Storage device
The memory device addresses the challenge of low leakage current and high on-current in cross-point type two-terminal memory devices by using a specific configuration of conductive layers and switching layers, enhancing data storage efficiency and reliability.
Patent Information
- Application Number
- JP2023047523
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing cross-point type two-terminal memory devices face challenges in achieving low leakage current and high on-current characteristics in their switching elements, which affect the reliability and efficiency of data storage.
The memory device incorporates a specific configuration of conductive layers and switching layers, including regions made of zinc oxide, tin oxide, tantalum oxide, niobium oxide, and vanadium oxide, with controlled thickness and Gibbs energy of formation, to enhance the switching element's performance.
This configuration results in a switching element with low half-selective leakage current and high on-current, improving the reliability and efficiency of data storage operations.
Smart Images

Figure 2024136413000001_ABST
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE The present invention relates to a storage device. [Background technology]
[0002] Cross-point type two-terminal memory devices are a type of large-capacity nonvolatile memory device. Cross-point type two-terminal memory devices facilitate miniaturization and high integration of memory cells.
[0003] A memory cell of a cross-point type two-terminal memory device has, for example, a resistance change element and a switching element. By having a switching element in the memory cell, a current flowing to memory cells other than the selected memory cell is suppressed.
[0004] The switching element is required to have excellent characteristics such as a low leakage current, a high on-current, and high reliability. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] U.S. Patent No. 9,029,187 Summary of the Invention [Problem to be solved by the invention]
[0006] An object of one embodiment of the present invention is to provide a memory device having a switching element with excellent characteristics. [Means for solving the problem]
[0007] A memory device according to an embodiment of the present invention includes a memory cell including a first conductive layer, a second conductive layer, a third conductive layer provided between the first conductive layer and the second conductive layer, a switching layer provided between the first conductive layer and the third conductive layer, and a resistance change layer provided between the third conductive layer and the second conductive layer. The switching layer includes a first region, a second region between the first region and the third conductive layer, and a third region between the first region and the second region. The first region includes at least one first element selected from the group consisting of zinc (Zn) and tin (Sn) and oxygen (O), the second region includes at least one second element selected from the group consisting of zinc (Zn) and tin (Sn) and oxygen (O), the third region includes at least one third element selected from the group consisting of tantalum (Ta), niobium (Nb) and vanadium (V) and oxygen (O), the first conductive layer includes at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au) and nickel (Ni), and the third conductive layer includes at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au) and nickel (Ni). [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a block diagram of a storage device according to the first embodiment. [Diagram 2] 2 is a schematic cross-sectional view of a memory cell of the memory device according to the first embodiment. [Diagram 3] FIG. 4 is an explanatory diagram of a problem of the storage device of the first embodiment. [Figure 4] FIG. 4 is an explanatory diagram of current-voltage characteristics of the switching element according to the first embodiment. [Diagram 5] FIG. 4 is a diagram illustrating the operation and effect of the storage device according to the first embodiment. [Figure 6] FIG. 4 is a diagram illustrating the operation and effect of the storage device according to the first embodiment. [Figure 7] FIG. 11 is a schematic cross-sectional view of a memory cell of a memory device according to a second embodiment. [Figure 8]FIG. 13 is a schematic cross-sectional view of a memory cell of a memory device according to a first modified example of the second embodiment. [Figure 9] FIG. 13 is a schematic cross-sectional view of a memory cell of a memory device according to a second modified example of the second embodiment. [Figure 10] FIG. 13 is a schematic cross-sectional view of a memory cell of a memory device according to a third modified example of the second embodiment. [Figure 11] FIG. 11 is a schematic cross-sectional view of a memory cell in a memory device according to a third embodiment. [Figure 12] FIG. 13 is a schematic cross-sectional view of a memory cell of a memory device according to a first modified example of the third embodiment. [Figure 13] FIG. 13 is a schematic cross-sectional view of a memory cell of a memory device according to a second modified example of the third embodiment. [Figure 14] FIG. 13 is a schematic cross-sectional view of a memory cell of a memory device according to a third modified example of the third embodiment. [Figure 15] FIG. 13 is a schematic cross-sectional view of a memory cell in a memory device according to a fourth embodiment. [Figure 16] FIG. 13 is a schematic cross-sectional view of a memory cell in a memory device according to a fifth embodiment. [Figure 17] FIG. 13 is a diagram showing a band structure of a switching element according to a fifth embodiment. [Figure 18] FIG. 13 is a schematic cross-sectional view of a memory cell in a comparative example of the fifth embodiment. [Figure 19] 13A to 13C are explanatory diagrams showing the operation and effect of the storage device according to the fifth embodiment. [Figure 20] 13A to 13C are explanatory diagrams showing the operation and effect of the storage device according to the fifth embodiment. [Figure 21] 13A to 13C are explanatory diagrams showing the operation and effect of the storage device according to the fifth embodiment. [Figure 22] 13A to 13C are explanatory diagrams showing the operation and effect of the storage device according to the fifth embodiment. [Diagram 23] FIG. 13 is a schematic cross-sectional view of a memory cell in a memory device according to a sixth embodiment. [Figure 24] FIG. 13 is a diagram showing a band structure of a switching element according to a sixth embodiment. [Diagram 25] 13A to 13C are explanatory diagrams showing the operation and effect of the storage device according to the sixth embodiment. [Figure 26] FIG. 13 is a schematic cross-sectional view of a memory cell in a memory device according to a seventh embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the following description, the same reference numerals will be used to designate the same or similar components, and the description of components that have already been described will be omitted as appropriate.
[0010] The qualitative and quantitative analysis of the chemical composition constituting the memory device in this specification can be performed by, for example, Rutherford Backscattering Spectroscopy (RBS), Secondary Ion Mass Spectroscopy (SIMS), Energy Dispersive X-ray Spectroscopy (EDS), Electron Energy Loss Spectroscopy (EELS), etc. In addition, for example, a transmission electron microscope (TEM) can be used to measure the thickness of the members constituting the memory device and the distance between the members. In addition, for example, X-ray Photoelectron Spectroscopy (XPS), Hard X-ray Photoelectron Spectroscopy (HAXPES), and EELS can be used to identify the constituent materials of the members constituting the memory device and measure the proportion of the constituent materials.
[0011] (First embodiment) A memory device according to a first embodiment includes a memory cell including a first conductive layer, a second conductive layer, a third conductive layer provided between the first conductive layer and the second conductive layer, a switching layer provided between the first conductive layer and the third conductive layer, and a resistance change layer provided between the third conductive layer and the second conductive layer. The switching layer includes a first region, a second region between the first region and the third conductive layer, and a third region between the first region and the second region. The first region includes at least one first element selected from the group consisting of zinc (Zn) and tin (Sn) and oxygen (O), the second region includes at least one second element selected from the group consisting of zinc (Zn) and tin (Sn) and oxygen (O), and the third region includes at least one third element selected from the group consisting of tantalum (Ta), niobium (Nb) and vanadium (V) and oxygen (O). The first conductive layer includes at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au) and nickel (Ni), and the third conductive layer includes at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au) and nickel (Ni).
[0012] The memory device of the first embodiment further includes a plurality of first wirings and a plurality of second wirings intersecting the plurality of first wirings, and the memory cell is provided in a region where one of the plurality of first wirings intersects one of the plurality of second wirings.
[0013] FIG. 1 is a block diagram of a storage device according to the first embodiment.
[0014] The memory cell array 100 of the storage device of the first embodiment includes, for example, a plurality of word lines 102 and a plurality of bit lines 103 intersecting the word lines 102 on a semiconductor substrate 101 via an insulating layer. The bit lines 103 are provided, for example, in an upper layer above the word lines 102. The word lines 102 may be provided in an upper layer above the bit lines 103. In addition, a first control circuit 104, a second control circuit 105, and a sense circuit 106 are provided around the memory cell array 100 as peripheral circuits.
[0015] The word line 102 is an example of a first wiring, and the bit line 103 is an example of a second wiring.
[0016] A plurality of memory cells MC are provided in the regions where the word lines 102 and the bit lines 103 intersect. The storage device of the first embodiment is a two-terminal magnetoresistive memory having a cross-point structure.
[0017] The word lines 102 are each connected to a first control circuit 104. The bit lines 103 are each connected to a second control circuit 105. The sense circuit 106 is connected to the first control circuit 104 and the second control circuit 105.
[0018] The first control circuit 104 and the second control circuit 105 have functions, for example, to select a desired memory cell MC and write data to the memory cell MC, read data from the memory cell MC, erase data from the memory cell MC, etc. When reading data, the data in the memory cell MC is read as the amount of current flowing between the word line 102 and the bit line 103, or as a change in potential of the bit line 103. The sense circuit 106 has a function to determine the amount of current and judge the polarity of the data. For example, it judges whether the data is "0" or "1".
[0019] The first control circuit 104, the second control circuit 105, and the sense circuit 106 are configured, for example, as electronic circuits using semiconductor devices formed on the semiconductor substrate 101.
[0020] 2 is a schematic cross-sectional view of a memory cell in the memory device of the first embodiment. Fig. 2 shows a cross-section of one memory cell MC indicated by, for example, a dotted circle in the memory cell array 100 of Fig. 1.
[0021] 2 , the memory cell MC includes a lower electrode 10, an upper electrode 20, an intermediate electrode 30, a switching layer 40, and a resistance change layer 50. The switching layer 40 includes a lower region 41, an upper region 42, and an intermediate region 43. The resistance change layer 50 includes a fixed layer 51, a tunnel layer 52, and a free layer 53.
[0022] The bottom electrode 10 is an example of a first conductive layer. The top electrode 20 is an example of a second conductive layer. The middle electrode 30 is an example of a third conductive layer. The bottom region 41 is an example of a first region. The top region 42 is an example of a second region. The middle region 43 is an example of a third region.
[0023] The lower electrode 10, the switching layer 40, and the intermediate electrode 30 constitute a switching element of the memory cell MC. The intermediate electrode 30, the resistance change layer 50, and the upper electrode 20 constitute a resistance change element of the memory cell MC.
[0024] The bottom electrode 10 is connected to the word line 102. The bottom electrode 10 includes at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The bottom electrode 10 includes at least one material selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The bottom electrode 10 is, for example, carbon (C), cobalt (Co), gold (Au), or nickel (Ni).
[0025] The lower electrode 10 may be a part of the word line 102 .
[0026] The upper electrode 20 is connected to the bit line 103. The upper electrode 20 is, for example, a metal. The upper electrode 20 includes, for example, at least one material selected from the group consisting of carbon, carbon nitride, tungsten, tungsten carbide, and tungsten nitride.
[0027] The upper electrode 20 may be a part of the bit line 103 .
[0028] The intermediate electrode 30 is provided between the lower electrode 10 and the upper electrode 20. The intermediate electrode 30 includes at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The intermediate electrode 30 includes at least one material selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni), for example. The intermediate electrode 30 is, for example, carbon (C), cobalt (Co), gold (Au), or nickel (Ni).
[0029] The switching layer 40 is provided between the lower electrode 10 and the intermediate electrode 30. The thickness of the switching layer 40 in a first direction from the lower electrode 10 toward the upper electrode 20 is, for example, not less than 5 nm and not more than 50 nm.
[0030] The switching layer 40 has a function of suppressing an increase in a half-selected leakage current flowing through a half-selected cell. The switching layer 40 has a nonlinear current-voltage characteristic in which the current rises sharply at a specific threshold voltage.
[0031] The switching layer 40 includes a lower region 41, an upper region 42, and an intermediate region 43. The upper region 42 is provided between the lower region 41 and the intermediate electrode 30. The intermediate region 43 is provided between the lower region 41 and the upper region 42.
[0032] The lower region 41 contacts, for example, the lower electrode 10. The lower region 41 contacts, for example, the middle region 43. The upper region 42 contacts, for example, the middle electrode 30. The upper region 42 contacts, for example, the middle region 43.
[0033] The lower region 41 of the switching layer 40 includes at least one first element selected from the group consisting of zinc (Zn) and tin (Sn) and oxygen (O). The lower region 41 includes, for example, a first oxide which is an oxide of the first element.
[0034] The first oxide is, for example, zinc oxide or tin oxide. The lower region 41 is, for example, zinc oxide or tin oxide.
[0035] The zinc oxide contained in the lower region 41 has a chemical composition represented by, for example, ZnO. The tin oxide contained in the lower region 41 has a chemical composition represented by, for example, SnO2.
[0036] The thickness of the lower region 41 in the first direction is, for example, not less than 1.6 nm and not more than 2.4 nm.
[0037] The upper region 42 of the switching layer 40 includes at least one second element selected from the group consisting of zinc (Zn) and tin (Sn) and oxygen (O). The upper region 42 includes a second oxide that is, for example, an oxide of the second element.
[0038] The first element and the second element are, for example, the same element. The first oxide and the second oxide are, for example, the same oxide.
[0039] The second oxide is, for example, zinc oxide or tin oxide. The upper region 42 is, for example, zinc oxide or tin oxide.
[0040] The zinc oxide contained in the upper region 42 has a chemical composition represented, for example, by ZnO. The tin oxide contained in the upper region 42 has a chemical composition represented, for example, by SnO2.
[0041] The thickness of the upper region 42 in the first direction is, for example, not less than 1.6 nm and not more than 2.4 nm.
[0042] The intermediate region 43 of the switching layer 40 contains at least one third element selected from the group consisting of tantalum (Ta), niobium (Nb), and vanadium (V), and oxygen (O). The intermediate region 43 contains a third oxide that is, for example, an oxide of the third element.
[0043] The third oxide is, for example, tantalum oxide, niobium oxide, or vanadium oxide. The intermediate region 43 is, for example, tantalum oxide, niobium oxide, or vanadium oxide.
[0044] The tantalum oxide contained in the intermediate region 43 has a chemical composition represented by, for example, Ta2O5. The niobium oxide contained in the intermediate region 43 has a chemical composition represented by, for example, Nb2O5. The vanadium oxide contained in the intermediate region 43 has a chemical composition represented by, for example, V2O5.
[0045] The thickness of the intermediate region 43 in the first direction is, for example, not less than 2.5 nm and not more than 4.0 nm.
[0046] The thickness in the first direction of the middle region 43 is, for example, thicker than the thickness in the first direction of the lower region 41. Also, the thickness in the first direction of the middle region 43 is, for example, thicker than the thickness in the first direction of the upper region 42.
[0047] The standard Gibbs energy of formation of the third oxide contained in the intermediate region 43 is smaller, for example, than the standard Gibbs energy of formation of the first oxide contained in the lower region 41. The standard Gibbs energy of formation of the third oxide contained in the intermediate region 43 is smaller, for example, than the standard Gibbs energy of formation of the second oxide contained in the upper region 42. When the standard Gibbs energy of formation has a negative value, a small standard Gibbs energy of formation means that the absolute value of the standard Gibbs energy of formation is large.
[0048] For example, the standard Gibbs energy of formation of tantalum oxide (Ta2O5), niobium oxide (Nb2O5), and vanadium oxide (V2O5) are smaller than the standard Gibbs energy of formation of zinc oxide (ZnO) and tin oxide (SnO2).
[0049] In addition, the standard Gibbs energies of formation of the first oxide, the second oxide, and the third oxide can be identified as their physical property values if the first oxide, the second oxide, and the third oxide can be identified.
[0050] The electron affinity of the third oxide contained in the intermediate region 43 is, for example, smaller than the electron affinity of the first oxide contained in the lower region 41. Also, the electron affinity of the third oxide contained in the intermediate region 43 is, for example, smaller than the electron affinity of the second oxide contained in the upper region 42.
[0051] The dielectric constant of the third oxide contained in the intermediate region 43 is, for example, greater than the dielectric constant of the first oxide contained in the lower region 41. Also, the dielectric constant of the third oxide contained in the intermediate region 43 is, for example, greater than the dielectric constant of the second oxide contained in the upper region 42.
[0052] The resistance change layer 50 is provided between the intermediate electrode 30 and the upper electrode 20. The resistance change layer 50 has a fixed layer 51, a tunnel layer 52, and a free layer 53. The resistance change layer 50 includes a magnetic tunnel junction constituted by the fixed layer 51, the tunnel layer 52, and the free layer 53.
[0053] The variable resistance layer 50 has a function of storing data by changing resistance. The variable resistance layer 50 has a characteristic that, for example, the electrical resistance changes when a predetermined voltage is applied.
