Multilayer ceramic electronic component, circuit board, electronic component package, and method for manufacturing multilayer ceramic electronic component
By optimizing pore cross-sectional areas and diameters in the inner and outer peripheries of multilayer ceramic capacitors and filling them with organic substances, the reliability and durability of these components are significantly enhanced.
Patent Information
- Application Number
- JP2023047255
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing multilayer ceramic capacitors suffer from insufficient crack suppression due to the absence of pores in the cover layer and imbalanced pore cross-sectional area ratios, leading to reduced reliability under stress.
The multilayer ceramic electronic component is designed with specific ratios of pore cross-sectional areas in inner and outer peripheral parts, controlled pore diameters, and filled with organic substances to enhance stress relief and crack resistance.
The design improves the reliability of the multilayer ceramic capacitors by effectively dispersing stress and preventing cracks, enhancing their durability and performance.
Smart Images

Figure 2024136218000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer ceramic electronic component, a circuit board, an electronic component package, and a method for manufacturing a multilayer ceramic electronic component. [Background technology]
[0002] Patent Document 1 describes a multilayer ceramic capacitor in which pores are formed in the side margins to suppress the occurrence of cracks, while Patent Document 2 describes a multilayer ceramic capacitor in which the ratio of the total cross-sectional area of pores per unit area of the outer dielectric to the total cross-sectional area of pores per unit area of the inner dielectric is 1 or less in the stacking direction. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-107239 A [Patent Document 2] JP 2016-82183 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the multilayer ceramic capacitor disclosed in Patent Document 1, pores are not formed in the cover layer, and there is a risk that the occurrence of cracks cannot be sufficiently suppressed. In addition, according to the cross-sectional area ratio of the pores disclosed in Patent Document 2, the area occupied by the pores in the inner dielectric is larger than that of the outer dielectric, so that when stress is applied to the multilayer ceramic capacitor from the outside, cracks are likely to occur starting from the pores in the capacitance part where the internal electrodes are laminated, and there is a risk of reducing reliability.
[0005] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a multilayer ceramic electronic component, a circuit board, an electronic component packaging body, and a method for manufacturing a multilayer ceramic electronic component that can improve reliability. [Means for solving the problem]
[0006] The multilayer ceramic electronic component of the present invention comprises a laminated portion having a substantially rectangular parallelepiped shape in which a plurality of dielectric layers and a plurality of internal electrode layers are laminated, an inner peripheral portion including a dielectric covering a periphery of the laminated portion in a cross-sectional view taken along a stacking direction of the laminated portion and a width direction of the laminated portion approximately perpendicular to the stacking direction, and an outer peripheral portion including a dielectric covering a periphery of the inner peripheral portion in the cross-sectional view, wherein a ratio of a sum of cross-sectional areas of pores in the inner peripheral portion to a cross-sectional area of the inner peripheral portion in the cross-sectional view is smaller than a ratio of a sum of cross-sectional areas of pores in the outer peripheral portion to a cross-sectional area of the outer peripheral portion.
[0007] In the above-mentioned monolithic ceramic electronic component, in the cross-sectional view, a ratio of a total cross-sectional area of pores in the inner peripheral portion to a cross-sectional area of the inner peripheral portion may be less than 3%, and a ratio of a total cross-sectional area of pores in the outer peripheral portion to a cross-sectional area of the outer peripheral portion may be 3% or more.
[0008] In the above monolithic ceramic electronic component, in the cross-sectional view, a ratio of a total cross-sectional area of the pores in the outer periphery to a cross-sectional area of the outer periphery may be 12% or less.
[0009] In the above-described monolithic ceramic electronic component, a cross-sectional area of the outer circumferential portion may be larger than a cross-sectional area of the inner circumferential portion in the cross-sectional view.
[0010] In the above monolithic ceramic electronic component, in the cross-sectional view, a cross-sectional area of the outer periphery may be 82% or more of a total cross-sectional area of the front first dielectric portion and a cross-sectional area of the outer periphery.
[0011] In the above monolithic ceramic electronic component, in the cross-sectional view, a cross-sectional area of the outer periphery may be 90% or less of a total cross-sectional area of the front first dielectric portion and the outer periphery.
[0012] In the above monolithic ceramic electronic component, in the cross-sectional view, the maximum diameter of the pores in the inner peripheral portion may be less than 0.4 μm, and the maximum diameter of the pores in the outer peripheral portion may be 0.4 μm or more.
[0013] In the above monolithic ceramic electronic component, the maximum diameter of the pores in the outer circumferential portion in the cross-sectional view may be 1.0 μm or less.
[0014] In the above-described multilayer ceramic electronic component, the size in a length direction substantially perpendicular to the stacking direction and the width direction may be 0.25 mm or less, the size in the width direction may be 0.125 mm or less, and the size in the stacking direction may be 0.125 mm or less.
[0015] In the above-mentioned multilayer ceramic electronic component, in the cross-sectional view, a ratio of a cross-sectional area of the outer periphery to a cross-sectional area of the inner periphery and the outer periphery outside a pair of faces of the laminate that are opposed to each other in the width direction may be greater than a ratio of the outer periphery to a cross-sectional area of the inner periphery and the outer periphery covering, from the stacking direction, another pair of faces of the laminate that are opposed to each other in the stacking direction.
[0016] In the above-mentioned multilayer ceramic electronic component, a thickness of the inner peripheral portion and the outer peripheral portion covering a pair of faces of the laminate opposing each other in the width direction may be 13% or more of a size of the multilayer ceramic electronic component in the width direction.
[0017] In the above-mentioned multilayer ceramic electronic component, a thickness of the inner peripheral portion and the outer peripheral portion covering a pair of faces of the laminated portion opposing each other in the width direction may be 15% or less of a size of the multilayer ceramic electronic component in the width direction.
[0018] In the above-mentioned monolithic ceramic electronic component, in the cross-sectional view, the number of pores in the outer peripheral portion having a ratio of the length of the shortest portion to the length of the longest portion of less than 0.45 may be 50% or less of the number of pores having a ratio of the length of the shortest portion to the length of the longest portion of 0.45 or more.
[0019] In the above-described monolithic ceramic electronic component, the pores in the outer periphery may be filled with an organic substance.
[0020] The circuit board of the present invention has a multilayer ceramic electronic component mounted thereon, the multilayer ceramic electronic component having a laminated portion in which a plurality of dielectric layers and a plurality of internal electrode layers are laminated, an inner peripheral portion including a dielectric covering a periphery of the laminated portion in a cross-sectional view taken along a stacking direction of the laminated portion and a width direction of the laminated portion approximately perpendicular to the stacking direction, and an outer peripheral portion including a dielectric covering a periphery of the inner peripheral portion in the cross-sectional view, wherein a ratio of a sum of cross-sectional areas of pores in the inner peripheral portion to a cross-sectional area of the inner peripheral portion in the cross-sectional view is smaller than a ratio of a sum of cross-sectional areas of pores in the outer peripheral portion to a cross-sectional area of the outer peripheral portion.
[0021] The electronic component packaging of the present invention has an accommodating section provided with a plurality of recesses for accommodating a multilayer ceramic electronic component, and a sealing section for sealing openings of the recesses, wherein the multilayer ceramic electronic component has a lamination section in which a plurality of dielectric layers and a plurality of internal electrode layers are laminated, an inner peripheral section including a dielectric that covers a periphery of the lamination section in a cross-sectional view taken along a lamination direction of the lamination section and a width direction of the lamination section that is approximately perpendicular to the lamination direction, and an outer peripheral section including a dielectric that covers a periphery of the inner peripheral section in the cross-sectional view, wherein a ratio of a sum of cross-sectional areas of pores in the inner peripheral section to a cross-sectional area of the inner peripheral section is smaller than a ratio of a sum of cross-sectional areas of pores in the outer peripheral section to a cross-sectional area of the outer peripheral section in the cross-sectional view.
[0022] a step of stacking the plurality of first dielectric green sheets such that the internal electrode patterns face each other via the first dielectric green sheets; a step of stacking a pair of second dielectric green sheets on both sides in the stacking direction of the plurality of stacked first dielectric green sheets; a step of stacking a pair of third dielectric green sheets, the pair of third dielectric green sheets containing more resin than the pair of second dielectric green sheets, on both sides in the stacking direction of the pair of second dielectric green sheets; a step of dividing the stacked plurality of first dielectric green sheets, the pair of second dielectric green sheets, and the pair of third dielectric green sheets into a plurality of laminates having a substantially rectangular parallelepiped shape; a step of forming a pair of first ceramic layers covering a pair of surfaces facing each other in a width direction of the laminate substantially perpendicular to the stacking direction of the laminate;
[0023] The above manufacturing method may further include a step of immersing the laminate in an organic substance so that the organic substance is contained in pores formed by volatilization of the resin in the step of firing the laminate.
