Film, method for producing the same, and polarizing plate
A film composition with specific (meth)acrylic polymer, aromatic vinyl, and cyclic acid anhydride monomer copolymer, along with rubber particles, addresses solvent resistance issues in conventional films, enhancing durability and transparency.
Patent Information
- Application Number
- JP2023047225
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Conventional optical films made of (meth)acrylic resin, styrene-maleic anhydride copolymer, and rubber components suffer from poor solvent resistance, particularly to alcohol, leading to chemical cracks and cracks during manufacturing, secondary processing, storage, and transportation, and exposure to high temperature and humidity conditions.
A film composition comprising a (meth)acrylic polymer, a copolymer with structural units derived from aromatic vinyl and cyclic acid anhydride monomers, and rubber particles, with controlled molecular weight distribution and limited content of aromatic vinyl monomer, is developed to enhance solvent resistance and heat resistance.
The film exhibits improved solvent resistance, particularly to alcohol, and maintains transparency and heat resistance, reducing the occurrence of cracks and maintaining optical properties under challenging conditions.
Smart Images

Figure 2024136194000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a film, a method for producing the same, and a polarizing plate using the same. [Background technology]
[0002] 2. Description of the Related Art Conventionally, optical films containing a (meth)acrylic resin, a styrene-maleic anhydride copolymer, and a rubber component have been known. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-109087 A [Patent Document 2] JP 2017-155184 A [Patent Document 3] JP 2018-109660 A [Patent Document 4] JP 2016-060910 A Summary of the Invention [Problem to be solved by the invention]
[0004] The above films may come into contact with solvents during the manufacturing process, secondary processing process, storage and transportation process, which may damage the surface, causing deterioration of the appearance and the occurrence of cracks and breaks.In addition, the above films may be exposed to high temperature and high temperature and humidity conditions during the manufacturing process, storage and transportation process, etc., so solvent resistance under such conditions is also important. In addition, due to the spread of the COVID-19 virus, people are increasingly using alcohol to disinfect their hands, doorknobs, and other surfaces that people touch, and this has dramatically increased the opportunities for alcohol to come into contact with smartphone screens via the hands when using the device. Therefore, the optical film is required to have even higher solvent resistance, particularly alcohol resistance.
[0005] Cracks and fractures that occur in films and other materials when they come into contact with solvents such as alcohol are called chemical cracks or solvent cracks, and it is believed that these cracks occur when the solvent penetrates the film and other materials that have been subjected to stress due to heating, etc., weakening the intermolecular interactions.
[0006] However, conventional films do not necessarily have sufficient solvent resistance, particularly ethanol resistance.
[0007] The present invention has been made in view of the above problems, and an object of the present invention is to provide a film or the like which is excellent in heat resistance and transparency and also has sufficient solvent resistance. [Means for solving the problem]
[0008] [1] A (meth)acrylic polymer (A), A copolymer (B) containing a structural unit derived from an aromatic vinyl monomer and a structural unit derived from a cyclic acid anhydride monomer; Rubber particles (C), A film having a content of structural units derived from an aromatic vinyl monomer of 15 parts by mass or less per 100 parts by mass of the total of the (meth)acrylic polymer (A) and the copolymer (B).
[0009] [2] The film according to [1], wherein the content of structural units derived from aromatic vinyl monomers per 100 parts by mass of the combined total of the (meth)acrylic polymer (A) and the copolymer (B) is 2 parts by mass or more.
[0010] [3] The film according to [1] or [2], wherein the rubber particles (C) are (meth)acrylic rubber particles.
[0011] [4] The film according to any one of [1] to [3], wherein the copolymer (B) does not contain a structural unit derived from methyl methacrylate.
[0012] [5] In the copolymer (B), the structural unit derived from the aromatic vinyl monomer is represented by formula (B-1): [ka] The structural unit derived from the cyclic acid anhydride monomer is represented by formula (B-2): [ka] The film according to any one of [1] to [4].
[0013] [6] The film according to any one of [1] to [5], wherein the ratio (Mw / Mn) of the mass average molecular weight (Mw) to the number average molecular weight (Mn) of the (meth)acrylic polymer (A) is 2.0 to 3.2.
[0014] [7] A polarizing plate comprising a polarizer and the film according to any one of [1] to [6] attached to at least one surface of the polarizer via an adhesive layer.
[0015] [8] A method for producing a film comprising the steps of melting and kneading a resin composition comprising a (meth)acrylic polymer (A), a copolymer (B) containing a structural unit derived from an aromatic vinyl monomer and a structural unit derived from a cyclic acid anhydride monomer, and rubber particles (C) at 210°C to 280°C or less, and forming the resin composition into a film; A method for producing a film, wherein the content of structural units derived from an aromatic vinyl monomer per 100 parts by mass of the combined total of a (meth)acrylic polymer (A) and a copolymer (B) is 15 parts by mass or less. Effect of the Invention
[0016] According to the present invention, there are provided films and the like which are excellent in heat resistance and transparency and also have sufficient solvent resistance. [Brief description of the drawings]
[0017] [Figure 1] 1 is a differential molecular weight distribution curve of the (meth)acrylic polymer (A) of Example 1. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a layer structure of the polarizing plate according to the present invention. [Diagram 3]FIG. 4 is a cross-sectional view showing another example of the layer structure of the polarizing plate according to the present invention. [Figure 4] FIG. 1 is a process flow diagram showing an example of a film manufacturing method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] (Film F) The film F according to the present embodiment contains a (meth)acrylic polymer (A), a copolymer (B) containing a structural unit derived from an aromatic vinyl monomer and a structural unit derived from a cyclic acid anhydride monomer, and rubber particles (C).
[0019] ((Meth)acrylic polymer (A)) The (meth)acrylic polymer (A) contains structural units derived from a (meth)acrylic ester. The (meth)acrylic polymer (A) may contain more than 50 mass % of structural units derived from a (meth)acrylic ester. In this specification, the "(meth)acrylic acid ester" refers to at least one selected from the group consisting of methacrylic acid esters and acrylic acid esters.
[0020] The (meth)acrylic polymer (A) preferably contains more than 50% by mass of structural units derived from methacrylic acid esters relative to the total structural units of the (meth)acrylic polymer (A). The proportion of structural units derived from methacrylic acid esters relative to 100% by mass of the total structural units of the (meth)acrylic polymer (A) may be 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 98.0% by mass or more, or even 100% by mass.
[0021] The (meth)acrylic polymer (A) may have only one type of structural unit derived from a methacrylic acid ester, or may have two or more different types of structural units derived from a methacrylic acid ester, or may have one or more types of structural units derived from a methacrylic acid ester and one or more types of structural units derived from other monomers such as an acrylic acid ester.
[0022] The methacrylic acid ester is preferably an alkyl methacrylate, such as methyl methacrylate, ethyl methacrylate, n-, i- or t-butyl methacrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, benzyl methacrylate, cyclohexyl methacrylate, etc., with methyl methacrylate being preferred. The alkyl group of the alkyl methacrylate usually has about 1 to 8 carbon atoms and may be linear, branched or cyclic.
[0023] The acrylic acid ester is preferably an alkyl acrylate, such as methyl acrylate, ethyl acrylate, butyl acrylate, propyl acrylate, n-butyl acrylate, sec-butyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, benzyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, cyclopentadiene acrylate, etc., and is preferably methyl acrylate or ethyl acrylate, more preferably methyl acrylate. The number of carbon atoms in the alkyl group of the alkyl acrylate is usually about 1 to 8.
[0024] The content of the structural units derived from the acrylic acid esters that can be contained in the (meth)acrylic polymer (A) may be 0 to 1.6% by mass, 0.9 to 1.6% by mass, or 1.2 to 1.5% by mass. However, this content is a value obtained by taking the total of the structural units derived from the methacrylic acid esters and the structural units derived from the acrylic acid esters contained in the (meth)acrylic polymer (A) as 100% by mass. In addition, such a content can be determined by analysis using, for example, pyrolysis gas chromatography (see JP 2021-155698 A).
[0025] The optional structural unit that may be contained in the (meth)acrylic polymer (A) may be, for example, a structural unit derived from another monomer copolymerizable with a methacrylic acid ester and / or an acrylic acid ester (hereinafter, also referred to as another monomer unit). Examples of monomers for forming such other structural units include monofunctional monomers having one radically polymerizable double bond and polyfunctional monomers having two or more radically polymerizable double bonds, and these may be used alone or in combination of two or more.
[0026] Examples of the monofunctional monomer include unsaturated carboxylic acids or acid anhydrides thereof, such as acrylic acid, methacrylic acid, maleic acid, itaconic acid, maleic anhydride, and itaconic anhydride; nitrogen-containing monomers, such as acrylamide, methacrylamide, acrylonitrile, and methacrylonitrile; styrene-based monomers, such as styrene and α-methylstyrene. It is preferable that the (meth)acrylic polymer (A) does not have a structural unit derived from an aromatic vinyl monomer, such as styrene.
