cBN SINTERED COMPACT

The cBN sintered body with controlled Ti-containing and Ti-free borides and Al nitride ratios enhances wear resistance and chipping resistance, addressing the limitations of existing cBN tools for high-speed cutting of high-hardness steel.

JP2024138951AInactive Publication Date: 2024-10-09MITSUBISHI MATERIALS CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023049687
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing cubic boron nitride (cBN) sintered bodies used as cutting tools for high-hardness steel face challenges in wear resistance and chipping resistance during high-speed cutting, limiting their tool life.

Method used

A cBN sintered body composition comprising cubic boron nitride particles and a binder phase with specific ratios of Ti-containing and Ti-free borides and Al nitride, optimized to enhance toughness and wear resistance.

Benefits of technology

The optimized cBN sintered body exhibits improved wear resistance and chipping resistance, resulting in extended tool life during high-speed cutting of high-hardness steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138951000001_ABST
    Figure 2024138951000001_ABST
Patent Text Reader

Abstract

To provide a cBN sintered compact having improved abrasion resistance and chipping resistance even when used as a cutting tool for high-speed cutting of a high hardness steel.SOLUTION: In a cBN sintered compact having a cubic boron nitride particle and a binder phase, the binder phase includes: a Ti-containing boride; a boride which is formed by binding of boron with at least one of Zr, Hf, V, Nb, Ta, Cr, Mo and W and is Ti-free; and an Al nitride. When representing an area ratio (%) of the Ti-containing boride in the binder phase as Sa, representing an area ratio (%) of the Ti-containing boride in contact with the Ti-free boride in the binder phase as Sb, and representing an area ratio (%) of the Al nitride in the binder phase as Sc, the binder phase is 0.09≤Sb / Sa≤0.78 and 0.20≤Sc / Sa≤0.80.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sintered body of cubic boron nitride (hereinafter sometimes referred to as cBN), which is a hard composite material. [Background technology]

[0002] Although cBN sintered compacts are inferior to diamond in hardness, they have the property of low reactivity with Fe-based and Ni-based materials, and therefore are used as cutting tools. In order to improve the life of these cutting tools, various proposals have been made, such as controlling the content and grain size of Al compounds, and adding Ti compounds and Al compounds to the binder phase.

[0003] For example, Patent Document 1 describes a cBN sintered body containing 30 to 95 volume % cubic boron nitride, the balance being a boride solid solution containing Ti and an element of Groups 4 to 6 of the periodic table (excluding Ti), AlN, at least one selected from the group consisting of a carbide, nitride, and carbonitride of Ti, a carbide solid solution, a nitride solid solution, and a carbonitride solid solution containing Ti and an element of Groups 4 to 6 of the periodic table (excluding Ti), and unavoidable impurities; the binding phase of the cBN sintered body is said to be strengthened, and the wear resistance and toughness of the sintered body are improved.

[0004] Furthermore, for example, Patent Document 2 describes a cBN sintered body that is composed of 30 to 80 volume % cBN, with the remainder being a binder phase consisting of at least one of carbides, nitrides, borides, and oxides of elements in Groups 4 to 6 of the periodic table, nitrides and oxides of Al, carbides and nitrides of Si, and mutual solid solutions thereof, and unavoidable impurities, in which the binder phase contains: (1) 30 to 80 volume % of the entire binder phase of at least one composite compound selected from composite nitrides and composite carbonitrides consisting of at least one of V, Nb, and Ta and Ti; (2) 5 to 40 volume % of at least one orthorhombic boride selected from V, Nb, and Ta, based on the entire binder phase; (3) 5 to 30 volume % of AlN, based on the entire binder phase; and (4) 2 to 20 volume % of Al2O3, based on the entire binder phase. It is said that this cBN sintered body can achieve approximately twice the life in interrupted cutting of high-hardness steel compared to conventional cBN sintered bodies.

