((METH)acrylic acid-based copolymer and producing method thereof, water treatment agent as well as scale adhesion prevention agent
A (meth)acrylic acid-based copolymer with specific monomer units addresses the issues of foaming and scale formation in water treatment agents, providing transparent and effective scale inhibition for silica, calcium phosphate, and calcium sulfate scales in piping systems.
Patent Information
- Application Number
- JP2023048458
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing water treatment agents used to suppress scale formation in piping systems are prone to foaming and lack transparency, and are ineffective against silica, calcium phosphate, calcium carbonate, and calcium sulfate scales.
A (meth)acrylic acid-based copolymer containing specific monomer units in a controlled ratio, including (meth)acrylic acid, unsaturated dicarboxylic acids, 2-acrylamido-2-methylpropanesulfonic acid, and vinyl or aromatic vinyl monomers, is used to form a transparent aqueous solution that minimizes foaming and inhibits scale formation.
The copolymer effectively suppresses the formation of silica, calcium phosphate, and calcium sulfate scales in piping systems, maintaining transparency and preventing foaming, thus enhancing the efficiency and handling of water treatment agents.
Smart Images

Figure 2024137086000001 
Figure 2024137086000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a water treatment agent or a scale adhesion inhibitor that satisfactorily inhibits the formation of scale containing at least silica among silica, calcium phosphate, calcium carbonate, and calcium sulfate, as well as a (meth)acrylic acid-based copolymer suitable as a main component thereof, and a method for producing the same. [Background technology]
[0002] Conventionally, water has been used in various industries, and water is usually transported through piping. However, repeated transport or retention of water can cause scale to form on the inner surface of the piping, including silicon compounds, calcium compounds, magnesium compounds, zinc compounds, etc., and therefore treatment agents (water treatment agents) that suppress such scale formation are used.
[0003] For example, Patent Document 1 describes a method for preventing the prevalence of silica or silicate formation in an aqueous system, comprising adding to the system: a) a water-soluble copolymer or terpolymer of (meth)acrylic acid or maleic acid or a salt thereof having a weight average molecular weight of about 1,000 to about 25,000, wherein the copolymer is composed of 1) about 20 to about 85% by weight of (meth)acrylic acid or maleic acid, and 2) greater than about 11 to about 80% by weight of (meth)acrylamidomethylpropanesulfonic acid or styrenesulfonic acid, or 3) about 5 to about 30% by weight of (meth)acrylamide or a substituted (meth)acrylamide, or 4) about 30 to about 60% by weight of isobutylene or diisobutylene, and the terpolymer is composed of 1) about 30 to about 80% by weight of (meth)acrylic acid or maleic acid, and 2) greater than about 11 to about 65% by weight of (meth)acrylamidomethylpropanesulfonic acid or styrenesulfonic acid. A method is disclosed which comprises adding an effective amount of a scale inhibitor selected from the group consisting of styrene sulfonic acid, 3) about 5 to about 30% by weight of (meth)acrylamide or substituted (meth)acrylamide, or 4) about 5 to about 30% by weight of vinyl alcohol, allyl alcohol, esters of vinyl or allyl alcohol, vinyl esters, styrene, isobutylene or diisobutylene, or 5) about 3 to about 30% by weight of styrene sulfonic acid when (meth)acrylaminomethylpropanesulfonic acid is present, b) magnesium ions, c) a mixture of said copolymer or terpolymer with aluminum ions or magnesium ions, or d) a mixture of poly(meth)acrylic acid or polymaleic acid or a salt thereof having a weight average molecular weight of about 1000 to about 25000 with aluminum ions or magnesium ions.
[0004] Patent Document 2 describes a method for stabilizing an aqueous system by suppressing precipitation of an inorganic salt, which comprises adding to the aqueous system: (a1) 40 to 60% by weight of an unsaturated sulfonic acid selected from one or more of 2-acrylamido-2-methyl-1-propanesulfonic acid, 2-methacrylamido-2-methyl-1-propanesulfonic acid, 3-methacrylamido-2-hydroxy-1-propanesulfonic acid, or a salt thereof; and (b1) a water-soluble polymer having a weight average molecular weight of about 3,000 to about 10,000 and having monomer units of 40 to 60% by weight of an unsaturated carboxyl monomer selected from acrylic acid, methacrylic acid, or a salt thereof; or (a2) 2-acrylamido-2-methyl-1-propanesulfonic acid, 2-methacrylamido-2-methyl-1-propanesulfonic acid, 3-methacrylamido-2-hydroxy-1-propanesulfonic acid, or a salt thereof. (b2) 30 to 60% by weight of an unsaturated sulfonic acid selected from the above; (b3) 35 to 65% by weight of an unsaturated carboxyl monomer selected from acrylic acid or methacrylic acid or a salt thereof; and (c2) a water-soluble polymer having a weight average molecular weight of about 3,000 to about 12,000, the water-soluble polymer having monomer units of 0.1 to 10% by weight of an unsaturated non-ionizable monomer selected from one or more of tert-butylacrylamide, tert-octylacrylamide, dimethylacrylamide, acrylamide, acryloylmorpholine, styrene, ethyl acrylate, butyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl acrylate; the aqueous system includes inorganic ions selected from one or more of iron, zinc, calcium, phosphate, or molybdate ions; and maintaining the aqueous system at a temperature greater than about 80° C.
[0005] Patent Document 3 discloses an acrylic acid-based copolymer that contains a structural unit (x) derived from acrylic acid or a sodium salt thereof and a structural unit (y) derived from 2-acrylamido-2-methylpropanesulfonic acid or a sodium salt thereof, and the content ratios of the structural unit (x) and the structural unit (y) are 35 to 90 mass% and 10 to 65 mass%, respectively, when the total of the two is taken as 100 mass%, and the content ratio of the acrylic acid-based copolymer having a weight average molecular weight Mw of 2000 to 30000 and a molecular weight of 70000 or more is 0.30 mass% or less relative to the total amount of all polymers. It is also disclosed that this acrylic acid-based copolymer is suitable as a component of a water treatment agent having an effect of suppressing scale formation on calcium phosphate.
