Zirconia powder for laser sintering, and method for producing zirconia sintered body by laser sintering

A zirconia powder with transition metal and rare earth elements facilitates laser sintering without alumina, achieving a dense zirconia sintered body with improved density and uniformity.

JP2024136187APending Publication Date: 2024-10-04TOSOH CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023047213
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing laser sintering methods for zirconia require the presence of alumina, which makes it difficult to achieve sintering without alumina intervention, and zirconia is less likely to sinter compared to alumina, limiting the production of a zirconia sintered body.

Method used

A zirconia powder containing transition metal elements and rare earth elements, with a controlled color tone, is used for laser sintering, allowing sintering without alumina intervention, resulting in a dense zirconia sintered body.

Benefits of technology

The zirconia powder enables uniform sintering of zirconia by laser irradiation, producing a dense zirconia sintered body with high actual density, surpassing conventional methods in terms of density and structural uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136187000001_ABST
    Figure 2024136187000001_ABST
Patent Text Reader

Abstract

To provide at least any one of novel zirconia powder for laser sintering by which sintering of zirconia by laser sintering is made possible without interposing alumina, particularly, novel zirconia powder for laser sintering by which a dense sintered body of zirconia is obtained by irradiating laser, and a method for producing a sintered body by laser sintering by using the powder.SOLUTION: Zirconia powder for laser sintering contains a compound containing at least either one of a transition metal element and a rare earth element, and zirconia, and furthermore, lightness value L* in L*a*b* color system is 90 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a zirconia powder for laser sintering and a method for producing a zirconia sintered body by laser sintering. [Background technology]

[0002] A method of sintering ceramics by irradiating them with a laser, known as laser sintering, is being investigated.

[0003] For example, Patent Document 1 discloses that a structure with high smoothness on the surface and sides can be obtained by sintering inorganic powder containing various absorbents on an alumina base material with a laser.

[0004] Furthermore, Patent Document 2 discloses laser sintering in which a mixed powder consisting of black yttria powder and aluminum oxide or aluminum nitride powder is molded and irradiated with a laser to form a sintered body. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-100141 A [Patent Document 2] International Publication No. 2021 / 172128 Summary of the Invention [Problem to be solved by the invention]

[0006] The laser sintering described in Patent Document 1 and Patent Document 2 is a sintering method in which an alumina eutectic and alumina are sintered by a laser, and both sintering methods require the inclusion of alumina. In contrast, zirconia, which is also an inorganic oxide, is more difficult to sinter than alumina. Thus, it has not been reported that a zirconia sintered body can be obtained by laser sintering without the inclusion of alumina.

[0007] In view of these problems, the present disclosure aims to provide at least one of a novel zirconia powder for laser sintering that enables sintering of zirconia by laser sintering without the intervention of alumina, in particular a novel zirconia powder for laser sintering that can produce a dense zirconia sintered body by irradiating it with a laser, and a method for producing a sintered body by laser sintering using the same. [Means for solving the problem]

[0008] The present inventors have investigated the sintering of zirconia by laser sintering, and have found that by controlling the color tone, laser sintering of zirconia can proceed without the intervention of alumina.

[0009] That is, the present invention is as described in the claims, and the gist of the present disclosure is as follows.

[0010] [1] A compound containing at least one of a transition metal element and a rare earth element, and zirconia, and L * a * b * Lightness L in color system * Zirconia powder for laser sintering, having a molecular weight of 90 or less. [2] The compound is an oxide containing one or more elements selected from the group consisting of Co, Fe, Mn, V, Mo, Cu, Ni, Pr, Nd, Er, Gd, Tb and Sc. The zirconia powder for laser sintering according to [1] above. [3] The zirconia powder for laser sintering according to the above [1] or [2], wherein the content of the compound relative to the mass of the zirconia powder for laser sintering is 0.5 mass% or more and 10 mass% or less, calculated as an oxide. [4] The zirconia powder for laser sintering according to any one of [1] to [3] above, wherein the zirconia is zirconia containing a stabilizing element. [5] The zirconia powder for laser sintering according to the above [4], wherein the stabilizing element is one or more selected from the group consisting of calcium, magnesium and yttrium. [6] A method for producing a sintered body, comprising the step of irradiating a molded body containing the zirconia powder for laser sintering described in any one of [1] to [5] above with laser light to obtain a sintered body. Effect of the Invention

