Conductive composition
A conductive composition using polythiophene-based polymers with specific particle sizes and antioxidants forms a durable conductive layer, addressing the durability issues in antistatic films for automotive applications, ensuring stability under harsh conditions.
Patent Information
- Application Number
- JP2023048207
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Conductive compositions used in antistatic films for automotive applications lack sufficient durability, particularly under harsh conditions such as high temperatures and humidity, necessitating improved resistance and stability.
A conductive composition comprising a polythiophene-based conductive polymer with specific particle sizes (D50=200 to 800 nm, D90=250 to 1000 nm) and an antioxidant, optionally with a binder, to form a conductive layer with enhanced durability.
The conductive layer exhibits excellent durability, maintaining low surface resistivity and optical properties under extreme conditions, with resistance to heat, humidity, and UV exposure, suitable for antistatic films in automotive and electronic devices.
Smart Images

Figure 2024136903000001 
Figure 2024136903000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive composition, and more particularly to a conductive composition capable of forming a conductive layer having excellent durability. [Background technology]
[0002] Optical films and optical filters used in liquid crystal display devices and the like may be required to have antistatic properties in addition to optical properties. For example, in a liquid crystal display device, a polarizing plate is placed on a liquid crystal cell, and only light of a specific polarized component of light irradiated from a light source and transmitted through a liquid crystal layer is emitted as display light. Here, if the liquid crystal orientation becomes unstable due to disturbance of the electric field in the liquid crystal cell, this leads to a disturbance of the displayed image. In order to prevent disturbance of the electric field, the polarizing plate is required to have antistatic properties in addition to polarization properties. Also, antistatic films are used to protect electronic products from static electricity and dust. As these films having antistatic properties, conductive laminates in which a coating film containing a conductive polymer is formed on a substrate are used.
[0003] With the recent trend toward electrification of automobiles, the applications of antistatic films are expanding, such as their use as components of in-vehicle liquid crystal displays and electronic devices. These films are required to have higher durability in harsher environments (e.g., high-temperature environments) than has been required in the past. It is known that the incorporation of an antioxidant can suppress the change in resistance over time even when exposed to air (Patent Document 1). However, there is room for further improvement in durability for in-vehicle applications. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2010-196022 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a conductive composition capable of forming a conductive layer having excellent durability. [Means for solving the problem]
[0006] The present inventors have found that a conductive layer having excellent durability can be formed by using a conductive composition containing a polythiophene-based conductive polymer having a specific particle size and an antioxidant, and have completed the present invention.
[0007] That is, the present invention relates to a conductive composition comprising a polythiophene-based conductive polymer and an antioxidant, wherein the polythiophene-based conductive polymer has a cumulative particle size, as measured by a dynamic light scattering method, of D50=200 to 800 nm and D90=250 to 1000 nm.
[0008] It is preferable that the composition further contains a binder.
[0009] The binder is preferably a thermosetting resin.
[0010] The amount of the antioxidant is preferably 0.1 to 500 parts by weight based on 100 parts by weight of the solid content of the polythiophene-based conductive polymer.
[0011] The content of the polythiophene-based conductive polymer is preferably 0.1 to 20% by weight based on the total solid content.
[0012] When a film with a thickness of 100 to 350 nm is formed on a substrate, the surface resistivity is 1×10 6 ~1×10 10 It is preferable that:
[0013] The present invention also provides a conductive laminate including a substrate and a conductive layer including a polythiophene-based conductive polymer formed on the substrate, the conductive layer having a surface resistivity of 1×10 or less when formed to a thickness of 50 to 4000 nm. 6 ~1×10 10 and the conductive layer satisfies any one or more of the following (A) to (C): (A) (Surface resistivity after 1000 hours of exposure under conditions of temperature 85°C and relative humidity 85%) / (Surface resistivity immediately after film formation)≦500 (B) (Surface resistivity after 1000 hours of exposure at 105°C) / (Surface resistivity immediately after film formation)≦500 (C) (wavelength 405 nm, illuminance 250 W / m 2 (Surface resistivity after 1000 hours of exposure to light of 1000 nm) / (Surface resistivity immediately after film formation)≦1000
[0014] The conductive laminate is preferably an antistatic film. Effect of the Invention
[0015] The conductive composition of the present invention can form a conductive layer having excellent durability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] <<Conductive composition>> The conductive composition of the present invention comprises a polythiophene-based conductive polymer and an antioxidant, and is characterized in that the polythiophene-based conductive polymer has a cumulative particle size, as measured by a dynamic light scattering method, of D50=200 to 800 nm and D90=250 to 1000 nm.
[0017] <Polythiophene-based conductive polymer> The polythiophene-based conductive polymer is a conductive polymer containing at least one thiophene ring having excellent conductivity in the molecule. As the polythiophene-based conductive polymer, poly(3,4-disubstituted thiophene) is preferable, and poly(3,4-dialkoxythiophene) or poly(3,4-alkylenedioxythiophene) is particularly preferable. As the poly(3,4-dialkoxythiophene) or poly(3,4-alkylenedioxythiophene), the following formula (I):
[0018] [ka]
[0019] Preferred is a cationic form of polythiophene consisting of repeating structural units of the formula: 1 and R 2 are each independently a hydrogen atom or C 1-4 or R 1 and R 2 When C is bonded 1-4 C represents an alkylene group. 1-4 The alkyl group of R is not particularly limited, but examples thereof include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a t-butyl group. 1 and R 2 If C is bonded 1-4 The alkylene group in is not particularly limited, but examples thereof include a methylene group, a 1,2-ethylene group, a 1,3-propylene group, a 1,4-butylene group, a 1-methyl-1,2-ethylene group, a 1-ethyl-1,2-ethylene group, a 1-methyl-1,3-propylene group, and a 2-methyl-1,3-propylene group. Among these, a methylene group, a 1,2-ethylene group, and a 1,3-propylene group are preferred, and a 1,2-ethylene group is more preferred. 1-4 and C 1-4 The alkylene group may have some of its hydrogen atoms substituted. 1-4 As the polythiophene having an alkylene group, poly(3,4-ethylenedioxythiophene) is particularly preferred.
