Stretched film
A stretched film with specific crystalline polyolefin and biomass plastic composition addresses transparency and gloss issues, enabling direct pattern printing without white solid printing and improving printability.
Patent Information
- Application Number
- JP2023048138
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Conventional resin films are highly transparent, requiring a white solid printing process before pattern printing, and films using biomass plastics suffer from low surface gloss leading to missing dots during gravure printing.
A stretched film composed of a crystalline polyolefin resin with a melting point of 135°C to 175°C and a biomass plastic, with opacity between 20% and 90% and glossiness of 15% or more, eliminating the need for white solid printing and enhancing printability.
The film achieves suppressed transparency and high gloss, ensuring excellent printability without missing dots, particularly during gravure printing.
Smart Images

Figure 2024136853000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a stretched film. [Background technology]
[0002] Resin films are excellent in various properties such as moisture resistance, water resistance, and oil resistance, as well as good mechanical strength, and therefore are widely used in a variety of applications, such as packaging materials for foods and medicines, and protective films for displays, making them highly valuable functional materials.
[0003] On the other hand, in recent years, various problems have been raised, such as the increase in the amount of discarded plastic materials and concerns about global warming caused by carbon dioxide generated during the incineration of plastic materials. For this reason, biodegradable biomass plastics have attracted much attention from the perspective of consideration for the global environment and the human body, and the development of various materials that combine conventional plastic materials with biomass plastics has been actively pursued (for example, see Patent Documents 1 and 2, etc.). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2008 / 23758 [Patent Document 2] Special Publication No. 2017-519863 Summary of the Invention [Problem to be solved by the invention]
[0005] Conventional resin films have a high degree of transparency, so that when a desired pattern is printed on the resin film, a solid white print is first performed, and then the desired pattern is printed on top of the solid white print. In order to omit the solid white print process, a translucent resin film with low transparency is desired.
[0006] In addition, in films using biomass plastics, the surface gloss is low due to the poor smoothness of the surface protective layer, and there is a problem that the printing surface is prone to the occurrence of so-called missing dots, which are areas where printing is not possible, particularly during gravure printing. For this reason, there is a demand for the development of a resin film that uses biomass plastics and has excellent printability.
[0007] An object of the present invention is to provide a stretched film that has reduced transparency and high gloss and is therefore excellent in printability. [Means for solving the problem]
[0008] As a result of extensive research into achieving the above-mentioned objective, the inventors discovered that the above-mentioned objective could be achieved by a stretched film containing a crystalline polyolefin resin having a specific melting point and a biomass plastic, wherein the content of the biomass plastic in the stretched film is within a specific range, and the opacity and glossiness are within specific ranges, and thus completed the present invention.
[0009] That is, the present invention relates to the following stretched film. 1. A stretched film having a layer a containing a resin component containing a crystalline thermoplastic resin A and a crystalline thermoplastic resin B, The crystalline thermoplastic resin A is a crystalline polyolefin resin having a melting point of 135°C to 175°C, The crystalline thermoplastic resin B is a biomass plastic, The content of the biomass plastic is 0.5 to 50% by mass, with the stretched film being 100% by mass, The opacity of the stretched film measured by the following measurement method is 20% or more and 90% or less, The gloss of the laminate measured at a measurement angle of 20° according to a measurement method in accordance with JIS Z8741 is 15% or more. A stretched film characterized by: (Method of measuring opacity) The total light transmittance of the stretched film is measured by a measurement method in accordance with JIS K7361-1, and the opacity is calculated according to the following formula. [Opacity (%)]=100-Total light transmittance (%) 2. The stretched film according to item 1, comprising a layer b on one or both sides of the layer a, the layer b not containing a biomass plastic. 3. The stretched film according to item 1 or 2, wherein the biomass plastic comprises starch. 4. The stretched film according to any one of items 1 to 3, wherein the biomass plastic contains at least starch and polylactic acid, and the starch content is 5 to 90% by mass, with the biomass plastic being 100% by mass. Effect of the Invention
[0010] The stretched film of the present invention has suppressed transparency and high gloss, and therefore has excellent printability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, embodiments of the present invention will be described in detail. In this specification, the expressions "containing" and "comprise" include the concepts of "containing", "comprises", "consists essentially of" and "consists only of".
[0012] The stretched film of the present invention is a stretched film having a layer a containing a resin component containing a crystalline thermoplastic resin A and a crystalline thermoplastic resin B, the crystalline thermoplastic resin A is a crystalline polyolefin resin having a melting point of 135°C to 175°C, the crystalline thermoplastic resin B is a biomass plastic, the content of the biomass plastic is 0.5 to 50% by mass based on 100% by mass of the stretched film, the opacity of the laminate measured by a measuring method conforming to JIS K7361-1 is 20% to 90% and the gloss of the laminate measured by a measuring method conforming to JIS Z8741 under a measuring angle of 20° is 15% or more. The stretched film of the present invention has a layer a containing a resin component containing a crystalline thermoplastic resin A and a crystalline thermoplastic resin B, contains a specific amount of the biomass plastic which is the crystalline thermoplastic resin B, and has an opacity of 20% to 90%, so that the film is white and has suppressed transparency. In addition, the stretched film of the present invention contains crystalline thermoplastic resin A having a melting point in a specific range, and has a glossiness of 15% or more measured at a measurement angle of 20°, thereby providing high glossiness and excellent printability. Therefore, with the stretched film of the present invention, the step of solid white printing can be omitted when printing a desired pattern on a resin film, and missing dots on the printed surface can be suppressed even when biomass plastic is used.
[0013] [Layer a] The stretched film of the present invention has at least a layer a. The layer a is a layer that serves as a core layer in the stretched film. The layer a contains a resin component containing a crystalline thermoplastic resin A and a crystalline thermoplastic resin B. Each component contained in the resin component will be described below.