[0005] Furthermore, for example, Patent Document 3 describes a cBN sintered body having a cBN content of 60 to 80 volume %, a binder phase content of 20 volume % or more and 40 volume % or less, the binder phase containing more than 0 volume % and less than 5 volume % of at least one Al compound selected from the group consisting of Al oxides, nitrides and borides, and Ti nitride, wherein the length of the interface between the cBN and the Al compound in a cross section is a specific ratio to the length of the interface between the cBN and the binder phase, and the cBN sintered body is said to have improved wear resistance and chipping resistance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 8-91936 [Patent Document 2] Patent No. 4830571 [Patent Document 3] Patent No. 7047503 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in consideration of the above circumstances and proposals, and has an object to obtain a cBN sintered body that has excellent wear resistance and fracture resistance and improves the life of a cutting tool, even when used as a cutting tool for high-speed cutting of high-hardness steel, for example. [Means for solving the problem]

[0008] The cubic boron nitride sintered body according to the embodiment of the present invention is It has cubic boron nitride particles and a binder phase, the binder phase includes a boride containing Ti, a boride not containing Ti in which boron is bonded to at least one of Zr, Hf, V, Nb, Ta, Cr, Mo, and W, and an Al nitride; The area ratio (%) of the Ti-containing boride in the binder phase is Sa, the area ratio (%) of the Ti-containing borides in contact with the Ti-free borides in the binder phase is Sb; When the area ratio (%) of the Al nitride in the binder phase is Sc, 0.09≦Sb / Sa≦0.78 0.20≦Sc / Sa≦0.80 It is.

[0009] Moreover, the cubic boron nitride sintered body according to the above embodiment may satisfy the following condition (1).

[0010] (1) When the area ratio (%) of the borides not containing Ti in the binder phase is Sd, 0.5≦Sd≦20.0 is satisfied. Effect of the Invention

[0011] The cubic boron nitride sintered body has excellent wear resistance and chipping resistance when used as a cutting tool. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a schematic diagram showing an example of the structure of a cBN sintered body according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present inventors have conducted extensive research to achieve the above-mentioned object, and have found that, although dispersing borides in the binder phase can improve the toughness of a cBN sintered body to a certain degree, in order to further improve the toughness, it is preferable to control the dispersion form of the borides and also disperse Al nitrides.

[0014] Hereinafter, the cBN sintered body according to the embodiment of the present invention will be described in detail. In the present specification and claims, when a numerical range is expressed as "A to B" (A and B are both numerical values), this is equivalent to "A or more and B or less," and the range includes an upper limit (B) and a lower limit (A). The units of the upper limit and the lower limit are the same. In addition, the numerical values ​​contain measurement errors.

[0015] In this embodiment, as shown in FIG. 1, there are cBN particles (1) and a binder phase, and the binder phase contains binder phase particles (2), Ti-containing borides (3), Ti-free borides (4), and Al nitrides (5). In this embodiment, it may be considered that there is substantially no component other than the cubic boron nitride particles and the binder phase.

[0016] 1. Cubic boron nitride particles The average particle size of cubic boron nitride particles (sometimes called cBN particles) and the content ratio of cBN particles in a cBN sintered compact will be described below.

[0017] (1) Average particle size The average particle size of the cBN particles used in this embodiment is not particularly limited, but is preferably in the range of 0.5 to 8.0 μm.

[0018] The reason is that, in addition to the fact that the inclusion of cBN particles in the sintered body enhances the chipping resistance, if the average particle size is 0.5 to 8.0 μm, when used as a cutting tool, not only chipping caused by the uneven shape of the cutting edge caused by the falling off of cBN particles on the tool surface is more reliably suppressed, but also the propagation of cracks that develop from the interface between the cBN particles and the binder phase caused by the stress applied to the cutting edge during cutting, or cracks that develop as the cBN particles break, is more suppressed, resulting in better chipping resistance. The average particle size is more preferably 2.0 to 6.0 μm, and even more preferably 3.0 to 5.0 μm.

[0019] (2) Measurement method for average particle size Here, the average particle size of the cBN particles can be determined by the following steps 1) to 5). 1) The surface or cross section of the cBN sintered body is mirror-finished, and the structure of the mirror-finished surface is observed using a scanning electron microscope (SEM) to obtain a secondary electron image. Next, the cBN grains in the obtained image are extracted using image processing.

[0020] 2) Here, when extracting the cBN particle portion of the image by image processing, in order to clearly distinguish between the cBN particles and the binder phase, a binarization process is performed by setting the brightness value of the cBN particles to 0 and the brightness values ​​of the other portions to 255. The threshold value in the binarization process should be set so that the cBN particles can be clearly distinguished from other portions.

[0021] 3) After the binarization process, a process is performed to separate areas where cBN grains are thought to be in contact with each other, for example, watershed processing is used to separate cBN grains that are thought to be in contact with each other.

[0022] 4) The areas (black areas) corresponding to the cBN particles in the obtained image are subjected to image analysis, and the maximum Feret diameter of each particle obtained is regarded as the diameter of each cBN particle.