[0020] The polythiophene-based conductive polymer may be a complex with a dopant. As the dopant, it is preferable to use a polyanion in terms of conductivity, chemical stability, and excellent productivity because a conductive layer can be formed at a low temperature in a short time. The polyanion forms a complex by forming an ion pair with the polythiophene ring, and the polythiophene ring can be stably dispersed in water. The polyanion is not particularly limited, but examples thereof include carboxylic acid polymers (e.g., polyacrylic acid, polymaleic acid, polymethacrylic acid, etc.), sulfonic acid polymers (e.g., polystyrene sulfonic acid, polyvinyl sulfonic acid, polyisoprene sulfonic acid, etc.), etc. These carboxylic acid polymers and sulfonic acid polymers may also be copolymers of vinyl carboxylic acids and vinyl sulfonic acids with other polymerizable monomers, such as acrylates, styrene, vinyl naphthalene, and other aromatic vinyl compounds. Among these, polystyrene sulfonic acid is particularly preferable.
[0021] The weight-average molecular weight of the polystyrene sulfonic acid is preferably 1000 to 2000000, and more preferably 2000 to 500000. When the molecular weight is within this range, the dispersion stability of the polythiophene-based conductive polymer in water tends to be improved. The weight-average molecular weight is a value measured by gel permeation chromatography (GPC).
[0022] The polythiophene conductive polymer has a cumulative particle size D50=200-800nm and D90=250-1000nm measured by dynamic light scattering. The cumulative particle size D50 is the particle size at 50% cumulative volume, and D90 is the particle size at 90% cumulative volume. When D50 is 200nm or more and D90 is 250nm or more, the conductive layer formed by the conductive composition tends to exhibit excellent durability. When D50 is 800nm or less and D90 is 1000nm or less, precipitation of the polythiophene conductive polymer can be prevented, and the conductive layer formed by the conductive composition can be made homogeneous. D50 is 200-800nm, but is preferably 250-750nm, and more preferably 300-700nm. D90 is 250-1000nm, but is preferably 300-950nm, and more preferably 350-900nm. The ratio of D90 to D50 (D90 / D50) is preferably 1.43 or less, more preferably 1.42 or less. Within the above range, the film tends to exhibit excellent durability. The lower limit of D90 / D50 is not particularly limited, but is generally 1 or more.
[0023] The electrical conductivity of the polythiophene-based conductive polymer is preferably 0.0001 to 2000 S / cm, more preferably 0.001 to 1000 S / cm, and even more preferably 0.001 to 500 S / cm. Within the above range, the conductive layer formed from the conductive composition tends to exhibit excellent electrical conductivity.
[0024] The content of the polythiophene-based conductive polymer in the conductive composition is preferably 0.1 to 20% by weight, more preferably 1 to 20% by weight, and even more preferably 5 to 20% by weight, based on the total solid content. Within the above range, the composition can exhibit sufficient conductivity and has optical properties that allow it to be used in liquid crystal displays and the like.
[0025] <Antioxidants> By blending an antioxidant in the conductive composition, the heat resistance, moist heat resistance, and ultraviolet resistance of the conductive layer can be improved. The antioxidant may be either a water-soluble antioxidant or a fat-soluble antioxidant, but in order to disperse it uniformly in the conductive composition and the conductive layer, a water-soluble antioxidant is preferred. Examples of the water-soluble antioxidant include reducing water-soluble antioxidants and non-reducing water-soluble antioxidants.
[0026] Examples of reducing water-soluble antioxidants include compounds having a lactone ring substituted with two hydroxyl groups, such as L-ascorbic acid, sodium L-ascorbate, potassium L-ascorbate, D(-)-isoascorbic acid (erythorbic acid), sodium erythorbate, and potassium erythorbate; monosaccharides or disaccharides, such as maltose, lactose, cellobiose, xylose, arabinose, glucose, fructose, galactose, and mannose (however, sucrose is not particularly limited). flavonoids such as catechin, rutin, myricetin, quercetin, kaempferol, and Sammelin (registered trademark) Y-AF; compounds having two or more phenolic hydroxyl groups such as tannic acid, gallic acid, propyl gallate, curcumin, rosmarinic acid, chlorogenic acid, hydroquinone, and 3,4,5-trihydroxybenzoic acid; and compounds having a thiol group such as cysteine, glutathione, and pentaerythritol tetrakis(3-mercaptobutyrate).
[0027] Examples of non-reducing water-soluble antioxidants include compounds that absorb ultraviolet light, which causes oxidative deterioration, such as phenylimidazole sulfonic acid, phenyltriazole sulfonic acid, 2-hydroxypyrimidine, phenyl salicylate, and sodium 2-hydroxy-4-methoxybenzophenone-5-sulfonate.
[0028] The water-soluble antioxidants listed above may be used alone or in combination of two or more. Among the water-soluble antioxidants listed above, reducing water-soluble antioxidants are preferred, more preferred are compounds having a lactone ring substituted with two hydroxyl groups, compounds having two or more phenolic hydroxyl groups, and sugar compounds having hydroxyl groups, and even more preferred are L-ascorbic acid, sodium L-ascorbate, tannic acid, gallic acid, isoascorbic acid, curcumin, hydroquinone, 4,6-di-tert-butylresorcinol, and fructose.
[0029] The content of the antioxidant in the conductive composition is preferably 0.5 to 25% by weight, more preferably 1 to 20% by weight, and even more preferably 2 to 18% by weight, based on the total solid content. The content of the antioxidant is preferably 10 to 500 parts by weight, more preferably 20 to 400 parts by weight, and even more preferably 50 to 300 parts by weight, based on 100 parts by weight of the solid content of the polythiophene-based conductive polymer. Within these ranges, the durability of the conductive layer can be improved, while excellent conductivity and optical properties can be imparted to the conductive layer. Also, stickiness of the conductive layer can be suppressed.
[0030] The conductive composition can be obtained by mixing a polythiophene-based conductive polymer, an antioxidant, and, if necessary, any optional components described below in any order. The pH of the conductive composition can be adjusted by adding an inorganic acid such as sulfuric acid, hydrochloric acid, nitric acid, or phosphoric acid, an organic acid such as acetic acid, formic acid, or benzoic acid, or an alkali agent such as NaOH or KOH.
[0031] The conductive composition has a surface resistivity of 1×10 when formed into a film with a thickness of 100 to 350 nm on a substrate. 6 ~1×10 10 Preferably, the concentration is 1×10 7 ~1×10 9 More preferably, it is 1×10 7 ~1×10 8 The surface resistivity is a value measured by the method described in the examples.
