Core-shell structure particle, ceramic composition, and method for producing core-shell structure particle

Core-shell structured particles with BaTiO3 cores and CaTiO3 or SrTiO3 shells enhance dielectric constants, addressing size and performance limitations in dielectric materials for miniaturized electronic components.

JP2024139244APending Publication Date: 2024-10-09SAMSUNG ELECTRO MECHANICS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023050101
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing dielectric materials and manufacturing methods do not effectively enhance the dielectric constant while maintaining a reduced particle size, which is crucial for miniaturization of electronic components.

Method used

The development of core-shell structured particles with a core made of BaTiO3 and a shell of CaTiO3 or SrTiO3, produced through solvothermal or hydrothermal synthesis, ensuring a uniform thickness of the shell phase to increase the interfacial area and maintain a small overall particle size.

Benefits of technology

The core-shell structure significantly enhances the dielectric constant of dielectric ceramics, allowing for reduced component size and improved DC bias characteristics, facilitating mass production and integration into electronic components like capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139244000001_ABST
    Figure 2024139244000001_ABST
Patent Text Reader

Abstract

SOLUTION: To provide core-shell structure particles which include core particles that have a particle diameter of 100 nm or less and are composed of BaTiO3, and a shell phase which is composed of CaTiO3 and / or SrTiO3, has thickness of 1 unit or more and 10 units or less of a perovskite structure, and covers the core particles, and to provide a method for producing core-shell structure particles which include: a core production step of placing a raw material containing a barium hydroxide hydrate, titanium oxide and a first solvent under high temperature and / or high pressure, subjecting the raw material to solvothermal synthesis, and producing core particles; and a shell production step of placing the core particles, at least one of Ca hydrate and Sr hydrate, and a second solvent under high temperature and / or high pressure, subjecting them to solvothermal synthesis, and producing a shell phase covering the core particles.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to core-shell structured particles, a ceramic composition, and a method for manufacturing the core-shell structured particles.

Background Art

[0002] Research on various dielectric materials has been underway (for example, Patent Documents 1 to 5).

[0003] Patent Document 1 describes "a ceramic superlattice in which at least two types of oxide ceramics are laminated, wherein the oxide ceramics are perovskite-type crystals and grow on a substrate while maintaining a certain crystal orientation relationship with each other, and the growth thickness of the layer of the perovskite-type crystal is an integer multiple of the unit lattice length of the perovskite-type crystal as a growth unit (Claim 1)". Patent Document 2 describes "a dielectric composition containing at least barium titanate and calcium titanate, wherein for the molar ratios of these two components, the molar ratio (X) of barium titanate is 0.3 < X < 0.5, and the molar ratio (Y) of calcium titanate is 1 - X (Claim 1)". Patent Document 3 describes "a core-shell ceramic particle (10) comprising a core particle structure (12) containing a plurality of primary fine particles (16) and a plurality of primary pores, and a shell that at least partially surrounds the core particle structure (12), wherein each of the primary fine particles (16) contains a plurality of secondary fine particles (20) and a plurality of secondary pores (22), and the shell contains a plurality of tertiary fine particles (24) and a plurality of tertiary pores (23) (Claim 1)". Patent Document 4 describes a method for forming a film made of a perovskite-type complex oxide on the surface of a core material, comprising: (I) a step of mixing a complex oxide precursor alkoxide containing two or more metal elements with a core material, and forming a core material-complex oxide alkoxide in the mixture in which the complex oxide alkoxide is bonded to the surface of the core material; (II) a step of adding water to the core material-complex oxide alkoxide to hydrolyze and polycondense the complex oxide alkoxide to form a core material-complex oxide alkoxide polycondensate; and (III) a step of calcining the core material-complex oxide alkoxide polycondensate (Claim 1). Patent Document 5 describes a method for producing dielectric ceramic particles having core particles mainly composed of a first composite oxide having a perovskite structure at 25°C, and a shell phase formed on the surface of the core particles and mainly composed of a second composite oxide different from the first composite oxide, the method comprising the steps of: dry-mixing the core particles with a raw material compound of the second composite oxide to coat the core particles with the raw material compound of the second composite oxide to obtain a raw material mixture; and subjecting the raw material mixture to a hydrothermal synthesis treatment or a solvothermal synthesis treatment, the dry mixing being carried out at a concentration of 6×10 3 The document describes a method for producing dielectric ceramic particles using a mechanical rotor having a mechanism for rotating at an angular velocity of rad / s or more (Claim 1). [Prior art document] [Patent documents] [Patent Document 1] Japanese Patent Application Laid-Open No. 5-221800 [Patent Document 2] JP 2001-110665 A [Patent Document 3] JP 2007-320847 A [Patent Document 4] JP 2015-51913 A [Patent Document 5] JP 2019-89705 A Summary of the Invention

[0004] In a first aspect of the present invention, there is provided a core-shell structured particle comprising a core particle and a shell phase. The core particle may have a particle diameter of 100 nm or less and may be made of BaTiO3. The shell phase may be made of CaTiO3 and / or SrTiO3. The shell phase may have a thickness of 1 to 10 units of the perovskite structure and may cover the core particle.