[0023] 5) Assuming each cBN particle is an ideal sphere with this diameter, calculate the volume of each particle to find the cumulative volume, and plot a graph based on this cumulative volume with the volume percentage (%) on the vertical axis and the diameter (μm) on the horizontal axis, and take the diameter when the volume percentage is 50% as the average diameter of the cBN particles. This is done for any three or more observation areas, and the average value is taken as the average diameter (μm) of the cBN particles.

[0024] When performing this particle analysis, the length per pixel (μm) is set using the scale value known in advance from the SEM. As the observation area used for image processing, when the average particle size of the cBN particles is about 4.0 μm, a viewing area of ​​about 40 μm (vertical) × 40 μm (horizontal) is preferable.

[0025] The binarization process, watershed image processing, and measurement of maximum Feret's diameter may be performed using the same image processing software, or each may be performed using different image processing software. There are no particular restrictions on the image processing software used, but for example, Image J can be used.

[0026] (3)Content ratio The content (area %) of cBN particles in the cBN sintered compact is not particularly limited, but is preferably 40 to 80 area %.

[0027] The reason is that if the content is less than 40% by area, the hard material in the cBN sintered body is small, and when used as a cutting tool, the chipping resistance may decrease, while if the content exceeds 80% by area, voids that become the starting points of cracks are generated in the cBN sintered body, and the chipping resistance may decrease.The content of cBN particles is more preferably 50 to 75% by area. Here, this area % can be treated as being equivalent to the volume % by assuming that the same area % exists in the thickness direction of the surface where the area was measured, but is expressed as an area %.

[0028] (4) Method for measuring content The cBN content is determined as follows. As in the case of determining the average grain size of cBN particles, the mirror-finished surface or cross section of the cBN sintered body is observed with an SEM (for example, at 5000x magnification), and the cBN particle portion within the observation area is extracted using a binarization process with image processing software. After the binarization process, a process is performed to separate the portions where the cBN particles are thought to be in contact with each other, for example, watershed image processing is used to separate the cBN particles that are thought to be in contact with each other, and the area occupied by the cBN particles is calculated to determine the area ratio of the cBN particles in the observation area. This is performed for any three or more observation areas, and the average of the values ​​determined for each observation area is taken as the cBN particle content ratio.

[0029] The size of the observation area is preferably the same as that when determining the average particle size of cBN particles. The area ratio occupied by cBN can also be determined using image processing software, and binarization, watershed image processing, and area ratio can be performed using the same image processing software or different software.

[0030] 2. Bonded phase (1) Ingredients The binder phase contains a boride containing Ti, a boride not containing Ti (which may contain a composite boride) in which boron is bonded to at least one of Zr, Hf, V, Nb, Ta, Cr, Mo, and W, and an Al nitride. Examples of other components contained in the binder phase include one or more of an Al boride and oxide, and one or more of a Ti nitride, carbide, and carbonitride. These other components constitute the binder phase particles. Note that each of the borides, Al borides, oxides, and Ti nitrides, carbides, and carbonitrides also contain unavoidable impurities, and the compositions of these compounds such as borides and oxides are not limited to stoichiometric compositions.

[0031] (2)Content ratio The content (area %) of the binder phase in the cBN sintered body is not particularly limited, but the content is treated as the balance of the content (area %) of the cBN particles, and is preferably 20 area % or more and 60 area % or less. The reason is that if the proportion of the binder phase is less than 20% by area, voids that can become the starting points of cracks are generated in the cBN sintered body, which can reduce the chipping resistance, while if it exceeds 60% by area, the amount of hard material in the cBN sintered body is small, which can reduce the chipping resistance when used as a cutting tool.The proportion of the binder phase is more preferably 25% or more and 50% or less by area.

[0032] (3) Borides containing Ti The Ti-containing borides in the binder phase are present at an area ratio (%) Sa relative to the entire binder phase, and when the area ratio (%) of the Ti-containing borides in contact with the Ti-free borides described below in the binder phase is Sb, it is preferable that Sb / Sa is 0.09 or more and 0.78 or less.

[0033] The reason for this is that if the Sb / Sa ratio is less than 0.09, there will be too few Ti-containing borides around the Ti-free borides, reducing the toughness of the binder phase; on the other hand, if it exceeds 0.78, there will be too few Ti-containing borides at the interface between the cBN and the binder phase, reducing the strength of this interface against shear stress, causing cBN grain shedding during cutting, and reducing the wear resistance. The contact with the boride not containing Ti will be explained later.