[0054] The fixed layer 51 is a ferromagnetic material. In the fixed layer 51, the magnetization direction does not change with respect to a predetermined write voltage, and the magnetization direction is fixed in a specific direction.
[0055] The tunnel layer 52 is an insulator. Electrons pass through the tunnel layer 52 by the tunnel effect.
[0056] The free layer 53 is a ferromagnetic material. In the free layer 53, the magnetization direction changes in response to a predetermined write voltage. The magnetization direction of the free layer 53 can be either parallel to the magnetization direction of the fixed layer 51 or anti-parallel to the magnetization direction of the fixed layer 51. For example, by applying a voltage and passing a current between the intermediate electrode 30 and the upper electrode 20, the magnetization direction of the free layer 53 can be changed.
[0057] The electrical resistance of the resistance change layer 50 changes by changing the magnetization direction of the free layer 53. When the magnetization direction of the free layer 53 is antiparallel to the magnetization direction of the fixed layer 51, a high resistance state is achieved in which current does not easily flow. On the other hand, when the magnetization direction of the free layer 53 is parallel to the magnetization direction of the fixed layer 51, a low resistance state is achieved in which current easily flows. The arrangement of the fixed layer 51 and the free layer 53 may be reversed. In other words, the intermediate electrode 30, the free layer 53, the tunnel layer 52, the fixed layer 51, and the upper electrode 20 may be stacked in this order.
[0058] Next, the operation and effects of the storage device of the first embodiment will be described.
[0059] As described above, in the memory device of the first embodiment, the resistance of the resistance change layer 50 changes by changing the magnetization direction of the free layer 53. When the magnetization direction of the free layer 53 is antiparallel to the magnetization direction of the fixed layer 51, a high resistance state is achieved in which current does not easily flow. On the other hand, when the magnetization direction of the free layer 53 is parallel to the magnetization direction of the fixed layer 51, a low resistance state is achieved in which current easily flows.
[0060] For example, the high resistance state of the resistance change layer 50 is defined as data "1", and the low resistance state is defined as data "0". The memory cell MC can store one bit of data, "0" or "1", by maintaining different resistance states. Writing to one memory cell MC is performed by applying a voltage between the bit line 103 and word line 102 connected to the memory cell MC to pass a current.
[0061] Fig. 3 is an explanatory diagram of the problem of the memory device of the first embodiment. Fig. 3 shows the voltage applied to a memory cell MC when one memory cell MC in the memory cell array is selected for a write operation. Each memory cell MC is represented by an intersection of a word line and a bit line.
[0062] The selected memory cell MC is memory cell A (selected cell). A write voltage Vwrite is applied to the word line connected to memory cell A. In addition, 0 V is applied to the bit line connected to memory cell A.
[0063] In the following, an example will be described in which a voltage that is half the write voltage (Vwrite / 2) is applied to the word lines and bit lines that are not connected to memory cell A.
[0064] The voltage applied to memory cells C (unselected cells) connected to word lines and bit lines not connected to memory cells A is 0 V. In other words, no voltage is applied.
[0065] On the other hand, a voltage (Vwrite / 2) that is half the write voltage Vwrite is applied to memory cell B (half-selected cell) connected to the word line connected to memory cell A or the bit line connected to memory cell A. Therefore, a half-selection leakage current flows through memory cell B (half-selected cell).
[0066] In addition, as an alternative to the above, a method may be used in which half the write voltage (Vwrite / 2) is applied to the word line connected to memory cell A, a negative voltage that is half the write voltage (-Vwrite / 2) is applied to the bit line, and 0V is applied to word lines and bit lines not connected to memory cell A.
[0067] 4 is an explanatory diagram of the current-voltage characteristics of the switching element of the first embodiment, in which the horizontal axis represents the voltage applied to the switching element, and the vertical axis represents the current flowing through the switching element.
[0068] The switching element has a nonlinear current-voltage characteristic in which the current rises sharply at a threshold voltage Vth, which is, for example, 0.5V or more and 3V or less.
[0069] In the switching element of the first embodiment, the write voltage Vwrite is set so that the write voltage Vwrite is higher than the threshold voltage Vth and half the write voltage Vwrite (Vwrite / 2) is lower than the threshold voltage. The current that flows through the switching element when the write voltage Vwrite is applied is the on-current (Ion in FIG. 4). The current that flows through the switching element when half the write voltage Vwrite (Vwrite / 2) is applied is the half-select leakage current (Ihalf in FIG. 4).
[0070] The read voltage Vread of the memory cells MC is set to a voltage higher than the threshold voltage Vth and lower than the write voltage Vwrite, for example, as shown in Fig. 4. Therefore, when reading the memory cells MC, the half-selection leakage current flowing through the half-selected cells can also be suppressed.
[0071] If the half-selection leakage current is large, for example, it will lead to an increase in the power consumption of the chip. Also, for example, the voltage drop in the wiring will increase, and a sufficiently high voltage will not be applied to the selected cell, making the write operation to the memory cell MC unstable. Also, if the on-current is small, for example, the current flowing through the selected cell will be insufficient, resulting in insufficient writing to the memory cell MC. Therefore, the current-voltage characteristics of the switching element are required to achieve both a low half-selection leakage current and a high on-current.
[0072] 5(a), 5(b), and 5(c) are explanatory diagrams of the operation and effect of the memory device of the first embodiment. 5(a), 5(b), and 5(c) are explanatory diagrams of the current-voltage characteristics of the switching element of the first embodiment. 5(a), 5(b), and 5(c) show the band structures of the lower electrode 10, the lower region 41, the intermediate region 43, the upper region 42, and the intermediate electrode 30.
[0073] Fig. 5(a) shows the case where no voltage is applied between the bottom electrode 10 and the intermediate electrode 30. Fig. 5(b) shows the case where a voltage (Vwrite / 2) that is half the write voltage (Vwrite) is applied between the bottom electrode 10 and the intermediate electrode 30. Fig. 5(c) shows the case where the write voltage (Vwrite) is applied between the bottom electrode 10 and the intermediate electrode 30.
[0074] As shown in Fig. 5(a), the electron affinity (Ea3) of the intermediate region 43 is smaller than the electron affinity (Ea1) of the lower region 41 and the electron affinity (Ea2) of the upper region 42. Therefore, as shown in Fig. 5(a), the switching element of the first embodiment has a band structure in which the electron barrier in the central portion is high. The switching element of the first embodiment is a switching element having a so-called crested type band structure.
[0075] When a voltage (Vwrite / 2) that is half the write voltage (Vwrite) is applied between the lower electrode 10 and the intermediate electrode 30, the current flow is small because the electron barrier in the center is high, as shown in FIG. 5(b). In other words, the semi-selection leakage current is kept low.
[0076] When a write voltage (Vwrite) is applied between the bottom electrode 10 and the intermediate electrode 30, the effective height of the electron barrier in the center becomes lower, as shown in Fig. 5(c), and a large tunnel current flows. In other words, a large on-current flows.
[0077] Fig. 6 is an explanatory diagram of the action and effect of the memory device of the first embodiment, and is a diagram showing the band structure of the switching element of the first embodiment.
[0078] The amount of current flowing between the lower electrode 10 and the intermediate electrode 30 of the switching element can be calculated by specifying the parameters of the band structure as shown in Fig. 6. Specifically, the amount of current can be calculated by specifying the first barrier height φb1 of the lower region 41, the second barrier height φb2 of the upper region 42, the third barrier height φb3 of the intermediate region 43, the first dielectric constant ε1 of the material constituting the lower region 41, the second dielectric constant ε2 of the material constituting the upper region 42, the third dielectric constant ε3 of the material constituting the intermediate region 43, the film thickness t1 of the lower region 41, the film thickness t2 of the upper region 42, and the film thickness t3 of the intermediate region 43.
[0079] The first barrier height φb1 is the difference between the first work function φm1 of the material constituting the lower electrode 10 and the electron affinity (Ea1) of the material constituting the lower region 41. The second barrier height φb2 is the difference between the second work function φm2 of the material constituting the intermediate electrode 30 and the electron affinity (Ea2) of the material constituting the upper region 42. The third barrier height φb3 is the difference between the first work function φm1 of the material constituting the lower electrode 10 or the second work function φm2 of the material constituting the intermediate electrode 30 and the electron affinity (Ea3) of the material constituting the intermediate region 43.
[0080] The voltages applied to the lower region 41, the upper region 42, and the middle region 43 are calculated from the first dielectric constant ε1, the second dielectric constant ε2, the third dielectric constant ε3, the film thickness t1, the film thickness t2, and the film thickness t3.
[0081] The inventors calculated the semi-selected leakage current and on-current flowing through the switching element by changing the above parameters of the band structure of the crested-type switching element, and found a combination of materials constituting the lower region 41, the upper region 42, the intermediate region 43, the lower electrode 10, and the intermediate electrode 30 that can achieve both a low semi-selected leakage current and a high on-current.
[0082] The switching element of the memory device of the first embodiment can achieve both a low semi-select leakage current and a high on-current by containing appropriate materials in the lower region 41, the upper region 42, the intermediate region 43, the lower electrode 10, and the intermediate electrode 30.
[0083] Consider a case in which, in the switching element of the memory device of the first embodiment, the lower region 41 contains a first oxide which is an oxide of the first element, the upper region 42 contains a second oxide which is an oxide of the second element, and the middle region 43 contains a third oxide which is an oxide of the third element. In this case, it is preferable that the standard Gibbs energy of formation of the third oxide is smaller than the standard Gibbs energy of formation of the first oxide, and the standard Gibbs energy of formation of the third oxide is smaller than the standard Gibbs energy of formation of the second oxide.
[0084] As described above, the intermediate region 43 has a high electron barrier and functions to suppress leakage current. If the standard Gibbs energy of formation of the third oxide contained in the intermediate region 43 is large, oxygen may be desorbed from the third oxide, resulting in the formation of oxygen vacancies. If the number of oxygen vacancies in the intermediate region 43 increases, current may flow through the oxygen vacancies, increasing the semi-selective leakage current.
[0085] By making the standard Gibbs energy of formation of the third oxide contained in the intermediate region 43 smaller than the standard Gibbs energy of formation of the first oxide contained in the lower region 41 and the standard Gibbs energy of formation of the second oxide contained in the upper region 42, desorption of oxygen from the intermediate region 43 is suppressed, and an increase in semi-selective leakage current is suppressed.
[0086] From the viewpoint of achieving both a low semi-selection leakage current and a high on-current, it is preferable that the thickness in the first direction of the intermediate region 43 is thicker than the thickness in the first direction of the lower region 41 and the thickness in the first direction of the upper region 42.
[0087] From the viewpoint of achieving both a low semi-selected leakage current and a high on-current, the thickness in the first direction of the lower region 41 and the thickness in the first direction of the upper region 42 are preferably 1.6 nm or more and 2.4 nm or less. From the viewpoint of achieving both a low semi-selected leakage current and a high on-current, the thickness in the first direction of the intermediate region 43 is preferably 2.5 nm or more and 4.0 nm or less.
[0088] As described above, according to the first embodiment, a switching element having excellent characteristics, such as a low semi-selection leakage current and a high on-current, can be realized, and further, a memory device having a switching element having excellent characteristics can be realized.
[0089] Second embodiment The memory device of the second embodiment differs from the memory device of the first embodiment in that it further includes a first sidewall including a fourth oxide and a second sidewall including a fifth oxide, and in a second direction perpendicular to the first direction from the first conductive layer to the second conductive layer, the first region is provided between the first sidewall and the second sidewall, and in the second direction, the second region is provided between the first sidewall and the second sidewall. The first region includes a first oxide that is an oxide of a first element, the second region includes a second oxide that is an oxide of a second element, the standard Gibbs energy of formation of the fourth oxide is greater than the standard Gibbs energy of formation of the first oxide, the standard Gibbs energy of formation of the fourth oxide is greater than the standard Gibbs energy of formation of the second oxide, the standard Gibbs energy of formation of the fifth oxide is greater than the standard Gibbs energy of formation of the first oxide, and the standard Gibbs energy of formation of the fifth oxide is greater than the standard Gibbs energy of formation of the second oxide. In the following, some of the contents that overlap with the storage device of the first embodiment may be omitted.
[0090] Fig. 7 is a schematic cross-sectional view of a memory cell in a memory device according to the second embodiment. Fig. 7 is a view corresponding to Fig. 2 of the first embodiment. Fig. 7 shows a cross section of one memory cell MC.
[0091] 7 , the memory cell MC includes a lower electrode 10, an upper electrode 20, an intermediate electrode 30, a switching layer 40, a resistance change layer 50, a first sidewall 61, and a second sidewall 62. The switching layer 40 includes a lower region 41, an upper region 42, and an intermediate region 43. The resistance change layer 50 includes a fixed layer 51, a tunnel layer 52, and a free layer 53.
[0092] The bottom electrode 10 is an example of a first conductive layer. The top electrode 20 is an example of a second conductive layer. The middle electrode 30 is an example of a third conductive layer. The bottom region 41 is an example of a first region. The top region 42 is an example of a second region. The middle region 43 is an example of a third region.
[0093] The lower electrode 10, the switching layer 40, and the intermediate electrode 30 constitute a switching element of the memory cell MC. The intermediate electrode 30, the resistance change layer 50, and the upper electrode 20 constitute a resistance change element of the memory cell MC.
[0094] The lower electrode 10 contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni).
[0095] The upper electrode 20 is, for example, a metal, and includes, for example, at least one material selected from the group consisting of carbon, carbon nitride, tungsten, tungsten carbide, and tungsten nitride.
[0096] The intermediate electrode 30 contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni).
[0097] The switching layer 40 includes a lower region 41, an upper region 42, and an intermediate region 43. The upper region 42 is provided between the lower region 41 and the intermediate electrode 30. The intermediate region 43 is provided between the lower region 41 and the upper region 42.
[0098] The lower region 41 contacts, for example, the lower electrode 10. The lower region 41 contacts, for example, the middle region 43. The upper region 42 contacts, for example, the middle electrode 30. The upper region 42 contacts, for example, the middle region 43.
[0099] The lower region 41 of the switching layer 40 includes at least one first element selected from the group consisting of zinc (Zn) and tin (Sn) and oxygen (O). The lower region 41 includes, for example, a first oxide which is an oxide of the first element.
[0100] The upper region 42 of the switching layer 40 includes at least one second element selected from the group consisting of zinc (Zn) and tin (Sn) and oxygen (O). The upper region 42 includes a second oxide that is, for example, an oxide of the second element.
[0101] The intermediate region 43 of the switching layer 40 contains at least one third element selected from the group consisting of tantalum (Ta), niobium (Nb), and vanadium (V), and oxygen (O). The intermediate region 43 contains a third oxide that is, for example, an oxide of the third element.
[0102] A direction perpendicular to the first direction from the lower electrode 10 toward the upper electrode 20 is defined as a second direction.
[0103] In the second direction, the switching layer 40 is provided between the first sidewall 61 and the second sidewall 62. In the second direction, the lower region 41 is provided between the first sidewall 61 and the second sidewall 62. In the second direction, the upper region 42 is provided between the first sidewall 61 and the second sidewall 62. In the second direction, the middle region 43 is provided between the first sidewall 61 and the second sidewall 62. The first sidewall 61 and the second sidewall 62 may be separated, but for example, in a cross section perpendicular to the first direction, the first sidewall 61 and the second sidewall 62 may be connected to surround the switching layer 40.
[0104] The first side wall 61 and the second side wall 62 contact, for example, the lower region 41, the upper region 42, and the middle region 43.
[0105] In the second direction, for example, the bottom electrode 10 and the intermediate electrode 30 are provided between the first sidewall 61 and the second sidewall 62. The first sidewall 61 and the second sidewall 62 contact the bottom electrode 10 and the intermediate electrode 30, for example.
[0106] The first sidewall 61 includes a fourth oxide, and the second sidewall 62 includes a fifth oxide.
[0107] The standard Gibbs energy of formation of the fourth oxide contained in the first side wall 61 is greater than the standard Gibbs energy of formation of the first oxide contained in the lower region 41. Also, the standard Gibbs energy of formation of the fourth oxide contained in the first side wall 61 is greater than the standard Gibbs energy of formation of the second oxide contained in the upper region 42.
