R-t-b based permanent magnet
Patent Information
- Application Number
- JP2024015723
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-23
- Filing Date
- 2024-02-05
- Publication Date
- 2024-10-07
AI Technical Summary
【0009】 上記の目的を達成するため、本開示の他の一側面に係るR-T-B系永久磁石は、R2T14B型結晶構造を有する結晶粒子を含む主相粒子、および、隣り合う2つ以上の前記主相粒子によって形成される粒界を有するR-T-B系永久磁石であって、 前記粒界中に、R-Fe-Co-Ga-Al濃縮部を有し、 前記R-Fe-Co-Ga-Al濃縮部は、Feを含有し、希土類元素の濃度が主相粒子における希土類元素の平均濃度よりも高く、Coの濃度が主相粒子におけるCoの平均濃度よりも高く、Gaの濃度が主相粒子におけるGaの平均濃度よりも高く、かつ、Alの濃度が主相粒子におけるAlの平均濃度よりも高い部分であり、 重希土類元素の含有量が0.30質量%以下(0質量%を含まない)である。
Smart Images

Figure 2024137722000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to RTB based permanent magnets. [Background technology]
[0002] Patent Document 1 discloses an RTB permanent magnet that has a low Co content and is excellent in magnetic properties and corrosion resistance. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-161812 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of one aspect of the present disclosure is to provide an RTB permanent magnet that has excellent corrosion resistance and magnetic properties (particularly coercive force at room temperature and at high temperatures) even with a small content of heavy rare earth elements. [Means for solving the problem]
[0005] In order to achieve the above object, an RTB permanent magnet according to one aspect of the present disclosure contains at least rare earth elements, Fe, Co, Al, Zr, Ga, B, and C, Contains heavy rare earth elements as rare earth elements, The content of rare earth elements is 28.50 mass% or more and 31.50 mass% or less, The content of heavy rare earth elements is 0.30 mass% or less (excluding 0 mass%), The Co content is 0.20 mass% or more and 0.80 mass% or less, The Al content is 0.40 mass% or more and 0.85 mass% or less, The Zr content is 0.21 mass% or more and 0.85 mass% or less, The Ga content is 0.04 mass% or more and 0.40 mass% or less, The B content is 0.90 mass% or more and 1.02 mass% or less, The C content is 0.05% by mass or more and 0.11% by mass or less, The O content is 0 mass % or more and 0.12 mass % or less.
[0006] The value obtained by dividing the Ga content by the Al content on a mass basis may be 0.04 or more and 0.59 or less.
[0007] The value obtained by dividing the C content by the total content of Zr and B on a mass basis may be 0.026 or more and 0.095 or less.
[0008] The magnet may have a concentration distribution of the heavy rare earth element that decreases from the surface to the inside.
[0009] In order to achieve the above object, an RTB permanent magnet according to another aspect of the present disclosure is 14 An RTB permanent magnet having main phase grains including crystal grains having a B-type crystal structure, and grain boundaries formed by two or more adjacent main phase grains, The grain boundaries have an R-Fe-Co-Ga-Al enriched portion, the R-Fe-Co-Ga-Al concentrated portion is a portion containing Fe, having a rare earth element concentration higher than the average rare earth element concentration in the main phase particles, a Co concentration higher than the average Co concentration in the main phase particles, a Ga concentration higher than the average Ga concentration in the main phase particles, and an Al concentration higher than the average Al concentration in the main phase particles; The content of heavy rare earth elements is 0.30 mass% or less (not including 0 mass%).
[0010] The RTB permanent magnet may have an R-Fe-Co-Ga-Al enriched portion near the center.
[0011] may contain at least the rare earth elements, Fe, Co, Al, Zr, Ga, B and C; The content of rare earth elements is 28.50 mass% or more and 31.50 mass% or less, The Co content is 0.20% by mass or more and 0.80% by mass or less, the Al content is 0.40% by mass or more and 0.85% by mass or less, the Zr content is 0.21% by mass or more and 0.85% by mass or less, the Ga content is 0.04% by mass or more and 0.40% by mass or less, the B content is 0.90% by mass or more and 1.02% by mass or less, the C content is 0.05% by mass or more and 0.11% by mass or less, and the O content may be 0% by mass or more and 0.12% by mass or less.
Brief Description of the Drawings
[0012] [Figure 1] It is a schematic diagram of the R-T-B-based permanent magnet according to this embodiment. [Diagram 2] It is an element mapping near the center of the magnet of Sample No. 4. [Diagram 3] It is an element mapping near the surface of the magnet of Sample No. 4. [Figure 4] It is an element mapping near the center of the magnet of Sample No. 15.
Modes for Carrying Out the Invention
[0013] (First Embodiment) Hereinafter, the present disclosure will be described based on the embodiments shown in the drawings.
[0014] <R-T-B-based Permanent Magnet> The R-T-B-based permanent magnet according to this embodiment has main phase particles including crystal particles having an R2T 14 type crystal structure. Further, it has grain boundaries formed by two or more adjacent main phase particles. In particular, the grain boundary formed by two adjacent main phase particles is called a two-particle grain boundary, and the grain boundary formed by three or more main phase particles is called a grain boundary triple point.
[0015] R-T-B-based permanent magnet and R2T 14In the B-type crystal structure, R represents a rare earth element, T represents a transition metal element, and B represents boron.
[0016] RTB permanent magnets and R2T 14 The rare earth element contained as R in the B-type crystal structure may be Sc, Y, or a lanthanoid, or may be Y and a lanthanoid. The transition metal element contained as T does not include a rare earth element. The transition metal element contained as T may be an iron group element. A part of the boron contained as B may be substituted with carbon.
[0017] There are no particular limitations on the shape of the RTB permanent magnet according to this embodiment.
[0018] The RTB permanent magnet according to this embodiment contains a number of specific elements in specific ranges, which allows for improved remanence Br, coercivity HcJ, squareness ratio Hk / HcJ, and corrosion resistance. Furthermore, it allows for improved HcJ at both room temperature and high temperature. Note that Br and Hk / HcJ are both values at room temperature.
