Resin composition
A resin composition with polyphenylene ether particles, epoxy resin, and inorganic filler addresses cracking and adhesion issues in circuit boards, ensuring good dielectric properties and stability under harsh conditions.
Patent Information
- Application Number
- JP2023048873
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2043-03-24
AI Technical Summary
Conventional resin compositions used for circuit boards, which provide good dielectric properties, tend to crack after desmear treatment and suffer from deteriorated adhesion with conductor layers under high temperature and high humidity conditions.
A resin composition comprising polyphenylene ether particles, an epoxy resin, a curing agent, and an inorganic filler, with specific particle size and content ratios, to enhance crack resistance and adhesion to conductor layers.
The composition achieves good crack resistance and adhesion to conductor layers even under high temperature and high humidity environments, while maintaining excellent dielectric properties.
Smart Images

Figure 2024137375000001 
Figure 2024137375000002 
Figure 2024137375000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, and further to a resin sheet, a cured product, a circuit board, and a semiconductor device. [Background technology]
[0002] Resin compositions containing epoxy resins and their curing agents produce cured products with excellent insulation properties, heat resistance, adhesion, and other properties, and therefore have been widely used as insulating materials for circuit boards such as printed wiring boards and rewiring boards for semiconductor chip packages.
[0003] On the other hand, with the recent increase in communication speed, insulating materials for circuit boards are required to have excellent dielectric properties (low dielectric tangent) in order to reduce transmission loss when operating in a high-frequency environment. Known insulating materials with excellent dielectric properties include those that use specific curing agents such as active ester curing agents that can reduce or suppress the generation of polar groups such as secondary hydroxyl groups in the curing reaction of epoxy resins, or those that employ specific compositions such as a high content of inorganic filler (for example, Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-157027 A [Patent Document 2] JP 2020-94213 A [Patent Document 3] JP 2020-152780 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the production of circuit boards, when an insulating layer is formed using a conventional resin composition that contributes to good dielectric properties, the obtained insulating layer tends to easily generate cracks after a desmear treatment.
[0006] In the course of investigating ways to improve crack resistance, the inventors found that adding organic particles can improve crack resistance to some extent. However, they also found that adding organic particles in an amount sufficient to improve crack resistance can cause problems such as deterioration of dielectric properties, thereby diminishing the originally desired effect, and deterioration of adhesion to the conductor layer when exposed to a high-temperature, high-humidity environment.
[0007] An object of the present invention is to provide a novel resin composition that can provide a cured product that exhibits good crack resistance and good adhesion to a conductor layer when exposed to a high-temperature, high-humidity environment, even when a composition that contributes to good dielectric properties is adopted. [Means for solving the problem]
[0008] As a result of intensive investigations, the present inventors have found that the above problems can be solved by a resin composition having the following configuration, and have completed the present invention.
[0009] That is, the present invention includes the following. [1] A resin composition comprising: (A) polyphenylene ether particles; (B) an epoxy resin; (C) a curing agent; and (D) an inorganic filler. [2] The resin composition according to [1], wherein the average particle size of the (A) component is 5 μm or less. [3] (A) 90% particle size of component D 90 The resin composition according to [1] or [2], wherein the particle size is 2 μm or less. [4] The resin composition according to any one of [1] to [3], wherein the content of the component (A) is 0.5% by mass or more when the resin components of the resin composition are taken as 100% by mass. [5] The resin composition according to any one of [1] to [4], wherein the component (C) contains (C-1) one or more curing agents selected from the group consisting of active ester curing agents, cyanate ester curing agents, and carbodiimide curing agents. [6] The resin composition according to [5], wherein a mass ratio of the component (C-1) to the component (B) (component (C-1) / component (B)) is 1 or more. [7] The resin composition according to any one of [1] to [6], wherein the content of the component (B) is 5% by mass or more when the resin component of the resin composition is taken as 100% by mass. [8] The resin composition according to any one of [1] to [7], wherein the content of the component (D) is 40% by mass or more, when the non-volatile components of the resin composition are taken as 100% by mass. [9] The resin composition according to any one of [1] to [8], wherein the component (A) is an emulsion polymer or a suspension polymer.
[10] The resin composition according to any one of [1] to [9], wherein the component (A) is insoluble in a solvent.
[11] The resin composition according to any one of [1] to
[10] , which is for use in an insulating layer of a circuit board.
[12] A resin sheet comprising a support and a layer of the resin composition according to any one of [1] to
[11] provided on the support.
[13] The resin sheet according to
[12] , wherein the support is a thermoplastic resin film or a metal foil.
[14] A cured product of the resin composition according to any one of [1] to
[11] .
[15] A circuit board comprising an insulating layer made of a cured product of the resin composition according to any one of [1] to
[11] .
[16] A semiconductor device comprising the circuit board according to
[15] . Effect of the Invention
[0010] According to the present invention, it is possible to provide a novel resin composition that exhibits good crack resistance even when a composition that contributes to good dielectric properties is adopted, and that can provide a cured product that exhibits good adhesion to a conductor layer when exposed to a high-temperature, high-humidity environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] <Terminology explanation> As used herein, the term "optionally substituted" in reference to a compound or group means both the case where none of the hydrogen atoms of the compound or group are substituted with a substituent, and the case where some or all of the hydrogen atoms of the compound or group are substituted with a substituent.
[0012] In this specification, unless otherwise specified, the term "substituent" means a halogen atom, an alkyl group, an alkenyl group, a cycloalkyl group, an alkoxy group, a cycloalkyloxy group, an alkylthio group, a cycloalkylthio group, an aryl group, an aryloxy group, an arylthio group, an arylalkyl group, an arylalkoxy group, a monovalent heterocyclic group, an alkylidene group, an acyl group, an acyloxy group, a hydroxy group, an amino group, a silyl group, a carboxy group, a sulfo group, a cyano group, a nitro group, a mercapto group, or an oxo group.
[0013] Examples of halogen atoms used as a substituent include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. The alkyl group used as a substituent may be either linear or branched. The number of carbon atoms in the alkyl group is preferably 1 to 12, more preferably 1 to 6, and even more preferably 1 to 3. The alkenyl group used as a substituent may be either linear or branched. The number of carbon atoms in the alkenyl group is preferably 2 to 12, more preferably 2 to 6, and even more preferably 2 or 3. The number of carbon atoms in the cycloalkyl group used as a substituent is preferably 3 to 12, more preferably 3 to 6. The alkoxy group used as a substituent may be either linear or branched. The number of carbon atoms in the alkoxy group is preferably 1 to 12, more preferably 1 to 6. The number of carbon atoms in the cycloalkyloxy group used as a substituent is preferably 3 to 12, more preferably 3 to 6. The alkylthio group used as a substituent may be either linear or branched. The number of carbon atoms in the alkylthio group is preferably 1 to 12, more preferably 1 to 6. The number of carbon atoms in the cycloalkylthio group used as a substituent is preferably 3 to 12, more preferably 3 to 6. The number of carbon atoms in the aryl group used as a substituent is preferably 6 to 14, more preferably 6 to 10. The number of carbon atoms in the aryloxy group used as a substituent is preferably 6 to 14, more preferably 6 to 10. The number of carbon atoms in the arylthio group used as a substituent is preferably 6 to 14, more preferably 6 to 10. The number of carbon atoms in the arylalkyl group used as a substituent is preferably 7 to 15, more preferably 7 to 11. The number of carbon atoms in the arylalkoxy group used as a substituent is preferably 7 to 15, more preferably 7 to 11. The monovalent heterocyclic group used as a substituent refers to a group obtained by removing one hydrogen atom from the heterocycle of a heterocyclic compound. The number of carbon atoms in the monovalent heterocyclic group is preferably 3 to 15, more preferably 3 to 9. The monovalent heterocyclic group also includes a monovalent aromatic heterocyclic group (heteroaryl group). The alkylidene group used as a substituent refers to a group in which two hydrogen atoms have been removed from the same carbon atom of an alkane.The number of carbon atoms in the alkylidene group is preferably 1 to 12, more preferably 1 to 6, and particularly preferably 1 to 3. The acyl group used as a substituent is a group represented by the formula -C(=O)-R (wherein R is an alkyl group or an aryl group). The alkyl group represented by R may be either linear or branched. The number of carbon atoms in the acyl group is preferably 2 to 13, and more preferably 2 to 7. The acyloxy group used as a substituent is a group represented by the formula -OC(=O)-R (wherein R is as defined above). The number of carbon atoms in the acyloxy group is preferably 2 to 13, and more preferably 2 to 7. The above-mentioned substituent may further have a substituent (sometimes referred to as a "secondary substituent"). Unless otherwise specified, the same as the above-mentioned substituent may be used as the secondary substituent.
[0014] Hereinafter, the present invention will be described in detail with reference to embodiments and examples. However, the present invention is not limited to the following embodiments and examples, and may be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.
[0015] [Resin composition] The resin composition of the present invention contains (A) polyphenylene ether particles, (B) an epoxy resin, (C) a curing agent, and (D) an inorganic filler.
[0016] As described above, in the manufacture of circuit boards, when an insulating layer was formed using a conventional resin composition that contributes to good dielectric properties (for example, a resin composition having a specific composition, such as a specific curing agent, such as an active ester-based curing agent, capable of reducing or suppressing the generation of polar groups, such as secondary hydroxyl groups, in the curing reaction of an epoxy resin, or a resin composition having a high content of inorganic filler), the obtained insulating layer tended to easily generate cracks after desmearing.
[0017] In the course of investigating ways to improve crack resistance, the inventors found that adding organic particles can improve crack resistance to some extent. However, they also found that adding organic particles in an amount sufficient to improve crack resistance can cause problems such as deterioration of dielectric properties, thereby diminishing the originally desired effect, and deterioration of adhesion to the conductor layer when exposed to a high-temperature, high-humidity environment.
[0018] In contrast, according to the present invention, which uses polyphenylene ether particles as an organic filler in a resin composition containing an epoxy resin, a curing agent, and an inorganic filler, even when a specific composition that contributes to good dielectric properties is adopted, a cured product can be obtained that exhibits good crack resistance and good adhesion to a conductor layer when exposed to a high-temperature and high-humidity environment. Furthermore, it has been confirmed that an insulating layer that exhibits good surface flatness with few undulations can be realized regardless of the surface pattern of the underlying substrate (surface unevenness pattern due to recesses such as degassing holes and protrusions such as surface circuits).
[0019] Each component will be described below.
[0020] <(A) Polyphenylene ether particles> The resin composition of the present invention contains polyphenylene ether particles as component (A), which makes it possible to obtain a cured product that exhibits good crack resistance and good adhesion to a conductor layer when exposed to a high-temperature and high-humidity environment, even when a specific composition that contributes to good dielectric properties is adopted in a resin composition containing an epoxy resin, a curing agent, and an inorganic filler.
[0021] In this specification, the term "polyphenylene ether particles" refers to a granular material made of a material containing at least a compound having a polyphenylene ether structure (hereinafter also simply referred to as "polyphenylene ether compound"). The polyphenylene ether particles may be solid particles made of a material containing at least a polyphenylene ether compound, hollow particles having a shell part made of a material containing at least a polyphenylene ether compound and a hollow part surrounded by the shell part, or a mixture thereof.
[0022] Even when a specific composition that contributes to good dielectric properties is adopted, from the viewpoint of providing a cured product that exhibits good crack resistance and good adhesion to the conductor layer when exposed to a high-temperature and high-humidity environment, the content of the polyphenylene ether compound in the material constituting the (A) component is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and even more preferably 90% by mass or more. The upper limit of the content is not particularly limited and may be 100% by mass. The polyphenylene ether compound may be used alone or in combination of two or more kinds.
[0023] From the viewpoint of obtaining the effects of the present invention more effectively, the polyphenylene ether compound preferably contains a polyphenylene ether structure containing a plurality of constitutional units represented by the following formula (1).
[0024] [ka] (In the formula, R each independently represents a halogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryl group, an optionally substituted amino group, a nitro group, or a carboxy group; m represents an integer of 0 to 4.
[0025] The alkyl group or alkoxy group in R may be either linear or branched, and has preferably 1 to 10 carbon atoms, more preferably 1 to 6, and further preferably 1 to 4 or 1 to 3. The number of carbon atoms does not include the number of carbon atoms of the substituent.
[0026] The number of carbon atoms in the aryl group for R is preferably 6 to 14, and more preferably 6 to 10. The number of carbon atoms does not include the number of carbon atoms of the substituent.
[0027] The substituent that the monovalent group represented by R may have is as described above, and among them, a halogen atom, an alkyl group, an alkoxy group, or an aryl group is preferable. Suitable examples of these substituents, including the number of carbon atoms, are as described above.
[0028] In formula (1), m represents an integer of 0 to 4, preferably an integer of 0 to 3, and more preferably an integer of 1 to 3.
[0029] Even in the case of adopting a specific composition that contributes to good dielectric properties, from the viewpoint of providing a cured product that exhibits good crack resistance and good adhesion to a conductor layer when exposed to a high-temperature and high-humidity environment, the polyphenylene ether structure is preferably a polyphenylene ether structure containing one or more units selected from the group consisting of 2,6-disubstituted-1,4-phenylene ether units, 2,5-disubstituted-1,4-phenylene ether units, and 2,3,6-trisubstituted-1,4-phenylene ether units, and particularly preferably a polyphenylene ether structure containing a plurality of 2,6-disubstituted-1,4-phenylene ether units (wherein the substituents at the 2,6 positions, the substituents at the 2,5 positions, and the substituents at the 2,3,6 positions correspond to R in formula (1)).
[0030] Specific examples of suitable polyphenylene ether structures include poly(2,6-disubstituted-1,4-phenylene ether) structures such as a poly(2,6-dialkyl-1,4-phenylene ether) structure, a poly(2-alkyl-6-aryl-1,4-phenylene ether) structure, a poly(2,6-diaryl-1,4-phenylene ether) structure, and a poly(2,6-dihalo-1,4-phenylene ether) structure; and polyphenylene ether structures containing a plurality of 2,6-disubstituted-1,4-phenylene ether units, such as a copolymer structure of 2,6-disubstituted phenol and another phenol compound (for example, 2,5-disubstituted phenol such as 2,5-dialkylphenol, 2-alkyl-5-arylphenol, and 2,5-diarylphenol, and 2,3,6-trisubstituted phenol such as 2,3,6-trialkylphenol and 2,3,6-trihalophenol), and a coupling reaction product of 2,6-disubstituted phenol and a biphenol compound or a bisphenol compound.
