Alloy powder for additive manufacturing
By controlling the HCP to FCC phase ratio and adjusting production parameters, the alloy powder for additive manufacturing minimizes manufacturing defects in additively manufactured objects, improving production consistency and reducing residual pores.
Patent Information
- Application Number
- JP2023047391
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Manufacturing defects, particularly residual pores, frequently occur in additively manufactured objects made from alloy powders of the same composition, and their frequency varies significantly.
The alloy powder for additive manufacturing is formulated with a controlled ratio of HCP to FCC phases, with a peak ratio of 1.00 or less, and specific compositions of Cr, Mo, W, Si, and optionally C, B, P, and S, produced using gas atomization methods, adjusting parameters like tapping temperature, nozzle diameter, and gas pressure to control cooling rates.
This formulation reduces variations in manufacturing defects, specifically residual pores, across multiple additively manufactured objects by stabilizing the HCP and FCC phase ratios, enhancing production consistency and reducing defects.
Smart Images

Figure 2024136308000001 
Figure 2024136308000002 
Figure 2024136308000003
Abstract
Description
[Technical field]
[0001] The present invention relates to alloy powders for use in additive manufacturing. [Background technology]
[0002] Patent Document 1 describes that an alloy frame included in a dental prosthesis is manufactured by additive manufacturing, etc. It also describes that a Co-Cr-W alloy, a Co-Cr-W-Mo alloy, etc. are used as alloys for manufacturing the alloy frame. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-14182 A Summary of the Invention [Problem to be solved by the invention]
[0004] When an additive manufacturing method is used to manufacture an additive manufacturing object, the additive manufacturing object is prone to have molding defects, and when a plurality of additive manufacturing objects are manufactured from alloy powder of the same composition, the frequency of occurrence of the molding defects is likely to vary. As a result of extensive investigation into the internal structure of the alloy powder used as a raw material for the additive manufacturing method, the inventors have found that by adjusting the ratio of the crystal structure in the alloy powder, the variation in the frequency of occurrence of the molding defects can be reduced, and have completed the present invention. [Means for solving the problem]
[0005] The alloy powder for additive manufacturing of the present invention contains Co, and in powder X-ray diffraction, the ratio of the HCP phase
[0101] peak to the FCC phase
[0200] peak is 1.00 or less.
[0006] The alloy powder for additive manufacturing may contain Cr, Mo, W, and Si. Here, the respective contents [mass%] of Cr, Mo, W, and Si may satisfy the conditions shown in the following formulas (I) to (IV). 22.0≦Cr≦27.0 (I) 3.0≦Mo≦7.0 (II) 3.0≦W≦7.0 (III) 0.0≦Si≦2.0 (IV)
[0007] The alloy powder for additive manufacturing may contain at least one of C, B, P, and S. Here, C may be 0.040 [mass%] or less, B may be 0.004 [mass%] or less, P may be 0.020 [mass%] or less, and S may be 0.010 [mass%] or less. Effect of the Invention
[0008] By manufacturing an additive manufacturing body using the alloy powder for additive manufacturing of the present invention, it is possible to reduce the variation in the number of molding defects among multiple additive manufacturing bodies. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The alloy powder for additive manufacturing of this embodiment (hereinafter simply referred to as "alloy powder") is an alloy powder used for producing additive manufacturing bodies, contains Co as a main component, and has a peak ratio HCP / FCC described below of 1.00 or less.
[0010] The peak ratio HCP / FCC is the ratio of the peak of the HCP phase
[0101] to the peak of the FCC phase
[0200] in powder X-ray diffraction. By X-ray diffraction using a Cu tube, the peak of the FCC phase
[0200] (planar spacing d = about 0.178 nm) appears at 2θ of about 51.2°, and the peak of the HCP phase
[0101] (planar spacing d = about 0.192 nm) appears at 2θ of about 47.4°. The peaks of the FCC phase
[0200] and the HCP phase
[0101] show the highest intensity in each phase among the peaks detected without overlapping each other.
