems can be solved by contacting a cured material layer formed on a substrate, the cured material layer being made of a cured material of a photosensitive composition containing a (meth)acrylic compound, with an acid-containing cleaning solution, and then contacting the cured material layer on the substrate with a stripping solution containing an inorganic base compound (A), a water-soluble alkanolamine (B), and a solvent (S), thereby peeling off the cured material layer formed on the substrate, and have thus completed the present invention.
[0007] A first aspect of the present invention is a method for peeling a cured material layer formed on a substrate from the substrate, comprising the steps of: The peeling method includes contacting the cured layer with an acid-containing cleaning solution; and peeling the cured layer, which has been in contact with the acid-containing cleaning solution, from the substrate by contacting the cured layer with a stripping solution; the cured material layer is made of a cured material of a photosensitive composition containing a (meth)acrylic compound, The stripping solution contains an inorganic basic compound (A), a water-soluble alkanolamine (B), and a solvent (S); The stripping method includes the inorganic basic compound (A) containing sodium metasilicate and sodium phosphate.
[0008] A second aspect of the present invention is a method for producing a substrate provided with a patterned cured material layer, comprising forming, by an imprint method, a patterned cured material layer made of a cured material of a photosensitive composition containing a (meth)acrylic compound on a substrate from which the cured material layer has been peeled off by the method according to the first aspect.
[0009] A third aspect of the present invention is a method for producing a water-soluble alkanolamine composition comprising: an inorganic basic compound (A); a water-soluble alkanolamine (B); and a solvent (S); The stripping solution contains the inorganic basic compound (A) as sodium metasilicate and sodium phosphate. Effect of the Invention
[0010] According to the present invention, it is possible to provide a method for peeling a cured film, which is capable of peeling a cured layer made of a cured product of a photosensitive composition containing a (meth)acrylic compound from a substrate while suppressing damage to metal; a peeling method for peeling a cured layer formed on a substrate by the above-mentioned peeling method using a stripping solution containing an inorganic base compound (A), a water-soluble alkanolamine (B) and a solvent (S) and an acid-containing cleaning solution; a method for producing a substrate having a cured layer patterned by an imprint method on the substrate from which the cured layer has been peeled; and the stripping solution. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] <Method for peeling off the cured layer from the substrate> Hereinafter, a peeling method for peeling the cured layer from the substrate (hereinafter also simply referred to as "peeling method") will be described.
[0012] The peeling method is a method for peeling off the cured material layer formed on the substrate from the substrate. The cured layer is made of a cured product of a photosensitive composition containing a (meth)acrylic compound. The above-mentioned peeling method includes contacting the cured layer with an acid-containing cleaning solution; and removing the cured layer, which has been in contact with the acid-containing cleaning solution, from the substrate by contacting the cured layer with a remover. The stripping solution contains an inorganic basic compound (A), a water-soluble alkanolamine (B), and a solvent (S). The inorganic basic compound (A) includes sodium metasilicate and sodium phosphate.
[0013] As described above, before the cured material layer is brought into contact with the stripping solution, the cured material layer is brought into contact with the acid-containing cleaning solution. The cured material layer is denatured by bringing the cured material layer into contact with the acid-containing cleaning solution. This improves the releasability of the cured material layer when the cured material layer is brought into contact with the stripping solution, and the cured material layer can be stripped in a short time.
[0014] <Removal solution> Hereinafter, a stripping solution that is suitably used in the method for stripping the cured material layer from the substrate, which will be described later, will be described.
[0015] The stripping solution contains an inorganic basic compound (A), a water-soluble alkanolamine (B), and a solvent (S). The inorganic basic compound (A) includes sodium metasilicate and sodium phosphate.
[0016] <Inorganic basic compound (A)> The inorganic basic compound (A) is not particularly limited as long as it is a compound that exhibits basicity according to the Bronsted definition in an aqueous solution at 20°C. Examples of the inorganic basic compound (A) include ammonia and basic inorganic compounds containing alkali metals or alkaline earth metals.Specific examples of basic inorganic compounds containing alkali metals or alkaline earth metals include hydroxides such as potassium hydroxide, sodium hydroxide, and calcium hydroxide; carbonates such as sodium carbonate and potassium carbonate; silicates such as sodium silicate and potassium silicate; metasilicates such as sodium metasilicate and potassium metasilicate; and phosphates such as sodium phosphate and potassium phosphate.Among these, sodium metasilicate and sodium phosphate are preferred.
[0017] As described above, the inorganic basic compound (A) contains sodium metasilicate and sodium phosphate. The inorganic basic compound (A) may contain, in addition to sodium metasilicate and sodium phosphate, one or more inorganic basic compounds other than sodium metasilicate and sodium phosphate. The content of the inorganic basic compound (A) in the stripping solution is not particularly limited as long as the desired effect is not impaired. The content of the inorganic basic compound (A) is preferably 0.5% by mass or more and 12% by mass or less, more preferably 2% by mass or more and 7% by mass or less, based on the mass of the stripping solution. The total content of sodium metasilicate and sodium phosphate is preferably from 1 mass % to 15 mass %, more preferably from 2.5 mass % to 12 mass %, based on the total mass of the inorganic basic compound (A). The ratio of the mass of sodium metasilicate to the total mass of sodium metasilicate and sodium phosphate is not particularly limited as long as the desired effect is not impaired. The ratio of the mass of sodium metasilicate to the total mass of sodium metasilicate and sodium phosphate is preferably 20% by mass or more and 90% by mass or more, more preferably 30% by mass or more and 80% by mass or less, and even more preferably 50% by mass or more and 70% by mass or less.