[0031] The compound having the polyphenylene ether structure, i.e., the polyphenylene ether compound, may have another structure as long as it has a polyphenylene ether structure. Such another structure is not particularly limited as long as it does not impair the effects of the present invention, and may be any structure that can react with an end group of the polyphenylene ether structure to form a molecule of the polyphenylene ether compound together with the polyphenylene ether structure, such as a structure derived from a crosslinkable monomer or a monofunctional monomer that can react with an end group of the polyphenylene ether structure.
[0032] Examples of the crosslinkable monomer include polyfunctional (meth)acrylic acid esters such as ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, and glycerin tri(meth)acrylate; polyfunctional acrylamide derivatives such as N,N'-methylenebis(meth)acrylamide and N,N'-ethylenebis(meth)acrylamide; polyfunctional allyl derivatives such as diallylamine and tetraallyloxyethane; and aromatic crosslinkable monomers such as divinylbenzene, divinylnaphthalene, and diallylphthalate.
[0033] Examples of the monofunctional monomer include alkyl (meth)acrylic acid esters having 1 to 16 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and cetyl (meth)acrylate; aromatic monofunctional monomers, such as styrene, α-methylstyrene, ethylvinylbenzene, vinyltoluene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, vinylbiphenyl, and vinylnaphthalene; dicarboxylic acid ester monomers, such as dimethyl maleate, diethyl fumarate, dimethyl fumarate, and diethyl fumarate; maleic anhydride; N-vinylcarbazole; and (meth)acrylonitrile.
[0034] When the polyphenylene ether compound has a structure derived from the above-mentioned crosslinkable monomer or monofunctional monomer, the polyphenylene ether compound may be prepared by reacting a raw material compound having a polyphenylene ether structure with one or more other raw material compounds selected from the group consisting of the above-mentioned crosslinkable monomers and monofunctional monomers. In this case, when the total amount of the raw material compound having a polyphenylene ether structure and the other raw material compounds is 100 parts by mass, it is preferable to use the raw material compound having a polyphenylene ether structure in an amount of preferably 20 parts by mass or more, more preferably 40 parts by mass or more, 50 parts by mass or more, 55 parts by mass or more, or 60 parts by mass or more.
[0035] The raw material compound having a polyphenylene ether structure is not particularly limited as long as it has a polyphenylene ether structure, but from the viewpoint of obtaining the effects of the present invention, preferred examples include homopolymers or copolymers of phenolic compounds selected from the group consisting of 2,6-disubstituted phenol, 2,5-disubstituted phenol, and 2,3,6-trisubstituted phenol; and coupling reaction products of phenolic compounds selected from the group consisting of 2,6-disubstituted phenol, 2,5-disubstituted phenol, and 2,3,6-trisubstituted phenol with biphenolic compounds or bisphenolic compounds. The number average molecular weight (Mn) of the raw material compound having a polyphenylene ether structure is preferably in the range of 500 to 4000. Here, the Mn of the raw material compound is the polystyrene-equivalent Mn measured by gel permeation chromatography (GPC). As the raw material compound having such a polyphenylene ether structure, commercially available products may be used, such as "OPE-2St" manufactured by Mitsubishi Gas Chemical Company, Inc. and "NORYL" manufactured by SABIC Corporation (both of which contain multiple 2,6-dialkyl-1,4-phenylene ether units).
[0036] The material constituting the component (A) may contain, in addition to the polyphenylene ether compound, other components as long as the effects of the present invention are not impaired.
[0037] Examples of such other components include a non-crosslinkable polymer, a dispersion stabilizer, a surfactant, and a polymerization initiator. The other components may be used alone or in combination of two or more.
[0038] Examples of the non-crosslinkable polymer include one or more selected from the group consisting of polyolefins, styrene-based polymers, (meth)acrylic acid-based polymers, and styrene-(meth)acrylic acid-based polymers. Examples of the polyolefins include polyethylene, polypropylene, and polyα-olefins. Examples of the styrene-based polymers include polystyrene, styrene-acrylonitrile copolymers, and acrylonitrile-butadiene-styrene copolymers. Examples of the (meth)acrylic acid-based polymers include polymethyl (meth)acrylate, polyethyl (meth)acrylate, polybutyl (meth)acrylate, and polypropyl (meth)acrylate. Examples of the styrene-(meth)acrylic acid-based polymers include styrene-methyl (meth)acrylate copolymers, styrene-ethyl (meth)acrylate copolymers, styrene-butyl (meth)acrylate copolymers, and styrene-propyl (meth)acrylate copolymers.
[0039] Examples of the dispersion stabilizer include polyvinyl alcohol, polycarboxylic acid, celluloses (hydroxyethyl cellulose, carboxymethyl cellulose, etc.), polyvinylpyrrolidone, etc. Examples of the dispersion stabilizer also include inorganic water-soluble polymer compounds such as sodium tripolyphosphate, phosphates such as calcium phosphate, magnesium phosphate, aluminum phosphate, zinc phosphate, etc., pyrophosphates such as calcium pyrophosphate, magnesium pyrophosphate, aluminum pyrophosphate, zinc pyrophosphate, etc., and poorly water-soluble inorganic compounds such as calcium carbonate, magnesium carbonate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, and colloidal silica.
[0040] As the surfactant, various surfactants such as anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants may be used.
[0041] Examples of the polymerization initiator include organic peroxides such as lauroyl peroxide, benzoyl peroxide, orthochlorobenzoyl peroxide, orthomethoxybenzoyl peroxide, 3,5,5-trimethylhexanoyl peroxide, t-butylperoxy-2-ethylhexanoate, and di-t-butyl peroxide; and azo compounds such as 2,2'-azobisisobutyronitrile, 1,1'-azobiscyclohexanecarbonitrile, and 2,2'-azobis(2,4-dimethylvaleronitrile).
[0042] In the material constituting the component (A), the content of such other components, i.e., components other than the polyphenylene ether compound, is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, and even more preferably 10% by mass or less. The lower limit of the content is not particularly limited and may be 0% by mass, but may also be 0.1% by mass or more, 0.3% by mass or more, 0.5% by mass or more, etc.
[0043] Even in cases where a specific composition that contributes to good dielectric properties is adopted, from the viewpoint of providing a cured product that exhibits better crack resistance and better adhesion to a conductor layer when exposed to a high-temperature and high-humidity environment, the average particle size of component (A) is preferably 5 μm or less, more preferably 4 μm or less, even more preferably 3 μm or less, still more preferably 2 μm or less, 1.5 μm or less, or 1 μm or less, and the lower limit is preferably 0.1 μm or more, 0.2 μm or more, or 0.3 μm or more.
[0044] In this specification, the average particle size of component (A) is the median diameter based on volume (50% particle size D 50 The average particle size of component (A) can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, a particle size distribution of component (A) is created on a volume basis using a laser diffraction / scattering particle size distribution analyzer, and the particle size at which the cumulative distribution value is 50% (median diameter, 50% particle size D 50) can be measured as the average particle size. A measurement sample can be prepared by weighing 100 mg of component (A) and 10 g of methyl ethyl ketone into a vial and dispersing the mixture ultrasonically for 10 minutes. An example of a laser diffraction particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.
[0045] Among these, from the viewpoint of providing a cured product that exhibits particularly good crack resistance and exhibits particularly good adhesion to a conductor layer when exposed to a high-temperature and high-humidity environment, it is preferable to use a 90% particle size D 90 is preferably 2 μm or less, more preferably 1.5 μm or less, further preferably 1.4 μm or less, 1.2 μm or less, or 1 μm or less, and the lower limit is preferably 0.1 μm or more, 0.2 μm or more, or 0.3 μm or more. 90 As mentioned above about the average particle size, when the particle size distribution of component (A) is plotted on a volume basis, the particle size at which the cumulative distribution value is 90% is the particle size. 90 can be measured in the same manner as the average particle size.
[0046] The manufacturing method of component (A) is not particularly limited, and may be a conventionally known method for manufacturing resin particles. As mentioned above, component (A) may be either solid particles or hollow particles. When component (A) is solid particles, it may be manufactured by any method, such as (1) preparing a material containing at least a polyphenylene ether compound, melting and kneading it as necessary, and then pulverizing and crushing it to a predetermined shape and size to obtain a granular material, or (2) solution-polymerizing a raw material compound having a polyphenylene ether structure with the above-mentioned crosslinkable monomer or monofunctional monomer, and then mixing with a poor solvent to precipitate particles. When component (A) is hollow particles, it may be manufactured by any method, such as reacting a raw material compound having a polyphenylene ether structure with the above-mentioned crosslinkable monomer or monofunctional monomer in an aqueous medium in the presence of a non-reactive oily solvent to obtain particles containing the non-reactive oily solvent in the inner pores, and then removing the non-reactive oily solvent to obtain hollow particles. The polyphenylene ether compound used in producing the solid particle (A) component may be a commercially available product, such as "Lupiace" manufactured by Mitsubishi Engineering Plastics Corporation and "Zylon" manufactured by Asahi Kasei Corp. As described above, in addition to these polyphenylene ether compounds, other components such as non-crosslinked polymers may be used in producing the (A) component.
[0047] An example of a method for producing the component (A) as hollow particles will be described below.
[0048] First, a raw material compound having a polyphenylene ether structure is reacted with the above-mentioned crosslinkable monomer or monofunctional monomer in an aqueous medium in the presence of a non-reactive oily solvent. The reaction is carried out by emulsion polymerization or suspension polymerization in which the non-reactive oily solvent containing the above-mentioned raw material compound and the like is used as an oil phase and the aqueous medium is used as an aqueous phase. Therefore, in one embodiment, the (A) component used in the present invention is an emulsion polymer or suspension polymer.
[0049] In such a reaction, preferably, a raw material compound having a polyphenylene ether structure, a crosslinkable monomer, a monofunctional monomer, and an oil phase containing a non-reactive oily solvent are added to and dispersed in an aqueous phase containing an aqueous medium, and then the mixture is heated to carry out a polymerization reaction.
[0050] Examples of the aqueous medium include water and a mixed medium of water and a lower alcohol (methanol, ethanol, etc.). The amount of the aqueous medium used is not particularly limited as long as the emulsion polymerization or suspension polymerization reaction proceeds appropriately, but is preferably in the range of 100 parts by mass to 5000 parts by mass, more preferably 150 parts by mass to 2000 parts by mass, relative to 100 parts by mass of the oil phase.
[0051] The non-reactive oily solvent is an oily solvent that does not exhibit chemical reactivity with any of the raw material compound having a polyphenylene ether structure, the crosslinkable monomer, and the monofunctional monomer, and acts as a hollowing agent that gives the particles a hollow portion. The non-reactive oily solvent is not particularly limited, but examples thereof include heptane, hexane, toluene, cyclohexane, methyl acetate, ethyl acetate, methyl ethyl ketone, chloroform, and carbon tetrachloride. Since it is easy to remove from the hollow particles, an oily solvent having a boiling point of less than 100°C is preferred. The amount of the non-reactive oily solvent used is preferably in the range of 20 parts by mass to 250 parts by mass with respect to 100 parts by mass of the total amount of the raw material compound having a polyphenylene ether structure, the crosslinkable monomer, and the monofunctional monomer, from the viewpoint of easy production of hollow particles.
[0052] The dispersion may be carried out by any dispersion method as long as the oil phase can be present in the form of droplets in the aqueous phase. For example, a dispersion method using a homomixer or a homogenizer may be employed.
[0053] During the dispersion, other components such as the non-crosslinked polymer and dispersion stabilizer described above may be added. For example, by using a non-crosslinked polymer, the phase separation between the polyphenylene ether compound and the non-reactive oily solvent produced in the polymerization reaction is promoted, and the formation of the shell portion can be promoted, which tends to facilitate the production of the (A) component as hollow particles. The amount of these other components used is as described above, but may be appropriately determined according to the purpose.
[0054] The polymerization temperature is not particularly limited as long as it allows the polymerization of the raw material compounds to proceed, but is preferably in the range of 30° C. to 80° C. The polymerization time is not particularly limited as long as it allows the polymerization of the raw material compounds to proceed and a desired polyphenylene ether compound can be obtained, but is preferably in the range of 1 hour to 48 hours.
[0055] After the polymerization reaction, it is preferable to carry out post-heating. The post-heating temperature is not particularly limited as long as the desired hollow particles are obtained, but is preferably in the range of 70° C. to 120° C., and the post-heating time is preferably in the range of 1 hour to 24 hours.
[0056] As the component (A), a commercially available product may be used. For example, a product having the above-mentioned preferable composition and dimensions is "XX-6655Z" (hollow polyphenylene ether particles, average particle size 0.4 μm, 90% particle size D 90 less than 1 μm), "XX-6714Z" (solid polyphenylene ether particles, average particle size 0.7 μm, 90% particle size D 90 are less than 1 μm).
[0057] Even when a specific composition contributing to good dielectric properties is adopted, from the viewpoint of providing a cured product that exhibits good crack resistance and good adhesion to a conductor layer when exposed to a high-temperature and high-humidity environment, the content of the (A) component in the resin composition is preferably 0.5% by mass or more, more preferably 1% by mass or more, 1.5% by mass or more, 2% by mass or more, or 2.5% by mass or more, and even more preferably 3% by mass or more, 3.5% by mass or more, 4% by mass or more, or 4.5% by mass or more, based on the resin component in the resin composition being 100% by mass. The upper limit of the content is preferably 35% by mass or less, more preferably 30% by mass or less, 25% by mass or less, or 20% by mass or less, from the viewpoint of easily realizing an insulating layer that exhibits good crack resistance and good adhesion to a conductor layer after exposure to a high-temperature and high-humidity environment, and has little undulations and good surface flatness regardless of the surface pattern of the substrate as the base.
[0058] In the present invention, the "resin component" of the resin composition refers to the non-volatile components constituting the resin composition excluding the inorganic filler (D) described below.