[0032] <Optional ingredients> The conductive composition may contain, in addition to the polythiophene-based conductive polymer and the antioxidant, a binder, a solvent, a leveling agent, a dispersant, a crosslinking agent, a catalyst, and the like.
[0033] The binder is not particularly limited, and a thermoplastic resin or a thermosetting resin can be used. Examples of the thermoplastic resin include acrylic resin, polyurethane resin, polyester resin, polyolefin resin, styrene resin, vinyl acetate resin, vinyl chloride resin, and fluorine resin. Examples of the thermosetting resin include silicone resin, epoxy resin, phenol resin, amino resin, polyimide resin, and thermoplastic resin having a reactive functional group. These binders are highly compatible with polythiophene conductive polymers, and the conductive layer made of the conductive composition containing these binders has good affinity with the substrate. Furthermore, the binder contained in the conductive composition may be a water-dispersible resin or a curable resin that hardens after being applied to the substrate. When the binder is a water-dispersible resin, the water-dispersible resin may be dispersed as a result of the addition of a hydrophilic functional group to the resin, or may be forcibly dispersed by an emulsifier. These binders may be used alone or in combination of two or more.
[0034] Examples of acrylic resins include (meth)acrylic resins, vinyl ester resins, etc. These acrylic resins may be polymers containing, as constituent monomers, polymerizable monomers having an acid group such as a carboxyl group, an acid anhydride group, a sulfonic acid group, or a phosphoric acid group, and examples of such polymerizable resins include homopolymers or copolymers of polymerizable monomers having an acid group, and copolymers of polymerizable monomers having an acid group and copolymerizable monomers.
[0035] The (meth)acrylic resin may be polymerized with a copolymerizable monomer so long as it contains a (meth)acrylic monomer as a main constituent monomer (e.g., 50 mol % or more). In this case, at least one of the (meth)acrylic monomer and the copolymerizable monomer may have an acid group. Examples of the (meth)acrylic resin include (meth)acrylic monomers having an acid group [(meth)acrylic acid, sulfoalkyl (meth)acrylate, sulfonic acid group-containing (meth)acrylamide, etc.] or copolymers thereof, copolymers of (meth)acrylic monomers which may have an acid group and other polymerizable monomers having an acid group [other polymerizable carboxylic acids, polymerizable polycarboxylic acids or anhydrides, vinyl aromatic sulfonic acids, etc.] and / or copolymerizable monomers [e.g., (meth)acrylic acid alkyl esters, glycidyl (meth)acrylate, (meth)acrylonitrile, aromatic vinyl monomers, etc.], copolymers of other polymer monomers having an acid group and (meth)acrylic copolymerizable monomers [e.g., (meth)acrylic acid alkyl esters, hydroxyalkyl (meth)acrylates, glycidyl (meth)acrylate, (meth)acrylonitrile, etc.], rosin-modified urethane acrylates, specially modified acrylic resins, urethane acrylates, epoxy acrylates, urethane acrylate emulsions, and the like.
[0036] Among these (meth)acrylic resins, (meth)acrylic acid-(meth)acrylic acid ester polymers (acrylic acid-methyl methacrylate copolymers, etc.), (meth)acrylic acid-(meth)acrylic acid ester-styrene copolymers (acrylic acid-methyl methacrylate-styrene copolymers, etc.), and the like are preferred.
[0037] The polyurethane resin is not particularly limited as long as it is a polymer compound obtained by copolymerizing a compound having an isocyanate group and a compound having a hydroxyl group, and examples thereof include ester-ether polyurethane, ether polyurethane, polyester polyurethane, carbonate polyurethane, and acrylic polyurethane.
[0038] The polyester resin is not particularly limited as long as it is a polymer compound obtained by polycondensation of a compound having two or more carboxyl groups in the molecule and a compound having two or more hydroxyl groups, and examples thereof include polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and polybutylene naphthalate.
[0039] The polyolefin resin is not particularly limited, but examples thereof include polyethylene, polypropylene, chlorinated polypropylene, maleic anhydride-modified polypropylene, maleic anhydride-modified chlorinated polypropylene, ethylene-vinyl acetate copolymer, and the like.
[0040] The styrene-based resin is not particularly limited as long as it is a resin whose main component is styrene, and examples thereof include polystyrene, acrylonitrile-styrene copolymer (AS), and acrylonitrile-butadiene-styrene copolymer (ABS).
[0041] The vinyl acetate resin is not particularly limited as long as it is a resin obtained by polymerization of vinyl acetate, and examples thereof include polyvinyl acetate, ethylene-vinyl acetate copolymer, and the like.
[0042] The vinyl chloride resin is not particularly limited as long as it is a resin obtained by polymerization of vinyl chloride, and examples thereof include polyvinyl chloride, ethylene-vinyl chloride copolymer, vinyl chloride-vinyl acetate copolymer, and the like.
[0043] Examples of the fluorine-based resin include polytetrafluoroethylene, polyvinylidene fluoride, Teflon (registered trademark), and polyvinyl fluoride.
[0044] Examples of silicone-based resins include oligomers of alkoxysilanes formed by condensation of alkoxysilane monomers represented by the following formula (I) and having one or more siloxane bonds (Si—O—Si) in one molecule. SiR 1 4(I) (In the formula, R1 is hydrogen, a hydroxyl group, an alkoxy group having 1 to 4 carbon atoms, an alkyl group having 1 to 12 carbon atoms which may have a substituent, or an aryl group having 6 to 20 carbon atoms which may have a substituent. 1 At least one of these is an alkoxy group having 1 to 4 carbon atoms or a hydroxyl group.)
[0045] In formula (I), R 1 Examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, and a butoxy group. 1 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a normal butyl group, a tertiary butyl group, a pentyl group, and a hexyl group. 1 The aryl group includes a phenyl group, a tolyl group, and a benzyl group.
[0046] Specific examples of the monomer represented by formula (I) include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, Examples of the isocyanate include isocyanate, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, methyltrimethoxysilane, phenyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, n-propyltrimethoxysilane, diisopropyldimethoxysilane, isobutyltrimethoxysilane, diisobutyldimethoxysilane, isobutyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, cyclohexylmethyldimethoxysilane, n-octyltriethoxysilane, n-decyltrimethoxysilane, tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane. Among these, tetramethoxysilane and tetraethoxysilane are preferred.
