Ferrite-austenite duplex stainless steel plate
A ferritic-austenitic duplex stainless steel sheet with controlled composition and heat treatment achieves high strength, smoothness, and flatness, addressing the challenges of miniaturization and weight reduction in electronic and precision equipment parts.
Patent Information
- Application Number
- JP2023048351
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Existing stainless steel sheets struggle to achieve high strength, thinning, smoothness of the etched surface, and flatness before and after etching, especially in the context of electronic and precision equipment parts, where miniaturization and weight reduction are desired.
A ferritic-austenitic duplex stainless steel sheet with specific chemical composition and microstructure is developed, utilizing precipitation strengthening through strain relief heat treatment at temperatures above 700°C, combined with controlled grain size and residual stress management.
The solution provides high strength, smooth etched surfaces, and maintained flatness, enabling the production of smaller and lighter electronic and precision equipment components.
Smart Images

Figure 2024137014000001 
Figure 2024137014000002 
Figure 2024137014000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a ferritic-austenitic duplex stainless steel sheet, and in particular to a high-strength ferritic-austenitic duplex stainless steel sheet suitable as a material for parts of electronic devices and precision machines. [Background technology]
[0002] Further miniaturization and weight reduction are required for parts used in electronic and precision equipment, and along with thinner sheets of the corresponding materials, higher strength is required to maintain the rigidity required for the parts. Furthermore, high dimensional accuracy is also required, and a good balance between strength and elongation is required, specifically, high strength while maintaining conventional workability (hereinafter simply referred to as high strength).
[0003] In addition, when manufacturing the above-mentioned parts, a method of partially thinning the plate thickness by etching is often used as one of the means for obtaining a predetermined shape with high precision. Therefore, the material of the above-mentioned parts is required to have small shape change and no plate warping after etching, that is, excellent flatness before and after etching and smoothness of the etched surface.
[0004] Sheet warpage refers to the deformation of the entire steel sheet after partial etching (herein referred to as "half etching") of the steel sheet surface. The warpage of the steel sheet after half etching is caused by the residual stress of the steel sheet. Therefore, the warpage can be reduced by carrying out a heat treatment for the purpose of relieving the stress after temper rolling, that is, a so-called stress relief heat treatment.
[0005] Furthermore, the material used for the above-mentioned parts is generally austenitic stainless steel, which has an excellent balance between strength and elongation among stainless steels and has had its strength increased by temper rolling, etc. In particular, metastable austenitic stainless steels such as SUS301 and SUS304 are used, which combine high strength associated with deformation-induced martensitic transformation with excellent workability due to the TRIP effect and which, among the austenitic stainless steels, can relatively easily obtain high strength.
[0006] The austenitic stainless steel sheet, the strength of which has been increased by temper rolling or the like, is further subjected to shape correction using a tension leveler, distortion relief heat treatment for the purpose of reducing residual stress, and the like. This is to make the steel sheet shaped and flat in response to the precision machining of the above-mentioned parts. In addition, when small pieces corresponding to parts are taken out from a material manufactured from a relatively large steel sheet or steel strip by pressing, etching, or the like, or when the thickness of a part of the small pieces is reduced by further etching, as described above, deformation due to residual stress occurs. Furthermore, the more excellent the smoothness of the processed surface, particularly the etched surface (hereinafter also referred to as the etched surface), the more precise parts with higher dimensional accuracy can be manufactured from the material.
[0007] Patent Document 1 discloses a stainless steel sheet for photoetching in which the average crystal grain size is refined so as to obtain a smooth etched surface, and which is further subjected to a distortion relief heat treatment.
[0008] Patent Document 2 discloses a method for manufacturing an austenitic stainless steel sheet in which cold rolling conditions and straightening conditions using a tension leveler are adjusted, and further a tension equivalent to 0.2% yield strength or less of the cold-rolled material is applied to perform a strain relief heat treatment. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2005-320587 A [Patent Document 2] JP 2001-226718 A Summary of the Invention [Problem to be solved by the invention]
[0010] On the other hand, from the viewpoint of further increasing the strength of component materials, it is expected that precipitation strengthening can be utilized by applying SUS630, SUS631, etc. However, it is considered difficult to utilize precipitation strengthening by strain relief heat treatment at a low temperature range of 600°C or less as shown in Patent Document 1. As such, with conventional stainless steel sheets, it has been difficult to achieve high strength that meets the demand for thinner component materials and ensure the smoothness of the etched surface and the flatness before and after etching.
[0011] The object of the present invention is to provide a ferritic-austenitic duplex stainless steel sheet that can meet the demands for further miniaturization and weight reduction of parts used in electronic and precision instruments, and can also meet the demands for thinner component materials, while maintaining higher strength than conventional materials and having smoothness of the etched surface and flatness before and after etching. [Means for solving the problem]
[0012] In order to solve the above problems, the present inventors have intensively studied the use of precipitation strengthening in duplex stainless steel and the use of stress relief heat treatment, which has been conventionally performed as an aging heat treatment for precipitation strengthening. As a result, it has been found that precipitation strengthening can be effectively utilized by performing stress relief heat treatment at a temperature of over 700°C, which is higher than conventional, in duplex stainless steel made of specific components. In addition, by regulating the temperature range of stress relief heat treatment, the residual stress of the steel sheet caused by temper rolling and shape correction using a tension leveler can be reduced, and flatness before and after etching can be maintained. Furthermore, it has been found that the average crystal grain size can be achieved to a predetermined value or less, and the smoothness of the etched surface can be ensured. The present invention has been completed by clarifying the characteristics of the chemical composition and metal structure of the steel sheet that can achieve these effects.
