Power storage device and separator for the power storage device

A polyolefin microporous membrane with controlled liquid absorption and tensile modulus, combined with an ion conductive layer, addresses electrolyte depletion and dendrite formation in lithium-ion batteries, improving cycle characteristics and safety.

JP2024138451AActive Publication Date: 2024-10-08ASAHI KASEI BATTERY SEPARATOR CORP
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2024111693
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-08
Estimated Expiration
2041-05-25

AI Technical Summary

Technical Problem

Lithium-ion secondary batteries face issues with lithium dendrite formation leading to electrolyte depletion, which causes short circuits, heat generation, and electrolyte consumption due to reductive decomposition, especially under low temperature and high current charging conditions.

Method used

A polyolefin microporous membrane with specific liquid absorption height, tensile modulus, and pore characteristics is developed to suppress electrolyte depletion by maintaining electrolyte flow and preventing separator collapse, featuring a design that includes an ion conductive layer between the separator and the negative electrode.

Benefits of technology

The membrane effectively prevents electrolyte depletion and dendrite formation, enhancing the cycle characteristics and safety of lithium-ion batteries by maintaining electrolyte levels and improving Li ion diffusivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138451000001
    Figure 2024138451000001
  • Figure 2024138451000002
    Figure 2024138451000002
  • Figure 2024138451000003
    Figure 2024138451000003
Patent Text Reader

Abstract

To provide a polyolefin microporous film capable of suppressing deterioration due to liquid shortage of a lithium ion battery, a lithium ion battery separator including them, and a lithium ion battery.SOLUTION: The present invention provides a polyolefin microporous film that in a liquid-absorptive test of a propylene carbonate, a liquid height of a longitudinal direction (MD) and a width direction (TD) is 1.0 mm or more and 50 mm or less, a leading extension elastic modulus of the MD and the TD is 3000 kgf / cm2 or large.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyolefin microporous membrane, a lithium ion battery separator, and a lithium ion battery. [Background technology]

[0002] Polyolefin microporous membranes (hereinafter sometimes simply referred to as "PO microporous membranes") are widely used for separating various substances, or as selective permeation separation membranes, separators, etc. Applications thereof include, for example, microfiltration membranes; separators for batteries such as lithium ion batteries, polymer electrolyte batteries, and fuel cells; separators for capacitors; and base materials for functional membranes in which functional materials are filled into the pores to produce new functions. Among these, PO microporous membranes are preferably used as separators for lithium ion batteries, which are widely used in mobile phones, smartphones, wearable devices, notebook personal computers (PCs), tablet PCs, digital cameras, etc.

[0003] Conventionally, in lithium ion batteries, an electrolytic solution is impregnated into a power generating element having a separator between a positive electrode plate and a negative electrode plate. The separator separates the positive electrode and the negative electrode, and can function as a membrane through which the electrolytic solution or ions can permeate. It has been proposed to improve battery characteristics such as cycle characteristics, energy density, energy capacity, and charge / discharge characteristics, and to suppress deterioration of battery characteristics by improving the separator or the negative electrode, which includes a microporous PO membrane (Patent Documents 1 to 3).

[0004] For example, Patent Document 1 describes the provision of a nonaqueous electrolyte secondary battery that has excellent wettability between the separator and the nonaqueous electrolyte and is excellent in battery capacity and charge / discharge characteristics by using a hydrophilic or hydrophilically treated separator. Patent Document 2 examines the white index (whiteness) and diethyl carbonate permeability of a separator including a microporous PO membrane from the viewpoint of suppressing deterioration of the battery characteristics of the secondary battery.

[0005] For example, Patent Document 3 proposes facilitating battery fabrication and improving the cycle life and energy density of a battery by surface treatment of a negative electrode with a negative electrode active layer including a first layer containing Li metal and a second layer made of a temporary protective metal capable of forming an alloy with Li metal or diffusible into Li metal. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 6-283153 [Patent Document 2] International Publication No. 2018 / 078707 [Patent Document 3] Special Publication No. 2003-515893 Summary of the Invention [Problem to be solved by the invention]

[0007] In lithium-ion secondary batteries, under conditions such as charging at a relatively low temperature and a relatively large current, lithium (Li) may precipitate on the negative plate, and metallic Li may grow from this negative plate as dendrites. In addition, the dissolution and precipitation reactions of Li ions are repeated in the battery, and a new electrode surface is formed each time, which may cause the reductive decomposition of the electrolyte to become more intense. As the reductive decomposition of the electrolyte and the formation of dendrites progresses due to the charge-discharge cycle of the battery, the electrolyte in the battery is consumed and depleted, which tends to cause not only short circuits or heat generation, but also the electrolyte to dry up. This tendency is prominent in battery systems with charge-discharge mechanisms that are prone to Li precipitation, or battery systems equipped with negative electrodes that can be made high-capacity.

[0008] However, the separators described in Patent Documents 1 and 2 and the negative electrode described in Patent Document 3 do not focus on the battery electrolyte depletion caused by the formation of Li dendrites, and there is room for further improvement in suppressing battery deterioration caused by electrolyte depletion.

[0009] Therefore, an object of the present invention is to provide a polyolefin microporous membrane capable of suppressing deterioration due to electrolyte depletion in a lithium ion battery, and a lithium ion battery separator and a lithium ion battery containing the same. [Means for solving the problem]

[0010] The present inventors have elucidated the mechanism of electrolyte starvation in lithium ion batteries caused by the formation of lithium (Li) dendrites, and have found that the above-mentioned problems can be solved by specifying the electrolyte absorption height and tensile modulus in an electrolyte absorption test of a polyolefin microporous membrane or a lithium ion battery separator, thereby completing the present invention. Examples of embodiments of the present invention are listed below. <1> In a liquid absorption test of propylene carbonate, the liquid absorption height in the machine direction (MD) and the transverse direction (TD) is 1.0 mm or more and 50 mm or less, MD and TD tensile modulus: 3000kgf / cm 2 That's all. Polyolefin microporous membrane. <2> The number of holes calculated by the gas-liquid method is 70 / μm 2 More than 500 pieces / μm 2 Item 2. The microporous polyolefin membrane according to item 1, having a porous layer which is: <3> 3. The polyolefin microporous membrane according to item 2, wherein the single-point total pore volume of the porous layer having pores with diameters of 98 nm or less as measured by a nitrogen gas adsorption test is 20% or more and 85% or less of the total pore volume. <4> 4. The polyolefin microporous membrane according to any one of items 1 to 3, wherein the polyolefin microporous membrane has a compression rate of 35% or less and a post-compression porosity of 35% or more in a compression test under conditions of a temperature of 25°C, a pressure of 10 MPa, and a compression time of 3 minutes. <5> The main component of the polyolefin microporous membrane is polyethylene, and 5. The microporous polyolefin membrane according to any one of items 1 to 4, wherein the polyethylene has a crystal long period of 30.0 nm or more as measured by small angle X-ray scattering (SAXS). <6> The main component of the polyolefin microporous membrane is polyethylene, and 6. The microporous polyolefin membrane according to any one of items 1 to 5, wherein the polyethylene has a crystallite size of 35.0 nm or less as measured by wide-angle X-ray scattering (WAXS). <7> In the propylene carbonate liquid absorption test, the liquid absorption height in MD and TD is 1.0 mm or more and 50 mm or less, and the tensile modulus of elasticity in MD and TD is 3000 kgf / cm 2 A lithium ion battery comprising the above-mentioned polyolefin microporous membrane as a separator. <8> 8. The lithium ion battery of claim 7, wherein an ion-conducting layer is present between the separator and a metal negative electrode. <9> Item 9. The lithium ion battery according to item 7 or 8, wherein the ion conductive layer is made of an inorganic material. <10> 1-4 below: 1. The Li ion concentration is 1.3 mol / L or more; 2. Contains an electrolyte salt having a bisfluorosulfonylimide structure; 3. Contains carbonates in which hydrogen atoms are replaced by halogen atoms; and 4. The electrolyte is an ionic liquid; The lithium ion battery according to any one of items 7 to 9, comprising an electrolyte solution characterized by at least one of the following: <11> 11. The lithium ion battery according to any one of items 7 to 10, comprising the polyolefin microporous membrane according to any one of items 1 to 6 as the separator. Effect of the Invention

[0011] According to the present invention, it is possible to provide a polyolefin microporous membrane capable of suppressing deterioration due to electrolyte depletion in a lithium ion battery, and a lithium ion battery separator and a lithium ion battery including the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Below, we will explain in detail the form for implementing the present invention (hereinafter sometimes abbreviated as "embodiment"); however, the present invention is not limited to this, and various modifications are possible without departing from the gist of the present invention.

[0013] In this specification, the flow direction of the membrane during membrane production is defined as MD, and the direction intersecting with MD at 90 degrees (°) in the membrane plane is defined as TD. In this specification, the upper and lower limit values ​​of each numerical range can be arbitrarily combined. In addition, containing a specific component as a main component means that the content of the specific component is 50 mass% or more.

[0014] <Polyolefin microporous membrane> In one embodiment of the present invention, a microporous polyolefin membrane (a microporous PO membrane) is provided. The microporous PO membrane contains a polyolefin resin as a main component and exhibits excellent electrical insulation and ion permeability, and can therefore be used in, for example, lithium ion batteries, specifically as a separator or separator substrate for lithium ion secondary batteries.

[0015] The microporous polyolefin membrane according to the first embodiment of the present invention has the following characteristics: In the propylene carbonate liquid absorption test, the liquid absorption height in MD and TD is 1.0 mm or more and 50 mm or less; and MD and TD tensile modulus: 3000kgf / cm 2 That's all.

[0016] The polyolefin microporous membrane characterized as above tends to suppress the deterioration of the lithium ion battery caused by the drying up of the electrolyte when used as a separator for the lithium ion battery. This tendency is remarkable in the lithium ion battery having a charge / discharge mechanism that easily deposits Li or a negative electrode that can increase the capacity, and furthermore, it also facilitates the improvement of the battery characteristics of the lithium ion battery including a negative electrode made of Li metal.

[0017] According to the present invention, the following two patterns have been found as mechanisms by which the formation of Li dendrites causes the electrolyte depletion in lithium-ion batteries: (a) Li dendrites cause irregularities on the negative electrode surface, especially on the surface of the Li metal negative electrode, which increases the specific surface area of ​​the negative electrode and increases the consumption of electrolyte due to reductive decomposition. (a) The Li dendrites formed on the surface of the negative electrode cause the separator located between the positive and negative electrodes to compress and deform, causing the separator to expel the electrolyte (i.e., the electrolyte impregnated in the separator expels the electrolyte).

[0018] In the first embodiment, based on the above mechanisms (a) and (b), the affinity with the electrolyte and the compression resistance of a microporous PO membrane that can be used as a separator are improved in order to suppress electrolyte depletion in a lithium ion battery.

[0019] From the viewpoint of improving affinity with the electrolyte, the PO microporous membrane has an MD and TD absorption height of 1.0 mm or more and 50 mm or less in a propylene carbonate electrolyte absorption test. When a PO microporous membrane with an absorption height controlled within a numerical range of 1.0 mm or more and 50 mm or less is used as a separator in a lithium ion battery, the electrolyte flows smoothly even if the electrolyte is consumed due to reductive decomposition or reduced due to compressive deformation, and an appropriate amount of electrolyte is retained in the pores of the separator, resulting in excellent cycle characteristics.

[0020] The liquid absorption test of propylene carbonate can be performed by the method described in the Examples. From the viewpoint of further improving the affinity between the PO microporous membrane and the electrolyte, the liquid absorption height is preferably in the range of 1.0 mm to 50 mm, more preferably in the range of 2.0 mm to 45 mm, further preferably in the range of 3.0 mm to 40 mm, and particularly preferably in the range of 4.0 mm to 30 mm, in each of MD and TD.

[0021] The volume of a lithium ion battery may change, causing the electrolyte held in the pores of the separator to flow. If the contact angle with propylene carbonate is within the above range, the electrolyte flows smoothly in response to the volume change, and an appropriate amount of electrolyte is held in the pores of the separator, resulting in excellent cycle characteristics.

[0022] The liquid absorption height of the PO microporous membrane in a propylene carbonate liquid absorption test can be adjusted to within the above-mentioned numerical range by, for example, including inorganic filler or inorganic particles in the PO microporous membrane, mixing polyolefin (PO) with a polymer having a polar group in the production process of the PO microporous membrane, or surface treatment of the PO microporous membrane.

[0023] The tensile modulus of the PO microporous membrane in the MD and TD is 3000 kgf / cm in order to improve compression resistance. 2 The microporous PO membrane having the MD and TD tensile moduli controlled within the above-mentioned ranges, when disposed as a separator between the positive and negative electrodes of a lithium ion battery, is resistant to crushing and compressive deformation even when Li dendrites are precipitated on the electrode surface, and can suppress the discharge of electrolyte.

[0024] The tensile modulus of the PO microporous membrane can be measured by the method described in the Examples. From the viewpoint of further improving the compression resistance of the PO microporous membrane, the tensile modulus of the PO microporous membrane in the MD and TD is 3,000 kgf / cm 2 More than 15,000kgf / cm 2 It is preferable that the resistance is within the range of 3,200 kgf / cm 2 More than 12,000kgf / cm 2 More preferably, it is within the range of 3,500 kgf / cm 2 More than 10,000kgf / cm 2 More preferably, it is within the range of 3,800 kgf / cm 2 More than 9,000kgf / cm 2 Even more preferably, it is within the following range:

[0025] The tensile modulus of the microporous PO membrane can be adjusted to within the above-mentioned range by controlling, for example, the selection of the raw material composition, the proportion of the plasticizer, the biaxial stretching temperature, the biaxial stretching ratio, the heat setting temperature, the stretching ratio during heat setting, and the relaxation rate during heat setting.

[0026] From the viewpoint of further improving compression resistance, the PO microporous membrane preferably has a compression ratio of 35% or less, more preferably 3% or more and 34% or less, even more preferably 5% or more and 33% or less, even more preferably 7% or more and 32% or less, particularly preferably 10% or more and 31% or less, and most preferably 11% or more and 30% or less, in a compression test under conditions of a temperature of 25°C, a pressure of 10 MPa, and a compression time of 3 minutes. From the same viewpoint, the PO microporous membrane preferably has a post-compression porosity of 35% or more, more preferably 36% or more, even more preferably 37% or more, even more preferably 38% or more, still more preferably 39% or more, and particularly preferably 40% or more, in a compression test under conditions of a temperature of 25°C, a pressure of 10 MPa, and a compression time of 3 minutes.

