Curable composition
The curable composition with quantum dots, polymerizable compounds, and a specific polymerization initiator addresses pattern formation issues in conventional compositions, achieving superior patterning and luminescence intensity.
Patent Information
- Application Number
- JP2023205012
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-23
- Filing Date
- 2023-12-05
- Publication Date
- 2024-10-07
AI Technical Summary
Conventional curable compositions fail to properly form patterns after exposure and development due to improper patterning.
A curable composition comprising quantum dots, a polymerizable compound, and a polymerization initiator, with specific compounds and ratios, including a compound represented by formula (DA) for the polymerization initiator, to enhance patterning properties.
The composition achieves excellent patterning properties, enabling the formation of high-quality patterns even at high quantum dot concentrations, with improved luminescence intensity and dispersibility.
Smart Images

Figure 2024137666000001 
Figure 2024137666000002 
Figure 2024137666000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable composition containing quantum dots, a cured film, and a display device. [Background technology]
[0002] Patent Document 1 describes a curable composition containing quantum dots and an oxime-based polymerization initiator, and a cured film and a display device formed using the curable composition. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2016 / 035603 Summary of the Invention [Problem to be solved by the invention]
[0004] The present inventors have conducted studies and found that a problem may occur in that a pattern after exposure and development is not properly formed according to a mask when using a conventional curable composition. The present invention provides a curable composition capable of properly forming a pattern. [Means for solving the problem]
[0005] The present invention includes the following inventions. [1] A method for producing a photosensitive material comprising the steps of: (A) a quantum dot; (C) a polymerizable compound; and (D) a polymerization initiator; The curable composition, wherein the polymerization initiator (D) comprises a compound represented by formula (DA): [ka] [In the formula, R d1 represents a branched hydrocarbon group having 3 to 20 carbon atoms which may have a substituent. R d2 ~R d5each independently represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. and n represents an integer of 0 to 4. The —CH 2 - may be replaced by -O-, -S-, -CO- or -OCO-. [2] The curable composition according to [1], wherein the polymerizable compound (C) contains a compound (Ca) having three or more ethylenically unsaturated bonds in the molecule and having an acidic functional group. [3] The curable composition according to [1] or [2], further comprising a resin (B). [4] The curable composition according to [3], wherein the acid value of the resin (B) is 30 mgKOH / g or more and 150 mgKOH / g or less, based on the solid content. [5] The curable composition according to [3] or [4], wherein the content of the quantum dots (A) is 30% by mass or more and 150% by mass or less based on the total amount of the resin (B) and the polymerizable compound (C). [6] R d1 The curable composition according to any one of [1] to [5], wherein is a branched saturated hydrocarbon group having 3 to 20 carbon atoms which may have a substituent. [7] R d2 ~R d5 each independently represents a saturated hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or an unsaturated hydrocarbon group having 2 to 20 carbon atoms which may have a substituent. [8] A cured film formed from the curable composition according to any one of [1] to [7]. [9] A display device comprising the cured film according to [8]. Effect of the Invention
[0006] According to the present invention, there is provided a curable composition having excellent patterning properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] <Curable composition> The curable composition according to the present invention contains quantum dots (A), a polymerizable compound (C) and a polymerization initiator (D).
[0008] <Quantum dots (A)> The quantum dots (A) are semiconductor fine particles having a particle diameter of 1 nm to 100 nm, which utilize the band gap of the semiconductor to absorb ultraviolet light or visible light and emit light. Quantum dots (A) include CdO, CdS, CdSe, CdTe, ZnO, ZnS, ZnSe, ZnTe, HgO, HgS, HgSe, HgTe, CdHgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdH Compounds of group 12 elements and group 16 elements, such as GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, InN, InP, InAs, InSb, GaNP, GaNAs, GaPAs, AlNP, AlNAs, AlPAs, InNP, InNAs, InPAs, GaAlNP, GaAlNAs, GaAlPAs, GaInNP, GaInNAs, GaInPAs, InAlNP, InAlNAs, InAlPAs; compounds of group 13 elements and group 15 elements, such as Ga 2 O 3 , Ga 2 S 3 , Ga 2 Se 3 , Ga 2 Te 3 , In 2 O 3 , In 2 S 3 , In 2 Se 3 , In 2 Te 3 Compounds of Group 13 elements and Group 16 elements such as AgInGaS; SnS 2Compounds of group 14 elements and group 16 elements such as SnS, SnSe, SnTe, PdS, PbSe, and PbTe; As 2 O 3 , As 2 S 3 , As 2 Se 3 , As 2 Te 3 , Sb 2 O 3 , Sb 2 S 3 , Sb 2 Se 3 , Sb 2 Te 3 , Bi 2 O 3 , Bi 2 S 3 , Bi 2 Se 3 , Bi 2 Te 3 compounds of Group 15 elements and Group 16 elements such as MgS, MgSe, MgTe, CaS, CaSe, CaTe, SrS, SrSe, SrTe, BaS, BaSe, BaTe; simple substances of Group 14 elements, Group 15 elements, or Group 16 elements such as Si and Ge; and the like.
[0009] When the quantum dots (A) contain S or Se, quantum dots whose surfaces are modified with a metal oxide or an organic substance may be used. By using surface-modified quantum dots, it is possible to prevent S or Se from being extracted by a reactive component that is or may be contained in the curable composition. The quantum dots (A) may also form a core-shell structure by combining the above compounds, such as fine particles having a CdSe core and a ZnS shell, or fine particles having an InP core and a ZnSeS shell.
[0010] Since the energy state of quantum dots (A) depends on their size, it is possible to freely select the emission wavelength by changing the particle diameter. For example, in the case of quantum dots composed only of CdSe, the peak wavelengths of the fluorescence spectrum are 528 nm, 570 nm, 592 nm, and 637 nm when the particle diameters are 2.3 nm, 3.0 nm, 3.8 nm, and 4.6 nm, respectively. In addition, the quantum dots (A) emit light with a narrow spectral width, and by combining light with such a steep peak, the color gamut that can be displayed can be expanded in a display device including a cured film formed from the curable composition. Furthermore, the quantum dots (A) have high responsiveness, and can efficiently utilize the light emitted from the light source.
[0011] The curable composition may contain only one type of quantum dot that emits light of a specific wavelength when exposed to light emitted from a light source, or may contain a combination of two or more types of quantum dots that emit light of different wavelengths. Examples of the light of the specific wavelength include red light, green light, and blue light.
[0012] The content of the quantum dots (A) in the curable composition is, for example, 1 mass% or more and 80 mass% or less, preferably 10 mass% or more and 70 mass% or less, more preferably 15 mass% or more and 60 mass% or less, even more preferably 20 mass% or more and 50 mass% or less, still more preferably 25 mass% or more and 40 mass% or less, and particularly preferably 30 mass% or more and 38 mass% or less, based on the total amount of solids in the curable composition. In this specification, the total amount of solids means the total amount of components contained in the curable composition excluding the solvent (F). The content in the solids of the curable composition can be measured by a known analytical method such as liquid chromatography or gas chromatography.
[0013] The content of the quantum dots (A) is, for example, 30% by mass or more and 150% by mass or less, preferably 45% by mass or more and 120% by mass or less, more preferably 50% by mass or more and 100% by mass or less, even more preferably 60% by mass or more and 90% by mass or less, and even more preferably 65% by mass or more and 85% by mass or less, based on the total amount of the resin (B) and the polymerizable compound (C). The present invention is extremely useful because it can provide a curable composition with excellent patterning properties even when the quantum dots (A) are contained at a high concentration. In addition, by containing the quantum dots (A) at a high concentration in the curable composition, improvement in luminescence intensity can be expected. Note that simply increasing the concentration of the quantum dots (A) may cause the quantum dots (A) to aggregate and become inactivated, resulting in a decrease in luminescence intensity. However, by appropriately adjusting the components and properties of the resin (B), polymerizable compound (C), and organic ligand (G) that can be used in the curable composition described later, the dispersibility of the quantum dots (A) can be increased.
[0014] When the curable composition contains an organic ligand (G), the total content of the quantum dots (A) and the organic ligand (G) is, for example, 35% by mass or more and 160% by mass or less, preferably 50% by mass or more and 140% by mass or less, more preferably 70% by mass or more and 100% by mass or less, even more preferably 80% by mass or more and 98% by mass or less, and even more preferably 88% by mass or more and 95% by mass or less, based on the total amount of the resin (B) and the polymerizable compound (C). The present invention provides a curable composition that has excellent patterning properties even when it contains a high concentration of quantum dots (A).
[0015] <Organic ligand (G)> The curable composition may further contain an organic ligand (G). The organic ligand (G) may be coordinated to the quantum dot (A) in the curable composition, or may be free in the curable composition.
[0016] The semiconductor particles, which are quantum dots (A), are preferably present in the curable composition in a state in which an organic ligand (G) is coordinated. Hereinafter, the semiconductor particles to which the organic ligand (G) is coordinated are also referred to as ligand-containing semiconductor particles. The ligand coordinated to the semiconductor particles can be, for example, an organic compound having a polar group that exhibits coordination ability with respect to the semiconductor particles. The organic ligand (G) may be an organic ligand (G) added due to constraints on the synthesis of the ligand-containing semiconductor particles or for stabilization. For example, in JP-A 2015-529698, the ligand-containing semiconductor particles contain hexanoic acid as the organic ligand (G) from the viewpoint of particle size control, and the organic ligand (G) is replaced with DDSA (dodecenyl succinic acid) for stabilization after synthesis. The organic ligand (G) can be coordinated, for example, to the surface of the semiconductor particle.
[0017] Examples of polar groups include thiol groups (-SH), carboxyl groups (-COOH), and amino groups (-NH 2 ) is preferably at least one group selected from the group consisting of. A polar group selected from this group can be advantageous in enhancing coordination with semiconductor particles. High coordination can contribute to improving color unevenness of the cured film and / or improving the patterning properties of the curable composition. In particular, from the viewpoint of obtaining a cured film (such as a wavelength conversion film) having superior light-emitting properties, it is more preferable that the polar group is at least one group selected from the group consisting of a thiol group and a carboxy group. The organic ligand (G) can have one or more polar groups.
[0018] The organic ligand (G) is, for example, a compound represented by the following formula (X): X A -R X (X) In the formula, X A is the polar group as above, and R Xis a monovalent hydrocarbon group which may contain a heteroatom (N, O, S, halogen atom, etc.). The hydrocarbon group may have one or more unsaturated bonds such as a carbon-carbon double bond. The hydrocarbon group may have a linear, branched, or cyclic structure. The number of carbon atoms in the hydrocarbon group is, for example, 1 to 40, and may be 1 to 30. The methylene group contained in the hydrocarbon group may be substituted with -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -C(=O)-NH-, -NH-, etc.
[0019] base R X may contain a polar group. Specific examples of the polar group include the polar group X A Reference is made to the above description.
[0020] polar group X A Specific examples of the organic ligand (G) having a carboxyl group as a carboxyl group include formic acid, acetic acid, and propionic acid, as well as saturated or unsaturated fatty acids. Specific examples of the saturated or unsaturated fatty acids include saturated fatty acids such as butyric acid, pentanoic acid, caproic acid, caprylic acid, capric acid, lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, arachidic acid, behenic acid, and lignoceric acid; monounsaturated fatty acids such as myristoleic acid, palmitoleic acid, oleic acid, icosenoic acid, erucic acid, and nervonic acid; and polyunsaturated fatty acids such as linoleic acid, α-linolenic acid, γ-linolenic acid, stearic acid, dihomo-γ-linolenic acid, arachidonic acid, eicosatetraenoic acid, docosadienoic acid, and adrenic acid (docosatetraenoic acid).
[0021] polar group X A Specific examples of the organic ligand (G) having a thiol group or an amino group as the polar group X include the above-exemplified organic ligands A The organic ligand (G) includes an organic ligand (G) in which the carboxy group of the organic ligand (G) having a carboxy group is replaced with a thiol group or an amino group.
[0022] Preferred examples of the organic ligand (G) represented by the above formula (X) include the compounds (J-1) and (J-2).
[0023] [Compound (J-1)] The compound (J-1) is a compound having a first functional group and a second functional group. The first functional group is a carboxy group (-COOH), and the second functional group is a carboxy group or a thiol group (-SH). Since the compound (J-1) has a carboxy group and / or a thiol group, it can be a ligand that coordinates to the quantum dot (A). The curable composition may contain only one type of compound (J-1), or may contain two or more types.
[0024] By including the compound (J-1) in the curable composition, the development speed of the curable composition can be sufficiently increased, and the luminescence intensity of the cured film formed from the curable composition can be increased. This is believed to be because both the carboxy group and the thiol group of the compound (J-1) can impart high developability with an alkaline developer to the curable composition, and can be well coordinated to the quantum dots (A) to increase the dispersibility of the quantum dots (A) in the curable composition. In particular, the carboxy group has a higher effect of increasing the developability with an alkaline developer, and the thiol group has a higher effect of increasing the dispersibility of the quantum dots (A).
[0025] Increasing the development speed of the curable composition can also contribute to increasing the luminescence intensity of the cured film, which is believed to be because it can reduce the penetration of water into the cured film during the development process.
[0026] An example of the compound (J-1) is a compound represented by the following formula (J-1a): The compound (J-1) may be an acid anhydride of the compound represented by formula (J-1a).
[0027] [ka] [In the formula, R B represents a divalent hydrocarbon group. BWhen present, they may be the same or different. The above-mentioned hydrocarbon group may have one or more substituents. When a plurality of substituents are present, they may be the same or different, and they may be bonded to each other to form a ring together with the atom to which they are bonded. The -CH contained in the above-mentioned hydrocarbon group 2 - is -O-, -S-, -SO 2 It may be replaced by at least one of -, -CO- and -NH-. and p represents an integer of 1 to 10.
[0028] R B Examples of the divalent hydrocarbon group represented by the formula (I) include a chain hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group.
[0029] Examples of the chain hydrocarbon group include linear or branched alkanediyl groups, and the number of carbon atoms therein is usually 1-50, preferably 1-20, and more preferably 1-10. Examples of linear or branched alkanediyl groups include a propane-1,2-diyl group, a propane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a nonane-1,9-diyl group, a decane-1,10-diyl group, an undecane-1,11-diyl group, a dodecane-1,12-diyl group, a propane-1,2-diyl group, a 1-methylbutane-1,3-diyl group, a 2-methylpropane-1,3-diyl group, a pentane-1,4-diyl group, and a 2-methylbutane-1,4-diyl group.
[0030] Examples of the alicyclic hydrocarbon group include monocyclic or polycyclic cycloalkanediyl groups, and the number of carbon atoms therein is usually 3 to 50, preferably 3 to 20, and more preferably 3 to 10. Examples of the monocyclic or polycyclic cycloalkanediyl group include a cyclobutane-1,3-diyl group, a cyclopentane-1,3-diyl group, a cyclohexane-1,4-diyl group, a norbornane-1,4-diyl group, a norbornane-2,3-diyl group, a norbornane-2,5-diyl group, a 5-norbornene-2,3-diyl group, an adamantane-1,5-diyl group, and an adamantane-2,6-diyl group.
[0031] An example of the aromatic hydrocarbon group is an arenediyl group, the number of carbon atoms of which is usually 6 to 20. Examples of the monocyclic or polycyclic arenediyl group include a benzenediyl group, a naphthalenediyl group, an anthracenediyl group, a phenanthrenediyl group, a pyrenediyl group, a pyridinediyl group, a pyrazinediyl group, and a pyrazolediyl group.
[0032] Examples of the substituent that the above-mentioned hydrocarbon group may have include an alkyl group having 1 to 50 carbon atoms, a cycloalkyl group having 3 to 50 carbon atoms, an aryl group having 6 to 20 carbon atoms, a carboxy group, an amino group, and a halogen atom.
[0033] Examples of the alkyl group having 1 to 50 carbon atoms include saturated or unsaturated linear or branched alkyl groups, specifically, methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, and 2-ethylhexyl groups.
[0034] Examples of the cycloalkyl group having 3 to 50 carbon atoms include a cyclopropyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group.
[0035] Examples of the aryl group having 6 to 20 carbon atoms include a phenyl group, a biphenyl group, a tolyl group, a xylyl group, an ethylphenyl group, and a naphthyl group.
[0036] Examples of halogen atoms include fluorine, chlorine, bromine and iodine atoms.
[0037] The substituent that the above-mentioned hydrocarbon group may have is preferably a carboxy group, an amino group or a halogen atom.
[0038] The -CH contained in the above hydrocarbon group 2 When - is replaced with at least one of -O-, -CO- and -NH-, -CH 2 The - is preferably replaced by at least one of -CO- and -NH-, and more preferably by -NH-. p is preferably 1 or 2.
[0039] Examples of the compound represented by formula (J-1a) include compounds represented by the following formulas (1-1) to (1-9).
[0040] [ka]
[0041] Specific examples of the compound represented by formula (J-1a) by chemical name include mercaptoacetic acid, 2-mercaptopropionic acid, 3-mercaptopropionic acid, 3-mercaptobutanoic acid, 4-mercaptobutanoic acid, mercaptosuccinic acid, mercaptostearic acid, mercaptooctanoic acid, 4-mercaptobenzoic acid, 2,3,5,6-tetrafluoro-4-mercaptobenzoic acid, L-cysteine, N-acetyl-L-cysteine, 3-methoxybutyl 3-mercaptopropionate, and 3-mercapto-2-methylpropionic acid. Of these, 3-mercaptopropionic acid and mercaptosuccinic acid are preferred.