[0024] In the above manufacturing method, the organic matter may be cellulose, PVB, or an aromatic material.
[0025] In the above manufacturing method, the pair of second dielectric green sheets or the second ceramic layer may contain a flocculant. Effect of the Invention
[0026] According to the present invention, the reliability of multilayer ceramic electronic components can be improved. [Brief description of the drawings]
[0027] [Figure 1]FIG. 1 is a perspective view showing an example of a multilayer ceramic capacitor. [Diagram 2] FIG. 2 is a cross-sectional view of the multilayer ceramic capacitor taken along line AA in FIG. [Diagram 3] 2 is a cross-sectional view of the multilayer ceramic capacitor taken along line BB in FIG. [Figure 4] 3 is a cross-sectional view of the multilayer ceramic capacitor taken along line CC in FIG. 2. [Diagram 5] FIG. 5 is a cross-sectional view showing an example of an inner peripheral portion and an outer peripheral portion of a multilayer ceramic capacitor. [Figure 6] FIG. 6 is a side view showing an example of a circuit board on which a multilayer ceramic capacitor is mounted. [Figure 7] FIG. 7 is a diagram showing examples of the shape of the pore P. [Figure 8] FIG. 8 is a plan view showing an example of a package in which a multilayer ceramic capacitor is packaged. [Figure 9] FIG. 9 is a flowchart showing an example of a manufacturing process for a multilayer ceramic capacitor. [Figure 10] FIG. 10 is a cross-sectional view showing an example of a process from a green sheet forming step to a pressure bonding step. [Figure 11] FIG. 11 is a side view (part 1) showing an example of an inner side margin forming step when the end face of the laminate before firing is viewed from the front. [Figure 12] FIG. 12 is a side view (part 2) showing an example of an inner side margin forming step when the end face of the laminate before firing is viewed from the front. [Figure 13] FIG. 13 is a side view (part 3) showing an example of an inner side margin forming step when the end face of the laminate before firing is viewed from the front. [Figure 14] FIG. 14 is a side view (part 1) showing an example of an outer side margin forming step when the end face of the laminate before firing is viewed from the front. [Figure 15] FIG. 15 is a side view (part 2) showing an example of an outer side margin forming step when the end face of the laminate before firing is viewed from the front. [Figure 16]FIG. 16 is a side view (part 3) showing an example of an outer side margin forming step when the end face of the laminate before firing is viewed from the front. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] [Embodiment] (Structure of multilayer ceramic capacitors) Fig. 1 is a perspective view showing an example of a multilayer ceramic capacitor 1. Fig. 2 is a cross-sectional view of the multilayer ceramic capacitor 1 taken along line AA in Fig. 1. Fig. 3 is a cross-sectional view of the multilayer ceramic capacitor 1 taken along line BB in Fig. 1. Fig. 4 is a cross-sectional view of the multilayer ceramic capacitor 1 taken along line CC in Fig. 2.
[0029] The multilayer ceramic capacitor 1 is an example of a multilayer ceramic electronic component. The multilayer ceramic capacitor 1 has a laminated chip 2 having a substantially rectangular parallelepiped shape, and external electrodes 3a, 3b provided on a pair of end faces 2A, 2B of the laminated chip 2 that face each other.
[0030] 1 to 4 show an X direction, a Y direction, and a Z direction which are approximately perpendicular to one another. The X direction is the length (L) direction of the multilayer ceramic capacitor 1, and coincides with the direction in which a pair of end faces 2A, 2B of the multilayer chip 2 face each other. The Y direction is the width (W) direction of the multilayer ceramic capacitor 1, and coincides with the direction in which a pair of side faces 2E, 2F of the multilayer chip 2 face each other. The Z direction is the height (H) direction of the multilayer ceramic capacitor 1, and coincides with the stacking direction of the multilayer ceramic capacitor 1. An upper surface 2C and a lower surface 2D of the multilayer chip 2 face each other in the stacking direction.
[0031] The laminated chip 2 has a laminated section 2s having a generally rectangular parallelepiped shape with a laminated structure, a pair of side margin sections 40, 41 that cover the laminated section 2s by sandwiching it from both sides in the width direction, and cover sections 20, 21 that cover the laminated section 2s by sandwiching it from both sides in the stacking direction.
[0032] The multilayer section 2s is formed by alternately stacking dielectric layers 22 containing a ceramic material that functions as a dielectric and internal electrode layers 23. The multilayer section 2s has a stacked structure in which the internal electrode layers 23 face each other with the dielectric layers 22 sandwiched therebetween in the stacking direction, and realizes the capacitance of the multilayer ceramic capacitor 1.
[0033] When viewed from the front in the lamination direction, the internal electrode layer 23 has a substantially rectangular shape, with one end alternately drawn out to the end faces 2A and 2B. In the example of Fig. 4, one end 23L of the internal electrode layer 23 in the length direction is drawn out to the end face 2A and connected to one of the external electrodes 3b. The other end 23R of the internal electrode layer 23 is not drawn out to the end face 2B and is not connected to the external electrode 3b. Both end portions 23U and 23D of the internal electrode layer 23 in the width direction are covered by side margin portions 40 and 41, respectively.
[0034] 3, the side margin portion 40 is provided on a side surface 2E of the laminated chip 2, and the side margin portion 41 is provided on a side surface 2F of the laminated chip 2. The side margin portions 40, 41 extend along the laminated chip 2 in the stacking direction.
[0035] The side margin portion 40 has an inner side margin layer 400 and an outer side margin layer 401 laminated in the width direction, and the side margin portion 41 has an inner side margin layer 410 and an outer side margin layer 411 laminated in the width direction. The outer side margin layer 401 is exposed to the side surface 2E, and the outer side margin layer 411 is exposed to the side surface 2F.
[0036] The inner side margin layers 400, 410 cover the side surfaces 2E, 2F of the laminate 2p. The inner side margin layers 400, 410 are covered by the outer side margin layers 401, 411 in the stacking direction and width direction of the laminated portion 2s, and are therefore not exposed on the upper surface 2C, the lower surface 2D, and the side surfaces 2E, 2F.
[0037] Each of the inner side margin layers 400, 410 and the outer side margin layers 401, 411 includes a plurality of pores P. The pores P are formed by volatilization of a binder such as a resin during the manufacturing process of the multilayer ceramic capacitor 1.
[0038] Moreover, the cover portion 20 is provided on the upper surface 2C of the laminated chip 2, and the cover portion 21 is provided on the lower surface 2D of the laminated chip 2. The cover portions 20, 21 extend between the side margin portions 40, 41 along the width direction of the laminated chip 2.
[0039] The cover part 20 has an inner cover layer 200 and an outer cover layer 201 laminated in the stacking direction of the laminated chip 2, and the cover part 21 has an inner cover layer 210 and an outer cover layer 211 laminated in the stacking direction of the laminated chip 2. The outer cover layer 201 is exposed on the upper surface 2C, and the outer cover layer 211 is exposed on the lower surface 2D.
[0040] Both ends of the inner cover layer 200 in the width direction are connected to the ends of the inner side margin layers 400, 410 on the upper surface 2C side. Both ends of the inner cover layer 210 in the width direction are connected to the ends of the inner side margin layers 400, 410 on the lower surface 2D side.
[0041] Both ends of the outer cover layer 201 in the width direction are connected to the ends of the outer side margin layers 401, 411 on the upper surface 2C side. Both ends of the outer cover layer 211 in the width direction are connected to the ends of the outer side margin layers 401, 411 on the lower surface 2D side.
[0042] The inner cover layers 200, 210 and the outer cover layers 201, 211 each contain a plurality of pores P. Note that the dielectric layer 22 also contains pores P, but these are not shown in the figure.
[0043] In this way, the periphery of the laminated portion 2s is covered by the inner side margin layers 400, 410 and the inner cover layers 200, 210, and the periphery of the inner side margin layers 400, 410 and the inner cover layers 200, 210 is further covered by the outer side margin layers 401, 411 and the outer cover layers 201, 211.
[0044] The internal electrode layer 23 is mainly composed of a base metal such as Ni (nickel), Cu (copper), or Sn (tin). Noble metals such as Pt (platinum), Pd (palladium), Ag (silver), or Au (gold), or alloys containing these metals, may also be used as the internal electrode layer 23. The thickness of the internal electrode layer 23 is, for example, 0.3 to 1.3 (μm).