[0014] (Crystalline thermoplastic resin A) The crystalline thermoplastic resin A is a crystalline polyolefin resin, and the type is not particularly limited as long as the melting point is 135°C to 175°C. In this specification, the crystalline thermoplastic resin refers to a thermoplastic resin that has a clear melting peak in the DSC curve when the resin is heated from -40°C to 300°C at a rate of 20°C / min under nitrogen flow using a differential scanning calorimeter (e.g., Perkin-Elmer's input compensation type DSC, Diamond DSC), held at 300°C for 5 minutes, cooled to -40°C at 20°C / min, held at -40°C for 5 minutes, and then heated again to 300°C at 20°C / min. On the other hand, the amorphous thermoplastic resin refers to a thermoplastic resin that does not have a clear melting peak in the above measurement using DSC.
[0015] In the present invention, a crystalline polyolefin resin is used as the crystalline thermoplastic resin A. As the crystalline polyolefin resin, a wide variety of known crystalline polyolefin resins can be used. As the crystalline polyolefin resin, for example, a polymer obtained by polymerizing an olefin, preferably a polymer obtained by polymerizing an olefin having 2 to 20 carbon atoms, more preferably a polymer having 2 to 10 carbon atoms, and even more preferably a polymer obtained by polymerizing an olefin having 3 to 6 carbon atoms, can be mentioned. Specifically, as the crystalline polyolefin resin, a crystalline polyethylene resin, a polypropylene resin, a poly(1-butene) resin, a polyisobutene resin, a poly(1-pentene) resin, and a poly(4-methylpentene-1) resin can be mentioned. The crystalline polyolefin resin is preferably a crystalline polypropylene resin in that it is easily mixed (compatible) with the biomass plastic. The crystalline polyolefin resin can be one type alone or a mixture of two or more types.
[0016] When the crystalline thermoplastic resin A is a crystalline polypropylene-based resin, the crystalline polypropylene-based resin is more preferably at least one selected from the group consisting of a propylene homopolymer and a propylene-ethylene copolymer. When the crystalline polyolefin-based resin is a crystalline propylene homopolymer, the mechanical strength and heat resistance of the film are likely to be improved, and when the crystalline polyolefin-based resin is a crystalline propylene-ethylene copolymer, the fold crack resistance at low temperatures is likely to be improved.
[0017] In addition, when the crystalline polyolefin resin contains two components, a crystalline propylene homopolymer and a crystalline propylene-ethylene copolymer, a film having excellent heat resistance and low-temperature fold crack resistance is easily obtained. The preferred mass ratio of the crystalline propylene homopolymer and the crystalline propylene-ethylene copolymer is crystalline propylene homopolymer (P1):crystalline propylene-ethylene copolymer (P2)=70:30-99:1, more preferably P1:P2=75:25-98:2, and even more preferably P1:P2=78:22-97:3.
[0018] As the crystalline propylene homopolymer, a crystalline isotactic polypropylene resin is preferred. Such a crystalline isotactic polypropylene resin preferably has a mesopentad fraction ([mmmm]), which is a degree of stereoregularity determined by high-temperature nuclear magnetic resonance (NMR) measurement, of 92% to 98%, more preferably 93% to 97%. When the mesopentad fraction [mmmm] is 92% or more, the crystallinity of the resin is improved due to the high stereoregularity component, and high thermal stability and mechanical strength are easily obtained. On the other hand, when the mesopentad fraction [mmmm] is 98% or less, the stretchability is easily improved.
[0019] There is no particular limitation on the high-temperature NMR device that can be used to measure the mesopentad fraction ([mmmm]). For example, a commercially available high-temperature nuclear magnetic resonance (NMR) device capable of measuring the stereoregularity of polyolefins can be used. An example of the device is the high-temperature Fourier transform nuclear magnetic resonance (high-temperature FT-NMR) JNM-ECP500 manufactured by JEOL Ltd. 13 The frequency is 125 C (125 MHz), the measurement temperature is 135°C, and the solvent used is ortho-dichlorobenzene (ODCB: a mixed solvent of ODCB and deuterated ODCB (volume ratio = 4 / 1)). The high-temperature NMR method can be performed by a known method, for example, the method described in "Japan Analytical Chemistry - Polymer Analysis Research Forum, ed., New Edition Polymer Analysis Handbook, Kinokuniya Shoten, 1995, p. 610". The measurement mode is single pulse proton broadband decoupling, pulse width 9.1 μsec (45° pulse), pulse interval 5.5 sec, number of accumulations 4500, and shift standard CH3 (mmmm) = 21.7 ppm.
[0020] The pentad fraction, which indicates the degree of stereoregularity, is calculated as a percentage from the integral intensity of each signal derived from a combination of five pentads (pentads) consisting of meso (m) pentads arranged in the same direction and racemo (r) pentads arranged in the opposite direction (mmmm, mrrm, etc.). For the assignment of each signal derived from mmmm, mrrm, etc., see, for example, the description of spectra in "T. Hayashi et al., Polymer, Vol. 29, p. 138 (1988)". The meso pentad fraction ([mmmm]) can be controlled by appropriately adjusting the polymerization conditions of the polypropylene resin, the type of catalyst, the amount of catalyst, and other polymerization conditions.
[0021] The crystalline thermoplastic resin A has a melting point of 135° C. to 175° C. If the melting point of the crystalline thermoplastic resin A is less than 135° C., the heat resistance of the resulting stretched film may decrease, the productivity of the stretched film may decrease, and the desired stretchability may not be obtained. If the melting point of the crystalline thermoplastic resin A is more than 175° C., it becomes difficult for the crystalline thermoplastic resin A and the crystalline thermoplastic resin B to be compatible with each other, and the desired stretchability may not be obtained.
[0022] The melting point of the crystalline thermoplastic resin A is preferably 138° C. to 170° C., more preferably 140° C. to 166° C., still more preferably 145° C. to 164° C., and particularly preferably 150° C. to 163° C. This improves the productivity of the stretched film and the heat resistance of the resulting film.