[0042] Another example of the compound (J-1) is a polycarboxylic acid compound, preferably a compound (J-1b) represented by the above formula (J-1a) in which -SH in the formula (J-1a) is replaced with a carboxy group (-COOH).
[0043] Examples of the compound (J-1b) include the following compounds. Succinic acid, glutaric acid, adipic acid, octafluoroadipic acid, azelaic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, dodecafluorosuberic acid, 3-ethyl-3-methylglutaric acid, hexafluoroglutaric acid, trans-3-hexenedioic acid, sebacic acid, hexadecafluorosebacic acid, acetylenedicarboxylic acid, trans-aconitic acid, 1,3-adamantanedicarboxylic acid, bicyclo[2.2.2]octane-1,4-dicarboxylic acid, cis-4-cyano Cyclohexene-1,2-dicarboxylic acid, 1,1-cyclopropanedicarboxylic acid, 1,1-cyclobutanedicarboxylic acid, cis- or trans-1,3-cyclohexanedicarboxylic acid, cis- or trans-1,4-cyclohexanedicarboxylic acid, 1,1-cyclopentanediacetic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, decahydro-1,4-naphthalenedicarboxylic acid, 2,3-norbornanedicarboxylic acid, 5-norbornene-2,3-dicarboxylic acid, phthalic acid, 3-fluorophthalic acid, isophthalic acid, tetrafluoroisophthalic acid Phthalic acid, terephthalic acid, tetrafluoroterephthalic acid, 2,5-dimethylterephthalic acid, 2,6-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,1'-ferrocenedicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 2,5-furandicarboxylic acid, benzophenone-2,4'-dicarboxylic acid monohydrate, benzophenone-4,4'-dicarboxylic acid, 2,3-pyrazinedicarboxylic acid, 2,3-pyridinedicarboxylic acid, 2,4-pyridinedicarboxylic acid, 3,5-Pyridinedicarboxylic acid, 2,5-Pyridinedicarboxylic acid, 2,6-Pyridinedicarboxylic acid, 3,4-Pyridinedicarboxylic acid, Pyrazole-3,5-dicarboxylic acid monohydrate, 4,4'-Stilbenedicarboxylic acid, Anthraquinone-2,3-dicarboxylic acid, 4-(carboxymethyl)benzoic acid, Chelidonic acid monohydrate, Azobenzene-4,4'-dicarboxylic acid, Azobenzene-3,3'-dicarboxylic acid, Chlorendic acid, 1H-Imidazole-4,5-dicarboxylic acid, 2,2-Bis(4-carboxyphenyl)hexafluoropropane, 1,10-bis(4-carboxyphenoxy)decane, dipropylmalonic acid, dithiodiglycolic acid, 3,3'-dithiodipropionic acid, 4,4'-dithiodibutanoic acid, 4,4'-dicarboxydiphenyl ether, 4,4'-dicarboxydiphenyl sulfone, ethylene glycol bis(4-carboxyphenyl)ether, 3,4-ethylenedioxythiophene-2,5-dicarboxylic acid, 4,4'-isopropylidenediphenoxyacetic acid, 1,3-acetonedicarboxylic acid, methylenedisalicylic acid, 5,5'-thiodisalicylic acid, tris(2-carboxyethyl)isocyanurate, tetrafluorosuccinic acid, α,α,α',α'-tetramethyl-1,3-benzenedipropionic acid, 1,3,5-benzenetricarboxylic acid, etc.
[0044] From the viewpoint of increasing the development speed of the curable composition and increasing the luminescence intensity of the cured film, the molecular weight of the compound (J-1) is preferably 3000 or less, more preferably 2000 or less, even more preferably 1000 or less, still more preferably 800 or less, and particularly preferably 500 or less. The molecular weight of the compound (J-1) is usually 100 or more.
[0045] The molecular weight may be a number average molecular weight or a weight average molecular weight, where the number average molecular weight and the weight average molecular weight are the number average molecular weight and the weight average molecular weight, respectively, measured by gel permeation chromatography (GPC) in terms of standard polystyrene.
[0046] In the curable composition, it is preferable that at least a part of the molecules of the compound (J-1) are coordinated to the quantum dot (A), and all or almost all of the molecules may be coordinated to the quantum dot (A). That is, the curable composition preferably contains the compound (J-1) coordinated to the quantum dot (A), but may contain the compound (J-1) that is not coordinated to the quantum dot (A) together with the compound (J-1) coordinated to the quantum dot (A). The inclusion of the compound (J-1) coordinated to the quantum dot (A) can be advantageous in terms of increasing the development speed of the curable composition and increasing the luminescence intensity of the cured film. The compound (J-1) can usually be coordinated to the quantum dot (A) via the first functional group and / or the second functional group. The compound (J-1) can be coordinated to, for example, the surface of the quantum dot (A).
[0047] The content ratio of the compound (J-1) to the quantum dot (A) in the curable composition is, in mass ratio, preferably 0.001 to 1, more preferably 0.01 to 0.5, and even more preferably 0.02 to 0.1. When the content ratio is within this range, it can be advantageous from the viewpoint of increasing the development speed of the curable composition and the viewpoint of increasing the luminescence intensity of the cured film.
[0048] From the viewpoint of increasing the development speed of the curable composition and increasing the luminescence intensity of the cured film, the content of compound (J-1) in the curable composition is preferably from 0.1 mass % to 20 mass % relative to the total amount of solids in the curable composition, more preferably from 0.1 mass % to 10 mass %, even more preferably from 0.2 mass % to 8 mass %, still more preferably from 0.2 mass % to 5 mass %, and particularly preferably from 0.5 mass % to 4 mass %.
[0049] [Compound (J-2)] Compound (J-2) is a compound (J-2) different from compound (J-1), which contains a polyalkylene glycol structure and has a polar group at the molecular end. The molecular end is preferably the end of the longest carbon chain (the carbon atom in the carbon chain may be replaced with another atom such as an oxygen atom) in compound (J-2). The curable composition may contain only one type of compound (J-2), or may contain two or more types. The compound containing a polyalkylene glycol structure and having the above-mentioned first functional group and second functional group is considered to belong to the compound (J-1).
[0050] From the viewpoint of increasing the development rate of the curable composition and the viewpoint of increasing the luminescence intensity of the cured film, the curable composition may contain the compound (J-1), or may contain the compound (J-1) and the compound (J-2).
[0051] The polyalkylene glycol structure is represented by the following formula:
[0052] [ka]
[0053] (n is an integer of 2 or more). In the formula, R C is an alkylene group, for example, an ethylene group, a propylene group, etc. A specific example of the compound (J-2) is a polyalkylene glycol compound represented by the following formula (J-2a).
[0054] [ka]
[0055] In formula (J-2a), X is a polar group, Y is a monovalent group, and Z C is a divalent or trivalent group. n is an integer of 2 or more. m is 1 or 2. R C is an alkylene group.
[0056] In the curable composition, at least a part of the molecules of the compound (J-2) are preferably coordinated to the quantum dot (A), and all or almost all of the molecules may be coordinated to the quantum dot (A). That is, the curable composition preferably contains the compound (J-2) coordinated to the quantum dot (A), but may contain the compound (J-2) that is not coordinated to the quantum dot (A) together with the compound (J-2) coordinated to the quantum dot (A). It may be advantageous to include the compound (J-2) coordinated to the quantum dot (A) in terms of increasing the development speed of the curable composition and increasing the luminescence intensity of the cured film. The compound (J-2a) can usually be coordinated to the quantum dot (A) via the polar group X. When the group Y contains a polar group, the compound (J-2a) can also be coordinated to the quantum dot (A) via the polar group of the group Y, or via the polar groups of the polar group X and the group Y. The compound (J-2) can be coordinated, for example, to the surface of the quantum dot (A).
[0057] The polar group X is preferably at least one group selected from the group consisting of a thiol group (-SH), a carboxyl group (-COOH) and an amino group (-NH2). The polar group selected from the group can be advantageous in increasing the coordination with the quantum dot (A). Among them, from the viewpoint of increasing the luminescence intensity of the cured film, it is more preferable that the polar group X is at least one group selected from the group consisting of a thiol group and a carboxyl group.
[0058] The group Y is a monovalent group. The group Y is not particularly limited, and may be a monovalent hydrocarbon group which may have a substituent (N, O, S, halogen atom, etc.). The -CH 2 - may be substituted by -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -C(=O)-NH-, -NH-, or the like.
[0059] The number of carbon atoms in the hydrocarbon group is, for example, from 1 to 12. The hydrocarbon group may have an unsaturated bond. Examples of the group Y include an alkyl group having 1 to 12 carbon atoms and a linear, branched, or cyclic structure; and an alkoxy group having 1 to 12 carbon atoms and a linear, branched, or cyclic structure. The number of carbon atoms in the alkyl group and alkoxy group is preferably 1 to 8, more preferably 1 to 6, and even more preferably 1 to 4. The -CH 2- may be substituted by -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -C(=O)-NH-, -NH-, etc. Among these, the group Y is preferably a linear or branched alkoxy group having 1 to 4 carbon atoms, and more preferably a linear alkoxy group having 1 to 4 carbon atoms.
[0060] The group Y may contain a polar group, such as a thiol group (-SH), a carboxyl group (-COOH), or an amino group (-NH 2 ) is at least one group selected from the group consisting of. However, as described above, the compound containing the polyalkylene glycol structure and having the first functional group and the second functional group is considered to belong to the compound (J-1). The polar group is preferably located at the end of the group Y.
[0061] Base Z C is a divalent or trivalent radical. The radical Z C is not particularly limited, and examples thereof include divalent or trivalent hydrocarbon groups which may contain heteroatoms (N, O, S, halogen atoms, etc.). The number of carbon atoms in the hydrocarbon group is, for example, 1 to 24. The hydrocarbon group may have an unsaturated bond.
[0062] The divalent group Z C Examples of the alkyl group include an alkylene group having a linear, branched or cyclic structure and a carbon number of 1 to 24; an alkenylene group having a linear, branched or cyclic structure and a carbon number of 1 to 24. The number of carbon atoms in the alkyl group and the alkenylene group is preferably 1 to 12, more preferably 1 to 8, and further preferably 1 to 4. The -CH 2 - may be substituted by -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -C(=O)-NH-, -NH-, etc. C Examples of the divalent group Z C Examples of groups obtained by removing one hydrogen atom from the above include:
[0063] Base Z C may have a branched structure. C may have a polyalkylene glycol structure other than the polyalkylene glycol structure represented by the above formula (J-2a) in a branched chain other than the branched chain containing the polyalkylene glycol structure represented by the above formula (J-2a).
[0064] Among them, the group Z C is preferably a linear or branched alkylene group having 1 or more and 6 or less carbon atoms, and more preferably a linear alkylene group having 1 or more and 4 or less carbon atoms.
[0065] R C is an alkylene group, preferably a linear or branched alkylene group having 1 or more and 6 or less carbon atoms, and more preferably a linear alkylene group having 1 or more and 4 or less carbon atoms.
[0066] In formula (J-2a), n is an integer of 2 or more, preferably 2 or more and 540 or less, more preferably 2 or more and 120 or less, and further preferably 2 or more and 60 or less.
[0067] The molecular weight of compound (J-2) may be, for example, about 150 or more and 10,000 or less. From the viewpoint of increasing the development rate of the curable composition and increasing the luminescence intensity of the cured film, the molecular weight is preferably 150 or more and 5,000 or less, and more preferably 150 or more and 4,000 or less.
[0068] The molecular weight may be a number average molecular weight or a weight average molecular weight, where the number average molecular weight and the weight average molecular weight are the number average molecular weight and the weight average molecular weight, respectively, measured by GPC in terms of standard polystyrene.
[0069] The content ratio of the compound (J-2) to the quantum dots (A) in the curable composition is, in terms of mass ratio, preferably from 0.001 to 2, more preferably from 0.01 to 1.5, and even more preferably from 0.1 to 1. When the content ratio is within this range, it can be advantageous from the viewpoint of increasing the development speed of the curable composition and from the viewpoint of increasing the luminescence intensity of the cured film.
[0070] When the curable composition contains an organic ligand (G), the ratio of the content of the organic ligand (G) to the quantum dot (A) in the curable composition is preferably 0.001 to 1, more preferably 0.01 to 0.8, and even more preferably 0.02 to 0.5, in terms of mass ratio. When the content ratio is within this range, it can be advantageous in terms of improving the stability and dispersibility of the quantum dot (A) and the luminescence intensity of the cured film. The content of the organic ligand (G) referred to here is the total content of all organic ligands contained in the curable composition.
[0071] When the curable composition contains an organic ligand (G), the total content of the quantum dots (A) and the organic ligand (G) in the curable composition is, from the viewpoint of improving the stability and dispersibility of the quantum dots (A) and the luminescence intensity of the cured film, preferably 10% by mass or more and 75% by mass or less, more preferably 20% by mass or more and 70% by mass or less, even more preferably 30% by mass or more and 65% by mass or less, and still more preferably 35% by mass or more and 50% by mass or less, based on the total amount of solids in the curable composition.
[0072] <Resin (B)> The curable composition may further contain a resin (B). Examples of the resin (B) include the following resins [K1] to [K5]. Resin [K1]: a copolymer having a structural unit derived from at least one monomer (a) (hereinafter also referred to as "(a)") selected from the group consisting of unsaturated carboxylic acids and unsaturated carboxylic anhydrides, and a structural unit derived from a monomer (c) (however different from (a)) (hereinafter also referred to as "(c)") copolymerizable with (a); Resin [K2]: a copolymer having a structural unit derived from the above (a) to which a monomer (b) (hereinafter also referred to as "(b)") having a cyclic ether structure having 2 to 4 carbon atoms and an ethylenically unsaturated bond has been added, and a structural unit derived from the above (c); Resin [K3]: a copolymer having a structural unit derived from the (b) to which the (a) has been added, and a structural unit derived from the (c); Resin [K4]: a copolymer having a structural unit obtained by adding the structural unit derived from the (a) to the structural unit derived from the (b) and further ester-bonding a carboxylic acid anhydride, and a structural unit derived from the (c); Resin [K5]: A copolymer having a structural unit obtained by adding the (a) to a structural unit derived from the (b) and further ester-bonding a carboxylic acid anhydride, and a structural unit derived from the (c).
[0073] Examples of (a) include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, o-, m-, and p-vinylbenzoic acid; Unsaturated dicarboxylic acids such as maleic acid, fumaric acid, citraconic acid, mesaconic acid, itaconic acid, 3-vinylphthalic acid, 4-vinylphthalic acid, 3,4,5,6-tetrahydrophthalic acid, 1,2,3,6-tetrahydrophthalic acid, dimethyltetrahydrophthalic acid, and 1,4-cyclohexenedicarboxylic acid; Bicyclounsaturated compounds containing a carboxy group, such as methyl-5-norbornene-2,3-dicarboxylic acid, 5-carboxybicyclo[2.2.1]hept-2-ene, 5,6-dicarboxybicyclo[2.2.1]hept-2-ene, 5-carboxy-5-methylbicyclo[2.2.1]hept-2-ene, 5-carboxy-5-ethylbicyclo[2.2.1]hept-2-ene, 5-carboxy-6-methylbicyclo[2.2.1]hept-2-ene, 5-carboxy-6-ethylbicyclo[2.2.1]hept-2-ene, etc. Unsaturated dicarboxylic acid anhydrides such as maleic anhydride, citraconic anhydride, itaconic anhydride, 3-vinylphthalic anhydride, 4-vinylphthalic anhydride, 3,4,5,6-tetrahydrophthalic anhydride, 1,2,3,6-tetrahydrophthalic anhydride, dimethyltetrahydrophthalic anhydride, 5,6-dicarboxybicyclo[2.2.1]hept-2-ene anhydride, etc.; Unsaturated mono[(meth)acryloyloxyalkyl] esters of divalent or higher polyvalent carboxylic acids, such as mono[2-(meth)acryloyloxyethyl] succinate and mono[2-(meth)acryloyloxyethyl] phthalate; Examples include unsaturated (meth)acrylates containing a hydroxy group and a carboxy group in the same molecule, such as α-(hydroxymethyl)(meth)acrylic acid. Among these, (meth)acrylic acid, maleic anhydride, etc. are preferred from the standpoint of copolymerization reactivity and solubility of the resulting resin in an alkaline aqueous solution. In this specification, (meth)acrylic acid means acrylic acid and / or methacrylic acid. The same applies to "(meth)acryloyl", "(meth)acrylate", etc.
[0074] (b) is, for example, a monomer having a cyclic ether structure having 2 to 4 carbon atoms (for example, at least one selected from the group consisting of an oxirane ring, an oxetane ring, and a tetrahydrofuran ring) and an ethylenically unsaturated bond. (b) is preferably a monomer having a cyclic ether structure having 2 to 4 carbon atoms and a (meth)acryloyloxy group.