[0045] The dielectric layer 22 has a main phase made of a ceramic material having a perovskite structure represented by the general formula ABO3. 3-α For example, the ceramic material includes BaTiO3 (barium titanate), CaZrO3 (calcium zirconate), CaTiO3 (calcium titanate), SrTiO3 (strontium titanate), MgTiO3 (magnesium titanate), BaTiO3 (barium titanate) which forms a perovskite structure, 1-x-y Ca x Sr y Ti 1-z Zr z O3 (0≦x≦1, 0≦y≦1, 0≦z≦1), etc. 1-x-y Ca x Sr y Ti 1-z Zr z O3 is barium strontium titanate, barium calcium titanate, barium zirconate, barium titanate zirconate, calcium titanate zirconate, barium calcium titanate zirconate, etc. The thickness of the dielectric layer 22 is, for example, 0.3 to 4.0 (μm). The side margin portions 40, 41 and the cover portions 20, 21 also have the same composition as the dielectric layer 22.
[0046] The external electrodes 3a, 3b cover the end faces 2A, 2B of the laminated chip 2 that face each other in the longitudinal direction of the laminated ceramic capacitor 1. The external electrodes 3a, 3b extend onto the upper face 2C, the lower face 2D, and the side faces 2E, 2F. However, the external electrodes 3a, 3b are spaced apart from each other on the upper face 2C, the lower face 2D, and the side faces 2E, 2F.
[0047] (Inner and outer pore area ratio) Fig. 5 is a cross-sectional view showing an example of an inner peripheral portion Sin and an outer peripheral portion Sout of a multilayer ceramic capacitor 1. Fig. 5 shows a cross-sectional view of a multilayer chip 2 taken along the lamination direction and width direction. In Fig. 5, the same components as those in Fig. 3 are given the same reference numerals, and the description thereof will be omitted.
[0048] The multilayer ceramic capacitor 1 has a multilayer portion 2s, and an inner peripheral portion Sin and an outer peripheral portion Sout surrounding the multilayer portion 2s. The inner peripheral portion Sin is a region sandwiched between boundary lines Bin and Bout, which are substantially rectangular in shape. The inner peripheral portion Sin includes a dielectric that covers the multilayer portion 2s. The outer peripheral portion Sout is a region outside the boundary line Bout. The outer peripheral portion Sout includes a dielectric that covers the inner peripheral portion Sin.
[0049] The ratio of the sum of the cross-sectional areas of the pores P in the inner circumferential portion Sin to the cross-sectional area of the inner circumferential portion Sin (hereinafter referred to as the pore area ratio of the inner circumferential portion Sin) is smaller than the ratio of the sum of the cross-sectional areas of the pores P in the outer circumferential portion Sout to the cross-sectional area of the outer circumferential portion Sout (hereinafter referred to as the pore area ratio of the outer circumferential portion Sout). Therefore, when stress acts on the laminated chip 2 from the outside, the stress can be alleviated by the pores P in the inner circumferential portion Sin and the outer circumferential portion Sout. Furthermore, since the pore area ratio of the inner circumferential portion Sin is smaller than the pore area ratio of the outer circumferential portion Sout, the occurrence of cracks originating from the pores P in the inner circumferential portion Sin and damage to the laminated portion 2s adjacent to the inner circumferential portion Sin is suppressed.
[0050] The inner peripheral portion Sin and the outer peripheral portion Sout are determined based on, for example, line segments V1 to V4 along the lamination direction and line segments H1 to H4 along the width direction. The line segments V2, V3, H2, and H3 surround a laminated portion 2s in which the dielectric layers 22 and the internal electrode layers 23 are alternately laminated.
[0051] The line segments V2 and V3 extend in the lamination direction along the ends of the internal electrode layers 23. Here, there is variation in the positions of the ends of the internal electrode layers 23 in the width direction, i.e., in the Y axis. For this reason, the coordinate of the line segment V2 in the Y axis direction is located inward from the side surface 2E by the average value of the distance in the Y axis direction between each end of the internal electrode layers 23 on the side surface 2E side and the side surface 2E. Also, the coordinate of the line segment V3 in the Y axis direction is located inward from the side surface 2F by the average value of the distance in the Y axis direction between each end of the internal electrode layers 23 on the side surface 2F side and the side surface 2F.
[0052] For example, when the number of the internal electrode layers 23 is 30 or less, the average value of the distances in the Y-axis direction between the ends of all the internal electrode layers 23 and the side surfaces 2E, 2F may be used. Also, when the number of the internal electrode layers 23 is more than 30, the average value of the distances in the Y-axis direction between the ends of the 10 internal electrode layers 23 close to the top surface 2C, the 10 internal electrode layers 23 close to the bottom surface 2D, and the 10 internal electrode layers 23 near the middle between the top surface 2C and the bottom surface 2D may be used.
[0053] Moreover, the line segment H2 extends in the width direction along the internal electrode layer 23 that is closest to the top surface 2C, and the line segment H3 extends in the width direction along the internal electrode layer 23 that is closest to the bottom surface 2D, among the internal electrode layers 23. The positions of the line segments H2 and H3 in the stacking direction, i.e., on the Z-axis, are determined, for example, by the line segment along the internal electrode layer 23 that is closest to the top surface 2C and the internal electrode layer 23 that is closest to the bottom surface 2D. Below, an explanation will be given using the internal electrode layer 23 closest to the top surface 2C as an example.
[0054] Symbol Ga is an enlarged view of a central portion (see dotted line frame) of the internal electrode layer 23 closest to the top surface 2C, the central portion having a length one-third the widthwise distance between line segments V2 and V3. The coordinate of line segment H2 in the stacking direction is determined from the average value of the coordinates in the stacking direction (coordinates on the Z axis) of any number (e.g., 30 points) of positions m on the surface on the top surface 2C side of the uneven internal electrode layer 23. Line segment H2 is an extension line extended along the Y direction to the side margin portions 40, 41 with its coordinate as the Y coordinate.
[0055] Moreover, the line segments V1, V4, H1, and H4 are set so as to surround the regions in which the pore area ratio is less than a predetermined value in the cover portions 20 and 21 and the side margin portions 40 and 41. Here, the predetermined value is, for example, 3(%), but is not limited thereto. The line segments V1 and V4 are parallel to the line segments V2 and V3, and the line segments H1 and H4 are parallel to the line segments H2 and H3. The position of the line segment V1 in the width direction is set at a position halfway through the thickness d1 of the side margin portion 40, or at a position closer to the laminated portion 2s side than that halfway position. The position of the line segment V4 in the width direction is set at a position halfway through the thickness d2 of the side margin portion 41, or at a position closer to the laminated portion 2s side than that halfway position.
[0056] The position of line segment H1 in the stacking direction is set to a position halfway through the thickness e1 of cover portion 20 on the upper surface 2C side, or a position closer to stack portion 2s than that halfway position. The position of line segment H4 in the stacking direction is set to a position halfway through the thickness e2 of cover portion 21 on the lower surface 2D side, or a position closer to stack portion 2s than that halfway position.
[0057] As a result, the line segments V1, V4, H1, and H4 define the boundary line Bout between the inner periphery Sin and the outer periphery Sout. Here, the four corners of the boundary line Bout have a shape in which the right-angled corners where the line segments V1, V4, H1, and H4 intersect are cut out. For example, the corner where the line segments H1 and V1 intersect is a corner cut out by a line j that is parallel to a line k that connects the intersection point of the line segment H1 and the line segment V2 and the intersection point of the line segment H2 and the line segment V1. Here, the line j is defined as follows:
[0058] Reference symbol Gb is an enlarged view of a cross section (see dotted frame) of a corner portion extending from the top surface 2C to the side surface 2E. First, an intersection point Qa between line segment H2 and line segment V2, an intersection point Qc between line segment H1 and line segment V1, and an intersection point Qb at which a line segment n passing through intersection point Qa intersects with the outer surface of the outer periphery Sout when extended are defined. If the distance between points Qa and Qb on line segment n is s, the distance a between line segment k and line segment j on line segment n is set to be equal to or less than one-fifth of the distance s. The other three corner portions are defined in the same manner. In this manner, the boundary line Bout is set.
[0059] Moreover, the line segments V2, V3, H2, and H3 define the boundary line Bin between the inner periphery Sin and the stacked portion 2s. Here, the four corners of the boundary line Bin are corners with a shape similar to the corners of the outer boundary line Bout. In this manner, the boundary line Bin is set.
[0060] For example, the pore area ratio of the inner peripheral portion Sin is less than 3(%), whereas the pore area ratio of the outer peripheral portion Sout is 3(%) or more. With this pore area ratio, the outer peripheral portion Sout exerts sufficient elastic force to suppress stress acting from the outside, and it is possible to sufficiently prevent cracks from occurring from the pores P of the inner peripheral portion Sin. More preferably, the pore area ratio of the inner peripheral portion Sin may be 2.5(%) or less, whereas the pore area ratio of the outer peripheral portion Sout may be 3(%) or more.
[0061] Also, the pore area ratio of the outer peripheral portion Sout is preferably 12(%) or less. This is because if the pore area ratio of the outer peripheral portion Sout is excessively large, the effect of crack generation due to insufficient hardness is stronger than the effect of relieving stress. More preferably, the pore area ratio of the outer peripheral portion Sout may be 10(%) or less.
