Method for producing composite semipermeable membrane
A composite semipermeable membrane is manufactured with a porous support layer and separation functional layer, addressing the lack of solvent resistance and desalting functions in conventional membranes, achieving effective organic solvent resistance and desalting capabilities.
Patent Information
- Application Number
- JP2023048687
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-07
AI Technical Summary
Conventional membrane constituent materials lack sufficient resistance to various organic solvents and do not consider desalination treatment conditions, with existing membranes not addressing the need for high organic solvent resistance and effective desalting functions.
A method involving the formation of a porous support layer with polyetherimide, crosslinking using a crosslinking component and hydrophilic agent, followed by a separation functional layer formation to create a composite semipermeable membrane with enhanced organic solvent resistance and desalting capabilities.
The method produces a membrane that effectively resists organic solvents and achieves sufficient desalting, suitable for treating liquids containing organic solvents, particularly aprotic polar solvents, with improved performance in separating and blocking organic solvents and salts.
Smart Images

Figure 2024137242000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a composite semipermeable membrane. [Background technology]
[0002] Conventionally, in the field of industrial wastewater treatment and the like, the importance of technology relating to membrane separation of wastewater containing organic solvents has been known, and materials with high resistance to organic solvents have been studied as constituent materials of separation membranes. For example, Patent Document 1 describes a microporous membrane made of polyetherimide having a specific structure. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 1-155909 Summary of the Invention [Problem to be solved by the invention]
[0004] However, some conventional membrane materials are not sufficiently resistant to certain types of solvents, and materials that can handle a variety of organic solvents are required. In addition, the microporous membrane described in Patent Document 1 is a membrane for filtering silica and bacteria, and the document does not consider the structure of the separation membrane that takes into account desalination processing, or the manufacturing conditions thereof.
[0005] Therefore, an object of one embodiment of the present invention is to provide a technique for producing a separation membrane that has high organic solvent resistance and sufficient desalination function. [Means for solving the problem]
[0006] One aspect of the present invention is a method for producing a composite semipermeable membrane, comprising: a porous support layer formation step of forming a porous support layer containing polyetherimide; a crosslinking step of crosslinking the polyetherimide by contacting the porous support layer with an aqueous solution containing a crosslinking component and a hydrophilizing agent; and a separation functional layer formation step of forming a separation functional layer on the porous support layer. Effect of the Invention
[0007] According to one aspect of the present invention, a technique for producing a separation membrane having high organic solvent resistance and sufficient desalination function can be provided. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 shows a schematic cross-sectional view of a composite semipermeable membrane according to one embodiment of the present invention. [Diagram 2] FIG. 1 shows a flow diagram of a method for producing a composite semipermeable membrane according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The separation membrane produced by the production method of this embodiment is a composite semipermeable membrane. FIG. 1 shows a schematic configuration of a composite semipermeable membrane 10. As shown in FIG. 1, the composite semipermeable membrane 10 includes a porous support layer 2 and a separation functional layer (also called an active layer or a skin layer) 1 provided on the porous support layer 2. The porous support layer 2 may be formed on a substrate 3. The separation functional layer 1 in the composite semipermeable membrane 10 is an extremely thin layer (0.01 μm or more and 1 μm or less) arranged at the top, and is a layer where separation processing of the composite semipermeable membrane 10 is mainly performed. The porous support layer 2 mainly plays a role of supporting the separation functional layer 1. The substrate 3 is a part that further supports the porous support layer 2. In this specification, the term "semipermeable membrane" refers to a membrane that allows some components of the liquid to be treated to pass through and does not allow other components to pass through. In addition, the term "composite" in the composite semipermeable membrane means that a plurality of layers having different functions or configurations are laminated.
[0010] A flow diagram of the manufacturing method according to this embodiment is shown in Figure 2. As shown in Figure 2, the manufacturing method according to this embodiment may include a porous support layer forming step (S10) of forming a porous support layer containing polyetherimide, a crosslinking step (S20) of crosslinking the polyetherimide by contacting the porous support layer with an aqueous solution containing a crosslinking component and a hydrophilizing agent, and a separation function layer forming step (S30) of forming a separation function layer on the porous support layer. Each step will be described in detail below.
[0011] <Porous Support Layer Forming Step (S10)> In the porous support layer forming step (S10), a porous support layer 2 containing polyetherimide can be formed on a substrate 3 as shown in FIG.
[0012] The substrate used in this embodiment may be a fiber planar structure, specifically, a woven fabric, a knitted fabric, a nonwoven fabric, or the like. Of these, a nonwoven fabric is preferred. The nonwoven fabric may be produced by a spunbond method, a spunlace method, a meltblowing method, a carding method, an airlaying method, a wet method, a chemical bonding method, a thermal bonding method, a needle punch method, a water jet method, a stitch bonding method, an electrospinning method, or the like. The type of fiber constituting the nonwoven fabric is not limited, but is preferably a synthetic fiber. Specific examples of fibers include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN), polypropylene (PP), polyethylene (PE), polyphenylene sulfide (PPS), polyvinylidene fluoride (PVDF), polyglycolic acid (PGA), polylactic acid (PLA), nylon 6, polycaprolactone (PCL), polyethylene adipate (PEA), polyhydroxyalkanoate (PHA), or copolymers thereof. Of these, it is preferable to use polyesters such as polyethylene terephthalate because they are inexpensive, have high dimensional stability and moldability, and have high oil resistance.