[0011] As can be understood from the examples described below, by setting the peak ratio HCP / FCC to 1.00 or less, it is possible to reduce the variation in the frequency (number) of molding defects that occur in multiple additively molded bodies when multiple additively molded bodies are manufactured from alloy powder.
[0012] In this embodiment, the variation in the occurrence frequency (number) of molding defects refers to the difference (absolute value) between the minimum number of molding defects and the maximum number of molding defects, focusing on the additive manufacturing body with the fewest number of molding defects and the additive manufacturing body with the most number of molding defects, among a predetermined number (e.g., five) of additive manufacturing bodies manufactured under the same conditions. An example of a molding defect is residual pores (voids) formed in the additive manufacturing body during molding.
[0013] The number of modeling defects can be measured within a predetermined observation area on the observation surface of each layered object. That is, the number of modeling defects can be measured by observing the observation area at the same position in each of a predetermined number of layered objects with an optical microscope or the like. For example, the observation area can be a region located at the center of the observation surface. The size of the modeling defects to be measured can be determined appropriately, but for example, modeling defects of 50 μm or more can be measured.
[0014] Methods for producing the alloy powder include, for example, water atomization, gas atomization, disk atomization, plasma atomization, and plasma rotating electrode method, among which gas atomization, which is most widely used industrially, is preferably used.
[0015] In the alloy powder produced by the above-mentioned method, in addition to the stable FCC phase, it is believed that some HCP phases (including martensite phases) coexist inside one alloy powder (particle). It is believed that the physical properties of the FCC phase and the HCP phase, such as magnetism, surface roughness and friction, degree of cohesion, and heat absorption rate during additive manufacturing, are different, and it is presumed that these differences in physical properties affect each other in a complex manner, and for example, in the powder bed during additive manufacturing, small areas where slight aggregation, voids, differences in packing density, etc. occur in a concentrated manner appear. Note that the instability of packing in the small areas of the powder bed occurs locally, and cannot be identified by simply measuring the particle size distribution, flow rate, apparent density, tap density, etc. of the powder.
[0016] When this powder bed is melted and solidified by a heat source such as a laser, molding defects such as residual pores are concentrated in one part of the layered object, and the frequency (number) of molding defects, in other words, the molding density, varies. By using an alloy powder with a peak ratio HCP / FCC of 1.00 or less as in this embodiment, it is possible to reduce the variation in the frequency (number) of molding defects when multiple layered objects are manufactured under the same conditions.
[0017] Even if the composition and particle size of the alloy powder are the same, the respective generation ratios of the FCC phase and the HCP phase change depending on the cooling rate when the alloy powder is produced. Specifically, the higher the cooling rate, the higher the generation ratio of the HCP phase. In other words, the lower the cooling rate, the lower the generation ratio of the HCP phase. Therefore, by controlling the cooling rate, it is possible to produce an alloy powder with a peak ratio HCP / FCC of 1.00 or less.
[0018] In the gas atomization method, raw materials are heated in a crucible to produce a molten alloy, and the molten alloy is poured from a pouring nozzle installed at the bottom of the crucible. Then, an atomizing gas of a given pressure is sprayed onto the poured molten alloy to pulverize the molten alloy while rapidly cooling it, thereby obtaining an alloy powder. For example, argon gas or nitrogen gas can be used as the atomizing gas.
[0019] In the above-mentioned process, parameters that affect the cooling rate of the molten alloy include the temperature of the molten alloy at the time of tapping (hereinafter referred to as "tap temperature"), the amount of molten alloy tapped per unit time, the pressure of the atomizing gas (hereinafter referred to as "atomizing gas pressure"), and the type of atomizing gas (hereinafter referred to as "atomizing gas type"). Here, the amount of molten alloy tapped per unit time can be changed by changing the inner diameter of the tapping nozzle (hereinafter referred to as "tap nozzle diameter").