[0006] Patent Document 4 discloses a calcium phosphate-based and silica-based scale inhibitor as a treatment agent for effectively preventing adhesion of calcium phosphate-based and silica-based scale to heat exchangers and the like in open circulating cooling water systems, which is characterized in that the active ingredient is a copolymer of (meth)acrylic acid, (meth)acrylamidomethylpropanesulfonic acid, and a (meth)acrylamide derivative having an alkyl group having 1 to 8 carbon atoms, the copolymer having 40 to 70 weight % of structural units derived from (meth)acrylic acid, 15 to 40 weight % of structural units derived from (meth)acrylamidomethylpropanesulfonic acid, and 5 to 25 weight % of structural units derived from a (meth)acrylamide derivative having an alkyl group having 1 to 8 carbon atoms, and the copolymer containing a skeleton derived from a hypophosphorous acid compound in the polymer chain, based on 100 weight % of structural units derived from all monomers. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 4-356580 [Patent Document 2] Japanese Patent Application Publication No. 8-224597 [Patent Document 3] International Publication No. 2016 / 047267 [Patent Document 4] JP 2018-130702 A Summary of the Invention [Problem to be solved by the invention]
[0008] Water treatment agents used to inhibit scale formation are usually aqueous solutions, and it is preferable for such water treatment agents to be transparent, since it is easy to visually determine whether or not they have acted on the water to be treated.Furthermore, since the scale formation inhibition effect of active ingredients such as polymers is easily exerted, it is preferable for the water treatment agent to be less likely to generate foaming when mixed with water containing precursor components that form scale components, such as silica, calcium phosphate, calcium carbonate, or calcium sulfate. An object of the present invention is to provide a (meth)acrylic acid-based copolymer which, when made into an aqueous solution, provides a water treatment agent and a scale adhesion inhibitor which have excellent transparency and are less likely to foam when mixed with water (water to be treated) containing precursor components that form silica, calcium phosphate, calcium carbonate, calcium sulfate, etc., and which satisfactorily suppresses the formation of scale containing at least silica out of the group consisting of silica, calcium phosphate, calcium carbonate, and calcium sulfate, in the mixed liquid, and a method for producing the same. [Means for solving the problem]
[0009] The present inventors have discovered a monomer unit derived from at least one monomer selected from the group consisting of (meth)acrylic acid and salts thereof, at least one monomer selected from the group consisting of unsaturated dicarboxylic acids and salts thereof, and unsaturated dicarboxylic anhydrides, and at least one monomer selected from the group consisting of 2-acrylamido-2-methylpropanesulfonic acid and salts thereof, each of which has a solubility of more than 7 g in 100 mL of water at 20° C. or 30° C.; a vinyl monomer having a solubility of 7 g or less in 100 mL of water at 20° C. or 30° C.; and an aromatic vinyl monomer having a solubility of 7 g or less in 100 mL of water at 20° C. or 30° C. and monomer units derived from at least one monomer selected from the group consisting of: and when a (meth)acrylic acid-based copolymer containing these four types of monomer units in a specific ratio is dissolved in water, a transparent aqueous solution can be obtained. It has been found that when this aqueous solution is used as a water treatment agent and brought into contact with water (water to be treated) containing precursor components that form silica, calcium phosphate, calcium carbonate, or calcium sulfate, foaming is unlikely to occur, and in each mixed solution of the water treatment agent and each water to be treated, the formation of scale containing these compounds is suppressed.
[0010] The present invention is illustrated below. [1] A (meth)acrylic acid-based copolymer consisting of the following monomer units (a), (b), (c) and (d): (a) a monomer unit derived from at least one monomer (ma) selected from the group consisting of (meth)acrylic acid and salts thereof; (b) a monomer unit derived from at least one monomer (mb) selected from the group consisting of unsaturated dicarboxylic acids and their salts, and unsaturated dicarboxylic anhydrides; (c) a monomer unit derived from at least one monomer (mc) selected from the group consisting of 2-acrylamido-2-methylpropanesulfonic acid and its salts; (d) a monomer unit derived from at least one monomer (md) selected from the group consisting of vinyl monomers having a solubility of 7 g or less in 100 mL of water at 20° C. or 30° C. and aromatic vinyl monomers; When the total amount of the monomer units (a), (b), (c) and (d) is taken as 100 mass%, the content ratios of the monomer units (a), (b), (c) and (d) are 65.1 to 95.7 mass%, 0.1 to 30.7 mass%, 4.1 to 29.9 mass% and 0.1 to 4.9 mass%, respectively. (Meth)acrylic acid-based copolymer. [2] The (meth)acrylic acid copolymer according to the above [1], which has a weight average molecular weight of 1,500 to 20,000. [3] The (meth)acrylic acid-based copolymer according to the above [2], wherein the content of the (meth)acrylic acid-based copolymer having a molecular weight of 1,000 or less is 15.0 mass% or less, and the content of the (meth)acrylic acid-based copolymer having a molecular weight of 200,000 or more is 0.10 mass% or less, based on the total amount of the (meth)acrylic acid-based copolymer. [4] A method for producing the (meth)acrylic acid-based copolymer described in [1] above, a preparation step of preparing a monomer mixture containing the monomer (ma), the monomer (mb), the monomer (mc), the monomer (md) and water; a polymerization step of continuously supplying the monomer mixture, a polymerization initiator, and an optional chain transfer agent to a reactor to polymerize the monomers; The method for producing a (meth)acrylic acid-based copolymer includes the steps of: [5] The method for producing a (meth)acrylic acid-based copolymer according to the above [4], wherein in the polymerization step, the time for supplying the monomer mixture to the reactor is 2 to 12 hours. [6] The method for producing a (meth)acrylic acid-based copolymer according to [5] above, wherein in the polymerization step, polymerization of the monomers is carried out while maintaining a residual concentration of the monomers (md) in the reactor of 0.3 g / 100 mL or less in total. [7] A water treatment agent containing the (meth)acrylic acid-based copolymer described in [1] above. [8] An agent for preventing adhesion of calcium phosphate scale, calcium carbonate scale, calcium sulfate scale, and silica scale, comprising the (meth)acrylic acid-based copolymer described in [1] above.
[0011] In this specification, the weight average molecular weight (hereinafter also referred to as "Mw") and number average molecular weight (hereinafter also referred to as "Mn") of the polymer are values calculated as standard sodium polyacrylate measured by gel permeation chromatography (hereinafter also referred to as "GPC"). In addition, the term "(meth)acrylic" means acrylic and methacrylic. Effect of the Invention
[0012] When the (meth)acrylic acid-based copolymer of the present invention is dissolved in water, a transparent aqueous solution can be obtained, and when this aqueous solution is used as a water treatment agent and contacted with water (water to be treated) containing precursor components that form silica, calcium phosphate, calcium carbonate, or calcium sulfate, foaming is unlikely to occur, and the formation of scale containing at least silica among silica, calcium phosphate, calcium carbonate, and calcium sulfate can be suitably suppressed in a mixture of the water treatment agent and each water to be treated. Therefore, the (meth)acrylic acid-based copolymer of the present invention can also be used as a drug component that prevents the adhesion of scale containing at least silica among silica, calcium phosphate, calcium carbonate, and calcium sulfate to the inner surface of a pipe or the like that comes into contact with water (water to be treated) containing precursor components that form scale. According to the method for producing a (meth)acrylic acid-based copolymer of the present invention, a (meth)acrylic acid-based copolymer having the above-mentioned effects can be efficiently produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The (meth)acrylic acid-based copolymer of the present invention (hereinafter referred to as "(meth)acrylic acid-based copolymer (P)") is characterized in that it comprises the following monomer units (a), (b), (c) and (d), and when the total of these monomer units (a), (b), (c) and (d) is taken as 100 mass%, the contents of the monomer units (a), (b) and (c) are 65.1 to 95.7 mass%, 0.1 to 30.7 mass%, 4.1 to 29.9 mass% and 0.1 to 4.9 mass%, respectively. (a) a monomer unit derived from at least one monomer (ma) selected from the group consisting of (meth)acrylic acid and salts thereof; (b) a monomer unit derived from at least one monomer (mb) selected from the group consisting of unsaturated dicarboxylic acids and their salts, and unsaturated dicarboxylic anhydrides; (c) a monomer unit derived from at least one monomer (mc) selected from the group consisting of 2-acrylamido-2-methylpropanesulfonic acid and its salts; (d) a monomer unit derived from at least one monomer (md) selected from the group consisting of vinyl monomers having a solubility of 7 g or less in 100 mL of water at 20° C. or 30° C. and aromatic vinyl monomers;
[0014] The monomer unit (a) constituting the (meth)acrylic acid-based copolymer (P) of the present invention is derived from at least one kind of monomer (ma), and is a monomer unit derived from at least one selected from acrylic acid, an acrylic acid salt, methacrylic acid, and a methacrylic acid salt.