[0018] <Water-soluble alkanolamine (B)> As the water-soluble alkanolamine (B), any of tertiary alkanolamines, secondary alkanolamines, and primary alkanolamines can be used. These water-soluble alkanolamines (B) can be used alone or in combination of two or more kinds.
[0019] Examples of tertiary alkanolamines include trialkanolamines such as trimethanolamine, triethanolamine, tri-n-propanolamine, triisopropanolamine, and methanoldiethanolamine; and N-alkyldialkanolamines such as N-methyldimethanolamine, N-ethyldimethanolamine, N-methyldiethanolamine, N-ethyldiethanolamine, N-methyldi-n-propanolamine, N-ethyldi-n-propanolamine, N-methyldiisopropanolamine, and N-ethyldiisopropanolamine. Examples of secondary alkanolamines include dialkanolamines such as dimethanolamine, diethanolamine, di-n-propanolamine, and diisopropanolamine; and N-alkyl monoalkanolamines such as N-methylmethanolamine, N-methylethanolamine, N-methyl n-propanolamine, N-methylisopropanolamine, N-ethylmethanolamine, N-ethylethanolamine, N-ethyl n-propanolamine, N-ethylisopropanolamine, Nn-propylmethanolamine, Nn-propylethanolamine, Nn-propyl n-propanolamine, Nn-propylisopropanolamine, N-isopropylmethanolamine, N-isopropylethanolamine, N-isopropyl n-propanolamine, and N-isopropylisopropanolamine. Primary alkanolamines include, for example, monoalkanolamines such as methanolamine, ethanolamine, n-propanolamine, and isopropanolamine. From the viewpoint of releasability of the cured product, it is preferable to use one or more types selected from trialkanolamines, dialkanolamines, and N-alkylmonoalkanolamines as the water-soluble alkanolamine (B).
[0020] <Solvent (S)> Examples of the solvent (S) include water, a water-soluble organic solvent, and an aqueous solution of a water-soluble organic solvent. As the solvent (S), water and an aqueous solution of a water-soluble organic solvent are preferred, and water is more preferred, since both the inorganic basic compound (A) and the water-soluble alkanolamine (B) are well dissolved therein. Examples of the water-soluble organic solvent include sulfolane; hexamethylphosphoric triamide; sulfoxides such as dimethyl sulfoxide; sulfones such as dimethyl sulfone, diethyl sulfone, ethyl methyl sulfone, ethyl isopropyl sulfone, 3-methyl sulfone, bis(2-hydroxyethyl) sulfone, and tetramethylene sulfone; amides such as N,N-dimethylformamide, N-methylformamide, N,N-dimethylacetamide, N-methylacetamide, and N,N-diethylacetamide; N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-propyl-2-pyrrolidone, N-hydroxymethyl-2-pyrrolidone, and N-hydroxyethyl. imidazolidinones such as 1,3-dimethyl-2-imidazolidinone, 1,3-diethyl-2-imidazolidinone, 1,3-diisopropyl-2-imidazolidinone, etc.; alkanols such as methanol, ethanol, isopropyl alcohol, etc.; glycols such as ethylene glycol, propylene glycol (propane-1,2-diol), 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 2,3-butylene glycol, diethylene glycol, etc.; glycerin; lactones such as β-propylactone, γ-butyrolactone, δ-pentyrolactone, etc.; and the like.
[0021] <Acid-containing cleaning solution> The acid-containing cleaning liquid contains an acid. The acid-containing cleaning liquid may be a liquid consisting of an acid in a liquid state at room temperature (e.g., 20°C), or may be a solution of an acid. The acid contained in the acid-containing cleaning liquid is not particularly limited, and may be an organic acid or an inorganic acid. Here, an aqueous solution of the acid contained in the acid-containing cleaning liquid exhibits acidity according to the Bronsted definition at 20°C. When the acid-containing cleaning solution is an acid solution, the solvent contained in the acid-containing cleaning solution is not particularly limited. The solvent that the acid-containing cleaning solution may contain may be water, an organic solvent, or an aqueous solution of an organic solvent, as long as the acid is well dissolved in the solvent. The acid-containing cleaning solution may contain one type of acid alone or two or more types of acids in combination.
[0022] Examples of the organic acid include carboxylic acid compounds such as formic acid, acetic acid, citric acid, oxalic acid, 2-nitrophenylacetic acid, 2-ethylhexanoic acid, dodecanoic acid, and 2-hydroxy-1,2,3-propanetricarboxylic acid; sugar acid compounds such as ascorbic acid, tartaric acid, and glucuronic acid; and organic sulfonic acid compounds such as methanesulfonic acid, butanesulfonic acid, trifluoromethanesulfonic acid, benzenesulfonic acid, and p-toluenesulfonic acid. Inorganic acids include hydrochloric acid, hydrobromic acid, sulfuric acid, nitric acid, phosphoric acid, phosphonic acid, boric acid, and the like. The acid contained in the pickling-containing cleaning solution is preferably an organic acid, more preferably a water-soluble organic acid, and particularly preferably a water-soluble organic sulfonic acid compound.