[0075] Examples of (b) include glycidyl (meth)acrylate, β-methyl glycidyl (meth)acrylate, β-ethyl glycidyl (meth)acrylate, glycidyl vinyl ether, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether, α-methyl-o-vinylbenzyl glycidyl ether, α-methyl-m-vinylbenzyl glycidyl ether, α-methyl-p-vinylbenzyl glycidyl ether, 2,3-bis(glycidyloxymethyl)styrene, and the like. Monomers having an oxirane ring and an ethylenically unsaturated bond, such as styrene, 2,4-bis(glycidyloxymethyl)styrene, 2,5-bis(glycidyloxymethyl)styrene, 2,6-bis(glycidyloxymethyl)styrene, 2,3,4-tris(glycidyloxymethyl)styrene, 2,3,5-tris(glycidyloxymethyl)styrene, 2,3,6-tris(glycidyloxymethyl)styrene, 3,4,5-tris(glycidyloxymethyl)styrene, and 2,4,6-tris(glycidyloxymethyl)styrene; Monomers having an oxetane ring and an ethylenically unsaturated bond, such as 3-methyl-3-methacryloyloxymethyloxetane, 3-methyl-3-acryloyloxymethyloxetane, 3-ethyl-3-methacryloyloxymethyloxetane, 3-ethyl-3-acryloyloxymethyloxetane, 3-methyl-3-methacryloyloxyethyloxetane, 3-methyl-3-acryloyloxyethyloxetane, 3-ethyl-3-methacryloyloxyethyloxetane, and 3-ethyl-3-acryloyloxyethyloxetane; Examples of the monomer include a monomer having a tetrahydrofuran ring and an ethylenically unsaturated bond, such as tetrahydrofurfuryl acrylate (for example, Viscoat V#150, manufactured by Osaka Organic Chemical Industry Co., Ltd.) and tetrahydrofurfuryl methacrylate. A monomer having an oxirane ring and an ethylenically unsaturated bond is preferred as (b) since the reactivity during production of the resins [K2] to [K5] is high and unreacted (b) is unlikely to remain.
[0076] Examples of (c) include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-methylcyclohexyl (meth)acrylate, tricyclo[5.2.1.0 2,6 ]decan-8-yl(meth)acrylate (commonly known in the art as "dicyclopentanyl(meth)acrylate" and sometimes called "tricyclodecyl(meth)acrylate"), tricyclo[5.2.1.0 2,6 ]Decen-8-yl(meth) (meth)acrylic acid esters such as acrylate (commonly referred to as "dicyclopentenyl (meth)acrylate" in the technical field), dicyclopentanyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, allyl (meth)acrylate, propargyl (meth)acrylate, phenyl (meth)acrylate, naphthyl (meth)acrylate, and benzyl (meth)acrylate; hydroxy group-containing (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; dicarboxylic acid diesters such as diethyl maleate, diethyl fumarate, and diethyl itaconate; Bicyclo[2.2.1]hept-2-ene, 5-methylbicyclo[2.2.1]hept-2-ene, 5-ethylbicyclo[2.2.1]hept-2-ene, 5-hydroxybicyclo[2.2.1]hept-2-ene, 5-hydroxymethylbicyclo[2.2.1]hept-2-ene, 5-(2'-hydroxyethyl)bicyclo[2.2.1]hept-2-ene, 5-methoxybicyclo[2.2.1]hept-2-ene Cyclo[2.2.1]hept-2-ene, 5-ethoxybicyclo[2.2.1]hept-2-ene, 5,6-dihydroxybicyclo[2.2.1]hept-2-ene, 5,6-di(hydroxymethyl)bicyclo[2.2.1]hept-2-ene, 5,6-di(2'-hydroxyethyl)bicyclo[2.2.1]hept-2-ene, 5,6-dimethoxybicyclo[2.2.1]hept 5-hydroxy-5-methylbicyclo[2.2.1]hept-2-ene, 5-hydroxy-5-ethylbicyclo[2.2.1]hept-2-ene, 5-hydroxymethyl-5-methylbicyclo[2.2.1]hept-2-ene, 5-tert-butoxycarbonylbicyclo[2.2.1]hept-2-ene, 5,6-diethoxybicyclo[2.2.1]hept-2-ene, 5-hydroxy-5-methylbicyclo[2.2.1]hept-2-ene, 5-tert-butoxycarbonylbicyclo[2.2.1]hept-2-ene, bicyclounsaturated compounds such as -ene, 5-cyclohexyloxycarbonylbicyclo[2.2.1]hept-2-ene, 5-phenoxycarbonylbicyclo[2.2.1]hept-2-ene, 5,6-bis(tert-butoxycarbonyl)bicyclo[2.2.1]hept-2-ene, and 5,6-bis(cyclohexyloxycarbonyl)bicyclo[2.2.1]hept-2-ene; dicarbonyl imide derivatives such as N-phenylmaleimide, N-cyclohexylmaleimide, N-benzylmaleimide, N-succinimidyl-3-maleimidobenzoate, N-succinimidyl-4-maleimidobutyrate, N-succinimidyl-6-maleimidocaproate, N-succinimidyl-3-maleimidopropionate, and N-(9-acridinyl)maleimide; Examples of the copolymer include styrene, α-methylstyrene, m-methylstyrene, p-methylstyrene, vinyltoluene, p-methoxystyrene, acrylonitrile, methacrylonitrile, vinyl chloride, vinylidene chloride, acrylamide, methacrylamide, vinyl acetate, 1,3-butadiene isoprene, and 2,3-dimethyl-1,3-butadiene. Among these, methyl (meth)acrylate, tricyclo[5.2.1.0]acrylate, and tricyclo[5.2.1.0]acrylate are preferred from the viewpoints of copolymerization reactivity and heat resistance of resin (B). 2,6 ]Decan-8-yl(meth)acrylate (dicyclopentanyl(meth)acrylate), styrene, vinyltoluene, N-phenylmaleimide, N-cyclohexylmaleimide, N-benzylmaleimide, bicyclo[2.2.1]hept-2-ene, and the like are preferred.
[0077] In the resin [K1], the ratio of structural units derived from each of them is as follows among all structural units constituting the resin [K1]: Structural units derived from (a): 2 mol % or more and 60 mol % or less Structural units derived from (c): 40 mol % or more and 98 mol % or less It is preferred that Structural units derived from (a): 10 mol % or more and 50 mol % or less Structural units derived from (c): 50 mol % or more and 90 mol % or less It is more preferable that: When the ratio of the structural units in the resin [K1] is within the above range, the storage stability of the curable composition, the developability when forming a cured pattern, and the solvent resistance of the obtained cured pattern tend to be excellent. In this specification, the term "cured pattern" refers to one aspect of a cured film, and refers to a cured film formed in a pattern.
[0078] Resin [K1] can be produced, for example, by referring to the method described in the literature "Experimental Methods of Polymer Synthesis" (written by Takayuki Otsu, published by Kagaku Dojin Co., Ltd., 1st edition, 1st printing, published on March 1, 1972) and the cited references described in said literature.
[0079] Specifically, a method in which predetermined amounts of (a) and (c), a polymerization initiator, a solvent, and the like are placed in a reaction vessel, and the atmosphere is made deoxygenated, for example, by replacing oxygen with nitrogen, and the mixture is heated and kept warm while being stirred, can be mentioned. The polymerization initiator and the solvent used here are not particularly limited, and those generally used in the field can be used. For example, the polymerization initiator can be an azo compound (2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile) etc.) or an organic peroxide (benzoyl peroxide etc.), and the solvent can be any one that dissolves each monomer, and can be the solvent described below as the solvent (F) that may be included in the curable composition of the present invention.
[0080] The obtained copolymer may be used as a solution after the reaction as it is, or may be used as a concentrated or diluted solution, or may be used as a solid (powder) extracted by a method such as reprecipitation. If a solvent (F) described later is used as a solvent during polymerization, the solution after the reaction can be used as it is for preparation of a curable composition, and therefore the production process of the curable composition can be simplified.
[0081] Resin [K2] can be produced by adding a cyclic ether having 2 to 4 carbon atoms contained in (b) to a carboxylic acid and / or a carboxylic acid anhydride contained in (a) to a copolymer of (a) and (c). First, a copolymer of (a) and (c) is produced in the same manner as described for the production method of resin [K1]. In this case, the ratio of the structural units derived from each is preferably the same as that described for resin [K1].
[0082] Next, a part of the carboxylic acid and / or carboxylic acid anhydride derived from (a) in the copolymer is reacted with a cyclic ether having 2 to 4 carbon atoms contained in (b). Following the production of the copolymer of (a) and (c), the atmosphere in the flask is replaced with air from nitrogen, and (b) is reacted in the presence of a reaction catalyst (e.g., an organic phosphorus compound, a metal complex, an amine compound, etc.) between a carboxylic acid or a carboxylic acid anhydride and a cyclic ether, and a polymerization inhibitor (e.g., hydroquinone, etc.) at 60°C or higher and 130°C or lower for 1 to 10 hours, to produce a resin [K2].
[0083] The amount of (b) used is preferably 5 to 80 mol, more preferably 10 to 75 mol, relative to 100 mol of (a). By using this range, the storage stability of the curable composition, the developability when forming a cured pattern, and the balance of the solvent resistance, heat resistance, mechanical strength, and sensitivity of the obtained cured pattern tend to be good.
[0084] As the organic phosphorus compound as the reaction catalyst, for example, triphenylphosphine can be used. As the amine compound as the reaction catalyst, for example, aliphatic tertiary amine compound or aliphatic quaternary ammonium salt compound can be used, and specific examples thereof include tris(dimethylaminomethyl)phenol, triethylamine, tetrabutylammonium bromide, tetrabutylammonium chloride, etc. From the viewpoint of developability and luminescence intensity of the cured film, the reaction catalyst is preferably an organic phosphorus compound.
[0085] The amount of the reaction catalyst used is preferably 0.001 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the total amount of (a), (b) and (c). The amount of the polymerization inhibitor used is preferably 0.001 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the total amount of (a), (b) and (c).
[0086] The reaction conditions such as the charging method, reaction temperature and time can be appropriately adjusted in consideration of the production equipment, the amount of heat generated by the polymerization, etc. As with the polymerization conditions, the charging method and reaction temperature can be appropriately adjusted in consideration of the production equipment, the amount of heat generated by the polymerization, etc.
[0087] Resin [K3] is produced in the first step by the same method as the above-mentioned resin [K1] to obtain a copolymer of (b) and (c). As in the above, the obtained copolymer may be used as it is in the form of a solution after the reaction, or may be a concentrated or diluted solution, or may be extracted as a solid (powder) by a method such as reprecipitation.
[0088] The ratios of the structural units derived from (b) and (c) to the total number of moles of all structural units constituting the copolymer are, respectively, Structural units derived from (b): 5 mol % or more and 95 mol % or less Structural units derived from (c): 5 mol % or more and 95 mol % or less It is preferred that Structural units derived from (b): 10 mol % or more and 90 mol % or less Structural units derived from (c): 10 mol % or more and 90 mol % or less It is more preferable that:
[0089] Resin [K3] can be obtained by reacting a cyclic ether derived from (b) contained in a copolymer of (b) and (c) with a carboxylic acid or carboxylic anhydride contained in (a) under the same conditions as in the production method of resin [K2]. The amount of (a) used to react with the copolymer is preferably 5 moles or more and 80 moles or less per 100 moles of (b).
[0090] Resin [K4] is a resin obtained by further reacting resin [K2] with a carboxylic acid anhydride. The hydroxyl group generated by the reaction of a carboxylic acid or a carboxylic acid anhydride with a cyclic ether is reacted with a carboxylic acid anhydride. Examples of carboxylic acid anhydrides include maleic anhydride, citraconic anhydride, itaconic anhydride, 3-vinylphthalic anhydride, 4-vinylphthalic anhydride, 3,4,5,6-tetrahydrophthalic anhydride, 1,2,3,6-tetrahydrophthalic anhydride, dimethyltetrahydrophthalic anhydride, and 5,6-dicarboxybicyclo[2.2.1]hept-2-ene anhydride. The amount of the carboxylic acid anhydride used is preferably 0.5 to 1 mol per 1 mol of the amount of (b) used.
[0091] Resin [K5] is a resin obtained by further reacting resin [K3] with carboxylic anhydride under the same conditions as those for producing resin [K4]. A hydroxyl group generated by the reaction of a cyclic ether with a carboxylic acid or a carboxylic anhydride is reacted with the carboxylic anhydride. As the carboxylic acid anhydride, the same ones as those exemplified for the resin [K4] can be used. The amount of the carboxylic acid anhydride used is preferably 0.5 to 1 mole per mole of the amount of (a) used.
[0092] Examples of the resin [K1], the resin [K2], the resin [K3], the resin [K4] and the resin [K5] include resin [K1] such as a benzyl (meth)acrylate / (meth)acrylic acid copolymer and a styrene / (meth)acrylic acid copolymer; Resins such as a resin obtained by adding glycidyl (meth)acrylate to a benzyl (meth)acrylate / (meth)acrylic acid copolymer, a resin obtained by adding glycidyl (meth)acrylate to a tricyclodecyl (meth)acrylate / styrene / (meth)acrylic acid copolymer, a resin obtained by adding glycidyl (meth)acrylate to a tricyclodecyl (meth)acrylate / benzyl (meth)acrylate / (meth)acrylic acid copolymer, and a resin obtained by adding glycidyl (meth)acrylate to a dicyclopentanyl (meth)acrylate / methyl (meth)acrylate / (meth)acrylic acid copolymer [K2]; Resins such as a resin obtained by adding (meth)acrylic acid to a copolymer of tricyclodecyl (meth)acrylate / glycidyl (meth)acrylate, and a resin obtained by adding (meth)acrylic acid to a copolymer of tricyclodecyl (meth)acrylate / styrene / glycidyl (meth)acrylate [K3]; Resins obtained by further ester-bonding tetrahydrophthalic anhydride to a resin obtained by adding glycidyl (meth)acrylate to a benzyl (meth)acrylate / (meth)acrylic acid copolymer, resins obtained by further ester-bonding tetrahydrophthalic anhydride to a resin obtained by adding glycidyl (meth)acrylate to a tricyclodecyl (meth)acrylate / benzyl (meth)acrylate / (meth)acrylic acid copolymer, resins obtained by further ester-bonding tetrahydrophthalic anhydride to a resin obtained by adding glycidyl (meth)acrylate to a dicyclopentanyl (meth)acrylate / methyl (meth)acrylate / (meth)acrylic acid copolymer, resins obtained by further ester-bonding tetrahydrophthalic anhydride to a resin obtained by adding glycidyl (meth)acrylate to a dicyclopentanyl (meth)acrylate / methyl (meth)acrylate / (meth)acrylic acid copolymer [K4]; Resins such as a resin in which (meth)acrylic acid is added to a copolymer of tricyclodecyl (meth)acrylate / glycidyl (meth)acrylate, and further tetrahydrophthalic anhydride is ester-bonded to the resin [K5]; etc. Among them, the resin (B) preferably contains at least one selected from the group consisting of the resin [K2], the resin [K3], the resin [K4] and the resin [K5].
[0093] Further examples of resin (B) include the alkali-soluble resins described in JP 2018-123274 A. Examples of the alkali-soluble resin include a polymer (hereinafter also referred to as "resin (Ba)") that has a double bond in a side chain, contains a structural unit (α) represented by the following formula (I) in the main chain, and contains a structural unit (β) represented by the following formula (II) and further contains an acid group. The acid group can be introduced into the resin (Ba) by, for example, including a structural unit (γ) derived from an acid group-containing monomer (e.g., (meth)acrylic acid, etc.). The resin (Ba) preferably includes the structural units (α), (β), and (γ) in the main chain skeleton.
[0094] [ka] [In the formula, R A and R Bare the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms. n represents the average number of repeating units of the structural unit represented by formula (I) and is a number of 1 or more.]
[0095] [ka] [In the formula, R C R may be the same or different and represents a hydrogen atom or a methyl group. D are the same or different and represent a linear or branched hydrocarbon group having 4 to 20 carbon atoms. m represents the average number of repeating units of the structural unit represented by formula (II) and is a number of 1 or more.]
[0096] In the resin (Ba), the content of the structural unit (α) is, for example, 0.5% by mass or more and 50% by mass or less, preferably 1% by mass or more and 40% by mass or less, and more preferably 5% by mass or more and 30% by mass or less, based on 100% by mass of the total amount of all monomer units that provide the main chain skeleton of the resin (Ba), from the viewpoint of the heat resistance and storage stability of the resin (Ba). n in the formula (I) represents the average number of repeating units of the structural unit (α) in the resin (Ba), and n can be set so that the content of the structural unit (α) falls within the above range.
[0097] From the viewpoint of the solvent resistance of the cured film, the content ratio of the structural unit (β) is, for example, 10% by mass or more and 90% by mass or less, preferably 20% by mass or more and 80% by mass or less, and more preferably 30% by mass or more and 75% by mass or less, based on the total amount of all monomer units that give the main chain skeleton of the resin (Ba) (100% by mass). m in the formula (II) represents the average number of repeating units of the structural unit (β) in the resin (Ba), and m can be set so that the content ratio of the structural unit (β) falls within the above-mentioned range.
[0098] From the viewpoint of the solubility of the resin (Ba) in alkaline substances and the solubility of the resin (Ba) in the solvent (F), the content of the structural unit (γ) is, for example, 0.5% by mass or more and 50% by mass or less, preferably 2% by mass or more and 50% by mass or less, and more preferably 5% by mass or more and 45% by mass or less, relative to 100% by mass of the total amount of all monomer units that provide the main chain skeleton of the resin (Ba).
[0099] The resin (B) can contain one or more resins selected from the group consisting of the above-mentioned resin [K1], resin [K2], resin [K3], resin [K4], resin [K5] and resin (Ba).
