Electrolyte composition comprising oligomeric silyl ester phosphonates

Phosphonic acid silyl esters in electrolyte compositions for lithium secondary batteries address issues of capacity retention, long-term performance, safety, and impedance by forming a protective coating on the cathode, enhancing the performance of high-capacity and high-voltage cathode active materials.

JP2024138291AActive Publication Date: 2024-10-08BASF SE
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024099408
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2017-12-13
Filing Date
2024-06-20
Publication Date
2024-10-08
Estimated Expiration
2038-12-11

AI Technical Summary

Technical Problem

Existing electrolyte compositions for lithium secondary batteries with high-capacity and high-voltage cathode active materials face challenges in maintaining high capacity retention, long-term performance, safety, reducing gas generation, and impedance build-up.

Method used

Incorporation of phosphonic acid silyl esters with a specific structure into the electrolyte composition, which includes aprotic organic solvents and conductive salts, to enhance the performance of electrochemical cells by forming a protective coating on the cathode and reducing undesirable reactions.

Benefits of technology

The electrolyte composition with phosphonic acid silyl esters improves capacity retention, long-term performance, safety, and reduces gas evolution and impedance build-up, facilitating better handling and storage of the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138291000001
    Figure 2024138291000001
  • Figure 2024138291000002
    Figure 2024138291000002
  • Figure 2024138291000003
    Figure 2024138291000003
Patent Text Reader

Abstract

To provide an electrolyte composition, an electrochemical cell comprising the electrolyte composition, and a method of making the electrochemical cell.SOLUTION: An electrolyte composition contains: at least one aprotic organic solvent; at least one conducting salt including at least one lithium salt; and at least one silyl ester phosphonate comprising the structure of the formula (I) in the figure. The electrolyte composition contains the at least one silyl ester phosphonate in an amount of 0.01 to 10 mass% based on the total mass of the electrolyte composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing 3 and an electrolyte composition comprising a phosphonic acid silyl ester comprising a structure of formula (I) having T; [ka] The present invention relates to the use of a phosphonic acid silyl ester containing the structure of formula (I) in an electrolyte composition for an electrochemical cell, and to an electrochemical cell comprising said electrolyte composition. [Background technology]

[0002] The storage of electrical energy remains a problem of growing interest. Efficient storage of electrical energy allows it to be generated when advantageous and used when needed. Electrochemical secondary batteries are well suited for this purpose, as they reversibly convert chemical energy into electrical energy (rechargeable). Lithium secondary batteries are of particular interest for energy storage, since they offer high energy density and specific energy due to the small atomic weight of the lithium ion and the resulting high battery voltage (typically 3-5 V) compared to other battery systems. These systems are therefore becoming widely used as power sources for many portable electronic devices, such as mobile phones, laptop computers, and mini cameras.

[0003] In lithium secondary batteries, such as lithium-ion batteries, organic carbonates, ethers, esters, ionic liquids, etc. are used as solvents polar enough to dissolve the conductive salts. Generally, most modern lithium-ion batteries contain a solvent mixture of different organic aprotic solvents rather than a single solvent.

[0004] In addition to the solvent and the conductive salt, the electrolyte composition usually further contains additives to improve certain properties of the electrolyte composition and the electrochemical cell containing said electrolyte composition. Common additives are, for example, flame retardants, overcharge protection additives, and film-forming additives that react during the first charge / discharge cycle with the electrode surface, thereby forming a film on the electrode. Various Si- and / or P-containing additives are known for use in the electrolyte composition.

[0005] US 8,734,668 B2 describes electrolyte compositions comprising silicon-containing compounds which may further contain heteroatoms such as B, Al, P, S, F, Cl, Br and I.

[0006] EP 2 573 854 A1 discloses an electrolyte composition for use in lithium ion batteries which contains a silyl ester group-containing phosphonic acid derivative to suppress the increase in battery resistance and the deterioration of battery performance in a high temperature environment.

[0007] US 2013 / 0164604 A1 refers to the use of phosphites, phosphonates and bisphosphonates as additives in electrolyte compositions for use in lithium ion batteries.

[0008] To improve the performance of lithium batteries, new cathode active materials are being used. These cathode active materials have higher specific energy and / or higher operating voltage. Examples of such cathode active materials include high-energy NCMs (lithiated mixed oxides of Ni, Co and Mn, so-called HE-NCMs), high-voltage manganese spinels with layered structures containing additional transition metals, and lithium nickel cobalt aluminum oxides (also called NCAs). Some of these cathode active materials require the use of high cut-off voltages during charging to obtain the desired high specific energy. These cathode active materials impose new demands on the electrolyte compositions used, for example, with regard to stability against high voltages, release of O2, metal dissolution due to dissolution of transition metal cations, gas evolution during storage, etc.

[0009] There remains a need to improve the performance of electrochemical cells, particularly those including the above-mentioned cathode active materials, with respect to, for example, high capacity retention, good long-term performance, high safety, reduced gassing, and reduced impedance build-up. Summary of the Invention [Problem to be solved by the invention]

[0010] It is an object of the present invention to provide an additive for use in an electrochemical cell that improves the performance of the electrochemical cell, for example, in terms of high capacity retention, good long-term performance, high safety, reduced gassing, and reduced impedance build-up. In particular, an additive should be provided for improving the performance of an electrochemical cell that includes a cathode active material having a high specific energy and / or a high operating voltage. Another object of the present invention is to provide an electrolyte composition for an electrochemical cell that results in an electrochemical cell with high capacity retention, good long-term performance, and high safety. In particular, an electrolyte composition for use with a cathode active material having a high specific energy and / or a high operating voltage should be provided. It is also an object of the present invention to provide an electrochemical cell that exhibits high capacity retention, good long-term performance, high safety, reduced gassing, and reduced impedance build-up. [Means for solving the problem]

[0011] Accordingly, there is provided an electrolyte composition comprising: (i) at least one aprotic organic solvent; (ii) at least one conductive salt; (iii) at least one phosphonic acid silyl ester containing the structure of formula (I) [ka] Where: T is [ka] and [ka] is selected from p is an integer from 0 to 6, (CH2) p One or more CH2 groups may be replaced by O, (CH2) p one or more H may be substituted with C1-C4 alkyl; R 1 are H, F, Cl, and R, respectively. 4 , OR 4 , OSi(R 5 )3, OSi(OR 4 )3, and OP(O)(OR 4 )R 5 are independently selected from R 4 are C1 to C 10 Alkyl, C3-C7 (hetero)cycloalkyl, C2-C 10 Alkenyl, C2-C 10 Alkynyl, C5-C7 (hetero)aryl, and C6-C 13 (hetero)aralkyl, and optionally substituted with one or more substituents selected from CN and F, and one or more CH groups of the alkyl, alkenyl, and alkynyl that are not directly bonded to a Si atom or an O atom may be replaced with O; R 3 and R 5 are each independently H, F, C1 to C 10 Alkyl, C3-C7 (hetero)cycloalkyl, C2-C 10 Alkenyl, C2-C 10 Alkynyl, C5-C7 (hetero)aryl and C6-C 13 (hetero)aralkyl, optionally substituted by one or more substituents selected from CN and F, wherein one or more CH groups of the alkyl, alkenyl and alkynyl that are not directly bonded to the P atom may be replaced by O, and (iv) optionally one or more additives.

[0012] Further provided is the use of phosphonic acid silyl esters containing units of formula (I) in electrochemical cells, for example as additives in electrochemical cells and electrolyte compositions for electrochemical cells. Electrochemical cells according to the invention exhibit good capacity retention, good long-term performance, reduced cell resistance, and reduced gas evolution during storage at elevated temperatures. The phosphonic acid silyl esters containing units of formula (I) are non-volatile under conditions during preparation, storage, and use of the electrochemical cells, which allows for easy handling and storage of the electrolyte compositions.

[0013] The present invention will be described in detail below. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Chemically, an electrolyte composition is any composition that contains free ions and, as a result, has electrical conductivity. The electrolyte composition serves as a medium for the transfer of ions involved in the electrochemical reaction taking place in an electrochemical cell. In the case of lithium batteries, the ions involved in the electrochemical reaction are usually lithium ions. The most common electrolyte compositions are aqueous ionic solutions, but molten electrolyte compositions and solid electrolyte compositions are possible as well. Thus, the electrolyte composition of the present invention is an electrically conductive medium due to the presence of at least one substance present primarily in the dissolved and / or molten state, i.e., electrical conductivity supported by the transfer of ionic species. In liquid or gel electrolyte compositions, the conductive salt is usually dissolved in one or more aprotic organic solvents.

[0015] The electrolyte composition contains at least one aprotic organic solvent (i). The at least one aprotic organic solvent may optionally be selected from fluorinated aprotic organic solvents, i.e. fluorinated aprotic organic solvents and non-fluorinated aprotic organic solvents. The electrolyte composition may contain a mixture of fluorinated and non-fluorinated aprotic organic solvents.

[0016] The aprotic organic solvent is preferably selected from optionally fluorinated cyclic and acyclic organic carbonates, optionally fluorinated acyclic ethers and polyethers, optionally fluorinated cyclic ethers, optionally fluorinated cyclic and acyclic acetals and ketals, optionally fluorinated orthocarboxylic acid esters, optionally fluorinated esters and diesters of cyclic and acyclic carboxylic acids, optionally fluorinated cyclic and acyclic sulfones, optionally fluorinated cyclic and acyclic nitriles and dinitriles, and optionally fluorinated cyclic and acyclic phosphates, and mixtures thereof.

[0017] Examples of optionally fluorinated cyclic carbonates are ethylene carbonate (EC), propylene carbonate (PC) and butylene carbonate (BC), in which one or more H may be replaced by F and / or C1 to C4 alkyl groups, such as 4-methylethylene carbonate, monofluoroethylene carbonate (FEC) and cis- and trans-difluoroethylene carbonate. Preferred optionally fluorinated cyclic carbonates are ethylene carbonate, monofluoroethylene carbonate, propylene carbonate, especially ethylene carbonate.

[0018] Examples of optionally fluorinated acyclic carbonates are di-C1-C 10 -alkyl carbonates, where each alkyl group is selected independently from the others, and one or more H may be replaced by F. Preferred are optionally fluorinated di-C1-C4-alkyl carbonates. Examples include, for example, diethyl carbonate (DEC), ethyl methyl carbonate (EMC), 2,2,2-trifluoroethyl methyl carbonate (TFEMC), dimethyl carbonate (DMC), trifluoromethyl carbonate (TFMMC), and methylpropyl carbonate. Preferred acyclic carbonates are diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC).

[0019] In one embodiment of the present invention, the electrolyte composition contains a mixture of an optionally fluorinated acyclic organic carbonate and a cyclic organic carbonate in a weight ratio of from 1:10 to 10:1, preferably from 3:1 to 1:1.

[0020] Examples of optionally fluorinated acyclic ethers and polyethers are optionally fluorinated di-C1-C 10 -alkyl ethers, optionally fluorinated di-C1-C4-alkyl-C2-C6 alkylene ethers, optionally fluorinated polyethers, and r H 2-r ) q -R″, where R′ is a C1-C 10 Alkyl group or C3-C 10 is a cycloalkyl group, and one or more H of the alkyl and / or cycloalkyl group are replaced by F, and R″ is H, F, C1-C 10 Alkyl group or C3-C 10 It is a cycloalkyl group, in which one or more H of the alkyl group and / or the cycloalkyl group are replaced with F; r is 1 or 2; and q is 1, 2, or 3.