[0019] Furthermore, the RTB permanent magnet according to this embodiment may have a concentration distribution in which the concentration of the heavy rare earth element decreases from the outside to the inside of the RTB permanent magnet 1. There are no particular limitations on the type of heavy rare earth element. For example, it may be Dy or Tb, or it may be Tb.
[0020] Specifically, as shown in FIG. 1, the rectangular parallelepiped RTB permanent magnet 1 according to this embodiment has a surface portion and a center portion, and the content of the heavy rare earth element in the surface portion may be 2% or more higher, 5% or more higher, or 10% or more higher by mass than the content of the heavy rare earth element in the center portion. The surface portion refers to the surface of the RTB permanent magnet 1. For example, POINTS C and C' (the centers of gravity of the surfaces facing each other in FIG. 1) in FIG. 1 are the surface portion. The center portion refers to the center of the RTB permanent magnet 1. For example, it refers to a portion that is half the thickness of the RTB permanent magnet 1. For example, POINT M (the midpoint between POINT C and POINT C') in FIG. 1 is the center portion. POINTS C and C' in FIG. 1 may be the center of gravity of the surface with the largest area among the surfaces of the RTB permanent magnet 1, and the center of gravity of the surface facing the surface.
[0021] Rare earth elements are generally classified into light rare earth elements and heavy rare earth elements. In the RTB permanent magnet according to this embodiment, the light rare earth elements are Sc, Y, La, Ce, Pr, Nd, Sm, and Eu, and the heavy rare earth elements are Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu.
[0022] There are no particular limitations on the method for forming the concentration distribution of the heavy rare earth element in the RTB permanent magnet according to this embodiment. For example, the concentration distribution of the heavy rare earth element can be formed in the RTB permanent magnet by grain boundary diffusion of the heavy rare earth element, which will be described later.
[0023] Furthermore, the main phase particles of the RTB permanent magnet according to this embodiment may be core-shell particles consisting of a core and a shell covering the core. At least the shell may contain a heavy rare earth element, Dy or Tb, or Tb may be present.
[0024] By having a heavy rare earth element present in the shell, the magnetic properties of the RTB permanent magnet can be efficiently improved.
[0025] In this embodiment, the shell is defined as a portion where the ratio of heavy rare earth elements to light rare earth elements (heavy rare earth elements / light rare earth elements (molar ratio)) is at least twice the ratio at the center of the main phase particle. Note that the ratio at the center of the main phase particle may be, for example, the ratio at a portion of the main phase particle whose depth from the particle surface is at least 30% of the particle diameter.
[0026] There is no particular limit to the thickness of the shell, but it may be 500 nm or less on average. There is no particular limit to the particle size of the main phase particles, but it may be 1.0 μm or more and 6.5 μm or less on average. When calculating the above average, a cross section of the RTB permanent magnet may be observed using an SEM. An observation range may be set large enough to accommodate 50 or more core-shell particles. The shell thicknesses of all core-shell particles within the observation range may be measured and averaged. The particle sizes of all main phase particles within the observation range may be measured and averaged. The observation range may be, for example, 100 μm x 100 μm.
[0027] There is no particular limitation on the method for making the main phase particles into the above-mentioned core-shell particles. For example, there is a method using grain boundary diffusion, which will be described later. The heavy rare earth element diffuses into the grain boundaries and replaces the rare earth element on the surface of the main phase particle, forming a shell with a high ratio of the heavy rare earth element, thereby forming the above-mentioned core-shell particle.
[0028] The RTB permanent magnet according to this embodiment may contain at least one selected from Nd and Pr as a light rare earth element, and may contain at least one selected from Dy and Tb as a heavy rare earth element. Also, the RTB permanent magnet according to this embodiment preferably contains at least Nd and Tb.
[0029] The RTB permanent magnet according to this embodiment may have a total content of rare earth elements other than Nd, Pr, Dy and Tb of 0.3 mass% or less, with the mass of the entire RTB permanent magnet being 100 mass%, or the total content of rare earth elements other than Nd, Pr and Tb may be 0.3 mass% or less.
[0030] The total content of rare earth elements (TRE) in the RTB permanent magnet according to this embodiment is 28.50% by mass or more and 31.50% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass. It may be 29.50% by mass or more and 31.10% by mass or less. If the TRE is low, HcJ at room temperature (23±1°C), HcJ at high temperatures (100°C or more and 200°C or less) and Hk / HcJ tend to decrease. If the TRE is high, Br and corrosion resistance tend to decrease.
[0031] There are no particular limitations on the total content of light rare earth elements in the RTB permanent magnet according to this embodiment, but it may be 28.25 mass% or more and 31.25 mass% or less, or 29.25 mass% or more and 30.85 mass% or less, with the mass of the entire RTB permanent magnet being 100 mass%.
[0032] When the RTB permanent magnet contains one or more selected from Nd and Pr, the Pr content may be 0.0 mass % or more and 10.0 mass % or less, or 0.0 mass % or more and 7.6 mass % or less.
[0033] The value obtained by dividing the Pr content by the total content of Nd and Pr on a mass basis may be 0 or more and 0.35 or less.
[0034] The RTB permanent magnet according to this embodiment does not necessarily have to intentionally contain Pr. If Pr is not intentionally contained, HcJ at high temperatures tends to be high. If Pr is not intentionally contained, it may contain less than 0.2 mass% Pr as an impurity, or may contain 0.1 mass% or less.
[0035] Furthermore, the RTB permanent magnet of this embodiment has a heavy rare earth element content (HRE) of 0.30 mass% or less (excluding 0 mass%) in total, with the mass of the entire RTB permanent magnet being 100 mass%. If the heavy rare earth element content is too high, the raw material cost increases. Furthermore, Br is likely to decrease. The heavy rare earth element content may be 0.10 mass% or more and 0.30 mass% or less, or may be 0.15 mass% or more and 0.25 mass% or less.
[0036] The Co content is 0.20% by mass or more and 0.80% by mass or less, with the total mass of the RTB permanent magnet being 100% by mass. It may be 0.40% by mass or more and 0.70% by mass or less. If the Co content is too high, the raw material cost tends to increase. If the Co content is too low, the corrosion resistance tends to decrease.