[0013] The porous support layer formed in the porous support layer forming step (S10) contains polyetherimide. In this specification, "polyetherimide" refers to a polymer obtained by polymerizing an aromatic bis(ether anhydride) and an organic diamine, for example. [ka] In the above formula (1), n may be an integer of 1 or more and 8 or less, preferably 2 or more and 6 or less, and more preferably 3 or more and 5 or less. n H 2n - may be a chain or alicyclic alkylene group, and in the case of a chain alkylene group, it may be a straight-chain alkylene group or a branched alkylene group.
[0014] In addition, with respect to the two phthalimide moieties in formula (1) (the moieties represented by the formula obtained by removing the hydrogen bonded to the nitrogen in phthalimide and the hydrogen bonded to the carbon of the benzene ring), the bonding positions of the "O" to the benzene ring of the phthalimide moieties may each independently be any position, and preferably may each independently be the 3rd or 4th position. That is, in the structural unit of the above formula (1), [ka] In the moiety represented by the formula: each "O" may be attached independently to the 3- or 4-position of the benzene ring.
[0015] In addition, with respect to the two phenol moieties in formula (1) (the moieties obtained by removing the hydrogen of the hydroxyl group in phenol and the carbon bonded to the benzene ring carbon), the bonding positions of "O" to the benzene ring in this phenol moiety may be independently any position, and preferably may be independently the 3rd or 4th position. That is, in the structural unit of the above formula (1), [ka] In the moiety represented by the formula: independently, each "O" may be attached to the 3-position or 4-position of the benzene ring.
[0016] Furthermore, with respect to the portion derived from the diamine in formula (1) (the portion obtained by removing two hydrogen atoms from each amino group in the diamine), the bonding position of N in this diamine portion may be the 3rd or 4th position. That is, [ka] In the moiety represented by the following formula, the relationship between the bonding positions of the two N's bonded to the benzene ring may be the 3-position or the 4-position, that is, the meta-position or the para-position.
[0017] Furthermore, the structural unit represented by the above formula (1) is [ka] In this specification, the polymer represented by formula (5) may be referred to as polyetherimide in the narrow sense.
[0018] The number of constituent units of the above formula (1) or (5) may be preferably 10 to 400, more preferably 30 to 150. The weight average molecular weight of the above polymer (polyetherimide in a broad sense) contained in the porous support layer may be preferably 5,000 to 500,000, more preferably 10,000 to 50,000. The weight average molecular weight in the above range provides suitable processability and improves the strength of the porous support layer and thus the composite semipermeable membrane. The specific gravity of the polymer used may be 1.2 to 1.3.
[0019] Specific examples of polyetherimide include Ultem 1000, 4000, CRS 5000, 6000, 9000, etc., which are part of the "Ultem (registered trademark)" series manufactured by SHPP US, with Ultem 1000 being preferred.
[0020] In the porous support layer forming step (S10), the method of forming the porous support layer is not particularly limited, and non-solvent induced phase separation (NIPS), thermally induced solvent phase separation (TIPS), etc. can be used. However, it is preferable to use non-solvent induced phase separation (NIPS) because it can produce a uniform and wide porous layer. More specifically, after dissolving polyetherimide represented by formula (1) in a solvent to obtain a membrane forming solution, the membrane forming solution is applied to a substrate such as a nonwoven fabric by a knife coater or the like. Then, the polyetherimide in the applied solution is solidified, and the remaining solution is removed.
[0021] When the porous support layer forming step (S10) is performed by a non-solvent induced phase separation method, a uniform membrane forming solution can be prepared when dissolving polyetherimide in a solvent, and good microphase separation can be obtained. Therefore, it is preferable that the solvent used is water-soluble and has a high boiling point. For example, it is preferable that the solvent used is a water-soluble solvent with a boiling point of 130°C or more and 250°C or less. Specific examples of the solvent include dimethylformamide (DMF), dimethylsulfoxide (DMSO), dimethylacetamide (DMAC), 1,3-dimethyl-2-imidazolidinone (DMI), N-methylpyrrolidone (NMP), γ-butyrolactone (GBL), etc.
[0022] When producing the above-mentioned membrane forming solution, in addition to the above-mentioned solvent, a pore-opening agent such as a polyoxyalkylene such as polyethylene glycol or polybutylene glycol, a water-soluble polymer such as polyvinyl alcohol or polyvinyl butyral, glycerin, diethylene glycol, water, acetone, 1,3-dioxolane, etc. can be added. By adding a predetermined amount of the pore-opening agent, the porosity, pore size, etc. of the porous support layer can be adjusted.
[0023] The material forming the porous support layer may contain components other than polyetherimide, such as polymers other than polyetherimide, additives, etc. Examples of additives include functional particles such as colloidal silica and zeolite. In this case, the content of polyetherimide in the porous support layer is preferably 90% by mass or more, more preferably 95% by mass or more. The porous support layer is preferably substantially made of polyetherimide or made of polyetherimide. In this specification, "substantially made of" a specific component means that it is acceptable to contain components other than the specific component that are inevitably generated or mixed in during production.
[0024] In addition, the porous support layer formed in the porous support layer forming step (S20) is preferably a homogeneous layer as a whole. In this specification, a homogeneous layer means that the porous layer is composed of a single phase, that is, a plurality of separate island-like polymer phases are not observed by a conventional method in the art.
