Reinforcement film, optical member and electronic member

The reinforcing film with a balanced adhesive layer composition addresses the flexibility and adhesion challenges of flexible devices by ensuring easy initial releasability and high adhesive strength, suitable for repeated bending and bending.

JP2024139312APending Publication Date: 2024-10-09NITTO DENKO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023050192
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing adhesive films for flexible devices lack flexibility and adhesion properties suitable for repeated bending and bending, as they either have too high initial adhesive strength or insufficient flexibility, making them difficult to handle and apply effectively.

Method used

A reinforcing film with an adhesive layer composed of polymers (A) and (B), where polymer (A) contains nitrogen-containing monomer units and a zirconium-containing compound, and polymer (B) includes a polyorganosiloxane skeleton, allowing for easy releasability and subsequent high adhesive strength, with specific ratios and amounts of monomer units to balance flexibility and adhesion.

Benefits of technology

The film exhibits easy peelability at initial attachment and significantly increased adhesive strength after heating, providing flexibility suitable for repeated bending and bending, enhancing the durability and handling of flexible devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139312000001_ABST
    Figure 2024139312000001_ABST
Patent Text Reader

Abstract

To provide a reinforcement film having an adhesive agent showing excellent flexibility, while being capable of exhibiting lighter detachability at an initial stage when adhered onto an adherend, and thereafter drastically increasing an adhesive strength.SOLUTION: An reinforcement film includes an adhesive layer containing a polymer (A) and a polymer (B). The polymer (B) includes: a monomer unit having a polyorganosiloxane skeleton; and a (meth)acrylic monomer unit. The polymer (A) is an acrylic polymer containing a monomer unit derived from a nitrogen-containing monomer. A weight WN [pts.wt.] of the monomer unit derived from the nitrogen-containing monomer contained in 100 pts.wt. of the polymer (A) is 14 pts.wt. or lower. The adhesive layer further contains WZr [pts.wt.] of a zirconium-containing compound with regard to 100 pts.wt. of the polymer (A), and a ratio (WN / WZr) is 4 or higher.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a reinforcing film, and an optical member and an electronic member to which the reinforcing film is attached. [Background technology]

[0002] Adhesives in the form of adhesive sheets are widely used in various applications in portable electronic devices such as mobile phones, smartphones, and tablet computers, as well as other electronic devices, for the purpose of bonding adherends together or fixing articles to adherends. For example, adhesive sheets are used as reinforcing materials (reinforcing films) that impart rigidity and impact resistance to optical components and electronic components that constitute the above-mentioned devices. Patent Documents 1 and 2 are cited as documents disclosing this type of prior art.

[0003] Moreover, in recent years, portable electronic devices that can be bent or rolled have been attracting attention, and the development of adhesive sheets that can be used for fixing flexible devices (typically image display devices such as organic electroluminescence (EL) and liquid crystal display devices) built into such electronic devices is progressing (Patent Documents 3 to 6).

[0004] Meanwhile, looking at the performance of the adhesive, recently, an adhesive sheet has been proposed that exhibits low adhesive strength when first applied to an adherend, and then can increase its adhesive strength significantly (Patent Document 7). An adhesive sheet with such properties exhibits reworkability (reworkability) that is useful for preventing a decrease in yield due to incorrect or failed application of the adhesive sheet before the increase in adhesive strength, and can exhibit strong adhesiveness that is suitable for the original intended use of the adhesive sheet after the increase in adhesive strength. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6366199 [Patent Document 2] Patent No. 6366200 [Patent Document 3] Patent No. 6376271 [Patent Document 4] JP 2016-108555 A [Patent Document 5] JP 2017-095657 A [Patent Document 6] JP 2017-095659 A [Patent Document 7] Patent No. 6373458 Summary of the Invention [Problem to be solved by the invention]

[0006] The reinforcing film can also be used in the flexible device. For example, in the manufacture of the flexible device, since the members constituting the device are often thin, it is desirable to apply a pressure-sensitive adhesive sheet as a reinforcing film to reinforce the device, prevent defects caused by deformation of the device, and improve handling. Flexible devices can be repeatedly folded or bent, so the pressure-sensitive adhesive constituting the reinforcing film used in the flexible device is required to have flexibility that allows it to follow the adherend well even in such a usage mode. Pressure-sensitive adhesives having such flexibility and reinforcing films provided with the pressure-sensitive adhesives can be used for various applications including flexible devices, and are therefore useful with few limitations on the range of application.

[0007] For example, as proposed in Patent Document 7, an adhesive that shows low adhesion at the beginning of application and then increases significantly in adhesion is also desired to have flexibility suitable for repeated folding and bending when used as a reinforcing film. One method for this purpose is, for example, a method of appropriately setting the storage modulus of the adhesive at low temperatures. However, in an adhesive designed to increase in adhesion as described above, if the storage modulus at low temperatures is changed, both the initial low adhesion and the increased adhesion are affected. If the flexibility of an adhesive that shows low adhesion at the beginning of application and then increases significantly in adhesion can be improved, it would be practically useful.

[0008] The present invention has been made in view of the above circumstances, and aims to provide a reinforcing film having an adhesive that exhibits easy peelability in the early stages after being attached to an adherend, and that is capable of significantly increasing its adhesive strength thereafter and exhibits good flexibility. Another aim of the present invention is to provide an optical member and an electronic member to which the reinforcing film is attached. [Means for solving the problem]

[0009] According to the present specification, there is provided a reinforcing film having a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer includes a polymer (A) and a polymer (B). The polymer (B) includes a monomer unit having a polyorganosiloxane skeleton and a (meth)acrylic monomer unit. The polymer (A) is an acrylic polymer including a monomer unit derived from a nitrogen-containing monomer, and the amount W of the monomer unit derived from the nitrogen-containing monomer contained in 100 parts by weight of the polymer (A) is N [Parts by weight] is 14 parts by weight or less. The pressure-sensitive adhesive layer is made of W Zr [parts by weight] of a zirconium-containing compound. Zr [Parts by weight] N [Part by weight] ratio (W N / W Zr ) is 4 or more.

[0010] According to the reinforcing film of the above configuration, the adhesive layer contains the polymer (A) and the polymer (B) containing a monomer unit having a polyorganosiloxane skeleton, so that it exhibits easy peelability at the initial stage after being attached to the adherend, and it is possible to greatly increase the adhesive strength thereafter. In addition, the amount W of the monomer unit derived from the nitrogen-containing monomer contained per 100 parts by weight of the polymer (A) is N By limiting the [parts by weight] to 14 parts by weight or less, the adhesive layer exhibits flexibility suitable for repeated folding and bending. Zr [Parts by weight] N [Part by weight] ratio (W N / W Zr ) is 4 or more, so W N It is possible to achieve both initial easy peelability and high adhesive strength after the adhesive strength increases while limiting the amount of the adhesive to 14 parts by weight or less.

[0011] In some embodiments of the technology disclosed herein (including reinforcing films, optical components, electronic components, adhesives used therein, and adhesive compositions for forming the adhesives; the same applies below), the adhesive layer contains a crosslinking agent. The use of a crosslinking agent allows the cohesive strength of the adhesive layer to be appropriately adjusted. Incidentally, containing a crosslinking agent here means containing the crosslinking agent in a form after a crosslinking reaction.

[0012] In some embodiments, the content of the polymer (B) in the pressure-sensitive adhesive layer is 0.1 to 10 parts by weight relative to 100 parts by weight of the polymer (A). By setting the amount of the polymer (B) to 0.1 parts by weight or more relative to 100 parts by weight of the polymer (A), it is easy to obtain light peelability at the initial stage of application. By setting the amount of the polymer (B) to 10 parts by weight or less, it is easy to obtain high adhesive strength after the adhesive strength has increased. In addition, by setting the amount of the polymer (B) used within the above range, it is easy to achieve both low initial adhesive strength and high adhesive strength after the increase, and good flexibility (for example, low storage modulus at low temperature).

