Method for producing microfibril cellulose and double disk refiner

The method and apparatus for producing microfibrillar cellulose using real-time clearance control and a monoflow system in a double disc refiner effectively prevent metal contamination, enhancing product quality by minimizing metal touch and maintaining brightness.

JP2024138894APending Publication Date: 2024-10-09NIPPON PAPER IND CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023049611
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing double disc refiners fail to adequately prevent metal touch during the production of microfibrillar cellulose, leading to increased metal contamination and issues such as decreased brightness and iron odor in the final product.

Method used

A method and apparatus for producing microfibrillar cellulose using a double disc refiner that includes real-time detection and control of the clearance between movable blades and a rotor, maintaining a predetermined gap of 0.01 mm to 0.5 mm, and utilizing a monoflow system to minimize metal contact.

Benefits of technology

Reduces the amount of metal contamination in the produced microfibrillar cellulose, preventing metal touch and maintaining product quality by ensuring precise blade-to-rotor spacing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138894000001_ABST
    Figure 2024138894000001_ABST
Patent Text Reader

Abstract

To produce microfibril cellulose while preventing blade wear and tear due to metal touch in a double disk refiner and mixing of iron powder into a raw material.SOLUTION: The present invention relates to a method for producing microfibril cellulose from a pulp raw material by using a double disc refiner, and comprises a beating process in which the pulp material is beaten by the double disc refiner, and a control process implemented during the beating process to control the clearance between a first mobile fixed tooth and a second mobile fixed tooth mounted across a rotor fixed in the direction of the rotation axis.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing microfibril cellulose and a double disc refiner used in the production of microfibril cellulose. [Background technology]

[0002] Cellulose nanofibers and microfibril cellulose obtained by pulp raw material pulping are fine fibers with a fiber width on the nano to micro order, and are expected to be used in various fields as new materials with functions not found in ordinary pulp, such as high strength, high elasticity, and thixotropy. For example, in the papermaking field, paper strength improvers are sometimes used to improve the strength of paper, and in order to reinforce the effect of these agents, the addition of microfibril cellulose, which has a lower degree of defibration than cellulose nanofibers and can be produced at low cost, has been considered.

[0003] Microfibril cellulose is produced by beating raw pulp using a double disc refiner or the like. When beating is performed using a double disc refiner, metal touch may occur due to contact between the rotary blade and the fixed blade. When metal touch occurs, it not only accelerates wear of the blade, but also causes problems such as a decrease in brightness and an iron odor due to iron powder being mixed into the raw material. Therefore, in the double disc refiner described in Patent Document 1, when the occurrence of metal touch is detected, the motor output is varied to control the gap between the rotary blade and the fixed blade to be widened. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-112069 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the double disc refiner disclosed in Patent Document 1 controls the gap between the rotating blade and the fixed blade to be wider after detecting the occurrence of metal touch, and therefore is unable to fully resolve problems such as blade wear due to metal touch and the contamination of the raw material with iron powder.

[0006] An object of the present invention is to reduce the amount of metal contained in the produced microfibril cellulose by preventing the occurrence of metal touch in a double disc refiner. [Means for solving the problem]

[0007] The present invention provides the following: (1) A method for producing microfibril cellulose, comprising the steps of: producing microfibril cellulose from a pulp raw material using a double disc refiner; and a control step, carried out during the beating step, of controlling the clearance between a rotor fixed in the direction of a rotation shaft and a first movable fixed blade and a second movable fixed blade disposed on either side of the rotor. (2) The method for producing microfibril cellulose described in (1), wherein the control process includes a detection process for detecting a clearance between the rotor and the first movable fixed blade and a clearance between the rotor and the second movable fixed blade, and a movement process for moving the first movable fixed blade and the second movable fixed blade in the direction of the rotation axis based on the detection result by the detection process so that the clearance with the rotor becomes a predetermined clearance. (3) The method for producing microfibril cellulose according to (1) or (2), wherein the predetermined clearance is 0.01 mm to 0.5 mm. (4) The method for producing microfibril cellulose according to (1) or (2), wherein the flow mode of the pulp raw material in the double disc refiner is a monoflow mode. (5) The method for producing microfibril cellulose according to (1) or (2), wherein the concentration of the pulp raw material beaten in the double disc refiner is 0.5% to 10%. (6) A double disc refiner comprising a rotor fixed in the direction of a rotation axis, a first movable fixed blade and a second movable fixed blade arranged on either side of the rotor in the direction of the rotation axis, and a control unit that moves the first movable fixed blade and the second movable fixed blade in the direction of the rotation axis to control the clearance with the rotor. (7) A double disc refiner as described in (6), wherein the control unit includes a detection unit that detects the clearance between the first movable fixed blade and the rotor and the clearance between the second movable fixed blade and the rotor, and a drive unit that moves the first movable fixed blade and the second movable fixed blade in the direction of the rotation axis so that the clearance with the rotor becomes a predetermined clearance based on the detection result by the detection unit. (8) A double disc refiner according to (6) or (7), wherein the predetermined clearance is 0.01 mm to 0.5 mm. (9) A double disc refiner according to (6) or (7), in which the flow mode of the pulp raw material is a monoflow mode. (10) A double disc refiner according to (6) or (7), further comprising a circulation pipe for circulating the beaten pulp material to the beating chamber. Effect of the Invention