[0047] The structure of the silicone resin is not particularly limited, and may be linear or branched. The silicone resin may be a condensation product of one type of monomer represented by formula (I) or two or more types of monomers.
[0048] Specific examples of silicone resins include methyl silicate oligomer and ethyl silicate oligomer.
[0049] The weight average molecular weight of the silicone resin is not particularly limited, but is preferably 200 to 10,000, and more preferably 400 to 5,000.
[0050] Examples of epoxy resins include bisphenol A type, bisphenol F type, phenol novolac type, tetrakis(hydroxyphenyl)ethane type or tris(hydroxyphenyl)methane type which are multifunctional types having a large number of benzene rings, biphenyl type, triphenolmethane type, naphthalene type, ortho-novolac type, dicyclopentadiene type, aminophenol type, alicyclic epoxy resins, silicone epoxy resins, and the like.
[0051] Examples of the reactive functional group of the thermoplastic resin having a reactive functional group include a hydroxyl group, a carboxyl group, an acid anhydride group, a sulfonic acid group, a phosphoric acid group, and a glycidyl group.
[0052] The binder is not particularly limited, but among the above-listed binders, thermosetting resins are preferred, and silicone-based resins and thermoplastic resins having reactive functional groups are more preferred.
[0053] The ratio of the solid content of the binder to the total solid content of the conductive composition is preferably 55 to 99.9% by weight, more preferably 60 to 99% by weight, and even more preferably 65 to 95% by weight. The content of the solid content of the binder is preferably 200 to 9900 parts by weight, more preferably 300 to 4900 parts by weight, per 100 parts by weight of the solid content of the polythiophene-based conductive polymer. Within this range, the conductive layer can have sufficient strength and conductivity.
[0054] Examples of the solvent include water; alcohols such as methanol, ethanol, 2-propanol, and 1-propanol; ethylene glycols such as ethylene glycol, diethylene glycol, trimethylene glycol, triethylene glycol, and tetraethylene glycol; glycol ethers such as ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, ethylene glycol diethyl ether, and diethylene glycol dimethyl ether; glycol ether acetates such as ethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate; propylene glycols such as propylene glycol, dipropylene glycol, and tripropylene glycol; propylene glycol ethers such as propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, propylene glycol dimethyl ether, and propylene glycol diethyl ether; propylene glycol ethers such as propylene glycol monomethyl ether acetate, and propylene glycol monomethyl ether acetate. ether acetates; ethers such as diethyl ether, diisopropyl ether, methyl t-butyl ether, and tetrahydrofuran; ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; hydrocarbons such as toluene, xylene (o-, m-, or p-xylene), hexane, and heptane; esters such as butyl acetate; halogens, acetonitrile, N-methylformamide, N,N-dimethylformamide, γ-butyrolactone, and N-methylpyrrolidone; amides such as 1,4-butanediol, 1,5- Examples of the compound include hydroxyl group-containing compounds such as pentanediol, 1,6-hexanediol, neopentyl glycol, catechol, cyclohexanediol, cyclohexanedimethanol, glycerin, diethylene glycol monoethyl ether, and propylene glycol monomethyl ether; carbonyl group-containing compounds such as isophorone, propylene carbonate, cyclohexanone, acetylacetone, ethyl acetate, ethyl acetoacetate, methyl orthoacetate, and ethyl orthoformate; and compounds having a sulfo group such as dimethyl sulfoxide.
[0055] Among these, water, alcohols, ethylene glycols, and compounds having a sulfo group are preferred, water, ethanol, ethylene glycol, and dimethyl sulfoxide are more preferred, and a mixed solvent of water and ethanol, ethylene glycol, or dimethyl sulfoxide is even more preferred. In the mixed solvent, the amount of water is preferably 20% by weight or more, more preferably 50% by weight or more, even more preferably 75% by weight or more, and particularly preferably 95% by weight or more and less than 100%. It is preferable that the solvent does not remain in the conductive layer formed using the conductive composition.
[0056] The solid content of the conductive composition can be adjusted by the blending amount of the solvent. The solid content of the conductive composition is not particularly limited, but is preferably 0.1 to 50% by weight, more preferably 0.5 to 30% by weight, and even more preferably 1 to 20% by weight. When the solid content is within the above range, sufficient conductivity can be exhibited, and the coating property during the production of the conductive layer and the storage stability of the conductive composition tend to be good. In this specification, there is no particular distinction between a substance that completely dissolves all the components of the conductive composition (i.e., a "solvent") and a substance that disperses insoluble components (i.e., a "dispersion medium"), and both are described as "solvent".
[0057] Adding a leveling agent to the conductive composition can increase the affinity for the substrate and suppress the occurrence of repelling and unevenness when forming the conductive layer. Examples of the leveling agent include silicone-based leveling agents, fluorine-based leveling agents, polyether-based leveling agents, polyester-based leveling agents, and acrylic-based leveling agents.
[0058] Examples of silicone-based leveling agents include polysiloxanes; reactive polysiloxanes having reactive groups such as amino groups, epoxy groups, hydroxyl groups, and carboxyl groups introduced therein; and non-reactive polysiloxanes having non-reactive groups such as alkyl groups, ester groups, aralkyl groups, phenyl groups, and polyether groups introduced therein.
[0059] Examples of fluorine-based leveling agents include perfluoropolyether-modified polydimethylsiloxane, perfluoropolyester-modified polydimethylsiloxane, perfluorobutanesulfonic acid, fluorine-containing, hydrophilic, and lipophilic group-containing oligomers, perfluoroalkyl group-containing carboxylates, and perfluoroalkyl group- and phosphate group-containing phosphate esters.
[0060] Examples of polyether-based leveling agents include cellulose ether; pullulan; polyethylene glycol; silicone-modified polyethers such as polyether-modified polydimethylsiloxane, polyether-modified siloxane, polyetherester-modified hydroxyl group-containing polydimethylsiloxane, and polyether-modified acrylic group-containing polydimethylsiloxane; polyglycerin; polyether polyol, polyoxyethylene-polyoxypropylene condensates, polyoxyethylene alkylphenyl ethers, alkyl ether derivatives such as lauryl alcohol alkoxylate, and alkyl ether sulfates.