[0037] The Fe content is the substantial remainder of the RTB permanent magnet. The Fe content is the substantial remainder of the RTB permanent magnet means that in the RTB permanent magnet, the remainder excluding the rare earth elements and Co described above, and the below-described B, Al, Zr, Ga, Cu, C, and O, is essentially Fe alone. For example, the total content of elements other than the rare earth elements, Fe, Co, B, Al, Zr, Ga, Cu, C, and O may be 1.0 mass% or less, assuming that the mass of the entire RTB permanent magnet is 100 mass%.
[0038] The B content in the RTB permanent magnet according to this embodiment is 0.90% by mass or more and 1.02% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass. It may be 0.90% by mass or more and 0.98% by mass or less. When B is low, Hk / HcJ and HcJ at high temperatures tend to decrease. When B is high, HcJ and HcJ at high temperatures tend to decrease.
[0039] The RTB permanent magnet according to this embodiment further contains Al. The Al content is 0.40% by mass or more and 0.85% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass. It may be 0.48% by mass or more and 0.80% by mass or less. When the Al content is low, the HcJ at room temperature and the HcJ at high temperatures tend to decrease. When the Al content is high, the Br and the HcJ at high temperatures tend to decrease.
[0040] The RTB permanent magnet according to this embodiment further contains Zr. The Zr content is 0.21% by mass or more and 0.85% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass. It may be 0.32% by mass or more and 0.68% by mass or less. When the Zr content is low, HcJ at room temperature, HcJ at high temperatures, and Hk / HcJ tend to decrease. When the Zr content is high, Br tends to decrease.
[0041] The RTB permanent magnet according to this embodiment further contains Ga. The Ga content is 0.04% by mass or more and 0.40% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass. It may be 0.08% by mass or more and 0.36% by mass or less. When the Ga content is low, HcJ at room temperature and HcJ at high temperatures tend to decrease. When the Ga content is high, Br tends to decrease.
[0042] The RTB permanent magnet according to this embodiment may further contain Cu. The Cu content may be from 0.03% to 0.50% by mass, from 0.04% to 0.45% by mass, or from 0.05% to 0.40% by mass, with the total mass of the RTB permanent magnet being 100% by mass.
[0043] The RTB permanent magnet according to this embodiment further contains C. The C content is 0.05% by mass or more and 0.11% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass. It may be 0.07% by mass or more and 0.09% by mass or less. When the C content is low, Br is likely to decrease. When the C content is high, HcJ at room temperature, HcJ at high temperatures, and Hk / HcJ are likely to decrease.
[0044] The RTB permanent magnet according to this embodiment may further contain O. The O content is 0% by mass or more and 0.12% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass. It may be 0.06% by mass or more and 0.11% by mass or less. In order to manufacture an RTB permanent magnet with low O content, it is necessary to reduce the oxygen concentration in the atmosphere during manufacture, so if there is little O, the manufacturing costs of the RTB permanent magnet are likely to increase. If there is a lot of O, Br, HcJ at room temperature, and HcJ at high temperatures are likely to decrease.
[0045] In the RTB permanent magnet according to this embodiment, the value of the Ga content divided by the Al content on a mass basis (hereinafter sometimes simply referred to as Ga / Al) may be 0.04 to 0.59, or 0.10 to 0.53. If Ga / Al is within the above range, it becomes easier to obtain an RTB permanent magnet that is good in all respects: Br, HcJ at room temperature, HcJ at high temperatures, Hk / HcJ, and corrosion resistance.
[0046] In the RTB permanent magnet according to this embodiment, the value obtained by dividing the C content by the total content of Zr and B on a mass basis (hereinafter sometimes simply referred to as C / (Zr+B)) may be 0.026 to 0.095, or 0.031 to 0.090. When C / (Zr+B) is within the above range, it becomes easier to obtain an RTB permanent magnet that is good in all respects: Br, HcJ at room temperature, HcJ at high temperatures, Hk / HcJ, and corrosion resistance.
[0047] The RTB permanent magnet according to this embodiment may contain other elements other than the above-mentioned rare earth elements, Fe, Co, Al, Zr, Ga, Cu, B, C, and O. There are no particular restrictions on the content of the other elements, as long as they do not significantly affect the magnetic properties and corrosion resistance of the RTB permanent magnet. For example, the content of each of the other elements may be 0.10% by mass or less, and the total content may be 1.0% by mass or less, assuming that the mass of the entire RTB permanent magnet is 100% by mass.
[0048] The various components contained in the RTB permanent magnet according to this embodiment can be measured by a method generally known in the art. The amounts of various elements are measured, for example, by X-ray fluorescence analysis and inductively coupled plasma emission spectrometry (ICP analysis). The O content is measured, for example, by inert gas fusion-non-dispersive infrared absorption spectrometry. The C content is measured, for example, by combustion in an oxygen stream-infrared absorption spectrometry.
[0049] There are no particular limitations on the shape of the RTB permanent magnet according to this embodiment, and examples include a rectangular parallelepiped and a C-shape.
[0050] Below, a method for producing an RTB based sintered magnet will be described in detail as one example of a method for producing an RTB based permanent magnet according to this embodiment, but the method for producing an RTB based permanent magnet is not limited to this, and other known methods may be used.
[0051] [Raw powder preparation process] The raw material powder can be prepared by a known method. In this embodiment, a one-alloy method using a single alloy will be described, but a so-called two-alloy method in which two or more alloys with different compositions are mixed to prepare the raw material powder may also be used.
[0052] First, a raw material alloy for the RTB permanent magnet is prepared (alloy preparation step). In the alloy preparation step, raw material metals corresponding to the composition of the RTB permanent magnet according to this embodiment are melted by a known method, and then cast to produce a raw material alloy having the desired composition.
[0053] As the raw material metal, for example, a simple substance of a rare earth element, a simple substance of a metal element such as Fe, Co, or Al, an alloy consisting of a plurality of kinds of metals (e.g., an Fe-Co alloy), or a compound consisting of a plurality of kinds of elements (e.g., ferroboron) can be appropriately used. There is no particular limitation on the casting method for casting the raw material alloy from the raw material metal. A strip casting method may be used to obtain an RTB permanent magnet with high magnetic properties. The obtained raw material alloy may be subjected to a homogenization treatment by a known method as necessary.