[0013] In some embodiments, the polymer (A) contains a monomer unit derived from a monomer having a nitrogen atom-containing ring as the monomer unit derived from the nitrogen-containing monomer. The polymer (A) containing a monomer unit derived from a monomer having a nitrogen atom-containing ring is likely to provide a high post-rise adhesive strength.

[0014] Some preferred embodiments of the reinforcing film have an adhesive strength (initial adhesive strength) N1 of 200 gf / 25 mm or less after 30 minutes at 23° C. after being attached to a polyimide film. A reinforcing film having an initial adhesive strength N1 of 200 gf / 25 mm or less can exhibit good easy peelability suitable for reworking and the like in the early stage after being attached to an adherend.

[0015] In some preferred embodiments, the reinforcing film has an adhesive strength (post-heat adhesive strength) N2 of 1000 gf / 25 mm or more after being attached to a polyimide film and heated at 60° C. for 1 hour and then at 23° C. for 30 minutes. A reinforcing film having a post-heat adhesive strength N2 of 1000 gf / 25 mm or more can exhibit high adhesive strength after the adhesive strength increases.

[0016] In some preferred embodiments, the reinforcing film has an increase rate [%] of 900% or more in adhesive strength N2 [gf / 25mm] after being attached to a polyimide film and heated at 60°C for 1 hour and then at 23°C for 30 minutes, relative to adhesive strength N1 [gf / 25mm] after being attached to a polyimide film and at 23°C for 30 minutes. A reinforcing film with an adhesive strength increase rate (N2 / N1) of 900% or more exhibits easy peelability suitable for reworking at the initial stage of attachment, and can greatly increase its adhesive strength by subsequent heating or the like.

[0017] In some preferred embodiments, the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer has a storage modulus (G′ -20 ) is 1000 kPa or less. Such a pressure-sensitive adhesive with a low storage modulus at -20°C exhibits high flexibility suitable for repeated bending and flexing.

[0018] The reinforcing film disclosed herein is suitable as a reinforcing film that imparts rigidity and impact resistance to an optical member such as a polarizing plate, a wavelength plate, etc., during processing or transport of the optical member. Thus, according to the present specification, there is provided an optical member to which any of the reinforcing films disclosed herein is attached.

[0019] The reinforcing film disclosed herein is also suitable as a reinforcing film for electronic components of devices such as portable electronic devices, etc. Thus, according to the present specification, there is provided an electronic component to which any of the reinforcing films disclosed herein is attached.

[0020] In addition, any suitable combination of the elements described in this specification may also be included within the scope of the invention for which patent protection is sought by this application. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a cross-sectional view illustrating a schematic configuration of a reinforcing film according to an embodiment. [Diagram 2] FIG. 4 is a cross-sectional view illustrating a schematic configuration of a reinforcing film according to another embodiment. [Diagram 3] FIG. 4 is a cross-sectional view illustrating a schematic configuration of a reinforcing film according to another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Preferred embodiments of the present invention will be described below. Matters necessary for carrying out the present invention other than those specifically mentioned in this specification can be understood by those skilled in the art based on the teachings on carrying out the invention described in this specification and the common general technical knowledge at the time of filing. The present invention can be carried out based on the contents disclosed in this specification and the common general technical knowledge in the relevant field. In the following drawings, the same reference numerals may be used to denote components or parts having the same function, and duplicated descriptions may be omitted or simplified. In addition, the embodiments shown in the drawings are schematic in order to clearly explain the present invention, and do not necessarily accurately represent the size or scale of the product actually provided.

[0023] In addition, in this specification, the term "acrylic polymer" refers to a polymer containing a monomer unit derived from a (meth)acrylic monomer in the polymer structure, and typically refers to a polymer containing a monomer unit derived from a (meth)acrylic monomer at a ratio of more than 50% by weight. In addition, the term "(meth)acrylic monomer" refers to a monomer having at least one (meth)acryloyl group in one molecule. Here, the term "(meth)acryloyl group" refers to an acryloyl group and a methacryloyl group in a comprehensive sense. Therefore, the concept of the (meth)acrylic monomer here can include both a monomer having an acryloyl group (acrylic monomer) and a monomer having a methacryloyl group (methacrylic monomer). Similarly, in this specification, "(meth)acrylic acid" refers to acrylic acid and methacrylic acid, and "(meth)acrylate" refers to acrylate and methacrylate in a comprehensive sense.

[0024] <Structural example of reinforcing film> The reinforcing film disclosed herein has the form of an adhesive sheet having an adhesive surface formed by an adhesive. The adhesive sheet used as the reinforcing film is configured to include an adhesive layer. The reinforcing film disclosed herein may be in the form of an adhesive sheet with a substrate in which the adhesive layer is laminated on one or both sides of a supporting substrate, or may be in the form of a substrate-less adhesive sheet that does not have a supporting substrate. Hereinafter, the supporting substrate may be simply referred to as a "substrate". In this specification, the term "reinforcing film" refers to an adhesive sheet (reinforcing adhesive film) used to reinforce an adherend as described below. The reinforcing film is not limited to the form of an adhesive sheet with a substrate, for example, since it can be reinforced by attaching a support material or the like to one adhesive surface of the reinforcing film and then attaching the other adhesive surface to the adherend to be reinforced. In this respect, it is understood as a broader concept than the "reinforcing film" described below, which has the form of an adhesive sheet with a substrate.

[0025] The structure of a reinforcing film according to one embodiment is shown in FIG. 1. The reinforcing film 1 is configured as a substrate-attached single-sided adhesive sheet including a sheet-like supporting substrate 10 having a first surface 10A and a second surface 10B, and an adhesive layer 21 provided on the first surface 10A side. The adhesive layer 21 is fixed to the first surface 10A side of the supporting substrate 10. The reinforcing film 1 is used by attaching the adhesive layer 21 to an adherend. The reinforcing film 1 before use (i.e., before being attached to an adherend) can be a component of a release-liner-attached reinforcing film 100 in which the surface (adhesive surface) 21A of the adhesive layer 21 is in contact with a release liner 31, at least the side facing the adhesive layer 21 being a release surface (release surface), as shown in FIG. As the release liner 31, for example, one configured to be a release surface by providing a release layer made of a release treatment agent on one side of a sheet-like substrate (liner substrate) can be preferably used. Alternatively, the release liner 31 may be omitted, a supporting substrate 10 having a release surface at its second surface 10B is used, and the reinforcing film 1 may be rolled up so that the adhesive surface 21A is in contact with the second surface 10B of the supporting substrate 10 (roll form). When attaching the reinforcing film 1 to an adherend, the release liner 31 or the second surface 10B of the supporting substrate 10 is peeled off from the adhesive surface 21A, and the exposed adhesive surface 21A is pressure-bonded to the adherend.

[0026] The structure of a reinforcing film according to another embodiment is shown in FIG. 2. The reinforcing film 2 is configured as a substrate-attached double-sided adhesive sheet including a sheet-like supporting substrate 10 having a first surface 10A and a second surface 10B, an adhesive layer 21 provided on the first surface 10A side, and an adhesive layer 22 provided on the second surface 10B side. The adhesive layer (first adhesive layer) 21 is fixed to the first surface 10A of the supporting substrate 10, and the adhesive layer (second adhesive layer) 22 is fixed to the second surface 10B of the supporting substrate 10. The reinforcing film 2 is used by attaching the adhesive layers 21 and 22 to different locations of an adherend. The locations to which the adhesive layers 21 and 22 are attached may be locations of different members, or may be different locations within a single member. As shown in Fig. 2, the reinforcing film 2 before use may be a component of a reinforcing film with a release liner 200 in which the surface (first adhesive surface) 21A of the pressure-sensitive adhesive layer 21 and the surface (second adhesive surface) 22A of the pressure-sensitive adhesive layer 22 are in contact with release liners 31, 32, each of which has a release surface on at least the side facing the pressure-sensitive adhesive layers 21, 22. As the release liners 31, 32, for example, a sheet-like substrate (liner substrate) may be preferably used, in which a release layer made of a release treatment agent is provided on one side of the substrate, so that the one side serves as the release surface. Alternatively, the release liner 32 may be omitted, and a release liner 31 having both sides as release surfaces may be used, which may be superimposed on the reinforcing film 2 and wound in a spiral shape to form a reinforcing film with a release liner in which the second adhesive surface 22A is in contact with the back surface of the release liner 31 (roll form).