[0108] The fourth oxide contained in the first side wall 61 is, for example, tungsten oxide, germanium oxide, manganese oxide, cobalt oxide, or bismuth oxide. The tungsten oxide contained in the first side wall 61 has a chemical composition represented, for example, by WO3 or WO2. The germanium oxide contained in the first side wall 61 has a chemical composition represented, for example, by GeO2. The manganese oxide contained in the first side wall 61 has a chemical composition represented, for example, by MnO2. The cobalt oxide contained in the first side wall 61 has a chemical composition represented, for example, by Co3O4 or CoO. The bismuth oxide contained in the first side wall 61 has a chemical composition represented, for example, by Bi2O3.
[0109] The standard Gibbs energy of formation of the fifth oxide contained in the second side wall 62 is greater than the standard Gibbs energy of formation of the first oxide contained in the lower region 41. Also, the standard Gibbs energy of formation of the fifth oxide contained in the second side wall 62 is greater than the standard Gibbs energy of formation of the second oxide contained in the upper region 42.
[0110] The fifth oxide contained in the second side wall 62 is, for example, tungsten oxide, germanium oxide, manganese oxide, cobalt oxide, or bismuth oxide. The tungsten oxide contained in the second side wall 62 has a chemical composition represented, for example, by WO3 or WO2. The germanium oxide contained in the second side wall 62 has a chemical composition represented, for example, by GeO2. The manganese oxide contained in the second side wall 62 has a chemical composition represented, for example, by MnO2. The cobalt oxide contained in the second side wall 62 has a chemical composition represented, for example, by Co3O4 or CoO. The bismuth oxide contained in the second side wall 62 has a chemical composition represented, for example, by Bi2O3.
[0111] Below is an example of the relationship between the standard Gibbs energies of formation of oxides. A group of oxides are listed in order from the highest standard Gibbs energy of formation to the lowest. The order from highest standard Gibbs energy of formation to the lowest is palladium oxide (PdO), bismuth oxide (Bi2O3), cobalt oxide (Co3O4), cobalt oxide (CoO), manganese oxide (MnO2), germanium oxide (GeO2), tungsten oxide (WO3), tin oxide (SnO2), molybdenum oxide (MoO2), tungsten oxide (WO2), indium oxide (In2O3), vanadium oxide (V2O5), zinc oxide (ZnO), and tin oxide (TiO2). Vanadium oxide (V2O4), gallium oxide (Ga2O3), chromium oxide (Cr2O3), niobium oxide (Nb2O5), manganese oxide (MnO), niobium oxide (NbO2), vanadium oxide (V2O3), tantalum oxide (Ta2O5), vanadium oxide (VO), silicon oxide (SiO2), titanium oxide (TiO2), zirconium oxide (ZrO2), aluminum oxide (Al2O3), hafnium oxide (HfO2), and yttrium oxide (Y2O3).
[0112] The thickness of the first side wall 61 in the second direction is, for example, not less than 2 nm and not more than 20 nm. The thickness of the second side wall 62 in the second direction is, for example, not less than 2 nm and not more than 20 nm.
[0113] Next, the operation and effects of the storage device of the second embodiment will be described.
[0114] Consider a case where the memory cell MC of the second embodiment does not have the first sidewall 61 and the second sidewall 62. In this case, for example, the on-current of the switching element may be reduced.
[0115] The reason why the on-current of the switching element becomes low is considered to be, for example, that oxygen is extracted from the lower region 41 to the lower electrode 10, and oxygen vacancies are generated in the lower region 41. It is considered that, due to the oxygen vacancies being generated in the lower region 41, the Fermi level of the lower electrode 10 is pinned to the lower region 41, and the first barrier height φb1 (see FIG. 6) between the lower electrode 10 and the lower region 41 becomes large.
[0116] Also, the reason why the on-current of the switching element becomes low is believed to be, for example, that oxygen is extracted from the upper region 42 to the intermediate electrode 30, and oxygen vacancies are generated in the upper region 42. It is believed that the generation of oxygen vacancies in the upper region 42 causes the Fermi level of the intermediate electrode 30 to be pinned to the upper region 42, and the second barrier height φb2 (see FIG. 6) between the intermediate electrode 30 and the upper region 42 becomes large.
[0117] The memory cell MC of the second embodiment is provided with a first sidewall 61. The standard Gibbs energy of formation of the fourth oxide contained in the first sidewall 61 is greater than the standard Gibbs energy of formation of the first oxide contained in the lower region 41. In other words, oxygen in the fourth oxide contained in the first sidewall 61 is more easily removed than oxygen in the first oxide contained in the lower region 41. For this reason, oxygen is removed from the first sidewall 61 and supplied to the lower region 41, filling the oxygen vacancies in the lower region 41. Therefore, the Fermi level pinning of the lower electrode 10 is suppressed, and the change in the first barrier height φb1 is suppressed. Therefore, the on-current of the switching element can be suppressed from decreasing.
[0118] Moreover, the standard Gibbs energy of formation of the fourth oxide contained in the first sidewall 61 is greater than the standard Gibbs energy of formation of the second oxide contained in the upper region 42. In other words, oxygen in the fourth oxide contained in the first sidewall 61 is more easily removed than oxygen in the second oxide contained in the upper region 42. For this reason, oxygen is removed from the first sidewall 61 and supplied to the upper region 42, filling oxygen vacancies in the upper region 42. Therefore, Fermi level pinning of the intermediate electrode 30 is suppressed, and a change in the second barrier height φb2 is suppressed. This makes it possible to suppress a decrease in the on-current of the switching element.
[0119] The memory cell MC of the second embodiment is provided with a second sidewall 62. The standard Gibbs energy of formation of the fifth oxide contained in the second sidewall 62 is greater than the standard Gibbs energy of formation of the first oxide contained in the lower region 41. In other words, oxygen in the fifth oxide contained in the second sidewall 62 is more easily removed than oxygen in the first oxide contained in the lower region 41. For this reason, oxygen is removed from the second sidewall 62 and supplied to the lower region 41, filling the oxygen vacancies in the lower region 41. Therefore, the Fermi level pinning of the lower electrode 10 is suppressed, and the change in the first barrier height φb1 is suppressed. Therefore, the on-current of the switching element can be suppressed from decreasing.
[0120] Moreover, the standard Gibbs energy of formation of the fifth oxide contained in the second sidewall 62 is greater than the standard Gibbs energy of formation of the second oxide contained in the upper region 42. In other words, oxygen in the fifth oxide contained in the second sidewall 62 is more easily removed than oxygen in the second oxide contained in the upper region 42. For this reason, oxygen is removed from the second sidewall 62 and supplied to the upper region 42, filling oxygen vacancies in the upper region 42. Therefore, Fermi level pinning of the intermediate electrode 30 is suppressed, and a change in the second barrier height φb2 is suppressed. This makes it possible to suppress a decrease in the on-current of the switching element.
[0121] Furthermore, by providing the first sidewall 61 and the second sidewall 62, a reduction in semi-selective leakage current of the switching element can be expected. For example, when the switching layer 40 is processed by reactive ion etching (RIE), oxygen vacancies are formed on the side surface of the switching layer 40 due to etching damage. In this case, leakage current due to the oxygen vacancies flows, and there is a risk of an increase in semi-selective leakage current.
[0122] Oxygen vacancies caused by etching damage are filled by oxygen being supplied to the side surface of the switching layer 40 from the first side wall 61 and the second side wall 62. Therefore, it is possible to reduce the semi-selective leakage current.
[0123] According to the second embodiment, a switching element having excellent characteristics such as a low semi-selection leakage current and a high on-current can be realized, similarly to the first embodiment. In addition, Fermi level pinning is suppressed, and the on-current of the switching element is further increased.
[0124] (First Modification) The storage device of the first modification of the second embodiment further includes a third sidewall including a sixth oxide and a fourth sidewall including a seventh oxide, wherein in the second direction, the third sidewall is provided between the first region and the first sidewall, in the second direction, the third sidewall is provided between the second region and the first sidewall, in the second direction, the fourth sidewall is provided between the first region and the second sidewall, in the second direction, the fourth sidewall is provided between the second region and the second sidewall, and the standard Gibbs energy of formation of the sixth oxide is greater than the standard Gibbs energy of formation of the first oxide, The memory device of the second embodiment differs from the memory device of the sixth oxide in that the standard Gibbs energy of formation of the sixth oxide is greater than the standard Gibbs energy of formation of the second oxide, the standard Gibbs energy of formation of the sixth oxide is less than the standard Gibbs energy of formation of the fourth oxide, the standard Gibbs energy of formation of the seventh oxide is greater than the standard Gibbs energy of formation of the first oxide, the standard Gibbs energy of formation of the seventh oxide is greater than the standard Gibbs energy of formation of the second oxide, and the standard Gibbs energy of formation of the seventh oxide is less than the standard Gibbs energy of formation of the fifth oxide.
[0125] Fig. 8 is a schematic cross-sectional view of a memory cell of a memory device according to a first modified example of the second embodiment. Fig. 8 corresponds to Fig. 7 of the second embodiment. Fig. 8 shows a cross section of one memory cell MC.
[0126] 8 , the memory cell MC includes a lower electrode 10, an upper electrode 20, an intermediate electrode 30, a switching layer 40, a resistance change layer 50, a first sidewall 61, a second sidewall 62, a third sidewall 63, and a fourth sidewall 64. The switching layer 40 includes a lower region 41, an upper region 42, and an intermediate region 43. The resistance change layer 50 includes a fixed layer 51, a tunnel layer 52, and a free layer 53.
[0127] In the second direction, the switching layer 40 is provided between the first sidewall 61 and the second sidewall 62. In the second direction, the lower region 41 is provided between the first sidewall 61 and the second sidewall 62. In the second direction, the upper region 42 is provided between the first sidewall 61 and the second sidewall 62. In the second direction, the middle region 43 is provided between the first sidewall 61 and the second sidewall 62. The first sidewall 61 and the second sidewall 62 may be separated, but for example, in a cross section perpendicular to the first direction, the first sidewall 61 and the second sidewall 62 may be connected to surround the switching layer 40.
[0128] In the second direction, the third sidewall 63 is provided between the lower region 41 and the first sidewall 61. In the second direction, the third sidewall 63 is provided between the upper region 42 and the first sidewall 61. In the second direction, the fourth sidewall 64 is provided between the lower region 41 and the second sidewall 62. In the second direction, the fourth sidewall 64 is provided between the upper region 42 and the second sidewall 62. The third sidewall 63 and the fourth sidewall 64 may be separated, but for example, in a cross section perpendicular to the first direction, the third sidewall 63 and the fourth sidewall 64 may be connected to surround the switching layer 40.
[0129] The third side wall 63 and the fourth side wall 64 contact, for example, the lower region 41, the upper region 42, and the middle region 43.
[0130] In the second direction, for example, the bottom electrode 10 and the intermediate electrode 30 are provided between the third sidewall 63 and the fourth sidewall 64. The third sidewall 63 and the fourth sidewall 64 contact the bottom electrode 10 and the intermediate electrode 30, for example.
[0131] The first side wall 61 is in contact with, for example, a third side wall 63. The second side wall 62 is in contact with, for example, a fourth side wall 64.
[0132] The first sidewall 61 includes a fourth oxide. The second sidewall 62 includes a fifth oxide. The third sidewall 63 includes a sixth oxide. The fourth sidewall 64 includes a seventh oxide.
[0133] The standard Gibbs energy of formation of the fourth oxide contained in the first side wall 61 is greater than the standard Gibbs energy of formation of the first oxide contained in the lower region 41. Also, the standard Gibbs energy of formation of the fourth oxide contained in the first side wall 61 is greater than the standard Gibbs energy of formation of the second oxide contained in the upper region 42.
[0134] The standard Gibbs energy of formation of the fifth oxide contained in the second side wall 62 is greater than the standard Gibbs energy of formation of the first oxide contained in the lower region 41. Also, the standard Gibbs energy of formation of the fifth oxide contained in the second side wall 62 is greater than the standard Gibbs energy of formation of the second oxide contained in the upper region 42.
[0135] The standard Gibbs energy of formation of the sixth oxide contained in the third side wall 63 is greater than the standard Gibbs energy of formation of the first oxide contained in the lower region 41. Also, the standard Gibbs energy of formation of the sixth oxide contained in the third side wall 63 is greater than the standard Gibbs energy of formation of the second oxide contained in the upper region 42. Also, the standard Gibbs energy of formation of the sixth oxide contained in the third side wall 63 is less than the standard Gibbs energy of formation of the fourth oxide contained in the first side wall 16.
[0136] The standard Gibbs energy of formation of the seventh oxide contained in the fourth side wall 64 is greater than the standard Gibbs energy of formation of the first oxide contained in the lower region 41. Also, the standard Gibbs energy of formation of the seventh oxide contained in the fourth side wall 64 is greater than the standard Gibbs energy of formation of the second oxide contained in the upper region 42. Also, the standard Gibbs energy of formation of the seventh oxide contained in the fourth side wall 64 is less than the standard Gibbs energy of formation of the fifth oxide contained in the second side wall 62.
[0137] The thickness of the third side wall 63 in the second direction is, for example, not less than 2 nm and not more than 20 nm. The thickness of the fourth side wall 64 in the second direction is, for example, not less than 2 nm and not more than 20 nm.
[0138] Consider a case where the third sidewall 63 and the fourth sidewall 64 are not provided in the memory cell MC of the first modification of the second embodiment. In this case, for example, a leakage current flows between the lower electrode 10 and the intermediate electrode 30, and the semi-selection leakage current may become high.
[0139] As described in the second embodiment, oxygen is desorbed from the first sidewall 61 and supplied to the lower region 41 and the upper region 42, filling the oxygen vacancies in the lower region 41 and the upper region 42. At this time, oxygen vacancies are formed in the first sidewall 61 from which oxygen has been desorbed. When the number of oxygen vacancies in the first sidewall 61 increases, a leakage current flows through the oxygen vacancies. For example, when the first sidewall 61 is in contact with the lower electrode 10 and the intermediate electrode 30, a leakage current flows between the lower electrode 10 and the intermediate electrode 30.
[0140] Similarly, oxygen is desorbed from the second sidewall 62 and supplied to the lower region 41 and the upper region 42, filling the oxygen vacancies in the lower region 41 and the upper region 42. At this time, oxygen vacancies are formed in the second sidewall 62 from which oxygen has been desorbed. When the number of oxygen vacancies in the second sidewall 62 increases, a leakage current flows through the oxygen vacancies. For example, when the second sidewall 62 is in contact with the lower electrode 10 and the intermediate electrode 30, a leakage current flows between the lower electrode 10 and the intermediate electrode 30.
[0141] In the memory cell MC of the first modification of the second embodiment, a third sidewall 63 is provided between the first sidewall 61 and the lower electrode 10 and intermediate electrode 30. Therefore, the first sidewall 61 is separated from the lower electrode 10 and intermediate electrode 30. Therefore, leakage current is prevented from flowing between the lower electrode 10 and intermediate electrode 30 through the first sidewall 61.
[0142] The standard Gibbs energy of formation of the sixth oxide contained in the third side wall 63 is greater than the standard Gibbs energy of formation of the first oxide contained in the lower region 41. In other words, oxygen in the sixth oxide contained in the third side wall 63 is more easily released than oxygen in the first oxide contained in the lower region 41. For this reason, oxygen is released from the third side wall 63 and supplied to the lower region 41, filling oxygen vacancies in the lower region 41.
[0143] Furthermore, the standard Gibbs energy of formation of the sixth oxide contained in the third side wall 63 is greater than the standard Gibbs energy of formation of the second oxide contained in the upper region 42. In other words, oxygen in the sixth oxide contained in the third side wall 63 is more easily released than oxygen in the second oxide contained in the upper region 42. For this reason, oxygen is released from the third side wall 63 and supplied to the upper region 42, filling oxygen vacancies in the upper region 42.
[0144] Moreover, in the memory cell MC of the first modified example of the second embodiment, a fourth sidewall 64 is provided between the second sidewall 62 and the bottom electrode 10 and intermediate electrode 30. Therefore, the second sidewall 62 is separated from the bottom electrode 10 and intermediate electrode 30. Therefore, a leakage current is prevented from flowing between the bottom electrode 10 and intermediate electrode 30 through the second sidewall 62.
[0145] The standard Gibbs energy of formation of the seventh oxide contained in the fourth side wall 64 is greater than the standard Gibbs energy of formation of the first oxide contained in the lower region 41. In other words, oxygen in the seventh oxide contained in the fourth side wall 64 is more easily released than oxygen in the first oxide contained in the lower region 41. For this reason, oxygen is released from the fourth side wall 64 and supplied to the lower region 41, filling oxygen vacancies in the lower region 41.