[0011] The present disclosure makes it possible to provide at least one of a novel zirconia powder for laser sintering that enables sintering of zirconia by laser sintering without the intervention of alumina, in particular a novel zirconia powder for laser sintering that can give a dense zirconia sintered body by irradiating it with a laser, and a method for producing a sintered body by laser sintering using the same. [Brief description of the drawings]

[0012] [Figure 1] FIG. 13 is a scanning electron microscope (SEM) image of the surface of the zirconia sintered body of Example 7 containing a transition metal compound and irradiated with a laser. [Diagram 2] FIG. 13 is a diagram showing a scanning electron microscope image of a cross section of a surface layer portion near a surface irradiated with a laser in a zirconia sintered body of Example 7 containing a transition metal compound or the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In this specification, a numerical range indicated using "~" indicates a range that includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively.

[0014] A "powder" is an aggregate of powder particles (at least one of primary particles and secondary particles) and is a composition having flowability. A "zirconia powder" is a powder whose main component is zirconia, and is essentially a powder consisting of zirconia. In this specification, the individual particles that make up the aggregate "powder" are called "powder particles" to distinguish them from the aggregate "powder."

[0015] A "molded body" is a composition having a certain shape composed of powder particles aggregated by physical force, and in particular, a composition in a state in which no heat treatment has been performed after the shape has been imparted (e.g., after molding). For example, a "molded body" can be obtained by agglomerating the "powder" by physical force and imparting a certain shape. A "zirconia molded body" is a molded body whose main component is zirconia, and is essentially made of zirconia. The term "molded body" is also used interchangeably with "powder compact."

[0016] A "sintered body" is a composition having a certain shape composed of crystal grains, and is a composition in a state in which it has been heat-treated at a temperature equal to or higher than the sintering temperature. For example, the "molded body" can be made into a "sintered body" by heat-treating it at a temperature equal to or higher than the sintering temperature. A "zirconia sintered body" is a sintered body whose main component is zirconia, and is essentially a sintered body made of zirconia.

[0017] A "major component" refers to a component that becomes the main phase (matrix, base material, parent phase) in the composition of the composition, and preferably a component that accounts for a mass proportion of the composition of 60 mass% or more, 75 mass% or more, 85 mass% or more, 90 mass% or more, 95 mass% or more, 98 mass% or more, or 99 mass% or more, or less than 100 mass%.

[0018] "Consisting essentially of component X" or "consisting substantially of component X" means that the mass ratio of component X in the composition is 98 mass% or more, 99 mass% or more, or 99.5 mass% or more, and is less than 100 mass%. "Consisting essentially of component X" or "consisting substantially of component X" can also be expressed as "consisting essentially only of component X" or "consisting substantially only of component X".

[0019] The term "stabilizing element" refers to an element that stabilizes the crystal phase of zirconia by dissolving in the zirconia.

[0020] "BET specific surface area" is the specific surface area [m2] measured by the BET multipoint method (5 points) using nitrogen as the adsorption gas in accordance with JIS R 1626:1996. 2 / g], in particular the BET specific surface area measured under the following conditions:

[0021] Adsorption medium: N2 Adsorption temperature: -196℃ Pretreatment conditions: Degassing in air at 250℃ for 1 hour or more The BET specific surface area can be measured using a general specific surface area measuring device (for example, Tristar II 320, manufactured by Shimadzu Corporation).

[0022] "Color tone (L * , a * , b * )" and "Saturation (C * ) can be obtained using a spectrophotometer (e.g. Spectrophotometer SD 3000, manufactured by Nippon Denshoku Industries Co., Ltd.) equipped with an illumination and light receiving optical system conforming to the geometric condition c of JIS Z 8722:2009, and using values ​​measured by the SCE method. Specific measurement conditions for color tone are as follows, using a white plate as the background (so-called white back measurement).