[0013] The present invention has been made based on the above findings and further studies, and the gist of the present invention, which has the object of solving the above problems, is as follows.
[0014] [1] Chemical composition, by mass%, C: 0.02 to 0.10%, Si: 0.1 to 1.0%, Mn: 0.5-5.0%, Cr: 20.0-28.0%, Ni: 1.0-7.0%, Cu: 0.2-2.0%, Mo: 0.3-5.0%, N: 0.10-0.50%, Nb: 0-0.50%, Ti: 0 to 0.50%, V: 0 to 0.50%, W: 0 to 0.50%, Co: 0-0.50%, B: 0 to 0.0050%, Sn: 0-0.50%, Al: 0-0.50%, Mg: 0 to 0.010%, Ca: 0 to 0.0100%, Ta: 0 to 0.050%, Ga: 0 to 0.050%, Zr: 0 to 0.50%, and Rare earth elements: 0~0.010% with the remainder being Fe and impurities, The average crystal grain size is 2.0 μm or less, Vickers hardness is 450HV or more. The average particle diameter of the precipitate is 150 nm or less, The volume fraction of the precipitate is 0.50% or more. This is a ferritic-austenitic duplex stainless steel plate characterized by: [2] The ferritic-austenitic duplex stainless steel sheet according to [1] above, characterized in that in the metal structure, the ferritic phase ratio is 20 to 80%. [3] A ferritic-austenitic duplex stainless steel sheet according to [1] or [2] above, characterized in that the radius of curvature after half-etching is 150 mm or more. [4] A ferritic-austenitic duplex stainless steel sheet according to [1] or [2] above, characterized in that it is used for parts of electronic devices or precision instruments. [5] A ferritic-austenitic duplex stainless steel sheet according to the above [3], characterized in that it is used for parts of electronic devices or precision instruments. Effect of the Invention
[0015] According to the present invention, it is possible to provide a ferritic-austenitic duplex stainless steel sheet that has high strength capable of supporting further miniaturization of parts such as electronic devices and precision machinery, and that has a smooth etched surface and flatness before and after etching. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, a ferritic-austenitic duplex stainless steel sheet according to an embodiment of the present invention (hereinafter, also referred to as "duplex stainless steel sheet", "stainless steel sheet" or "steel sheet") will be described in detail.
[0017] 1. Ferritic-austenitic duplex stainless steel plate (chemical composition) First, the chemical composition of the duplex stainless steel sheet according to this embodiment will be described in detail. The austenite phase (γ phase) constituting the duplex stainless steel sheet according to this embodiment is composed of a stable γ phase that does not exhibit deformation-induced transformation. In other words, the chemical composition of the duplex stainless steel sheet according to this embodiment is a component system that does not exhibit deformation-induced transformation. The specific chemical composition will be described below. Note that, unless otherwise noted, % for element content in this specification means mass %.
[0018] C: 0.02 to 0.10% Carbon (C) is an element that acts as a stabilizing element for the austenite phase. C also has the effect of improving strength as a solid solution strengthening element. If the C content is less than 0.02%, the improvement in strength may be insufficient. Therefore, the C content is set to 0.02% or more. It is preferably 0.03% or more. If the C content exceeds 0.10%, Cr carbides may be excessively generated during cooling after finish annealing and stress relief heat treatment (especially stress relief heat treatment), which may reduce the corrosion resistance of the steel sheet. Therefore, the C content is set to 0.10% or less. It is preferably 0.09% or less, more preferably 0.07% or less.
[0019] Si: 0.1 to 1.0% Silicon (Si) is an element that acts as a stabilizing element for the ferrite phase. If the Si content is less than 0.1%, it will lead to an increase in manufacturing costs. Therefore, the Si content is set to 0.1% or more. It is preferably 0.2% or more, and more preferably 0.3% or more. On the other hand, if the Si content exceeds 1.0%, it will promote cracking during manufacturing. Therefore, the Si content is set to 1.0% or less. It is preferably 0.9% or less, more preferably 0.8% or less, and even more preferably 0.7% or less.
[0020] Mn: 0.5-5.0% Mn is an element that acts as a stabilizing element for the austenite phase. If the Mn content is less than 0.5%, the effect of suppressing the decrease in strength during strain relief heat treatment may not be obtained. Therefore, the Mn content is set to 0.5% or more. It is preferably set to 1.0% or more, and more preferably set to 1.5% or more. On the other hand, if the Mn content exceeds 5.0%, it will lead to an increase in manufacturing costs. Therefore, the Mn content is set to 5.0% or less. It is preferably set to 4.5% or less, and more preferably set to 4.0% or less.