[0021] According to the present invention, optionally fluorinated di-C1-C 10 - each alkyl group of the alkyl ether is selected independently from the other, and one or more H of the alkyl group may be replaced with F. 10 Examples of -alkyl ethers are dimethyl ether, ethyl methyl ether, diethyl ether, methyl propyl ether, diisopropyl ether, di-n-butyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (CF2HCF2CH2OCF2CF2H) and 1H,1H,5H-perfluoropentyl-1,1,2,2-tetrafluoroethyl ether (CF2H(CF2)3CH2OCF2CF2H).

[0022] Examples of optionally fluorinated di-C1-C4-alkyl-C2-C6-alkylene ethers are 1,2-dimethoxyethane, 1,2-diethoxyethane, diglyme (diethylene glycol dimethyl ether), triglyme (triethylene glycol dimethyl ether), tetraglyme (tetraethylene glycol dimethyl ether) and diethylene glycol diethyl ether.

[0023] Examples of suitable optionally fluorinated polyethers are polyalkylene glycols, preferably poly-C1-C4-alkylene glycols, in particular polyethylene glycols, in which one or more H of the alkyl or alkylene groups may be replaced by F. The polyethylene glycols may contain up to 20 mol % of one or more C1-C4-alkylene glycols in copolymerized form. The polyalkylene glycols are preferably dimethyl- or diethyl-endcapped polyalkylene glycols. The molecular weight Mw of suitable polyalkylene glycols, in particular suitable polyethylene glycols, may be at least 400 g / mol. The molecular weight Mw of suitable polyalkylene glycols, in particular suitable polyethylene glycols, may be up to 5 000 000 g / mol, preferably up to 2 000 000 g / mol.

[0024] Formula R'-(O-CF p H 2-p ) q Examples of -R" fluorinated ethers are 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (CF2HCF2CH2OCF2CF2H) and 1H,1H,5H-perfluoropentyl-1,1,2,2-tetrafluoroethyl ether (CF2H(CF2)3CH2OCF2CF2H).

[0025] Examples of optionally fluorinated cyclic ethers are 1,4-dioxane, tetrahydrofuran and derivatives thereof, such as, for example, 2-methyltetrahydrofuran, in which one or more H of the alkyl group may be replaced by F.

[0026] Examples of optionally fluorinated acyclic acetals are 1,1-dimethoxymethane and 1,1-diethoxymethane. Examples of cyclic acetals are 1,3-dioxane, 1,3-dioxolane and their derivatives, such as, for example, methyldioxolane, in which one or more H may be replaced by F.

[0027] Examples of optionally fluorinated acyclic orthocarboxylic acid esters are the tri-C1-C4 alkoxymethanes, in particular trimethoxymethane and triethoxymethane. Examples of suitable cyclic orthocarboxylic acid esters are 1,4-dimethyl-3,5,8-trioxabicyclo[2.2.2]octane and 4-ethyl-1-methyl-3,5,8-trioxabicyclo[2.2.2]octane, in which one or more H may be replaced by F.

[0028] Examples of optionally fluorinated acyclic esters of carboxylic acids are ethyl formate and methyl formate, ethyl acetate and methyl acetate, ethyl propionate and butanoate, and esters of dicarboxylic acids such as 1,3-dimethylpropanedioate, in which one or more H may be replaced by F. An example of a cyclic ester (lactone) of a carboxylic acid is γ-butyrolactone.

[0029] Examples of optionally fluorinated cyclic and acyclic sulfones are ethyl methyl sulfone, dimethyl sulfone and tetrahydrothiophene-S,S-dioxide (sulfolane).

[0030] Examples of optionally fluorinated cyclic and acyclic nitriles and dinitriles, in which one or more H may be replaced by F, are adipodinitrile, acetonitrile, propionitrile and butyronitrile.

[0031] Examples of optionally fluorinated cyclic and acyclic phosphates are trialkyl phosphates, such as trimethyl phosphate, triethyl phosphate and tris(2,2,2-trifluoroethyl) phosphate, in which one or more H of the alkyl group may be replaced by F.

[0032] More preferably, the aprotic organic solvent is selected from optionally fluorinated ethers and polyethers, optionally fluorinated cyclic and acyclic organic carbonates, optionally fluorinated cyclic and acyclic esters and diesters of carboxylic acids, and mixtures thereof. Even more preferably, the aprotic solvent is selected from optionally fluorinated ethers and polyethers, optionally fluorinated cyclic and acyclic organic carbonates, and mixtures thereof.

[0033] According to one embodiment, the electrolyte composition contains at least a solvent selected from compounds of fluorinated ethers and polyethers, such as the fluorinated ethers of the formula R’-(O-CF p H 2-p ) q -R” as defined above, such as CF2HCF2CH2OCF2CF2H or CF2H(CF2)3CH2OCF2CF2H.

[0034] According to another embodiment, the electrolyte composition contains at least one solvent selected from fluorinated cyclic carbonates, such as 1-fluoroethyl carbonate.

[0035] According to a further embodiment, the electrolyte composition contains at least one solvent selected from fluorinated cyclic carbonates, such as 1-fluoroethyl carbonate, and at least one solvent selected from compounds of fluorinated ethers and polyethers, such as the fluorinated ethers of the formula R’-(O-CF r H 2-r ) s -R” as defined above, such as CF2HCF2CH2OCF2CF2H or CF2H(CF2)3CH2OCF2CF2H.

[0036] According to another embodiment, the electrolyte composition contains at least one fluorinated cyclic carbonate, such as 1-fluoroethyl carbonate, and at least one non-fluorinated acyclic organic carbonate, such as dimethyl carbonate, diethyl carbonate, or ethyl methyl carbonate.

[0037] The electrolyte composition contains at least one conductive salt (ii). The electrolyte composition serves as a medium for the transfer of ions involved in the electrochemical reactions occurring in the electrochemical cell. The conductive salt (ii) present in the electrolyte composition is usually solvated in an aprotic organic solvent (i). Preferably, the at least one conductive salt (ii) is selected from lithium salts. Examples of lithium ion-containing conductive salts are: Li[F6-xP(CyF 2y+1 ) x In the formula, x is an integer ranging from 0 to 6, and y is an integer ranging from 1 to 20; Li[B(R I )4], Li[B(R I )2(OR II O)] and Li[B(OR II O)2], where each R I are each independently selected from F, Cl, Br, I, C1-C4 alkyl, C2-C4 alkenyl, C2-C4 alkynyl, OC1-C4 alkyl, OC2-C4 alkenyl and OC2-C4 alkynyl, where alkyl, alkenyl and alkynyl are selected from one or more of OR III may be substituted with OR III is selected from C1-C6 alkyl, C2-C6 alkenyl, and C2-C6 alkynyl; (OR II O) is a divalent radical derived from a 1,2- or 1,3-diol, a 1,2- or 1,3-dicarboxylic acid or a 1,2- or 1,3-hydroxycarboxylic acid, which divalent radical forms a 5- or 6-membered ring via the central B atom and both oxygen atoms; LiClO4; LiAsF6; LiCF3SO3; Li2SiF6; LiSbF6; LiAlCl4; Li(N(SO2F)2); lithium tetrafluoro(oxalato)phosphate; lithium oxalate; and · General formula Li[Z(C n F 2n+1 SO2) m wherein m and n are defined as follows: When Z is selected from oxygen and sulfur, m=1; When Z is selected from nitrogen and phosphorus, m=2; When Z is selected from carbon and silicon, m=3; n is an integer ranging from 1 to 20.

[0038] Divalent group (OR II Suitable 1,2- and 1,3-diols from which O) originate may be aliphatic or aromatic and may be selected, for example, from 1,2-dihydroxybenzene, propane-1,2-diol, butane-1,2-diol, propane-1,3-diol, butane-1,3-diol, cyclohexyl-trans-1,2-diol and naphthalene-2,3-diol, optionally substituted with one or more F and / or at least one linear or branched non-fluorinated, partially fluorinated or fully fluorinated C1-C4 alkyl group. An example of such a 1,2- or 1,3-diol is 1,1,2,2-tetra(trifluoromethyl)-1,2-ethanediol. By "fully fluorinated C1-C4 alkyl group" is meant that all H atoms of the alkyl group are replaced with F.

[0039] Divalent group (OR IISuitable 1,2- or 1,3-dicarboxylic acids from which O) originate may be aliphatic or aromatic, for example oxalic acid, malonic acid (propane-1,3-dicarboxylic acid), phthalic acid or isophthalic acid, preferably oxalic acid. The 1,2- or 1,3-dicarboxylic acids are optionally substituted by one or more F and / or at least one linear or branched non-fluorinated, partially fluorinated or fully fluorinated C1-C4 alkyl group.

[0040] Divalent group (OR II Suitable 1,2- or 1,3-hydroxycarboxylic acids from which O) originate may be aliphatic or aromatic, such as salicylic acid, tetrahydrosalicylic acid, malic acid and 2-hydroxyacetic acid, optionally substituted by one or more F and / or at least one linear or branched non-fluorinated, partially fluorinated or fully fluorinated C1-C4 alkyl group. An example of such a 1,2- or 1,3-hydroxycarboxylic acid is 2,2-bis(trifluoromethyl)-2-hydroxy-acetic acid.

[0041] Li[B(R I )4], Li[B(R I )2(OR II O)] and Li[B(OR II Examples of lithium difluorooxalatoborate are LiBF4, lithium difluorooxalatoborate and lithium dioxalatoborate.

[0042] Preferably, the at least one lithium ion-containing conductive salt is selected from LiPF6, LiAsF6, LiSbF6, LiCF3SO3, LiBF4, lithium bis(oxalato)borate, LiClO4, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2 and LiPF3(CF2CF3)3, more preferably the conductive salt is selected from LiPF6, LiN(SO2F)2 and LiBF4, and the most preferred conductive salt is LiPF6.

[0043] The conductive salt is usually present in a minimum concentration of at least 0.1 mol / l relative to the total electrolyte composition, preferably the concentration of the ion-containing conductive salt is from 0.5 to 2 mol / l.

[0044] The electrolyte composition comprises at least one phosphonic acid silyl ester comprising a structure of formula (I): [ka] During the ceremony, T is [ka] and [ka] Selected from; p is an integer from 0 to 6, (CH2) p One or more CH2 groups may be replaced by O, (CH2) p one or more H may be replaced with C1-C4 alkyl; R 1 are H, F, Cl, and R, respectively. 4 , OR 4 , OSi(R 5 )3, OSi(OR 4 )3, and OP(O)(OR 4 )R 5 are independently selected from; R 4 Each of C1 to C6 optionally substituted with one or more substituents selected from CN and F 10 Alkyl, C3-C7 (hetero)cycloalkyl, C2-C 10 Alkenyl, C2-C 10 Alkynyl, C5-C7 (hetero)aryl, and C6-C 13 (hetero)aralkyl, wherein one or more CH groups of the alkyl, alkenyl, and alkynyl that are not directly bonded to a Si atom or an O atom may be replaced with O; R 3 and R 5each of H, F, C1 to C2 optionally substituted with one or more substituents selected from CN and F; 10 Alkyl, C3-C7 (hetero)cycloalkyl, C2-C 10 Alkenyl, C2-C 10 Alkynyl, C5-C7 (hetero)aryl and C6-C 13 (hetero)aralkyl, where one or more CH2 groups of the alkyl, alkenyl, and alkynyl that are not directly bonded to a P atom may be replaced with O.