[0023] Light source: D65 light source Viewing angle: 10° Measurement method: SCE Lightness L * is an index of brightness and has a value between 0 and 100. * and b * is an index of color tone and has a value between -100 and 100. * is an index of vividness, and hue a * and b * From C * ={(a * ) 2 +(b * ) 2} 0.5 It is calculated by:

[0024] In this embodiment, the color tone of the powder may be measured by sieving the powder through a sieve with an opening of 500 μm, uniaxially pressing the powder at 50 MPa to form a disk-shaped molded body with a diameter of 12 mm and a thickness of 1±0.5 mm, and measuring the color tone of the surface of the molded body. Note that the "diameter" is the diameter of the circumscribing circle of the disk shape, and is a value that can be measured with a vernier caliper or the like.

[0025] "Measured density" is the density of the sample [cm 3 ] and the value [g / cm 3 The mass was determined by weighing the sample. The volume was determined by the Archimedes method according to JIS R 1634:1998. The Archimedes method used ion-exchanged water as the solvent, and the pretreatment was performed by boiling.

[0026] <Zirconia powder for laser sintering> Hereinafter, the zirconia powder for laser sintering of the present disclosure will be described with reference to an example of an embodiment. The present embodiment includes a compound containing at least one of a transition metal element and a rare earth element, and zirconia, and further includes L * a * b * Lightness L in color system * A zirconia powder for laser sintering, having a molecular weight of 90 or less.

[0027] The zirconia powder for laser sintering of the present embodiment is a zirconia powder that can be sintered by laser irradiation without the intermediation of alumina, and in particular has a lightness L * and saturation C * In this respect, the zirconia powder exhibits a color other than the color that zirconia (ZrO2) originally has. In other words, the zirconia powder for laser sintering of the present embodiment is a zirconia powder having a color tone that can absorb laser light.

[0028] As described above, the zirconia powder for laser sintering of this embodiment is a new zirconia powder for laser sintering that enables sintering of zirconia by laser sintering without the intervention of alumina, and in particular is a new zirconia powder for laser sintering that can obtain a dense zirconia sintered body by irradiating a laser. Since sintering of zirconia by laser irradiation proceeds more uniformly regardless of a decrease in the sintering temperature due to a eutectic such as alumina, it is preferable that the zirconia powder for laser sintering of this embodiment does not contain alumina.

[0029] By laser sintering the zirconia powder for laser sintering of this embodiment, a sintered body having a thickness of, for example, 1.0±0.5 mm can be obtained, in which the surface layer and the deep layer in the thickness direction are sintered uniformly and densely. The measured density of the zirconia sintered body obtained by laser sintering the zirconia powder for laser sintering of this embodiment is higher than that of a conventional zirconia sintered body obtained by laser sintering, and is, for example, 4.00 g / cm 3 Above 5.00g / cm 3 , or even 5.40g / cm 3 This is because the relative density (true density) is 6.05 g / cm 3 This corresponds to 70% or more, more preferably 80% or more, and further 90% or more as the relative density. The relative density is 100% or less.

[0030] (Zirconia) The zirconia powder for laser sintering of this embodiment contains zirconia. The zirconia is preferably zirconia containing a stabilizing element. The zirconia containing a stabilizing element is more preferably zirconia containing one or more selected from the group consisting of calcium (Ca), magnesium (Mg) and yttrium (Y), and is even more preferably zirconia containing yttrium. The stabilizing element only needs to have a function of stabilizing the crystal structure of zirconia, and does not have to substantially contribute to increasing the laser absorption efficiency in the zirconia powder for laser sintering.

[0031] The zirconia powder for laser sintering of the present embodiment contains zirconia in the form of a powder.

[0032] The content of zirconia in the zirconia powder for laser sintering of this embodiment is appropriately set according to the content of the compound containing at least one of a transition metal element and a rare earth element. The content of zirconia relative to the mass of the zirconia powder for laser sintering is preferably 60 mass% or more and 99.5 mass% or less, 90 mass% or more and 99.5 mass% or less, 70 mass% or more and 99 mass% or less, or 90 mass% or more and 98 mass% or less. This makes it possible to obtain a zirconia powder for laser sintering containing zirconia as the main component.

