Method for manufacturing electronic component, and temporary fixing material
A curable compound and gas generating agent-based temporary fixing material, applied via an inkjet device, addresses the challenge of shaping thick electrodes by enabling precise formation and easy peeling, suitable for electronic components.
Patent Information
- Application Number
- JP2023050010
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional methods struggle to form thick electrodes into desired shapes due to etching limitations, and existing temporary fixing materials lack versatility and effective peeling performance.
A method involving a temporary fixing material containing a curable compound and a gas generating agent, applied using an inkjet device, which is cured and then peeled off by stimulating gas generation, allowing for the formation of thick electrodes with precise shaping and easy removal.
Enables the formation of thick electrodes with desired shapes and facilitates easy peeling without damage, suitable for components like diodes, transistors, and ICs, with high adhesive strength and flexibility.
Smart Images

Figure 2024139181000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing an electronic component. The present invention also relates to a temporary fixing material. [Background technology]
[0002] During processing of electronic components such as semiconductors, in order to facilitate the handling of the electronic components and prevent them from being damaged, the electronic components are protected by fixing them to a support plate via a temporary fixing material made of a resin composition, or by attaching an adhesive tape made of a temporary fixing material having an adhesive layer containing a resin composition to the electronic components. For example, when a thick-film wafer cut from a high-purity silicon single crystal or the like is ground to a predetermined thickness to form a thin-film wafer, the thick-film wafer is adhered to a support plate via a temporary fixing material.
[0003] The temporary fixing material used for such electronic components is required to have high adhesiveness capable of firmly fixing the electronic components during the processing step, and also to be able to be peeled off without damaging the electronic components after the processing step is completed (hereinafter, also referred to as "high adhesion and easy peeling"). As a means for achieving high adhesion and easy peeling, for example, Patent Document 1 discloses an adhesive sheet using an adhesive in which a polyfunctional monomer or oligomer having a radiation-polymerizable functional group is bonded to the side chain or main chain of the polymer. By utilizing the fact that the polymer has a radiation-polymerizable functional group and is cured by exposure to ultraviolet light, the adhesive strength is reduced by exposure to ultraviolet light during peeling, allowing peeling without leaving any adhesive residue. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-32946 Summary of the Invention [Problem to be solved by the invention]
[0005] Conventionally, when manufacturing metal electrodes, a solid pattern electrode is first prepared, then a resist is applied, and the electrode is fabricated by photolithography, in which the electrode coated with the resist is exposed to light to develop a circuit pattern, and the fabricated electrode is then etched into the desired shape.
[0006] Meanwhile, power devices such as diodes, transistors, and ICs, which have come into widespread use in recent years, have required thick electrodes because of their large current capacity and voltage resistance. However, due to the constraints of etching, it was difficult to fabricate thick electrodes with the desired shape using conventional electrode manufacturing methods. Therefore, a new manufacturing method for electronic components capable of fabricating thick electrodes, and a new temporary fixing material that could be applied to the new manufacturing method, were needed.
[0007] The present invention provides a method for producing an electronic component, which is capable of forming an electrode into a desired shape even when the electrode is thick. The present invention also provides a temporary fixing material that is highly versatile for the shape of an adherend to be temporarily fixed and has excellent peeling performance. [Means for solving the problem]
[0008] Disclosure 1 is a method for producing electronic components, including a step (I) of applying a temporary fixing material containing a curable compound and a gas generating agent onto a substrate, a step (II) of curing the temporary fixing material by a stimulus (S1), and a step (III) of generating gas from the gas generating agent by a stimulus (S2) different from the stimulus (S1), thereby peeling off the temporary fixing material. Disclosure 2 relates to the method for producing an electronic component according to Disclosure 1, in which the temporary fixing material is applied using an inkjet device in step (I). The present disclosure 3 is a method for producing an electronic component according to the present disclosure 1 or 2, which includes, after the above step (I), a step (IV) of applying a wall material onto the above temporary fixing material. The present disclosure 4 is the method for producing an electronic component according to the present disclosure 3, wherein in the step (IV), the wall material is applied using an inkjet device. The present disclosure 5 is a method for producing an electronic component according to the present disclosure 3 or 4, including, after the above step (IV), a step (V) of forming a plating between the wall materials. The present disclosure 6 is a method for producing an electronic component according to the present disclosure 5, in which the plating has a thickness of 1 μm or more. The present disclosure 7 is the method for producing an electronic device according to the present disclosure 3, 4, 5 or 6, wherein in the step (III), the temporary fixing material and the wall material are simultaneously peeled off. The present disclosure 8 is a method for producing an electronic device according to the present disclosure 1, 2, 3, 4, 5, 6, or 7, wherein both of the stimulus (S1) and the stimulus (S2) are light. The present disclosure 9 is the method for manufacturing an electronic component according to the present disclosure 8, wherein the wavelength of the light of the stimulus (S1) is longer than the wavelength of the light of the stimulus (S2). The present disclosure 10 comprises a curable compound that is cured by a stimulus (S3) and a gas generating agent that generates a gas by a stimulus (S4) different from the stimulus (S3), the curable compound having a viscosity of 150 mPa s or less at 25°C, a 180° peel force against a silicon wafer after curing by the stimulus (S3) of 0.05 N / inch or more and 0.5 N / inch or less, and a tensile storage modulus at 25°C after curing by the stimulus (S3) of 1.0 × 10 8 It is a temporary fixing material with a strength of tensile strength of 100 Pa or more. Disclosure 11 is the temporary fixing material of Disclosure 10, in which the curable compound contains (meth)acrylate. Disclosure 12 is the temporary fixing material of Disclosure 11, in which the (meth)acrylate includes a urethane (meth)acrylate. Disclosure 13 is the temporary fixing material according to Disclosure 11 or 12, in which the (meth)acrylate contains a polyfunctional (meth)acrylate. Disclosure 14 is the temporary fixing material of Disclosure 10, 11, 12, or 13, which does not contain a solvent or has a solvent content of 1 mass% or less. Disclosure 15 is the temporary fixing material of Disclosures 10, 11, 12, 13, or 14, in which the degree of elongation after hardening due to the above-mentioned stimulus (S3) is 1% or more. Disclosure 16 is the temporary fixation material of Disclosures 10, 11, 12, 13, 14, or 15, wherein both the stimulus (S3) and the stimulus (S4) are light. Disclosure 17 is the temporary fixing material of Disclosure 16, wherein the stimulus (S3) is light having a longer wavelength than the stimulus (S4).
[0009] The present invention will be described in detail below.
[0010] The present inventors have studied a temporary fixing material containing a curable compound and a gas generating agent, by applying the temporary fixing material to a substrate, curing the temporary fixing material, and releasing the temporary fixing material by generating gas from the gas generating agent. As a result, they have found that even if the electronic component is thick, it is possible to form the electronic component into a desired shape, and have completed the present invention. By using the method for manufacturing electronic parts of the present invention, it is possible to create a high aspect ratio (thick even though it is narrow in width) hardened resin body by repeatedly applying resin using an inkjet device or the like and then curing it, and by using this as a mold to create metal plating, it is possible to form thick metal into the desired shape.
[0011] The method for producing an electronic component of the present invention includes a step (I) of applying a temporary fixing material containing a curable compound and a gas generating agent onto a substrate.
[0012] In the above step (I), examples of the method for applying the temporary fixing material include a method using a bar coater, a method using a dispenser, and a method using an inkjet device, among which a method using an inkjet device is preferred. By using an inkjet device, it becomes easier to prepare a cured product of the temporary fixing material that is thick even if it is narrow in width by repeatedly performing the above steps (I) and (II). As a result, when the cured product of the temporary fixing material is used as a mold to prepare a metal plating, it becomes possible to more easily form a thick metal in a desired shape.
[0013] The temporary fixing material is preferably liquid at 25° C. When the temporary fixing material is liquid at 25° C., an inkjet device can be more suitably used in the step (I), and the material can be more easily applied in any shape with high precision.
[0014] The preferred upper limit of the viscosity of the temporary fixing material at 25° C. is 150 mPa·s. The temporary fixing material has a viscosity of 150 mPa·s or less at 25° C., so that the temporary fixing material can be more suitably used in the inkjet device. A more preferable upper limit of the viscosity of the temporary fixing material at 25° C. is 100 mPa·s. Furthermore, the preferred lower limit of the viscosity of the temporary fixing material at 25° C. is 1 mPa·s. When the viscosity of the temporary fixing material at 25° C. is 1 mPa·s or more, the material can be ejected by an inkjet device, and therefore the inkjet device can be used more preferably. The more preferred lower limit of the viscosity of the temporary fixing material at 25° C. is 5 mPa·s. The viscosity of the temporary fixing material at 25° C. can be measured, for example, using a Brookfield viscometer under conditions of 25° C. and 25 rpm.
