Method for producing cement-based hardened body
By using Kanuma or Hyuga soil in specific ratios, the efflorescence issue in cement-based products is addressed, achieving effective suppression without inhibitors, thus reducing costs and maintaining product integrity.
Patent Information
- Application Number
- JP2023050135
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing cement-based hardened products face the issue of efflorescence, which is aesthetically undesirable and often requires high amounts of efflorescence inhibitors, increasing production costs.
Incorporating Kanuma soil or Hyuga soil as additives in specific ratios within the production process of cement-based hardened products to suppress efflorescence without the need for efflorescence inhibitors.
Effectively reduces efflorescence by adjusting the pH of the hardened material, thereby preventing white substance formation without the use of inhibitors, maintaining cost-effectiveness and production feasibility.
Smart Images

Figure 2024139269000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a cement-based hardened body by hardening a composition containing a cement-based binder, aggregate, and water, which can provide an efflorescence prevention effect, and more particularly, to a method for producing a cement-based hardened body by using Kanuma soil or Hyuga soil in a specific range as an additive, without using an efflorescence prevention agent. [Background technology]
[0002] Cement used in the manufacture of cement-based hardened bodies is an inorganic powder whose main components are clinker and gypsum, and has the property of hardening when it reacts with water. Concrete, which is made by mixing cement with water, fine aggregate, and coarse aggregate, is an essential material for the formation of social capital, and when properly manufactured and managed, it becomes a structural material with excellent load-bearing and durability properties.
[0003] Meanwhile, interest in the aesthetics and design of concrete has been growing in recent years. For example, in interlocking block paving, the color tone of the blocks and the design and geometric pattern when laid are considered important, and harmony with aesthetics as well as functionality is sought. In addition, exposed concrete, which does not undergo a surface finishing process after demolding, is widely used as one of the designs for modern architecture, and the unique texture and feel of concrete can improve the aesthetics of structures.
[0004] However, the cement-based hardened body has an aesthetic problem of efflorescence, where free components such as calcium in the hardened body are dissolved on the surface together with the water that has penetrated into the hardened body, and carbonatize to produce a white substance. For example, in water-retentive paving blocks used in recent years as a measure against the heat island effect in urban areas, efflorescence becomes more pronounced due to the water-retentive materials used to improve the water-retentive capacity.
[0005] In order to prevent or suppress this efflorescence phenomenon, anti-efflorescence agents have been proposed that are mixed with the raw materials for the cement-based hardened body (see, for example, Patent Documents 1 and 2), and some of these have also been commercialized. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 11-60301 [Patent Document 2] JP 2017-218364 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0007] However, in order to sufficiently suppress efflorescence using an efflorescence inhibitor, it is usually necessary to add a very large amount of the agent, which has been problematic in that it increases the production costs of the cement-based hardened body.
[0008] Therefore, the present invention provides a method for producing a cement-based hardened body that is capable of suppressing efflorescence without using an efflorescence inhibitor that is usually used to prevent efflorescence in cement-based hardened bodies. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to solve the above problems, and have found that by using Kanuma soil or Hyuga soil in a specific range as an additive in the production of cement-based hardened bodies, efflorescence can be suppressed without the addition of an efflorescence inhibitor. As a result of further investigation, the present invention has been completed.
[0010] That is, the present invention relates to a method for producing a cement-based hardened body by mixing aggregate, a cement-based binder, and water and hardening the mixture, characterized in that 4 to 11 parts by mass of Kanuma soil are mixed with the cement-based binder. The second invention is a method for producing a cement-based hardened body by mixing aggregate, a cement-based binder, and water and hardening the mixture, characterized in that 2 to 8 parts by mass of Hyuga soil is mixed with the cement-based binder. Effect of the Invention
[0011] According to the present invention, by using an appropriate amount of Kanuma soil or Hyuga soil as an additive, it is possible to suppress efflorescence of the cement-based hardened body without using an efflorescence inhibitor. It is presumed that efflorescence is suppressed because Kanuma soil and Hyuga soil are weakly acidic, and by using an appropriate amount of these, the pH of the resulting cement-based hardened body is lowered. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The cement-based binder in the present invention refers to cement and inorganic powder admixtures among the components mixed during the production of a cement-based hardened body. Cement may be used alone, or admixtures may be appropriately mixed within a range in which desired performance such as strength and durability can be obtained.