[0033] The content of the stabilizing element contained in the zirconia powder for laser sintering of this embodiment is any within a range that stabilizes the crystal structure of zirconia so that cubic or tetragonal crystals become the main phase. For example, the content of the stabilizing element calculated as an oxide relative to the zirconia and the stabilizing element calculated as an oxide contained in the zirconia powder for laser sintering of this embodiment can be 2 mol% or more or 2.5 mol% or more, and 8 mol% or less, 7 mol% or less, or 4.5 mol% or less.

[0034] When performing calculations based on the composition, such as calculating the content of stabilizing elements, hafnia, which is an inevitable impurity of zirconia, may be calculated by regarding it as zirconia.

[0035] The zirconia powder for laser sintering of the present embodiment may contain one type of zirconia alone, or may contain two or more types of zirconia in combination at any ratio.

[0036] (Transition metal elements, etc.) The zirconia powder for laser sintering of this embodiment contains a compound containing at least one of a transition metal element and a rare earth element (hereinafter also referred to as "transition metal element, etc."). By containing a compound containing a transition metal element, etc., the zirconia powder for laser sintering of this embodiment has a color tone that can absorb laser light, so it is thought that sintering of zirconia by laser irradiation proceeds more uniformly regardless of a decrease in sintering temperature due to a eutectic such as alumina.

[0037] The compound containing a transition metal element or the like (hereinafter also referred to as a "transition metal compound") may be at least either an organic compound or an inorganic compound, and examples thereof include one or more compounds selected from the group consisting of organometallic complexes, organic acid metal salts, metal alkoxides, halides, nitrates, sulfates, phosphates, carbonates, hydroxides, oxyhydroxides, and oxides. The transition metal compound is preferably an oxide containing a transition metal element or the like, more preferably an oxide containing one or more elements selected from the group consisting of cobalt (Co), iron (Fe), manganese (Mn), vanadium (V), molybdenum (Mo), copper (Cu), nickel (Ni), praseodymium (Pr), neodymium (Nd), erbium (Er), gadolinium (Gd), terbium (Tb) and scandium (Sc), still more preferably an oxide containing one or more elements selected from the group consisting of cobalt, iron, manganese, vanadium, molybdenum, copper and nickel, still more preferably an oxide containing one or more elements selected from the group consisting of iron, cobalt, manganese and nickel, and particularly preferably one or more elements selected from the group consisting of iron oxide, cobalt oxide, manganese oxide and nickel oxide.

[0038] The zirconia powder for laser sintering of the present embodiment may contain one type of transition metal compound alone, or may contain two or more types of transition metal compounds in combination at any ratio.

[0039] The zirconia powder for laser sintering of the present embodiment contains a compound of a transition metal or the like in the form of a powder.

[0040] The content of the transition metal compound in the zirconia powder for laser sintering of this embodiment is the lightness L * is an arbitrary amount as long as it shows a desired value. The content of the transition metal compound, etc., calculated as an oxide relative to the mass of the zirconia powder for laser sintering is preferably 0.5% by mass or more and 40% by mass or less, 0.5% by mass or more and 10% by mass or less, 1% by mass or more and 30% by mass or less, or 2% by mass or more and 10% by mass or less. This makes it easier for the zirconia powder for sintering to proceed with sintering during laser sintering.

[0041] The oxide equivalents of transition metal compounds are: cobalt is Co3O4, iron is Fe2O3, manganese is Mn3O4, vanadium is V2O5, molybdenum is Mo3O4, copper is CuO, nickel is NiO2, and praseodymium is Pr7O. 11 , neodymium is Nd2O3, erbium is Er2O3, gadolinium is Gd2O3, terbium is Tb7O 11 and scandium may be Sc2O3.

[0042] (Other Ingredients) The zirconia powder for laser sintering of this embodiment may contain components other than zirconia, stabilizing elements, and transition metal compounds, etc., as long as the effects are not impaired. Examples of such components include at least one of a solvent and a binder. Examples of the solvent include at least one of water and an organic solvent, and further at least one of water and an alcohol. By including a solvent in the zirconia powder for laser sintering of this embodiment, it can be applied as a slurry. On the other hand, the binder improves the moldability and shape retention of the zirconia powder for laser sintering of this embodiment. Examples of the binder include polymer binders, and further one or more selected from the group consisting of polyvinyl butyral, polyvinyl acetate, polyvinyl alcohol, acrylic esters, and emulsions of acrylic esters.