[0027] Examples of polyfunctional monomers include unsaturated carboxylic acid diesters of glycols such as ethylene glycol dimethacrylate and butanediol dimethacrylate; alkenyl esters of unsaturated carboxylic acids such as allyl acrylate, allyl methacrylate and allyl cinnamate; alkenyl esters of polybasic acids such as diallyl phthalate, diallyl maleate, triallyl cyanurate and triallyl isocyanurate; unsaturated carboxylic acid esters of polyhydric alcohols such as trimethylolpropane triacrylate; and divinylbenzene.
[0028] The (meth)acrylic polymer (A) may consist of a single type of polymer, or may be a mixture of multiple types of polymers.
[0029] The content of the structural unit derived from the methacrylic acid ester contained in the (meth)acrylic polymer (A) is preferably 98.0% by mass or more relative to 100% by mass of all structural units contained in the (meth)acrylic polymer (A) (requirement (1)). The content of the structural unit derived from the methacrylic acid ester contained in the (meth)acrylic polymer (A) is preferably 98.4% by mass or more relative to 100% by mass of all structural units contained in the (meth)acrylic polymer (A), and is usually 100.0% by mass or less, more preferably 98.4 to 99.1% by mass, and even more preferably 98.5 to 98.8% by mass. The content can be determined, for example, by analysis using pyrolysis gas chromatography.
[0030] In the differential molecular weight distribution curve of the (meth)acrylic polymer (A), when W1 is the ratio (%) of the peak area from the starting point to a molecular weight of 30,000 to the peak area from the starting point to the end point, it is preferable that W1 is 10 to 25 (requirement (2)). In the (meth)acrylic polymer (A), the value of W1 is preferably 14 to 22, more preferably 17 to 19. If the value of W1 is higher than 25, the Charpy impact strength may decrease. If the value of W1 is lower than 10, the flowability may decrease.
[0031] In addition, when W2 is the ratio (%) of the peak area from the molecular weight of 300,000 to the end point to the peak area from the start point to the end point in the differential molecular weight distribution curve of the (meth)acrylic polymer (A), it is also preferable that W2 is 3 to 15 (requirement (3)). The value of W2 is preferably 5 to 10. If the value of W2 is higher than 15, the flowability may decrease. If the value of W2 is lower than 3, the solvent resistance may decrease.
[0032] Furthermore, it is preferable that the ratio of the mass average molecular weight to the number average molecular weight (Mw / Mn) of the (meth)acrylic polymer (A) is 2.0 to 3.2 (requirement (4)). The ratio of the mass average molecular weight to the number average molecular weight (Mw / Mn) of the (meth)acrylic polymer (A) is preferably 2.4 to 3.2, more preferably 2.5 to 2.6.
[0033] It is preferable that the (meth)acrylic polymer (A) satisfies all of the requirements (1) to (4).
[0034] W1 and W2, the mass average molecular weight and the number average molecular weight can be determined using a conventionally known size exclusion chromatography (SEC) such as gel permeation chromatography (GPC) in accordance with JIS K 7252-1 to 4 (Plastics - Determination of average molecular weight and molecular weight distribution of polymers by size exclusion chromatography - Parts 1 to 4).
[0035] More specifically, first, a calibration curve showing the correlation between the elution time (t) and the logarithm (logM) of the molecular weight (M) is prepared in advance using a monodisperse molecular weight standard substance (a standard substance having a known molecular weight such as a number average molecular weight or a mass average molecular weight and a narrow molecular weight distribution) of a commercially available (meth)acrylic polymer (A).
[0036] Next, a sample of the (meth)acrylic polymer (A) to be measured is dissolved in an appropriate solvent to prepare a dilute solution. This solution is injected into the mobile phase (eluent) and introduced into the SEC column. The SEC column is filled with non-adsorbing fine particles having pores of uniform size or pores of various sizes. As the samples pass through the SEC column, they can be separated from each other due to differences in molecular weight (hydrodynamic volume). In the SEC column, the (meth)acrylic polymer (A) with a large molecular weight cannot penetrate into the pores and is eluted earlier. On the other hand, the (meth)acrylic polymer (A) with a small molecular weight can penetrate into the pores and is eluted slower. The concentration of the (meth)acrylic polymer (A) in the eluent is continuously detected by a concentration detector to obtain a SEC chromatogram.
[0037] Here, the molecular weight (M) of the (meth)acrylic polymer (A) corresponding to any elution time (t) in the SEC chromatogram is determined using a calibration curve previously prepared using monodisperse molecular weight standard substances.
[0038] Based on the data obtained above, a "differential molecular weight distribution curve" is created by plotting dW / d(logM) against the molecular weight (M) of the (meth)acrylic polymer (A), where "W" represents the concentration fraction.
[0039] More specifically, such a differential molecular weight distribution curve can be prepared by plotting dWi / d(logMi) calculated according to the following formula against the molecular weight (Mi) of the (meth)acrylic polymer (A) from the molecular weight (Mi) of the (meth)acrylic polymer (A) and its signal intensity (Hi) at each elution time (ti).
[0040]
number
[0041] In the formula, I represents the data collection interval (min).
[0042] As an example of the differential molecular weight distribution curve created above, the differential molecular weight distribution curve of the (meth)acrylic polymer (A) shown in Figure 1 is referred to. As shown in Figure 1, among the points where the differential molecular weight distribution curve intersects with the straight line of dW / d(logM)=0, the point on the low molecular weight side is point A (start point) and the point on the high molecular weight side is point B (end point). If the area enclosed by the curve from the start point to the end point and the straight line (referred to as the peak area in this specification) is 100, the ratio (%) of the peak area from the start point to a molecular weight of 30,000 to the peak area from the start point to the end point is "W1", and the ratio (%) of the area from a molecular weight of 300,000 to the end point is W2.
[0043] The syndiotacticity (rr) of the polymer (A) expressed as a triad is, for example, 40% or more, and from the viewpoint of increasing the toughness and heat resistance of a film formed from the (meth)acrylic resin composition, it is preferably 43% or more, more preferably 45% or more. The syndiotacticity (rr) of the polymer (A) expressed as a triad is usually 90% or less, and may be 85% or less. The syndiotacticity (rr) of the triad is the proportion of two chains (diads, diads) in a chain (triad) of three consecutive structural units that are both racemo (denoted as rr). The syndiotacticity (rr) (%) of the triad is measured in CDCL3 at 30°C. 1 The H-NMR spectrum is measured, and the area (X) of the region from 0.6 to 0.95 ppm and the area (Y) of the region from 0.6 to 1.35 ppm are measured from the spectrum when the internal standard TMS is set to 0 ppm, and the area is calculated as (X / Y)×100.
[0044] (Copolymer (B)) The copolymer (B) contains structural units derived from an aromatic vinyl monomer and structural units derived from a cyclic acid anhydride monomer. The copolymer (B) may contain structural units derived from an aromatic vinyl monomer and structural units derived from a cyclic acid anhydride monomer in a total amount of more than 50 mass% based on all structural units. In this specification, the aromatic vinyl monomer means a monomer having a structure in which an unsubstituted vinyl group or a substituted vinyl group is bonded to an aromatic ring. The aromatic vinyl monomer is easily copolymerized with a cyclic acid anhydride monomer.
[0045] Specific examples of structural units derived from aromatic vinyl monomers include those represented by the following formula (1):
[0046] [ka] (R in the formula 3 and R 4 each independently represents a hydrogen atom, a halogen atom, a hydroxyl group, an alkoxy group, a nitro group or an alkyl group having 1 to 12 carbon atoms, and n represents an integer of 1 to 3.
[0047] Examples of the halogen atom in the formula (1) include a fluorine atom, a chlorine atom, and a bromine atom. Examples of the alkyl group having 1 to 12 carbon atoms include a straight-chain or branched-chain alkyl group such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, and a 2-ethylhexyl group, and the like. An alkyl group having 1 to 8 carbon atoms is preferable, an alkyl group having 1 to 4 carbon atoms is more preferable, and a methyl group is even more preferable.
[0048] R 3 R is preferably a hydrogen atom or an alkyl group having 1 to 12 carbon atoms (particularly an alkyl group having 1 to 8 carbon atoms, and especially an alkyl group having 1 to 4 carbon atoms), more preferably a hydrogen atom or a methyl group. 4 is preferably a hydrogen atom or an alkyl group having 1 to 12 carbon atoms (particularly an alkyl group having 1 to 8 carbon atoms, and especially an alkyl group having 1 to 4 carbon atoms), more preferably a hydrogen atom. n is preferably 1. R 3 and R 4 may be the same as or different from each other.