[0005] In the above, the shell phase may cover the entire surface of the core particle with a substantially uniform thickness.

[0006] In the above, the core particle may have a cubic or rectangular parallelepiped shape.

[0007] In the above, the core particle may have a cubic or rectangular parallelepiped shape with rounded corners.

[0008] In a second aspect of the present invention, there is provided a ceramic composition comprising any of the core-shell structured particles described above.

[0009] In a third aspect of the present invention, there is provided a method for producing any of the core-shell structured particles described above. The production method may include a core generation step and a shell phase generation step. In the core generation step, a raw material including barium hydroxide hydrate, titanium oxide, and a first solvent may be subjected to high temperature and / or high pressure to perform solvothermal synthesis to produce a core particle. In the shell generation step, a core particle, at least one of Ca hydroxide and Sr hydroxide, and a second solvent may be subjected to high temperature and / or high pressure to perform solvothermal synthesis or hydrothermal synthesis to produce a shell phase covering the core particle.

[0010] In the above, the production method may further include an acid treatment step, in which the product obtained in the shell formation step may be treated with acid.

[0011] In the above, the solvothermal synthesis in the core formation step and / or the shell formation step may be carried out at a temperature of 100° C. or more and 300° C. or less for 5 hours or more and 100 hours or less.

[0012] In the above, the first solvent and the second solvent may be selected from water or alcohol.

[0013] In the above, the amount of at least one of Ca hydroxide and Sr hydroxide added in the shell formation stage may be 10 parts by weight or more and 90 parts by weight or less with respect to 100 parts by weight of the added amount of the core particles.

[0014] The above summary of the invention does not list all of the features of the present invention. Also, subcombinations of these features may also be inventions. [Brief description of the drawings]

[0015] [Figure 1] An example of a core-shell structure particle in this embodiment is shown below. [Diagram 2] 2 shows an enlarged view of part A in FIG. [Diagram 3] 2 shows an example of the dielectric ceramic according to the present embodiment. [Figure 4] An example of a production flow of the core-shell structured particles in this embodiment will be described. [Diagram 5] 1 shows an example of a core particle after the core generation step. [Figure 6A] The HAADF-STEM photograph of the core particle is shown. [Figure 6B] The HAADF-STEM photograph of the core particle is shown. [Figure 7A] The following is a photograph of a core-shell structured particle observed by HAADF-STEM. [Figure 7B] The following is a photograph of a core-shell structured particle observed by HAADF-STEM. [Figure 8A] The following is a photograph of a core-shell structured particle observed by HAADF-STEM. [Figure 8B] The following is a photograph of a core-shell structured particle observed by HAADF-STEM. [Figure 9] Photographs of core-shell structured particles are shown. [Figure 10] An enlarged photograph of FIG. 9 is shown. [Figure 11] Photographs of core-shell structured particles are shown. [Figure 12] An enlarged photograph of FIG. 11 is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will be described below through embodiments of the invention, but the following embodiments do not limit the scope of the invention according to the claims. Furthermore, not all of the combinations of features described in the embodiments are necessarily essential to the solution of the invention.

[0017] [1] Core-shell structured particles: The core-shell structure particles according to this embodiment will be described.

[0018] 1 shows an example of a core-shell structured particle 10 in this embodiment. In this embodiment, the core-shell structured particle 10 is composed of a core particle 20 and a shell phase 30.

[0019] The core particle 20 is made of barium titanate (BaTiO3). The core particle 20 may be a BaTiO3 crystal.

[0020] The core particle 20 may be a cube, a rectangular parallelepiped, a polyhedron, a cylinder, a sphere, an ellipsoid, an irregular shape, or other shapes. The core particle 20 may preferably be a cube or a rectangular parallelepiped. In this case, the corners and / or sides of the cube and rectangular parallelepiped may be rounded.