[0008] According to the method for producing microfibril cellulose and the double disc refiner of the present invention, the amount of metal contained in the produced microfibril cellulose can be reduced. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a diagram showing the configuration of a double disc refiner of the present invention. [Diagram 2] FIG. 1 is a diagram showing the system configuration of a double disc refiner of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the method for producing microfibril cellulose of the present invention and the double disc refiner used in the production of microfibril cellulose will be described with reference to the drawings. In the present invention, "to" includes the end values. In other words, "X to Y" includes the value X and the value Y at both ends.

[0011] (Microfibril Cellulose) Microfibril cellulose (hereinafter also referred to as "MFC") is a fiber with an average fiber width of 500 nm or more obtained by defibrating or beating cellulosic raw materials such as pulp, and chemically modified microfibril cellulose (hereinafter also referred to as "chemically modified MFC") is MFC obtained by defibrating or beating the chemically modified cellulosic raw material obtained by chemically modifying a cellulosic raw material.

[0012] In the present invention, the average fiber width is the length-weighted average fiber width, and the fiber width can be measured using a fiber tester manufactured by ABB Corporation or a fractionator manufactured by Valmet. The lower limit of the fiber width is preferably 500 nm or more, and the upper limit is not particularly limited, but is about 60 μm or less. MFC is obtained by relatively weakly defibrating or beating a cellulosic raw material using a beater, disperser, refiner, etc. Therefore, compared with cellulose nanofibers obtained by strongly defibrating a cellulosic raw material using a high-pressure homogenizer, etc., MFC includes various fibers of different sizes, such as fibers with cellulose microfibril fluff on the fiber surface and fibers defibrated to a fiber width on the order of submicrons, and also includes fibers with a fiber width on the order of microns.

[0013] (Raw pulp) Examples of raw pulp include unbleached softwood kraft pulp (NUKP), bleached softwood kraft pulp (NBKP), unbleached hardwood kraft pulp (LUKP), bleached hardwood kraft pulp (LBKP), unbleached softwood sulfite pulp (NUSP), bleached softwood sulfite pulp (NBSP), unbleached hardwood sulfite pulp (LUSP), bleached hardwood sulfite pulp (LBSP), thermomechanical pulp (TMP), pressurized groundwood pulp (PGW), refiner groundwood pulp (RGP), alkaline hydrogen peroxide mechanical pulp (APMP), alkaline hydrogen peroxide thermomechanical pulp (APTMP), pulp derived from herbs such as linter, jute, hemp, paper mulberry, Mitsumata, and kenaf, pulp derived from bamboo, recycled pulp, and waste paper pulp, but are not limited to these.

[0014] (chemical modification) Chemical modification refers to the introduction of functional groups into pulp, and the chemical modification is preferably anionic modification, i.e., the chemically modified pulp preferably has anionic groups. Examples of the anionic groups include acid groups such as a carboxyl group, a carboxyl group-containing group, a phosphoric acid group, a phosphoric acid group-containing group, and a sulfate ester group. Examples of the carboxyl group-containing group include -COOH group, -R-COOH (R is an alkylene group having 1 to 3 carbon atoms), and -OR-COOH (R is an alkylene group having 1 to 3 carbon atoms). Examples of the phosphoric acid group-containing group include a polyphosphoric acid group, a phosphorous acid group, a phosphonic acid group, and a polyphosphonic acid group. Depending on the reaction conditions, these acid groups may be introduced in the form of a salt (for example, a carboxylate group (-COOM, M is a metal atom)). In the present invention, the chemical modification is preferably oxidation or etherification.

[0015] The oxidation can be carried out as known in the art. For example, a method of oxidizing raw pulp in water using an oxidizing agent in the presence of an N-oxyl compound and a substance selected from the group consisting of bromides, iodides, and mixtures thereof can be mentioned. According to this method, the primary hydroxyl group at the C6 position of the glucopyranose ring on the surface of cellulose is selectively oxidized to generate a group selected from the group consisting of an aldehyde group, a carboxyl group, and a carboxylate group. Alternatively, an ozone oxidation method can be mentioned. According to this oxidation reaction, at least the hydroxyl groups at the 2- and 6-positions of the glucopyranose ring constituting cellulose are oxidized, and the cellulose chain is decomposed.

[0016] The term "N-oxyl compound" refers to a compound capable of generating a nitroxy radical. Any compound that can promote the desired oxidation reaction can be used as the N-oxyl compound. Examples include 2,2,6,6-tetramethylpiperidine-1-oxy radical (TEMPO) and its derivatives (e.g., 4-hydroxyTEMPO).