[0023] <Photosensitive composition> The photosensitive composition contains a (meth)acrylic compound. The (meth)acrylic compound is a radical polymerizable compound having a (meth)acryloyl group. The (meth)acryloyl group refers to both an acryloyl group and a methacryloyl group.
[0024] [(Meth)acrylic compounds] The (meth)acrylic compound may be a mono(meth)acrylic compound having one (meth)acryloyl group, or a poly(meth)acrylic compound having two or more (meth)acryloyl groups.
[0025] Examples of mono(meth)acrylic compounds include methyl(meth)acrylate, ethyl(meth)acrylate, n-propyl(meth)acrylate, isopropyl(meth)acrylate, n-butyl(meth)acrylate, isobutyl(meth)acrylate, sec-butyl(meth)acrylate, tert-butyl(meth)acrylate, allyl(meth)acrylate, benzyl(meth)acrylate, cyclohexyl(meth)acrylate, phenyl(meth)acrylate, 2-methoxyethyl(meth)acrylate, 2-phenoxyethyl(meth)acrylate, methoxydiethylene glycol(meth)acrylate, methoxyethyl ... Examples of the acrylate esters include (meth)acrylic acid esters such as polyethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, methoxydipropylene glycol (meth)acrylate, isobornyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, 2-aminoethyl (meth)acrylate, 2-dimethylaminoethyl (meth)acrylate, 2-aminopropyl (meth)acrylate, 2-dimethylaminopropyl (meth)acrylate, 3-aminopropyl (meth)acrylate, 3-dimethylaminopropyl (meth)acrylate, and glycidyl (meth)acrylate.
[0026] Examples of poly(meth)acrylic compounds include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexane glycol di(meth)acrylate, dimethylol tricyclodecane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, glycerin di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol dimeth ... Examples of the polyfunctional compounds include pentane erythritol hexa(meth)acrylate, 2,2-bis(4-(meth)acryloxydiethoxyphenyl)propane, 2,2-bis(4-(meth)acryloxypolyethoxyphenyl)propane, 2-hydroxy-3-(meth)acryloyloxypropyl(meth)acrylate, ethylene glycol diglycidyl ether di(meth)acrylate, diethylene glycol diglycidyl ether di(meth)acrylate, phthalic acid diglycidyl ester di(meth)acrylate, glycerin tri(meth)acrylate, glycerin polyglycidyl ether poly(meth)acrylate, methylene bis(meth)acrylamide, (meth)acrylamide methylene ether, and a condensate of a polyhydric alcohol and N-methylol(meth)acrylamide, as well as triacrylformal. In addition, organopolysiloxanes having two or more (meth)acryloyl groups introduced therein can also be used as the poly(meth)acrylic compound. The organopolysiloxanes having two or more (meth)acryloyl groups introduced therein can be silsesquioxanes having two or more (meth)acryloyl groups introduced therein.
[0027] From the viewpoint of easiness in forming a patterned cured product by the imprint method, it is preferable to use (meth)acrylic acid esters, which are mono(meth)acrylic compounds, as the (meth)acrylic compound.
[0028] <Photopolymerization initiator> The photosensitive composition contains a photopolymerization initiator in order to polymerize the (meth)acrylic compound. The photopolymerization initiator is not particularly limited, and any conventionally known photopolymerization initiator can be used.
[0029] Specific examples of photopolymerization initiators include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 1-(4-dodecylphenyl)-2-hydroxy-2-methylpropan-1-one, 2,2-dimethoxy-1,2-diphenylethane-1-one, bis(4-dimethylaminophenyl) ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one (Irgacure 907), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one (Irgacure 907), and 1-methyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one (Irgacure 907). 369), O-acetyl-1-[6-(2-methylbenzoyl)-9-ethyl-9H-carbazol-3-yl]ethanone oxime, O-acetyl-1-[6-(pyrrol-2-ylcarbonyl)-9-ethyl-9H-carbazol-3-yl]ethanone oxime, (9-ethyl-6-nitro-9H-carbazol-3-yl)[4-(2-methoxy-1-methylethoxy)-2-methylphenyl]methanone O-acetyl oxime, 2-(benzoyloxyimino)-1-[4-(phenylthio)phenyl]-1-octanone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 4-benzoyl-4'-methyldimethylsulf , 4-dimethylaminobenzoic acid, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, butyl 4-dimethylaminobenzoate, 4-dimethylamino-2-ethylhexylbenzoic acid, 4-dimethylamino-2-isoamylbenzoic acid, benzyl-β-methoxyethyl acetal, benzyl dimethyl ketal, 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)oxime, methyl o-benzoylbenzoate, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 1-chloro-4-propoxythioxanthone, thioxanthene, 2-chlorothioxanthene, 2,4-Diethylthioxanthene, 2-Methylthioxanthene, 2-Isopropylthioxanthene, 2-Ethylanthraquinone, Octamethylanthraquinone, 1,2-Benzanthraquinone, 2,3-Diphenylanthraquinone, Azobisisobutyronitrile, Benzoyl peroxide, Cumene hydroperoxide, 2-Mercaptobenzimidazole, 2-Mercaptobenzoxazole, 2-Mercaptobenzothiazole, 2-(o-Chlorophenyl)-4,5-di(m-methoxyphenyl)-imidazolyl dimer, Benzophenone, 2-Chlorobenzo Phenone, p,p'-bisdimethylaminobenzophenone, 4,4'-bisdiethylaminobenzophenone, 4,4'-dichlorobenzophenone, 3,3-dimethyl-4-methoxybenzophenone, benzil, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin isobutyl ether, benzoin butyl ether, acetophenone, 2,2-diethoxyacetophenone, p-dimethylacetophenone, p-dimethylaminopropiophenone, dichloroacetophenone Phenone, trichloroacetophenone, p-tert-butylacetophenone, p-dimethylaminoacetophenone, p-tert-butyltrichloroacetophenone, p-tert-butyldichloroacetophenone, α,α-dichloro-4-phenoxyacetophenone, thioxanthone, 2-methylthioxanthone, 2-isopropylthioxanthone, dibenzosuberone, pentyl-4-dimethylaminobenzoate, 9-phenylacridine, 