Biodegradable nonwoven fabric and production method thereof

By incorporating crimped poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) short fibers and employing a controlled production method, biodegradable thermal bond nonwoven fabrics with enhanced texture and biodegradability are achieved, addressing the gap in existing technologies.

JP2024136658AInactive Publication Date: 2024-10-04KANEKA CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023047842
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

There is a lack of biodegradable thermal bond nonwoven fabrics containing poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) fibers, which are known for their biodegradability and thermal bonding properties, and existing technologies do not adequately address their texture and feel.

Method used

Incorporation of poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) short fibers with specific fiber length, crimps, and crimping process to create a biodegradable thermal bonded nonwoven fabric, using a method that includes preheating, crimping, and thermal bonding at controlled temperatures.

Benefits of technology

The resulting nonwoven fabric exhibits excellent feel, texture, and biodegradability, with improved entanglement and ease of production due to crimped fibers, and maintains fiber shape during thermal bonding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136658000001
    Figure 2024136658000001
Patent Text Reader

Abstract

To provide a biodegradable thermally bonded nonwoven fabric including poly-(3-hydroxy butylate-co-3-hydroxy hexanoate) fiber.SOLUTION: A biodegradable thermally bonded nonwoven fabric includes at least poly-(3-hydroxy butylate-co-3-hydroxy hexanoate)-based short fiber. The poly-(3-hydroxy butylate-co-3-hydroxy hexanoate)-based short fiber has a fiber length of 11 to 160 mm and is crimped.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a biodegradable nonwoven fabric and a method for producing the same. [Background technology]

[0002] In recent years, plastic waste has become a major source of stress for the global environment, with problems including its impact on ecosystems, the generation of harmful gases during combustion, and global warming due to the large amount of heat generated by combustion. As a solution to these problems, biodegradable plastics have been actively developed.

[0003] Among these biodegradable plastics, the carbon dioxide emitted when biodegradable plastics made from plant-derived raw materials are burned is the same as that which was originally in the air, and does not increase the amount of carbon dioxide in the atmosphere. This is called carbon neutral, and is considered important under the Kyoto Protocol, which imposes carbon dioxide reduction targets, and active use of such plastics is desired.

[0004] Recently, from the viewpoints of biodegradability and carbon neutrality, aliphatic polyester resins have been attracting attention as biodegradable plastics that are produced by microorganisms using plant-derived raw materials as a carbon source.

[0005] Patent Document 1 discloses a biodegradable staple fiber nonwoven fabric that is made by blending staple fibers made of an aliphatic polyester polymer, which is a biodegradable thermoplastic polymer, with cellulosic staple fibers, and in which the constituent fibers are three-dimensionally entangled with each other. Furthermore, Patent Document 2 discloses a biodegradable short-fiber nonwoven fabric that is composed of short fibers made of a biodegradable thermoplastic polymer and is characterized in that the constituent fibers are three-dimensionally entangled to retain their shape. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 6-200457 [Patent Document 2] Japanese Patent Application Publication No. 9-13255 Summary of the Invention [Problem to be solved by the invention]

[0007] As a nonwoven fabric, a thermally bonded nonwoven fabric is known. Poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) is also known as a biodegradable plastic. However, the above-mentioned Patent Documents 1 and 2 do not disclose either a thermal bonded nonwoven fabric or poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate). Further, up to now, no thermally bonded nonwoven fabric containing poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based fibers has been provided.

[0008] Therefore, an object of the present invention is to provide a biodegradable thermally bonded nonwoven fabric containing poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based fibers, and an object of the present invention is to provide a biodegradable thermally bonded nonwoven fabric containing poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based fibers and having excellent touch, texture, and biodegradability. [Means for solving the problem]

[0009] As a result of extensive research to solve the above problems, the present inventors have found that by controlling the fiber length of the poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based staple fibers contained in the biodegradable thermal bonded nonwoven fabric within a specified range and by having the poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based staple fibers have crimps, a biodegradable thermal bonded nonwoven fabric containing poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) fibers can be obtained. The present inventors have also discovered that such a biodegradable thermally bonded nonwoven fabric is excellent in feel, texture and biodegradability.

[0010] That is, the first aspect of the present invention is a fiber material comprising at least poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based short fibers, The poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based staple fiber relates to a biodegradable thermal bonded nonwoven fabric having a fiber length of 11 to 160 mm and crimped.

[0011] The second aspect of the present invention is a method for producing the biodegradable thermobonded nonwoven fabric, comprising the steps of: preheating poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) based drawn filaments; crimping the preheated poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) based drawn filaments using a stuffing box; a step of cutting the crimped poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based drawn filaments to a predetermined fiber length to obtain poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based short fibers; and a step of thermally bonding the fibers containing the poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based short fibers under temperature conditions of 40°C to 180°C. Effect of the Invention

[0012] According to the present invention, a biodegradable thermally bonded nonwoven fabric containing poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) fibers can be provided, which has excellent touch, texture, and biodegradability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, one embodiment of the present invention will be described.

[0014] <Biodegradable thermal bond nonwoven fabric> The biodegradable thermally bonded nonwoven fabric according to this embodiment (hereinafter, simply referred to as "nonwoven fabric") has fibers that include at least poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based staple fibers. The poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based short fibers have a fiber length of 11 to 160 mm. The poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) based staple fibers have crimps.

[0015] The nonwoven fabric according to this embodiment is a thermally bonded nonwoven fabric, and therefore is soft, has excellent drapeability, and is excellent in feel and texture.

[0016] (Poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) staple fiber) The biodegradable nonwoven fabric according to this embodiment contains poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) (hereinafter also referred to as "P3HB3HH-based staple fibers") that contain poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) (hereinafter also referred to as "P3HB3HH"). The nonwoven fabric according to this embodiment contains P3HB3HH staple fibers, and thus is soft and has excellent drapeability, texture, and biodegradability.