[0100] Resin (B) preferably has a weight average molecular weight, calculated based on standard polystyrene, of not more than 9000 as measured by gel permeation chromatography (GPC). When resin (B) has the above weight average molecular weight, a cured film having a high development speed and high luminescence intensity tends to be obtained even in a thick film. The weight average molecular weight of resin (B) in terms of standard polystyrene is, for example, 1,000 or more and 100,000 or less, and from the viewpoints of development speed and luminescence intensity, preferably 2,000 or more and 50,000 or less, more preferably 3,000 or more and 20,000 or less. The weight average molecular weight of the resin (B) in terms of standard polystyrene is measured according to the measurement method in the section of Examples described later. In order to set the weight average molecular weight of the resin (B) within the above range, it can be adjusted by appropriately combining reaction conditions such as the selection of raw materials to be used, the charging method, the reaction temperature and time.
[0101] The molecular weight distribution [weight average molecular weight (Mw) / number average molecular weight (Mn)] of the resin (B) measured by GPC is, for example, 1.0 or more and 6.0 or less, and from the viewpoint of the developability of the cured film, preferably 1.2 or more and 4.0 or less.
[0102] The acid value of the resin (B) is preferably 30 mgKOH / g or more and 150 mgKOH / g or less based on the solid content, and from the viewpoint of the developability of the cured film, it is preferably 35 mgKOH / g or more and 140 mgKOH / g or less, more preferably 40 mgKOH / g or more and 130 mgKOH / g or less. Here, the acid value is a value measured as the amount (mg) of potassium hydroxide required to neutralize 1 g of the resin (B), and can be determined, for example, by titration using an aqueous potassium hydroxide solution. The acid value of the resin (B) is measured according to the measurement method in the Examples section described later.
[0103] The resin (B) may contain a resin having a double bond equivalent of, for example, 300 g / eq or more and 2000 g / eq or less, preferably 500 g / eq or more and 1500 g / eq or less. By containing a resin having a double bond equivalent of 300 g / eq or more and 2000 g / eq or less, the phenomenon of quenching during the process of producing a cured pattern tends to be easily prevented. When the resin (B) contains a resin having a double bond equivalent of more than 2000 g / eq, the resin (B) tends to have a reduced ability to effectively protect the quantum dots (A). When the resin (B) contains a resin having a double bond equivalent of less than 300 g / eq, the cured film tends to peel off easily without being dissolved during development. Examples of the resin having a double bond equivalent of 300 g / eq or more and 2000 g / eq or less include a (meth)acrylic resin. The resin (B) is preferably a (meth)acrylic resin.
[0104] The content of the resin (B) in the curable composition is, for example, 5% by mass or more and 80% by mass or less, preferably 10% by mass or more and 70% by mass or less, more preferably 13% by mass or more and 60% by mass or less, and even more preferably 17% by mass or more and 55% by mass or less, based on the total amount of solids in the curable composition. When the content of the resin (B) is within the above range, the quantum dots (A) tend to be easily dispersed, and the luminous efficiency tends to be easily maintained high during the process of producing a cured pattern.
[0105] In the curable composition, the mass ratio (solid content ratio) of the resin (B) to the polymerizable compound (C) described later is, for example, 1 or more, and from the viewpoints of the developability and luminescence intensity of the cured film, it is preferably 1.5 or more, more preferably 2 or more, and even more preferably 2.5 or more.
[0106] <Polymerizable compound (C)> The polymerizable compound (C) is a compound that can be polymerized by an active radical, an acid, or the like generated from a polymerization initiator (D) described later. Examples of the polymerizable compound (C) include photopolymerizable compounds such as compounds having an ethylenically unsaturated bond, such as (meth)acrylic acid ester compounds. Another example of the polymerizable compound (C) is a thermally polymerizable compound. The composition may contain two or more types of polymerizable compounds (C).
[0107] The polymerizable compound (C) is preferably a photopolymerizable compound having three or more ethylenically unsaturated bonds in the molecule. The weight average molecular weight of the polymerizable compound (C) is preferably 150 or more and 2900 or less, more preferably 250 or more and 1500 or less.
[0108] Examples of the photopolymerizable compound having three or more ethylenically unsaturated bonds in the molecule include a compound (Ca) having three or more ethylenically unsaturated bonds in the molecule and having an acidic functional group, and a compound (Cb) having three or more ethylenically unsaturated bonds in the molecule and not having an acidic functional group. The polymerizable compound (C) preferably contains at least one of the compounds (Ca) and (Cb), and may contain two or more of the compounds (Ca), two or more of the compounds (Cb), or at least one of the compounds (Ca) and at least one of the compounds (Cb).
[0109] Examples of the acidic functional group include a carboxy group, a sulfonic acid group, a phosphoric acid group, etc. Among these, the acidic functional group is preferably a carboxy group.
[0110] By including the compound (Ca) in the polymerizable compound (C), the dispersibility of the quantum dots (A) can be improved, and the emission intensity of the cured film can be improved. In addition, by including the compound (Ca) in the polymerizable compound (C), the curability and heat resistance of the curable composition can be improved. When the polymerizable compound (C) includes the compound (Ca), the content of the compound (Ca) in 100% by mass of the polymerizable compound (C) is preferably 5 to 100% by mass, more preferably 15 to 65% by mass, and even more preferably 35 to 50% by mass. By making the content of the compound (Ca) equal to or greater than the lower limit, the emission intensity of the cured film becomes good.
[0111] The ethylenically unsaturated bond in the compound (Ca) is preferably a (meth)acryloyloxy group. The number of ethylenically unsaturated bonds in one molecule of the compound (Ca) is preferably 3 to 5, more preferably 3. The number of acidic functional groups in one molecule of the compound (Ca) is 1 or more. When the compound (Ca) has two or more acidic functional groups, the respective acidic functional groups may be different or the same, but it is preferable that the compound (Ca) has at least one carboxy group.
[0112] Examples of the compound (Ca) include compounds obtained by modifying a compound having three or more (meth)acryloyloxy groups and one or more hydroxyl groups, such as pentaerythritol tri(meth)acrylate or dipentaerythritol penta(meth)acrylate, with a polybasic acid. Examples of the compound include a compound obtained by monoesterifying pentaerythritol tri(meth)acrylate and succinic acid, a compound obtained by monoesterifying dipentaerythritol penta(meth)acrylate and succinic acid, a compound obtained by monoesterifying pentaerythritol tri(meth)acrylate and maleic acid, and a compound obtained by monoesterifying dipentaerythritol penta(meth)acrylate and maleic acid. Among these, a compound obtained by monoesterifying pentaerythritol tri(meth)acrylate and succinic acid is preferred.
[0113] Examples of commercially available products of compound (Ca) include "ARONIX M-510" manufactured by Toagosei Co., Ltd., which contains a dibasic acid anhydride adduct of pentaerythritol tri(meth)acrylate as the main component, and "ARONIX M-520D" manufactured by Toagosei Co., Ltd., which contains a dibasic acid anhydride adduct of dipentaerythritol penta(meth)acrylate as the main component. These commercially available products have a carboxy group as the acidic functional group.
[0114] The ethylenically unsaturated bond contained in the compound (Cb) is preferably a (meth)acryloyloxy group. The number of ethylenically unsaturated bonds contained in one molecule of the compound (Cb) is preferably 3 to 6.
[0115] Examples of the compound (Cb) include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol octa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, tetrapentaerythritol nona(meth)acrylate, tris( 2-(meth)acryloyloxyethyl)isocyanurate, ethylene glycol modified pentaerythritol tetra(meth)acrylate, ethylene glycol modified dipentaerythritol hexa(meth)acrylate, propylene glycol modified pentaerythritol tetra(meth)acrylate, propylene glycol modified dipentaerythritol hexa(meth)acrylate, caprolactone modified pentaerythritol tetra(meth)acrylate, caprolactone modified dipentaerythritol hexa(meth)acrylate, etc. Among them, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, etc. are preferred.
[0116] From the viewpoint of improving the development speed of the curable composition, the polymerizable compound (C) preferably contains a compound (Cb). When the polymerizable compound (C) contains a compound (Cb), the content of the compound (Cb) in 100% by mass of the polymerizable compound (C) is preferably 5 to 100% by mass, more preferably 30 to 95% by mass, and further preferably 50 to 85% by mass. By making the content of the compound (Cb) equal to or more than the lower limit, the development speed of the curable composition becomes good.
[0117] From the viewpoint of improving the luminescence intensity of the cured film and improving the solvent resistance (film remaining rate) of the cured film, it is preferable that the polymerizable compound (C) contains a compound (Ca) and a compound (Cb), and the content ratio of the compounds (Ca) and (Cb) (compound (Ca):compound (Cb)) is preferably 5:95 to 95:5, more preferably 15:85 to 85:15, and even more preferably 35:65 to 65:35, on a mass basis.
[0118] The content of the polymerizable compound (C) in the curable composition is preferably 7% by mass or more and 60% by mass or less, more preferably 10% by mass or more and 45% by mass or less, and even more preferably 13% by mass or more and 30% by mass or less, based on the total amount of solids in the curable composition. When the content of the polymerizable compound (C) is within the above range, the solvent resistance (film remaining rate) of the cured film tends to be improved.
[0119] <Polymerization initiator (D)> The polymerization initiator (D) is a compound that generates active radicals, acids, etc. by the action of light or heat, and can initiate polymerization of the polymerizable compound (C). The composition can contain one or more polymerization initiators (D).
[0120] The polymerization initiator (D) contains a compound represented by formula (DA) as an essential component. When the polymerization initiator (D) contains a compound represented by formula (DA), a curable composition with excellent patterning properties can be obtained. In particular, in the composition of a conventional curable composition, when the quantum dots (A) are highly concentrated, a good cured pattern may not be obtained. However, when the compound represented by formula (DA) is contained, a good cured pattern can be formed even in a curable composition containing a high concentration of quantum dots (A). Here, the "curable composition containing a high concentration of quantum dots (A)" may refer to a curable composition in which the content of quantum dots (A) relative to the total amount of resin (B) and polymerizable compound (C) is, for example, 30% by mass or more, more specifically, 45% by mass or more.
[0121] [ka] [In the formula, R d1 represents a branched hydrocarbon group having 3 to 20 carbon atoms which may have a substituent. R d2 ~R d5 each independently represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. and n represents an integer of 0 to 4. The —CH 2 - may be replaced by -O-, -S-, -CO- or -OCO-.
[0122] R d1 Examples of the branched hydrocarbon group having 3 to 20 carbon atoms represented by the formula (I) include a branched saturated hydrocarbon group having 3 to 20 carbon atoms and a branched unsaturated hydrocarbon group having 3 to 20 carbon atoms.
[0123] R d1Examples of the branched saturated hydrocarbon group having 3 to 20 carbon atoms represented by the formula (I) include a 1-methylethyl group (isopropyl group), a 1-methylpropyl group (sec-butyl group), a 2-methylpropyl group (isobutyl group), a 1,1-dimethylethyl group (tert-butyl group), a 1,1-dimethylpropyl group, a 2,2-dimethylpropyl group, a 1,2-dimethylpropyl group, a 1-ethylpropyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 3-methylbutyl group, a 1,1-dimethylbutyl group, and a 2,2-dimethylbutyl group. , 3,3-dimethylbutyl group, 1,2-dimethylbutyl group, 1,3-dimethylbutyl group, 2,3-dimethylbutyl group, 1-ethylbutyl group, 2-ethylbutyl group, 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 4-methylpentyl group, 1,1-dimethylpentyl group, 2,2-dimethylpentyl group, 3,3-dimethylpentyl group, 1,2-dimethylpentyl group, 1,3-dimethylpentyl group, 2,3-dimethylpentyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3 -ethylpentyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methylhexyl group, 4-methylhexyl group, 1,1-dimethylhexyl group, 2,2-dimethylhexyl group, 3,3-dimethylhexyl group, 1,2-dimethylhexyl group, 1,3-dimethylhexyl group, 2,3-dimethylhexyl group, 1-ethylhexyl group, 2-ethylhexyl group, 3-ethylhexyl group, 1-methylheptyl group, 2-methylheptyl group, 3-methylheptyl group, 4-methylheptyl group, 1,1-dimethylhexyl group butyl group, 2,2-dimethylheptyl group, 3,3-dimethylheptyl group, 1,2-dimethylheptyl group, 1,3-dimethylheptyl group, 2,3-dimethylheptyl group, 1-ethylheptyl group, 2-ethylheptyl group, 3-ethylheptyl group, 1-methyloctyl group, 2-methyloctyl group, 3-methyloctyl group, 4-methyloctyl group, 1,1-dimethyloctyl group, 2,2-dimethyloctyl group, 3,3-dimethyloctyl group, 1,2-dimethyloctyl group, 1,3-dimethyloctyl group, 2,Branched alkyl groups such as 3-dimethyloctyl group, 1-ethyloctyl group, 2-ethyloctyl group, 3-ethyloctyl group, 1-methylnonyl group, 2-methylnonyl group, 3-methylnonyl group, 4-methylnonyl group, dimethylnonyl group, ethylnonyl group, methyldecyl group, dimethyldecyl group, ethyldecyl group, methylundecyl group, dimethylundecyl group, ethylundecyl group, and methyldodecyl group are included. R d1 The branched alkyl group represented by the formula (I) may be a primary branched alkyl group, a secondary branched alkyl group, or a tertiary branched alkyl group. R d1 The number of carbon atoms in the branched saturated hydrocarbon group represented by the formula (I) is preferably 4 or more, more preferably 5 or more, and is preferably 16 or less, more preferably 12 or less, and further preferably 10 or less.
[0124] R d1 The branched unsaturated hydrocarbon group represented by the above-mentioned R d1 Examples of the branched saturated hydrocarbon group include those in which at least one carbon-carbon single bond contained in the branched saturated hydrocarbon group represented by the following formula (I) is replaced with a carbon-carbon double bond or a carbon-carbon triple bond. R d1 Examples of the branched unsaturated hydrocarbon group represented by the formula (I) include alkenyl groups such as an isopropenyl group, an isobutenyl group, an isopentenyl group, an isohexenyl group, an isoheptenyl group, an isooctenyl group, an isononyl group, and an isodecenyl group; and alkynyl groups such as an isopropynyl group, an isobutynyl group, an isopentynyl group, an isohexynyl group, an isoheptynyl group, an isooctynyl group, an isononynyl group, and an isodecynyl group. R d1 The branched unsaturated hydrocarbon group represented by the formula (I) has preferably 4 or more, more preferably 5 or more, and preferably 16 or less, more preferably 12 or less, and further preferably 10 or less.
[0125] R d2 , R d3 , R d4 and R d5Examples of the hydrocarbon group having 1 to 20 carbon atoms represented by the formula (I) include a saturated hydrocarbon group having 1 to 20 carbon atoms, an unsaturated hydrocarbon group having 2 to 20 carbon atoms, and an aromatic hydrocarbon group having 6 to 20 carbon atoms. d2 , R d3 , R d4 and R d5 The hydrocarbon groups represented by the following formula may be the same or different.
[0126] Examples of the saturated hydrocarbon group having 1 to 20 carbon atoms include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, hexadecyl, and icosyl groups; branched alkyl groups such as isopropyl, isobutyl, isopentyl, neopentyl, and 2-ethylhexyl groups; and alicyclic saturated hydrocarbon groups having 3 to 20 carbon atoms such as cyclopropyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, and tricyclodecyl groups. The number of carbon atoms in the saturated hydrocarbon group is preferably 1 to 18, more preferably 1 to 15, even more preferably 1 to 10, and even more preferably 1 to 8.
[0127] Examples of the unsaturated hydrocarbon group having 2 to 20 carbon atoms include alkenyl groups such as vinyl group, allyl group, butenyl group, pentenyl group, hexenyl group, heptenyl group, octenyl group, nonenyl group, decenyl group, undecenyl group, dodecenyl group, hexadecenyl group, octadecenyl group, and icosenyl group; alkynyl groups such as ethynyl group, propynyl group, hexynyl group, decynyl group, and icosenyl group; cycloalkenyl groups such as cyclopentenyl group, cyclohexenyl group, and cycloheptenyl group; etc. The number of carbon atoms in the unsaturated hydrocarbon group is preferably 2 to 18, more preferably 2 to 15, and even more preferably 2 to 10.
[0128] Examples of the aromatic hydrocarbon group having 6 to 20 carbon atoms include a phenyl group, a xylyl group, a trimethylphenyl group, a dipropylphenyl group, a di(2,2-dimethylpropyl)phenyl group, a naphthyl group, a benzyl group, a phenylethyl group, a phenylbutyl group, etc. The number of carbon atoms in the aromatic hydrocarbon group is preferably 6 to 18, more preferably 6 to 15, and further preferably 6 to 12.
[0129] R d1 , R d2 , R d3 , R d4 and R d5 Examples of the substituent that the hydrocarbon group represented by the formula (I) may have include a halogen atom, a cyano group, and a nitro group. The halogen atom is preferably a fluorine atom, a bromine atom, a chlorine atom, or an iodine atom.
[0130] The —CH 2 - may be replaced by -O-, -S-, -CO- or -OCO-, and adjacent -CH 2 - is not simultaneously replaced by the same group, and the terminal -CH 2 - is never replaced.
[0131] n represents an integer of 0 to 4, preferably an integer of 0 to 3, more preferably an integer of 0 to 2, further preferably an integer of 0 or 1, and even more preferably 0.
[0132] *-OCO-R d4 The bonding position of the group (* represents a bond to the phenyl group) is the *-OCO-R d4 The group may be bonded to any of the 2-, 3- or 4-positions of the phenyl group, but is preferably bonded to the 3- or 4-position, more preferably to the 4-position.