[0034] (4) Borides not containing Ti Borides (which may include composite borides) not containing Ti in which boron is bonded to at least one of Zr, Hf, V, Nb, Ta, Cr, Mo, and W in the binder phase are present at an area ratio (%) Sd relative to the entire binder phase, and Sd is more preferably 0.5 area % or more and 20.0 area % or less. The reason is that when Sd is less than 0.5% by area, the amount of Ti-free borides, which have excellent toughness, and the amount of Ti-containing borides generated after sintering are insufficient, so that the wear resistance and chipping resistance of the binder phase are sometimes insufficient, and cracks generated during cutting are less likely to reach the Ti-free borides, so that crack propagation cannot be sufficiently suppressed and the toughness of the binder phase may decrease. On the other hand, when Sd exceeds 20.0% by area, the amount of Ti-free borides becomes excessive, and the toughness may decrease.

[0035] (5) Aluminum nitride The Al nitride in the binder phase is present at an area ratio (%) Sc relative to the entire binder phase, and it is preferable that 0.20≦Sc / Sa≦0.80. There is no particular restriction on the absolute value of Sc, so long as Sc / Sa is within this range.

[0036] The reason is that if Sc / Sa is less than 0.20, the amount of Ti-containing borides will be excessive, or the amount of Al nitrides that are generated mainly at the interface between cBN and the binder phase during sintering will be insufficient, resulting in a decrease in toughness and a decrease in wear resistance due to a decrease in the strength of the interface between cBN and the binder phase; on the other hand, if it exceeds 0.80, the amount of Ti-containing borides will be insufficient or the amount of Al nitrides will be excessive, resulting in a decrease in the wear resistance and toughness of the binder phase.

[0037] (6)Measurement method Sa, Sb, Sc, and Sd are measured as follows.

[0038] 1) Set three or more square observation regions, each measuring, for example, 5 μm (vertical) × 5 μm (horizontal), that contain three or more borides that do not contain Ti and are to be identified by the method described below. When setting each observation region, select the observation region so that the cBN content is ±10% by area of ​​the cBN content calculated above. The centers of each observation region (intersections of the diagonals of the squares) are spaced apart by 100 μm or more.

[0039] 2) As mentioned above, cBN particles are specified, and the parts other than the cBN particles are regarded as the binder phase. The reason for this treatment is that, as mentioned above, it is acceptable to consider that nothing other than the cBN particles and the binder phase exists.

[0040] 3) For the binder phase identified in 2) above, a mapping image of the elements B, N, Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, and W is obtained by Auger electron spectroscopy, and a process is performed in which the region where Ti and B overlap is treated as a boride containing Ti, the regions where Zr, Hf, V, Nb, Ta, Cr, Mo, and W overlap with B are treated as a boride not containing Ti, and the region where Al and N overlap is treated as an Al nitride, and the interfaces between the borides containing Ti, the borides not containing Ti, and the Al nitride are defined.

[0041] 4) The area ratios Sa, Sd and Sc of the Ti-containing borides, Ti-free borides and Al nitrides identified in 3) above in the binder phase are calculated.

[0042] 5) A circle with a radius of 10 nm having its center on the interface of the boride not containing Ti defined in 3) above is moved along said interface, and for the borides containing Ti at least a part of which is present within this circle (this also applies to borides which are in contact with the circumference of the circle at a single point), the area of ​​the entire borides containing Ti is calculated, and the area fraction Sb of the total area of ​​the binder phase is calculated. That is, in this specification and claims, a boride containing Ti that is in contact with a boride not containing Ti means a boride containing Ti, at least a part of which is contained within this circle with a radius of 10 nm.

[0043] Here, the definition of the interface in 3) above and the calculation of the area ratios Sa, Sb, Sc and Sd can be easily performed by combining known image processing software (eg, Image J) with commercially available graphic drawing software. The area ratios Sa, Sb, Sc and Sd are calculated as the average values ​​of the measured values ​​obtained in the above-mentioned three or more observation regions.

[0044] 2.Coating layer When the cBN sintered body of this embodiment is used as a cutting tool, it may be coated with a known coating layer by a known method.

[0045] 3. Manufacturing method The cBN sintered body of this embodiment can be manufactured, for example, by the following procedure.

[0046] (1) Preparation of raw powders of binder phase components The main raw powders for the binder phase are Ti compound powders (e.g. TiC powder, TiN powder, TiCN powder, TiO2 powder), Al compound powders (e.g. TiAl3 powder, Al2O3 powder), As an auxiliary raw material for the binder phase, boride powder not containing Ti (e.g., ZrB2 powder, CrB2 powder, NbB2 powder, TaB2 powder) is prepared.

