Multistep heat decomposition method of polyolefin
The multistage pyrolysis process for polyolefins addresses inefficiencies in thermal decomposition by using microwave heating in a fixed bed reactor, achieving high yields of ethylene and acetylene monomers with improved energy efficiency and adaptability.
Patent Information
- Application Number
- JP2023046686
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing methods for polyolefin thermal decomposition lack specific reaction conditions, stability in temperature control, and scalability, leading to decreased production efficiency and increased device size due to low heat transfer area and responsiveness.
A multistage pyrolysis process involving a first step of rough decomposition at 400°C to 700°C followed by a second step of decomposition at 1000°C or higher using microwave heating in a fixed bed reactor, with a compact design and temperature-responsive heating to manage raw material variability.
This method enhances the yield of high-value olefin monomers like ethylene and acetylene, while being energy-efficient and adaptable to raw material changes, with improved heat transfer and reactor compactness.
Smart Images

Figure 2024135811000002 
Figure 2024135811000003 
Figure 2024135811000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a multi-stage pyrolysis process for polyolefins. [Background technology]
[0002] Among plastics, polyolefins such as polyethylene and polypropylene are produced and disposed of in large quantities. For example, thermal decomposition of polyolefins is known as a chemical recycling method for polyolefins. In the thermal decomposition of polyolefins, the decomposition products have a molecular weight distribution and undergo phase changes from solid to liquid and from liquid to gas phase, so precise design of the thermal decomposition temperature is required to efficiently obtain monomers or their derivatives.
[0003] As a method for efficiently pyrolyzing polyolefins, for example, an apparatus or method is known in which pyrolysis is divided into two steps, the first step is decomposed to oil or wax, and the second step is heated to produce a gaseous product consisting of a plastic raw material and a composite of the raw material (see, for example, Patent Document 1, Non-Patent Documents 1 and 2). Patent Document 1 describes an apparatus in which a hydrocarbon-containing material is decomposed to gaseous hydrocarbons in a first reactor, and then transferred to a second reactor at a higher temperature for pyrolysis. Non-Patent Documents 1 and 2 describe that a light gas can be efficiently obtained from polyethylene by a two-stage decomposition method using a first reactor at about 500°C and a second reactor at about 800°C to 900°C. In particular, it describes that repolymerization and aromatization of the decomposition product can be suppressed by shortening the residence time in the second reactor. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2014-503610 [Non-patent literature]
[0005] [Non-Patent Document 1] Artetxe M. et al., Industrial & Engineering Chemistry Research, Vol. 51, January 19, 2012, 13915) [Non-Patent Document 2] Della Zassa M. et al., Journal of Analytical and Applied Pyrolysis, Vol. 87, June 22, 2009, 248) Summary of the Invention [Problem to be solved by the invention]
[0006] In Patent Document 1, plastics are exemplified, but the decomposition reaction of specific plastics is not described. In addition, there are no examples using plastics as raw materials, and no description of specific decomposition conditions. In addition, in Non-Patent Document 1, the temperature of the first reactor is constant at 500°C and the temperature of the second reactor is 800°C to 950°C in the decomposition of polyethylene, but the decomposition results at temperatures higher than 950°C are not described. In addition, in Non-Patent Documents 1 and 2, external heating of the tube reactor is adopted for heating the second reactor, and in the decomposition of waste plastics with an unstable raw material composition, the appropriate decomposition temperature due to the resin composition is likely to change, and there is a concern that the production stability of olefins will decrease due to the low responsiveness of temperature control. In addition, there is a problem that the device will become larger when scaling up, such as by lengthening the tube, from the viewpoint of heat transfer area.
[0007] The present invention has been made in view of the above circumstances, and aims to provide a thermal decomposition method for obtaining high-value-added olefin monomer derivatives such as ethylene, which is a chemically recyclable olefin monomer, and especially acetylene, in high yields in the thermal decomposition of polyolefins. In addition, the present invention aims to provide a thermal decomposition method suitable for raw material changes and supply-demand balance by using microwave heating that is energy-saving and has good temperature responsiveness, and to provide a thermal decomposition method in a compact reactor by increasing the heat transfer area in a fixed-bed reactor. In addition, the present invention aims to provide a compact reactor by increasing the heat transfer area in a fixed-bed reactor by taking advantage of the characteristics of microwaves that are energy-saving and highly temperature responsive, in order to easily respond to raw material changes and supply-demand balance. [Means for solving the problem]
[0008] The present invention has the following aspects. [1] A process for pyrolyzing polyolefins, comprising the steps of: A first step of roughly decomposing polyolefins by heating; A second step of decomposing the crude decomposition product obtained in the first step by heating at 1000°C or higher. [2] The method for multi-stage pyrolysis of polyolefins according to [1], wherein the polyolefins include at least one of polyethylene and polypropylene. [3] The method for multi-stage pyrolysis of polyolefins according to [1] or [2], wherein the polyolefins are heated under a flow of inert gas having an oxygen concentration of 0.5 ppm or less. [4] The method for multi-stage pyrolysis of polyolefins according to any one of [1] to [3], wherein the heating in the first step includes a temperature range of 400° C. or higher and 700° C. or lower. [5] The method for multi-stage pyrolysis of polyolefins according to any one of [1] to [4], wherein the heating in the second step is microwave heating. [6] The method for multi-stage pyrolysis of polyolefins according to [5], wherein the microwave heating is carried out in a fixed-bed reactor packed with a microwave absorber. Effect of the Invention
[0009] According to the present invention, a thermal decomposition method can be provided in which, in the thermal decomposition of polyolefins, ethylene, which is a chemically recyclable olefin monomer, and especially high-value-added olefin monomer derivatives such as acetylene, can be obtained in high yield. In addition, by using microwave heating that is energy-saving and has good temperature responsiveness, a thermal decomposition method suitable for raw material changes and supply-demand balance can be provided, and a thermal decomposition method in a compact reactor can be provided by increasing the heat transfer area in a fixed-bed reactor. In addition, in order to easily respond to raw material changes and supply-demand balance, a compact reactor can be provided by increasing the heat transfer area in a fixed-bed reactor by taking advantage of the characteristics of microwaves that are energy-saving and have high temperature responsiveness. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic diagram showing a polyolefin cracking apparatus used in a polyolefin multi-stage pyrolysis method according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing a reaction vessel constituting a polyolefin cracking apparatus used in a polyolefin multi-stage thermal cracking method according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described in detail. The symbol "~" indicating a range of numerical values means that the numerical values before and after it are included as the lower limit and upper limit.