[0015] The temporary fixing material contains a curable compound. When the temporary fixing material contains a curable compound, the temporary fixing material can be cured by a stimulus (S1) described later.
[0016] The curable compound may be a photocurable compound that is cured by light or a thermosetting compound that is cured by heat. Among them, a photocurable compound is preferable from the viewpoint of easy control of curing in the step (II) described later, shortening the process time, and improving the work efficiency.
[0017] The curable compound preferably contains a (meth)acrylate. By including a (meth)acrylate in the curable compound, the 180° peel strength of the cured temporary fixing material from the silicon wafer can be adjusted to an appropriate range. As a result, the cured temporary fixing material has a more suitable adhesive strength. Furthermore, in the step (III) described below, the cured temporary fixing material can be more easily peeled off. In this specification, "(meth)acrylate" means acrylate or methacrylate.
[0018] The (meth)acrylate preferably contains urethane (meth)acrylate. When the (meth)acrylate contains urethane (meth)acrylate, the elongation of the temporary fixing material after curing, which will be described later, can be more easily adjusted to an appropriate range. As a result, in the step (III) described later, the temporary fixing material after curing can be more easily peeled off.
[0019] The urethane (meth)acrylate can be obtained, for example, by reacting an isocyanate compound with a (meth)acrylic acid derivative having a hydroxyl group in the presence of a catalytic amount of a tin compound.
[0020] Examples of the isocyanate compound that is a raw material for the urethane (meth)acrylate include isophorone diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, diphenylmethane-4,4'-diisocyanate (MDI), hydrogenated MDI, polymeric MDI, 1,5-naphthalene diisocyanate, norbornane diisocyanate, tolidine diisocyanate, xylylene diisocyanate (XDI), hydrogenated XDI, lysine diisocyanate, triphenylmethane triisocyanate, tris(isocyanatephenyl)thiophosphate, tetramethylxylylene diisocyanate, and 1,6,11-undecane triisocyanate.
[0021] As the isocyanate compound serving as a raw material for the urethane (meth)acrylate, a chain-extended isocyanate compound obtained by reacting a polyol with an excess of an isocyanate compound can also be used. Examples of the polyol include ethylene glycol, propylene glycol, glycerin, sorbitol, trimethylolpropane, carbonate diol, polyether diol, polyester diol, and polycaprolactone diol.
[0022] Examples of the (meth)acrylic acid derivative having a hydroxyl group include hydroxyalkyl mono(meth)acrylates, mono(meth)acrylates of dihydric alcohols, mono(meth)acrylates or di(meth)acrylates of trihydric alcohols, and epoxy (meth)acrylates. Examples of the hydroxyalkyl mono(meth)acrylate include 2-hydroxyethyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, 2-hydroxybutyl(meth)acrylate, and 4-hydroxybutyl(meth)acrylate. Examples of the dihydric alcohol include ethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, and polyethylene glycol. Examples of the trihydric alcohol include trimethylolethane, trimethylolpropane, and glycerin. The epoxy (meth)acrylate may, for example, be bisphenol A type epoxy acrylate.
[0023] When the curable compound contains the urethane (meth)acrylate, the preferred lower limit of the content of the urethane (meth)acrylate in 100 parts by mass of the curable compound is 20 parts by mass, and the preferred upper limit is 90 parts by mass. When the content of the urethane (meth)acrylate is within such a range, the elongation degree of the temporary fixing material after curing, which will be described later, can be easily adjusted to an appropriate range. As a result, in the step (III) described later, the temporary fixing material after curing can be more easily peeled off. The more preferred lower limit of the content of the urethane (meth)acrylate is 40 parts by mass, and the more preferred upper limit is 60 parts by mass.
[0024] The (meth)acrylate may include a monofunctional (meth)acrylate having one (meth)acryloyloxy group, or may include a polyfunctional (meth)acrylate having a plurality of (meth)acryloyloxy groups. Among them, the (meth)acrylate preferably includes a polyfunctional (meth)acrylate. By including a polyfunctional (meth)acrylate in the (meth)acrylate, the 180° peel strength of the cured temporary fixing material from the silicon wafer can be easily adjusted to an appropriate range, so that the cured temporary fixing material has a more suitable adhesive strength. In addition, the tensile storage modulus of the cured temporary fixing material can be easily adjusted to an appropriate range, so that the adhesiveness of the cured temporary fixing material to the adherend is improved. As a result, in the step (III) described below, the gas generated by the gas generating agent can be retained by the adhesive surface, so that the cured temporary fixing material can be more easily peeled off. In this specification, "(meth)acryloyloxy" means acryloyloxy or methacryloyloxy.
[0025] The upper limit of the number of the (meth)acryloyloxy groups in the polyfunctional (meth)acrylate is preferably 6. By making the number of the (meth)acryloyloxy groups 6 or less, it becomes easier to adjust the viscosity of the (meth)acrylate at 25°C to an appropriate range. The upper limit of the number of the (meth)acryloyloxy groups is preferably 4, and more preferably the number of the (meth)acryloyloxy groups is 2.
[0026] Examples of the polyfunctional (meth)acrylate include tricyclodecane dimethanol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, etc. The curable compound may contain the urethane (meth)acrylate as the polyfunctional (meth)acrylate.
[0027] Examples of the monofunctional (meth)acrylate include ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc. The curable compound may contain the urethane (meth)acrylate as the monofunctional (meth)acrylate.
[0028] The (meth)acrylate may have, in addition to a (meth)acryloyloxy group, a functional group other than the (meth)acryloyloxy group.
[0029] The lower limit of the content of the (meth)acrylate in 100 parts by mass of the curable compound is preferably 30 parts by mass. When the content of the (meth)acrylate is 30 parts by mass or more, the 180° peel strength of the cured temporary fixing material from the silicon wafer, which will be described later, can be easily adjusted to an appropriate range. As a result, the cured temporary fixing material has a more suitable adhesive strength. Furthermore, in the step (III) described later, the cured temporary fixing material can be more easily peeled off. The lower limit of the content of the (meth)acrylate is more preferably 40 parts by mass, and even more preferably 50 parts by mass. From the viewpoint of ease of peeling from the adherend, the upper limit of the content of the (meth)acrylate is preferably 80 parts by mass.
[0030] The temporary fixing material preferably further contains a polymerization initiator. By including a polymerization initiator in the temporary fixing material, the curable compound reacts with the polymerization initiator in response to the stimulus (S1), and the temporary fixing material can be cured more easily.
[0031] The polymerization initiator may be a photopolymerization initiator or a thermal polymerization initiator. However, a photopolymerization initiator is preferred from the viewpoint of improving the work efficiency by making it easier to control the curing and shortening the process time in the step (II) described later.
[0032] The photopolymerization initiator is preferably a compound having an absorption edge on the long wavelength side of 600 nm or less. When the photopolymerization initiator has an absorption edge on the long wavelength side of 600 nm or less, the generation of gas from the gas generating agent described below can be further suppressed in the step (II) described below, and the temporary fixing material after curing can be more easily peeled off from the adherend in the step (III) described below. In this specification, the "absorption edge on the long wavelength side" means the wavelength on the longest wavelength side among the wavelengths at which the photopolymerization initiator absorbs when the absorption spectrum of the photopolymerization initiator is measured (for example, a solution is prepared using a solvent that has no absorption in the wavelength region at which the photopolymerization initiator absorbs, and the absorption spectrum of the solution is measured using a spectrophotometer).
[0033] Examples of the photopolymerization initiator include oxime ester compounds, acetophenone derivatives, benzophenone derivatives, and thioxanthone derivatives.
[0034] Examples of the oxime ester compound include Adeka Arcles NCI-730 (manufactured by Adeka Corporation), Omnirad OXE03, Omnirad OXE04, and Omnirad 1312 (all manufactured by IGM Resins). Examples of the acetophenone derivatives include Omnirad 184, Omnirad 907, and Omnirad 651 (all manufactured by IGM Resins). Examples of the benzophenone derivatives include Omnirad EMK, Omnirad BP, and Omnirad 4MBZ (all manufactured by IGM Resins). The thioxanthone derivatives include, for example, Omnirad DETX (manufactured by IGM Resins).