[0045] The phosphonic acid silyl ester containing the structure of formula (I) is also referred to as component (iii) of the electrolyte composition.

[0046] As used herein, the term “C1-C 10 "Alkyl" means a linear or branched saturated hydrocarbon group having 1 to 10 carbon atoms with one free valence, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, 2,2-dimethylpropyl, n-hexyl, 2-ethylhexyl, n-heptyl, isoheptyl, n-octyl, isooctyl, n-nonyl, n-decyl, etc. Preferred are C1 to C6 alkyl, more preferred are C1 to C4 alkyl, even more preferred are methyl, ethyl, and n- and isopropyl, and most preferred are methyl and ethyl.

[0047] As used herein, the term "C3-C7 (hetero)cycloalkyl" refers to a saturated 3- to 7-membered hydrocarbon ring having one free valence, in which one or more C atoms of the saturated ring may be replaced by heteroatoms selected from N, S, O and P, independently of one another. Examples of C3-C7 cycloalkyl include cyclopropyl, cyclobutyl, cyclopentyl and cyclohexyl, with cyclohexyl being preferred. Examples of C3-C7 heterocycloalkyl are oxiranyl, tetrahydrofuryl, pyrrolidyl, piperidyl and morpholinyl.

[0048] As used herein, the term “C2-C 10 "Alkenyl" refers to an unsaturated linear or branched hydrocarbon group having 2 to 10 carbon atoms with one free valence. Unsaturated means that the alkenyl group contains at least one C-C double bond. 10 Examples of alkenyl include ethenyl, propenyl, 1-n-butenyl, 2-n-butenyl, isobutenyl, 1-pentenyl, 1-hexenyl, 1-heptenyl, 1-octenyl, 1-nonenyl, 1-decenyl, etc. Preferred are C2-C6 alkenyl groups, more preferred are C2-C4 alkenyl groups, even more preferred are ethenyl and propenyl, and most preferred is 1-propen-3-yl, also known as allyl.

[0049] As used herein, the term “C2-C 10 "Alkynyl" means an unsaturated linear or branched hydrocarbon group having 2 to 10 carbon atoms with one free valence, the hydrocarbon group containing at least one C-C triple bond. Examples of C2-C6 alkynyl include ethynyl, propynyl, 1-n-butynyl, 2-n-butynyl, isobutynyl, 1-pentynyl, 1-hexynyl, 1-heptynyl, 1-octynyl, 1-nonyl, 1-decynyl, and the like. Preferred is C2-C6 alkynyl, even more preferred is C2-C4 alkynyl, and even more preferred is ethynyl and 1-propyn-3-yl (propargyl).

[0050] As used herein, the term "C5-C7 (hetero)aryl" refers to an aromatic 5-7 membered hydrocarbon ring or fused ring having one free valence, in which one or more of the C atoms of the aromatic ring may be replaced by heteroatoms selected from N, S, O and P, independently of one another. Examples of C5-C7 (hetero)aryl are pyrrolyl, furanyl, thiophenyl, pyridinyl, pyranyl, thiopyranyl and phenyl. Phenyl is preferred.

[0051] As used herein, the term “C6-C 13 "(Hetero)aralkyl" refers to an aromatic 5- to 7-membered hydrocarbon ring substituted with one or more C1-C6 alkyls, and one or more of the C atoms of the aromatic ring may be substituted, independently of one another, with a heteroatom selected from N, S, O and P. 13 A (hetero)aralkyl group contains a total of 6 to 13 C atoms and heteroatoms and has one free valence. The free valence may be located in an aromatic ring or in a C1 to C6 alkyl group, i.e., 13 (Hetero)aralkyl groups may be attached via the (hetero)aromatic portion or via the alkyl portion of the group. 13 Examples of (hetero)aralkyl include methylphenyl, 2-methylpyridyl, 1,2-dimethylphenyl, 1,3-dimethylphenyl, 1,4-dimethylphenyl, ethylphenyl, 2-propylphenyl, benzyl, 2-CH2-pyridyl, and the like.

[0052] R 1 are H, F, Cl, and R, respectively. 4 , OR 4 , OSi(R 5 )3, OSi(OR 4 )3, and OP(O)(OR 4 )R 5 are independently selected from

[0053] R 4 Each of C1 to C6 optionally substituted with one or more substituents selected from CN and F 10 Alkyl, C3-C7 (hetero)cycloalkyl, C2-C 10 Alkenyl, C2-C 10 Alkynyl, C5-C7 (hetero)aryl, and C6-C 13 One or more CH groups of alkyl, alkenyl, and alkynyl independently selected from (hetero)aralkyl that are not directly bonded to a Si atom or an O atom may be replaced with O. Preferably, R 4 Each of C1 to C6 optionally substituted with one or more substituents selected from CN and F10 One or more CH groups of alkyl, alkenyl and alkynyl independently selected from alkyl and not directly bonded to a Si atom or an O atom may be replaced with O, more preferably R 4 are each independently selected from C1-C4 alkyl optionally substituted with one or more substituents selected from CN and F. For example, R 4 may be selected from methyl, ethyl, n-propyl, i-propyl, phenyl, cyclohexyl, CF3, CF2CF3 or CH2CN.

[0054] R 5 each of H, F, C1 to C2 optionally substituted with one or more substituents selected from CN and F; 10 Alkyl, C3-C7 (hetero)cycloalkyl, C2-C 10 Alkenyl, C2-C 10 Alkynyl, C5-C7 (hetero)aryl, and C6-C 13 (hetero)aralkyl, one or more CH groups of alkyl, alkenyl and alkynyl that are not directly bonded to a P atom may be replaced with O, preferably R 5 each of H, F, and C1 to C4 each optionally substituted with one or more F and / or CN; 10 Independently selected from alkyl, one or more CH groups of the alkyl that are not directly bonded to the P atom may be replaced with O, and more preferred R 5 Each of C1 to C may be substituted with one or more F and / or CN. 10 More preferably, R is independently selected from alkyl. 5 are independently selected from H and C1-C4 alkyl, optionally substituted with one or more F and / or CN, where applicable. For example, R 5 may be selected from H, F, methyl, ethyl, n-propyl, i-propyl, phenyl, cyclohexyl, CF3, CF2CF3, or CH2CN.

[0055] Preferably, R 1 are H, F, Cl, C1-C, respectively.10 Alkyl and OC1-C 10 alkyl, which may be substituted by one or more substituents selected from CN and F, and one or more CH groups of the alkyl that are not directly bonded to a Si atom or an O atom may be substituted by O, and even more preferred R 1 is C1 to C6 optionally substituted with one or more substituents selected from CN and F; 10 R is independently selected from alkyl, and particularly preferred 1 is independently selected from C1-C4 alkyl optionally substituted with one or more substituents selected from CN and F. 1 are each independently selected from, for example, H, F, Cl, methyl, methoxy, ethyl, ethoxy, n-propyl, n-propoxy, i-propoxy, i-propyl, phenyl, phenoxy, CF, OCF, CFCF, OCFCF, and CHCN, and are preferably selected from methyl, ethyl, i-propyl, and n-propyl.

[0056] R 3 each of H, F, C1 to C2 optionally substituted with one or more substituents selected from CN and F; 10 Alkyl, C3-C7 (hetero)cycloalkyl, C2-C 10 Alkenyl, C2-C 10 Alkynyl, C5-C7 (hetero)aryl, and C6-C 13 One or more CH groups of alkyl, alkenyl, and alkynyl independently selected from (hetero)aralkyl and not directly bonded to a P atom may be replaced by O, preferably R 3 each of H, F, C1 to C2 optionally substituted with one or more substituents selected from CN and F; 10 independently selected from alkyl, C-C (hetero)cycloalkyl, C-C (hetero)aryl, one or more CH groups of alkyl, alkenyl and alkynyl that are not directly bonded to a P atom may be replaced with O, more preferably R 3each of H, F, and C1 to C4 each optionally substituted with one or more F and / or CN; 10 Independently selected from alkyl, one or more CH groups of the alkyl that are not directly bonded to the P atom may be replaced with O, and even more preferred R 3 are each H and C1 to C which may be substituted with one or more F and / or CN. 10 Independently selected from alkyl, one or more CH groups of the alkyl that are not directly bonded to the P atom may be replaced with O. 3 are each independently selected from H and C1-C4 alkyl optionally substituted with one or more F and / or CN. 3 R may be selected from, for example, H, F, methyl, ethyl, n-propyl, i-propyl, cyclohexyl, phenyl, CF, CFCF, CHCHOCH, CHCHOCH, and CHCN. 3 It is particularly preferred that is H.

[0057] T is [ka] and [ka] p is an integer from 0 to 6, and may be 1, 2, 3, 4, 5, or 6. (CH2) p One or more CH2 groups may be replaced by O, resulting in, for example, CH2-O-CH2 or CH2-O-CH2-O-CH2. When one or more CH2 groups are replaced by O, the CH2 groups replaced by O are not adjacent. (CH2) p One or more H may be substituted with C1-C4 alkyl. Examples of (CH2)p in which one or more H is substituted with C1-C4 alkyl are C(CH3)H, C(CH3)2, C(CH3)HCH2, C(CH3)HC(CH3)H, and C(CH3)HC(C2H4)H.

[0058] Examples of structures of formula (I) are structures (I.1) to (I.5) below.

[0059] [ka]

[0060] Preferably, the phosphonic acid silyl ester containing the structure of formula (I) is -P(O)R 3 With a phosphonic acid group selected from -OC1-C6 alkyl, more preferably -P(O)R 3 With a phosphonic acid group selected from -OC1-C4 alkyl, particularly preferred is -P(O)R 3 -OCH3 and -P(O)R 3 It is terminated by a phosphonic acid group selected from -OCH2CH3.

[0061] According to one embodiment, the phosphonic acid silyl ester comprises the structure of formula (II): [ka]

[0062] In the formula, Q 1 is a chemical bond or a monomeric or oligomeric group containing one or more monomeric units of formula (II.1), Q 2 is a chemical bond or a monomeric or oligomeric group containing one or more monomeric units of formula (II.2).

[0063] [ka]

[0064] In the formula, T * are each independently Si or Si-(CH2) p -Si, p is an integer from 0 to 6, i.e., p is selected from 0, 1, 2, 3, 4, 5, and 6, (CH2) p One or more CH2 groups may be replaced by O, (CH2) pOne or more H may be replaced with C1-C4 alkyl, and T * If is Si, then q 1 is an integer between 0 and 2, q 2 is an integer between 0 and 2, q 1 +q 2 = 2, i.e., q 1 andq 2 is selected from 0, 1, and 2, and q 1 +q 2 = 2;T * Si-(CH2) p - For Si, q 1 is an integer between 0 and 4, q 2 is an integer between 0 and 4, q 1 +q 2 = 4, i.e. q 1 andq 2 is selected from 0, 1, 2, 3, and 4; q 1 +q 2 = 4; - * is a continuation of the phosphonic acid silyl ester backbone by branching; and R 1 and R 3 is defined as above and as preferred.

[0065] Q 1 Examples of [ka] It is.

[0066] Q 2 Examples of [ka] It is.

[0067] Q 1 and Q 2 The monomer units of can be arranged in any manner, for example randomly, or in blocks, or in alternating order.