[0049] Specific examples of aromatic vinyl monomers include styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 2-methyl-4-chlorostyrene, 2,4,6-trimethylstyrene, α-methylstyrene, cis-β-methylstyrene, trans-β-methylstyrene, 4-methyl-α-methylstyrene, 4-fluoro-α-methylstyrene, 4-chloro-α-methylstyrene, 4-bromo-α-methylstyrene, 4-tert-butylstyrene, 2-fluorostyrene, 3-fluorostyrene, 4-fluorostyrene, 2,4-difluorostyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 2,4-dichlorostyrene, 2,6-dichlorostyrene, 2-bromostyrene, 3-bromostyrene, 4-bromostyrene, 2,4-dibromostyrene, α-bromostyrene, β-bromostyrene, 2-hydroxystyrene and 4-hydroxystyrene. Among them, styrene and α-methylstyrene are preferred. Two or more aromatic vinyl monomers may be used in combination.
[0050] The content of the structural units derived from aromatic vinyl monomers in the copolymer (B) is preferably 50% by mass or more, based on 100% by mass of the structural units derived from all monomers constituting the copolymer (B). The content of the structural units derived from aromatic vinyl monomers in the copolymer (B) is preferably 50 to 90% by mass, more preferably 52 to 88% by mass, and further preferably 55 to 85% by mass.
[0051] In the present invention, a specific example of the structural unit derived from a cyclic acid anhydride monomer is a cyclic acid anhydride monomer unit represented by the following formula (2).
[0052] [ka] (R in the formula 1 and R 2 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, or a phenyl group, and m represents an integer of 0 or 1.
[0053] Examples of the halogen atom and the alkyl group having 1 to 12 carbon atoms include the same as those exemplified in the aromatic vinyl monomer unit represented by the above formula (2).
[0054] R 1 and R 2 is preferably a hydrogen atom. 1 and R 2 may be the same or different from each other.
[0055] Examples of the cyclic acid anhydride monomer include maleic anhydride, glutaric anhydride, citraconic anhydride, dimethylmaleic anhydride, dichloromaleic anhydride, bromomaleic anhydride, dibromomaleic anhydride, phenylmaleic anhydride, and diphenylmaleic anhydride, with maleic anhydride being preferred. Two or more cyclic acid anhydride monomers may be used in combination.
[0056] In the copolymer (B), the structural unit derived from the aromatic vinyl monomer is represented by the formula (B-1), [ka] The structural unit derived from the cyclic acid anhydride monomer may be represented by formula (B-2). [ka]
[0057] The content of structural units derived from cyclic acid anhydride monomers in copolymer (B) is preferably 5 to 35 mass%, more preferably 10 to 30 mass%, and even more preferably 15 to 27 mass%, relative to 100 mass% of structural units derived from all monomers constituting copolymer (B), in terms of the transparency and heat resistance of film F and dimensional stability in a high-temperature environment.
[0058] The copolymer (B) contained in the film F may contain a structural unit derived from a (meth)acrylic monomer in addition to a structural unit derived from an aromatic vinyl monomer and a structural unit derived from a cyclic acid anhydride monomer.
[0059] In the present invention, the structural unit derived from a (meth)acrylic monomer that can constitute the copolymer (B) is methacrylic acid, acrylic acid, a methacrylic acid ester, or a structural unit derived from an acrylic acid ester. Examples of the methacrylic acid ester include alkyl esters or cycloalkyl esters of methacrylic acid having 1 to 8 carbon atoms, such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, 2-ethylhexyl methacrylate, and cyclohexyl methacrylate. Two or more kinds of methacrylic acid esters may be used in combination. Among them, alkyl esters of methacrylic acid having 1 to 7 carbon atoms are preferred, and methyl methacrylate is more preferred in terms of the heat resistance and transparency of the film F.
[0060] Examples of the acrylic acid ester include alkyl esters or cycloalkyl esters of acrylic acid having 1 to 8 carbon atoms, such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, and cyclohexyl acrylate. Two or more kinds of acrylic acid esters may be used in combination. Among them, alkyl ester monomers of acrylic acid having 1 to 7 carbon atoms are preferred, and methyl acrylate is more preferred in terms of the heat resistance and transparency of the film F.
[0061] In terms of transparency of film F, the content of structural units derived from (meth)acrylic monomers in copolymer (B) may be 5 to 40 mass%, 5 to 35 mass%, 5 to 30 mass%, or 5 to 25 mass%, relative to 100 mass% of structural units derived from all monomers constituting copolymer (B).
[0062] The copolymer (B) contained in the film F may not contain a structural unit derived from methyl methacrylate, and may not contain a structural unit derived from a (meth)acrylic acid ester.
[0063] In the present invention, the copolymer (B) may contain structural units derived from other monomers in addition to structural units derived from aromatic vinyl monomers, structural units derived from cyclic acid anhydride monomers, and structural units derived from (meth)acrylic monomers, as long as the effects of the present invention are not impaired. The other monomers may be monomers capable of copolymerizing with at least one monomer forming the copolymer (B), and are preferably monomers capable of copolymerizing with all of the aromatic vinyl monomers and cyclic acid anhydride monomers forming the copolymer (B), and (meth)acrylic monomers when included. When the structural units derived from the other monomers are contained, the content thereof is preferably less than 50% by mass, more preferably 30% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of structural units derived from all monomers constituting the copolymer (B). The lower limit of the content of the structural units derived from the other monomers described above is, for example, 0% by mass or more. Examples of the other monomer include monofunctional monomers such as alkenyl cyanides, such as acrylonitrile and methacrylonitrile, N-substituted maleimides, and polyfunctional monomers, such as polyunsaturated carboxylic acid esters of polyhydric alcohols, such as ethylene glycol dimethacrylate, butanediol dimethacrylate, and trimethylolpropane triacrylate, alkenyl esters of unsaturated carboxylic acids, such as allyl acrylate, allyl methacrylate, and allyl cinnamate, polyalkenyl esters of polybasic acids, such as diallyl phthalate, diallyl maleate, triallyl cyanurate, and triallyl isocyanurate, and aromatic polyalkenyl compounds, such as divinylbenzene.
[0064] The weight average molecular weight (Mw) of the copolymer (B) is preferably 10,000 to 300,000, more preferably 30,000 to 280,000, and even more preferably 50,000 to 250,000, from the viewpoint of handleability during molding of the film F or handleability of the film F during stretching.
[0065] The number average molecular weight (Mn) of the copolymer (B) is preferably 4,000 to 100,000, more preferably 12,000 to 90,000, and even more preferably 45,000 to 85,000, from the viewpoint of handleability during molding of the film F or handleability of the film during stretching of the film F. In the present invention, the weight average molecular weight (Mw) and number average molecular weight (Mn) of the copolymer B can be measured, for example, by gel permeation chromatography (GPC) measurement in terms of polymethyl methacrylate.
[0066] The molecular weight distribution (Mw / Mn) of the copolymer (B) is preferably 1.3 to 4, more preferably 1.5 to 3.5, and even more preferably 1.7 to 3, from the viewpoint of moldability into the film F.
[0067] The melt mass flow rate (MFR) of the copolymer (B) is 0.4 g / 10 min or more, preferably 0.5 g / 10 min or more, more preferably 0.6 g / 10 min or more, and preferably 12 g / 10 min or less, more preferably 10 g / 10 min or less, and even more preferably 9 g / 10 min or less. When the MFR of the copolymer B is the above lower limit or more, it is possible to suppress the decarboxylation reaction caused by the cyclic acid anhydride monomer unit during melt kneading when producing the film F by melt extrusion molding. When the MFR of the copolymer B is the above upper limit or less, the stability of the discharge amount of the molten resin is good when producing the film F by melt extrusion molding. The MFR of the polymer in the present invention can be measured according to JIS K7210 under the conditions of a measurement temperature of 230 ° C. and a load of 21.2 N.
[0068] The copolymer (B) can be produced by polymerizing each of the constituent monomers by a known method such as bulk polymerization, solution polymerization, emulsion polymerization, suspension polymerization, cast polymerization, etc. The content of each monomer unit in the copolymer (B) can be controlled by changing the amount of each monomer used.
[0069] (Rubber particles (C)) In order to improve the flexibility of the film F and enhance its handling properties, rubber particles (C) are blended with the (meth)acrylic resin. The rubber particles (C) are rubber elastomer particles including a layer exhibiting rubber elasticity. The rubber particles may be particles consisting of only a layer exhibiting rubber elasticity, or may be particles having a multi-layer structure having a layer exhibiting rubber elasticity and other layers. Examples of rubber elastomers include olefin-based elastic polymers, diene-based elastic polymers, styrene-diene-based elastic copolymers, and (meth)acrylic elastic polymers. Among these, (meth)acrylic elastic polymers are preferred from the viewpoints of surface hardness, light resistance, and transparency of the (meth)acrylic resin film. The (meth)acrylic elastic polymer is an elastic polymer containing a structural unit derived from a (meth)acrylic acid ester. As described above, in this specification, the "(meth)acrylic acid ester" is at least one selected from the group consisting of a methacrylic acid ester and an acrylic acid ester. In other words, the (meth)acrylic elastic polymer is an elastic polymer containing a structural unit derived from at least one of a methacrylic acid ester and an acrylic acid ester. The (meth)acrylic elastic polymer can be a rubber elastic body having 50 mass% or more of the total structural units including the structural unit derived from a (meth)acrylic acid ester. The (meth)acrylic elastic polymer may be a polymer mainly composed of alkyl acrylate, i.e., containing 50% by mass or more of structural units derived from alkyl acrylate based on the total structural units. The (meth)acrylic elastic polymer may be a homopolymer of alkyl acrylate, or a copolymer containing 50% by mass or more of structural units derived from alkyl acrylate and 50% by mass or less of structural units derived from other polymerizable monomers.