[0062] Also, the cross-sectional area of the outer peripheral portion Sout is larger than that of the inner peripheral portion Sin. Therefore, compared with the case where the cross-sectional areas of the outer peripheral portion Sout and the inner peripheral portion Sin are equal, the number of pores P in the outer peripheral portion Sout can be increased, and cracks can be more effectively suppressed. From this viewpoint, for example, the cross-sectional area of the outer peripheral portion Sout is preferably 82(%) or more of the total cross-sectional area of the inner peripheral portion Sin and the outer peripheral portion Sout. Also, since cracks originating from the pores P in the inner peripheral portion Sin may occur and damage the laminated portion 2s adjacent to the inner peripheral portion Sin, from the viewpoint that it is desirable to secure a minimum pore area ratio of the inner peripheral portion Sin, the cross-sectional area of the outer peripheral portion Sout is preferably 90(%) or less of the total cross-sectional area of the inner peripheral portion Sin and the outer peripheral portion Sout.
[0063] From the viewpoint of suppressing cracks, it is preferable that the maximum diameter of the pores P in the inner circumferential portion Sin is less than 0.4 (μm) and the maximum diameter of the pores P in the outer circumferential portion Sout is 0.4 (μm) or more. This is because the smaller the diameter of the pores P in the inner circumferential portion Sin, the less likely cracks will occur due to the pores P, and the larger the diameter of the pores P in the outer circumferential portion Sout, the more the stress can be relaxed. More preferably, the maximum diameter of the pores P in the inner circumferential portion Sin may be less than 0.1 (μm) and the maximum diameter of the pores P in the outer circumferential portion Sout may be 0.45 (μm) or more. In addition, the maximum diameter of the pores P in the outer circumferential portion Sout may be 1.0 (μm) or less. In this case, if the diameter of the pores P in the outer circumferential portion Sout becomes excessively large, the effect of cracks occurring due to insufficient hardness will be stronger than the effect of relaxing stress, so that cracks are more effectively suppressed.
[0064] Moreover, the ratio of the cross-sectional area of the outer peripheral portion Sout to the cross-sectional area of the side margin portions 40, 41 may be larger than the ratio of the cross-sectional area of the outer peripheral portion Sout to the cross-sectional area of the cover portions 20, 21. In this case, the thickness of the outer peripheral portion Sout can be increased in the width direction rather than in the stacking direction of the stacked portion 2s, so that the pressure Ph applied from the width direction to the stacked chip 2 can be dispersed more effectively than the pressure Pv applied from the stacking direction to protect the stacked portion 2s from the pressure.
[0065] Here, the pressure Pv applied from the stacking direction acts substantially perpendicularly to the electrode surfaces of the internal electrode layers 23, and the pressure Ph applied from the width direction acts parallel to the ends of the internal electrode layers 23. For this reason, in the internal electrode layers 23, the area of the region to which the pressure Pv is applied is larger than the area to which the pressure Ph is applied, so that the pressure Pv is more easily dispersed than the pressure Ph. Conversely, the pressure Ph is less easily dispersed, so that it has a greater effect on the internal electrode layers 23 (for example, short circuits between the internal electrode layers 23) than the pressure Pv.
[0066] Therefore, by making the area ratio of the outer circumferential portion Sout in the side margin portions 40, 41 larger than the area ratio of the outer circumferential portion Sout in the cover portions 20, 21 as described above, the laminate portion 2s can be effectively protected from the pressure Ph. Note that the side margin portions 40, 41 are an example of the inner circumferential portion Sin and the outer circumferential portion Sout on the outer side from a pair of faces of the laminate portion 2s facing each other in the width direction, and the cover portions 20, 21 are an example of the inner circumferential portion Sin and the outer circumferential portion Sout that cover, from the stacking direction, the faces of another pair of laminate portions 2s facing each other in the stacking direction.
[0067] Furthermore, the thicknesses d1, d2 of the side margin portions 40, 41 in the width direction may be 13% or more of the width direction size of the multilayer ceramic capacitor 1, i.e., the width W. In this case, too, the multilayer portion 2s can be effectively protected from the pressure Ph for the same reasons as above. More preferably, the thicknesses d1, d2 of the side margin portions 40, 41 may be 15% or more of the width W of the multilayer ceramic capacitor 1.
[0068] Furthermore, in order to reduce stress when mounted on a circuit board, the size of the multilayer ceramic capacitor 1 is specified to be 1.9 mm in the length direction, 0.125 mm in the width direction, and 0.125 mm or less in the lamination direction.
[0069] Fig. 6 is a side view showing an example of a circuit board 9 on which a multilayer ceramic capacitor 1 is mounted. In Fig. 6, the same components as in Fig. 1 are given the same reference numerals and their description will be omitted. The multilayer ceramic capacitor 1 is connected to pads (not shown) of the circuit board 9 by solder 90 via external electrodes 3a and 3b.
[0070] 6 shows a state when the circuit board 9 is not deflected (normal state) and a state when the circuit board 9 is deflected (deflected state). When the circuit board 9 is deflected, a stress F acts on the multilayer ceramic capacitor 1 from the external electrodes 3a, 3b toward the outside along the circuit board 9. For this reason, the smaller the size of the multilayer ceramic capacitor 1, the greater the stress applied per unit volume, and therefore the more effectively the stress can be dispersed by the pores P.
[0071] Therefore, when the size of the multilayer ceramic capacitor 1 is 0.25 mm or less in the length direction, 0.125 mm or less in the width direction, and 0.125 mm or less in the lamination direction, the pores P can disperse stress more effectively.
[0072] Fig. 7 is a diagram showing an example of the shape of a pore P. In this embodiment, the shape of a pore P is defined by the length RL of the longest part of the pore P and the length RS of the shortest part of the pore P. For example, when the ratio of the length RS to the length RL (RS / RL) is less than 0.45, the pore P has a shape in which two circles are joined together, as shown in the upper part of the page of Fig. 7. In this case, since the joined part is constricted, when stress is applied, cracks are likely to occur from the constriction, as shown by the symbol X.
[0073] Furthermore, when RS / RL is 0.45 or more, the pores P are substantially circular, as shown in the lower part of the page in Fig. 7. In this case, there are no constrictions in the pores P that serve as the starting points for cracks, so cracks are less likely to occur than when RS / RL is less than 0.45.
[0074] Therefore, in the cross-sectional view shown in Figure 5, for example, when the number of pores P within the inner peripheral portion Sin having an RS / RL of less than 0.45 is 50% or less of the number of pores P having an RS / RL of 0.45 or more, the occurrence of cracks is suppressed.
[0075] In addition, it is preferable that the pores P in the inner peripheral portion Sin and the outer peripheral portion Sout are filled with an organic material such as a resin. In this way, not only is stress relieved by the fluid resin, but the hardness of the outer peripheral portion Sout is maintained by filling the gaps of the pores P with the resin, so that cracks due to stress and cracks due to insufficient hardness are simultaneously suppressed. An example of the resin is an epoxy resin, but is not limited thereto. In addition, a mixture of multiple types of organic materials may be contained in the pores P. The content of the organic material is determined, for example, according to the size of the pores P. If the maximum particle size of the pores P is 0.4 to 1.0 (μm) or less, the viscosity of the organic material is preferably 3.2 (P). In addition, only the pores P close to the outer surface of the multilayer ceramic capacitor 1 may be filled with the organic material.
[0076] (Multilayer ceramic capacitor packaging) 8 is a plan view showing an example of a packaging body 8 that packages a multilayer ceramic capacitor 1. The packaging body 8 is an example of an electronic component packaging body. The packaging body 8 has a tape-like form extending in a predetermined direction, and contains a plurality of multilayer ceramic capacitors 1 arranged in that direction.
[0077] The packaging body 8 has a housing portion 80 and a sealing portion 81. The housing portion 80 is, for example, a carrier tape, and extends in a predetermined direction. In the housing portion 80, recesses 800 for housing the multilayer ceramic capacitors 1 are formed at predetermined intervals. The size of the recesses 800 is set according to the size of the multilayer ceramic capacitor 1 to be housed.
[0078] The sealing portion 81 is provided on the housing portion 80 so as to seal the opening 800a of the recess 800, which serves as an outlet for the multilayer ceramic capacitor 1. The sealing portion 81 is attached to the surface of the housing portion 80 in a releasable manner.
[0079] (Manufacturing method of multilayer ceramic capacitors) 9 is a flow chart showing an example of a manufacturing process for the multilayer ceramic capacitor 1. This manufacturing process is an example of a method for manufacturing a multilayer ceramic electronic component.
[0080] 10 is a cross-sectional view showing an example of a process from the green sheet forming step St1 to the pressure bonding step St6. FIG 10 shows a cross section along the lamination direction and the width direction.