[0017] An example of a method for measuring the amount of carboxyl groups is explained below. 60 mL of a 0.5% by mass slurry (aqueous dispersion) of oxidized cellulose is prepared, and a 0.1 M aqueous hydrochloric acid solution is added to adjust the pH to 2.5, after which a 0.05 N aqueous sodium hydroxide solution is added dropwise and the electrical conductivity is measured until the pH reaches 11. The amount of carboxyl groups can be calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of a weak acid, where the change in electrical conductivity is gradual. Amount of carboxyl groups [mmol / g oxidized cellulose] = a [mL] x 0.05 / weight of oxidized cellulose [g]

[0018] The amount of carboxyl groups in oxidized cellulose measured in this manner is preferably 0.1 mmol / g or more, more preferably 0.5 mmol / g or more, and even more preferably 0.8 mmol / g or more, based on the bone dry weight. The upper limit of this amount is preferably 3.0 mmol / g or less, more preferably 2.5 mmol / g or less, and even more preferably 2.0 mmol / g or less. Thus, this amount is preferably 0.1 mmol / g or more and 3.0 mmol / g or less, more preferably 0.5 mmol / g or more and 2.5 mmol / g or less, and even more preferably 0.8 mmol / g or more and 2.0 mmol / g or less.

[0019] Examples of etherification include carboxymethylation, methylation, ethylation, cyanoethylation, hydroxyethylation, hydroxypropylation, ethylhydroxyethylation, and hydroxypropylmethylation. Among these, carboxymethylation is preferred. Carboxymethylation can be carried out, for example, by mercerizing the raw pulp as the bottom raw material, followed by etherification.

[0020] The degree of carboxymethyl substitution per glucose unit of carboxymethyl cellulose can be measured, for example, by the following method. That is, 1) Weigh out about 2.0 g of carboxymethyl cellulose (bone dry) and place it in a 300 mL Erlenmeyer flask with a stopper. 2) Add 100 mL of a solution of 100 mL of concentrated nitric acid in 1000 mL of nitric acid methanol, and shake for 3 hours to convert the carboxymethyl cellulose salt (carboxymethyl cellulose) into hydrogen type carboxymethyl cellulose. 3) Weigh out about 1.5 g to 2.0 g of hydrogen type carboxymethyl cellulose (bone dry) and place it in a 300 mL Erlenmeyer flask with a stopper. 4) Wet the hydrogen type carboxymethyl cellulose with 15 mL of 80% methanol, add 100 mL of 0.1 N NaOH, and shake at room temperature for 3 hours. 5) Using phenolphthalein as an indicator, back titrate the excess NaOH with 0.1 N H2SO4. 6) Calculate the degree of carboxymethyl substitution (DS) by the following formula. A = [(100 × F'-(0.1N H2SO4) (mL) × F) × 0.1] / (bone-dry weight of hydrogen-type carboxymethyl cellulose (g)) DS = 0.162 x A / (1-0.058 x A) A: The amount of 1N NaOH required to neutralize 1 g of hydrogen-type carboxymethyl cellulose (mL) F: Factor of 0.1N H2SO4 F': factor of 0.1N NaOH

[0021] The degree of carboxymethyl substitution per anhydrous glucose unit in carboxymethylated cellulose is preferably 0.01 or more, more preferably 0.05 or more, and even more preferably 0.10 or more. The upper limit of the degree of substitution is preferably 0.50 or less, more preferably 0.40 or less, and even more preferably 0.35 or less. Therefore, the degree of carboxymethyl group substitution is preferably 0.01 or more and 0.50 or less, more preferably 0.05 or more and 0.40 or less, and even more preferably 0.10 or more and 0.35 or less.

[0022] (Beating process) In this process, the chemically modified pulp with the adjusted solid content concentration is beaten using a double disc refiner. Beating the chemically modified pulp causes the fibers to become finer (fiber length and width are reduced) and to become fibrillated (fiber fluff is increased). In the beating process of the present invention, the beating process using the double disc refiner may be a circulating process, or a continuous process in which the beating process is continuously performed using multiple double disc refiners.

[0023] In the present invention, when beating is performed using a double disc refiner that performs partial circulation using a circulation piping, the actual number of times the raw material is processed (the number of times the raw material actually passes between the blade clearances) is calculated by multiplying the number of times the raw material to be processed passes through one double disc refiner (number of passes) by n as shown below, and in the case of monoflow processing, further multiplying it by 2. n=1 / (1-a) Here, a = circulation ratio. (When the circulation ratio is 50%, a = 0.5, and when the circulation ratio is 75%, a = 0.75. When partial circulation is not performed, a = 0.)

[0024] When multiple double disc refiners with partial circulation are used for continuous processing, the actual number of times the beating process is performed should be calculated for each double disc refiner using the method described above and then added together.