[0146] Furthermore, the standard Gibbs energy of formation of the seventh oxide contained in the fourth side wall 64 is greater than the standard Gibbs energy of formation of the second oxide contained in the upper region 42. In other words, oxygen in the seventh oxide contained in the fourth side wall 64 is more easily released than oxygen in the second oxide contained in the upper region 42. For this reason, oxygen is released from the fourth side wall 64 and supplied to the upper region 42, filling oxygen vacancies in the upper region 42.
[0147] Therefore, similarly to the second embodiment, it is possible to prevent the on-current of the switching element from decreasing.
[0148] Oxygen vacancies are formed in the third side wall 63 from which oxygen has been desorbed. However, the standard Gibbs energy of formation of the sixth oxide contained in the third side wall 63 is smaller than the standard Gibbs energy of formation of the fourth oxide contained in the first side wall 61. In other words, oxygen in the fourth oxide contained in the first side wall 61 is more likely to escape than oxygen in the sixth oxide contained in the third side wall 63. For this reason, oxygen is desorbed from the first side wall 61 and supplied to the third side wall 63, filling the oxygen vacancies in the third side wall 63. Therefore, leakage current is prevented from flowing between the lower electrode 10 and the intermediate electrode 30 through the third side wall 63.
[0149] Oxygen vacancies are formed in the fourth side wall 64 from which oxygen has been desorbed. However, the standard Gibbs energy of formation of the seventh oxide contained in the fourth side wall 64 is smaller than the standard Gibbs energy of formation of the fifth oxide contained in the second side wall 62. In other words, oxygen in the fifth oxide contained in the second side wall 62 is more likely to escape than oxygen in the seventh oxide contained in the fourth side wall 64. For this reason, oxygen is desorbed from the second side wall 62 and supplied to the fourth side wall 64, filling the oxygen vacancies in the fourth side wall 64. Therefore, leakage current is prevented from flowing between the lower electrode 10 and the intermediate electrode 30 through the fourth side wall 64.
[0150] Therefore, according to the first modification of the second embodiment, the half-selection leakage current is prevented from becoming high.
[0151] (Second Modification) The memory device of the second variant of the second embodiment differs from the memory device of the second embodiment in that the first sidewall is separated from the first conductive layer or the third conductive layer, and the second sidewall is separated from the first conductive layer or the third conductive layer.
[0152] Fig. 9 is a schematic cross-sectional view of a memory cell of a memory device according to a second modification of the second embodiment. Fig. 9 corresponds to Fig. 7 of the second embodiment. Fig. 9 shows a cross section of one memory cell MC.
[0153] 9 , the memory cell MC includes a lower electrode 10, an upper electrode 20, an intermediate electrode 30, a switching layer 40, a resistance change layer 50, a first sidewall 61, and a second sidewall 62. The switching layer 40 includes a lower region 41, an upper region 42, and an intermediate region 43. The resistance change layer 50 includes a fixed layer 51, a tunnel layer 52, and a free layer 53.
[0154] The first side wall 61 is spaced apart from the intermediate electrode 30. In addition, the second side wall 62 is spaced apart from the intermediate electrode 30.
[0155] As described in the second embodiment, oxygen is desorbed from the first sidewall 61 and supplied to the lower region 41 and the upper region 42, filling the oxygen vacancies in the lower region 41 and the upper region 42. At this time, oxygen vacancies are formed in the first sidewall 61 from which oxygen has been desorbed. When the number of oxygen vacancies in the first sidewall 61 increases, a leakage current flows through the oxygen vacancies. For example, when the first sidewall 61 is in contact with the lower electrode 10 and the intermediate electrode 30, a leakage current flows between the lower electrode 10 and the intermediate electrode 30.
[0156] Similarly, oxygen is desorbed from the second sidewall 62 and supplied to the lower region 41 and the upper region 42, filling the oxygen vacancies in the lower region 41 and the upper region 42. At this time, oxygen vacancies are formed in the second sidewall 62 from which oxygen has been desorbed. When the number of oxygen vacancies in the second sidewall 62 increases, a leakage current flows through the oxygen vacancies. For example, when the second sidewall 62 is in contact with the lower electrode 10 and the intermediate electrode 30, a leakage current flows between the lower electrode 10 and the intermediate electrode 30.
[0157] In the memory cell MC according to the second modification of the second embodiment, the first sidewall 61 and the intermediate electrode 30 are spaced apart. Also, the second sidewall 62 and the intermediate electrode 30 are spaced apart.
[0158] Therefore, a leakage current is suppressed from flowing between the lower electrode 10 and the intermediate electrode 30 through the first side wall 61. In addition, a leakage current is suppressed from flowing between the lower electrode 10 and the intermediate electrode 30 through the second side wall 62.
[0159] Therefore, according to the second modification of the second embodiment, the half-selection leakage current is prevented from increasing.
[0160] It is also possible to adopt a configuration in which the first sidewall 61 is separated from the lower electrode 10, and the second sidewall 62 is separated from the lower electrode 10. It is also possible to adopt a configuration in which the first sidewall 61 is separated from the intermediate electrode 30 and the lower electrode 10, and the second sidewall 62 is separated from the intermediate electrode 30 and the lower electrode 10.
[0161] (Third Modification) The memory device of the third variant of the second embodiment differs from the memory device of the second embodiment in that the thickness in the second direction of the first sidewall located in the second direction of the first region is different from the thickness in the second direction of the first sidewall located in the second direction of the second region, and the thickness in the second direction of the second sidewall located in the second direction of the first region is different from the thickness in the second direction of the second sidewall located in the second direction of the second region.
[0162] Fig. 10 is a schematic cross-sectional view of a memory cell of a memory device according to a third modified example of the second embodiment. Fig. 10 corresponds to Fig. 7 of the second embodiment. Fig. 10 shows a cross section of one memory cell MC.
[0163] 10 , the memory cell MC includes a lower electrode 10, an upper electrode 20, an intermediate electrode 30, a switching layer 40, a resistance change layer 50, a first sidewall 61, and a second sidewall 62. The switching layer 40 includes a lower region 41, an upper region 42, and an intermediate region 43. The resistance change layer 50 includes a fixed layer 51, a tunnel layer 52, and a free layer 53.
[0164] The first side wall 61 has a tapered shape. A first thickness in the second direction of the first side wall 61 located in the second direction of the lower region 41 (tx1 in FIG. 10) is different from a second thickness in the second direction of the first side wall 61 located in the second direction of the upper region 42 (tx2 in FIG. 10).
[0165] The first thickness tx1 of the first side wall 61 is thicker than the second thickness tx2 of the first side wall 61. The first thickness tx1 is, for example, not less than 10 times and not more than 100 times the second thickness tx2.
[0166] The second side wall 62 has a tapered shape. A third thickness in the second direction (ty1 in FIG. 10) of the second side wall 62 located in the second direction of the lower region 41 is different from a fourth thickness in the second direction (ty2 in FIG. 10) of the second side wall 62 located in the second direction of the upper region 42.
[0167] The second thickness ty1 of the second side wall 62 is thicker than the fourth thickness ty2 of the second side wall 62. The second thickness ty1 is, for example, not less than 10 times and not more than 100 times the fourth thickness ty2.
[0168] As described in the second embodiment, oxygen is desorbed from the first sidewall 61 and supplied to the lower region 41 and the upper region 42, filling the oxygen vacancies in the lower region 41 and the upper region 42. At this time, oxygen vacancies are formed in the first sidewall 61 from which oxygen has been desorbed. When the number of oxygen vacancies in the first sidewall 61 increases, a leakage current flows through the oxygen vacancies. For example, when the first sidewall 61 is in contact with the lower electrode 10 and the intermediate electrode 30, a leakage current flows between the lower electrode 10 and the intermediate electrode 30.
[0169] Similarly, oxygen is desorbed from the second sidewall 62 and supplied to the lower region 41 and the upper region 42, filling the oxygen vacancies in the lower region 41 and the upper region 42. At this time, oxygen vacancies are formed in the second sidewall 62 from which oxygen has been desorbed. When the number of oxygen vacancies in the second sidewall 62 increases, a leakage current flows through the oxygen vacancies. For example, when the second sidewall 62 is in contact with the lower electrode 10 and the intermediate electrode 30, a leakage current flows between the lower electrode 10 and the intermediate electrode 30.
[0170] In the memory cell MC according to the third modification of the second embodiment, the first sidewall 61 and the second sidewall 62 have a tapered shape and have a thin region. The thin regions of the first sidewall 61 and the second sidewall 62 have high resistance.
[0171] Therefore, the leakage current flowing between the lower electrode 10 and the intermediate electrode 30 through the first side wall 61 is suppressed. Also, the leakage current flowing between the lower electrode 10 and the intermediate electrode 30 through the second side wall 62 is suppressed.
[0172] Therefore, according to the third modification of the second embodiment, the half-selection leakage current is prevented from becoming high.
[0173] It is also possible for the first side wall 61 and the second side wall 62 to have an inverse tapered shape. In this case, the first thickness tx1 of the first side wall 61 is thinner than the second thickness tx2 of the first side wall 61. In addition, the second thickness ty1 of the second side wall 62 is thinner than the fourth thickness ty2 of the second side wall 62.
[0174] As described above, according to the second embodiment and its modification, a switching element having excellent characteristics, such as a low semi-selection leakage current and a high on-current, can be realized. Furthermore, a memory device having a switching element having excellent characteristics can be realized.
[0175] (Third embodiment) The memory device of the third embodiment further includes a fourth region provided between the first conductive layer and the third conductive layer and in contact with either the first region or the second region, and the fourth region is different from the memory device of the first embodiment in that it includes at least one element combination selected from the group consisting of an element combination of indium (In), tin (Sn), and oxygen (O), an element combination of gallium (Ga), tin (Sn), and oxygen (O), an element combination of gallium (Ga), zinc (Zn), and oxygen (O), and an element combination of aluminum (Al), zinc (Zn), and oxygen (O). Hereinafter, some of the contents that overlap with the first embodiment may be omitted.
[0176] Fig. 11 is a schematic cross-sectional view of a memory cell in a memory device according to the third embodiment. Fig. 11 is a view corresponding to Fig. 2 of the first embodiment. Fig. 11 shows a cross section of one memory cell MC.
[0177] 11 , the memory cell MC includes a lower electrode 10, an upper electrode 20, an intermediate electrode 30, a switching layer 40, and a resistance change layer 50. The switching layer 40 includes a lower region 41, an upper region 42, an intermediate region 43, a first conductive region 44, and a second conductive region 45. The resistance change layer 50 includes a fixed layer 51, a tunnel layer 52, and a free layer 53.
[0178] The bottom electrode 10 is an example of a first conductive layer. The top electrode 20 is an example of a second conductive layer. The middle electrode 30 is an example of a third conductive layer. The bottom region 41 is an example of a first region. The top region 42 is an example of a second region. The middle region 43 is an example of a third region. The first conductive region 44 is an example of a fourth region. The second conductive region 45 is an example of a fourth region.
[0179] The lower electrode 10, the switching layer 40, and the intermediate electrode 30 constitute a switching element of the memory cell MC. The intermediate electrode 30, the resistance change layer 50, and the upper electrode 20 constitute a resistance change element of the memory cell MC.
[0180] The lower electrode 10 contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni).
[0181] The upper electrode 20 is, for example, a metal, and includes, for example, at least one material selected from the group consisting of carbon, carbon nitride, tungsten, tungsten carbide, and tungsten nitride.
[0182] The intermediate electrode 30 contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni).
[0183] The switching layer 40 includes a lower region 41, an upper region 42, a middle region 43, a first conductive region 44, and a second conductive region 45. The upper region 42 is provided between the lower region 41 and the intermediate electrode 30. The middle region 43 is provided between the lower region 41 and the upper region 42. The first conductive region 44 is provided between the lower electrode 10 and the lower region 41. The second conductive region 45 is provided between the intermediate electrode 30 and the upper region 42.
[0184] The first conductive region 44 contacts, for example, the lower electrode 10. The first conductive region 44 contacts, for example, the lower region 41. The lower region 41 contacts, for example, the middle region 43. The second conductive region 45 contacts, for example, the middle electrode 30. The second conductive region 45 contacts, for example, the upper region 42. The upper region 42 contacts, for example, the middle region 43.
[0185] The lower region 41 of the switching layer 40 includes at least one first element selected from the group consisting of zinc (Zn) and tin (Sn) and oxygen (O). The lower region 41 includes, for example, a first oxide which is an oxide of the first element.
[0186] The upper region 42 of the switching layer 40 includes at least one second element selected from the group consisting of zinc (Zn) and tin (Sn) and oxygen (O). The upper region 42 includes a second oxide that is, for example, an oxide of the second element.
[0187] The intermediate region 43 of the switching layer 40 contains at least one third element selected from the group consisting of tantalum (Ta), niobium (Nb), and vanadium (V), and oxygen (O). The intermediate region 43 contains a third oxide that is, for example, an oxide of the third element.
[0188] The first conductive region 44 has electrical conductivity. The first conductive region 44 includes at least one element combination selected from the group consisting of an element combination of indium (In), tin (Sn), and oxygen (O), an element combination of gallium (Ga), tin (Sn), and oxygen (O), an element combination of gallium (Ga), zinc (Zn), and oxygen (O), and an element combination of aluminum (Al), zinc (Zn), and oxygen (O). The first conductive region 44 includes, for example, indium tin oxide, gallium tin oxide, gallium-doped zinc oxide, or aluminum-doped zinc oxide. The first conductive region 44 is, for example, indium tin oxide, gallium tin oxide, gallium-doped zinc oxide, or aluminum-doped zinc oxide.
[0189] The second conductive region 45 has electrical conductivity. The second conductive region 45 includes at least one element combination selected from the group consisting of an element combination of indium (In), tin (Sn), and oxygen (O), an element combination of gallium (Ga), tin (Sn), and oxygen (O), an element combination of gallium (Ga), zinc (Zn), and oxygen (O), and an element combination of aluminum (Al), zinc (Zn), and oxygen (O). The second conductive region 45 includes, for example, indium tin oxide, gallium tin oxide, gallium-doped zinc oxide, or aluminum-doped zinc oxide. The second conductive region 45 is, for example, indium tin oxide, gallium tin oxide, gallium-doped zinc oxide, or aluminum-doped zinc oxide.
[0190] The thickness of the first conductive region 44 in the first direction is, for example, not less than 2 nm and not more than 20 nm. The thickness of the second conductive region 45 in the first direction is, for example, not less than 2 nm and not more than 20 nm.
[0191] Next, the operation and effects of the storage device of the third embodiment will be described.
[0192] Consider a case where the memory cell MC of the third embodiment is not provided with the first conductive region 44 and the second conductive region 45. In this case, for example, the on-current of the switching element may be reduced.
[0193] The reason why the on-current of the switching element becomes low is considered to be, for example, that oxygen is extracted from the lower region 41 to the lower electrode 10, and oxygen vacancies are generated in the lower region 41. It is considered that, due to the oxygen vacancies being generated in the lower region 41, the Fermi level of the lower electrode 10 is pinned to the lower region 41, and the first barrier height φb1 (see FIG. 6) between the lower electrode 10 and the lower region 41 becomes large.
[0194] Also, the reason why the on-current of the switching element becomes low is believed to be, for example, that oxygen is extracted from the upper region 42 to the intermediate electrode 30, and oxygen vacancies are generated in the upper region 42. It is believed that the generation of oxygen vacancies in the upper region 42 causes the Fermi level of the intermediate electrode 30 to be pinned to the upper region 42, and the second barrier height φb2 (see FIG. 6) between the intermediate electrode 30 and the upper region 42 becomes large.
[0195] The memory cell MC of the third embodiment is provided with a first conductive region 44. The first conductive region 44 has a function of releasing oxygen. The oxygen released from the first conductive region 44 is supplied to the lower region 41, and oxygen vacancies in the lower region 41 are filled. Therefore, Fermi level pinning of the lower electrode 10 is suppressed, and a change in the first barrier height φb1 is suppressed. Therefore, a decrease in the on-current of the switching element can be suppressed.
[0196] The memory cell MC of the third embodiment is provided with a second conductive region 45. The second conductive region 45 has a function of releasing oxygen. The oxygen released from the second conductive region 45 is supplied to the upper region 42, and oxygen vacancies in the upper region 42 are filled. Therefore, the Fermi level pinning of the intermediate electrode 30 is suppressed, and the change in the second barrier height φb2 is suppressed. Therefore, the on-current of the switching element can be suppressed from decreasing.