[0012] [Multi-stage pyrolysis of polyolefins] A multi-stage pyrolysis method for polyolefins according to one embodiment of the present invention comprises a first step of roughly decomposing polyolefins by heating, and a second step of decomposing the roughly decomposed product obtained in the first step by heating at 1000°C or higher, thereby decomposing polyolefins. The polyolefin multi-stage pyrolysis method of the present invention may also have a step other than the first and second steps. For example, a polyolefin pretreatment step, a desalting step, a neutralization step, a washing step, a sterilization step, a detoxification step, a heat exchange step, a distillation step, a withdrawal step, etc. may be included. Although other steps may be provided between the first and second steps, it is preferable that the first and second steps are carried out continuously and kept warm in order to prevent blockage due to solidification of the crude decomposition product caused by heat radiation and a decrease in the furnace temperature in the second step.
[0013] "Polyolefin" In the multi-stage pyrolysis method of polyolefin according to the present embodiment, examples of the polyolefin to be treated include polyethylene, polypropylene, polybutene, polyisobutylene, polybutadiene, poly-α-olefin, polystyrene, etc. The polyolefin preferably contains at least one of polyethylene and polypropylene. That is, it may contain only polyethylene or polypropylene, or it may contain polyethylene and polypropylene. The polyolefin may be a copolymer polymerized using two or more types of monomers. Polyolefins are used from plastic waste recovered after use, or from plastics recovered during manufacturing and molding processes.
[0014] It is preferable to pretreat the polyolefin before decomposing it. If the polyolefin is contaminated, the polyolefin is washed to remove the contaminants. Polyolefins come in various shapes. If polyolefins are pyrolyzed in this state, they may not be pyrolyzed uniformly. Therefore, the rate of decomposition can be improved by crushing the polyolefins in advance.
[0015] Since polyolefin molded products are bulky, it is preferable to reduce the volume by crushing or compressing them. The shape of the polyolefin after pulverization may be, for example, any one of shavings, flakes, granules, powder, chips, sheets, or a combination thereof. As a means for pulverizing polyolefin, for example, a device is used in which polyolefin is fed from a hopper into the interior of a cylindrical rotating shaft equipped with a fixed blade, and cut by the action of the rotating blade. The means for compressing the polyolefin may be, for example, either physical compression using a press or volume reduction treatment using a single-screw or multi-screw extruder, or a combination of these.
[0016] "First step" In the first step, a polyolefin is roughly decomposed by heating the polyolefin, and the resulting roughly decomposed product is supplied to the second step. In the present invention, crude decomposition refers to breaking down polyolefins into compounds having a molecular weight of 1000 or less. The upper limit of the molecular weight of the crude decomposition product in the first step is 1000 or less, preferably 800 or less, and more preferably 700 or less. When the molecular weight of the crude decomposition product is equal to or less than the upper limit, it becomes possible to supply the crude decomposition product to the second step in a gas phase or liquid phase, improving the yield of the olefin monomer and preventing blockage of the flow path between the first step and the second step due to solidification of the crude decomposition product.
[0017] The molecular weight of the crude decomposition product is measured by analyzing it by laser desorption ionization mass spectrometry (LDI-MS). The LDI-MS measurement is performed by placing the crude decomposition product on a target plate, and analyzing it under the conditions of Nd:YLF laser intensity 53%, delay time 300 ns, and no matrix. The molecular weight of the crude decomposition product is determined by considering the peak of a compound that does not contain a heteroatom as a significant peak in the obtained LDI-MS (+) spectrum, and the compound whose peak height is 1% or more of the maximum peak intensity in the spectrum among the significant peaks is determined as the maximum molecular weight of the polyolefin decomposition product.
[0018] The reactor used in the first step is not particularly limited as long as it can heat the polyolefin, and may be, for example, a batch reactor, a tank reactor, or a tubular reactor, or a combination of these. The type of reactor may be a fixed bed, a fluidized bed, a suspension bed, a spouted bed, a kiln, or a rotary kiln, or a combination of these. The method of heating the reactor may be steam heating, oil heating, burner heating, high-frequency induction heating, high-frequency dielectric heating, halogen lamp heating, plasma heating, or microwave heating, or a combination of these.