[0059] In particular, from the viewpoint of providing a cured product having exceptionally excellent crack resistance and adhesion to a conductor layer after exposure to a high-temperature, high-humidity environment, when the total of the (B) epoxy resin and (C-1) one or more curing agents selected from the group consisting of an active ester curing agent, a cyanate ester curing agent, and a carbodiimide curing agent is taken as 100 parts by mass, the content of the (A) component is preferably 2.2 parts by mass or more, more preferably 2.5 parts by mass or more, even more preferably 3 parts by mass or more, 3.5 parts by mass or more, or 4 parts by mass or more. The upper limit of the content is preferably 38 parts by mass or less, more preferably 35 parts by mass or less, 30 parts by mass or less, or 25 parts by mass or less, from the viewpoint of easily realizing an insulating layer that exhibits excellent crack resistance and excellent adhesion to a conductor layer after exposure to a high-temperature, high-humidity environment, while exhibiting less undulations and exceptionally good surface flatness regardless of the surface pattern of the substrate as the base.
[0060] <(B) Epoxy resin> The resin composition of the present invention contains an epoxy resin as component (B).
[0061] Examples of epoxy resins include bisphenol type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, glycidylamine type epoxy resins, glycidyl ester type epoxy resins, cresol novolac type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, naphthylene ether type epoxy resins, trimethylol type epoxy resins, and tetraphenylethane type epoxy resins. Bisphenol type epoxy resins refer to epoxy resins having a bisphenol structure, and examples thereof include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, and bisphenol AF type epoxy resins. Biphenyl type epoxy resin refers to an epoxy resin having a biphenyl structure, where the biphenyl structure may have a substituent such as an alkyl group, an alkoxy group, or an aryl group. Therefore, bixylenol type epoxy resin and biphenyl aralkyl type epoxy resin are also included in biphenyl type epoxy resin. The epoxy resin may be used alone or in combination of two or more kinds.
[0062] The epoxy resin is preferably an aromatic epoxy resin, where the aromatic epoxy resin means an epoxy resin having an aromatic ring in the molecule.
[0063] The epoxy resin preferably has two or more epoxy groups in one molecule. When the non-volatile component of the epoxy resin is taken as 100 mass%, the ratio of the epoxy resin having two or more epoxy groups in one molecule is preferably 50 mass% or more, more preferably 60 mass% or more, and further preferably 70 mass% or more.
[0064] There are two types of epoxy resins: epoxy resins that are liquid at a temperature of 20° C. (hereinafter referred to as "liquid epoxy resins"), and epoxy resins that are solid at a temperature of 20° C. (hereinafter referred to as "solid epoxy resins").
[0065] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.
[0066] Preferred liquid epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, naphthalene type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins such as alicyclic epoxy resins having an ester skeleton, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, and epoxy resins having a butadiene structure.
[0067] Specific examples of liquid epoxy resins include "HP-4032", "HP-4032D", and "HP-4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "jER828EL", "825", and "Epicoat 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; and "630" and "630LSD" (glycidyl amine type epoxy resins) manufactured by Mitsubishi Chemical Corporation. resin); "ZX1059" manufactured by Nippon Steel Chemical & Material Co., Ltd. (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin); "EX-721" manufactured by Nagase ChemteX Corporation (glycidyl ester type epoxy resin); "Celloxide 2021P" manufactured by Daicel Corporation (alicyclic epoxy resin with an ester skeleton); "PB-3600" manufactured by Daicel Corporation (epoxy resin with a butadiene structure); "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.
[0068] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.
[0069] As the solid epoxy resin, bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, and tetraphenylethane type epoxy resin are preferred.
[0070] Specific examples of solid epoxy resins include DIC Corporation's "HP-4032H" (naphthalene type epoxy resin); DIC Corporation's "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resin); DIC Corporation's "N-690" (cresol novolac type epoxy resin); DIC Corporation's "N-695" (cresol novolac type epoxy resin); DIC Corporation's "HP-7200HH", "HP-7200H", and "HP-7200" (dicyclopentadiene epoxy resin). diene type epoxy resins); "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", and "HP6000" (naphthylene ether type epoxy resins) manufactured by DIC; "EPPN-502H" (trisphenol type epoxy resins) manufactured by Nippon Kayaku; "NC7000L" (naphthol novolac type epoxy resins) manufactured by Nippon Kayaku; "NC3000H", "NC3000", and "NC3000L" manufactured by Nippon Kayaku ","NC3100" (biphenyl type epoxy resin); "ESN475V" (naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX4000HK" (bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; " Examples of epoxy resins include "YX8800" (anthracene type epoxy resin); "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals; "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical; "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical; "jER1010" (solid bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical; and "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical.
[0071] The resin composition of the present invention may contain only a liquid epoxy resin as an epoxy resin, may contain only a solid epoxy resin, or may contain a combination of a liquid epoxy resin and a solid epoxy resin. When a liquid epoxy resin and a solid epoxy resin are used in combination, the ratio of the amounts (liquid epoxy resin:solid epoxy resin) is preferably 1:0.01 to 1:50, more preferably 1:0.05 to 1:20, and even more preferably 1:0.1 to 1:10, by mass.
[0072] The epoxy equivalent of the epoxy resin is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., even more preferably 80 g / eq. to 2000 g / eq., and even more preferably 110 g / eq. to 1000 g / eq. The epoxy equivalent is the mass of an epoxy resin containing one equivalent of an epoxy group. This epoxy equivalent can be measured according to JIS K7236.
[0073] The weight average molecular weight (Mw) of the epoxy resin is preferably from 100 to 5000, more preferably from 250 to 3000, and further preferably from 400 to 1500. The Mw of the epoxy resin can be measured by the GPC method as a polystyrene-equivalent value.
[0074] In combination with the above-mentioned (A) component and the later-described (C) and (D) components, from the viewpoint of providing a cured product that exhibits good crack resistance and good adhesion to a conductor layer when exposed to a high-temperature and high-humidity environment, the content of the (B) component in the resin composition is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 12% by mass or more, 14% by mass or more, or 15% by mass or more, when the resin components in the resin composition are taken as 100% by mass. The upper limit of the content is not particularly limited and may be determined depending on the properties required of the resin composition, but may be, for example, 60% by mass or less, 55% by mass or less, or 50% by mass or less.
[0075] <(C) Hardener> The resin composition of the present invention contains a curing agent as component (C).
[0076] Examples of the component (C) include active ester-based curing agents, cyanate ester-based curing agents, carbodiimide-based curing agents, phenol-based curing agents, naphthol-based curing agents, acid anhydride-based curing agents, amine-based curing agents, etc. The component (C) may be used alone or in combination of two or more.
[0077] By using a specific curing agent that can reduce or suppress the generation of polar groups such as secondary hydroxyl groups in the curing reaction of epoxy resins, a resin composition that provides good dielectric properties can be achieved. Examples of curing agents that contribute to such good dielectric properties include active ester curing agents, cyanate ester curing agents, and carbodiimide curing agents.
[0078] As mentioned above, when an insulating layer was formed by using a specific composition that contributes to good dielectric properties in the manufacture of a circuit board, the resulting insulating layer tended to crack easily after desmearing. It was confirmed that crack resistance could be improved somewhat by adding organic particles, but it was found that adding organic particles in an amount that could improve crack resistance would cause problems such as a deterioration in dielectric properties, reducing the originally desired effect, or a deterioration in adhesion to a conductor layer when exposed to a high-temperature, high-humidity environment. It was also confirmed that the deterioration in adhesion to a conductor layer after exposure to a high-temperature, high-humidity environment was significant when a specific curing agent such as an active ester curing agent was compounded in high amounts in order to achieve even better dielectric properties.
[0079] In contrast, according to the present invention, which uses the above-mentioned component (A), even when a specific composition that contributes to good dielectric properties is adopted, it is possible to obtain a cured product that exhibits good crack resistance and also exhibits good adhesion to a conductor layer when exposed to a high-temperature, high-humidity environment.
[0080] Therefore, in one embodiment, the (C) component contains one or more curing agents selected from the group consisting of (C-1) active ester curing agents, cyanate ester curing agents, and carbodiimide curing agents. The resin composition of the present invention is advantageous because it can provide a cured product that exhibits good crack resistance and good adhesion to a conductor layer when exposed to a high-temperature and high-humidity environment while enjoying the excellent effects inherent to the (C-1) component (contributing to good dielectric properties).
[0081] -Active ester hardener- As the active ester curing agent, a compound having one or more active ester groups in one molecule can be used. Among them, as the active ester curing agent, a compound having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, is preferable. The active ester curing agent is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester curing agent derived from a carboxylic acid compound is preferable, an active ester curing agent obtained from a carboxylic acid compound and a hydroxy compound is more preferable, and an active ester curing agent obtained from a carboxylic acid compound and an aromatic hydroxy compound is even more preferable.
[0082] The carboxylic acid compound may be either an aromatic carboxylic acid compound or an aliphatic carboxylic acid, and examples thereof include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid.
[0083] Examples of aromatic hydroxy compounds include (i) polyaddition products of unsaturated aliphatic cyclic compounds containing two double bonds in one molecule and phenols, (ii) various bisphenol compounds, (iii) aromatic polyols having two or more hydroxyl groups bonded to the carbon atoms on the aromatic ring, and (iv) aromatic monools having one hydroxyl group bonded to the carbon atoms on the aromatic ring. Examples of polyaddition products of unsaturated aliphatic cyclic compounds and phenols include polyaddition products of unsaturated aliphatic cyclic compounds such as dicyclopentadiene, tetrahydroindene, norbornadiene, limonene, and vinylcyclohexene with phenols that may have a substituent (e.g., phenol, cresol, xylenol, ethylphenol, propylphenol, vinylphenol, allylphenol, phenylphenol, benzylphenol, halophenol, etc.), and specifically, for example, dicyclopentadiene-phenols polyaddition products. Examples of bisphenol compounds include bisphenol A, bisphenol F, bisphenol AF, bisphenol AP, bisphenol B, bisphenol BP, bisphenol C, and bisphenol M. Examples of aromatic polyols having two or more hydroxy groups bonded to carbon atoms on an aromatic ring include hydroquinone, resorcinol, catechol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucinol, benzenetriol, and phenol novolak. Examples of aromatic monools having one hydroxy group bonded to a carbon atom on an aromatic ring include phenol, cresol, xylenol, ethylphenol, propylphenol, vinylphenol, allylphenol, phenylphenol, benzylphenol, halophenol, naphthol, methylnaphthol, dimethylnaphthol, ethylnaphthol, propylnaphthol, vinylnaphthol, allylnaphthol, phenylnaphthol, benzylnaphthol, and halonaphthol.
[0084] Suitable specific examples of the active ester curing agent include an active ester compound containing a dicyclopentadiene-type diphenol structure, an active ester compound containing a naphthalene structure, an active ester compound containing an acetylated product of phenol novolac, and an active ester compound containing a benzoylated product of phenol novolac. Among them, an active ester compound containing a naphthalene structure and an active ester compound containing a dicyclopentadiene-type diphenol structure are more preferred from the viewpoint of providing good dielectric properties in combination with the (A) component, the (B) component, and the (D) component described later. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentalene-phenylene.
[0085] Commercially available active ester curing agents include active ester resins containing a dicyclopentadiene-type diphenol structure such as "EXB-9451", "EXB-9460", "EXB-9460S", "HPC-8000-65T", "HPC-8000H-65TM", and "HPC-8000L-65TM" (manufactured by DIC Corporation); active ester resins containing a naphthalene structure such as "EXB-8100L-65T", "EXB-8150-60T", "EXB-8150-62T", "EXB-9416-70BK", "HPC-8150-60T", and "HPC-8150-62T"; Examples of such active ester resins include "HP-B-8151-62T" and "HP-C-8151-62T" (manufactured by DIC Corporation); "EXB9401" (manufactured by DIC Corporation) as a phosphorus-containing active ester resin; "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester resin which is an acetylated product of phenol novolac; "YLH1026", "YLH1030", and "YLH1048" (manufactured by Mitsubishi Chemical Corporation) as active ester resins which are benzoylated products of phenol novolac; and "PC1300-02-65MA" (manufactured by Air Water Corporation) as an active ester resin containing a styryl group and a naphthalene structure.
[0086] -Cyanate ester hardener- Examples of cyanate ester curing agents include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine.
[0087] Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (phenol novolac type multifunctional cyanate ester resins), "ULL-950S" (multifunctional cyanate ester resin), "BA230", and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.
[0088] -Carbodiimide hardener- The carbodiimide curing agent is a compound having one or more, preferably two or more, carbodiimide groups (-N=C=N-) in one molecule. Specific examples of the carbodiimide curing agent include Carbodilite (registered trademark) V-03 (carbodiimide group equivalent: 216 g / eq.), V-05 (carbodiimide group equivalent: 262 g / eq.), V-07 (carbodiimide group equivalent: 200 g / eq.), V-09 (carbodiimide group equivalent: 200 g / eq.), and Stavaxol (registered trademark) P (carbodiimide group equivalent: 302 g / eq.) manufactured by Rhein Chemie.
[0089] In the resin composition of the present invention, the component (C) may contain a curing agent other than the component (C-1). For example, the component (C) may contain one or more curing agents selected from the group consisting of (C-2) phenol-based curing agents, naphthol-based curing agents, acid anhydride-based curing agents, and amine-based curing agents.
[0090] -Phenol-based hardeners and naphthol-based hardeners- As the phenol-based curing agent and naphthol-based curing agent, those having a novolac structure are preferred from the viewpoint of heat resistance and water resistance. Also, from the viewpoint of adhesion to the conductor layer, nitrogen-containing phenol-based curing agents and nitrogen-containing naphthol-based curing agents are preferred, and triazine skeleton-containing phenol-based curing agents and triazine skeleton-containing naphthol-based curing agents are more preferred. From the viewpoint of realizing an insulating layer having good heat resistance, water resistance, and adhesion to the conductor layer, phenol-based curing agents and naphthol-based curing agents having both a triazine skeleton and a novolac structure are particularly suitable.
[0091] Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", "MEH-7851", and "MEH-8000H" manufactured by Meiwa Chemical Industry Co., Ltd.; "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd.; and "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-495V", and "SN-37" manufactured by Nippon Steel Chemical & Material Co., Ltd. 5" and "SN-395" manufactured by DIC Corporation; "TD-2090", "TD-2090-60M", "LA-7052", "LA-7054", "LA-1356", "LA-3018", "LA-3018-50P", "EXB-9500", "HPC-9500", "KA-1160", "KA-1163", and "KA-1165" manufactured by Gun-ei Chemical Co., Ltd.; and the like.