[0197] (First Modification) The memory device of the first modified example of the third embodiment differs from the memory device of the third embodiment in that the fourth region is provided only between the first conductive layer and the first region.
[0198] Fig. 12 is a schematic cross-sectional view of a memory cell of a memory device according to a first modified example of the third embodiment. Fig. 12 is a view corresponding to Fig. 11 of the third embodiment. Fig. 12 shows a cross section of one memory cell MC.
[0199] 12, the memory cell MC includes a lower electrode 10, an upper electrode 20, an intermediate electrode 30, a switching layer 40, and a resistance change layer 50. The switching layer 40 includes a lower region 41, an upper region 42, an intermediate region 43, and a first conductive region 44. The resistance change layer 50 includes a fixed layer 51, a tunnel layer 52, and a free layer 53.
[0200] The bottom electrode 10 is an example of a first conductive layer. The top electrode 20 is an example of a second conductive layer. The middle electrode 30 is an example of a third conductive layer. The bottom region 41 is an example of a first region. The top region 42 is an example of a second region. The middle region 43 is an example of a third region. The first conductive region 44 is an example of a fourth region.
[0201] The switching layer 40 includes a lower region 41, an upper region 42, a middle region 43, and a first conductive region 44. The upper region 42 is provided between the lower region 41 and the middle electrode 30. The middle region 43 is provided between the lower region 41 and the upper region 42. The first conductive region 44 is provided between the lower electrode 10 and the lower region 41.
[0202] The first conductive region 44 contacts, for example, the lower electrode 10. The first conductive region 44 contacts, for example, the lower region 41. The lower region 41 contacts, for example, the middle region 43. The upper region 42 contacts, for example, the middle electrode 30. The upper region 42 contacts, for example, the middle region 43.
[0203] The memory cell MC of the first modification of the third embodiment is provided with a first conductive region 44. The first conductive region 44 has a function of releasing oxygen. The oxygen released from the first conductive region 44 is supplied to the lower region 41, and oxygen vacancies in the lower region 41 are filled. Therefore, Fermi level pinning of the lower electrode 10 is suppressed, and a change in the first barrier height φb1 is suppressed. Therefore, a decrease in the on-current of the switching element can be suppressed.
[0204] (Second Modification) The memory device of the second modification of the third embodiment differs from the memory device of the third embodiment in that the fourth region is provided only between the third conductive layer and the second region.
[0205] Fig. 13 is a schematic cross-sectional view of a memory cell of a memory device according to a second modified example of the third embodiment. Fig. 13 corresponds to Fig. 11 of the third embodiment. Fig. 13 shows a cross section of one memory cell MC.
[0206] 13, the memory cell MC includes a lower electrode 10, an upper electrode 20, an intermediate electrode 30, a switching layer 40, and a resistance change layer 50. The switching layer 40 includes a lower region 41, an upper region 42, an intermediate region 43, and a second conductive region 45. The resistance change layer 50 includes a fixed layer 51, a tunnel layer 52, and a free layer 53.
[0207] The bottom electrode 10 is an example of a first conductive layer. The top electrode 20 is an example of a second conductive layer. The middle electrode 30 is an example of a third conductive layer. The bottom region 41 is an example of a first region. The top region 42 is an example of a second region. The middle region 43 is an example of a third region. The second conductive region 45 is an example of a fourth region.
[0208] The switching layer 40 includes a lower region 41, an upper region 42, a middle region 43, and a second conductive region 45. The upper region 42 is provided between the lower region 41 and the middle electrode 30. The middle region 43 is provided between the lower region 41 and the upper region 42. The second conductive region 45 is provided between the middle electrode 30 and the upper region 42.
[0209] The lower region 41 contacts, for example, the lower electrode 10. The lower region 41 contacts, for example, the middle region 43. The second conductive region 45 contacts, for example, the middle electrode 30. The second conductive region 45 contacts, for example, the upper region 42. The upper region 42 contacts, for example, the middle region 43.
[0210] The memory cell MC of the second modification of the third embodiment is provided with a second conductive region 45. The second conductive region 45 has a function of releasing oxygen. The oxygen released from the second conductive region 45 is supplied to the upper region 42, and oxygen vacancies in the upper region 42 are filled. Therefore, the Fermi level pinning of the intermediate electrode 30 is suppressed, and the change in the second barrier height φb2 is suppressed. Therefore, the on-current of the switching element can be suppressed from decreasing.
[0211] (Third Modification) The storage device of the third modified example of the third embodiment differs from the storage device of the third embodiment in that the fourth area is provided between the first area and the third area.
[0212] Fig. 14 is a schematic cross-sectional view of a memory cell of a memory device according to a third modification of the third embodiment. Fig. 14 corresponds to Fig. 11 of the third embodiment. Fig. 14 shows a cross section of one memory cell MC.
[0213] 14, the memory cell MC includes a lower electrode 10, an upper electrode 20, an intermediate electrode 30, a switching layer 40, and a resistance change layer 50. The switching layer 40 includes a lower region 41, an upper region 42, an intermediate region 43, and a first conductive region 44. The resistance change layer 50 includes a fixed layer 51, a tunnel layer 52, and a free layer 53.
[0214] The bottom electrode 10 is an example of a first conductive layer. The top electrode 20 is an example of a second conductive layer. The middle electrode 30 is an example of a third conductive layer. The bottom region 41 is an example of a first region. The top region 42 is an example of a second region. The middle region 43 is an example of a third region. The first conductive region 44 is an example of a fourth region.
[0215] The switching layer 40 includes a lower region 41, an upper region 42, a middle region 43, and a first conductive region 44. The upper region 42 is provided between the lower region 41 and the middle electrode 30. The middle region 43 is provided between the lower region 41 and the upper region 42. The first conductive region 44 is provided between the lower region 41 and the middle region 43.
[0216] The lower region 41 contacts, for example, the lower electrode 10. The first conductive region 44 contacts, for example, the lower region 41 and the middle region 43. The upper region 42 contacts, for example, the middle electrode 30. The upper region 42 contacts, for example, the middle region 43.
[0217] A first conductive region 44 is provided in the memory cell MC of the third modification of the third embodiment. The first conductive region 44 has a function of releasing oxygen. The oxygen released from the first conductive region 44 is supplied to the lower region 41, and oxygen vacancies in the lower region 41 are filled. Therefore, Fermi level pinning of the lower electrode 10 is suppressed, and a change in the first barrier height φb1 is suppressed. Therefore, a decrease in the on-current of the switching element can be suppressed.
[0218] The first conductive region 44 may be provided between the upper region 42 and the intermediate region 43. The first conductive region 44 may be provided both between the lower region 41 and the intermediate region 43 and between the upper region 42 and the intermediate region 43.
[0219] As described above, according to the third embodiment and its modification, a switching element having excellent characteristics, such as a low semi-selection leakage current and a high on-current, can be realized. Furthermore, a memory device having a switching element having excellent characteristics can be realized.
[0220] (Fourth embodiment) The storage device of the fourth embodiment is different from the storage device of the first embodiment in that it further comprises at least one of a first layer provided between the first conductive layer and the first region, the first layer including at least one first metal element selected from the group consisting of silver (Ag), iridium (Ir), osmium (Os), ruthenium (Ru), and rhodium (Rh), and oxygen (O), and a second layer provided between the third conductive layer and the second region, the second layer including at least one second metal element selected from the group consisting of silver (Ag), iridium (Ir), osmium (Os), ruthenium (Ru), and rhodium (Rh), and oxygen (O). Hereinafter, some of the contents overlapping with the first embodiment may be omitted.
[0221] Fig. 15 is a schematic cross-sectional view of a memory cell in a memory device according to the fourth embodiment. Fig. 15 is a view corresponding to Fig. 2 of the first embodiment. Fig. 15 shows a cross section of one memory cell MC.
[0222] 15 , the memory cell MC includes a lower electrode 10, an upper electrode 20, an intermediate electrode 30, a switching layer 40, a resistance change layer 50, a first metal oxide layer 81, and a second metal oxide layer 82. The switching layer 40 includes a lower region 41, an upper region 42, and an intermediate region 43. The resistance change layer 50 includes a fixed layer 51, a tunnel layer 52, and a free layer 53.
[0223] The bottom electrode 10 is an example of a first conductive layer. The top electrode 20 is an example of a second conductive layer. The middle electrode 30 is an example of a third conductive layer. The bottom region 41 is an example of a first region. The top region 42 is an example of a second region. The middle region 43 is an example of a third region. The first metal oxide layer 81 is an example of a first layer. The second metal oxide layer 82 is an example of a second layer.
[0224] The lower electrode 10, the first metal oxide layer 81, the switching layer 40, the second metal oxide layer 82, and the intermediate electrode 30 constitute a switching element of the memory cell MC. The intermediate electrode 30, the resistance change layer 50, and the upper electrode 20 constitute a resistance change element of the memory cell MC.
[0225] The lower electrode 10 contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni).
[0226] The upper electrode 20 is, for example, a metal, and includes, for example, at least one material selected from the group consisting of carbon, carbon nitride, tungsten, tungsten carbide, and tungsten nitride.
[0227] The intermediate electrode 30 contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni).
[0228] The switching layer 40 includes a lower region 41, an upper region 42, and an intermediate region 43. The upper region 42 is provided between the lower region 41 and the intermediate electrode 30. The intermediate region 43 is provided between the lower region 41 and the upper region 42.
[0229] The lower region 41 may, for example, be adjacent to the middle region 43. The upper region 42 may, for example, be adjacent to the middle region 43.
[0230] The lower region 41 of the switching layer 40 includes at least one first element selected from the group consisting of zinc (Zn) and tin (Sn) and oxygen (O). The lower region 41 includes, for example, a first oxide which is an oxide of the first element.
[0231] The upper region 42 of the switching layer 40 includes at least one second element selected from the group consisting of zinc (Zn) and tin (Sn) and oxygen (O). The upper region 42 includes a second oxide that is, for example, an oxide of the second element.
[0232] The intermediate region 43 of the switching layer 40 contains at least one third element selected from the group consisting of tantalum (Ta), niobium (Nb), and vanadium (V), and oxygen (O). The intermediate region 43 contains a third oxide that is, for example, an oxide of the third element.
[0233] The first metal oxide layer 81 is provided between the lower electrode 10 and the lower region 41. The first metal oxide layer 81 is in contact with the lower electrode 10, for example. The first metal oxide layer 81 is in contact with the lower region 41, for example.
[0234] The first metal oxide layer 81 contains at least one first metal element selected from the group consisting of silver (Ag), iridium (Ir), osmium (Os), ruthenium (Ru), and rhodium (Rh), and oxygen (O). The first metal oxide layer 81 contains, for example, a first metal oxide of the first metal element.
[0235] The first metal oxide is, for example, silver oxide, iridium oxide, osmium oxide, ruthenium oxide, or rhodium oxide.
[0236] The standard Gibbs energy of formation of the first metal oxide is, for example, greater than the standard Gibbs energy of formation of the first oxide contained in the lower region 41 .
[0237] The first metal oxide layer 81 is electrically conductive.
[0238] The second metal oxide layer 82 is provided between the intermediate electrode 30 and the upper region 42. The second metal oxide layer 82 is in contact with, for example, the intermediate electrode 30. The second metal oxide layer 82 is in contact with, for example, the upper region 42.
[0239] The second metal oxide layer 82 contains at least one second metal element selected from the group consisting of silver (Ag), iridium (Ir), osmium (Os), ruthenium (Ru), and rhodium (Rh), and oxygen (O). The second metal oxide layer 82 contains, for example, a second metal oxide of the second metal element.
[0240] The second metal oxide is, for example, silver oxide, iridium oxide, osmium oxide, ruthenium oxide, or rhodium oxide.
[0241] The standard Gibbs energy of formation of the second metal oxide is, for example, greater than the standard Gibbs energy of formation of the second oxide contained in upper region 42 .
[0242] The second metal oxide layer 82 is electrically conductive.
[0243] The thickness of the first metal oxide layer 81 in the first direction is, for example, not less than 2 nm and not more than 20 nm. The thickness of the second metal oxide layer 82 in the first direction is, for example, not less than 2 nm and not more than 20 nm.
[0244] Next, the operation and effects of the storage device of the fourth embodiment will be described.
[0245] Consider a case where the first metal oxide layer 81 and the second metal oxide layer 82 are not provided in the memory cell MC of the fourth embodiment. In this case, for example, the on-current of the switching element may be reduced.
[0246] The reason why the on-current of the switching element becomes low is considered to be, for example, that oxygen is extracted from the lower region 41 to the lower electrode 10, and oxygen vacancies are generated in the lower region 41. It is considered that, due to the oxygen vacancies being generated in the lower region 41, the Fermi level of the lower electrode 10 is pinned to the lower region 41, and the first barrier height φb1 (see FIG. 6) between the lower electrode 10 and the lower region 41 becomes large.
[0247] Also, the reason why the on-current of the switching element becomes low is believed to be, for example, that oxygen is extracted from the upper region 42 to the intermediate electrode 30, and oxygen vacancies are generated in the upper region 42. It is believed that the generation of oxygen vacancies in the upper region 42 causes the Fermi level of the intermediate electrode 30 to be pinned to the upper region 42, and the second barrier height φb2 (see FIG. 6) between the intermediate electrode 30 and the upper region 42 becomes large.
[0248] The memory cell MC of the fourth embodiment is provided with a first metal oxide layer 81. The standard Gibbs energy of formation of the first metal oxide contained in the first metal oxide layer 81 is greater than the standard Gibbs energy of formation of the first oxide contained in the lower region 41. In other words, oxygen in the first metal oxide contained in the first metal oxide layer 81 is more easily removed than oxygen in the first oxide contained in the lower region 41. For this reason, oxygen is removed from the first metal oxide layer 81 and supplied to the lower region 41, filling the oxygen vacancies in the lower region 41. Therefore, the Fermi level pinning of the lower electrode 10 is suppressed, and the change in the first barrier height φb1 is suppressed. Therefore, it is possible to suppress the on-current of the switching element from decreasing.
[0249] Moreover, the memory cell MC of the fourth embodiment is provided with a second metal oxide layer 82. The standard Gibbs energy of formation of the second metal oxide contained in the second metal oxide layer 82 is greater than the standard Gibbs energy of formation of the second oxide contained in the upper region 42. In other words, oxygen in the second metal oxide contained in the second metal oxide layer 82 is more easily removed than oxygen in the second oxide contained in the upper region 42. For this reason, oxygen is removed from the second metal oxide layer 82 and supplied to the upper region 42, filling the oxygen vacancies in the upper region 42. Therefore, the Fermi level pinning of the intermediate electrode 30 is suppressed, and the change in the second barrier height φb2 is suppressed. Therefore, it is possible to suppress the on-current of the switching element from decreasing.
[0250] For example, when the lower electrode 10 is made of carbon (C), the thermal conductivity of the first metal oxide layer 81 is smaller than the thermal conductivity of the lower electrode 10. Therefore, the first metal oxide layer 81 has a function of trapping heat in the switching layer 40. By trapping heat in the switching layer 40, the operation of the switching element becomes stable.
[0251] Similarly, for example, when the intermediate electrode 30 is made of carbon (C), the thermal conductivity of the second metal oxide layer 82 is smaller than the thermal conductivity of the intermediate electrode 30. Therefore, the second metal oxide layer 82 has the function of trapping heat in the switching layer 40. By trapping heat in the switching layer 40, the operation of the switching element becomes stable.
[0252] As described above, according to the fourth embodiment, a switching element having excellent characteristics, such as a low semi-selection leakage current and a high on-current, can be realized, and further, a memory device having a switching element having excellent characteristics can be realized.
[0253] Fifth embodiment A memory device according to a fifth embodiment includes a memory cell including a first conductive layer, a second conductive layer, a third conductive layer provided between the first conductive layer and the second conductive layer, a switching layer provided between the first conductive layer and the third conductive layer, and a resistance change layer provided between the third conductive layer and the second conductive layer. The switching layer includes a first region, a second region between the first region and the third conductive layer, and a third region between the first region and the second region. The first region includes at least one first metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, strontium-doped lanthanum manganate, and iron oxide; the second region includes at least one second metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, strontium-doped lanthanum manganate, and iron oxide; and the third region includes at least one material selected from the group consisting of zirconium oxide, silicon nitride, strontium titanate, titanium oxide, tantalum oxide, hafnium oxide, copper aluminate, lanthanum oxide, yttrium oxide, aluminum oxide, hafnium silicate, barium titanate, silicon carbide, germanium oxide, copper oxide, magnesium oxide, and aluminum nitride.