[0020] The value of the peak ratio HCP / FCC is related to the four parameters mentioned above. As will be seen from the examples described later, each parameter has a tendency to be explained below.
[0021] When only the tapping temperature is changed, the higher the tapping temperature, the slower the cooling rate of the molten alloy and the lower the peak ratio HCP / FCC tends to be. In other words, the lower the tapping temperature, the faster the cooling rate of the molten alloy and the higher the peak ratio HCP / FCC tends to be.
[0022] In addition, the greater the amount and flow rate of the atomizing gas that the molten alloy receives per unit weight, the greater the cooling rate of the molten alloy, and therefore the smaller the diameter of the outlet nozzle and the higher the atomizing gas pressure, the greater the cooling rate of the molten alloy. When only the outlet nozzle diameter is changed, the smaller the outlet nozzle diameter, the higher the peak ratio HCP / FCC tends to be, in other words, the larger the outlet nozzle diameter, the lower the peak ratio HCP / FCC tends to be. When only the atomizing gas pressure is changed, the higher the atomizing gas pressure, the higher the peak ratio HCP / FCC tends to be, in other words, the lower the atomizing gas pressure, the lower the peak ratio HCP / FCC tends to be.
[0023] In addition, the cooling capacity of the molten alloy differs depending on the type of atomizing gas, and when nitrogen gas is used as the atomizing gas, the cooling rate of the molten alloy tends to be higher and the peak ratio HCP / FCC tends to be higher than when argon gas is used.
[0024] By adjusting at least one of the four parameters described above, the cooling rate of the molten alloy can be changed to change the respective generation ratios of the FCC phase and the HCP phase. By conducting a preliminary experiment, the cooling rate conditions that can produce an alloy powder with a peak ratio HCP / FCC of 1.00 or less can be determined.
[0025] As described above, the peak ratio HCP / FCC may be set to 1.00 or less, but it is preferable to set the peak ratio HCP / FCC to 0.90 or less, and more preferably to set it to 0.85 or less, which makes it easier to reduce the variation in the occurrence frequency (number) of molding defects.
[0026] On the other hand, in a typical powder alloy manufacturing method, it is not easy to make the peak ratio HCP / FCC less than 0.30, and in order to make the peak ratio HCP / FCC less than 0.20, it is necessary to add a post-process such as heat treatment, which increases the manufacturing cost. In addition, even if the peak ratio HCP / FCC is not excessively low, the variation in the occurrence frequency of molding defects (residual pores) occurring in multiple layered molded bodies can be reduced. Therefore, the peak ratio HCP / FCC can be 0.30 or more, and preferably 0.50 or more.
[0027] The alloy powder may contain Cr, Mo, W, and Si. The respective contents [mass%] of Cr, Mo, W, and Si preferably satisfy the conditions shown in the following formulas (1) to (4). As shown in the following formula (4), Si does not have to be contained in the alloy powder. 22.0≦Cr≦27.0 (1) 3.0≦Mo≦7.0 (2) 3.0≦W≦7.0 (3) 0.0≦Si≦2.0 (4)
[0028] The composition of the alloy powder containing Cr, Mo, W, and Si that satisfy the conditions shown in the above formulas (1) to (4), with the balance being Co and unavoidable impurities, is a typical composition of the alloy powder used in the production of additive manufacturing objects. It is known that such a composition exhibits excellent biocompatibility, mechanical properties, and corrosion resistance (for example, cobalt-chromium (Co-Cr-Mo-W) alloy powder for three-dimensional additive manufacturing that has been approved for manufacture and sale (approval number: 23000BZX00121000)).
[0029] The alloy powder may contain at least one of C, B, P, and S. C, B, P, and S may be added intentionally or may be mixed in unavoidably. By setting upper limits for the contents of C, B, P, and S, it is possible to prevent the average density of the additive manufacturing body from decreasing. C is a source of CO gas that reduces the average density of the additive manufacturing body. B, P, and S are factors that cause microcracks to occur due to solidification segregation, and the microcracks reduce the average density of the additive manufacturing body.