[0025] <Crosslinking step (S20)> After the porous support layer forming step (S10), the porous support layer, specifically the polyetherimide forming the porous layer, is crosslinked in the crosslinking step (S20). Crosslinking the polyetherimide increases the resistance to organic solvents, particularly aprotic polar solvents (described below). Crosslinking can be performed by applying a liquid containing a crosslinking component to the porous support layer formed in the previous step.
[0026] In the crosslinking step (S20), a solution of a crosslinking component (crosslinking component solution) is brought into contact with or attached to the porous support layer side of the structure consisting of the substrate and the porous support layer obtained in the porous support layer forming step (S10). For example, at least the porous support layer part of the structure consisting of the substrate and the porous support layer may be immersed in the crosslinking component solution, or the crosslinking component solution may be applied to the porous support layer side of the structure.
[0027] The cross-linking component used in the cross-linking step (S20) is a component capable of cross-linking polyetherimide molecules to form a cross-linked polyetherimide. The cross-linking component may be a compound having two or more nucleophilic groups, more specifically, a compound having two or more functional groups capable of reacting with the imide ring of the polyetherimide, and preferably a compound having two or more amino groups, i.e., a diamine or polyamine.
[0028] Examples of the crosslinking component include hydrocarbon compounds having two or more nucleophilic groups, polyether amines, polyethyleneimines, and derivatives thereof.
[0029] The hydrocarbon compound may be a compound in which two or more hydrogen atoms of a hydrocarbon are substituted with an amino group, for example, H2N-R1-NH2 (6) [wherein R1 is a chain alkylene group or an alicyclic alkylene group having from 2 to 20 carbon atoms], or H2N-R2-Ar-R3-NH2 (7) [wherein Ar is a substituted or unsubstituted arylene group having 6 to 10 carbon atoms, R2 and R3 are each independently a single bond or an alkylene group, and the total number of carbon atoms in R2 and R3 is 2 to 10.] When Ar is a substituted arylene group, the substituent may be an alkyl group having 1 to 3 carbon atoms.
[0030] When the crosslinking component is a diamine having formula (6) or formula (7), the diamine crosslinking component can move relatively flexibly during the crosslinking reaction, and the crosslinking reaction between polyetherimides is promoted (the crosslinking points can be increased), so that the organic solvent resistance can be further improved and a separation membrane capable of continuously removing both salts and organic solvents over a long period of time can be provided. In addition, the distance between the polymers in the polyetherimide after crosslinking is appropriately maintained, and it is considered that the polymer constituting the porous support layer has appropriate properties (hardness, elasticity, etc.).
[0031] As is apparent from formulas (6) and (7) above, the cross-linking component may be an aliphatic or aromatic diamine.
[0032] When the crosslinking component is an aliphatic diamine, R1 in formula (6) may be an alkylene group having preferably 3 to 20 carbon atoms, more preferably 4 to 8 carbon atoms, and even more preferably 5 to 7 carbon atoms. The lower limit of the carbon number allows the diamine crosslinking component to move flexibly during the crosslinking reaction, and the effect of promoting the crosslinking reaction between polyetherimides can be improved. The upper limit of the carbon number allows the distance between the polymers in the polyetherimide after crosslinking to be appropriately maintained, and the effect of obtaining appropriate properties as a polymer constituting the porous support layer can be improved. R1 may be a chain alkylene group or an alicyclic alkylene group, and in the case of a chain alkylene group, it may be a straight-chain alkylene group or a branched alkylene group. However, from the viewpoint of allowing the crosslinking component to move flexibly, a straight-chain alkylene group is preferred.
[0033] When the crosslinking component is an aliphatic diamine, specific examples thereof include hexamethylenediamine, heptamethylenediamine, octamethylenediamine, pentamethylenediamine, 1,4-butanediamine, 1,3-propanediamine, ethylenediamine, trimethylhexamethylenediamine, isophoronediamine, 1,3-cyclohexanebis(methylamine), and the like.
[0034] When the crosslinking component is an aromatic diamine, the total number of carbon atoms of R2 and R3 in formula (7) may be an alkylene group having preferably 3 to 9 carbon atoms, more preferably 4 to 8 carbon atoms, and even more preferably 5 to 7 carbon atoms. The lower limit of the total number of carbon atoms allows the diamine crosslinking component to move flexibly during the crosslinking reaction, and the effect of promoting the crosslinking reaction between polymers can be improved. In addition, the upper limit of the total number of carbon atoms allows the distance between polymers in the polyetherimide after crosslinking to be appropriately maintained, and the effect of obtaining appropriate properties as a polymer constituting the porous support layer can be improved. In addition, R2 and R3 may be a straight-chain alkylene group or a branched alkylene group. However, from the viewpoint of allowing the crosslinking component to move flexibly, either R2 or R3, preferably both, may be a straight-chain alkylene group.
[0035] The aromatic diamine represented by formula (7) is preferable from the viewpoint that the presence of the arylene group improves the organic solvent resistance of the crosslinked portion in the polyetherimide after crosslinking, thereby improving the organic solvent resistance of the porous support layer. Ar in formula (7) is preferably a substituted or unsubstituted phenylene group, more preferably a substituted or unsubstituted p-phenylene group. When Ar is a phenylene group, the crosslinking reaction between polyetherimides can be maintained without excessively inhibiting the flexible movement of the diamine crosslinking component during the crosslinking reaction, and since it is chemically stable, the organic solvent resistance of the crosslinked portion in the polyetherimide after crosslinking can be further improved. In addition, from the viewpoint that the crosslinking component can move flexibly, Ar is preferably an unsubstituted arylene group.