[0068] Preferably, Q 1and / or Q 2は , respectively, comprising at least one monomer unit of formula (II.1) or formula (II.2) which is not a branched or bridging unit, i.e. where T * are Si or Si-(CH2), respectively. p -Si, and p is an integer from 0 to 6, (CH2) p One or more CH2 groups may be replaced by O, (CH2) p One or more H may be replaced with C1-C4 alkyl, and T * If is Si, then q 1 is zero, and q 2 is 2, and T * Si-(CH2) p - If Si, then q 1 is zero, and q 2 is 4.

[0069] According to another embodiment, the phosphonic acid silyl ester has the formula (III): [ka] During the ceremony, Q 1 ,Q 2 , T and R 3 is defined as above; R 6 and R 7 is R 8 and Si(OR 8 )3 and Si(R 9 ) 3 independently selected; R 8 Each of C1 to C6 optionally substituted with one or more substituents selected from CN and F 10 Alkyl, C3-C7 (hetero)cycloalkyl, C2-C 10 Alkenyl, C2-C 10 Alkynyl, C5-C7 (hetero)aryl, and C6-C 13 (hetero)aralkyl, wherein one or more CH groups of alkyl, alkenyl and alkynyl that are not directly bonded to an O atom or a Si atom may be replaced with O; and R9 each of H, F, Cl, C1 to C4, each of which may be substituted with one or more substituents selected from CN and F; 10 Alkyl, C3-C7 (hetero)cycloalkyl, C2-C 10 Alkenyl, C2-C 10 Alkynyl, C5-C7 (hetero)aryl, and C6-C 13 One or more CH2 groups of alkyl, alkenyl and alkynyl independently selected from (hetero)aralkyl that are not directly bonded to an O atom may be replaced with O.

[0070] R 6 and R 7 However, independently, C1~C 10 Alkyl, Si(OC1-C 10 alkyl)3 and Si(R 9 ) 3, R 9 are H, F, Cl, and C1 to C 10 More preferably, R is independently selected from alkyl. 9 is selected from H, F, Cl, and C1-C4 alkyl. 6 and R 7 R may be selected from, for example, methyl, ethyl, n-propyl, i-propyl, Si(CH3)3, Si(OCH3)3, Si(CH3)2Cl, and Si(CH3)Cl2. 6 and R 7 are independently selected from C1-C4 alkyl, i.e., the phosphonic acid silyl ester is terminated with an alkoxy group such as methoxy, ethoxy, n-propoxy and n-butoxy, and particularly preferred are methoxy and ethoxy terminated phosphonic acid silyl esters.

[0071] In particular, the phosphonic acid silyl ester may have the formula (IV): [ka] During the ceremony, R 1 , R 3 , R 6 , R7 , T, T * , q 1 and q 2 is defined as above and is preferred; and r 1 and r 2 are independent integers between 0 and 300.

[0072] According to one embodiment of the present invention, the phosphonic acid silyl ester containing the structure of formula (I) is used as a mixture of different phosphonic acid silyl esters having different molecular weights, in particular a mixture of a monomeric phosphonic acid silyl ester containing the structure of formula (I) that does not contain a repeating monomer unit and at least one oligomeric or polymeric phosphonic acid silyl ester containing the structure of formula (I) and one or more repeating monomer units, for example, r 1 and r 2 are both 0, and a compound of formula (IV) and r 1 +r 2 In the present case, the phosphonic acid silyl ester is used as a mixture with at least one oligomeric or polymeric phosphonic acid silyl ester of formula (IV) where R 1 is an integer from 1 to 10;

[0073] The preparation of analogous phosphonic acid silyl esters containing the structure of formula (I) is known to those skilled in the art, see, for example, K. Kellner, L. Rodewald, Monatshefte für Chemie, Vol. 121 (1990), pp. 1031-1038. The oligomeric phosphonic acid silyl esters used according to the present invention can be prepared in a similar manner. Depending on the starting material, linear compounds or compounds with branching or crosslinking functions are obtained. For example, the reaction of (CH3)2SiCl2 with dimethyl phosphite gives linear phosphonic acid silyl esters. When part of (CH3)2SiCl2 is replaced by (CH3)SiCl3 or SiCl4, a monomer unit is introduced into the phosphonic acid silyl ester that functions as a branching or crosslinking point. In addition, (CH3)2SiCl2 can be replaced by alkylidene interval dichlorodisilanes, such as Cl(CH3)2Si(CH2)2Si(CH3)2Cl. Depending on the starting compounds, molar ratios and reaction conditions, different phosphonic acid silyl esters and often mixtures of monomeric and one or more oligomeric and polymeric phosphonic acid silyl esters of different molecular weights are obtained.

[0074] Another aspect of the present invention is the use of phosphonic acid silyl esters containing the structure of formula (I) in electrolyte compositions for electrochemical cells, such as lithium ion capacitors, double layer capacitors and lithium batteries, particularly lithium secondary batteries as described below. Phosphonic acid silyl esters containing the structure of formula (I) are particularly suitable as cathode active materials that can interact with the cathode at the cathode-electrolyte interface, thereby reducing undesirable reactions between the cathode active material and the electrolyte composition, for example, by forming a coating on the cathode or by preventing the formation of electrolyte decomposition products (e.g., HF) that are harmful to the operation of the battery, and can suppress direct contact between the components of the electrolyte composition and the cathode active material. Direct contact between the electrolyte composition and the cathode often causes decomposition reactions.

[0075] The phosphonic acid silyl esters containing the structure of formula (I) can also be used as additives to reduce gas generation in electrolyte compositions for electrochemical cells, such as lithium ion capacitors, double layer capacitors and lithium batteries, particularly lithium secondary batteries, as described below. Unwanted gas generation in electrochemical cells is a safety issue, as an increase in internal pressure can lead to leakage of the battery and loss of electrolyte composition, increasing the possibility of fire and emission of harmful compounds.

[0076] The phosphonic acid silyl ester containing the structure of formula (I) is typically used in the electrolyte composition at the concentrations given below by adding the desired amount of the compound of formula (I) to the electrolyte composition. Depending on the molecular weight and the presence of branching / bridging units, the phosphonic acid silyl ester may be soluble or swollen in the non-aqueous solvent (ii).

[0077] The electrolyte composition may contain one type of phosphonic acid silyl ester containing the structure of formula (I), or may contain two or more types of phosphonic acid silyl ester containing the structure of formula (I), for example, two or three or more types.

[0078] Usually, the electrolyte composition contains at least one phosphonic acid silyl ester containing the structure of formula (I) in a total amount of at least 0.01 mass%, preferably at least 0.02 mass%, more preferably at least 0.1 mass%, based on the total mass of the electrolyte composition. The upper limit of the total concentration of the phosphonic acid silyl ester containing the structure of formula (I) in the electrolyte composition is usually 10 mass%, preferably 5 mass%, more preferably 3 mass%, based on the total mass of the electrolyte composition. Usually, the electrolyte composition contains at least one phosphonic acid silyl ester containing the structure of formula (I) in a total amount of 0.01 to 10 mass%, preferably 0.02 to 10 mass%, more preferably 0.1 to 5 mass%, most preferably 0.1 to 3 mass%, based on the total mass of the electrolyte composition.

[0079] In addition, the electrolyte composition may contain at least one additional additive different from the phosphonic acid silyl ester containing the structure of formula (I). The at least one additional additive different from the phosphonic acid silyl ester containing the structure of formula (I) may be selected from polymers, film-forming additives, flame retardants, overcharge additives, wetting agents, HF and / or H2O scavengers, stabilizers for LiPF6 salts, ionic solvation promoters, corrosion inhibitors, and gelling agents.

[0080] The minimum concentration of the at least one further additive is usually 0.005% by weight, preferably 0.01% by weight, more preferably 0.1% by weight, based on the total weight of the electrolyte composition. The maximum concentration of the at least one further additive is usually 25% by weight.

[0081] One class of further additives is polymer.Polymer can be selected from polyvinylidene fluoride, polyvinylidene-hexafluoropropylene copolymer, polyvinylidene-hexafluoropropylene-chlorotrifluoroethylene copolymer, Nafion, polyethylene oxide, polymethylmethacrylate, polyacrylonitrile, polypropylene, polystyrene, polybutadiene, polyethylene glycol, polyvinylpyrrolidone, polyaniline, polypyrrole and / or polythiophene.Polymer can be added to the formulation according to the invention to transform the liquid agent into a semi-solid or solid electrolyte during aging, thus improving solvent retention.In this case, the polymer functions as a gelling agent.

[0082] Examples of flame retardants are organophosphorus compounds such as cyclophosphazenes, phosphoramides, alkyl and / or aryl trisubstituted phosphates, alkyl and / or aryl di- or trisubstituted phosphates, alkyl and / or aryl disubstituted phosphonates, alkyl and / or aryl trisubstituted phosphines, and fluorinated derivatives thereof. Examples of HF and / or HO scavengers are optionally halogenated cyclic and acyclic silylamines.

[0083] Examples of overcharge protection additives include cyclohexylbenzene, o-terphenyl, p-terphenyl, and biphenyl, with cyclohexylbenzene and biphenyl being preferred.

[0084] Another class of additives are film-forming additives, also called SEI-forming additives. The SEI-forming additives according to the present invention are compounds that decompose on the electrode to form a non-passivation layer on the electrode that prevents the decomposition of the electrolyte and / or the electrode. In this way, the life of the battery is significantly extended. Preferably, the SEI-forming additive forms a passivation layer on the anode. The anode in the context of the present invention is understood as the negative electrode of the battery. Preferably, the anode has a reduction potential of 1 volt or less with respect to lithium, such as a lithium intercalated graphite anode. To determine whether a compound qualifies as an anode film-forming additive, an electrochemical cell can be prepared that includes a graphite electrode and a metal counter electrode, as well as an electrolyte that contains a small amount of said compound, typically 0.1-10% by weight of the electrolyte composition, preferably 0.2-5% by weight of the electrolyte composition. When a voltage is applied between the anode and the lithium metal, the differential capacity of the electrochemical cell is recorded between 0.5V and 2V. If a large differential capacity is observed during the first cycle, e.g., −150 mAh / V at 1 V, but not observed or essentially not observed during any of the subsequent cycles in said voltage range, the compound can be considered an SEI forming additive.

[0085] According to the present invention, the electrolyte composition preferably contains at least one SEI-forming additive. SEI-forming additives are known to those skilled in the art. More preferably, the electrolyte composition contains at least one SEI-forming additive selected from vinylene carbonate and its derivatives, such as vinylene carbonate and methylvinylene carbonate; fluorinated ethylene carbonate and its derivatives, such as monofluoroethylene carbonate, cis- and trans-difluorocarbonate; organic sultones, such as propylene sultone, propane sultone and their derivatives; ethylene sulfite and its derivatives; oxalates, including compounds such as lithium oxalate, dimethyl oxalate, oxalatoborates, including lithium bis(oxalato)borate, lithium difluoro(oxalato)borate and ammonium bis(oxalato)borate, and oxalatophosphates, including lithium tetrafluoro(oxalato)phosphate; and sulfur-containing additives, as described in detail in WO 2013 / 026854 A1, in particular the sulfur-containing additives described on page 12, line 22 to page 15, line 10.

[0086] The added compound may have more than one effect in the electrolyte composition and in the electrochemical cell that contains the electrolyte composition, for example, lithium oxalatoborate may be added as an additive to promote SEI formation but also function as a conductive salt.