[0030] The C content is preferably 0.040 [mass %] or less. Here, since the lower the C content, the more the number of molding defects (residual pores) formed in the layered molded body can be reduced, the C content is more preferably 0.024 [mass %] or less, and further preferably 0.009 [mass %] or less.
[0031] The content of B is preferably 0.004 [mass %] or less. Here, the lower the content of B, the more the number of molding defects (residual pores) formed in the layered product can be reduced, so the content of B is more preferably 0.003 [mass %] or less, and even more preferably 0.002 [mass %] or less.
[0032] The P content is preferably 0.020 [mass %] or less. Here, the lower the P content, the more the number of molding defects (residual pores) formed in the layered molded body can be reduced, so the P content is more preferably 0.010 [mass %] or less, and even more preferably 0.004 [mass %] or less.
[0033] The content of S is preferably 0.010 [mass %] or less. Here, the lower the content of S, the more the number of molding defects (residual pores) formed in the layered product can be reduced, so the content of S is more preferably 0.006 [mass %] or less, and even more preferably 0.004 [mass %] or less.
[0034] In addition, the density of the additive manufacturing body can be improved by deoxidizing the alloy powder during production by adding a small amount of C. In consideration of this point, the C content is preferably 0.001 [mass%] or more, and more preferably 0.002 [mass%] or more. EXAMPLES
[0035] (Manufacturing of alloy powder) Alloy powders (Examples 1 to 17 and Comparative Examples 1 to 4) having the compositions shown in the following Tables 1 to 4 were produced by a gas atomization method. Table 1 shows the compositions of the alloy powders (Examples 1 to 5 and Comparative Example 1), Table 2 shows the compositions of the alloy powders (Examples 6 to 9 and Comparative Example 2), Table 3 shows the compositions of the alloy powders (Examples 10 to 13 and Comparative Example 3), and Table 4 shows the compositions of the alloy powders (Examples 14 to 17 and Comparative Example 4).
[0036] [Table 1]
[0037] [Table 2]
[0038] [Table 3]
[0039] [Table 4]
[0040] The amount of the alloy powder raw material melted was set to 30 kg, and the raw material was heated (high-frequency induction heating) in a refractory crucible under an argon gas atmosphere, and the molten alloy was discharged from a discharge nozzle installed at the bottom of the crucible. The molten alloy was rapidly cooled while being refined by spraying an atomizing gas at a predetermined pressure onto the molten alloy, and a plurality of alloy powders were obtained. As the atomizing gas, argon gas (Examples 1 to 3, 5, 7 to 17 and Comparative Examples 1 to 3) or nitrogen gas (Examples 4, 6 and Comparative Example 4) was used. The obtained alloy powder was then sieved to obtain alloy powders having a predetermined particle size or less.
[0041] The conditions of the gas atomization method include the tapping temperature, the tapping nozzle diameter, the type of atomizing gas, and the injection gas pressure. By changing these conditions, the cooling rate can be changed even for alloy powders with the same composition and particle size, and the peak ratio HCP / FCC ratio can be changed.
[0042] (Evaluation of alloy powder) For the sieved alloy powders (Examples 1 to 17 and Comparative Examples 1 to 4), the average particle size D50, fluidity, apparent density, tap density, and peak ratio HCP / FCC were measured.
[0043] The particle size distribution of each alloy powder was measured using Microtrac MT3000 (manufactured by Nikkiso Co., Ltd.), and the average particle size D50 was determined based on the measurement results. The average particle size D50 here means the particle size at 50% of the cumulative value in the particle size distribution obtained by the laser diffraction / scattering method. The flow rate was measured according to the provisions of JIS Z2502 (2020), the apparent density was measured according to the provisions of JIS Z2504 (2020), and the tap density was measured according to the provisions of JIS Z2512 (2012).