[0254] The memory device of the fifth embodiment further includes a plurality of first wirings and a plurality of second wirings intersecting the plurality of first wirings, and the memory cell is provided in a region where one of the plurality of first wirings intersects one of the plurality of second wirings.
[0255] The storage device of the fifth embodiment differs from the storage device of the first embodiment in that the configuration of the switching elements is different. In the following, some of the contents that overlap with the first embodiment may be omitted.
[0256] The storage device of the fifth embodiment has a configuration similar to that shown in the block diagram of FIG. 1 of the first embodiment.
[0257] Fig. 16 is a schematic cross-sectional view of a memory cell in a memory device of the fifth embodiment. Fig. 16 shows a cross-section of one memory cell MC indicated by, for example, a dotted circle in the memory cell array 100 of Fig. 1.
[0258] 16, the memory cell MC includes a lower electrode 10, an upper electrode 20, an intermediate electrode 30, a switching layer 40, and a resistance change layer 50. The switching layer 40 includes a lower region 41, an upper region 42, and an intermediate region 43. The resistance change layer 50 includes a fixed layer 51, a tunnel layer 52, and a free layer 53.
[0259] The bottom electrode 10 is an example of a first conductive layer. The top electrode 20 is an example of a second conductive layer. The middle electrode 30 is an example of a third conductive layer. The bottom region 41 is an example of a first region. The top region 42 is an example of a second region. The middle region 43 is an example of a third region.
[0260] The lower electrode 10, the switching layer 40, and the intermediate electrode 30 constitute a switching element of the memory cell MC. The intermediate electrode 30, the resistance change layer 50, and the upper electrode 20 constitute a resistance change element of the memory cell MC.
[0261] The lower electrode 10 includes at least one element selected from the group consisting of, for example, carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The lower electrode 10 includes at least one material selected from the group consisting of, for example, carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The lower electrode 10 is, for example, carbon (C), cobalt (Co), gold (Au), or nickel (Ni).
[0262] The lower electrode 10 includes at least one metal element selected from the group consisting of, for example, titanium (Ti), platinum (Pt), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), and palladium (Pd). The lower electrode 10 includes at least one material selected from the group consisting of, for example, titanium (Ti), platinum (Pt), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), and palladium (Pd). The lower electrode 10 is, for example, titanium (Ti), platinum (Pt), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), or palladium (Pd).
[0263] The lower electrode 10 includes at least one metal element selected from the group consisting of titanium (Ti), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), and palladium (Pd), and nitrogen (N). The lower electrode 10 includes at least one material selected from the group consisting of titanium nitride, tungsten nitride, chromium nitride, molybdenum nitride, iron nitride, copper nitride, and palladium nitride. The lower electrode 10 is, for example, titanium nitride, tungsten nitride, chromium nitride, molybdenum nitride, iron nitride, copper nitride, or palladium nitride.
[0264] The lower electrode 10 includes, for example, indium (In), tin (Sn), and oxygen (O). The lower electrode 10 includes, for example, indium tin oxide. The lower electrode 10 is, for example, indium tin oxide.
[0265] The upper electrode 20 is, for example, a metal, and includes, for example, at least one material selected from the group consisting of carbon, carbon nitride, tungsten, tungsten carbide, and tungsten nitride.
[0266] The intermediate electrode 30 is provided between the lower electrode 10 and the upper electrode 20 .
[0267] The intermediate electrode 30 includes at least one element selected from the group consisting of, for example, carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The intermediate electrode 30 includes at least one material selected from the group consisting of, for example, carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The intermediate electrode 30 is, for example, carbon (C), cobalt (Co), gold (Au), or nickel (Ni).
[0268] The intermediate electrode 30 includes at least one metal element selected from the group consisting of, for example, titanium (Ti), platinum (Pt), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), and palladium (Pd). The intermediate electrode 30 includes at least one material selected from the group consisting of, for example, titanium (Ti), platinum (Pt), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), and palladium (Pd). The intermediate electrode 30 is, for example, titanium (Ti), platinum (Pt), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), or palladium (Pd).
[0269] The intermediate electrode 30 includes at least one metal element selected from the group consisting of titanium (Ti), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), and palladium (Pd), and nitrogen (N). The intermediate electrode 30 includes at least one material selected from the group consisting of titanium nitride, tungsten nitride, chromium nitride, molybdenum nitride, iron nitride, copper nitride, and palladium nitride. The intermediate electrode 30 is, for example, titanium nitride, tungsten nitride, chromium nitride, molybdenum nitride, iron nitride, copper nitride, or palladium nitride.
[0270] The intermediate electrode 30 includes, for example, indium (In), tin (Sn), and oxygen (O). The intermediate electrode 30 includes, for example, indium tin oxide. The intermediate electrode 30 is, for example, indium tin oxide.
[0271] The switching layer 40 is provided between the lower electrode 10 and the intermediate electrode 30. The thickness of the switching layer 40 in a first direction from the lower electrode 10 toward the upper electrode 20 is, for example, not less than 5 nm and not more than 50 nm.
[0272] The switching layer 40 has a function of suppressing an increase in a half-selected leakage current flowing through a half-selected cell. The switching layer 40 has a nonlinear current-voltage characteristic in which the current rises sharply at a specific threshold voltage.
[0273] The switching layer 40 includes a lower region 41, an upper region 42, and an intermediate region 43. The upper region 42 is provided between the lower region 41 and the intermediate electrode 30. The intermediate region 43 is provided between the lower region 41 and the upper region 42.
[0274] The lower region 41 contacts, for example, the lower electrode 10. The lower region 41 contacts, for example, the middle region 43. The upper region 42 contacts, for example, the middle electrode 30. The upper region 42 contacts, for example, the middle region 43.
[0275] The lower region 41 of the switching layer 40 includes at least one first metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, lanthanum titanate, strontium-doped lanthanum manganate, and iron oxide. The lower region 41 is, for example, the first metal oxide.
[0276] The niobium oxide contained in the lower region 41 has a chemical composition expressed, for example, as NbO2. The vanadium oxide contained in the lower region 41 has a chemical composition expressed, for example, as VO2. The chromium-doped vanadium oxide contained in the lower region 41 has a chemical composition expressed, for example, as VO2. x Cr 1-x The nickel oxide contained in the lower region 41 has a chemical composition represented by, for example, NiO. The lanthanum titanate contained in the lower region 41 has a chemical composition represented by, for example, LaTiO. The strontium-doped lanthanum manganate contained in the lower region 41 has a chemical composition represented by, for example, La 1-x Sr x It has a chemical composition represented by MnO3. The iron oxide contained in the lower region 41 has a chemical composition represented by Fe3O4, for example.
[0277] The first metal oxide contained in the lower region 41 is a Mott insulator. A Mott insulator is a material in which a Mott transition occurs. The Mott transition is a metal-insulator transition. The Mott insulator undergoes a phase transition from an insulating phase to a metallic phase, for example, by application of a voltage. Note that the Mott transition is reversible, and for example, the phase transition from the metallic phase to the insulating phase occurs by stopping the application of a voltage.
[0278] The thickness of the lower region 41 in the first direction is, for example, not less than 1 nm and not more than 10 nm.
[0279] The upper region 42 of the switching layer 40 includes at least one second metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, lanthanum titanate, strontium-doped lanthanum manganate, and iron oxide. The upper region 42 is, for example, the second metal oxide.
[0280] The niobium oxide contained in the upper region 42 has a chemical composition expressed, for example, as NbO2. The vanadium oxide contained in the upper region 42 has a chemical composition expressed, for example, as VO2. The chromium-doped vanadium oxide contained in the upper region 42 has a chemical composition expressed, for example, as VO2. x Cr 1-x The nickel oxide contained in the upper region 42 has a chemical composition represented by, for example, NiO. The lanthanum titanate contained in the upper region 42 has a chemical composition represented by, for example, LaTiO. The strontium-doped lanthanum manganate contained in the upper region 42 has a chemical composition represented by, for example, La 1-x Sr x The iron oxide contained in the upper region 42 has a chemical composition represented by, for example, Fe3O4.
[0281] The first metal oxide contained in the upper region 42 is a Mott insulator.
[0282] The first metal oxide and the second metal oxide are, for example, the same metal oxide.
[0283] The thickness of the upper region 42 in the first direction is, for example, not less than 1 nm and not more than 10 nm.
[0284] The intermediate region 43 of the switching layer 40 includes at least one material selected from the group consisting of zirconium oxide, silicon nitride, strontium titanate, titanium oxide, tantalum oxide, hafnium oxide, copper aluminate, lanthanum oxide, yttrium oxide, aluminum oxide, hafnium silicate, barium titanate, silicon carbide, germanium oxide, copper oxide, magnesium oxide, and aluminum nitride. The intermediate region 43 is, for example, zirconium oxide, silicon nitride, strontium titanate, titanium oxide, tantalum oxide, hafnium oxide, copper aluminate, lanthanum oxide, yttrium oxide, aluminum oxide, hafnium silicate, barium titanate, silicon carbide, germanium oxide, copper oxide, magnesium oxide, or aluminum nitride.
[0285] The zirconium oxide contained in the intermediate region 43 has a chemical composition represented, for example, by ZrO2. The silicon nitride contained in the intermediate region 43 has a chemical composition represented, for example, by Si3N4. The strontium titanate contained in the intermediate region 43 has a chemical composition represented, for example, by SrTiO3. The titanium oxide contained in the intermediate region 43 has a chemical composition represented, for example, by TiO2. The tantalum oxide contained in the intermediate region 43 has a chemical composition represented, for example, by Ta2O5. The hafnium oxide contained in the intermediate region 43 has a chemical composition represented, for example, by HfO2. The copper aluminate contained in the intermediate region 43 has a chemical composition represented, for example, by CuAlO2. The lanthanum oxide contained in the intermediate region 43 has a chemical composition represented, for example, by La2O3. The yttrium oxide contained in the intermediate region 43 has a chemical composition represented, for example, by Y2O3. The aluminum oxide contained in the intermediate region 43 has a chemical composition represented, for example, by Al2O3. The hafnium silicate contained in the intermediate region 43 has a chemical composition represented, for example, by HfSiO4. The barium titanate contained in the intermediate region 43 has a chemical composition represented, for example, by BaTiO3. The silicon carbide contained in the intermediate region 43 has a chemical composition represented, for example, by SiC. The germanium oxide contained in the intermediate region 43 has a chemical composition represented, for example, by GeO2. The copper oxide contained in the intermediate region 43 has a chemical composition represented, for example, by Cu2O. The magnesium oxide contained in the intermediate region 43 has a chemical composition represented, for example, by MgO. The aluminum nitride contained in the intermediate region 43 has a chemical composition represented, for example, by AlN.
[0286] The material contained in the intermediate region 43 is a non-Mott insulator. A non-Mott insulator is a material in which the Mott transition does not occur.
[0287] The thickness of the intermediate region 43 in the first direction is, for example, not less than 1 nm and not more than 10 nm.
[0288] FIG. 17 is a diagram showing a band structure of the switching element of the fifth embodiment.
[0289] The electron affinity of the substance contained in the intermediate region 43 (Ea3 in FIG. 17) is smaller than, for example, the electron affinity of the first metal oxide contained in the lower region 41 (Ea1 in FIG. 17). In addition, the electron affinity of the substance contained in the intermediate region 43 (Ea3 in FIG. 17) is smaller than, for example, the electron affinity of the second metal oxide contained in the upper region 42 (Ea2 in FIG. 17).
[0290] The electron affinity (Ea3 in FIG. 17) of the substance contained in the intermediate region 43 is, for example, 3.0 eV or less.
[0291] The dielectric constant of the material contained in the intermediate region 43 (ε3 in FIG. 17) is greater than, for example, the dielectric constant of the first metal oxide contained in the lower region 41 (ε1 in FIG. 17). Also, the dielectric constant of the material contained in the intermediate region 43 is greater than, for example, the dielectric constant of the second metal oxide contained in the upper region 42 (ε2 in FIG. 17).
[0292] The electron affinity (Ea3 in FIG. 17) of the material contained in the intermediate region 43 is smaller than, for example, the work function (φm1 in FIG. 17) of the material contained in the lower electrode 10. The electron affinity (Ea3 in FIG. 17) of the material contained in the intermediate region 43 is smaller than, for example, the work function (φm2 in FIG. 17) of the material contained in the intermediate electrode 30.
[0293] In addition, the charge neutral level (Ex in FIG. 17) of the material contained in the intermediate region 43 is smaller than, for example, the work function (φm1 in FIG. 17) of the material contained in the lower electrode 10. The charge neutral level (Ex in FIG. 17) of the material contained in the intermediate region 43 is smaller than, for example, the work function (φm2 in FIG. 17) of the material contained in the intermediate electrode 30. The charge neutral level Ex is the energy difference between the energy level at which Fermi level pinning occurs and the vacuum level.
[0294] The pinning factor of the material contained in the intermediate region 43 is, for example, 0.5 or less. The pinning factor is a physical property value that indicates the likelihood of Fermi level pinning occurring in a material. The smaller the pinning factor, the more likely Fermi level pinning occurs.
[0295] In addition, if the substance can be identified, the dielectric constant, electron affinity, work function, charge neutrality level, and pinning coefficient of the substance can be identified as the physical property values of the substance.
[0296] The resistance change layer 50 is provided between the intermediate electrode 30 and the upper electrode 20. The resistance change layer 50 has a fixed layer 51, a tunnel layer 52, and a free layer 53. The resistance change layer 50 includes a magnetic tunnel junction constituted by the fixed layer 51, the tunnel layer 52, and the free layer 53.
[0297] The variable resistance layer 50 has a function of storing data by changing resistance. The variable resistance layer 50 has a characteristic that, for example, the electrical resistance changes when a predetermined voltage is applied.
[0298] Next, the operation and effects of the storage device of the fifth embodiment will be described.
[0299] Fig. 18 is a schematic cross-sectional view of a memory cell of a memory device of a comparative example of the fifth embodiment, and corresponds to Fig. 16 of the fifth embodiment.
[0300] The memory cell MC of the memory device of the comparative example differs from the memory cell MC of the memory device of the fifth embodiment in that the switching layer 40 is formed only of the Mott insulator region 91.
[0301] The Mott insulator region 91 of the switching layer 40 includes at least one metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, lanthanum titanate, strontium-doped lanthanum manganate, and iron oxide. The Mott insulator region 91 is, for example, the above-mentioned metal oxide.
[0302] The metal oxide contained in the Mott insulator region 91 is a Mott insulator.
[0303] Fig. 19 is an explanatory diagram of the operation and effect of the memory device of the fifth embodiment. Fig. 19 is a schematic cross-sectional view of a memory cell of a memory device of a comparative example. Fig. 19 shows a case where the switching element of the comparative example is in an on state.
[0304] When a voltage is applied to the switching element and reaches a predetermined voltage, at least a part of the Mott insulator region 91 undergoes a phase transition from the insulating phase 91x to the metallic phase 91y. For example, the metallic phase 91y is connected between the lower electrode 10 and the intermediate electrode 30, and a high on-current flows. The switching element has a nonlinear current-voltage characteristic in which the current rises sharply at the threshold voltage Vth.
[0305] The formation of the metallic phase 91y in the Mott insulator region 91 increases the on-current of the switching element. However, there is a risk that the semi-selective leakage current will not be sufficiently low. For example, the recovery of the insulating phase 91x from the metallic phase 91y after the application of the voltage is stopped may not be complete, and defects may remain in the Mott insulator region 91, which may result in the semi-selective leakage current not being sufficiently low.
[0306] The switching element of the memory device of the fifth embodiment includes an intermediate region 43 containing a non-Mott insulator between a lower region 41 of a Mott insulator and an upper region 42 of a Mott insulator.
[0307] 20, 21(a) and 21(b) are explanatory diagrams of the operation and effects of the storage device of the fifth embodiment.
[0308] Fig. 20 is a schematic cross-sectional view of a memory cell of the storage device of the fifth embodiment. Fig. 20 shows the case where the switching element of the fifth embodiment is in the on state.
[0309] 21(a) and 21(b) are diagrams showing band structures of the switching element of the fifth embodiment, in which (a) shows the band structure when the switching element is in the off state, and (b) shows the band structure when the switching element is in the on state.
[0310] 20, when the switching element is in the on state, a metallic phase 91y is formed in the lower region 41 of the Mott insulator and in the upper region 42 of the Mott insulator. On the other hand, no metallic phase 91y is formed in the intermediate region 43 including a non-Mott insulator.