[0027] The structure of a reinforcing film according to yet another embodiment is shown in FIG. 3. This reinforcing film 3 is configured as a substrate-less double-sided adhesive sheet made of an adhesive layer 21. The reinforcing film 3 is used by attaching a first adhesive surface 21A formed by one surface (first surface) of the adhesive layer 21 and a second adhesive surface 21B formed by the other surface (second surface) of the adhesive layer 21 to different positions on an adherend. As shown in FIG. 3, the reinforcing film 3 before use can be a component of a reinforcing film 300 with a release liner in which the first adhesive surface 21A and the second adhesive surface 21B are in contact with release liners 31 and 32, each of which has a release surface at least on the side facing the adhesive layer 21. Alternatively, the release liner 32 may be omitted, and a release liner 31 having release surfaces on both sides may be used, which is then overlapped with the reinforcing film 3 and rolled up in a spiral shape to form a reinforcing film with a release liner in which the second adhesive surface 21B is in contact with the back surface of the release liner 31 (roll form).

[0028] The reinforcing film may be in the form of a roll or a sheet, and may be cut, punched, or otherwise processed into an appropriate shape depending on the application or mode of use. The pressure-sensitive adhesive layer in the technology disclosed herein is typically formed continuously, but is not limited thereto, and may be formed in a regular or random pattern, such as a dotted or striped pattern.

[0029] <Adhesive layer> The reinforcing film disclosed herein includes a pressure-sensitive adhesive layer containing a polymer (A) and a polymer (B). Such a pressure-sensitive adhesive layer may be formed from a pressure-sensitive adhesive composition containing a polymer (A) that is a complete or partial polymer of a monomer raw material A, and a polymer (B). The form of the pressure-sensitive adhesive composition is not particularly limited, and may be in various forms, such as a solvent type, a water-dispersed type, a hot melt type, or an active energy ray curable type (e.g., a photocurable type).

[0030] (Polymer (A)) As the polymer (A) in the pressure-sensitive adhesive layer, an acrylic polymer can be preferably used. When an acrylic polymer is used as the polymer (A), good compatibility with the polymer (B) tends to be easily obtained. Good compatibility between the polymer (A) and the polymer (B) is preferable because it can contribute to reducing the initial adhesive strength and improving the adhesive strength after heating through improving the mobility of the polymer (B) in the pressure-sensitive adhesive layer. In addition, acrylic polymers, which have a high degree of freedom in molecular design, are suitable as pressure-sensitive adhesive materials that can improve adhesive properties and flexibility in a well-balanced manner. While limiting the amount of the nitrogen-containing monomer to a predetermined amount or less, N / W Zr The desired effect achieved by making the ratio (R) equal to or greater than a predetermined value is effectively achieved in a configuration in which an acrylic polymer is used as the polymer (A).

[0031] In the reinforcing film disclosed herein, the polymer (A) is typically the main component of the polymer components contained in the pressure-sensitive adhesive layer, i.e., a component that accounts for more than 50% by weight, and may be, for example, a component that accounts for 75% by weight or more, 85% by weight or more, 90% by weight or more, or 95% by weight or more (e.g., 97% by weight or more) of the above polymer components. In some embodiments, the polymer (A) may be, for example, a component that accounts for more than 50% by weight of the entire pressure-sensitive adhesive layer, a component that accounts for 70% by weight or more, a component that accounts for 80% by weight or more, a component that accounts for 90% by weight or more, or a component that accounts for 95% by weight or more (e.g., 97% by weight or more).

[0032] The polymer (A) contains at least a monomer unit derived from a nitrogen-containing monomer, and typically contains a monomer unit derived from a nitrogen-containing monomer and a monomer unit derived from an alkyl (meth)acrylate ester.

[0033] For example, the polymer (A) may be a polymer in which the amount of monomer units derived from (meth)acrylic acid alkyl esters contained in 100 parts by weight of the polymer (A) is 50 parts by weight or more, that is, a polymer in which 50% by weight or more of the total amount of the monomer components (monomer raw material A) for preparing the polymer (A) is a (meth)acrylic acid alkyl ester. The (meth)acrylic acid alkyl ester may be a monomer having 1 to 20 carbon atoms (i.e., C 1-20 Of the monomer raw materials A, (meth)acrylic acid alkyl esters having linear or branched alkyl groups are preferably used. 1-20 The proportion of alkyl ester may be, for example, 50% by weight or more, or 60% by weight or more. In some preferred embodiments, the (meth)acrylic acid C in the monomer raw material A is 1-20 The proportion of alkyl ester is 70% by weight or more, more preferably 80% by weight or more, and even more preferably 85% by weight or more. By using a polymer (A) having such a monomer composition, it is easy to obtain a pressure-sensitive adhesive that has a good balance between increased adhesive strength and flexibility. In addition, from the viewpoint of easily obtaining the effect of using a nitrogen-containing monomer, (meth)acrylic acid C in the monomer raw material A is preferably used. 1-20 The proportion of alkyl ester is suitably 99.9% by weight or less or 99.8% by weight or less, and may be 99.5% by weight or less, or may be 99% by weight or less. In some embodiments, the proportion of (meth)acrylic acid C in the monomer raw material A is 99.9% by weight or less or 99.8% by weight or less. 1-20 The proportion of alkyl esters may be, for example, 98% by weight or less, 95% by weight or less, or 92% by weight or less.

[0034] (Meth)acrylic acid C 1-20Non-limiting examples of alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl ... and isopropyl (meth)acrylate. Examples of such acrylates include isooctyl, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0035] Among these, at least (meth)acrylic acid C 1-18 It is preferable to use an alkyl ester, and at least (meth)acrylic acid C 1-14 It is more preferred to use alkyl esters. In some embodiments, the acrylic polymer is (meth)acrylic acid C 4-12 Alkyl ester (preferably acrylic acid C 4-10 Alkyl esters, such as acrylic acid C 6-10 The acrylic polymer may contain at least one selected from the group consisting of n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA) as a monomer unit. For example, an acrylic polymer containing one or both of n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA) is preferred, and an acrylic polymer containing at least 2EHA is particularly preferred.

[0036] In some preferred embodiments, the acrylic acid C is used as the monomer raw material A for preparing the polymer (A). 6-10 Alkyl ester (preferably acrylic acid C 8-9The proportion of alkyl ester, typically 2EHA) is 70% by weight or more, more preferably 80% by weight or more, and even more preferably 85% by weight or more. An acrylic polymer having such a monomer composition is particularly suitable for achieving the effects of the technology disclosed herein. In addition, acrylic acid C in the monomer raw material A is 6-10 Alkyl ester (preferably acrylic acid C 8-9 The proportion of the alkyl ester (typically 2EHA) may be, for example, 99.9% by weight or less, 99.5% by weight or less, or 99% by weight or less, and from the viewpoint of initial light peelability and the like, it may be 98% by weight or less, 95% by weight or less, or 92% by weight or less.