[0047] (2) Pre-grinding The binder phase auxiliary materials are filled into a container lined with cemented carbide together with cemented carbide balls and acetone, and pulverized in a ball mill. After pulverization, the resulting mixed slurry is dried and classified using a centrifuge to obtain pre-pulverized auxiliary component powder.

[0048] (3) Mixing and grinding of raw materials for the binder phase The pre-ground subcomponent powder (2) and the main raw material powder of the binder phase (1) are filled into a ball mill container lined with cemented carbide together with cemented carbide balls and acetone, and mixed and ground by a ball mill. This mixing and grinding by a ball mill is carried out for, for example, 4 hours or more until the pre-ground subcomponent powder is sufficiently mixed and ground with the main raw material powder. The obtained slurry is then dried to obtain a pre-sintered binder phase mixed raw material powder.

[0049] (4) Mixing and grinding with cBN powder The pre-sintering binder phase mixed raw material powder (3) is filled together with cBN powder, which is the raw material for the hard phase, into a ball mill container lined with cemented carbide, together with cemented carbide balls and acetone, and mixed and pulverized by a ball mill. The resulting slurry is then dried to obtain a pre-sintering mixed raw material powder.

[0050] (5) Molding and sintering The pre-sintered mixed raw material powder obtained in (4) above is molded under a predetermined pressure to produce a molded body, which is then pre-sintered at a predetermined temperature in a vacuum atmosphere, and then sintered in an ultra-high pressure sintering apparatus under predetermined conditions, for example, a pressure of 4 to 6 GPa and a temperature of 1200 to 1600°C, to produce the cBN sintered body of this embodiment. In addition, each step up to sintering is preferably carried out in a non-oxidizing protective atmosphere in order to prevent oxidation of the raw material powder. EXAMPLES

[0051] Next, examples will be described, but the present invention is not limited to the examples.

[0052] The examples were prepared according to the following procedure. (1) TiC powder, TiCN powder, TiN powder, and TiAl3 powder were prepared as main raw material powders for the binder phase, and ZrB2 powder, NbB2 powder, and TaB2 powder were prepared as auxiliary raw material powders for the binder phase. They were mixed in the ratios shown in Table 1.

[0053] (2) The powdered auxiliary raw material was packed into a container lined with cemented carbide together with cemented carbide balls and acetone, and pre-ground using a ball mill. The slurry was dried and classified using a centrifuge to obtain a pre-ground auxiliary component powder with an average particle size of 200 nm.

[0054] (3) The pre-ground auxiliary component powder (2) and the main raw material powder (1) were charged into a ball mill container lined with cemented carbide together with cemented carbide balls and acetone, and mixed and ground in a ball mill for 5 hours. The slurry was dried to obtain a pre-sintering binder phase mixed raw material powder.

[0055] (4) The pre-sintering binder phase mixed raw material powder (3) and cBN powder, which is the raw material for the hard phase, were charged into a lined container together with cemented carbide balls and acetone, and mixed and ground in a ball mill. The mixture was then dried to obtain a pre-sintering mixed raw material powder.

[0056] (5) The pre-sintered mixed raw material powder obtained in (4) above was press-molded at a molding pressure of 1 MPa to a size of 50 mm in diameter x 1.5 mm in thickness, and then this molded body was pre-sintered at 1000°C in a vacuum atmosphere with a pressure of 1 Pa or less. After the pre-sintering, high-pressure sintering was performed in an ultra-high-pressure sintering apparatus under conditions of a pressure of 6 GPa and a temperature of 1400°C, thereby obtaining Examples 1 to 7.

[0057] The above steps were carried out in a non-oxidizing atmosphere.

[0058] For comparison, a comparative example was prepared according to the following procedure. (1) TiC powder, TiCN powder, TiN powder, and TiAl3 powder were prepared as main raw material powders for the binder phase, and NbB2 powder and TaB2 powder were prepared as auxiliary raw material powders for the binder phase. These were mixed in the ratios shown in Table 1.

[0059] (2) The auxiliary raw material powders, NbB2 powder and TaB2 powder, were packed into a container lined with cemented carbide together with cemented carbide balls and acetone, and pre-grinding was carried out using a ball mill. The slurry was dried and classified using a centrifuge to obtain a pre-grinding auxiliary component powder with an average particle size of 200 nm.