[0013] The cement used in the present invention may be any known cement specified by the JIS standard, and specific examples thereof include JIS R 5210 "Portland cement", JIS R 5211 "Blast-furnace cement", JIS R 5212 "Silica cement", JIS R 5213 "Fly ash cement", and JIS R 5214 "Ecocement".
[0014] The inorganic powder admixture used in the present invention can be any known inorganic powder that contributes to improving the physical properties, such as the fresh properties, setting, strength development, and durability, of cement-based mixtures such as mortar and concrete. Specific examples include inorganic powders specified as minor mixed components in JIS R 5210 "Portland cement", JIS A 6201 "fly ash for concrete", JIS A 6207 "silica fume for concrete", and limestone fine powder, of which 21% or more by weight pass through a sieve with 150 μm openings.
[0015] Of the above cements, it is preferable to apply the present invention when producing a cement-based hardened body using ecocement, which is generally prone to efflorescence.
[0016] The greatest feature of the present invention is that, among the water, cement and aggregates generally used in the production of cement-based hardened bodies, Kanuma soil or Hyuga soil is used as an additive as part of the aggregate.
[0017] Kanuma soil is a general term for pumice produced near Kanuma City, Tochigi Prefecture, and is composed of weathered pumice, pumice grains, imogolite, rock fragments, and voids. It is a porous material with a porosity of 70% or more, and is generally used in agriculture and horticulture. Kanuma soil has a pH of about 4 to 5, and is slightly acidic in nature.
[0018] Hyuga soil is a type of hard pumice made from volcanic gravel that is formed by the deposition of volcanic material found in the southern part of Miyazaki Prefecture, and the particles contain minute voids. It is generally used in agriculture and horticulture. Hyuga soil has a pH of about 6, and is slightly acidic in nature.
[0019] The Kanuma soil or Hyuga soil used as the additive in the present invention may be any known Kanuma soil or Hyuga soil, specifically, Kanuma soil or Hyuga soil used for agriculture and horticulture.
[0020] By using such specific materials in specific ranges, the efflorescence phenomenon of the produced cement-based hardened body can be suppressed or prevented without using an efflorescence inhibitor.
[0021] The Kanuma soil or Hyuga soil used as an additive in the present invention preferably has a particle size range of less than 10% sieve residue on a 2.5 mm sieve and less than 15% passing through a 1.2 mm sieve. When the cement-based hardened body obtained by the manufacturing method of the present invention is used as an interlocking block, the interlocking block has a porous structure, and the voids between the aggregates affect its strength. However, if the sieve residue and sieve passing rate of the Kanuma soil or Hyuga soil are within this range, there will be few voids between the aggregates, and the effect on strength will be small. More preferably, the 2.5 mm sieve residue is less than 7% and the 1.2 mm sieve passing rate is less than 12%.
[0022] In the present invention, the amount of Kanuma clay used must be 40 to 110 parts by mass per 100 parts by mass of cement binder. If it is less than 40 parts by mass, it is assumed that the effect on the alkalinity in the cement hardened body is small and the pH does not decrease, but efflorescence cannot be sufficiently prevented. Also, if it exceeds 110 parts by mass, the porous Kanuma clay absorbs the mixing water, making it impossible to knead and mold.
[0023] In the present invention, the amount of the above-mentioned Hyuga soil must be 20 to 80 parts by mass per 100 parts by mass of the cement binder. If it is less than 20 parts by mass, it is assumed that the effect on the alkalinity in the cement hardened body is small and the pH does not decrease, but efflorescence cannot be sufficiently prevented. Also, if it exceeds 80 parts by mass, the porous Hyuga soil absorbs the mixing water, making it impossible to knead and mold.
[0024] In the present invention, when producing a cement-based hardened body, other known aggregates can be used as aggregates (fine aggregates, coarse aggregates) in addition to Kanuma soil or Hyuga soil without any restrictions. As the aggregate, for example, natural aggregates such as crushed stone and crushed sand, slag aggregates specified in JIS A 5011, lightweight aggregates, water-retaining materials, etc. can be used without any particular restrictions. When using these aggregates in the production of a cement-based hardened body, the amount of Kanuma soil or Hyuga soil used should be within the above range, and the total amount of Kanuma soil or Hyuga soil and other aggregates should be within the desired range.
[0025] Fine aggregate is defined as aggregate that passes completely through a 10 mm sieve, passes through a 5 mm sieve at a rate of 85% or more by weight, and remains on a 150 μm sieve at a rate of 80% or more by weight. Coarse aggregate is defined as aggregate that remains on a 5 mm sieve at a rate of 85% or more by weight.