[0027] If desired, an ion-conducting layer, an inorganic coating layer, or an organic (adhesive) layer can be formed on the surface of the microporous PO membrane.

[0028] If desired, multiple microporous PO membranes can be laminated together, or one microporous PO membrane can be laminated with another microporous membrane.

[0029] The preferred properties and components of the microporous PO membrane are described below.

[0030] (Porosity measured by nitrogen gas adsorption test) The microporous PO membrane preferably has a single-point total pore volume having a pore diameter of 98 nm or less, as measured by a nitrogen gas adsorption test, of 20% to 85% of the total pore volume. When the microporous PO membrane has a porous layer, it is also preferable that the single-point total pore volume of the porous layer having a pore diameter of 98 nm or less, as measured by a nitrogen gas adsorption test, is 20% to 85% of the total pore volume.

[0031] The nitrogen gas adsorption test can be carried out by the method described in the Examples below. The total pore volume is defined as the adsorption amount at a nitrogen relative pressure (p / p0) of 0.98, and the single-point total pore volume (pore diameter 98 nm or less) is derived. The ratio of the pore volume (pore diameter 98 nm or less) to the total pore volume can be calculated by comparing this value with the total pore volume of the microporous membrane. The higher this ratio, the smaller the pores the microporous membrane is formed from. From the viewpoint of making the microporous membrane more dense and efficiently delaying the growth of lithium dendrites and foreign matter-derived dendrites associated with the elution of metal foreign matter, the single-point total pore volume (pore diameter 98 nm or less) is preferably 20% or more of the total pore volume, more preferably 25% or more, and even more preferably 30% or more. In the nitrogen gas adsorption test of the microporous membrane or porous layer by the single-point method, the lower limit of the pore diameter can exceed 0 nm in this technical field.

[0032] On the other hand, if the single-point total pore volume (pore diameter 98 nm or less) of the microporous membrane or porous layer exceeds 85% of the total pore volume, the separator will become clogged and the resistance increase will be concentrated in certain areas, which will result in the promotion of dendrite formation and a decrease in the capacity maintenance cycle. From these viewpoints, the single-point total pore volume (pore diameter 98 nm or less) is preferably 85% or less of the total pore volume, and more preferably 80% or less.

[0033] The ratio of the one-point total pore volume (pore diameter 98 nm or less) to the total pore volume can be controlled, for example, by densifying the microporous membrane. More specifically, in the production process of the PO microporous membrane described below, for example, by including a high molecular weight PE having a molecular weight described below in an amount described below; performing a stretching step before the extraction step; stretching under conditions of an areal stretching ratio of 50 times or more and / or a stretching temperature of 128°C or less; adjusting each of the longitudinal and transverse stretching ratios in the stretching step to 5 times or more; adjusting the heat setting temperature in the heat setting (HS) step to 115°C or more and 140°C or less; adjusting the HS stretching ratio to 1.5 times or more and 2.2 times or less; and adjusting the HS relaxation ratio to 0.7 times or more and less than 0.95 times, either alone or in suitable combination, to be controlled to be within the range of the pore volume ratio described above.

[0034] Furthermore, the pore volume ratio can also be controlled by the viscosity average molecular weight of the PE used. From the viewpoint that the pores become smaller in diameter in the stretching process and the pores are less likely to be blocked in the heat setting process by using a polymeric PE, the viscosity average molecular weight (Mv) of the PO microporous membrane is preferably 450,000 or more, more preferably 500,000 or more, and the content of PE with Mw of 450,000 or more in the resin composition of the membrane is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more. This content can be 100% by mass. In addition, in order to prevent the pore ratio from exceeding 85%, the Mv of the membrane is preferably 6,000,000 or less, preferably 5,000,000 or less, and even more preferably 3,000,000 or less.

[0035] The pore ratio can also be controlled within a specified range by the molecular structure of the PO used. Although the reason is unclear, the pore ratio tends to fall within a specified range as the polydispersity (weight average molecular weight Mw / number average molecular weight Mn and z average molecular weight Mz / weight average molecular weight Mw) of the raw polymer increases.

[0036] (Number of holes calculated by gas-liquid method) The number of pores B of the PO microporous membrane calculated by the gas-liquid method is 70 / μm 2 It is preferable that the number of particles is 500 or more per μm. 2 When the microporous PO membrane has a porous layer, the number of pores in the porous layer calculated by a gas-liquid method is preferably 70 / μm or less. 2 More than 500 pieces / μm 2 It is also preferable that:

[0037] The number of pores (B) per cross section calculated by the gas-liquid method is set to 70 pores / μm from the viewpoint of efficiently suppressing local dendrite generation by diffusing lithium ions and metal ions accompanying the elution of foreign matter in the microporous membrane or porous layer, and from the viewpoint of suppressing an increase in the number of local resistance increasing points and improving cycle characteristics. 2 More than 80 particles / μm is preferable. 2 More preferably, it is 90 particles / μm or more. 2 More preferably, it is 100 particles / μm or more. 2 More preferably, the number is 110 / μm or more. 2 The number of pores (B) is particularly preferably 500 / μm2 or more, from the viewpoint that the microporous membrane or porous layer has high strength and can suppress the growth of dendrites. 2 It is preferable that the number of particles is less than 350 / μm. 2 The number of pores per cross section (B) calculated by the gas-liquid method is adjusted to be within the above range by adjusting the plasticizer ratio in all raw materials (i.e., the resin ratio in all raw materials), the heat setting temperature, etc. in the production process of the microporous PO membrane described later.

[0038] (Porosity) The microporous PO membrane preferably has a porosity ε of 42% or more. Hereinafter, the porosity (ε) may be referred to as "(pre-compression) porosity".

[0039] The porosity (ε) of the microporous PO membrane is preferably 42% or more, more preferably 44% or more, even more preferably 47% or more, and particularly preferably 50% or more, from the viewpoints of reducing membrane resistance and improving ion diffusivity to thereby efficiently suppress the generation of dendrites, achieving a certain membrane strength and low air permeability, and having high ion conductivity and high output characteristics. Furthermore, from the viewpoints of improving membrane strength to thereby suppress the growth of dendrites and improving voltage resistance, the porosity (ε) is preferably 80% or less, more preferably 70% or less, even more preferably 65% ​​or less, and particularly preferably 60% or less.

[0040] (Mean flow diameter measured by half-dry method) The PO microporous membrane preferably has a mean flow diameter d of 0.020 μm or more and 0.070 μm or less as measured by the half-dry method. In this specification, the pore diameter of the PO microporous membrane means the mean flow diameter as measured by the half-dry method using a perm porometer (Porous Materials, Inc.: CFP-1500AE).

[0041] By measuring the mean flow diameter (d) by the half-dry method, the pore diameter of the narrowed portion in the pore structure of the microporous membrane can be known. The mean flow diameter d measured by the half-dry method is preferably 0.070 μm or less, more preferably 0.065 μm or less, even more preferably 0.060 μm or less, even more preferably 0.055 μm or less, and particularly preferably 0.050 μm or less, from the viewpoint of physically suppressing the growth of dendrites by densifying the microporous membrane and from the viewpoint of increasing the number of pores (B) per cross section and improving ion diffusivity. In addition, from the viewpoint of preventing the occurrence of a concentrated portion of increased resistance due to clogging, which results in the promotion of dendrite generation, and from the viewpoint of improving cycle characteristics, the mean flow diameter is preferably 0.020 μm or more, and more preferably 0.025 μm or more.

[0042] Examples of means for controlling the pore size or porosity (ε) of the PO microporous membrane within the above-mentioned numerical ranges include, in a production method for a PO microporous membrane described below, containing a high-molecular-weight PE having a molecular weight described below in an amount described below; performing a stretching step before the extraction step; adjusting the longitudinal and transverse stretching ratios in the stretching step to 5 times or more and performing stretching at a temperature of 128°C or less; adjusting the heat setting temperature in the heat setting (HS) step to 115°C or more and 140°C or less, adjusting the HS stretching ratio to 1.5 times or more and 2.2 times or less, and adjusting the HS relaxation ratio to 0.7 times or more and less than 0.9 times, which can be used alone or in suitable combination.

[0043] (Film thickness) From the viewpoints of lithium ion battery capacity, high ion permeability and good rate characteristics, retarding dendrite growth, and reducing the volume occupied by the separator to improve battery capacity when used in a high-capacity battery, the membrane thickness of the microporous PO membrane is preferably 20 μm or less, more preferably 18 μm or less, even more preferably 16 μm or less, even more preferably 1 μm to 14 μm, particularly preferably 3 μm to 13 μm, and most preferably 5 μm to 12 μm. The membrane thickness of the microporous PO membrane is sometimes referred to as the "average membrane thickness (before compression)" below.

[0044] The average film thickness (before compression) of the PO microporous membrane can be adjusted to within the above-mentioned range by controlling the distance between the cast rolls, the cast clearance, the stretch ratio in the biaxial stretching step, the HS ratio, the HS temperature, etc. in the production process of the PO microporous membrane.

[0045] (Air permeability) From the viewpoint of the output characteristics and cycle characteristics of lithium-ion batteries, the air permeability of the PO microporous membrane is set to 100 cm of air. 3 The lower limit of the air permeability is preferably 200 seconds or less, more preferably 190 seconds or less, per 100 cm of air, from the viewpoint of the membrane strength. 3 Preferably, the time is 20 seconds or more.

[0046] (Puncture strength converted to basis weight, Puncture strength, Basis weight) The puncture strength of the PO microporous membrane converted into basis weight is 50gf / (g / m 2 ) or more. 2 ) or more represents a membrane structure with high membrane strength per resin basis weight and resistant to crushing under compressive stress, and for example, during a nail penetration test or pressure test, a microporous PO membrane used as a separator substrate is less likely to break even if it has high porosity and low air permeability, which tends to improve the safety of lithium-ion batteries. The pin strength converted into basis weight is measured by the method described in the Examples, and is obtained by measuring the pin strength not converted into basis weight (hereinafter simply referred to as pin strength) at three points along the TD of the membrane, two points 10% inside the full width from both ends toward the center and one point in the center, and dividing the average value by the basis weight.

[0047] The advantage of controlling the pin puncture strength is remarkable when an electrode that easily expands and contracts in a lithium-ion battery cell is used, and is even more remarkable when a high-capacity electrode used in an in-vehicle battery or a silicon (Si)-containing negative electrode is used. From this perspective, the pin puncture strength of the PO microporous membrane converted into basis weight is 40 gf / (g / m 2 )~150gf / (g / m 2 ), and more preferably 50 gf / (g / m 2 )~140gf / (g / m 2 ), and more preferably 55 gf / (g / m 2 )~130gf / (g / m 2 ), and more preferably 70 gf / (g / m 2 )~120gf / (g / m 2 ) is particularly preferred.

[0048] From the same viewpoint as above, from the viewpoint of achieving a certain membrane strength and low air permeability, and from the viewpoint of improving short circuit resistance, the basis weight of the PO microporous membrane is 1.0 g / m 2 ~15g / m 2 It is preferable that the range is within the range of 100 μm.

[0049] From the same viewpoints as above, from the viewpoint of safety when the lithium-ion battery is subjected to an impact, and from the viewpoint of suppressing interelectrode short circuit or voltage resistance failure caused by separator rupture due to foreign matter unintentionally mixed inside the lithium-ion battery, the puncture strength of the PO microporous membrane is preferably 200 gf or more, more preferably 220 gf or more, even more preferably 250 gf or more, even more preferably 280 gf or more, and particularly preferably 300 gf or more. The upper limit of the puncture strength is not particularly limited and can be determined depending on the crystallinity of the membrane, the heat shrinkability of the membrane, and the suppressed electrical resistance, and may be, for example, 900 gf or less, 850 gf or less, 700 gf or less, or 680 gf or less.

[0050] The pin puncture strength and basis weight converted pin puncture strength of the PO microporous membrane can be adjusted within the above-mentioned numerical ranges by controlling, for example, the molecular weight and blending ratio of polymer raw materials such as polyolefin, the stretching ratio in the biaxial stretching step, the MD / TD stretching temperature in the biaxial stretching step, the heat setting (HS) ratio, etc. in the production process of the PO microporous membrane.

[0051] (Components) Examples of the PO microporous membrane include a porous membrane containing a polyolefin resin; a porous membrane containing, in addition to a polyolefin resin, a resin such as polyketone, maleic anhydride-modified polyolefin, polycarbonate, polyethylene oxide, polyethylene terephthalate, polycycloolefin, polyethersulfone, polyamide, polyimide, polyimideamide, polyaramid, nylon, polytetrafluoroethylene, etc.; a woven fabric of polyolefin-based fibers; a nonwoven fabric of polyolefin-based fibers, etc. Among these, from the viewpoints of the reduction or suppression of the increase in the electrical resistance of the membrane, the compression resistance and structural uniformity of the membrane, etc., a microporous membrane containing a polyolefin resin is preferred, and a microporous membrane containing polyethylene as a main component is more preferred.

[0052] (Ingredients included) The microporous PO membrane is formed from a resin composition containing a polyolefin resin. If desired, the resin composition may further contain inorganic fillers or inorganic particles, resins other than polyolefin, etc.

[0053] From the viewpoint of improving the shutdown performance of a lithium-ion battery, the microporous PO membrane is preferably a porous membrane formed from a polyolefin resin composition in which polyolefin resin accounts for 50% by mass to 100% by mass of the resin components constituting the porous membrane. The proportion of polyolefin resin in the polyolefin resin composition is more preferably 60% by mass to 100% by mass, even more preferably 70% by mass to 100% by mass, and most preferably 95% by mass to 100% by mass.

[0054] The polyolefin resin used is not particularly limited, and examples thereof include polymers (e.g., homopolymers, copolymers, multi-stage polymers, etc.) obtained by polymerizing monomers such as ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene. These polymers can be used alone or in combination of two or more.

[0055] In addition, from the viewpoint of rigidifying the membrane and improving its compression resistance, the polyolefin resin contained in the PO microporous membrane preferably has a melting point in the range of 120°C or more and 150°C or less, more preferably 125°C or more and 140°C or less, and / or a DSC 1st peak temperature in the range of 136°C to 144°C.