[0023] The glass transition temperature of the crystalline thermoplastic resin A is not particularly limited and can be, for example, 50°C or lower, more preferably -30°C to 30°C.
[0024] In the present invention, the melting point and glass transition temperature of the crystalline resin A are values measured using a differential scanning calorimeter (for example, input compensation type DSC, Diamond DSC manufactured by Perkin-Elmer).
[0025] The melt mass flow rate of the crystalline thermoplastic resin A is not particularly limited. The melt mass flow rate of the crystalline thermoplastic resin A is preferably 0.5 g / 10 min to 8 g / 10 min, more preferably 1 g / 10 min to 6 g / 10 min, in order to ensure that the fluidity of the resin is within an appropriate range, and the size of the fine dispersion is easily controlled, making it easy to produce a desired stretched film. The melt mass flow rate referred to in this specification refers to a value measured at 230°C and 21.18 N in accordance with JIS K-7210 (1999).
[0026] The crystalline thermoplastic resin A can be produced by a known method. For example, when the crystalline thermoplastic resin A is a crystalline propylene homopolymer, it can be produced by a method of polymerizing propylene in a hydrocarbon solvent, a method of polymerizing in liquid propylene (bulk polymerization), a method of polymerizing in a gas phase, etc., using a Ziegler catalyst system consisting of titanium and aluminum compounds. The crystalline propylene homopolymer can be obtained from commercial products, etc., and representative commercial products include, for example, homopolymers of the Prime Polypro (registered trademark) series manufactured by Prime Polymer Co., Ltd., PC412A manufactured by Sunallomer Co., Ltd., homopolymers of the Novatec (registered trademark) series manufactured by Japan Polypropylene Corporation, Daploy series manufactured by Borealis, 5014L series manufactured by Taihan Petrochemical Co., Ltd., and homopolymers of the Sumitomo Noblen (registered trademark) series manufactured by Sumitomo Chemical Co., Ltd.
[0027] When the crystalline thermoplastic resin A is a crystalline propylene-ethylene copolymer, it may be either a random copolymer of propylene and ethylene or a block copolymer of propylene and ethylene. The content of ethylene units in the crystalline propylene-ethylene copolymer may be 50% by mass or less. The crystalline propylene-ethylene copolymer may be produced by a known method or may be obtained from a commercial product. Representative commercial products include, for example, copolymers of the Prime Polypro (registered trademark) series manufactured by Prime Polymer Co., Ltd., copolymers of the Novatec PP (registered trademark) series and Wintech (registered trademark) series manufactured by Japan Polypropylene Corporation, and copolymers of the Sumitomo Noblen (registered trademark) series manufactured by Sumitomo Chemical Co., Ltd.
[0028] The content of the crystalline thermoplastic resin A in the layer a is 100 mass% of the resin components forming the layer a. The layer a contains 30 to 96 mass% of the crystalline thermoplastic resin A with respect to the total mass of the crystalline thermoplastic resin A and the crystalline thermoplastic resin B. This makes the crystalline thermoplastic resin A and the crystalline thermoplastic resin B compatible, and allows a stretched film having a desired haze and stretch ratio to be obtained. In addition, by having the content of the crystalline thermoplastic resin A in the above range, a film having a desired transparency and excellent mechanical strength can be easily obtained.
[0029] The content of the crystalline thermoplastic resin A is preferably 40 to 99.5 mass%, more preferably 50 to 95 mass%, further preferably 50 to 90 mass%, and particularly preferably 60 to 80 mass%, based on 100 mass% of the resin components forming the layer a. By having the content of the crystalline thermoplastic resin A within the above range, the transparency of the stretched film is further suppressed and the glossiness is improved, thereby further improving the printability.
[0030] (Crystalline thermoplastic resin B) The type of the crystalline thermoplastic resin B is not particularly limited as long as it is a biomass plastic, and can be a wide variety of known biomass plastics. As such a crystalline thermoplastic resin B, for example, starch, cellophane, polylactic acid, polyethylene, polypropylene, nylon, polyethylene terephthalate, polyethylene terephthalate, cellulose, chitin, chitosan, gluten, gelatin, zein, soy protein, collagen, keratin, and other biomass-derived resins obtained from plants such as rice, corn, and sugar cane can be used. Among these, starch, cellophane, polylactic acid, polyethylene, polypropylene, nylon, polyethylene terephthalate, and cellulose are preferred, and starch is more preferred in that the transparency of the stretched film is more suppressed, and rice-derived starch is even more preferred in that the transparency of the stretched film is more suppressed and the stretched film can be white.
[0031] As the crystalline thermoplastic resin B, a biodegradable aliphatic polyester resin may also be used.
[0032] Examples of biodegradable aliphatic polyester resins include aliphatic polyester resins such as polylactic acid, polyhydroxyalkanoic acid (excluding polylactic acid), polyhydroxybutyrate, polycaprolactone, polybutylene succinate, polybutylene succinate / adipate, polyethylene succinate, polymalic acid, polyglycolic acid, polydioxanone, and poly(2-oxetanone).
[0033] The crystalline thermoplastic resin B may be used alone or in combination of two or more.
[0034] As the crystalline thermoplastic resin B, it is preferable to use the above-mentioned starch in combination with an aliphatic polyester. The aliphatic polyester is preferable because it is easily mixed uniformly with the above-mentioned crystalline thermoplastic resin A. As the aliphatic polyester, one or more selected from the group consisting of polylactic acid, polyhydroxyalkanoic acid, and polymers of mixed monomers containing lactic acid and polyhydroxyalkanoic acid are preferable, and polylactic acid is more preferable. In other words, it is more preferable that the biomass plastic used in the crystalline thermoplastic resin B contains starch and polylactic acid.