[0021] In particular, when the core particles 20 are cubic or rectangular, the area of ​​the interface where the surfaces of different particles contact each other increases when mixed with barium titanate particles. As a result, the relative dielectric constant of the dielectric ceramics produced from the core-shell structure particles 10 can be increased. Even if the shape is other than a cube or a rectangle, an interface where the surfaces of different particles contact each other is still generated, so the shape is not limited to a cube or a rectangle.

[0022] The particle diameter of the core particle 20 may be 100 nm or less, preferably 60 nm or less, and more preferably 45 nm or less. When such a particle diameter is satisfied, the size of an electric part manufactured using the core-shell structured particle 10 can be reduced. Furthermore, since the interface area per weight increases, the relative dielectric constant can be increased.

[0023] When the core particle 20 has a cubic or rectangular parallelepiped shape, the particle diameter may be the average or median of the length of one side of a cube or the long side of a rectangular parallelepiped observed with an electron microscope (SEM) etc. When the core particle 20 has a spherical, ellipsoidal or irregular shape, the particle diameter may be the average or median of the length of the long side observed with an electron microscope (SEM) etc. Alternatively, the particle diameter of the core particle 20 may be the average particle diameter measured with a laser diffraction particle size distribution meter.

[0024] There is no particular limitation on the method for producing the core particle 20, and various known methods may be used to produce the core particle 20. As will be described later, the core particle 20 having a cubic shape can be produced by using solvothermal synthesis.

[0025] The shell phase 30 covers the core particle 20. The shell phase 30 may cover the entire surface of the core particle 20. Alternatively, the shell phase 30 may partially cover a part of the surface of the core particle 20.

[0026] The shell phase 30 may be a compound in which barium in barium titanate is replaced with a group 2 element. For example, the shell phase 30 is made of CaTiO3 and / or SrTiO3. The shell phase 30 may be a layer in which CaTiO3 and SrTiO3 are mixed.

[0027] The shell phase 30 may have a thickness of 1 to 10 units, more preferably 1 to 5 units, and even more preferably 1 to 3 units, of the perovskite structure formed by CaTiO3, SrTiO3, etc. By making the thickness of the shell phase 30 within the above range, the size of the core-shell structured particles can be kept approximately the same as that of the core particles 20. This allows the size of parts using dielectric ceramics containing the core-shell structured particles to be reduced.

[0028] The shell phase may cover the entire surface of the core particle with a substantially uniform thickness. This ensures that an interface between the core particle and other particles, such as barium titanate particles, can be formed when the core particle is mixed with the other particles. The state of the shell phase 30 can be observed and analyzed by a scanning transmission electron microscope (STEM) and energy dispersive X-ray spectroscopy (EDS), etc.

[0029] When the shell phase 30 partially covers the core particle 20, the thickness of the covering portion may fall within the above range. When the shell phase 30 entirely covers the core particle 20, the entire, average or part of the thickness of the covering portion may fall within the above range. Since the thickness of the shell phase 30 is very small compared to the particle size of the core particle 20, the particle size of the core-shell structured particle 10 can be regarded as approximately the same as the particle size of the core particle 20.

[0030] Fig. 2 shows an enlarged view of part A in Fig. 1. In the core particle 20, a lattice of a perovskite structure is formed by Ba atoms 210, Ti atoms 220, and O atoms (not shown). In the shell phase 30, a perovskite structure is formed by Ti atoms 222 and Ca atoms or Sr atoms 230.

[0031] 2, the Ti atom 222 located at the center of the perovskite structure is present in the shell phase 30 portion with a thickness equivalent to two atoms. That is, the shell phase 30 portion is formed with a thickness equivalent to two lattices of the perovskite structure.

[0032] [2] Porcelain composition: The ceramic composition according to this embodiment will be described. The ceramic composition includes the core-shell structure particles described above. Preferably, the ceramic composition may include core-shell structure particles, barium titanate particles, and a binder resin. The ceramic composition may also include a solvent and other additives as necessary.

[0033] The barium titanate particles may be cubic, rectangular, spherical, ellipsoidal, irregular, or other shapes. The barium titanate particles may preferably be cubic or rectangular, and in this case, the corners and / or sides may be rounded. Such a shape can increase the area of ​​the interface where the surfaces of the particles contact each other when aggregated with core-shell structure particles, and can increase the relative dielectric constant when used in a ceramic composition.

[0034] The barium titanate particles may have a particle size of 100 nm or less, preferably 60 nm or less, more preferably 45 nm or less. The particle size may be defined in the same way as the particle size of the core-shell structured particles.