[0081] (Green sheet molding process) First, a green sheet forming step St1 is performed. In this step, a binder such as polyvinyl butyral (PVB) resin, an organic solvent such as ethanol or toluene, and a plasticizer are added to a dielectric material obtained by adding various additive compounds (such as sintering aids) to ceramic powder, and then wet-mixed. The obtained slurry is used to coat the dielectric green sheets 7, 70a, 70b, 71a, and 71b on a substrate by, for example, a die coater method or a doctor blade method, and then dried. The substrate is, for example, a PET (polyethylene terephthalate) film.
[0082] As additive compounds for the ceramic powder, oxides of Mg (magnesium), Mn (manganese), V (vanadium), Cr (chromium), rare earth elements (Y (yttrium), Sm (samarium), Eu (europium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium) and Yb (ytterbium)), as well as oxides or glasses of Co (cobalt), Ni, Li (lithium), B (boron), Na (sodium), K (potassium) and Si (silicon) are used.
[0083] The dielectric green sheet 7 is an example of a first dielectric green sheet. The dielectric green sheet 7 mainly forms the dielectric layer 22.
[0084] The dielectric green sheets 70a and 70b are examples of the second dielectric green sheets, and the dielectric green sheets 71a and 71b are examples of the third dielectric green sheets. The dielectric green sheet 70a mainly forms the inner cover layer 200, and the dielectric green sheet 71a mainly forms the outer cover layer 201. The dielectric green sheet 70b mainly forms the inner cover layer 210, and the dielectric green sheet 71b mainly forms the outer cover layer 211.
[0085] The dielectric green sheets 71a and 71b contain more resin as a binder than the dielectric green sheets 70a and 70b. The difference in the weight ratio of the resin amount to the ceramic powder between the dielectric green sheets 71a and 71b is preferably, for example, 3% or more.
[0086] (Internal electrode printing process) Next, the internal electrode printing process St2 is performed. In this process, the conductive paste containing ceramic particles is applied to the surfaces of the dielectric green sheets 7 to form the internal electrode patterns 6. The internal electrode patterns 6 have a shape corresponding to the internal electrode layers 23.
[0087] In this process, a metal conductive paste for forming internal electrodes containing an organic binder is printed on the dielectric green sheet 7 on the substrate by gravure printing or the like to form a film of multiple internal electrode patterns 6 spaced apart from one another. Ceramic particles are added to the conductive paste as a co-material. The main component of the ceramic particles is not particularly limited, but is preferably the same as the main ceramic component of the dielectric layer 22.
[0088] (Dielectric layer lamination process) Next, a dielectric layer lamination step St3 is performed. In this step, a plurality of dielectric green sheets 7 on which internal electrode patterns 6 that become the internal electrode layers 23 are printed are laminated.
[0089] (Inner cover layer lamination process) Next, an inner cover layer lamination step St4 is performed. In this step, the dielectric green sheets 70a and 70b which will become the inner cover layers 200 and 210 are laminated on both sides of the laminated plurality of dielectric green sheets 7 in the lamination direction.
[0090] (Outer cover layer lamination process) Next, an outer cover layer lamination step St5 is performed. In this step, the dielectric green sheets 71a and 71b which will become the outer cover layers 201 and 211 are laminated on both sides of the laminated dielectric green sheets 70a and 70b in the lamination direction.
[0091] (Crimping process) Next, a pressure bonding step St6 is performed. In this step, pressure is applied to the laminated dielectric green sheets 7, 70a, 70b, 71a, and 71b to bond them together. Examples of pressure bonding methods include, but are not limited to, a hydrostatic press.
[0092] (cutting process) Next, a cutting step St7 is performed. This step is an example of a step of dividing the laminated sheet 7S obtained by pressing into a plurality of laminates each having a substantially rectangular parallelepiped shape. In this step, the laminated sheet 7S is cut in the stacking direction along a predetermined cutting line LW with a blade, thereby obtaining a plurality of pre-fired laminates. This laminate is obtained by covering the above-mentioned laminated portion 2s with cover portions 20 and 21 on both sides in the stacking direction.
[0093] (Inner side margin forming process) Next, an inner side margin forming step St8 is performed. In this step, ceramic sheets that will become the inner side margin layers 400, 410 after firing are formed.
[0094] 11 to 13 are side views showing an example of the inner side margin forming step St8 when the end face 2A of the laminate 2p before firing is viewed from the front. In this example, a process of forming an inner side margin layer 410 on one side face 2F is shown, but the process of forming an inner side margin layer 400 on the other side face 2E is also similar.
[0095] First, as shown in Fig. 11, a ceramic sheet 50 is placed on the plate surface of a flat elastic body BS. The ceramic sheet 50 corresponds to an inner side margin layer 410 after firing. The ceramic sheet 50 is an example of a first ceramic layer.
[0096] One side surface 2E of the laminate 2p is fixed with tape TS, and the laminate 2p is placed above the ceramic sheet 50 so that the other side surface 2F faces the surface of the ceramic sheet 50. At this time, the ceramic sheet 50 has an area substantially equal to the area of the region R on the side surface 2F of the laminate 2p within the range from one inner cover layer 200 to the other inner cover layer 210, as shown by the dotted line.
[0097] Next, the tape TS is moved downward by a pressing device (not shown), whereby the laminate 2p moves toward the ceramic sheet 50 as indicated by the reference symbol D. After the movement, the ceramic sheet 50 comes into contact with the region R of the side surface 2F of the laminate 2p.
[0098] 12, the side surface 2F of the laminate 2p is pressed against the surface of the ceramic sheet 50. Therefore, the surface of the ceramic sheet 50 is attached to the region R of the side surface 2F of the laminate 2p. As a result, the ceramic sheet 50 covers the region R of the side surface 2F. The side surfaces 2F and 2E are an example of a pair of surfaces facing each other in the width direction of the laminate 2p.
[0099] 13, the tape TS is moved upward by a pressing device (not shown). This causes the laminate 2p to move away from the elastic body BS as indicated by the symbol U. At this time, the ceramic sheet 50 is attached to the side surface 2F of the laminate portion 2s, and is formed as an inner side margin layer 410 after firing.
[0100] (External side margin forming process) Next, an outer side margin forming step St9 is performed. In this step, ceramic sheets that will become the outer side margin layers 401, 411 after firing are formed.
[0101] 14 to 16 are side views showing an example of an outer side margin forming step St9 when the end face 2A of the laminate 2p before firing is viewed from the front. In this example, a process of forming an outer side margin layer 411 on one side face 2F is shown, but the process of forming an outer side margin layer 401 on the other side face 2E is similar.
[0102] 14, a ceramic sheet 51 is placed on the plate surface of a flat elastic body BS. The ceramic sheet 51 corresponds to the outer side margin layer 411 after firing. The ceramic sheet 51 contains more resin than the ceramic sheet 50.
[0103] One side surface 2E of the laminate 2p is fixed with tape TS, and the laminate 2p is placed above the ceramic sheet 51 so that the other side surface 2F faces the surface of the ceramic sheet 51. At this time, the ceramic sheet 51 has an area larger than the side surface 2F of the laminate 2p.
[0104] Next, the tape TS is moved downward by a pressing device (not shown). This causes the laminate 2p to move toward the ceramic sheet 51 as indicated by the symbol Da. After the movement, the ceramic sheet 51 comes into contact with the ceramic sheet 50 attached onto the side surface 2F of the laminate 2p.
[0105] 15, the ceramic sheet 50 on the side surface 2F of the laminate 2p is pressed against the surface of the ceramic sheet 51. Therefore, the surface of the ceramic sheet 51 sticks to the surface of the ceramic sheet 50.
[0106] At this time, the pressed portion of the ceramic sheet 51 is depressed by the pressure from the ceramic sheet 50 on the laminate 2p side, and the elastic body BS below it is also depressed. The corresponding portion of the ceramic sheet 51 is pressed against the ceramic sheet 50 on the laminate 2p side by the restoring force from the elastic body BS. As a result, a part of the ceramic sheet 51 is attached so as to cover the exposed ends 2Fa, 2Fb on the side surface 2F and the exposed surface of the ceramic sheet 50. Here, the ends 2Fa, 2Fb correspond to the end faces in the width direction of the outer cover layers 211, 201, respectively.
[0107] At this time, the ceramic sheet 50 on the side surface 2F is located inside the lower ceramic sheet 51, and therefore no exposed portion is present. When the pressing force of the laminate 2p increases thereafter, a shear force is generated between the portion to which the ceramic sheet 51 is attached and the other portion, and the two portions are separated from each other.