[0035] When the biomass plastic used in the crystalline thermoplastic resin B contains starch and polylactic acid, the content of the starch is preferably 5 to 90 mass%, more preferably 10 to 80 mass%, further preferably 20 to 70 mass%, and particularly preferably 30 to 60 mass%, based on 100 mass% of the biomass plastic. When the lower limit of the starch content is within the above range, the transparency of the stretched film is further suppressed, and the stretched film can exhibit a whiter color. When the lower limit of the starch content is within the above range, the gloss of the stretched film is improved, and the printability is further improved.
[0036] As the polylactic acid, a wide variety of known polylactic acids can be used, such as polylactic acid obtained by polycondensing lactic acid components as raw material monomers. The polylactic acid may contain only one of the optical isomers L-lactic acid (L-form) and D-lactic acid (D-form), or both.
[0037] Examples of polyhydroxyalkanoic acids include polymers of hydroxycarboxylic acid components including at least one of hydroxybutyric acid, hydroxyvaleric acid, hydroxypentanoic acid, hydroxycaproic acid, hydroxyheptanoic acid, and glycolic acid.
[0038] Examples of the polymer of a mixed monomer containing lactic acid and polyhydroxyalkanoic acid include a polymer obtained by polycondensation of a lactic acid monomer with the above-mentioned hydroxycarboxylic acid component.
[0039] The melting point of the crystalline thermoplastic resin B is preferably 110°C to 200°C, more preferably 120°C to 190°C, even more preferably 130°C to 185°C, and particularly preferably 140°C to 180°C. When the lower limit of the melting point of the crystalline thermoplastic resin B is within the above range, the heat resistance of the resulting stretched film is improved, and the productivity of the stretched film is further improved. When the upper limit of the melting point of the crystalline thermoplastic resin B is within the above range, the compatibility between the crystalline thermoplastic resin B and the crystalline thermoplastic resin A is further improved, the adjustment of the stretching ratio becomes easier, and the desired stretched film is more easily obtained.
[0040] The glass transition temperature of the crystalline thermoplastic resin B is not particularly limited and can be, for example, from -40°C to 70°C, and more preferably from 0°C to 70°C.
[0041] In the present invention, the melting point and glass transition temperature of the crystalline thermoplastic resin B are values measured using a differential scanning calorimeter (for example, a power compensation type DSC, Diamond DSC manufactured by Perkin-Elmer).
[0042] The melt mass flow rate of the crystalline thermoplastic resin B is not particularly limited. The melt mass flow rate of the crystalline thermoplastic resin B is preferably 0.5 g / 10 min to 15 g / 10 min, more preferably 1 g / 10 min to 10 g / 10 min, and even more preferably 2 g / 10 min to 10 g / 10 min, in order to ensure that the fluidity of the resin is within an appropriate range, and the size of the fine dispersion is easily controlled, making it easy to produce a desired stretched film. The melt mass flow rate referred to in this specification refers to a value measured at 230°C and 21.18 N in accordance with JIS K-7210 (1999).
[0043] The method for producing the crystalline thermoplastic resin B is not particularly limited, and for example, a method for producing a known biomass plastic can be widely adopted. The crystalline thermoplastic resin B can also be obtained from commercial products. Representative commercial products of polylactic acid include "4032D" (melting point 163°C) manufactured by NatureWorks, "L175" (melting point 175°C), "LX175" (melting point 155°C), and "LX930" (melting point 130°C) manufactured by Total Corbion. Other representative commercial products of the crystalline thermoplastic resin B include polyhydroxyalkanoate "ENMAT (registered trademark) Y1000P" manufactured by Tianan Biologic Material, polybutylene succinate "BioPBS (registered trademark) FZ91" and "BioPBS (registered trademark) FD82" manufactured by Mitsubishi Chemical Corporation.
[0044] The content of the biomass plastic, which is the crystalline thermoplastic resin B, is 0.5 to 50% by mass, with the weight of the entire stretched film being 100% by mass. If the lower limit of the biomass plastic content is less than 0.5% by mass, the transparency of the stretched film cannot be obtained. If the upper limit of the biomass plastic content exceeds 50% by mass, the glossiness decreases and the printability decreases. The content of the biomass plastic is preferably 5 to 40% by mass, and more preferably 10 to 30% by mass.
[0045] (Other resins) The resin components constituting the layer a may consist only of the crystalline thermoplastic resin A and the crystalline thermoplastic resin B. However, in this case, components inevitably contained in the resin components are not excluded. Furthermore, the resin components constituting the layer a may contain resins other than the crystalline thermoplastic resin A and the crystalline thermoplastic resin B, as long as the effects of the present invention are not impaired.
[0046] Examples of resins other than the crystalline thermoplastic resin A and the crystalline thermoplastic resin B include styrene-based resins, vinyl-based resins, polyester-based resins, polyurethane-based resins, nylon-based resins, and copolymers thereof, for example, vinyl monomer-diene monomer copolymers such as styrene-butadiene copolymers, and vinyl monomer-diene monomer-vinyl monomer copolymers such as styrene-butadiene-styrene copolymers.
[0047] The content of the other resin is preferably 15% by mass or less, and more preferably 10% by mass or less, based on 100% by mass of the total mass of the resin components contained in the layer a. The lower limit of the content of the other resin is not particularly limited, and is, for example, 0% by mass or 1% by mass.
[0048] [layer b] The stretched film of the present invention may have a single-layer structure having only layer a (i.e., a core layer), or may have a so-called laminated structure having layers other than layer a. Layer b can serve as a so-called skin layer, which makes the surface of the stretched film smoother and can further improve the glossiness and printability of the stretched film.
[0049] When the stretched film of the present invention has a laminated structure, for example, it may be a laminate obtained by laminating another layer to one or both sides of layer a. An example of such another layer is layer b, which is made of a resin and does not contain biomass plastics. That is, the layer structure of the stretched film of the present invention may be a layer structure in which layer b is provided on one or both sides of layer a, and layer b does not contain biomass plastics.
[0050] The resin contained in the layer b may be, for example, a crystalline polyolefin resin C having a melting point of 100 to 175°C.