[0035] The barium titanate particles may have the same shape as the core-shell structure particles. For example, both the barium titanate particles and the core-shell structure particles may be cubic or rectangular. The barium titanate particles may have the same or approximately the same particle size as the core-shell structure particles. For example, the barium titanate particles may be core particles 20 that are obtained by removing the shell phase 30 from the core-shell structure particles 10.

[0036] Since the barium titanate particles and the core-shell structured particles have the same shape and / or particle size, when the ceramic composition is subsequently fired, the two particles are three-dimensionally accumulated into a block shape, and the interface between the two particles is well formed, thereby increasing the dielectric constant.

[0037] The binder resin is not particularly limited as long as it is one that is normally used in ceramic compositions. For example, polyvinyl alcohol, polyvinyl butyral, or acrylic resins may be used. The amount of the binder resin is not particularly limited, but may be, for example, 0.01% by weight or more and 20% by weight or less, preferably 0.5% by weight or more and 15% by weight or less, based on the total amount of the barium titanate particles and the core-shell structure particles. This makes it possible to improve the density of the dielectric ceramics that are molded later while maintaining moldability.

[0038] The ceramic composition is press-molded or sheet-molded into a predetermined shape, and then laminated, to produce a dielectric ceramic. The binder removal treatment may be a heat treatment, for example, a treatment of heating at 300°C to 800°C, preferably 400°C to 600°C.

[0039] The dielectric ceramics of the present embodiment can be used in various applications requiring a high relative dielectric constant. For example, the dielectric ceramics can be used as a dielectric for a capacitor, which is an electronic component. In particular, the dielectric ceramics can be suitably used as a capacitor for a power device substrate or a capacitor for a power supply substrate.

[0040] 3 shows an example of a dielectric ceramic 300 according to this embodiment. The dielectric ceramic 300 of this embodiment may have a structure in which barium titanate 310 and a core-shell structure 320 are assembled to form an interface with each other. The barium titanate 310 is formed from barium titanate particles. The core-shell structure 320 is formed from core-shell structure particles.

[0041] For example, as shown in the figure, barium titanate 310 may have a cubic shape derived from the shape of barium titanate particles, and core-shell structure 320 may also have a cubic shape derived from the shape of core-shell structure particles. Blocks derived from these particles are regularly stacked and three-dimensionally accumulated. An interface 330 is formed between the barium titanate 310 and the part of core-shell structure 320 corresponding to the shell phase made of CaTiO3 and / or SrTiO3.

[0042] It is speculated that the crystal lattice is distorted at the interface 330 between the barium titanate 310 and the core-shell structure 320, resulting in a huge dielectric constant. The dielectric ceramic 300 of this embodiment has many fine interfaces, and therefore exhibits a very high dielectric constant and is also excellent in DC bias characteristics.

[0043] In addition, an example of a structure in which different types of particles are adjacent to each other is shown in Fig. 3. In reality, the dielectric ceramic 300 is formed by a random collection of the same and different types of particles, and may include cases in which adjacent particles are of the same type.

[0044] [3] Manufacturing method of core-shell structured particles: A method for producing the core-shell structured particles according to this embodiment will be described.

[0045] 4 shows an example of a production flow of core-shell structured particles in this embodiment. Core-shell structured particles may be produced by processes from S100 to S300. Some of S100 to S300 may be omitted. Other processes may be performed in addition to S100 to S300.

[0046] First, in S100, a core generation step is performed. In the core generation step, a core particle may be generated by performing a solvothermal synthesis. For example, the solvothermal synthesis may be performed by subjecting a raw material including barium hydroxide hydrate, titanium oxide, and a first solvent to high temperature and / or high pressure.

[0047] The barium hydroxide hydrate is preferably the octahydrate (Ba(OH)2·8H2O), but may alternatively be another hydrate such as the monohydrate (Ba(OH)2·1H2O) or anhydrous.

[0048] Titanium oxide is of anatase type, rutile type and brookite type, among which anatase type is preferred. Titanium oxide is preferably particles having a particle size of 100 nm or less, preferably 50 nm or less, more preferably 25 nm or less, as measured by a laser diffraction particle size distribution analyzer or a long side measurement by SEM. Titanium oxide may be used in an amount of 10 mol to 100 mol, preferably 20 mol to 50 mol, per 100 mol of barium hydroxide hydrate.