[0015] Examples of the monomer (ma) include acrylic acid, sodium acrylate, potassium acrylate, magnesium acrylate, calcium acrylate, methacrylic acid, sodium methacrylate, potassium methacrylate, magnesium methacrylate, and calcium methacrylate.
[0016] In the present invention, from the viewpoint of the transparency of an aqueous solution of the (meth)acrylic acid-based copolymer (P), it is preferable that the monomer unit (a) contains a monomer unit derived from an acrylate salt.
[0017] In the present invention, the content of the monomer unit (a) constituting the (meth)acrylic acid-based copolymer (P) is 65.1 to 95.7% by mass, assuming that the total of the monomer units (a), (b), (c) and (d) is 100% by mass. The lower limit is preferably 65.2% by mass, more preferably 65.3% by mass. The upper limit is preferably 80% by mass, more preferably 70% by mass.
[0018] The monomer (b) constituting the (meth)acrylic acid-based copolymer (P) of the present invention is derived from at least one kind of monomer (mb), and is a monomer unit derived from at least one kind selected from the group consisting of unsaturated dicarboxylic acids and their salts, and unsaturated dicarboxylic acid anhydrides.
[0019] Examples of the monomer (mb) include maleic acid, fumaric acid, itaconic acid, citraconic acid and their anhydrides, as well as salts formed by a carboxy group contained in an unsaturated dicarboxylic acid and a monovalent or polyvalent cation (lithium salt, sodium salt, potassium salt, ammonium salt, trimethylamine salt, triethylamine salt, triethanolamine salt, etc.).
[0020] In the present invention, from the viewpoints of the chelating effect on scale and polymerizability, the monomer unit (b) preferably contains a monomer unit derived from maleic anhydride.
[0021] In the present invention, the content of the monomer unit (b) constituting the (meth)acrylic acid-based copolymer (P) is 0.1 to 30.7% by mass, assuming that the total of the monomer units (a), (b), (c) and (d) is 100% by mass. The lower limit is preferably 1% by mass, more preferably 5% by mass. The upper limit is preferably 25% by mass, more preferably 20% by mass.
[0022] The monomer unit (c) constituting the (meth)acrylic acid-based copolymer (P) of the present invention is derived from at least one kind of monomer (mc), and is a monomer unit derived from at least one selected from 2-acrylamido-2-methylpropanesulfonic acid and its salts.
[0023] Examples of the monomer (mc) include 2-acrylamido-2-methylpropanesulfonic acid and sodium 2-acrylamido-2-methylpropanesulfonate.
[0024] In the present invention, from the viewpoint of improving the solubility of the copolymer, it is preferable that the monomer unit (c) contains a monomer unit derived from 2-acrylamido-2-methylpropanesulfonate.
[0025] In the present invention, the content of the monomer unit (c) constituting the (meth)acrylic acid-based copolymer (P) is 4.1 to 29.9% by mass, assuming that the total of the monomer units (a), (b), (c) and (d) is 100% by mass. The lower limit is preferably 10% by mass, more preferably 20% by mass. The upper limit is preferably 29.5% by mass, more preferably 29.0% by mass.
[0026] The monomer unit (d) constituting the (meth)acrylic acid-based copolymer (P) of the present invention is derived from at least one type of monomer (md), and is at least one type selected from the group consisting of vinyl monomers having a solubility of 7 g or less in 100 mL of water at 20°C or 30°C, and aromatic vinyl monomers. Examples of vinyl monomers having a solubility of 7 g or less in 100 mL of water at 20° C. or 30° C. include ethyl acrylate, n-butyl acrylate, isobutyl acrylate, propyl vinyl ether, butyl vinyl ether, isobutyl vinyl ether, tert-butyl vinyl ether, butylene, isobutylene, N-tert-butylacrylamide (TBAM), etc. In the present invention, vinyl monomers having a solubility of 0.1 g or less are preferred. Examples of the aromatic vinyl monomer include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, β-methylstyrene, ethylstyrene, p-tert-butylstyrene, vinyltoluene, vinylxylene, and vinylnaphthalene.
[0027] In the present invention, from the viewpoints of the water solubility of the (meth)acrylic acid-based copolymer (P), the transparency of the resulting aqueous solution, and the inhibition of the formation of scale containing at least silica among silica, calcium phosphate, calcium carbonate, and calcium sulfate, the monomer unit (d) preferably contains a monomer unit derived from ethyl acrylate, n-butyl acrylate, isobutyl acrylate, N-tert-butylacrylamide (TBAM), or styrene.
[0028] In the present invention, the content of the monomer unit (d) constituting the (meth)acrylic acid-based copolymer (P) is 0.1 to 4.9% by mass, assuming that the total of the monomer units (a), (b), (c) and (d) is 100% by mass. The lower limit is preferably 0.2% by mass, more preferably 0.4% by mass. The upper limit is preferably 3.0% by mass, more preferably 2.0% by mass.
[0029] Specific examples of the (meth)acrylic acid copolymer (P) of the present invention are shown below. (1) Acrylate-maleic anhydride-2-acrylamido-2-methylpropanesulfonate-styrene copolymer (2) Acrylate-maleic anhydride-2-acrylamido-2-methylpropanesulfonate-ethyl acrylate copolymer (3) Acrylate-maleic anhydride-2-acrylamido-2-methylpropanesulfonate-n-butyl acrylate copolymer (4) Acrylate-maleic anhydride-2-acrylamido-2-methylpropanesulfonate-isobutyl acrylate copolymer (5) Acrylate-maleic anhydride-2-acrylamido-2-methylpropanesulfonate-N-tert-butylacrylamide (TBAM) copolymer
[0030] The structure of the (meth)acrylic acid copolymer (P) of the present invention is not particularly limited, but is preferably a random copolymer.
[0031] From the viewpoint of inhibiting the formation of at least silica-containing scale among silica, calcium phosphate, calcium carbonate, and calcium sulfate, the (meth)acrylic acid-based copolymer (P) of the present invention has an Mw of preferably 1,500 to 20,000, more preferably 2,000 to 15,000, and even more preferably 3,000 to 10,000. The polydispersity, which is the ratio of Mw to Mn (Mw / Mn), is preferably 1.2 to 2.5, and more preferably 1.2 to 2.0.
[0032] The (meth)acrylic acid copolymer (P) of the present invention can have the above-mentioned preferred Mw by assembling copolymers with different molecular weights. In the present invention, a (meth)acrylic acid copolymer having a molecular weight of 1,000 or less (hereinafter referred to as "(meth)acrylic acid copolymer (P1)") or a (meth)acrylic acid copolymer having a molecular weight of 200,000 or more (hereinafter referred to as "(meth)acrylic acid copolymer (P2)") may be included, but the content of the (meth)acrylic acid copolymer (P1) is preferably 15.0 mass% or less, more preferably 10.0 mass% or less, and even more preferably 5.0 mass% or less, based on the total amount of the (meth)acrylic acid copolymer (P) of the present invention, and the content of the (meth)acrylic acid copolymer (P2) is preferably 0.10 mass% or less, more preferably 0.05 mass% or less, based on the total amount of the (meth)acrylic acid copolymer (P) of the present invention.