[0035] The thermal polymerization initiator is preferably a compound having a decomposition temperature of 100° C. or more and 200° C. or less. When the decomposition temperature of the thermal polymerization initiator is within the above range, the generation of gas from the gas generating agent described below can be further suppressed in the step (II) described below, and the hardened temporary fixing material can be more easily peeled off from the adherend in the step (III) described below.
[0036] The thermal polymerization initiator may, for example, be a peroxide compound.
[0037] Examples of the peroxide compound include Luperox 270, Luperox 7, Luperox P, Luperox 555, and Luperox TAP (all manufactured by Arkema).
[0038] The preferred lower limit of the content of the polymerization initiator relative to 100 parts by mass of the curable compound is 0.1 parts by mass, and the preferred upper limit is 20 parts by mass. By having the content of the polymerization initiator within the above range, it becomes easier to adjust the 180° peel force from the silicon wafer after the temporary fixing material has been cured, the tensile storage modulus at 25°C after the temporary fixing material has been cured, and the elongation degree after the temporary fixing material has been cured, which will be described later, within appropriate ranges. The more preferred lower limit of the content of the polymerization initiator is 1 part by mass, and the more preferred upper limit is 15 parts by mass.
[0039] The temporary fixing material further contains a gas generating agent. By including a gas-generating agent in the temporary fixing material, gas generated from the gas-generating agent is released to the adhesive surface by stimulation (S2) in step (III) described below, and the hardened temporary fixing material can be easily peeled off.
[0040] The gas generating agent may be a photo-generated gas generating agent that generates gas by irradiation with light, or a thermal gas generating agent that generates gas by heating. Among them, a photo-generated gas generating agent is preferred from the viewpoint of improving the working efficiency by making it easier to control the gas generation and shortening the process time in the step (III) described later.
[0041] The photo-gas generating agent is preferably a compound having an absorption edge on the long wavelength side of 450 nm or less. By using the photo-gas generating agent having an absorption edge on the long wavelength side of 450 nm or less, the generation of gas from the photo-gas generating agent can be further suppressed in the step (II) described below, and the temporary fixing material after hardening can be more easily peeled off in the step (III) described below.
[0042] Examples of the photo gas generator include azo compounds, azide compounds, carbonates, and tetrazole compounds. Among them, the azo compounds 2,2'-azobis(N-cyclohexyl-2-methylpropionamide), 2,2'-azobis[N-(2-methylpropyl)-2-methylpropionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), 2,2'-azobis[N-(2-methylethyl)-2-methylpropionamide], 2,2'-azobis(N-hexyl-2-methylpropionamide), 2,2'-azobis(N-propyl-2-methylpropionamide), and 2,2'-azobis(N-ethyl-2-methylpropionamide) are preferred.
[0043] The thermal gas generating agent is preferably a compound having a decomposition temperature of 100° C. or more and 300° C. or less. When the decomposition temperature of the thermal gas generating agent is within the above range, the generation of gas from the thermal gas generating agent can be further suppressed in the step (II) described below, and the hardened temporary fixing material can be more easily peeled off in the step (III) described below.
[0044] Examples of the above-mentioned thermal gas generating agent include azo compounds, azide compounds, carbonates, and tetrazole compounds.Among them, the azo compounds 2,2'-azobis(N-cyclohexyl-2-methylpropionamide), 2,2'-azobis[N-(2-methylpropyl)-2-methylpropionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), 2,2'-azobis[N-(2-methylethyl)-2-methylpropionamide], 2,2'-azobis(N-hexyl-2-methylpropionamide), 2,2'-azobis(N-propyl-2-methylpropionamide), and 2,2'-azobis(N-ethyl-2-methylpropionamide) are preferred.
[0045] The preferred lower limit of the content of the gas generating agent relative to 100 parts by mass of the curable compound is 5 parts by mass, and the preferred upper limit is 50 parts by mass. When the content of the gas generating agent is 5 parts by mass or more, the temporary fixing material after curing can be more easily peeled off in the step (III) described below. When the content of the gas generating agent is 50 parts by mass or less, the temporary fixing material after curing can maintain sufficient adhesive strength. The more preferred lower limit of the content of the gas generating agent is 10 parts by mass, and the more preferred upper limit is 30 parts by mass.
[0046] The temporary fixing material preferably does not contain a solvent or has a solvent content of 1 mass % or less. By the temporary fixing material not containing a solvent or having a solvent content of 1 mass % or less, it is possible to prevent the solvent from seeping out during the process in the method for producing an electronic component of the present invention, thereby preventing a decrease in the efficiency of the production process. When the temporary fixing material contains a solvent, the upper limit of the content of the solvent is more preferably 0.1 mass %. It is most preferable that the temporary fixing material does not contain a solvent.
[0047] The temporary fixing material may contain additives such as a plasticizer, an emulsifier, a softener, a filler, a pigment, a dye, a silane coupling agent, and an antioxidant, if necessary.
[0048] Examples of a method for producing the temporary fixing material include a method in which the curable compound and the gas generating agent, as well as the polymerization initiator and additives that are blended as necessary, are mixed using a bead mill, ultrasonic dispersion, homogenizer, high-output disperser, roll mill, or the like.
[0049] The method for producing an electronic component of the present invention includes a step (II) of curing the temporary fixing material by applying a stimulus (S1). Since the method for producing an electronic component of the present invention includes the above-mentioned step (II), the adhesive strength of the temporary fixing material is reduced by curing, and the temporary fixing material can be easily peeled off in the step (III) described below. The stimulus (S1) may be light or heat. Among them, the stimulus (S1) is preferably light from the viewpoint of improving the work efficiency by making the process (II) easier to control and shortening the process time.
[0050] As a method for curing the temporary fixing material with light, a method is used in which light is irradiated under conditions that can cure the curable compound and make it difficult for the gas generating agent to generate gas. More specifically, for example, when the gas generating agent has an absorption edge on the long wavelength side of 420 nm and the photopolymerization initiator has an absorption edge on the long wavelength side of 460 nm, the wavelength of the light irradiation of the stimulus (S1) is irradiated with light having a wavelength in the range of more than 420 nm and not more than 460 nm, thereby making it possible to cure the curable compound without the gas generating agent generating gas. In other words, by irradiating light with a wavelength that is not absorbed by the gas generating agent and is absorbed by the photopolymerization initiator, it becomes possible to perform curing and gas generation separately. In this case, the irradiation intensity is 100 mW / cm 2 More than 3000mW / cm 2 The temporary fixing material may be cured by irradiating it with light for 1 second or more and 120 seconds or less. Furthermore, in the case where an inkjet device is used in the above step (I), if the inkjet device is equipped with a light source, the temporary fixing material may be cured using the light source immediately after application.
[0051] The method of curing the temporary fixing material by heat is a method of heating under conditions that can cure the curable compound and make it difficult for the gas generating agent to generate gas. More specifically, for example, when a compound with a decomposition temperature of 200° C. or more and 300° C. or less is used as the gas generating agent, a thermal polymerization initiator that starts polymerization at a temperature lower than the decomposition temperature is used, and the temporary fixing material is cured by heating at 100° C. or more and less than 200° C. for 10 minutes to 1 hour, for example.
[0052] The preferred lower limit of the 180° peeling force of the temporary fixing material from the silicon wafer after curing in the step (II) is 0.05 N / inch, and the preferred upper limit is 0.5 N / inch. When the 180° peeling force of the temporary fixing material from the silicon wafer after curing is 0.05 N / inch or more, the temporary fixing material after curing has a more suitable adhesive force. When the 180° peeling force of the temporary fixing material from the silicon wafer after curing is 0.5 N / inch or less, the temporary fixing material after curing can be more easily peeled off in the step (III) described below. The more preferred lower limit of the 180° peeling force of the temporary fixing material from the silicon wafer after curing is 0.08 N / inch, and the more preferred upper limit is 0.4 N / inch. The 180° peel strength of the cured temporary fixing material against a silicon wafer can be measured, for example, by a method in accordance with JIS Z0237:2009, in which a peel test is performed under conditions of 25°C, a peel speed of 300 mm / min, and a peel angle of 180°.