[0019] The temperature in the reactor during the decomposition of the polyolefin in the first step is not particularly limited, but the lower limit is 400°C, preferably 500°C, and more preferably 550°C. When the temperature in the reactor during the decomposition is equal to or higher than the lower limit, the polyolefin is thermally decomposed to lower molecular weight, and can be supplied to the second step in a gas phase or liquid phase. The upper limit of the temperature in the reactor is 700°C, preferably 650°C, and more preferably 625°C. When the temperature in the reactor during the decomposition is equal to or lower than the upper limit, the production of polycyclic aromatic hydrocarbons due to excessive decomposition of the polyolefin is suppressed, and the yield of olefin monomers and their derivative gases is improved.
[0020] In the first step, the inert atmosphere flowing through the reactor in the crude decomposition of polyolefin is not particularly limited, and may be, for example, any of nitrogen, argon, helium, carbon dioxide, and water vapor, or a combination thereof. The inert atmosphere may contain hydrogen and light paraffin gas. The upper limit of the oxygen concentration of the inert atmosphere is 0.5 ppm, preferably 0.1 ppm, and more preferably 0.02 ppm. By keeping the oxygen concentration of the inert atmosphere below the upper limit, thermal runaway due to oxidation of polyolefin, which is an exothermic reaction, is suppressed, and the yield of olefin monomer and its derivative gas is improved.
[0021] The reactor used in the first step and the reactor used in the second step are preferably connected, although there is no particular limitation therebetween. By connecting the reactor used in the first step and the reactor used in the second step, the process of increasing and decreasing the temperature is not required, and it is possible to prevent unnecessary energy consumption and to prevent blockage due to cooling and solidification of the crude cracked gas. In addition, there may be a temperature gradient between the reactor used in the first step and the reactor used in the second step.
[0022] "Second step" In the second step, the crude polyolefin decomposition product obtained in the first step is heated to 1000° C. or higher in a reactor to thermally decompose the crude polyolefin decomposition product.
[0023] The reactor used in the second step is not particularly limited as long as it can heat the polyolefin decomposition product roughly decomposed in the first step, but may be, for example, any of a batch reactor, a tank reactor, and a tubular reactor, with a tubular reactor being preferred. The reactor type may be any of a fixed bed, a fluidized bed, a suspension bed, a spouted bed, a kiln, and a rotary kiln, with a fixed bed flow reactor being preferred. The reaction method may be either a batch method or a flow method, with a flow method being preferred. When the decomposition reactor in the second step is the fixed bed flow reactor, the heat transfer area between the packing and the heated material can be increased, and the reactor size can be reduced.
[0024] The reactor is preferably heated by microwave heating, which employs internal heating to directly heat the microwave heating element packed in the reactor, making it easy to control the heating power, quick temperature response, and uniform heating possible, suppressing repolymerization of decomposition gas due to excessive pyrolysis, and increasing the yield of olefin monomer and its derivative gas.
[0025] In the second step, it is preferable to irradiate microwaves to a microwave heating element packed in a reactor to heat the microwave heating element to 1000°C or higher, and to thermally decompose the crude polyolefin produced in the first step by contacting the microwave heating element.
[0026] The microwave heating element is not particularly limited, but examples thereof include silicon carbide, boron carbide, tungsten carbide, titanium carbide, activated carbon, carbon black, graphite, graphene, mesoporous carbon, carbon nanotubes, carbon fibers, carbon dots, carbon nanowires, soot, and carbides derived from organic matter. Carbon black may be, for example, hard carbon, soft carbon, furnace, channel black, acetylene black, thermal black, Ketjen black, or a combination thereof. The shape of the microwave heating element is not particularly limited, but examples thereof include powder, sphere, pellet, extrusion, ring, and honeycomb. The microwave heating element may be supported or coated on a carrier.
[0027] The particle size of the microwave heating element is not particularly limited, but the lower limit is 0.1 mm, preferably 0.5 mm, and more preferably 1 mm. By having a particle size equal to or greater than the above lower limit, pressure loss and clogging of the reaction tube can be prevented, and the efficiency of microwave heating can be improved by heat storage. In addition, the upper limit of the particle size of the microwave heating element is 100 mm, preferably 75 mm, and more preferably 50 mm. By having a particle size equal to or less than the above upper limit, the surface area can be increased and uniform microwave heating can be achieved.
[0028] The frequency of the microwave irradiated to the reactor in the second step is not particularly limited, but is 300 MHz to 300 GHz, and is preferably 902 MHz to 928 MHz, 2.2 to 2.7 GHz, or 5.55 GHz to 6.05 GHz, which are ISM frequencies according to general industrial standards. The intensity of the microwave may be appropriately controlled by a control unit, and for example, feedback control using the sensing results of temperature, etc. is used.
[0029] The temperature in the reactor when decomposing the polyolefin in the second step is not particularly limited, but the lower limit is 1000°C, preferably 1020°C, and more preferably 1050°C. By having the temperature in the reactor during decomposition be equal to or higher than the above lower limit, high-value-added olefin monomer derivatives such as ethylene, propylene, and especially acetylene can be obtained at a high yield. The upper limit is 1500°C, preferably 1300°C, and more preferably 1200°C. By having the temperature in the reactor during decomposition be equal to or lower than the above upper limit, the by-production of methane due to excessive decomposition of the polyolefin tends to be suppressed, and the monomer yield or selectivity tends to be improved. In addition, the denaturation and sintering of the microwave heating element also tend to be suppressed.
[0030] The temperature during the decomposition is measured by detecting infrared rays emitted from the heated packing when microwaves are irradiated to the microwave heating element packed in the reactor, using a quartz transmission type radiation thermometer (effective wavelength 1.95 μm to 2.6 μm) previously calibrated with a blackbody standard.