[0054] After the raw alloy is prepared, it is pulverized (pulverization step). The atmosphere in each step from the pulverization step to the sintering step can have a low oxygen concentration in order to obtain high magnetic properties. For example, the oxygen concentration in the atmosphere in each step can be set to 200 ppm or less. By controlling the oxygen concentration in the atmosphere in each step, the O content in the RTB permanent magnet can be controlled.
[0055] The following describes the case where the pulverization process is carried out in two stages: a coarse pulverization process in which the particles are pulverized to a particle size of several hundred μm to several mm, and a fine pulverization process in which the particles are pulverized to a particle size of approximately several μm. However, the process may be carried out in a single stage, namely, the fine pulverization process alone.
[0056] In the coarse pulverization step, the material is coarsely pulverized until the particle size is about several hundred μm to several mm. This produces a coarsely pulverized powder. There is no particular limitation on the method of coarse pulverization, and it can be performed by a known method such as a method of hydrogen absorption pulverization or a method using a coarse pulverizer.
[0057] Next, the obtained coarsely pulverized powder is pulverized until the average particle size is about several μm (fine pulverization step). This produces finely pulverized powder (raw powder). The average particle size of the finely pulverized powder may be 1 μm or more and 10 μm or less, 2 μm or more and 6 μm or less, or 2 μm or more and 4 μm or less.
[0058] There is no particular limitation on the method of fine pulverization, and it can be carried out, for example, by a method using various fine pulverizers.
[0059] When the coarsely pulverized powder is pulverized, various grinding aids such as lauric acid amide and oleic acid amide can be added to obtain a finely pulverized powder in which the crystal grains tend to be oriented in a specific direction when pressed and molded in a magnetic field. In addition, the C content in the RTB permanent magnet can be controlled by changing the amount of grinding aid added.
[0060] [Molding process] In the molding process, the finely pulverized powder is molded into a desired shape. There are no particular limitations on the molding method. In this embodiment, the finely pulverized powder is filled into a mold and pressurized in a magnetic field. The resulting molded body has crystal grains oriented in a specific direction, resulting in an RTB permanent magnet with a higher Br.
[0061] The pressure during molding can be 20 MPa or more and 300 MPa or less. The magnetic field applied can be 950 kA / m or more, or 950 kA / m or more and 1600 kA / m or less. The magnetic field applied is not limited to a static magnetic field, and can also be a pulsed magnetic field. A static magnetic field and a pulsed magnetic field can also be used in combination.
[0062] As a molding method, in addition to the dry molding in which the finely pulverized powder is molded as is as described above, wet molding in which a slurry in which the finely pulverized powder is dispersed in a solvent such as oil can also be applied.
[0063] There is no particular restriction on the shape of the compact obtained by compacting the finely pulverized powder. The density of the compact at this stage is 4.0 Mg / m 3 ~4.3Mg / m 3 It can be said that:
[0064] [Sintering process] The sintering process is a process in which the compact is sintered in a vacuum or in an inert gas atmosphere to obtain a sintered body. The sintering conditions need to be adjusted depending on various conditions such as the composition, the crushing method, the particle size and particle size distribution, etc. For example, the compact is sintered by, for example, heating in a vacuum or in an inert gas atmosphere at 1000°C to 1200°C for 1 hour to 20 hours. By sintering under the above sintering conditions, a high-density sintered body can be obtained. In this embodiment, the density is at least 7.45 Mg / m 3 The density of the sintered body is 7.50Mg / m 3 It may be more than that.
[0065] [Aging treatment process] The aging treatment step is a step of subjecting the sintered body to a heat treatment (aging treatment) at a temperature lower than the sintering temperature. There is no particular limit to whether or not the aging treatment is performed, and there is no particular limit to the number of times the aging treatment is performed. Hereinafter, an embodiment in which the aging treatment is performed twice will be described.
[0066] The first aging step is called the first aging step, the second aging step is called the second aging step, the aging temperature of the first aging step is called T1, and the aging temperature of the second aging step is called T2.
[0067] There is no particular limitation on T1 and the aging time in the first aging step. T1 can be 700° C. or more and 950° C. or less. The aging time can be 1 hour or more and 10 hours or less.
[0068] There is no particular limitation on T2 and the aging time in the second aging step. T2 can be 450° C. or more and 700° C. or less. The aging time can be 1 hour or more and 10 hours or less.
[0069] [Processing process (before grain boundary diffusion)] If necessary, a process may be included in which the sintered body according to the present embodiment is processed into a desired shape. Examples of the processing method include shaping such as cutting and grinding, and chamfering such as barrel polishing.
[0070] [Grain boundary diffusion process] The grain boundary diffusion step can be carried out by attaching a diffusion material to the surface of the sintered body and heating the sintered body to which the diffusion material is attached. Then, an RTB permanent magnet is obtained. In this embodiment, there is no particular limitation on the type of diffusion material. The diffusion material may include a hydride of a heavy rare earth element (e.g., Tb), or the diffusion material may include a heavy rare earth element and Cu.
[0071] In the grain boundary diffusion process, as the temperature rises, the grain boundary phase, which has a high concentration of rare earth elements present in the grain boundaries of the magnet base material (sintered body), becomes a liquid phase, and the diffusion material dissolves into the liquid phase, causing the components of the diffusion material to diffuse from the surface of the magnet base material into the interior of the magnet base material.
[0072] The magnet base material according to this embodiment has the characteristic that the Al content is within a predetermined range, etc. The diffusion material according to this embodiment has the above-mentioned characteristics.
[0073] Therefore, in this embodiment, the liquid phase generated during heating contains Al within a predetermined range. Furthermore, compared to a magnet base material that does not contain Al, the reaction rate between the components of the diffusion material and the liquid phase is slower in a magnet base material that contains Al. Furthermore, since the volume diffusion of the heavy rare earth element into the main phase particles is suppressed, the heavy rare earth element is more likely to diffuse to the center of the magnet base material. Therefore, good characteristics can be obtained with a relatively small amount of diffusion of the heavy rare earth element.
[0074] In addition, in the magnet base material before grain boundary diffusion, the Al concentration is approximately the same in the main phase particles and the grain boundary phase. Therefore, during grain boundary diffusion, a fine structure with high interfacial compatibility is formed near the main phase particles. Therefore, it is believed that sufficiently high properties, especially sufficiently high coercivity, can be obtained regardless of whether or not aging treatment is performed. If aging treatment is not performed, manufacturing costs can be reduced.