[0056] Among these, from the viewpoints of reducing or suppressing an increase in the electrical resistance of the membrane, the compression resistance and structural uniformity of the membrane, etc., preferred polyolefin resins are polyethylene, polypropylene, ethylene-propylene copolymers, copolymers of ethylene-propylene and other monomers, and mixtures of these.

[0057] From the viewpoints of the crystallinity, high strength, compression resistance, etc. of the PO microporous membrane, and of expressing fusing properties, a microporous membrane formed from a polyethylene composition in which polyethylene accounts for 50 to 100 mass% of the resin component constituting the microporous membrane is preferred. The proportion of polyethylene (PE) in the resin component constituting the microporous membrane is more preferably 60 to 100 mass%, more preferably 70 to 100 mass%, even more preferably 80 to 100 mass%, and most preferably 90 to 100 mass%.

[0058] The WAXS measurement of the polyolefin microporous membrane is described in detail in the Examples, and the crystallite size obtained by the WAXS measurement is considered to be related to the structure of polyethylene, which improves the structural uniformity and compression resistance of the membrane and the reaction uniformity in a non-aqueous secondary battery. When the main component of the PO microporous membrane is polyethylene (PE), the polyethylene contained as the main component in the PO microporous membrane preferably has a crystallite size of MDND plane (110) of 35.0 nm or less. The crystallite size of MDND plane (110) of polyethylene can be measured by X-ray diffraction (XRD) or wide-angle X-ray scattering (WAXS), as described in detail in the Examples.

[0059] When the MDND plane (110) crystallite size of the polyethylene is 35.0 nm or less, the polyolefin microporous membrane containing the polyethylene tends to become rigid and the compression resistance of the membrane is improved, so that even if the volume of the electrode changes during use of the nonaqueous secondary battery, high output and high cycle characteristics can be achieved at the same time. From this viewpoint, the MDND plane (110) crystallite size of the polyethylene, which is the main component of the membrane, is more preferably 33.0 nm or less, and further preferably 10.0 nm to 32.0 nm, or 15.0 nm to 31.0 nm, or 15.0 nm to 30.0 nm, or 15.0 nm to 25.0 nm. In particular, when the MDND plane (110) crystallite size of the polyethylene is 25.0 nm or less, the rigidity of the membrane is increased and the compression resistance is improved.

[0060] The M, D, N, D plane (110) crystallite size of polyethylene, which is the main component of the polyolefin microporous membrane, can be adjusted to within the above-mentioned numerical range by, for example, controlling the molecular weight of the polyolefin raw material, the molecular weight of the polyethylene raw material, the stretch ratio in the biaxial stretching process, the stretch ratio and temperature in the biaxial stretching process, the stretch ratio and temperature in the biaxial stretching process, etc. in the production process of the polyolefin microporous membrane.

[0061] Although not wishing to be bound by theory, it is believed that the crystal long period of the polyolefin microporous membrane correlates with the porosity after compression of the membrane. From the viewpoints explained above, the crystal long period of the polyolefin microporous membrane is preferably within the range of 30.0nm or more, or 30.0nm to 60.0nm, or 31.0nm to 55.0nm, or 32.0nm to 50.0nm, or 33.0nm to 50.0nm, or 35.0nm to 50.0nm, or 37.0nm to 50.0nm.

[0062] The crystal long period of the polyolefin microporous membrane can be measured, for example, by small angle X-ray scattering (SAXS), and can be adjusted to within the above-described numerical ranges by controlling, for example, the molecular weight of the polyolefin raw material, the molecular weight of the polyethylene raw material, the stretching ratio in the biaxial stretching process, the stretching ratio and temperature in the biaxial stretching process, and the stretching ratio and temperature in the biaxial stretching process in the production process of the polyolefin microporous membrane.

[0063] From the viewpoints of high strength, compression resistance, suppression of electrical resistance, etc., when a microporous PO membrane is formed as a separator substrate, the PE ratio in the polyolefin resin is preferably 30% by mass or more, more preferably 50% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, and is preferably 100% by mass or less, more preferably 95% by mass or less, and even more preferably 95% by mass or less. Note that a PE ratio of 50% or more is also preferred from the viewpoint of exhibiting a highly responsive fuse behavior.

[0064] The viscosity average molecular weight (Mv) of the polyolefin resin used as the raw material of the microporous PO membrane is preferably 30,000 to 6,000,000, more preferably 80,000 to 3,000,000, and even more preferably 150,000 to 2,000,000. When Mv is 30,000 or more, it is preferred because the strength tends to be high due to the entanglement of the polymers. On the other hand, when Mv is 6,000,000 or less, it is preferred from the viewpoint of improving the moldability in the extrusion and stretching steps.

[0065] In one embodiment, when the PO microporous membrane contains polyethylene (PE), from the viewpoints of membrane orientation and rigidity, the Mv of at least one type of PE is preferably 600,000 or more, more preferably 700,000 or more, and the upper limit of the Mv of PE may be, for example, 2,000,000 or less. From the viewpoints of a decrease in fluidity when the membrane is melted and short-circuit resistance in a nail penetration test, the proportion of PE with an Mv of 600,000 or more in the polyolefin resin constituting the PO microporous membrane is preferably 30% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, particularly preferably 70% by mass or more, and may be 100% by mass.

[0066] In another embodiment, the PO microporous membrane (PO microporous layer) preferably contains 45% by mass or more, more preferably 50% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more of a PE raw material having an Mv of 500,000 to 6,000,000 based on the mass of the PO microporous membrane. When the PO microporous layer contains 45% by mass or more of a PE raw material having an Mv of 500,000 to 6,000,000, the crystals are highly oriented during stretching, and the PO microporous layer tends to have a small pore size or to be dense. From the same viewpoint, the PO raw material used in the production of the PO microporous layer or the PO microporous membrane is preferably an ethylene homopolymer, more preferably an ethylene homopolymer having an Mv of 500,000 to 6,000,000.

[0067] The content of the polyolefin resin in the PO microporous membrane (PO microporous layer) is 50 mass% or more, preferably 60 mass% or more, preferably 70 mass% or more, and preferably 80 mass% or more, and may be 90 mass% or more, or 100 mass% or less, based on the mass of the PO microporous membrane (PO microporous layer).

[0068] Furthermore, examples of polyolefin resins include low-density polyethylene (density 0.910 g / cm 3 More than 0.930g / cm 3 less than 0.910g / cm 3 More than 0.940g / cm 3 less than 0.930g / cm 3 More than 0.942g / cm 3 less than 0.942g / cm 3 or more), ultra-high molecular weight polyethylene (density 0.910g / cm 3 More than 0.970g / cm 3 Examples of the polypropylene include polyethylene, polypropylene, polybutene, ethylene propylene rubber, etc. These may be used alone or in combination of two or more. Among these, it is preferable to use polyethylene alone, polypropylene alone, or a mixture of polyethylene and polypropylene from the viewpoint of obtaining a uniform film.

[0069] From the viewpoint of safety of lithium-ion batteries equipped with a PO microporous membrane as a separator, the polyolefin resin should be 0.930 g / cm 3 More than 0.942g / cm 3 Preferably, the PO microporous membrane is a medium-density polyethylene (MDPE) having a density of less than 1,000,000, and may be, for example, a PE other than high-density polyethylene (HDPE). From the viewpoint of improving the safety of lithium-ion batteries even when the PO microporous membrane is a thin film, the PO microporous membrane may be a medium-density polyethylene having a viscosity-average molecular weight of less than 1,000,000, or a medium-density polyethylene having a viscosity-average molecular weight of 1,000,000 or more and 2,000,000 or less and a density of 0.930 g / cm. 3More than 0.942g / cm 3 The microporous PO membrane preferably contains 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more of at least one selected from ultrahigh molecular weight polyethylenes of less than 1000 g / mole, based on the mass of the microporous PO membrane.

[0070] The polyolefin resin preferably contains polypropylene (PP) from the viewpoint of ensuring safety in the high temperature range (160°C or higher) where it is difficult to ensure safety with PE. As the polypropylene, a propylene homopolymer is preferable from the viewpoint of heat resistance. From the viewpoint of further improving heat resistance, the polyolefin resin more preferably contains polyethylene and polypropylene as main components. Therefore, the ratio of the PP raw material in the PO raw material is preferably more than 0 mass% and 10 mass% or less from the viewpoints of film formability and film rupture resistance in the stretching process.

[0071] When PE and PP are used in combination, the polyethylene should be a medium-density polyethylene with a viscosity-average molecular weight of less than 1 million, or a polyethylene with a viscosity-average molecular weight of 1 million to 2 million and a density of 0.930 g / cm. 3 More than 0.942g / cm 3 By using at least one selected from ultra-high molecular weight polyethylenes having a molecular weight of less than 1000 mm, it is preferable to balance the strength and permeability and to maintain an appropriate fuse temperature.

[0072] The viscosity average molecular weight of the polyolefin resin (measured according to the measurement method in the examples described later) is preferably 50,000 or more, more preferably 100,000 or more, more preferably 500,000 or more, more preferably 700,000 or more, more preferably 1 million or more, and the upper limit is preferably 6 million or less, preferably 3 million or less, preferably 1.9 million or less. A viscosity average molecular weight of 50,000 or more is preferable from the viewpoint of maintaining high melt tension during melt molding to ensure good moldability, or from the viewpoint of imparting sufficient entanglement to the resin to increase the strength of the microporous membrane. On the other hand, a viscosity average molecular weight of 6 million or less is preferable from the viewpoint of realizing uniform melt kneading and improving the moldability, particularly thickness moldability, of the sheet.

[0073] The polydispersity (Mw / Mn) of the polyethylene raw material is preferably 4.0 or more and 10.0 or less. The polydispersity (Mw / Mn) is measured according to the measurement method in the Examples described later. Although the reason is unclear, setting the polydispersity of the raw polymer within the above range tends to make the PO microporous membrane have an appropriately high pore ratio and a uniform pore structure. From this viewpoint, the polydispersity of the polyethylene raw material is more preferably 6.0 or more, and even more preferably 7.0 or more.

[0074] Furthermore, the ratio of z-average molecular weight to weight-average molecular weight (Mz / Mw) of the polyethylene raw material is preferably 2.0 or more and 7.0 or less. Mz / Mw is measured according to the measurement method in the Examples described later. Although the reason is unclear, setting the Mz / Mw of the raw material polymer within the above range tends to make the PO microporous membrane have an appropriately high pore ratio and a uniform pore structure. From this perspective, the Mz / Mw of the polyethylene raw material is more preferably 4.0 or more, and even more preferably 5.0 or more.

[0075] The above resin composition may be mixed with various known additives, such as inorganic fillers or inorganic particles; resins other than polyolefins having polar groups; antioxidants such as phenol-based, phosphorus-based, or sulfur-based antioxidants; metal soaps such as calcium stearate and zinc stearate; ultraviolet absorbers, light stabilizers, antistatic agents, antifogging agents, and coloring pigments, as necessary.

[0076] The inorganic filler of the PO microporous membrane is not particularly limited, and examples thereof include oxide ceramics such as alumina, silica (silicon oxide), titania, zirconia, magnesia, ceria, yttria, zinc oxide, and iron oxide; nitride ceramics such as silicon nitride, titanium nitride, and boron nitride; ceramics such as silicon carbide, calcium carbonate, aluminum sulfate, barium sulfate, aluminum hydroxide, potassium titanate, talc, kaolin clay, kaolinite, halloysite, pyrophyllite, montmorillonite, sericite, mica, amesite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, and silica sand; and glass fiber. These may be used alone or in combination of two or more. Among these, from the viewpoint of electrochemical stability, at least one selected from the group consisting of silica, alumina, and barium sulfate is preferable as the inorganic particles.

[0077] When the PO microporous membrane contains an inorganic filler, the inorganic filler content is preferably 1% by mass or more and 50% by mass or less, more preferably 3% by mass or more and 30% by mass or less, even more preferably 5% by mass or more and 20% by mass or less, and particularly preferably 10% by mass or more and 18% by mass or less. By containing 1% by mass or more of an inorganic filler, the affinity with an electrolyte solution having a high polarity is increased, and the liquid absorption of propylene carbonate can be improved. By containing 50% by mass or less of an inorganic filler, the pore size of the PO microporous membrane can be prevented from becoming excessively large, and overcharging during charging can be suppressed.

[0078] Resins having polar groups other than polyolefins are not particularly limited, and include olefin copolymers such as ethylene-vinyl acetate copolymer and ethylene-acrylic acid-maleic anhydride copolymer; polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyvinyl acetates; polyvinyl alcohols; polyvinyl acetals; polyvinyl butyrals; synthetic fluorinated polybenzoxazole; acrylic resins; methacrylic resins such as polymethyl methacrylate; polyacrylonitriles; acrylonitrile-butadiene-styrene copolymer and other acrylonitrile copolymers; styrene copolymers such as styrene-methacrylic acid copolymer and styrene-acrylonitrile copolymer; polystyrenes. Examples of suitable materials include ionic polymers such as sodium sulfonate and sodium polyacrylate; acetal resins; polyamides such as nylon 66; gelatin; gum arabic; polycarbonates, polyester carbonates; cellulose resins; polyketones; polyethers; phenolic resins; urea resins; epoxy resins; unsaturated polyester resins; alkyd resins; melamine resins; polyurethanes; diaryl phthalate resins; polyphenylene oxides; polyphenylene sulfide polysulfones; polyphenylsulfones; polyimides; bismaleimide triazine resins; fluorine-containing resins; polyimide amides; polyether sulfones; polyether ketones; polyether imides, etc. From the viewpoint of affinity with the electrolyte, fluorine-containing resins, polycarbonates, polyketones, polyethers, and polyacrylonitriles are preferred.

[0079] When the microporous PO membrane contains a polymer having a polar group, the content is preferably 1% by mass or more and 50% by mass or less, more preferably 3% by mass or more and 35% by mass or less, even more preferably 5% by mass or more and 30% by mass or less, and particularly preferably 10% by mass or more and 23% by mass or less. By containing 1% by mass or more of a polymer having a polar group, the affinity with an electrolyte solution having a high polarity is increased, and the liquid absorption of propylene carbonate can be improved. By containing 50% by mass or less of a polymer having a polar group, the microporous PO membrane can be given an appropriate strength.