[0017] The P3HB3HH staple fibers preferably contain more than 50% by weight of P3HB3HH, more preferably 80% by weight or more, and even more preferably 90% by weight or more.

[0018] The method for producing P3HB3HH is not particularly limited, but examples thereof include a method in which P3HB3HH is produced by a microorganism capable of producing P3HB3HH. An example of a P3HB3HH-producing bacterium is Alcaligenes eutrophus AC32 (FERM BP-6038) (T. Fukui, Y. Doi, J. Bacteriol., 179, pp. 4821-4830 (1997)), into which genes encoding P3HA synthases have been introduced to increase the productivity of P3HB3HH. P3HB3HH can be produced by culturing a microorganism under appropriate conditions, allowing P3HB3HH to accumulate in the cells, and then recovering the P3HB3HH. Culture conditions, including the type of substrate, can be optimized according to the microorganism used.

[0019] The P3HB3HH has excellent biodegradability. In this embodiment, "biodegradability" refers to a property that can be decomposed into low molecular weight compounds by microorganisms in nature. Specifically, the presence or absence of biodegradability can be determined based on tests suitable for each environment, such as ISO 14855 (compost) and ISO 14851 (activated sludge) under aerobic conditions, and ISO 14853 (aqueous phase) and ISO 15985 (solid phase) under anaerobic conditions. In addition, the decomposition by microorganisms in seawater can be evaluated by measuring biochemical oxygen demand.

[0020] The P3HB3HH contains 3-hydroxybutyrate (3HB) as a structural unit in an amount of preferably 85.0 mol % to 99.5 mol %, and more preferably 85.0 mol % to 97.0 mol %. When the P3HB3HH contains 85.0 mol % or more of 3-hydroxybutyrate (3HB) as a structural unit, the rigidity of the P3HB3HH-based short fibers is increased. Furthermore, since the P3HB3HH contains 99.5 mol % or less of 3-hydroxybutyrate (3HB) as a structural unit, the P3HB3HH-based short fibers have excellent flexibility. The ratio of 3-hydroxybutyrate (3HB) as a structural unit in P3HB3HH can be determined by the method described below.

[0021] The P3HB3HH-based short fibers may contain a biodegradable resin other than P3HB3HH. Examples of the other biodegradable resins include polycaprolactone, polylactic acid, polybutylene succinate, polybutylene succinate adipate, polybutylene adipate terephthalate, polyethylene succinate, polyvinyl alcohol, polyglycolic acid, unmodified starch, modified starch, cellulose acetate, chitosan, and poly(4-hydroxyalkanoate)-based resins. Furthermore, the other biodegradable resins include poly(3-hydroxyalkanoate) resins other than P3HB3HH. Examples of poly(3-hydroxyalkanoate) resins other than P3HB3HH include P3HB, P3HB3HV, P3HB4HB, poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), poly(3-hydroxybutyrate-co-3-hydroxyoctadecanoate), and the like. Here, P3HB means the homopolymer poly(3-hydroxybutyrate). P3HB3HV means poly(3-hydroxybutyrate-co-3-hydroxyvalerate). P3HB4HB means poly(3-hydroxybutyrate-co-4-hydroxybutyrate). The P3HB3HH staple fibers may contain one or more other biodegradable resins.

[0022] The P3HB3HH staple fibers may contain additives.

[0023] Examples of the additives include crystal nucleating agents, lubricants, stabilizers (antioxidants, ultraviolet absorbers, etc.), colorants (dyes, pigments, etc.), plasticizers, inorganic fillers, organic fillers, and antistatic agents.

[0024] In order to promote the crystallization of the P3HB3HH, the P3HB3HH-based short fibers preferably contain a crystal nucleating agent. The crystal nucleating agent is a compound that has the effect of promoting the crystallization of the P3HB3HH, and has a melting point higher than that of the P3HB3HH. Examples of the crystal nucleating agent include inorganic substances (boron nitride, titanium oxide, talc, layered silicates, calcium carbonate, sodium chloride, metal phosphates, etc.); sugar alcohol compounds derived from natural products (pentaerythritol, erythritol, galactitol, mannitol, arabitol, etc.); polyvinyl alcohol; chitin; chitosan; polyethylene oxide; aliphatic carboxylates; aliphatic alcohols; aliphatic carboxylate esters; dicarboxylic acid derivatives (dimethyl adipate, dibutyl adipate, diisodecyl adipate, dibutyl selenite, etc.); Examples include cyclic compounds having C=O and a functional group selected from NH, S and O in the molecule (indigo, quinacridone, quinacridone magenta, etc.); sorbitol derivatives (bisbenzylidene sorbitol, bis(p-methylbenzylidene)sorbitol, etc.); compounds containing a nitrogen-containing heteroaromatic nucleus (pyridine ring, triazine ring, imidazole ring, etc.) (pyridine, triazine, imidazole, etc.); phosphate ester compounds; bisamides of higher fatty acids; metal salts of higher fatty acids; and branched polylactic acid. P3HB can also be used as a crystal nucleating agent. These may be used alone or in combination of two or more.

[0025] As the crystal nucleating agent, from the viewpoint of the effect of improving the crystallization rate of P3HB3HH and from the viewpoint of compatibility and affinity with P3HB3HH, sugar alcohol compounds, polyvinyl alcohol, chitin, and chitosan are preferred. Among the sugar alcohol compounds, pentaerythritol is preferred.