[0044] Powder X-ray diffraction was performed using a Cu tube, and the diffraction peak value of the FCC phase
[0200] and the diffraction peak value of the HCP phase
[0101] were identified based on the obtained X-ray diffraction pattern. The peak ratio HCP / FCC was calculated based on these diffraction peak values.
[0045] (Layered Modeling) A 3D additive manufacturing machine (EOS-M290, EOS (Electro Optical Systems) Corporation) was used to mold each alloy powder (Examples 1 to 17 and Comparative Examples 1 to 4) to produce blocks (additively molded bodies). The standard parameters (MP1) of the 3D additive manufacturing machine were used as the laser irradiation conditions during additive manufacturing. Blocks of 10 mm x 10 mm x 10 mm were molded at the center of a 250 mm x 250 mm molding plate and at four peripheral positions (four locations) 100 mm away from this center position in the four corner directions. As a result, five blocks were obtained from alloy powder of the same composition.
[0046] (Evaluation of additive manufacturing products) After each block was cut from the modeling plate by wire cutting, it was embedded in resin and the observation surface was polished, and this observation surface was observed with an optical microscope. The observation surface was a surface parallel to the modeling direction. The observation surface was photographed at 25x magnification and a measurement area of 3mm x 3mm (9mm 2 The number of residual pores (air holes) of 50 μm or more was counted within the block (region A). Depending on the alloy powder molding, pores may remain inside the block. Here, the measurement region for residual pores was set to the same predetermined position (center) on the observation surface of the five blocks.
[0047] For five blocks manufactured from alloy powders of the same composition, the average value (referred to as "average number of residual pores") was calculated from the number of residual pores measured in each block. In addition, among the five blocks, the block with the fewest number of residual pores and the block with the most number of residual pores were identified, and the difference between the fewest number of residual pores and the most number of residual pores ("maximum - minimum number of pores") was calculated.
[0048] The evaluation results of the above-mentioned alloy powder and the above-mentioned layered manufactured body (block) are shown in the following Tables 5 to 8. Table 5 shows the evaluation results for the alloy powder (Examples 1 to 5 and Comparative Example 1), Table 6 shows the evaluation results for the alloy powder (Examples 6 to 9 and Comparative Example 2), Table 7 shows the evaluation results for the alloy powder (Examples 10 to 13 and Comparative Example 3), and Table 8 shows the evaluation results for the alloy powder (Examples 14 to 17 and Comparative Example 4).
[0049] [Table 5]
[0050] [Table 6]
[0051] [Table 7]
[0052] [Table 8]
[0053] The effect of the peak ratio HCP / FCC on the maximum-minimum pore number is discussed.
[0054] As shown in Tables 5 to 8 above, in Examples 1 to 17, the peak ratio HCP / FCC was 1.00 or less, and the maximum-minimum pore number was 3 [pores / 9 mm 2 On the other hand, in Comparative Examples 1 to 4, the peak ratio HCP / FCC was higher than 1.00, and the maximum-minimum pore number was 5 to 7 [pores / 9 mm 2Therefore, when a plurality of additively molded bodies (blocks) were manufactured from alloy powder of the same composition, the maximum-minimum pore count could be reduced by setting the peak ratio HCP / FCC to 1.00 or less, in comparison with the case where the peak ratio HCP / FCC was set to a value higher than 1.00, in other words, the variation in the number of remaining pores (i.e., the variation in the frequency of occurrence of molding defects) could be reduced.
[0055] According to Tables 5 to 8 above, when the peak ratio HCP / FCC is higher than 1.00, the maximum-minimum pore number is 5 [pores / 9 mm 2 When the peak ratio HCP / FCC was 1.00 or less and higher than 0.90 (Example 6), the maximum-minimum pore number was 3 [pores / 9 mm 2 When the peak ratio HCP / FCC was 0.90 or less and higher than 0.85 (Example 4), the maximum-minimum pore number was 2 [pores / 9 mm 2 When the peak ratio HCP / FCC was 0.85 or less (Examples 1 to 3, 5, and 7 to 17), the maximum-minimum pore number was 1 [pores / 9 mm 2 According to this result, in terms of reducing the maximum-minimum pore number, the peak ratio HCP / FCC is preferably 0.90 or less, and more preferably 0.85 or less.