[0021] Cr: 20.0~28.0% Chromium (Cr) is an element that acts on the phase ratio as a stabilizing element of the ferrite phase. Cr is also important as an element that generates Cr nitride precipitates during stress relief heat treatment. If the Cr content is less than 20.0%, the volume fraction of the precipitates is small, and strength may be insufficient. Therefore, the Cr content is set to 20.0% or more. It is preferably 20.5% or more, and more preferably 21.0% or more. On the other hand, if the Cr content exceeds 28.0%, manufacturability may be reduced. Therefore, the Cr content is set to 28.0% or less. It is preferably 27.0% or less, and more preferably 26.0% or less.
[0022] Ni: 1.0-7.0% Nickel (Ni) is an element that acts as a stabilizing element for the austenite phase. If the Ni content is less than 1.0%, the corrosion resistance may be insufficient. Therefore, the Ni content is set to 1.0% or more. It is preferably 1.3% or more, and more preferably 1.6% or more. On the other hand, if the Ni content exceeds 7.0%, it may lead to an increase in alloy costs and an impairment of manufacturability. Therefore, the Ni content is set to 7.0% or less. It is preferably 5.7% or less, and more preferably 5.4% or less.
[0023] Cu: 0.2-2.0% Copper (Cu) is an effective element that contributes to precipitation strengthening during strain relief heat treatment. In addition, Cu acts as an austenite stabilizing element in a solid solution state. If the Cu content is less than 0.2%, precipitates are not generated, and the strength of the steel sheet may be insufficient. Therefore, the Cu content is set to 0.2% or more. It is preferably 0.3% or more, and more preferably 0.4% or more. On the other hand, if the Cu content exceeds 2.0%, the effect of containing Cu on improving strength is saturated. Therefore, the Cu content is set to 2.0% or less. It is preferably 1.7% or less, and more preferably 1.4% or less.
[0024] Mo: 0.3-5.0% Molybdenum (Mo) is an element that acts as a stabilizing element for the ferrite phase. Mo also has the effect of improving strength as a solid solution strengthening element. If the Mo content is less than 0.3%, the strength improving effect may not be sufficiently obtained. Therefore, the Mo content is set to 0.3% or more. It is preferably 0.4% or more, more preferably 0.5% or more. On the other hand, if the Mo content exceeds 2.0%, the effect of improving strength by the solid solution strengthening is saturated. In addition, since Mo is an expensive element, excessive inclusion of Mo leads to an increase in manufacturing costs. Therefore, the Mo content is set to 5.0% or less. It is preferably 4.5% or less, more preferably 4.0% or less.
[0025] N: 0.10~0.50% Nitrogen (N), like C, is an element that stabilizes the austenite phase and acts as an effective solid solution strengthening element. In addition, N forms Cr nitrides during strain relief heat treatment, contributing to precipitation strengthening. However, N is an interstitial solid solution element that easily diffuses, and is thought to precipitate even in strain relief heat treatment at 700°C or less. If the N content is less than 0.10%, the volume fraction of the precipitates is small, so the strength may be insufficient. Therefore, the N content is 0.10% or more. It is preferably 0.12% or more, more preferably 0.14% or more. On the other hand, if the N content exceeds 0.50%, the average particle diameter of the precipitates increases excessively, so the strength may be insufficient. Therefore, the N content is 0.50% or less. It is preferably 0.45% or less, more preferably 0.40% or less.
[0026] The above is the basic chemical composition of the ferritic-austenitic stainless steel sheet of this embodiment, with the remainder being iron (Fe) and impurities. Furthermore, the ferritic-austenitic stainless steel sheet of this embodiment may optionally contain one or more of Nb, Ti, V, W, Co, B, and Sn in order to further improve workability, corrosion resistance, and hot workability. The lower limits of these elements are 0% or more, and preferably more than 0%.
[0027] Nb: 0.50% or less Niobium (Nb) forms nitrides (NbN) and carbides (NbC) and has the effect of improving workability. Therefore, the Nb content may be 0.01% or more. However, if the Nb content exceeds 0.50%, there is a risk of reducing ductility, so the Nb content is preferably 0.50% or less. The Nb content is more preferably 0.30% or less, and even more preferably 0.20% or less.
[0028] Ti: 0.50% or less Titanium (Ti), like Nb, forms nitrides (TiN) and carbides (TiC) and has the effect of improving workability. Therefore, the Ti content may be 0.01% or more. However, if the Ti content exceeds 0.50%, there is a risk of reducing ductility, so the Ti content is preferably 0.50% or less. The Ti content is more preferably 0.30% or less, and even more preferably 0.20% or less.
[0029] V: 0.50% or less Vanadium (V) forms nitrides and has the effect of improving workability. Therefore, the V content may be 0.01% or more. However, if the V content exceeds 0.50%, there is a risk of reducing ductility and hot workability, so the V content is preferably 0.50% or less, and more preferably 0.40% or less.