[0051] The crystalline polyolefin resin C having a melting point of 100 to 175°C is, for example, a polymer obtained by polymerizing an olefin, similar to the crystalline thermoplastic resin A, and preferably includes a polymer obtained by polymerizing an olefin having 2 to 20 carbon atoms, more preferably 2 to 10 carbon atoms, and even more preferably 3 to 6 carbon atoms. Specifically, the crystalline polyolefin resin includes crystalline polyethylene resin, polypropylene resin, poly(1-butene) resin, polyisobutene resin, poly(1-pentene) resin, and poly(4-methylpentene-1) resin, as well as α-olefin copolymers such as ethylene-propylene copolymer, propylene-butene copolymer, ethylene-butene copolymer, and propylene-ethylene-butene copolymer. The crystalline polyolefin resin C can be one type alone or a mixture of two or more types. The crystalline polyolefin resin C contained in the layer b may be the same as the crystalline thermoplastic resin A contained in the layer a.
[0052] The resin contained in layer b may be only crystalline thermoplastic resin C. Alternatively, the resin contained in layer b may contain, in addition to crystalline thermoplastic resin C, one or more selected from the group consisting of crystalline thermoplastic resin A and crystalline thermoplastic resin B. Furthermore, the resin contained in layer b may contain the other resins described above. In other words, the resin contained in layer b essentially contains crystalline thermoplastic resin C, and may further contain at least one selected from the group consisting of crystalline thermoplastic resin A, crystalline thermoplastic resin B, and the other resins.
[0053] In order to further improve the glossiness of the stretched film, the resin contained in Layer b is preferably only the crystalline thermoplastic resin C. When Layer b contains a resin other than the crystalline thermoplastic resin C, the content of the crystalline thermoplastic resin C relative to the total mass of Layer b is 80 mass% or more, preferably 90 mass% or more, more preferably 95 mass% or more, and even more preferably 99 mass% or more.
[0054] When the stretched film of the present invention includes layer b, layer b may be laminated by being directly bonded to layer a, or another layer may be interposed between layer a and layer b. Since the haze of the stretched film can be reduced, it is preferable that layer b is laminated by being directly bonded to layer a.
[0055] When layers b are formed on both sides of layer a, the layers b may be formed of the same component or may be formed of different components.
[0056] [layer c] The stretched film of the present invention may further have a layer c other than the layer b, so long as the effects of the present invention are not impaired. Examples of the layer c include a layer having one or more of various functions such as antifogging properties, antistatic properties, adhesive properties, smoothness, glossiness, printability, blocking resistance, slipping properties, strength imparting properties, gas barrier properties against oxygen gas, ethylene gas, etc., water vapor barrier properties, odor component barrier properties, prevention of component migration of packaged contents, antibacterial properties, antifungal properties, etc., and a layer having one or more of these various functions and heat sealability.
[0057] The layer c may be laminated by being directly attached to the layer a, or another layer (for example, the layer b) may be interposed between the layer a and the layer c. When the layer c is formed on both sides of the layer a, the layers c may be formed of the same component or may be formed of different components.
[0058] As described above, the stretched film of the present invention may have at least one layer selected from the group consisting of layer b and layer c laminated thereon as necessary, with layer a as the core layer. More specifically, the stretched film of the present invention may include a laminate (i.e., b / a / b) in which layer a is the core layer and layer b is directly laminated to one or both sides of the core layer. The stretched film of the present invention may also include a laminate (i.e., b / a / c) in which layer a is the core layer and layer b is directly laminated to one side of the core layer, and layer c is laminated to the opposite side of the core layer. The stretched film of the present invention may also include a laminate (i.e., c / a / c) in which layer a is the core layer and layer c is directly laminated to both sides of the core layer. Furthermore, the stretched film of the present invention may include a laminate (i.e., a / c) in which layer a is the core layer and layer c is laminated to one side of the core layer.
[0059] The stretched film of the present invention is preferably a laminate in which layer a is used as a core layer and layer b is directly laminated to one or both sides of the core layer.
[0060] (Additives) The stretched film of the present invention may contain additives as optional components, if necessary. Examples of the additives include a wide variety of known additives that are applied to stretched films, such as heat stabilizers, antioxidants, organic and inorganic lubricants, chlorine scavengers, and antistatic agents.
[0061] Examples of the heat stabilizer and the antioxidant include phenol-based, hindered amine-based, phosphite-based, lactone-based, and tocopherol-based heat stabilizers and antioxidants. Specific examples include dibutyl hydroxytoluene, pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (BASF Japan Ltd., "Irganox (registered trademark) 1010"), 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxy)benzene (BASF Japan Ltd., "Irganox (registered trademark) 1330"), and tris(2,4-di-t-butylphenyl)phosphite (BASF Japan Ltd., "Irgafos (registered trademark) 168"), etc. Among these, at least one selected from phenol-based antioxidants or a combination thereof, a combination of a phenol-based antioxidant and a phosphite-based antioxidant, a combination of a phenol-based antioxidant and a lactone-based antioxidant, or a combination of a phenol-based antioxidant, a phosphite-based antioxidant and a lactone-based antioxidant are preferred from the viewpoint of imparting chemical stability to the stretched film.
[0062] Examples of lubricants include organic lubricants such as aliphatic amides such as stearic acid amide and erucic acid amide, lauric acid diethanolamide, alkyldiethanolamine, aliphatic monoglycerides, aliphatic diglycerides, and silicone crosslinked polymers, and inorganic lubricants such as silica and alumina. However, organic lubricants that cause less staining on printing plates in printing applications are preferred.
[0063] Examples of chlorine scavengers include calcium stearate, metal soaps, and hydrotalcite.