[0056] On the other hand, it has been found that the peak ratio HCP / FCC can be adjusted by adjusting at least one parameter among the tapping temperature, tapping nozzle diameter, atomizing gas pressure, and atomizing gas type, as described below. These parameters affect the cooling rate of the molten alloy when producing alloy powder, and by adjusting the cooling rate of the molten alloy, the peak ratio HCP / FCC can be adjusted.
[0057] First, we consider the effect of the outlet temperature on the peak ratio HCP / FCC.
[0058] In Table 5 above, looking at Examples 1 to 3, and 5 and Comparative Example 1, the discharge nozzle diameter, spray gas pressure, and spray gas type were all the same, but the discharge temperature was different between Example 1, Examples 2, 3, and 5, and Comparative Example 1. In Examples 2, 3, and 5, the discharge temperature was also the same (1600°C), and the peak ratios HCP / FCC showed similar values (0.75, 0.72, 0.77), which were less than 1.00.
[0059] For Example 1, the outlet temperature was 1660 [°C], which was higher than the outlet temperature (1600 [°C]) of Examples 2, 3, and 5, and the peak ratio HCP / FCC showed a value (0.56) lower than that of Examples 2, 3, and 5. On the other hand, for Comparative Example 1, the outlet temperature was 1510 [°C], which was lower than the outlet temperature (1600 [°C]) of Examples 2, 3, and 5, and the peak ratio HCP / FCC showed a value (1.13) higher than that of Examples 2, 3, and 5.
[0060] From the above results, it was found that the temperature of the tap water affects the peak ratio HCP / FCC, and the higher the tap water temperature, the lower the peak ratio HCP / FCC tends to be, in other words, the lower the tap water temperature, the higher the peak ratio HCP / FCC tends to be. Therefore, it was found that by adjusting the tap water temperature, the peak ratio HCP / FCC can be adjusted to 1.00 or less.
[0061] Next, the effect of the tapping nozzle diameter on the peak ratio HCP / FCC is considered.
[0062] In Table 6, looking at Examples 7 to 9 and Comparative Example 2, the discharge temperature, spray gas pressure, and spray gas type were all the same, but the discharge nozzle diameter was different between Examples 7 to 9 and Comparative Example 2. In Examples 7 to 9, the discharge nozzle diameter was also the same (5 mm), and the peak ratios HCP / FCC were equivalent (0.81, 0.85, 0.82), which were less than 1.00. On the other hand, in Comparative Example 2, the discharge nozzle diameter was 4 mm, which was smaller than the discharge nozzle diameter (5 mm) of Examples 7 to 9, and the peak ratio HCP / FCC was 1.06.
[0063] From the above results, it was found that the diameter of the outlet nozzle affects the peak ratio HCP / FCC, and the smaller the outlet nozzle diameter, the higher the peak ratio HCP / FCC tends to be, in other words, the larger the outlet nozzle diameter, the lower the peak ratio HCP / FCC tends to be. Therefore, it was found that the peak ratio HCP / FCC can be adjusted to 1.00 or less by adjusting the outlet nozzle diameter.
[0064] Next, the effect of the atomizing gas pressure on the peak ratio HCP / FCC is considered.
[0065] Looking at Table 7 above, looking at Examples 10 to 13 and Comparative Example 3, the outlet temperature, outlet nozzle diameter, and spray gas type were all the same, but the spray gas pressure was different between Examples 10, 11, and 13 and Example 12 and Comparative Example 3. In Examples 10, 11, and 13, the spray gas pressure was also the same (5.1 [MPa]), and the peak ratios HCP / FCC showed similar values (0.63, 0.62), which were less than 1.00.