[0025] When the beating process is performed multiple times and batch processing is performed by complete circulation without partial circulation, the actual number of times the beating process is performed is the number of times the raw material to be processed actually passes through the blade clearance of the double disc refiner before being recovered.

[0026] (Double disc refiner) A double disc refiner is equipped with two discs DA and DB with beating blades and a disc DM with another beating blade between them, and either the discs DA and DB or the disc DM are fixed and the other rotates, or the discs DA and DB and the disc DM rotate in opposite directions. Examples of double disc refiners in which the two discs DA and DB are fixed discs and the DM is a floating disc that rotates freely between them include the double disc refiner manufactured by Aikawa Iron Works Co., Ltd., the double disc refiner manufactured by Mitsubishi Heavy Industries / Beloit (Jones), the twin hydra disc manufactured by Ishikawajima Industrial Machinery / Black & Clawson, and the twin disc refiner manufactured by Hitachi Zosen (Hitachi Zosen Tomioka Machinery) / Escher Wyss.

[0027] The blade width of the two disks DA and DB is preferably 0.3 to 4.0 mm, more preferably 0.5 to 1.3 mm. The groove width of the disks DA and DB is preferably 0.5 to 4.0 mm, more preferably 0.8 to 1.7 mm. The blade width and groove width of the disks DA and DB may be the same or different. The blade angle is not particularly limited, but is preferably 0 to 40°, and more preferably 5 to 20°.

[0028] Double disc refiners are broadly classified into two types, monoflow type and duoflow type, according to the raw material flow system. In the monoflow type, the raw material flows from the beating gap close to the raw material inlet side to the other beating gap, while in the duoflow type, the raw material is inserted from the center and flows in parallel through the beating gaps formed on both sides of the disc DM. In the manufacturing method of the present invention, the monoflow type is preferred as the raw material flow system from the viewpoint of efficient defibration.

[0029] The double disc refiner used in the present invention will be described with reference to Figure 1. Figure 1 is a cross-sectional view showing an outline of a double disc refiner with a monoflow material flow system.

[0030] In the double disc refiner 2, a rotating disc DM (rotor) 8 is disposed in a beating chamber 6 which beats the pulp raw material fed from a raw material inlet 4, and blades having a predetermined blade width and groove width are attached to both sides of the rotating disc DM8. The rotating disc DM8 is attached to a drive shaft 14 which is connected to a motor 16 and driven to rotate. Here, the position of the rotating disc DM8 in the direction of the drive shaft 14 is fixed. A fixed disc DA (first movable fixed blade) 10 and a fixed disc DB (second movable fixed blade) 12 are disposed on the inner wall of the beating chamber 6, facing the blades attached to both sides of the rotating disc DM8. Blades having a predetermined blade width and groove width are attached to the fixed disc DA10 and the fixed disc DB12.

[0031] A circulation pipe 18 for circulating the beaten raw material to the beating chamber 6 is connected to the beating chamber 6. A discharge port 20 for discharging the beaten raw material to the outside of the beating chamber 6 is formed in the beating chamber 6, and an outlet pipe 22 for sending the beaten raw material to a recovery tank (not shown) is connected to the discharge port 20. The circulation pipe 18 and the outlet pipe 22 are provided with valves 24 for adjusting the flow rate.

[0032] In the beating chamber 6, a first sensor 26 for detecting the clearance between the rotating disk DM8 and the fixed disk DA10 and a second sensor 28 for detecting the clearance between the rotating disk DM8 and the fixed disk DA12 are provided. Further, a first drive unit 30 for moving the fixed disk DA10 in the direction of the drive shaft 14 so that the clearance between the rotating disk DM8 and the fixed disk DA10 becomes a predetermined value based on the detection result by the first sensor 26, and a second drive unit 32 for moving the fixed disk DA12 in the direction of the drive shaft 14 so that the clearance between the rotating disk DM8 and the fixed disk DA12 becomes a predetermined value based on the detection result by the second sensor 28 are provided.

[0033] 2 is a diagram showing the system configuration of a double disc refiner 2 of the present invention. The double disc refiner 2 is equipped with a control unit 40 that controls the entire device. The motor 16, the first sensor 26, the second sensor 28, the first drive unit 30, and the second drive unit 32 are connected to the control unit 40.

[0034] When the double disc refiner 2 is used to beat the pulp raw material, the pulp raw material is input from the raw material inlet 4 of the double disc refiner 2 and sent to the beating chamber 6. The pulp raw material sent to the beating chamber 6 is first beaten in the beating gap formed between the fixed disc DA10 and the rotating disc DM8, then beaten in the beating gap formed between the fixed disc DB12 and the rotating disc DM8, and a part of the pulp raw material is sent again to the beating chamber 6 via the circulation pipe 18. The beaten pulp raw material is discharged from the discharge port 20 and sent to a recovery tank (not shown) via the outlet pipe 22. The amount of circulating pulp raw material and the amount of beaten pulp raw material discharged from the discharge port 20 are adjusted by a manual valve 24.