[0080] (Method of manufacturing microporous PO membrane) The method for producing the microporous PO membrane is not particularly limited, but may be, for example, A mixing step (a) of mixing a resin composition containing a polyolefin resin, a pore-forming material, and various additives as desired; an extrusion step (b) of melt-kneading and extruding the mixture obtained in the step (a); a sheet forming step (c) of forming the extrudate obtained in step (b) into a sheet; A primary stretching step (d) of stretching the sheet-like molded product obtained in the step (c) at least once in at least one axial direction; an extraction step (e) of extracting the pore-forming material from the first stretched membrane obtained in step (d); and a heat setting step (f) of heat setting (HS) the extracted film obtained in the step (e) at a predetermined temperature.

[0081] The above-mentioned method for producing a microporous PO membrane can provide a microporous PO membrane that, when used as a separator for a lithium ion battery, is capable of suppressing lithium dendrites, suppressing chemical micro-short-circuiting caused by metallic foreign matter, and achieving high output characteristics and cycle characteristics at the same time. In particular, the method of stretching in MD and TD in the primary stretching step (d) and then heat-setting in TD in the heat-setting step (f) tends to make it easier to adjust the pore ratio and pore size of the resulting microporous PO membrane to within the numerical ranges explained above. The method for producing a microporous PO membrane of this embodiment is not limited to the above-mentioned method, and various modifications are possible without departing from the gist of the method.

[0082] [Mixing step (a)] The mixing step (a) is a step of mixing a resin composition containing a polyolefin resin, a pore-forming material, and various additives as desired. In the mixing step (a), other components may be mixed with the resin composition as necessary.

[0083] The pore-forming material may be any material as long as it is distinguished from the material of the PO resin, and may be, for example, a plasticizer. The plasticizer may be a non-volatile solvent capable of forming a homogeneous solution at or above the melting point of the PO resin, such as hydrocarbons, e.g., liquid paraffin (LP), paraffin wax, etc.; esters, e.g., dioctyl phthalate, dibutyl phthalate, etc.; higher alcohols, e.g., oleyl alcohol, stearyl alcohol, etc.

[0084] The content of the plasticizer in the resin composition is preferably 60% by mass to 90% by mass, more preferably 71% by mass to 85% by mass, even more preferably 73% by mass to 85% by mass, and particularly preferably 75% by mass to 85% by mass. By adjusting the content of the plasticizer to 60% by mass or more, the number of pores in the film increases, ion diffusivity increases, and the generation of dendrites can be efficiently suppressed. In addition, the melt viscosity of the resin composition decreases, and melt fracture is suppressed, which tends to improve the film formability during extrusion. On the other hand, by adjusting the content of the plasticizer to 90% by mass or less, the elongation of the original film during the film formation process can be suppressed.

[0085] In step (a), the resin composition containing PO may contain any additives, which are not particularly limited, but may include, for example, resins or polymers other than polyolefin resins, inorganic fillers or inorganic particles, antioxidants such as phenolic compounds, phosphorus compounds, and sulfur compounds, metal soaps such as calcium stearate and zinc stearate, ultraviolet absorbers, light stabilizers, antistatic agents, antifogging agents, and color pigments.

[0086] From the viewpoint of adjusting the MD and TD absorption heights of the obtained microporous PO membrane in a propylene carbonate absorption test within the above-mentioned numerical ranges, it is preferable to mix an inorganic filler such as silica or barium sulfate, and / or a polar polymer such as polyketone, maleic anhydride-modified polyolefin, polycarbonate, or polyethylene oxide with the resin composition.

[0087] The total amount of these additives added is preferably more than 0 and not more than 50 parts by mass, more preferably not more than 40 parts by mass, and even more preferably not more than 35 parts by mass, per 100 parts by mass of the polyolefin resin.

[0088] The method of mixing in step (a) is not particularly limited, but examples thereof include a method in which a part or all of the raw materials are premixed as necessary using a Henschel mixer, a ribbon blender, a tumbler blender, etc. Among these, a method in which mixing is performed using a Henschel mixer is preferred.

[0089] [Extrusion step (b)] The extrusion step (b) is a step of melt-kneading and extruding the resin composition obtained in the step (a). In the extrusion step (b), components other than the polyolefin resin may be mixed with the resin composition as necessary.

[0090] The method of melt kneading in step (b) is not particularly limited, but examples thereof include a method of melt kneading all raw materials including the mixture mixed in step (a) with a screw extruder such as a single screw extruder or a twin screw extruder; a kneader; a mixer, etc. Among them, it is preferable to perform melt kneading using a screw of a twin screw extruder. In addition, when performing melt kneading, it is preferable to add the plasticizer in two or more separate steps, and further, when adding the additive in multiple separate steps, it is preferable to adjust the amount of the first addition to 80% by weight or less of the total amount added, from the viewpoint of suppressing aggregation of the contained components and dispersing them uniformly. As a result, the obtained microporous film is preferable from the viewpoint of suppressing heat generation by shutting down over a large area and improving the safety of the cell as a separator.

[0091] When a pore-forming material is used in step (b), the temperature of the melt-kneading section is preferably less than 200° C. from the viewpoint of uniformly kneading the resin composition. The lower limit of the temperature of the melt-kneading section is equal to or higher than the melting point of the polyolefin from the viewpoint of uniformly dissolving the polyolefin resin in the pore-forming material such as a plasticizer.

[0092] In the kneading, although not particularly limited, it is preferable to mix the antioxidant with the raw material PO at a predetermined concentration, replace the atmosphere around the mixture with a nitrogen atmosphere, and perform melt kneading while maintaining the nitrogen atmosphere. The temperature during melt kneading is preferably 160°C or higher, more preferably 180°C or higher, and is preferably lower than 300°C.

[0093] In step (b), the kneaded product obtained through the above kneading is extruded by an extruder such as a T-die or a circular die. At this time, it may be single-layer extrusion or co-extrusion. The conditions for extrusion are not particularly limited, and for example, known methods can be used. In addition, from the viewpoint of the thickness of the obtained microporous PO membrane, it is preferable to control the (die) lip clearance, etc.

[0094] [Sheet forming process (c)] The sheet forming step (c) is a step of forming the extrudate obtained in the extrusion step (b) into a sheet. The sheet-shaped molded product obtained in the sheet forming step (c) may be a single layer or a laminate. The method of forming the sheet is not particularly limited, but for example, the method of compressing and cooling the extrudate to solidify it can be mentioned.

[0095] The compression cooling method is not particularly limited, but examples thereof include a method in which the extrudate is directly brought into contact with a cooling medium such as cold air or cooling water, a method in which the extrudate is brought into contact with a metal roll, a press, etc., cooled with a refrigerant, etc. Among these, the method in which the extrudate is brought into contact with a metal roll, a press, etc., cooled with a refrigerant is preferred in that the film thickness can be easily controlled.

[0096] After the melt-kneading in step (b), the set temperature in the step of forming the molten material into a sheet is preferably set to a temperature higher than that of the extruder. The upper limit of the set temperature in the sheet forming step is preferably 300°C or lower, more preferably 260°C or lower, from the viewpoint of thermal degradation of the polyolefin resin. For example, when continuously producing a sheet-shaped molded product from an extruder, the set temperature in the step of forming the sheet after the melt-kneading step, i.e., the set temperature of the path from the extruder outlet to the T-die and the T-die is set to a temperature higher than that of the extrusion step, which is preferable because it is possible to form the molten material into a sheet without separating the resin composition and the pore-forming material. In addition, it is preferable to control the cast clearance, etc., from the viewpoint of the thickness of the resulting microporous PO film.

[0097] [Primary stretching process (d)] The primary stretching step (d) is a step of stretching the sheet-like molded product obtained in the sheet molding step (c) at least once in at least one uniaxial direction. This stretching step (a stretching step performed before the next extraction step (e)) is called "primary stretching", and the film obtained by the primary stretching is called "primary stretched film". In the primary stretching, the sheet-like molded product can be stretched in at least one direction, and may be stretched in both MD and TD, or may be stretched in only one of MD or TD.

[0098] The stretching method for the first stretching is not particularly limited, and examples thereof include uniaxial stretching with a roll stretching machine, TD uniaxial stretching with a tenter, sequential biaxial stretching with a roll stretching machine and a tenter or a combination of a plurality of tenters, simultaneous biaxial stretching with a simultaneous biaxial tenter or by inflation molding, etc. Among these, from the viewpoint of the stability of the physical properties of the obtained microporous PO membrane, simultaneous biaxial stretching is preferred.

[0099] The stretching ratio in MD and / or TD of the first stretching is preferably 5 times or more, more preferably 6 times or more. When the stretching ratio in MD and / or TD of the first stretching is 5 times or more, the resulting microporous PO membrane tends to form dense fibrils to have small pores and to have improved strength. Furthermore, the stretching ratio in MD and / or TD of the first stretching is preferably 9 times or less, more preferably 8 times or less or 7 times or less. When the stretching ratio in MD and / or TD of the first stretching is 9 times or less, breakage during stretching tends to be suppressed. When biaxial stretching is performed, either sequential stretching or simultaneous biaxial stretching may be used, and the stretching ratio in each axial direction is preferably 5 times or more and 9 times or less, more preferably 6 times or more and 8 times or less, or 6 times or more and 7 times or less.

[0100] The primary stretching temperature can be selected with reference to the composition and concentration of the raw material resins contained in the PO resin composition. The stretching temperature in MD and / or TD is preferably 110° C. or higher, more preferably 115° C. or higher, from the viewpoints of reducing the pore size and suppressing breakage. The stretching temperature in MD and / or TD is preferably 128° C. or lower, more preferably 126° C. or lower, even more preferably 124° C. or lower, and particularly preferably 122° C. or lower, from the viewpoints of increasing the membrane strength or reducing the pore size.

[0101] [Extraction step (e)] The extraction step (e) is a step of extracting the pore-forming material from the first stretched membrane obtained in the first stretching step (d) to obtain an extracted membrane. For example, a method of removing the pore-forming material may be used, such as immersing the first stretched membrane in an extraction solvent to extract the pore-forming material and drying the membrane thoroughly. The method of extracting the pore-forming material may be either a batch method or a continuous method. In addition, the amount of the pore-forming material, particularly the plasticizer, remaining in the porous membrane is preferably less than 1% by mass.

[0102] The extraction solvent used when extracting the pore-forming material is preferably a poor solvent for the polyolefin resin, a good solvent for the pore-forming material or the plasticizer, and has a boiling point lower than the melting point of the polyolefin resin. Such an extraction solvent is not particularly limited, but examples thereof include hydrocarbons such as n-hexane and cyclohexane; halogenated hydrocarbons such as methylene chloride and 1,1,1-trichloroethane; non-chlorine halogenated solvents such as hydrofluoroethers and hydrofluorocarbons; alcohols such as ethanol and isopropanol; ethers such as diethyl ether and tetrahydrofuran; and ketones such as acetone and methyl ethyl ketone. These extraction solvents may be recovered and reused by operations such as distillation.

[0103] [Heat setting process (f)] The heat setting step (f) is a step of heat setting the extracted film obtained in the extraction step (e) at a predetermined temperature. The heat treatment method at this time is not particularly limited, but may be a heat setting method using a tenter or roll stretching machine to perform stretching and relaxation operations.

[0104] The stretching operation in the heat setting step (f) is an operation of stretching the microporous PO membrane in at least one of MD and TD, and may be performed in both MD and TD, or only in MD or TD.

[0105] The stretching ratios in MD and TD in the heat setting step (f) are preferably 1.5 to 2.2 times, more preferably 1.7 to 2.1 times. The stretching ratios in MD and TD in the step (f) are preferably 1.5 times or more from the viewpoint of developing the strength of the film, and are preferably 2.2 times or less from the viewpoint of preventing breakage.

[0106] The stretching temperature in this stretching operation is preferably 115° C. or higher, and more preferably 120° C. or higher, from the viewpoint of suppressing breakage during stretching. Moreover, the stretching temperature in the heat setting step (f) is preferably 140° C. or lower, and more preferably 138° C. or lower, more preferably 134° C. or lower, more preferably 131° C. or lower, more preferably 128° C. or lower, or more preferably 125° C. or lower, from the viewpoint of increasing the number of pores and increasing the porosity. Moreover, when the stretching temperature is within the above numerical range, the pore size of the obtained microporous PO membrane tends to be easily controlled.

[0107] The relaxation operation in the heat setting step (f) is an operation of shrinking the microporous PO membrane in at least one of MD and TD, and may be performed in both MD and TD, or only in MD or TD. The relaxation ratio in the heat setting step (f) is preferably 0.95 times or less, more preferably 0.90 times or less, and even more preferably 0.85 times or less. When the relaxation ratio in the step (f) is 0.95 times or less, the heat shrinkage of the membrane tends to be suppressed. In addition, from the viewpoint of increasing the relaxation temperature or increasing the number of holes and the porosity, the relaxation ratio is preferably 0.5 times or more, more preferably 0.7 times or more. Here, the "relaxation ratio" refers to the value obtained by dividing the membrane dimension after the relaxation operation by the membrane dimension before the relaxation operation, and when both MD and TD are relaxed, it refers to the value obtained by multiplying the relaxation ratio in MD and the relaxation ratio in TD. Relaxation ratio = (membrane dimension after relaxation (m)) / (membrane dimension before relaxation (m))

[0108] The relaxation temperature in this relaxation operation is preferably 115° C. or higher from the viewpoint of preventing breakage, and more preferably 120° C. or higher. From the viewpoints of increasing the number of pores and the porosity, it is preferably 140° C. or lower, and more preferably 138° C. or lower, more preferably 134° C. or lower, more preferably 131° C. or lower, more preferably 128° C. or lower, or more preferably 125° C. or lower. When the relaxation temperature is within the above-mentioned range, the pore size of the obtained microporous PO membrane tends to be easily controlled to be small and uniform.

[0109] The order of the above steps (a) to (f) can be changed as desired as long as the effects of the present invention are not impaired. After the above steps (a) to (f), the total stretch ratio of the microporous PO membrane is preferably in the range of 50 to 100, more preferably 70 to 100. Here, the "total stretch ratio" refers to the value obtained by multiplying the MD and / or TD stretch ratio in the primary stretching step (d) by the stretch ratio and / or relaxation ratio in the heat setting step.

[0110] [Other steps] The method for producing a microporous PO membrane may include steps other than the above steps (a) to (f) including, but not limited to, the above-mentioned heat setting step and, for example, a lamination step of laminating a plurality of single-layer microporous PO membranes to obtain a laminated microporous PO membrane.