1,7-bis-(9-acridinyl)heptane, 1,5-bis-(9-acridinyl)pentane, 1,3-bis s-(9-acridinyl)propane, p-methoxytriazine, 2,4,6-tris(trichloromethyl)-s-triazine, 2-methyl-4,6-bis(trichloromethyl)-s-triazine, 2-[2-(5-methylfuran-2-yl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 2-[2-(furan-2-yl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 2-[2-(4-diethylamino-2-methylphenyl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 2-[2-(3,4-dimethoxyphenyl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-ethoxystyryl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-n-butoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2,4-bis-trichloromethyl-6-(3-bromo-4-methoxy)phenyl-s-triazine, 2,4-bis-trichloromethyl-6-(2-bromo-4-methoxy)phenyl-s-triazine, 2,4-bis-trichloromethyl-6-(3-bromo-4-methoxy)styrylphenyl-s-triazine, 2,4-bis-trichloromethyl-6-(2-bromo-4-methoxy)styrylphenyl-s-triazine, and the like.
[0030] These photopolymerization initiators can be used alone or in combination of two or more kinds.
[0031] The content of the photopolymerization initiator in the photosensitive composition is preferably 0.01 parts by mass or more and 20 parts by mass or less, more preferably 0.05 parts by mass or more and 15 parts by mass or less, and even more preferably 0.1 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the total of the (meth)acrylic compounds contained in the photosensitive composition.
[0032] <Solvent> The photosensitive composition may contain a solvent for the purpose of adjusting the coating property, etc. The type of the solvent is not particularly limited, but is typically an organic solvent.
[0033] Examples of organic solvents that can be incorporated in the photosensitive composition include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ...ethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol (Poly)alkylene glycol monoalkyl ethers such as dipropylene glycol monomethyl ether and tripropylene glycol monoethyl ether; (Poly)alkylene glycol monoalkyl ether acetates such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate; other ethers such as diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, and tetrahydrofuran; ketones such as methyl ethyl ketone, cyclohexanone, 2-heptanone, and 3-heptanone; alkyl esters of lactate such as methyl 2-hydroxypropionate and ethyl 2-hydroxypropionate;Ethyl 2-hydroxy-2-methylpropionate, Methyl 3-methoxypropionate, Ethyl 3-methoxypropionate, Methyl 3-ethoxypropionate, Ethyl 3-ethoxypropionate, Ethoxyethyl acetate, Ethyl hydroxyacetate, Methyl 2-hydroxy-3-methylbutanoate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutylpropionate, Ethyl acetate, n-propyl acetate, Isopropyl acetate, n-butyl acetate ethyl, isobutyl acetate, n-pentyl formate, isopentyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, isopropyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl 2-oxobutanoate and other esters; aromatic hydrocarbons such as toluene and xylene; amides such as N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide;
[0034] The range of the content of the solvent in the photosensitive composition is not particularly limited. For example, the content of the solvent in the photosensitive composition may be 95% by mass or less, 80% by mass or less, 50% by mass or less, 30% by mass or less, or 20% by mass or less, based on the mass of the photosensitive composition. Furthermore, when the photosensitive composition contains a solvent, the content of the solvent in the photosensitive composition may be 1 mass % or more, 5 mass % or more, 10 mass % or more, 20 mass % or more, or 30 mass % or more, relative to the mass of the photosensitive composition.
[0035] <Other ingredients> The photosensitive composition may contain various additives in addition to the components described above. Examples of the additives that may be added to the photosensitive composition include dispersants, adhesion promoters such as silane coupling agents, antioxidants, anti-aggregation agents, antifoaming agents, and surfactants.
[0036] The surfactant is not particularly limited, and known components such as fluorine-based surfactants and silicone-based surfactants can be used. Specific examples of fluorine-based surfactants include commercially available fluorine-based surfactants such as BM-1000, BM-1100 (all manufactured by BM Chemie), Megafac F142D, Megafac F172, Megafac F173, Megafac F183 (all manufactured by Dainippon Ink and Chemicals), Fluorad FC-135, Fluorad FC-170C, Fluorad FC-430, Fluorad FC-431 (all manufactured by Sumitomo 3M), Surflon S-112, Surflon S-113, Surflon S-131, Surflon S-141, Surflon S-145 (all manufactured by Asahi Glass Co., Ltd.), SH-28PA, SH-190, SH-193, SZ-6032, and SF-8428 (all manufactured by Toray Silicones), but are not limited thereto. As the silicone surfactant, an unmodified silicone surfactant, a polyether-modified silicone surfactant, a polyester-modified silicone surfactant, an alkyl-modified silicone surfactant, an aralkyl-modified silicone surfactant, a reactive silicone surfactant, and the like can be preferably used. As the silicone surfactant, commercially available silicone surfactants can be used. Specific examples of commercially available silicone surfactants include Paintad M (manufactured by Toray Dow Corning Co., Ltd.), Topika K1000, Topika K2000, Topika K5000 (all manufactured by Takachiho Sangyo Co., Ltd.), XL-121 (polyether-modified silicone surfactant, manufactured by Clariant), and BYK-310 (polyester-modified silicone surfactant, manufactured by BYK-Chemie Co., Ltd.).