[0035] Here, in the double disc refiner 2, while the beating process of the pulp raw material is being performed, the control unit 40 acquires the value of the clearance between the rotating disc DM8 and the fixed disc DA10 detected by the first sensor 26 and the value of the clearance between the rotating disc DM8 and the fixed disc DB12 detected by the second sensor 28. The control unit 40 then controls the first drive unit 30 to move the fixed disc DA10 in the direction of the drive shaft 14 so that the clearance between the rotating disc DM8 and the fixed disc DA10 becomes a predetermined value. The control unit 40 also controls the second drive unit 32 to move the fixed disc DB12 in the direction of the drive shaft 14 so that the clearance between the rotating disc DM8 and the fixed disc DB12 becomes a predetermined value.

[0036] In the production method of the present invention, when a double disc refiner 2 is used, the operating conditions are such that the clearance between the fixed disc DA10 and the rotary disc DM8 and between the fixed disc DB12 and the rotary disc DM8 is preferably 0.5 mm or less, more preferably 0.4 mm or less, and even more preferably 0.2 mm or less. There is no particular lower limit, but in order to avoid metal touch, it is preferably 0.01 mm or more. The operating temperature is preferably 5 to 120°C. Note that the flow rate, treatment time, and other conditions are appropriately adjusted so as to obtain chemically modified microfibril cellulose having the desired fiber width.

[0037] In the manufacturing method of the present invention, the solid content of the chemically modified pulp raw material to be subjected to the beating process is 10% by mass or less, preferably 0.5 to 10% by mass, and more preferably 0.5 to 6% by mass, from the viewpoint of transportation of the pulp raw material. If the solid content is too low, the pulp will not come into contact with the blade of the beating plate during beating, resulting in poor beating efficiency. Although the solid content may vary during mechanical treatments including beating, in the present invention, the solid content at the start of beating is referred to as the solid content in the beating process.

[0038] Dilution can be used as a method for adjusting the solid content concentration of the chemically modified pulp to 10% by mass or less. The pH of the chemically modified pulp to be subjected to the beating process is preferably 6 or more, more preferably 7 or more, from the viewpoint of ease of defibration. Methods for adjusting the pH to the above range include adding chemicals such as NaOH, KOH, and sodium bicarbonate, or reducing the amount of acidic chemicals added after chemical modification. The pH of the chemically modified pulp can vary during mechanical treatments including beating, but in the present invention, the pH at the start of beating is defined as the pH in the beating process.

[0039] The chemically modified pulp to be subjected to the beating process may be one that has been subjected to an alkali treatment. Any alkali, such as NaOH or KOH, can be used for this alkali treatment. When the chemically modified pulp used in the present invention is an anion-modified pulp, the terminal of the modified group becomes a Na type or the like by adding an alkali, and the repulsion between the fibers increases. Therefore, the electrostatic repulsion of the fibers can be utilized to efficiently carry out mechanical treatments such as beating, defibration, and fiber defibration.

[0040] The chemically modified pulp to be subjected to the beating process may be one that has been subjected to an acid treatment. When the chemically modified pulp used in the present invention is an anion-modified pulp, the acid treatment causes the terminal of the modifying group to become H-type, thereby reducing the affinity for water.

[0041] In addition, the manufacturing method of the present invention may include one or more mechanical treatment steps in which mechanical treatment is performed using a device other than the double disc refiner before or after the beating treatment step using the double disc refiner.

[0042] According to the present invention, the position of the fixed disk DA10 in the direction of rotation axis 14 relative to the rotating disk DM8 and the position of the fixed disk DB12 in the direction of rotation axis 14 relative to the rotating disk DM8 are controlled so that the clearance between the rotating disk DM8 and fixed disk DA10 of the double disk refiner, and the clearance between the rotating disk DM8 and fixed disk DB12 are set to predetermined values, thereby preventing the occurrence of metal touch and reducing the amount of metal contained in the produced microfibril cellulose.

[0043] In addition, in conventional double disc refiners, only one side of the fixed blade can be mechanically positioned, while the other side cannot be positioned, and the rotary blade is often in a state where it can move freely in the axial direction between the fixed blade on the motor side and the fixed blade on the cover side (floating disc), and when the monoflow method is adopted as the raw material flow method, it is difficult to balance the pressure on the raw material inlet side and the raw material outlet side in the beating chamber, and the rotary blade is biased toward one of the fixed blades. Furthermore, in conventional double disc refiners, the clearance state between the rotary blade and the fixed blade is not detected, so fine clearance adjustment is not possible, and there is a problem that metal touch occurs when the rotary blade and the fixed blade are packed together to a certain extent.