[0033] The (meth)acrylic acid copolymer (P) of the present invention contains a specific monomer unit at a specific content ratio and has the above-mentioned preferred Mw, so that an aqueous solution with excellent transparency can be obtained. When this aqueous solution is used as a water treatment agent and contacted with water (water to be treated) containing a precursor component forming calcium phosphate or silica, foaming is unlikely to occur, and the formation of scale containing at least silica among silica, calcium phosphate, calcium carbonate, and calcium sulfate can be suppressed in a mixed liquid of the water treatment agent and each water to be treated. The present inventors presume that the reason why foaming is unlikely to occur when the water treatment agent is mixed with the water to be treated is that the monomer unit (d) has a hydrophobic group, and therefore, in the (meth)acrylic acid copolymer (P) containing 0.1 to 4.9 mass% of this monomer unit (d), the balance between the hydrophobic group and the hydrophilic group can be controlled within a range that does not act as a surfactant.
[0034] The (meth)acrylic acid copolymer (P) of the present invention can be produced by a conventional method. In order to obtain a preferable composition of the (meth)acrylic acid copolymer (P), not only the monomers are polymerized but also the reaction product obtained by polymerization may be purified.
[0035] The method for producing the (meth)acrylic acid copolymer (P) of the present invention (hereinafter referred to as the "production method of the present invention") sequentially comprises a preparation step of preparing a monomer mixture containing monomer (ma), monomer (mb), monomer (mc), monomer (md) and water, and a polymerization step of continuously supplying the obtained monomer mixture, a polymerization initiator and an optional chain transfer agent to a reactor, respectively, and polymerizing the monomers. Note that, when the monomers to be polymerized contain at least (meth)acrylic acid of (meth)acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid, and a (meth)acrylic acid copolymer (P) containing a monomer unit derived from a (meth)acrylic acid salt and / or a monomer unit derived from a 2-acrylamido-2-methylpropanesulfonic acid salt is produced, it is preferable to subject the copolymer obtained by the polymerization step to a neutralization reaction (neutralization step) after the polymerization step. Furthermore, after either the polymerization step or the neutralization step, a step of removing unreacted monomers may be provided.
[0036] In the above preparation process, the method of obtaining the monomer mixture is not particularly limited. In the present invention, since a hydrophobic monomer (MD) is used, it is preferable to first dissolve the monomer (MD) in the monomer (MA), and then mix the obtained solution with the monomer (MB), the monomer (MC) and water. The mixing method is not particularly limited.
[0037] The amounts of each monomer and water used in the above preparation steps are as follows. The amount of the monomer (ma) used is 65.1 to 95.7% by mass based on the total amount of the monomers (ma), (mb), (mc) and (md). The lower limit is preferably 65.2% by mass, more preferably 65.3% by mass. The upper limit is preferably 80% by mass, more preferably 70% by mass. The amount of the monomer (mb) used is 0.1 to 30.7% by mass based on the total amount of the monomers (ma), (mb), (mc) and (md). The lower limit is preferably 1% by mass, more preferably 5% by mass. The upper limit is preferably 25% by mass, more preferably 20% by mass. The amount of the monomer (mc) used is 4.1 to 29.9% by mass based on the total amount of the monomers (ma), (mb), (mc) and (md). The lower limit is preferably 10% by mass, more preferably 20% by mass. The upper limit is preferably 29.5% by mass, more preferably 29.0% by mass. The amount of the monomer (md) used is 0.1 to 4.9% by mass based on the total amount of the monomers (ma), (mb), (mc) and (md). The lower limit is preferably 0.2% by mass, more preferably 0.4% by mass. The upper limit is preferably 3.0% by mass, more preferably 2.0% by mass. The amount of water used is preferably 5 to 80 parts by mass, and more preferably 20 to 60 parts by mass, relative to 100 parts by mass of the total of the monomers (ma), (mb), (mc) and (md).
[0038] Next, in the polymerization step, the monomer mixture obtained in the preparation step, the polymerization initiator, and an optional chain transfer agent are continuously supplied to a reactor, and the monomers are polymerized, preferably while stirring the reaction system. At this time, water may also be continuously supplied, if necessary. As the reactor, a reactor (reaction device) having a conventionally known configuration, which is equipped with a means for supplying a monomer mixture, a means for supplying a chain transfer agent, a means for supplying a polymerization initiator, a stirring means, a means for adjusting the temperature of the reaction system, a reflux cooling means, a means for supplying a neutralizing agent, a means for discharging the reaction liquid, and the like, can be used.
[0039] In the polymerization process according to the present invention, a copolymer having desired physical properties can be efficiently produced by setting the supply time of the monomer mixture to the reactor within a specific range. The supply time of the monomer mixture is preferably 2 to 12 hours, more preferably 2 to 10 hours, and even more preferably 2 to 6 hours. The polymerization process is usually not terminated simultaneously with the completion of the supply of the monomer mixture.
[0040] In addition, the supply rate of the monomer mixture to the reactor is preferably constant, but the supply rate may be changed while checking the change with time of the polymerization conversion rate.
[0041] Examples of the polymerization initiator include hydrogen peroxide; persulfates such as sodium persulfate, potassium persulfate, and ammonium persulfate; dimethyl 2,2'-azobis(2-methylpropionate), 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(isobutyric acid) dimethyl, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methylpropionate), Examples of the azo compounds include 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] disulfate dihydrate, and 1,1'-azobis(cyclohexane-1-carbonitrile); and organic peroxides such as benzoyl peroxide, lauroyl peroxide, peracetic acid, di-t-butyl peroxide, and cumene hydroperoxide. These may be used alone or in combination of two or more.
[0042] The amount of the polymerization initiator used is preferably 0.1 to 10.0 parts by mass, and more preferably 0.1 to 2.0 parts by mass, relative to 100 parts by mass in total of the monomers (ma), (mb), (mc) and (md).
[0043] The method of using the polymerization initiator is not particularly limited, and it is preferable to start the supply of the polymerization initiator simultaneously with the monomer mixture, or to start the supply of the polymerization initiator after the supply of the monomer mixture. The supply of the polymerization initiator is terminated preferably 5 minutes or more, particularly preferably 10 minutes or more later than the completion of the supply of the monomer mixture.
[0044] Examples of the chain transfer agent include phosphorous acid, hypophosphorous acid and salts thereof (sodium hypophosphite, potassium hypophosphite, etc.); sulfurous acid, hydrogen sulfite, dithionous acid, metabisulfite and salts thereof (sodium hydrogen sulfite, potassium hydrogen sulfite, sodium dithionite, potassium dithionite, sodium metabisulfite, potassium metabisulfite, etc.); mercaptoethanol, thioglycerol, thioglycolic acid, 2-mercaptopropionic acid, 3-mercaptopropionic acid, thiomalic acid, octyl thioglycolate, octyl 3-mercaptopropionate, 2-mercaptoethanesulfonic acid, n-dodecyl mercaptan, octyl mercaptan, butyl thioglycolate, and other thiols. These may be used alone or in combination of two or more.
[0045] The amount of the chain transfer agent used is preferably 0.1 to 30 parts by mass, and more preferably 1 to 15 parts by mass, per 100 parts by mass in total of the monomers (ma), (mb), (mc) and (md).
[0046] The method of using the chain transfer agent is not particularly limited, and the supply of the chain transfer agent is terminated preferably 10 minutes or more, particularly preferably 20 minutes or more, earlier than the completion time of the supply of the monomer mixture.
[0047] In the polymerization step, the presence of polyvalent metal ions in the reaction system can promote the decomposition of the polymerization initiator and the chain transfer agent during the polymerization reaction. Materials that form such polyvalent metal ions include ammonium iron(III) sulfate or its hydrate, iron(III) sulfate or its hydrate, and iron(II) sulfate or its hydrate.