[0070] As the alkyl acrylate constituting the (meth)acrylic elastic polymer, one having an alkyl group with 4 to 8 carbon atoms is usually used. Examples of the other polymerizable monomers include monofunctional monomers such as alkyl methacrylates, such as methyl methacrylate and ethyl methacrylate; styrene-based monomers, such as styrene and alkylstyrene; unsaturated nitriles, such as acrylonitrile and methacrylonitrile; and polyfunctional monomers, such as alkenyl esters of unsaturated carboxylic acids, such as allyl (meth)acrylate and methallyl (meth)acrylate; dialkenyl esters of dibasic acids, such as diallyl maleate; and unsaturated carboxylic acid diesters of glycols, such as alkylene glycol di(meth)acrylate.
[0071] The rubber particles containing the (meth)acrylic elastic polymer are preferably particles of a multilayer structure having a layer of the (meth)acrylic elastic polymer. Specifically, there are two-layer structures having a hard polymer layer mainly made of alkyl methacrylate on the outside of the layer of the (meth)acrylic elastic polymer, and three-layer structures having a hard polymer layer mainly made of alkyl methacrylate on the inside of the layer of the (meth)acrylic elastic polymer. The alkyl methacrylate is preferably methyl methacrylate. In this specification, "mainly" may mean 50% by mass or more.
[0072] The rubber particles preferably have an average particle size in the range of 10 nm to 350 nm up to the rubber elastomer layer (the layer of the (meth)acrylic elastomer) contained therein. An average particle size in this range is advantageous in terms of increasing the toughness of the film F and its adhesion to the polarizer. The average particle size is more preferably 30 nm or more, even more preferably 50 nm or more, and more preferably 320 nm or less, even more preferably 300 nm or less.
[0073] The average particle diameter of the rubber particles up to the rubber elastomer layer (the layer of the (meth)acrylic elastomer) can be measured as follows. That is, when such rubber particles are mixed with a (meth)acrylic resin to form a film and the cross section is dyed with an aqueous solution of ruthenium oxide, only the rubber elastomer layer is colored and observed to be almost circular, and the (meth)acrylic resin of the parent layer is not dyed. From the cross section of the film dyed in this way, a thin section is prepared using a microtome or the like and observed under an electron microscope. Then, 100 dyed rubber particles are randomly extracted, and the particle diameter of each particle (diameter up to the rubber elastomer layer) is calculated, and the number average value is taken as the average particle diameter. Since the average particle diameter is measured in this way, the average particle diameter obtained is the number average particle diameter.
[0074] In the case of a rubber particle in which the outermost layer is a hard polymer mainly composed of methyl methacrylate and a rubber elastomer layer (a layer of a (meth)acrylic elastomer) is enclosed within it, when it is mixed with a parent (meth)acrylic resin, the outermost layer of the rubber particle is mixed with the parent (meth)acrylic resin. Therefore, when the cross section is stained with ruthenium oxide and observed under an electron microscope, the rubber particle is observed as a particle in a state in which the outermost layer is removed. Specifically, in the case of a rubber particle having a two-layer structure in which the inner layer is a (meth)acrylic elastomer and the outer layer is a hard polymer mainly composed of methyl methacrylate, the (meth)acrylic elastomer part of the inner layer is stained and observed as a particle of a single layer structure. In addition, in the case of a rubber particle having a three-layer structure in which the innermost layer is a hard polymer mainly made of methyl methacrylate, the middle layer is a (meth)acrylic elastomeric polymer, and the outermost layer is a hard polymer mainly made of methyl methacrylate, the center part of the particle in the innermost layer is not stained, and only the (meth)acrylic elastomeric polymer part of the middle layer is stained, so that the particle is observed as having a two-layer structure.
[0075] (Additives) The film F may contain additives as necessary, such as lubricants, antiblocking agents, heat stabilizers, antioxidants, ultraviolet absorbers, infrared absorbers, antistatic agents, impact resistance improvers, surfactants, release agents, and inorganic particles.
[0076] The antioxidant may be a primary antioxidant, a secondary antioxidant, or a combination thereof. For example, a phenol-based antioxidant or an amine-based antioxidant may be used as the primary antioxidant, and for example, a phosphorus-based antioxidant or a sulfur-based antioxidant may be used as the secondary antioxidant. In addition, a phosphorus / phenol complex type antioxidant may be used as the antioxidant. The phosphorus / phenol complex type antioxidant is a compound having one or more phosphorus atoms and one or more phenol structures in the molecule, and has the functions of both a primary antioxidant and a secondary antioxidant. Two or more types of antioxidants may be used in combination.
[0077] Examples of the phenol-based antioxidant include Irganox (registered trademark) 1010 (Irganox 1010: pentaerythritol tetrakis [3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], manufactured by BASF Ltd.), Irganox 1076 (Irganox 1076: octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, manufactured by BASF Ltd.), Irganox 1330 (Irganox 1330: 3,3',3'',5,5',5''-hexa-tert-butyl-a,a',a''-(mesitylene-2,4,6-triyl) tri-p-cresol, manufactured by BASF Ltd.), and Irganox 3114 (Irganox 3114: 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Co., Ltd.), 3790 (Irganox 3790: 1,3,5-tris((4-tert-butyl-3-hydroxy-2,6-xylyl)methyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Co., Ltd.), 1035 (Irganox 1035: thiodiethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], manufactured by BASF Co., Ltd.), 1135 (Irganox 1135: 3,5-bis(1,1-dimethylethyl)-4-hydroxy-C7-C9 side chain alkyl ester of benzenepropanoic acid, manufactured by BASF Co., Ltd.), 1520L (Irganox 1520L: 4,6-bis(octylthiomethyl)-o-cresol, manufactured by BASF Co., Ltd.), 3125 (Irganox 3125, manufactured by BASF Co., Ltd.), 565 (Irganox 565: 2,4-bis(n-octylthio)-6-(4-hydroxy-3',5'-di-tert-butylanilino)-1,3,5-triazine, manufactured by BASF Co., Ltd.), Adeka STAB (registered trademark) AO-80 (Adeka STAB AO-80: 3,9-bis(2-(3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy)-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro(5,5) Undecane (manufactured by ADEKA Co., Ltd.), Sumilizer (registered trademark) BHT, Sumilizer GA-80, and Sumilizer GS (all manufactured by Sumitomo Chemical Co., Ltd.), Cyanox (registered trademark) 1790 (manufactured by Cytec Co., Ltd.), and Vitamin E (manufactured by Eisai Co., Ltd.).
[0078] Examples of amine-based antioxidants include Sumilizer (registered trademark) BPA (N,N'-di-sec-butyl-p-phenylenediamine), Sumilizer (registered trademark) BPA-M1, Sumilizer (registered trademark) 4ML (p-phenylenediamine derivative), and Sumilizer (registered trademark) 9A (alkalinated diphenylamine).
[0079] Examples of phosphorus-based antioxidants include Irgafos (registered trademark) 168 (Irgafos 168: tris(2,4-di-tert-butylphenyl)phosphite, manufactured by BASF Co., Ltd.), Irgafos 12 (Irgafos 12: tris[2-[[2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphine-6-yl]oxy]ethyl]amine, manufactured by BASF Co., Ltd.), Irgafos 38 (Irgafos 38: bis(2,4-bis(1,1-dimethylethyl)-6-methylphenyl)ethyl ester phosphorous acid, manufactured by BASF Co., Ltd.), Adeka STAB (registered trademark) 329K, Adeka STAB PEP36, Adeka STAB PEP-8 (all manufactured by ADEKA Co., Ltd.), Sandstab Examples include P-EPQ (manufactured by Clariant), Weston (registered trademark) 618, Weston 619G (all manufactured by GE), and Ultranox 626 (manufactured by GE).
[0080] Examples of phosphorus / phenol complex antioxidants include Sumilizer (registered trademark) GP (6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenz[d,f][1.3.2]dioxaphosphepine) (manufactured by Sumitomo Chemical Co., Ltd.).
[0081] Examples of the sulfur-based antioxidant include dialkyl thiodipropionate compounds such as dilauryl, dimyristyl, and distearyl thiodipropionate, and β-alkyl mercaptopropionate compounds of polyols such as tetrakis[methylene(3-dodecylthio)propionate]methane.