[0044] In the double disc refiner of the present invention, the position of the fixed disc DA10 in the direction of the rotation axis 14 relative to the rotating disc DM8, and the position of the fixed disc DB12 in the direction of the rotation axis 14 relative to the rotating disc DM8 are each controlled, so even when a monoflow method is adopted as the raw material flow method, the clearance between the rotating disc and the fixed disc can be finely adjusted, and the occurrence of metal touch can be prevented.

[0045] The chemically modified microfibril cellulose obtained by the manufacturing method of the present invention is made from chemically modified pulp and has functional groups on the fiber surface, and therefore has various functionalities derived from the functional groups. Therefore, the chemically modified microfibril cellulose obtained by the manufacturing method of the present invention can be used for various purposes, and can be used as a thickener, gelling agent, paste, food additive, excipient, paint additive, adhesive additive, abrasive, rubber / plastic compounding material, water retention material, shape retention agent, muddy water regulator, filter aid, overflow prevention agent, admixture, etc. in various fields where additives are generally used. Examples of such fields include food, beverages, cosmetics, medicine, papermaking, various chemical products, paints, sprays, agricultural chemicals, civil engineering, construction, electronic materials, flame retardants, household goods, adhesives, detergents, fragrances, lubricating compositions, etc. EXAMPLES

[0046] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.

[0047] Example 1 <Preparation of chemically modified pulp> 55 kg (bone-dry) of bleached unbeaten kraft pulp (brightness 85%: Nippon Paper Industries Co., Ltd.) derived from conifers was added to 5500 L of an aqueous solution containing 429 g (0.05 mmol per 1 g of bone-dry cellulose) of TEMPO (Sigma Aldrich) and 5654 g (1.0 mmol per 1 g of bone-dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. Aqueous sodium hypochlorite solution was added to the reaction system so that the sodium hypochlorite concentration was 5.5 mmol / g, and the oxidation reaction was started at room temperature. The pH of the system decreased during the reaction, but 3 M aqueous sodium hydroxide solution was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. After adding hydrochloric acid to the reaction mixture to adjust the pH to 2, the pulp was thoroughly washed by repeated dehydration and dilution with water, and finally dehydrated until the pulp solids concentration reached 20% by mass to obtain a chemically modified pulp (TEMPO oxidized pulp). The pulp yield was 90%, and the carboxyl group content was 1.45 mmol / g.

[0048] The obtained TEMPO oxidized pulp was dispersed in tap water, sodium hydroxide was added, and the mixture was stirred to obtain an aqueous dispersion of TEMPO oxidized pulp with a pH of 7.6 and a solid content of 1.2% by mass.

[0049] <Beating> 1000 kg of the obtained aqueous dispersion of TEMPO oxidized pulp was beaten using a double disc refiner (new DDR: AWU20 (raw material flow method: monoflow type) manufactured by Aikawa Iron Works Co., Ltd.) for 30 minutes under conditions of a clearance of 0.03 mm and a circulation rate of 90.9%, and the TEMPO oxidized pulp was obtained as MFC. The number of passes in the beating process was 3 (actual number of passes: 65.9). The MFC was evaluated by the method described below. The results are shown in Table 1.

[0050] Example 2 The beating time by the double disc refiner was changed to 20 minutes, and the number of passes of the beating process was changed to two (actual number of passes: 44), but the beating process was performed in the same manner as in Example 1 to obtain an MFC. The MFC was evaluated by the method described below. The results are shown in Table 1.

[0051] Example 3 An MFC was obtained by beating in the same manner as in Example 1, except that the solid content concentration of the aqueous dispersion of TEMPO oxidized pulp beaten by a double disc refiner was changed to 1.0 mass%, the circulation rate was 72.7%, the beating time was 7 minutes, and the number of passes of the beating was 1 (actual number of passes: 7.3). The MFC was evaluated by the method described below. The results are shown in Table 1.

[0052] Example 4 An MFC was obtained by beating in the same manner as in Example 1, except that the solid content concentration of the aqueous dispersion of TEMPO oxidized pulp beaten by a double disc refiner was changed to 1.0 mass%, the circulation rate was 0%, the beating time was 7 minutes, and the number of passes of the beating was 1 (actual number of passes: 2). The MFC was evaluated by the method described below. The results are shown in Table 1.

[0053] Comparative Example 1 Chemically modified pulp (TEMPO oxidized pulp) was obtained in the same manner as in Example 1. The amount of carboxyl groups was 1.36 mmol / g. This TEMPO oxidized pulp was dispersed in tap water, and sodium hydroxide was added and stirred to obtain an aqueous dispersion of TEMPO oxidized pulp with a pH of 7.7 and a solid content of 1.1% by mass. 3,000 kg of the obtained aqueous dispersion of TEMPO oxidized pulp was beaten using a double disc refiner (conventional DDR: AWN20 (raw material flow method: monoflow type)) for 45 minutes at a clearance of 0.03 mm and a circulation rate of 75.5%, to produce TEMPO oxidized pulp as MFC. The number of passes in the beating process was two (actual number of passes: 16.3). The MFC was evaluated using the method described below. The results are shown in Table 1.