[0037] The monomer component (monomer raw material A) for preparing the polymer (A) includes a nitrogen-containing monomer, i.e., a monomer containing a nitrogen atom. By appropriately using the nitrogen-containing monomer, the cohesive strength and polarity of the adhesive can be adjusted, and the adhesive strength after the adhesive strength increase (for example, the adhesive strength to a polyimide film) can be improved. The nitrogen-containing monomer can be used alone or in appropriate combination of two or more kinds.

[0038] Non-limiting examples of nitrogen-containing monomers include: Monomers having a nitrogen atom-containing ring: for example, N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloylmorpholine, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, N-vinylisothiazole, N-vinylpyridazine, etc.; For example, monomers having a succinimide skeleton, such as N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, and N-(meth)acryloyl-8-oxyhexamethylene succinimide; Maleimides, such as, for example, N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, N-phenylmaleimide, and the like; and For example, itaconimides such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, and N-laurylitaconimide. Amide group-containing monomers: for example, (meth)acrylamide; N,N-dialkyl(meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(t-butyl)(meth)acrylamide; N-alkyl(meth)acrylamides such as N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, and Nn-butyl(meth)acrylamide; N-vinyl carboxylic acid amides such as N-vinylacetamide; monomers having a hydroxyl group and an amide group, for example, N-(2-hydroxyethyl)(meth)acrylamide; N-hydroxyalkyl (meth)acrylamide, such as N-(2-hydroxypropyl) (meth)acrylamide, N-(1-hydroxypropyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(2-hydroxybutyl) (meth)acrylamide, N-(3-hydroxybutyl) (meth)acrylamide, and N-(4-hydroxybutyl) (meth)acrylamide; monomers having an alkoxy group and an amide group, such as N-alkoxyalkyl (meth)acrylamide, such as N-methoxymethyl (meth)acrylamide, N-methoxyethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide; and others, such as N,N-dimethylaminopropyl (meth)acrylamide. Aminoalkyl (meth)acrylates: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate. Cyano group-containing monomers: for example, acrylonitrile, methacrylonitrile, etc. Isocyanate group-containing monomers: for example, 2-isocyanatoethyl (meth)acrylate.

[0039] In some embodiments, from the viewpoint of ease of synthesis of the polymer (A) and copolymerizability with other monomer components (e.g., (meth)acrylic acid alkyl esters), etc., a nitrogen-containing monomer having an N-vinyl group or an N-(meth)acryloyl group (e.g., one or more selected from the group consisting of a monomer having a nitrogen atom-containing ring, an amide group-containing monomer, and an aminoalkyl (meth)acrylate) can be preferably used as the nitrogen-containing monomer.

[0040] The amount of the nitrogen-containing monomer used is the amount W of the nitrogen-containing monomer contained in 100 parts by weight of the polymer (A). N W is an amount such that the nitrogen-containing monomer is 14% by weight or less of the total amount of the monomer components (monomer raw material A) used to prepare the polymer (A). N By limiting the amount of the nitrogen-containing monomer in the monomer raw material A to 14 parts by weight or less, the flexibility of the adhesive in the low temperature range can be improved (for example, the storage modulus at -20°C can be reduced), and flexibility suitable for repeated bending and flexing can be achieved. From the viewpoint of improving the flexibility, in some embodiments, the content of the nitrogen-containing monomer in the monomer raw material A is 12% by weight or less (i.e., W N It is suitable that the nitrogen-containing monomer is used in an amount of 12 parts by weight or less, advantageously 10% by weight or less, preferably 8.0% by weight or less, more preferably 5.0% by weight or less, and may be 4.0% by weight or less, 3.0% by weight or less, or 2.0% by weight or less. The amount of the nitrogen-containing monomer used is usually 0.01% by weight or more (preferably 0.1% by weight or more, for example 0.3% by weight or more) of the monomer raw material A. From the viewpoint of easily obtaining a higher effect of use, in some embodiments, the amount of the nitrogen-containing monomer used is 0.5% by weight or more of the monomer raw material A (i.e., W N The content of the sucrose ionizing agent may be 0.5 parts by weight or more), or may be 0.7% by weight or more, 1.0% by weight or more, 1.2% by weight or more, or 1.5% by weight or more.

[0041] In some embodiments, the monomer raw material A may contain a monomer having a nitrogen atom-containing ring as the nitrogen-containing monomer. By adopting a monomer having a nitrogen atom-containing ring as at least a part of the nitrogen-containing monomer, the compatibility between the polymer (A) formed from the monomer raw material A and the polymer (B) tends to improve. This improves the increase in adhesive strength, making it easier to obtain a reinforcing film with high adhesive strength (e.g., adhesive strength to a polyimide film) after the increase.

[0042] The monomer having a nitrogen atom-containing ring can be selected from the above examples, and can be used alone or in combination of two or more. In some embodiments, the monomer raw material A preferably contains at least one monomer selected from the group consisting of N-vinyl cyclic amides and cyclic amides having a (meth)acryloyl group as the monomer having a nitrogen atom-containing ring.

[0043] Specific examples of N-vinyl cyclic amides include N-vinyl-2-pyrrolidone, N-vinyl-2-piperidone, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, etc. Preferred examples are N-vinyl-2-pyrrolidone (NVP) and N-vinyl-2-caprolactam. Specific examples of cyclic amides having a (meth)acryloyl group include N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloylmorpholine, etc. A suitable example is N-acryloylmorpholine (ACMO).

[0044] The amount of the monomer having a nitrogen atom-containing ring to be used is not particularly limited, and the amount W RN [Parts by weight] is the amount W of the nitrogen-containing monomer described above. NIn other words, the amount [wt %] of the monomer having a nitrogen atom-containing ring in the total amount of the monomer raw material A can be appropriately set within a range not exceeding the amount [wt %] of the nitrogen-containing monomer in the total amount of the monomer raw material A. Therefore, the amount W of the monomer having a nitrogen atom-containing ring contained in 100 parts by weight of the polymer (A) RN is 14 parts by weight or less, and the amount of the monomer having a nitrogen atom-containing ring of the total amount of monomer feed A is 14 weight percent or less. In some embodiments, the amount of the monomer having a nitrogen atom-containing ring used is 12 weight percent or less of monomer feed A (i.e., W RN It is appropriate that the amount of the monomer having a nitrogen atom-containing ring used is 12 parts by weight or less), advantageously 10% by weight or less, preferably 8.0% by weight or less, more preferably 5.0% by weight or less, and may be 4.0% by weight or less, 3.0% by weight or less, or 2.0% by weight or less. The amount of the monomer having a nitrogen atom-containing ring used is usually 0.01% by weight or more (preferably 0.1% by weight or more, for example 0.3% by weight or more) of the monomer raw material A, and from the viewpoint of easily obtaining a higher effect of use, it is appropriate that the amount of the monomer having a nitrogen atom-containing ring used is 0.5% by weight or more (i.e., W RN The content of the sucrose ionizing agent may be 0.5 parts by weight or more), or may be 0.7% by weight or more, 1.0% by weight or more, 1.2% by weight or more, or 1.5% by weight or more.

[0045] In an embodiment using a monomer having a nitrogen atom-containing ring, the ratio of the monomer having a nitrogen atom-containing ring among the nitrogen-containing monomers contained in the monomer raw material A may be, for example, 30% by weight or more, preferably 50% by weight or more, more preferably 70% by weight or more, 85% by weight or more, 90% by weight or more, 95% by weight or more, or 100% by weight or more. In some embodiments, the amount of nitrogen-containing monomers not corresponding to monomers having a nitrogen atom-containing ring in the total amount of the monomer raw material A is, for example, 5% by weight or less, preferably 3% by weight or less, more preferably 1% by weight or less, 0.5% by weight or less, or 0.1% by weight or less. It is not necessary to use a nitrogen-containing monomer not corresponding to a monomer having a nitrogen atom-containing ring. In some embodiments, a suitable combination of a monomer having a nitrogen atom-containing ring and another nitrogen-containing monomer may be used, and in such an embodiment, the ratio of the monomer having a nitrogen atom-containing ring among the nitrogen-containing monomers contained in the monomer raw material A may be, for example, 98% by weight or less, 93% by weight or less, 80% by weight or less, 60% by weight or less, or 40% by weight or less.