[0036] When the crosslinking component is an aromatic diamine, specific examples thereof include p-xylylenediamine and m-xylylenediamine.
[0037] Furthermore, when the crosslinking component is a polyetheramine, it may be a compound having ethylene oxide (EO) and / or propylene oxide (PO) as the main skeleton and having two or more amino groups. Examples of polyetheramines or derivatives thereof include polyoxyethylenediamine, polyoxypropylenediamine, poly(oxyethylene / oxypropylene)diamine, triethyleneglycoldiamine, etc. Examples of polyethyleneimines or derivatives thereof include diethylenetriamine, triethylenetetramine, hexaethylenepentamine, pentaethylenehexamine, tris(2-aminoethyl)amine, dimethylethylenediamine, etc. When the crosslinking component is a polyethyleneimine, it is preferable that the number of nitrogen atoms in the compound is 6 or more.
[0038] The crosslinking component used in the crosslinking step (S20) may be one type alone or two or more types in combination, in which case an aliphatic diamine and an aromatic diamine may be combined.
[0039] The content of the crosslinking component in the crosslinking component solution may be preferably 0.5% by mass or more and 25% by mass or less, more preferably 1% by mass or more and 20% by mass or less, and even more preferably 3% by mass or more and 15% by mass or less, based on the total amount of the crosslinking component solution. By setting the concentration of the crosslinking component solution to 0.5% by mass or more, sufficient crosslinking can be formed, and the organic solvent resistance of the porous support layer can be improved. In addition, by setting the concentration of the crosslinking component solution to 25% by mass or less, the membrane performance of the porous support layer, including water permeability, can be maintained.
[0040] Furthermore, the crosslinking component solution used in the crosslinking step (S20) contains a hydrophilizing agent in addition to the above crosslinking component. The hydrophilizing agent is an agent that has a function of hydrophilizing (increasing hydrophilicity) the surface of the crosslinked polyetherimide porous support layer without inhibiting the crosslinking reaction between the crosslinking component and the polyetherimide. In addition, the hydrophilizing agent is preferably one that does not swell the polyetherimide before crosslinking. For example, the hydrophilizing agent may be a compound having a lipophilic group and a hydrophilic group in one molecule, for example, an organic acid having a strong acid group. Therefore, examples of the hydrophilic group contained in the hydrophilizing agent include strong acid groups that dissociate in water, such as acid groups derived from aromatic sulfonic acid, aliphatic sulfonic acid, alicyclic sulfonic acid, trifluoroacetic acid, nitric acid, hydrochloric acid, sulfuric acid, etc. The hydrophilizing agent is particularly preferably an organic acid having a sulfonic acid group. In addition, the lipophilic group contained in the hydrophilizing agent may be a substituted or unsubstituted hydrocarbon group having 5 to 50 carbon atoms. The hydrophilizing agent is preferably an aromatic hydrocarbon having a sulfonic acid group or an alicyclic hydrocarbon having a sulfonic acid group, and specific examples of the hydrophilizing agent include camphorsulfonic acid (CSA) and paratoluenesulfonic acid (pTSA).
[0041] After the crosslinking step (S20), the subsequent separation functional layer forming step (S30) is performed. In order to properly form the separation functional layer, it is preferable that the surface of the porous support layer after crosslinking is highly hydrophilic. In this embodiment, as described above, a hydrophilizing agent is added to the crosslinking component solution used in the crosslinking step (S20), so that the porous polyetherimide layer after crosslinking is given high hydrophilicity. Therefore, the wettability of the porous support layer after crosslinking with respect to the polyfunctional amine aqueous solution (described later) that is first applied to the porous support layer is improved, and the desired separation functional layer can be formed.
[0042] The content of the hydrophilizing agent in the total amount of the crosslinking component solution may be preferably 1% by mass or more and 20% by mass or less, more preferably 3% by mass or more and 15% by mass or less. When the content of the hydrophilizing agent is 3% by mass or more, the effect of hydrophilizing the surface of the porous support layer described above can be improved. In addition, when the content of the hydrophilizing agent is 15% by mass or less, the desired separation functional layer can be formed without inhibiting the reaction in the separation functional layer forming step (S30).
[0043] In the crosslinking step (S20), the porous support layer can be contacted with the crosslinking component solution as described above, and then heat treated. The crosslinking rate is increased by heat treatment, so the time required for the crosslinking step (S20) can be shortened, and the manufacturing time can be shortened. In addition, when heat treatment is performed, the hydrophilicity of the surface may decrease due to the evaporation of the aqueous component from the surface of the porous support layer. However, in this embodiment, the above-mentioned hydrophilizing agent is added to the crosslinking component solution applied to the porous support layer, so that such a decrease in the hydrophilicity of the surface can be prevented. Therefore, the manufacturing time can be shortened, and an appropriate separation functional layer can be formed, and a composite semipermeable membrane having an appropriate desalination function can be obtained.
[0044] In the crosslinking step (S20), when a heat treatment is performed after application of the crosslinking component solution, the heat treatment temperature may be preferably 60°C or more and 200°C or less, more preferably 80°C or more and 150°C or less. By setting the heat treatment temperature at 60°C or more, the crosslinking speed can be increased, which contributes to shortening the production time. In addition, by setting the heat treatment temperature at 200°C or less, it is possible to prevent the porous support layer from being degenerated due to thermal shrinkage or the like. The time for the heat treatment may be preferably 30 seconds or more and 60 minutes or less, more preferably 1 minute or more and 40 minutes or less.