[0031] The inert atmosphere through which the polyolefin is decomposed in the second step is not particularly limited, and may be, for example, any of nitrogen, argon, helium, carbon dioxide, and water vapor, or a combination thereof. The inert atmosphere may contain hydrogen and light paraffin gas. The upper limit of the oxygen concentration of the inert atmosphere is 0.5 ppm, preferably 0.1 ppm, and more preferably 0.02 ppm. By keeping the oxygen concentration of the inert atmosphere below the upper limit, thermal runaway due to oxidation of polyolefin, which is an exothermic reaction, is suppressed, and the yield of olefin monomer and its derivative gas is improved.
[0032] "Polyolefin cracking device" Next, a method for decomposing polyolefins using a microwave decomposition apparatus will be described, but the apparatus and the like are not limited to this. Fig. 1 is a schematic diagram showing a polyolefin cracking apparatus used in the multi-stage thermal cracking method of polyolefin according to the present embodiment. Fig. 2 is a schematic diagram showing a reaction vessel constituting the polyolefin cracking apparatus shown in Fig. 1. As shown in FIG. 1, the polyolefin decomposition apparatus 1 includes a polyolefin supply section 10, an electric furnace heating device section 20, a microwave heating device section 30, an electric furnace heating temperature measuring section 40, a microwave heating temperature measuring section 50, a reaction vessel 60, and a control PC 70.
[0033] The polyolefin supply section 10 has an airless feed cock 11, a connector 12, and a Y-shaped tube 13. These components are connected in this order. The connector 12 has a branch tube for introducing an inert gas into the reaction vessel 60 through an introduction tube 91.
[0034] The electric furnace heating device section 20 has an electric furnace 21. The electric furnace heating device section 20 roughly decomposes the polyolefin dropped and introduced from the polyolefin supply section 10 by heating with the electric furnace 21. The electric furnace heating device section 20 is placed vertically so that the hollow section 22 is vertical, and a reaction vessel 60 is placed in the hollow section 22.
[0035] The microwave heating device section 30 has a microwave oscillator 31, a coaxial cable 32, an impedance matcher 33, a coaxial-waveguide converter 34, a resonator 35, a detector 36, and a window 37. These members are arranged in this order, and the resonator 35 is connected to one end (the lower side of the drawing) of the electric furnace 21. The microwave (traveling wave) generated from the microwave oscillator 31 propagates through the coaxial cable 32, and the microwave matched by the impedance matcher 33 propagates through the coaxial-waveguide converter 34 and is introduced into the resonator 35. The microwave (reflected wave) reflected by the reaction vessel 60 or the like and returned to the microwave oscillator 31 side is detected by the power monitor output signal in the microwave oscillator 31. The microwave oscillator 31 is connected to the control PC 71. The resonator 35 has a detector 36 and a radiation thermometer 51. The detector 36 and the radiation thermometer 51 are connected to a control PC 71 and measure the resonance frequency of the workpiece and the internal temperature of the reaction vessel 60 . The resonator 35 is also provided with a window 37 for observing the reaction vessel 60 inserted in the resonator 35 .
[0036] The electric furnace heating temperature measuring section 40 has a thermocouple 41, a temperature regulator 42, and a data logger 43. The internal temperature of the electric furnace heating device section 20 is measured by the thermocouple 41, the temperature is controlled by the temperature regulator 42, and the measurement data is recorded by the data logger 43.
[0037] The microwave heating temperature measuring unit 50 has a radiation thermometer 51. The radiation thermometer 51 is disposed in the window 37. The radiation thermometer 51 is also connected to the control PC 71.
[0038] The reaction vessel 60 has a cylindrical shape. As shown in Fig. 2, the reaction vessel 60 accommodates a filler 101 at the upper part in the longitudinal direction and a microwave heating element 102 at the lower part. The reaction vessel 60 also accommodates glass wool 103 so as to contact the lower end of the filler 101 in the longitudinal direction of the reaction vessel 60, and the glass wool 103 is accommodated so as to contact the lower end of the microwave heating element 102 in the longitudinal direction of the reaction vessel 60.
[0039] The reaction vessel 60 is disposed in the electric furnace heating device section 20 and the resonator 35. In detail, the reaction vessel 60 is inserted into a through hole penetrating the electric furnace heating device section 20, and the center of the filler 101 is disposed in the center of the electric furnace heating device section 20. The resonator 35 is provided with a window 37 for observing the reaction vessel 60 inserted in the resonator 35. The center of the filler 101 is disposed relative to the center of the resonator 35 so that the microwave heating element 102 faces the window 37. The reaction vessel 60 is connected to one end 61 (upper side of the drawing) with a Y-shaped tube 13, a connector 12, and an airless feed cock 11. The connector 12 is connected to an inlet pipe 91 for introducing nitrogen gas into the reaction vessel 60. The reaction vessel 60 is connected to the other end 62 (lower side of the drawing) with an outlet pipe 92 for discharging decomposition gas from the reaction vessel 60. A gas bag is connected to the end of the discharge pipe 92 opposite to the reaction vessel 60 .
[0040] To thermally decompose polyolefins using the polyolefin decomposition apparatus 1, first, filler 101 and glass wool 103 are placed in the upper part of reaction vessel 60 and fixed to the upper part of reaction vessel 60. In addition, microwave heating element 102 and glass wool 103 are placed in the lower part of reaction vessel 60 and fixed to the lower part of reaction vessel 60.