[0064] Examples of antistatic agents include alkylmethyl dibetaine, alkylamine diethanol and / or alkylamine ethanol ester and / or alkylamine diethanol diester. Two or more of these antistatic agents may be used in combination, and aliphatic alcohol may also be used in combination. Among these, the combined use of stearyl diethanolamine monostearate and stearyl diethanolamine is preferred because it provides excellent antistatic performance and improves printability. Representative examples of commercially available antistatic agents include the Electrostripper (registered trademark) series manufactured by Kao Corporation.
[0065] The additive may be contained in layer a, or when the stretched film of the present invention has layers other than layer a (such as layers b and c), the other layers may contain the additive. The content of the additive can be adjusted arbitrarily to the extent that the effects of the present invention are not impaired, and can be, for example, 1% by mass or less based on the total mass of the stretched film, preferably 0.5% by mass or less, more preferably 0.1% by mass or less, and even more preferably 0.01% by mass or less.
[0066] The thickness of the stretched film of the present invention is not particularly limited and can be appropriately set depending on the intended use. The thickness of the stretched film is, for example, preferably 10 to 150 μm, more preferably 15 to 100 μm, and further preferably 15 to 60 μm.
[0067] [Characteristics of stretched film] The stretched film of the present invention has an opacity of 20% or more and 90% or less. If the opacity is less than 20%, the process of solid white printing cannot be omitted when printing a desired pattern, and the process is complicated. If the opacity exceeds 90%, the content of biomass plastic needs to be increased, and the glossiness decreases and the printability decreases. The lower limit of the opacity is preferably 30% or more, and more preferably 40% or more. The upper limit of the opacity is preferably 80% or less, and more preferably 70% or less.
[0068] The opacity of the stretched film can be measured by the following method. (Method of measuring opacity) The total light transmittance of the stretched film is measured by a measurement method in accordance with JIS K7361-1, and the opacity is calculated according to the following formula. [Opacity (%)]=100-Total light transmittance (%)
[0069] [Characteristics of stretched film] The stretched film of the present invention has an opacity of 20% or more and 90% or less, measured by a measurement method in accordance with JIS K7361-1. If the opacity is less than 20%, the process of solid white printing cannot be omitted when printing a desired pattern, and the process is complicated. If the opacity exceeds 90%, the content of biomass plastic needs to be increased, and the glossiness decreases, resulting in a decrease in printability. The lower limit of the opacity is preferably 30% or more, and more preferably 40% or more. The upper limit of the opacity is preferably 80% or less, and more preferably 70% or less.
[0070] The stretched film of the present invention has a glossiness of 15% or more, measured at a measurement angle of 20° according to a measurement method in accordance with JIS Z8741. If the glossiness is less than 15%, the printability of the stretched film decreases. The lower limit of the glossiness is preferably 20% or more, more preferably 30% or more. The upper and lower limits of the glossiness are not particularly limited, and may be 100%, 90%, etc.
[0071] The stretched film of the present invention can be suitably used for packaging, food packaging, pharmaceutical packaging, decoration (including fashion), labels, tape substrates, printing substrates, stationery, home appliances, poster paper, thermal paper substrates, recording paper substrates, interior and exterior use of homes, automobiles, and the like.
[0072] [Manufacturing method of stretched film] The method for producing the stretched film of the present invention is not particularly limited, and for example, known production methods can be widely adopted. For example, the stretched film of the present invention can be produced by extruding a resin raw material containing at least the crystalline thermoplastic resin A and the crystalline thermoplastic resin B to obtain a resin sheet, and stretching the resin sheet. This production method is abbreviated as "production method A".
[0073] The resin raw material used in manufacturing method A may contain other resins as required. Furthermore, the resin raw material used in manufacturing method A may contain additives as required. The content ratio of each component in the resin raw material is the same as the content ratio of each resin in the resin component contained in layer a described above.
[0074] The resin raw material can be prepared by, for example, the same method as known preparation methods, and examples thereof include a method of dry blending resin pellets, powder, etc. using a batch mixer such as a tumbler or mixer, or a continuous metering mixer; or a method of supplying resin pellets, powder, etc., together with other resin pellets, powder, and / or additives as necessary, to a kneader and melt-kneading to obtain a melt blend resin composition; etc. Among these, it is preferable to prepare the resin raw material by melt-kneading, and in this case, the crystalline thermoplastic resin A and the crystalline thermoplastic resin B are easily mixed uniformly, and a stretched film with high gloss and excellent printability is easily obtained.
[0075] As the kneader used for melt kneading, a known kneader can be used, and a single screw type, a twin screw type, or a multi-screw type having more than two screws can be used, and further, in the case of a screw type having two or more screws, either a co-rotating or counter-rotating kneading type can be used. A co-rotating twin screw type kneader is preferred because the crystalline thermoplastic resin A and the crystalline thermoplastic resin B are easily mixed uniformly.
[0076] The kneading temperature of the melt kneading is preferably 140 to 270°C, more preferably 160 to 240°C. By setting the temperature within the above range, the crystalline thermoplastic resin A and the crystalline thermoplastic resin B can be mixed more uniformly. In order to prevent deterioration of the resin during melt kneading, an inert gas such as nitrogen can be purged. The melt-kneaded resin can be pelletized to an appropriate size using a commonly known granulator to obtain melt blend resin composition pellets.
[0077] In the manufacturing method A, a resin sheet can be obtained using the resin raw material obtained as described above. Specifically, the resin raw material is fed to an extruder, heated and melted, and, if necessary, fine foreign matter and the like is removed using a filter or the like, and then the melt is extruded into a sheet shape from a T-die, thereby obtaining a resin sheet.
[0078] The extruder used to obtain the resin sheet can be, for example, a wide variety of known extruders. There is no limitation on the screw type of the extruder, and a single screw type, a twin screw type, or a multi-screw type having more than one screw may be used. When the resin raw material is prepared by the dry blending, the use of a twin screw type or a multi-screw type having more than one screw tends to provide excellent mixing and dispersibility. The extrusion temperature is preferably 140 to 270°C, more preferably 160 to 240°C. In order to prevent thermal deterioration of the resin during extrusion, an inert gas such as nitrogen can be purged.