[0030] W: 0.50% or less Tungsten (W) is an element that improves corrosion resistance, and in order to exert this effect, the W content is preferably 0.05% or more. However, if the W content exceeds 0.50%, there is a risk of reducing workability, so the W content is preferably 0.50% or less, and more preferably 0.40% or less.
[0031] Co:0.50% or less Cobalt (Co) has the effect of increasing high-temperature strength and improving hot workability. Therefore, the Co content is preferably 0.01% or more. However, if the Co content exceeds 0.50%, there is a risk of reducing toughness, so the Co content is preferably 0.50% or less, and more preferably 0.30% or less.
[0032] B: 0.0050% or less Boron (B) is an element that segregates to grain boundaries and improves hot workability. To achieve this effect, the B content is preferably 0.0002% or more. However, if the B content exceeds 0.0050%, the corrosion resistance may be significantly deteriorated, so the B content is preferably 0.0050% or less, and more preferably 0.0030% or less.
[0033] Sn: 0.50% or less Tin (Sn) is an element that can improve corrosion resistance. To achieve this effect, the Sn content is preferably 0.01% or more, and more preferably 0.03% or more. However, if the Sn content exceeds 0.50%, there is a risk of deteriorating hot workability, so the Sn content is preferably 0.50% or less, and more preferably 0.4% or less.
[0034] Furthermore, the ferritic-austenitic stainless steel sheet of this embodiment may optionally contain one or more of Al, Ca, Mg, Ta, Ga, Zr, and rare earth elements for deoxidization and desulfurization during refining. The lower limit of these elements is 0% or more, preferably more than 0%.
[0035] Al: 0.50% or less Aluminum (Al) may be contained in small amounts for desulfurization and deoxidation. The above effects are exhibited when the Al content is 0.01%, so the Al content is preferably 0.01% or more. However, when the Al content exceeds 0.50%, there is a risk of increasing manufacturing defects and increasing raw material costs, so the Al content is preferably 0.50% or less.
[0036] Mg: 0.010% or less Magnesium (Mg) not only deoxidizes but also has the effect of refining the solidified structure. To achieve these effects, the Mg content is preferably 0.0002% or more. However, if the Mg content exceeds 0.010%, it will increase the cost of the steelmaking process, so the Mg content should be 0.010% or less.
[0037] Ca:0.0100% or less A small amount of calcium (Ca) may be contained for desulfurization and deoxidization. The above effects are exhibited when the Ca content is 0.0001% or more, so the Ca content is preferably 0.0001% or more. However, if the Ca content exceeds 0.0100%, there is a risk of hot work cracking and a decrease in corrosion resistance, so the Ca content is preferably 0.0100% or less, and more preferably 0.0050% or less.
[0038] Ta:0.050% or less Tantalum (Ta) is an element that improves corrosion resistance by modifying inclusions, and may be contained as necessary. In order to exert this effect, the Ta content is preferably 0.0002% or more. However, if the Ta content exceeds 0.050%, there is a risk of causing a decrease in room temperature ductility and toughness, so the Ta content is preferably 0.050% or less, more preferably 0.030% or less.
[0039] Ga: 0.050% or less Gallium (Ga) is an element that improves corrosion resistance and suppresses hydrogen embrittlement, and may be contained as necessary. In order to exert this effect, the Ga content is preferably 0.0002% or more. However, if the Ga content exceeds 0.050%, there is a risk of causing a decrease in workability, so the Ga content is preferably 0.050% or less, and more preferably 0.030% or less.
[0040] Zr: 0.50% or less Zirconium (Zr) has a similar effect to Nb and Ti, and is also an element that improves oxidation resistance. To achieve these effects, the Zr content is preferably 0.01% or more. However, if the Zr content exceeds 0.50%, it will lead to an increase in raw material costs, so the Zr content is preferably 0.50% or less, and more preferably 0.30% or less.
[0041] Rare earth elements: 0.010% or less Rare earth elements (REM) are elements that improve hot workability. The above effects are achieved when the total content of rare earth elements is 0.0002% or more, so the content of rare earth elements may be 0.0002% or more. However, if the total content of rare earth elements exceeds 0.010%, manufacturability is impaired and costs increase, so the upper limit of rare earth elements is preferably 0.010%. A more preferable content range of rare earth elements is 0.0005 to 0.008%.
[0042] Here, rare earth elements (REM) refer to two elements, scandium (Sc) and yttrium (Y), and 15 elements (lanthanoids) from lanthanum (La) to lutetium (Lu). In this specification, "rare earth elements" refers to one or more elements selected from these rare earth elements, and "content of rare earth elements" refers to the total amount of rare earth elements.
[0043] The stainless steel sheet of this embodiment contains, in addition to the elements described above, Fe and impurities (including unavoidable impurities). However, in addition to the elements described above, other elements can also be contained within a range that does not impair the effects of the present invention.
[0044] In addition, scrap materials are often used in the manufacture of stainless steel sheets. Therefore, various impurity elements are often inevitably mixed into the stainless steel sheets, and it is difficult to determine the content of the impurity elements uniquely. Therefore, the impurities in this embodiment refer to elements contained in an amount that does not impair the effects of the present invention.