[0049] The first solvent may be selected from water or alcohol. The alcohol may be selected from methanol, ethanol, 1-propanol, 1-butanol, etc. The amount of the first solvent may be 10 parts by weight or more and 2000 parts by weight or less, preferably 100 parts by weight or more and 1000 parts by weight or less, based on 100 parts by weight of the solid content.

[0050] Further, titanium alkoxide may be included as a raw material. For example, titanium alkoxide may be titanium tetraisopropoxide ([(CH3)2CHO]4Ti). Titanium alkoxide may be used in an amount of 3 to 30 moles, preferably 5 to 20 moles, per 100 moles of barium hydroxide hydrate.

[0051] The above-mentioned raw materials may be placed in a sample container and mixed. Then, the sample container may be placed in a high-pressure reaction and decomposition container. Then, the high-pressure reaction and decomposition container may be placed in a heating device and heated with the heating device to perform solvothermal synthesis.

[0052] Heating in the solvothermal synthesis may be carried out at a temperature of from 100° C. to 300° C., preferably from 150° C. to 250° C., more preferably from 180° C. to 220° C. Heating in the solvothermal synthesis may be carried out for a period of from 5 hours to 100 hours, preferably from 50 hours to 90 hours, more preferably from 70 hours to 80 hours.

[0053] The product obtained by the solvothermal synthesis may be separated, washed, and dried to obtain a product. The product obtained through the solvothermal synthesis is a cubic or rectangular prism-shaped barium titanate crystal particle. The product after the core formation step is the core particle portion of the core-shell structure particle. The product after the core formation step can also be used as barium titanate particles for a ceramic composition.

[0054] FIG. 5 shows an example of a core particle after the core generation stage. FIG. 5 shows an enlarged view of the surface of the core particle as shown in part A of FIG. 1. In the inner part 50 of the core particle, a perovskite structure of barium titanate is formed. On the other hand, in the outer part 52 of the core particle, Ba atoms 210 are not present, and Ti atoms 222 are precipitated.

[0055] Next, in S200, a shell formation step is performed. In the shell formation step, a solvothermal synthesis or hydrothermal synthesis may be performed to form a shell phase that covers the core particles. For example, the core particles formed in S100, the Group II hydroxide, and the second solvent may be subjected to high temperature and / or high pressure to perform the solvothermal synthesis or hydrothermal synthesis.

[0056] The Group 2 hydroxide preferably contains at least one of Ca hydroxide (Ca(OH)2) and Sr hydroxide (Sr(OH)2), but may be another Group 2 hydroxide. The Group 2 hydroxide may be contained in an amount of 10 to 1000 moles, preferably 50 to 300 moles, more preferably 100 to 150 moles, per 100 moles of the core particles. The Group 2 hydroxide may be contained in an amount of 10 to 90 parts by weight, per 100 parts by weight of the core particles.

[0057] The second solvent may be selected from water or alcohol. The alcohol may be selected from methanol, ethanol, 1-propanol, 1-butanol, etc. The amount of the second solvent may be 10 parts by weight or more and 2000 parts by weight or less, preferably 500 parts by weight or more and 1500 parts by weight or less, based on 100 parts by weight of the solid content.

[0058] The above-mentioned raw materials may be placed in a sample container and mixed. Then, the sample container may be placed in a high-pressure reaction and decomposition container. Then, the high-pressure reaction and decomposition container may be placed in a heating device and heated with the heating device to perform solvothermal synthesis or hydrothermal synthesis.

[0059] Heating in the solvothermal synthesis or hydrothermal synthesis may be carried out at a temperature of from 100° C. to 300° C., preferably from 100° C. to 200° C., and more preferably from 100° C. to 150° C. Heating in the solvothermal synthesis or hydrothermal synthesis may be carried out for a period of from 5 hours to 100 hours, preferably from 7 hours to 30 hours, and more preferably from 10 hours to 20 hours.

[0060] The product obtained by solvothermal synthesis or hydrothermal synthesis may be separated, washed, and dried to obtain the product. The product obtained through solvothermal synthesis or hydrothermal synthesis is a particle in which a shell phase derived from Group 2 hydroxide is formed on the surface of the core particle. Specifically, the Group 2 hydroxide reacts with the outer portion 52 in FIG. 5 to form a perovskite structure (CaTiO3 or SrTiO3) of the shell phase.