[0048] In the polymerization step, it is preferable to add water to the reactor before supplying each raw material to the reactor, so that the raw materials supplied to the reactor are mixed efficiently and the polymerization reaction proceeds smoothly. The added material may be water alone, water containing a chain transfer agent, water containing polyvalent metal ions, or the like.
[0049] The polymerization temperature of the monomers in the polymerization step (the temperature of the reaction system) is appropriately selected depending on the type of polymerization initiator, etc., and is not particularly limited. The preferred polymerization temperature is 70°C or higher. In a reaction system in which no side reactions occur, the temperature is preferably near the boiling point of the polymerization solvent (water), and particularly preferably the boiling point of the polymerization solvent (water). When the polymerization initiator is started to be supplied after the supply of the monomer mixture is started, the temperature of the reaction system at the start of the supply of the monomer mixture may be lower than the predetermined polymerization temperature. When set in this way, it is sufficient to adjust to the predetermined polymerization temperature after the supply of the polymerization initiator is started.
[0050] In the polymerization step according to the present invention, the residual concentration (total concentration) of the monomer (mc) per 100 mL of the reaction solution in the reactor can be adjusted to preferably 0.3 g or less, more preferably 0.1 g or less, throughout the entire process from the start of polymerization to the end of the supply of the polymerization initiator, so that the (meth)acrylic acid-based copolymer (P) having the desired physical properties can be efficiently produced. The polymerization step is preferably terminated after a maximum of 12 hours have elapsed since the completion of the supply of the monomer mixture.
[0051] When the production method of the present invention includes a neutralization step after the polymerization step, an alkali agent or an aqueous solution thereof can be used, such as an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide, an alkaline earth metal hydroxide such as calcium hydroxide or magnesium hydroxide, ammonia, or an organic amine salt such as monoethanolamine or triethanolamine. As the alkali agent, an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide is preferred, and sodium hydroxide is particularly preferred.
[0052] When the neutralization step is carried out, the pH of the reaction solution is adjusted to preferably 7.0 or less, more preferably within the range of 1.0 to 5.0.
[0053] According to the production method of the present invention, it is possible to efficiently produce a (meth)acrylic acid-based copolymer (P) in which the content ratios of the monomer units (a), (b) and (c) are within a predetermined range and the content of the unreacted monomers (ma), (mb), (mc) and (md) as well as the content of the above-mentioned (meth)acrylic acid-based copolymers (P1) and (P2) are as small as possible.
[0054] In the case where water is not removed from the reaction solution after the polymerization step and the neutralization step according to the production method of the present invention, the reaction solution usually consists of an aqueous solution of the (meth)acrylic acid-based copolymer (P). Using this aqueous solution, a water treatment agent that suppresses scale formation in cooling water systems, boiler water systems, geothermal power generation water systems, seawater desalination equipment, pulp dissolving pots, black liquor concentrating pots, etc., and a scale adhesion inhibitor that prevents scale adhesion to the inner surface of cooling water piping, the heat transfer surface of a heat exchanger, etc., can be easily produced. Furthermore, since the aqueous solution of the (meth)acrylic acid-based copolymer (P) can be made clear and transparent, the water treatment agent and the scale adhesion inhibitor obtained using this aqueous solution can also be transparent and easy to handle.
[0055] The water treatment agent of the present invention contains a (meth)acrylic acid-based copolymer (P) and is preferably in the form of a liquid (aqueous solution). The content of the (meth)acrylic acid-based copolymer (P) in this aqueous solution is preferably 1 to 1000 mg / L, more preferably 5 to 100 mg / L, since the effect as a water treatment agent, i.e., the effect of inhibiting scale formation, can be sufficiently obtained.
[0056] The water treatment agent of the present invention may contain, as necessary, conventionally known scale formation inhibitors, bactericides, anticorrosive agents, slime inhibitors, defoamers, etc., such as polyacrylic acid or a salt thereof, polymaleic acid or a salt thereof, other (meth)acrylic acid-based copolymers, and styrene-maleic acid-based copolymers.
[0057] The water treatment agent of the present invention is suitable for application to water (water to be treated) containing at least a precursor component that forms silica scale among silica scale, calcium phosphate scale, calcium carbonate scale, and calcium sulfate. For example, in an open circulation cooling water system, in order to reduce the amount of cooling water discharged outside the system from the viewpoint of water saving and resource saving, the cooling water may be concentrated to form poorly soluble salts such as calcium phosphate and calcium carbonate. In such a case, by using the water treatment agent of the present invention, problems such as a decrease in heat exchange efficiency and blockage of piping can be suppressed. In addition, in a cooling water system, a boiler water system, or a geothermal power generation water system that is equipped with a heat exchanger, a refrigerator, etc. and performs a highly concentrated operation, silica scale may be formed. When silica scale adheres to a component of the equipment, it is often difficult to remove it, so by using the water treatment agent of the present invention, the formation of silica scale can be suitably suppressed. The pH and temperature of the water (water to be treated) are not particularly limited.
[0058] When the water treatment agent of the present invention is used, for example, it is added to water (water to be treated) containing the precursor components that form the above-mentioned scale material, and stirred as necessary.
[0059] The scale adhesion preventive agent of the present invention contains a (meth)acrylic acid-based copolymer (P) and is preferably in the form of a liquid (aqueous solution). The content of the (meth)acrylic acid-based copolymer (P) in this aqueous solution is preferably 1 to 1000 mg / L, more preferably 5 to 100 mg / L, since the effect as a scale adhesion preventive agent, for example, the effect of preventing scale adhesion to structural members such as condensers, heat exchangers, and piping that come into contact with water such as industrial water, tap water, and groundwater, can be sufficiently obtained.
[0060] When the scale adhesion preventive agent of the present invention is used, for example, it is added to water (water to be treated) containing the precursor components that form the above-mentioned scale materials, and stirred as necessary. EXAMPLES
[0061] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to these examples. In the following, % and ppm are by mass unless otherwise specified.
[0062] 1. Raw materials for manufacturing (meth)acrylic acid copolymers Various polymers were produced using the following raw materials.
[0063] 1-1.Monomer AA: Acrylic acid MLA: Maleic anhydride ATBS: Sodium 2-acrylamido-2-methylpropanesulfonate St: styrene EA: Ethyl acrylate The solubility in 100 mL of water at 20°C is 1.5 g. BA: n-butyl acrylate The solubility in 100 mL of water at 20°C is 0.14 g. IBA: Isobutyl acrylate The solubility in 100 mL of water at 20°C is 0.79 g. TBAM: N-tert-butylacrylamide The solubility in 100 mL of water at 30°C is 0.1 g.
[0064] 1-2. Polymerization initiator Sodium persulfate
[0065] 1-3. Chain transfer agents Sodium Bisulfite
[0066] 1-4.Neutralizer 50% aqueous solution of sodium hydroxide
[0067] 2. Method for evaluating (meth)acrylic acid copolymer or its aqueous solution 2-1. Measurement of molecular weight distribution of (meth)acrylic acid copolymers The Mw and Mn of the (meth)acrylic acid-based copolymer were measured by GPC using an "LC-20AD" (model name) manufactured by SHIMADZU CORPORATION. <GPC measurement conditions> Column: Tosoh Corporation's G4000PWxl, G3000PWxl, and G2500PWxl connected Eluent: 0.1M - NaCl + phosphate buffer (pH 7) Detector: RI Column temperature: 40 °C Standard substance: Sodium polyacrylate manufactured by Sowa Chemical Co., Ltd.