[0133] R d1 The branched hydrocarbon group having 3 to 20 carbon atoms represented by the formula: A branched saturated hydrocarbon group having 3 to 20 carbon atoms is preferred. A branched alkyl group having 3 to 20 carbon atoms is more preferable. A branched alkyl group having 3 to 10 carbon atoms is more preferable. It is preferable that the alkyl group is one or more selected from the group consisting of a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 1-ethylpentyl group, a 2-ethylpentyl group, a 3-ethylpentyl group, a 1-methylhexyl group, a 2-methylhexyl group, a 3-methylhexyl group, a 1-ethylhexyl group, a 2-ethylhexyl group, a 3-ethylhexyl group, a 1-methylheptyl group, a 2-methylheptyl group, a 3-methylheptyl group, a 1-ethylheptyl group, a 2-ethylheptyl group, and a 3-ethylheptyl group.
[0134] R d2 , R d3 , R d4 and R d5 The hydrocarbon group having 1 to 20 carbon atoms represented by the formula: A saturated hydrocarbon group having 1 to 20 carbon atoms and an unsaturated hydrocarbon group having 2 to 20 carbon atoms are preferred. A saturated hydrocarbon group having 1 to 20 carbon atoms is more preferable. A chain-like saturated hydrocarbon group having 1 to 10 carbon atoms is more preferable. A chain alkyl group having 1 to 8 carbon atoms is even more preferred. R d2 is preferably a chain alkyl group having 1 to 8 carbon atoms, and more preferably a chain alkyl group having 1 to 6 carbon atoms. R d3 is preferably a chain alkyl group having 1 to 8 carbon atoms, and more preferably a chain alkyl group having 1 to 3 carbon atoms. R d4 is preferably a chain alkyl group having 1 to 8 carbon atoms, and more preferably a chain alkyl group having 1 to 3 carbon atoms. R d5 is preferably a linear or branched alkyl group having 1 to 8 carbon atoms, and more preferably a linear or branched alkyl group having 1 to 6 carbon atoms.
[0135] Examples of the polymerization initiator (D) other than the compound represented by formula (DA) include polymerization initiators such as oxime compounds (excluding the compound represented by formula (DA)), alkylphenone compounds, biimidazole compounds, triazine compounds and acylphosphine compounds, and thermal polymerization initiators such as azo compounds and organic peroxides.
[0136] An example of the oxime compound (excluding the compound represented by formula (DA)) is an oxime compound having a first molecular structure represented by the following formula (1). Hereinafter, this oxime compound is also referred to as "oxime compound (1)".
[0137] [ka] [In formula (1), R 1 is R 11 , OR 11 , C.O.R. 11 , S.R. 11 ,CONR 12 R 13 or CN. * represents a bond to a second molecular structure, which is a molecular structure other than the first molecular structure that the oxime compound (1) has.]
[0138] Inclusion of the oxime compound (1) as the polymerization initiator (D) can be advantageous in terms of improving the luminescence intensity of the cured film. One of the reasons for this effect is presumed to be that the absorption wavelength of the oxime compound (1) changes significantly before and after the cleavage (decomposition) of the oxime compound (1), which is necessary for the oxime compound (1) to initiate photopolymerization, due to the unique molecular structure of the oxime compound (1), and therefore the oxime compound (1) has a high photoradical polymerization initiation ability.
[0139] R 11 , R 12 and R 13 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. R 11 , R12 or R 13 The hydrogen atoms of the group represented by OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , CN, halogen atom or COOR 21 may be substituted with. R 21 , R 22 and R 23 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. R 21 , R 22 or R 23 The hydrogen atom of the group represented by the formula (I) may be substituted by CN, a halogen atom, a hydroxy group or a carboxy group. R 11 , R 12 , R 13 , R 21 , R 22 or R 23 When the group represented by the formula (I) has an alkylene portion, the alkylene portion is preferably -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-, -NR 24 COO-, -OCONR 24 It may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS- or -CSO-. R 24 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. R 11 , R 12 , R13 , R 21 , R 22 or R 23 When the group represented by R 12 and R 13 and R 22 and R 23 may be joined together to form a ring.
[0140] R in formula (1) 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 Examples of the alkyl group having 1 to 20 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a tert-pentyl group, a hexyl group, a heptyl group, an octyl group, an isooctyl group, a 2-ethylhexyl group, a tert-octyl group, a nonyl group, an isononyl group, a decyl group, an isodecyl group, an undecyl group, a dodecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, an icosyl group, a cyclopentyl group, a cyclohexyl group, a cyclohexylmethyl group, and a cyclohexylethyl group.
[0141] R in formula (1) 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 Examples of the aryl group having 6 to 30 carbon atoms represented by the formula (I) include a phenyl group, a tolyl group, a xylyl group, an ethylphenyl group, a naphthyl group, an anthryl group, a phenanthryl group, a phenyl group substituted with one or more of the above-mentioned alkyl groups, a biphenylyl group, a naphthyl group, and an anthryl group.
[0142] R in formula (1) 11 , R 12 , R 13 , R 21 , R22 , R 23 and R 24 Examples of the aralkyl group having 7 to 30 carbon atoms represented by the following formula include a benzyl group, an α-methylbenzyl group, an α,α-dimethylbenzyl group, and a phenylethyl group.
[0143] R in formula (1) 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 Examples of the heterocyclic group having 2 to 20 carbon atoms represented by the formula (I) include a pyridyl group, a pyrimidyl group, a furyl group, a thienyl group, a tetrahydrofuryl group, a dioxolanyl group, a benzoxazol-2-yl group, a tetrahydropyranyl group, a pyrrolidyl group, an imidazolidyl group, a pyrazolidyl group, a thiazolidyl group, an isothiazolidyl group, an oxazolidyl group, an isoxazolidyl group, a piperidyl group, a piperazyl group, and a morpholinyl group, and are preferably 5- to 7-membered heterocyclic rings.
[0144] R in formula (1) 12 and R 13 and R 22 and R 23 may be joined together to form a ring, R 12 and R 13 and R 22 and R 23 means that they may be taken together to form a ring with the nitrogen atom, carbon atom or oxygen atom to which they are attached. R in formula (1) 12 and R 13 and R 22 and R 23 Examples of the ring that can be formed by combining with each other include a cyclopentane ring, a cyclohexane ring, a cyclopentene ring, a benzene ring, a piperidine ring, a morpholine ring, a lactone ring, and a lactam ring, and preferably a 5- to 7-membered ring.
[0145] R in formula (1) 11 , R 12 , R 13 , R 21 , R22 and R 23 Examples of the halogen atom which may be contained as a substituent include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.
[0146] R in formula (1) 1 is preferably R 11 and more preferably an alkyl group having 1 to 20 carbon atoms, even more preferably an alkyl group having 1 to 10 carbon atoms, and even more preferably an alkyl group having 1 to 6 carbon atoms.
[0147] An example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (2): The second molecular structure means a molecular structure portion other than the first molecular structure possessed by the oxime compound (1). The bond represented by "*" in formula (2) is directly bonded to the bond represented by "*" in formula (1). In other words, when the second molecular structure is a structure represented by formula (2), the benzene ring having "-*" in formula (2) and the carbonyl group having "-*" in formula (1) are directly bonded.
[0148] [ka]
[0149] [In formula (2), R 2 and R 3 are each independently R 11 , OR 11 , S.R. 11 , C.O.R. 11 ,CONR 12 R 13 , N.R. 12 COR 11 , O.C.O.R. 11 , COOR 11 , SCOR 11 , OCSR 11 , C.O.S.R. 11 , C.S.O.R. 11 , CN or a halogen atom. R 2When multiple are present, they may be the same or different. R 3 When multiple are present, they may be the same or different. R 11 , R 12 and R 13 has the same meaning as above. s and t each independently represent an integer of 0 to 4. L is a sulfur atom, CR 31 R 32 , CO or NR 33 Represents. R 31 , R 32 and R 33 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an aralkyl group having 7 to 30 carbon atoms. R 31 , R 32 or R 33 When the group represented by R 31 , R 32 and R 33 may each independently form a ring together with either adjacent benzene ring. R 4 represents a hydroxy group, a carboxy group, or a group represented by the following formula (2-1).
[0150] [ka] [In formula (2-1), L 1 -O-, -S-, -NR 22 -, -NR 22 CO-, -SO 2 -, -CS-, -OCO- or -COO-. R 22 has the same meaning as above. L 2represents a group obtained by removing v hydrogen atoms from an alkyl group having 1 to 20 carbon atoms, a group obtained by removing v hydrogen atoms from an aryl group having 6 to 30 carbon atoms, a group obtained by removing v hydrogen atoms from an aralkyl group having 7 to 30 carbon atoms, or a group obtained by removing v hydrogen atoms from a heterocyclic group having 2 to 20 carbon atoms. L 2 When the group represented by the formula (I) has an alkylene portion, the alkylene portion is preferably -O-, -S-, -COO-, -OCO-, -NR 22 -, -NR 22 COO-, -OCONR 22 It may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS- or -CSO-, and the alkylene portion may be branched or cyclic. R 4a OR 41 , S.R. 41 ,CONR 42 R 43 , N.R. 42 COR 43 , O.C.O.R. 41 , COOR 41 , SCOR 41 , OCSR 41 , C.O.S.R. 41 , C.S.O.R. 41 , CN or a halogen atom. R 4a When multiple are present, they may be the same or different. R 41 , R 42 and R 43 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an aralkyl group having 7 to 30 carbon atoms; R 41 , R 42 and R 43 When the group represented by R 42 and R 43 may be joined together to form a ring. v represents an integer from 1 to 3. * represents a bond to the first molecular structure of the oxime compound (1).
[0151] R in Equation (2) 11 , R 12 , R 13 , R 21 , R 22 , R 23 , R 24 , R 31 , R 32 and R 33 and R in the above formula (2-1) 22 , R 41 , R 42 and R 43 Examples of the alkyl group having 1 to 20 carbon atoms, the aryl group having 6 to 30 carbon atoms, and the aralkyl group having 7 to 30 carbon atoms are represented by R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 The example for is similar.
[0152] R in Equation (2) 11 , R 12 , R 13 , R 21 , R 22 , R 23 , R 24 and R in the above formula (2-1) 22 Examples of the heterocyclic group having 2 to 20 carbon atoms represented by the formula (1) include R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 The example for is similar.
[0153] R in Equation (2) 31 , R 32 and R 33 may each independently form a ring together with either adjacent benzene ring, R 31 , R 32 and R 33 means that each of them may independently form a ring together with either adjacent benzene ring and the nitrogen atom to which it is connected. R in Equation (2)31 , R 32 and R 33 Examples of rings that may be formed by combining with either adjacent benzene ring include R 12 and R 13 and R 22 and R 23 The same is true for the ring which may be formed by combining with each other.
[0154] L in the above formula (2-1) 2 represents a group in which v hydrogen atoms have been removed from an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.
[0155] Examples of the group obtained by removing v hydrogen atoms from an alkyl group having 1 to 20 carbon atoms, when v is 1, include alkylene groups such as a methylene group, an ethylene group, a propylene group, a methylethylene group, a butylene group, a 1-methylpropylene group, a 2-methylpropylene group, a 1,2-dimethylpropylene group, a 1,3-dimethylpropylene group, a 1-methylbutylene group, a 2-methylbutylene group, a 3-methylbutylene group, a 4-methylbutylene group, a 2,4-dimethylbutylene group, a 1,3-dimethylbutylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, a decylene group, a dodecylene group, a tridecylene group, a tetradecylene group, a pentadecylene group, an ethane-1,1-diyl group, and a propane-2,2-diyl group.
[0156] Examples of the group in which v hydrogen atoms have been removed from an aryl group having 6 to 30 carbon atoms, when v is 1, include arylene groups such as a 1,2-phenylene group, a 1,3-phenylene group, a 1,4-phenylene group, a 2,6-naphthylene group, a 1,4-naphthylene group, a 2,5-dimethyl-1,4-phenylene group, a diphenylmethane-4,4'-diyl group, a 2,2-diphenylpropane-4,4'-diyl group, a diphenylsulfide-4,4'-diyl group, and a diphenylsulfone-4,4'-diyl group.
[0157] Examples of the group in which v hydrogen atoms have been removed from an aralkyl group having 7 to 30 carbon atoms, when v is 1, include groups represented by the following formula (a) and groups represented by the following formula (b).
[0158] [ka] [In formulas (a) and (b), L 3 and L 5 represents an alkylene group having 1 to 10 carbon atoms; L 4 and L 6 represents a single bond or an alkylene group having 1 to 10 carbon atoms.]
[0159] Examples of the alkylene group having 1 to 10 carbon atoms include a methylene group, an ethylene group, a propylene group, a methylethylene group, a butylene group, a 1-methylpropylene group, a 2-methylpropylene group, a 1,2-dimethylpropylene group, a 1,3-dimethylpropylene group, a 1-methylbutylene group, a 2-methylbutylene group, a 3-methylbutylene group, a 4-methylbutylene group, a 2,4-dimethylbutylene group, a 1,3-dimethylbutylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, and a decylene group.
[0160] Examples of the group in which v hydrogen atoms have been removed from a heterocyclic group having 2 to 20 carbon atoms, when v is 1, include divalent heterocyclic groups such as a 2,5-pyridinediyl group, a 2,6-pyridinediyl group, a 2,5-pyrimidinediyl group, a 2,5-thiophenediyl group, a 3,4-tetrahydrofurandiyl group, a 2,5-tetrahydrofurandiyl group, a 2,5-furandiyl group, a 3,4-thiazolediyl group, a 2,5-benzofurandiyl group, a 2,5-benzothiophenediyl group, an N-methylindole-2,5-diyl group, a 2,5-benzothiazolediyl group, and a 2,5-benzoxazolediyl group.
[0161] R in Equation (2) 2 and R 3 and R in the above formula (2-1) 4aExamples of the halogen atom represented by the formula (I) include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.
[0162] From the viewpoint of solubility in the solvent (F) and the developability of the composition, a preferred example of the structure represented by formula (2) is a structure represented by the following formula (2a).
[0163] [ka] [In formula (2a), L′ is a sulfur atom or NR 50 R 50 represents a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms; R 2 , R 3 , R 4 , s and t have the same meanings as above. * represents a bond to the first molecular structure of the oxime compound (1).
[0164] From the same viewpoint as above, another preferable example of the structure represented by formula (2) is a structure represented by the following formula (2b).
[0165] [ka] [In formula (2b), R 44 represents a hydroxy group, a carboxy group, or a group represented by the following formula (2-2).
[0166] [ka] [In formula (2-2), L 11 represents -O- or **-OCO-, and ** represents L 12 represents a bond with L 12 represents an alkylene group having 1 to 20 carbon atoms, which may be interrupted by 1 to 3 -O-; R 44a OR 55 or COOR 55 R 55represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.] * represents a bond to the first molecular structure of the oxime compound (1).
[0167] R 44 is preferably a group represented by formula (2-2), which is advantageous in terms of the solubility of the oxime compound (1) in the solvent (F) and the developability of the composition.
[0168] L 12 The alkylene group represented by the following formula (1) preferably has 1 to 10 carbon atoms, and more preferably has 1 to 4 carbon atoms. R 44a is preferably a hydroxy group or a carboxy group, and more preferably a hydroxy group.
[0169] The method for producing the oxime compound (1) having the second molecular structure represented by formula (2) is not particularly limited, but it can be produced, for example, by the method described in JP-A-2011-132215.
[0170] Another example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (3). The bond represented by "*" in formula (3) is directly bonded to the bond represented by "*" in formula (1). In other words, when the second molecular structure is a structure represented by formula (3), the benzene ring having "-*" in formula (3) and the carbonyl group having "-*" in formula (1) are directly bonded.
[0171] [ka] [In formula (3), R 5 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. R 5When the group represented by the following formula (I) has an alkyl portion, the alkyl portion may be branched or cyclic. R 5 The hydrogen atoms of the group represented by R 21 , OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , N.R. 22 COR 21 , O.C.O.R. 21 , COOR 21 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , SCOR 21 , OCSR 21 , C.O.S.R. 21 , C.S.O.R. 21 , hydroxyl group, nitro group, CN, halogen atom or COOR 21 may be substituted with. R 21 , R 22 and R 23 has the same meaning as above. R 21 , R 22 or R 23 The hydrogen atom of the group represented by the formula (I) may be substituted by CN, a halogen atom, a hydroxy group or a carboxy group. R 21 , R 22 and R 23 When the group represented by the formula (I) has an alkylene portion, the alkylene portion is preferably -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-, -NR 24 COO-, -OCONR 24 It may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS- or -CSO-. R 24has the same meaning as above. R 21 , R 22 and R 23 When the group represented by R 22 and R 23 may be joined together to form a ring. R 6 , R 7 , R 8 and R 9 are each independently R 61 , OR 61 , S.R. 61 , C.O.R. 62 ,CONR 63 R 64 , N.R. 65 COR 61 , O.C.O.R. 61 , COOR 62 , SCOR 61 , OCSR 61 , C.O.S.R. 62 , C.S.O.R. 61 , a hydroxyl group, a nitro group, CN or a halogen atom. R 61 , R 62 , R 63 , R 64 and R 65 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. R 61 , R 62 , R 63 , R 64 or R 65 The hydrogen atoms of the group represented by OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , -C(=N-OR 21 )-R 22, -C(=N-OCOR 21 )-R 22 , CN, halogen atom or COOR 21 may be substituted with. R 6 and R 7 , R 7 and R 8 and R 8 and R 9 may be joined together to form a ring. * represents a bond to the first molecular structure of the oxime compound (1).