[0045] The time for contacting the porous support layer with the crosslinking component solution, for example, the time for immersing the porous support layer in the crosslinking component solution, varies depending on conditions such as the type and concentration of the crosslinking component, and the presence or absence of heat treatment, but may be preferably 5 seconds or more and 180 minutes or less, more preferably 30 seconds or more and 120 minutes or less, and even more preferably 1 minute or more and 90 minutes or less. By setting the time for immersing the porous support layer in the diamine crosslinking component solution within the above range, sufficient crosslinking can be formed, the organic solvent resistance of the crosslinked polyetherimide can be improved, the water permeability of the obtained porous support layer can be maintained, and the productivity can be improved. In addition, when the above-mentioned heat treatment is performed, the time for contacting the porous support layer with the crosslinking component solution can be shortened. Depending on the conditions of the heat treatment, the time for contacting the porous support layer with the crosslinking component solution can be, for example, 60 minutes or less, 30 minutes or less, 10 minutes or less, or 5 minutes or less.
[0046] The temperature when the crosslinking component solution is brought into contact with the porous support layer may be preferably from 10° C. to 70° C., more preferably from 15° C. to 40° C. By setting the temperature in the crosslinking step within the above range, freezing of the solution and evaporation of the solvent can be prevented.
[0047] After the crosslinking step (S20), the separation functional layer forming step (S30) is performed. However, before the separation functional layer forming step (S30), a washing step may be performed to remove remaining excess components (crosslinking components and / or hydrophilizing agents). In the washing step, at least the crosslinked porous support layer is washed with one or more washing solutions of water and lower alcohol. For example, at least the crosslinked porous support layer is immersed in one or more washing solutions of water and lower alcohol. The lower alcohol may be methanol, ethanol, isopropyl alcohol, etc., and isopropyl alcohol is preferred. In this case, the washing solution may be heated to 40°C or higher and 80°C or lower. When the porous support layer is immersed in the washing solution, the immersion time may be 30 minutes or more and 120 minutes or less.
[0048] <Separation functional layer formation step (S30)> In the separation functional layer formation step (S30), a solution of a polyfunctional amine compound is applied to the surface of the crosslinked polyetherimide porous support layer formed on the substrate as described above (S31), and then the solution is brought into contact with a solvent solution of an acid halide compound (S32). This allows interfacial polymerization between the polyfunctional amine and the acid halide to proceed, forming a crosslinked polyamide separation functional layer.
[0049] The polyfunctional amine (a compound having two or more reactive amine groups) may be an aromatic polyfunctional amine, an aliphatic polyfunctional amine, or a combination thereof. Specific examples of aromatic polyfunctional amines include m-phenylenediamine, p-phenylenediamine, 1,3,5-triaminobenzene, or N-alkylated products thereof, such as N,N-dimethyl m-phenylenediamine, N,N-diethyl m-phenylenediamine, N,N-dimethyl p-phenylenediamine, and N,N-diethyl p-phenylenediamine, with m-phenylenediamine being preferred. The aliphatic polyfunctional amine may be a chain or alicyclic polyfunctional amine. Specific examples of aliphatic polyfunctional amines include ethylenediamine and ethylenediamine derivatives, chain diamines such as 1,6-diaminohexane, cyclic diamines such as 1,3-diaminocyclohexane, 1,2-diaminocyclohexane, and 1,4-diaminocyclohexane, piperazine, and piperazine derivatives. Examples of piperazine derivatives include 2,5-dimethylpiperazine, 2-methylpiperazine, 2,6-dimethylpiperazine, 2,3,5-trimethylpiperazine, 2,5-diethylpiperazine, 2,3,5-triethylpiperazine, 2-n-propylpiperazine, 2,5-di-n-butylpiperazine, ethylenediamine, etc., among which piperazine is preferred. The above-mentioned polyfunctional amines can be used alone or in combination of two or more kinds.
[0050] When an aromatic polyfunctional amine such as m-phenylenediamine is used in forming the separation functional layer, a composite semipermeable membrane suitable for selectively separating monovalent salts can be obtained. When an aliphatic polyfunctional amine such as piperazine is used, a composite semipermeable membrane suitable for selectively separating divalent salts can be obtained.
[0051] The acid halide compound is not particularly limited as long as it can give a polyamide by reacting with the polyfunctional amine, but it is preferable that the acid halide has two or more halide carbonyl groups in one molecule.Specific examples of the acid halide compound include halide compounds of fatty acids such as oxalic acid, malonic acid, maleic acid, fumaric acid, glutaric acid, 1,3,5-cyclohexane tricarboxylic acid, 1,3-cyclohexane dicarboxylic acid, and 1,4-cyclohexane dicarboxylic acid, and acid halide compounds of aromatic acids such as phthalic acid, isophthalic acid, 1,3,5-benzene tricarboxylic acid, 1,2,4-benzene tricarboxylic acid, 1,3-benzene dicarboxylic acid, and 1,4-benzene dicarboxylic acid.These acid halide compounds can be used alone or in combination of two or more kinds.