[0037] The photosensitive composition may contain an antioxidant. The antioxidant is not particularly limited, and any conventionally known antioxidant may be used, such as a hindered phenol-based antioxidant, a hindered amine-based antioxidant, a phosphorus-based antioxidant, or a sulfur-based antioxidant.
[0038] <Method of preparing photosensitive composition> The photosensitive composition is prepared by mixing and stirring the above-mentioned components in a conventional manner. Examples of devices that can be used when mixing and stirring the above-mentioned components include a dissolver, a homogenizer, and a three-roll mill. After the above-mentioned components are mixed uniformly, the resulting mixture may be further filtered using a mesh, a membrane filter, or the like.
[0039] <Cured material layer formation method> The cured layer can be formed by a cured layer forming method including a step of applying the above-mentioned photosensitive composition onto a substrate to form a coating film (hereinafter also simply referred to as a "coating film forming step") and a step of curing the coating film. The method for forming a cured material layer preferably further includes a pattern forming step, and specifically, preferably further includes (1) a step of pressing a mold against the surface of the coating film to form a pattern in the coating film (imprint method), or (2) a step of curing the coating film by position-selective exposure and further includes a step of developing the position-selectively exposed coating film to form a pattern (development method).
[0040] The material of the substrate can be selected depending on various applications, and examples of the material of the substrate include quartz, glass, ceramic materials, metals, paper, SOG (Spin On Glass), polymers, conductive metal oxides, and semiconductor materials. Metals include Ni, Cu, Cr, Fe, and Al, and alloys of these metals. Polymers include polyester, polycarbonate, and polyimide. Semiconductor materials include silicon, silicon nitride, polysilicon, silicon oxide, and amorphous silicon. In addition, the substrate may be an optical film, a TFT array substrate, an electrode plate of a PDP, etc. The surface of the substrate may be a deposition film, a magnetic film, a reflective film, etc.
[0041] The shape of the substrate is not particularly limited. Typically, the substrate is in the form of a plate. When the substrate is made of a flexible material, the substrate may be wound in a roll. Furthermore, the substrate may be either a light-transmitting substrate or a light-non-transmitting substrate depending on the application of the substrate.
[0042] In the coating film forming process, the photosensitive composition is applied onto a substrate on which a cured layer is to be formed using a contact transfer type coating device such as an inkjet, roll coater, reverse coater, or bar coater, or a non-contact type coating device such as a spinner (rotary coating device), dispenser, spray, screen printing, or curtain flow coater, and if necessary, the solvent is removed by drying (pre-baking) to form a coating film. The thickness of the coating film is not particularly limited, but is preferably from 10 nm to 50 μm, more preferably from 50 nm to 30 μm, even more preferably from 100 nm to 10 μm, and particularly preferably from 150 nm to 5 μm. For convenience, droplets piled up on a substrate, a photosensitive composition embedded in the recesses of a substrate having projections and recesses, a photosensitive composition filled in the recesses of a mold, and the like are also referred to as a "coating film."
[0043] When forming a pattern by the imprint method as described above in (1), a mold is pressed against the surface of the pattern-forming layer in order to transfer the pattern to the coating film. This allows the fine pattern previously formed on the pressing surface of the mold to be transferred to the coating film. Alternatively, a photosensitive composition may be applied to a mold having a pattern, and a substrate may be pressed against the mold. The coating film can be cured by pressing a light-transmitting mold against the surface of the coating film and exposing the back side of the mold to light. Alternatively, the photosensitive composition can be applied onto a light-transmitting substrate, pressed against the mold, and exposed from the back side of the substrate to light to cure the photosensitive composition.
[0044] The molding material is not particularly limited, but may be any material having a certain strength and durability. Specific examples of the light-transmitting molding agent include glass, quartz, light-transmitting resin, transparent metal deposition film, flexible film such as polydimethylsiloxane, photocured film, metal film, etc. Examples of the light-transmitting resin include polymethyl methacrylate (PMMA), polycarbonate resin, polyethylene terephthalate (PET), etc.
[0045] The non-light-transmitting molding material is not particularly limited, but may be any material having a predetermined strength, and may be any of the materials mentioned above as the material for the substrate. The shape of the mold is not particularly limited, and may be either a plate-shaped mold or a roll-shaped mold. A roll-shaped mold is particularly applicable when continuous productivity of transfer is required.