[0092] -Acid anhydride curing agent- Examples of the acid anhydride curing agent include a curing agent having one or more acid anhydride groups in one molecule. Specific examples of the acid anhydride curing agent include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, and benzophenonetetracarboxylic dianhydride. Examples of acid anhydrides include polymeric acid anhydrides such as anhydrides, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and styrene-maleic acid resins, which are copolymers of styrene and maleic acid. Commercially available acid anhydride hardeners include "MH-700" manufactured by New Japan Chemical Co., Ltd.
[0093] -Amine-based hardener- Examples of the amine-based curing agent include curing agents having one or more amino groups in one molecule, such as aliphatic amines, polyether amines, alicyclic amines, aromatic amines, etc. Specific examples of the amine-based curing agent include 4,4'-methylenebis(2,6-dimethylaniline), diphenyldiaminosulfone, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenylether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, 2,2-bis(3-amino-4-hydroxyphenyl)- ... bis(4-aminophenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, etc. The amine-based curing agent may be a commercially available product, for example, "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd., and "Epicure W" manufactured by Mitsubishi Chemical Corporation.
[0094] From the viewpoint of easily realizing a resin composition that provides good dielectric properties in combination with the (A) component, the (B) component, and the (D) component described later, the content of the (C) component in the resin composition is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, 35% by mass or more, or 40% by mass or more, when the resin components in the resin composition are taken as 100% by mass. The upper limit of the content is not particularly limited and may be determined depending on the properties required for the resin composition, but may be, for example, 80% by mass or less, 75% by mass or less, 70% by mass or less, or 65% by mass or less.
[0095] In order to realize a resin composition that provides good dielectric properties in combination with the (A) component, the (B) component, and the (D) component described later, the content of the (C-1) component in the (C) component is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 85% by mass or more, 90% by mass or more, or 95% by mass or more, when the non-volatile components of the (C) component are taken as 100% by mass. The upper limit of the content is not particularly limited and may be 100% by mass, but may also be, for example, 99.5% by mass or less, 99% by mass or less, etc.
[0096] In the resin composition of the present invention, the mass ratio of the (C-1) component to the (B) component ((C-1) component / (B) component) is preferably 1 or more, more preferably 1.1 or more, and even more preferably 1.2 or more or 1.4 or more, from the viewpoint of obtaining a cured product having excellent dielectric properties. As described above, according to the resin composition of the present invention using the (A) component, even if the (C-1) component is contained to an extent that excellent dielectric properties can be realized, a cured product that exhibits good crack resistance and exhibits good adhesion to a conductor layer when exposed to a high-temperature and high-humidity environment can be obtained. For example, in the resin composition of the present invention, the mass ratio of the (C-1) component to the (B) component may be increased to 1.5 or more, 1.6 or more, or 1.7 or more. The upper limit of the mass ratio ((B) component / (A) component) may be, for example, 2.5 or less, 2.4 or less, 2.2 or less, 2 or less, etc.
[0097] <(D) Inorganic filler> The resin composition of the present invention contains an inorganic filler as component (D), which can further reduce the linear thermal expansion coefficient and the dielectric loss tangent.
[0098] Examples of materials for component (D) include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum silicate, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. Moreover, spherical silica is preferred as the silica. The component (D) may be used alone or in combination of two or more.
[0099] Examples of commercially available products of component (D) include "UFP-30" manufactured by Denka Chemical Industry Co., Ltd.; "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", and "YA010C" manufactured by Admatechs Co., Ltd.; "UFP-30" manufactured by Denka Company; "Silfil NSS-3N", "Silfil NSS-4N", and "Silfil NSS-5N" manufactured by Tokuyama Corporation; "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.; "DAW-03" and "FB-105FD" manufactured by Denka Company; "Cellfiers" and "MGH-005" manufactured by Taiheiyo Cement Corporation; and "Sferique" and "BA-1" manufactured by JGC Catalysts and Chemicals Co., Ltd.
[0100] The average particle size of component (D) is not particularly limited, but is preferably 10 μm or less, more preferably 5 μm or less, even more preferably 3 μm or less, 2 μm or less, 1 μm or less, or 0.7 μm or less. The lower limit of the average particle size is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.07 μm or more, 0.1 μm or more, or 0.2 μm or more. The average particle size of component (D) is the volume-based median diameter (50% particle size D 50 ) and can be measured in the same manner as the average particle size of component (A).
[0101] The specific surface area of component (D) is not particularly limited, but is preferably 0.1 m 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, 3m 2 / g or more or 5m 2 The upper limit of the specific surface area is not particularly limited, but is preferably 100 m 2 / g or less, more preferably 80m 2 / g or less, more preferably 60m 2 / g or less, 50m 2 / g or less or 40m 2 The specific surface area of component (D) is obtained by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) in accordance with the BET method, and calculating the specific surface area using the BET multipoint method.
[0102] The (D) component is preferably surface-treated with a suitable surface treatment agent. By performing the surface treatment, the moisture resistance and dispersibility of the (D) component can be improved. Examples of the surface treatment agent include silane coupling agents such as vinyl silane coupling agents, epoxy silane coupling agents, styryl silane coupling agents, (meth)acrylic silane coupling agents, amino silane coupling agents, isocyanurate silane coupling agents, ureido silane coupling agents, mercapto silane coupling agents, isocyanate silane coupling agents, and acid anhydride silane coupling agents; non-silane coupling-alkoxysilane compounds such as methyltrimethoxysilane and phenyltrimethoxysilane; and silazane compounds. The surface treatment agent may be used alone or in combination of two or more.
[0103] Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), and Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane).
[0104] The degree of surface treatment with the surface treatment agent is preferably within a predetermined range from the viewpoint of improving the dispersibility of the component (D). Specifically, 100% by mass of the inorganic filler is preferably surface-treated with 0.2 to 5% by mass of the surface treatment agent.
[0105] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2On the other hand, from the viewpoint of preventing an increase in the melt viscosity of the resin composition or the melt viscosity in the form of a sheet, it is more preferable that the melt viscosity is 1.0 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is more preferable. The carbon amount per unit surface area of component (D) can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the carbon amount per unit surface area of the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, an "EMIA-320V" manufactured by Horiba, Ltd., or the like can be used.
[0106] The content of the (D) component in the resin composition is, for example, 40% by mass or more, preferably 50% by mass or more, when the non-volatile components in the resin composition are 100% by mass, from the viewpoint of easily realizing a resin composition that provides better dielectric properties in combination with the (A) to (C) components. As described above, according to the present invention using the (A) component, even when a specific composition that contributes to good dielectric properties is adopted, a cured product that exhibits good crack resistance and good adhesion to a conductor layer when exposed to a high-temperature and high-humidity environment can be obtained. For example, in the resin composition of the present invention, the content of the (D) component may be increased to 60% by mass or more, 65% by mass or more, or 70% by mass or more. The upper limit of the content of the (D) component is not particularly limited, but may be, for example, 90% by mass or less, 85% by mass or less, etc.
[0107] <(E) Radical polymerizable resin> The resin composition of the present invention may contain a radically polymerizable resin as the component (E).
[0108] The type of radical polymerizable resin is not particularly limited as long as it has one or more (preferably two or more) radical polymerizable unsaturated groups in one molecule. For example, the radical polymerizable resin may be a resin having one or more radical polymerizable unsaturated groups selected from maleimide group, vinyl group, allyl group, styryl group, vinylphenyl group, acryloyl group, methacryloyl group, fumaroyl group, and maleoyl group. Among them, from the viewpoint of obtaining a cured product exhibiting better dielectric properties, the radical polymerizable resin is preferably one or more selected from maleimide resin, (meth)acrylic resin, and styryl resin.
[0109] There is no particular limitation on the type of maleimide resin, so long as it has one or more (preferably two or more) maleimide groups (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl groups) in one molecule. Examples of maleimide resins include (1) maleimide resins having an aliphatic skeleton (preferably an aliphatic skeleton having 36 carbon atoms derived from dimer diamine), such as "BMI-3000J", "BMI-5000", "BMI-1400", "BMI-1500", "BMI-1700", and "BMI-689" (all manufactured by Designer Molecules), and "SLK6895-T90" (manufactured by Shin-Etsu Chemical Co., Ltd.); (2) maleimide resins having an indane skeleton, as described in the Japan Institute of Invention and Innovation Disclosure Technical Bulletin No. 2020-500211; and (3) maleimide resins having an aromatic ring skeleton directly bonded to the nitrogen atom of the maleimide group, such as "MIR-3000-70MT" (manufactured by Nippon Kayaku Co., Ltd.), "BMI-4000" (manufactured by Daiwa Kasei Co., Ltd.), and "BMI-80" (manufactured by Keiai Kasei Co., Ltd.).
[0110] The (meth)acrylic resin is not particularly limited in type, and may be a monomer or oligomer, as long as it has one or more (preferably two or more) (meth)acryloyl groups in one molecule. Here, the term "(meth)acryloyl group" is a general term for acryloyl and methacryloyl groups. Examples of methacrylic resins include (meth)acrylate monomers, as well as (meth)acrylic resins such as "A-DOG" (manufactured by Shin-Nakamura Chemical Co., Ltd.), "DCP-A" (manufactured by Kyoeisha Chemical Co., Ltd.), "NPDGA", "FM-400", "R-687", "THE-330", "PET-30", and "DPHA" (all manufactured by Nippon Kayaku Co., Ltd.).
[0111] The styryl resin is not particularly limited in type, and may be a monomer or oligomer, as long as it has one or more (preferably two or more) styryl groups or vinylphenyl groups in one molecule. Examples of the styryl resin include styrene monomers, as well as styryl resins such as "OPE-2St", "OPE-2St 1200", and "OPE-2St 2200" (all manufactured by Mitsubishi Gas Chemical Company, Inc.).
[0112] When the resin composition of the present invention contains the (E) component, the content of the (E) component in the resin composition may be determined according to the properties required for the resin composition, but when the resin components in the resin composition are taken as 100 mass%, it is, for example, 0.1 mass% or more, preferably 0.3 mass% or more, more preferably 0.5 mass% or more, 0.6 mass% or more, 0.8 mass% or more, or 1 mass% or more. The upper limit of the content of the (E) component is not particularly limited, but may be, for example, 15 mass% or less, 10 mass% or less, 8 mass% or less, etc.
[0113] <(F) Curing accelerator> The resin composition of the present invention may contain a curing accelerator as the component (F).
[0114] Examples of the (F) component include phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, metal-based curing accelerators, peroxide-based curing accelerators, etc. The curing accelerators may be used alone or in combination of two or more.
[0115] When the resin composition of the present invention contains the (F) component, the content of the (F) component in the resin composition, relative to 100 mass% of the resin components in the resin composition, is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, even more preferably 0.1 mass% or more, and is preferably 2 mass% or less, more preferably 1.5 mass% or less, or 1 mass% or less.
[0116] <(G)Thermoplastic resin> The resin composition of the present invention may contain a thermoplastic resin as the component (G).
[0117] Examples of the thermoplastic resin include phenoxy resin, polyvinyl acetal resin, polyolefin resin, polybutadiene resin, polyimide resin, polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polycarbonate resin, polyetheretherketone resin, and polyester resin. The thermoplastic resin may be used alone or in combination of two or more.
[0118] The polystyrene-equivalent Mw of the thermoplastic resin is preferably in the range of 8,000 to 70,000, more preferably in the range of 10,000 to 60,000, and even more preferably in the range of 20,000 to 60,000. The polystyrene-equivalent Mw of the thermoplastic resin is measured by a GPC method. Specifically, the polystyrene-equivalent weight average molecular weight of the thermoplastic resin is measured at a column temperature of 40°C using a measuring device LC-9A / RID-6A manufactured by Shimadzu Corporation, a column Shodex K-800P / K-804L / K-804L manufactured by Showa Denko KK, and chloroform or the like as a mobile phase, and can be calculated using a calibration curve of standard polystyrene.
[0119] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. The phenoxy resin may be used alone or in combination of two or more. Specific examples of phenoxy resins include "1256" and "4250" (both of which are phenoxy resins containing a bisphenol A skeleton), "YX8100" (phenoxy resin containing a bisphenol S skeleton), and "YX6954" (phenoxy resin containing a bisphenol acetophenone skeleton) manufactured by Mitsubishi Chemical Corporation. Other examples include "FX280" and "FX293" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "YX7553", "YL6794", "YL7213", "YL7290", and "YL7482" manufactured by Mitsubishi Chemical Corporation.
[0120] Examples of polyvinyl acetal resins include polyvinyl formal resins and polyvinyl butyral resins, and polyvinyl butyral resins are preferred.Specific examples of polyvinyl acetal resins include Denka Butyral 4000-2, Denka Butyral 5000-A, Denka Butyral 6000-C, Denka Butyral 6000-EP, and S-LEC BH series, BX series, KS series, BL series, and BM series, all of which are manufactured by Sekisui Chemical Co., Ltd.
[0121] As the polyimide resin, a resin having an imide structure (preferably a cyclic imide structure) can be used, and for example, an imide compound of an acid anhydride and a diamine compound or a diisocyanate compound may be used.