[0043] For example, when the zirconia powder for laser sintering of this embodiment is a zirconia powder for laser sintering containing iron oxide and a polymer binder, and the zirconia is yttrium-stabilized zirconia, the mass of the zirconia powder for laser sintering can be calculated from Fe2O3+Y2O3+ZrO2, the iron oxide content can be calculated from {Fe2O3 / (Fe2O3+Y2O3+ZrO2)}×100 [mass%], the zirconia content can be calculated from {(Y2O3+ZrO2) / (Fe2O3+Y2O3+ZrO2)}×100 [mass%], and the stabilizing element content can be calculated from {Y2O3 / (Y2O3+ZrO2)}×100 [mol%]. The content of the polymer binder can be calculated from {(W2-W1) / W2} x 100 [mass %] (where W1 is the mass of the zirconia powder for laser sintering after heat treatment in the air at 150°C for 2 hours, and W2 is the mass of the zirconia powder for laser sintering before the heat treatment).

[0044] (color tone) The zirconia powder for laser sintering of this embodiment is L * a * b * Lightness L in color system * The L of the zirconia powder for laser sintering of this embodiment is 90 or less, and preferably 85 or less or 70 or less. * a * b * Lightness L in color system * By setting the upper limit of the above range, the laser absorption efficiency can be increased, and the sintering of zirconia proceeds quickly and sufficiently. * is 0 or more, and the lightness L * The L of the zirconia powder for laser sintering of this embodiment may be 0 or more, 20 or more, 50 or more, or 60 or more. * a * b * Lightness L in color system * When the lower limit is within the above range, sintering by laser sintering can proceed in a relatively short time.

[0045] The color tone of the zirconia powder for laser sintering of this embodiment is the above-mentioned brightness L * If it satisfies, then hue a * and b * are arbitrary, and can be, for example, −100 or more and 100 or less, further −40 or more and 40 or less, and further −10 or more and 25 or less. The zirconia powder for laser sintering of this embodiment preferably exhibits a chromatic color, and the chroma C * may be 2 or more, 4 or more, or 6 or more, and 30 or less, 20 or less, or 16 or less.

[0046] (Method of manufacturing zirconia powder for laser sintering) The zirconia powder for laser sintering of this embodiment may be produced by any method as long as it satisfies the above requirements. An example of such a method is a production method having a step of mixing zirconia powder and at least one of a transition metal compound and a precursor thereof.

[0047] The zirconia powder to be subjected to the step of mixing the zirconia powder and at least one of the transition metal compound and its precursor (hereinafter also referred to as the "mixing step") is a zirconia powder that does not contain components that color zirconia, such as the transition metal compound, and has a color value of, for example, L * is preferably a zirconia powder having a molecular weight of more than 90 and not more than 100. Furthermore, the zirconia powder is preferably a powder of zirconia containing a stabilizing element, more preferably a powder of zirconia containing one or more elements selected from the group consisting of calcium (Ca), magnesium (Mg) and yttrium (Y), and further preferably a powder of yttrium-containing zirconia.

[0048] The content of the stabilizing element contained in the zirconia powder is arbitrary, but examples thereof include a content of the stabilizing element calculated as an oxide relative to the zirconia and the stabilizing element calculated as an oxide contained in the zirconia powder of 2 mol% or more or 2.5 mol% or more, and 8 mol% or less, 7 mol% or less, or 4.5 mol% or less.

[0049] At least one of the transition metal compound and its precursor subjected to the mixing process may be a compound containing the above-mentioned transition metal element, etc., and may be the same as the transition metal compound contained in the zirconia powder for laser sintering of this embodiment.

[0050] Examples of the transition metal compound include one or more selected from the group consisting of Fe3O4, Co3O4, Mn3O4, and NiO2, and examples of the precursor include one or more selected from the group consisting of Co(OH)2, MnO2, and Ni(OH)2. When a precursor of a transition metal compound is subjected to the mixing step, the type of the precursor of the transition metal compound to be subjected to the mixing step may be selected so that a desired transition metal compound is produced by the mixing step.