[0045] (Metal structure) In the metal structure of the ferritic-austenitic duplex stainless steel sheet of this embodiment, when the ferritic phase ratio is within a predetermined range, the average crystal grain size can be easily refined. The ferritic phase ratio is preferably 20% or more and 80% or less, more preferably 25% or more and 75% or less, and even more preferably 30% or more and 70% or less. It is considered that the ferritic phase and the austenitic phase each suppress the grain growth of the other, thereby refining the crystal grains. Therefore, the ferritic phase ratio is most preferably 50%.
[0046] (Average grain size) In order to obtain excellent smoothness of the etched surface, it is effective to make the average crystal grain size 2.0 μm or less. If the average crystal grain size exceeds 2.0 μm, the etched surface becomes rough, and good smoothness of the etched surface cannot be obtained. The average crystal grain size is preferably 1.5 μm or less, and more preferably 1.0 μm or less. The lower limit of the average crystal grain size is not particularly limited, but may be 0.4 μm or more for practical purposes.
[0047] (Vickers hardness) As a material that can accommodate the miniaturization and weight reduction of electronic devices and precision machinery, it is effective for the steel plate to have a Vickers hardness (hereinafter also simply referred to as "hardness") of 450 HV or more. The hardness is preferably 455 HV or more, and more preferably 460 HV or more. On the other hand, the upper limit of the hardness is not particularly limited, but may be 485 HV or less for practical use. On the other hand, if the hardness is less than 450 HV, the strength required for the component material cannot be ensured.
[0048] In the ferritic-austenitic duplex stainless steel sheet of this embodiment, in order to ensure a hardness of 450 HV or more, it is effective that the average particle diameter (average grain size, average diameter) of the precipitates is 150 nm or less. The average particle diameter of the precipitates is preferably 130 nm or less, and more preferably 110 nm or less.
[0049] From the viewpoint of hardness, it is also effective that the volume fraction of the precipitates is 0.50% or more. The volume fraction of the precipitates is preferably 0.75% or more, and more preferably 1.00% or more. If either the average particle diameter or the volume fraction of the precipitates does not satisfy the above range, a hardness of 450 HV or more cannot be obtained. Note that the "precipitates" referred to in this specification are not particularly limited, and examples thereof include Cu-based precipitates (Cu particles) and Cr nitrides (CrN, Cr2N).
[0050] The average particle diameter and volume fraction of the precipitates can be measured by the following method. First, a thin film sample is prepared from a position of 1 / 4 the thickness of the steel sheet, and an image is taken with a transmission electron microscope (TEM). Here, the average particle diameter and volume fraction of the precipitates are measured using the image. The TEM magnification is 30,000 times for measuring the average particle diameter, and 10,000 times for measuring the volume fraction. It is considered that the precipitation strengthening in the ferritic-austenitic duplex stainless steel sheet of this embodiment is mainly achieved by precipitates mainly composed of Cu. The precipitates also include Cr nitrides containing elements such as Cr, Fe, N, and C, and are presumed to play a part in the precipitation strengthening. Here, for convenience, they are collectively referred to as "Cr nitrides". However, Cr nitrides precipitate even in strain relief heat treatment at 700°C or less, and are considered to contribute to the strength of general ferritic-austenitic duplex stainless steels containing N after general strain relief heat treatment. The precipitates can be identified by composition analysis using TEM-EDX, and Cr nitrides can also be confirmed.
[0051] The average particle diameter of the precipitates can be determined by the following method. The area of one precipitate is measured using the image analysis software "Image J" and converted into a circle equivalent diameter. The above measurement and conversion are performed for 100 or more precipitates, and the average value is defined as the average particle diameter of the precipitates. The precipitates to be measured are various precipitates regardless of their type. However, as described above, the precipitates in the duplex stainless steel of this embodiment are mainly Cu particles and Cr nitrides, and since these are considered to contribute greatly to precipitation strengthening, the measurement targets may be mainly Cu particles and Cr nitrides. The measurement targets may include precipitates other than Cu particles and Cr nitrides.
[0052] The volume fraction of precipitates can be determined by the following method. First, the total area of the precipitates in the TEM image is calculated using the image analysis software "Image J". The total area of the precipitates is then divided by the total area of the photographed field of view to calculate the percentage of the precipitates in the photographed field of view. In this embodiment, the percentage of the precipitates in the photographed field of view is defined as the volume fraction of the precipitates.
[0053] (Radius of curvature after half etching) In order to obtain flatness of the steel sheet before and after etching, it is effective that the radius of curvature after half etching is 150 mm or more. The radius of curvature after half etching is preferably 160 mm or more, and more preferably 170 mm or more. On the other hand, the upper limit of the radius of curvature after half etching is desirably ∞ (infinity), i.e., no warping, and is not particularly limited, but may be 400 mm or less in practical use.
[0054] The term "half etching" used here refers to etching one of the rolled surfaces of a steel sheet in the sheet thickness direction until the sheet thickness is reduced to half. Half etching is performed by coating the rolled surface with nail polish and immersing it in an etching solution such as ferric chloride.