[0075] The diffusing material may be a slurry containing a solvent in addition to the above-mentioned heavy rare earth element hydride, etc. The solvent contained in the slurry may be a solvent other than water. For example, it may be an organic solvent such as alcohol, aldehyde, ketone, etc. Furthermore, the diffusing material may contain a binder. There is no particular limit to the type of binder. For example, a resin such as an acrylic resin may be contained as a binder. By containing a binder, the diffusing material is more likely to adhere to the surface of the sintered body.
[0076] The diffusion material may be a paste containing a solvent and a binder in addition to the above-mentioned heavy rare earth element hydride, etc. The paste has flowability and high viscosity. The viscosity of the paste is higher than that of the slurry.
[0077] Before the diffusion treatment described below, the sintered body to which the slurry or paste has been applied may be dried to remove the solvent and binder.
[0078] The holding temperature during drying may be 200°C or higher and 800°C or lower, and the holding time may be 10 minutes or higher and 10 hours or lower. The drying atmosphere is in an inert gas. By drying the sintered body to which the slurry or paste is attached, the generation of carbides of the heavy rare earth element formed on the surface of the magnet base material can be suppressed, and the amount of the heavy rare earth element used can be further reduced.
[0079] The diffusion treatment in the grain boundary diffusion step according to this embodiment may be performed consecutively from the drying. Alternatively, the diffusion treatment may be performed by cooling to room temperature once after the drying and then heating again. The holding temperature during the diffusion treatment may be 700°C or higher and 1000°C or lower. In the grain boundary diffusion step, the temperature of the magnet base material may be gradually increased from a temperature lower than the diffusion treatment temperature to the diffusion treatment temperature.
[0080] The time during which the temperature of the substrate is maintained at the diffusion treatment temperature (diffusion treatment time) may be, for example, 1 hour or more and 50 hours or less. The atmosphere around the substrate in the diffusion treatment step may be a non-oxidizing atmosphere. The non-oxidizing atmosphere may be, for example, a rare gas such as argon. The pressure of the atmosphere around the magnet substrate in the diffusion step may be 1 kPa or less. By creating such a reduced pressure atmosphere, the dehydrogenation reaction of the hydride is promoted, and the dissolution of the diffusion material into the liquid phase is easily promoted.
[0081] [Processing process (after grain boundary diffusion)] After the grain boundary diffusion step, polishing may be performed to remove any remaining diffusion material on the surface of the RTB permanent magnet. The RTB permanent magnet may also be subjected to other processing. For example, surface processing such as shaping, such as cutting and grinding, and chamfering, such as barrel polishing, may be performed.
[0082] In this embodiment, processing steps are performed before and after the grain boundary diffusion, but these steps do not necessarily have to be performed.
[0083] In particular, the R-T-B-based permanent magnet after grain boundary diffusion is likely to have a concentration distribution in which the concentration of the heavy rare earth element decreases from the outside to the inside of the R-T-B-based permanent magnet. Further, the main phase particles contained in the R-T-B-based permanent magnet after grain boundary diffusion are likely to have the above core-shell structure.
[0084] The R-T-B-based permanent magnet according to this embodiment thus obtained has desired characteristics. Specifically, Br, HcJ at room temperature, HcJ at high temperature, and Hk / HcJ are high, and the corrosion resistance is also excellent.
[0085] The R-T-B-based permanent magnet according to this embodiment obtained by the above method becomes a magnetized R-T-B-based permanent magnet when magnetized.
[0086] The R-T-B-based permanent magnet according to this embodiment is suitably used in applications such as motors and generators.
[0087] (Second Embodiment) Hereinafter, the second embodiment will be described. Matters not particularly described are the same as those in the first embodiment.
[0088] <R-T-B-based permanent magnet> The R-T-B-based permanent magnet according to this embodiment has main phase particles containing crystal particles having an R2T 14 B-type crystal structure. Further, it has grain boundaries formed by two or more adjacent main phase particles. In particular, the grain boundary formed by two adjacent main phase particles is called a two-particle grain boundary, and the grain boundary formed by three or more main phase particles is called a grain boundary triple point.
[0089] In the R-T-B-based permanent magnet according to this embodiment, an R-Fe-Co-Ga-Al enriched portion may be formed in the grain boundary. The R-Fe-Co-Ga-Al enriched portion contains Fe, and the concentration of the rare earth element is higher than the average concentration of the rare earth element in the main phase particles, the concentration of Co is higher than the average concentration of Co in the main phase particles, the concentration of Ga is higher than the average concentration of Ga in the main phase particles, and the concentration of Al is higher than the average concentration of Al in the main phase particles.
[0090] The R-Fe-Co-Ga-Al enriched portion may be formed near the center of the magnet. When the magnet has a shape such as a rectangular parallelepiped, the area near the center of the magnet may be the area where the center of gravity is the same as that of the magnet, the area is approximately similar to that of the magnet, and the area is 50% of that of the magnet. When observing the cross section of the magnet, the area near the center of the magnet may be the area where the center of gravity is the same as that of the magnet, the area is approximately similar to that of the magnet, and the area is 50% of that of the magnet. When the magnet has a shape such as a C-shape, the area near the center of the magnet may be the area 10% or more inside the magnet thickness from all the surfaces of the magnet. When the magnet has a C-shape, the magnet thickness may be the longest distance when a perpendicular line is drawn from the inner arc to the outer arc of the magnet. The part other than the area near the center of the magnet may be the surface area of the magnet. By forming the R-Fe-Co-Ga-Al enriched portion in the grain boundary, high corrosion resistance and HcJ can be obtained.
[0091] It is believed that the formation of R-Fe-Co-Ga-Al enriched parts in the grain boundaries of the magnet reduces the ratio of the RO phase, which has relatively low corrosion resistance, and therefore improves the corrosion resistance of the magnet. The RO phase refers to a phase in which the R concentration is higher than the average R concentration in the main phase, and the O concentration is higher than the average O concentration in the main phase. The RO phase may further contain elements other than R and O, such as C, N, etc.