[0052] When the polyfunctional amine is applied to the porous support layer (S31), the ring imide structure in the polyetherimide contained in the porous support layer opens and bonds to form an amide bond (-CO-NH-). When the polyfunctional amine is further contacted with a solution of an acid halide (S32), the amino group remaining in the polyfunctional amine reacts with trimesic acid trichloride to form a further amide bond (-CO-NH-). In this way, by using the polyfunctional amine, it is possible to obtain a state in which the polyetherimide and the acid halide are bonded via the polyfunctional amine. This strengthens the bond between the porous support layer and the separation functional layer, and prevents the occurrence of delamination and leak spots during use of the composite semipermeable membrane.
[0053] The concentration of the polyfunctional amine solution used in applying the polyfunctional amine solution to the porous support layer (S31) may be 0.5% by mass or more and 15% by mass or less. When the polyfunctional amine is an aromatic polyfunctional amine, the concentration may be preferably 1.8% by mass or more and 15% by mass or less, more preferably 1.8% by mass or more and 10% by mass or less, even more preferably 1.8% by mass or more and 13% by mass or less, and even more preferably 2% by mass or more and 10% by mass or less. When the polyfunctional amine is an aliphatic polyfunctional amine, the concentration may be preferably 0.5% by mass or more and 15% by mass or less, more preferably 0.5% by mass or more and 10% by mass or less, and even more preferably 1.5% by mass or more and 10% by mass or less.
[0054] Furthermore, the pH of the polyfunctional amine solution may be preferably 6.5 or more and 13.5 or less, more preferably 7 or more and 13 or less. The pH of the polyfunctional amine solution can be appropriately adjusted by adding, for example, an acid such as hydrochloric acid and / or an alkali such as sodium hydroxide to the solution.
[0055] In the composite semipermeable membrane manufactured by the manufacturing method of this embodiment, the crosslinking component solution used in the crosslinking step (S20) contains a hydrophilizing agent, so that a crosslinked polyamide separation function layer is appropriately formed in the separation function layer formation step (S30). Therefore, the obtained composite semipermeable membrane has a good salt separation function regardless of the processing method in the crosslinking step (S20), even if it is subjected to, for example, heat treatment. In addition, since the polyetherimide of the porous support layer is crosslinked in the crosslinking step (S20), the resistance of the porous support layer to organic solvents is improved.
[0056] The composite semipermeable membrane obtained in this embodiment is suitable for treating a liquid containing an organic solvent. Here, the organic solvent may include a nonpolar solvent, a protic solvent, and an aprotic polar solvent, but the composite semipermeable membrane in this embodiment is particularly excellent in resistance to aprotic polar solvents, particularly to solvents having a relative dielectric constant of 6 or more and 64 or less. In addition, the aprotic polar solvent may be a solvent that has a high ability to dissolve the pre-crosslinked polymer (polyetherimide in a broad sense) that is used as the base for forming the porous support layer.
[0057] Specific examples of aprotic polar solvents include N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (THF), ethyl acetate (EtOAc), acetone, N,N-dimethylformamide (DMF), acetonitrile, dimethyl sulfoxide (DMSO), methyl ethyl ketone (MEK), dimethylacetamide (DMAc), N-ethyl-2-pyrrolidone, N,N-diethylformamide, N,N-diethylacetamide, dichloromethane (DCM), propylene carbonate (PC), hexamethylphosphoric triamide (HMPA), etc. Among these, the composite semipermeable membrane according to this embodiment has high resistance to one or more of dimethylacetamide (DMAc), ethyl acetate (EtOAc), and acetone, and particularly high resistance to dimethylacetamide (DMAc).
[0058] Examples of non-polar solvents include hexane, chloroform, 1,4-dioxane, benzene, toluene, xylene, ethylbenzene, etc. Examples of protic solvents include formic acid, IPA, ethanol, methanol, acetic acid, etc.
[0059] Furthermore, the composite semipermeable membrane constructed according to this embodiment is also excellent in the performance of separating an organic solvent from a liquid containing the above-mentioned organic solvent (organic solvent rejection performance), and is particularly excellent in the performance of separating an aprotic polar solvent from a liquid to be treated that contains an aprotic polar solvent. Here, the rejection performance includes the rejection rate of the solute by the composite semipermeable membrane and the water permeability. The composite semipermeable membrane according to this embodiment can realize a high rejection rate for both organic solvents and salts, and can therefore be suitably used in processes for obtaining reclaimed water from various industrial wastewater. Since the organic solvent and salt contained in the liquid to be treated can be removed in one step, it is possible to avoid the complication of the treatment equipment and the complication of the treatment process.
[0060] The composite semipermeable membrane obtained in this embodiment is suitably used for desalination of a liquid to be treated that contains an organic solvent, particularly for desalination of a liquid to be treated that contains an aprotic polar solvent. Examples of such a liquid to be treated include wastewater generated in oil refineries, petrochemical plants, thermal power plants, automobile manufacturing plants, oil and fat manufacturing plants, food manufacturing plants, etc., wastewater generated in homes, seawater containing an organic solvent, or liquid obtained by pretreating these.
[0061] The composite semipermeable membrane obtained in this embodiment is preferably configured in a flat membrane shape. The flat composite semipermeable membrane according to this embodiment can be suitably used in a spiral-type membrane module configured by winding the composite semipermeable membrane in a spiral shape around the outside of a water collection pipe. It can also be applied to a disk-tube-type flat membrane module.