[0046] The monomer raw material A may contain, as necessary, other monomers (copolymerizable monomers) that are copolymerizable with the (meth)acrylic acid alkyl ester, in addition to the nitrogen-containing monomer and typically further the (meth)acrylic acid alkyl ester. As the copolymerizable monomer, a monomer having a polar group (e.g., a carboxy group, a hydroxyl group, etc.) can be suitably used. The monomer having a polar group can be useful for introducing a crosslinking point into the polymer (A) or for increasing the cohesive force of the polymer (A). The copolymerizable monomer can be used alone or in combination of two or more kinds.

[0047] Non-limiting examples of copolymerizable monomers include the following: Hydroxyl group-containing monomers: for example, hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. Carboxy group-containing monomers: for example, acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, isocrotonic acid, and the like. Acid anhydride group-containing monomers: for example, maleic anhydride, itaconic anhydride. Monomers containing a sulfonic acid group or a phosphoric acid group: for example, styrene sulfonic acid, allyl sulfonic acid, sodium vinyl sulfonate, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid, 2-hydroxyethyl acryloyl phosphate, etc. Epoxy group-containing monomers: for example, epoxy group-containing acrylates such as glycidyl (meth)acrylate and 2-ethyl glycidyl ether (meth)acrylate, allyl glycidyl ether, and glycidyl ether (meth)acrylate. Alkoxy group-containing monomers: for example, alkoxyalkyl (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, and ethoxypropyl (meth)acrylate; alkoxyalkylene (meth)acrylates such as methoxyethylene glycol (meth)acrylate and methoxypolypropylene glycol (meth)acrylate. (Meth)acrylic acid esters having an alicyclic hydrocarbon group: for example, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and the like. (Meth)acrylic acid esters having an aromatic hydrocarbon group: for example, phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, and the like. Vinyl ethers: for example, vinyl alkyl ethers such as methyl vinyl ether and ethyl vinyl ether. Vinyl esters: for example, vinyl acetate, vinyl propionate, etc. Aromatic vinyl compounds: for example, styrene, α-methylstyrene, vinyltoluene, etc. Olefins: For example, ethylene, butadiene, isoprene, isobutylene, etc. Other examples include heterocyclic ring-containing (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate, halogen atom-containing (meth)acrylates such as vinyl chloride and fluorine atom-containing (meth)acrylates, silicon atom-containing (meth)acrylates such as silicone (meth)acrylate, and (meth)acrylic acid esters obtained from alcohols derived from terpene compounds.

[0048] When such a copolymerizable monomer is used, the amount of the copolymerizable monomer is not particularly limited, but is usually suitably 0.01% by weight or more of the monomer raw material A. From the viewpoint of better exerting the effect of using the copolymerizable monomer (for example, the effect of improving the cohesiveness), the amount of the copolymerizable monomer may be 0.1% by weight or more of the monomer raw material A, or may be 0.5% by weight or more. In some embodiments, the content of the copolymerizable monomer in the monomer raw material A is preferably 0.7% by weight or more, more preferably 1% by weight or more, may be 3% by weight or more, may be 5% by weight or more, may be 7% by weight or more (for example, 8% by weight or more). In addition, the amount of the copolymerizable monomer may be, for example, 50% by weight or less of the monomer raw material A, suitably 30% by weight or less, preferably 20% by weight or less, more preferably 15% by weight or less (for example, 12% by weight or less), may be 10% by weight or less, 8% by weight or less, 6% by weight or less, 4% by weight or less, or 2% by weight or less. Limiting the amount of copolymerizable monomer used can be advantageous from the standpoint of improving the flexibility of the PSA (particularly, flexibility in the low temperature range).

[0049] In some preferred embodiments, the monomer raw material A includes a hydroxyl group-containing monomer. By using the hydroxyl group-containing monomer, the cohesive strength and polarity of the adhesive can be adjusted, and the effects of the technology disclosed herein can be preferably realized. In addition, the hydroxyl group-containing monomer provides a reaction site with a crosslinking agent (e.g., an isocyanate-based crosslinking agent) described later, and can increase the cohesive strength of the adhesive through a crosslinking reaction.

[0050] As the hydroxyl group-containing monomer, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, N-(2-hydroxyethyl)(meth)acrylamide, etc. can be suitably used. Among them, preferred examples include 2-hydroxyethyl acrylate (HEA) and 4-hydroxybutyl acrylate (4HBA). From the viewpoint of improving the cohesive strength while suppressing the decrease in flexibility of the adhesive, 4HBA is particularly preferred.

[0051] The amount of the hydroxyl group-containing monomer used is not particularly limited, and is usually appropriate to be 40% by weight or less of the monomer raw material A, may be 30% by weight or less, or may be 20% by weight or less. In some embodiments, from the viewpoint of the flexibility of the adhesive (particularly, flexibility in the low temperature range), the content of the hydroxyl group-containing monomer in the monomer raw material A is preferably 15% by weight or less (e.g., less than 15% by weight), more preferably 12% by weight or less, may be 10% by weight or less, 8% by weight or less, 6% by weight or less, 4% by weight or less, or 2% by weight or less. By limiting the amount of the hydroxyl group-containing monomer used, the mobility of the polymer (B) in the adhesive layer is improved, and it is easy to realize an increase in adhesive strength. In addition, the amount of the hydroxyl group-containing monomer used is appropriate to be 0.01% by weight or more of the monomer raw material A (preferably 0.1% by weight or more, for example 0.5% by weight or more). From the viewpoint of obtaining an appropriate cohesive strength, in some embodiments, the amount of the hydroxyl group-containing monomer used is preferably 0.7% by weight or more of the monomer raw material A, more preferably 1% by weight or more, even 3% by weight or more, 5% by weight or more, or 7% by weight or more (for example, 8% by weight or more).

[0052] In some embodiments, a nitrogen-containing monomer (e.g., a monomer having a nitrogen atom-containing ring) and a hydroxyl-containing monomer can be used in combination as the copolymerizable monomer. In this case, the total amount of the nitrogen-containing monomer and the hydroxyl-containing monomer can be, for example, 0.1% by weight or more of the monomer raw material A, preferably 1% by weight or more, more preferably 3% by weight or more, even more preferably 5% by weight or more, particularly preferably 7% by weight or more (e.g., 9% by weight or more), and may be 10% by weight or more, 15% by weight or more, 20% by weight or more, or 25% by weight or more. In addition, the total amount of the nitrogen-containing monomer and the hydroxyl-containing monomer can be, for example, 50% by weight or less of the monomer raw material A, and preferably 30% by weight or less. In some preferred embodiments, the total amount of the nitrogen-containing monomer and the hydroxyl-containing monomer is 20% by weight or less of the monomer raw material A, more preferably 15% by weight or less (e.g., 12% by weight or less).

[0053] In an embodiment in which the monomer raw material A contains a combination of a nitrogen-containing monomer (e.g., a monomer having a nitrogen atom-containing ring) and a hydroxyl group-containing monomer, the content of the nitrogen-containing monomer in the monomer raw material A (W N ) and the content of hydroxyl group-containing monomers (W OH The relationship (weight basis) between W and W is not particularly limited. N / W OH may be, for example, 0.01 or more, and is usually 0.05 or more, may be 0.10 or more, or may be 0.12 or more. N / W OH may be, for example, 10 or less, and is usually suitably 1 or less, and is preferably 0.50 or less, or may be 0.30 or less, or may be 0.20 or less, or may be 0.15 or less.