[0087] In one embodiment of the present invention, the water content of the electrolyte composition is preferably less than 100 ppm, more preferably less than 50 ppm, and most preferably less than 30 ppm, based on the weight of the respective inventive formulation. The water content can be determined by titration, for example according to DIN 51777 or Karl Fischer, as detailed in ISO 760:1978. The minimum water content of the electrolyte composition can be selected from 3 ppm, preferably from 5 ppm.

[0088] In one embodiment of the present invention, the HF content of the electrolyte composition is preferably less than 100 ppm, more preferably less than 50 ppm, and most preferably less than 30 ppm, based on the weight of each inventive formulation. The HF content may be determined by titration.

[0089] The electrolyte composition is preferably liquid at the conditions of use, even more preferably the electrolyte composition is liquid at 1 bar and 25° C., even more preferably the electrolyte composition is liquid at 1 bar and −15° C., in particular the electrolyte composition is liquid at 1 bar and −30° C., even more preferably the electrolyte composition is liquid at 1 bar and −50° C. Such liquid electrolyte compositions are particularly suitable for use in outdoor applications, e.g. in automotive batteries.

[0090] The electrolyte composition (A) can be prepared by methods known to those skilled in the art in the field of electrolyte manufacturing, generally by dissolving the lithium conductive salt (i) in a corresponding solvent or solvent mixture (ii) and adding at least one phosphonic acid silyl ester containing the structure of formula (I) and, optionally, further additives (iv), as described above.

[0091] The electrochemical cell containing the electrolyte composition (A) may be a lithium battery, a double layer capacitor, or a lithium ion capacitor. The general structure of such electrochemical devices is well known and batteries are known to those skilled in the art.

[0092] Preferably, the electrochemical cell of the present invention is a lithium battery. As used herein, the term "lithium battery" refers to an electrochemical cell in which the anode contains lithium metal or lithium ions at some point during charging / discharging of the cell. The anode may contain lithium metal or a lithium metal alloy, a material that absorbs and releases lithium ions, or other lithium-containing compounds. The lithium battery is preferably a lithium secondary battery, i.e., a rechargeable lithium battery.

[0093] In a particularly preferred embodiment, the electrochemical cell is a lithium ion cell, i.e., a secondary lithium ion electrochemical cell comprising a cathode (A) comprising a cathode active material capable of reversibly absorbing and releasing lithium ions, and an anode (B) comprising an anode active material capable of reversibly absorbing and releasing lithium ions.

[0094] The anode (A) comprises an anode active material capable of reversibly absorbing and releasing lithium ions or forming an alloy with lithium. In particular, a carbonaceous material capable of reversibly absorbing and releasing lithium ions can be used as the anode active material.

[0095] Suitable carbonaceous materials include graphitic materials, more particularly crystalline carbons such as natural graphite, graphitized coke, graphitized MCMB and graphitized MPCF; amorphous carbons such as coke, mesocarbon microbeads (MCMB) calcined at 1500° C. or less, and mesophase pitch-based carbon fibers (MPCF); hard carbons; carbon anode active materials (pyrolytic carbon, coke, graphite) such as carbon composites, burned organic polymers, and carbon fibers. The preferred carbonaceous material is graphite.

[0096] Further examples of anode active materials are lithium metal and lithium metal alloys, i.e., materials containing elements capable of forming alloys with lithium. Non-limiting examples of materials containing elements capable of forming alloys with lithium include metals, metalloids, or alloys thereof. As used herein, the term "alloy" should be understood to refer to both alloys of two or more metals and alloys of one or more metals with one or more metalloids. If the alloy has metallic properties overall, the alloy may contain non-metallic elements. The texture of the alloy may be a solid solution, a eutectic (eutectic mixture), an intermetallic compound, or two or more of them coexist. Examples of such metal or metalloid elements include, but are not limited to, titanium (Ti), tin (Sn), lead (Pb), aluminum, indium (In), zinc (Zn), antimony (Sb), bismuth (Bi), gallium (Ga), germanium (Ge), arsenic (As), silver (Ag), hafnium (Hf), zirconium (Zr), yttrium (Y), and silicon (Si). Metal elements and metalloid elements of Group 4 or Group 14 of the long-period table of elements are preferred, and titanium, silicon, and tin are particularly preferred, with silicon being especially preferred. Examples of tin alloys include those having one or more elements selected from the group consisting of silicon, magnesium (Mg), nickel, copper, iron, cobalt, manganese, zinc, indium, silver, titanium (Ti), germanium, bismuth, antimony, and chromium (Cr) as the second constituent element other than tin. Examples of silicon alloys include those that contain, as a second constituent element other than silicon, one or more elements selected from the group consisting of tin, magnesium, nickel, copper, iron, cobalt, manganese, zinc, indium, silver, titanium, germanium, bismuth, antimony and chromium.

[0097] Further possible anode active materials are silicon-containing materials. Silicon-containing materials include silicon itself, such as amorphous and crystalline silicon, silicon-containing compounds, such as 0.1% silicon, 0.2% silicon, 0.3% silicon, 0.4% silicon, 0.5% silicon, 0.6% silicon, 0.7% silicon, 0.8% silicon, 0.9% silicon, 0.1% silicon, 0.2% silicon, 0.4% silicon, 0.5% silicon, 0.6% silicon, 0.7% silicon, 0.8% silicon, 0.9% silicon, 0.9% silicon, 0.9% silicon, 0.1% silicon, 0.1% silicon, 0.2% silicon, 0.3% silicon, 0.4% silicon, 0.5% silicon, 0.6% silicon, 0.7% silicon, 0.8% silicon, 0.9% silicon, 0.9% silicon, 0.9% silicon, 0. <x<1.5のSiO x, and Si alloys, and compositions containing silicon and / or silicon-containing compounds, such as silicon / graphite composites and carbon-coated silicon-containing materials. Silicon itself can be used in different forms, such as nanowires, nanotubes, nanoparticles, films, nanoporous silicon, or silicon nanotubes. Silicon can be deposited on a current collector. The current collector may be selected from a coated metal wire, a coated metal grid, a coated metal web, a coated metal sheet, a coated metal foil, or a coated metal plate. Preferably, the current collector is a coated metal foil, such as a coated copper foil. The thin film of silicon may be deposited on the metal foil by any technique known to those skilled in the art, for example, by a sputtering technique. One method for producing silicon thin film electrodes is described by R.Elazari et al.; Electrochem.Comm. 2012,14,21-24.

[0098] Another possible anode active material is a lithium ion intercalated oxide of Ti.

[0099] Preferably, the anode active material comprises a carbonaceous material capable of reversibly absorbing and releasing lithium ions, and more preferably, a carbonaceous material capable of reversibly absorbing and releasing lithium ions. The carbonaceous material that can be used is selected from crystalline carbon, hard carbon and amorphous carbon; Graphite is particularly preferred. It is also preferred that the anode active material comprises a silicon-containing material. It is further preferred that the anode active material comprises a lithium ion intercalated oxide of Ti.

[0100] The electrochemical cell of the present invention comprises a cathode (B) comprising at least one cathode active material, the at least one cathode active material comprising a material capable of absorbing and releasing lithium ions and selected from mixed lithium transition metal oxides containing Mn and at least one secondary transition metal, lithium intercalate mixed oxides containing Ni, Al and at least one secondary transition metal, LiNiPO4, LiNiPO4, and LiCoPO4.

[0101] Examples of mixed lithium transition metal oxides containing Mn and at least one second transition metal include those represented by the formula (II): Li 1+e (NiaCo b Mn c M d ) 1-e O2 (II) During the ceremony, a is in the range of 0.05 to 0.9, preferably in the range of 0.1 to 0.8; b is in the range of 0 to 0.35; c is in the range of 0.1 to 0.9, preferably in the range of 0.2 to 0.8; d is in the range of 0 to 0.2, e is in the range of 0 to 0.3, preferably in the range of greater than 0 to 0.3, more preferably in the range of 0.05 to 0.3; a+b+c+d=1, M is one or more metals selected from Na, K, Al, Mg, Ca, Cr, V, Mo, Ti, Fe, W, Nb, Zr and Zn.

[0102] The cobalt-containing compounds of formula (II) are also known as NCMs.

[0103] The mixed lithium transition metal oxides having the layered structure of formula (II) where e is greater than 0 are also called perlithiated.

[0104] Preferred lithium transition metal oxides having a layered structure of formula (II) are compounds in which the LiM'O2 phase, where M' is one or more transition metals selected from Ni and optionally Co and Mn, is mixed with the Li2MnO3 phase to form a solid solution, in which one or more metals M as defined above may be present. The one or more metals M are usually present in trace amounts, for example up to 10 mol% M, or up to 5 mol% M, or up to 1 mol%, based on the total amount of metals other than lithium present in the transition metal oxide, and are therefore also called "dopants" or "doping metals". When one or more metals M are present, they are usually present in an amount of at least 0.01 mol% or at least 0.1 mol%, based on the total amount of metals other than lithium present in the transition metal oxide. These compounds also have the formula (IIa) zLiM'O2·(1-z)Li2MnO3 (IIa) In the formula, M' is Ni and at least one metal selected from Mn and Co; z is between 0.1 and 0.8; One or more metals selected from Na, K, Al, Mg, Ca, Cr, V, Mo, Ti, Fe, W, Nb, Zr and Zn may be present.

[0105] Electrochemically, the Ni and, if present, Co atoms of the LiM'O2 phase participate in reversible oxidation and reduction reactions, and Li + At voltages below 4.5 V vs. Li, the Li2MnO3 phase undergoes Li ion deintercalation and intercalation, respectively, when the oxidation state of Mn in the Li2MnO3 phase is +4. + It only participates in oxidation and reduction reactions at voltages above 4.5 V vs. ZnO / Li. Thus, electrons are not removed from the Mn atoms in this phase but from the 2p orbitals of the oxygen ions, resulting in the removal of oxygen from the lattice structure in the form of O2 gas, at least during the first charging cycle.

[0106] These compounds are also called HE-NCMs because they have a higher energy density than conventional NCMs. Both HE-NCMs and NCMs are Li / Li + Although they have an operating voltage of about 3.0-3.8 V for Li / Li, in order to actually reach full charge and reap the benefits of their higher energy density, a higher cut-off voltage must be used for both activation and cycling of HE-NCMs. + The upper cut-off voltage of the cathode during charging to 1000 V is at least 4.5 V, preferably at least 4.6 V, more preferably at least 4.7 V, and even more preferably at least 4.8 V to activate the HE-NCM. + The term "upper cut-off voltage during charging to a Li / Li battery" refers to a voltage that constitutes the upper limit of the voltage to which an electrochemical cell is charged. + This refers to the voltage of the cathode in an electrochemical cell relative to a reference anode. An example of a HE-NCM is 0.33Li2MnO3 0.67Li(Ni 0.4 Co 0.2 Mn 0.4 )O2, 0.42Li2MnO3·0.58Li(Ni 0.4 Co 0.2 Mn 0.4 )O2, 0.50Li2MnO3·0.50Li(Ni 0.4 Co 0.2 Mn 0.4 )O2, 0.40Li2MnO3·0.60Li(Ni 0.8 Co 0.1 Mn 0.1 )O2 and 0.42Li2MnO3·0.58Li(Ni 0.6 Mn 0.4 )O2.