[0108] Next, as shown in Fig. 16, the tape TS is moved upward by a pressing device (not shown). As a result, the laminate 2p moves away from the elastic body BS as indicated by the symbol Ua. At this time, the ceramic sheet 51a separated from the ceramic sheet 51 is attached to the side surface 2F of the laminated portion 2s so as to cover the inner ceramic sheet 50 in the lamination direction and width direction of the laminate 2p, and is formed as an inner side margin layer 410 after firing. The ceramic sheet 51a is an example of a second ceramic layer.
[0109] In this manner, the inner side margin forming process St8 forms a pair of ceramic sheets 50 covering the side surfaces 2F, 2E, and the outer side margin forming process St9 forms a pair of ceramic sheets 51a covering the pair of ceramic sheets 50 in the width direction and stacking direction of the laminate 2p. In this manner, the side margin portions 41, 40 are formed on the side surfaces 2F, 2E of the laminate 2p, respectively, and the pre-fired laminated chip 2 as shown in FIG.
[0110] (Firing process) Next, a firing step St10 is performed. In this step, the laminated chip 2 before firing is subjected to a binder removal process in an N2 atmosphere at 250 to 500°C, and then fired for about 1 hour at a firing temperature of 1200°C or higher in a reducing atmosphere with an oxygen partial pressure of 0.003 (Pa), thereby sintering each particle in the laminated chip 2. As a result, the dielectric green sheet 7 becomes the dielectric layer 22, the dielectric green sheets 70a, 70b, 71a, and 71b become the cover parts 20 and 21, and the internal electrode pattern 6 becomes the internal electrode layer 23.
[0111] By this process, the resin contained in the dielectric green sheets 70a, 70b, 71a, 71b and the ceramic sheets 50, 51a volatilizes to form pores P. Here, the dielectric green sheets 71a, 71b contain more resin as a binder than the dielectric green sheets 70a, 70b. The ceramic sheet 51 contains more resin than the ceramic sheet 50. For this reason, as described above, the pore area ratio of the inner peripheral portion Sin is smaller than the pore area ratio of the outer peripheral portion Sout. Also, the pores P of the inner peripheral portion Sin can be made smaller than the pores P of the outer peripheral portion Sout. Also, since the amount of resin in the outer peripheral portion Sout is large, the adhesion of the outer peripheral portion Sout to the inner peripheral portion Sin is improved compared to when the amount of resin is small.
[0112] In addition, in order to increase the diameter of the pores P in the outer peripheral portion Sout, a flocculant may be added to the slurry of the dielectric green sheets 71a, 71b and the ceramic sheet 51. Here, the flocculant includes a material that flocculates resin. The flocculant acts to evaporate the flocculated resin, thereby increasing the diameter of the pores P. Examples of the flocculant include polyacrylamide, polyacrylamide, polyacrylic acid ester, polyacrylic acid ester, polydadomac, polymian, and dicyandiamide.
[0113] (Resin impregnation process) Next, a resin impregnation step St11 is performed. In this step, the laminated chip 2 is immersed in resin so that the resin is contained in the pores P. This allows the resin to be impregnated into the pores P near the outer surface. For example, the viscosity of the resin is 0.1 to 0.2 (P), and the immersion time is one hour. At this time, the resin in which the laminated chip 2 is immersed may be heated to allow the resin to be impregnated into the inner pores P as well. In this case, the viscosity of the resin may be 2.2 to 3.2 (P). The resin may be, but is not limited to, an epoxy resin.
[0114] Thereafter, the laminated chip 2 is degassed using a vacuum heating degassing device. At this time, the pressure around the laminated chip 2 is reduced to 0.1 (MPa) and the degassing process is repeated until degassing is confirmed. Thereafter, the laminated chip 2 is immersed in resin again so that the resin is contained in the pores P. Note that other organic matter may be contained in the pores P instead of resin. Examples of organic matter include cellulose, PVB, and aromatics. These have the advantage of being highly stable and not easily denatured.
[0115] (External electrode formation process) Next, an external electrode formation process St12 is performed. In this process, a conductive paste containing, for example, metal powder, glass frit, binder, and solvent is applied to each end face 2A, 2B, upper face 2C, lower face 2D, and each side face 2E, 2F of the laminated chip 2. After the conductive paste is applied, it is dried to form the external electrodes 3a, 3b. EXAMPLES
[0116] Next, the results of fabricating and evaluating the multilayer ceramic capacitor 1 will be described.
[0117] (Pore area ratio) [Table 1]
[0118] Table 1 shows the pore area ratios of the inner peripheral portion Sin and the outer peripheral portion Sout, and the crack occurrence rate (%). 100 samples of the multilayer ceramic capacitor 1 were produced according to the above manufacturing process, and the crack occurrence rate was measured. The size of each sample was length L of 4.5 (mm), width W of 3.2 (mm), and height H of 2.5 (mm). The pore area ratio of the inner peripheral portion Sin of the sample was 0.1 to 3.0 (%), and the pore area ratio of the outer peripheral portion Sout of the sample was 1.0 to 12.5 (%).
[0119] The crack occurrence rate was measured by a bending test of printed circuit boards. In this test, a sample was mounted on a printed circuit board with a thickness of 1.6 mm, with the mounting side facing downward, and a position of the printed circuit board equidistant (45 mm) from the sample was supported from below by a pair of support members, and the mounting position of the sample on the printed circuit board was pressed from above with a pressing jig until the bending depth was 3 mm. Samples with a crack occurrence rate of less than 45% were judged to be good products, and samples with a crack occurrence rate of 45% or more were judged to be defective products. The dotted frame in Table 1 indicates the range where the crack occurrence rate is less than 45%.
[0120] The pore area ratio was measured by imaging the cross section of each sample at the center in the longitudinal direction as shown in FIG. 5 using a SEM (Scanning Electron Microscope). At this time, the cross-sectional shape of the pore is not only circular as described above, but also a shape in which two circles are combined. Therefore, the cross-sectional area of the pore was calculated by binarizing the pore portion using image processing software. This method was also used in the following examples.
[0121] When the pore area ratio of the inner peripheral portion Sin is less than 3(%) and the pore area ratio of the outer peripheral portion Sout is 3(%) or more and 12(%) or less, the crack occurrence rate is less than 45(%). With this pore area ratio, the outer peripheral portion Sout exerts sufficient elastic force to suppress the stress acting from the outside, and the occurrence of cracks from the pores P of the inner peripheral portion Sin is sufficiently suppressed. More preferably, the pore area ratio of the inner peripheral portion Sin may be less than 2.5(%), while the pore area ratio of the outer peripheral portion Sout may be 3(%) or more.
[0122] In addition, when the pore area ratio of the inner peripheral portion Sin is less than 3(%) and the pore area ratio of the outer peripheral portion Sout is 12(%) or less, the crack occurrence rate is less than 45(%). This is because when the pore area ratio of the outer peripheral portion Sout is increased more than necessary, the effect of crack occurrence due to insufficient hardness is stronger than the effect of relieving stress. More preferably, the pore area ratio of the outer peripheral portion Sout may be 10(%) or less.
[0123] (Outer periphery area ratio) [Table 2]
[0124] Table 2 shows the ratio (%) of the area of the outer peripheral portion Sout to the total of the cross-sectional views of the inner peripheral portion Sin and the outer peripheral portion Sout (hereinafter referred to as the outer peripheral portion area ratio), and the crack occurrence rate (%). 100 samples of the multilayer ceramic capacitor 1 were produced according to the above manufacturing process, and the crack occurrence rate was measured. The size of each sample was 4.5 (mm) in length L, 3.2 (mm) in width W, and 2.5 (mm) in height H. The pore area ratio of the inner peripheral portion Sin of the sample was 2.5 (%), and the pore area ratio of the outer peripheral portion Sout of the sample was 12 (%). The outer peripheral portion area ratio was 30 to 93 (%).
[0125] The crack incidence was measured by the above-mentioned measurement method. Samples with a crack incidence rate of less than 35(%) were judged as good products, and samples with a crack incidence rate of 35(%) or more were judged as defective products. The dotted frame in Table 2 shows the range where the crack incidence rate is less than 35(%).
[0126] When the outer peripheral area ratio is 82 to 90(%), the crack occurrence rate is less than 35(%). When the outer peripheral area ratio is 82(%) or more, the outer peripheral portion Sout having a high pore area ratio relieves stress, so that cracks can be suppressed. Furthermore, when cracks originating from pores occur in a portion close to the capacitance portion, the laminated portion 2s may be damaged and the electrical characteristics may deteriorate, so that the outer peripheral area ratio is preferably 90(%) or less.
[0127] (Maximum pore diameter) [Table 3]
[0128] Table 3 shows the maximum diameter of the pores P in the inner peripheral portion Sin and the pores P in the outer peripheral portion Sout, and the occurrence rate of cracks (%). 100 samples of the multilayer ceramic capacitor 1 were produced according to the above manufacturing process, and the occurrence rate of cracks was measured. The size of each sample was a length L of 4.5 (mm), a width W of 3.2 (mm), and a height H of 2.5 (mm). The pore area ratio of the inner peripheral portion Sin of the sample was 2.5 (%), and the pore area ratio of the outer peripheral portion Sout of the sample was 12 (%). The maximum diameter of the pores P in the inner peripheral portion Sin was 0.1 to 0.4 (μm), and the maximum diameter of the pores P in the outer peripheral portion Sout was 1.0 to 3.0 (μm).