[0122] The acid anhydride for preparing the polyimide resin is not particularly limited, but is preferably a tetracarboxylic acid anhydride, for example, an aromatic tetracarboxylic acid dianhydride, or an aliphatic tetracarboxylic acid dianhydride, with an aromatic tetracarboxylic acid dianhydride being preferred. Examples of aromatic tetracarboxylic dianhydrides include benzenetetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, anthracenetetracarboxylic dianhydride, diphthalic dianhydride, etc., and preferably diphthalic dianhydride. The diphthalic dianhydride is not particularly limited as long as it is a compound containing two phthalic anhydride structures in the molecule, and each benzene ring in the phthalic anhydride structure may have 1 to 3 optional substituents. The two phthalic anhydride structures in the diphthalic dianhydride may be directly bonded, or may be bonded via a linker structure having 1 to 100 skeletal atoms selected from the group consisting of carbon atoms, oxygen atoms, sulfur atoms, and nitrogen atoms. An example of the "linker structure" in the diphthalic dianhydride is -[R e -Ph] me -R e -[Ph-R e ] ne In this formula, R eeach independently represents a single bond, -(substituted or unsubstituted alkylene group)-, -O-, -S-, -CO-, -SO2-, -CONH-, -NHCO-, -COO-, or -OCO-; me and ne each independently represent an integer of 0 to 2 (preferably 0 or 1). In this specification, "Ph" represents a 1,4-phenylene group, a 1,3-phenylene group, or a 1,2-phenylene group, unless otherwise specified. Specific examples of linker structures include -CH2-, -CH2CH2-, -CH2CH2CH2-, -CH2CH2CH2CH2-, -CH2CH2CH2CH2CH2-, -CH(CH3)-, -C(CH3)2-, -O-, -CO-, -SO2-, -Ph-, -O-Ph-O-, -O-Ph-SO2-Ph-O-, -O-Ph-C(CH3)2-Ph-O-, and the like.Examples of diphthalic dianhydrides include 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 2,2',3,3'-biphenyl tetracarboxylic dianhydride, 2,3,3',4'-biphenyl tetracarboxylic dianhydride, carboxylic dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 2,3,3',4'-diphenylethertetracarboxylic dianhydride, 2,3,3',4'-diphenylsulfonetetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxyphenoxyphenyl)sulfone dianhydride, 4,4'-oxydiphthalic anhydride, methylene-4,4'-diphthalic dianhydride, 1,1-ethynylidene-4 ,4'-Diphthalic dianhydride, 2,2-Propylidene-4,4'-diphthalic dianhydride, 1,2-Ethylene-4,4'-diphthalic dianhydride, 1,3-Trimethylene-4,4'-diphthalic dianhydride, 1,4-Tetramethylene-4,4'-diphthalic dianhydride, 1,5-Pentamethylene-4,4'-diphthalic dianhydride, 1,3-Bis(3,4-dicarboxyphenyl)benzene dianhydride, 1,4-Bis(3,4-dicarboxyphenyl)benzene dianhydride Examples of such anhydrides include 1,3-bis(3,4-dicarboxyphenyl)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, and 4,4'-(4,4'-isopropylidenediphenoxy)bisphthalic dianhydride.
[0123] The diamine compound for preparing the polyimide resin is not particularly limited as long as it is a compound having two amino groups in the molecule, and examples thereof include aliphatic diamine compounds and aromatic diamine compounds. Examples of the aliphatic diamine compound include linear aliphatic diamine compounds such as 1,2-ethylenediamine and 1,10-diaminodecane; branched aliphatic diamine compounds such as 1,2-diamino-2-methylpropane and 2-methyl-1,5-diaminopentane; alicyclic diamine compounds such as 1,3-bis(aminomethyl)cyclohexane and 4,4'-methylenebis(cyclohexylamine); and dimer diamine, among which dimer diamine is preferred. Dimer diamine refers to a diamine compound obtained by replacing the two terminal carboxylic acid groups (-COOH) of a dimer acid with aminomethyl groups (-CH2-NH2) or amino groups (-NH2). Examples of aromatic diamine compounds include phenylenediamine compounds, naphthalenediamine compounds, and dianiline compounds, among which dianiline compounds are preferred. The dianiline compound refers to a compound containing two aniline structures in the molecule. Each of the benzene rings in the aniline structure may have 1 to 3 optional substituents. The two aniline structures in the dianiline compound may be directly bonded to each other, or may be bonded to each other via a linker structure having 1 to 100 skeletal atoms selected from the group consisting of carbon atoms, oxygen atoms, sulfur atoms, and nitrogen atoms. Specific examples of the "linker structure" in the dianiline compound include -NHCO-, -CONH-, -OCO-, -COO-, -CH2-, -CH2CH2-, -CH2CH2CH2-, -CH2CH2CH2CH2-, -CH2CH2CH2CH2CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -CH=CH-, -O-, -S-, -CO-, -SO2-, -NH-, Examples of such groups include -Ph-, -Ph-Ph-, -C(CH3)2-Ph-C(CH3)2-, -O-Ph-O-, -O-Ph-Ph-O-, -O-Ph-SO2-Ph-O-, -O-Ph-C(CH3)2-Ph-O-, -Ph-CO-O-Ph-, -C(CH3)2-Ph-C(CH3)2-, a group represented by the following formula (e-1), a group represented by the following formula (e-2), and a group consisting of a combination thereof. In formulas (e-1) and (e-2), "*" represents a bond.
[0124] [ka]
[0125] Examples of the dianiline compound include 4,4'-diamino-2,2'-ditrifluoromethyl-1,1'-biphenyl, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfide, 4-aminophenyl 4-aminobenzoate, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 2,2-bis(4-aminophenyl)propane, 4,4'-(hexafluoroisopropylidene)dianiline, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, [4-(4-aminophenoxy)phenyl]hexafluoropropane, α,α-bis[4-(4-aminophenoxy)phenyl]-1,3-diisopropylbenzene, α,α-bis[4-(4-aminophenoxy)phenyl]-1,4-diisopropylbenzene, 4,4'-(9-fluorenylidene)dianiline, 2,2-bis(3-methyl-4-aminophenyl)propane, 2,2-bis(3-methyl-4-aminophenyl)benzene, 4,4'-diamino-3,3'-dimethyl-1,1'-biphenyl, 4,4'-diamino-2,2'-dimethyl-1,1'-biphenyl, 9,9'-bis(3-methyl-4-aminophenyl)fluorene, 5-(4-aminophenoxy)-3-[4-(4-aminophenoxy)phenyl]-1,1,3-trimethylindane, and the like. The diamine compound may be used alone or in combination of two or more kinds.
[0126] The diisocyanate compound for preparing the polyimide resin is not particularly limited as long as it is a compound having two isocyanate groups in the molecule, and examples thereof include aliphatic diisocyanate compounds and aromatic diisocyanate compounds. Examples of the aliphatic diisocyanate compound include linear aliphatic diisocyanate compounds such as 1,4-butane diisocyanate and 1,6-hexane diisocyanate; branched aliphatic diisocyanate compounds such as 2,2,4-trimethylhexamethylene diisocyanate and 2,4,4-trimethylhexamethylene diisocyanate; and alicyclic diisocyanate compounds such as norbornane diisocyanate, isophorone diisocyanate, hydrogenated xylylene diisocyanate, and hydrogenated diphenylmethane diisocyanate. Examples of aromatic diisocyanate compounds include tolylene diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, 4,4'-diisocyanato-3,3'-dimethylbiphenyl, and o-tolidine diisocyanate. As described above, the diisocyanate compound may have two isocyanate groups in the molecule, and may be, for example, a diisocyanate compound having a urethane bond, which is obtained by reacting the diisocyanate compound with a diol compound. The diol compound is not particularly limited as long as it is a compound having two hydroxyl groups in the molecule, and may be, for example, a diol compound having a saturated or unsaturated aliphatic skeleton (e.g., an alkylene skeleton, an alkenylene skeleton, an alkapolyenyl group) (an example is a bifunctional hydroxyl group-terminated polybutadiene described later); an aromatic diol compound having an aromatic skeleton, such as a biphenol compound, a bisphenol compound, or a polyarylene ether having a terminal hydroxyl group.
[0127] Therefore, in a preferred embodiment, the polyimide resin is an imide of an acid anhydride and a diamine compound. In another preferred embodiment, the polyimide resin is an imide of an acid anhydride and a diisocyanate compound. The terminal functional group of the polyimide resin may be modified by reacting with the above-mentioned diol compound or the like.
[0128] Other specific examples of polyimide resins include "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd. Specific examples of polyimide resins also include modified polyimides such as linear polyimides obtained by reacting bifunctional hydroxyl-terminated polybutadiene, a diisocyanate compound, and a tetrabasic acid anhydride (disclosed in JP-A-2006-37083), and polysiloxane skeleton-containing polyimides (disclosed in JP-A-2002-12667 and JP-A-2000-319386, etc.).
[0129] Specific examples of polyamide-imide resins include "Viromax HR11NN" and "Viromax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins also include modified polyamide-imides such as polysiloxane skeleton-containing polyamide-imides "KS9100" and "KS9300" manufactured by Hitachi Chemical Co., Ltd.
[0130] A specific example of the polyethersulfone resin is "PES5003P" manufactured by Sumitomo Chemical Co., Ltd.
[0131] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.
[0132] When the resin composition of the present invention contains the (G) component, the content of the (G) component in the resin composition may be determined according to the properties required for the resin composition, but when the resin component in the resin composition is 100 mass%, it is, for example, 0.1 mass% or more, preferably 0.3 mass% or more, more preferably 0.5 mass% or more, 0.6 mass% or more, or 0.8 mass% or more. The upper limit of the content of the (G) component is not particularly limited, but may be, for example, 15 mass% or less, 10 mass% or less, 8 mass% or less, 6 mass% or less, etc.
[0133] <Optional Additives> The resin composition of the present invention may further contain any additive. Examples of such additives include radical polymerization initiators such as peroxide radical polymerization initiators and azo radical polymerization initiators; organometallic compounds such as organic copper compounds, organic zinc compounds, and organic cobalt compounds; organic fillers other than component (A) (e.g., rubber particles; provided that, when the total of the organic fillers is taken as 100 parts by mass, the amount of component (A) is preferably 50 parts by mass or more, more preferably 70 parts by mass or more, and even more preferably 80 parts by mass or more, 90 parts by mass or more, or 95 parts by mass or more); colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone leveling agents and acrylic polymer leveling agents; thickeners such as bentone and montmorillonite; defoamers such as silicone defoamers, acrylic defoamers, fluorine defoamers, and vinyl resin defoamers; and bentonite. antioxidants such as hindered phenol antioxidants; fluorescent brighteners such as stilbene derivatives; surfactants such as fluorine-based surfactants and silicone-based surfactants; flame retardants such as phosphorus-based flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus), nitrogen-based flame retardants (e.g., melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (e.g., antimony trioxide); dispersants such as phosphate ester dispersants, polyoxyalkylene dispersants, acetylene dispersants, silicone-based dispersants, anionic dispersants, and cationic dispersants; and stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic acid anhydride-based stabilizers. The content of such additives may be determined depending on the properties required for the resin composition.
[0134] <Organic solvent> The resin composition of the present invention may further contain an organic solvent as a volatile component. Examples of the organic solvent include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, and diphenyl ether; alcohol-based solvents such as methanol, ethanol, propanol, butanol, and ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, and methyl methoxypropionate. Examples of the organic solvent include ether ester solvents such as ethyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate; ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butyl carbitol); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane; and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. The organic solvent may be used alone or in combination of two or more.
[0135] The resin composition of the present invention can be produced, for example, by adding and mixing components (A), (B), (C), and (D), and, if necessary, components (E), (F), and (G), other additives, and organic solvents, in any order and / or all at once in any preparation vessel. In addition, the temperature can be appropriately set during the process of adding and mixing each component, and heating and / or cooling may be performed temporarily or throughout. In addition, during or after the process of adding and mixing, the resin composition may be stirred or shaken using a stirring device or shaking device such as a mixer to disperse the resin composition uniformly. Simultaneous with stirring or shaking, degassing may be performed under low pressure conditions such as under vacuum.
[0136] Even when the resin composition of the present invention contains an organic solvent, the component (A) is insoluble in the organic solvent and is also incompatible with other components including the components (B) and (C), so that the preferred dimensions, such as the average particle size, can be maintained. Thus, in one embodiment, the component (A) is insoluble in the solvent.
[0137] As described above, the resin composition of the present invention containing component (A) in combination with components (B) to (D) can provide a cured product that exhibits good crack resistance and good adhesion to a conductor layer when exposed to a high-temperature and high-humidity environment, even when a specific composition that contributes to good dielectric properties is adopted. Furthermore, an insulating layer that has few undulations and exhibits good surface flatness can be realized regardless of the surface pattern of the underlying substrate (surface unevenness pattern due to recesses such as degassing holes and protrusions such as surface circuits).
[0138] In one embodiment, the cured product of the resin composition of the present invention is characterized by a low dielectric loss tangent (Df). For example, when measured at 5.8 GHz and 23° C. as described in the section [Test Example 1: Measurement of Dielectric Loss Tangent (Df)] below, the dielectric loss tangent (Df) of the cured product of the resin composition of the present invention may be preferably 0.006 or less, 0.005 or less, 0.004 or less, 0.0038 or less, 0.0036 or less, 0.0034 or less, 0.0032 or less, or 0.003 or less.
[0139] In one embodiment, the cured product of the resin composition of the present invention is characterized by high adhesion to a conductor layer. For example, when exposed to high temperature and humidity conditions of 130°C and 85% RH for 100 hours as described in the section [Test Example 3: Measurement of copper foil peel strength after high temperature and humidity environmental test (HAST)] below, the adhesion strength to the conductor foil after exposure to high temperature and humidity conditions is preferably 0.35 kgf / cm or more, 0.4 kgf / cm or more, 0.42 kgf / cm or more, 0.44 kgf / cm or more, or 0.45 kgf / cm or more.
[0140] As described above, even when a specific composition that contributes to good dielectric properties is adopted, the resin composition of the present invention can provide a cured product that exhibits good crack resistance and good adhesion to a conductor layer when exposed to a high-temperature and high-humidity environment. Furthermore, an insulating layer that has few undulations and exhibits good surface flatness can be realized regardless of the surface pattern of the underlying substrate. Therefore, the resin composition of the present invention can be suitably used as a resin composition for forming an insulating layer of a printed wiring board (resin composition for insulating layer of printed wiring board), and can be more suitably used as a resin composition for forming an interlayer insulating layer of a printed wiring board (resin composition for insulating interlayer of printed wiring board). The resin composition of the present invention can also be suitably used when the printed wiring board is a circuit board with built-in components. The resin composition of the present invention can also be suitably used as a resin composition for forming an insulating layer of a rewiring board of a semiconductor package (resin composition for insulating layer of rewiring board). In the present invention, printed wiring boards and rewiring boards are also collectively referred to as "circuit boards", and therefore the resin composition of the present invention can be suitably used for the insulating layer of a circuit board.