[0046] As described above in (1), when forming a pattern by the imprint method, it is preferable to perform the pattern formation at a mold pressure of 10 atmospheres or less. When the mold pressure is 10 atmospheres or less, the mold and the substrate tend not to deform easily, and the pattern accuracy tends to improve. In addition, a mold pressure of 10 atmospheres or less is also preferable because the low pressure tends to allow the device to be reduced in size. It is preferable to select a mold pressure in a range where the residual film of the photosensitive composition on the mold convex parts is small and the uniformity of the mold transfer can be ensured. As a preliminary step to the exposure described below, a vacuum state is used to prevent the inclusion of air bubbles, suppress the decrease in reactivity due to the inclusion of oxygen, and improve the adhesion between the mold and the photosensitive composition, so exposure may be performed in a vacuum state. -1 The pressure ranges from Pa to atmospheric pressure.
[0047] Next, the formed coating film is cured by exposure to light. The light source used for exposure is not particularly limited, and examples thereof include high pressure mercury lamps, ultra-high pressure mercury lamps, xenon lamps, carbon arc lamps, LEDs, etc. Using such a light source, the coating film can be exposed by irradiating it with radiation or electromagnetic waves such as ArF excimer laser, KrF excimer laser, F2 excimer laser, extreme ultraviolet ray (EUV), vacuum ultraviolet ray (VUV), electron beam, X-ray, soft X-ray, g-ray, i-ray, h-ray, j-ray, k-ray, etc. The coating film may be exposed position-selectively through a negative mask. The exposure amount varies depending on the composition of the photosensitive composition, but is, for example, 10 mJ / cm. 2 More than 2,000mJ / cm 2 Less than 100 mJ / cm is preferable. 2 More than 1,500mJ / cm 2 Less than 200 mJ / cm is more preferable. 2 More than 1,200mJ / cm 2 The exposure illuminance varies depending on the composition of the photosensitive composition, but is more preferably 1 mW / cm 2 More than 50mW / cm 2 The following ranges are preferred:
[0048] As in the above-mentioned development method (2), the step of curing the coating film is carried out by site-selective exposure, and the site-selectively exposed coating film is developed to obtain a patterned cured layer.
[0049] In the development step, the exposed coating film is developed with a developer to form a cured product patterned into a desired shape. The development method is not particularly limited, and a dipping method, a spray method, a paddle method, a dynamic dispensing method, etc. can be used. Specific examples of developers containing organic solvents include alcohol-based solvents or glycol ether-based solvents such as PE (propylene glycol monomethyl ether), ether-based solvents such as tetrahydrofuran, ester-based solvents such as butyl acetate, and ketone-based solvents such as acetone and methyl amyl ketone. Specific examples of alkaline developers include organic ones such as monoethanolamine, diethanolamine, and triethanolamine, and aqueous solutions of sodium hydroxide, potassium hydroxide, sodium carbonate, ammonia, and quaternary ammonium salts.
[0050] If necessary, the cured product after exposure or the patterned cured product after development may be post-baked to further heat-curing. The post-baking temperature is preferably 150° C. or higher and 270° C. or lower.
[0051] <Removal method> The cured material layer formed on the substrate is brought into contact with the above-mentioned stripping liquid to peel off the cured material layer from the substrate. The method of bringing the cured material layer into contact with the stripping liquid is not particularly limited. Examples of the method of bringing the cured material layer into contact with the stripping liquid include a method of applying the stripping liquid to the surface of the cured material layer, a method of pouring the stripping liquid onto the surface of the cured material layer, a method of spraying the stripping liquid onto the surface of the cured material layer, and a method of immersing the substrate having the cured material layer in the stripping liquid. Among these methods, the method of immersing the substrate having the cured material layer in the stripping liquid is preferred because it is easy to peel the cured material layer from the substrate.
[0052] The temperature of the stripping solution when the substrate having the cured layer is brought into contact with the stripping solution is not particularly limited, but is preferably from 60° C. to 100° C., and more preferably from 70° C. to 90° C. The contact time is typically preferably from 1 minute to 60 minutes, more preferably from 10 minutes to 50 minutes, and particularly preferably from 20 minutes to 40 minutes. After the substrate is brought into contact with the stripping solution, the substrate from which the cured layer has been stripped is washed with pure water or an organic solvent, and then the substrate is dried, thereby obtaining a substrate from which the cured layer has been stripped.
[0053] As described above, before the substrate having the cured material layer is contacted with the stripping solution, the cured material layer is contacted with the acid-containing cleaning solution. By contacting the cured material layer with the acid-containing cleaning solution, the peelability of the cured material layer from the substrate is good when the substrate having the cured material layer is contacted with the stripping solution. The temperature of the acid-containing cleaning solution when the cured material layer is contacted with the acid-containing cleaning solution is not particularly limited. The temperature of the acid-containing cleaning solution is preferably 60°C or more and 100°C or less, more preferably 70°C or more and 90°C or less. The contact time is typically preferably 1 minute or more and 60 minutes or less, more preferably 1 minute or more and 30 minutes or less, and particularly preferably 5 minutes or more and 15 minutes or less. After the substrate having the cured material layer is brought into contact with the acid-containing cleaning solution, the substrate may be washed with water or an organic solvent, if necessary, and then the cured material layer may be peeled off from the substrate with a stripping solution.