[0061] Examples of polyester-based leveling agents include polyester-modified acrylic group-containing polydimethylsiloxane, polyester-modified polydimethylsiloxane, and polyester polyol.
[0062] Examples of the acrylic leveling agent include acrylic copolymers made of silicone and acrylic.
[0063] The content of the leveling agent is not particularly limited, but is preferably 0.1 to 20 parts by weight, more preferably 1 to 10 parts by weight, based on the total solid content of the conductive composition. When the content of the conductive composition is within the above range, the coating property on the substrate, the dispersion stability of the blended components, and the film strength when formed into a conductive layer are good.
[0064] Examples of the crosslinking agent include melamine-based, carbodiimide-based, oxazoline-based, epoxy-based, isocyanate-based, acrylate-based, etc. When the conductive composition contains a crosslinking agent, the content is not particularly limited, but is preferably 30% by weight or less, and more preferably 20% by weight or less, of the solid content of the conductive composition.
[0065] When the conductive composition contains a thermosetting binder or a crosslinking agent, a catalyst may be added. The catalyst is not particularly limited, and examples thereof include a photopolymerization initiator, a thermal polymerization initiator, and an acid catalyst. These may be used alone or in combination of two or more kinds.
[0066] The acid catalyst may be an inorganic acid or an organic acid. The inorganic acid is not particularly limited, but examples thereof include formic acid, acetic acid, oxalic acid, hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, fluoroboric acid, hydrofluoric acid, and perchloric acid. The organic acid is not particularly limited, but in consideration of thermosetting property and stability, it is preferable that the molecular weight is 20,000 or less. Specifically, examples thereof include aliphatic sulfonic acids such as methanesulfonic acid, trifluoromethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, hexanesulfonic acid, octanesulfonic acid, nonanesulfonic acid, decanesulfonic acid, hexadecanesulfonic acid, and camphorsulfonic acid, and aromatic sulfonic acids such as p-toluenesulfonic acid, benzenesulfonic acid, styrenesulfonic acid, dodecylbenzenesulfonic acid, and naphthalenesulfonic acid. Among these, aromatic sulfonic acids are preferred, and dodecylbenzenesulfonic acid is more preferred. The content of the acid catalyst is not particularly limited, but is preferably 20% by weight or less, more preferably 10% by weight or less, and even more preferably 5% by weight or less, based on the solid content of the conductive composition.
[0067] <<Conductive laminate>> The conductive laminate of the present invention includes a substrate and a conductive layer formed on the substrate, the conductive layer containing a polythiophene-based conductive polymer. When the conductive layer is formed to a thickness of 50 to 4000 nm, the surface resistivity of the conductive layer is 1×10 6 ~1×1010 and is characterized in that any one or more of the following (A) to (C) is satisfied: (A) (Surface resistivity after 1000 hours of exposure under conditions of temperature 85°C and relative humidity 85%) / (Surface resistivity immediately after film formation)≦500 (B) (Surface resistivity after 1000 hours of exposure at 105°C) / (Surface resistivity immediately after film formation)≦500 (C) (wavelength 405 nm, illuminance 250 W / m 2 (Surface resistivity after 1000 hours of exposure to light of 1000 nm) / (Surface resistivity immediately after film formation)≦1000
[0068] Examples of materials for the substrate include glass, polyester resins such as polyethylene terephthalate (PET), polyethylene naphthalate, modified polyester, etc., polyolefin resins such as polyethylene (PE) resin, polypropylene (PP) resin, polystyrene resin, cyclic olefin resin, etc., vinyl resins such as polyvinyl chloride and polyvinylidene chloride, polyether ether ketone (PEEK) resin, polysulfone (PSF) resin, polyethersulfone (PES) resin, polycarbonate (PC) resin, polyamide resin, polyimide resin, acrylic resin, triacetyl cellulose (TAC) resin, and metals such as copper and aluminum.
[0069] The shape of the substrate is not particularly limited, but is preferably a film. The thickness of the substrate is preferably 10 to 10,000 μm, more preferably 25 to 5,000 μm. The total light transmittance of the substrate is preferably 60% or more, more preferably 70% or more.
[0070] The thickness of the conductive layer containing the polythiophene-based conductive polymer is preferably 50 to 4000 nm, more preferably 75 to 2000 nm, even more preferably 100 to 1000 nm, and even more preferably 100 to 350 nm. The thickness of the conductive layer is calculated from the solid content of the conductive composition used to form the conductive layer and the amount applied to the substrate. In the conductive laminate, the amount of the polythiophene-based conductive polymer per unit area of the conductive layer is 0.1 to 500 mg / m 2is preferable, and 1 to 200 mg / m 2 is more preferred.
[0071] The conductive layer has a surface resistivity of 1×10 when formed on the substrate with a thickness of 50 to 4000 nm. 6 ~1×10 10 and 1 × 10 7 ~1×10 9 Preferably, the concentration is 1×10 7 ~1×10 8 The surface resistivity is a value measured by the method described in the examples.
[0072] When the thickness of the conductive layer is 50 to 4000 nm, the total light transmittance of the conductive laminate including the conductive layer and the substrate is preferably 70% or more, more preferably 80% or more, and particularly preferably 85% or more. The upper limit of the total light transmittance is 100%. The haze value of the conductive laminate including the conductive layer and the substrate is preferably 3% or less, more preferably 2% or less, even more preferably 1% or less, and particularly preferably 0.5% or less. Since the haze value is preferably as small as possible, the lower limit is not particularly limited, but is, for example, 0.01%. The total light transmittance and the haze value can be evaluated by the method described in the examples.
[0073] The method for producing the conductive laminate is not particularly limited, but for example, the conductive laminate can be produced by a method including a step of forming a coating film of a conductive composition on a substrate and a step of drying the coating film. The composition of the conductive composition is not particularly limited, but it is preferable to use a conductive composition that contains the polythiophene conductive polymer and an antioxidant, and has a cumulative particle size of D50=200 to 800 nm and D90=250 to 1000 nm measured by a dynamic light scattering method for the polythiophene conductive polymer.