[0062] The composite semipermeable membrane obtained by the manufacturing method of this embodiment has a property of being difficult to deform even when pressure is applied for a long time, that is, has excellent pressure resistance. It can fully cope with operation at high operating pressures by reverse osmosis, for example, operating pressures of 1 to 12 MPa. More specifically, the compressibility of the part of the composite semipermeable membrane consisting of the porous support layer and the separation functional layer, that is, the ratio of the thickness reduced by compression at a predetermined pressure for a predetermined time (the initial thickness minus the thickness after compression) to the initial thickness, is also small. For example, in the composite semipermeable membrane according to this embodiment, the compressibility when the treated liquid is treated at an operating pressure of 5.5 MPa for 2 hours can be 20% or less, preferably 10% or less, more preferably 5% or less.
[0063] The porosity (air porosity) of the porous support layer before use of the composite semipermeable membrane is preferably 40% or more and 70% or less, and more preferably 55% or more and 65% or less. By having a porosity in the above range, appropriate salt blocking performance and water permeability as a reverse osmosis membrane can be obtained, and the pressure resistance and strength of the composite semipermeable membrane can be improved. Furthermore, even when the composite semipermeable membrane is compressed and reduced in thickness by application of a long time or high pressure, high permeability can be maintained.
[0064] The average pore size on the surface of the porous support layer is preferably 5 nm to 50 nm, more preferably 7 nm to 20 nm, which allows the reverse osmosis membrane to have appropriate salt blocking performance and water permeability.
[0065] The thickness of the entire composite semipermeable membrane may be 60 μm or more and 250 μm or less. The thickness of the porous layer may be 10 μm or more and 100 μm or less. The thickness of the separation functional layer may be 0.01 μm or more and 1 μm or less. The thickness of the substrate may be 50 μm or more and 200 μm or less.
[0066] One embodiment of the present invention may be a composite semipermeable membrane produced by a production method including a porous support layer formation step of forming a porous support layer containing polyetherimide, a crosslinking step of crosslinking the polyetherimide by contacting the porous support layer with an aqueous solution containing a crosslinking component and a hydrophilizing agent, and a separation functional layer formation step of forming a separation functional layer on the porous support layer. EXAMPLES
[0067] Hereinafter, the embodiments of the present invention will be described based on examples, but the present invention is not limited to these examples.
[0068] Example 1 20 parts by mass of polyetherimide (SHPP US "Ultem 1000", weight average molecular weight: 32,000), 51 parts by mass of N,N-dimethylacetamide, and 29 parts by mass of 1,3-dioxolane were dissolved by heating at 50°C to prepare a homogeneous film-forming solution. The film-forming solution was cooled to room temperature and then poured onto a polyester nonwoven fabric substrate (thickness 0.1 mm, density 0.7 g / cm 3 After a running distance of 200 mm, the plate was immersed in a coagulating liquid (water) at 40°C to coagulate, and then washed in a water washing tank at 70°C.
[0069] The thus obtained membrane consisting of the substrate and the polyetherimide porous support layer was immersed in a liquid tank filled with a crosslinking component aqueous solution for 1 hour at 25°C so that only the support membrane layer side of the membrane was in contact with the liquid tank. The crosslinking component aqueous solution was an aqueous solution containing 3.0% by mass of hexamethylenediamine (HDA) and 6% by mass of camphorsulfonic acid (CSA) as a hydrophilizing agent. After the above immersion, the membrane was removed from the liquid tank and further placed in an oven (ADVANTEC's "DRM620DA") and heated at 130°C for 30 minutes. After the heating was completed, the membrane was removed from the oven and washed with water. This resulted in a membrane after crosslinking treatment.
[0070] Furthermore, the surface of the porous support layer of the membrane after the crosslinking treatment was contacted with a 3.0% by mass aqueous solution of m-phenylenediamine, and then the excess m-phenylenediamine aqueous solution was removed. Then, the side of the porous layer that was contacted with the m-phenylenediamine aqueous solution was contacted with a naphthene solution containing 0.1% by mass of trimesic acid trichloride (aromatic acid halide compound) and 0.13% by mass of isophthalic acid chloride for 30 seconds. As a result, a crosslinked polyamide layer (separation functional layer) was formed on the porous layer. Then, by drying in a dryer at 140°C, a composite semipermeable membrane was obtained in which the substrate, the porous layer, and the separation functional layer were arranged in this order.
[0071] Example 2 A composite semipermeable membrane was obtained in the same manner as in Example 1, except that a membrane consisting of a substrate and a polyetherimide porous support layer was immersed in an aqueous solution of a crosslinking component and then washed without heating.
[0072] Example 3 A composite semipermeable membrane was obtained in the same manner as in Example 1, except that the membrane consisting of the substrate and the polyetherimide porous support layer was immersed in the aqueous crosslinking component solution for 5 minutes.
[0073] Example 4 A composite semipermeable membrane was obtained by treating in the same manner as in Example 2, except that the membrane consisting of the substrate and the polyetherimide porous support layer was immersed in the crosslinking component aqueous solution for 5 minutes. That is, after the immersion time of 5 minutes, the membrane was washed without heating.
[0074] Comparative Example 1 A composite semipermeable membrane was obtained by treating in the same manner as in Example 1, except that a 3.0 mass% aqueous solution of hexamethylenediamine (HDA) was used as the cross-linking component aqueous solution in which the membrane consisting of the substrate and the polyetherimide porous support layer was immersed, that is, a cross-linking component aqueous solution not containing a hydrophilizing agent was used.
[0075] Comparative Example 2 After obtaining a membrane consisting of a substrate and a polyetherimide porous support layer, a composite semipermeable membrane was obtained in the same manner as in Example 1, except that a separation functional layer was formed without crosslinking the porous support layer.