[0054] As described above, the present inventors provide the following (1) to (8). (1) A method for peeling off a cured material layer formed on a substrate from the substrate, comprising the steps of: The peeling method is contacting the cured layer with an acid-containing cleaning solution; and peeling the cured layer from the substrate by contacting the cured layer with a stripping solution; the cured material layer is made of a cured material of a photosensitive composition containing a (meth)acrylic compound, The stripping solution contains an inorganic basic compound (A), a water-soluble alkanolamine (B), and a solvent (S); A stripping method, wherein the inorganic basic compound (A) comprises sodium metasilicate and sodium phosphate. (2) The stripping method according to (1), wherein the acid-containing cleaning solution contains an organic sulfonic acid compound. (3) The method according to (1) or (2), wherein the substrate has an aluminum-containing layer on its surface, and the cured layer is formed on the aluminum-containing layer. (4) The stripping method according to any one of (1) to (3), wherein the water-soluble alkanolamine (B) is at least one selected from trialkanolamines, dialkanolamines, and N-alkylmonoalkanolamines. (5) The peeling method according to any one of (1) to (4), wherein the cured material layer is contacted with the stripping solution at a temperature of 60° C. or more and 100° C. or less for 10 minutes or more and 60 minutes or less. (6) The hardened layer is forming a coating film of a photosensitive composition on a substrate; Pressing the mold against the coating film to transfer the shape of the mold to the coating film; exposing the coating film to light and curing it while the mold is pressed against the coating film to form a patterned cured layer; Releasing the mold from the cured material layer; and The peeling method according to any one of (1) to (5), wherein the cured layer is formed by a method comprising the steps of: (7) A method for producing a substrate provided with a patterned cured material layer, comprising: forming, by an imprint method, a patterned cured material layer made of a cured material of a photosensitive composition containing a (meth)acrylic compound on a substrate from which the cured material layer has been peeled off by the method according to any one of (1) to (6). (8) A composition comprising an inorganic basic compound (A), a water-soluble alkanolamine (B), and a solvent (S), A stripping solution, wherein the inorganic basic compound (A) comprises sodium metasilicate and sodium phosphate. (9) The stripping solution according to (8), wherein the water-soluble alkanolamine (B) is at least one selected from the group consisting of trialkanolamines, dialkanolamines, and N-alkylmonoalkanolamines. EXAMPLES
[0055] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0056] <Preparation of Photosensitive Resin Composition for Imprinting> A photosensitive composition for imprints was obtained by mixing 80 parts by mass of isobornyl acrylate (Light Acrylate IB-XA, manufactured by Kyoeisha Chemical Co., Ltd.), 20 parts by mass of methacrylate-modified silsesquioxane (MAC-SQLP-35, manufactured by Toagosei Co., Ltd.), 10 parts by mass of 2-methyl-1-methyl[4-(methylthio)phenyl]-2-morpholinopropan-1-one (Irgacure907, manufactured by BASF)), and 2 parts by mass of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one (Irgacure907, manufactured by BASF)).
[0057] <Preparation of a substrate with a nanoimprint pattern> The above photosensitive composition for imprints was applied onto an aluminum-deposited glass substrate (manufactured by Nippon Electronic Glass Co., Ltd.) using an inkjet head (KM-512MHX (manufactured by Konica Minolta, Inc.)) to form a photosensitive layer. Specifically, the above prepared photosensitive composition for imprints was discharged with a droplet volume of 14 pL per nozzle, while controlling the discharge timing so that the pattern was in a square arrangement with a middle distance (pitch) of 300 μm, thereby coating the photosensitive composition over the entire surface of the aluminum-deposited layer to form a photosensitive layer. Using a nanoimprint transfer device (ST200 (Toshiba Machine Co., Ltd.)), a mold with a 50 nm line and space pattern was pressed against the photosensitive layer for 4 seconds under vacuum with a pressure of 0.5 MPa to deform the photosensitive layer. UV light with a wavelength of 365 nm was applied to the deformed photosensitive layer for an exposure length of 1,000 mJ / cm. 2 The photosensitive layer was cured by exposure to light at 400 nm, and the mold was then peeled off to form a cured layer patterned in a line and space pattern.
[0058] <Preparation of inorganic alkaline stripping solution> An inorganic alkaline stripping solution was prepared by mixing 2.5 parts by mass of sodium metasilicate, 1.0 part by mass of sodium phosphate, and 96.5 parts by mass of water.
[0059] <Preparation of stripping solution> Example 1 Stripping solution 1 was prepared by adding 2.5 parts by mass of N-methylethanolamine to 100 parts by mass of the inorganic alkaline stripping solution described above.
[0060] Example 2 Stripping solution 2 was prepared by adding 1.25 parts by mass of N-methylethanolamine to 100 parts by mass of the inorganic alkaline stripping solution described above.
[0061] <Acid-containing cleaning solution> The organic acids shown below were used as the acid-containing cleaning solutions shown in Table 1. All of the organic acids below are liquid at room temperature. MSA: Methanesulfonic acid TFMSA: Trifluoromethanesulfonic acid BSA: butanesulfonic acid
[0062] <Removal of the patterned cured layer from the substrate> In Example 3, a substrate having the above-mentioned patterned cured material layer was immersed in the above-mentioned acid-containing cleaning solution MSA at 80°C for 5 minutes (acid cleaning step), and then washed with water. The water-washed substrate was then immersed in stripping solution 1 at 80°C for 15 minutes (peeling step). After immersion, the substrate was washed with ultrapure water. Nitrogen gas was sprayed onto the washed substrate to dry it. This resulted in a substrate from which the patterned cured material layer had been peeled off. In Examples 4 to 8 and Comparative Examples 1 to 9, the cured film was peeled off from the substrate having the patterned cured material layer in the same manner as in Example 3, except that the conditions of the acid washing step and the peeling step were changed to those shown in Table 1. In addition, the acid washing step was not performed in Comparative Examples 1 to 5. In Comparative Examples 6 to 9, the peeling step was not performed.