[0051] The mixing method in the mixing step may be such that the zirconia powder and at least one of the transition metal compound and its precursor are mixed uniformly. Examples of such a mixing method include at least one of wet mixing and dry mixing, and further, pulverization mixing using a ball mill.

[0052] After mixing, the resulting mixture may be dried, if necessary.

[0053] <Method of manufacturing zirconia sintered body> Hereinafter, the manufacturing method of the zirconia sintered body of the present disclosure will be described with reference to an example of the embodiment. The zirconia sintered body according to this embodiment can be manufactured by a manufacturing method having a step of irradiating a molded body containing the zirconia powder for laser sintering with a laser. That is, the manufacturing method of the zirconia sintered body according to this embodiment has a step of irradiating a laser beam to a molded body containing the zirconia powder for laser sintering of this embodiment to obtain a sintered body.

[0054] The above step (hereinafter also referred to as the "irradiation step") is a step of obtaining a sintered body by irradiating a molded body containing the zirconia powder for laser sintering of this embodiment with laser light.

[0055] (Molded body) The molded body to be subjected to the irradiation step is a molded body containing the zirconia powder for laser sintering of this embodiment, and is preferably a molded body consisting of only the zirconia powder for laser sintering of this embodiment.

[0056] The molded body can be obtained by a known molding method for ceramic powder. The molding method may be one or more molding methods selected from the group consisting of uniaxial pressing, CIP treatment, sheet molding, injection molding, and slip casting molding. For example, the zirconia powder for laser sintering of the present embodiment is filled into a mold, and uniaxially pressed at a molding pressure of 20 MPa to 80 MPa to obtain a molded body.

[0057] (conditions) In the irradiation step, the molded article is irradiated with a laser.

[0058] From the viewpoint of reactivity, it is preferable to use a laser having a wavelength of 500 nm or more and 11 μm or less as the light source of the laser. The laser used in the irradiation step may be one or more selected from the group consisting of a fiber laser, a Nd:YAG laser, a Nd:YVO laser, a Nd:YLF laser, a titanium sapphire laser, and a carbon dioxide gas laser.

[0059] The laser irradiation conditions may be appropriately selected depending on the sintered area (also referred to as the main area) of the molded body of the zirconia powder for laser sintering, the sintered depth of the molded body, and the like.

[0060] For smooth sintering, the laser output is set to 50W / cm 2 More than 2000W / cm 2 Below that, 100W / cm 2 More than 500W / cm 2 The irradiation time is preferably 1 second or more or 5 seconds or more and 60 minutes or less or 30 minutes or less.

[0061] The atmosphere for laser irradiation is not particularly limited as long as it is an oxygen atmosphere or a reducing atmosphere, and examples of the atmosphere include an air atmosphere, a nitrogen atmosphere, an argon atmosphere, and a helium atmosphere, and the air atmosphere is sufficient.

[0062] Prior to the laser irradiation, the molded body may be preheated. This allows the sintering by laser sintering to proceed more easily. The preheating temperature is 300°C or higher or 400°C or higher, and 1000°C or lower. The preheating method is not particularly limited, and may be one or more selected from the group consisting of an infrared lamp, a halogen lamp, resistance heating, high-frequency induction heating, and microwave heating.

[0063] The method of laser irradiation may be any method that allows the sintering of the molded body to proceed, but when sintering a large area of ​​a molded body, examples include a method in which the molded body is fixed and the laser is irradiated while moving, and a method in which the laser light path is changed through a light diffusion lens and the molded body is irradiated while moving, and still other examples include a method in which the laser light path is fixed and the molded body is irradiated while moving.

[0064] <Zirconia sintered body> The zirconia sintered body produced by the method for producing a zirconia sintered body of the present embodiment is also included in the scope of the present disclosure. Since the zirconia sintered body of the present embodiment is produced by the method for producing a zirconia sintered body of the present embodiment, it can be a dense zirconia sintered body.

[0065] The zirconia sintered body of this embodiment is preferably a sintered body consisting of crystal grains formed by sintering the particles constituting the zirconia powder for laser sintering according to this embodiment.