[0054] In some embodiments, it is preferable that the monomer raw material A does not contain a monomer (monomer S1) having a polyorganosiloxane skeleton, which is preferably used as a constituent of the monomer raw material B described later, or that the content of the monomer is less than 10% by weight (more preferably less than 5% by weight, for example less than 2% by weight) of the monomer raw material A. With the monomer raw material A having such a composition, a reinforcing film that preferably achieves both initial reworkability and strong adhesion after the adhesion strength increases can be preferably realized. For the same reason, in some other embodiments, it is preferable that the monomer raw material A does not contain monomer S1, or if it contains monomer S1, its content (weight basis) is lower than the content of monomer S1 in the monomer raw material B.

[0055] Glass transition temperature T of polymer (A) A is not particularly limited and can be selected to obtain preferred properties in the reinforcing film disclosed herein. In some embodiments, T A A polymer (A) having a temperature of less than 0° C. can be preferably used. Since a pressure-sensitive adhesive containing such a polymer (A) exhibits appropriate fluidity (e.g., mobility of the polymer chain contained in the pressure-sensitive adhesive), it is suitable for realizing a reinforcing film whose adhesive strength increases to a predetermined value or more upon heating. The reinforcing film disclosed herein has a temperature of less than 0° C.A may be preferably carried out using a polymer (A) having a temperature of less than -10°C, less than -20°C, less than -30°C or less than -35°C. A may be less than −40° C. or less than −45° C. In some embodiments, in order to improve flexibility in the low temperature range, T A is preferably −50° C. or lower, more preferably −55° C. or lower, and even more preferably −58° C. or lower, and may be −60° C. or lower, −62° C. or lower, or −65° C. or lower. A There is no particular restriction on the lower limit of T. From the viewpoint of material availability and improving the cohesive strength of the adhesive layer, T A Preferably, the polymer (A) has a temperature of -80°C or higher, -75°C or higher, or -70°C or higher. A may be, for example, −65° C. or higher, or −63° C. or higher.

[0056] In this specification, the glass transition temperature (Tg) of a polymer refers to a nominal value described in literature, catalogs, etc., or a Tg calculated by the Fox formula based on the composition of the monomer raw materials used in the preparation of the polymer. The Fox formula is a relational expression between the Tg of a copolymer and the glass transition temperature Tgi of a homopolymer obtained by homopolymerizing each of the monomers constituting the copolymer, as shown below. 1 / Tg=Σ(Wi / Tgi) In the above Fox formula, Tg represents the glass transition temperature (unit: K) of the copolymer, Wi represents the weight fraction (copolymerization ratio by weight) of monomer i in the copolymer, and Tgi represents the glass transition temperature (unit: K) of a homopolymer of monomer i. When the target polymer for which Tg is specified is a homopolymer, the Tg of the homopolymer and the Tg of the target polymer are the same.

[0057] The glass transition temperature of the homopolymer used to calculate Tg is a value listed in a publicly known document. Specifically, the values ​​are listed in "Polymer Handbook" (3rd Edition, John Wiley & Sons, Inc., 1989). For monomers for which multiple values ​​are listed in the Polymer Handbook, the highest value is used.

[0058] As the glass transition temperature of a homopolymer of a monomer not described in the Polymer Handbook, a value obtained by the following measurement method is used. Specifically, 100 parts by weight of monomer, 0.2 parts by weight of 2,2'-azobisisobutyronitrile, and 200 parts by weight of ethyl acetate as a polymerization solvent are charged into a reactor equipped with a thermometer, a stirrer, a nitrogen inlet tube, and a reflux condenser tube, and stirred for 1 hour while passing nitrogen gas through it. After removing oxygen from the polymerization system in this way, the temperature is raised to 63°C and the reaction is carried out for 10 hours. Then, the mixture is cooled to room temperature to obtain a homopolymer solution with a solid content concentration of 33% by weight. Next, this homopolymer solution is cast and applied onto a release liner, and dried to prepare a test sample (sheet-shaped homopolymer) with a thickness of about 2 mm. This test sample is punched out into a disk with a diameter of 7.9 mm, sandwiched between parallel plates, and the viscoelasticity is measured in shear mode using a viscoelasticity tester (manufactured by TA Instruments Japan, model name "DHR-2") while applying a shear strain of 1 Hz frequency and at a temperature range of -70°C to 150°C at a heating rate of 5°C / min. The temperature corresponding to the peak top temperature of tan δ is taken as the Tg of the homopolymer.

[0059] Although not particularly limited, the weight average molecular weight (Mw) of the polymer (A) is usually about 20×10 4 It is appropriate that the Mw of the polymer (A) is 30×10 or more. A PSA exhibiting good cohesiveness is easily obtained by using the polymer (A) having such Mw. From the viewpoint of obtaining higher cohesive strength, in some preferred embodiments, the Mw of the polymer (A) is, for example, 30×10 4 It may be 40×10 or more. 4 More than 50 x 10 is fine. 4More than 60 x 10 is fine. 4 More than 80 x 10 is fine. 4 The Mw of the polymer (A) is usually about 500×10 4 It is appropriate that the Mw of the polymer (A) is not too high. Since the polymer (A) with such Mw is likely to form an adhesive that exhibits moderate fluidity (mobility of the polymer chain), it is suitable for realizing a reinforcing film that has low initial adhesive strength after application and a large increase in adhesive strength. It is also preferable from the viewpoint of improving compatibility with the polymer (B) that the Mw of the polymer (A) is not too high. In some preferred embodiments, the Mw of the polymer (A) is, for example, 250×10 4 may be less than or equal to 200 x 10 4 Less than 150×10 is also fine. 4 Less than 100 x 10 4 Less than 70×10 is fine. 4 The following is also fine.

[0060] In this specification, the Mw of the polymer (A) and the polymer (B) described later can be determined in terms of polystyrene by gel permeation chromatography (GPC). More specifically, the Mw can be measured according to the method and conditions described in the examples described later.

[0061] The method for obtaining the polymer (A) is not particularly limited, and various polymerization methods such as solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, and photopolymerization can be appropriately adopted. In some embodiments, the solution polymerization method can be preferably adopted. The polymerization temperature when carrying out the solution polymerization can be appropriately selected depending on the type of monomer and solvent used, the type of polymerization initiator, and the like, and can be, for example, about 20°C to 170°C (typically about 40°C to 140°C).

[0062] The initiator used for polymerization can be appropriately selected from conventionally known thermal polymerization initiators, photopolymerization initiators, etc., depending on the polymerization method. The polymerization initiator can be used alone or in combination of two or more kinds.

[0063] Examples of the thermal polymerization initiator include azo-based polymerization initiators (e.g., 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionic acid) dimethyl, 4,4'-azobis-4-cyanovaleric acid, azobisisovaleronitrile, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(5-methyl-2 -imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis(2-methylpropionamidine)disulfate, 2,2'-azobis(N,N'-dimethyleneisobutylamidine)dihydrochloride, etc.); persulfates such as potassium persulfate; peroxide-based polymerization initiators (e.g., dibenzoyl peroxide, t-butyl permaleate, lauroyl peroxide, etc.); redox-based polymerization initiators, etc. The amount of the thermal polymerization initiator used is not particularly limited, but can be, for example, within the range of 0.01 to 5 parts by weight, preferably 0.05 to 3 parts by weight, relative to 100 parts by weight of the monomer component (monomer raw material A) used in the preparation of the acrylic polymer.