[0053] The preferred lower limit of the tensile storage modulus at 25° C. after hardening of the temporary fixing material in the step (II) is 1.0×10 8 The tensile storage modulus of the above temporary fixing material at 25°C after hardening is 1.0 × 10 8By setting the tensile storage modulus at 25° C. after curing to be equal to or higher than 5.0×10 Pa, the adhesiveness of the cured temporary fixing material to the adherend is improved. As a result, in the step (III) described below, the gas generated by the gas generating agent can be retained by the adhesive surface, so that the cured temporary fixing material can be more easily peeled off. A more preferable lower limit of the tensile storage modulus at 25° C. after curing of the temporary fixing material is 5.0×10 8 Pa, and a more preferable lower limit is 6.0×10 8 It is Pa. The preferred upper limit of the tensile storage modulus of the temporary fixing material at 25° C. after hardening is 1.0×10 10 The tensile storage modulus of the above temporary fixing material at 25°C after hardening is 1.0 × 10 10 By setting the tensile storage modulus at 25° C. after curing to be equal to or less than 5.0×10 Pa, the temporary fixing material after curing has a more suitable adhesive strength. 9 It is Pa. The tensile storage modulus of the above-mentioned temporary fixing material at 25°C after hardening can be measured, for example, by performing dynamic viscoelasticity measurement using a dynamic viscoelasticity measuring device (such as "DVA-200" manufactured by IT Measurement & Control Co., Ltd.) under conditions of a tensile direction, a frequency of 10 Hz, a heating rate of 3°C / min, and a temperature range of 0°C to 70°C.
[0054] The preferred lower limit of the elongation of the temporary fixing material after curing in the step (II) is 1%. When the elongation of the temporary fixing material after curing is 1% or more, the temporary fixing material after curing has appropriate flexibility. As a result, the temporary fixing material after curing can be more easily peeled off in the step (III) described below. The more preferred lower limit of the elongation of the temporary fixing material after curing is 5%. Moreover, the preferred upper limit of the elongation of the temporary fixing material after hardening is 20%. By setting the elongation of the temporary fixing material after hardening to 20% or less, the hardened temporary fixing material has more suitable adhesive strength. The more preferred upper limit of the elongation of the temporary fixing material after hardening is 10%. The degree of elongation of the temporary fixing material after hardening can be measured, for example, by the following method. That is, a laminated film is prepared by curing the temporary fixing material applied to a PET film with light, and a test piece is prepared by cutting the laminated film into a flat rectangular shape of 10 mm wide x 70 mm long (50 μm thick). The obtained test piece is subjected to a tensile test in the longitudinal direction at a tensile mode and a tensile speed of 5 mm / min using an autograph (Shimadzu Corporation, "AG-IS, load cell (SBL-50N)" or the like), and the length of elongation of the test piece until it breaks is measured. Using the obtained elongation length, the ratio (%) of the elongation length to the length of the test piece before the tensile test is calculated, and the elongation degree of the temporary fixing material of the present invention after curing can be obtained by taking this value as the elongation degree.
[0055] The method for producing an electronic component of the present invention includes a step (III) of generating a gas from the gas generating agent by a stimulus (S2) different from the stimulus (S1) to peel off the temporary fixing material. By including the step (III) in the method for producing an electronic component of the present invention, the temporary fixing material after hardening can be easily peeled off.
[0056] The stimulus used as the stimulus (S2) may be any stimulus different from the stimulus (S1), and may be light or heat. Among them, the stimulus (S2) is preferably light from the viewpoint of improving the work efficiency by making it easier to control the gas generation in the step (III) and shortening the process time. The method of generating gas from the gas generating agent varies depending on the gas generating agent contained in the temporary fixing material. In the case of the photo-induced gas generating agent, for example, when a compound having an absorption edge on the long wavelength side of 450 nm or less is used as the photo-induced gas generating agent, the method is a wavelength of 450 nm or less and an irradiation intensity of 100 mW / cm. 2 More than 3000mW / cm 2 Examples of the method include irradiating the following light for 1 second or more and 120 seconds or less. In the case of the thermal gas generating agent, for example, when a compound having a decomposition temperature of 100°C or higher and 300°C or lower is used as the thermal gas generating agent, a method of heating at a temperature equal to or higher than the decomposition temperature for 10 minutes to 1 hour can be mentioned.
[0057] In this specification, the stimulus (S2) is "different from the stimulus (S1)" means the following cases. When stimulus (S1) is light and stimulus (S2) is heat When stimulus (S1) is heat and stimulus (S2) is light When both stimuli (S1) and (S2) are light, but the wavelengths of the light are different When both stimuli (S1) and (S2) are heat, but the heating temperatures are different That is, the stimulus (S1) and the stimulus (S2) may both be light or may both be heat. In the method for producing an electronic component of the present invention, it is preferable that the stimulus (S1) and the stimulus (S2) are both light, from the viewpoint of ease of control and short process time.
[0058] When both the stimulus (S1) and the stimulus (S2) are light, it is preferable that the stimulus (S1) is light having a longer wavelength than the stimulus (S2). By using the stimulus (S1) as light having a longer wavelength than the stimulus (S2), the generation of gas from the gas generating agent can be more easily suppressed in the step (II), and the temporary fixing material after hardening can be more easily peeled off in the step (III). Examples of cases in which both the stimulus (S1) and the stimulus (S2) are light include a case in which the wavelength of the light of the stimulus (S1) is 450 nm and the wavelength of the light of the stimulus (S2) is 365 nm, and a case in which the wavelength of the light of the stimulus (S1) is 405 nm and the wavelength of the light of the stimulus (S2) is 365 nm.
[0059] When the stimulus (S1) and the stimulus (S2) are both heat, it is preferable that the stimulus (S1) has a lower heating temperature than the stimulus (S2). By the stimulus (S1) having a lower heating temperature than the stimulus (S2), the generation of gas from the gas generating agent can be more easily suppressed in the step (II), and the temporary fixing material after hardening can be more easily peeled off in the step (III). Examples of cases in which the stimulus (S1) and the stimulus (S2) are both heat include a case in which the heating temperature of the stimulus (S1) is 100°C and the heating temperature of the stimulus (S2) is 200°C, a case in which the heating temperature of the stimulus (S1) is 150°C and the heating temperature of the stimulus (S2) is 250°C, etc.
[0060] The method for manufacturing an electronic component of the present invention may include the above steps (I), (II), and (III), but may also include other steps as long as the effects of the present invention are not impaired.
[0061] The method for producing an electronic component of the present invention preferably includes, after the step (I), a step (IV) of applying a wall material onto the temporary fixing material. By including the above step (IV) in the method for producing an electronic component of the present invention, it becomes possible to increase the thickness of the plating in step (V) described below by using the wall material as a mold.
[0062] The wall material preferably contains a curable compound. By including a curable compound in the wall material, the wall material can be cured and the adhesion to the temporary fixing material can be further improved, and as a result, the wall material can be used as a plating mold to be prepared in the step (V) described below. Furthermore, in the step (III), the wall material can be more easily peeled off together with the hardened temporary fixing material. Examples of the curable compound include the same curable compounds as those in the above-mentioned temporary fixing material.
[0063] The wall material preferably further contains a polymerization initiator. When the wall material contains a polymerization initiator, the wall material can be cured more easily. Examples of the polymerization initiator include the same polymerization initiators as those in the above-mentioned temporary fixing material.
[0064] The wall material is preferably curable under the same conditions as the temporary fixing material. By allowing the wall material to be cured under the same conditions as the temporary fixing material, the manufacturing efficiency of the method for manufacturing an electronic component of the present invention is further improved.
[0065] In the above step (IV), the method of applying the wall material includes, for example, a method using a bar coater, a method using a dispenser, a method using an inkjet device, etc., and among these, a method using an inkjet device is preferable. By using an inkjet device, it becomes easier to prepare a thick cured wall material even if it is narrow in width by repeatedly performing the above step (IV) and curing the wall material. As a result, it becomes possible to prepare a thick metal plating using the cured wall material as a mold.
[0066] The method for producing an electronic component of the present invention preferably includes, after the step (IV), a step (V) of forming a plating between the wall materials. By including the step (V) in the method for producing an electronic component of the present invention, it becomes easier to produce a thick metal in a desired shape. Examples of the method for forming the plating between the wall materials include electrolytic plating, electroless plating, sputtering, and the like.
[0067] The preferred lower limit of the plating thickness is 1 μm. When the plating has a thickness of 1 μm or more, it becomes possible to withstand a high voltage. A more preferable lower limit of the plating thickness is 10 μm, and an even more preferable lower limit is 100 μm. Further, there is no particular upper limit to the thickness of the plating, but from the viewpoint of forming the wall material, the limit is about 1000 μm. The thickness of the plating can be measured, for example, by a laser displacement meter, a contact thickness meter, or the like.
[0068] In the method for producing an electronic component of the present invention, it is preferable that the temporary fixing material and the wall material are peeled off simultaneously in the step (III). Since the method for producing an electronic component of the present invention can peel off the temporary fixing material and the wall material simultaneously, the production efficiency of the method for producing an electronic component of the present invention is further improved.