[0026] The P3HB3HH staple fibers contain a crystal nucleating agent in an amount of preferably 0.1 part by weight or more, more preferably 0.2 part by weight or more, and even more preferably 0.4 part by weight or more, based on 100 parts by weight of the P3HB3HH. The P3HB3HH short fibers contain 0.1 part by weight or more of a crystal nucleating agent based on 100 parts by weight of the P3HB3HH, thereby making it possible to promote the crystallization of P3HB3HH. The P3HB3HH staple fibers contain a crystal nucleating agent in an amount of preferably 4 parts by weight or less, more preferably 3 parts by weight or less, and even more preferably 2.5 parts by weight or less, based on 100 parts by weight of the P3HB3HH. By containing 4 parts by weight or less of a crystal nucleating agent per 100 parts by weight of the P3HB3HH, the viscosity of the molten material can be reduced when the P3HB3HH short fibers are produced by a melt spinning method, which has the advantage of making it easier to produce the P3HB3HH short fibers.

[0027] The P3HB3HH short fibers contain pentaerythritol in an amount of preferably 0.1 parts by weight or more, more preferably 0.2 parts by weight or more, and even more preferably 0.4 parts by weight or more, per 100 parts by weight of the P3HB3HH, and preferably 4 parts by weight or less, more preferably 3 parts by weight or less, and even more preferably 2.5 parts by weight or less, per 100 parts by weight of the P3HB3HH.

[0028] The P3HB3HH staple fibers preferably contain the lubricant, which improves the lubricating properties of the P3HB3HH staple fibers. The lubricant may, for example, be a fatty acid amide. The fatty acid amide preferably includes at least one selected from lauric acid amide, myristic acid amide, stearic acid amide, behenic acid amide, and erucic acid amide.

[0029] The P3HB3HH staple fibers contain a lubricant in an amount of preferably 0.1 part by weight or more, more preferably 0.2 part by weight or more, and even more preferably 0.4 part by weight or more, based on 100 parts by weight of the P3HB3HH. The P3HB3HH staple fibers contain 0.1 part by weight or more of a lubricant per 100 parts by weight of the P3HB3HH, which provides the advantage of excellent lubrication of the P3HB3HH staple fibers. The P3HB3HH staple fibers preferably contain 4 parts by weight or less, more preferably 3 parts by weight or less, and even more preferably 2.5 parts by weight or less of a lubricant based on 100 parts by weight of the P3HB3HH. The P3HB3HH staple fibers contain 4 parts by weight or less of a lubricant per 100 parts by weight of the P3HB3HH, which has the advantage that bleeding out of the lubricant onto the surface of the P3HB3HH staple fibers can be suppressed.

[0030] The P3HB3HH staple fibers contain, based on 100 parts by weight of the P3HB3HH, preferably 0.1 parts by weight or more, more preferably 0.2 parts by weight or more, and even more preferably 0.4 parts by weight or more of fatty acid amide, and based on 100 parts by weight of the P3HB3HH, preferably 4 parts by weight or less, more preferably 3 parts by weight or less, and even more preferably 2.5 parts by weight or less of fatty acid amide.

[0031] From the viewpoint of practical use, the fiber length of the P3HB3HH staple fiber is from 11 to 160 mm, preferably from 15 to 160 mm, more preferably from 20 to 110 mm, and further preferably from 25 to 76 mm. The fiber length means the "average fiber length" obtained by "c) C method (substitution method)" of "8.4.1 Average fiber length" of "8.4 Fiber length" of JIS L1015:2021 "Test methods for chemical fiber staples".

[0032] The P3HB3HH staple fibers have crimps, in other words, the P3HB3HH staple fibers are in the form of crimped yarns (crimped yarns). The crimped nature of the P3HB3HH staple fibers has the advantage that the fibers tend to entangle with each other when preparing a web to be used for producing a thermal bonded nonwoven fabric, as described below, making the web easier to prepare, and as a result, making it easier to produce a thermal bonded nonwoven fabric.

[0033] The number of crimps of the P3HB3HH staple fibers is preferably 5 to 25 crimps / 25 mm, more preferably 6 to 20 crimps / 25 mm, further preferably 7 to 18 crimps / 25 mm, and particularly preferably 8 to 17 crimps / 25 mm. The P3HB3HH staple fibers having a crimp number of 5 crimps / 25 mm or more have the advantage that the fibers tend to be entangled with each other when producing a web, facilitating the production of the web. The P3HB3HH staple fibers having a crimp number of 25 / 25 mm or less have the advantage that the P3HB3HH staple fibers can be prevented from clumping together during web production, making it easier to produce the web. The crimp number of P3HB3HH staple fibers means the number of crimps per 25 mm of P3HB3HH staple fibers. The crimp number of P3HB3HH staple fibers means the average number of crimps of 15 randomly selected P3HB3HH staple fibers. When there are less than 15 P3HB3HH staple fibers, the average number of crimps of all P3HB3HH staple fibers is meant. The crimp number of each P3HB3HH staple fiber can be determined by counting the number of crimp peaks in a 25 mm length of the P3HB3HH staple fibers using a microscope. When the length of each P3HB3HH staple fiber is less than 25 mm, the number of crimps per 25 mm may be determined by counting the number of crimp peaks in the entire length using a microscope.

[0034] The weight average molecular weight (Mw) of the P3HB3HH short fibers is preferably in the range of 50,000 to 2.5 million, more preferably 70,000 to 1 million, and further preferably 100,000 to 400,000. When the weight average molecular weight is 2.5 million or less, the productivity can be easily improved when obtaining poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based drawn filaments, which will be described later, by spinning through a nozzle extrusion. When the weight average molecular weight is 50,000 or more, the physical properties (strength, etc.) of the P3HB3HH short fibers are improved. Resins with the optimum weight average molecular weight can be used according to the required "productivity" and "physical properties of P3HB3HH-based short fibers."