[0060] (3) The pre-ground auxiliary component powder (2) and the main raw material powder (1) as raw materials for the binder phase, and cBN powder as raw material for the hard phase were charged into a ball mill container lined with cemented carbide together with cemented carbide balls and acetone, mixed and ground in a ball mill, and dried to obtain a pre-sintered mixed raw material powder.

[0061] (4) The pre-sintered mixed raw material powder of (3) was press-molded to a size of 50 mm in diameter and 1.5 mm in thickness at a molding pressure of 1 MPa, and then this molded body was pre-sintered at 1000°C in a vacuum atmosphere with a pressure of 1 Pa or less. After the pre-sintering, high-pressure sintering was performed in an ultra-high-pressure sintering apparatus under conditions of a pressure of 6 GPa and a temperature of 1400°C, thereby obtaining Comparative Examples 1' to 6'.

[0062] Each process for producing the comparative sintered body was also carried out in a non-oxidizing atmosphere.

[0063] The measurements were carried out for Examples 1 to 7 and Comparative Examples 1' to 6' as described above. First, SEM observation was performed, and the obtained secondary electron images were binarized by Otsu's binarization method using ImageJ (version 1.44p) as image processing software to determine the average cBN particle size, cBN area ratio, and bonded phase area ratio. Furthermore, each boride was identified using Auger electron spectroscopy, and Sa, Sb, Sc, and Sd were calculated using ImageJ (version 1.44p) in the same manner. The results are shown in Table 2.

[0064] [Table 1]

[0065] In Table 1, "-" indicates that no ingredient was added.

[0066] [Table 2]

[0067] In Tables 1 and 2, the compositions of the borides not containing Ti are representative compositions, and include those in which the metal component and boron are bonded with atomic ratios other than those shown.

[0068] Next, the above-prepared Examples 1 to 7 and Comparative Examples 1' to 6' were cut to specified dimensions using a wire EDM machine, and the brazing portions (corner portions) of the WC-based cemented carbide insert body having a composition of 5 mass% Co, 5 mass% TaC, and the remainder WC and an insert shape conforming to ISO standard CNGA120408 were brazed using Ag brazing material (having a composition of 26 mass% Cu, 5 mass% Ti, and the remainder Ag). The upper and lower surfaces and outer periphery were polished and honed to produce Example cutting tools 1 to 7 and Comparative Example cutting tools 1' to 6' having an insert shape conforming to ISO standard CNGA120408.

[0069] Next, a dry cutting test was carried out on the cutting tools 1 to 7 of the examples and the cutting tools 1' to 6' of the comparative examples under the following cutting conditions.

[0070] Dry cutting test conditions Work material: Carburized steel (JIS SCR420, hardness: HRC58~62) round bar Cutting speed: 200 m / min Cutting depth: 0.2 mm Feed: 0.1 mm / rev The tool life was defined as the time until chipping occurred, and the cutting edge was observed every 30 seconds of cutting time to check for the presence or absence of chipping on the cutting edge, and the cutting time until chipping occurred (referred to as "tool life (seconds)" in Table 3) was measured.

[0071] [Table 3]

[0072] As is clear from Table 3, the cutting tools of the examples are excellent in wear resistance and chipping resistance, and all have a long tool life in high-speed cutting of high-hardness steel, while the cutting tools of the comparative examples all reach the end of their life in a short period of time. [Explanation of symbols]

[0073] 1 cBN particle 2 Bonded phase particles 3. Borides containing Ti 4. Borides not containing Ti 5. Aluminum nitride

Claims

1. A cBN sintered body having cubic boron nitride particles and a binder phase, the binder phase includes a boride containing Ti, a boride not containing Ti in which boron is bonded to at least one of Zr, Hf, V, Nb, Ta, Cr, Mo, and W, and an Al nitride; The area ratio (%) of the Ti-containing boride in the binder phase is Sa, the area ratio (%) of the Ti-containing boride in contact with the Ti-free boride in the binder phase is Sb; When the area ratio (%) of the Al nitride in the binder phase is Sc, 0.09≦Sb / Sa≦0.78 0.20≦Sc / Sa≦0.80 A cBN sintered body characterized by:

2. 2. The cBN sintered body according to claim 1, wherein the area ratio (%) of the binder phase occupied by the borides not containing Ti is Sd, and 0.5≦Sd≦20.0 is satisfied.

Citation Information

Patent Citations

  • JP1973030571A

  • Sintered material of boron nitride of cubic system

    JP1996091936A

  • Cubic boron nitride sintered body and tool having cubic boron nitride sintered body

    JP7047503B2