[0111] From the viewpoint of controlling the liquid absorption height in the above-described propylene carbonate liquid absorption test, the method for producing a PO microporous membrane may include a surface treatment step of subjecting the surface of the PO microporous membrane to electron beam irradiation, plasma irradiation, F2O2 gas treatment, corona discharge treatment, UV treatment, UV ozone treatment, sulfurous acid gas treatment, oxidation treatment with a potassium dichromate solution or a potassium permanganate solution, etching treatment with a sodium treatment solution, application of a surfactant, chemical modification, or the like. Among these, F2O2 gas treatment or plasma irradiation is preferred from the viewpoint of excellent treatment of the inside of the PO microporous membrane in the thickness direction. Furthermore, a material for an inorganic porous layer or an organic (adhesive) layer may be applied to one or both sides of the PO microporous membrane to obtain a PO microporous membrane having at least one layer.

[0112] [Formation of inorganic coating layer] From the viewpoints of safety, dimensional stability, heat resistance, etc., an inorganic coating layer can be provided on the surface of the microporous PO membrane. The inorganic coating layer is a layer containing inorganic components such as inorganic particles, and may optionally contain a binder resin that bonds the inorganic particles together, a dispersant that disperses the inorganic particles in a solvent, etc.

[0113] Examples of the material of the inorganic particles contained in the inorganic coating layer include oxide ceramics such as alumina, silica, titania, zirconia, magnesia, ceria, yttria, zinc oxide, and iron oxide; nitride ceramics such as silicon nitride, titanium nitride, and boron nitride; ceramics such as silicon carbide, calcium carbonate, magnesium sulfate, aluminum sulfate, barium sulfate, aluminum hydroxide, aluminum oxide hydroxide (AlOOH, alumina monohydrate, or boehmite), potassium titanate, talc, kaolinite, dickite, nacrite, halloysite, pyrophyllite, montmorillonite, sericite, mica, amesite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, and silica sand; and glass fibers. The inorganic particles may be used alone or in combination.

[0114] Examples of the binder resin include a conjugated diene polymer, an acrylic polymer, a polyvinyl alcohol resin, a fluorine-containing resin, etc. The binder resin may be in the form of a latex and may contain water or a water-based solvent.

[0115] The dispersant is a substance that adsorbs to the surface of inorganic particles in the slurry and stabilizes the inorganic particles by electrostatic repulsion or the like, and examples of such a dispersant include polycarboxylates, sulfonates, polyoxyethers, and surfactants.

[0116] The inorganic coating layer can be formed, for example, by applying a slurry of the above-described components to the surface of the microporous polypropylene membrane and drying the applied slurry.

[0117] [Formation of adhesive layer] Laminated batteries have been increasingly adopted in recent years for in-vehicle batteries in order to increase energy density. To prevent deformation or swelling due to gas generation in laminated batteries, an adhesive layer containing a thermoplastic resin can be provided on the surface of the microporous PO membrane.

[0118] The thermoplastic resin contained in the adhesive layer is not particularly limited, and examples thereof include polyolefins such as polyethylene and polypropylene; fluorine-containing resins such as polyvinylidene fluoride and polytetrafluoroethylene; fluorine-containing rubbers such as vinylidene fluoride-hexafluoropropylene copolymers, vinylidene fluoride-tetrafluoroethylene copolymers, vinylidene fluoride-hexafluoropropylene tetrafluoroethylene copolymers, and ethylene-tetrafluoroethylene copolymers; styrene-butadiene copolymers and hydrogenated products thereof, acrylonitrile-butadiene copolymers and hydrogenated products thereof, acrylonitrile-butadiene-styrene copolymers and hydrogenated products thereof, and the like. Examples of the polymerizable compound include rubbers such as acrylate copolymers and their hydrogenated products, (meth)acrylate copolymers, styrene-acrylate copolymers, acrylonitrile-acrylate copolymers, ethylene propylene rubber, polyvinyl alcohol, and polyvinyl acetate; cellulose derivatives such as ethyl cellulose, methyl cellulose, hydroxyethyl cellulose, and carboxymethyl cellulose; and resins having a melting point and / or glass transition temperature of 180° C. or higher, such as polyphenylene ether, polysulfone, polyethersulfone, polyphenylene sulfide, polyetherimide, polyamideimide, polyamide, and polyester.

[0119] Furthermore, after the heat setting step (f), lamination step or surface treatment step, the master roll on which the PO microporous membrane is wound may be aged under a predetermined temperature condition, and then the master roll may be rewound. This tends to facilitate the production of a PO microporous membrane having higher thermal stability than the PO microporous membrane before rewinding. When the master roll is aged and rewound, the temperature at which the master roll is aged is not particularly limited, but is preferably 35° C. or higher, more preferably 45° C. or higher, and even more preferably 60° C. or higher. From the viewpoint of maintaining the permeability of the PO microporous membrane, the temperature at which the master roll is aged is preferably 120° C. or lower. The time required for the aging treatment is not particularly limited, but is preferably 24 hours or more, since the above-mentioned effect is easily achieved.

[0120] <Lithium-ion battery separator> The lithium ion battery separator may be a single layer separator made of the microporous PO membrane described above, or may be a laminated separator including a substrate such as a microporous PO membrane and at least one layer disposed on the substrate. In general, the at least one layer included in the laminated separator may have, for example, insulating properties, adhesive properties, thermoplastic properties, inorganic porosity, etc., and may be formed of a single film or a pattern formed by dot coating, stripe coating, etc.

[0121] From the viewpoint of improving Li ion diffusibility in a lithium ion battery, flattening Li deposition on the electrode surface, and suppressing battery battery battery dry-up, the separator preferably includes an ion conductive layer disposed on at least a portion of at least one side of the microporous PO membrane. The ion conductive layer may be made of either an organic or inorganic material, but is more preferably made of an inorganic material. The structure and method of forming the ion conductive layer made of an inorganic material may be the same as those of the inorganic coating layer described above.

[0122] Examples of materials for the ion conductive layer made of an inorganic substance include, in addition to the configuration of the inorganic coating layer described above, glasses selected from the group consisting of lithium silicate, lithium borate, lithium aluminate, lithium phosphate, lithium nitride, lithium phosphorus-oxynitride, lithium silicosulfide, lithium germanosulfide, lithium lanthanum oxide, lithium tantalum oxide, lithium niobium oxide, lithium titanium oxide, lithium fluoride, lithium borosulfide, lithium aluminosulfide, lithium phosphosulfide, graphene oxide, and combinations thereof.

[0123] Examples of the ion-conducting layer made of an organic material include, but are not limited to, polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyvinyl acetates; polyvinyl alcohols; polyvinyl acetals; polyvinyl butyrals; synthetic fluorine polybenzoxazole; acrylic resins; methacrylic resins such as polymethyl methacrylate; polyacrylonitriles; acrylonitrile-butadiene-styrene copolymers and other acrylonitrile copolymers; styrene copolymers such as styrene-methacrylic acid copolymers and styrene-acrylonitrile copolymers; ion-conducting resins such as polysodium styrene sulfonate and sodium polyacrylate. Examples of the resins include carboxylic polymers, acetal resins, polyamides such as nylon 66, gelatin, gum arabic, polycarbonates, polyester carbonates, cellulose resins, polyketones, polyethers, phenolic resins, urea resins, epoxy resins, unsaturated polyester resins, alkyd resins, melamine resins, polyurethanes, diaryl phthalate resins, polyphenylene oxides, polyphenylene sulfide polysulfones, polyphenylsulfones, polyimides, bismaleimide triazine resins, fluorine-containing resins, polyimide amides, polyether sulfones, polyether ketones, polyether imides, etc. From the viewpoint of affinity with the electrolyte, fluorine-containing resins, polycarbonates, polyketones, polyethers, and polyacrylonitriles are preferred.

[0124] From the viewpoint of planarizing the Li deposition on the electrode surface, it is also preferable to arrange the ion conductive layer of the separator so as to abut or face the negative electrode surface (or the Li deposition surface) of the lithium ion battery, thereby eliminating the Li ion concentration distribution and controlling the Li deposition morphology (suppressing the formation of Li dendrites).

[0125] <Lithium-ion battery> In another aspect of the present invention, a lithium ion battery is provided. In general, a lithium ion battery is composed of a positive electrode, a negative electrode, a liquid, gel or solid containing an electrolyte, a separator, and an exterior body. Examples of the lithium ion battery include a non-aqueous electrolyte lithium ion secondary battery, a non-aqueous gel secondary battery, a non-aqueous solid secondary battery, a lithium ion capacitor, and an electric double layer capacitor.

[0126] The lithium ion battery may include a separator, a positive electrode plate, a negative electrode plate, and a non-aqueous electrolyte (including a non-aqueous solvent and a metal salt dissolved therein). Specifically, for example, a positive electrode plate including a transition metal oxide capable of absorbing and releasing lithium ions and a negative electrode plate capable of absorbing and releasing lithium ions are wound or stacked so as to face each other with a separator interposed therebetween, retaining the non-aqueous electrolyte, and housed in a device container or a device exterior body.

[0127] The lithium ion battery according to the second embodiment of the present invention has a liquid absorption height of 1.0 mm or more and 50 mm or less in the MD and TD in a propylene carbonate liquid absorption test, and a tensile modulus of elasticity of 3000 kgf / cm in the MD and TD. 2 The lithium ion battery according to the second embodiment is characterized in that it comprises the above-mentioned microporous PO membrane as a separator. In addition, in the lithium ion battery according to the second embodiment, it is preferable that an ion conductive layer is present between the separator and the metal negative electrode. The lithium ion battery characterized as above can have a high capacity by comprising a metal negative electrode, and deterioration due to drying up of the electrolyte can be suppressed.

[0128] In the second embodiment, based on the above-described (a) and (b) as the mechanism by which the electrolyte drying-up of a lithium-ion battery is likely to occur, the affinity of a microporous PO membrane that can be used as a separator with the electrolyte and the compression resistance are improved, and the ion-conducting layer present between the separator and the metal negative electrode increases Li ion diffusivity to make the Li deposition flat.

[0129] The affinity of the PO microporous membrane usable as a separator with the electrolyte is specified by the liquid absorption height of 1.0 mm or more and 50 mm or less in the MD and TD in the propylene carbonate liquid absorption test, and the compression resistance is specified by the tensile modulus of 3000 kgf / cm in the MD and TD. 2 The separator according to the second embodiment may be a single-layer separator made of the microporous PO membrane according to the first embodiment, or a multilayer separator including a substrate such as a microporous PO membrane and at least one layer such as the inorganic coating layer, adhesive layer, or ion-conducting layer described above.

[0130] The ion-conducting layer between the separator and the metal negative electrode is preferably made of an inorganic material from the viewpoint of further increasing Li ion diffusivity and flattening Li deposition. The configuration and forming method of the ion-conducting layer according to the second embodiment may be the same as those of the ion-conducting layer that can be formed in the microporous PO membrane according to the first embodiment, as described above.

[0131] The positive electrode will be described below. As the positive electrode active material, for example, lithium composite metal oxides such as lithium nickel oxide, lithium manganate, or lithium cobalt oxide, lithium composite metal phosphates such as lithium iron phosphate, etc. can be used. The positive electrode active material is kneaded with a conductive agent and a binder, and applied as a positive electrode paste to a positive electrode current collector such as aluminum foil, dried, rolled to a predetermined thickness, and then cut to a predetermined size to form a positive electrode plate. Here, as the conductive agent, a metal powder stable under the positive electrode potential, for example, carbon black such as acetylene black, or a graphite material can be used. In addition, as the binder, a material stable under the positive electrode potential, for example, polyvinylidene fluoride, modified acrylic rubber, or polytetrafluoroethylene, etc. can be used.

[0132] The metal negative electrode will be described below. As the negative electrode active material, lithium (Li) metal, copper (Cu) foil, or a metal material capable of absorbing lithium can be used, and Li metal is preferred from the viewpoint of compatibility with the separator. In the second embodiment, the separator is provided with an ion-conducting layer, and the metal negative electrode can also be provided with an ion-conducting layer.

[0133] It is preferable to provide an ion-conducting layer on the surface of the negative electrode facing the separator. The ion-conducting layer may be made of either an organic or inorganic material, but is more preferably made of an inorganic material. Examples of the ion-conducting layer include the same ion-conducting layer on the separator described above, but alumina, titanium oxide, lithium phosphate, lithium nitride, lithium silicate, etc. are particularly preferable.

[0134] Any known method can be used to provide an ion-conducting layer on a metal negative electrode. Examples include physical vapor deposition, chemical vapor deposition, extrusion, and electroplating. Examples of suitable physical vapor deposition or chemical vapor deposition include, but are not limited to, thermal evaporation (e.g., resistance heating, induction heating, radiation heating, electron beam heating, etc.), sputtering (e.g., diode, DC magnetron, RF, RF magnetron, pulse, dual magnetron, AC, MF, and reactive sputtering, etc.), plasma chemical vapor deposition, laser chemical vapor deposition, ion plating, cathodic arc, jet deposition, and laser ablation. In addition, a method of treating a metal negative electrode with a gas or liquid to form an ion-conducting layer by a chemical reaction, or a method of forming an ion-conducting layer by a reaction during charging and discharging of a battery may be used.

[0135] The non-aqueous electrolyte will be described below. The non-aqueous electrolyte generally contains a non-aqueous solvent and a metal salt, such as a lithium salt, a sodium salt, or a calcium salt, dissolved therein.

[0136] In the second embodiment, in order to planarize Li deposition by stabilizing the reduction product (low resistance), the following steps 1 to 4 are performed: 1. The Li ion concentration is 1.3 mol / L or more; 2. Contains an electrolyte salt having a bisfluorosulfonylimide structure; 3. Contains carbonates in which hydrogen atoms are replaced by halogen atoms; and 4. The electrolyte is an ionic liquid; The electrolyte is preferably characterized by at least one of the following:

[0137] The Li ion concentration in the nonaqueous electrolyte is preferably 1.3 mol / L or more, more preferably 1.8 to 5.0 mol / L, and even more preferably 2.8 to 3.5 mol / L. The Li ion concentration of 1.3 mol / L or more suppresses the generation of highly resistant reduction products due to an increase in solvated solvent molecules, keeps the metal deposition surface flat, and reduces the specific surface area to suppress consumption of the electrolyte. The Li ion concentration of 5.0 mol / L or less ensures sufficient ion conductivity.