[0066] For Example 12, the spray gas pressure was 4.2 [MPa], which was lower than the spray gas pressure (5.1 [MPa]) of Examples 10, 11, and 13, and the peak ratio HCP / FCC showed a value (0.32) lower than that of Examples 10, 11, and 13. On the other hand, for Comparative Example 3, the spray gas pressure was 6.5 [MPa], which was higher than the spray gas pressure (5.1 [MPa]) of Examples 10, 11, and 13, and the peak ratio HCP / FCC showed a value (1.25) higher than that of Examples 10, 11, and 13.
[0067] From the above results, it was found that the spray gas pressure has an effect on the peak ratio HCP / FCC, and the higher the spray gas pressure, the higher the peak ratio HCP / FCC tends to be, in other words, the lower the spray gas pressure, the lower the peak ratio HCP / FCC tends to be. Therefore, it was found that the peak ratio HCP / FCC can be adjusted to 1.00 or less by adjusting the spray gas pressure.
[0068] Next, we consider the effect of the type of atomizing gas on the peak ratio HCP / FCC.
[0069] In Table 8, looking at Examples 14 to 17 and Comparative Example 4, the tapping temperature, tapping nozzle diameter, and spray gas pressure were all the same, but the type of spray gas was different between Examples 14 to 17 and Comparative Example 4. When argon gas was used as the spray gas as in Examples 14 to 17, the peak ratio HCP / FCC was the same (0.73 to 0.78), less than 1.00. On the other hand, when nitrogen gas was used as the spray gas as in Comparative Example 4, the peak ratio HCP / FCC was 1.05.
[0070] On the other hand, looking at Examples 1 and 4 in Table 5, although the tapping temperature of Example 4 (1670[°C]) is higher than that of Example 1 (1660[°C]), the peak ratio HCP / FCC of Example 4 (0.88) is higher than that of Example 1 (0.56). This contradicts the tendency that the higher the tapping temperature, the lower the peak ratio HCP / FCC, as described above. This is thought to be because the nitrogen gas (Example 4) has a higher cooling rate than the argon gas (Example 1), and is therefore significantly affected by the type of spray gas, resulting in a higher peak ratio HCP / FCC in Example 4 than in Example 1. In this way, it can be seen that the value of the peak ratio HCP / FCC is interrelated with the four parameters described above (here, the tapping temperature and the type of spray gas).
[0071] Next, in Table 6, looking at Example 6 and Examples 7 to 9, although the diameter of the outlet nozzle of Example 6 (6 [mm]) is larger than the diameter of the outlet nozzle of Examples 7 to 9 (5 [mm]), the peak ratio HCP / FCC of Example 6 (0.96) is higher than that of Examples 7 to 9 (0.81 to 0.85). This is contrary to the tendency that the larger the outlet nozzle diameter, the lower the peak ratio HCP / FCC, as described above. This is because the cooling rate of nitrogen gas (Example 6) is higher than that of argon gas (Examples 7 to 9), and therefore the effect of the type of spray gas is greater, which is considered to have resulted in the peak ratio HCP / FCC of Example 6 being higher than that of Examples 7 to 9. In this way, it can be seen that the value of the peak ratio HCP / FCC is mutually related to the four parameters described above (here, the diameter of the outlet nozzle and the type of spray gas).
[0072] From the above results, it was found that the type of spray gas affects the peak ratio HCP / FCC, and in particular, it was found that the peak ratio HCP / FCC tends to be higher when nitrogen gas is used rather than argon gas. Therefore, it was found that the peak ratio HCP / FCC can be adjusted to 1.00 or less by changing the type of spray gas.
[0073] Next, we focused on the average number of residual pores.