[0082] From the viewpoint of enhancing the heat resistance of the film F, the antioxidant is preferably a combination of a primary antioxidant and a secondary antioxidant, and more preferably a combination of a phenolic antioxidant and a phosphorus-based antioxidant. When a secondary antioxidant (preferably a phosphorus-based antioxidant) and a primary antioxidant (preferably a phenolic antioxidant) are used in combination, the content of the secondary antioxidant (preferably a phosphorus-based antioxidant):the content of the primary antioxidant (preferably a phenolic antioxidant) in the film F is preferably 1:5 to 2:1, more preferably 1:2 to 2:1, in mass ratio.
[0083] The content of the antioxidant is preferably 0.4 parts by mass or more, more preferably 0.45 parts by mass or more, even more preferably 0.5 parts by mass or more, and even more preferably 0.55 parts by mass or more, per 100 parts by mass of the rubber particles (C), from the viewpoint of improving the heat resistance of the film F. From the viewpoint of avoiding bleed-out of the antioxidant from the film F, the content is preferably 5.0 parts by mass or less, more preferably 4.5 parts by mass or less, even more preferably 4.0 parts by mass or less, and even more preferably 3.5 parts by mass or less, per 100 parts by mass of the rubber particles (C).
[0084] By including an ultraviolet absorbing agent in the film F, it is possible to suppress deterioration of the film F due to ultraviolet rays. In addition, by including an ultraviolet absorbing agent in the film F, it is possible to suppress the generation of gel when the film F is subjected to a thermal load.
[0085] Examples of the ultraviolet absorber include oxybenzophenone compounds, benzotriazole compounds, salicylic acid ester compounds, benzophenone compounds, cyanoacrylate compounds, nickel complex compounds, etc. Among them, benzotriazole compounds are preferred from the viewpoint of suppressing the generation of gel.
[0086] When an ultraviolet absorbent is blended, the blending amount is usually 1 part by mass or more, preferably 1.5 parts by mass or more, and usually 3 parts by mass or less, preferably 2.5 parts by mass or less, based on 100 parts by mass of the total amount of the (meth)acrylic copolymer (A), the copolymer (B), and the rubber particles (C) in the film F. Methods for incorporating an ultraviolet absorbent include a method of blending an ultraviolet absorbent in advance into an acrylic resin, and a method of directly supplying the ultraviolet absorbent during melt extrusion molding, and either method may be adopted.
[0087] (Amount of each component in film F) The content of the (meth)acrylic polymer (A) in the film F is usually 10 to 95 mass%, preferably 40 to 90 mass%, more preferably 50 to 85 mass%, and even more preferably 60 to 80 mass%, based on the total mass of the film F. When the content of the (meth)acrylic polymer (A) in the film F is within the above range, the heat resistance can be further improved, and a film with better appearance can be obtained.
[0088] In the film F, the content G of the structural unit derived from an aromatic vinyl monomer relative to 100 parts by mass of the total of the (meth)acrylic polymer (A) and the copolymer (B) is 15 parts by mass or less. This content G may be 14 parts by mass or less, 13 parts by mass or less, 12 parts by mass or less, 10 parts by mass or less, or 9 parts by mass or less. In addition, this content G may be 2 parts by mass or more, 3 parts by mass or more, 4 parts by mass or more, or 5 parts by mass or more. From the viewpoint of the heat resistance, transparency, and solvent resistance of the film F, the content G of the structure derived from an aromatic vinyl monomer relative to 100 parts by mass of the total of the (meth)acrylic polymer (A) and the copolymer (B) is preferably 2 to 15 parts by mass, more preferably 3 to 13 parts by mass, and even more preferably 5 to 9 parts by mass. The amount of the copolymer (B) in the film F can be appropriately set within a range that satisfies the content G above.
[0089] The content F of the rubber particles (C) in the film F can be 1 to 50 parts by mass relative to 80 parts by mass of the total of the (meth)acrylic polymer (A) and the copolymer (B). The content F may be 2 parts by mass or more, 3 parts by mass or more, or 5 parts by mass or more. The content F may be 40 parts by mass or less, 30 parts by mass or less, or 25 parts by mass or less.
[0090] (Form of Film F) The thickness of the film F is usually 5 μm or more and 200 μm or less, preferably 10 μm or more and 120 μm or less, more preferably 10 μm or more and 85 μm or less, and further preferably 15 μm or more and 65 μm or less. The thickness of the film F may be 60 μm or less, or may be 50 μm or less. Reducing the thickness of the film F is advantageous for reducing the thickness of a polarizing plate containing the film F, and furthermore, an image display device to which the film F is applied, and the like. The film F may be either an unstretched film or a uniaxially or biaxially stretched film. The biaxial stretching may be simultaneous biaxial stretching in which the film is stretched simultaneously in two stretching directions, or sequential biaxial stretching in which the film is stretched in a first direction and then stretched in a second direction different from the first direction.
[0091] The film F may have a surface treatment layer (coating layer) on one side or both sides. Examples of the surface treatment layer include a hard coat layer, an antiglare layer, an antireflection layer, a light diffusion layer, an antistatic layer, an antifouling layer, a conductive layer, etc., and a hard coat layer is preferred. Examples of the surface treatment layer include a cured product layer of a curable resin composition containing an active energy ray curable compound. The active energy ray curable compound is a compound that is polymerized and cured by irradiation with active energy rays such as ultraviolet rays and electron beams. Examples of the active energy ray curable compound include monofunctional, bifunctional, or trifunctional or higher (meth)acrylate compounds. One or more active energy ray curable compounds can be used.
[0092] The thickness of the surface treatment layer such as a hard coat layer is, for example, 0.1 μm to 50 μm, preferably 0.5 μm to 30 μm, more preferably 1 μm to 20 μm, and further preferably 1 μm to 10 μm.
[0093] (Manufacturing method of Film F) The above film F can be produced by a process in which a resin composition containing a (meth)acrylic polymer (A), a copolymer (B) containing a structural unit derived from an aromatic vinyl monomer and a structural unit derived from a cyclic acid anhydride monomer, and rubber particles (C) is melted and kneaded at 210°C to 280°C or less, and formed into a film. In the resin composition, the content of structural units derived from an aromatic vinyl monomer is 15 parts by mass or less per 100 parts by mass of the total of the (meth)acrylic polymer (A) and the copolymer (B). The melting and kneading can be carried out by a known single-screw or twin-screw kneader.
[0094] (Applications of Film F) Film F of this embodiment can be suitably used as an optical film, for example, a protective film for a polarizer.
[0095] <Polarizing plate> The polarizing plate of this embodiment is an optical laminate including a polarizer and the above-mentioned film F laminated on one or both sides of the polarizer. In the polarizing plate, the polarizer and the above-mentioned film F are laminated via an adhesive layer. The adhesive layer is a layer formed from an adhesive composition, for example, a cured layer of the adhesive composition. The polarizing plate may include a film or layer other than the polarizer and the above-mentioned film F.
[0096] The polarizing plate according to the present invention comprises a polarizer, an adhesive layer, and the above film F, in this order. Usually, the polarizer and the adhesive layer are in contact with each other, and the adhesive layer and the above film F are in contact with each other. The polarizing plate according to the present invention uses the above film F as a protective film for the polarizer, which can improve the durability of the polarizing plate. The polarizing plate according to the present invention can be suitably used in image display devices such as liquid crystal display devices and organic EL devices.
[0097] [1] Polarizing plate structure Examples of the layer structure of the polarizing plate according to the present invention are shown in FIG. 2 and FIG. 2, a polarizing plate 100 according to an example of the present invention can include a polarizer 30, a first adhesive layer 15, and a first film 10 in this order, that is, a polarizer 30 and a first film 10 laminated to one surface of the polarizer 30 via the first adhesive layer 15. As the first film 10, the above-mentioned film F is used. A primer layer may be interposed between the first adhesive layer 15 and the first film 10, or the first adhesive layer 15 may be in direct contact with the first film 10. It is preferable that the polarizer 30 and the first adhesive layer 15 are in direct contact with each other.
[0098] As shown in FIG. 3, another polarizing plate 100 according to the present invention may include a polarizer 30, a first film 10 laminated to one surface of the polarizer 30 via a first adhesive layer 15, and a second film 20 laminated to the other surface of the polarizer 30 via a second adhesive layer 25. The first adhesive layer 15 and the first film 10 are preferably in direct contact with each other. The polarizer 30 and the first adhesive layer 15 are preferably in direct contact with each other. The second adhesive layer 25 and the second film 20 are preferably in direct contact with each other. The polarizer 30 and the second adhesive layer 25 are preferably in direct contact with each other. As the first film 10, the above film F is used.
[0099] The polarizing plate according to the present invention is preferably incorporated into an image display device so that the first film 10 side is the viewing side. The film F used as the first film 10 is preferably a protective film laminated on the viewing side of the polarizer 30.