[0079] The melt-extruded resin sheet is molded into a sheet shape by a known method, for example, by adhering the sheet to at least one metal drum set at a temperature of 20 to 80° C. using an air knife or other rolls, or by static electricity, and the resin sheet is obtained as a so-called raw sheet. The temperature of the metal drum is more preferably 30 to 80° C.
[0080] The manufacturing method A may further include, for example, a lamination step, which allows a resin sheet having a laminated structure to be obtained. For example, when a stretched film having the layer b formed on one or both sides of the layer a is to be obtained, the manufacturing method A may include a lamination step.
[0081] In the lamination step, for example, a wide variety of lamination methods that have been conventionally employed can be used, and examples thereof include films obtained by laminating using a coextrusion method, a lamination method, or the like.
[0082] Specifically, when producing a stretched film having a laminated structure, two or more dry blend and / or melt blend resin compositions (each resin composition may have a different or the same composition) are co-extruded to obtain a resin sheet having a laminated structure, and the resin sheet having such a laminated structure can be stretched. Alternatively, a stretched film having a laminated structure can be produced by laminating a monolayer stretched film with another film. In addition, a stretched film having a laminated structure can be produced by stretching a multilayer non-stretched film (each layer may have a different or the same composition of the resin composition constituting each layer) obtained by laminating two or more layers of non-stretched films extruded as monolayers together.
[0083] Examples of the coextrusion method include a pre-die lamination method in which molten resins are brought into contact in a feed block before a die, an in-die lamination method in which they are brought into contact along a path inside a die, such as a multi-manifold die, and an out-die lamination method in which they are discharged from multiple concentric lips and brought into contact, etc. For example, in the case of the in-die lamination method, a multi-layer die such as a three-layer multi-manifold die can be used to form a three-layer structure of layer b / layer a / layer b, consisting of a surface layer (skin layer: layer b) and a core layer (middle layer: layer a).
[0084] Examples of the lamination method include an extrusion lamination method in which a film of molten resin is directly extruded onto another film using equipment for the melt extrusion molding method used in the T-die method to form a laminated film.
[0085] Examples of heat sealing methods include an external heating method in which a heated metal body is pressed against multiple laminated films from the outside of the films and the conducted heat melts the films to bond them, and an internal heating method in which high-frequency radio waves or ultrasound are used to generate heat in the films and bond them.
[0086] In the manufacturing method A, the above lamination methods can be used alone or in combination.
[0087] As described above, when the manufacturing method A has a lamination step, the resin sheet can have a laminated structure, and when the manufacturing method A does not have a lamination step, the resin sheet has a single-layer structure. By performing the stretching described below using a resin sheet having a single-layer structure, a stretched film consisting of layer a can be obtained. When performing the stretching described below using a resin sheet having a single-layer structure, a multilayer stretched film having at least layer a can be obtained.
[0088] In the manufacturing method A, the resin sheet (raw sheet) having the above-mentioned single layer or laminate structure is stretched. As the stretching method, known methods such as stretching between rolls with a peripheral speed difference, a tenter method, a tubular method, etc. can be used. As the stretching direction, uniaxial stretching, biaxial stretching, biaxial stretching in an oblique direction, etc. are possible, and in the case of stretching in two or more axes, both sequential stretching and simultaneous stretching are applicable. Among these, the simultaneous biaxial stretching method by the tenter method, the sequential biaxial stretching method by the tenter method, and the sequential biaxial stretching method in which the longitudinal (flow, MD) stretching is performed between rolls with a peripheral speed difference and then the transverse (width, TD) stretching is performed by the tenter method are preferred from the viewpoint of easiness of obtaining the desired stretched film. Hereinafter, a method of obtaining the stretched film of the present invention by the sequential biaxial stretching method will be described, but it is not limited thereto.
[0089] In the sequential biaxial stretching method, it is preferable to adjust the stretching temperature and stretching ratio according to the melting point and glass transition temperature of the resin used. First, the resin sheet (raw sheet) is kept at a temperature of preferably 100 to 160°C, more preferably 120 to 150°C, and stretched in the longitudinal direction preferably 2 to 10 times, more preferably 2.5 to 8 times, even more preferably 3 to 6 times, and particularly preferably 4 to 5 times by passing between rolls with a difference in peripheral speed or by a tenter method. Subsequently, the stretched film is stretched in the transverse direction preferably 2 to 12 times, more preferably 4 to 11.5 times, even more preferably 6 to 11 times, and particularly preferably 8 to 10 times by a tenter method at a temperature of preferably 160°C or higher, and then relaxed, heat set, and wound up.
[0090] The wound film can be cut to a desired product width after being subjected to an aging treatment preferably in an atmosphere of about 20 to 45° C. In this manner, the stretched film of the present invention can be produced. EXAMPLES
[0091] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples. In addition, unless otherwise specified, "parts" and "%" respectively indicate "parts by mass" and "% by mass".
[0092] The resins used in the examples and comparative examples are as follows.
[0093] (Crystalline thermoplastic resin A) Resin A-1: SunAllomer (registered trademark) PC412A (SunAllomer Co., Ltd., polypropylene homopolymer, MFR = 3g / 10min, melting point 160°C) Resin A-1: Wintec (registered trademark) WFW5T polymer (manufactured by Japan Polypropylene Corporation, melting point 142°C)
[0094] (Crystalline thermoplastic resin B) Resin B-1: Starch Product name Rice Resin R50E-4 (Made by Minami-Uonuma Biomass Resin Co., Ltd., MFR=5g / 10min) Resin B-2: Luminy (registered trademark) LX175 (Total Corbion PLA, polylactic acid)
[0095] Example 1 As shown in Table 1, 99.5% by mass of resin A-1 pellets as crystalline thermoplastic resin A for forming layer a and 0.5% by mass of resin B-1 pellets as crystalline thermoplastic resin B (biomass plastic) for forming layer a were mixed and dry-blended in a mixer to prepare a resin raw material. The obtained resin raw material was fed from a hopper into an apparatus in which a twin-screw extruder (L / D=25) equipped with a strand die was connected to a Labo Plastomill (registered trademark) (Model 4C150) manufactured by Toyo Seiki Seisakusho Co., Ltd., and melt-kneaded at 230°C. The resin raw material was extruded in a strand shape, cooled with water, and cut into pellets with a strand cutter to obtain melt-blend resin composition pellets. The melt-blend resin composition pellets were fed from a hopper into a single-screw type extruder a, melted, and extruded from a single-layer die. The extruded resin layer was cooled and solidified while being pressed by air pressure using an air knife onto a cooling drum controlled at 45°C to obtain a raw sheet.