[0172] R in Equation (3) 5 , R 21 , R 22 , R 23 , R 24 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of the alkyl group having 1 to 20 carbon atoms, the aryl group having 6 to 30 carbon atoms, the aralkyl group having 7 to 30 carbon atoms, and the heterocyclic group having 2 to 20 carbon atoms, which are represented by the formula (1), are R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 The example for is similar.
[0173] R in Equation (3) 22 and R 23 may be joined together to form a ring, R 22 and R 23 means that they may be taken together to form a ring with the nitrogen atom, carbon atom or oxygen atom to which they are attached. R in Equation (3) 22 and R 23 Examples of rings that may be formed by combining with each other include R 12 and R 13 and R 22 and R 23 The same is true for the ring which may be formed by combining with each other.
[0174] R in Equation (3) 6 , R 7 , R 8 and R 9 Halogen atoms represented by R 5 , R 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of halogen atoms which may replace the hydrogen atoms of include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.
[0175] In one preferred embodiment, from the viewpoint of solubility in the solvent (F) and developability of the composition, R 5 is a group represented by the following formula (3-1).
[0176] [ka] [In formula (3-1), Z represents a group in which one hydrogen atom has been removed from an alkyl group having 1 to 20 carbon atoms, a group in which one hydrogen atom has been removed from an aryl group having 6 to 30 carbon atoms, a group in which one hydrogen atom has been removed from an aralkyl group having 7 to 30 carbon atoms, or a group in which one hydrogen atom has been removed from a heterocyclic group having 2 to 20 carbon atoms, When the group represented by Z has an alkylene portion, the alkylene portion is preferably -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 COO-, -OCONR 24 may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS- or -CSO-, and the alkylene portion may be branched or cyclic; R 21 , R 22 and R 24 has the same meaning as above.]
[0177] From the same viewpoint as above, Z in formula (3-1) is preferably a methylene group, an ethylene group, or a phenylene group. R in formula (3-1) 21 and R 22 From the same viewpoint as above, is preferably an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 30 carbon atoms, and more preferably a methyl group, an ethyl group, or a phenyl group. From the same viewpoint as above, in another preferred embodiment, R 7 is a nitro group.
[0178] The method for producing the oxime compound (1) having the second molecular structure represented by formula (3) is not particularly limited, but it can be produced by, for example, the methods described in JP-A-2000-80068 and JP-A-2011-178776.
[0179] Yet another example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (4). The bond represented by "*" in formula (4) is directly bonded to the bond represented by "*" in formula (1). In other words, when the second molecular structure is a structure represented by formula (4), the benzene ring having "-*" in formula (4) and the carbonyl group having "-*" in formula (1) are directly bonded.
[0180] [ka] [In formula (4), R 71 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. R 71 When the group represented by the following formula (I) has an alkyl portion, the alkyl portion may be branched or cyclic. R 71 The hydrogen atoms of the group represented by R 21 , OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R 23 ,CONR22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , N.R. 22 COR 21 , O.C.O.R. 21 , COOR 21 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , SCOR 21 , OCSR 21 , C.O.S.R. 21 , C.S.O.R. 21 , hydroxyl group, nitro group, CN, halogen atom or COOR 21 may be substituted with. R 21 , R 22 and R 23 has the same meaning as above. R 21 , R 22 or R 23 The hydrogen atom of the group represented by the formula (I) may be substituted by CN, a halogen atom, a hydroxy group or a carboxy group. R 21 , R 22 and R 23 When the group represented by the formula (I) has an alkylene portion, the alkylene portion is preferably -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-, -NR 24 COO-, -OCONR 24 It may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS- or -CSO-. R 24 has the same meaning as above. R 21 , R 22 and R 23 When the group represented by R 22 and R 23 may be joined together to form a ring. R 72, R 73 and 3 R 74 are each independently R 61 , OR 61 , S.R. 61 , C.O.R. 62 ,CONR 63 R 64 , N.R. 65 COR 61 , O.C.O.R. 61 , COOR 62 , SCOR 61 , OCSR 61 , C.O.S.R. 62 , C.S.O.R. 61 , a hydroxyl group, a nitro group, CN or a halogen atom. R 61 , R 62 , R 63 , R 64 and R 65 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. R 61 , R 62 , R 63 , R 64 or R 65 The hydrogen atoms of the group represented by OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , CN, halogen atom or COOR 21 may be substituted with. R 72 and R 73 and two R 74 may be joined together to form a ring. * represents a bond to the first molecular structure of the oxime compound (1).
[0181] R in Equation (4) 71 , R 21 , R 22 , R 23 , R 24 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of the alkyl group having 1 to 20 carbon atoms, the aryl group having 6 to 30 carbon atoms, the aralkyl group having 7 to 30 carbon atoms, and the heterocyclic group having 2 to 20 carbon atoms, which are represented by the formula (1), are R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 The example for is similar.
[0182] R in Equation (4) 22 and R 23 may be joined together to form a ring, R 22 and R 23 means that they may be taken together to form a ring with the nitrogen atom, carbon atom or oxygen atom to which they are attached. R in Equation (4) 22 and R 23 Examples of rings that may be formed by combining with each other include R 12 and R 13 and R 22 and R 23 The same is true for the ring which may be formed by combining with each other.
[0183] R in Equation (4) 72 , R 73 and R 74 Halogen atoms represented by R 71 , R 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R 64 and R 65Examples of halogen atoms which may replace the hydrogen atoms of include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.
[0184] The method for producing the oxime compound (1) having the second molecular structure represented by formula (4) is not particularly limited, and it can be produced, for example, by the methods described in WO 2017 / 051680 and WO 2020 / 004601.
[0185] Yet another example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (5). The bond represented by "*" in formula (5) is directly bonded to the bond represented by "*" in formula (1). That is, when the second molecular structure is a structure represented by formula (5), the pyrrole ring having "-*" in formula (5) and the carbonyl group having "-*" in formula (1) are directly bonded.
[0186] [ka] [In formula (5), R 81 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. R 81 When the group represented by the following formula (I) has an alkyl portion, the alkyl portion may be branched or cyclic. R 81 The hydrogen atoms of the group represented by R 21 , OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , N.R. 22 COR 21 , O.C.O.R.21 , COOR 21 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , SCOR 21 , OCSR 21 , C.O.S.R. 21 , C.S.O.R. 21 , hydroxyl group, nitro group, CN, halogen atom or COOR 21 may be substituted with. R 21 , R 22 and R 23 has the same meaning as above. R 21 , R 22 or R 23 The hydrogen atom of the group represented by the formula (I) may be substituted by CN, a halogen atom, a hydroxy group or a carboxy group. R 21 , R 22 and R 23 When the group represented by the formula (I) has an alkylene portion, the alkylene portion is preferably -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-, -NR 24 COO-, -OCONR 24 It may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS- or -CSO-. R 24 has the same meaning as above. R 21 , R 22 and R 23 When the group represented by R 22 and R 23 may be joined together to form a ring. R 82 , R 83 , R 84 , R 85 and R 86 are each independently R 61 , OR 61 , S.R. 61 , C.O.R. 62,CONR 63 R 64 , N.R. 65 COR 61 , O.C.O.R. 61 , COOR 62 , SCOR 61 , OCSR 61 , C.O.S.R. 62 , C.S.O.R. 61 , a hydroxyl group, a nitro group, CN or a halogen atom. R 61 , R 62 , R 63 , R 64 , and R 65 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. R 61 , R 62 , R 63 , R 64 or R 65 The hydrogen atoms of the group represented by OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , CN, halogen atom or COOR 21 may be substituted with. R 83 and R 84 , R 84 and R 85 and R 85 and R 86 may be joined together to form a ring. * represents a bond to the first molecular structure of the oxime compound (1).
[0187] R in Equation (5) 81 , R21 , R 22 , R 23 , R 24 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of the alkyl group having 1 to 20 carbon atoms, the aryl group having 6 to 30 carbon atoms, the aralkyl group having 7 to 30 carbon atoms, and the heterocyclic group having 2 to 20 carbon atoms, which are represented by the formula (1), are R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 The example for is similar.
[0188] R in Equation (5) 22 and R 23 may be joined together to form a ring, R 22 and R 23 means that they may be taken together to form a ring with the nitrogen atom, carbon atom or oxygen atom to which they are attached. R in Equation (5) 22 and R 23 Examples of rings that may be formed by combining with each other include R 12 and R 13 and R 22 and R 23 The same is true for the ring which may be formed by combining with each other.
[0189] R in Equation (5) 82 , R 83 , R 84 , R 85 and R 86 Halogen atoms represented by R 81 , R 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of halogen atoms which may replace the hydrogen atoms of include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.
[0190] The method for producing the oxime compound (1) having the second molecular structure represented by formula (5) is not particularly limited, but can be produced, for example, by the methods described in WO 2017 / 051680 and WO 2020 / 004601.
[0191] Yet another example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (6). The bond represented by "*" in formula (6) is directly bonded to the bond represented by "*" in formula (1). In other words, when the second molecular structure is a structure represented by formula (6), the benzene ring having "-*" in formula (6) and the carbonyl group having "-*" in formula (1) are directly bonded.
[0192] [ka] [In formula (6), 4 R's 91 , R 92 , R 93 , R 94 , R 95 , R 96 and R 97 are each independently R 61 , OR 61 , S.R. 61 , C.O.R. 62 ,CONR 63 R 64 , N.R. 65 COR 61 , O.C.O.R. 61 , COOR 62 , SCOR 61 , OCSR 61 , C.O.S.R. 62 , C.S.O.R. 61 , a hydroxyl group, a nitro group, CN or a halogen atom. R 61 , R 62 , R 63 , R 64 and R 65each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. R 61 , R 62 , R 63 , R 64 or R 65 The hydrogen atoms of the group represented by OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , CN, halogen atom or COOR 21 may be substituted with. R 21 , R 22 and R 23 has the same meaning as above. R 92 and R 93 , R 94 and R 95 , R 95 and R 96 and R 96 and R 97 may be joined together to form a ring. * represents a bond to the first molecular structure of the oxime compound (1).
[0193] R in Equation (6) 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of the alkyl group having 1 to 20 carbon atoms, the aryl group having 6 to 30 carbon atoms, the aralkyl group having 7 to 30 carbon atoms, and the heterocyclic group having 2 to 20 carbon atoms, which are represented by the formula (1), are R 11, R 12 , R 13 , R 21 , R 22 and R 23 The example for is similar.
[0194] R in Equation (6) 22 and R 23 may be joined together to form a ring, R 22 and R 23 means that they may be taken together to form a ring with the nitrogen atom, carbon atom or oxygen atom to which they are attached. R in Equation (6) 22 and R 23 Examples of rings that may be formed by combining with each other include R 12 and R 13 and R 22 and R 23 The same is true for the ring which may be formed by combining with each other.
[0195] R in Equation (6) 91 , R 92 , R 93 , R 94 , R 95 , R 96 and R 97 Halogen atoms represented by R 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of halogen atoms which may replace the hydrogen atoms of include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.
[0196] The method for producing the oxime compound (1) having the second molecular structure represented by formula (6) is not particularly limited, but can be produced, for example, by the methods described in WO 2017 / 051680 and WO 2020 / 004601.
[0197] Examples of oxime compounds other than the compound represented by formula (DA) and the oxime compound (1) include oxime compounds having a partial structure represented by the following formula (d1): * represents a bond.
[0198] [ka]
[0199] Examples of the oxime compound having a partial structure represented by formula (d1) include N-benzoyloxy-1-(4-phenylsulfanylphenyl)butan-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)-3-cyclopentylpropan-1-one-2-imine, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethan-1-imine, N-acetoxy-1-[9-ethyl-6-{2-methyl-4-(3,3-dimethyl-2-phenyl)ethyl]ethane-1-imine, and N-acetoxy-1-[9-ethyl-6-{2-methyl-4-(3,3-dimethyl-2-phenyl)ethyl]ethane-1-imine. ,4-dioxacyclopentanylmethyloxy)benzoyl}-9H-carbazol-3-yl]ethane-1-imine, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-3-cyclopentylpropan-1-imine, N-benzoyloxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-3-cyclopentylpropan-1-one-2-imine; compounds described in JP 2011-132215 A, WO 2008 / 78678, WO 2008 / 78686, and WO 2012 / 132558. Commercially available products such as Irgacure (registered trademark) OXE01, OXE02, and OXE03 (all manufactured by BASF), N-1919, NCI-930, and NCI-831 (all manufactured by ADEKA) may also be used.
[0200] Among these, the oxime compound having a partial structure represented by formula (d1) is preferably at least one selected from the group consisting of N-benzoyloxy-1-(4-phenylsulfanylphenyl)butan-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine, and N-benzoyloxy-1-(4-phenylsulfanylphenyl)-3-cyclopentylpropan-1-one-2-imine, and more preferably N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine.
[0201] The alkylphenone compound is a compound having a partial structure represented by the following formula (d2) or a partial structure represented by the following formula (d3). In these partial structures, the benzene ring may have a substituent. * represents a bond.
[0202] [ka]
[0203] Examples of the compound having the structure represented by formula (d2) include 2-methyl-2-morpholino-1-(4-methylsulfanylphenyl)propan-1-one, 2-dimethylamino-1-(4-morpholinophenyl)-2-benzylbutan-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]butan-1-one, etc. Commercially available products such as OMNIRAD (registered trademark) 369, 907, and 379 (all manufactured by IGM Resins) may also be used.
[0204] Examples of compounds having a structure represented by formula (d3) include 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]propan-1-one, 1-hydroxycyclohexyl phenyl ketone, oligomers of 2-hydroxy-2-methyl-1-(4-isopropenylphenyl)propan-1-one, α,α-diethoxyacetophenone, and benzyl dimethyl ketal.
[0205] In terms of sensitivity, the alkylphenone compound is preferably a compound having a structure represented by formula (d2).
[0206] An example of the biimidazole compound is a compound represented by the formula (d5).
[0207] [ka] [In formula (d5), R E ~R J represents an aryl group having 6 to 10 carbon atoms which may have a substituent.]
[0208] Examples of the aryl group having 6 to 10 carbon atoms include a phenyl group, a toluyl group, a xylyl group, an ethylphenyl group, and a naphthyl group, and preferably a phenyl group. Examples of the substituent include a halogen atom and an alkoxy group having 1 to 4 carbon atoms. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, and preferably a chlorine atom. Examples of the alkoxy group having 1 to 4 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, and a butoxy group, and preferably a methoxy group.
[0209] Examples of the biimidazole compound include 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(2,3-dichlorophenyl)-4,4',5,5'-tetraphenylbiimidazole (see, for example, JP-A-06-75372 and JP-A-06-75373), 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetra(alkoxyphenyl) phenyl)biimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetra(dialkoxyphenyl)biimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetra(trialkoxyphenyl)biimidazole (see, for example, JP-B-48-38403 and JP-A-62-174204), imidazole compounds in which the phenyl groups at the 4,4',5,5'-positions are substituted with carboalkoxy groups (see, for example, JP-A-7-10913), etc. Among these, the compounds represented by the following formula or mixtures thereof are preferred.
[0210] [ka]
[0211] Examples of the triazine compound include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-piperonyl-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxystyryl)-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[ 2-(5-methylfuran-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)ethenyl]-1,3,5-triazine, etc. Among them, 2,4-bis(trichloromethyl)-6-piperonyl-1,3,5-triazine is preferred.
[0212] Examples of the acylphosphine compound include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, etc. Commercially available products such as OMNIRAD (registered trademark) 819 (manufactured by IGM Resins) may also be used.
[0213] Other examples of the polymerization initiator include benzoin compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; benzophenone compounds such as benzophenone, o-benzoyl methyl benzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzophenone, and 4,4'-bis(diethylamino)benzophenone; quinone compounds such as 9,10-phenanthrenequinone, 2-ethylanthraquinone, and camphorquinone; 10-butyl-2-chloroacridone, benzyl, methyl phenylglyoxylate, and titanocene compounds.
[0214] From the viewpoint of forming a cured film having excellent patterning properties, the content of the compound represented by formula (DA) in the polymerization initiator (D) is preferably 30% by mass or more and 100% by mass or less, more preferably 50% by mass or more and 100% by mass or less, even more preferably 70% by mass or more and 100% by mass or less, still more preferably 80% by mass or more and 100% by mass or less, especially preferably 90% by mass or more and 100% by mass or less, and particularly preferably 95% by mass or more and 100% by mass or less, and may be 100% by mass.
[0215] The content of the polymerization initiator (D) in the composition is, for example, 0.01 mass% or more and 20 mass% or less, relative to the total amount of solids in the composition. From the viewpoint of increasing the sensitivity of the composition and increasing the luminescence intensity and heat resistance of the film, the content is preferably 0.1 mass% or more and 15 mass% or less, more preferably 0.2 mass% or more and 10 mass% or less, even more preferably 0.3 mass% or more and 8 mass% or less, still more preferably 0.5 mass% or more and 5 mass% or less, and particularly preferably 3 mass% or less.
[0216] The content of the polymerization initiator (D) is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less, relative to 100 parts by mass of the polymerizable compound (C). When the content of the polymerization initiator (D) is within the above range, a composition capable of forming a cured film having an excellent film retention rate and a cured film having excellent heat resistance can be obtained.
[0217] <Polymerization initiator aid (D1)> The curable composition may further contain a polymerization initiator (D1) together with the polymerization initiator (D). The polymerization initiator (D1) is a compound used to promote the polymerization of the polymerizable compound (C) initiated by the polymerization initiator (D), or a sensitizer. Examples of the polymerization initiator (D1) include an amine compound, an alkoxyanthracene compound, a thioxanthone compound, and a carboxylic acid compound.