[0141] The resin composition of the present invention can further be used in a wide range of applications requiring a resin composition, such as sheet-like laminate materials such as resin sheets and prepregs, solder resists, underfill materials, die bonding materials, hole filling resins, sealing resins, and component embedding resins.
[0142] [Sheet-type laminated materials (resin sheets, prepregs)] The resin composition of the present invention can be used as it is, but it may also be used in the form of a sheet-like laminate material containing the resin composition.
[0143] As the sheet-like laminate material, the following resin sheets and prepregs are preferred.
[0144] In one embodiment, the resin sheet includes a support and a layer of a resin composition (hereinafter simply referred to as a "resin composition layer") provided on the support, and is characterized in that the resin composition layer is formed from the resin composition of the present invention.
[0145] The thickness of the resin composition layer may vary depending on the application, and may be appropriately determined depending on the application. For example, the thickness of the resin composition layer is preferably 100 μm or less, 80 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, or 30 μm or less from the viewpoint of thinning of printed wiring boards and semiconductor packages. The lower limit of the thickness of the resin composition layer is not particularly limited, but may usually be 1 μm or more, 5 μm or more, etc.
[0146] Examples of the support include a thermoplastic resin film, a metal foil, and a release paper, and a thermoplastic resin film and a metal foil are preferred. Thus, in a preferred embodiment, the support is a thermoplastic resin film or a metal foil.
[0147] When a thermoplastic resin film is used as the support, examples of the thermoplastic resin include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), acrylics such as polycarbonate (PC) and polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.
[0148] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.
[0149] The support may be subjected to a matte treatment, a corona treatment, or an antistatic treatment on the surface to be bonded to the resin composition layer. In addition, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used as the support. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.
[0150] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.
[0151] When a metal foil is used as the support, a metal foil with a support substrate may be used, which is a thin metal foil with a peelable support substrate attached thereto. In one embodiment, the metal foil with a support substrate includes a support substrate, a release layer provided on the support substrate, and a metal foil provided on the release layer. When a metal foil with a support substrate is used as the support, the resin composition layer is provided on the metal foil.
[0152] In the metal foil with a supporting substrate, the material of the supporting substrate is not particularly limited, and examples thereof include copper foil, aluminum foil, stainless steel foil, titanium foil, copper alloy foil, etc. When copper foil is used as the supporting substrate, it may be electrolytic copper foil or rolled copper foil. In addition, the release layer is not particularly limited as long as it can release the metal foil from the supporting substrate, and examples thereof include an alloy layer of an element selected from the group consisting of Cr, Ni, Co, Fe, Mo, Ti, W, and P; an organic coating, etc.
[0153] In the metal foil with a supporting substrate, the material of the metal foil is preferably, for example, copper foil or copper alloy foil.
[0154] In the metal foil with a supporting substrate, the thickness of the supporting substrate is not particularly limited, but is preferably in the range of 10 μm to 150 μm, more preferably in the range of 10 μm to 100 μm, and the thickness of the metal foil may be, for example, in the range of 0.1 μm to 10 μm.
[0155] In one embodiment, the resin sheet may further include an optional layer as necessary. For example, such an optional layer may be a protective film provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, it is possible to suppress adhesion of dirt and the like to the surface of the resin composition layer and scratches.
[0156] The resin sheet can be produced, for example, by preparing a liquid resin composition as is or a resin varnish by dissolving the resin composition in an organic solvent, applying this onto a support using a die coater or the like, and then drying to form a resin composition layer.
[0157] The organic solvent may be the same as the organic solvent described as a component of the resin composition. The organic solvent may be used alone or in combination of two or more kinds.
[0158] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of the organic solvent in the resin composition layer becomes 10% by mass or less, preferably 5% by mass or less. Although it varies depending on the boiling point of the organic solvent in the resin composition or resin varnish, for example, when a resin composition or resin varnish containing 30% by mass to 60% by mass of the organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.
[0159] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it can be used by peeling off the protective film.
[0160] In one embodiment, the prepreg is formed by impregnating a sheet-like fiber substrate with the resin composition of the present invention.
[0161] The sheet-like fiber substrate used for the prepreg is not particularly limited, and can be a substrate commonly used for prepreg, such as glass cloth, aramid nonwoven fabric, or liquid crystal polymer nonwoven fabric. From the viewpoint of thinning of printed wiring boards and semiconductor chip packages, the thickness of the sheet-like fiber substrate is preferably 50 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and particularly preferably 20 μm or less. The lower limit of the thickness of the sheet-like fiber substrate is not particularly limited. It is usually 10 μm or more.
[0162] The prepreg can be produced by a known method such as a hot melt method or a solvent method.
[0163] The thickness of the prepreg may be in the same range as that of the resin composition layer in the above-mentioned resin sheet.
[0164] The sheet-like laminate material of the present invention can be suitably used to form an insulating layer of a printed wiring board (for the insulating layer of a printed wiring board), and can be more suitably used to form an interlayer insulating layer of a printed wiring board (for the insulating edge layer of a printed wiring board). The sheet-like laminate material of the present invention can also be suitably used to form an insulating layer of a rewiring board of a semiconductor package (for the insulating layer of a rewiring board). That is, the sheet-like laminate material of the present invention can be suitably used as an insulating layer of a circuit board.
[0165] [Circuit board] The resin composition of the present invention can be used to form an insulating layer for a circuit board. The present invention also provides such a circuit board, i.e., a circuit board including an insulating layer made of a cured product of the resin composition of the present invention.
[0166] <Printed wiring board> In one embodiment, the circuit board of the present invention is a printed wiring board.
[0167] The printed wiring board can be produced, for example, by using the above-mentioned resin sheet, by a method including the following steps (I) and (II). (I) A step of laminating a resin sheet on an inner layer substrate such that a resin composition layer of the resin sheet is bonded to the inner layer substrate. (II) A step of curing (e.g., heat curing) the resin composition layer to form an insulating layer.
[0168] The "inner layer substrate" used in step (I) is a member that becomes the substrate of the printed wiring board, and examples thereof include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. The substrate may have a conductor layer on one or both sides, and the conductor layer may be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of the substrate may be called an "inner layer circuit substrate". In addition, an intermediate product on which an insulating layer and / or a conductor layer is to be formed during the manufacture of a printed wiring board is also included in the "inner layer substrate" of the present invention. When the printed wiring board is a circuit board with built-in components, an inner layer substrate with built-in components may be used.
[0169] The lamination of the inner layer substrate and the resin sheet can be carried out, for example, by thermocompression bonding the resin sheet to the inner layer substrate from the support side. Examples of the member for thermocompression bonding the resin sheet to the inner layer substrate (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). The thermocompression bonding member may be pressed directly onto the resin sheet, or may be pressed via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the inner layer substrate.
[0170] The lamination of the inner layer substrate and the resin sheet may be performed by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination may be performed under reduced pressure conditions, preferably at a pressure of 26.7hPa or less.
[0171] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.
[0172] After lamination, the laminated resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.
[0173] The support may be removed between step (I) and step (II), or after step (II). When a metal foil is used as the support, the conductor layer may be formed using the metal foil without peeling off the support. When a metal foil with a support substrate is used as the support, the support substrate (and the peel layer) may be peeled off. Then, the conductor layer can be formed using the metal foil.
[0174] In step (II), the resin composition layer is cured (for example, thermally cured) to form an insulating layer made of a cured product of the resin composition. The curing conditions for the resin composition layer are not particularly limited, and conditions that are usually adopted when forming an insulating layer for a printed wiring board may be used.
[0175] For example, the thermal curing conditions for the resin composition layer vary depending on the type of resin composition, etc., but in one embodiment, the curing temperature is preferably 140° C. to 250° C., more preferably 150° C. to 240° C., and even more preferably 180° C. to 230° C. The curing time is preferably 5 minutes to 240 minutes, more preferably 10 minutes to 150 minutes, and even more preferably 15 minutes to 120 minutes.
[0176] Before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature of 50° C. to 140° C., preferably 60° C. to 135° C., more preferably 70° C. to 130° C. for 5 minutes or more, preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes.
[0177] In manufacturing a printed wiring board, the steps of (III) drilling holes in the insulating layer, (IV) roughening the insulating layer, and (V) forming a conductor layer may be further carried out. These steps (III) to (V) may be carried out according to various methods known to those skilled in the art that are used in manufacturing printed wiring boards. When the support is removed after step (II), the removal of the support may be carried out between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V). In addition, the formation of the insulating layer and the conductor layer in steps (I) to (V) may be repeated to form a multilayer wiring board, as necessary.
[0178] In another embodiment, the printed wiring board of the present invention can be manufactured using the above-mentioned prepreg. The manufacturing method is basically the same as when a resin sheet is used.
[0179] Step (III) is a step of drilling holes in the insulating layer, which allows holes such as via holes and through holes to be formed in the insulating layer. Step (III) may be performed using, for example, a drill, a laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The dimensions and shape of the holes may be appropriately determined depending on the design of the printed wiring board.
[0180] Step (IV) is a step of roughening the insulating layer. Usually, in this step (IV), smear removal (desmear) is also performed. The procedure and conditions of the roughening treatment are not particularly limited, and known procedures and conditions that are usually used when forming an insulating layer of a printed wiring board can be adopted. For example, the insulating layer can be roughened by performing a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid in this order.
[0181] The swelling liquid used in the roughening treatment is not particularly limited, but includes an alkaline solution, a surfactant solution, etc., and is preferably an alkaline solution, and more preferably a sodium hydroxide solution or a potassium hydroxide solution. Examples of commercially available swelling liquids include "Swelling Dip Securigans P" and "Swelling Dip Securigans SBU" manufactured by Atotech Japan. The swelling treatment using the swelling liquid is not particularly limited, but can be performed by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 to 20 minutes, for example. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes.
[0182] The oxidizing agent used in the roughening treatment is not particularly limited, but examples thereof include an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 minutes to 30 minutes. The concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securigans P" manufactured by Atotech Japan.
[0183] The neutralizing solution used in the roughening treatment is preferably an acidic aqueous solution, and a commercially available product such as "Reduction Solution Securigant P" manufactured by Atotech Japan can be mentioned.
[0184] The treatment with the neutralizing solution can be carried out by immersing the surface that has been roughened with an oxidizing agent in a neutralizing solution at 30° C. to 80° C. for 5 to 30 minutes. From the viewpoint of workability, etc., a method in which the object that has been roughened with an oxidizing agent is immersed in a neutralizing solution at 40° C. to 70° C. for 5 to 20 minutes is preferred.
[0185] Step (V) is a step of forming a conductor layer, and the conductor layer is formed on the insulating layer. The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among these, from the viewpoints of versatility in forming the conductor layer, cost, ease of patterning, and the like, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.
[0186] The conductor layer may be a single-layer structure or a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.
[0187] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is generally 3 μm to 35 μm, preferably 5 μm to 30 μm.
[0188] In one embodiment, the conductor layer may be formed by plating. From the viewpoint of facilitating the formation of fine wiring, it is preferable to form the conductor layer by a semi-additive method. An example of forming the conductor layer by the semi-additive method will be described below.
[0189] First, a plating seed layer is formed on the surface of an insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a part of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like to form a conductor layer having a desired wiring pattern.
[0190] In another embodiment, the conductor layer may be formed using a metal foil. When the conductor layer is formed using a metal foil, it is preferable to carry out the step (V) between the steps (I) and (II). For example, after the step (I), the support is removed, and a metal foil is laminated on the exposed surface of the resin composition layer. The lamination of the resin composition layer and the metal foil may be carried out by a vacuum lamination method. The lamination conditions may be the same as those described for the step (I). Then, the step (II) is carried out to form an insulating layer. Thereafter, a conductor layer having a desired wiring pattern can be formed by a conventionally known technique such as a modified semi-additive method, using the metal foil on the insulating layer.
[0191] The metal foil can be produced by a known method such as an electrolytic method, a rolling method, etc. Commercially available metal foils include, for example, HLP foil and JXUT-III foil manufactured by JX Metals, and 3EC-III foil and TP-III foil manufactured by Mitsui Kinzoku Co., Ltd.
[0192] Alternatively, when a metal foil or a metal foil with a supporting substrate is used as the support for the resin sheet, the conductor layer may be formed using the metal foil, as described above.
[0193] <Rewiring substrate for semiconductor packages> In one embodiment, the circuit board of the present invention is a rewiring board (rewiring layer) of a semiconductor package. Hereinafter, a method for manufacturing a semiconductor package will be described.
[0194] The semiconductor package includes an insulating layer made of the cured product of the resin composition of the present invention as an insulating layer of a rewiring board. The semiconductor package may also include a sealing layer made of the cured product of the resin composition of the present invention.
[0195] A semiconductor package can be manufactured, for example, by a method including the following steps (1) to (6) using the resin composition and resin sheet of the present invention. The resin composition and resin sheet of the present invention may be used to form a rewiring formation layer (insulating layer for forming a rewiring board) in step (5) or a sealing layer in step (3). An example of forming a rewiring formation layer or a sealing layer using a resin composition or a resin sheet is shown below, but the technology for forming a rewiring formation layer or a sealing layer of a semiconductor package is publicly known, and a person skilled in the art can manufacture a semiconductor package using the resin composition and resin sheet of the present invention according to a publicly known technology. (1) A step of laminating a temporary fixing film onto a substrate; (2) a step of temporarily fixing a semiconductor chip on a temporary fixing film; (3) forming an encapsulation layer on the semiconductor chip; (4) peeling the substrate and the temporary fixing film from the semiconductor chip; (5) forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film have been peeled off; and (6) A process of forming a rewiring layer as a conductor layer on the rewiring formation layer.
[0196] -Process (1)- The material used for the substrate is not particularly limited. Examples of the substrate include semiconductor wafers such as silicon wafers, glass wafers, glass substrates, metal substrates such as copper, titanium, stainless steel, and cold-rolled steel (SPCC), substrates in which glass fibers are impregnated with epoxy resin or the like and subjected to a heat curing treatment (e.g., FR-4 substrates), and substrates made of bismaleimide triazine resin (BT resin).
[0197] The material of the temporary fixing film is not particularly limited as long as it can be peeled off from the semiconductor chip in step (4) and can temporarily fix the semiconductor chip. A commercially available product can be used as the temporary fixing film. An example of the commercially available product is Riva Alpha manufactured by Nitto Denko Corporation.