[0069] According to the method for producing an electronic component of the present invention, even if the electrode is thick, the electrode can be formed into a desired shape, and is particularly suitable for use as electrodes for power devices such as diodes, transistors, and ICs.
[0070] The present invention relates to a curable composition comprising a curable compound which is cured by a stimulus (S3) and a gas generating agent which generates gas by a stimulus (S4) different from the stimulus (S3), the composition having a viscosity of 150 mPa s or less at 25°C, a 180° peel force from a silicon wafer after curing by the stimulus (S3) of 0.05 N / inch or more and 0.5 N / inch or less, and a tensile storage modulus at 25°C after curing by the stimulus (S3) of 1.0×10 8 The present invention also includes a temporary fixing material having a compressive strength of at least 10 Pa. The temporary fixing material of the present invention can be suitably used in the method for producing an electronic component of the present invention.
[0071] The temporary fixing material of the present invention is preferably liquid at 25° C. When the temporary fixing material of the present invention is liquid at 25° C., an inkjet device can be more suitably used, and the temporary fixing material of the present invention can be more easily applied in any shape with high precision.
[0072] The upper limit of the viscosity of the temporary fixing material of the present invention at 25°C is 150 mPa·s. The temporary fixing material of the present invention can be suitably used in inkjet printing because the viscosity of the temporary fixing material at 25° C. is 150 mPa s or less. The preferred upper limit of the viscosity of the temporary fixing material of the present invention at 25° C. is 100 mPa s. Furthermore, the preferred lower limit of the viscosity of the temporary fixing material of the present invention at 25°C is 1 mPa s. When the temporary fixing material of the present invention has a viscosity of 1 mPa s or more at 25°C, it can be easily ejected by inkjet, and therefore an inkjet device can be more suitably used. The more preferred lower limit of the viscosity of the temporary fixing material of the present invention at 25°C is 5 mPa s. The viscosity of the temporary fixing material of the present invention at 25° C. can be measured, for example, by using a Brookfield viscometer under conditions of 25° C. and 25 rpm.
[0073] The temporary fixing material of the present invention contains a hardenable compound that hardens in response to a stimulus (S3). Since the temporary fixing material of the present invention contains a curable compound that is cured by the stimulus (S3), the temporary fixing material of the present invention can be cured by the stimulus (S3).
[0074] The curable compound may be a photocurable compound that cures using light as the stimulus (S3) or a thermosetting compound that cures using heat as the stimulus (S3). Among them, the curable compound is preferably a photocurable compound from the viewpoint of easy control of curing and shortening the process time when curing the temporary fixing material of the present invention.
[0075] The curable compound preferably contains a (meth)acrylate. By including a (meth)acrylate in the curable compound, the 180° peel strength of the cured temporary fixing material from a silicon wafer, which will be described later, can be easily adjusted to an appropriate range. As a result, the cured temporary fixing material of the present invention has a more suitable adhesive strength and can be more easily peeled off.
[0076] The (meth)acrylate preferably contains urethane (meth)acrylate. When the (meth)acrylate contains urethane (meth)acrylate, the degree of elongation of the temporary fixing material after curing, which will be described later, can be more easily adjusted to an appropriate range. As a result, when the temporary fixing material of the present invention is peeled off by generating gas with a gas generating agent, which will be described later, the temporary fixing material of the present invention after curing can be peeled off more easily.
[0077] The urethane (meth)acrylate can be obtained, for example, by reacting an isocyanate compound with a (meth)acrylic acid derivative having a hydroxyl group in the presence of a catalytic amount of a tin compound.
[0078] Examples of the isocyanate compound that is a raw material for the urethane (meth)acrylate include isophorone diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, diphenylmethane-4,4'-diisocyanate (MDI), hydrogenated MDI, polymeric MDI, 1,5-naphthalene diisocyanate, norbornane diisocyanate, tolidine diisocyanate, xylylene diisocyanate (XDI), hydrogenated XDI, lysine diisocyanate, triphenylmethane triisocyanate, tris(isocyanatephenyl)thiophosphate, tetramethylxylylene diisocyanate, and 1,6,11-undecane triisocyanate.
[0079] As the isocyanate compound serving as a raw material for the urethane (meth)acrylate, a chain-extended isocyanate compound obtained by reacting a polyol with an excess of an isocyanate compound can also be used. Examples of the polyol include ethylene glycol, propylene glycol, glycerin, sorbitol, trimethylolpropane, carbonate diol, polyether diol, polyester diol, and polycaprolactone diol.
[0080] Examples of the (meth)acrylic acid derivative having a hydroxyl group include hydroxyalkyl mono(meth)acrylates, mono(meth)acrylates of dihydric alcohols, mono(meth)acrylates or di(meth)acrylates of trihydric alcohols, and epoxy (meth)acrylates. Examples of the hydroxyalkyl mono(meth)acrylate include 2-hydroxyethyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, 2-hydroxybutyl(meth)acrylate, and 4-hydroxybutyl(meth)acrylate. Examples of the dihydric alcohol include ethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, and polyethylene glycol. Examples of the trihydric alcohol include trimethylolethane, trimethylolpropane, and glycerin. The epoxy (meth)acrylate may, for example, be bisphenol A type epoxy acrylate.
[0081] When the curable compound contains the urethane (meth)acrylate, the preferred lower limit of the content of the urethane (meth)acrylate in 100 parts by mass of the curable compound is 20 parts by mass, and the preferred upper limit is 90 parts by mass. When the content of the urethane (meth)acrylate is within such a range, the degree of elongation after curing of the temporary fixing material described below can be easily adjusted to an appropriate range. As a result, when the temporary fixing material is peeled off by generating gas with a gas generating agent described below, the temporary fixing material of the present invention after curing can be peeled off more easily. The more preferred lower limit of the content of the urethane (meth)acrylate is 40 parts by mass, and the more preferred upper limit is 60 parts by mass.
[0082] The (meth)acrylate may include a monofunctional (meth)acrylate having one (meth)acryloyloxy group, or may include a polyfunctional (meth)acrylate having a plurality of (meth)acryloyloxy groups. Among these, it is preferable that the (meth)acrylate includes a polyfunctional (meth)acrylate. By including a polyfunctional (meth)acrylate in the (meth)acrylate, the 180° peel strength of the cured temporary fixing material from a silicon wafer can be easily adjusted to an appropriate range, so that the cured temporary fixing material of the present invention has a more suitable adhesive strength. In addition, the tensile storage modulus at 25°C of the cured temporary fixing material can be easily adjusted to an appropriate range, so that the adhesiveness of the cured temporary fixing material of the present invention to an adherend is improved. As a result, when the gas is generated by the gas generating agent to be described later and the temporary fixing material is peeled off, the gas generated by the gas generating agent to be described later can be retained by the adhesive surface, so that the cured temporary fixing material of the present invention can be peeled off more easily.
[0083] The upper limit of the number of the (meth)acryloyloxy groups in the polyfunctional (meth)acrylate is preferably 6. By making the number of the (meth)acryloyloxy groups 6 or less, it becomes easier to adjust the viscosity of the (meth)acrylate at 25°C to an appropriate range. The upper limit of the number of the (meth)acryloyloxy groups is preferably 4, and more preferably the number of the (meth)acryloyloxy groups is 2.
[0084] Examples of the polyfunctional (meth)acrylate include tricyclodecane dimethanol diacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol hexaacrylate, etc. The curable compound may contain the urethane (meth)acrylate as the polyfunctional (meth)acrylate.
[0085] Examples of the monofunctional (meth)acrylate include ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, etc. The curable compound may contain the urethane (meth)acrylate as the monofunctional (meth)acrylate.
[0086] The (meth)acrylate may have, in addition to a (meth)acryloyloxy group, a functional group other than the (meth)acryloyloxy group.
[0087] A preferred lower limit of the content of the (meth)acrylate in 100 parts by mass of the curable compound is 30 parts by mass. When the content of the (meth)acrylate is 30 parts by mass or more, the 180° peel strength of the temporary fixing material of the present invention after curing, which will be described later, against the silicon wafer can be easily adjusted to an appropriate range. As a result, the temporary fixing material of the present invention after curing has a more suitable adhesive strength. In addition, when the temporary fixing material of the present invention is peeled off by generating gas using a gas generating agent, which will be described later, the temporary fixing material of the present invention after curing can be peeled off more easily. A more preferred lower limit of the content of the (meth)acrylate is 50 parts by mass. Furthermore, the preferred upper limit of the content of the (meth)acrylate is not particularly limited, and may be 100 parts by mass.