[0061] Next, an acid treatment step is performed in S300. In the acid treatment step, the product obtained in the shell generation step in S200 may be treated with acid. For example, an acid is added to the product in S200 and stirred. An aqueous solution of a weak acid such as acetic acid may be used as the acid. For example, an aqueous solution of 1% to 10% by volume of acetic acid may be used as the acid for the acid treatment. An amount of acid used may be 1 part by weight to 100 parts by weight, preferably 20 parts by weight to 70 parts by weight, based on the product. After the acid treatment, the product may be separated, washed, and stirred. The purpose of the acid treatment is to wash off unreacted Ca and Sr, and may be omitted. Core-shell structured particles can be produced without the acid treatment step.

[0062] Thus, according to the present application, core-shell structured particles can be produced by steps S100 to S300. In particular, according to this embodiment, core-shell structured particles can be produced without significant cost or time. Furthermore, according to this embodiment, core-shell structured particles can be produced on a relatively large scale. This can greatly contribute to the mass production of core-shell structured particles, ceramic compositions using the same, and dielectric ceramics.

[0063] The core particles produced in S100 may be used as barium titanate particles in a ceramic composition together with the core-shell structured particles produced in S300, in which case the acid treatment step in S300 may be applied to the core particles produced in S100.

[0064] [Example] The present invention will be described below with reference to examples. However, the technical scope of the present invention is not limited to the following examples.

[0065] [Example 1: Production of core particles] The following raw materials were placed in a 100 mL polytetrafluoroethylene (PTFE) sample container and stirred (350 rpm, 5 minutes). Ba(OH)2·8H2O: 20 mmol (6.3 g), TiO2 (particle size <25 nm, polymorph, anatase type): 7.5 mmol (0.60 g), [(CH3)2CHO]4Ti:2.5mmol(0.71g), 1-Butanol: 40mL

[0066] Next, the PTFE sample container was placed in a high-pressure reaction and decomposition container (HUT-100, manufactured by San-Ai Scientific Co., Ltd.). The high-pressure reaction and decomposition container was then placed in a dryer and heated. The heating conditions were temperature: 200°C, time: 72 hours.

[0067] Next, the heated product was centrifuged three times for 5 minutes at 10,000 rpm using water as a solvent, and then centrifuged twice for 5 minutes at 10,000 rpm using methanol as a solvent. The separated solid was dried overnight at 80°C.

[0068] 2 ml of acetic acid was placed in a 50 ml measuring flask and diluted with water to prepare 50 ml of acetic acid solution. The dried product (1.0 g) was placed in a beaker and stirred (350 rpm, 5 minutes) with 50 ml of acetic acid solution.

[0069] The stirred material was centrifuged three times for 5 minutes at 10,000 rpm using water as a solvent, and then centrifuged twice for 5 minutes at 10,000 rpm using methanol as a solvent. The separated solid was dried overnight at 80°C.

[0070] Observation of the dried product under an electron microscope revealed that the surface of the BaTiO3 cubes was reconstructed by Ti columns. The length of one side of the cube was about 80 nm. The corners of the cubes were slightly rounded.

[0071] [Example 2: Production of core-shell structured particles containing Sr] The following raw materials were placed in a 100 mL polytetrafluoroethylene (PTFE) sample container and stirred (350 rpm, 5 minutes). Ba(OH)2·8H2O: 20 mmol (6.3 g), TiO2 (particle size <25nm, polymorph, anatase type): 7.5mmol (0.60g), [(CH3)2CHO]4Ti:2.5mmol(0.71g), 1-butanol: 40mL

[0072] Next, the PTFE sample container was placed in a high-pressure reaction and decomposition container (HUT-100, manufactured by San-Ai Scientific Co., Ltd.). The high-pressure reaction and decomposition container was then placed in a dryer and heated. The heating conditions were temperature: 200°C, time: 72 hours.

[0073] Next, the heated composite was centrifuged three times for 5 minutes at 10,000 rpm using water as a solvent. Then, it was centrifuged twice for 5 minutes at 10,000 rpm using methanol as a solvent. The separated solid was dried overnight at 80°C. This resulted in the core particles, which were BaTiO3 nanocubes.

[0074] Next, the following raw materials were placed in a 100 mL polytetrafluoroethylene (PTFE) sample container and stirred (350 rpm, 5 minutes). Core particle: 8.6 mmol (2.0 g), Sr(OH)2: 10mmol (1.2g), Water: 40ml

[0075] Next, the PTFE sample container was placed in a high-pressure reaction and decomposition container (HUT-100, manufactured by San-Ai Scientific Co., Ltd.). The high-pressure reaction and decomposition container was then placed in a dryer and heated. The heating conditions were temperature: 100°C, time: 12 hours.