[0041] Next, the reaction vessel 60 containing the filler 101 and the microwave heating element 102 is arranged so as to pass through the electric furnace heating device section 20 and the resonator 35. At this time, the reaction vessel 60 is fixed so that the center of the filler 101 is arranged at the center of the electric furnace heating device section 20, and the center of the microwave heating element 102 is arranged at the center of the resonator 35 where the electric field is maximum.
[0042] Next, a polyolefin supply unit 10, which is connected to an airless feed cock 11 containing polyolefin under a nitrogen atmosphere, a connector 12, and a Y-shaped tube 13, is connected to one end 61 (upper side of the paper surface) of a reaction vessel 60. At this time, a thermocouple 41 is fixed so that the thermocouple 41 is located from the Y-shaped tube 13 to the center of the upper filler 101 in the reaction vessel 60.
[0043] Next, nitrogen gas is started to flow from the inlet tube 91 through the connector 12 into the reaction vessel 60, and the reaction vessel 60 is left in this state for several minutes to create a nitrogen atmosphere inside the reaction vessel 60. Next, a gas bag is connected to the end of the discharge pipe 92 opposite to the reaction vessel 60 . Next, under nitrogen flow, the electric furnace heating device section 20 and the temperature regulator 42 are started, and the filler 101 in the reaction vessel 60 is heated with a predetermined temperature control until a predetermined temperature is reached and the temperature is left to stand for several minutes until it becomes constant.
[0044] Next, the microwave oscillator 31 is started under nitrogen flow, and while irradiating microwaves to the microwave heating element 102 in the reaction vessel 60 with a predetermined temperature control, the impedance matching device 33 is adjusted so that the difference between the forward wave and the reflected wave is maximized. When microwaves are irradiated to the microwave heating element 102, the microwave heating element 102 generates heat and reaches a predetermined temperature, and is left to stand for several minutes until the temperature becomes constant.
[0045] Next, the airless feed cock 11 is rotated to intermittently feed the polyolefin thereinto, thereby pyrolyzing the polyolefin. The cracked gas generated by the thermal decomposition of the polyolefin is discharged to the outside of the reaction vessel 60 through the exhaust pipe 92 and collected in a gas bag. The recovered cracked gas contains olefin monomers, olefin monomer derivatives, paraffins including methane, and hydrogen.
[0046] According to the multi-stage pyrolysis method of polyolefins of the present invention, it is possible to provide a pyrolysis method capable of obtaining, with high yields, olefin monomers in the pyrolysis of polyolefins, such as ethylene and propylene, and particularly high-value-added olefin monomer derivatives such as acetylene, etc. In addition, by using microwave heating that is energy-saving and has good temperature responsiveness, it is possible to provide a pyrolysis method suitable for raw material changes and supply-demand balance in a compact fixed-bed reactor. EXAMPLES
[0047] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0048] [Example 1] As the polyolefin decomposition device, a device was used in which a single-mode microwave heating device (manufactured by Ryowa Electronics, MR-2G-100, excitation frequency 2.4 GHz to 2.5 GHz, cylindrical TM010 mode) was connected to a ceramic electric tubular furnace (manufactured by Asahi Rika Seisakusho, ARF-16KC) as shown in FIG. 1. A quartz tube (tube length 40 cm, inner diameter 8 mm) was used as the reaction vessel. 0.982 g of Dixon packing (manufactured by Tohto Enji Co., Ltd.) was put into the reaction vessel as a filler for the electric tubular furnace part, glass wool was packed under the filler, and the filler was accommodated in the reaction vessel. In addition, 0.604 g of silicon carbide (manufactured by Tohto Enji Co., Ltd., carborundum 16 mesh) as a microwave heating element was put in, glass wool was packed under the filler, and the filler was accommodated in the reaction vessel. The reaction vessels were fixed in the electric tubular furnace and the microwave heating device in positions where the contents were centered. The top of the reaction vessel was connected to a Y-shaped connecting tube, a thermocouple was inserted from one side to a position half the depth of the Dixon packing filling, and an airless feed cock (manufactured by Asahi Seisakusho Co., Ltd.) containing 0.5089 g of high-density polyethylene (manufactured by Sigma-Aldrich Co., Ltd.) under nitrogen was connected to the other side. Nitrogen (G3 standard, oxygen concentration 0.5 volppm) was circulated into the reaction vessel from the blowing tube at the top of the reaction vessel at a flow rate of 20 mL / min, and the vessel was left to stand for 5 minutes in that state, creating a nitrogen atmosphere inside the reaction vessel. A gas bag was connected to the bottom of the reaction vessel. Under the nitrogen flow, the electric tubular furnace was heated to 600°C, the microwave oscillator was started, and the double slug was adjusted to maximize the difference between the forward wave and the reflected wave. The temperature of the microwave absorber inside the reaction vessel was measured with a quartz transmission type radiation thermometer (model name: FLHX-TNE0220, manufactured by Japan Sensor Co., Ltd.) and stabilized at the set value of 1000°C by feedback control. The temperature adjustment end time of the electric tube furnace and the microwave heating device was set as the reaction start time. The cock of the airless feed cock was rotated, and polyethylene pellets were charged into the reaction vessel at 15 mg to 30 mg per minute for a total of 15 minutes of reaction. The decomposition gas of the polyolefin was recovered into the gas bag. The internal temperature of the electric tube furnace during the reaction was 600 °C, and the temperature of the microwave absorber was 1000 °C. The yield of the obtained decomposition gas was 63%. Regarding the gas components, gas chromatography measurement was performed under the following conditions, and the amounts of acetylene, ethylene, ethane, propylene, propane, and methane were quantified. As a result, the acetylene selectivity was 15.2%, the ethylene selectivity was 43.6%, the ethane selectivity was 1.2%, the propylene selectivity was 6.9%, the propane selectivity was 0.3%, and the methane selectivity was 32.6%. From the results, when calculating the (acetylene + ethylene) / ethane ratio, it was 50.8. Regarding the crude decomposition product obtained in the first step, when measuring the maximum molecular weight by LDI-MS under the following conditions, it was 698.