[0088] The temporary fixing material of the present invention preferably further contains a polymerization initiator. By containing a polymerization initiator in the temporary fixing material of the present invention, the curable compound reacts with the polymerization initiator in response to the stimulus (S3), and the temporary fixing material can be cured more easily.
[0089] The photopolymerization initiator is preferably a compound whose absorption edge on the long wavelength side has a maximum absorption wavelength of 600 nm or less. When the absorption edge on the long wavelength side of the photopolymerization initiator is 600 nm or less, the generation of gas from the gas generating agent described below can be further suppressed when the temporary fixing material described below is cured, and when the temporary fixing material of the present invention is peeled off by generating gas from the gas generating agent described below, the cured temporary fixing material of the present invention can be more easily peeled off from the adherend.
[0090] Examples of the photopolymerization initiator include oxime ester compounds, acetophenone derivatives, benzophenone derivatives, and thioxanthone derivatives.
[0091] Examples of the oxime ester compound include Adeka Arcles NCI-730 (manufactured by Adeka Corporation), Omnirad OXE03, Omnirad OXE04, and Omnirad 1312 (all manufactured by IGM Resins). Examples of the acetophenone derivatives include Omnirad 184, Omnirad 907, and Omnirad 651 (all manufactured by IGM Resins). Examples of the benzophenone derivatives include Omnirad EMK, Omnirad BP, and Omnirad 4MBZ (all manufactured by IGM Resins). The thioxanthone derivatives include, for example, Omnirad DETX (manufactured by IGM Resins).
[0092] The thermal polymerization initiator is preferably a compound having a decomposition temperature of 100° C. or more and 200° C. or less. When the decomposition temperature of the thermal polymerization initiator is within the above range, the generation of gas from the gas generating agent described below can be further suppressed when the temporary fixing material described below is cured, and when the temporary fixing material of the present invention is peeled off by generating gas from the gas generating agent described below, the cured temporary fixing material of the present invention can be more easily peeled off from the adherend.
[0093] The thermal polymerization initiator may, for example, be a peroxide compound.
[0094] Examples of the peroxide compound include Luperox 270, Luperox 7, Luperox P, Luperox 555, and Luperox TAP (all manufactured by Arkema).
[0095] The preferred lower limit of the content of the polymerization initiator relative to 100 parts by mass of the curable compound is 0.1 parts by mass, and the preferred upper limit is 20 parts by mass. By having the content of the polymerization initiator within the above range, it becomes easier to adjust the 180° peel force from the silicon wafer after the temporary fixing material has been cured, the tensile storage modulus at 25°C after the temporary fixing material has been cured, and the elongation degree after the temporary fixing material has been cured, which will be described later, within appropriate ranges. The more preferred lower limit of the content of the polymerization initiator is 1 part by mass, and the more preferred upper limit is 15 parts by mass.
[0096] The temporary fixing material of the present invention further contains a gas generating agent that generates gas in response to a stimulus (S4). Since the temporary fixing material of the present invention contains a gas generating agent that generates gas in response to stimulation (S4), the gas generated from the gas generating agent in response to the stimulation (S4) is released onto the adhesive surface, and the temporary fixing material of the present invention after hardening can be easily peeled off.
[0097] The gas generating agent may be a photo-generated gas generating agent that generates gas using light as the stimulus (S4) or a thermal gas generating agent that generates gas using heat as the stimulus (S4) as long as the stimulus (S4) for generating gas from the gas generating agent is different from the stimulus (S3) for curing the temporary fixing material of the present invention. Among these, the gas generating agent is preferably a photo-generated gas generating agent from the viewpoint of easy control and shortening the process time when generating gas from the temporary fixing material of the present invention.
[0098] In this specification, the above stimulus (S4) being "different from the above stimulus (S3)" means the following cases. When the stimulus (S3) is light and the stimulus (S4) is heat When the stimulus (S3) is heat and the stimulus (S4) is light When stimuli (S3) and (S4) are both light, but the wavelengths of the light are different When both stimuli (S3) and (S4) are heat, but the heating temperatures are different That is, the above-mentioned stimulus (S3) and the above-mentioned stimulus (S4) may both be light or may both be heat. In particular, when the temporary fixing material of the present invention is cured and when the temporary fixing material of the present invention generates gas, it is preferable that the above-mentioned stimulus (S3) and the above-mentioned stimulus (S4) are both light from the viewpoint of easy control and shortening the process time.
[0099] When both the stimulus (S3) and the stimulus (S4) are light, it is preferable that the stimulus (S3) is light having a longer wavelength than the stimulus (S4). By using the stimulus (S3) as light having a longer wavelength than the stimulus (S4), it is possible to further suppress the generation of gas from the gas generating agent when the temporary fixing material of the present invention is cured, and it is possible to more easily peel off the hardened temporary fixing material of the present invention when the temporary fixing material of the present invention is peeled off by generating gas from the gas generating agent. Examples of cases in which the stimulus (S3) and the stimulus (S4) are both light include a case in which the wavelength of the light of the stimulus (S3) is 450 nm and the wavelength of the light of the stimulus (S4) is 365 nm, and a case in which the wavelength of the light of the stimulus (S3) is 405 nm and the wavelength of the light of the stimulus (S4) is 365 nm.
[0100] When the stimulus (S3) and the stimulus (S4) are both heat, it is preferable that the stimulus (S3) has a lower heating temperature than the stimulus (S4). By having the stimulus (S3) have a lower heating temperature than the stimulus (S4), it is possible to further suppress the generation of gas from the gas generating agent when the temporary fixing material of the present invention is cured, and when the temporary fixing material of the present invention is peeled off by generating gas from the gas generating agent, the cured temporary fixing material of the present invention can be peeled off more easily. Examples of cases in which the stimulus (S3) and the stimulus (S4) are both heat include a case in which the heating temperature of the stimulus (S3) is 100°C and the heating temperature of the stimulus (S4) is 200°C, or a case in which the heating temperature of the stimulus (S3) is 150°C and the heating temperature of the stimulus (S4) is 250°C.
[0101] The photo-gas generating agent is preferably a compound having an absorption edge on the long wavelength side of 450 nm or less. When the photo-gas generating agent has an absorption edge on the long wavelength side of 450 nm or less, the generation of gas from the gas generating agent can be further suppressed when the temporary fixing material of the present invention described below is cured, and when the temporary fixing material of the present invention is peeled off by generating gas from the gas generating agent, the cured temporary fixing material of the present invention can be peeled off more easily.
[0102] Examples of the photo gas generator include azo compounds, azide compounds, carbonates, and tetrazole compounds. Among them, the azo compounds 2,2'-azobis(N-cyclohexyl-2-methylpropionamide), 2,2'-azobis[N-(2-methylpropyl)-2-methylpropionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), 2,2'-azobis[N-(2-methylethyl)-2-methylpropionamide], 2,2'-azobis(N-hexyl-2-methylpropionamide), 2,2'-azobis(N-propyl-2-methylpropionamide), and 2,2'-azobis(N-ethyl-2-methylpropionamide) are preferred.
[0103] The thermal gas generating agent is preferably a compound having a decomposition temperature of 100° C. or more and 300° C. or less. When the decomposition temperature of the thermal gas generating agent is within the above range, the generation of gas from the gas generating agent can be further suppressed when the temporary fixing material of the present invention, which will be described later, is cured, and when the temporary fixing material of the present invention is peeled off by generating gas from the gas generating agent, the cured temporary fixing material of the present invention can be peeled off more easily.
[0104] Examples of the above-mentioned thermal gas generating agent include azo compounds, azide compounds, carbonates, and tetrazole compounds.Among them, the azo compounds 2,2'-azobis(N-cyclohexyl-2-methylpropionamide), 2,2'-azobis[N-(2-methylpropyl)-2-methylpropionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), 2,2'-azobis[N-(2-methylethyl)-2-methylpropionamide], 2,2'-azobis(N-hexyl-2-methylpropionamide), 2,2'-azobis(N-propyl-2-methylpropionamide), and 2,2'-azobis(N-ethyl-2-methylpropionamide) are preferred.
[0105] The method of generating gas from the gas generating agent varies depending on the gas generating agent contained in the temporary fixing material of the present invention. In the case of the photo-induced gas generating agent, for example, when a compound having an absorption edge on the long wavelength side of 450 nm or less is used as the photo-induced gas generating agent, the method is carried out at a wavelength of 450 nm or less and an irradiation intensity of 100 mW / cm. 2 More than 3000mW / cm 2 Examples of the method include irradiating the following light for 1 second or more and 120 seconds or less. In the case of the thermal gas generating agent, for example, when a compound having a decomposition temperature of 100°C or higher and 300°C or lower is used as the thermal gas generating agent, a method of heating at a temperature equal to or higher than the decomposition temperature for 10 minutes to 1 hour can be mentioned.