[0035] In the present embodiment, the weight average molecular weight is measured from the polystyrene equivalent molecular weight distribution by gel permeation chromatography (GPC) using chloroform as an eluent. As the column for the GPC, a column suitable for measuring the molecular weight may be used. For example, the weight average molecular weight (Mw) can be determined by setting the column temperature at 40°C, injecting 10 μl of 3 mg of the target substance dissolved in 2 ml of chloroform, and setting the flow rate of the chloroform eluent (mobile phase) to 1.0 ml / min. The GPC device used is an LC-10A system (manufactured by Shimadzu Corporation), and the column used is a GPCK-806M (manufactured by Showa Denko Corporation).

[0036] The lower limit temperature of the crystal melting peak range of P3HB3HH staple fibers measured by differential scanning calorimetry (DSC) is preferably 40°C or higher, more preferably 50°C or higher, and even more preferably 60°C or higher. When the lower limit temperature is 40° C. or higher, there is an advantage that handling is easy during heat bonding and heat fusion can be achieved from a low temperature range. The lower limit of the temperature is preferably 115° C. or lower, more preferably 110° C. or lower, and even more preferably 105° C. or lower. By setting the lower limit temperature to 115°C or less, it is possible to further prevent the P3HB3HH staple fibers from shrinking and becoming unstable in size during thermal bonding, which has the advantage of making it easier to bond the fibers while maintaining their shape in a better condition.

[0037] The upper limit temperature of the crystal melting peak range is preferably 180°C or lower, more preferably 177°C or lower, and even more preferably 175°C or lower. By setting the upper limit of the temperature to 180° C. or less, there is an advantage that heat fusion can be easily performed at a temperature equal to or lower than the decomposition temperature of the resin during thermal adhesion. The upper limit of the temperature is preferably 145° C. or higher, more preferably 150° C. or higher, and even more preferably 155° C. or higher. By setting the upper limit temperature to 145° C. or higher, there is an advantage that the molten state of the fiber surface becomes more favorable near the melting point of the P3HB3HH staple fiber during thermal bonding, facilitating bonding.

[0038] The lower limit temperature and the upper limit temperature of the crystal melting peak range can be measured in accordance with JIS K7121-1987 "Method of measuring transition temperature of plastics." Specifically, a differential scanning calorimeter (e.g., DSC25 differential scanning calorimeter manufactured by TA Instruments) is used, and approximately 6.0 mg of P3HB3HH short fibers as a sample are filled into a measurement container, and the sample is heated and cooled between 0°C and 185°C at a heating and cooling rate of 10°C / min under a nitrogen gas flow rate of 50 ml / min, to determine the lower and upper limits of the crystal melting peak range.

[0039] The lower limit temperature can be increased, for example, by increasing the ratio of 3-hydroxybutyrate (3HB) as a structural unit in P3HB3HH. In addition, the upper limit of the temperature can be lowered, for example, by increasing the ratio of 3-hydroxybutyrate (3HB) as a structural unit in P3HB3HH.

[0040] The P3HB3HH staple fibers are preferably multifilaments. The P3HB3HH staple fibers have 1 or more, preferably 30 or more, more preferably 30 to 500,000, and further preferably 50 to 300,000 single fibers.

[0041] The multifilament preferably further has a spinning oil on the surface of the single filaments from the viewpoint of suppressing fusion between adjacent single filaments and suppressing separation of adjacent single filaments due to static electricity. Examples of the spinning oil include cationic surfactants, anionic surfactants, nonionic surfactants, refined esterified oils, mineral oils, poly(oxyethylene) alkyl ethers, silicone oils, paraffin waxes, etc. These may be used alone or in combination of two or more. From the viewpoint of suppressing fusion between adjacent single fibers, the spinning oil is preferably silicone oil. From the viewpoint of preventing adjacent single fibers from being separated from each other due to static electricity, the spinning oil is preferably an anionic surfactant or a nonionic surfactant. As the spinning oil, for example, a spinning oil containing silicone oil and an anionic surfactant (for example, "Polymax FKY" manufactured by Marubishi Chemical Co., Ltd.) can be used.

[0042] The single fiber fineness of the P3HB3HH staple fibers is preferably 0.1 to 100 dtex, more preferably 0.5 to 50 dtex, and further preferably 1.0 to 20 dtex. The P3HB3HH staple fiber has a single fiber fineness of 100 dtex or less, which has the advantage of providing a nonwoven fabric with a better feel to the touch. The P3HB3HH staple fiber has a single fiber fineness of 0.1 dtex or more, which has the advantage that a nonwoven fabric having a practical strength can be produced uniformly. The single fiber fineness of the P3HB3HH staple fiber can be adjusted by adjusting the flow rate of the molten material discharged from the spinning nozzle and the draw ratio at which the raw yarn is drawn by a drawing roll in the melt spinning method described below.

[0043] In this embodiment, the single fiber fineness refers to the thickness of a single fiber, and is defined as the weight per unit length, and is expressed in units of weight (g) per 10,000 m (dtex). In this embodiment, the single fiber fineness can be determined as follows. First, the fineness (total fineness) of the P3HB3HH staple fibers is measured, and the number of single fibers contained in the P3HB3HH staple fibers is calculated. Then, the single fiber fineness is calculated using the following formula. Single fiber fineness = Fineness of P3HB3HH staple fiber / Number of single fibers in P3HB3HH staple fiber

[0044] The single fiber tensile strength of the P3HB3HH staple fiber is preferably 0.1 to 10 cN / dtex, and more preferably 0.3 to 10 cN / dtex. The single fiber tensile strength of the P3HB3HH staple fiber is 0.1 cN / dtex or more, which increases the strength of the nonwoven fabric. The single fiber tensile strength of the P3HB3HH staple fiber can be adjusted by adjusting the draw ratio at which the raw yarn is drawn with a drawing roll in the melt spinning method described below.