[0049] <GC measurement> Gas chromatograph: GC-2014 (model name), manufactured by Shimadzu Corporation Column: ShincarbonST 50 / 80 (1.0 m · 3 mm, manufactured by Shinwa Chemical Industries Co., Ltd.) Column oven temperature: 40 °C Mobile phase: He 30 mL / min Analysis time: 30 min Detection: TCD detector Sample: 1 mL injection <LDI-MS measurement> Laser desorption ionization time-of-flight mass spectrometer: JMS-S3000 (model name), manufactured by JEOL Ltd. Laser: Nd:YLF laser (349 nm) Intensity: 53% Delay Time: 300 nsec Detector: 70 Ion convergence mode: spiral mode Detected ions: positive ion detection Scanning mass range: 50 to 5000 (m / z) Matrix: None
[0050] [Example 2] As the polyolefin decomposition device, a device was used in which a single-mode microwave heating device (manufactured by Ryowa Electronics, MR-2G-100, excitation frequency 2.4 GHz to 2.5 GHz, cylindrical TM010 mode) was connected to a ceramic electric tubular furnace (manufactured by Asahi Rika Seisakusho, ARF-16KC) as shown in FIG. 1. A quartz tube (tube length 40 cm, inner diameter 8 mm) was used as the reaction vessel. 0.986 g of Dixon packing (manufactured by Tohto Enji Co., Ltd.) was put into the reaction vessel as a filler for the electric tubular furnace part, glass wool was packed under the filler, and the filler was accommodated in the reaction vessel. In addition, 0.5097 g of silicon carbide (manufactured by Tohto Chemical Co., Ltd., carborundum 16 mesh) as a microwave heating element was put in, glass wool was packed under the filler, and the filler was accommodated in the reaction vessel. The reaction vessels were fixed in the electric tubular furnace and the microwave heating device in positions where the contents were centered. The top of the reaction vessel was connected to a Y-shaped connecting tube, a thermocouple was inserted from one side to a position half the depth of the Dixon packing filling, and an airless feed cock (manufactured by Asahi Seisakusho Co., Ltd.) containing 0.5075 g of high density polyethylene (manufactured by Sigma-Aldrich Co., Ltd.) under nitrogen was connected to the other side. Nitrogen (G3 standard, oxygen concentration 0.5 volppm) was circulated into the reaction vessel from the blowing tube at the top of the reaction vessel at a flow rate of 20 mL / min, and the vessel was left to stand for 5 minutes in that state, creating a nitrogen atmosphere inside the reaction vessel. A gas bag was connected to the bottom of the reaction vessel. Under the above nitrogen flow, the electric tubular furnace was heated to 450°C, the microwave oscillator was started, and the double slug was adjusted to maximize the difference between the forward wave and the reflected wave. The temperature of the microwave absorber inside the reaction vessel was measured with a quartz transmission type radiation thermometer (model name: FLHX-TNE0220, manufactured by Japan Sensor Co., Ltd.) and stabilized at the set value of 1200°C by feedback control. The reaction started when the temperature adjustment of the electric tubular furnace and microwave heating device was completed, and the airless feed cock was rotated to feed 15 mg to 30 mg of polyethylene pellets into the reaction vessel every minute. The reaction was carried out for a total of 30 minutes, and the decomposition gas of the polyolefin was collected in a gas bag. The internal temperature of the electric tubular furnace during the reaction was 450°C, and the temperature of the microwave absorber was 1200°C. The yield of the cracked gas obtained was 56%. In addition, gas components were measured by gas chromatography in the same manner as in Example 1 to quantify the amounts of acetylene, ethylene, ethane, propylene, propane and methane, and the acetylene selectivity was 18.8%, the ethylene selectivity was 45.4%, the ethane selectivity was 1.6%, the propylene selectivity was 8.2%, the propane selectivity was 0.3%, and the methane selectivity was 24.1%. From the results, the (acetylene + ethylene) / ethane ratio was calculated to be 39.6. In addition, the crude hydrolyzate obtained in the first step was subjected to LDI-MS measurement in the same manner as in Example 1, and the maximum molecular weight was found to be 726.