[0092] When R-Fe-Co-Ga-Al enriched parts are formed in the grain boundaries of a magnet, a magnet with a high HcJ can be obtained through grain boundary diffusion, which will be described later. When Tb is diffused into the grain boundaries, the R-Fe-Co-Ga-Al enriched parts are less likely to contain Tb than the RO phase, so it is believed that by dispersing the R-Fe-Co-Ga-Al enriched parts at the grain boundaries, Tb can be efficiently diffused into the interior of the magnet, improving the HcJ of the magnet.
[0093] In this embodiment, unlike the first embodiment, there are no particular limitations on the composition of the RTB permanent magnet other than the content of the heavy rare earth element. Considering that an R-Fe-Co-Ga-Al enriched portion is formed in the grain boundary of the RTB permanent magnet, the composition contains at least R, Fe, Co, Ga, and Al. It also contains a heavy rare earth element. The content of the heavy rare earth element is the same as in the first embodiment.
[0094] The total content of rare earth elements (TRE) in the RTB permanent magnet according to this embodiment may be 28.50 mass% or more and 31.50 mass% or less, or 29.50 mass% or more and 31.10 mass% or more, with the mass of the entire RTB permanent magnet being 100 mass%.
[0095] The Co content may be from 0.20 mass % to 0.80 mass %, or from 0.40 mass % to 0.70 mass %, with the mass of the entire RTB permanent magnet being 100 mass %.
[0096] The Fe content may be the substantial remainder of the RTB permanent magnet.
[0097] The content of B may be 0.90% by mass or more and 1.02% by mass or less, or 0.90% by mass or more and 0.98% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass. When the content of B is 0.90% by mass or more, the average thickness of the two-particle grain boundary tends to be 30 nm or less.
[0098] The Al content may be 0.40 mass % or more and 0.85 mass % or less, or 0.48 mass % or more and 0.80 mass % or less, with the mass of the entire RTB permanent magnet being 100 mass %.
[0099] The Zr content may be from 0.21 mass % to 0.85 mass %, or from 0.32 mass % to 0.68 mass %, with the mass of the entire RTB permanent magnet being 100 mass %.
[0100] The Ga content may be 0.04 mass % or more and 0.40 mass % or less, or 0.08 mass % or more and 0.36 mass % or less, with the mass of the entire RTB permanent magnet being 100 mass %.
[0101] The Cu content may be 0.03 mass% or more and 0.50 mass% or less, 0.04 mass% or more and 0.45 mass% or less, or 0.05 mass% or more and 0.40 mass% or less, with the mass of the entire RTB permanent magnet being 100 mass%.
[0102] The C content may be 0.05% by mass or more and 0.11% by mass or less, or 0.07% by mass or more and 0.09% by mass or less, with the mass of the entire RTB permanent magnet being 100% by mass.
[0103] The O content may be from 0 to 0.12 mass %, or from 0.06 to 0.11 mass %, with the mass of the entire RTB permanent magnet being 100 mass %.
[0104] Hereinafter, a method for producing an RTB based sintered magnet will be described as an example of a method for producing an RTB based permanent magnet according to this embodiment. The method for producing an RTB based sintered magnet according to this embodiment is the same as the method for producing an RTB based sintered magnet according to the first embodiment, except for the following points.
[0105] When the two-alloy method is adopted, the R-Fe-Co-Ga-Al enriched portion is easily formed in the grain boundary by setting the Al content of the grain boundary phase alloy to 3 mass % or more.
[0106] The aging time in the second aging step may be set to 5 hours or less. By setting the aging time to 5 hours or less, the R-Fe-Co-Ga-Al enriched portion is easily formed near the center of the magnet.
[0107] It should be noted that the present disclosure is not limited to the above-described embodiments, and various modifications can be made within the scope of the present disclosure.
[0108] The manufacturing method of the RTB permanent magnet is not limited to the above method and may be changed as appropriate. For example, the manufacturing method of the RTB permanent magnet described above is a manufacturing method by sintering, but the RTB permanent magnet according to this embodiment may be manufactured by hot working. The method of manufacturing an RTB permanent magnet by hot working includes the following steps. (a) A melting and quenching process in which raw metal is melted and the resulting bath is quenched to obtain a thin strip. (b) A grinding process in which the ribbon is pulverized to obtain a flake-shaped raw powder. (c) Cold forming process in which the crushed raw powder is cold-formed (d) A preheating step of preheating the cold-formed body (e) A hot forming process in which the preheated cold-formed body is hot-formed. (f) A hot plastic working process in which the hot-formed body is plastically deformed into a desired shape. (g) Aging treatment process for aging RTB permanent magnets The aging treatment step may be omitted. The steps after the aging treatment step are the same as those in the case of production by sintering. EXAMPLES
[0109] The present disclosure will be described below based on more detailed examples, but the present disclosure is not limited to these examples.
[0110] (Production of RTB permanent magnets) A raw material alloy was prepared by the strip casting method so that the composition of the RTB permanent magnet finally obtained would be the composition of each sample shown in Tables 1 to 3. The Pr content was 0% by mass or more and 12% by mass or less. Tb was not included in the raw material alloy, but was included only in the diffusion material paste described below. N, H, Si, Ca, La, Ce, Cr, and the like may be detected as other elements not listed in Tables 1 to 3. Si may be mixed in mainly from the ferroboron raw material and the crucible used when melting the alloy. Ca, La, and Ce may be mixed in from the rare earth raw material. Cr may be mixed in from the electrolytic iron. The Fe content in Tables 1 to 3 is listed as bal. This is to indicate that the Fe content is the substantial remainder when the entire RTB permanent magnet including these other elements is taken as 100% by mass.
[0111] Next, hydrogen gas was flowed into the raw alloy at room temperature for 1 hour to absorb hydrogen, and then the atmosphere was switched to Ar gas, and dehydrogenation treatment was carried out at 500° C. for 1 hour, and the raw alloy was hydrogen-absorbed and crushed.
[0112] Next, 0.1% by mass of oleic acid amide was added as a grinding aid to the raw alloy powder, and the mixture was mixed using a Nauta mixer.