[0138] Examples of electrolyte salts used in the non-aqueous electrolyte include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, LiSCN, LiC(CF3SO2)3, (CF3SO2)2NLi, (FSO2)2NLi, chloroborane lithium, lower aliphatic carboxylate lithium, tetraphenyllithium borate, lithium imide, lithium bis(trifluoromethane sulfonyl)imide (LiTFSI) represented by (CF3SO2)2NLi, lithium bis(fluorosulfonyl)imide (LiFSI) represented by (FSO2)2NLi, etc. Among them, from the viewpoint of being difficult to generate voids without electrolyte that inhibit ion permeation due to gas generation, those having a bisfluorosulfonyl imide structure such as lithium bis(trifluoromethane sulfonyl)imide with high chemical stability are preferred.

[0139] Examples of non-aqueous electrolyte solvents include carbonate solvents (e.g., propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, butylene carbonate, vinylene carbonate, ethyl methyl carbonate, methyl propyl carbonate, butyl methyl carbonate, ethyl propyl carbonate, butyl ethyl carbonate, dipropyl carbonate, etc.), halogenated carbonate solvents in which some or more of the hydrogen atoms of a carbonate solvent are substituted with halogen atoms (e.g., fluoroethylene carbonate, difluoroethylene carbonate, etc.), lactone solvents (e.g., γ-butyrolactone, etc.), ester solvents (e.g., methyl acetate, ethyl acetate, etc.), chain ether solvents (e.g., 1,2-dimethoxyethane, dimethyl ether, diethyl ether, etc.), cyclic ether solvents (e.g., tetrahydrofuran, 2-methyltetrahydrofuran, dioxolane, 4-methyldioxolane, etc.), ketone solvents (e.g., cyclopentanone, etc.), sulfolane solvents (e.g., sulfolane, 3-methylsulfolane, 2,4-dimethylsulfolane, etc.), sulfoxide solvents (e.g., dimethylsulfoxide, etc.), nitrile solvents (e.g., acetonitrile, propionitrile, benzonitrile, etc.), amide solvents (e.g., N,N-dimethylformamide, N,N-dimethylacetamide, etc.), urethane solvents (e.g., 3-methyl-1,3-oxazolidin-2-one, etc.), polyoxyalkylene glycol solvents (e.g., diethylene glycol, etc.) and other aprotic solvents. Among these, from the viewpoints of facilitating the production of a reduction product with low resistance, suppressing unevenness in ion permeation to thereby maintain a flat metal deposition surface, and reducing the specific surface area to thereby suppress consumption of the electrolyte, it is preferable for the non-aqueous electrolyte solvent to contain a halogenated carbonate solvent, and it is more preferable for it to contain fluoroethylene carbonate or difluoroethylene carbonate.

[0140] When the non-aqueous electrolyte solvent contains a halogenated carbonate solvent, the content of the halogenated carbonate solvent is preferably 5% by volume or more and 50% by volume or less with respect to the total volume of the non-aqueous electrolyte solvent.

[0141] Ionic liquids can also be used as the non-aqueous electrolyte. Ionic liquids are preferred because they have high ionic conductivity, increase the diffusibility of ions to suppress non-uniformity, keep the metal deposition surface flat, and reduce the specific surface area to suppress consumption of electrolyte. Ionic liquids are composed of cations and anions.

[0142] Ionic liquids are classified according to the cation species into imidazolium, ammonium, pyrrolidinium, piperidinium, pyridinium, morpholinium, phosphonium, sulfonium, etc. Cations constituting imidazolium ionic liquids include, for example, alkylimidazolium cations such as 1-butyl-3-methylimidazolium (BMI).

[0143] Examples of cations constituting ammonium-based ionic liquids include alkyl ammonium cations such as N,N,N-trimethyl-N-propyl ammonium, in addition to tetraamyl ammonium. Examples of cations constituting pyrrolidinium-based ionic liquids include alkyl pyrrolidinium cations such as N-methyl-N-propyl pyrrolidinium (Py13) and 1-butyl-1-methyl pyrrolidinium. Examples of cations constituting piperidinium-based ionic liquids include alkyl piperidinium cations such as N-methyl-N-propyl piperidinium (PP13) and 1-butyl-1-methyl piperidinium. Examples of cations constituting pyridinium-based ionic liquids include alkyl pyridinium cations such as 1-butyl pyridinium and 1-butyl-4-methyl pyridinium. Examples of cations constituting morpholinium-based ionic liquids include alkyl morpholinium cations such as 4-ethyl-4-methyl morpholinium. Examples of cations constituting phosphonium-based ionic liquids include alkyl phosphonium cations such as tetrabutyl phosphonium and tributyl methyl phosphonium. Examples of cations constituting sulfonium-based ionic liquids include alkylsulfonium cations such as trimethylsulfonium and tributylsulfonium. Examples of anions paired with these cations include bis(trifluoromethanesulfonyl)imide (TFSI), bis(fluorosulfonyl)imide, tetrafluoroborate (BF4), hexafluorophosphate (PF6), bis(pentafluoroethanesulfonyl)imide (BETI), trifluoromethanesulfonate (triflate), acetate, dimethylphosphate, dicyanamide, and trifluoro(trifluoromethyl)borate. These ionic liquids may be used alone or in combination.

[0144] An electrolyte salt may be included in the non-aqueous solvent or ionic liquid. As the electrolyte salt, one that can be uniformly dispersed in the solvent can be used. One having a cation of lithium and the above anion can be used as the lithium salt, and examples thereof include, but are not limited to, lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(pentafluoroethanesulfonyl)imide (LiBETI), lithium tetrafluoroborate (LiBF4), lithium hexafluorophosphate (LiPF6), and lithium triflate. These electrolyte salts may be used alone or in combination.

[0145] The ether-based solvent constitutes a solvated electrolyte salt and a solvated ionic liquid. As an ether-based solvent, a known glyme (RO(CH2CH2O)) that exhibits properties similar to those of ionic liquids is used. n -R' {wherein R and R' are saturated hydrocarbons, and n is an integer} is a general term for symmetric glycol diethers. From the viewpoint of ion conductivity, tetraglyme (tetraethylene dimethyl glycol, G4), triglyme (triethylene glycol dimethyl ether, G3), pentaglycle (pentaethylene glycol dimethyl ether, G5), and hexaglyme (hexaethylene glycol dimethyl ether, G6) can be preferably used. In addition, crown ethers ((-CH2-CH2-O) n {wherein n is an integer}) can be used. Specifically, 12-crown-4, 15-crown-5, 18-crown-6, dibenzo-18-crown-6, etc. can be preferably used, but are not limited to these. These ether solvents may be used alone or in combination. It is preferable to use tetraglyme or triglyme because they can form a complex structure with the solvated electrolyte salt.

[0146] The solvated electrolyte salt may be, but is not limited to, lithium salts such as LiFSI, LiTFSI, LiBETI, etc. As the non-aqueous solvent, a mixture of an ether solvent and a solvated electrolyte salt may be used alone or in combination.

[0147] The above-mentioned various parameters are measured according to the measurement methods in the examples described below, unless otherwise specified. EXAMPLES

[0148] Next, the present embodiment will be described in more detail with reference to examples and comparative examples, but the present embodiment is not limited to the following examples as long as it does not deviate from the gist of the present embodiment. The physical properties in the examples were measured by the following methods. Unless otherwise specified, measurements were taken at room temperature of 23°C and humidity of 40%.

[0149] (1) Single-point total pore volume and pore ratio (1a) Single-point total pore volume (also known as single-point volumetric adsorption) (pore diameter 98 nm) (cm 3 / g) Nitrogen gas adsorption tests were performed using the constant volume method based on JIS Z8831-2:2010 Pore distribution and pore characteristics of powders (solids), "Part 2: Measurement method for mesopores and macropores by gas adsorption". Specifically, the gas adsorption amount converted to standard state temperature and pressure (STP) with a nitrogen relative pressure (p / p0) of 0.98 was defined as the volumetric equivalent of the liquid volume of the adsorbate, and the single-point volumetric adsorption amount (pore diameter 98 nm) was derived. At this time, assuming a cylindrical pore with a pore radius of rp, a relative pressure (p / p0) of 0.98 is expressed as rp=rk+t, which corresponds to a pore diameter of 98.8 nm. Here, rk is the radius of curvature of the adsorbate condensed in the pore, and is expressed by the following formula. rk=-0.953 / ln(p / p0). Furthermore, t is the average thickness of the nitrogen multilayer adsorption film at the relative pressure obtained from an experimentally or theoretically determined reference adsorption isotherm, and is expressed by the following formula: t=0.354*[-5 / ln(p / p0)]^1 / 3

[0150] (1b) Pore ratio (pore diameter 98 nm or less) (%) The porosity consisting of pores with a pore diameter of 98 nm or less was calculated using the above single-point total pore volume (pore diameter of 98 nm or less) A and the resin raw material density using the following formula. Porosity of pores with a diameter of 98 nm or less P (%) = A / (A+1 / density of resin raw material) x 100 The pore ratio was calculated by calculating the ratio of the above porosity to the porosity of the entire membrane, which will be described later. Pore ​​ratio (pore diameter 98 nm or less) (%) = (P / porosity of entire membrane) × 100

[0151] (2) Density (g / cm 3 ) The density of the sample was measured by the density gradient tube method (23° C.) in accordance with JIS K7112:1999.

[0152] (3) Film thickness (μm) The thickness of the PO microporous membrane was measured at room temperature of 23±2° C. using a microthickness gauge, KBM (trademark), manufactured by Toyo Seiki Co., Ltd. The average membrane thickness (μm) of the microporous membrane (before compression) and the membrane thickness (μm) of the porous membrane (before compression) were measured as follows.

[0153] [Average thickness of microporous membrane (before compression) (μm)] The thickness was measured using a Toyo Seiki Micro Thickness Meter (Type KBM, terminal diameter Φ5 mm) at an ambient temperature of 23 ± 2° C. When measuring the thickness, the microporous membrane was sampled in an area of ​​10 cm × 10 cm, multiple sheets of the microporous membrane were stacked so that the thickness was 15 μm or more, and measurements were taken at nine points to obtain an average, which was then divided by the number of sheets stacked to obtain the thickness of one sheet.

[0154] (4) Porosity of the entire membrane (%) A 10 cm x 10 cm square sample was cut from the microporous membrane and its volume (cm 3 ) and mass (g), and then calculate the density (g / cm 3 ) the porosity was calculated using the following equation. Porosity (%) = (volume-mass / density) / volume x 100

[0155] (5) Air permeability (sec / 100cm 3 ) The air permeability was determined as the air resistance in accordance with JIS P-8117. The air permeability of the microporous membrane was measured in accordance with JIS P-8117 using a Gurley air permeability meter, G-B2 (trademark), manufactured by Toyo Seiki Co., Ltd., in an atmosphere at a temperature of 23°C and a humidity of 40%, and the air permeability of the multilayer porous membrane or the air resistance of the PO microporous membrane was measured and defined as the air permeability.

[0156] However, in addition to the above (4) and (5), the porosity (%) (before compression) and the air permeability (sec / 100 cm 3 ) and the compression press test were performed as follows.

[0157] [Porosity (before compression) (%)] A sample of 3 cm x 3 cm square, 1 cm x 1 cm square, 5 cm x 5 cm square, or 10 cm x 10 cm square was cut from the polyolefin microporous membrane, and its volume (cm 3 ) and mass (g), and then calculate the density (g / cm 3 ) was calculated using the following formula: Porosity (%) = (volume-mass / density of mixed composition) / volume x 100 The density of the mixed composition was calculated from the density and mixing ratio of each of the polyolefin resin and other components used. The porosity (before compression) of the multilayer porous membrane can be calculated by the following formula. Porosity of multilayer porous membrane=(Porosity of polyolefin resin microporous membrane as substrate)×(Average thickness of polyolefin resin microporous membrane as substrate)÷(Total thickness of multilayer porous membrane)+(Porosity of coating layer)×(Thickness of coating layer)÷(Total thickness of multilayer porous membrane) Here, the porosity of the coating layer was set to 50% and the porosity of the multilayer porous film was calculated. When the porosity of the coating layer is not 50%, the porosity of the coating layer can be calculated as necessary in the same manner as the porosity of the polyolefin microporous film using the above formula. Specifically, the thickness of the coating layer is measured from direct observation with an SEM or from the change in film thickness before and after coating, and the volume of a coating layer sample of a specific area is determined. The porosity of the coating layer is then calculated using the mass average density of the coating components calculated from the material ratios of the components constituting the coating layer.

[0158] [Air permeability (before compression) (sec / 100cm 3 )] The air permeability was measured using Asahi Seiko Co., Ltd.'s Oken air permeability measuring instrument "EGO2." The air permeability was measured at three points along the membrane's transverse direction (TD): two points 10% inward of the total width from both ends toward the center, and one point in the center, and the average of these values ​​was calculated.

[0159] [Compression press test] A 0.8 mm thick rubber cushioning material, a 0.1 mm thick PET film, two microporous membranes, the PET film, and the cushioning material were laminated in this order, and the resulting laminate was left stationary, and a compression test was performed by applying pressure to one side of the cushioning material surface of the laminate. The microporous membrane used here was 5 x 5 cm square, and the average thickness (average of 9 points), basis weight, and air permeability were measured before use in the press test. The porosity before the compression press test was also calculated from the basis weight and average thickness. The compression test was performed using a press at a pressure of 10 MPa under conditions of a temperature of 25°C and a compression time of 3 minutes. One hour after unloading, the microporous membrane was removed from the laminate, and the average membrane thickness after compression (average of 9 points) and the air permeability after compression were measured. The porosity after compression was calculated from the basis weight and the average membrane thickness after compression.

[0160] (6) Weight (g / m 2 ), piercing strength (gf) and area weight conversion piercing strength (gf / (g / m 2 )) The weight is calculated by the unit area (1m 2The weight (g) of the polyolefin microporous membrane per unit area (1 m) was measured using an electronic balance (AUW120D) manufactured by Shimadzu Corporation after sampling to 1 m x 1 m. If it was not possible to sample to 1 m x 1 m, the membrane was cut to an appropriate area, the weight was measured, and the unit area (1 m) was then used. 2 The weight was converted to weight (g) per unit.