[0045] In this embodiment, the single fiber tensile strength can be determined as follows. First, the tensile strength of each of all the single fibers constituting the staple fibers is measured. Alternatively, 10 or more single fibers are randomly selected from the staple fibers, and the tensile strength of each of the single fibers is measured. That is, since it may be impractical to measure the tensile strength of each of the single fibers constituting the staple fibers, 10 or more single fibers may be randomly selected from the staple fibers, and the tensile strength of each of the single fibers may be measured. Then, the arithmetic mean value of the tensile strength of the single fibers is calculated from the tensile strength of each single fiber, and this value is regarded as the single fiber tensile strength.

[0046] The tensile strength of each single fiber can be measured based on JIS L 1015:2021 "Test method for chemical fiber staples" at an initial length of 20 mm and a speed of 20 mm / min. For example, the tensile strength of each single fiber can be determined as follows. First, the load (cN) at the time of breaking of each single fiber is measured under the following conditions using a tensile measuring device Autograph AG-I (manufactured by Shimadzu Corporation). Initial length of each single fiber: 20mm Tensile speed: 20mm / min Load cell: A load cell with a rated capacity of 5N The fineness of each single fiber is also measured. The fineness of each single fiber can be measured, for example, by an autobibroscope method. Then, the tensile strength of each single fiber is calculated according to the following formula. Tensile strength of each single fiber (cN / dtex) = Load at break of each single fiber (cN) / Fineness of each single fiber

[0047] The cross-sectional shape of the single fiber is, for example, circular (a concept including a perfect circle, an approximately circular shape, an ellipse, and an approximately ellipse).

[0048] (Biodegradable polysaccharide short fibers) The nonwoven fabric according to this embodiment preferably contains biodegradable polysaccharide staple fibers that contain at least one type of biodegradable polysaccharide. The nonwoven fabric of this embodiment contains biodegradable polysaccharide-based short fibers, which has the advantage that when the P3HB3HH-based short fibers and the biodegradable polysaccharide-based short fibers are heat-fused to obtain a thermal-bonded nonwoven fabric, it is mainly the P3HB3HH-based short fibers that are heat-melted, making it easier for the biodegradable polysaccharide-based short fibers to maintain the shape of the short fibers in the thermal-bonded nonwoven fabric. Furthermore, the nonwoven fabric according to this embodiment contains biodegradable polysaccharide short fibers, and thus has excellent biodegradability.

[0049] Examples of the biodegradable polysaccharides include cellulose, chitin, and chitosan. As the biodegradable polysaccharide, cellulose is preferred from the viewpoint of easy availability of fibers. The biodegradable polysaccharide is preferably a polysaccharide containing a cellulose group. Examples of biodegradable polysaccharide staple fibers containing cellulose include regenerated cellulose fibers and natural cellulose fibers. Examples of the regenerated cellulose fiber include lyocell, rayon, polynosic, and cupra. The natural cellulose may be, for example, pulped plant materials, such as wood, cotton, bamboo, hemp, shoots, and kenaf.

[0050] The biodegradable polysaccharide short fibers preferably contain more than 50% by weight of biodegradable polysaccharides, more preferably 80% by weight or more, and even more preferably 90% by weight or more.

[0051] The fiber length of the biodegradable polysaccharide short fibers is preferably 11 to 160 mm, more preferably 15 to 160 mm, even more preferably 20 to 110 mm, and most preferably 25 to 76 mm.

[0052] The biodegradable polysaccharide staple fibers may be crimped. The biodegradable polysaccharide staple fibers may be multifilaments or monofilaments.

[0053] The single fiber fineness of the biodegradable polysaccharide short fibers is preferably 0.1 to 100 dtex, more preferably 0.5 to 80 dtex, and even more preferably 1.0 to 60 dtex.

[0054] The nonwoven fabric according to this embodiment contains the P3HB3HH staple fibers in an amount of preferably 20% by weight to 80% by weight, more preferably 30% by weight to 70% by weight, and even more preferably 40% by weight to 60% by weight. The nonwoven fabric according to this embodiment contains the biodegradable polysaccharide short fibers in an amount of preferably 20% by weight to 80% by weight, more preferably 30% by weight to 70% by weight, and even more preferably 40% by weight to 60% by weight. The nonwoven fabric according to this embodiment contains 20% by weight or more and 80% by weight or less of the P3HB3HH-based short fibers and 20% by weight or more and 80% by weight or less of the biodegradable polysaccharide-based short fibers, thereby providing even better touch, texture, and biodegradability.

[0055] The nonwoven fabric according to this embodiment contains the P3HB3HH staple fibers and the biodegradable polysaccharide staple fibers in a total amount of preferably 50 to 100% by weight, more preferably 70 to 100% by weight, even more preferably 80 to 100% by weight, particularly preferably 90 to 100% by weight, and most preferably 100% by weight.

[0056] The basis weight of the nonwoven fabric according to this embodiment is preferably 5 to 500 g / m 2 , more preferably 10 to 300 g / m 2 It is. The weight of the nonwoven fabric is 5g / m 2 By setting the weight per unit area to 5 g / m or more, the strength and elongation of the nonwoven fabric are increased. 2 As a result of the above, the efficiency of particles (dust, etc.) being captured by the nonwoven fabric is further improved. The weight of the nonwoven fabric is 500g / m 2 By satisfying the above condition, the liquid permeability (water permeability, etc.) or air permeability of the nonwoven fabric can be improved.

[0057] The basis weight of the nonwoven fabric can be determined as follows. First, a test piece is obtained from the nonwoven fabric. The size of the test piece can be, for example, 100 mm x 100 mm, 200 mm x 200 mm, etc. Next, the weight of the test piece is measured using an electronic balance or the like. The weight of the test piece is then divided by the area of ​​the test piece to calculate the basis weight.