[0129] The crack incidence was measured by the above-mentioned measurement method. Samples with a crack incidence rate of less than 30(%) were judged as good products, and samples with a crack incidence rate of 30(%) or more were judged as defective products. The dotted frame in Table 3 shows the range where the crack incidence rate is less than 30(%).
[0130] When the maximum diameter of the pores P in the inner circumferential portion Sin is 0.1 to 0.35 (μm) and the maximum diameter of the pores P in the outer circumferential portion Sout is 0.4 to 1.0 (μm), the occurrence rate of cracks is less than 30 (%). When the maximum diameter of the pores P in the inner circumferential portion Sin is less than 0.4 (μm) and the maximum diameter of the pores P in the outer circumferential portion Sout is 0.4 (μm) or more, the smaller the diameter of the pores P in the inner circumferential portion Sin, the less likely the cracks caused by the pores P will occur, and the larger the diameter of the pores P in the outer circumferential portion Sout, the more stress can be relieved, so that the occurrence of cracks is effectively suppressed. In addition, when the maximum diameter of the pores P in the outer circumferential portion Sout is 1.0 (μm) or less, if the pore area ratio of the outer circumferential portion Sout is increased more than necessary, the effect of cracks occurring due to insufficient hardness works stronger than the effect of relieving stress, so that cracks are more effectively suppressed. Furthermore, when the maximum diameter of the pores P in the inner circumferential portion Sin is 0.1 (μm) or less and the maximum diameter of the pores P in the outer circumferential portion Sout is 0.45 (μm) or more, the occurrence of cracks is further suppressed.
[0131] (Stacked chip size) [Table 4]
[0132] Table 4 shows the size (length L x width W x height H (mm)) of the multilayer ceramic capacitor 1, the crack occurrence rate (%) of the examples and the comparative examples, and the difference therebetween. 100 samples of the multilayer ceramic capacitor 1 of the examples were produced according to the above manufacturing process, and the crack occurrence rate was measured. The pore area ratio of the inner peripheral portion Sin of the sample of the examples was less than 3 (%), and the pore area ratio of the outer peripheral portion Sout of the sample was 3 (%) or more and 12 (%) or less. The sizes of the multilayer ceramic capacitor 1 were 4.3 x 3.2 x 2.5 (mm), 3.2 x 2.5 x 2.5 (mm), 2.0 x 1.25 x 1.25 (mm), 1.0 x 0.5 x 0.5 (mm), 0.4 x 0.2 x 0.2 (mm), and 0.25 x 0.125 x 0.125 (mm).
[0133] In addition, 100 comparative samples were prepared for the samples of the embodiment. The comparative samples are multilayer ceramic capacitors that do not have a distinction between an inner circumferential portion Sin and an outer circumferential portion Sout, unlike the examples, and have a cover layer and a side margin portion with a pore area ratio of 3(%) or more. The size of the comparative samples is the same as above.
[0134] The crack occurrence rate was measured by the above-mentioned measurement method. Samples of the embodiment with a difference of 29(%) or more from the crack occurrence rate of the comparative example were judged to be good products, and samples with a difference of less than 29(%) were judged to be defective products.
[0135] Only the difference in the example sample having a size of 0.25×0.125×0.125 (mm) was 29(%) or more. Therefore, in the multilayer ceramic capacitor 1, when the size in the length direction is 0.25 (mm) or less, the size in the width direction is 0.125 (mm) or less, and the size in the stacking direction is 0.125 (mm) or less, the stress can be dispersed more effectively by the pores P.
[0136] (Peripheral area ratio) [Table 5]
[0137] Table 5 shows the ratio of the cross-sectional area of the outer peripheral portion Sout to the cross-sectional area of the side margin portions 40, 41 (side margin outer peripheral area ratio) (%), the ratio of the cross-sectional area of the outer peripheral portion Sout to the cross-sectional area of the cover portions 20, 21 (cover layer outer peripheral area ratio) (%), and the occurrence rate of cracks (%).
[0138] Rside=Sside_outer / (Sside_outer+Sside_inner) ···(1) Rcover=Scover_outer / (Scover_outer+Scover_inner) ···(2)
[0139] The side margin outer periphery area ratio Rside is calculated by the above formula (1). In formula (1), Sside_outer represents the cross-sectional area of the outer periphery Sout in the side margin portions 40, 41, and Sside_inner represents the cross-sectional area of the inner periphery Sin in the side margin portions 40, 41.
[0140] The cover layer outer periphery area ratio Rcover is calculated by the above formula (2), where Scover_outer represents the cross-sectional area of the outer periphery Sout in the cover portions 20, 21, and Scover_inner represents the cross-sectional area of the inner periphery Sin in the cover portions 20, 21.
[0141] 100 samples of the multilayer ceramic capacitor 1 were produced according to the above manufacturing process, and the occurrence rate of cracks was measured. The size of each sample was a length L of 0.25 (mm), a width W of 3.2 (mm), and a height H of 2.5 (mm). The pore area ratio of the inner peripheral portion Sin of the sample was 2.5 (%), and the pore area ratio of the outer peripheral portion Sout of the sample was 12 (%). The side margin outer peripheral area ratio was 70 to 95 (%), and the cover layer outer peripheral area ratio was 70 to 95 (%).
[0142] The crack incidence was measured by the above-mentioned measurement method. Samples with a crack incidence of 13% or less were judged as good products, and samples with a crack incidence of more than 13% were judged as defective products. The dotted frame in Table 5 indicates the range in which the crack incidence is 13% or less.
[0143] When the cover layer outer periphery area ratio was 80(%) and the side margin outer periphery area ratio was 85(%) or more, and when the cover layer outer periphery area ratio was 85(%) and the side margin outer periphery area ratio was 90(%) or more, the crack occurrence rate was 13(%) or less. In this way, when the side margin outer periphery area ratio>the cover layer outer periphery area ratio is established, as described with reference to Fig. 5, the thickness of the outer periphery portion Sout can be increased in the width direction from the stacking direction of the laminated portion 2s, so that the pressure Ph applied from the width direction to the laminated chip 2 can be distributed more effectively than the pressure Pv applied from the stacking direction to protect the laminated portion 2s from pressure.
[0144] (Side margin thickness) [Table 6]
[0145] Table 6 shows the ratio (side margin thickness ratio) (%) of the thicknesses d1 and d2 (see FIG. 5) of the side margin portions 40 and 41 in the width direction to the width W of the multilayer ceramic capacitor 1, the short-circuit rate (%) of the multilayer ceramic capacitor 1, and the difference (%) in capacitance with respect to the multilayer ceramic capacitor 1 having a side margin thickness ratio of 8 (%). Here, the side margin thickness ratio is calculated by d1 / W or d2 / W. 100 samples of the multilayer ceramic capacitor 1 were produced according to the above manufacturing process, and the short-circuit rate was measured. The size of each sample was set to a length L of 0.25 (mm), a width W of 0.125 (mm), and a height H of 0.125 (mm). The pore area ratio of the inner peripheral portion Sin of the sample was 2.5 (%), and the pore area ratio of the outer peripheral portion Sout of the sample was 12 (%). The side margin thickness ratio was set to 8 to 20 (%).
[0146] The short-circuit rate and capacitance were measured using a detector manufactured by Hewlett-Packard Co. Samples with a short-circuit rate of 23% or less were judged to be good products, and samples with a short-circuit rate of more than 23% were judged to be defective products. The dotted frame in Table 6 indicates the range in which the short-circuit rate is 23% or less.
[0147] When the side margin thickness ratio is 13% or more, the short-circuit rate is 23% or less. At this side margin thickness ratio, the side margin portions 40, 41 are thick, so that the laminated portion 2s is protected from the pressure Ph and short-circuiting can be suppressed. Furthermore, when the side margin thickness ratio is 13 to 15%, the reduction rate of the capacitance difference is smaller than in the cases of other side margin thickness ratios, which is preferable from the viewpoint of electrostatic capacitance.
[0148] (Pore shape) [Table 7]
[0149] Table 7 shows the ratio (pore number ratio) of the number of pores P in which the ratio (RS / RL) of the length RS to the length RL shown in FIG. 7 is less than 0.45 among the pores P in the inner peripheral portion Sin to the number of pores P in which RS / RL is 0.45 or more, and the occurrence rate of cracks (%). 100 samples of the multilayer ceramic capacitor 1 were produced according to the above manufacturing process, and the occurrence rate of cracks was measured. The size of each sample was set to a length L of 0.25 (mm), a width W of 0.125 (mm), and a height H of 0.125 (mm). The pore area ratio of the inner peripheral portion Sin of the sample was 2.5 (%), and the pore area ratio of the outer peripheral portion Sout of the sample was 12 (%). The pore number ratio was set to 30 to 90 (%).