[0113] Next, the mixture was finely pulverized in a nitrogen gas flow using a collision plate type jet mill to obtain a fine powder (raw powder) having an average particle size of about 3.0 μm. The average particle size was the average particle size D50 measured by a laser diffraction type particle size distribution analyzer.
[0114] The obtained fine powder was molded in a magnetic field to produce a compact. The magnetic field applied was a static magnetic field of 1200 kA / m. The pressure during molding was 120 MPa. The magnetic field application direction and the pressure direction were perpendicular to each other.
[0115] Next, the green body was sintered to obtain a sintered body. The optimum sintering conditions differ depending on the composition, etc., but the temperature was kept within the range of 1030°C to 1070°C for 4 hours. The sintering atmosphere was a vacuum. The sintered density was 7.51 Mg / m3 ~7.55Mg / m 3 As described above, sintered bodies from which the samples shown in Tables 1 to 3 were obtained by grain boundary diffusion were prepared.
[0116] (Preparation of diffusion material paste) Next, a diffusion material paste to be used for grain boundary diffusion was prepared.
[0117] First, hydrogen gas was flowed at room temperature to metal Tb with a purity of 99.9% to absorb hydrogen. Then, the atmosphere was switched to Ar gas, and dehydrogenation was performed at 500°C for 1 hour, and metal Tb was hydrogen-absorbed and crushed. Next, zinc stearate was added as a grinding aid at 0.05 mass% relative to 100 mass% metal Tb, and mixed using a Nauta mixer. After that, fine grinding was performed using a jet mill in an atmosphere containing 3000 ppm oxygen, and finely ground powder of Tb hydride with an average particle size of about 10.0 μm was obtained.
[0118] A diffusion material paste was prepared by kneading 60 parts by mass of finely pulverized powder of Tb hydride, 10 parts by mass of metallic Cu powder, 25 parts by mass of alcohol, and 5 parts by mass of acrylic resin. Note that the alcohol is a solvent, and the acrylic resin is a binder.
[0119] (Application of diffusion paste and heat treatment) The above sintered body was processed to a size of 11 mm long x 11 mm wide x 4.2 mm thick (thickness in the direction of easy magnetization 4.2 mm). Then, the body was immersed in a mixed solution of nitric acid and ethanol (100% by mass ethanol and 3% by mass nitric acid) for 3 minutes, and then immersed in ethanol for 1 minute, for an etching treatment. The etching treatment of immersing in the mixed solution for 3 minutes and then immersing in ethanol for 1 minute was performed twice.
[0120] Next, the above-mentioned diffusion material paste was applied to the entire surface of the sintered body after the etching treatment. The amount of the diffusion material paste applied was set so that the Tb content in the final RTB permanent magnet would be the value shown in Tables 1 to 3.
[0121] Next, the sintered body was dried. Specifically, the sintered body coated with the diffusion material paste was left in an oven at 400°C in an Ar gas atmosphere for 3 hours to remove the solvent and binder in the diffusion material paste. Then, the sintered body was heated at 900°C for 30 hours while flowing Ar at atmospheric pressure (1 atm). Furthermore, aging treatment was performed by heating at 500°C for 1 hour while flowing Ar at atmospheric pressure (1 atm). From the above, RTB permanent magnets of each sample shown in Tables 1 to 3 were obtained.
[0122] After shaving off 0.1 mm of the surface of the RTB permanent magnet on each side, the composition, microstructure, element distribution, magnetic properties and corrosion resistance were evaluated.
[0123] The RTB permanent magnet was processed vertically to a size of 11 mm long x 11 mm wide x 4.2 mm thick (the easy axis direction of magnetization is 4.2 mm), and the magnetic properties were evaluated at room temperature using a BH tracer. The RTB permanent magnet was magnetized using a pulse magnetic field of 4000 kA / m before measuring the magnetic properties. Since the RTB permanent magnet was thin, three magnets were stacked to evaluate the magnetic properties. In this embodiment, Hk / HcJ was calculated by Hk / HcJ x 100 (%), where Hk (kA / m) is the magnetic field when the magnetization is 90% of Br in the second quadrant of the magnetization J-magnetic field H curve (JH demagnetization curve). HcJ at high temperatures, i.e., HcJ when heated to 150°C, was also measured.
[0124] In this embodiment, a Br of 1400mT or more for the RTB permanent magnet was rated as good, with 1410mT or more being even better. A HcJ of 1850kA / m or more at room temperature for the RTB permanent magnet was rated as good, with 1900kA / m or more being even better. A high-temperature HcJ of 700kA / m or more for the RTB permanent magnet was rated as good, with 715kA / m or more being even better. A Hk / HcJ of 93.0% or more for the RTB permanent magnet was rated as good, with 95.0% or more being even better.
[0125] The microstructure and element distribution of the RTB permanent magnets were confirmed. Specifically, a field emission type EPMA (Electron Probe Micro Analyzer) manufactured by JEOL Ltd. was used to observe the microstructure and perform element mapping. The observation sample was prepared by cutting the magnet so that it would fit into a cube with a side length of 10 mm or less, including the area near the center of the magnet, embedding the cut magnet in resin, and then mirror polishing it. The measurement conditions were an acceleration voltage of 15 kV, an irradiation current of 100 nA, and a magnification of 2000 times, with a field of view of 51.2 μm x 51.2 μm being observed.
[0126] A corrosion resistance test was conducted on the RTB permanent magnet. The corrosion resistance test was carried out using a PCT test (Pressure Cooker Test) under saturated vapor pressure. Specifically, the RTB permanent magnet was placed in an environment of 2 atmospheres and 100% RH for 1000 hours, and the change in mass was measured before and after the test. The absolute value of the mass change per surface area of the RTB permanent magnet was 0.3 mg / cm 2 Corrosion resistance is considered to be good when the corrosion rate is less than 0.1 mg / cm 2 The corrosion resistance was deemed to be better when the following conditions were met: If the RTB permanent magnet itself crumbled into pieces, this was noted as "collapsed" in the corrosion resistance column.
[0127] A comprehensive evaluation was performed on each sample in Tables 1 to 3. Samples in which Br, HcJ at room temperature, HcJ at high temperature, Hk / HcJ and corrosion resistance were all better were rated A. Samples in which Br, HcJ at room temperature, HcJ at high temperature, Hk / HcJ or corrosion resistance were not good were rated C. Samples in which none of the above were good were rated B. The results are shown in Tables 1 to 3.