[0066] According to the method for producing a zirconia sintered body of the present embodiment, for example, a sintered body having a thickness of 1.0±0.5 mm can be obtained, in which the surface layer and the deep layer in the thickness direction are sintered uniformly and densely. Therefore, the measured density of the zirconia sintered body is 4.00 g / cm, which is higher than that of a conventional zirconia sintered body obtained by laser sintering. 3 Above 5.00g / cm 3 , or even 5.40g / cm 3 This is because the relative density (true density) is 6.05 g / cm 3Assuming that the density is 6.00 g / cm3, this corresponds to 70% or more, more preferably 80% or more, and even more preferably 90% or more. The higher the measured density, the better, but 3 Less than or equal to 5.65g / cm 3 The following can be given as examples.

[0067] The shape and size of the crystal grains of the zirconia sintered body of the present embodiment are not particularly limited, and examples thereof include a crystal grain diameter of 0.5 μm or more or 4 μm or more and 13 μm or less or 10 μm or less. The "crystal grain diameter" is a value measured by an intercept method.

[0068] The shape of the zirconia sintered body of the present embodiment is not particularly limited, and can be any shape depending on the purpose and use, such as a sphere, an oval sphere, a polyhedron, a line, a plate, or an irregular shape.

[0069] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. EXAMPLES

[0070] The present disclosure will be described below using examples, but the present disclosure is not limited to these.

[0071] Example 1 47.5g of 3mol% yttria-containing zirconia powder (product name: TZ-3YS, manufactured by Tosoh Corporation), 2.5g of iron oxide (Fe2O3) powder, and ethanol were mixed to form a slurry, and the resulting slurry was mixed for 24 hours in a ball mill equipped with zirconia balls having a diameter of 10 mm as a medium, and after removing the zirconia balls, the solvent was removed using an evaporator and the mixture was dried to obtain the zirconia powder for laser sintering of this example. The composition of the zirconia powder for laser sintering of this example is shown in Table 1.

[0072] 0.2 g of the obtained powder was filled into a tablet molding machine and uniaxially pressed at a molding pressure of 10 MPa to form a disk-shaped molded body with a diameter of 10 mm and a thickness of 1 mm.

[0073] [Examples 2 to 11] The zirconia powders for laser sintering of Examples 2 to 11 were prepared in the same manner as in Example 1, except that the transition metal oxides shown in Table 1 were used as the transition metal compounds instead of the iron oxide powder, and that the content of the transition metal oxides was the amount shown in Table 1.

[0074] Comparative Example 1 A zirconia powder of Comparative Example 1 was prepared in the same manner as in Example 1, except that no transition metal compound was used.

[0075] [Table 1]

[0076] [Evaluation of color tone] The color tones of the powders of the examples and comparative examples were measured by the following method. The powders sieved through a sieve with 500 μm openings were uniaxially pressed at 50 MPa to form disk-shaped molded bodies with a diameter of 12 mm and a thickness of 1±0.5 mm, and the color tones of the main surfaces of the molded bodies were measured under the following conditions. That is, measurements were performed using a color difference meter (Spectrophotometer SD 3000, manufactured by Nippon Denshoku Industries Co., Ltd.) with a white plate as the background (so-called white back measurement) under the following conditions. The results are shown in Table 2. Light source: D65 light source Viewing angle: 10° Measurement method: SCE

[0077] [Table 2]

[0078] All the powders in the examples have a lightness of L * On the other hand, the powder of the comparative example had a lightness L * was over 90.

[0079] [Evaluation of sinterability] The powder compacts of the examples and comparative examples were placed and fixed on a SUS sample stage, and in an air atmosphere, the entire main surface (face with a diameter of 10 mm) of the compacts not in contact with the sample stage was irradiated with a fiber laser (wavelength: 1070 nm) while continuously sweeping. The conditions for laser irradiation were a spot diameter of 9 mm, a laser output of 200 W, and an irradiation time of 30 seconds. In this way, zirconia sintered bodies (laser sintered bodies) of the comparative examples and each example were obtained. The actual density of the obtained sintered bodies was measured by the following method. That is, the samples were weighed to determine the mass. In addition, the volume was obtained by the Archimedes method according to JIS R 1634:1998. The Archimedes method used ion-exchanged water as the solvent, and pretreatment was performed by boiling. The obtained volume [cm 3 ], the measured density [g / cm 3 The relative density was calculated by multiplying the true density by 6.05 g / cm. 3 The results are shown in Table 3.