[0068] 2-2. Quantification of unreacted monomers contained in the (meth)acrylic acid copolymer (1) AA or its sodium salt, and ATBS were measured by high performance liquid chromatography (hereinafter referred to as "HPLC") using "LC-20AD" (model name) manufactured by SHIMADZU Corporation. <HPLC measurement conditions> Column: ODS-80Ts manufactured by Tosoh Corporation Eluent: 0.17% aqueous solution of tetrabutylammonium hydrogen sulfide: acetonitrile = 90:10 Column temperature: 40 °C Detector: UV-vis (205 nm)
[0069] 2-3. Quantification of unreacted monomers contained in the (meth)acrylic acid copolymer (2) St, EA, BA, IBA, and TBAM were measured by gas chromatography (hereinafter referred to as "GC") using "GC-2014AF" (model name) manufactured by SHIMADZU Corporation. <GC measurement conditions> Column: HR-1 manufactured by Tosoh Corporation Carrier gas: He Sample injection port temperature: 250 °C Temperature rising conditions: 70 °C → 150 °C (temperature rising rate: 20 °C per minute) Detector: FID Detector temperature: 250 °C
[0070] 3. Production of (meth)acrylic acid copolymer Hereinafter, production examples of various (meth)acrylic acid copolymers are shown.
[0071] Example 1-1 First, 3.5 g of styrene (St) was dissolved in 424 g of acrylic acid (AA), and 70 g of maleic anhydride, 449 g of a 50% aqueous solution of sodium 2-acrylamido-2-methylpropanesulfonate (ATBS), and 14 g of pure water were added to this mixture, followed by thorough stirring to obtain a monomer mixture. Then, 420 g of pure water was charged into a reactor equipped with a reflux condenser, and the temperature was raised to 75° C., after which 9.3 g of a 30% aqueous solution of sodium bicarbonate was added while stirring the inside of the reactor. Then, the above-mentioned monomer mixture, a 5% aqueous solution of sodium persulfate, and a 30% aqueous solution of sodium bicarbonate were continuously fed into the reactor to carry out a polymerization reaction. The feed amount and feed time of the monomer mixture were 4.0 g / min and 4 hours, respectively. The feed amount and feed time of the 5% aqueous solution of sodium persulfate were 0.71 g / min and 4 hours and 10 minutes, respectively. The feed amount and feed time of the 30% aqueous solution of sodium bicarbonate were 0.29 g / min and 3 hours and 40 minutes, respectively. During the polymerization reaction, the temperature inside the reactor was maintained at 75° C. In addition, the residual concentration of styrene (St), which is the monomer (md), per 100 mL of the reaction liquid was maintained at less than 0.1 g. After the supply of the 5% aqueous solution of sodium persulfate was completed, the reaction solution was heated to 85°C and held for 1 hour. The pH of the reaction solution was then adjusted to 2.3 using a neutralizing agent to obtain an aqueous solution of a (meth)acrylic acid-based copolymer (hereinafter also referred to as "copolymer (F1)") with a solid content of 46%. This aqueous solution was clear and transparent.
[0072] A sample taken one hour after the start of polymerization was subjected to gas chromatography (GC), and the residual monomer (md) concentration was found to be less than 0.1 g / 100 mL (see Table 1).
[0073] Thereafter, copolymer (F1) was subjected to gel permeation chromatography (GPC), and the results showed that Mw was 17790, Mn was 7050, and Mw / Mn was about 2.5. The content of (meth)acrylic acid-based copolymers having a molecular weight of 1000 or less in copolymer (F1) was 1.6%, and the content of (meth)acrylic acid-based copolymers having a molecular weight of 200000 or more was 0.0% (see Table 1).
[0074] Furthermore, quantitative analysis of the unreacted monomers contained in the copolymer (F1) revealed that AA and its sodium salt were less than 10,000 ppm, ATBS was less than 10,000 ppm, and St was below the detection limit (0.1 ppm) (see Table 1).
[0075] Examples 1-2 to 1-9 Using monomers having the compositions shown in Table 1, (meth)acrylic acid-based copolymers (F2) to (F9) were produced in the same manner as in Example 1-1 (see Table 1).
[0076] Comparative Example 1-1 First, 473 g of acrylic acid (AA), 496 g of a 50% aqueous solution of sodium 2-acrylamido-2-methylpropanesulfonate (ATBS), and 14 g of pure water were thoroughly stirred to obtain a monomer mixture. Then, 420 g of pure water was charged into a reactor equipped with a reflux condenser, and the temperature was raised to 75° C., and 9 g of a 30% aqueous solution of sodium bicarbonate was added while stirring the inside of the reactor. Then, the above-mentioned monomer mixture, a 5% aqueous solution of sodium persulfate, and a 30% aqueous solution of sodium bicarbonate were continuously fed into the reactor to carry out a polymerization reaction. The feed rate and feed time of the monomer mixture were 4.1 g / min and 4 hours, respectively. The feed rate and feed time of the 5% aqueous solution of sodium persulfate were 0.3 g / min and 4 hours and 10 minutes, respectively. The feed rate and feed time of the 30% aqueous solution of sodium bicarbonate were 0.7 g / min and 3 hours and 40 minutes, respectively. During the polymerization reaction, the temperature inside the reactor was maintained at 75° C. After the supply of the 5% aqueous solution of sodium persulfate was completed, the reaction liquid was heated to 85° C. and maintained at that temperature for 1 hour. Next, the pH of the reaction solution was adjusted to 2.3 using a neutralizing agent to obtain an aqueous solution of a (meth)acrylic acid-based copolymer (hereinafter also referred to as "copolymer (FF1)") with a solid content concentration of 45%. This aqueous solution was clear and not turbid.
[0077] Thereafter, the copolymer (FF1) was subjected to gel permeation chromatography (GPC), and the results showed that the copolymer had an Mw of 6730, an Mn of 4130, and an Mw / Mn ratio of about 1.6. The content of (meth)acrylic acid-based copolymers having a molecular weight of 1000 or less in the copolymer (FF1) was 0.8%, and the content of (meth)acrylic acid-based copolymers having a molecular weight of 200000 or more was 0.0% (see Table 1).
[0078] Furthermore, a quantitative analysis of the unreacted monomers contained in the copolymer (FF1) revealed that the amounts of AA and its sodium salt were 66 ppm, and that of ATBS was 123 ppm (see Table 1).
[0079] Comparative Example 1-2 First, 35 g of styrene (St) was dissolved in 315 g of acrylic acid (AA), and 774 g of a 50% aqueous solution of sodium 2-acrylamido-2-methylpropanesulfonate (ATBS) and 14 g of pure water were added to this mixture and thoroughly stirred to obtain a monomer mixture. Then, 420 g of pure water was charged into a reactor equipped with a reflux condenser, and the temperature was raised to 75° C., and 9 g of a 30% aqueous solution of sodium bicarbonate was added while stirring the inside of the reactor. Then, the above-mentioned monomer mixture, a 5% aqueous solution of sodium persulfate, and a 30% aqueous solution of sodium bicarbonate were continuously fed into the reactor to carry out a polymerization reaction. The feed rate and feed time of the monomer mixture were 4.7 g / min and 4 hours, respectively. The feed rate and feed time of the 5% aqueous solution of sodium persulfate were 0.3 g / min and 4 hours and 10 minutes, respectively. The feed rate and feed time of the 30% aqueous solution of sodium bicarbonate were 0.7 g / min and 3 hours and 40 minutes, respectively. During the polymerization reaction, the temperature inside the reactor was maintained at 75° C. After the supply of the 5% aqueous solution of sodium persulfate was completed, the reaction liquid was heated to 85° C. and maintained at that temperature for 1 hour. Next, the pH of the reaction solution was adjusted to 2.6 using a neutralizing agent to obtain an aqueous solution of a (meth)acrylic acid-based copolymer (hereinafter referred to as "copolymer (FF2)") with a solid content of 42%. This aqueous solution was turbid and opaque.