[0107] An example of a manganese-containing transition metal oxide having a layered structure of formula (II) in which d is 0 is LiNi 0.33 Mn 0.67 O2, LiNi 0.25 Mn 0.75 O2, LiNi 0.35 Co 0.15 Mn 0.5 O2, LiNi 0.21 Co0.08 Mn 0.71 O2, LiNi 0.22 Co 0.12 Mn 0.66 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2 and LiNi 0.5 Co 0.2 Mn 0.3 O2. It is preferred that the transition metal oxide of general formula (II) where d is 0 does not contain significant amounts of further cations or anions.

[0108] An example of a manganese-containing transition metal oxide having a layered structure of formula (II) where d is greater than 0 is 0.33Li2MnO3 0.67Li(Ni 0.4 Co 0.2 Mn 0.4 )O2, 0.42Li2MnO3·0.58Li(Ni 0.4 Co 0.2 Mn 0.4 )O2, 0.50Li2MnO3·0.50Li(Ni 0.4 Co 0.2 Mn 0.4 )O2, 0.40Li2MnO3·0.60Li(Ni 0.8 Co 0.1 Mn 0.1 )O2 and 0.42Li2MnO3·0.58Li(Ni 0.6 Mn 0.4 )O2, and one or more metals M may be present, selected from Na, K, Al, Mg, Ca, Cr, V, Mo, Ti, Fe, W, Nb, Zr and Zn. Preferably, the one or more doping metals are present in an amount of up to 1 mol %, based on the total amount of metals, excluding lithium, present in the transition metal oxide.

[0109] Other preferred compounds of formula (II) are Ni-rich compounds, having a Ni content of at least 50 mol % based on the total amount of transition metals present. This includes compounds of formula (IIb): Li 1+e (Nia Co b Mn c M d ) 1-e O2 (IIb) During the ceremony, a is in the range of 0.5 to 0.9, preferably in the range of 0.5 to 0.8; b is in the range of 0 to 0.35; c is in the range of 0 to 0 and in the range of 0.2 to 0.5; d is in the range of 0 to 0.2; e is in the range of 0 to 0.3; a+b+c+d=1 M is one or more metals selected from Na, K, Al, Mg, Ca, Cr, V, Mo, Ti, Fe, W, Nb, Zr, and Zn.

[0110] Examples of Ni-rich compounds of formula (I) include Li[Ni 0.8 Co 0.1 Mn 0.1 ]O2(NCM811), Li[Ni 0.6 Co 0.2 Mn 0.2 ]O2(NCM622), and Li[Ni 0.5 Co 0.2 Mn 0.3 ]O2(NCM523) is one example.

[0111] Further examples of mixed lithium transition metal oxides containing Mn and at least one second transition metal include manganese-containing spinels of formula (III): Li 1+t M 2-t O 4-s (III) During the ceremony, s is between 0 and 0.4, t is from 0 to 0.4, M is at least one further metal selected from Mn and Co and Ni, preferably M is Mn and Ni, and optionally Co, i.e. one portion of M is Mn and another portion of M, and optionally a further portion of M is selected from Co.

[0112] The cathode active material may also be selected from lithium intercalation mixed oxides containing Ni, Al and at least one second transition metal, such as lithium intercalation mixed oxides of Ni, Co and Al. An example of a mixed oxide of Ni, Co and Al is the compound of formula (IV): Li[Ni h Co i Al j ]O2 (IV) During the ceremony, h is from 0.7 to 0.9, preferably from 0.8 to 0.87, more preferably from 0.8 to 0.85; i is between 0.15 and 0.20; and j is from 0.02 to 10, preferably from 0.02 to 1, more preferably from 0.2 to 0.1, and most preferably from 0.02 to 0.03.

[0113] The cathode active material may also be selected from LiMnPO4, LiNiPO4 and LiCoPO4. These phosphates usually exhibit an olivine structure and usually need to be used for charging an upper cut-off voltage of at least 4.5V.

[0114] The cathode (B) may further contain further components such as binders and conductive materials such as conductive carbon. For example, the cathode (B) may contain a conductive polymorph of carbon, for example selected from graphite, carbon black, carbon nanotubes, graphene or a mixture of at least two of the aforementioned materials. Examples of binders used in the cathode (B) may include organic polymers such as polyethylene, polyacrylonitrile, polybutadiene, polypropylene, polystyrene, polyacrylate, polyvinyl alcohol, polyisoprene, and copolymers of at least two comonomers selected from ethylene, propylene, styrene, (meth)acrylonitrile and 1,3-butadiene, in particular styrene-butadiene copolymers, and halogenated (co)polymers such as polyvinylidene chloride, polyvinyl chloride, polyvinyl fluoride, polyvinylidene fluoride (PVdF), polytetrafluoroethylene, copolymers of tetrafluoroethylene and hexafluoropropylene, copolymers of tetrafluoroethylene, vinylidene fluoride and polyacrylonitrile.

[0115] The anode (A) and cathode (B) can be prepared by preparing an electrode slurry composition by dispersing the electrode active material, binder, optional conductive material, and optionally a thickener in a solvent, and coating the slurry composition onto a current collector. The current collector can be a metal wire, metal grid, metal web, metal sheet, metal foil, or metal plate. Preferably, the current collector is a metal foil, such as a copper foil or an aluminum foil.

[0116] The electrochemical cell of the present invention may further contain further components, as is customary per se, such as separators, housings, cable connections, etc. The housing may be of any shape, for example a cubic or cylindrical shape, the shape of a prism or the housing used is a metal-plastic composite film processed as a pouch. Suitable separators are, for example, glass fiber separators and polymer-based separators, such as polyolefin separators or Nafion separators.

[0117] Several electrochemical cells of the invention may be connected to each other, for example in a series or parallel connection. A series connection is preferred. The invention further provides the use of an electrochemical cell of the invention as described above in a device, in particular a mobile device. Examples of mobile devices include vehicles, such as automobiles, bicycles, aircraft, or water vehicles, such as boats and ships. Other examples of mobile devices are portable devices, such as computers, in particular laptop computers, telephones, or power tools, for example from the construction field, in particular drills, battery-powered screwdrivers or battery-powered staplers. However, the electrochemical cell of the invention can also be used for stationary energy storage.

[0118] The present invention is further illustrated by the following examples which should not be construed as limiting the invention. EXAMPLES

[0119] I. Additives: I.1 Overview of electrolyte additives used: [ka]

[0120] The units in square brackets indicate the repeating monomer units. The oligomers are typically terminated with -OP(O)H-OCH3 or -OP(O)H-OCH2CH3, except for oligomers containing Si(CH3)3 end groups.

[0121] I.2 Preparation of the additive Comparative additive R1 was used commercially. Comparative additive R2 was prepared according to R. Rabinowitz, J. Org. Chem. Vol. 28 (1963), pp. 2975-2978. Additive mixtures M1 to M12 containing molecular entities A1 to A19 were synthesized according to K. Kellner, L. Rodewald, Monatshefte für Chemie, Vol. 121 (1990), pp. 1031-1038.

[0122] All compounds were prepared directly 1 H NMR spectroscopy and 31 The samples were analyzed using P NMR spectroscopy. Samples were prepared and run under an inert atmosphere using CDCl3 (7.26 ppm) as the reference; when analyzing electrolytes, a screw-cap NMR tube was used with the inner tube filled with C6D6 (7.16 ppm) as the reference. Spectra were recorded using a Bruker Avance III or 1 H: 500.36MHz, 31 P: Recorded on a Varian NMR System 400 operating at a frequency of 202.56 MHz. 31 P NMR data was collected isolated from protons: {1H} for clarity. 31 The relaxation time D1 for P NMR measurements was increased to 60 s, and the amount of each P species was determined accordingly. MNova software was used to analyze the spectra.

[0123] Viscosity measurements were performed using an Anton Paar Physica MCR 51. Measurements were performed at 20°C for 1 to 1000 s. -1 A shear stress profile of 0.01 mm was performed and the average value was calculated to obtain the given value. A summary of all additive mixtures prepared is given in Table 1.

[0124] Experiment 1 - Mixture M1: According to the method described above, Me2SiCl2 (1.0 eq, 800 mmol, 104.8 g) was added to dimethyl phosphite (1.0 eq, 800 mmol, 88.0 g) at room temperature (RT) and stirred at 90 °C for 1 h until the formation of volatile methyl chloride ceased. The flask with the formed colorless residue was fitted with a distillation bridge and heated (1 h, 100 °C, 0.2 mbar) to give the silyl-H-phosphonate M1 as a colorless oil (105 g, 95% yield; chloride content 55 ppm).

[0125] M1 was obtained as a mixture of A1, dimer A2, and oligomer A3, which have a repeating unit of [PHO(OSiMe2O)] and a CH3OP(O)H terminus. The ratio of A1:A2:A3 was: 31 In the P NMR spectrum, the chromaticity was evaluated by integrating all signals in the ranges of -14 to -17.5 ppm (for A3), -2.5 ppm (for A2), and 10.4 ppm (for A1). Under the above conditions, the ratio of A1:A2:A3 was 1:27:72.

[0126] Viscosity: 170mPas Mn(M1)=957g / mol is 31 The oligomer A3 may theoretically be divided into different units: two P-containing end groups [2×CH3OP(O)H-, total 158.03 g / mol], n Si- and P-containing repeating units [n×(CH3)2SiO2P(O)H units, 138.14 g / mol per unit], and the structure [ka] by one additional (CH3)2SiO2 unit (90.15 g / mol).

[0127] To calculate the number average molecular weight, 31 The signal of the end groups in the P-NMR spectrum (quantitatively measured with relaxation time D1 = 60 s) was set to 2. As a result, the number of repeating units n was obtained from the signal of the repeating units. The number average molecular weight was calculated by adding the molecular weight of the end groups, n × the molecular weight of the repeating units, and the molecular weight of the additional (CH3)2SiO2 units.

[0128] The reaction yield was calculated based on the difference between the amount of starting material, the amount of alkyl chloride released, and the mass of the resulting oligomer mixture.

[0129] Experiment 2 - Mixture M2: Following the conditions described in experiment 1, Me2SiCl2 (0.9 eq, 765 mmol, 98.7 g), MeSiCl3 (0.1 eq, 85 mmol, 12.7 g) and dimethyl phosphite (1.0 eq, 850 mmol, 93.5 g) were converted to give M2 (95.0 g, 87% yield). The ratio of A1:A2:A4 was: 31 In the P NMR spectrum, the chromaticity was evaluated by integrating all signals in the ranges of -14 to -17.5 ppm (for A4), -2.5 ppm (for A2), and 10.4 ppm (for A1). Under the above conditions, the ratio of A1:A2:A4 was 2:35:63.

[0130] Viscosity: 180mPas

[0131] Test 3 - Mixture M3: Following the conditions described in experiment 1, Me2SiCl2 (0.9 eq, 72 mmol, 9.47 g), SiCl4 (0.1 eq, 8 mmol, 1.4 g), and dimethyl phosphite (1.0 eq, 80 mmol, 8.8 g) were converted to give M3. The ratio of A1:A2:A5 was: 31 In the P NMR spectrum, the peaks were evaluated by integrating all signals in the ranges of -14 to -17.5 ppm (for A5), -2.5 ppm (for A2), and 10.4 ppm (for A1). Under the above conditions, the ratio of A1:A2:A5 was = 1:20:79.