[0055] (Thickness) The thickness of the duplex stainless steel plate according to this embodiment is not particularly limited, but may be 3.0 to 0.05 mm. Preferably, it is 0.08 mm or more. Furthermore, by making the thickness 1.5 mm or less, it becomes easy to refine the metal structure, and the above-mentioned metal structure can be easily ensured. The thickness may be 1.0 mm or less. Preferably, it is 0.5 mm or less.
[0056] 2. Manufacturing method of ferritic-austenitic duplex stainless steel sheet (Manufacturing method) A method for manufacturing the ferritic-austenitic duplex stainless steel sheet of this embodiment will now be described. The ferritic-austenitic duplex stainless steel sheet according to the present embodiment can achieve the above-mentioned effects regardless of the manufacturing method. However, in order to achieve both strength, smoothness of the etched surface, and flatness before and after etching, it is necessary to control the metal structure (particularly the average crystal grain size, precipitate size, and precipitate ratio) and hardness as described above. The above-mentioned metal structure and hardness can be achieved by combining the chemical composition of the steel with appropriate manufacturing conditions. A preferred manufacturing method for obtaining the ferritic-austenitic duplex stainless steel sheet of this embodiment will be described below.
[0057] First, a steel slab having the above-mentioned chemical composition, which is produced by continuous casting or ingot casting after melting, is hot-rolled into a steel sheet (hot rolling process). Then, a hot-rolled sheet annealing process, a pickling process, and a cold rolling process are performed to obtain a cold-rolled sheet having a predetermined thickness. The hot-rolled sheet annealing may be performed as necessary, and may be omitted. Each of the above processes may be a general manufacturing method for ferritic-austenitic duplex stainless steel sheet.
[0058] (Finish annealing process) Finish annealing is performed on the cold-rolled steel sheet controlled to a predetermined thickness in the cold rolling process. The finish annealing temperature is 850°C or more and 1050°C or less. If the finish annealing temperature is less than 850°C, the metal structure will be a mixture of recrystallized grains and non-recrystallized grains, resulting in a state in which the hardness between the crystal grains varies. If the hardness varies between the crystal grains, good flatness cannot be obtained after shape correction by a tension leveler. On the other hand, if the finish annealing temperature exceeds 1050°C, the average crystal grain size after the finish annealing will become coarse, and the average crystal grain size after the distortion relief heat treatment will also become coarse. Therefore, the finish annealing temperature is 850°C or more and 1050°C or less. The annealing time (holding time) in the finish annealing process can be set appropriately. Typically, it is 600 seconds or less. It is preferably 400 seconds or less, more preferably 150 seconds or less. From the viewpoint of recrystallization, the lower limit of the annealing time in the final annealing step may be set to 5 seconds or more.
[0059] After the finish annealing process, the steel sheet is cooled to room temperature (around 25°C). The average cooling rate during cooling may be 1°C / sec to 100°C / sec. If the average cooling rate is less than 1°C / sec, grain growth may occur during the cooling process. In addition, taking into consideration productivity and pickling properties, the average cooling rate is preferably 5 to 50°C / sec. Here, the "average cooling rate" is defined as the temperature drop of the steel sheet from the start of cooling (end of holding) to room temperature divided by the time required to cool from the start of cooling to room temperature.
[0060] (Temper rolling process) After the finish annealing process, temper rolling is performed (temper rolling process). Temper rolling is a process for improving the strength of the material (steel plate). The temper rolling in this embodiment may be a common manufacturing method in stainless steel manufacturing, and the temper rolling reduction ratio may be adjusted according to the desired strength. For example, the temper rolling ratio may be 40 to 70%. Note that the austenite phase of the ferritic-austenitic duplex stainless steel in this embodiment is in a stable state, and deformation-induced martensite is not generated during temper rolling.
[0061] (shape correction process) The steel sheet after the temper rolling is repeatedly bent while applying a tension of 0.5 to 3.0% elongation by a tension leveler, thereby performing shape correction (shape correction process). Shape correction by a tension leveler is a process for ensuring the flatness of the steel sheet, and is usually controlled by the elongation. The shape correction process in this embodiment can be performed under general conditions in the production of ferritic-austenitic duplex stainless steel sheets, but it is preferable to set the elongation to 0.5 to 3.0%. If the elongation is less than 0.5%, warping after half etching may become large. On the other hand, if the elongation exceeds 3.0%, hardening may occur in the production line. From the viewpoint of stable production, the elongation is preferably in the range of 0.5% to 1.5%.
[0062] (Distortion heat treatment process) The steel sheet after the shape correction by the tension leveler is subjected to a stress relief heat treatment at a temperature range of 720°C or more and 780°C or less (strain relief heat treatment process). By the stress relief heat treatment in this temperature range, the residual stress caused by the temper rolling and the shape correction by the tension leveler is significantly reduced, and precipitation strengthening is achieved. If the temperature range of the stress relief heat treatment is 720°C or more, the flatness before and after the etching process can be ensured, but if it is less than 720°C, the volume fraction of the precipitates is small, and the strength is insufficient. On the other hand, if it exceeds 780°C, the flatness before and after the etching process can be ensured, but the average particle diameter of the precipitates becomes coarse, and the strength is insufficient. Therefore, the temperature of the stress relief heat treatment is 720°C or more and 780°C or less. It is preferably 725°C or more and 775°C or more.