[0106] The preferred lower limit of the content of the gas generating agent relative to 100 parts by mass of the curable compound is 5 parts by mass, and the preferred upper limit is 50 parts by mass. When the content of the gas generating agent is 5 parts by mass or more, the temporary fixing material of the present invention can be more easily peeled off. When the content of the gas generating agent is 50 parts by mass or less, the temporary fixing material of the present invention becomes a liquid material with appropriate fluidity, and is more easily ejected by inkjet. The more preferred lower limit of the content of the gas generating agent is 10 parts by mass, and the more preferred upper limit is 30 parts by mass.
[0107] The temporary fixing material of the present invention preferably does not contain a solvent or has a solvent content of 1 mass % or less. By the temporary fixing material of the present invention not containing a solvent or having a solvent content of 1 mass % or less, it is possible to prevent the solvent from seeping out during the process in the method for producing electronic components of the present invention using the temporary fixing material of the present invention, thereby preventing a decrease in work efficiency. When the temporary fixing material of the present invention contains a solvent, the upper limit of the content of the solvent is more preferably 0.1 mass %. It is most preferable that the temporary fixing material of the present invention does not contain a solvent.
[0108] The temporary fixing material of the present invention may contain additives such as a plasticizer, an emulsifier, a softener, a filler, a pigment, a dye, a silane coupling agent, and an antioxidant, if necessary.
[0109] Examples of a method for producing the temporary fixing material of the present invention include a method in which the curable compound and the gas generating agent, as well as the polymerization initiator and additives that are blended as necessary, are mixed using a bead mill, ultrasonic dispersion, homogenizer, high-output disperser, roll mill, or the like.
[0110] As a method for curing the temporary fixing material of the present invention by light, a method of irradiating light under conditions that can cure the curable compound and make it difficult for the gas generating agent to generate gas is used. For example, when the absorption end on the long wavelength side of the gas generating agent is 420 nm and the absorption end on the long wavelength side of the photopolymerization initiator is 460 nm, the wavelength of the light irradiation of the stimulus (S3) is irradiated with light having a wavelength in the range of more than 420 nm and not more than 460 nm, so that the curable compound can be cured without the gas generating agent generating gas. In other words, by irradiating light with a wavelength that is not absorbed by the gas generating agent and is absorbed by the photopolymerization initiator, it becomes possible to perform curing and gas generation separately. In this case, the irradiation intensity is 100 mW / cm 2 More than 3000mW / cm 2 and a method of curing the temporary fixing material by irradiating the temporary fixing material with the following light for 1 second to 120 seconds. Furthermore, in the case where the temporary fixing material of the present invention is applied by the above-mentioned inkjet device, if the inkjet device used is equipped with a light source, the temporary fixing material of the present invention may be cured using the light source immediately after application.
[0111] The method for curing the temporary fixing material of the present invention by heat is a method of heating under conditions that can cure the curable compound and make it difficult for the gas generating agent to generate gas. More specifically, for example, when a compound with a decomposition temperature of 200° C. or more and 300° C. or less is used as the gas generating agent, a thermal polymerization initiator that starts polymerization at a temperature lower than the decomposition temperature is used, and the temporary fixing material is cured by heating at 100° C. or more and less than 200° C. for 10 minutes to 1 hour, for example.
[0112] The temporary fixing material of the present invention has a lower limit of 0.05 N / inch and an upper limit of 0.5 N / inch for the 180° peeling force against a silicon wafer after curing due to the above-mentioned stimulus (S3) (hereinafter, sometimes simply referred to as "180° peeling force against a silicon wafer after curing"). When the 180° peeling force of the temporary fixing material of the present invention against a silicon wafer after curing is 0.05 N / inch or more, the temporary fixing material of the present invention after curing has a suitable adhesive force. When the 180° peeling force of the temporary fixing material of the present invention against a silicon wafer after curing is 0.5 N / inch or less, the temporary fixing material of the present invention after curing can be easily peeled off when the temporary fixing material of the present invention is peeled off by generating gas with the gas generating agent. The preferred lower limit of the 180° peeling force of the temporary fixing material of the present invention against a silicon wafer after curing is 0.08 N / inch and the preferred upper limit is 0.4 N / inch. The 180° peel strength of the cured temporary fixing material of the present invention against a silicon wafer can be measured, for example, by a method in accordance with JIS Z0237:2009, in which a peel test is carried out under conditions of 25°C, a peel speed of 300 mm / min, and a peel angle of 180°.
[0113] The temporary fixing material of the present invention has a lower limit of the tensile storage modulus at 25° C. after curing due to the above-mentioned stimulus (S3) (hereinafter, may be simply referred to as the “tensile storage modulus at 25° C. after curing”) of 1.0×10 8 The tensile storage modulus of the temporary fixing material of the present invention at 25°C after hardening is 1.0 × 10 8 By having a tensile storage modulus of 5.0×10 Pa or more, the adhesiveness of the temporary fixing material of the present invention to the adherend after curing is improved. As a result, when the gas is generated by the gas generating agent and the temporary fixing material of the present invention is peeled off, the gas generated by the gas generating agent can be retained by the adhesive surface, so that the temporary fixing material of the present invention after curing can be easily peeled off. The preferred lower limit of the tensile storage modulus at 25° C. of the temporary fixing material of the present invention after curing is 5.0×10 8 Pa, more preferably the lower limit is 6.0×10 8 It is Pa. The preferred upper limit of the tensile storage modulus at 25° C. after hardening of the temporary fixing material of the present invention is 1.0×10 10 The tensile storage modulus of the temporary fixing material of the present invention at 25°C after hardening is 1.0 × 10 10 By setting the tensile storage modulus at 25° C. after curing to 5.0×10 Pa or less, the temporary fixing material of the present invention after curing has a more suitable adhesive strength. 9 It is Pa. The tensile storage modulus at 25°C after hardening of the temporary fixing material of the present invention can be measured, for example, by performing dynamic viscoelasticity measurement using a dynamic viscoelasticity measuring device (such as "DVA-200" manufactured by IT Measurement & Control Co., Ltd.) under conditions of a tensile direction, a frequency of 10 Hz, a heating rate of 3°C / min, and a temperature range of 0°C to 70°C.
[0114] The temporary fixing material of the present invention has a preferred lower limit of the elongation after curing due to the above-mentioned stimulus (S3) (hereinafter, sometimes simply referred to as "elongation after curing") of 1%. When the temporary fixing material of the present invention has an elongation after curing of 1% or more, the temporary fixing material of the present invention has appropriate flexibility after curing. As a result, when the temporary fixing material of the present invention is peeled off by generating gas with the above-mentioned gas generating agent, the temporary fixing material of the present invention after curing can be peeled off more easily. A more preferred lower limit of the elongation after curing of the temporary fixing material of the present invention is 5%. Moreover, the preferred upper limit of the elongation of the temporary fixing material of the present invention after curing is 20%. By setting the elongation of the temporary fixing material of the present invention after curing to 20% or less, the temporary fixing material of the present invention after curing has more suitable adhesive strength. The more preferred upper limit of the elongation of the temporary fixing material of the present invention after curing is 10%. The degree of elongation of the temporary fixing material of the present invention after hardening can be measured, for example, by the following method. That is, a laminated film is prepared by curing the temporary fixing material applied to a PET film with light, and a test piece is prepared by cutting the laminated film into a flat rectangular shape of 10 mm wide x 70 mm long (50 μm thick). The obtained test piece is subjected to a tensile test in the longitudinal direction at a tensile mode and a tensile speed of 5 mm / min using an autograph (Shimadzu Corporation, "AG-IS, load cell (SBL-50N)" or the like), and the length of elongation of the test piece until it breaks is measured. Using the obtained elongation length, the ratio (%) of the elongation length to the length of the test piece before the tensile test is calculated, and the elongation degree of the temporary fixing material of the present invention after curing can be obtained by taking this value as the elongation degree.