[0051] [Example 3] As the polyolefin decomposition device, a device was used in which a single-mode microwave heating device (manufactured by Ryowa Electronics, MR-2G-100, excitation frequency 2.4 GHz to 2.5 GHz, cylindrical TM010 mode) was connected to a ceramic electric tubular furnace (manufactured by Asahi Rika Seisakusho, ARF-16KC) as shown in FIG. 1. A quartz tube (tube length 40 cm, inner diameter 8 mm) was used as the reaction vessel. 0.999 g of Dixon packing (manufactured by Tohto Enji Co., Ltd.) was put into the reaction vessel as a filler for the electric tubular furnace part, glass wool was packed under the filler, and the filler was accommodated in the reaction vessel. In addition, 0.5278 g of silicon carbide (manufactured by Tohto Enji Co., Ltd., carborundum 16 mesh) as a microwave heating element was put in, glass wool was packed under the filler, and the filler was accommodated in the reaction vessel. The reaction vessels were fixed in the electric tubular furnace and the microwave heating device in positions where the contents were centered. The top of the reaction vessel was connected to a Y-shaped connecting tube, a thermocouple was inserted from one side to a position half the depth of the Dixon packing filling, and an airless feed cock (manufactured by Asahi Seisakusho Co., Ltd.) containing 0.5014 g of polypropylene (manufactured by Sigma-Aldrich Co., Ltd.) under nitrogen was connected to the other side. Nitrogen (G3 standard, oxygen concentration 0.5 volppm) was circulated into the reaction vessel from the blowing tube at the top of the reaction vessel at a flow rate of 20 mL / min, and the vessel was left to stand for 5 minutes in that state, creating a nitrogen atmosphere inside the reaction vessel. A gas bag was connected to the bottom of the reaction vessel. Under the above nitrogen flow, the electric tubular furnace was heated to 450°C, the microwave oscillator was started, and the double slug was adjusted to maximize the difference between the forward wave and the reflected wave. The temperature of the microwave absorber inside the reaction vessel was measured with a quartz transmission type radiation thermometer (model name: FLHX-TNE0220, manufactured by Japan Sensor Co., Ltd.) and stabilized at the set value of 1200°C by feedback control. The reaction started when the temperature adjustment of the electric tubular furnace and microwave heating device was completed, and the airless feed cock was rotated to feed 15 mg to 30 mg of polyethylene pellets into the reaction vessel every minute. The reaction was carried out for a total of 30 minutes, and the decomposition gas of the polyolefin was collected in a gas bag. The internal temperature of the electric tubular furnace during the reaction was 450°C, and the temperature of the microwave absorber was 1200°C. The yield of the cracked gas obtained was 86%. In addition, gas components were measured by gas chromatography in the same manner as in Example 1 to quantify the amounts of acetylene, ethylene, ethane, propylene, propane and methane, and the acetylene selectivity was 12.8%, the ethylene selectivity was 33.3%, the ethane selectivity was 2.4%, the propylene selectivity was 17.3%, the propane selectivity was 0.3%, and the methane selectivity was 31.4%. From the results, the (acetylene + ethylene) / ethane ratio was calculated to be 19.1.
[0052] [Comparative Example 1] As the polyolefin decomposition device, a device was used in which a single-mode microwave heating device (manufactured by Ryowa Electronics, MR-2G-100, excitation frequency 2.4 GHz to 2.5 GHz, cylindrical TM010 mode) was connected to a ceramic electric tubular furnace (manufactured by Asahi Rika Seisakusho, ARF-16KC) as shown in FIG. 1. A quartz tube (tube length 40 cm, inner diameter 8 mm) was used as the reaction vessel. 0.964 g of Dixon packing (manufactured by Tohto Enji Co., Ltd.) was put into the reaction vessel as a filler for the electric tubular furnace part, glass wool was packed under the filler, and the filler was accommodated in the reaction vessel. In addition, 0.602 g of silicon carbide (manufactured by Tohto Chemical Co., Ltd., carborundum 16 mesh) as a microwave heating element was put in, glass wool was packed under the filler, and the filler was accommodated in the reaction vessel. The reaction vessels were fixed in the electric tubular furnace and the microwave heating device in positions where the contents were centered. The top of the reaction vessel was connected to a Y-shaped connecting tube, a thermocouple was inserted from one side to a position half the depth of the Dixon packing filling, and an airless feed cock (manufactured by Asahi Seisakusho Co., Ltd.) containing 0.5058 g of high-density polyethylene (manufactured by Sigma-Aldrich Co., Ltd.) under nitrogen was connected to the other side. Nitrogen (G3 standard, oxygen concentration 0.5 volppm) was circulated into the reaction vessel from the blowing tube at the top of the reaction vessel at a flow rate of 20 mL / min, and the vessel was left to stand for 5 minutes in that state, creating a nitrogen atmosphere inside the reaction vessel. A gas bag was connected to the bottom of the reaction vessel. Under the above nitrogen flow, the electric tubular furnace was heated to 600°C, the microwave oscillator was started, and the double slug was adjusted to maximize the difference between the forward wave and the reflected wave. The temperature of the microwave absorber inside the reaction vessel was measured with a quartz transmission type radiation thermometer (model name: FLHX-TNE0220, manufactured by Japan Sensor Co., Ltd.) and stabilized at the set value of 900°C by feedback control. The reaction started when the temperature adjustment of the electric tubular furnace and microwave heating device was completed, and the airless feed cock was rotated to feed 15 mg to 30 mg of polyethylene pellets into the reaction vessel every minute. The reaction was carried out for a total of 15 minutes, and the decomposition gas of the polyolefin was collected in a gas bag. The internal temperature of the electric tubular furnace during the reaction was 600°C, and the temperature of the microwave absorber was 900°C. The yield of the cracked gas obtained was 61%. In addition, gas components were measured by gas chromatography in the same manner as in Example 1 to quantify the amounts of acetylene, ethylene, ethane, propylene, propane and methane, and the acetylene selectivity was 0.4%, the ethylene selectivity was 49.6%, the ethane selectivity was 7.0%, the propylene selectivity was 17.4%, the propane selectivity was 1.4%, and the methane selectivity was 22.2%. From the results, the (acetylene + ethylene) / ethane ratio was calculated to be 7.2.