[0150] The crack incidence was measured by the above-mentioned measurement method. Samples with a crack incidence of 3% or less were judged as good products, and samples with a crack incidence of more than 3% were judged as defective products. The dotted frame in Table 7 shows the range where the crack incidence is 3% or less.
[0151] When the pore number ratio is 30 to 50%, the crack occurrence rate is 3% or less. When the pore number ratio is 50% or less, the number of pores P each having a shape in which two circles are joined together is smaller than the number of pores P each having a substantially circular shape in the cross section shown in Fig. 5, so that cracks are less likely to occur as described with reference to Fig. 7.
[0152] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]
[0153] 1. Multilayer ceramic capacitors 2 Stacked chips 2s stacking section 8 Packaging 80 Storage unit 81 Sealing part 800 Recess 800a Aperture 9 Circuit Board 20,21 Cover part 22 Dielectric layer 23 Internal electrode layer 40,41 Side margin 50,51,51a Ceramic sheet P pore Sin inner circumference Sout outer periphery
Claims
1. a laminated portion having a substantially rectangular parallelepiped shape in which a plurality of dielectric layers and a plurality of internal electrode layers are laminated; an inner peripheral portion including a dielectric covering the periphery of the laminated portion in a cross-sectional view taken along a lamination direction of the laminated portion and a width direction of the laminated portion that is substantially perpendicular to the lamination direction; an outer circumferential portion including a dielectric covering the inner circumferential portion in the cross-sectional view; a ratio of a sum of cross-sectional areas of pores in the inner circumferential portion to a cross-sectional area of the inner circumferential portion is smaller than a ratio of a sum of cross-sectional areas of pores in the outer circumferential portion to a cross-sectional area of the outer circumferential portion.
2. 2. The multilayer ceramic electronic component according to claim 1, wherein, in the cross-sectional view, a ratio of a total cross-sectional area of pores in the inner peripheral portion to a cross-sectional area of the inner peripheral portion is less than 3%, and a ratio of a total cross-sectional area of pores in the outer peripheral portion to a cross-sectional area of the outer peripheral portion is 3% or more.
3. 3. The multilayer ceramic electronic component according to claim 2, wherein in the cross-sectional view, a ratio of a total cross-sectional area of the pores in the outer periphery to a cross-sectional area of the outer periphery is 12% or less.
4. 3. The multilayer ceramic electronic component according to claim 1, wherein, in the cross-sectional view, a cross-sectional area of the outer periphery is larger than a cross-sectional area of the inner periphery.
5. 5. The multilayer ceramic electronic component according to claim 4, wherein in the cross-sectional view, the cross-sectional area of the outer periphery is 82% or more of the total cross-sectional area of the inner periphery and the outer periphery.
6. 5. The multilayer ceramic electronic component according to claim 4, wherein in the cross-sectional view, the cross-sectional area of the outer periphery is 90% or less of the total cross-sectional area of the inner periphery and the outer periphery.
7. 3. The multilayer ceramic electronic component according to claim 1, wherein, in the cross-sectional view, the maximum diameter of the pores in the inner peripheral portion is less than 0.4 μm, and the maximum diameter of the pores in the outer peripheral portion is 0.4 μm or more.
8. 8. The multilayer ceramic electronic component according to claim 7, wherein the maximum diameter of the pores in the outer circumferential portion is 1.0 μm or less in the cross-sectional view.
9. The size in the length direction substantially perpendicular to the stacking direction and the width direction is 0.25 mm or less, The size in the width direction is 0.125 mm or less, 3. The multilayer ceramic electronic component according to claim 1, wherein the size in the lamination direction is 0.125 mm or less.
10. 3. The multilayer ceramic electronic component according to claim 1, wherein, in the cross-sectional view, a ratio of a cross-sectional area of the outer periphery to a cross-sectional area of the inner periphery and the outer periphery outside a pair of faces of the laminated portions that face each other in the width direction is greater than a ratio of the outer periphery to a cross-sectional area of the inner periphery and the outer periphery covering, from the stacking direction, another pair of faces of the laminated portions that face each other in the stacking direction.
11. 3. The multilayer ceramic electronic component according to claim 1, wherein a thickness of the inner peripheral portion and the outer peripheral portion covering a pair of faces of the laminated portion opposing each other in the width direction is 13% or more of a size of the multilayer ceramic electronic component in the width direction.
12. 3. The multilayer ceramic electronic component according to claim 1, wherein a thickness of the inner peripheral portion and the outer peripheral portion covering a pair of faces of the laminated portion opposing each other in the width direction is 15% or less of a size of the multilayer ceramic electronic component in the width direction.
13. 3. The multilayer ceramic electronic component according to claim 1, wherein, in the cross-sectional view, the number of pores in the outer peripheral portion having a ratio of the length of the shortest portion to the length of the longest portion of less than 0.45 is 50% or less of the number of pores having a ratio of the length of the shortest portion to the length of the longest portion of 0.45 or more.
14. 3. The multilayer ceramic electronic component according to claim 1, wherein the pores in the outer periphery are filled with an organic substance.
15. In a circuit board on which multilayer ceramic electronic components are mounted, The multilayer ceramic electronic component comprises: a laminated portion in which a plurality of dielectric layers and a plurality of internal electrode layers are laminated; an inner peripheral portion including a dielectric covering the periphery of the laminated portion in a cross-sectional view taken along a lamination direction of the laminated portion and a width direction of the laminated portion that is substantially perpendicular to the lamination direction; an outer circumferential portion including a dielectric covering the inner circumferential portion in the cross-sectional view; A circuit board characterized in that, in the cross-sectional view, a ratio of a sum of cross-sectional areas of pores in the inner circumferential portion to a cross-sectional area of the inner circumferential portion is smaller than a ratio of a sum of cross-sectional areas of pores in the outer circumferential portion to a cross-sectional area of the outer circumferential portion.
16. a housing portion provided with a plurality of recesses for housing the multilayer ceramic electronic components; a sealing portion that seals the opening of the recess, The multilayer ceramic electronic component comprises: a laminated portion in which a plurality of dielectric layers and a plurality of internal electrode layers are laminated; an inner peripheral portion including a dielectric covering the periphery of the laminated portion in a cross-sectional view taken along a lamination direction of the laminated portion and a width direction of the laminated portion that is substantially perpendicular to the lamination direction; an outer circumferential portion including a dielectric covering the inner circumferential portion in the cross-sectional view; An electronic component packaging body, characterized in that, in the cross-sectional view, a ratio of the sum of the cross-sectional areas of the pores in the inner peripheral portion to the cross-sectional area of the inner peripheral portion is smaller than a ratio of the sum of the cross-sectional areas of the pores in the outer peripheral portion to the cross-sectional area of the outer peripheral portion.
17. forming an internal electrode pattern on the surfaces of a plurality of first dielectric green sheets; laminating the plurality of first dielectric green sheets such that the internal electrode patterns face each other via the first dielectric green sheets; laminating a pair of second dielectric green sheets on both sides of the laminated first dielectric green sheets in a lamination direction; laminating a pair of third dielectric green sheets containing more resin than the pair of second dielectric green sheets on both sides of the pair of second dielectric green sheets in the lamination direction; a step of dividing the plurality of laminated first dielectric green sheets, the pair of second dielectric green sheets, and the pair of third dielectric green sheets into a plurality of laminates each having a substantially rectangular parallelepiped shape; forming a pair of first ceramic layers covering a pair of surfaces opposed to each other in a width direction of the laminate, the width direction being substantially perpendicular to a stacking direction of the laminate; forming a pair of second ceramic layers containing a larger amount of resin than the pair of first ceramic layers and covering the pair of first ceramic layers in the width direction and the stacking direction; and firing the laminate.
18. 18. The method for producing a multilayer ceramic electronic component according to claim 17, further comprising the step of immersing the laminate in an organic substance so that the organic substance is contained in pores formed by volatilization of the resin in the step of firing the laminate.
19. 20. The method for producing a multilayer ceramic electronic component according to claim 18, wherein the organic matter is cellulose, PVB, or an aromatic material.
20. 20. The method for producing a multilayer ceramic electronic component according to claim 17, wherein the pair of second dielectric green sheets or the second ceramic layer contains a flocculant.
Citation Information
Patent Citations
Multilayer ceramic capacitor and multilayer ceramic capacitor series including the same, and multilayer ceramic capacitor mounting body
JP2016082183A
Multilayer ceramic capacitor and method for manufacturing the same
JP2018107239A