[0076] Next, the heated product was centrifuged three times for 5 minutes at 10,000 rpm using water as a solvent, and then centrifuged twice for 5 minutes at 10,000 rpm using methanol as a solvent. The separated solid was dried overnight at 80°C.

[0077] 2 ml of acetic acid was placed in a 50 ml measuring flask and diluted with water to prepare 50 ml of acetic acid solution. The dried product (1.0 g) was placed in a beaker and stirred (350 rpm, 5 minutes) with 50 ml of acetic acid solution.

[0078] The stirred material was centrifuged three times for 5 minutes at 10,000 rpm using water as a solvent, and then centrifuged twice for 5 minutes at 10,000 rpm using methanol as a solvent. The separated solid was dried overnight at 80°C.

[0079] Observation of the dried product under an electron microscope confirmed that the core particles were BaTiO3 cubes and the shells were SrTiO3. The core-shell particles were cubic with sides of approximately 80 nm, and the shell phase had a thickness of two units of the perovskite structure. The corners of the cubes were slightly rounded.

[0080] [Example 3: Production of Ca-containing core-shell structured particles] The following raw materials were placed in a 100 mL polytetrafluoroethylene (PTFE) sample container and stirred (350 rpm, 5 minutes). Ba(OH)2·8H2O: 20 mmol (6.3 g), TiO2 (particle size <25 nm, polymorph, anatase type): 7.5 mmol (0.60 g), [(CH3)2CHO]4Ti:2.5mmol(0.71g), 1-butanol: 40mL

[0081] Next, the PTFE sample container was placed in a high-pressure reaction and decomposition container (HUT-100, manufactured by San-Ai Scientific Co., Ltd.). The high-pressure reaction and decomposition container was then placed in a dryer and heated. The heating conditions were temperature: 200°C, time: 72 hours.

[0082] Next, the heated composite was centrifuged three times for 5 minutes at 10,000 rpm using water as a solvent. Then, it was centrifuged twice for 5 minutes at 10,000 rpm using methanol as a solvent. The separated solid was dried overnight at 80°C. This resulted in the core particles, which were BaTiO3 nanocubes.

[0083] Next, the following raw materials were placed in a 100 mL polytetrafluoroethylene (PTFE) sample container and stirred (350 rpm, 5 minutes). Core particle: 8.6 mmol (2.0 g), Ca(OH)2: 10mmol (0.74g), Water: 40ml

[0084] Next, the PTFE sample container was placed in a high-pressure reaction and decomposition container (HUT-100, manufactured by San-Ai Scientific Co., Ltd.). The high-pressure reaction and decomposition container was then placed in a dryer and heated. The heating conditions were temperature: 100°C, time: 12 hours.

[0085] Next, the heated product was centrifuged three times for 5 minutes at 10,000 rpm using water as a solvent, and then centrifuged twice for 5 minutes at 10,000 rpm using methanol as a solvent. The separated solid was dried overnight at 80°C.

[0086] 2 ml of acetic acid was placed in a 50 ml measuring flask and diluted with water to prepare 50 ml of acetic acid solution. The dried product (1.0 g) was placed in a beaker and stirred (350 rpm, 5 minutes) with 50 ml of acetic acid solution.

[0087] The stirred material was centrifuged three times for 5 minutes at 10,000 rpm using water as a solvent, and then centrifuged twice for 5 minutes at 10,000 rpm using methanol as a solvent. The separated solid was dried overnight at 80°C.

[0088] Observation of the dried product under an electron microscope confirmed that the core particles were BaTiO3 cubes and the shells were CaTiO3 core-shell structure particles. The core-shell structure particles were cubic with sides of approximately 80 nm, and the shell phase had a thickness of two units of the perovskite structure. The corners of the cubes were slightly rounded.

[0089] Figures 6A and 6B show HAADF-STEM observation images of the core particle. Figure 6A shows the results of observation of the entire core particle produced in Example 1 by HAADF-STEM (High-Angle Annular Dark Field Scanning Transmission Electron Microscopy). Figure 6B shows an enlarged view of a portion of the left side of the particle in Figure 6A. As shown in the figure, a layer of Ti atoms (small white dots in the photograph) equivalent to two units of the perovskite structure is formed on the outside (left side of the figure).

[0090] Figures 7A and 7B show HAADF-STEM observation images of core-shell structured particles. Figure 7A shows the results of HAADF-STEM observation of the entire core-shell structured particle produced in Example 2, in which the shell phase is SrTiO3. Figure 7B shows an enlarged view of a portion of the upper left corner of the particle in Figure 7A. As shown in the figure, a shell phase of two units of a perovskite structure is formed on the outside (left side of the figure).