[0026] The water used in the method for producing a cement-based hardened body of the present invention can be any water known for preparing mortar or concrete, without any particular limitation. Specifically, industrial water, tap water, etc.
[0027] In the method for producing a cement-based hardened body of the present invention, it is possible to suppress efflorescence without using an efflorescence inhibitor, but an efflorescence inhibitor may be used if necessary. The efflorescence inhibitor is generally a chemical agent consisting of a mixture of fatty acid salts, surfactants, water repellents, waterproofing agents, organic compounds, etc., and is a type of admixture that is added simultaneously with other materials when kneading the cement-based hardened body.
[0028] Specific examples of fatty acid salts that are the main components of the efflorescence prevention agent include higher fatty acid salts such as calcium stearate, magnesium stearate, aluminum stearate, potassium stearate, sodium oleate, calcium laurate, calcium myristate, calcium palmitate, calcium behenate, and calcium oleate. Stearate-based efflorescence prevention agents are particularly common, and efflorescence prevention agents containing calcium stearate are most preferred.
[0029] In the method for producing a cement-based hardened product of the present invention, known additives that are generally mixed in the preparation of mortar or concrete, such as air-entraining water-reducing agents, high-range water-reducing agents, high-range air-entraining water-reducing agents, air content adjusters, and setting accelerators, may be further added within a range that does not impair the effects of the present invention.
[0030] In the cement-based hardened product of the present invention, the water-cement ratio is not particularly limited as long as it is within the range used in general mortar and concrete, specifically, the water-cement ratio is in the range of 20 to 60%.
[0031] In the present invention, the method for producing the cement-based hardened body by mixing Kanuma soil or Hyuga soil, aggregate, cement-based binder, water, and other materials as necessary, and hardening them can be any conventional method used in ready-mix concrete factories or secondary concrete product factories, with no particular restrictions.
[0032] In the present invention, the mixer used for mixing the hardened cement product can be any mixer generally used for mixing mortar or concrete, without any restrictions. Specific examples include a pan mixer, a forced twin-shaft mixer, a tilting mixer, a mortar mixer, a hand mixer, etc.
[0033] In the present invention, the method for curing the cement-based hardened body after mixing Kanuma soil or Hyuga soil, aggregate, cement-based binder, and water and hardening can be any conventional curing method used in ready-mix concrete factories or secondary concrete product factories, without any particular restrictions.Specific examples include wet curing, underwater curing, steam curing, autoclave curing, and air curing.
[0034] The cement-based hardened body in the present invention is a mixture and hardening product of the above-mentioned Kanuma soil or Hyuga soil, aggregate, cement-based binder, water, and other materials added as necessary, but is generally called mortar or concrete. Mortar is a mixture of cement-based binder, water, fine aggregate, and admixture, while concrete is a mixture of cement-based binder, water, fine aggregate, coarse aggregate, and admixture. EXAMPLES
[0035] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0036] The evaluation of efflorescence was done visually by 10 evaluators according to the criteria shown in Table 1. In other words, when efflorescence was judged to be minimal, it was marked as "Good", when it was judged to have a moderate amount, it was marked as "Good", and when it was judged to have a significant amount, it was marked as "Poor".
[0037] JIS Ecocement (EC), water, standard sand, water-retentive material (Komatsu Matere: Greenbiz), Kanuma soil or Hyuga soil, and efflorescence prevention agent (Fuji Fine Chemical: Eflex NP: stearate-based) were mixed in the proportions shown in Table 1 and mixed in a Hobart mixer at 20°C to produce mortar measuring 40 x 40 x 160 mm. The Kanuma soil used had a passing rate of 99% by weight through a 5 mm sieve and a remaining rate of 99% by weight through a 150 μm sieve. The Hyuga soil had a passing rate of 100% by weight through a 5 mm sieve and a remaining rate of 99% by weight through a 150 μm sieve.
[0038] One day after mixing, the mortar was removed from the mold and cured for 14 days in an environment with a temperature of 20°C and a humidity of 60%. After curing, the mortar was dried in an environment of 100°C for 24 hours, and the sides were sealed with aluminum adhesive tape with the poured surface of the mortar facing up. The mortar was then immersed in water up to half its height in an environment with a temperature of 5°C and a humidity of 30%, and after 14 days of immersion, the occurrence of efflorescence on the top surface of the mortar was confirmed. The evaluation results are also shown in Table 1.