[0161] Using a handy compression tester KES-G5 (trademark) manufactured by Kato Tech, the microporous membrane was fixed with a sample holder having an opening diameter of 11.3 mm. Next, a puncture test was performed on the center of the fixed microporous membrane at a room temperature of 23°C and a humidity of 40% with a needle tip curvature radius of 0.5 mm and a puncture speed of 2 mm / sec, to measure the puncture strength (gf) as the maximum puncture load. The measured value of the puncture test was measured along the TD of the membrane at three points, two points 10% inside the full width from both ends to the center and one point in the center, and the average value was calculated. The puncture strength converted into basis weight is calculated using the following formula. Penetration strength converted to basis weight [gf / (g / m 2 )]=Piercing strength [gf] / Weight [g / m 2 ] Here, with regard to the pin puncture strength and basis weight equivalent pin puncture strength of a multilayer porous membrane having at least one layer provided on a polyolefin microporous membrane substrate, the properties were evaluated based on the pin puncture strength and basis weight equivalent pin puncture strength of the polyolefin microporous membrane substrate from the viewpoint of evaluating the strength of the resin and the strength per basis weight.

[0162] (7) Number of pores in the porous membrane or layer determined by the gas-liquid method (pores / μm 2 ) It is known that the fluid inside a capillary follows Knudsen flow when the mean free path of the fluid is larger than the pore diameter of the capillary, and follows Poiseuille flow when it is smaller. Therefore, it is assumed that the air flow in the air permeability measurement of a porous membrane or porous layer follows Knudsen flow, and the water flow in the water permeability measurement of a porous membrane or porous layer follows Poiseuille flow. In this case, the average pore size d (μm) of the porous membrane and the tortuosity τ a (Dimensionless) is the air permeation rate constant R gas(m 3 / (m 2 sec Pa), water permeation rate constant R liq (m 3 / (m 2 sec Pa), molecular speed of air ν (m / sec), viscosity of water η (Pa sec), standard pressure P s (=101,325 Pa), porosity ε (%), and film thickness L (μm) were used to calculate the pressure drop. d = 2ν × (R liq / R gas )×(16η / 3Ps)×10 6 τ a =(d×(ε / 100)×ν / (3L×P s ×R gas )) 1 / 2 Here, R gas was calculated from the air permeability (sec) using the following formula: R gas =0.0001 / (air permeability × (6.424 × 10 -4 )×(0.01276×101325)) Also, R liq is the permeability (cm 3 / (cm 2 sec Pa) using the following formula: Ta. R liq =water permeability / 100 The water permeability was determined as follows: A porous membrane or porous layer, which had been soaked in ethanol beforehand, was placed in a stainless steel liquid permeation cell having a diameter of 41 mm, and the ethanol in the membrane or layer was washed with water. After that, water was allowed to pass through the membrane or layer at a pressure difference of about 50,000 Pa. The amount of water permeated (cm 3 ) the amount of water permeable per unit time, unit pressure and unit area was calculated, and this was taken as the permeability. In addition, ν is the gas constant R (= 8.314), absolute temperature T (K), pi, and the average molecular weight of air M (= 2.896 × 10 -2 kg / mol) using the following formula: ν=((8R×T) / (π×M)) 1 / 2 Furthermore, the number of holes B (pieces / μm 2) was calculated using the following formula: B = 4 × (ε / 100) / (π × d 2 ×τ a )

[0163] (8) Pore diameter (8a) Mean flow diameter (μm) by half-dry method The average pore size (μm) was measured using a perm porometer (Porous Materials, Inc.: CFP-1500AE) in accordance with the half-dry method. Perfluoropolyester (trade name "Galwick", surface tension 15.6 dyn / cm) manufactured by the same company was used as the immersion liquid. The applied pressure and air permeability were measured for the dry curve and wet curve, and the average pore size dHD (μm) was calculated from the pressure PHD (Pa) at which the half curve of the obtained dry curve and the wet curve intersect, using the following formula, and was taken as the average flow diameter. dHD=2860×γ / PHD

[0164] (9) Viscosity average molecular weight (Mv) Based on ASTM-D4020, the intrinsic viscosity [η] (dl / g) in decalin solvent at 135°C was determined. For the microporous PO membrane and the polyethylene raw material, Mv was calculated by the following formula. [η]=6.77×10 -4 Mv 0.67 For polypropylene raw materials, Mv was calculated using the following formula: [η]=1.10×10 -4 Mv 0.80

[0165] (10) MD and TD tensile modulus (MPa) For the measurement of MD and TD, MD samples (MD120mm x TD10mm) and TD samples (MD10mm x TD120mm) were cut out. The tensile modulus of the samples in MD and TD was measured using a Shimadzu tensile tester, Autograph AG-A (trademark), in accordance with JIS K7127 under conditions of an atmospheric temperature of 23±2°C and humidity of 40±2%. The sample was set so that the chuck distance was 50mm, and the sample was stretched at a tensile speed of 200mm / min until the chuck distance reached 60mm, i.e., the strain reached 20.0%. The tensile modulus (MPa) was determined from the slope of the resulting stress-strain curve from 1.0% to 4.0% strain.

[0166] (11) Crystal structure analysis The long crystal period in the polyolefin microporous film was measured by small-angle X-ray scattering in the transmission method using a Rigaku NANOPIX. The sample was irradiated with CuKα radiation, and the scattering was detected by a semiconductor detector HyPix-6000. The measurement was performed under the following conditions: sample-detector distance 1312 mm, output 40 kV, 30 mA. The optical system used a point focus, and the slit diameters were 1st slit: φ=0.55 mm, 2nd slit: open, guard slit: φ=0.35 mm. The sample was set so that the sample surface was perpendicular to the X-ray incidence direction.

[0167] In addition, the crystallite size of the polyethylene MDND plane (110) in the polyolefin microporous membrane was measured by wide-angle X-ray scattering in the transmission method using a Rigaku NANOPIX. The sample was irradiated with CuKα radiation, and scattering was detected by an imaging plate. The measurement was performed under the conditions of a sample-detector distance of 110 mm and an output of 40 kV and 30 mA. A point focus was used for the optical system, and the slit diameters were 1st slit: φ=1.2 mm, guard slit: φ=0.35 mm. The sample was set so that the angle between the sample surface and the X-ray incidence direction was 11.0°. At this time, the X-ray incidence direction and the MD of the sample were perpendicular to each other.

[0168] (crystal long period [nm]) For the X-ray scattering pattern obtained from the HyPix-6000, a SAXS profile I(q) was obtained by circular averaging. -1 < q < 0.6 nm -1 A straight line baseline was drawn in the range and fitted with a Gaussian function. The position of maximum intensity was determined as the peak position q due to the crystal long period. m The crystal long period was calculated from Equation 4. d = 2π / q m formula 4 {In the formula, d(nm): Crystal long period q m (mm -1 ): Position of the peak originating from the lamella in the SAXS profile}

[0169] (Crystallite size) The range of 2θ=10.0° to 2θ=30.0° of the obtained XRD profile was separated into three peaks, an orthorhombic (110) diffraction peak, an orthorhombic (200) diffraction peak, and an amorphous peak. The crystallite size was calculated from the full width at half maximum of the (110) diffraction peak according to Scherrer's formula (Formula 1). The (110) diffraction peak and the (200) diffraction peak were approximated by a Voigt function, and the amorphous peak was approximated by a Gaussian function. The peak position of the amorphous peak was fixed at 2θ=19.6°, and the full width at half maximum was fixed at 6.3°, while the peak position and full width at half maximum of the crystalline peak were not fixed. The crystallite size was calculated from the full width at half maximum of the (110) diffraction peak calculated by peak separation according to Scherrer's formula (Formula 1). D(110)=Kλ / (βcosθ) Equation 1 {wherein D(110) is the crystallite size (nm) K: 0.9 (constant) λ: wavelength of X-rays (nm) β:(β1 2 -β2 2 ) 0.5 β1: Full width at half maximum (rad) of the (hkl) peak calculated as a result of peak separation β2: Full width at half maximum of the incident beam divergence (rad) θ: Bragg angle}

[0170] (12) Liquid absorption test of propylene carbonate A MD sample (MD50mm×TD10mm) and a TD sample (MD10mm×TD50mm) were cut out in strips from the microporous membrane. Next, a horizontal bar of a predetermined height was placed on a glass water tank containing propylene carbonate, and the end of the strip-shaped sample was pinned to the horizontal bar so that the long side was parallel to the vertical direction. Then, the horizontal bar was lowered to immerse the end of the sample piece in propylene carbonate by 10 mm, and the maximum height (mm) from the liquid surface at the position where the propylene carbonate rose up the microporous membrane after this immersion for 60 minutes was measured, and the measured value was the liquid absorption height of propylene carbonate in MD and TD. The measurement was performed in a 25° C. environment, and the average value of three measurements each in MD and TD was adopted.

[0171] (13) Battery testing

[0172] <Cycle test> Each battery assembled in the Examples and Comparative Examples described below was charged at 25° C. with a current value of 3 mA (about 0.5 C) up to a battery voltage of 4.3 V, and then the current value was started to be reduced from 3 mA so as to maintain 4.3 V. This method was used for the initial charging after the battery was fabricated for a total of about 3 hours, and then the battery was discharged at a current value of 3 mA down to a battery voltage of 3.0 V. The cycle characteristics were evaluated according to the following criteria, using the number of cycles at which the capacity retention rate fell below 80% of the initial capacity (capacity in the first cycle) for the first time. Cycle performance evaluation criteria A: More than 300 cycles B: 200 to less than 300 cycles C: 100 to less than 200 cycles D: 50 to less than 100 cycles E: 1 cycle or more but less than 50 cycles

[0173] <Initial overcharge test> A cell assembled by the method described in the Examples, separate from the cell for cycle testing, was charged to 4.3 V with constant current (CC)-constant voltage (CV) at a set current value of 0.1 C (convergence current value of cut-off condition: 0.03 mA) to measure the normal charge amount (i). A new cell was prepared in addition to the cell used to measure the normal charge capacity (i), and the overloaded battery (ii) was measured by CC-CV charging to 4.3 V at a set current value of 20 mA / cm2 (Cut Off condition: 25 mAh or convergence current value 0.03 mA). The value of (ii)-(i) was taken as the overcharge value due to dendrite short circuit and evaluated according to the following criteria. [Evaluation Rank] A: Less than 0.05mAh B: 0.05mAh or more and less than 0.1mAh C: 0.1mAh or more and less than 0.5mAh D: 0.5mAh or more but less than 1.0mAh E: 1.0mAh or more and 20.0mAh or less

[0174] a. Preparation of polyolefin microporous membrane Polyolefin microporous membranes a1 to a12 were produced under the following conditions. The properties of the polyolefin microporous membranes are shown in Table 1.

[0175] [a1] A microporous polyolefin membrane was produced by the following procedure: The resin raw material consisted of 93 parts by mass of high-density polyethylene having a melting point of 135° C. and a viscosity average molecular weight of 900,000, and 7 parts by mass of isotactic polypropylene having a melting point of 161° C. and a viscosity average molecular weight of 400,000. An appropriate amount of pentaerythrityl-tetrakis-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] was added as an antioxidant to the resin composition and mixed in a Henschel mixer. The resulting mixture was fed to the feed port of a twin-screw co-rotating extruder by a feeder. In addition, liquid paraffin was added to the twin-screw extruder cylinder by side feed in two batches so that the liquid paraffin (LP) amount ratio in the total mixture (100 parts by mass) to be melt-kneaded and extruded was 77.0 parts by mass. The set temperatures were 160°C for the kneading section and 200°C for the T-die. The molten mixture was then extruded into a sheet from the T-die and cooled with a cooling roll controlled to a surface temperature of 90°C to obtain a sheet-shaped molded product.

[0176] The obtained sheet-like molded product was introduced into a simultaneous biaxial stretching machine to obtain a first stretched membrane (first stretching step). The set stretching conditions were MD stretching ratio 7 times, TD stretching ratio 6.4 times, and MD and TD biaxial stretching temperature 121 ° C. The obtained first stretched membrane was then introduced into a methylene chloride tank and thoroughly immersed to extract and remove the liquid paraffin, which is a plasticizer, and then the methylene chloride was dried and removed to obtain an extracted membrane.

[0177] The extracted membrane was then introduced into a TD uniaxial tenter for heat setting. In the heat setting step, the drawn membrane was stretched at a TD stretching temperature of 125°C and a TD stretching ratio of 1.92 times, and then relaxed at a relaxation temperature of 125°C and a relaxation ratio of 0.78 times to obtain a polyolefin microporous membrane a1.

[0178] [a2] After preparing a polyolefin microporous membrane in the same manner as a1, the polyolefin microporous membrane was treated with a mixed gas in which the partial pressure ratio of the concentration of F2, O2 and N2 gases was adjusted to obtain a polyolefin microporous membrane a2. The mixed gas of O2 and N2 to be mixed with F2 was mixed in a ratio of 2:8 similar to the composition of air, and the partial pressure of the mixed gas of F2, O2 and N2 was adjusted to 1:9 and mixed in a buffer tank to produce a mixed treatment gas. The prepared polyolefin microporous membrane was placed in a reaction chamber and the mixed treatment gas was added. The concentration of the mixed treatment gas was adjusted to a pressure condition of 30 KPa using a gas valve between the buffer tank and the reaction chamber in a vacuum state, and the reaction time was adjusted to 20 minutes.

[0179] [a3] Polyolefin microporous membrane a3 was produced in the same manner as a1, except that the composition of the resin raw materials was 70 parts by mass of high-density polyethylene with a melting point of 135°C and a viscosity average molecular weight of 900,000, 20 parts by mass of polyketone with a melting point of 220°C, a melt index of 3.0 g / 10 min at a temperature of 240°C measured according to ASTM D1238 and a load of 2.16 kg at 240°C, and 10 parts by mass of maleic anhydride-modified polyethylene with a melting point of 131°C and a viscosity average molecular weight of 70,000, and the amount of liquid paraffin (LP) in the total mixture (100 parts by mass) to be extruded was 65.0 parts by mass.

[0180] [a4] Polyolefin microporous membrane a4 was produced in the same manner as a1, except that the composition of the resin raw material was 70 parts by mass of high-density polyethylene having a melting point of 135°C and a viscosity average molecular weight of 900,000, and 30 parts by mass of high-density polyethylene having a melting point of 135°C and a viscosity average molecular weight of 250,000, the amount of liquid paraffin (LP) in the total mixture (100 parts by mass) to be extruded was 75.0 parts by mass, the biaxial stretching temperature was 126°C, and as the heat setting process, a stretching operation was performed under conditions of a TD stretch ratio of 1.90 times, followed by a relaxation operation under conditions of a relaxation temperature of 136°C and a relaxation ratio of 0.84 times.