[0091] Figures 8A and 8B show HAADF-STEM observation images of core-shell structured particles. Figure 8A shows the results of HAADF-STEM observation of the entire core-shell structured particle produced in Example 3, in which the shell phase is CaTiO3. Figure 8B shows an enlarged view of a portion of the right side of the particle in Figure 8A. As shown in the figure, a shell phase equivalent to two units of a perovskite structure is formed on the outside (right side of the figure).

[0092] Fig. 9 shows an observation photograph of a core-shell structured particle. Fig. 9 is an electron microscope photograph (EDX Elemental Mapping) of a core-shell structured particle produced in Example 3, the shell phase of which is CaTiO3. Fig. 10 is an enlarged view of a part of Fig. 9. As shown in the figure, a thin Ca shell phase is formed on the outside of the cubic core particle.

[0093] Fig. 11 shows an observation photograph of a core-shell structured particle. Fig. 11 is an electron microscope photograph (EDX Elemental Mapping) of a core-shell structured particle produced in Example 2, in which the shell phase is SrTiO3. Fig. 12 is an enlarged view of a part of Fig. 11. As shown in the figure, a thin Sr shell phase is formed on the outside of the cubic core particle.

[0094] In the above, an example was described in which cubic core particles were produced using solvothermal synthesis and then coated with a shell phase, but the method for producing core-shell structured particles is not limited to this. For example, existing barium titanate particles may be coated with a shell phase to produce core-shell structured particles.

[0095] Although the present invention has been described above using the embodiments, the technical scope of the present invention is not limited to the scope described in the above embodiments. It is clear to those skilled in the art that various modifications and improvements can be made to the above embodiments. It is clear from the description of the claims that such modifications and improvements can also be included in the technical scope of the present invention.

[0096] It should be noted that the order of execution of each process, such as operations, procedures, steps, and stages, in the devices, systems, programs, and methods shown in the claims, specifications, and drawings is not specifically stated as "before," "prior to," etc., and may be realized in any order unless the output of a previous process is used in a later process. Even if the operational flow in the claims, specifications, and drawings is explained using "first," "next," etc. for convenience, it does not mean that it is essential to perform the process in this order. [Explanation of symbols]

[0097] 10 Core-shell structured particles 20 Core Particles 30 Shell Phase 50 Internal part 52 Outer part 210 Ba atoms 220 Ti atoms 222 Ti atoms 230 Ca atom or Sr atom 300 Dielectric Ceramics 310 Barium titanate 320 Core-shell structure 330 Interface

Claims

1. The particle size is 100 nm or less, and BaTiO 3 A core particle consisting of CaTiO 3 and / or SrTiO 3 a shell phase having a thickness of 1 unit or more and 10 units or less of a perovskite structure and covering the core particle; The core-shell structured particle comprises:

2. The shell phase covers the entire surface of the core particle with a substantially uniform thickness. The core-shell structured particle according to claim 1.

3. The core particles have a cubic or rectangular parallelepiped shape. The core-shell structured particle according to claim 1.

4. The core particles have a cubic or rectangular parallelepiped shape with rounded corners. The core-shell structured particle according to claim 3.

5. The core-shell structured particles according to any one of claims 1 to 4, Porcelain composition.

6. A method for producing the core-shell structured particles according to any one of claims 1 to 4, comprising the steps of: a core generation step of subjecting a raw material including barium hydroxide hydrate, titanium oxide, and a first solvent to high temperature and / or high pressure to solvothermal synthesis to generate the core particles; a shell formation step in which the core particles, at least one of Ca hydroxide and Sr hydroxide, and a second solvent are subjected to high temperature and / or high pressure to perform solvothermal synthesis or hydrothermal synthesis to form the shell phase that covers the core particles; A method for producing core-shell structured particles comprising the steps of:

7. an acid treatment step of treating the product obtained in the shell formation step with an acid; The method for producing core-shell structured particles according to claim 6, further comprising:

8. The solvothermal synthesis and hydrothermal synthesis in the core production step and / or the shell production step are carried out at a temperature of 100 to 300 ° C. for 5 to 100 hours; The method of claim 7.

9. The first solvent and the second solvent are selected from water or alcohol; The method of claim 7.

10. The amount of at least one of the Ca hydroxide and the Sr hydroxide added in the shell formation step is 10 parts by weight or more and 90 parts by weight or less with respect to 100 parts by weight of the core particles added. The method of claim 7.