[0100] The polarizing plate according to the present invention may include layers (or films) other than those described above, without being limited to the examples in Fig. 2 and Fig. 3. Examples of the other layers include a pressure-sensitive adhesive layer laminated on the outer surface of the first film 10, the second film 20, and / or the polarizer 30; a separate film (also called a "release film") laminated on the outer surface of the pressure-sensitive adhesive layer; a protective film (also called a "surface protection film") laminated on the outer surface of the first film 10, the second film 20, and / or the polarizer 30; and an optically functional film (or layer) laminated on the outer surface of the first film 10, the second film 20, and / or the polarizer 30 via an adhesive layer or a pressure-sensitive adhesive layer.
[0101] [2] Polarizer The polarizer 30 is a film having a function of selectively transmitting linearly polarized light in one direction from natural light. Examples of the polarizer 30 include an iodine-based polarizer in which iodine as a dichroic pigment is adsorbed and oriented on a polyvinyl alcohol-based resin film, a dye-based polarizer in which a dichroic dye as a dichroic pigment is adsorbed and oriented on a polyvinyl alcohol-based resin film, and a coating-type polarizer in which a dichroic dye in a lyotropic liquid crystal state is coated, oriented, and fixed. These polarizers are called absorption-type polarizers because they selectively transmit linearly polarized light in one direction from natural light and absorb linearly polarized light in the other direction.
[0102] The polarizer 30 is not limited to an absorptive polarizer, and may be a reflective polarizer that selectively transmits linearly polarized light in one direction from natural light and reflects linearly polarized light in the other direction, or a scattering polarizer that scatters linearly polarized light in the other direction. However, an absorptive polarizer is preferred because it provides excellent visibility when the polarizing plate is applied to an image display device, etc.
[0103] The thickness of the polarizer 30 can be 30 μm or less, and is preferably 25 μm or less (for example, 20 μm or less, further 15 μm or less, further 10 μm or less, and further 8 μm or less). The thickness of the polarizer 30 is usually 2 μm or more. Reducing the thickness of the polarizer 30 is advantageous for reducing the thickness of the polarizing plate, and further the image display device to which the polarizer is applied.
[0104] [3] Film 2 The second film 20 can be a film made of a light-transmitting (preferably optically transparent) thermoplastic resin, for example, a polyolefin resin such as a chain polyolefin resin (polyethylene resin, polypropylene resin, etc.) or a cyclic polyolefin resin (norbornene resin, etc.); a cellulose ester resin such as triacetyl cellulose or diacetyl cellulose; a polyester resin such as polyethylene terephthalate, polyethylene naphthalate, or polybutylene terephthalate; a polycarbonate resin; or a (meth)acrylic resin.
[0105] The second film 20 may be the above-mentioned film F. When the second film 20 is film F, the resin component constituting the second film 20 may be the same as or different from the resin component constituting the first film 10 in terms of composition, etc. Furthermore, when the second film 20 is film F, the thickness may be the same as or different from that of the first film 10.
[0106] The second film 20 may be either an unstretched film or a uniaxially or biaxially stretched film. The biaxial stretching may be simultaneous biaxial stretching in which the film is stretched in two directions at the same time, or sequential biaxial stretching in which the film is stretched in a first direction and then stretched in a second direction different from the first direction.
[0107] The second film 20 may be a protective film that plays a role in protecting the polarizer 30, or may be a protective film that also has an optical function such as a retardation film. For example, a film made of the above-mentioned thermoplastic resin may be stretched (uniaxially or biaxially stretched, etc.) or a liquid crystal layer or the like may be formed on the thermoplastic resin film, thereby making it possible to obtain a retardation film having an arbitrary retardation value.
[0108] The second film 20 may contain additives as necessary, such as lubricants, antiblocking agents, heat stabilizers, antioxidants, ultraviolet absorbers, infrared absorbers, antistatic agents, impact resistance improvers, surfactants, release agents, and inorganic particles.
[0109] In one embodiment, the first film 10 is the above-mentioned film F, and the second film 20 is a polyolefin-based resin film (preferably a cyclic polyolefin-based resin film), a cellulose ester-based resin film, or a polyester-based resin film. In another embodiment, the first film 10 is the above-mentioned film F, and the second film 20 is a (meth)acrylic polymer film. The second film 20 may be the above-mentioned film F.
[0110] The second film 20 may have a coating layer (surface treatment layer) such as a hard coat layer, an antiglare layer, an antireflection layer, a light diffusion layer, an antistatic layer, an antifouling layer, or a conductive layer on its outer surface (the surface opposite the polarizer 30).
[0111] The thickness of the second film 20 is usually 5 μm or more and 200 μm or less, preferably 10 μm or more and 120 μm or less, more preferably 10 μm or more and 85 μm or less, and further preferably 15 μm or more and 65 μm or less. The thickness of the second film 20 may be 60 μm or less, or may be 50 μm or less. Reducing the thickness of the second film 20 is advantageous for reducing the thickness of the polarizing plate, and furthermore, the image display device to which the polarizing plate is applied.
[0112] [4] Manufacture of polarizing plates and adhesive layers A polarizing plate having the configuration shown in Figure 2 can be obtained by laminating and adhering a first film 10, which is film F, to one surface of the polarizer 30 via a first adhesive layer 15, and a polarizing plate having the configuration shown in Figure 3 can be obtained by further laminating and adhering a second film 20 to the other surface of the polarizer 30 via a second adhesive layer 25.
[0113] Examples of the adhesive composition forming the first adhesive layer 15 and the second adhesive layer 25 include a water-based adhesive or an active energy ray-curable adhesive. The adhesive composition forming the first adhesive layer 15 and the adhesive composition forming the second adhesive layer 25 may be the same or different. The adhesive used for bonding the film F according to the present invention to the polarizer is preferably an active energy ray-curable adhesive.
[0114] Examples of the aqueous adhesive include conventionally known adhesive compositions using polyvinyl alcohol resin or urethane resin as the main component. The active energy ray curable adhesive is an adhesive that is cured by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays. When an active energy ray curable adhesive is used, the adhesive layer of the polarizing plate is a cured layer of the adhesive.
[0115] The active energy ray curable adhesive can be an adhesive containing an epoxy compound that cures by cationic polymerization as a curable component, and is preferably an ultraviolet ray curable adhesive containing such an epoxy compound as a curable component. The epoxy compound means a compound having an average of one or more, preferably two or more, epoxy groups in the molecule. The epoxy compound may be used alone or in combination of two or more.
[0116] Examples of epoxy compounds include hydrogenated epoxy compounds (glycidyl ethers of polyols having alicyclic rings) obtained by reacting epichlorohydrin with alicyclic polyols obtained by hydrogenating the aromatic rings of aromatic polyols; aliphatic epoxy compounds such as polyglycidyl ethers of aliphatic polyhydric alcohols or their alkylene oxide adducts; and alicyclic epoxy compounds, which are epoxy compounds having one or more epoxy groups bonded to an alicyclic ring in the molecule.
[0117] The active energy ray curable adhesive may contain a radically polymerizable (meth)acrylic compound as a curable component, instead of or together with the above-mentioned epoxy compound. Examples of the (meth)acrylic compound include (meth)acryloyloxy group-containing compounds such as (meth)acrylate monomers having one or more (meth)acryloyloxy groups in the molecule; and (meth)acrylate oligomers obtained by reacting two or more functional group-containing compounds and having at least two (meth)acryloyloxy groups in the molecule.
[0118] When the active energy ray-curable adhesive contains an epoxy compound that cures by cationic polymerization as a curable component, it is preferable that the active energy ray-curable adhesive contains a photocationic polymerization initiator. Examples of the photocationic polymerization initiator include aromatic diazonium salts, onium salts such as aromatic iodonium salts and aromatic sulfonium salts, and iron-allene complexes. When the active energy ray-curable adhesive contains a radical polymerizable component such as a (meth)acrylic compound, it preferably contains a photoradical polymerization initiator. Examples of the photoradical polymerization initiator include acetophenone-based initiators, benzophenone-based initiators, benzoin ether-based initiators, thioxanthone-based initiators, xanthone, fluorenone, camphorquinone, benzaldehyde, and anthraquinone.
[0119] When an active energy ray curable adhesive is used, the adhesive composition layer is cured by irradiating active energy rays. The light source used for irradiating active energy rays may be any light source capable of generating ultraviolet rays, electron beams, X-rays, etc. In particular, light sources having an emission distribution of wavelengths of 400 nm or less, such as low pressure mercury lamps, medium pressure mercury lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, chemical lamps, black light lamps, microwave excited mercury lamps, metal halide lamps, etc., are preferably used.
[0120] The thickness of the first adhesive layer 15 and the second adhesive layer 25 is, for example, 0.1 μm to 100 μm, preferably 0.5 μm to 80 μm, more preferably 1 μm to 60 μm, and even more preferably 2 μm to 50 μm in the polarizing plate. From the viewpoint of thinning the polarizing plate, it is also preferable to set the thickness of the adhesive layer to 30 μm or less, and further 20 μm or less. When a water-based adhesive is used, the thickness of the adhesive layer may be smaller than the above. The first adhesive layer 15 and the second adhesive layer 25 may have the same thickness or different thicknesses.