[0063] The process described above makes it possible to manufacture the ferritic-austenitic duplex stainless steel sheet according to this embodiment. EXAMPLES
[0064] In order to confirm the effects of the present invention in detail, the following experiment was carried out. Note that this example shows one embodiment of the present invention, and the present invention is not limited to the following configuration.
[0065] Steel having the chemical composition shown in Table 1 was melted to obtain an ingot having a thickness of 100 mm. The ingot was then heated to 1230°C, and hot-rolled to obtain a hot-rolled sheet having a thickness of 5.0 mm. The hot-rolled sheet was then annealed (annealing temperature: 1070°C, annealing time: 45 seconds), and cold-rolled with intermediate annealing repeatedly performed to obtain a cold-rolled sheet having a thickness of 0.18 to 0.33 mm. The cold-rolled sheet was then heated at the finish annealing temperature in Table 2 for 60 seconds, and then cooled to room temperature to obtain a finish annealed sheet. The finish annealed sheet was then subjected to temper rolling at the temper rolling rate and tension leveler elongation (TL elongation) shown in Table 2, and shape correction was performed with a tension leveler (TL) to obtain a steel sheet having a thickness of 0.10 mm. The steel sheet was then subjected to strain relief heat treatment for 60 seconds under the conditions shown in Table 2 to obtain a duplex stainless steel sheet. The resulting duplex stainless steel sheets were subjected to the following various evaluation tests.
[0066] (Method of measuring average crystal grain size) The average crystal grain size was determined as follows: The L-section (plane including the rolling direction and the sheet thickness direction) of the steel sheet prepared by electrolytic polishing was measured by electron backscatter diffraction (EBSD). The measurement area was 100 μm × 300 μmL at the center of the sheet thickness, and the measurement step size was 0.1 μm. Using the analysis software "OIM-Analysis" made by TSL Solutions, plot data with a Confidence Index value of more than 0.1 was extracted from the measured data, and the average grain size was calculated by quadrature. If the crystal orientation difference between adjacent plot data was less than 15°, they were considered to be the same grain, and if the orientation difference was 15° or more, they were treated as different grains. In addition, no distinction was made between the ferrite phase and the austenite phase when calculating the average grain size.
[0067] (Method of measuring average particle diameter and volume fraction of precipitates) First, a thin film sample was prepared from 1 / 4 the thickness of the steel plate, and images were taken with a transmission electron microscope (TEM). The images were used to measure the average particle diameter and volume fraction of the precipitates. The TEM magnification was 30,000 times for measuring the average particle diameter, and 10,000 times for measuring the volume fraction. The precipitates were identified through composition analysis using TEM-EDX.
[0068] The average particle diameter of the precipitates was determined as follows: First, the area of one precipitate was measured using image analysis software and converted into a circle-equivalent diameter. The above measurement and conversion were performed for 100 or more precipitates, and the average value was defined as the average particle diameter of the precipitates.
[0069] The volume fraction of the precipitates was determined as follows: First, the total area of precipitates in the TEM image was calculated using image analysis software "Image J". The total area of precipitates was then divided by the total area of the photographed field of view to calculate the percentage of precipitates in the photographed field of view. In this example, the percentage of precipitates in the photographed field of view was defined as the volume fraction of precipitates. When no precipitates mainly composed of Cu or Cr nitrides were observed in the photographed field of view, the items "average particle diameter" and "volume fraction" in Table 2 were written as "no precipitates".
[0070] (Hardness measurement method) The hardness of the steel plate surface was measured using a Vickers hardness tester in accordance with JIS Z 2244:2009. The steel plate surface was measured 10 times under a load of 0.5 kgf, and the average value was calculated and used as the representative value. If the hardness of the steel plate was 450 HV or more, it was determined to be high strength.
[0071] (Method of measuring ferrite phase ratio) The measurement of the ferrite phase ratio was specified as follows: Cut out multiple test pieces of thickness t x 40 mm from the steel plate, stack them so that the total thickness is 2 mm or more, and measure them using a ferrite meter. The measurement is carried out five times, and the average value is the ferrite phase ratio of the steel plate.
[0072] (Evaluation test of smoothness of etched surface) One surface of a test piece cut from a steel plate with a thickness of 0.1 mm x 50 mm x 50 mm was etched by spraying an aqueous solution of ferric chloride with a specific gravity of 1.35 heated to 50°C for 4 minutes. The smoothness of the etched surface was measured using a contact surface roughness meter to measure the arithmetic mean roughness Ra along the direction perpendicular to the rolling direction. If Ra was 0.6 μm or less, the etched surface was judged to have good smoothness (passed).