[0132] Test 4 - Mixture M4: Following the conditions described in experiment 1, Me2SiCl2 (0.9 eq, 99 mmol, 12.9 g), Me3SiCl (0.1 eq, 11 mmol, 1.21 g) and dimethyl phosphite (0.73 eq, 80 mmol, 8.80 g) were converted to M4 (8.80 g, 80% yield). The ratio of A1:A2:A6 was: 31In the P NMR spectrum, the chromatograms were evaluated by integrating all signals in the ranges of -14 to -17.5 ppm (for A6), -2.5 ppm (for A2), and 10.4 ppm (for A1). Under the above conditions, the ratio of A1:A2:A6 was 1:34:65.

[0133] Test 5 - Mixture M5: Following the conditions described in experiment 1, Me2SiCl2 (1.0eq, 850mmol, 109.7g) and dimethyl phosphite (1.0eq, 850mmol, 93.5g) were reacted for a long time (4h) using a vertical powerful condenser with a cooling medium of -10°C, and after distillation of volatile substances, M5 was obtained (116.0g, 98% yield). The ratio of A1:A2:A3 was: 31 In the P NMR spectrum, the chromatograms were evaluated by integrating all signals in the ranges of -14 to -17.5 ppm (for A3), -2.5 ppm (for A2), and 10.4 ppm (for A1). Under the above conditions, the ratio of A1:A2:A3 was 1:11:88.

[0134] Mn = 2021 g / mol, as in experiment 1. 31 Determined by P NMR.

[0135] Viscosity: 750mPas

[0136] Test 6 - Mixture M6: Following the conditions described in experiment 5, Me2SiCl2 (1.0 eq, 83 mmol, 107.5 g) and dimethyl phosphite (0.90 eq, 75 mmol, 82.5 g) were converted to M6 (103.0 g, 99% yield). The ratio of A1:A2:A3 was: 31 In the P NMR spectrum, the chromaticity was evaluated by integrating all signals in the ranges of -14 to -17.5 ppm (for A3), -2.5 ppm (for A2), and 10.4 ppm (for A1). Under the above conditions, the ratio of A1:A2:A3 was 0:3:97.

[0137] Test 7 - Mixture M7: Following the conditions described in experiment 1, Me2SiCl2 (1.0 eq, 70 mmol, 9.12 g) and dimethyl methylphosphonate (1.0 eq, 70 mmol, 8.95 g) were converted to M7 (9.80 g, 92% yield). The ratio of A7:A8:A9 was: 31 In the P NMR spectrum, the ratios of A7:A8:A9=1:30:69 were obtained by integrating all signals in the ranges of 8-12 ppm (for A9), 21-23 ppm (for A8), and 33 ppm (for A7).

[0138] Test 8 - Mixture M8: Following the conditions described in experiment 1, Me2SiCl2 (1.0 eq, 50 mmol, 6.45 g) and diethyl phosphite (1.0 eq, 50 mmol, 7.12 g) were converted to M8 (3.80 g, 53% yield). The ratio of A10:A11:A12 was: 31 The P NMR spectra were evaluated by integrating all signals in the ranges of -14 to -17.5 ppm (for A12), -4.2 ppm (for A11), and 7.2 ppm (for A10). Under the above conditions, the ratio of A10:A11:A12 was 1:81:18.

[0139] Test 10 - Mixture M10: Following the conditions described in experiment 1, Me2SiCl2 (1.0 eq, 70 mmol, 9.17 g) and dimethylphenylphosphonate (1.0 eq, 70 mmol, 13.30 g) were converted to M10 neu (13.6 g, 88% yield). The ratio of A13 neu:A14 neu:A15 neu was: 31 In the P NMR spectra, the neutrons were evaluated by integrating all signals in the range of -0.2 to -2.5 ppm (for A15 new), 10.4 ppm (for A14 new), and 21.5 ppm (for A13 new). Under the above conditions, the ratio of A13 neu:A14 neu:A15 neu was 1:55:44.

[0140] Viscosity: 1519mPas Mn = 753 g / mol, as explained in Experiment 1 31 by P NMR; except for the end groups [2 × CHOP(O)H-, total 310.24 g / mol], n Si- and P-containing repeating units [n × (CH)SiOP(O)H units, 214.25 g / mol per unit], and one additional (CH)SiO unit (90.15 g / mol) according to the structure.

[0141] Test 11-Mixture M11: Following the conditions described in experiment 1, Et2SiCl2 (1.0 eq, 70 mmol, 7.86 g) and dimethyl phosphite (1.0 eq, 70 mmol, 11.34 g) were converted to give M11 (15.3 g, 98% yield). The ratio of A17:A16:A12 was: 31 The P NMR spectra were evaluated by integrating all signals in the ranges of -14 to -17.5 ppm (for A17), -4.2 ppm (for A16), and 10.4 ppm (for A1). Under the above conditions, the ratio of A1:A16:A17 was 2:90:8.

[0142] Test 12 - Mixture M12: Following the conditions described in Run 1, ClMe2SiOSiMe2Cl (1.0 eq, 80 mmol, 6.45 g) and dimethyl phosphite (1.0 eq, 80 mmol, 9.00 g) were converted to M12 (15.40 g, 87% yield). The ratio of A1:A18:A19 was: 31 The P NMR spectra were evaluated by integrating all signals in the ranges of -15 to -17.5 ppm (for A12), -2.7 ppm (for A11), and 10.4 ppm (for A1). Under the above conditions, the ratio of A1:A18:A19 was 1:9:80.

[0143] Experiments 9 to 12 - Mixtures M9 to M12: Mixtures M9 to M12 were prepared and evaluated as described in Experiment 1, using the educts, educt ratios and reaction conditions listed in Table 1. The compositions of the resulting mixtures are also shown in Table 1.

[0144] [Table 1]

[0145] II. Electrolyte composition The electrolyte compositions were prepared by dissolving 1.0M LiPF6 in various mixtures of ethyl carbonate (EC, BASF), diethyl carbonate (DEC, BASF), monofluoroethylene carbonate (FEC, BASF), 1H,1H,5H-perfluoropentyl-1,1,1,2,2-tetrafluoroethyl ether (CF2H(CF2)3CH2OCF2CF2H, FPEE, Foosung co. Ltd.). Comparative additives R1 and R2 and additive mixtures M1, M2 and M7 of the present invention were added to these compositions as shown in Table 2. R2, M1, M2 and M7 were used without further purification. "Volume %" indicates the volume of the solvent in the electrolyte composition, and "mass %" indicates the total mass of the electrolyte composition. All solvents were dry (water content < 3 ppm).

[0146] All electrolyte compositions were prepared and stored in an Ar-filled glove box with oxygen and water levels below 1.0 ppm. The electrolyte compositions used are summarized in Table 2.

[0147] [Table 2]

[0148] III. Electrochemical Cells III.1) HE-NCM / Graphite 2032 Full Coin Cell The positive electrode for electrochemical cycling experiments was prepared by coating a slurry containing 92.5 wt% of the cathode active material suspended in N-ethyl-2-pyrrolidinone (NEP), 2 wt% graphite, 2 wt% Super C65 carbon black, and 3.5 wt% polyvinylidene fluoride (PVdF) binder onto aluminum foil. The cathode active material was HE-NCM 0.42Li2MnO 3· 0.56Li(Ni 0.4 Mn 0.4 Co 0.2 )O2, HE-NCM, BASF) was used. A commercially available graphite coated tape from Elexcel Corporation Ltd. was used as the negative electrode. 2032 coin cells were fabricated using the positive and negative composite electrodes, polypropylene separators (Celgard), and the respective electrolytes. All cells were assembled in an argon-filled glove box with oxygen and water levels below 1.0 ppm, and their electrochemical testing was performed in a Maccor 4000 battery test fixture.

[0149] III.2) NCM622 / Graphite and NCM811 / Graphite Pouch Batteries The positive electrode for electrochemical cycling experiments in pouch cells was prepared by coating a slurry containing the cathode active material suspended in N-methyl-2-pyrrolidinone (NMP), carbon black, and polyvinylidene fluoride (PVdF) binder onto an aluminum foil (thickness = 17 μm) using a roll coater. The electrode tape was dried in a hot air chamber and further dried at 130 °C under vacuum for 8 h, after which the electrode was pressed using a roll press machine. The cathode active material used was Li(Ni 0.8 Co 0.1 Mn 0.1 )O2(NCM811) or Li(Ni 0.6 Co 0.2 Mn 0.2)O2 (NCM622). For the negative electrode, graphite and carbon black were mixed with CMC (carboxymethyl cellulose) and SBR (styrene butadiene rubber) to prepare an aqueous slurry solution. The resulting slurry was applied onto a copper foil (thickness = 9 μm) using a roll coater and dried in a hot air chamber (80 °C to 120 °C). The loading of the resulting electrode was approximately 10 mg / cm. 2 It was found that the electrode was 0.01 to 0.01 μm thick. The electrodes were pressed by roll press to an approximate thickness of 72 μm. Pouch cells (250 mAH) containing a separator stacked between the cathode and anode along with the NCM positive electrode and graphite negative electrode were assembled in an Ar-filled glove box. All cells were then filled with electrolyte as described in Table 2 in an argon-filled glove box with oxygen and water levels below 1.0 ppm, and their electrochemical testing was carried out in a Maccor 4000 battery testing system.

[0150] IV. Electrochemical Cell Evaluation IV.1) Cycling and Battery Resistance Evaluation of HE-NCM / Graphite 2032 Coin Full Cells at 25°C The battery was charged to a voltage of 4.7 V at a constant current of 0.067 C and discharged to a discharge voltage of 2.0 V at a constant current of 0.067 C at 25 °C (activation cycle 1). Immediately after, the battery was charged to a voltage of 4.6 V at a constant current of 0.1 C at 25 °C. The battery was further charged at 4.6 V until the current reached a value of 0.05 C, and then discharged to a discharge voltage of 2.0 V at a constant current of 0.1 C (cycle 2). The same procedure as in cycle 2 was repeated once (cycle 3). The battery was then charged to a voltage of 4.6 V at a constant current of 0.1 C and discharged to a discharge voltage of 2.0 V at a constant current of 0.1 C (cycle 4). The charge capacity of this cycle is used as a reference value for the next cycle (cycle 5), in which the battery is charged to 40% of the charge capacity (SOC 40%) at a constant current of 0.1 C in the next cycle (cycle 5). Once the battery reached 40% SOC, a current interrupt of 0.2C was applied for 10 seconds to measure the DC internal resistance (DCIR).

[0151] In cycles 6 to 7, the cell was charged at 25° C. with a constant current of 0.2 C to a voltage of 4.6 V. The cell was further charged at 4.6 V until the current reached a value of 0.05 C, and then discharged at a constant current of 0.5 C to a discharge voltage of 2.0 V. The cell was then charged at a constant current of 0.7 C to a voltage of 4.6 V, and charged at 4.6 V until the current reached a value of 0.05 C, and while keeping these charging conditions constant, the cell was discharged at a constant current of 1 C (twice, cycles 8 to 9), 2 C (twice, cycles 10 to 11), and 3 C (twice, cycles 12 to 13) to a discharge voltage of 2.0 V. The discharge capacity recorded in cycle 13 is expressed as a percentage of the discharge capacity obtained in cycle 3 (see Table 3, Discharge Capacity Ratio 3 C / 0.1 C (%)).

[0152] Following the change in discharge capacity, extended cycling was performed by charging at a constant current of 0.7C to a voltage of 4.6V, charging at 4.6V until the current reached a value of 0.05C, and discharging at a constant current of 1C to a discharge voltage of 2.0V (cycle 14). The discharge capacity measured at cycle 14 was recorded as the first discharge capacity at 1C. This charge-discharge procedure was repeated at least 200 times or until the measured charge capacity was 70% or less of the charge capacity at cycle 14. During the extended cycling experiments, DC internal resistance (DCIR) measurements were performed at 40% SOC every 100 cycles. The latter was achieved by repeating the cycling sequence described for cycles 2 to 5 every 100 1C cycles. The results of various examples are shown in Table 3.