[0121] [5] Other components of polarizing plates [5-1] Optically functional film The polarizing plate may include an optically functional film other than the polarizer 30 in order to impart a desired optical function, and a suitable example of such a film is a retardation film. As described above, the second film 20 may also function as a retardation film, but a retardation film may also be laminated separately from the second film 20.
[0122] Examples of the retardation film include a birefringent film composed of a stretched film of a thermoplastic resin having light transmission properties; a film in which discotic liquid crystal or nematic liquid crystal is oriented and fixed; and a film in which the above-mentioned liquid crystal layer is formed on a substrate film. The substrate film is usually a film made of a thermoplastic resin, and an example of the thermoplastic resin is a cellulose ester resin such as triacetyl cellulose. As the thermoplastic resin forming the birefringent film, those described for the second film 20 can be used.
[0123] Examples of other optically functional films (optical members) that can be included in the polarizing plate include a light collecting plate, a brightness enhancing film, a reflective layer (reflective film), a semi-transmissive reflective layer (semi-transmissive reflective film), a light diffusing layer (light diffusing film), etc. These are generally provided when the polarizing plate is a polarizing plate disposed on the back side (backlight side) of the liquid crystal cell.
[0124] [5-2] Adhesive layer The polarizing plate according to the present invention may include an adhesive layer for attaching it to an image display element such as a liquid crystal cell or an organic EL element, or other optical members. The adhesive layer may be laminated on the outer surface (the surface opposite to the first film 10) of the polarizer 30 in the polarizing plate having the configuration shown in Fig. 2, or on the outer surface of the first film 10 or the second film 20 in the polarizing plate having the configuration shown in Fig. 3.
[0125] In a polarizing plate according to a preferred embodiment, the pressure-sensitive adhesive layer is laminated on the outer surface of the second film 20, i.e., on the surface opposite to the first film 10 side with respect to the polarizer 30. In this embodiment, when the polarizing plate is attached to an image display element, the polarizing plate is attached to the image display element via the pressure-sensitive adhesive layer so that the first film 10 side becomes the viewing side.
[0126] The adhesive used in the adhesive layer may be one having a base polymer such as a (meth)acrylic resin, a silicone resin, a polyester resin, a polyurethane resin, a polyether resin, etc. Among these, a (meth)acrylic adhesive is preferred from the viewpoints of transparency, adhesive strength, reliability, weather resistance, heat resistance, reworkability, etc.
[0127] The thickness of the pressure-sensitive adhesive layer is determined depending on its adhesive strength, etc., but is suitably in the range of 1 μm or more and 50 μm or less, and preferably 2 μm or more and 40 μm or less.
[0128] The polarizing plate may include a separate film laminated on the outer surface of the pressure-sensitive adhesive layer. The separate film may be a film made of a polyethylene-based resin such as polyethylene, a polypropylene-based resin such as polypropylene, a polyester-based resin such as polyethylene terephthalate, or the like. Among them, a stretched film of polyethylene terephthalate is preferred.
[0129] The pressure-sensitive adhesive layer may contain, as necessary, fillers made of glass fibers, glass beads, resin beads, metal powders or other inorganic powders, pigments, colorants, antioxidants, ultraviolet absorbing agents, antistatic agents, and the like.
[0130] [5-3] Protective film The polarizing plate according to the present invention may include a protective film for protecting its surface (film surface, polarizer surface, etc.) After the polarizing plate is attached to, for example, an image display element or other optical members, the protective film is peeled off and removed together with the pressure-sensitive adhesive layer that the polarizing plate has. In a preferred embodiment, a polarizer is laminated onto the surface of the first film 10 .
[0131] The protective film is composed of, for example, a base film and an adhesive layer laminated thereon. The adhesive layer is as described above. The resin constituting the base film may be, for example, a thermoplastic resin such as a polyethylene-based resin such as polyethylene, a polypropylene-based resin such as polypropylene, a polyester-based resin such as polyethylene terephthalate or polyethylene naphthalate, or a polycarbonate-based resin. A polyester-based resin such as polyethylene terephthalate is preferred. EXAMPLES
[0132] [Raw material resin] The raw material resins used in the examples and comparative examples are the following four types. (Meth)acrylic polymer (A): A radical copolymer having a triad syndiotacticity (rr) of 51% with a mass ratio of methyl methacrylate / methyl acrylate of 98.6 / 1.4. The weight average molecular weight Mw is 107×10 3 The weight average molecular weight Mw / number average molecular weight Mn is 2.6. W1 (%) and W2 (%) are 18.9 and 5.5, respectively. Styrene-maleic anhydride copolymer (B-1): SMA700 (trade name, manufactured by Jiaxing Huawen Chemical Co., content of maleic anhydride-derived structural units: approximately 18% by mass) was purchased from the market and used. Styrene-maleic anhydride copolymer (B-2): SMA725 (trade name, manufactured by Jiaxing Huawen Chemical Co., content of maleic anhydride-derived structural units: approximately 25% by mass) was purchased from the market and used. Rubber particle (C): (meth)acrylic rubber particle which is a (meth)acrylic multilayer polymer having a three-layer structure (first layer (innermost layer): hard copolymer containing methyl methacrylate, methyl acrylate, and allyl methacrylate (mass ratio 93.8 / 6.0 / 0.2) / second layer: soft elastic copolymer containing butyl acrylate, styrene, and allyl methacrylate (mass ratio 80.6 / 17.4 / 2.0) / third layer (outermost layer): hard copolymer containing methyl methacrylate and methyl acrylate (mass ratio 94 / 6)).
[0133] [Preparation of resin film] The cooling unit 4 consisting of the extruder 1, the T-die 2, and the first to third cooling rolls 5, 6, and 7 was arranged as shown in FIG. 4. Each raw material component was charged into a single screw extruder (LABO PLASTOMILL 4C150-01, manufactured by TOYOSEIKI) in the ratio shown in Table 1, and melt-kneaded at 245°C to obtain a molten resin of a resin composition. Next, this molten resin was supplied to the T-die 2 with a set temperature of 245°C, and the film-like molten resin 3 extruded from the T-die was sandwiched between the first cooling roll 5 and the second cooling roll 6 arranged opposite each other, and was wrapped around the third cooling roll 7 for molding and cooling to obtain a resin film A with a thickness of 60 μm. The surface temperature of the first cooling roll was 95°C, the surface temperature of the second cooling roll was 95°C, and the surface temperature of the third cooling roll was 65°C. These temperatures were measured values of the surface temperature of each cooling roll. The amounts of the (meth)acrylic polymer, styrene-maleic anhydride copolymer, and rubber particles in Table 1 are in parts by mass.
[0134] [Table 1]
[0135] [Measurement and Evaluation] Glass transition temperature (Tg) Using a DSC device (EXSTAR6000, manufactured by Seiko Instruments Inc.), according to the differential scanning calorimetry based on JIS K7121:1987, the resin film was cooled to -80°C at a rate of 10°C / min with a nitrogen flow rate of 40mL / min, held for 10 minutes, then heated to 160°C at a rate of 10°C / min and held for 10 minutes. Next, the temperature was lowered from 160°C to -80°C at a rate of 10°C / min, held for 10 minutes, and then heated to 160°C at a rate of 10°C / min to determine the onset glass transition temperature (Tg), which was taken as the glass transition temperature (°C). The larger this value, the higher the heat resistance.
[0136] Elastic modulus at 80℃ The resin film obtained above was cut into a rectangle of length 70 mm x width 10 mm. The length direction of the test piece was the MD direction of the resin film, and the width direction was the TD direction (direction perpendicular to the MD direction) of the resin film. Next, the test piece was clamped at both ends in the length direction (MD direction of the resin film) with the upper and lower grips of a tensile tester (Autograph AG-1S tester, manufactured by Shimadzu Corporation) so that the distance between the grips was 5 cm, and the test piece was pulled in the length direction (MD direction of the resin film) at a pulling speed of 50 mm / min in an environment of 80 ° C., and the tensile modulus (MPa) in the MD direction of the resin film at 80 ° C. was calculated from the slope of the initial straight line in the obtained stress-strain curve.
[0137] density The density of the film (g / cm) was measured by the gas displacement method using a dry automatic density meter (Acubix II 1340, Shimadzu Corporation). 3 The measurement temperature was 25°C, and nitrogen was used as the filling gas.
[0138] Internal Haze Dimethyl phthalate (Tokyo Chemical Industry Co., Ltd.) was dripped onto both sides of a film cut to 30 mm x 30 mm, the film was sandwiched between PMMA plates (Sumipex E00 1.0 mm), and the haze was measured in accordance with JIS K7136 using a haze meter (HM-150N, Murakami Color Research Laboratory Co., Ltd.).