[0058] The nonwoven fabric according to the present embodiment can be used in a wide range of applications, including household goods such as draining garbage bags, tea bags, and ventilation fan filters; surface materials for disposable diapers (e.g., disposable diapers for infants and disposable diapers for adults) and surface materials for sanitary napkins; and hygiene materials such as wipers.

[0059] The biodegradable nonwoven fabric according to this embodiment is configured as described above. Next, a method for producing the biodegradable nonwoven fabric according to this embodiment will be described.

[0060] <Manufacturing method of biodegradable thermal bonded nonwoven fabric> As a result of extensive research, the present inventors have discovered that a specific manufacturing method makes it easier to produce a biodegradable thermally bonded nonwoven fabric containing poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based fiber.

[0061] That is, in the method for producing a biodegradable thermobonded nonwoven fabric according to this embodiment (hereinafter also simply referred to as a "nonwoven fabric production method"), the nonwoven fabric is produced. The manufacturing method of the thermally bonded nonwoven fabric of this embodiment includes the steps of preheating poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based drawn filaments (hereinafter also referred to as "P3HB3HH-based drawn filaments"), crimping the preheated P3HB3HH-based drawn filaments, cutting the crimped P3HB3HH-based drawn filaments to a predetermined fiber length to obtain P3HB3HH-based short fibers, and thermally bonding fibers containing the P3HB3HH-based short fibers.

[0062] In the preheating step, the P3HB3HH drawn filaments are preheated at a temperature of preferably 50 to 100°C, more preferably 60 to 90°C. The method for producing a nonwoven fabric according to this embodiment has the advantage that the P3HB3HH drawn filaments are more likely to be sufficiently crimped in the crimping process by virtue of the preheating step. The preheating temperature of 50° C. or higher has the advantage that the P3HB3HH drawn filaments are easily and sufficiently crimped in the crimping process. The preheating temperature of 100° C. or less has the advantage that the filament shape of the P3HB3HH-based drawn filament is easily maintained.

[0063] In the crimping step, the preheated P3HB3HH drawn filaments are crimped.

[0064] The P3HB3HH-based drawn filaments used in the crimping process can be produced, for example, by a conventional melt spinning method (for example, International Publication No. 2022 / 202397). In the melt spinning method, the material for the P3HB3HH-based drawn filament is kneaded while being heated to obtain a melt. The melt is then discharged from a spinning nozzle with an outlet hole to obtain a molten raw yarn. The molten raw yarn is then cooled by blowing gas onto it. The cooled raw yarn is then drawn with a drawing roll to obtain a P3HB3HH-based drawn filament.

[0065] The single fiber tensile strength of the P3HB3HH-based drawn filament is preferably 0.5 to 10 cN / dtex, more preferably 0.7 to 10 cN / dtex. The P3HB3HH staple fiber has a single fiber tensile strength of 0.5 cN / dtex or more, which is advantageous in that the strength of the resulting nonwoven fabric is high. The single fiber tensile strength of P3HB3HH staple fibers is 10 cN / dtex or less, which has the advantage of suppressing an increase in the heat shrinkage rate of the staple fibers and improving dimensional stability during processing into nonwoven fabrics.

[0066] In the crimping step, it is preferable to crimp the P3HB3HH drawn filaments using a stuffing box. The stuffing pressure (gauge pressure) when the P3HB3HH drawn filaments are crimped using a stuffing box is preferably 0.001 to 0.3 MPa, and more preferably 0.01 to 0.1 MPa. By setting the stuffing pressure to 0.001 MPa or more, the P3HB3HH-based drawn filaments can be sufficiently crimped. tree This has the advantage that The stuffing pressure of 0.3 MPa or less has the advantage that excessive crimping and fusion and solidification of the fibers due to excessive heat can be suppressed, and a crimped yarn with excellent elasticity can be obtained. The stuffing pressure means the pressure applied to the P3HB3HH drawn filaments in the stuffing box.

[0067] In the step of obtaining the P3HB3HH staple fibers, the crimped P3HB3HH drawn filaments are cut to a predetermined fiber length to obtain the P3HB3HH staple fibers. The predetermined fiber length is preferably 11 to 160 mm, more preferably 15 to 160 mm, further preferably 20 to 110 mm, and particularly preferably 25 to 76 mm.

[0068] In the thermal bonding step, the fibers containing the P3HB3HH staple fibers are thermally bonded to obtain a thermally bonded nonwoven fabric. In the thermal bonding step, the fibers are thermally bonded under temperature conditions of preferably 40°C to 180°C, more preferably 50°C to 170°C, and even more preferably 60°C to 160°C. The temperature condition of 40° C. or higher has the advantage that the fibers can be in sufficient thermal contact. By setting the temperature condition to 180° C. or less, it is possible to prevent the fibers from melting too much, and this has the advantage that the shape of the fibers can be easily maintained. In the thermal bonding step, a carding machine is used to obtain a web from fibers containing P3HB3HH staple fibers, and the fibers contained in the web are thermally bonded.

[0069] Methods for thermally bonding fibers include flat type, open type, embossed type, and the like. In the flat type, the fibers are thermally bonded together while pressing the web with a smooth heated roll, resulting in a flat, thin nonwoven fabric. In the open type, an oven is used to blow hot air, which is passed through the web in the oven to thermally bond the fibers together, resulting in a fluffy, bulky nonwoven fabric. In the embossed type, the fibers are thermally bonded together while pressing the web with a heated roll with an embossed pattern, resulting in a nonwoven fabric with an embossed pattern.

[0070] In the thermal bonding step, it is preferable to thermally bond the fibers to each other while applying a load (pressure) to the web. This has the advantage that the fibers can be easily thermally bonded even at low temperatures for a short period of time, that is, the fibers can be sufficiently thermally bonded while maintaining their fiber shape. Another advantage is that it becomes easier to obtain nonwoven fabrics with excellent texture.