[0128] [Table 1]
[0129] [Table 2]
[0130] [Table 3]
[0131] As can be seen from Tables 1 to 3, in each of the examples in which all compositions were within a specific range, good magnetic properties and corrosion resistance were obtained.
[0132] As can be seen from Table 1, samples No. 14 and No. 15, which contained too little Al, had low HcJ at room temperature and at high temperatures. Sample No. 20, which contained too little Co, had low corrosion resistance.
[0133] From Table 2, it can be seen that sample No. 33, which had too little Ga content, had low HcJ at room temperature and low HcJ at high temperatures.
[0134] From Table 3, it can be seen that sample No. 53, which contained too much HRE, had a decreased Br.
[0135] For all the RTB permanent magnets of the examples and comparative examples, the Tb concentration distribution was analyzed using an electron probe microanalyzer (EPMA), and it was confirmed that the Tb concentration distribution decreased from the outside to the inside.
[0136] It was confirmed that the average thickness of the grain boundary between two particles was 30 nm or less for the RTB permanent magnets of all the examples.
[0137] FIG. 2 shows the results of elemental mapping by EPMA for the magnet of sample No. 4, which is located 2 mm from the magnet surface near the center of the magnet. FIG. 3 shows the results of elemental mapping for the magnet of sample No. 4, which is located 100 μm from the magnet surface near the magnet surface near the magnet surface. FIG. 4 shows the results of elemental mapping for the magnet of sample No. 15, which is located 2 mm from the magnet surface near the center of the magnet. Each figure is arranged in the order of Nd mapping image, Tb mapping image, Fe mapping image, Co mapping image, Ga mapping image, and Al mapping image from the left. The position of the R-Fe-Co-Ga-Al enriched portion 11 is shown in the Al mapping image. From the elemental mapping results in FIG. 2 and FIG. 3, it can be seen that the R-Fe-Co-Ga-Al enriched portion 11 exists in the grain boundary of the magnet of sample No. 4. Note that the region where the high concentrations of R, Fe, Co, Ga, and Al coincide in the elemental mappings in FIG. 2 to FIG. 4 is the R-Fe-Co-Ga-Al enriched portion 11. In particular, there are more R-Fe-Co-Ga-Al enriched portions 11 in the grain boundaries near the center of the magnet compared to the vicinity of the magnet surface. On the other hand, in sample No. 15, no R-Fe-Co-Ga-Al enriched portion 11 was observed in the grain boundary.
[0138] It was also confirmed that in all of the magnets of the examples, R-Fe-Co-Ga-Al enriched portions 11 were present in the grain boundaries, similar to the magnet of sample No. 4, and that in particular there were more R-Fe-Co-Ga-Al enriched portions 11 in the grain boundaries near the center of the magnet compared to near the surface of the magnet. On the other hand, it was confirmed that in samples No. 14, 20, and 33, R-Fe-Co-Ga-Al enriched portions 11 were not observed in the grain boundaries, similar to the magnet of sample No. 15. [Explanation of symbols]
[0139] 1...RTB permanent magnet 11…R-Fe-Co-Ga-Al enrichment section
Claims
1. Contains at least rare earth elements, Fe, Co, Al, Zr, Ga, B and C; Contains heavy rare earth elements as rare earth elements, The content of rare earth elements is 28.50% by mass or more and 31.50% by mass or less, The content of heavy rare earth elements is 0.30% by mass or less (excluding 0% by mass), The Co content is 0.20 mass% or more and 0.80 mass% or less, The Al content is 0.40 mass% or more and 0.85 mass% or less, The Zr content is 0.21 mass% or more and 0.85 mass% or less, The Ga content is 0.04 mass% or more and 0.40 mass% or less, The B content is 0.90 mass% or more and 1.02 mass% or less, The C content is 0.05 mass% or more and 0.11 mass% or less, An RTB system permanent magnet having an O content of 0 mass % or more and 0.12 mass % or less.
2. 2. The R-T-B system permanent magnet according to claim 1, wherein the value obtained by dividing the Ga content by the Al content on a mass basis is 0.04 or more and 0.59 or less.
3. 3. The R-T-B system permanent magnet according to claim 1, wherein the value obtained by dividing the C content by the total Zr and B content on a mass basis is 0.026 or more and 0.095 or less.
4. 3. The R-T-B system permanent magnet according to claim 1, wherein the concentration of the heavy rare earth element is distributed in a manner that decreases from the surface of the magnet toward the inside.
5. R 2 T 14 An R-T-B system permanent magnet having main phase grains including crystal grains having a B-type crystal structure, and grain boundaries formed by two or more adjacent main phase grains, The grain boundaries have an R—Fe—Co—Ga—Al enriched portion, the R-Fe-Co-Ga-Al concentrated portion is a portion that contains Fe, has a rare earth element concentration higher than the average rare earth element concentration in the main phase particles, has a Co concentration higher than the average Co concentration in the main phase particles, has a Ga concentration higher than the average Ga concentration in the main phase particles, and has an Al concentration higher than the average Al concentration in the main phase particles; An RTB system permanent magnet having a heavy rare earth element content of 0.30 mass % or less (not including 0 mass %).
6. 6. The RTB system permanent magnet according to claim 5, which has an R-Fe-Co-Ga-Al concentrated portion near the center of the RTB system permanent magnet.
7. Contains at least rare earth elements, Fe, Co, Al, Zr, Ga, B and C; The content of rare earth elements is 28.50% by mass or more and 31.50% by mass or less, The Co content is 0.20 mass% or more and 0.80 mass% or less, The Al content is 0.40 mass% or more and 0.85 mass% or less, The Zr content is 0.21 mass% or more and 0.85 mass% or less, The Ga content is 0.04 mass% or more and 0.40 mass% or less, The B content is 0.90 mass% or more and 1.02 mass% or less, The C content is 0.05 mass% or more and 0.11 mass% or less, 7. The R-T-B system permanent magnet according to claim 5, wherein the O content is from 0% by mass to 0.12% by mass.
Citation Information
Patent Citations
R-t-b based permanent magnet
JP2020161812A