[0064] The photopolymerization initiator is not particularly limited, but for example, a benzoin ether-based photopolymerization initiator, an acetophenone-based photopolymerization initiator, an α-ketol-based photopolymerization initiator, an aromatic sulfonyl chloride-based photopolymerization initiator, a photoactive oxime-based photopolymerization initiator, a benzoin-based photopolymerization initiator, a benzyl-based photopolymerization initiator, a benzophenone-based photopolymerization initiator, a ketal-based photopolymerization initiator, a thioxanthone-based photopolymerization initiator, an acylphosphine oxide-based photopolymerization initiator, etc. can be used. The amount of the photopolymerization initiator used is not particularly limited, but for example, it can be in the range of 0.01 to 5 parts by weight, preferably 0.05 to 3 parts by weight, relative to 100 parts by weight of the monomer raw material A.

[0065] In some embodiments, the polymer (A) may be included in the pressure-sensitive adhesive composition for forming the pressure-sensitive adhesive layer in the form of a partial polymer (polymer syrup) obtained by irradiating a mixture of the monomer raw material A and a polymerization initiator with ultraviolet (UV) light to polymerize a part of the monomer component. The pressure-sensitive adhesive composition containing such a polymer syrup can be applied to a predetermined substrate and irradiated with ultraviolet light to complete the polymerization. That is, the polymer syrup can be understood as a precursor of the polymer (A). The pressure-sensitive adhesive layer disclosed herein can be formed, for example, using a pressure-sensitive adhesive composition containing the polymer syrup and polymer (B).

[0066] (Polymer (B)) The polymer (B) in the technology disclosed herein is a polymer of a monomer component (monomer raw material B) containing a monomer having a polyorganosiloxane skeleton (hereinafter also referred to as "monomer S1") and a (meth)acrylic monomer. The polymer (B) can be said to be a copolymer of the monomer S1 and a (meth)acrylic monomer. The polymer (B) can be used alone or in combination of two or more. The polymer (B) can function as an adhesive strength increase retarder that suppresses the adhesive strength at the initial stage of application to an adherend due to the low polarity and mobility of the polyorganosiloxane structure derived from the monomer S1, and increases the adhesive strength to the adherend by heating. The monomer S1 is not particularly limited, and any monomer containing a polyorganosiloxane skeleton can be used. The monomer S1 promotes uneven distribution of the polymer (B) on the surface of the adhesive layer in the reinforcing film before use (before application to the adherend) due to the low polarity derived from its structure, and exhibits light peelability (low adhesiveness) at the initial stage of application. As the monomer S1, a structure having a polymerizable reactive group at one end can be preferably used. According to a configuration including such a monomer S1 unit and a (meth)acrylic monomer unit, a polymer (B) having a polyorganosiloxane skeleton in a side chain is formed. The polymer (B) having such a structure is likely to have a low initial adhesive strength and a high adhesive strength after heating due to the mobility and ease of movement of the side chain. In some embodiments, the monomer S1 is preferably one having a polymerizable reactive group at one end and not having a functional group at the other end that causes a crosslinking reaction with the polymer (A). The polymer (B) in which the monomer S1 having such a structure is copolymerized is likely to have a low initial adhesive strength and a high adhesive strength after heating due to the mobility of the polyorganosiloxane structure derived from the monomer S1.

[0067] As the monomer S1, for example, a compound represented by the following general formula (1) or (2) can be used. More specifically, examples of the silicone oil having a reactive end, manufactured by Shin-Etsu Chemical Co., Ltd., include X-22-174ASX, X-22-2426, X-22-2475, and KF-2012. The monomer S1 can be used alone or in combination of two or more. [ka] [ka] Here, R in the above general formulas (1) and (2) 3 is hydrogen or methyl, and R 4 is a methyl group or a monovalent organic group, and m and n are integers of 0 or greater.

[0068] The functional group equivalent of the monomer S1 can be an appropriate value within a range where the desired effect is achieved by using the monomer S1, and is not limited to a specific range. From the viewpoint of sufficiently suppressing the initial adhesive strength, the functional group equivalent is, for example, 100 g / mol or more, or 200 g / mol or more, and is suitably 300 g / mol or more (for example, 500 g / mol or more), preferably 800 g / mol or more, and more preferably 1500 g / mol or more. In a particularly preferred embodiment, from the viewpoint of achieving both low adhesive strength at the initial stage of application and an increase in adhesive strength after heating at a high level, the functional group equivalent is suitably 2000 g / mol or more, and may be, for example, 2500 g / mol or more, 3000 g / mol or more, 4000 g / mol or more, or 5000 g / mol or more. In some other embodiments, the functional group equivalent may be, for example, 9000 g / mol or more, 12000 g / mol or more, or 15000 g / mol or more.

[0069] From the viewpoint of sufficiently increasing the adhesive strength, the functional group equivalent is, for example, suitably 30000 g / mol or less, may be 20000 g / mol or less, may be less than 15000 g / mol, or may be less than 10000 g / mol. In some preferred embodiments, the functional group equivalent of the monomer S1 is 7000 g / mol or less, more preferably 5500 g / mol or less, even more preferably 5000 g / mol or less, may be 4500 g / mol or less, may be 4200 g / mol or less, may be 4000 g / mol or less, may be 3500 g / mol or less, or may be 3200 g / mol or less. When the functional group equivalent weight of monomer S1 is within the above range, compatibility within the adhesive layer (e.g., compatibility with polymer (A)) is likely to be good, the mobility of the polyorganosiloxane skeleton (chain) of polymer (B) is good, and the mobility of polymer (B) can be easily adjusted within an appropriate range, making it easier to realize an adhesive layer that achieves both a high level of initial low adhesion and an increase in adhesive strength after heating.

[0070] Here, the term "functional group equivalent" refers to the weight of the main skeleton (e.g., polydimethylsiloxane) bound to one functional group. The unit g / mol is calculated based on 1 mol of functional group. The functional group equivalent of the monomer S1 can be calculated, for example, based on nuclear magnetic resonance (NMR). 1 It can be calculated from the H-NMR (proton NMR) spectrum intensity. 1 The functional group equivalent weight (g / mol) of monomer S1 was calculated based on the H-NMR spectrum intensity as follows: 1 This can be done based on a general structural analysis method related to H-NMR spectrum analysis, and if necessary, by referring to the description in Japanese Patent No. 5951153. In the functional group equivalent of the monomer S1, the functional group means a polymerizable functional group (for example, an ethylenically unsaturated group such as a (meth)acryloyl group, a vinyl group, or an allyl group).

[0071] In addition, when two or more kinds of monomers having different functional group equivalents are used as the monomer S1, the functional group equivalent of the monomer S1 can be an arithmetic average value. That is, when n kinds of monomers having different functional group equivalents (monomer S11, monomer S12, ..., monomer S1 n The functional group equivalent of the monomer S1 consisting of (a) can be calculated by the following formula. Functional group equivalent of monomer S1 (g / mol) = (functional group equivalent of monomer S11 × amount of monomer S11 + functional group equivalent of monomer S12 × amount of monomer S12 + + monomer S1 n Functional group equivalent weight × monomer S1 n (amount of monomer S11 + amount of monomer S12 + + monomer S1 n (amount of mixture)

[0072] The content of the monomer S1 can be an appropriate value within a range in which the desired effect is achieved using the monomer S1, and is not limited to a specific range. From the viewpoint of sufficiently suppressing the initial adhesive strength, in some embodiments, the content of the monomer S1 in the total amount of the monomer components (monomer raw material B) for preparing the polymer (B) may be, for example, 5% by weight or more, and from the viewpoint of better exerting the effect as an adhesive strength increase retarder, it is preferably 10% by weight or more, more preferably 12% by weight or more, even more preferably 15% by weight or more, particularly preferably 18% by weight or more, and may be 20% by weight or more. In addition, from the viewpoint of polymerization reactivity and compatibility, the content of the monomer S1 in the monomer raw material B may be, for example, 80% by weight or less, and it is appropriate to set it to 60% by weight or less, preferably 50% by weight or less, more preferably 40% by weight or less, and even more preferably 30% by weight or less. By setting the polymerization ratio of the monomer S1 within an appropriate range, the increase in adhesive strength can be suitably expressed.