[0080] [Table 3]

[0081] Lightness L * By laser sintering the zirconia powder for laser sintering of the example having a density of 90 or less, the measured density is 5.00 g / cm 3 A zirconia sintered body (laser sintered body) with a lightness L * The powder of the comparative example having a zirconia sintering density of 99.2 was laser sintered, and the measured density of the obtained zirconia sintered body (laser sintered body) was 3.54 g / cm 3 It was confirmed that the sintered body consisting of zirconia alone did not undergo densification.

[0082] [Evaluation by X-ray diffraction method] When the zirconia sintered body of Example 1 was analyzed by X-ray diffraction, a peak attributed to the tetragonal crystal of yttrium-stabilized zirconia was confirmed as a peak having a peak top at 2θ=30.2 deg. On the other hand, a peak having a peak top at about 2θ=28.2 deg. and a peak having a peak top at about 2θ=31.5 deg., which are attributed to the monoclinic crystal of yttrium-stabilized zirconia, were not confirmed. Similarly, when the zirconia sintered body of Example 2 was analyzed by X-ray diffraction, a peak attributed to the tetragonal crystal of yttrium-stabilized zirconia was confirmed, and a peak attributed to the monoclinic crystal of yttrium-stabilized zirconia was not confirmed.

[0083] [Evaluation of deep sintering] Fig. 1 is a scanning electron microscope (SEM) image (magnification: 2500 times) of the surface of the zirconia sintered body of Example 7 irradiated with a laser, and Fig. 2 is an SEM image (magnification: 1000 times) of a cross section in a deep layer near the surface irradiated with a laser in the zirconia sintered body of Example 7. As shown in the SEM images of Fig. 1 and Fig. 2, it was confirmed that the zirconia sintered body of Example 7 had a dense crystal structure formed from the surface to the deep layer in both the surface and deep layers irradiated with the laser.

[0084] From the above results, it is considered that the transition metal compounds and zirconia are included, and L * a * b * Lightness L in color system * It was shown that the zirconia powders for laser sintering of the examples, which have a value of 90 or less, can be irradiated with a laser to obtain a zirconia sintered body without the interposition of alumina. Furthermore, it was shown that the zirconia sintered body obtained by laser sintering the zirconia powders for laser sintering of the examples has a dense crystal structure formed from the surface layer to the deep layer. [Industrial Applicability]

[0085] According to the present disclosure, it is possible to obtain a zirconia sintered body in which grains have been sufficiently grown in the depth direction from the surface. Therefore, it is possible to efficiently manufacture components known as uses of the zirconia sintered body, including, for example, structural materials, decorative materials, exterior components for electronic devices, high-temperature components (heat dissipation components, heat treatment containers, setters, furnace core tubes, temperature measuring protective tubes, etc.), insulating materials, light emitting tubes, etc.

Claims

1. A compound containing at least one of a transition metal element and a rare earth element, and zirconia, and further comprising L * a * b * Lightness L in color system * A zirconia powder for laser sintering, having a molecular weight of 90 or less.

2. The compound is an oxide containing one or more elements selected from the group consisting of Co, Fe, Mn, V, Mo, Cu, Ni, Pr, Nd, Er, Gd, Tb and Sc. The zirconia powder for laser sintering according to claim 1.

3. The zirconia powder for laser sintering according to claim 1 or 2, wherein the content of the compound relative to the mass of the zirconia powder for laser sintering is 0.5 mass% or more and 10 mass% or less in terms of oxide.

4. The zirconia powder for laser sintering according to claim 1 or 2, wherein the zirconia is zirconia containing a stabilizing element.

5. The zirconia powder for laser sintering according to claim 4 , wherein the stabilizing element is one or more selected from the group consisting of calcium, magnesium and yttrium.

6. A method for producing a sintered body, comprising the step of irradiating a molded body containing the zirconia powder for laser sintering according to claim 1 or 2 with laser light to obtain a sintered body.

Citation Information

Patent Citations

  • Inorganic material powder, and method for producing structure

    JP2020100141A

  • Method for manufacturing sintered body

    WO2021172128A1