[0311] As shown in FIG. 21(a), when the switching element is in the off state, the current is suppressed by a first barrier height φb1 between the bottom electrode 10 and the lower region 41 of the Mott insulator, a second barrier height φb2 between the intermediate electrode 30 and the upper region 42, and a third barrier height φb3 between the bottom electrode 10 and the intermediate electrode 30 and the intermediate region 43.
[0312] Even if defects that cause semi-selected leakage current remain in the lower region 41 of the Mott insulator and the upper region 42 of the Mott insulator, an increase in the semi-selected leakage current can be suppressed by the barrier formed in the intermediate region 43 containing a non-Mott insulator.
[0313] 21(b), when the switching element is in the on state, a high on-current flows by tunneling through the intermediate region 43. In the on state, the lower region 41 and the upper region 42 are metallized by the Mott transition. Therefore, the Fermi level of the lower electrode 10 and the Fermi level of the lower region 41 match, and the Fermi level of the intermediate electrode 30 and the Fermi level of the upper region 42 match.
[0314] From the viewpoint of reducing the semi-selection leakage current, it is preferable that the third barrier height φb3 is high. Therefore, it is preferable that the electron affinity (Ea3 in FIG. 17) of the material contained in the intermediate region 43 is small. It is preferable that the electron affinity Ea of the material contained in the intermediate region 43 is 3.0 eV or less.
[0315] In order to effectively apply an electric field to the lower region 41 of the Mott insulator and the upper region 42 of the Mott insulator and promote the Mott transition, it is preferable that the material contained in the intermediate region 43 has a large dielectric constant.
[0316] Fig. 22 is an explanatory diagram of the action and effect of the storage device of the fifth embodiment. Fig. 22 is a diagram showing the band structure of the switching element of the fifth embodiment. Fig. 22 shows the band structure when the switching element is in the on state.
[0317] When the switching element is in the on state, if Fermi pinning occurs, for example, the work function of the lower electrode 10 and the lower region 41 changes from the first work function (φm1 in FIG. 22) to a first effective work function (φm1_eff in FIG. 22). The first effective work function φm1_eff coincides with the charge neutrality level Ex of the material contained in the intermediate region 43.
[0318] When the first effective work function φm1_eff after the occurrence of Fermi pinning becomes small, the tunnel current becomes easy to flow, and the on-current of the switching element becomes high. Therefore, it is preferable that the charge neutral level Ex of the material contained in the intermediate region 43 is small, and the pinning coefficient is also small.
[0319] From the viewpoint of a substance having a small electron affinity, a large dielectric constant, a small neutral charge level, and a small pinning coefficient, the substance contained in the intermediate region 43 is preferably zirconium oxide, silicon nitride, strontium titanate, titanium oxide, tantalum oxide, hafnium oxide, copper aluminate, lanthanum oxide, yttrium oxide, aluminum oxide, or hafnium silicate, more preferably zirconium oxide, silicon nitride, strontium titanate, titanium oxide, tantalum oxide, hafnium oxide, or copper aluminate, and even more preferably zirconium oxide or silicon nitride.
[0320] From the viewpoint of increasing the third barrier height (φb3 in FIG. 17) and suppressing the semi-selective leakage current, it is preferable that the electron affinity (Ea3 in FIG. 17) of the material contained in the intermediate region 43 is smaller than the electron affinity (Ea1 in FIG. 17) of the first metal oxide contained in the lower region 41. In addition, it is preferable that the electron affinity (Ea3 in FIG. 17) of the material contained in the intermediate region 43 is smaller than the electron affinity (Ea2 in FIG. 17) of the second metal oxide contained in the upper region 42.
[0321] In order to increase the first barrier height (φb1 in FIG. 17), the second barrier height (φb2 in FIG. 17), and the third barrier height (φb3 in FIG. 17) and suppress the semi-selected leakage current, it is preferable that the first work function (φm1 in FIG. 17) of the lower electrode 10 and the second work function (φm2 in FIG. 17) of the intermediate electrode 30 are large.
[0322] From the above viewpoint, the lower electrode 10 preferably contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The lower electrode 10 preferably contains at least one substance selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The lower electrode 10 is preferably carbon (C), cobalt (Co), gold (Au), or nickel (Ni).
[0323] From the above viewpoint, the intermediate electrode 30 preferably contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The intermediate electrode 30 preferably contains at least one substance selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The intermediate electrode 30 is preferably carbon (C), cobalt (Co), gold (Au), or nickel (Ni).
[0324] As described above, according to the fifth embodiment, a switching element having excellent characteristics, such as a low semi-selection leakage current and a high on-current, can be realized, and further, a memory device having a switching element having excellent characteristics can be realized.
[0325] Sixth embodiment A memory device according to a sixth embodiment includes a memory cell including a first conductive layer, a second conductive layer, a third conductive layer provided between the first conductive layer and the second conductive layer, a switching layer provided between the first conductive layer and the third conductive layer, and a resistance change layer provided between the third conductive layer and the second conductive layer. The switching layer includes a first region, a second region between the first region and the third conductive layer, and a third region between the first region and the second region. The first region includes at least one first metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, lanthanum titanate, strontium-doped lanthanum manganate, and iron oxide, the second region includes at least one second metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, strontium-doped lanthanum manganate, and iron oxide, and the third region includes at least one third metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, strontium-doped lanthanum manganate, and iron oxide. The electron affinity of the third metal oxide is smaller than that of the first metal oxide, and the electron affinity of the third metal oxide is smaller than that of the second metal oxide.
[0326] The memory device of the sixth embodiment further includes a plurality of first wirings and a plurality of second wirings intersecting the plurality of first wirings, and the memory cell is provided in a region where one of the plurality of first wirings intersects one of the plurality of second wirings.
[0327] The storage device of the sixth embodiment differs from the storage device of the first embodiment in that the configuration of the switching element is different. The storage device of the sixth embodiment also differs from the storage device of the fifth embodiment in that a Mott insulator is included in the intermediate region 43. Hereinafter, some of the contents that overlap with the first or fifth embodiment may be omitted.
[0328] The storage device of the sixth embodiment has a configuration similar to that shown in the block diagram of FIG. 1 of the first embodiment.
[0329] Fig. 23 is a schematic cross-sectional view of a memory cell in a memory device of embodiment 6. Fig. 23 shows a cross-section of one memory cell MC indicated by, for example, a dotted circle in the memory cell array 100 of Fig. 1.
[0330] 23, the memory cell MC includes a lower electrode 10, an upper electrode 20, an intermediate electrode 30, a switching layer 40, and a resistance change layer 50. The switching layer 40 includes a lower region 41, an upper region 42, and an intermediate region 43. The resistance change layer 50 includes a fixed layer 51, a tunnel layer 52, and a free layer 53.
[0331] The bottom electrode 10 is an example of a first conductive layer. The top electrode 20 is an example of a second conductive layer. The middle electrode 30 is an example of a third conductive layer. The bottom region 41 is an example of a first region. The top region 42 is an example of a second region. The middle region 43 is an example of a third region.
[0332] The lower electrode 10, the switching layer 40, and the intermediate electrode 30 constitute a switching element of the memory cell MC. The intermediate electrode 30, the resistance change layer 50, and the upper electrode 20 constitute a resistance change element of the memory cell MC.
[0333] The lower electrode 10 includes at least one element selected from the group consisting of, for example, carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The lower electrode 10 includes at least one material selected from the group consisting of, for example, carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The lower electrode 10 is, for example, carbon (C), cobalt (Co), gold (Au), or nickel (Ni).
[0334] The lower electrode 10 includes at least one metal element selected from the group consisting of, for example, titanium (Ti), platinum (Pt), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), and palladium (Pd). The lower electrode 10 includes at least one material selected from the group consisting of, for example, titanium (Ti), platinum (Pt), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), and palladium (Pd). The lower electrode 10 is, for example, titanium (Ti), platinum (Pt), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), or palladium (Pd).
[0335] The lower electrode 10 includes at least one metal element selected from the group consisting of titanium (Ti), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), and palladium (Pd), and nitrogen (N). The lower electrode 10 includes at least one material selected from the group consisting of titanium nitride, tungsten nitride, chromium nitride, molybdenum nitride, iron nitride, copper nitride, and palladium nitride. The lower electrode 10 is, for example, titanium nitride, tungsten nitride, chromium nitride, molybdenum nitride, iron nitride, copper nitride, or palladium nitride.
[0336] The lower electrode 10 includes, for example, indium (In), tin (Sn), and oxygen (O). The lower electrode 10 includes, for example, indium tin oxide. The lower electrode 10 is, for example, indium tin oxide.
[0337] The upper electrode 20 is, for example, a metal, and includes, for example, at least one material selected from the group consisting of carbon, carbon nitride, tungsten, tungsten carbide, and tungsten nitride.
[0338] The intermediate electrode 30 is provided between the lower electrode 10 and the upper electrode 20 .
[0339] The intermediate electrode 30 includes at least one element selected from the group consisting of, for example, carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The intermediate electrode 30 includes at least one material selected from the group consisting of, for example, carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The intermediate electrode 30 is, for example, carbon (C), cobalt (Co), gold (Au), or nickel (Ni).
[0340] The intermediate electrode 30 includes at least one metal element selected from the group consisting of, for example, titanium (Ti), platinum (Pt), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), and palladium (Pd). The intermediate electrode 30 includes at least one material selected from the group consisting of, for example, titanium (Ti), platinum (Pt), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), and palladium (Pd). The intermediate electrode 30 is, for example, titanium (Ti), platinum (Pt), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), or palladium (Pd).
[0341] The intermediate electrode 30 includes at least one metal element selected from the group consisting of titanium (Ti), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), copper (Cu), and palladium (Pd), and nitrogen (N). The intermediate electrode 30 includes at least one material selected from the group consisting of titanium nitride, tungsten nitride, chromium nitride, molybdenum nitride, iron nitride, copper nitride, and palladium nitride. The intermediate electrode 30 is, for example, titanium nitride, tungsten nitride, chromium nitride, molybdenum nitride, iron nitride, copper nitride, or palladium nitride.
[0342] The intermediate electrode 30 includes, for example, indium (In), tin (Sn), and oxygen (O). The lower electrode 10 includes, for example, indium tin oxide. The intermediate electrode 30 is, for example, indium tin oxide.
[0343] The switching layer 40 is provided between the lower electrode 10 and the intermediate electrode 30. The thickness of the switching layer 40 in a first direction from the lower electrode 10 toward the upper electrode 20 is, for example, not less than 5 nm and not more than 50 nm.
[0344] The switching layer 40 has a function of suppressing an increase in a half-selected leakage current flowing through a half-selected cell. The switching layer 40 has a nonlinear current-voltage characteristic in which the current rises sharply at a specific threshold voltage.
[0345] The switching layer 40 includes a lower region 41, an upper region 42, and an intermediate region 43. The upper region 42 is provided between the lower region 41 and the intermediate electrode 30. The intermediate region 43 is provided between the lower region 41 and the upper region 42.
[0346] The lower region 41 contacts, for example, the lower electrode 10. The lower region 41 contacts, for example, the middle region 43. The upper region 42 contacts, for example, the middle electrode 30. The upper region 42 contacts, for example, the middle region 43.
[0347] The lower region 41 of the switching layer 40 includes at least one first metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, lanthanum titanate, strontium-doped lanthanum manganate, and iron oxide. The lower region 41 is, for example, the first metal oxide.
[0348] The niobium oxide contained in the lower region 41 has a chemical composition expressed, for example, as NbO2. The vanadium oxide contained in the lower region 41 has a chemical composition expressed, for example, as VO2. The chromium-doped vanadium oxide contained in the lower region 41 has a chemical composition expressed, for example, as VO2. x Cr 1-x The nickel oxide contained in the lower region 41 has a chemical composition represented by, for example, NiO. The lanthanum titanate contained in the lower region 41 has a chemical composition represented by, for example, LaTiO. The strontium-doped lanthanum manganate contained in the lower region 41 has a chemical composition represented by, for example, La 1-xSr x It has a chemical composition represented by MnO3. The iron oxide contained in the lower region 41 has a chemical composition represented by Fe3O4, for example.
[0349] The first metal oxide contained in the lower region 41 is a Mott insulator.
[0350] The thickness of the lower region 41 in the first direction is, for example, not less than 1 nm and not more than 10 nm.
[0351] The upper region 42 of the switching layer 40 includes at least one second metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, lanthanum titanate, strontium-doped lanthanum manganate, and iron oxide. The upper region 42 is, for example, the second metal oxide.
[0352] The niobium oxide contained in the upper region 42 has a chemical composition expressed, for example, as NbO2. The vanadium oxide contained in the upper region 42 has a chemical composition expressed, for example, as VO2. The chromium-doped vanadium oxide contained in the upper region 42 has a chemical composition expressed, for example, as VO2. x Cr 1-x The nickel oxide contained in the upper region 42 has a chemical composition represented by, for example, NiO. The lanthanum titanate contained in the upper region 42 has a chemical composition represented by, for example, LaTiO. The strontium-doped lanthanum manganate contained in the upper region 42 has a chemical composition represented by, for example, La 1-x Sr x The iron oxide contained in the upper region 42 has a chemical composition represented by, for example, Fe3O4.
[0353] The first metal oxide contained in the upper region 42 is a Mott insulator.
[0354] The first metal oxide and the second metal oxide are, for example, the same metal oxide.
[0355] The thickness of the upper region 42 in the first direction is, for example, not less than 1 nm and not more than 10 nm.
[0356] The intermediate region 43 of the switching layer 40 includes at least one third metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, lanthanum titanate, strontium-doped lanthanum manganate, and iron oxide. The intermediate region 43 is, for example, a third metal oxide.
[0357] The niobium oxide contained in the intermediate region 43 has a chemical composition expressed, for example, as NbO2. The vanadium oxide contained in the intermediate region 43 has a chemical composition expressed, for example, as VO2. The chromium-doped vanadium oxide contained in the intermediate region 43 has a chemical composition expressed, for example, as VO2. x Cr 1-x The nickel oxide contained in the intermediate region 43 has a chemical composition represented by, for example, NiO. The lanthanum titanate contained in the intermediate region 43 has a chemical composition represented by, for example, LaTiO. The strontium-doped lanthanum manganate contained in the intermediate region 43 has a chemical composition represented by, for example, La 1-x Sr x The iron oxide contained in the intermediate region 43 has a chemical composition represented by, for example, Fe3O4.
[0358] The first metal oxide contained in the intermediate region 43 is a Mott insulator.
[0359] The third metal oxide, the first metal oxide and the second metal oxide are different metal oxides.
[0360] The thickness of the intermediate region 43 in the first direction is, for example, not less than 1 nm and not more than 10 nm.
[0361] FIG. 24 is a diagram showing a band structure of the switching element of the sixth embodiment.
[0362] The electron affinity (Ea3 in FIG. 24) of the third metal oxide contained in the intermediate region 43 is smaller than the electron affinity (Ea1 in FIG. 24) of the first metal oxide contained in the lower region 41. In addition, the electron affinity (Ea3 in FIG. 24) of the third metal oxide contained in the intermediate region 43 is smaller than the electron affinity (Ea2 in FIG. 24) of the second metal oxide contained in the upper region 42.
[0363] For example, when the third metal oxide is nickel oxide (NiO) and the first metal oxide and the second metal oxide are niobium oxide (NbO2), the electron affinity Ea of the third metal oxide is smaller than the electron affinity Ea1 of the first metal oxide and the electron affinity Ea2 of the second metal oxide.
[0364] The resistance change layer 50 is provided between the intermediate electrode 30 and the upper electrode 20. The resistance change layer 50 has a fixed layer 51, a tunnel layer 52, and a free layer 53. The resistance change layer 50 includes a magnetic tunnel junction constituted by the fixed layer 51, the tunnel layer 52, and the free layer 53.
[0365] The variable resistance layer 50 has a function of storing data by changing resistance. The variable resistance layer 50 has a characteristic that, for example, the electrical resistance changes when a predetermined voltage is applied.
[0366] Next, the operation and effects of the storage device of the sixth embodiment will be described.
[0367] Fig. 25 is an explanatory diagram of the operation and effect of the memory device of the sixth embodiment. Fig. 25 is a schematic cross-sectional view of a memory cell of the memory device of the sixth embodiment. Fig. 25 shows the case where the switching element of the sixth embodiment is in the on state.