[0139] Preparation of samples for chemical resistance tests The resin film was cut into a square of 80 mm long x 80 mm wide, and the resin film was attached to an alkali-free glass substrate (thickness: 0.7 mm) using an acrylic adhesive with a thickness of 25 μm to prepare a sample for chemical resistance test (a sample before chemical resistance test). This sample was left to stand at 80 ° C for 5 minutes, and immediately after being taken out to 23 ° C / 55% RH, 1.5 mL of a mixed solvent of ethanol and water (99.5% ethyl alcohol Fujifilm Wako Pure Chemical Industries, Ltd. / pure water = 9 / 1, weight ratio)) was dropped on the surface of the resin film. Then, a cylindrical weight of 0.6 kg and a diameter of 5.5 cm covered with a clean wiper (CFW8009L, CHANG-FONG TEXTILE TECHNOLOGY CO., LTD.) was placed on the resin film so that the bottom of the cylinder was in contact with the droplet of the mixed solvent, and left to stand for 30 seconds. Next, the cylindrical weight was removed from the film to obtain a sample after the chemical resistance test. The following evaluations were performed on the sample before the chemical resistance test and the sample after the chemical resistance test.
[0140] Chemical resistance test (1) Appearance evaluation The appearance of the samples was visually inspected before and after the chemical resistance test and evaluated according to the following criteria. ○: No change in appearance before and after chemical resistance test ×: After the chemical resistance test, the film surface became cloudy and cracks occurred.
[0141] (2) ΔHaze (chemical resistance) evaluation The haze values (%) of the samples before and after the chemical resistance test were measured using a haze meter (HM-150N, manufactured by Murakami Color Research Laboratory Co., Ltd.) in accordance with JIS K7136. The haze value of the sample after the chemical resistance test minus the haze value of the sample before the chemical resistance test was taken as ΔHaze (chemical resistance) and used as an index of chemical resistance. A smaller ΔHaze (chemical resistance) value indicates less change due to contact with alcohol and better chemical resistance.
[0142] (3) Sa(post-test) / Sa(pre-test) evaluation The surface roughness of the samples before and after the chemical resistance test was evaluated using a laser microscope (LEXT OLS5000, manufactured by OLYMPUS). The arithmetic mean height Sa (μm) was used as an index of surface roughness. The ratio of the Sa value of the sample before the chemical resistance test (Sa(before test)) to the Sa value of the sample after the chemical resistance test (Sa(after test)), Sa(after test) / Sa(before test), was used as an index of chemical resistance. The smaller the value of Sa(after test) / Sa(before test), the smaller the change due to contact with alcohol and the better the chemical resistance.
[0143] Durability evaluation at 80℃ for 750 hours The haze value (%) of a resin film cut to 30 mm x 30 mm was measured using a haze meter (HM-150N, manufactured by Murakami Color Research Laboratory). This value was taken as the initial haze value. The resin film was then stored in an 80°C environment for 750 hours, and the haze value of the resin film after storage was measured in the same manner. This value was taken as the haze value after the durability test. The value obtained by subtracting the initial haze value from the haze value after this durability test was taken as ΔHaze (80°C 750 hours), and was used as an index of 80°C durability. A smaller ΔHaze (80°C 750 hours) value indicates better durability.
[0144] GPC analysis conditions Measuring device: Tosoh Corporation HLC-8320GPC Column configuration: Sample column: Two TSKgel SuperMultipore HZ-M columns and one TSKguardColumn SuperMP(HZ)-M column connected in series Reference column: Two TSKgel Super H-RC columns connected in series Detector: RI (differential refractometer) detector ·Calculation method: Molecular weight calculation ·Internal standard: Chloroform was used as the internal standard. Allowable time for internal standard peak: 0.15 min Elution time of internal standard peak: This was set as the elution time of chloroform when the standard sample for the calibration curve was measured. Reference sample: THF (special grade, Fujifilm Wako Pure Chemical Industries, Ltd.) Measurement sample: A measurement sample was prepared by thoroughly dissolving 25 mg of the methacrylic resin composition in 5 mL of a THF / chloroform solution prepared by dissolving chloroform (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) as an internal standard in THF (special grade, manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) to a concentration of 0.04 vol%. Column temperature: 40℃ ·Injection volume: 10μL Sample pump flow rate: 0.35ml / min Reference pump flow rate: 0.60ml / min
[0145] Under the above GPC analysis conditions, the RI detection intensity was measured against the elution time of the (meth)acrylic polymer. As standard samples for the calibration curve, the following seven types of methacrylic resins (Shodex STANDARD M-75, Showa Denko K.K.) with known monodisperse mass average molecular weights and different molecular weights were used. Peak Molecular Weight Standard sample 1:1,050,000 Standard sample 2: 569,000 Standard sample 3: 211,000 Standard sample 4: 68,800 Standard sample 5: 18,500 Standard sample 6: 7,360 Standard sample 7: 3,070 The standard samples for the calibration curve were measured under the same conditions as the (meth)acrylic polymer, and the peak top elution time of each standard sample was obtained. From the obtained elution times and peak molecular weights, the following third-order approximation equation was obtained and used as the calibration equation for analyzing the measurement results of the (meth)acrylic polymer. ·Log M(molecular weight)=At3+Bt2+Ct+D A, B, C, D: Variables ·t: Elution time
[0146] (How to calculate W1, W2 and Mw / Mn) The (meth)acrylic polymer was analyzed by the above GPC measurement to obtain Mw / Mn. The obtained GPC curve was output at elution time intervals of 500 ms to create a differential molecular weight distribution curve. FIG. 1 is a graph showing a differential molecular weight distribution curve for the (meth)acrylic polymer (A). Among the points where the differential molecular weight distribution curve intersects with the straight line of dW / d(logM)=0, the point on the low molecular weight side was designated as point A (start point), and the point on the high molecular weight side was designated as point B (end point). When the area enclosed by the curve and the straight line was designated as 100, the percentage (%) of the area from the start point to a molecular weight of 30,000 was calculated as "W1", and the percentage (%) of the area from a molecular weight of 300,000 to the end point was calculated as W2.
[0147] [Table 2]
[0148] As described above, it is found that the increase in the glass transition temperature, elastic modulus, and density results in a hard and dense film, which suppresses the occurrence of chemical cracks and exhibits sufficient ethanol resistance. According to the present invention, by setting the content of structural units derived from aromatic vinyl monomers to a predetermined value relative to 100 parts by mass of the total of the (meth)acrylic polymer (A) and the copolymer (B), it is possible to provide a film or the like that is excellent in heat resistance and transparency and has sufficient solvent resistance. [Explanation of symbols]
[0149] 100...polarizing plate, 30...polarizer, 10...first film, 20...second film, F...film.
Claims
1. A (meth)acrylic polymer (A), A copolymer (B) containing a structural unit derived from an aromatic vinyl monomer and a structural unit derived from a cyclic acid anhydride monomer; Rubber particles (C), A film having a content of structural units derived from an aromatic vinyl monomer of 15 parts by mass or less per 100 parts by mass of the total of the (meth)acrylic polymer (A) and the copolymer (B).
2. The film according to claim 1, wherein the content of the structural unit derived from an aromatic vinyl monomer is 2 parts by mass or more per 100 parts by mass of the total of the (meth)acrylic polymer (A) and the copolymer (B).
3. The film according to claim 1 or 2, wherein the rubber particles (C) are (meth)acrylic rubber particles.
4. The film according to claim 1 or 2, wherein the copolymer (B) does not contain a structural unit derived from methyl methacrylate.
5. In the copolymer (B), the structural unit derived from the aromatic vinyl monomer is represented by formula (B-1), 【Chemistry 1】 The structural unit derived from the cyclic acid anhydride monomer is represented by formula (B-2): 【Chemistry 2】 The film according to claim 1 or 2.
6. The film according to claim 1 or 2, wherein the ratio (Mw / Mn) of the mass average molecular weight (Mw) to the number average molecular weight (Mn) of the (meth)acrylic polymer (A) is 2.0 to 3.
2.
7. A polarizing plate comprising a polarizer and the film according to claim 1 or 2 attached to at least one surface of the polarizer via an adhesive layer.
8. The method includes a step of melting and kneading a resin composition including a (meth)acrylic polymer (A), a copolymer (B) containing a structural unit derived from an aromatic vinyl monomer and a structural unit derived from a cyclic acid anhydride monomer, and rubber particles (C) at 210° C. to 280° C. or less, and forming the resin composition into a film; A method for producing a film, wherein the content of structural units derived from an aromatic vinyl monomer per 100 parts by mass of the combined total of the (meth)acrylic polymer (A) and the copolymer (B) is 15 parts by mass or less.
Citation Information
Patent Citations
Optical film
JP2008276203A
Transparent rubber-modified styrenic resin composition and molding of the same
JP2013104042A
Thermoplastic resin film
JP2016060910A
Resin film
JP2017155184A
Thermoplastic resin composition
JP2018109087A