[0054] Comparative Example 2 The beating time by the double disc refiner was changed to 90 minutes, and the number of passes of the beating process was changed to 4 (actual number of passes: 32.7), but the beating process was performed in the same manner as in Comparative Example 1 to obtain an MFC. The MFC was evaluated by the method described below. The results are shown in Table 1.

[0055] Comparative Example 3 Chemically modified pulp (TEMPO oxidized pulp) was obtained in the same manner as in Example 1. The amount of carboxyl groups was 1.45 mmol / g. This TEMPO oxidized pulp was dispersed in tap water, and sodium hydroxide was added and stirred to obtain an aqueous dispersion of TEMPO oxidized pulp with a pH of 7.6 and a solid content of 1.2% by mass.

[0056] 1000 kg of the obtained aqueous dispersion of TEMPO oxidized pulp was beaten using a double disc refiner (conventional DDR: AWN20 (raw material flow method: duo-flow type)) for 15 minutes under conditions of a clearance of 0.03 mm and a circulation rate of 0%, to obtain TEMPO oxidized pulp as MFC. The number of passes in the beating process was 3 (actual number of passes: 3.0). The MFC was evaluated using the method described below. The results are shown in Table 1.

[0057]

Table 1

[0058] The physical properties and characteristics were evaluated as follows. <Average fiber length, average fiber width> The slurry of microfibrillated cellulose was diluted with water so that the solid content concentration became 0.25%, and about 250 g each (50 g of which was used for measurement) were passed through the fractionator twice under the conditions of a flow rate of 5.7 L / min, a water temperature of 25 ± 1 °C, and a total effluent volume of 22 L. Approximately 2000 images of the microfibrillated cellulose classified by flow rate were acquired inside the apparatus using the CCD camera attached to the fractionator. The fiber analysis parameters of the analysis software IMG (Metso) were set as shown in Tables 2 to 4, and the approximately 2000 acquired images were analyzed to obtain data such as average fiber length · average fiber width and fiber length distribution. The average value obtained from two measurements and analyses was adopted as the measurement data.

[0059]

Table 2

[0060]

Table 3

[0061]

Table 4

[0062] <BET specific surface area> The BET specific surface area was measured by the following method with reference to the nitrogen gas adsorption method (JIS Z 8830): (1) To the treated dispersion, ion-exchanged water was added as necessary to prepare an approximately 2% slurry (dispersion medium: water), and this was separated into approximately 0.1 g of solids and placed in a centrifuge container, to which 100 mL of ethanol was added. (2) A stirrer was added and the mixture was stirred at 500 rpm for at least 30 minutes. (3) The stirrer was removed, and the fibrillated chemically modified cellulose fibers were sedimented in a centrifuge at 7,000 G for 30 minutes at 30°C. (4) The supernatant was removed while trying to avoid removing as much of the fibrillated chemically modified cellulose fibers as possible. (5) 100 mL of ethanol was added, a stir bar was added, and the mixture was stirred under the conditions of (2), centrifuged under the conditions of (3), and the supernatant was removed under the conditions of (4). This process was repeated three times. (6) The solvent in (5) was changed from ethanol to t-butanol, and the stirring, centrifugation, and removal of the supernatant were repeated three times in the same manner as in (5) at room temperature above the melting point of t-butanol. (7) After the final solvent removal, 30 mL of t-butanol was added and mixed gently, then transferred to a recovery flask and frozen in an ice bath. (8) Cool in the freezer for at least 30 minutes. (9) The mixture was attached to a freeze-dryer and freeze-dried for 3 days. (10) BET measurements were performed using a BET measurement device (Micromeritics) (pretreatment conditions: 2 hours at 105°C under nitrogen flow, relative pressure of 0.01 to 0.30, sample amount of approximately 30 mg).

[0063] <Viscosity> Ion-exchanged water was added to the treated dispersion to prepare a 1% by mass slurry, which was then left to stand at 25°C for 3 hours and then stirred for 5 minutes using a PRIMIX homodisper (3000 rpm). Immediately after stirring, the viscosity was measured after 3 minutes at a rotation speed of 60 rpm using a B-type viscometer (TOKI SANGYO CO., LTD.) with an appropriate rotor.

[0064] <Transparency> An aqueous dispersion of microfibril cellulose (solid content 1% (w / v), dispersion medium: water) was prepared, and the transmittance of light with a wavelength of 660 nm was measured using a UV-VIS spectrophotometer UV-1800 (Shimadzu Corporation) with a square cell with an optical path length of 10 mm.

[0065] <Electrical conductivity> An aqueous dispersion of microfibril cellulose was prepared so that the sample concentration was 1.0% by mass, and the conductivity was measured at pH 6 using a portable electrical conductivity meter manufactured by Horiba.