[0074] The coating film is formed by applying the conductive composition onto the substrate. Examples of the coating method include blade coating, bar coating, gravure coating, roll coating, bar coating, dip coating, spin coating, casting, die coating, curtain coating, spray coating, doctor coating, slit coating, letterpress printing, screen printing, offset printing, gravure printing, spray printing, inkjet printing, and pad printing.
[0075] Before forming a coating film of the conductive composition on the substrate, the surface of the substrate may be subjected to a surface treatment in advance. Examples of the surface treatment include corona treatment, plasma treatment, itro treatment, and flame treatment. The conductive composition may be applied directly to the substrate surface, or may be applied on a separate layer such as a primer layer that is provided on the substrate in advance.
[0076] By drying the coating film formed on the substrate, the volatile components contained in the coating film are removed, and a conductive layer is obtained. Heat drying is preferred as the drying method, and examples thereof include methods using a blower oven, an infrared oven, a vacuum oven, etc. The temperature condition during heat drying is preferably 60 to 200°C, more preferably 80 to 180°C. The treatment time of the heat treatment is not particularly limited, but is preferably 0.1 to 20 minutes, more preferably 1 to 5 minutes.
[0077] The conductive laminate of the present invention has a conductive layer with excellent durability, such as resistance to moist heat, heat, and weather.
[0078] (A) Moisture and heat resistance The conductive layer preferably has a rate of change in surface resistivity after a moist heat resistance test, as represented by the following formula, of 500 or less, more preferably 400 or less, even more preferably 300 or less, even more preferably 100 or less, and particularly preferably 50 or less. The moist heat resistance can be evaluated by the method described in the examples. (Surface resistivity after 1000 hours of exposure under conditions of 85°C and 85% relative humidity) / (Surface resistivity immediately after film formation)
[0079] (B) Heat resistance The conductive layer preferably has a rate of change in surface resistivity after a heat resistance test, as represented by the following formula, of 500 or less, more preferably 400 or less, even more preferably 300 or less, even more preferably 100 or less, and particularly preferably 50 or less. The heat resistance can be evaluated by the method described in the examples. (Surface resistivity after 1000 hours exposure at 105°C) / (Surface resistivity immediately after film formation)
[0080] (C) Weather resistance The conductive layer preferably has a rate of change in surface resistivity after a weather resistance test, as represented by the following formula, of 1000 or less, more preferably 500 or less, and even more preferably 100 or less. Weather resistance can be evaluated by the method described in the examples. (Wavelength 405nm, illuminance 250W / m 2 (Surface resistivity after 1000 hours of exposure to light of 1000 nm) / (Surface resistivity immediately after film formation)
[0081] Since the laminate has excellent electrical conductivity, it can be suitably used for applications such as antistatic films, polarizing plates, surface protective films, transparent conductive films, conductive hard coats, and conductive adhesives, and is preferably used as an antistatic film for liquid crystal display devices and the like. EXAMPLES
[0082] The present invention will be described below with reference to examples, but the present invention is not limited to the following examples. In the following, "parts" and "%" mean "parts by weight" and "% by weight", respectively, unless otherwise specified.
[0083] (1) Materials used (1-1) Polythiophene-based conductive polymer PEDOT / PSS1 (prepared in Example 1) PEDOT / PSS2 (prepared in Example 2) PEDOT / PSS3 (prepared in Example 3) PEDOT / PSS4 (prepared in Example 4) PEDOT / PSS5 (prepared in Example 5) PEDOT / PSS6 (prepared in Example 6) PEDOT / PSS7 (prepared in Example 7) PEDOT / PSS8 (prepared in Example 8)
[0084] (1-2) Binder Methyl silicate oligomer (SiO2 content 52%) (Mitsubishi Chemical, MS-51) Polyester resin (Aronmelt PES-2405A30, manufactured by Toa Gosei Co., Ltd.) Acrylic resin (Nikasol RX-66E, manufactured by Nippon Carbide) Polyurethane resin (Superflex 130, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) Olefin resin (TOYOBO, Hardlen EW-5303) Tetraethoxysilane (Tokyo Chemical Industry Co., Ltd.)
[0085] (1-3) Antioxidants Tannic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) Ascorbic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) Gallic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) Isoascorbic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0086] (1-4) Leveling agent Polyether surfactant (Clariant, product name: Emulsogen LCN070)
[0087] (1-5) Catalyst Sodium dodecylbenzenesulfonate (Tokyo Chemical Industry Co., Ltd.)
[0088] (1-6) Solvent Ethylene glycol (Tokyo Chemical Industry Co., Ltd.) Dimethyl sulfoxide (Tokyo Chemical Industry Co., Ltd.) Ethanol (Tokyo Chemical Industry Co., Ltd.)
[0089] (1-7) Base material PET film (Toray, Lumirror T-60) Glass (CORNING, Eagle XG)
[0090] (2) Production of polythiophene-based conductive polymers (2-1) Production Example 1 66.89g of a 20% by weight aqueous solution of poly(4-styrenesulfonic acid) (PSS: molecular weight 500000) and 0.05g of iron sulfate were added to 500g of pure water. 3.42g of 3,4-ethylenedioxythiophene (EDOT) and 6.30g of sodium persulfate were further added, and pure water was added to prepare a mixed solution so that the total mass became 1200g, and the mixed solution was placed in a temperature-controllable reaction vessel. The mixed solution was subjected to an oxidative polymerization reaction at 25°C for 14 hours in an air atmosphere. The reaction solution was removed from the reaction vessel, anion exchange resin and cation exchange resin were added, and the mixture was stirred for another 2 hours. The obtained ion-exchanged liquid was filtered with a glass filter to obtain PEDOT / PSS1 (solid content 1.2% by weight).
[0091] (2-2) Production Example 2 66.89g of a 20% by weight aqueous solution of poly(4-styrenesulfonic acid) (PSS: molecular weight 500000) and 0.05g of iron sulfate were added to 500g of pure water. 3.42g of 3,4-ethylenedioxythiophene (EDOT) and 17.18g of sodium persulfate were further added, and pure water was added to prepare a mixed solution so that the total mass became 1200g, and the mixed solution was placed in a temperature-controllable reaction vessel. The mixed solution was subjected to an oxidative polymerization reaction at 25°C for 14 hours in an air atmosphere. The reaction solution was removed from the reaction vessel, anion exchange resin and cation exchange resin were added, and the mixture was stirred for another 2 hours. The obtained ion-exchanged liquid was filtered with a glass filter to obtain PEDOT / PSS2 (solid content 1.2% by weight).