[0218] Examples of the amine compound include triethanolamine, methyldiethanolamine, triisopropanolamine, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, 2-dimethylaminoethyl benzoate, 2-ethylhexyl 4-dimethylaminobenzoate, N,N-dimethyl-p-toluidine, 4,4'-bis(dimethylamino)benzophenone (commonly known as Michler's ketone), 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(ethylmethylamino)benzophenone, etc., and among these, 4,4'-bis(diethylamino)benzophenone is preferred. Commercially available products such as EAB-F (manufactured by Hodogaya Chemical Co., Ltd.) may also be used.
[0219] Examples of the alkoxyanthracene compound include 9,10-dimethoxyanthracene, 2-ethyl-9,10-dimethoxyanthracene, 9,10-diethoxyanthracene, 2-ethyl-9,10-diethoxyanthracene, 9,10-dibutoxyanthracene, and 2-ethyl-9,10-dibutoxyanthracene.
[0220] Examples of thioxanthone compounds include 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-diethylthioxanthone, 2,4-dichlorothioxanthone, and 1-chloro-4-propoxythioxanthone.
[0221] Examples of the carboxylic acid compound include phenylsulfanylacetic acid, methylphenylsulfanylacetic acid, ethylphenylsulfanylacetic acid, methylethylphenylsulfanylacetic acid, dimethylphenylsulfanylacetic acid, methoxyphenylsulfanylacetic acid, dimethoxyphenylsulfanylacetic acid, chlorophenylsulfanylacetic acid, dichlorophenylsulfanylacetic acid, N-phenylglycine, phenoxyacetic acid, naphthylthioacetic acid, N-naphthylglycine, and naphthoxyacetic acid.
[0222] When the curable composition contains the polymerization initiation aid (D1), the content of the polymerization initiation aid (D1) in the curable composition is preferably 0.1 parts by mass or more and 300 parts by mass or less, more preferably 0.1 parts by mass or more and 200 parts by mass or less, relative to 100 parts by mass of the polymerizable compound (C). The content of the polymerization initiation aid (D1) in the curable composition is preferably 0.1 parts by mass or more and 30 parts by mass or less, more preferably 1 part by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the total amount of the resin (B) and the polymerizable compound (C). When the content of the polymerization initiation aid (D1) is within the above range, the sensitivity of the curable composition can be further increased.
[0223] <Antioxidants (E)> The curable composition may further comprise an antioxidant (E). The antioxidant (E) is not particularly limited as long as it is an antioxidant generally used industrially, and examples of the antioxidant that can be used include phenol-based antioxidants, phosphorus-based antioxidants, phosphorus / phenol complex antioxidants, and sulfur-based antioxidants. Two or more types of antioxidants (E) may be used in combination.
[0224] The phosphorus / phenol complex type antioxidant may be a compound having one or more phosphorus atoms and one or more phenol structures in the molecule. Among them, from the viewpoint of the developability and luminescence intensity of the cured film, it is preferable that the antioxidant (E) contains a phosphorus / phenol complex type antioxidant.
[0225] Examples of phenol-based antioxidants include Irganox (registered trademark) 1010 (Irganox 1010: pentaerythritol tetrakis [3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], manufactured by BASF Ltd.), Irganox 1076 (Irganox 1076: octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, manufactured by BASF Ltd.), Irganox 1330 (Irganox 1330: 3,3',3'',5,5',5''-hexa-tert-butyl-a,a',a''-(mesitylene-2,4,6-triyl) tri-p-cresol, manufactured by BASF Ltd.), and Irganox 3114 (Irganox 3114: 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Co., Ltd.), 3790 (Irganox 3790: 1,3,5-tris((4-tert-butyl-3-hydroxy-2,6-xylyl)methyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Co., Ltd.), 1035 (Irganox 1035: thiodiethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], manufactured by BASF Co., Ltd.), 1135 (Irganox 1135: 3,5-bis(1,1-dimethylethyl)-4-hydroxy-C7-C9 side chain alkyl ester of benzenepropanoic acid, manufactured by BASF Co., Ltd.), 1520L (Irganox 1520L: 4,6-bis(octylthiomethyl)-o-cresol, manufactured by BASF Co., Ltd.), 3125 (Irganox 3125, manufactured by BASF Co., Ltd.), 565 (Irganox 565: 2,4-bis(n-octylthio)-6-(4-hydroxy-3',5'-di-tert-butylanilino)-1,3,5-triazine, manufactured by BASF Co., Ltd.), Adeka STAB (registered trademark) AO-80 (Adeka STAB AO-80: 3,9-bis(2-(3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy)-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro(5,5) Undecane (manufactured by ADEKA Co., Ltd.), Sumilizer (registered trademark) BHT, Sumilizer GA-80, and Sumilizer GS (all manufactured by Sumitomo Chemical Co., Ltd.), Cyanox (registered trademark) 1790 (manufactured by Cytec Co., Ltd.), and Vitamin E (manufactured by Eisai Co., Ltd.).
[0226] Examples of phosphorus-based antioxidants include Irgafos (registered trademark) 168 (Irgafos 168: tris(2,4-di-tert-butylphenyl)phosphite, manufactured by BASF Co., Ltd.), Irgafos 12 (Irgafos 12: tris[2-[[2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphine-6-yl]oxy]ethyl]amine, manufactured by BASF Co., Ltd.), Irgafos 38 (Irgafos 38: bis(2,4-bis(1,1-dimethylethyl)-6-methylphenyl)ethyl ester phosphorous acid, manufactured by BASF Co., Ltd.), Adeka STAB (registered trademark) 329K, Adeka STAB PEP36, Adeka STAB PEP-8 (all manufactured by ADEKA Co., Ltd.), Sandstab Examples of such antibacterial agents include P-EPQ (manufactured by Clariant), Weston (registered trademark) 618, Weston 619G (all manufactured by GE), and Ultranox 626 (manufactured by GE).
[0227] Examples of phosphorus / phenol complex antioxidants include Sumilizer (registered trademark) GP (6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenz[d,f][1.3.2]dioxaphosphepine) (manufactured by Sumitomo Chemical Co., Ltd.).
[0228] Examples of the sulfur-based antioxidant include dialkyl thiodipropionate compounds such as dilauryl, dimyristyl, and distearyl thiodipropionate, and β-alkyl mercaptopropionate compounds of polyols such as tetrakis[methylene(3-dodecylthio)propionate]methane.
[0229] The content of the antioxidant (E) in the curable composition is, for example, 0.05 mass% or more and 20 mass% or less, preferably 0.1 mass% or more and 10 mass% or less, more preferably 0.5 mass% or more and 7 mass% or less, and even more preferably 1 mass% or more and 5 mass% or less, relative to the total amount of solids in the curable composition.
[0230] The content of the antioxidant (E) in the curable composition is, for example, 1 part by mass or more and 50 parts by mass or less relative to 100 parts by mass of the resin (B). From the viewpoint of the amount of light emission and heat resistance of the cured film, the content is preferably 5 parts by mass or more and 40 parts by mass or less, more preferably 7 parts by mass or more and 30 parts by mass or less, and even more preferably 9 parts by mass or more and 25 parts by mass or less.
[0231] The content ratio of the antioxidant (E) to the polymerization initiator (D) in the curable composition (antioxidant (E) / polymerization initiator (D)), in terms of mass ratio, is preferably greater than 1, more preferably 1.1 or more, and even more preferably 1.2 or more, from the viewpoint of increasing the luminescence intensity of the cured film.
[0232] <Solvent (F)> The solvent (F) is not particularly limited as long as it dissolves the polymerizable compound (C), the polymerization initiator (D), and the resin (B) used as necessary, and a solvent commonly used in the field can be used. For example, ester solvents (solvents containing -COO- in the molecule and not containing -O-), ether solvents (solvents containing -O- in the molecule and not containing -COO-), ether ester solvents (solvents containing -COO- and -O- in the molecule), ketone solvents (solvents containing -CO- in the molecule and not containing -COO-), alcohol solvents (solvents containing OH in the molecule and not containing -O-, -CO- and COO-), aromatic hydrocarbon solvents, amide solvents, dimethyl sulfoxide, etc. can be mentioned.
[0233] Examples of the ester solvent include methyl lactate, ethyl lactate, n-butyl lactate, methyl 2-hydroxyisobutanoate, ethyl acetate, n-butyl acetate, isobutyl acetate, n-pentyl formate, isopentyl acetate, n-butyl propionate, isopropyl butyrate, ethyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, cyclohexyl acetate, and γ-butyrolactone.
[0234] Examples of the ether solvent include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, 3-methoxy-1-butanol, 3-methoxy-3-methylbutanol, tetrahydrofuran, tetrahydropyran, 1,4-dioxane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, anisole, phenetole, and methylanisole.
[0235] The ether ester solvents include methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, ethyl ethoxyacetate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, methyl 2-ethoxypropionate, ethyl 2-ethoxypropionate, methyl 2-methoxy-2-methyl ... Examples of the alkyl ether acetates include ethyl methoxy-2-methylpropionate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate.
[0236] Examples of ketone solvents include 4-hydroxy-4-methyl-2-pentanone, acetone, 2-butanone, 2-heptanone, 3-heptanone, 4-heptanone, 4-methyl-2-pentanone, cyclopentanone, cyclohexanone, and isophorone.
[0237] Examples of the alcohol solvent include methanol, ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, propylene glycol, and glycerin.
[0238] Aromatic hydrocarbon solvents include benzene, toluene, xylene, and mesitylene.
[0239] Examples of the amide solvent include N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.
[0240] As the solvent (F), propylene glycol monomethyl ether acetate, ethyl lactate, propylene glycol monomethyl ether, cyclohexyl acetate, ethyl 3-ethoxypropionate, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, 4-hydroxy-4-methyl-2-pentanone or toluene, or a mixture of two or more of these, is preferred.
[0241] The solvent (F) is a component other than the solid content, and for example, the solvent contained in the quantum dots (A) and the resin (B) is also included in the solvent (F). The content of the solvent (F) in the curable composition is the ratio of the total mass of all the solvents contained in the composition to the total amount of the composition, and is, for example, 40% by mass or more and 95% by mass or less, preferably 55% by mass or more and 90% by mass or less, relative to the total amount of the curable composition. In other words, the solid content of the curable composition is preferably 5% by mass or more and 60% by mass or less, more preferably 10% by mass or more and 45% by mass or less. When the content of the solvent (F) is within the above range, the flatness of the composition layer during application is improved, and a cured film with an appropriate thickness tends to be easily formed.
[0242] <Leveling agent (G)> The curable composition may further comprise a leveling agent (G). The leveling agent (G) may be a silicone surfactant, a fluorine surfactant, or a silicone surfactant having a fluorine atom. These may have a polymerizable group in the side chain. From the viewpoint of the developability and luminescence intensity of the cured film, the leveling agent (G) is preferably a fluorine surfactant.
[0243] Examples of silicone surfactants include surfactants having a siloxane bond in the molecule.Specific examples include Toray Silicone DC3PA, SH7PA, DC11PA, SH21PA, SH28PA, SH29PA, SH30PA, and SH8400 (trade name: manufactured by Toray Dow Corning Co., Ltd.), KP321, KP322, KP323, KP324, KP326, KP340, and KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.), TSF400, TSF401, TSF410, TSF4300, TSF4440, TSF4445, TSF4446, TSF4452, and TSF4460 (manufactured by Momentive Performance Materials Japan LLC).
[0244] Examples of fluorine-based surfactants include surfactants having a fluorocarbon chain in the molecule.Specific examples include Fluorad (registered trademark) FC430, FC431 (manufactured by Sumitomo 3M Limited), Megafac (registered trademark) F142D, F171, F172, F173, F177, F183, F554, F575, R30, RS-718-K (manufactured by DIC Corporation), F-top (registered trademark) EF301, EF303, EF351, EF352 (manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd.), Surflon (registered trademark) S381, S382, SC101, SC105 (manufactured by Asahi Glass Co., Ltd.), and E5844 (manufactured by Daikin Fine Chemicals Research Institute Co., Ltd.).
[0245] Examples of silicone surfactants having fluorine atoms include surfactants having a siloxane bond and a fluorocarbon chain in the molecule, such as Megafac (registered trademark) R08, BL20, F475, F477, and F443 (manufactured by DIC Corporation).
[0246] When the curable composition contains a leveling agent (G), the content of the leveling agent (G) in the curable composition is, for example, 0.001% by mass or more and 1.0% by mass or less, preferably 0.005% by mass or more and 0.75% by mass or less, more preferably 0.01% by mass or more and 0.5% by mass or less, and even more preferably 0.03% by mass or more and 0.5% by mass or less, based on the total amount of the curable composition. When the content of the leveling agent (G) is within the above range, the flatness of the cured film can be improved.
[0247] <Light scattering agent (H)> The curable composition may further contain a light scattering agent (H). Examples of the light scattering agent (H) include metal or metal oxide particles, glass particles, and the like. Metal oxides include TiO 2 , SiO 2 , BaTiO 3 , ZnO, etc. The particle size of the light scattering agent (H) is, for example, about 0.03 μm or more and 20 μm or less, preferably 0.05 μm or more and 1 μm or less, and more preferably 0.05 μm or more and 0.5 μm or less.
[0248] The light scattering agent (H) may be a dispersion in advance in a part or the whole of the solvent (F) using a dispersant. Commercially available dispersants can be used as the dispersant. Examples of commercially available products include: DISPERBYK-101, 102, 103, 106, 107, 108, 109, 110, 111, 116, 118, 130, 140, 154, 161, 162, 163, 164, 165, 166, 170, 171, 174, 180, 181, 182, 183, 184, 185, 190, 192, 20 00, 2001, 2020, 2025, 2050, 2070, 2095, 2150, 2155;ANTI-TERRA-U, U100, 203, 204, 250;BY K-P104, P104S, P105, 220S, 6919; BYK-LPN6919, 21116; LACTIMON, LACTIMON-WS; Bykumen, etc.; Lubrizol Japan SOLSPERSE-3000, 9000, 13000, 13240, 13650, 13940, 16000, 17000, 18000, 20000, 21000, 24000, 26000, 27000, 28000, 31845, 32000, 32500, 32550, 33500, 32600, 34750, 35100, 36600, 38500, 41000, 41090, 53095, 55000, 76500, etc. BASF EFKA-46, 47, 48, 452, 4008, 4009, 4010, 4015, 4020, 4047, 4050, 4055, 4060, 4080, 4400, 4401, 4402, 4403, 4406, 4408, 4300, 4310, 4320, 4330, 4340, 450, 451, 453, 4540, 4550, 4560, 4800, 5010, 5065, 5066, 5070, 7500, 7554, 1101, 120, 150, 1501, 1502, 1503, etc.; Examples of such polyvinyl chloride resins include Ajisper PA111, PB711, PB821, PB822, and PB824 manufactured by Ajinomoto Fine-Techno Co., Ltd.
[0249] The content of the light scattering agent (H) in the curable composition is, for example, from 0.001% by mass to 50% by mass, based on the total amount of solids in the curable composition, and from the viewpoints of the developability and luminescence intensity of the cured film, is preferably from 1% by mass to 30% by mass, and more preferably from 2% by mass to 10% by mass.
[0250] The curable composition may further contain additives known in the technical field, such as a polymerization inhibitor, a filler, another polymer compound, an adhesion promoter, a light stabilizer, and a chain transfer agent, as necessary.
[0251] <Method of producing curable composition> The method for producing the curable composition may include a step of mixing the quantum dots (A), the polymerizable compound (C), the polymerization initiator (D), and other components used as necessary. The method for producing the curable composition may further include a step of preparing the resin (B).
[0252] <Cured film> The cured film according to the present invention can be obtained by applying the curable composition according to the present invention to a substrate and curing the composition by the action of light and, if necessary, by the action of heat. The cured film contains the quantum dots (A) contained in the curable composition. The cured film also contains a cured reaction product of the polymerizable compound (C) and the polymerization initiator (D) contained in the curable composition. The cured reaction product is a substance containing a structure resulting from the structure of the polymerizable compound (C) and the polymerization initiator (D). The structure resulting from the structure of the polymerizable compound (C) and the polymerization initiator (D) is, for example, a skeletal structure or a part thereof other than the curing reaction site of the polymerizable compound (C) and the polymerization initiator (D). The cured film also contains a resin (B) used in the curable composition as necessary.
[0253] The cured film may be formed on the entire surface of the substrate, or may be formed on a part of the substrate (i.e., a cured pattern). As described above, the cured pattern is one aspect of the cured film, and refers to a cured film formed in a pattern.
[0254] Examples of the method for forming a cured film on a part of the substrate include a photolithography method, an inkjet method, a printing method, etc. Among them, the photolithography method is preferable. The photolithography method is a method in which a curable composition is applied to a substrate, dried as necessary to form a composition layer, and the composition layer is exposed through a photomask and developed.
[0255] Examples of a method for forming a cured film over the entire surface of a substrate include a method in which a curable composition is applied to a substrate, and dried as necessary to form a composition layer, and then the composition layer is heated and / or the entire surface of the composition layer is exposed to light.
[0256] Examples of the substrate include glass plates such as quartz glass, borosilicate glass, alumina silicate glass, and soda lime glass with a silica-coated surface; resin plates such as polycarbonate, polymethyl methacrylate, and polyethylene terephthalate; silicon; and the above-mentioned substrates on which thin films of aluminum, silver, and silver / copper / palladium alloys are formed.
[0257] The formation of a cured pattern by photolithography can be carried out using known or conventional devices and conditions. For example, the pattern can be produced as follows.