[0080] A sample taken one hour after the start of polymerization was subjected to gas chromatography (GC), and the residual monomer (md) concentration was found to be less than 0.1 g / 100 mL (see Table 1).
[0081] Thereafter, the copolymer (FF2) was subjected to gel permeation chromatography (GPC), and the results showed that the copolymer had an Mw of 7700, an Mn of 4640, and an Mw / Mn ratio of about 1.7. The content of (meth)acrylic acid-based copolymers having a molecular weight of 1000 or less in the copolymer (FF2) was 0.5%, and the content of (meth)acrylic acid-based copolymers having a molecular weight of 200000 or more was 0.0% (see Table 1).
[0082] Furthermore, a quantitative analysis of the unreacted monomers contained in the copolymer (FF2) revealed that AA and its sodium salt were present at 66 ppm, and ATBS was present at 628 ppm (see Table 1).
[0083] Comparative Example 1-3 First, 70 g of styrene (St) was dissolved in 469 g of acrylic acid (AA), and 357 g of a 50% aqueous solution of sodium 2-acrylamido-2-methylpropanesulfonate (ATBS) and 14 g of pure water were added to this mixture and thoroughly stirred to obtain a monomer mixture. Then, 420g of pure water was charged into a reactor equipped with a reflux condenser, and the temperature was raised to 75°C. Then, 9g of a 30% aqueous solution of sodium bicarbonate was added while stirring the inside of the reactor. Then, while maintaining the temperature inside the reactor at 75°C, the amount and time of the monomer mixture fed into the reactor were 3.8g / min and 4 hours, respectively, the amount and time of the 5% aqueous solution of sodium persulfate were 0.3g / min and 4 hours 10 minutes, respectively, and the amount and time of the 30% aqueous solution of sodium bicarbonate were 0.7g / min and 3 hours 40 minutes, respectively, to start a polymerization reaction. However, during the polymerization reaction, a precipitate was formed in the reactor, and the production of a (meth)acrylic acid-based copolymer (hereinafter referred to as "copolymer (FF3)") was stopped.
[0084] Comparative Example 1-4 First, 70 g of maleic anhydride, 449 g of a 50% aqueous solution of sodium 2-acrylamido-2-methylpropanesulfonate (ATBS), and 14 g of pure water were added to 427 g of acrylic acid (AA), and the mixture was thoroughly stirred to obtain a monomer mixture. Then, 420 g of pure water was charged into a reactor equipped with a reflux condenser, and the temperature was raised to 75° C., and 9.3 g of a 30% aqueous solution of sodium bicarbonate was added while stirring the inside of the reactor. Then, the above-mentioned monomer mixture, a 5% aqueous solution of sodium persulfate, and a 30% aqueous solution of sodium bicarbonate were continuously fed into the reactor to carry out a polymerization reaction. The feed rate and feed time of the monomer mixture were 4.0 g / min and 4 hours, respectively. The feed rate and feed time of the 5% aqueous solution of sodium persulfate were 0.29 g / min and 4 hours and 10 minutes, respectively. The feed rate and feed time of the 30% aqueous solution of sodium bicarbonate were 0.71 g / min and 3 hours and 40 minutes, respectively. During the polymerization reaction, the temperature inside the reactor was maintained at 75° C. After the supply of the 5% aqueous solution of sodium persulfate was completed, the reaction liquid was heated to 85° C. and maintained at that temperature for 1 hour. Next, the pH of the reaction solution was adjusted to 2.3 using a neutralizing agent to obtain an aqueous solution of a (meth)acrylic acid-based copolymer (hereinafter also referred to as "copolymer (FF4)") with a solid content of 45%. This aqueous solution was clear and not turbid.
[0085] Thereafter, gel permeation chromatography (GPC) revealed that the copolymer had a Mw of 10,780, a Mn of 5,650, and a Mw / Mn of approximately 1.9. The content of (meth)acrylic acid-based copolymers having a molecular weight of 1,000 or less in this copolymer (FF4) was 1.1%, and the content of (meth)acrylic acid-based copolymers having a molecular weight of 200,000 or more was 0.0% (see Table 1).
[0086] Furthermore, quantitative analysis of the unreacted monomers contained in the copolymer (FF4) revealed that the amounts of AA and its sodium salt were 1260 ppm, and ATBS was 1235 ppm (see Table 1).
[0087] Comparative Examples 1-5 First, 70 g of styrene (St) was dissolved in 456 g of acrylic acid (AA), and to this mixture were added 35 g of maleic anhydride, 139 g of a 50% aqueous solution of sodium 2-acrylamido-2-methylpropanesulfonate (ATBS), and 14 g of pure water, followed by thorough stirring to obtain a monomer mixture. Then, 420g of pure water was charged into a reactor equipped with a reflux condenser, and the temperature was raised to 75°C. Then, 9g of a 30% aqueous solution of sodium bicarbonate was added while stirring the inside of the reactor. Then, while maintaining the temperature inside the reactor at 75°C, the amount and time of the monomer mixture fed into the reactor were 4.0g / min and 4 hours, respectively, the amount and time of the 5% aqueous solution of sodium persulfate were 0.3g / min and 4 hours 10 minutes, respectively, and the amount and time of the 30% aqueous solution of sodium bicarbonate were 0.7g / min and 3 hours 40 minutes, respectively, to start a polymerization reaction. However, during the polymerization reaction, a precipitate was formed in the reactor, and the production of a (meth)acrylic acid-based copolymer (hereinafter also referred to as "copolymer (FF5)") was stopped.
[0088] [Table 1]
[0089] 4. Evaluation of water treatment agents (1) Scaling inhibition test for silica, calcium phosphate, calcium carbonate and calcium sulfate The aqueous solutions of the (meth)acrylic acid copolymers obtained in the above Examples 1-1 to 1-9 and Comparative Examples 1-1, 1-2 and 1-4 were adjusted to a concentration of 1000 ppm to prepare water treatment agents (S). The effect of inhibiting scale formation on silica, calcium phosphate, calcium carbonate and calcium sulfate was confirmed by the following method. The results are shown in Table 2. In the following calcium phosphate scale inhibition test, calcium carbonate scale inhibition test, and calcium sulfate scale inhibition test, "blank" refers to the test result of a solution in which no water treatment agent (S) is added and inorganic salts are at a specified concentration.