[0092] (2-3) Production Example 3 66.89g of a 20% by weight aqueous solution of poly(4-styrenesulfonic acid) (PSS: molecular weight 500000) and 0.05g of iron sulfate were added to 500g of pure water. 3.42g of 3,4-ethylenedioxythiophene (EDOT) and 22.9g of sodium persulfate were further added, and pure water was added to prepare a mixed solution so that the total mass became 1200g, and the mixed solution was placed in a temperature-controllable reaction vessel. The mixed solution was subjected to an oxidative polymerization reaction at 25°C for 14 hours in an air atmosphere. The reaction solution was removed from the reaction vessel, anion exchange resin and cation exchange resin were added, and the mixture was stirred for another 2 hours. The obtained ion-exchanged liquid was filtered with a glass filter to obtain PEDOT / PSS3 (solid content 1.2% by weight).
[0093] (2-4) Production Example 4 66.89g of a 20% by weight aqueous solution of poly(4-styrenesulfonic acid) (PSS: molecular weight 200,000) and 0.05g of iron sulfate were added to 500g of pure water. 3.42g of 3,4-ethylenedioxythiophene (EDOT) and 6.30g of sodium persulfate were further added, and pure water was added to prepare a mixed solution so that the total mass became 1200g, and the mixed solution was placed in a temperature-controllable reaction vessel. The mixed solution was subjected to an oxidative polymerization reaction at 35°C for 14 hours in an air atmosphere. The reaction solution was removed from the reaction vessel, anion exchange resin and cation exchange resin were added, and the mixture was stirred for another 2 hours. The obtained ion-exchanged liquid was filtered with a glass filter to obtain PEDOT / PSS4 (solid content 1.2% by weight).
[0094] (2-5) Production Example 5 66.89g of a 20% by weight aqueous solution of poly(4-styrenesulfonic acid) (PSS: molecular weight 500000) and 0.05g of iron sulfate were added to 500g of pure water. 3.42g of 3,4-ethylenedioxythiophene (EDOT) and 17.18g of sodium persulfate were further added, and pure water was added to prepare a mixed solution so that the total mass became 1200g, and the mixed solution was placed in a temperature-controllable reaction vessel. The mixed solution was subjected to an oxidative polymerization reaction at 35°C for 14 hours in an air atmosphere. The reaction solution was removed from the reaction vessel, anion exchange resin and cation exchange resin were added, and the mixture was stirred for another 2 hours. The obtained ion-exchanged liquid was filtered with a glass filter to obtain PEDOT / PSS5 (solid content 1.2% by weight).
[0095] (2-6) Production Example 6 66.89g of a 20% by weight aqueous solution of poly(4-styrenesulfonic acid) (PSS: molecular weight 500000) and 0.05g of iron sulfate were added to 500g of pure water. 3.42g of 3,4-ethylenedioxythiophene (EDOT) and 22.9g of sodium persulfate were further added, and pure water was added to prepare a mixed solution so that the total mass became 1200g, and the mixed solution was placed in a temperature-controllable reaction vessel. The mixed solution was subjected to an oxidative polymerization reaction at 15°C for 14 hours in an air atmosphere. The reaction solution was removed from the reaction vessel, anion exchange resin and cation exchange resin were added, and the mixture was stirred for another 2 hours. The obtained ion-exchanged liquid was filtered through a glass filter to obtain PEDOT / PSS6 (solid content 1.2% by weight).
[0096] (2-7) Production Example 7 66.89g of a 20% by weight aqueous solution of poly(4-styrenesulfonic acid) (PSS: molecular weight 200,000) and 0.05g of iron sulfate were added to 500g of pure water. 3.42g of 3,4-ethylenedioxythiophene (EDOT) and 6.30g of sodium persulfate were further added, and pure water was added to prepare a mixed solution so that the total mass became 1200g, and the mixed solution was placed in a temperature-controllable reaction vessel. The mixed solution was subjected to an oxidative polymerization reaction at 15°C for 14 hours in an air atmosphere. The reaction solution was removed from the reaction vessel, anion exchange resin and cation exchange resin were added, and the mixture was stirred for another 2 hours. The obtained ion-exchanged liquid was filtered through a glass filter to obtain PEDOT / PSS7 (solid content 1.2% by weight).
[0097] (2-8) Production Example 8 66.89g of a 20% by weight aqueous solution of poly(4-styrenesulfonic acid) (PSS: molecular weight 200000) and 0.05g of iron sulfate were added to 500g of pure water. 3.42g of 3,4-ethylenedioxythiophene (EDOT) and 6.30g of sodium persulfate were further added, and pure water was added to prepare a mixed solution so that the total mass became 1200g, and the mixed solution was placed in a temperature-controllable reaction vessel. The mixed solution was subjected to an oxidative polymerization reaction at 15°C for 14 hours in an air atmosphere. The reaction solution was removed from the reaction vessel, anion exchange resin and cation exchange resin were added, and the mixture was stirred for another 2 hours. The obtained ion-exchanged liquid was filtered with a glass filter, and then homogenized 30 times at 60 MPa with a high-pressure homogenizer to obtain PEDOT / PSS8 (solid content 1.2% by weight).
[0098] The cumulative particle diameters D50 and D90 of the polythiophene-based conductive polymer were determined by measuring diluted dispersions of the polythiophene-based conductive polymers of Production Examples 1 to 8 using a Zetasizer Nano ZS manufactured by Malvern. The results are shown in Table 1.
[0099] (3) Production of Conductive Composition and Conductive Laminate (Examples 1 to 19, Comparative Examples 1 to 2) The components shown in Table 1 were mixed to prepare a conductive composition. The blending amounts of the components other than the solvent are shown as weight ratios, and the solvent is shown as the weight % relative to the entire conductive composition. The conductive composition was applied to one side of the substrate shown in Table 1 by a bar coating method, and dried at 120°C for 5 minutes using an air dryer to form a conductive layer on the substrate film. The thickness of the conductive layer was adjusted to 100 to 350 nm by appropriately selecting the number of the bar coater.