[0063] [Table 1]
[0064] <Evaluation> The substrates that had been subjected to the prescribed treatments in Examples 3 to 8 and Comparative Examples 1 to 9 were used to evaluate removability and Al damage resistance according to the following methods. Furthermore, a patterned cured layer was formed again on the substrates obtained in Examples 3 to 8 and Comparative Examples 1 to 9, and the re-imprintability of the substrates was evaluated. The evaluation results are shown in Table 2.
[0065] [Removability] The obtained substrate was observed with a scanning electron microscope (S-4700 (manufactured by Hitachi High-Technologies Corporation)), and the removability of the patterned cured material layer was evaluated according to the following criteria. ◯: The patterned cured material layer was completely removed. ×: Residues of the patterned cured material layer were observed.
[0066] [Al Damage] The Al film thickness of the obtained substrate was measured from the measured density obtained by X-ray fluorescence (XRF) measurement (ZSX Primus (Rigaku Corporation)). The Al film thickness T1 of the obtained substrate was compared with the Al film thickness T0 of the aluminum-deposited glass substrate before the peeling treatment, and was evaluated according to the following criteria. Al thickness variation (nm) = T0-T1 ○: Absolute value of aluminum film thickness fluctuation is less than 5 nm ×: Absolute value of Al film thickness fluctuation is 5 nm or more
[0067] [Re-imprintability] Using the substrates obtained in Examples 3 to 8 and Comparative Examples 1 to 9, a re-patterned cured material layer was formed on the substrate in the same manner as in the preparation of the substrate on which the nanoimprint pattern was formed as described above. The patterned cured material layer was observed with a scanning electron microscope (S-4700 (manufactured by Hitachi High-Technologies Corporation)), and the re-imprintability was evaluated according to the following criteria. A: The pattern was formed over the entire surface of the substrate. ×: The pattern was not formed on a part of the substrate surface or on the entire surface.
[0068] [Table 2]
[0069] According to Table 2, in Examples 3 to 8 in which a cured layer formed on a substrate using a photosensitive composition containing a (meth)acrylic compound was brought into contact with an acid-containing cleaning liquid and then brought into contact with a stripping liquid containing sodium metasilicate and sodium phosphate as the inorganic basic compound (A), a water-soluble alkanolamine (B), and a solvent (S), it is clear that the cured layer was successfully removed while suppressing damage to the aluminum film, and a substrate having excellent re-imprintability was obtained. On the other hand, in Comparative Examples 1 to 5 in which the acid washing step using an acid-containing washing solution was not performed, and in Comparative Examples 6 to 9 in which the peeling step was not performed, at least one of the following could not be achieved: satisfactory removal of the cured layer and suppression of damage to the aluminum film. In addition, the substrates obtained in Comparative Examples 1 to 9 all had poor re-imprintability.
Claims
1. A peeling method for peeling a cured material layer formed on a substrate from the substrate, comprising: The peeling method comprises: contacting the cured material layer with an acid-containing cleaning solution; and peeling the cured material layer from the substrate by contacting the cured material layer with a stripping solution, the cured material layer is made of a cured material of a photosensitive composition containing a (meth)acrylic compound, the stripping solution contains an inorganic basic compound (A), a water-soluble alkanolamine (B), and a solvent (S); The stripping method, wherein the inorganic basic compound (A) comprises sodium metasilicate and sodium phosphate.
2. The stripping method according to claim 1 , wherein the acid-containing cleaning solution contains an organic sulfonic acid compound.
3. The peeling method according to claim 1 or 2, wherein the substrate has an aluminum-containing layer on a surface thereof, and the cured product layer is formed on the aluminum-containing layer.
4. 3. The stripping method according to claim 1, wherein the water-soluble alkanolamine (B) is at least one selected from trialkanolamines, dialkanolamines, and N-alkylmonoalkanolamines.
5. The stripping method according to claim 1 or 2, wherein the cured product layer is brought into contact with the stripping solution at a temperature of 60° C. or higher and 100° C. or lower for 10 minutes or longer and 60 minutes or shorter.
6. The cured material layer is forming a coating film of the photosensitive composition on the substrate; pressing a mold against the coating film to transfer the shape of the mold to the coating film; exposing the coating film to light and curing it while the mold is pressed against the coating film to form a patterned cured layer; separating the mold from the cured material layer; The peeling method according to claim 1 or 2, wherein the cured product layer is formed by a method comprising the steps of:
7. 3. A method for producing a substrate provided with a patterned cured material layer, the method comprising: forming, by an imprint method, a patterned cured material layer made of a cured material of a photosensitive composition containing a (meth)acrylic compound on a substrate from which the cured material layer has been peeled by the method according to claim 1 or 2.
8. The composition contains an inorganic basic compound (A), a water-soluble alkanolamine (B), and a solvent (S), The stripping solution, wherein the inorganic basic compound (A) contains sodium metasilicate and sodium phosphate.
9. 9. The stripping solution according to claim 8, wherein the water-soluble alkanolamine (B) is at least one selected from trialkanolamines, dialkanolamines, and N-alkylmonoalkanolamines.
Citation Information
Patent Citations
Resist removal liquid
WO2018061064A1