[0090] <Silica scale inhibition test> Using the water treatment agent (S) and sodium silicate, 240 mL of a solution with a concentration of 150 mg / L of (meth)acrylic acid copolymer and 351 mg / L of sodium silicate was prepared and left at 70 ° C for 30 minutes. Then, while stirring this solution, 44 mL of 0.5% magnesium chloride aqueous solution, 31.6 mL of 0.5% calcium chloride aqueous solution, and 36 mL of 0.5% sodium bicarbonate aqueous solution were added. Next, while stirring this mixed solution, 40 mL of 0.21% sodium bicarbonate aqueous solution was added, and the pH was adjusted to 8.0 with 1 mol / L hydrochloric acid aqueous solution. After that, after leaving it at 70 ° C for 3 hours, the presence or absence of turbidity and precipitation of the solution due to silica was visually observed, and the scale inhibition was evaluated according to the following criteria. ◎: No precipitation was observed, but the liquid was slightly cloudy. ○: No precipitation was observed, but the liquid was very cloudy. ×: Precipitation was observed
[0091] <Calcium phosphate scale inhibition test> Using the water treatment agent (S), disodium hydrogen phosphate, and calcium chloride, 360 mL of a liquid having a concentration of 20 mg / L of (meth)acrylic acid copolymer, 90 mg / L of disodium hydrogen phosphate, and 375 mg / L of calcium chloride was prepared. Next, while stirring this liquid, 40 mL of 0.21% sodium bicarbonate aqueous solution was added, and the pH was adjusted to 8.5 with 50% sodium hydroxide aqueous solution. After that, it was left at 60°C for 3 hours, and the presence or absence of turbidity and precipitation of the liquid due to calcium phosphate was visually observed, and the scale inhibition was evaluated according to the following criteria. ◎: No turbidity or precipitation was observed ○: Turbidity and precipitation were observed, but the Ca concentration in the supernatant after filtration was higher than that of the blank. ×: Turbidity and precipitation were observed, but there was no difference in Ca concentration in the supernatant after filtration compared to the blank.
[0092] <Calcium carbonate scale inhibition test> Using the water treatment agent (S), sodium bicarbonate, and calcium chloride, 400 mL of a solution containing a (meth)acrylic acid copolymer concentration of 10 mg / L, a sodium bicarbonate concentration of 420 mg / L, and a calcium chloride concentration of 375 mg / L was prepared. Next, this solution was adjusted to pH 8.5 with a 1M aqueous sodium hydroxide solution. After that, it was left at 60°C for 20 hours, and the presence or absence of turbidity and precipitation due to calcium carbonate was visually observed, and the scale inhibition was evaluated according to the following criteria. ◎: No turbidity or precipitation was observed ○: Turbidity and precipitation were observed, but the Ca concentration in the supernatant after filtration was higher than that of the blank. ×: Turbidity and precipitation were observed, but there was no difference in Ca concentration in the supernatant after filtration compared to the blank.
[0093] <Calcium sulfate scale inhibition test> Using the water treatment agent (S), sodium sulfate, and calcium chloride, 400 mL of a solution containing a (meth)acrylic acid copolymer at a concentration of 4 mg / L, a sodium sulfate at a concentration of 6000 mg / L, and a calcium chloride at a concentration of 6200 mg / L was prepared. After leaving the solution at 60°C for 3 hours, the solution was visually observed for turbidity and precipitation due to calcium sulfate, and the scale inhibition was evaluated according to the following criteria. ◎: No turbidity or precipitation was observed ○: Turbidity and precipitation were observed, but the Ca concentration in the supernatant after filtration was higher than that of the blank. ×: Turbidity and precipitation were observed, but there was no difference in Ca concentration in the supernatant after filtration compared to the blank.
[0094] (2) Foaming evaluation test The aqueous solutions of the (meth)acrylic acid copolymers obtained in the above Examples 1-1 to 1-9 and Comparative Examples 1-1, 1-2 and 1-4 were adjusted to a concentration of 1% to prepare water treatment agents (T), and 10 g of the aqueous solutions were placed in a resin disposable cup (volume: 1 L, size: inner diameter upper diameter 122 mm, lower diameter 102.5 mm, height 147 mm) manufactured by AS ONE Co., Ltd., and stirred at maximum speed for 30 seconds using a hand mixer "SUPER HAND MIXER MODEL HE-133" manufactured by SCARLETT Co., Ltd. (attachment is beater type). The foaming height immediately after the start of stirring and the time from the start of stirring until the generated foam disappeared were measured, and the foaming property was evaluated according to the following criteria. The results are shown in Table 2. ◎: Almost no foaming immediately after stirring (approximately 1 cm or less), and the foam disappeared immediately (approximately within 15 seconds) ○: The bubbles disappeared within about 1 minute of stirring. ×: Bubbles did not disappear within about 1 minute of stirring.
[0095] [Table 2] [Industrial Applicability]
[0096] The (meth)acrylic acid-based copolymer of the present invention is suitable as a component of a water treatment agent having an excellent effect of inhibiting scale formation, which contains at least silica among silica, calcium phosphate, calcium carbonate, and calcium sulfate, or a scale adhesion inhibitor having an excellent effect of inhibiting scale adhesion to components of equipment in a cooling water system, a boiler water system, or a geothermal power generation water system.
Claims
1. A (meth)acrylic acid-based copolymer consisting of the following monomer units (a), (b), (c) and (d): (a) a monomer unit derived from at least one monomer (ma) selected from the group consisting of (meth)acrylic acid and salts thereof; (b) a monomer unit derived from at least one monomer (mb) selected from the group consisting of unsaturated dicarboxylic acids and their salts, and unsaturated dicarboxylic anhydrides; (c) a monomer unit derived from at least one monomer (mc) selected from the group consisting of 2-acrylamido-2-methylpropanesulfonic acid and its salts (d) a monomer unit derived from at least one monomer (md) selected from the group consisting of vinyl monomers having a solubility of 7 g or less in 100 mL of water at 20° C. or 30° C. and aromatic vinyl monomers; The (meth)acrylic acid-based copolymer has contents of the monomer units (a), (b), (c) and (d) of 65.1 to 95.7% by mass, 0.1 to 30.7% by mass, 4.1 to 29.9% by mass and 0.1 to 4.9% by mass, respectively, when the total of the monomer units (a), (b), (c) and (d) is taken as 100% by mass.
2. The (meth)acrylic acid copolymer according to claim 1, having a weight average molecular weight of 1,500 to 20,000.
3. 3. The (meth)acrylic acid-based copolymer according to claim 2, wherein the content of the (meth)acrylic acid-based copolymer having a molecular weight of 1,000 or less is 15.0% by mass or less, and the content of the (meth)acrylic acid-based copolymer having a molecular weight of 200,000 or more is 0.10% by mass or less, based on the total amount of the (meth)acrylic acid-based copolymer.
4. A method for producing the (meth)acrylic acid-based copolymer according to claim 1, comprising the steps of: a preparation step of preparing a monomer mixture containing the monomer (ma), the monomer (mb), the monomer (mc), the monomer (md) and water; a polymerization step of continuously supplying the monomer mixture, a polymerization initiator, and an optional chain transfer agent to a reactor to polymerize the monomers; The method for producing a (meth)acrylic acid-based copolymer includes the steps of:
5. The method for producing a (meth)acrylic acid-based copolymer according to claim 4, wherein in the polymerization step, the monomer mixture is supplied to the reactor for a time period of 2 to 12 hours.
6. The method for producing a (meth)acrylic acid-based copolymer according to claim 5, wherein, in the polymerization step, polymerization of the monomers is carried out while maintaining a residual concentration of the monomers (md) in the reactor at 0.3 g / 100 mL or less in total.
7. A water treatment agent comprising the (meth)acrylic acid copolymer according to claim 1.
8. An anti-adhesion agent for calcium phosphate scale, calcium carbonate scale, calcium sulfate scale, and silica scale, comprising the (meth)acrylic acid-based copolymer according to claim 1.
Citation Information
Patent Citations
Prevention of silica scale
JP1992356580A
Method for preventing scale form being formed in aqueous system
JP1996224597A
Calcium phosphate type scale and silica type scale preventive agent
JP2018130702A
Acrylic acid-based copolymer, method for producing same and water treatment agent