[0071] [Disclosure items] Each of the following sections is a disclosure of a preferred embodiment. [Item 1] At least poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) based short fibers are included, The poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) staple fibers have a fiber length of 11 to 160 mm and are crimped, forming a biodegradable thermally bonded nonwoven fabric. [Item 2] The poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based staple fiber is contained in an amount of 20% by weight or more and 80% by weight or less, 2. The biodegradable thermal bonded nonwoven fabric according to item 1, comprising 20% ​​by weight or more and 80% by weight or less of biodegradable polysaccharide-based short fibers containing at least one kind of biodegradable polysaccharide. [Item 3] The poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based staple fiber has a lower limit temperature of a crystal melting peak range measured by differential scanning calorimetry (DSC) of 40° C. or higher; 3. The biodegradable thermally bonded nonwoven fabric according to item 1 or 2, wherein the upper limit of the crystalline melting peak range is 180° C. or lower. [Item 4] 4. The biodegradable thermally bonded nonwoven fabric according to any one of items 1 to 3, wherein the poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) staple fiber has a crimp number of 5 to 25 crimps / 25 mm. [Item 5] 5. The biodegradable thermally bonded nonwoven fabric according to any one of items 1 to 4, wherein the poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based staple fiber has a single fiber fineness of 0.1 to 100 dtex. [Item 6] 6. The biodegradable thermobonded nonwoven fabric according to any one of items 1 to 5, wherein the biodegradable polysaccharide is a polysaccharide from the cellulose group. [Item 7] A method for producing a biodegradable thermobonded nonwoven fabric according to any one of items 1 to 6, comprising the steps of: preheating poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) based drawn filaments; crimping the preheated poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) based drawn filaments using a stuffing box; a step of cutting the crimped poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based drawn filaments to a predetermined fiber length to obtain poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based short fibers; and heat-bonding the fibers containing the poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) staple fibers at a temperature of 40°C to 180°C. [Item 8] 8. The method for producing a biodegradable thermally bonded nonwoven fabric according to item 7, wherein the poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based drawn filaments have a single fiber tensile strength of 0.5 to 10 cN / dtex.

[0072] The present invention is not limited to the above-described embodiment. The present invention is also not limited to the above-described effects. Furthermore, the present invention can be modified in various ways without departing from the scope of the present invention. EXAMPLES

[0073] The present invention will now be described in more detail with reference to examples and comparative examples, although the present invention is not limited to these examples in any way.

[0074] (Ratio of HH and HB in P3HB3HH) The ratio of 3-hydroxyhexanoate (HH) and 3-hydroxybutyrate (HB) as structural units in P3HB3HH in the Examples and Comparative Examples described below was determined as follows. First, 20 mg of dried P3HB3HH was mixed with 2 mL of a mixture of sulfuric acid and methanol (volume of sulfuric acid:volume of methanol = 15:85) and 2 mL of chloroform, and the mixture was sealed. The sample was then heated at 100°C for 140 minutes in a sealed state to obtain a first reaction solution containing the methyl ester, which is a decomposition product of P3HB3HH. The first reaction liquid was then cooled, and 1.5 g of sodium hydrogen carbonate was gradually added to the cooled first reaction liquid to neutralize it, and the liquid was left to stand until the evolution of carbon dioxide gas ceased, thereby obtaining a second reaction liquid. Furthermore, the second reaction solution and 4 mL of diisopropyl ether were thoroughly mixed to obtain a mixture. The mixture was then centrifuged to obtain a supernatant. The monomer unit composition of the decomposition product in the supernatant was analyzed by capillary gas chromatography under the conditions described below to determine the ratio of 3-hydroxyhexanoate (HH) and 3-hydroxybutyrate (HB) as structural units in P3HB3HH. The measured values ​​are shown in Table 1 below. Gas chromatograph: Shimadzu GC-17A Capillary column: NEUTRA BOND-1 manufactured by GL Sciences (column length: 25 m, column inner diameter: 0.25 mm, liquid film thickness: 0.4 μm) Carrier gas: He Column inlet pressure: 100kPa Sample volume: 1μL As for the temperature conditions, the temperature was increased at a rate of 8°C / min from 100 to 200°C, and further increased at a rate of 30°C / min from 200 to 290°C.

[0075] (Measurement of Short Fiber Parameters) For the staple fibers in the Examples and Comparative Examples described below, the fiber length, single fiber fineness, single fiber tensile strength, weight average molecular weight, number of crimps, and the lower and upper limits of the crystal melting peak range determined by DSC measurement were measured by the methods described above. The measured values ​​are shown in Table 1 below.

[0076] Example 1 The materials shown in Table 1 below were mixed in the compounding ratios shown in Table 1 below to obtain a P3HB3HH composition (melt), and the P3HB3HH-based drawn filaments shown in Table 1 below were obtained by melt spinning. Next, the P3HB3HH-based drawn filaments were preheated at a temperature of 75° C., and the preheated P3HB3HH-based drawn filaments were subjected to crimp processing using a stuffing box under a stuffing pressure of 0.03 MPa. The crimped P3HB3HH drawn filaments were then cut to obtain P3HB3HH staple fibers. Next, the P3HB3HH staple fibers and Lyocell staple fibers shown in Table 1 below, which serve as biodegradable polysaccharide staple fibers, were mixed in the weight ratios shown in Table 1 below, and a web was produced using a carding machine. The web was heated at 165° C. for 5 minutes using a uniform heat dryer without applying any load to the web, thereby thermally bonding (thermally fusing) the fibers.