[0100] (4) Evaluation of the conductive layer (4-1)Surface resistivity The surface resistivity of the conductive layer on the conductive laminate was measured using a UA probe of a resistivity meter (Mitsubishi Chemical Corporation, Hiresta UP (MCP-HT450 type)) and an ESP probe of a resistivity meter (Mitsubishi Chemical Corporation, Loresta GP (MCP-T600 type)). The probe was pressed against the surface of the conductive layer, and the surface resistivity (SR, unit Ω / □) was determined when an applied voltage of 10 V was maintained for 10 seconds.
[0101] (4-2) Moisture and heat resistance test The conductive laminate was maintained for 1000 hours under conditions of a temperature of 85° C. and a relative humidity of 85%. The rate of change in surface resistivity before and after the moist heat resistance test was determined from the surface resistivity immediately after the formation of the conductive layer and the surface resistivity after the test. (Change rate of surface resistivity)=(Surface resistivity after test) / (Surface resistivity immediately after forming the conductive layer)
[0102] (4-3) Heat resistance test The conductive laminate was held for 1000 hours under the condition of a temperature of 105° C. The rate of change in surface resistivity before and after the heat resistance test was determined using the same calculation method as in the moist heat resistance test.
[0103] (4-4) Weather resistance test The conductive laminate is illuminated with a wavelength of 405 nm and an illuminance of 250 W / m 2 The rate of change in surface resistivity before and after the weather resistance test was calculated using the same calculation method as for the heat and humidity resistance test.
[0104] (4-5) Total light transmittance (Tt) / Haze value The total light transmittance and haze value of the conductive laminate including the conductive layer and the substrate were measured according to JIS K 7150 using a haze computer HGM-2B manufactured by Suga Test Instruments Co., Ltd.
[0105] The evaluation results of the conductive layer are shown in Table 1. [Table 1]
[0106] In Comparative Examples 1 and 2, the cumulative particle size of the polythiophene-based conductive polymer was small, so that the conductivity of the conductive layer was impaired and the surface resistivity increased significantly after the moist heat resistance test, heat resistance test, and weather resistance test. In Examples 1 to 19, the conductivity of the conductive layer was maintained even after each test.
[0107] The present disclosure (1) is a conductive composition comprising a polythiophene-based conductive polymer and an antioxidant, wherein the polythiophene-based conductive polymer has a cumulative particle size, as measured by a dynamic light scattering method, of D50=200 to 800 nm and D90=250 to 1000 nm.
[0108] The present disclosure (2) is the conductive composition according to the present disclosure (1), further comprising a binder.
[0109] The present disclosure (3) is the conductive composition according to the present disclosure (1) or (2), in which the binder is a thermosetting resin.
[0110] The present disclosure (4) is the conductive composition according to any one of the present disclosures (1) to (3), in which the amount of the antioxidant is 0.1 to 500 parts by weight based on 100 parts by weight of the solid content of the polythiophene-based conductive polymer.
[0111] The present disclosure (5) is the conductive composition according to any one of the present disclosures (1) to (4), in which the blending amount of the polythiophene-based conductive polymer is 0.1 to 20% by weight based on the total solid content.
[0112] The present disclosure (6) provides a method for forming a film having a thickness of 100 to 350 nm on a substrate, the surface resistivity of which is 1×10 6 ~1×10 10 The conductive composition according to any one of the present disclosures (1) to (5),
[0113] The present disclosure (7) is a conductive laminate including a substrate and a conductive layer including a polythiophene-based conductive polymer formed on the substrate, the conductive layer having a surface resistivity of 1×10 6 ~1×10 10 and the conductive layer satisfies any one or more of the following (A) to (C): (A) (Surface resistivity after 1000 hours of exposure under conditions of temperature 85°C and relative humidity 85%) / (Surface resistivity immediately after film formation)≦500 (B) (Surface resistivity after 1000 hours of exposure at 105°C) / (Surface resistivity immediately after film formation)≦500 (C) (wavelength 405 nm, illuminance 250 W / m 2 (Surface resistivity after 1000 hours of exposure to light of 1000 nm) / (Surface resistivity immediately after film formation)≦1000
[0114] The present disclosure (8) is the conductive laminate according to the present disclosure (7), which is an antistatic film.
Claims
1. Contains a polythiophene-based conductive polymer and an antioxidant, The polythiophene-based conductive polymer has a cumulative particle size D50 of 200 to 800 nm and D90 of 250 to 1000 nm as measured by a dynamic light scattering method. Conductive composition.
2. The conductive composition of claim 1 further comprising a binder.
3. The conductive composition of claim 2 , wherein the binder is a thermosetting resin.
4. 3. The conductive composition according to claim 1, wherein the amount of the antioxidant is 0.1 to 500 parts by weight based on 100 parts by weight of the solid content of the polythiophene-based conductive polymer.
5. 3. The conductive composition according to claim 1, wherein the content of the polythiophene-based conductive polymer is 0.1 to 20% by weight based on the total solid content.
6. When a film having a thickness of 100 to 350 nm is formed on a substrate, the surface resistivity is 1×10 6 ~1×10 10 The conductive composition according to claim 1 or 2,
7. A conductive laminate including a substrate and a conductive layer formed on the substrate, the conductive layer including a polythiophene-based conductive polymer, When the film is formed to a thickness of 50 to 4000 nm, the surface resistivity of the conductive layer is 1×10 6 ~1×10 10 and A conductive laminate, wherein the conductive layer satisfies any one or more of the following (A) to (C): (A) (Surface resistivity after exposure for 1000 hours under conditions of a temperature of 85° C. and a relative humidity of 85%) / (Surface resistivity immediately after film formation)≦500 (B) (Surface resistivity after exposure to a temperature of 105° C. for 1000 hours) / (Surface resistivity immediately after film formation)≦500 (C) (wavelength 405 nm, illuminance 250 W / m 2(surface resistivity after 1000 hours of exposure under irradiation with light of 1000 nm) / (surface resistivity immediately after film formation)≦1000
8. The conductive laminate according to claim 7 , which is an antistatic film.
Citation Information
Patent Citations
Organic conductive film
JP2013058470A
Conductive resin composition and transparent conductive laminate
JP2015117364A
Electroconductive dispersion
JP2015221871A
Conductive particle and method for producing the same, and conductive resin composition
JP2019075265A
Compositions useful for forming antistatic layers or electromagnetic radiation shielding
JP2020506986A