[0198] -Process (2)- The semiconductor chips can be temporarily fixed using known devices such as a flip chip bonder, a die bonder, etc. The layout and number of semiconductor chips can be appropriately set depending on the shape and size of the temporary fixing film, the number of semiconductor packages to be produced, etc., and for example, the semiconductor chips can be temporarily fixed by arranging them in a matrix shape of multiple rows and multiple columns.
[0199] -Process (3)- A resin composition layer of the resin sheet of the present invention is laminated on a semiconductor chip, or the resin composition of the present invention is applied onto a semiconductor chip and cured (for example, thermally cured) to form an encapsulating layer.
[0200] For example, the semiconductor chip and the resin sheet can be laminated by removing the protective film of the resin sheet and then heat-pressing the resin sheet to the semiconductor chip from the support side. Examples of the member for heat-pressing the resin sheet to the semiconductor chip (hereinafter also referred to as the "heat-pressing member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the heat-pressing member not directly onto the resin sheet but via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the semiconductor chip. The semiconductor chip and the resin sheet may be laminated by a vacuum lamination method, and the lamination conditions are the same as those described in relation to the manufacturing method of the printed wiring board, and the preferred ranges are also the same.
[0201] After lamination, the resin composition is thermally cured to form the encapsulating layer under the same conditions as those described in relation to the method for producing a printed wiring board.
[0202] The support of the resin sheet may be peeled off after the resin sheet is laminated on the semiconductor chip and thermally cured, or the support may be peeled off before the resin sheet is laminated on the semiconductor chip.
[0203] When the resin composition of the present invention is applied to form a sealing layer, the application conditions are the same as the application conditions when forming the resin composition layer described in relation to the resin sheet of the present invention, and the preferred ranges are also the same.
[0204] -Process (4)- The method for peeling off the substrate and the temporary fixing film can be appropriately changed depending on the material of the temporary fixing film, and examples of the method include a method in which the temporary fixing film is heated and foamed (or expanded) to peel it off, and a method in which ultraviolet light is irradiated from the substrate side to reduce the adhesive strength of the temporary fixing film and then peeled off.
[0205] In the method of heating and foaming (or expanding) the temporary fixing film to peel it off, the heating conditions are usually 100 to 250° C. for 1 to 90 seconds or 5 to 15 minutes. In the method of irradiating ultraviolet light from the substrate side to reduce the adhesive strength of the temporary fixing film to peel it off, the irradiation dose of ultraviolet light is usually 10 mJ / cm. 2 ~1000mJ / cm 2 It is.
[0206] -Process (5)- The resin composition and resin sheet of the present invention are used to form a rewiring formation layer (insulating layer of a rewiring board).
[0207] After forming the redistribution layer, a via hole may be formed in the redistribution layer to connect the semiconductor chip to a conductor layer described later. The via hole may be formed by a known method depending on the material of the redistribution layer.
[0208] -Process (6)- The formation of the conductor layer on the rewiring formation layer may be carried out in the same manner as in step (V) described in relation to the method for producing a printed wiring board. Note that steps (5) and (6) may be repeated to alternately stack (build up) the conductor layer (rewiring layer) and the rewiring formation layer (insulating layer).
[0209] In manufacturing the semiconductor package, the steps of (7) forming a solder resist layer on the conductor layer (rewiring layer), (8) forming bumps, and (9) dicing a plurality of semiconductor packages into individual semiconductor packages may be further carried out. These steps may be carried out according to various methods used in manufacturing semiconductor packages and known to those skilled in the art.
[0210] By forming a rewiring formation layer (insulating layer) using the resin composition and resin sheet of the present invention, which can provide a cured product that exhibits excellent dielectric properties, good crack resistance, and good adhesion to a conductor layer when exposed to a high-temperature and high-humidity environment, a semiconductor package with extremely low transmission loss can be realized without concern for a decrease in conductor adhesion, regardless of whether the semiconductor package is a fan-in (Fan-In) type package or a fan-out (Fan-Out) type package. In one embodiment, the semiconductor package of the present invention is a fan-out (Fan-Out) type package. The resin composition and resin sheet of the present invention can be applied to any type of package, whether it is a fan-out type panel level package (FOPLP) or a fan-out type wafer level package (FOWLP). In one embodiment, the semiconductor package of the present invention is a fan-out type panel level package (FOPLP) or a fan-out type wafer level package (FOWLP).
[0211] [Semiconductor Devices] The semiconductor device of the present invention includes a layer made of a cured product of the resin composition layer of the present invention. The semiconductor device of the present invention can be produced by using the circuit board of the present invention.
[0212] Examples of the semiconductor device include various semiconductor devices used in electric appliances (for example, computers, mobile phones, digital cameras, and televisions) and vehicles (for example, motorcycles, automobiles, trains, ships, and aircraft). EXAMPLES
[0213] The present invention will be specifically described below with reference to examples. The present invention is not limited to these examples. In the following, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Unless otherwise specified, the temperature and pressure conditions are room temperature (25°C) and atmospheric pressure (1 atm).
[0214] <Synthesis Example 1: Synthesis of Fine Particle A> Polyphenylene ether resin ("Lupiace LN91" manufactured by Mitsubishi Engineering Plastics Corporation) was disintegrated in methanol solvent using a homomixer (HM-300 type, manufactured by AS ONE Corporation) at 25°C, 8000 rpm, and 4 hours. Thereafter, the methanol solvent was dried and removed, and the polyphenylene ether (PPE) powder was recovered by sieving through a JIS test sieve with 12 μm openings. 198 parts of toluene and 3 parts of polystyrene (Polystyrene Japan Co., Ltd. "SX-300") were placed in a flask and stirred to dissolve the polystyrene. Next, 50 parts of the previously prepared PPE powder was added and stirred for 2 hours to obtain a dispersion of PPE particles (20% by mass). This was named Fine Particles A (average particle size 1.2 μm, 90% particle size D 90 is less than 1.8 μm).
[0215] <Synthesis Example 2: Synthesis of Maleimide Compound B> According to the method described in Synthesis Example 1 of the Japan Institute of Invention and Innovation's Technical Journal Publication No. 2020-500211, a MEK solution of maleimide compound B (70% by mass of non-volatile components) was synthesized.
[0216] <Synthesis Example 3: Synthesis of Polyimide Resin C> A flask equipped with a stirrer, a thermometer, and a condenser was charged with 271.7 parts of propylene glycol methyl ether acetate (PGMAc), 14.1 parts (0.064 mol) of isophorone diisocyanate (IPDI), and 112.2 parts (0.03 mol) of polybutadiene having OH groups at both ends ("G-3000" manufactured by Nippon Soda Co., Ltd., hydroxyl value: 30 mgKOH / g). The mixed solution was heated to 50°C and then held at this temperature for 1 hour. Then, it was confirmed that the amount of isocyanate groups was equal to or less than a predetermined value, and 145.2 parts (0.09 mol) of oligophenylene ether resin containing phenolic hydroxyl groups at both ends ("SA90-100" manufactured by Sabic, hydroxyl equivalent: 807 g / mol) and 1 part (0.003 mol) of benzophenone tetracarboxylic dianhydride (BTDA) were added to the mixed solution. The mixture was then heated to 140° C. and the reaction was continued for 4 hours. -1 The reaction was terminated when it was confirmed that the absorption peak of had completely disappeared and the increase in viscosity had ceased. In this manner, polyimide resin C having a structure in which the molecular ends were sealed with phenol resin (oligophenylene ether resin containing phenolic hydroxyl groups at both ends) was synthesized. The non-volatile content was 50% by mass.
[0217] <Synthesis Example 4: Synthesis of Polyimide Resin D> A 500 mL separable flask equipped with a water content receiver connected to a reflux condenser, a nitrogen inlet tube, and a stirrer was prepared. 20.3 g of 4,4'-oxydiphthalic anhydride (ODPA), 200 g of γ-butyrolactone, 20 g of toluene, and 29.6 g of 5-(4-aminophenoxy)-3-[4-(4-aminophenoxy)phenyl]-1,1,3-trimethylindane were added to this flask, and the mixture was stirred at 45°C for 2 hours under a nitrogen stream to carry out a reaction. Next, the reaction solution was heated and, while maintaining the temperature at about 160°C, condensed water was azeotropically removed together with toluene under a nitrogen stream. It was confirmed that a predetermined amount of water had accumulated in the water content receiver and that no water was flowing out. After confirmation, the reaction solution was further heated and stirred at 200°C for 1 hour. The mixture was then cooled to obtain a solution (20% by mass of non-volatile components) containing polyimide resin D having a 1,1,3-trimethylindane skeleton. The obtained polyimide resin D had a repeating unit represented by the following formula (X1) and a repeating unit represented by the following formula (X2). The weight average molecular weight of polyimide resin D was 12,000.
[0218] [ka]
[0219] [Example 1] (1) Preparation of resin composition 12 parts of biphenyl type epoxy resin ("NC3000" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent approximately 269 g / eq.) and 6 parts of bisphenol type epoxy resin ("ZX1059" manufactured by Nippon Steel Chemical & Material Co., Ltd., 1:1 mixture of bisphenol A type and bisphenol F type, epoxy equivalent approximately 169 g / eq.) were heated and dissolved in 40 parts of methyl ethyl ketone with stirring. This was cooled to room temperature to prepare a dissolved composition of the epoxy resin. The epoxy resin solution composition was mixed with hollow PPE particles ("XX-6655Z" manufactured by Sekisui Chemical Co., Ltd., average particle size 0.4 μm, 90% particle size D 90The mixture consisted of 3 parts of an active ester curing agent (DIC Corporation's "HPC-8151-62T", active ester group equivalent weight approx. 240 g / eq., toluene solution with non-volatile content of 62% by mass), 50 parts of spherical silica (Admatechs Corporation's "SO-C2", average particle size 0.5 μm, specific surface area 5.8 m) surface-treated with a silane coupling agent (Shin-Etsu Chemical Co., Ltd.'s "KBM-573"). 2 A resin composition was prepared by mixing 150 parts of a phenolic curing agent containing a triazine skeleton (DIC Corporation's "LA-3018-50P", active group equivalent of approximately 151 g / eq., 2-methoxypropanol solution with a non-volatile content of 50%), 4 parts of an imidazole curing accelerator (Shikoku Chemical Industry Co., Ltd.'s "1B2PZ", 1-benzyl-2-phenylimidazole), and 2 parts of a phenoxy resin (Mitsubishi Chemical Corporation's "YX7553BH30", a 1:1 solution of MEK and cyclohexanone with a non-volatile content of 30% by mass) and dispersing the mixture uniformly using a high-speed rotating mixer.
[0220] (2) Manufacturing of resin sheets A polyethylene terephthalate film with a release layer ("AL5" manufactured by Lintec Corporation, thickness 38 μm) was prepared as a support. The resin composition prepared in (1) above was uniformly applied onto the release layer of this support so that the thickness of the resin composition layer after drying would be 40 μm. Thereafter, the resin composition was dried at 80°C to 100°C (average 90°C) for 4 minutes to obtain a resin sheet having a layer structure of a resin composition layer / support.
[0221] [Example 2] A resin composition was prepared and a resin sheet was obtained in the same manner as in Example 1, except that (1) the amount of hollow PPE particles ("XX-6655Z" manufactured by Sekisui Chemical Co., Ltd.) was changed from 3 parts to 20 parts, (2) the amount of spherical silica ("SO-C2" manufactured by Admatechs Co., Ltd.) surface-treated with a silane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed from 150 parts to 200 parts, (3) 5 parts of styryl resin ("OPE-2St 2200" manufactured by Mitsubishi Gas Chemical Co., Ltd., toluene solution with non-volatile content of 65%) was further used, and (4) 4 parts of a carbodiimide-based curing agent ("V-03" manufactured by Nisshinbo Chemical Inc., active group equivalent of approximately 216 g / eq., toluene solution with non-volatile content of 50%) was further used.
[0222] [Example 3] (1) Instead of hollow PPE particles (“XX-6655Z” manufactured by Sekisui Plastics Co., Ltd.), solid PPE particles (“XX-6714Z” manufactured by Sekisui Plastics Co., Ltd., average particle size 0.7 μm, 90% particle size D 90 (1) 3 parts of an active ester curing agent (HPC-8000-65T manufactured by DIC Corporation, active ester group equivalent weight of about 223 g / eq., non-volatile content of 65% in toluene solution) was used instead of an active ester curing agent (HPC-8151-62T manufactured by DIC Corporation); (2) 50 parts of an active ester curing agent (HPC-8000-65T manufactured by DIC Corporation, active ester group equivalent weight of about 223 g / eq., non-volatile content of 65% in toluene solution) was used instead of an active ester curing agent (HPC-8151-62T manufactured by DIC Corporation); (3) 6 parts of the imide resin C obtained in Synthesis Example 3 were further used; (4) a carbodiimide curing agent (HPC-8000-65T manufactured by DIC Corporation, active ester group equivalent weight of about 223 g / eq., non-volatile content of 65% in toluene solution) was used instead of an active ester curing agent (HPC-8151-62T manufactured by DIC Corporation). A resin composition was prepared and a resin sheet was obtained in the same manner as in Example 1, except that (4 parts of "V-03" manufactured by Seibo Chemical Co., Ltd., active group equivalent weight of approximately 216 g / eq., toluene solution with non-volatile content of 50%) was further used, and (5) the amount of spherical silica ("SO-C2" manufactured by Admatechs Co., Ltd.) surface-treated with a silane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed from 150 parts to 160 parts.
[0223] [Example 4] A resin composition was prepared and a resin sheet was obtained in the same manner as in Example 1, except that (1) 3 parts of solid PPE particles ("XX-6714Z" manufactured by Sekisui Chemical Co., Ltd., average particle size 0.7 μm) were used instead of the hollow PPE particles ("XX-6655Z" manufactured by Sekisui Chemical Co., Ltd.), (2) 3 parts of a bismaleimide compound ("BMI-1500" manufactured by DMI Corporation) were further used, and (3) the amount of spherical silica ("SO-C2" manufactured by Admatechs Co., Ltd.) surface-treated with a silane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed from 150 parts to 160 parts.