[0153] [Table 3]

[0154] The discharge capacity and battery resistance of the batteries containing the oligomeric phosphonic acid silyl ester are comparable or significantly better than those of the monomeric additives, and the oligomeric additives have the advantage of being less volatile, which makes it easier to prepare and handle the electrolyte composition and to keep the additive concentration constant during the filling of the electrolyte composition into the battery. Typically, a vacuum is applied to the battery before filling the battery with the liquid electrolyte to ensure good filling of the battery with the liquid electrolyte composition and good wetting of all parts.

[0155] IV.2 Cycling evaluation of pouch cells containing NCM622 and 811 cathodes and graphite anodes IV.2.1) Formation Pouchful batteries containing NCM622 or NCM811 cathodes and graphite anodes were charged at a constant current of 0.1 C to a voltage of 3.7 V or for up to 2 hours. The batteries were then stored at 45° C. for 17 hours, followed by degassing and initial volume measurement via Archimedes measurement in water at ambient temperature.

[0156] IV.2.2) High temperature storage of pouchful batteries containing NCM622 / / graphite and NCM811 / / graphite at 60°C After completion of the formation procedure, the cells were charged to 4.2 V at ambient temperature and stored at 60° C. for 14 days. The amount of gas (mL) generated during storage was determined by Archimedes measurement in water at ambient temperature, and the results are summarized in Table 6. The final charge (CCCV charge, 0.2 C, 4.2 V, 0.015 C cutoff) and discharge (CC discharge, 0.2 C, 3.0 V cutoff) capacities were measured after the storage test. The capacity retention after cycling is expressed as the ratio of the final discharge capacity to the initial discharge capacity. The cell resistance after cycling was determined by charging to 50% SOC and measuring the DC internal resistance (DCIR) by applying a current interrupt. The results from various examples are shown in Tables 4 and 5. The electrochemical cell of the present invention shows a clearly lower gas generation amount compared to the comparative cell.

[0157] [Table 4]

[0158]

Table 5

Claims

1. (i) at least one aprotic organic solvent; (ii) at least one conductive salt; (iii) at least one phosphonic acid silyl ester comprising the structure of formula (I); 【Chemistry 1】 During the ceremony, T is 【Chemistry 2】 and 【Chemistry 3】 is selected from p is an integer from 0 to 6, (CH 2 ) p One or more CH 2 The group may be substituted with O, (CH 2 ) p One or more H is C 1 ~C 4 may be substituted with alkyl; R 1 are H, F, Cl, and R, respectively. 4 , OR 4 , OSi(R 5 ) 3 , OSi(OR 4 ) 3 , and OP(O)(OR 4 ) R 5 are independently selected from R 4 each of which is optionally substituted with one or more substituents selected from CN and F; 1 ~C 10 Alkyl, C 3 ~C 7 (Hetero)cycloalkyl, C 2 ~C 10 Alkenyl, C 2 ~C 10 Alkynyl, C 5 ~C 7 (Hetero)aryl, and C 6 ~C 13 (hetero)aralkyl, wherein one or more CH of alkyl, alkenyl, and alkynyl that are not directly bonded to a Si atom or an O atom are independently selected from 2 The group may be substituted with O; R 3 and R 5 each represents H, F, and C, which may be substituted with one or more substituents selected from CN and F; 1 ~C 10 Alkyl, C 3 ~C 7 (Hetero)cycloalkyl, C 2 ~C 10 Alkenyl, C 2 ~C 10 Alkynyl, C 5 ~C 7 (Hetero)aryl and C 6 ~C 13 (hetero)aralkyl, one or more CH of alkyl, alkenyl, and alkynyl that are not directly bonded to a P atom; 2 The group may be substituted with O; and (vi) optionally one or more additives; An electrolyte composition comprising:

2. The phosphonic acid silyl ester comprises the structure of formula (II): 【Chemistry 4】 During the ceremony, Q 1 is a chemical bond or a monomeric or oligomeric group comprising one or more monomeric units of formula (II.1), Q 2 is a chemical bond or a monomeric or oligomeric group comprising one or more monomeric units of formula (II.2), 【Chemistry 5】 During the ceremony, T * Each independently represents Si or Si-(CH 2 ) p -Si, p is an integer from 0 to 6, (CH 2 ) p One or more CH 2 The group may be substituted with O, (CH 2 ) p One or more H is C 1 ~C 4 may be substituted with alkyl, and T * When is Si, q 1 is an integer from 0 to 2, q 2 is an integer from 0 to 2, q 1 +q 2 = 2, T * Si-(CH 2 ) p - In the case of Si, q 1 is an integer from 0 to 4, q 2 is an integer from 0 to 4, q 1 +q 2 = 4; - * The electrolyte composition of claim 1 , wherein:

3. The phosphonic acid silyl ester is represented by formula (III): 【Chemistry 6】 During the ceremony, R 6 and R 7 is R 8 , Si(OR 8 ) 3 and Si(R 9 ) 3 are each independently selected from R 8 each of which is optionally substituted with one or more substituents selected from CN and F; 1 ~C 10 Alkyl, C 3 ~C 7 (Hetero)cycloalkyl, C 2 ~C 10 Alkenyl, C 2 ~C 10 Alkynyl, C 5 ~C 7 (Hetero)aryl, and C 6 ~C 13 (hetero)aralkyl, wherein one or more CH of alkyl, alkenyl, and alkynyl are independently selected from (hetero)aralkyl and are not directly bonded to an O atom or a Si atom; 2 The group may be substituted with O; and R 9 each represents H, F, Cl, and C optionally substituted with one or more substituents selected from CN and F; 1 ~C 10 Alkyl, C 3 ~C 7 (Hetero)cycloalkyl, C 2 ~C 10 Alkenyl, C 2 ~C 10 Alkynyl, C 5 ~C 7 (Hetero)aryl, and C 6 ~C 13 (hetero)aralkyl, wherein one or more CH of alkyl, alkenyl, and alkynyl are not directly bonded to an O atom 2 The electrolyte composition of claim 2 , wherein the group is optionally substituted with O.

4. The phosphonic acid silyl ester is represented by the formula (IV): 【Chemistry 7】 During the ceremony, r 1 and r 2 The electrolyte composition according to claim 2 or 3, wherein each of the formulas is independently an integer from 0 to 300.

5. R 6 and R 7 is C 1 ~C 10 Alkyl, Si(OC 1 ~C 10 Alkyl) 3 and Si(R 9 ) 3 are independently selected from R 9 are H, F, Cl, and C, respectively. 1 ~C 10 5. The electrolyte composition of claim 3 or 4, wherein the alkyl is independently selected from alkyl.

6. R 1 are H, F, Cl, and C, respectively. 1 ~C 10 Alkyl and O.C. 1 ~C 10 independently selected from alkyl, which may be substituted by one or more substituents selected from CN and F, and one or more CH of the alkyl that is not directly bonded to a Si atom or an O atom; 2 The electrolyte composition according to any one of claims 1 to 5, wherein the group is optionally substituted by O.

7. R 3 are H and C, each of which may be substituted with one or more of F and / or CN; 1 ~C 10 one or more CH of alkyl independently selected from alkyl that is not directly bonded to a P atom; 2 The electrolyte composition according to any one of claims 1 to 6, wherein the group is optionally substituted with O.

8. The structure of formula (I) is 【Chemistry 8】 The electrolyte composition according to any one of claims 1 to 7, wherein the electrolyte composition is selected from the group consisting of:

9. 9. The electrolyte composition according to any one of claims 1 to 8, wherein the aprotic organic solvent (i) is selected from fluorinated and non-fluorinated cyclic and acyclic organic carbonates, fluorinated and non-fluorinated ethers and polyethers, fluorinated and non-fluorinated cyclic ethers, fluorinated and non-fluorinated cyclic and acyclic acetals and ketals, fluorinated and non-fluorinated orthocarboxylic acid esters, fluorinated and non-fluorinated cyclic and acyclic esters and diesters of carboxylic acids, fluorinated and non-fluorinated cyclic and acyclic sulfones, fluorinated and non-fluorinated cyclic and acyclic nitriles and dinitriles, fluorinated and non-fluorinated cyclic and acyclic phosphates, and mixtures thereof.

10. 10. The electrolyte composition according to any one of claims 1 to 9, wherein the at least one aprotic organic solvent (i) is selected from fluorinated and non-fluorinated ethers and polyethers, fluorinated and non-fluorinated cyclic and acyclic organic carbonates, and mixtures thereof.

11. 11. The electrolyte composition according to any one of claims 1 to 10, wherein said at least one conductive salt (ii) is chosen from lithium salts.

12. The electrolyte composition according to any one of claims 1 to 11, wherein the electrolyte composition comprises 0.01% to 10% by weight of the phosphonic acid silyl ester, based on the total weight of the electrolyte composition.

13. A phosphonic acid silyl ester having a structure represented by formula (1): 【Chemistry 9】 During the ceremony, T is 【Chemistry 10】 and 【Chemistry 11】 is selected from p is an integer from 0 to 6, (CH 2 ) p One or more CH 2 The group may be substituted with O, (CH 2 ) p One or more H is C 1 ~C 4 may be substituted with alkyl; R 1 are H, F, Cl, and R, respectively. 4 , OR 4 , OSi(R 5 ) 3 , OSi(OR 4 ) 3 , and OP(O)(OR 4 ) R 5 are independently selected from R 4 each of which is optionally substituted with one or more substituents selected from CN and F; 1 ~C 10 Alkyl, C 3 ~C 7 (Hetero)cycloalkyl, C 2 ~C 10 Alkenyl, C 2 ~C 10 Alkynyl, C 5 ~C 7 (Hetero)aryl, and C 6 ~C 13 (hetero)aralkyl, one or more CH of alkyl, alkenyl, and alkynyl that are not directly bonded to a Si atom or an O atom; 2 The group may be substituted with O; R 3 and R 5 each represents H, F, and C, which may be substituted with one or more substituents selected from CN and F; 1 ~C 10 Alkyl, C 3 ~C 7 (Hetero)cycloalkyl, C 2 ~C 10 Alkenyl, C 2 ~C 10 Alkynyl, C 5 ~C 7 (Hetero)aryl and C 6 ~C 13 (hetero)aralkyl, one or more CH of alkyl, alkenyl, and alkynyl that are not directly bonded to a P atom; 2 The group may be substituted with O. in an electrolyte composition for an electrochemical cell.

14. An electrochemical cell comprising the electrolyte composition of any one of claims 1 to 12.

15. 15. The electrochemical cell of claim 14, wherein the electrochemical cell is a lithium battery, a double layer capacitor, and a lithium ion capacitor.

Citation Information

Patent Citations

  • Non-aqueous electrolyte of lithium ion battery and lithium ion battery

    CN105789698A

  • Method for correcting pattern of photomask and method for manufacturing photomask, method for manufacturing semiconductor device, pattern correction device and program

    JP2010117404A

  • Lithium-sulfur battery

    JP2013508927A

  • Novel manganese-containing nanostructures

    JP2014534277A

  • Nonaqueous electrolyte and power storage device using the same

    JP2015159120A