[0039] [Table 1]
[0040] Reference Examples 1, 2, 3, 4, and 5 are experimental results confirming the prevention of efflorescence using only the conventional efflorescence prevention agent, and are the efflorescence test results of mortars prepared by adding 0 mass%, 0.25 mass%, 0.50 mass%, 0.75 mass%, and 1.0 mass% to ecocement (100 mass%). 0 out of 10 evaluators evaluated that there was little efflorescence when the efflorescence prevention agent was added at a rate of 0 to 0.50 mass%, and 8 out of 10 evaluated that there was little efflorescence when the addition rate was 0.75 mass%. All evaluators evaluated that there was little efflorescence when the addition rate was 1.0 mass%. From this, it can be said that it is difficult to suppress the efflorescence phenomenon using only the efflorescence prevention agent when the amount added is 0.75 mass% or less.
[0041] Comparative Example 1 shows the results of an efflorescence test in which ecocement was mixed into the cement-based binder, Kanuma soil was mixed into part of the aggregate as an additive, the ratio of Kanuma soil to the cement-based binder (Kanuma soil / binder) was 30 parts by mass, and no efflorescence prevention agent was added. All evaluators judged there to be a lot of efflorescence, and it can be seen that efflorescence is not suppressed by using Kanuma soil alone.
[0042] Examples 1 and 2 show the results of an efflorescence test in which ecocement was mixed into the cement-based binder, Kanuma soil was mixed into part of the aggregate as an additive, the ratio of Kanuma soil to the cement-based binder (Kanuma soil / binder) was 60 and 90 parts by mass, and no efflorescence prevention agent was added. All evaluators judged there to be little efflorescence, and it can be seen that the use of Kanuma soil suppresses efflorescence.
[0043] Comparative Example 2 shows the results of an efflorescence test in which ecocement was mixed into the cement-based binder, Kanuma soil was mixed into part of the aggregate as an additive, the ratio of Kanuma soil to the cement-based binder (Kanuma soil / binder) was 120 parts by mass, and no efflorescence prevention agent was added. With this mix, Kanuma soil absorbed the mixing water, making it difficult to mix the mortar.
[0044] Examples 3 and 4 show the results of efflorescence tests in which ecocement was mixed into the cement-based binder, Hyuga soil was mixed into part of the aggregate as an additive, the ratio of Hyuga soil to the cement-based binder (Hyuga soil / binder) was 30 and 60 parts by mass, and no efflorescence prevention agent was added. In both cases, most of the evaluators judged there to be little efflorescence, and it can be seen that efflorescence was suppressed.
[0045] Comparative Example 3 shows the results of an efflorescence test in which ecocement was mixed into the cement binder, Hyuga soil was mixed into part of the aggregate as an additive, the ratio of Hyuga soil to the cement binder (Hyuga soil / binder) was 90 parts by mass, and an efflorescence inhibitor was added. In this mix, Hyuga soil absorbed the mixing water, making it difficult to mix the mortar.
Claims
1. A method for producing a cement-based hardened body by mixing aggregate, a cement-based binder and water and hardening the mixture, comprising mixing 40 to 110 parts by mass of Kanuma soil with 100 parts by mass of the cement-based binder.
2. A method for producing a cement-based hardened body by mixing aggregate, a cement-based binder, and water and hardening the mixture, comprising mixing 20 to 80 parts by mass of Hyuga soil per 100 parts by mass of the cement-based binder.
3. 3. The method for producing a cement-based hardened product according to claim 1 or 2, wherein the cement-based binder is ecocement.
4. A hardenable composition comprising a cement binder and an aggregate, the hardenable composition comprising 40 to 110 parts by mass of Kanuma clay per 100 parts by mass of the cement binder.
5. A hardenable composition comprising a cement binder and an aggregate, the hardenable composition comprising 20 to 80 parts by mass of Hyuga soil per 100 parts by mass of the cement binder.
6. A cement-based hardened product which is a hardened product of the hardenable composition according to claim 4 or 5.
Citation Information
Patent Citations
Manufacture of lightweight artificial stones
JP1982088062A
Wall decorating material using mylonekton as main raw material
JP2004284881A
Environment improving pavement material, environment improving pavement construction method, and its washing method
JP2005350949A
Paving stone block body having both water holding properties and permeability and method for shaping the same
JP2006306684A
Method of producing cement based hardened body
JP2022016828A