[0053] [Comparative Example 2] As the polyolefin decomposition device, a device was used in which a single-mode microwave heating device (manufactured by Ryowa Electronics, MR-2G-100, excitation frequency 2.4 GHz to 2.5 GHz, cylindrical TM010 mode) was connected to a ceramic electric tubular furnace (manufactured by Asahi Rika Seisakusho, ARF-16KC) as shown in FIG. 1. A quartz tube (tube length 40 cm, inner diameter 8 mm) was used as the reaction vessel. 0.988 g of Dixon packing (manufactured by Tohto Enji Co., Ltd.) was put into the reaction vessel as a filler for the electric tubular furnace part, glass wool was packed under the filler, and the filler was accommodated in the reaction vessel. In addition, 2.0177 g of silicon carbide (manufactured by Tohto Enji Co., Ltd., carborundum 16 mesh) as a microwave heating element was put in, glass wool was packed under the filler, and the filler was accommodated in the reaction vessel. The reaction vessels were fixed in the electric tubular furnace and the microwave heating device in positions where the contents were centered. The top of the reaction vessel was connected to a Y-shaped connecting tube, a thermocouple was inserted from one side to a position half the depth of the Dixon packing filling, and an airless feed cock (manufactured by Asahi Seisakusho Co., Ltd.) containing 0.5090 g of polypropylene (manufactured by Sigma-Aldrich Co., Ltd.) under nitrogen was connected to the other side. Nitrogen (G3 standard, oxygen concentration 0.5 volppm) was circulated into the reaction vessel from the blowing tube at the top of the reaction vessel at a flow rate of 20 mL / min, and the vessel was left to stand in that state for 5 minutes, creating a nitrogen atmosphere inside the reaction vessel. A gas bag was connected to the bottom of the reaction vessel. Under the above nitrogen flow, the electric tubular furnace was heated to 620°C, the microwave oscillator was started, and the double slug was adjusted to maximize the difference between the forward wave and the reflected wave. The temperature of the microwave absorber inside the reaction vessel was measured with a quartz transmission type radiation thermometer (model name: FLHX-TNE0220, manufactured by Japan Sensor Co., Ltd.) and stabilized at the set value of 950°C by feedback control. The reaction started when the temperature adjustment of the electric tubular furnace and microwave heating device was completed, and the airless feed cock was rotated to feed 15 mg to 30 mg of polyethylene pellets into the reaction vessel every minute. The reaction was carried out for a total of 15 minutes, and the decomposition gas of the polyolefin was collected in a gas bag. The internal temperature of the electric tubular furnace during the reaction was 620°C, and the temperature of the microwave absorber was 950°C. The yield of the cracked gas obtained was 98%. In addition, gas components were measured by gas chromatography under the following conditions, and the amounts of acetylene, ethylene, ethane, propylene, propane and methane were quantified, giving acetylene selectivity of 0.2%, ethylene selectivity of 21.0%, ethane selectivity of 10.3%, propylene selectivity of 40.0%, propane selectivity of 1.5%, and methane selectivity of 22.7%. From the results, the (acetylene + ethylene) / ethane ratio was calculated to be 2.1.
[0054] The results of Examples 1 to 3 and Comparative Examples 1 and 2 are shown in Table 1.
[0055] [Table 1]
[0056] From the results shown in Table 1, it was found that Examples 1 to 3 were excellent in yield of ethylene, which is a chemically recyclable olefin monomer, and high-value-added acetylene. It was also found that polyolefin decomposition was possible in a compact reactor using a fixed-bed flow reactor in the second step. [Industrial Applicability]
[0057] The multi-stage pyrolysis method for polyolefins of the present invention is extremely useful as a method for recycling polyolefins, since it provides a high yield of decomposition gases of chemically recyclable olefin monomers and their derivatives and has excellent selectivity for the (acetylene+ethylene) / ethane ratio. [Explanation of symbols]
[0058] 1 Polyolefin cracking equipment 10 Polyolefin Supply Section 20 Electric Furnace Heating Equipment Section 30 Microwave Heating Device Section 40 Electric furnace heating temperature measuring section 50 Microwave heating temperature measuring section 60 Reaction vessel 70 Control PC
Claims
1. A process for pyrolyzing polyolefins, comprising the steps of: A first step of roughly decomposing a polyolefin by heating; A second step of decomposing the crude decomposition product obtained in the first step by heating at 1000° C. or higher.
2. 2. The multi-stage pyrolysis process for polyolefins according to claim 1, wherein the polyolefin comprises at least one of polyethylene and polypropylene.
3. 2. The method for multi-stage pyrolysis of polyolefins according to claim 1, wherein the polyolefins are heated in a stream of inert gas having an oxygen concentration of 0.5 ppm or less.
4. The method for multi-stage pyrolysis of polyolefins according to claim 1 , wherein the heating in the first step includes a region of 400° C. or more and 700° C. or less.
5. 2. The method for multi-stage pyrolysis of polyolefins according to claim 1, wherein the heating in the second step is microwave heating.
6. 6. The method for multi-stage pyrolysis of polyolefins according to claim 5, wherein the microwave heating is carried out in a fixed bed reactor packed with a microwave absorber.
Citation Information
Patent Citations
Thermal cracking process for selective production of olefin and aromatic hydrocarbon from hydrocarbon
JP1985001138A
Olefin production method
JP1994507647A
Method and apparatus for plastic thermal decomposition
JP2005220179A
Ultraviolet ray chemical reaction apparatus
JP2012040458A
Processing apparatus and method
JP2014503610A
Cited By
Olefin production method and implementation step
WO2026204851A1