[0076] The composite semipermeable membrane of each example was evaluated as follows.
[0077] <Membrane performance evaluation> The obtained composite semipermeable membrane was evaluated for its sufficient performance as a reverse osmosis membrane. A membrane evaluation device (Nitto Denko Corporation, flow-type flat membrane test cell, Membrane Master C70-F, effective permeation area 32.5 cm) was used. 2 ). A 3.2% by mass NaCl aqueous solution was used, and the operation was carried out for 1 hour in a cross-flow mode at 25°C, with a supply flow rate of 5 L / min and a pressure of 5.5 MPa. The NaCl concentrations were measured on the supply side and the permeation side, and the salt rejection rate (%) was calculated. In addition, in the above rejection evaluation, the amount of feed water passing through the membrane was measured, and the value converted into the amount of water passing through per square meter of separation membrane per day was calculated as the permeation flux (m 3 / m 2 / d). The evaluation criteria were as follows: 〇: Salt rejection rate is 99% or more and permeation flux is 0.3m 3 / m 2 / d) or higher. ×: Salt rejection rate is less than 99% or permeation flux is less than 0.3 m 3 / m 2 / d).
[0078] <Evaluation of organic solvent resistance> Furthermore, the organic solvent resistance of the obtained composite semipermeable membrane was evaluated. The entire composite semipermeable membrane was immersed in 100% by mass of N,N-dimethylacetamide at 25°C for 1 hour, and then the state was visually observed. The evaluation criteria were as follows. ◯: The porous support layer was completely or almost completely dissolved. Δ: Part of the porous support layer was dissolved. ×: The porous support layer was almost or completely dissolved.
[0079] The results are shown in Table 1.
[0080] [Table 1]
[0081] As shown in Table 1, it was found that a composite semipermeable membrane having sufficient desalination performance can be obtained by adding a hydrophilizing agent to the crosslinking component aqueous solution in the crosslinking step of crosslinking the polyetherimide in the porous support layer to form a crosslinked polyetherimide (Examples 1 to 4). In contrast, in an example in which a hydrophilizing agent was not added to the crosslinking component aqueous solution in the crosslinking step (Comparative Example 1), the obtained composite semipermeable membrane did not have sufficient membrane performance. It was also found that the composite semipermeable membrane produced without the crosslinking step (Comparative Example 2) was inferior in organic solvent resistance to the composite semipermeable membrane obtained through the crosslinking step.
[0082] It was also found that sufficient membrane performance and organic solvent resistance could be obtained by carrying out the crosslinking step (Examples 1 to 4). Furthermore, it was found that sufficient improvement in membrane performance and organic solvent resistance could be obtained by carrying out heating even if the immersion time was 5 minutes (Example 3). In other words, when attempting to obtain a membrane with equal or higher membrane performance and organic solvent resistance, it can be said that heating shortens the production time. [Explanation of symbols]
[0083] 1 Separation functional layer 2 Porous layer (porous support layer) 3 Base material 10 Composite semipermeable membrane
Claims
1. forming a porous support layer comprising a polyetherimide; a crosslinking step of crosslinking the polyetherimide by contacting the porous support layer with an aqueous solution containing a crosslinking component and a hydrophilizing agent; and forming a separation functional layer on the porous support layer.
2. The method for producing a composite semipermeable membrane according to claim 1 , wherein the crosslinking step comprises immersing the porous support layer in the aqueous solution and then heat treating the porous support layer.
3. The method for producing a composite semipermeable membrane according to claim 2, wherein the heat treatment is carried out at a temperature of 60°C or higher and 200°C or lower.
4. The method for producing a composite semipermeable membrane according to claim 1 or 2, wherein the hydrophilizing agent is an organic acid having a strong acid group.
5. The method for producing a composite semipermeable membrane according to claim 4, wherein the hydrophilizing agent comprises at least one of camphorsulfonic acid (CSA) and paratoluenesulfonic acid (pTSA).
6. The method according to claim 1 or 2, wherein the concentration of the hydrophilizing agent is from 3% by mass to 15% by mass.
7. The method for producing a composite semipermeable membrane according to claim 1 or 2, wherein the crosslinking component comprises a crosslinking component containing two or more functional groups capable of reacting with an imide ring in the polyetherimide.
8. The cross-linking component is selected from the group consisting of hexamethylenediamine, heptamethylenediamine, octamethylenediamine, pentamethylenediamine, 1,4-butanediamine, 1,3-propanediamine, ethylenediamine, trimethylhexamethylenediamine, isophoronediamine, and 1,3-cyclohexanebis(methylamine); p-xylylenediamine, m-xylylenediamine; polyoxyethylenediamine, polyoxypropylenediamine, poly(oxyethylene / oxypropylene)diamine, and triethylene glycol diamine; and The method for producing a composite semipermeable membrane according to claim 1 or 2, comprising one or more selected from the group consisting of diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, tris(2-aminoethyl)amine, and dimethylethylenediamine.
9. The method for producing a composite semipermeable membrane according to claim 1 or 2, further comprising a washing step of washing the porous support layer after the crosslinking step.
10. 3. The method for producing a composite semipermeable membrane according to claim 1 or 2, wherein the separation functional layer forming step comprises forming a crosslinked polyamide separation functional layer by reacting with a polyfunctional amine and an acid chloride on the surface of the porous support layer.
Citation Information
Patent Citations
Microporous membrane used in filtering and its production
JP1989155909A