[0077] (Examples 2 to 7) A nonwoven fabric was obtained in the same manner as in Example 1, except that the conditions were changed as shown in Table 1 below. In Table 1, "with heat press" means that a load was applied to the web by heat pressing. Also, "with load" in Table 1 means that the web was sandwiched between plates and a load was applied to the web with a weight (a load was applied at a lower pressure than "with heat press").

[0078] (Comparative Examples 1 and 2) An attempt was made to produce a web in the same manner as in Example 1, except that crimp-free P3HB3HH staple fibers (number of crimps: 0 / 25 mm) were used and the conditions were changed to those shown in Table 1 below. However, the fibers did not entangle with each other, and a web could not be produced.

[0079] (Met) The basis weight of the nonwoven fabric was measured by the method described above. The measured values ​​are shown in Table 1 below.

[0080] (Texture) In this specification, the texture of a nonwoven fabric refers to the feel of the surface of the nonwoven fabric. The texture of the nonwoven fabric was evaluated according to the following criteria. Good: Soft and fluffy texture Poor: Rough or hard to the touch The results are shown in Table 1 below.

[0081] (texture) In this specification, the texture of a nonwoven fabric refers to the characteristics of the material (nonwoven fabric) itself. The texture of the nonwoven fabric was evaluated according to the following criteria. Very good: In better condition than "good" below. Good: Almost no fused material or foreign matter, thin and firm like Japanese paper Poor: The paper or cloth is hard like a scrubbing pad or plastic and does not retain its shape. The results are shown in Table 1 below.

[0082] (soil degradability) A predetermined amount of nonwoven fabric samples cut to 5 cm x 5 cm were placed in a polypropylene net and buried in soil (Takii Seed's water-containing cell culture soil: early fertilizer type). After water was poured to thoroughly soak the net with soil, a simple soil acidity meter and soil moisture meter (Fujiwara Sangyo Co., Ltd.) were used to keep the moisture content in the soil constant at a moisture level of 4 to 7, and the weight change over time of decomposition was measured. During the test period, the temperature of the culture soil was 25 to 35°C, and the pH was 6 to 7. Before burial, the samples were dried at 60°C for 12 hours and weighed (W3). After 2 weeks and 4 weeks of burial, samples (n=2) were collected, thoroughly washed with running water, dried at 120°C for 1.5 hours, and weighed (W4). The weight loss rate of the nonwoven fabric was calculated using the following formula. Weight reduction rate (%)=(W3-W4) / W3×100 In the above formula, W3 is the dry weight of the sample before being buried in the soil, and W4 is the dry weight of the sample after being buried in the soil for a certain period of time. And it was evaluated according to the following criteria. ○: Weight decreased due to decomposition. ×: No weight loss. The results are shown in Table 1 below.

[0083] [Table 1]

[0084] As shown in Table 1, the nonwoven fabrics of Examples 1 to 7, which are within the scope of the present invention, were rated as good or better for feel and texture, and ◯ for soil decomposition. Therefore, it is seen that the present invention can provide a nonwoven fabric that is excellent in touch, texture and biodegradability.

[0085] Furthermore, in Examples 2 and 3, in which a load was applied when the fibers were thermally bonded, the texture of the nonwoven fabric was even better than in Example 1, in which no load was applied when the fibers were thermally bonded, even though the HH ratios were similar. Furthermore, in Example 5, in which a load was applied to the web by a heat press when the fibers were thermally bonded, the texture of the nonwoven fabric was even better than in Example 4, in which the HH ratio was similar but a load was applied with a smaller pressure than in Example 5 when the fibers were thermally bonded. Therefore, it can be seen that by applying a large pressure when thermally bonding the fibers, the surfaces of the fibers come into firmer contact, and when heat is applied and the fibers develop adhesive properties, the fibers are firmly bonded to each other, resulting in an even better texture of the nonwoven fabric.

Claims

1. At least poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based short fibers are included, The poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based staple fibers have a fiber length of 11 to 160 mm and are crimped.

2. The poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based staple fiber is contained in an amount of 20% by weight or more and 80% by weight or less, 2. The biodegradable thermally bonded nonwoven fabric according to claim 1, comprising 20% ​​by weight or more and 80% by weight or less of biodegradable polysaccharide-based short fibers containing at least one kind of biodegradable polysaccharide.

3. The poly(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based staple fiber has a lower limit temperature of a crystal melting peak range measured by differential scanning calorimetry (DSC) of 40° C. or higher; 3. The biodegradable thermally bonded nonwoven fabric according to claim 1 or 2, wherein the upper limit of the crystalline melting peak range is 180°C or lower.

4. 3. The biodegradable thermally bonded nonwoven fabric according to claim 1, wherein the poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) staple fiber has a crimp number of 5 to 25 crimps / 25 mm.

5. 3. The biodegradable thermobonded nonwoven fabric according to claim 1, wherein the poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) staple fiber has a single fiber fineness of 0.1 to 100 dtex.

6. 3. The biodegradable thermobonded nonwoven fabric according to claim 1 or 2, wherein the biodegradable polysaccharide is a polysaccharide from the cellulose group.

7. A method for producing the biodegradable thermobonded nonwoven fabric according to claim 1 or 2, comprising the steps of: preheating poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) based drawn filaments; crimping the preheated poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) based drawn filaments using a stuffing box; a step of cutting the crimped poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based drawn filaments to a predetermined fiber length to obtain poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based short fibers; and heat-bonding the fibers containing the poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)-based staple fibers at a temperature of 40° C. to 180° C.

8. The method for producing a biodegradable thermally bonded nonwoven fabric according to claim 7, wherein the poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) based drawn filaments have a single fiber tensile strength of 0.5 to 10 cN / dtex.

Citation Information

Patent Citations

  • Biodegradable short fiber non-woven fabric

    JP1994200457A

  • Biodegradable staple fiber nonwoven fabric and its production

    JP1997013255A