[0368] As shown in Fig. 25, when a voltage is applied to the switching element and reaches a predetermined voltage, the lower region 41 of the Mott insulator, the upper region 42 of the Mott insulator, and the intermediate region 43 of the Mott insulator undergo a phase transition from an insulating phase 91x to a metallic phase 91y. When the switching element is in an on state, a metallic phase 91y is formed in the lower region 41 of the Mott insulator, the upper region 42 of the Mott insulator, and the intermediate region 43 of the Mott insulator. For example, the metallic phase 91y is connected between the lower electrode 10 and the intermediate electrode 30, and a high on-current flows through the switching element. The switching element has a nonlinear current-voltage characteristic in which the current rises sharply at a threshold voltage Vth.
[0369] The switching element of the memory device of the sixth embodiment includes an intermediate region 43 containing a third metal oxide having a small electron affinity. Therefore, the intermediate region 43 has a third barrier height (φb3 in FIG. 24) higher than the first barrier height (φb1 in FIG. 24) formed in the lower region 41 and the second barrier height (φb2 in FIG. 24) formed in the upper region 42.
[0370] If the intermediate region 43 that forms a high barrier is not provided, the barrier is low and the semi-selection leakage current of the switching element may increase. The switching element of the memory device of the sixth embodiment can reduce the semi-selection leakage current by including the intermediate region 43 that contains the third metal oxide with low electron affinity.
[0371] From the viewpoint of increasing the first barrier height (φb1 in FIG. 24), the second barrier height (φb2 in FIG. 24), and the third barrier height (φb3 in FIG. 24), it is preferable that the first work function (φm1 in FIG. 24) of the lower electrode 10 and the second work function (φm2 in FIG. 24) of the intermediate electrode 30 are large.
[0372] From the above viewpoint, the lower electrode 10 preferably contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The lower electrode 10 preferably contains at least one substance selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The lower electrode 10 is preferably carbon (C), cobalt (Co), gold (Au), or nickel (Ni).
[0373] From the above viewpoint, the intermediate electrode 30 preferably contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The intermediate electrode 30 preferably contains at least one substance selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni). The intermediate electrode 30 is preferably carbon (C), cobalt (Co), gold (Au), or nickel (Ni).
[0374] As described above, according to the sixth embodiment, a switching element having excellent characteristics, such as a low semi-selection leakage current and a high on-current, can be realized, and further, a memory device having a switching element having excellent characteristics can be realized.
[0375] Seventh embodiment The storage device of the seventh embodiment differs from the storage device of the first embodiment in that the storage device of the seventh embodiment is a resistive random access memory (ReRAM). In the following, some of the descriptions that overlap with the first embodiment will be omitted.
[0376] Fig. 26 is a schematic cross-sectional view of a memory cell in a memory device according to the seventh embodiment. Fig. 26 shows a cross-section of one memory cell MC indicated by, for example, a dotted circle in the memory cell array 100 in Fig. 1.
[0377] 26, the memory cell MC includes a lower electrode 10, an upper electrode 20, an intermediate electrode 30, a switching layer 40, and a resistance change layer 50. The resistance change layer 50 includes a high resistance layer 50x and a low resistance layer 50y.
[0378] The lower electrode 10 is an example of a first conductive layer, the upper electrode 20 is an example of a second conductive layer, and the intermediate electrode 30 is an example of a third conductive layer.
[0379] The lower electrode 10, the switching layer 40, and the intermediate electrode 30 constitute a switching element of the memory cell MC. The intermediate electrode 30, the resistance change layer 50, and the upper electrode 20 constitute a resistance change element of the memory cell MC.
[0380] The configuration of the switching elements is similar to that of the storage device of the first embodiment.
[0381] The resistance change layer 50 includes a high resistance layer 50x and a low resistance layer 50y.
[0382] The high-resistance layer 50x is, for example, a metal oxide, such as aluminum oxide, hafnium oxide, zirconium oxide, tantalum oxide, or niobium oxide.
[0383] The low resistance layer 50y is, for example, a metal oxide. The metal oxide contained in the low resistance layer 50y is different from the metal oxide contained in the high resistance layer 50x. The low resistance layer 50y is, for example, titanium oxide, niobium oxide, tantalum oxide, or tungsten oxide.
[0384] The variable resistance layer 50 has a function of storing data by changing resistance. The variable resistance layer 50 has a characteristic that, for example, the electrical resistance changes when a predetermined voltage is applied.
[0385] By applying a voltage to the resistance change layer 50, the resistance change layer 50 changes from a high resistance state to a low resistance state, or from a low resistance state to a high resistance state. By applying a voltage to the resistance change layer 50, oxygen ions move between the high resistance layer 50x and the low resistance layer 50y, and the amount of oxygen vacancies (amount of oxygen vacancies) in the low resistance layer 50y changes. The conductivity of the resistance change layer 50 changes according to the amount of oxygen vacancies in the low resistance layer 50y. The low resistance layer 50y is a so-called vacancy modulated conductive oxide.
[0386] For example, the high resistance state is defined as data “1” and the low resistance state is defined as data “0.” The memory cell MC is capable of storing one bit of data, “0” and “1.”
[0387] As described above, according to the memory device of the seventh embodiment, a switching element having excellent characteristics such as a low semi-selection leakage current and high reliability can be realized, similarly to the first embodiment. Therefore, according to the seventh embodiment, a memory device having a switching element with excellent characteristics can be realized.
[0388] Although the first to sixth embodiments have been described using a magnetoresistive memory as an example of a two-terminal storage device, and the seventh embodiment has been described using a resistance change memory as an example of a two-terminal storage device, the present invention can be applied to other two-terminal storage devices. For example, the present invention can be applied to a phase change memory (PCM) or a ferroelectric random access memory (FeRAM).
[0389] In addition, in the seventh embodiment, a resistance change memory having the switching element of the first embodiment has been described as an example of a memory device, but it is also possible to use a resistance change memory having the switching element of the second to sixth embodiments.
[0390] In the first to seventh embodiments, the switching element is provided below the resistance change element. However, the switching element may be provided above the resistance change element.
[0391] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. For example, components of one embodiment may be replaced or changed with components of another embodiment. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0392] 10 Lower electrode (first conductive layer) 20 Upper electrode (second conductive layer) 30 Intermediate electrode (third conductive layer) 40 Switching Layer 41 Lower Area (First Area) 42 Upper region (second region) 43 Intermediate Zone (Third Zone) 44 First conductive region (fourth region) 45 Second conductive region (fourth region) 50 Resistance change layer 61 First side wall 62 Second Side Wall 63 Third Sidewall 64 Fourth Sidewall 81 First metal oxide layer (first layer) 82 Second metal oxide layer (second layer) 102 Word line (first wiring) 103 Bit line (second line) MC memory cell
Claims
1. A first conductive layer; and A second conductive layer; and a third conductive layer provided between the first conductive layer and the second conductive layer; a switching layer provided between the first conductive layer and the third conductive layer; a resistance change layer provided between the third conductive layer and the second conductive layer; The switching layer comprises: a first region, a second region between the first region and the third conductive layer, and a third region between the first region and the second region; The first region contains at least one first element selected from the group consisting of zinc (Zn) and tin (Sn) and oxygen (O), The second region includes at least one second element selected from the group consisting of zinc (Zn) and tin (Sn) and oxygen (O), The third region includes at least one third element selected from the group consisting of tantalum (Ta), niobium (Nb), and vanadium (V), and oxygen (O); the first conductive layer contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni); The third conductive layer includes at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni).
2. The thickness of the third region in a first direction from the first conductive layer to the second conductive layer is 2. The storage device according to claim 1, wherein the thickness of the first region in the first direction is greater than the thickness of the second region in the first direction.
3. The thickness of the third region in the first direction is 2.5 nm or more and 4.0 nm or less, 3. The storage device according to claim 2, wherein the thickness of said first region in said first direction and the thickness of said second region in said first direction are not less than 1.6 nm and not more than 2.4 nm.
4. the first region includes a first oxide that is an oxide of the first element; the second region includes a second oxide that is an oxide of the second element; the third region includes a third oxide that is an oxide of the third element; The standard Gibbs energy of formation of the third oxide is smaller than the standard Gibbs energy of formation of the first oxide; The storage device according to claim 1 , wherein the standard Gibbs energy of formation of said third oxide is smaller than the standard Gibbs energy of formation of said second oxide.
5. a first sidewall comprising a fourth oxide; a second sidewall comprising a fifth oxide; Further comprising: the first region is provided between the first sidewall and the second sidewall in a second direction perpendicular to a first direction from the first conductive layer toward the second conductive layer; In the second direction, the second region is provided between the first sidewall and the second sidewall, the first region includes a first oxide that is an oxide of the first element; the second region includes a second oxide that is an oxide of the second element; The standard Gibbs energy of formation of the fourth oxide is greater than the standard Gibbs energy of formation of the first oxide; The standard Gibbs energy of formation of the fourth oxide is greater than the standard Gibbs energy of formation of the second oxide; The standard Gibbs energy of formation of the fifth oxide is greater than the standard Gibbs energy of formation of the first oxide; The storage device according to claim 1 , wherein the standard Gibbs energy of formation of said fifth oxide is greater than the standard Gibbs energy of formation of said second oxide.
6. a third sidewall comprising a sixth oxide; a fourth sidewall including a seventh oxide; Further comprising: the third sidewall is provided between the first region and the first sidewall in the second direction; the third sidewall is provided between the second region and the first sidewall in the second direction; the fourth sidewall is provided between the first region and the second sidewall in the second direction; the fourth side wall is provided between the second region and the second side wall in the second direction; The standard Gibbs energy of formation of the sixth oxide is greater than the standard Gibbs energy of formation of the first oxide; The standard Gibbs energy of formation of the sixth oxide is greater than the standard Gibbs energy of formation of the second oxide; The standard Gibbs energy of formation of the sixth oxide is smaller than the standard Gibbs energy of formation of the fourth oxide; The standard Gibbs energy of formation of the seventh oxide is greater than the standard Gibbs energy of formation of the first oxide; The standard Gibbs energy of formation of the seventh oxide is greater than the standard Gibbs energy of formation of the second oxide; The storage device according to claim 5 , wherein the standard Gibbs energy of formation of the seventh oxide is smaller than the standard Gibbs energy of formation of the fifth oxide.
7. the first sidewall is spaced apart from the first conductive layer or the third conductive layer; The memory device according to claim 5 , wherein the second sidewall is spaced apart from the first conductive layer or the third conductive layer.
8. a thickness in the second direction of the first sidewall located in the second direction of the first region is different from a thickness in the second direction of the first sidewall located in the second direction of the second region, 6. The storage device of claim 5, wherein a thickness in the second direction of the second sidewall located in the second direction of the first region is different from a thickness in the second direction of the second sidewall located in the second direction of the second region.
9. a fourth region provided between the first conductive layer and the third conductive layer and in contact with either the first region or the second region; 2. The storage device according to claim 1, wherein the fourth region includes at least one element combination selected from the group consisting of an element combination of indium (In), tin (Sn), and oxygen (O), an element combination of gallium (Ga), tin (Sn), and oxygen (O), an element combination of gallium (Ga), zinc (Zn), and oxygen (O), and an element combination of aluminum (Al), zinc (Zn), and oxygen (O).
10. 10. The storage device according to claim 9, wherein the thickness of said fourth region in a first direction from said first conductive layer to said second conductive layer is not less than 2 nm and not more than 20 nm.
11. a first layer provided between the first conductive layer and the first region, the first layer including at least one first metal element selected from the group consisting of silver (Ag), iridium (Ir), osmium (Os), ruthenium (Ru), and rhodium (Rh) and oxygen (O); a second layer provided between the third conductive layer and the second region, the second layer including at least one second metal element selected from the group consisting of silver (Ag), iridium (Ir), osmium (Os), ruthenium (Ru), and rhodium (Rh) and oxygen (O); The storage device according to claim 1 , further comprising at least one of the following:
12. the first layer comprises a first metal oxide of the at least one first metallic element; the second layer comprises a second metal oxide of the at least one second metallic element; the first region includes a first oxide that is an oxide of the at least one first element; the second region includes a second oxide that is an oxide of the at least one second element; the standard Gibbs energy of formation of the first metal oxide is greater than the standard Gibbs energy of formation of the first oxide; The storage device of claim 11 , wherein the standard Gibbs energy of formation of the second metal oxide is greater than the standard Gibbs energy of formation of the second oxide.
13. The memory device according to claim 1 , wherein the resistance change layer includes a magnetic tunnel junction.
14. The resistance change layer changes electrical resistance when a predetermined voltage is applied to the resistance change layer. The storage device according to claim 1 , wherein the switching layer has a nonlinear current-voltage characteristic in which a current rises at a specific threshold voltage.
15. A plurality of first wirings; a plurality of second wirings intersecting the plurality of first wirings; 2. The memory device according to claim 1, wherein said memory cell is provided in a region where one of said plurality of first wirings and one of said plurality of second wirings intersect.
16. A first conductive layer; and A second conductive layer; and a third conductive layer provided between the first conductive layer and the second conductive layer; a switching layer provided between the first conductive layer and the third conductive layer; a resistance change layer provided between the third conductive layer and the second conductive layer; The switching layer comprises: a first region, a second region between the first region and the third conductive layer, and a third region between the first region and the second region; the first region includes at least one first metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, lanthanum titanate, strontium-doped lanthanum manganate, and iron oxide; the second region includes at least one second metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, lanthanum titanate, strontium-doped lanthanum manganate, and iron oxide; The third region includes at least one material selected from the group consisting of zirconium oxide, silicon nitride, strontium titanate, titanium oxide, tantalum oxide, hafnium oxide, copper aluminate, lanthanum oxide, yttrium oxide, aluminum oxide, hafnium silicate, barium titanate, silicon carbide, germanium oxide, copper oxide, magnesium oxide, and aluminum nitride.
17. the electron affinity of the at least one material is less than the electron affinity of the at least one first metal oxide; 17. The memory device of claim 16, wherein the electron affinity of the at least one material is less than the electron affinity of the at least one second metal oxide.
18. the first conductive layer contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni); 17. The storage device according to claim 16, wherein the third conductive layer contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni).
19. The memory device of claim 16 , wherein the resistance change layer includes a magnetic tunnel junction.
20. The resistance change layer changes electrical resistance when a predetermined voltage is applied to the resistance change layer.
17. The storage device according to claim 16, wherein the switching layer has a nonlinear current-voltage characteristic in which a current rises at a specific threshold voltage.
21. A plurality of first wirings; a plurality of second wirings intersecting the plurality of first wirings; 17. The memory device according to claim 16, wherein the memory cell is provided in a region where one of the plurality of first wirings and one of the plurality of second wirings intersect.
22. A first conductive layer; and A second conductive layer; and a third conductive layer provided between the first conductive layer and the second conductive layer; a switching layer provided between the first conductive layer and the third conductive layer; a resistance change layer provided between the third conductive layer and the second conductive layer; The switching layer comprises: a first region, a second region between the first region and the third conductive layer, and a third region between the first region and the second region; the first region includes at least one first metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, lanthanum titanate, strontium-doped lanthanum manganate, and iron oxide; the second region includes at least one second metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, lanthanum titanate, strontium-doped lanthanum manganate, and iron oxide; the third region includes at least one third metal oxide selected from the group consisting of niobium oxide, vanadium oxide, chromium-doped vanadium oxide, nickel oxide, lanthanum titanate, strontium-doped lanthanum manganate, and iron oxide; the electron affinity of the third metal oxide is smaller than the electron affinity of the first metal oxide; The third metal oxide has an electron affinity smaller than an electron affinity of the second metal oxide.
23. the first conductive layer contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni); 23. The storage device according to claim 22, wherein the third conductive layer contains at least one element selected from the group consisting of carbon (C), cobalt (Co), gold (Au), and nickel (Ni).
24. The memory device of claim 22 , wherein the resistance change layer includes a magnetic tunnel junction.
25. The resistance change layer changes electrical resistance when a predetermined voltage is applied to the resistance change layer.
23. The storage device according to claim 22, wherein the switching layer has a nonlinear current-voltage characteristic in which a current rises at a specific threshold voltage.
26. A plurality of first wirings; a plurality of second wirings intersecting the plurality of first wirings; 23. The memory device according to claim 22, wherein the memory cell is provided in a region where one of the plurality of first wirings and one of the plurality of second wirings intersect.
Citation Information
Patent Citations
Using multi-layer MIMCAPs with defective barrier layers as selector element for a cross bar memory array
US9029187B1