[0073] (Evaluation test of flatness before and after etching) A test piece measuring 0.1 mm thick x 12 mm wide x 100 mm wide was cut from the steel plate, which was then half-etched in an aqueous solution of ferric chloride. The radius of curvature of the test piece was measured when the thickness had been reduced by half. If the radius of curvature after half-etching was 150 mm or more, the test piece was deemed to have passed the test, as it had the necessary flatness before and after etching.
[0074] The results of the various evaluation tests are shown in Table 2. Note that the underlines in Tables 1 and 2 indicate that the results are outside the scope of the present invention or the preferred manufacturing conditions and properties of the present invention. Inventive Examples Nos. 1 to 21 and 32 to 41, in which the chemical composition, hardness, average crystal grain size, average particle diameter of precipitates, volume fraction of precipitates, and radius of curvature after half-etching were within the prescribed ranges, all satisfied the high strength, smoothness of the etched surface, and flatness before and after etching. In addition, in these inventive examples as well as the comparative examples described later, the radius of curvature of the steel sheet before half-etching was almost ∞ (infinity), and the steel sheet was adjusted to a flat shape without warping.
[0075] In No. 22, the temperature of the stress relief heat treatment was too low, so the volume fraction of precipitates was smaller than the specified value, and the strength was insufficient.
[0076] In No. 23, the temperature of the stress relief heat treatment was too high, which resulted in the average particle diameter of the precipitates becoming larger than the specified value, and the strength was insufficient.
[0077] No. 24 had insufficient strength due to an insufficient N content. No. 25 had insufficient strength due to excessive N content.
[0078] No. 26 had insufficient strength due to an insufficient Cr content. No. 27 had insufficient strength due to an insufficient Cu content.
[0079] Nos. 28 to 30 had steel compositions outside the range of the present invention, and therefore all of them had insufficient strength.
[0080] No. 31 is a ferritic stainless steel. In No. 31, the grains grew rapidly during the finish annealing, and the average crystal grain size became coarse, which resulted in insufficient smoothness of the etched surface. The strength was also insufficient.
[0081] In No. 32, the temperature of the finish annealing was too high, which caused the average crystal grain size to become coarse, resulting in insufficient smoothness of the etched surface and insufficient strength. For No. 33, the temperature of the final annealing was too low, resulting in a metal structure with a mixture of recrystallized and non-recrystallized grains, which resulted in variation in hardness between the crystal grains, and therefore good flatness could not be obtained after shape correction using a tension leveler. Note that, since good flatness could not be obtained after shape correction, a half-etching test was not performed on No. 33.
[0082] [Table 1]
[0083] [Table 2A]
[0084] [Table 2B] [Industrial Applicability]
[0085] The ferritic-austenitic duplex stainless steel sheet of the present invention combines high strength, flatness before and after etching, and smoothness of the etched surface. In other words, by using the ferritic-austenitic duplex stainless steel sheet of the present invention as a component material, it is expected that, for example, electronic devices and precision machinery that are etched during component manufacturing will be made smaller and lighter.
Claims
1. Chemical composition, in mass%, C: 0.02-0.10%, Si: 0.1-1.0%, Mn: 0.5-5.0%, Cr: 20.0-28.0%, Ni: 1.0 to 7.0%, Cu: 0.2-2.0%, Mo: 0.3 to 5.0%, N: 0.10-0.50%, Nb: 0 to 0.50%, Ti: 0 to 0.50%, V: 0 to 0.50%, W: 0 to 0.50%, Co: 0 to 0.50%, B: 0 to 0.0050%, Sn: 0 to 0.50%, Al: 0-0.50%, Mg: 0 to 0.010%, Ca: 0-0.0100%, Ta: 0 to 0.050%, Ga: 0 to 0.050%, Zr: 0 to 0.50%, and Rare earth elements: 0-0.010% with the remainder being Fe and impurities, The average crystal grain size is 2.0 μm or less, Vickers hardness is 450 HV or more, The average particle diameter of the precipitate is 150 nm or less; The volume fraction of the precipitate is 0.50% or more. The ferritic-austenitic duplex stainless steel sheet is characterized by the above.
2. 2. The ferritic-austenitic duplex stainless steel sheet according to claim 1, characterized in that in the metal structure, the ferritic phase ratio is 20 to 80%.
3. 3. The ferritic-austenitic duplex stainless steel sheet according to claim 1, wherein the radius of curvature after half etching is 150 mm or more.
4. 3. The ferritic-austenitic duplex stainless steel sheet according to claim 1 or 2, which is used for parts of electronic devices or precision devices.
5. The ferritic-austenitic duplex stainless steel sheet according to claim 3, which is used for parts of electronic devices or precision instruments.
Citation Information
Patent Citations
High-strength stainless steel sheet with plural phases for welded structure, and manufacturing method therefor
JP2003328083A
Ferritic-austenitic stainless steel sheet having excellent press formability, and method for producing the same
JP2011184792A
Ferrite-austenite 2-phase stainless steel plate for fastening parts, fastening parts using the same, and spot welding method
JP2022023289A
Ferritic-austenitic two-phase stainless steel material and method for manufacturing same
WO2017141907A1
Welded structure and storage tank
WO2021201122A1