[0181] [a5] The composition of the resin raw material was 40 parts by mass of high-density polyethylene having a melting point of 135°C and a viscosity average molecular weight of 700,000, 40 parts by mass of high-density polyethylene having a melting point of 135°C and a viscosity average molecular weight of 250,000, 5 parts by mass of isotactic polypropylene having a melting point of 161°C and a viscosity average molecular weight of 400,000, and 15 parts by weight of silica "DM10C" (trademark, manufactured by Tokuyama Corporation. Hydrophobized with dimethyldichlorosilane). The amount of liquid paraffin (LP) in the total mixture (100 parts by mass) to be extruded was 70.0 parts by mass, the biaxial stretching temperature was 127°C, and as the heat setting process, a stretching operation was performed under conditions of a stretching temperature of 129°C and a TD stretch ratio of 1.90 times, followed by a relaxation operation under conditions of a relaxation temperature of 136°C and a relaxation ratio of 0.79 times. A polyolefin microporous membrane a5 was produced in the same manner as a1.

[0182] [a6] Polyolefin microporous membrane a6 was produced in the same manner as a1, except that the composition of the resin raw material was 30 parts by mass of high-density polyethylene having a melting point of 135°C and a viscosity average molecular weight of 900,000, and 70 parts by mass of high-density polyethylene having a melting point of 135°C and a viscosity average molecular weight of 250,000, the amount of liquid paraffin (LP) in the total mixture (100 parts by mass) to be extruded was 71.0 parts by mass, the biaxial stretching temperature was 128°C, and the heat setting process involved a stretching operation under conditions of a stretching temperature of 128°C and a TD stretch ratio of 1.70 times, followed by a relaxation operation under conditions of a relaxation temperature of 128°C and a relaxation ratio of 0.94 times.

[0183] [a7] After preparing a polyolefin microporous membrane in the same manner as a4, the prepared polyolefin microporous membrane was plasma-treated to obtain polyolefin microporous membrane a7. In the plasma treatment, a dielectric barrier discharge type electrode was used under atmospheric pressure, 300ml of nitrogen per minute as carrier gas and 1ml of oxygen per minute as reactive gas were injected, and plasma was discharged at a power of 3.6kW and a voltage of 12kV, and both sides of the polyolefin microporous membrane were simultaneously contacted with plasma for 3 seconds. The distance between the electrode and the microporous membrane during the plasma discharge was fixed at 3mm.

[0184] [a8] The composition of the resin raw materials was 47.5 parts by mass of high-density polyethylene having a melting point of 135°C and a viscosity average molecular weight of 700,000, 47.5 parts by mass of high-density polyethylene having a melting point of 135°C and a viscosity average molecular weight of 250,000, and 5 parts by mass of isotactic polypropylene having a melting point of 161°C and a viscosity average molecular weight of 400,000, the amount of liquid paraffin (LP) in the total mixture (100 parts by mass) to be extruded was 68.0 parts by mass, the biaxial stretching temperature was 120°C, and as the heat setting process, a stretching operation was performed under conditions of a stretching temperature of 130°C and a TD stretch ratio of 1.75 times, followed by a relaxation operation under conditions of a relaxation temperature of 131°C and a relaxation ratio of 0.86 times. Except for this, a polyolefin microporous membrane produced in the same manner as a1 was treated with a mixed gas of F2, O2 and N2 in the same manner as a2, to obtain polyolefin microporous membrane a8.

[0185] [a9] The composition of the resin raw material was 70 parts by mass of high-density polyethylene having a melting point of 135°C and a viscosity average molecular weight of 700,000, 23 parts by mass of high-density polyethylene having a melting point of 135°C and a viscosity average molecular weight of 250,000, and 7 parts by mass of isotactic polypropylene having a melting point of 161°C, a viscosity average molecular weight of 400,000, and a molecular weight distribution of 6.0, the amount of liquid paraffin (LP) in the total mixture to be extruded (100 parts by mass) was 71.0 parts by mass, the biaxial stretching temperature was 125°C, and as the heat setting process, a stretching operation was performed under conditions of a stretching temperature of 130°C and a TD stretch ratio of 1.90 times, and then a relaxation operation was performed under conditions of a relaxation temperature of 128°C and a relaxation ratio of 0.83 times. A polyolefin microporous membrane a9 was produced in the same manner as a1, except that

[0186] [a10] A polyolefin microporous membrane a10 was obtained in the same manner as a8, except that the treatment with the mixed gas of F2, O2 and N2 was not performed.

[0187] [a11] A polypropylene (PP) resin having a melt index of 0.25 g / 10 min at a temperature of 190° C. and a load of 2.16 kg, measured according to ASTM D1238, was melted in a 2.5-inch extruder and fed to an annular die using a gear pump. The die temperature was set to 260° C., and the molten polymer was cooled by blown air and then wound up on a roll. Similarly, a high-density polyethylene (PE) resin having a melt index of 0.38 g / 10 min at a temperature of 190° C. and a load of 2.16 kg was melted in a 2.5-inch extruder and fed to an annular die using a gear pump. The die temperature was set to 230° C., and the molten polymer was cooled by blown air and then wound up on a roll. The polypropylene and polyethylene precursors (raw film) wound up on the roll each had a thickness of 5 μm, and then the PP and PE precursors were bonded to form PP / PE / PP to obtain a raw film having a three-layer structure of PP / PE / PP. This raw film was annealed for 20 minutes at 125° C. The annealed film was then cold stretched to 15% at room temperature, then hot stretched 1.5 times in MD at 115° C., relaxed to 0.69 times in MD at 125° C., and then treated with F2, O2, and N2 gas in the same manner as a2 to obtain a polyolefin microporous membrane a11.

[0188] [a12] The composition of the resin raw material was 70 parts by mass of ultra-high molecular weight polyethylene with a melting point of 134°C and a viscosity average molecular weight of 4.5 million, 30 parts by mass of polyethylene wax with a melting point of 113°C and a viscosity average molecular weight of 1000, and a pore size of 0.1 μm and a BET specific surface area of ​​11.6 m, so that the ratio of the total volume was 36%. 2 / g of calcium carbonate was added. An appropriate amount of pentaerythrityl-tetrakis-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] was added as an antioxidant to the resin composition and mixed with a Henschel mixer. The resulting mixture was fed to the feed port of a twin-screw co-rotating extruder by a feeder and extruded into a sheet from a T-die set at 200°C. The sheet was rolled using a pair of rolls at a surface temperature of 150°C to produce a rolled sheet. The rolled sheet was then immersed in hydrochloric acid (4 mol / L) containing 0.5% by weight of a nonionic surfactant to remove calcium carbonate, and then stretched 7.0 times in the MD, and the stretching ratio was fixed and heat set at 123°C to obtain a polyolefin microporous membrane a12.

[0189] b. Preparation of the positive electrode A positive electrode b1 was prepared under the following conditions. Lithium nickel manganese cobalt composite oxide (Li[Ni 1 / 3 Mn 1 / 3 Co 1 / 3 91.2 parts by mass of ]O2), 2.3 parts by mass each of flake graphite and acetylene black as conductive materials, and 4.2 parts by mass of polyvinylidene fluoride (PVdF) as a resin binder were prepared, and these were dispersed in N-methylpyrrolidone (NMP) to prepare a slurry. This slurry was applied to one side of an aluminum foil with a thickness of 20 μm to serve as a positive electrode current collector using a die coater, with the positive electrode active material coating amount being 120 g / m 2 After drying at 130°C for 3 minutes, the positive electrode active material was pressed using a roll press so that the bulk density of the positive electrode active material was 2.90 g / cm 3 This was compression molded to obtain a positive electrode with an area of ​​2.00 cm. 2 It was punched into a circular shape.

[0190] c. Preparation of negative electrode Negative electrodes c1 and c2 were prepared under the following conditions.

[0191] [c1] Thickness 0.5mm, area 2.00cm 2A circular lithium metal (Honjo Metals) was placed in a SUS glove box under a nitrogen atmosphere with a steady supply of high-purity nitrogen gas (99.99%) and left at 60°C for 2 hours to produce a lithium metal negative electrode c1 with lithium nitride formed on the surface.

[0192] [c2] Thickness 0.5mm, area 2.00cm 2 A circular metallic lithium (Honjo Metals) was used as the negative electrode c2.

[0193] d. Preparation of non-aqueous electrolyte Electrolyte solutions d1 to d8 were prepared under the following conditions.

[0194] [d1] An electrolyte solution d1 was prepared by dissolving LiPF6 as a solute in a mixed solvent of ethylene carbonate:ethyl methyl carbonate=1:2 (volume ratio) to a concentration of 2.0 mol / L.

[0195] [d2] An electrolyte solution d2 was prepared by dissolving LiPF6 as a solute in a mixed solvent of ethylene carbonate:ethyl methyl carbonate=1:2 (volume ratio) to a concentration of 1.3 mol / L.

[0196] [d3] An electrolyte solution d3 was prepared by dissolving LiPF6 as a solute in a mixed solvent of fluoroethylene carbonate:ethyl methyl carbonate=1:2 (volume ratio) to a concentration of 1.0 mol / L.

[0197] [d4] An electrolyte solution d4 was prepared by dissolving LiTFSI as a solute in a mixed solvent of ethylene carbonate:ethyl methyl carbonate=1:2 (volume ratio) to a concentration of 1.0 mol / L.

[0198] [d5] An electrolyte solution d5 was prepared by dissolving LiPF6 as a solute in a mixed solvent of ethylene carbonate:ethyl methyl carbonate=1:2 (volume ratio) to a concentration of 3.0 mol / L.

[0199] [d6] An electrolyte solution was prepared by dissolving LiPF6 in 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIMBF4) as an ionic liquid so that the LiPF6 concentration was 1.0 mol / L, and electrolyte solution d6 was obtained.

[0200] [d7] Tetraglyme (G4) and LiTFSI were placed in a beaker in a molar ratio of 1:1, and mixed until a homogeneous solution was formed, thereby preparing an electrolyte solution d7.

[0201] [d8] An electrolyte solution d8 was prepared by dissolving LiPF6 as a solute in a mixed solvent of ethylene carbonate:ethyl methyl carbonate=1:2 (volume ratio) to a concentration of 1.0 mol / L.

[0202] e. Battery assembly <Examples 1 to 11 and Comparative Examples 1 to 4> The combinations of the polyolefin microporous membranes prepared in the steps a and b, the positive electrode, the negative electrode, and the electrolyte were changed as shown in Table 2, and the batteries of Examples 1 to 11 and Comparative Examples 1 to 4 were prepared under the following conditions. In an argon box, the negative electrode, separator, and positive electrode were stacked in this order from the bottom so that the active material of the positive electrode and the negative electrode faced each other. This laminate was stored in a lidded stainless steel metal container insulated from the container body and the lid so that the lithium foil of the negative electrode and the aluminum foil of the positive electrode were in contact with the container body and the lid, respectively, to obtain a cell. This cell was dried at 25°C for 10 hours under reduced pressure. Thereafter, a nonaqueous electrolyte was injected into the container in an argon box and sealed to obtain a battery. Table 2 shows the combinations of polyolefin microporous membranes, positive electrodes, negative electrodes, and electrolytes in Examples 1 to 11, Example 12, and Comparative Examples 1 to 4. When the negative electrode c1 was used, the surface on which lithium nitride was formed was opposed to the polyolefin microporous membrane side to assemble the battery.

[0203] <Example 12> Polyvinylidene fluoride resin particles (melting point 140°C, particle size 0.2μm) were dissolved in acetone to a concentration of 8.0wt% to prepare a coating solution. The prepared coating solution was applied with a bar coater to one side of a polyolefin microporous membrane prepared in the same manner as in a1 above, and dried at 40°C for 1 hour to obtain a separator with PVdF applied to one side. The coating amount of the PVdF layer was 3.2g / m 2 Using the obtained PVdF-coated separator, positive electrode b1, negative electrode c2, and electrolyte d2, a battery was assembled in the same manner as in Examples 1 to 11 and Comparative Examples 1 to 4. The PVdF-coated surface of the separator was placed so as to face the negative electrode.

[0204] Table 2 shows the configurations of Examples 1 to 12 and Comparative Examples 1 to 4 and the results of the battery evaluation.

[0205] [Table 1-1]

[0206] [Table 1-2]

[0207] [Table 2-1]

[0208] [Table 2-2]

[0209] [Table 2-3]

Claims

1. A polyolefin microporous membrane for use in a separator for a non-aqueous electrolyte battery, the membrane having an ion-conducting layer between the separator and a metal negative electrode, A polyolefin microporous membrane having a liquid absorption height in the machine direction (MD) and the width direction (TD) of 1.0 mm or more and 50 mm or less in a propylene carbonate liquid absorption test.

2. The microporous polyolefin membrane according to claim 1 , which is a laminated separator.

3. The process is as follows: (1) preparing a lidded stainless steel metal container insulated from the container body and the lid, and a non-aqueous electrolyte; (2) preparing a polyolefin microporous membrane as a separator, the polyolefin microporous membrane having a liquid absorption height in the machine direction (MD) and the transverse direction (TD) of 1.0 mm or more and 50 mm or less in a propylene carbonate liquid absorption test; (3) providing a metal negative electrode having an ion-conducting layer on at least one surface thereof; (4) preparing a positive electrode; (5) preparing a laminate in which the ion conductive layer of the metal negative electrode and the separator are opposed to each other and the metal negative electrode, the separator, and the positive electrode are stacked in this order; and (6) A process of producing a cell by housing the laminate in a lidded stainless steel metal container insulated from the container body and the lid so that the metal negative electrode and positive electrode are in contact with the container body and the lid, respectively, and then drying the cell under reduced pressure at 25° C. for 10 hours, injecting a nonaqueous electrolyte into the container and sealing it, thereby producing a battery. The method for producing a non-aqueous electrolyte battery, comprising:

Citation Information

Patent Citations

  • Electric double layer capacitor

    JP1994036972A

  • Porous membrane and its production

    JP1998316781A

  • Separator

    JP2002343329A

  • Nonaqueous electrolyte battery, electrode for nonaqueous electrolyte battery, and manufacturing method of this electrode for nonaqueous electrolyte battery

    JP2007123237A

  • Separator for electric double layer capacitor

    JP2010087435A