[0096] The obtained raw sheet was stretched using a Bruckner batch biaxial stretching machine KARO. The stretching method was a sequential biaxial stretching method in which the film was stretched in the longitudinal direction and then in the transverse direction. The film was preheated in an oven with a set temperature of 150°C until the film temperature (Ts) reached 135°C, and then stretched to 5 times in the longitudinal direction at a stretching speed of 6 times / second. Next, the film was preheated in an oven with a set temperature of 165°C until the film temperature reached 145°C, and stretched to 10 times in the transverse direction at a stretching speed of 1 time / second. Next, in the same oven, the film was relaxed to 9.5 times in the transverse direction at a relaxation speed of 0.5 times / second, and then heat-set for 10 seconds, and then removed from the oven and cooled to room temperature to prepare a stretched film with a thickness of 25 μm.
[0097] (Examples 2 to 6, Comparative Examples 1 and 2) A stretched film having a thickness of 25 μm was prepared in the same manner as in Example 1, except that the resin composition of crystalline thermoplastic resin A and crystalline thermoplastic resin B (biomass plastic) for forming layer a was changed as shown in Table 1.
[0098] (Evaluation method) The resins used in the examples and comparative examples and the stretched films prepared were evaluated as follows.
[0099] [Resin melting point, glass transition temperature] The melting point and glass transition temperature of the resins used in the examples and comparative examples were calculated using a Perkin-Elmer input compensation type DSC, Diamond DSC, according to the following procedure. 5 mg of each resin was weighed out, packed into an aluminum sample holder, and set in a DSC device. Under nitrogen flow, the temperature was raised from -40°C to 300°C at a rate of 20°C / min, held at 300°C for 5 minutes, cooled to -40°C at 20°C / min, and held at -40°C for 5 minutes. The melting point and glass transition temperature were obtained from the DSC curve when the temperature was raised again to 300°C at 20°C / min. The melting peak (the maximum melting peak when multiple melting peaks are shown) defined in 9.1(1) of JIS-K7121 was taken as the melting point, and the midpoint glass transition temperature defined in 9.3(1) of JIS-K7121 was taken as the glass transition temperature.
[0100] [Stretched film thickness] The thickness of the stretched film was measured using a micrometer (JIS B-7502) in accordance with JIS C-2151.
[0101] [Opacity of stretched film] The total light transmittance of the stretched film was measured by a measurement method in accordance with JIS K7361-1, and the opacity was calculated according to the following formula. [Opacity (%)]=100-Total light transmittance (%)
[0102] [Glossiness of stretched film] The gloss of the surface of the stretched film was measured in accordance with JIS Z8741 at a measurement angle of 20° using a variable angle glossmeter GM-3D manufactured by Murakami Color Research Laboratory Co., Ltd. The measurement was performed in both the longitudinal and transverse directions of the film, and the average value of both was used as the measured value.
[0103] [Suitability of stretched film for gravure printing] The stretched film was gravure printed using a printing bureau gravure printing tester, and the degree of missing dots in the 10% gradation halftone dot area was visually observed and evaluated according to the following evaluation criteria. Note that a rating of ○ or higher is considered to be satisfactory for practical use. .circle-solid.: No missing dots are observed. ◯: Almost no missing dots. △: A few missing dots are observed. ×: Approximately a dozen missing dots are observed.
[0104] The evaluation results are shown in Table 1.
[0105] [Table 1]
[0106] The results in Table 1 show that the stretched film obtained in the examples has layer a in which a crystalline polyolefin resin having a specific melting point and a biomass plastic having a specific melting point are formed in a specified ratio, and therefore has reduced transparency and high gloss, resulting in excellent printability.
Claims
1. A stretched film having a layer a containing a resin component containing a crystalline thermoplastic resin A and a crystalline thermoplastic resin B, The crystalline thermoplastic resin A is a crystalline polyolefin resin having a melting point of 135° C. to 175° C., The crystalline thermoplastic resin B is a biomass plastic, The content of the biomass plastic is 0.5 to 50% by mass, with the stretched film being 100% by mass, The opacity of the stretched film measured by the following measurement method is 20% or more and 90% or less, The gloss of the stretched film measured at a measurement angle of 20° according to a measurement method in accordance with JIS Z8741 is 15% or more. A stretched film characterized by: (Method of Measuring Opacity) The total light transmittance of the stretched film is measured by a measurement method in accordance with JIS K7361-1, and the opacity is calculated according to the following formula. [Opacity (%)] = 100 - Total light transmittance (%)
2. The stretched film according to claim 1 , further comprising a layer b on one or both sides of the layer a, the layer b not containing a biomass plastic.
3. The stretched film according to claim 1 or 2, wherein the biomass plastic comprises starch.
4. The stretched film according to claim 1 or 2, wherein the biomass plastic contains at least starch and polylactic acid, and the starch content is 5 to 90 mass% relative to 100 mass% of the biomass plastic.
Citation Information
Patent Citations
Polymeric blends and articles made therefrom
JP2017519863A
Thermoplastic resin composition and molded article obtained from the same
WO2008023758A1