[0066] <X-ray fluorescence measurement> Each of the obtained aqueous dispersions (compositions) of microfibril cellulose was adjusted to a solid content concentration of 1% by mass, and then a smooth PET film was spread on a horizontal surface, 100 g of the aqueous dispersion composition was evenly spread on the PET film, and dried overnight using a blower dryer (105°C). The obtained web-like material was peeled off from the PET film to obtain an MFC sheet.

[0067] The obtained MFC sheet was cut into a size of about 2 cm square, and fluorescent X-ray measurement was performed using an energy dispersive X-ray fluorescence analyzer EDX-8000 (Shimadzu Corporation). The irradiation diameter was 5 mm, and the measurement was performed in a vacuum atmosphere. The compound form was considered to be metallic, and the intensity (cps / μA) of the iron and potassium elements contained in the MFC sheet was obtained. Each measurement was performed twice to calculate the average value, and this was used as the intensity X derived from iron atoms. Fe and the intensity X from potassium atoms K It was decided.

[0068] As can be seen from Example 1, Example 2, Comparative Example 2, and Comparative Example 3 in Table 1, in Comparative Example 1 and Comparative Example 2, metal touch occurred, so that the X-ray fluorescence measurement Fe / X k The value of X is large in Example 1 and Example 2. Fe / X k The small value of indicates that metal touch is prevented. In addition, the double disc refiner of Example 1 in Table 1 is of the monoflow type, so the material passes between the blades twice before passing through the device once, whereas the double disc refiner of Comparative Example 3 is of the duoflow type, so the material passes between the blades once before passing through the device once (when the circulation rate is 0%). Therefore, it can be seen that the monoflow type makes it easier to proceed with processing using a single device. Also, from Examples 3 and 4 in Table 1, it can be seen that when the circulation rate is higher, the processing progresses more easily even with the same number of passes. [Explanation of symbols]

[0069] 2...Double disc refiner, 4...Raw material inlet, 6...Beating chamber, 8...Rotary disc DM, 10...Fixed disc DA, 12...Fixed disc DB, 14...Drive shaft, 16...Motor, 18...Circulation pipe, 20...Discharge port, 22...Outlet pipe, 24...Manual valve, 26...First sensor, 28...Second sensor, 30...First drive unit, 32...Second drive unit, 40...Control unit

Claims

1. A method for producing microfibril cellulose from a pulp raw material using a double disc refiner, comprising the steps of: A beating process in which the pulp raw material is beaten by the double disc refiner; A method for producing microfibril cellulose, comprising a control step, carried out during the beating step, of controlling a clearance between a first movable fixed blade and a second movable fixed blade, the first movable fixed blade and the rotor, the first movable fixed blade and the rotor being fixed in the direction of a rotation shaft.

2. The control step includes a detection step of detecting a clearance between the rotor and the first movable fixed blade and a clearance between the rotor and the second movable fixed blade; 2. The method for producing microfibril cellulose according to claim 1, further comprising a moving step of moving the first movable fixed blade and the second movable fixed blade in the direction of the rotation axis so that the clearance between the first movable fixed blade and the rotor becomes a predetermined clearance based on a detection result from the detection step.

3. The method according to claim 1 or 2, wherein the predetermined clearance is 0.01 mm to 0.5 mm. A method for producing microfibril cellulose.

4. 3. The method for producing microfibril cellulose according to claim 1 or 2, wherein the flow mode of the pulp raw material in the double disc refiner is a monoflow mode.

5. The method for producing microfibril cellulose according to claim 1 or 2, wherein the concentration of the pulp raw material beaten in the double disc refiner is 0.5% to 10%.

6. A rotor fixed in the direction of a rotation axis; a first movable fixed blade and a second movable fixed blade provided on either side of the rotor in the direction of the rotation axis; a control unit that moves the first movable fixed blade and the second movable fixed blade in the rotation axis direction to control a clearance between the rotor and the first movable fixed blade; A double disc refiner equipped with

7. The control unit includes a detection unit that detects a clearance between the first movable fixed blade and the rotor and a clearance between the second movable fixed blade and the rotor; a drive unit that moves the first movable fixed blade and the second movable fixed blade in the direction of the rotation axis so that a clearance between the first movable fixed blade and the rotor becomes a predetermined clearance based on a detection result by the detection unit; The double disc refiner of claim 6 comprising:

8. The double disc refiner according to claim 6 or claim 7, wherein the predetermined clearance is between 0.01 mm and 0.5 mm.

9. 8. The double disc refiner according to claim 6 or claim 7, wherein the flow mode of the pulp material is a monoflow mode.

10. The double disc refiner according to claim 6 or claim 7, further comprising a circulation pipe for circulating the beaten pulp material to the beating chamber.

Citation Information

Patent Citations

  • Method of controlling double disk refiner

    JP2003112069A