[0224] [Example 5] A resin composition was prepared and a resin sheet was obtained in the same manner as in Example 1, except that (1) the amount of hollow PPE particles ("XX-6655Z" manufactured by Sekisui Chemical Co., Ltd.) was changed from 3 parts to 1 part, (2) 6 parts of bisphenol A type epoxy resin ("828EL" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: approximately 180) was used instead of 6 parts of bisphenol type epoxy resin ("ZX1059" manufactured by Nippon Steel Chemical & Material Co., Ltd.), and (3) 5 parts of the maleimide compound B obtained in Synthesis Example 2 was further used.
[0225] [Example 6] (1) 6 parts of bisphenol-type epoxy resin (Nippon Steel Chemical & Material Co., Ltd. "ZX1059") was replaced with 6 parts of bisphenol A-type epoxy resin (Mitsubishi Chemical Co., Ltd. "828EL", epoxy equivalent: approximately 180); (2) 50 parts of active ester-type curing agent (DIC Corporation "HPC-8151-62T") was replaced with 50 parts of active ester-type curing agent (DIC Corporation "HPC-8000-65T", active ester group equivalent: approximately 223 g / eq., toluene solution with non-volatile content of 65%); (3) 150 parts of spherical silica (Admatechs Co., Ltd. "SO-C2") surface-treated with a silane coupling agent (Shin-Etsu Chemical Co., Ltd. "KBM-573") was replaced with spherical silica (Denka Co., Ltd. "UFP-30", average particle size: 0.3 μm, specific surface area: 30.7 m) surface-treated with the same agent. 2 / g, carbon content per unit surface area 0.22mg / m 2A resin composition was prepared and a resin sheet was obtained in the same manner as in Example 1, except that (1) 70 parts of the methyl cellulose acetate copolymer were used, and (2) the amount of the phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation) was changed from 2 parts to 10 parts.
[0226] [Example 7] (1) The amount of active ester-based hardener (DIC Corporation's "HPC-8000-65T") was changed from 50 parts to 10 parts, (2) 20 parts of a cyanate ester-based hardener (Lonza Japan's "BA230S75", a prepolymer of bisphenol A dicyanate, cyanate equivalent of approximately 232 g / eq., MEK solution with a non-volatile content of 75% by mass) was further used, and (3) a triazine skeleton-containing phenol-based hardener (DIC Corporation's "LA-3018-50P") was used. (4) 70 parts of surface-treated spherical silica ("UFP-30" manufactured by Denka Co., Ltd.) were replaced with 70 parts of the same surface-treated spherical silica ("SO-C2" manufactured by Admatechs Co., Ltd., average particle size 0.5 μm, specific surface area 5.8 m). 2 A resin composition was prepared and a resin sheet was obtained in the same manner as in Example 6, except that (120 parts of 1-benzyl-2-phenylimidazole was used instead of (5) 1 part of a 1 mass % MEK solution of cobalt (III) acetylacetonate (manufactured by Tokyo Chemical Industry Co., Ltd.), was used instead of 0.5 parts of the imidazole curing accelerator ("1B2PZ" manufactured by Shikoku Chemical Industry Co., Ltd., 1-benzyl-2-phenylimidazole).
[0227] [Example 8] A resin composition was prepared and a resin sheet was obtained in the same manner as in Example 1, except that 15 parts of the fine particles A prepared in Synthesis Example 1 were used instead of 3 parts of the hollow PPE particles ("XX-6655Z" manufactured by Sekisui Chemical Co., Ltd.).
[0228] [Example 9] A resin composition was prepared and a resin sheet was obtained in the same manner as in Example 1, except that 6 parts of polyimide resin D obtained in Synthesis Example 4 was used instead of 2 parts of a phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of MEK with a non-volatile component of 30% by mass and cyclohexanone).
[0229] [Comparative Example 1] A resin composition was prepared and a resin sheet was obtained in the same manner as in Example 1, except that 3 parts of hollow PPE particles ("XX-6655Z" manufactured by Sekisui Plastics Co., Ltd.) were not used.
[0230] [Comparative Example 2] A resin composition was prepared and a resin sheet was obtained in the same manner as in Example 1, except that 3 parts of rubber particles ("Staphyloid AC3816N" manufactured by Aica Kogyo Co., Ltd., average particle size 0.3 μm) were used instead of 3 parts of hollow PPE particles ("XX-6655Z" manufactured by Sekisui Chemical Co., Ltd.).
[0231] [Comparative Example 3] A resin composition was prepared and a resin sheet was obtained in the same manner as in Example 1, except that 3 parts of acrylic particles ("MX-80H3wT" manufactured by Soken Chemical Industries, Ltd., average particle size 0.8 μm) were used instead of 3 parts of hollow PPE particles ("XX-6655Z" manufactured by Sekisui Chemical Industry Co., Ltd.).
[0232] [Comparative Example 4] A resin composition was prepared and a resin sheet was obtained in the same manner as in Example 1, except that 3 parts of styrene particles ("SX-500H" manufactured by Soken Chemical Industries, Ltd., average particle size 5.0 μm) were used instead of 3 parts of hollow PPE particles ("XX-6655Z" manufactured by Sekisui Chemical Industry Co., Ltd.).
[0233] [Comparative Example 5] A resin composition was prepared and a resin sheet was obtained in the same manner as in Example 6, except that 3 parts of hollow PPE particles ("XX-6655Z" manufactured by Sekisui Plastics Co., Ltd.) were not used.
[0234] [Comparative Example 6] A resin composition was prepared and a resin sheet was obtained in the same manner as in Example 7, except that 3 parts of hollow PPE particles ("XX-6655Z" manufactured by Sekisui Plastics Co., Ltd.) were not used.
[0235] <Various evaluation tests> [Test Example 1: Measurement of dielectric tangent (Df)] The resin sheets produced in the Examples and Comparative Examples were heated at 200°C for 90 minutes to thermally cure the resin composition layers, and then the support was peeled off to obtain a cured film formed of the cured product of the resin composition. The cured film was cut into a piece 2 mm wide and 80 mm long to obtain a cured product A for evaluation.
[0236] The dielectric loss tangent (Df value) of the obtained cured product A for evaluation was measured by the cavity resonance perturbation method at a measurement frequency of 5.8 GHz and a measurement temperature of 23° C. using an “HP8362B” manufactured by Agilent Technologies Inc. Measurements were performed on three test pieces, and the average value was calculated.
[0237] [Test Example 2: Evaluation of cracks after desmear treatment (roughening treatment)] As the inner layer substrate, a core material (Hitachi Chemical Co., Ltd. "E705GR", thickness 400 μm) was prepared in which circular copper pads (copper thickness 35 μm) with a diameter of 350 μm were formed in a grid pattern at intervals of 400 μm so that the residual copper rate was 60%. Then, the resin sheets produced in the examples and comparative examples were laminated on both sides of the inner layer substrate using a batch-type vacuum pressure laminator (Nikko Materials Co., Ltd. two-stage build-up laminator "CVP700") so that the resin composition layer was bonded to the inner layer substrate. The lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at a temperature of 100 ° C and a pressure of 0.74 MPa for 30 seconds. Next, the resin composition layer was placed in a 130 ° C oven and heated for 30 minutes, and then transferred to a 170 ° C oven and heated for 30 minutes to thermally cure the resin composition layer to form an insulating layer. After peeling off the support to expose the insulating layer, the obtained substrate was immersed in a swelling liquid (Atotech Japan's "Swelling Dip Securigant P") for 10 minutes at 60°C, then in a roughening liquid (Atotech Japan's "Concentrate Compact P", an aqueous solution of KMnO4: 60g / L and NaOH: 40g / L) for 30 minutes at 80°C, and finally in a neutralizing liquid (Atotech Japan's "Reduction Solution Securigant P") for 5 minutes at 40°C. After the treatment, 100 copper pads of the circuit substrate were observed to check for cracks in the insulating layer, and the results were evaluated according to the following criteria.
[0238] Crack resistance rating criteria: ○: 10 or less cracks △: More than 10 but no more than 20 cracks ×: More than 20 cracks
[0239] [Test Example 3: Measurement of copper foil peel strength after high temperature and high humidity environmental test (HAST)] (1) Copper foil preparation The shiny side of Mitsui Kinzoku's "3EC-III" (electrolytic copper foil, 35μm) was etched with a micro-etching agent (Mech's "CZ8101") to roughen the copper surface by 1μm, and then anti-rust treatment (CL8300) was applied. Furthermore, it was heated in an oven at 130℃ for 30 minutes. This copper foil is called CZ copper foil.
[0240] (2) Preparation of inner layer board Both sides of a glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, substrate thickness 0.4 mm, Panasonic "R1515A") with an inner layer circuit formed were etched 1 μm with a microetching agent (Mec "CZ8101") to roughen the copper surface.
[0241] (3) Preparation of evaluation board The resin sheets obtained in the examples and comparative examples were laminated on both sides of the inner layer substrate so that the resin composition layer was in contact with the inner layer substrate using a batch-type vacuum pressure laminator (two-stage build-up laminator "CVP700" manufactured by Nikko Materials Co., Ltd.). The lamination was performed by reducing the pressure for 30 seconds to adjust the air pressure to 13 hPa or less, and then pressing at 120°C and a pressure of 0.74 MPa for 30 seconds. Next, the sheets were smoothed by hot pressing at 100°C and a pressure of 0.5 MPa for 60 seconds. After smoothing, the support was peeled off. The treated surface of the CZ copper foil was laminated on the exposed resin composition layer under the same conditions as above. Then, the resin composition layer was cured under a curing condition of 200°C for 90 minutes to form an insulating layer, and an evaluation substrate having a structure of CZ copper foil / insulating layer / inner layer substrate / insulating layer / CZ copper foil was produced.
[0242] (4) Measurement of copper foil peel strength after HAST The obtained evaluation board was subjected to a high temperature and high humidity environmental test for 100 hours under the conditions of 130°C and 85% RH using a highly accelerated life tester (Kusumoto Chemical Industries, Ltd., "PM422"). After that, the evaluation board after HAST was cut into small pieces of 150 x 30 mm. A cutter was used to make a 10 mm wide and 100 mm long cut in the copper foil part of the small piece, one end of the cut was peeled off and held with a gripper of a tensile tester (TSE Corporation, "AC-50C-SL"), and the load [kgf / cm] was measured when 35 mm was peeled off vertically at a speed of 50 mm / min at room temperature. The obtained load value was taken as the copper foil peel strength after HAST. The measurement was performed in accordance with JIS C6481.
[0243] [Test Example 4: Evaluation of Undulation] As the inner layer substrate, a core material (Hitachi Chemical Co., Ltd. "E705GR", thickness 400 μm, copper thickness 35 μm) in which circular degassing holes with a diameter of 200 μm were formed in a lattice shape at intervals of 2 mm was prepared. Then, the resin sheets obtained in the examples and comparative examples were laminated on both sides of the inner layer substrate using a batch type vacuum pressure laminator (Nikko Materials Co., Ltd. two-stage build-up laminator "CVP700") so that the resin composition layer was bonded to the inner layer substrate. The lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at a temperature of 100°C and a pressure of 0.74 MPa for 30 seconds. This was placed in an oven at 130°C and heated for 30 minutes, and then transferred to an oven at 170°C and heated for 30 minutes to harden the resin composition layer to form an insulating layer. After peeling off the support to expose the insulating layer, the heights of the top and bottom of the insulating layer were measured using a non-contact surface roughness meter (WYKO NT3300, manufactured by B-CO Instruments) and evaluated according to the following criteria: Undulation was defined as the difference in height (μm) between the top and bottom of the insulating layer.
[0244] Undulation criteria: ○: When undulation is 2μm or less △: When undulation is greater than 2μm and less than 3μm ×: Undulation is larger than 3 μm
[0245] The results of Examples 1 to 9 and Comparative Examples 1 to 6 are shown in Table 1.
[0246] [Table 1]
Claims
1. A resin composition comprising (A) polyphenylene ether particles, (B) an epoxy resin, (C) a curing agent, and (D) an inorganic filler.
2. 2. The resin composition according to claim 1, wherein the average particle size of the component (A) is 5 μm or less.
3. 90% particle size D of component (A) 90 The resin composition according to claim 1, wherein the particle size is 2 μm or less.
4. The resin composition according to claim 1 , wherein the content of the component (A) is 0.5% by mass or more when the resin components of the resin composition are taken as 100% by mass.
5. The resin composition according to claim 1, wherein the component (C) comprises (C-1) one or more curing agents selected from the group consisting of active ester curing agents, cyanate ester curing agents, and carbodiimide curing agents.
6. The resin composition according to claim 5, wherein the mass ratio of the component (C-1) to the component (B) (component (C-1) / component (B)) is 1 or more.
7. The resin composition according to claim 1 , wherein the content of the component (B) is 5% by mass or more when the resin component of the resin composition is 100% by mass.
8. The resin composition according to claim 1, wherein the content of the component (D) is 40% by mass or more when the non-volatile components of the resin composition are taken as 100% by mass.
9. The resin composition according to claim 1 , wherein the component (A) is an emulsion polymer or a suspension polymer.
10. The resin composition according to claim 1 , wherein the component (A) is insoluble in a solvent.
11. The resin composition according to claim 1, which is used for an insulating layer of a circuit board.
12. A resin sheet comprising a support and a layer of the resin composition according to any one of claims 1 to 11 provided on the support.
13. The resin sheet according to claim 12, wherein the support is a thermoplastic resin film or a metal foil.
14. A cured product of the resin composition according to any one of claims 1 to 11.
15. A circuit board comprising an insulating layer made of a cured product of the resin composition according to any one of claims 1 to 11.
16. A semiconductor device comprising the circuit board according to claim 15.
Citation Information
Patent Citations
Flame-retardant curable resin composition
JP2005105009A
Resin composition, prepreg and laminated board using the same
JP2008050526A
Ultrafine poly(phenylene ether) particles and compositions derived therefrom
JP2015522087A
Particulate poly(phenylene ether)-containing varnish compositions, composites, laminates prepared therefrom, and methods of making composites
JP2017534723A
Thermosetting resin composition, and prepreg, metal-clad laminate or printed wiring board using the same
JP2018035217A
Cited By
Resin composition, cured product, resin composite sheet, prepreg, metal foil-clad laminate, printed wiring board, and semiconductor device
WO2026204190A1