[0115] The temporary fixing material of the present invention is liquid and has a low viscosity, and can be applied using an inkjet device. Therefore, the temporary fixing material can be applied in any shape with high precision, and is highly versatile for the shape of the adherend. In addition, the temporary fixing material of the present invention has excellent peeling performance, and is therefore suitable for temporary fixing of electronic components in the manufacture of electronic components that require precise processing accuracy, and is particularly suitable for the manufacture of thick electrodes. Effect of the Invention
[0116] According to the present invention, it is possible to provide a method for manufacturing an electronic component, which is capable of forming an electrode into a desired shape even when the electrode is thick. Also, according to the present invention, it is possible to provide a temporary fixing material which is highly versatile for the shape of an adherend to be temporarily fixed and has excellent peeling performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0117] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0118] (Examples 1 to 4, Comparative Examples 1 to 3) (1) Preparation of temporary fixing material After replacing the atmosphere in a reactor equipped with a stirrer with nitrogen, the components shown in Table 1 were added and mixed uniformly to obtain a temporary fixing material.
[0119] (2) Viscosity of temporary fixing material at 25°C Immediately after preparation of the temporary fixing material prepared in "(1) Preparation of temporary fixing material" above, the viscosity (mPa s) of the temporary fixing material at 25°C was measured using a Brookfield viscometer ("LV-DV2T" manufactured by Brookfield Corporation) at 25°C and 25 rpm. The results are shown in Table 1.
[0120] (3) 180° peel strength of the temporary fixing material against the silicon wafer after hardening The temporary fixing material prepared in "(1) Preparation of temporary fixing material" above was applied to a silicon wafer using a bar coater to a thickness of 100 μm, and then exposed to UV light at a wavelength of 450 nm and an irradiation intensity of 500 mW / cm using a batch-type UV-LED device (manufactured by CCS Corporation, "HLDL-120V50U65-PSU"). 2 The temporary fixing material was cured by irradiating it with light for 30 seconds. The cured temporary fixing material was cut into a size of 25 mm in width and 100 mm in length to obtain a test sample. The obtained test samples were subjected to a 180° peel test at 25°C and a peel speed of 300 mm / min in accordance with JIS Z0237:2009 using an autograph (Shimadzu Corporation, "AG-IS, load cell (SBL-50N)") to measure the 180° peel force (N / inch). The results are shown in Table 1.
[0121] (4) Tensile storage modulus at 25°C after hardening of temporary fixing material The temporary fixing material prepared in "(1) Preparation of temporary fixing material" above was applied to a PET film using a bar coater to a thickness of 50 μm, and the applied light was measured with an ultraviolet thin illuminometer (manufactured by Ushio Inc., "UIT-OLED") at a wavelength of 450 nm and an irradiation intensity of 500 mW / cm. 2 The temporary fixing material was cured by irradiation with light of 1000 nm for 30 seconds to obtain a measurement sample. The obtained measurement samples were subjected to dynamic viscoelasticity measurement in tension mode under a nitrogen atmosphere at a frequency of 10 Hz, a heating rate of 3°C / min, and a temperature range of 0°C to 70°C using a dynamic viscoelasticity measuring device (manufactured by IT Measurement & Control Co., Ltd., "DVA-200") to obtain the tensile storage modulus (Pa) at 25°C. The results are shown in Table 1.
[0122] (5) Elongation of temporary fixing material after hardening The temporary fixing material prepared in the above "(1) Preparation of temporary fixing material" was applied to a PET film having a thickness of 50 μm using a bar coater. The film was then irradiated with a batch-type UV-LED device (HLDL-120V50U65-PSU, manufactured by CCS Corporation) at a wavelength of 450 nm and an irradiation intensity of 500 mW / cm. 2 The temporary fixing material was cured by irradiating it with light for 30 seconds to prepare a laminated film. The obtained laminated film was cut into a flat rectangular shape of 10 mm width × 70 mm length to obtain a test piece. An autograph (Shimadzu Corporation, "AG-IS, load cell (SBL-50N)") was attached to the prepared test specimen with the upper and lower grips set at 1 cm. A tensile test was then performed at 25°C, in tensile mode, at a tensile speed of 5 mm / min, in the longitudinal direction, to measure the length the test specimen stretched until it broke. The stretched length was used to calculate the ratio (%) of the stretched length to the length of the test specimen before the tensile test, and the degree of elongation (%) of the temporary fixing material after hardening was obtained. The results are shown in Table 1.
[0123] (6) Gas floating property of temporary fixing material after hardening The temporary fixing material prepared in the above "(1) Preparation of temporary fixing material" was applied to a silicon wafer using a bar coater so as to have a width of 3 cm, length of 3 cm, and thickness of 50 μm. The applied temporary fixing material was irradiated with light having a wavelength of 450 nm and an irradiation intensity of 500 mW / cm. 2 The temporary fixing material was cured by irradiation with light of 1000 nm for 30 seconds to obtain a test sample. The obtained test sample was further irradiated with light having a wavelength of 365 nm and an intensity of 500 mW / cm 2 After irradiating the adhesive surface of the cured temporary fixing material with light for 60 seconds, a batch-type UV-LED device (manufactured by CCS Corporation, "HLDL-120V50U65-PSU") was used to observe any bubbles that had formed on the adhesive surface of the cured temporary fixing material. The gas floating property of the temporary fixing material after hardening was evaluated as follows: when the observed bubble area ratio was 95% or more of the total adhesive surface area of the temporary fixing material, it was rated as "◎", when it was 80% or more but less than 95%, it was rated as "◯", when it was 40% or more but less than 80%, it was rated as "△", and when it was less than 40%, it was rated as "X". The results are shown in Table 1. Note that no evaluation was performed for Comparative Example 3.
[0124] [Table 1] [Industrial Applicability]
[0125] According to the present invention, it is possible to provide a method for manufacturing an electronic component, which is capable of forming an electrode into a desired shape even when the electrode is thick. Also, according to the present invention, it is possible to provide a temporary fixing material which is highly versatile for the shape of an adherend to be temporarily fixed and has excellent peeling performance.
Claims
1. A step (I) of applying a temporary fixing material containing a curable compound and a gas generating agent onto a substrate; A step (II) of hardening the temporary fixing material by a stimulus (S1); and A step (III) of generating gas from the gas generating agent by a stimulus (S2) different from the stimulus (S1) to peel off the temporary fixing material. A method for manufacturing an electronic component, comprising:
2. 2. The method for producing an electronic component according to claim 1, wherein in the step (I), the temporary fixing material is applied using an inkjet device.
3. 3. The method for producing an electronic component according to claim 1, further comprising, after the step (I), a step (IV) of applying a wall material onto the temporary fixing material.
4. 4. The method for producing an electronic component according to claim 3, wherein in the step (IV), the wall material is applied using an inkjet device.
5. 4. The method for producing an electronic component according to claim 3, further comprising the step (V) of forming a plating between the wall materials after the step (IV).
6. 6. The method for manufacturing an electronic component according to claim 5, wherein the plating has a thickness of 1 [mu]m or more.
7. 4. The method for producing an electronic component according to claim 3, wherein in the step (III), the temporary fixing material and the wall material are peeled off simultaneously.
8. 3. The method for manufacturing an electronic component according to claim 1, wherein both the stimulus (S1) and the stimulus (S2) are light.
9. 9. The method for manufacturing an electronic component according to claim 8, wherein the wavelength of the light of the stimulus (S1) is longer than the wavelength of the light of the stimulus (S2).
10. The composition contains a curable compound that is cured by a stimulus (S3) and a gas generating agent that generates gas by a stimulus (S4) different from the stimulus (S3), The viscosity at 25°C is 150 mPa·s or less, The 180° peel force against the silicon wafer after hardening due to the stimulus (S3) is 0.05 N / inch or more and 0.5 N / inch or less; The tensile storage modulus at 25° C. after curing due to the stimulation (S3) was 1.0×10 8 Pa or more A temporary fixing material characterized by:
11. The temporary fixing material according to claim 10 , wherein the curable compound includes a (meth)acrylate.
12. The temporary fixing material according to claim 11 , wherein the (meth)acrylate includes a urethane (meth)acrylate.
13. The temporary fixing material according to claim 11 or 12, wherein the (meth)acrylate includes a polyfunctional (meth)acrylate.
14. 13. The temporary fixing material according to claim 10, 11 or 12, which does not contain a solvent or has a solvent content of 1 mass % or less.
15. The temporary fixing material according to claim 10, 11 or 12, wherein the degree of elongation after hardening due to the stimulation (S3) is 1% or more.
16. The temporary fixing material according to claim 10, 11 or 12, wherein the stimulus (S3) and the stimulus (S4) are both light.
17. The temporary fixing material according to claim 16, wherein the stimulus (S3) is light having a longer wavelength than the stimulus (S4).
Citation Information
Patent Citations
Releasable tacky adhesive polymer
JP1993032946A