[0074] According to Table 5 above, when the peak ratio HCP / FCC is 1.00 or less (Examples 1 to 5), if the C content in the alloy powder is 0.040 [mass%] or less, not only can the maximum-minimum pore count be reduced, but also the average number of residual pores can be reduced. That is, in Example 5, when the C content is 0.055 [mass%], the average number of residual pores is 4.4 [pores / 9 mm 2However, in Examples 1 to 4, the C content was 0.040 [mass%] or less, and the average number of residual pores was reduced compared to Example 5. Furthermore, the C content decreased in the order of Examples 5, 4, 3, 2, and 1, and the lower the C content, the more the average number of residual pores decreased. Therefore, in terms of reducing the average number of residual pores, it is preferable that the C content in the alloy powder is 0.040 [mass%] or less.
[0075] According to Table 6 above, when the peak ratio HCP / FCC is 1.00 or less (Examples 6 to 9), if the B content in the alloy powder is 0.004 [mass%] or less, not only can the maximum-minimum pore count be reduced, but also the average number of residual pores can be reduced. That is, in Example 9, when the B content is 0.009 [mass%], the average number of residual pores is 4.2 [pores / 9 mm 2 However, in Examples 6 to 8, the B content was 0.004 [mass%] or less, and the average number of residual pores was reduced compared to Example 9. Furthermore, the B content decreased in the order of Examples 9, 8, 7, and 6, and the lower the B content, the more the average number of residual pores decreased. Therefore, in terms of reducing the average number of residual pores, it is preferable that the B content in the alloy powder is 0.004 [mass%] or less.
[0076] According to Table 7 above, when the peak ratio HCP / FCC is 1.00 or less (Examples 10 to 13), if the P content in the alloy powder is 0.020 [mass%] or less, not only can the maximum-minimum pore count be reduced, but also the average number of residual pores can be reduced. That is, in Example 13, when the P content is 0.025 [mass%], the average number of residual pores is 3.8 [pores / 9 mm 2 However, in Examples 10 to 12, the P content was 0.020 [mass%] or less, and the average number of residual pores was reduced compared to Example 13. Furthermore, the P content decreased in the order of Examples 13, 12, 11, and 10, and the lower the P content, the more the average number of residual pores decreased. Therefore, in terms of reducing the average number of residual pores, it is preferable that the P content in the alloy powder is 0.020 [mass%] or less.
[0077] According to Table 8 above, when the peak ratio HCP / FCC is 1.00 or less (Examples 14 to 17), if the S content in the alloy powder is 0.010 [mass%] or less, not only can the maximum-minimum pore count be reduced, but also the average number of residual pores can be reduced. That is, in Example 17, when the S content is 0.016 [mass%], the average number of residual pores is 4.2 [pores / 9 mm 2 In Examples 14 to 16, the S content was 0.010 [mass%] or less, and the average number of residual pores was reduced compared to Example 17. The S content decreased in the order of Examples 17, 16, 15, and 14, and the lower the S content, the more the average number of residual pores decreased. Therefore, in terms of reducing the average number of residual pores, it is preferable that the S content in the alloy powder is 0.010 [mass%] or less.
Claims
1. Contains C, An alloy powder for additive manufacturing, characterized in that in powder X-ray diffraction, the ratio of the HCP phase [101] peak to the FCC phase [200] peak is 1.00 or less.
2. Including Cr, Mo, W and Si; The alloy powder for additive manufacturing according to claim 1, characterized in that the respective contents [mass%] of Cr, Mo, W and Si satisfy the conditions shown in the following formulas (I) to (IV). 22.0≦Cr≦27.0...(I) 3.0≦Mo≦7.0...(II) 3.0≦W≦7.0...(III) 0.0≦Si≦2.0...(IV)
3. At least one of C, B, P, and S is included; C is 0.040 [mass%] or less, B is 0.004 [mass%] or less, P is 0.020 [mass%] or less, The alloy powder for additive manufacturing according to claim 1 or 2, characterized in that S is 0.010 [mass %] or less.
Citation Information
Patent Citations
Alloy for baking dental ceramics having excellent oxidation resistance and dental prothesis
JP2016014182A