[0258] First, a curable composition is applied onto a substrate, and volatile components such as a solvent are removed by heating and drying (pre-baking) and / or drying under reduced pressure to obtain a composition layer. Examples of the application method include spin coating, slit coating, and slit and spin coating.
[0259] The temperature when drying by heating is preferably from 30° C. to 120° C., and more preferably from 50° C. to 110° C. The heating time is preferably from 10 seconds to 60 minutes, and more preferably from 30 seconds to 30 minutes. When drying under reduced pressure is performed, it is preferable to perform the drying under a pressure of 50 Pa or more and 150 Pa or less at a temperature range of 20° C. or more and 25° C. or less.
[0260] The film thickness of the composition layer is not particularly limited and may be appropriately selected depending on the film thickness of the desired cured pattern, and is, for example, from 1 μm to 20 μm, preferably from 1.5 μm to 18 μm, more preferably from 2 μm to 14 μm, and even more preferably from 2 μm to 12 μm.
[0261] The composition layer is then exposed through a photomask to form a desired cured pattern, the shape of the pattern on the photomask being not particularly limited.
[0262] The light source used for exposure is preferably a light source that generates light having a wavelength of 250 nm or more and 450 nm or less. For example, from the light having the wavelength, light having a wavelength of around 436 nm, around 408 nm, or around 365 nm may be selectively extracted by a bandpass filter according to the absorption wavelength of the polymerization initiator (D). Specific examples of the light source include a mercury lamp, a light-emitting diode, a metal halide lamp, and a halogen lamp.
[0263] It is preferable to use an exposure device such as a mask aligner or a stepper, since it is possible to uniformly irradiate the entire exposure surface with parallel light rays and to accurately align the photomask with the substrate on which the composition layer is formed. The exposed composition layer is cured by polymerization of the polymerizable compound (C) and the like contained in the composition layer.
[0264] By contacting the composition layer after exposure with a developer and developing it, the unexposed portion of the composition layer is dissolved and removed in the developer, and a cured pattern is obtained. Examples of the developer include an aqueous solution of an alkaline compound such as potassium hydroxide, sodium bicarbonate, sodium carbonate, and tetramethylammonium hydroxide, and an organic solvent. The concentration of the alkaline compound in the aqueous solution is preferably 0.01% by mass or more and 10% by mass or less, and more preferably 0.03% by mass or more and 5% by mass or less. Examples of the organic solvent include the same as the above-mentioned solvent (F). The developer may contain a surfactant.
[0265] The developing method may be any of a puddle method, a dipping method, a spray method, etc. Furthermore, the substrate may be inclined at an arbitrary angle during the developing.
[0266] It is preferable to further heat (post-bake) the cured pattern obtained by development. The heating temperature is preferably 150°C or more and 250°C or less, more preferably 160°C or more and 235°C or less. The heating time is preferably 1 minute or more and 120 minutes or less, more preferably 10 minutes or more and 60 minutes or less. By heating after development, the polymerization of the unreacted polymerizable compound (C) contained in the cured pattern can be promoted, so that a cured pattern with better chemical resistance can be obtained. Even when development is not performed, it is preferable to further heat (post-bake) the exposed composition layer.
[0267] By irradiating the cured film with ultraviolet light or visible light, the cured film can emit light with a wavelength different from that of the irradiated light. By selecting the components and particle size of the quantum dots (A) in the curable composition used to form the cured film, the wavelength of the emitted light can be adjusted. Since the cured film has the function of converting the wavelength of the irradiated light as described above, it can be used as a color conversion layer (wavelength conversion film) of a display device.
[0268] The cured film can exhibit good emission intensity. The cured film preferably has an emission intensity of 400 mW·sr as measured according to the measurement method in the Examples section below. -1 m -2 nm -1 More preferably, 500 mW·sr -1 m -2 nm -1 More preferably, 600 mW·sr -1 m -2 nm -1 More preferably, 650 mW·sr -1 m -2 nm -1 More preferably, 700 mW·sr -1 m -2 nm -1 More preferably, 750 mW·sr -1 m -2 nm -1 More preferably, 800 mW·sr -1 m -2 nm -1 In order to obtain the above-mentioned luminescence intensity of the cured film, the content of the quantum dots (A) relative to the total amount of solids in the curable composition is preferably from 20% by mass to 80% by mass, particularly preferably from 30% by mass to 70% by mass.
[0269] The curable composition according to the present invention can appropriately form a pattern, and is therefore useful as a color conversion layer for a display device, particularly a liquid crystal display device, an organic EL display device, or an inorganic EL display device. Examples of such a display device include the display devices described in JP-A-2006-309219, JP-A-2006-310303, JP-A-2013-15812, JP-A-2009-251129, and JP-A-2014-2363.
[0270] The display device includes at least a light source and the cured film. The display device is not particularly limited, and may further include layers such as a light absorbing layer, a light reflecting member (such as a reflecting film), a diffusion film, a brightness enhancing section, a prism sheet, a light guide plate, and a medium material layer between elements.
[0271] The light absorbing layer is a layer having wavelength selectivity that transmits light in a specific wavelength range and absorbs light in the other wavelength range. The light absorbing layer is usually a layer containing a colorant such as a dye or pigment, and can be disposed on the cured film. As the light absorbing layer, a conventionally known color filter can be used.
[0272] The light reflecting member is a member for reflecting light from a light source toward the cured film, and may be a reflecting mirror, a film of reflecting particles, a reflecting metal film, a reflector, etc. The diffusion film is a film for diffusing light from a light source or light emitted from the cured film, and may be an amplifying diffusion film, etc. The brightness enhancing portion is a member for reflecting a portion of light back toward the direction from which the light was transmitted.
[0273] Typically, the prism sheet has a base portion and a prism portion. The base portion may be omitted depending on the adjacent member. The prism sheet can be attached to the adjacent member via any suitable adhesive layer (e.g., an adhesive layer, a pressure-sensitive adhesive layer). The prism sheet is configured by arranging a plurality of unit prisms that are convex on the opposite side (back side) from the viewing side in parallel. By arranging the convex portion of the prism sheet facing the back side, the light that passes through the prism sheet is easily concentrated. Furthermore, by arranging the convex portion of the prism sheet facing the back side, less light is reflected without entering the prism sheet compared to when the convex portion is arranged facing the viewing side, and a display device with high brightness can be obtained.
[0274] As the light guide plate, any appropriate light guide plate can be used, for example, a light guide plate having a lens pattern formed on the back surface side so as to be able to deflect light from the lateral direction in the thickness direction, or a light guide plate having a prism shape or the like formed on the back surface side and / or the viewing side can be used.
[0275] The display device may include a layer of one or more media materials in the optical path between adjacent elements (layers), which may include any suitable material, including, but not limited to, vacuum, air, gas, optical material, adhesive, optical adhesive, glass, polymer, solid, liquid, gel, curable material, optical bonding material, index matching or index mismatching material, index gradient material, cladding or anti-cladding material, spacer, silica gel, brightness enhancing material, scattering or diffusing material, reflective or anti-reflective material, wavelength selective material, wavelength selective anti-reflective material, or other suitable media known in the art.
[0276] Specific examples of the display device include those equipped with wavelength conversion materials for EL displays and liquid crystal displays.Specific examples include a display device in which the above-mentioned cured film as a wavelength conversion layer is disposed between a blue light source (A) and a light guide plate along the end face (side face) of the light guide plate, forming a backlight (on-edge type backlight) that emits white light, and a light absorbing layer is disposed on the light guide plate side; a display device in which the above-mentioned cured film as a wavelength conversion layer is disposed on a light guide plate, forming a backlight (surface mount type backlight) that emits light irradiated to the wavelength conversion layer from a blue light source placed on the end face (side face) of the light guide plate through the light guide plate as white light, and a light absorbing layer is disposed on the wavelength conversion layer; a display device in which the above-mentioned cured film is disposed near the light emitting part of the blue light source as a wavelength conversion layer, forming a backlight (on-chip type backlight) that emits irradiated light as white light, and a light absorbing layer is disposed on the wavelength conversion layer, and the like. EXAMPLES
[0277] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.
[0278] <Evaluation of film patterning properties> The obtained pattern was observed using a microscope (magnification: 1000 times; VHX-2000; manufactured by Keyence Corporation), and the patterning property was evaluated according to the following evaluation criteria. The results are shown in Table 1. A: The pattern is formed in lines according to the mask. B: Other than A (There are some areas where the spaces are not properly formed, there are some areas where the line pattern is not properly formed or is collapsed, etc.)
[0279] <Evaluation of the luminescence intensity of the film> The backlight unit was made by placing a light diffusion plate on a backlight that used a blue LED lamp with a peak emission wavelength of 450 nm as a point light source. The backlight unit was placed with the light diffusion plate facing upwards, and a spectroradiometer (Topcon Corporation's "SR-UL1R") was installed 60 cm above the surface of the light diffusion plate. A substrate having a cured film made from the composition was placed on the diffusion plate. In this state, the backlight was turned on, and the light emitted from the cured film was measured as the integrated radiant flux in the wavelength range of 480 nm to 780 nm, and the luminous intensity L of the cured film [mW·sr -1 m -2 nm -1 The obtained luminescence intensity L was evaluated according to the following evaluation criteria. S: 790mW·sr -1 m -2 nm -1 End A:740mW·sr -1 m -2 nm -1 More than 790mW sr -1 m -2 nm -1 less than B: 700mW·sr -1 m -2 nm -1 More than 740mW sr -1 m -2 nm -1 less than
[0280] <Weight average molecular weight of resin (Mw)> The weight average molecular weight (Mw) of the resin (B-1) was measured by a GPC method under the following conditions. Equipment: K2479 (Shimadzu Corporation) Column: SHIMADZU Shim-pack GPC-80M Column temperature: 40°C Solvent: Tetrahydrofuran Flow rate; 1.0mL / min Detector: RI Calibration standard material: TSK STANDARD POLYSTYRENE F-40, F-4, F-288, A-2500, A-500 (manufactured by Tosoh Corporation)
[0281] <Acid value of resin> 3 g of the resin (B-1) solution was precisely weighed and dissolved in a mixed solvent of 90 g of acetone and 10 g of water. Using a 0.1 N KOH aqueous solution as a titrant, the acid value of the resin (B-1) solution was measured with an automatic titrator (manufactured by Hiranuma Sangyo Co., Ltd., product name: COM-555). The acid value per 1 g of solids (AV) was calculated from the acid value of the solution and the solids content of the solution.
[0282] (Production Example 1: Preparation of Dispersion of Quantum Dots (A-1)) A toluene dispersion of InP / ZnSeS quantum dots coordinated with oleic acid as an organic ligand (G-1) was prepared. The dispersion was distilled under reduced pressure to remove the toluene. 70 parts of cyclohexyl acetate were added to 30 parts of solids to obtain a dispersion of quantum dots (A-1) (solids 30%).
[0283] (Production Example 2: Preparation of Dispersion of Light Scattering Agent (H-1)) To 70 parts of titanium oxide nanoparticles, 3 parts of DISPERBYK21116 (manufactured by BYK Japan) in terms of solid content and propylene glycol monomethyl ether acetate (hereinafter referred to as "PGMEA") were added so that the total amount became 100 parts, and the mixture was stirred with a paint shaker until sufficiently dispersed to obtain a dispersion liquid (solid content 73%) of light scattering agent (H-1).
[0284] (Production Example 3: Preparation of Resin (B-1) Solution) 110 parts of PGMEA was placed in a flask equipped with a stirrer, a reflux condenser with a thermometer, a dropping funnel, and a nitrogen inlet tube, and then stirred while replacing with nitrogen and heated to 80° C. A solution of 25 parts of dicyclopentanyl methacrylate, 23 parts of methyl methacrylate, 19 parts of methacrylic acid, and 10 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) dissolved in 110 parts of PGMEA was dropped from the dropping funnel into the flask, and then stirred at 80° C. for 3 hours. Next, 16 parts of glycidyl methacrylate, 0.4 parts of 2,2'-methylenebis(4-methyl-6-tert-butylphenol), and 0.8 parts of triphenylphosphine were added to the flask, and the mixture was heated to 110°C and stirred for 8 hours to react the carboxylic acid and epoxy group in the polymer, thereby introducing a polymerizable unsaturated bond. Next, 17 parts of 1,2,3,6-tetrahydrophthalic anhydride were added and the reaction was continued for 3 hours to introduce a carboxylic acid group into the side chain. The reaction solution was cooled to room temperature to obtain a resin (B-1) solution. The resin (B-1) had a weight average molecular weight of 8,400 in terms of standard polystyrene, an acid value of 120 mgKOH / g, and the solid content in the resin (B-1) solution was 40 mass %.
[0285] <Examples 1 to 4, Comparative Examples 1 to 2> A curable composition was prepared by mixing the dispersion of the quantum dots (A-1) obtained in Production Example 1, the dispersion of the light scattering agent (H-1) obtained in Production Example 2, the resin (B-1) solution obtained in Production Example 3, and the other components shown in Table 1 in predetermined amounts.
[0286] The content of each component in the curable composition calculated from the amount added is as shown in Table 1. In Table 1, the contents of the components other than the solvent (F) are calculated as solid contents (unit: parts by mass). The unit of the content of the solvent (F) is parts by mass. For example, the quantum dots (A-1) are blended as a dispersion of the quantum dots (A-1) in the preparation of the curable composition, and the content shown in Table 1 is the amount of the quantum dots (A-1) themselves contained in the solution. The solvent (F) in Table 1 includes the solvent contained in the dispersion or solution used in the preparation of the curable composition.
[0287] [Table 1]
[0288] Details of the abbreviations of the components shown in Table 1 are as follows. Polymerizable compound (C-1): ARONIX (registered trademark) M-510 (carboxy group-containing multifunctional (meth)acrylate, manufactured by Toagosei Co., Ltd., solid content 100%) Polymerizable compound (C-2): A-9550 (dipentaerythritol polyacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd., solid content 100%) Polymerization initiator (D-1): a compound represented by the following formula (DA-1) Polymerization initiator (D-2): Irgacure (registered trademark) OXE02 (manufactured by BASF), a compound represented by the following formula (DA-2) [ka] Antioxidant (E-1): Sumilizer-GP (phosphorus / phenol complex antioxidant, manufactured by Sumitomo Chemical Co., Ltd., solid content 100%) Solvent (F-1): A mixture of PGMEA (propylene glycol monomethyl ether acetate) and cyclohexyl acetate Leveling agent (G-1): SH8400 (silicone-based leveling agent, manufactured by Dow Corning Toray Co., Ltd., solid content 100%) Dispersant (I-1): DISPERBYK21116 (manufactured by BYK Japan)
[0289] The composition was applied by spin coating onto a 5 cm square glass substrate (Eagle XG; Corning Incorporated) so that the thickness after post-baking would be 8.0 μm, and then pre-baked in a clean oven at 100° C. for 3 minutes to obtain a composition layer. After cooling, the substrate was exposed to light at 200 mJ / cm 2 in the air using an exposure machine (UPE-1255MA; Ushio Lighting Co., Ltd.) with a distance of 150 μm between the substrate on which the composition layer was formed and a quartz glass photomask. 2The layer was irradiated with light at an exposure dose of 1000 nm (based on wavelength 365 nm). A photomask for forming a 1:1 line and space pattern of 20 μm was used. The composition layer after the light irradiation was developed by immersing it in an aqueous solution containing 0.14% nonionic surfactant and 0.048% potassium hydroxide at 25° C. for 20 seconds, washed with water, and then post-baked in an oven at 180° C. for 30 minutes to obtain a pattern made of a cured film in which a line and space pattern (having 10 lines and 10 spaces) with a line width of 20 μm was formed.
[0290] The patterning ability and luminescence intensity of the obtained cured films were measured and evaluated as described above. The results are also shown in Table 1. Note that in Comparative Example 1 and Comparative Example 2, the luminescence intensity was not evaluated because a suitable cured pattern was not obtained.
Claims
1. A composition comprising quantum dots (A), a polymerizable compound (C) and a polymerization initiator (D), The curable composition, wherein the polymerization initiator (D) comprises a compound represented by formula (DA): 【Chemistry 1】 [In the formula, R d1 represents a branched hydrocarbon group having 3 to 20 carbon atoms which may have a substituent. R d2 ~R d5 each independently represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. n represents an integer of 0 to 4. The —CH contained in the hydrocarbon group 2 - may be replaced by -O-, -S-, -CO- or -OCO-.]
2. The curable composition according to claim 1 , wherein the polymerizable compound (C) contains a compound (Ca) having three or more ethylenically unsaturated bonds in the molecule and having an acidic functional group.
3. The curable composition according to claim 1 , further comprising a resin (B).
4. The curable composition according to claim 3, wherein the acid value of the resin (B) is from 30 mgKOH / g to 150 mgKOH / g based on the solid content.
5. The curable composition according to claim 3 , wherein the content of the quantum dots (A) is 30% by mass or more and 150% by mass or less based on the total amount of the resin (B) and the polymerizable compound (C).
6. R d1 The curable composition according to claim 1, wherein is a branched, saturated hydrocarbon group having 3 to 20 carbon atoms which may have a substituent.
7. R d2 ~R d5 each independently represents a saturated hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or an unsaturated hydrocarbon group having 2 to 20 carbon atoms which may have a substituent.
8. A cured film formed from the curable composition according to any one of claims 1 to 7.
9. A display device comprising the cured film according to claim 8.
Citation Information
Patent Citations
Curable composition
WO2016035603A1