[0073] The monomer raw material B contains, in addition to the monomer S1, a (meth)acrylic monomer copolymerizable with the monomer S1. By using one or more (meth)acrylic monomers, the mobility of the polymer (B) in the adhesive layer can be suitably adjusted. This can also be useful for improving the compatibility between the polymer (B) and the polymer (A). The polymer (B) containing a (meth)acrylic monomer unit can be well compatible with the polymer (A) (acrylic polymer), and therefore, by improving the mobility of the polymer (B) in the adhesive layer, it is easy to reduce the initial adhesive strength and improve the adhesive strength after heating.

[0074] In the polymer (B) used in the technology disclosed herein, the composition of the (meth)acrylic monomer contained in the monomer raw material B is such that the glass transition temperature T B1 is the glass transition temperature T of polymer (A). A It is preferable that the temperature is set higher than T B1 can be set to be higher than 0° C., for example. Here, the glass transition temperature T B1 means the Tg calculated by the Fox formula based on the composition of only the (meth)acrylic monomer among the monomer components used in the preparation of the polymer (B). B1 The glass transition temperature T can be calculated from the glass transition temperature of the homopolymer of each (meth)acrylic monomer and the weight fraction of each (meth)acrylic monomer in the total amount of the (meth)acrylic monomers by applying the above-mentioned Fox formula to only the (meth)acrylic monomers among the monomer components used in the preparation of the polymer (B). B1 The initial adhesive strength is easily suppressed by the polymer (B) having a relatively high glass transition temperature T B1 By using the polymer (B) having a relatively high T (typically higher than 0° C.), a reinforcing film having a large rate of increase in adhesive strength can be easily obtained.

[0075] In some preferred embodiments, T B1is 10° C. or higher, more preferably 30° C. or higher, further preferably 40° C. or higher, and may be 45° C. or higher. B1 As the temperature increases, the initial adhesive strength tends to be better suppressed. B1 It is considered that, when the polymer (B) has a temperature of at least a predetermined temperature, the increase in the mobility and movement of the polyorganosiloxane structural portion that accompanies an increase in temperature to room temperature or to a region somewhat higher than room temperature is effectively suppressed by the monomer units derived from the (meth)acrylic monomer contained in the polymer (B), and the low adhesion caused by the presence of the polyorganosiloxane structural portion can be better maintained. From the viewpoint of more stably maintaining the low adhesion at the initial stage of application, in some embodiments, T B1 may be, for example, 50° C. or more, 55° C. or more, or 60° C. or more. B1 For example, T may be 120° C. or less, or may be 100° C. or less. B1 When T is low, the adhesive strength tends to increase more easily by heating. B1 is, for example, 90° C. or less, more preferably 70° C. or less, further preferably 60° C. or less, and particularly preferably 55° C. or less (for example, 50° C. or less).

[0076] T B1 From the viewpoint of easily exerting the effect of appropriately setting, the total amount of monomer S1 and the (meth)acrylic monomer in all monomer components for preparing polymer (B) may be, for example, 50% by weight or more, 70% by weight or more, 85% by weight or more, 90% by weight or more, 95% by weight or more, or substantially 100% by weight.

[0077] Glass transition temperature T of polymer (B) B is not particularly limited and can be selected so as to obtain preferred properties in the reinforcing film disclosed herein. B may be, for example, less than 50° C., 30° C. or less, 20° C. or less, 15° C. or less, or 10° C. or less.B When the T of the polymer (B) is lowered, the mobility (typically temperature-sensitive mobility) of the polymer (B) is improved, and the adhesive strength can be significantly increased. In some preferred embodiments, the T of the polymer (B) B is 5° C. or less, may be less than 0° C., may be −5° C. or less, or may be −10° C. or less. In some embodiments, the T B may be, for example, −40° C. or higher, or −30° C. or higher. B The higher the T of the polymer (B), the more the polymer (B) unevenly distributed on the surface side of the pressure-sensitive adhesive layer when attached to an adherend contributes to a decrease in the initial adhesive strength, and the more the adhesive layer tends to have excellent easy peelability at the initial stage of attachment. B is -20°C or higher, and may be -15°C or higher. B By setting this within an appropriate range, it is possible to control the easy peelability at the initial stage of application and the increase in adhesive strength after heating within preferred ranges.

[0078] In some embodiments, the composition of the monomer components for preparing the polymer (B) is T B1 T B To be higher, i.e. T B1 -T B can be set to be greater than 0° C. With such a composition, the effect of adjusting the mobility of the polymer (B) by the composition of the (meth)acrylic monomer contained in the monomer component is easily exhibited. B1 -T B For example, T may be about 40° C. to 100° C., or about 50° C. to 90° C. In some preferred embodiments, T B1 -T B is 45° C. or more, more preferably 50° C. or more, and even more preferably 55° C. or more (for example, 58° C. or more). B1 -T B is preferably 80° C. or less, more preferably 70° C. or less, and further preferably 65° C. or less (for example, 62° C. or less).

[0079] From the viewpoint of facilitating control of the mobility of the polymer (B) in the pressure-sensitive adhesive layer, in some embodiments, the composition of the monomer components for preparing the polymer (B) is selected from the group consisting of a monomer having a glass transition temperature T A In relation to T B T A 20°C higher than T B -T A In some preferred embodiments, T B -T A is, for example, 30° C. or higher, more preferably 40° C. or higher, and even more preferably 50° C. or higher, and may be 60° C. or higher, or may be 70° C. or higher. B -T A For example, the temperature may be 130°C or less, 120°C or less, preferably 100°C or less, more preferably 80°C or less, and even more preferably 65°C or less, may be 55°C or less, or may be 45°C or less.

[0080] Examples of (meth)acrylic monomers that can be used for monomer raw material B include (meth)acrylic acid alkyl esters. The term "alkyl" as used here refers to chain-like (including linear and branched) alkyl (groups) and does not include alicyclic hydrocarbon groups, which will be described later. For example, one or more of the monomers exemplified above as (meth)acrylic acid alkyl esters that can be used for polymer (A) can be used as constituents of monomer raw material B. In some embodiments, monomer raw material B is (meth)acrylic acid C. 4-12 Alkyl ester (preferably (meth)acrylic acid C 4-10 Alkyl esters, such as (meth)acrylic acid C 6-10 In some other embodiments, the monomer feedstock B may contain at least one of methacrylic acid C 1-18 Alkyl ester (preferably methacrylic acid C 1-14 Alkyl esters, such as methacrylic acid C 1-10The monomer raw material B may contain at least one (meth)acrylic monomer selected from, for example, MMA, n-butyl methacrylate (BMA), and 2-ethylhexyl methacrylate (2EHMA).

[0081] Other examples of the (meth)acrylic monomer include (meth)acrylic acid esters having an alicyclic hydrocarbon group. For example, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, 1-adamantyl (meth)acrylate, etc. can be used. In some embodiments, the monomer raw material B can contain at least one selected from dicyclopentanyl methacrylate, isobornyl methacrylate, and cyclohexyl methacrylate as the (meth)acrylic monomer.

[0082] The content of the (meth)acrylic acid alkyl ester and the (meth)acrylic acid ester having an alicyclic hydrocarbon group in the monomer raw material B may be, for example, 10% by weight or more and 95% by weight or less, 20% by weight or more and 95% by weight or less, 30% by weight or more and 90% by weight or less, 40% by weight or more and 90% by weight or less, or 50% by weight or more and 85% by weight or less. From the viewpoint of the ease of increasing the adhesive strength by heating, the use of the (meth)acrylic acid alkyl ester may be advantageous. In some embodiments, the content of the (meth)acrylic acid ester having an alicyclic hydrocarbon group may be less than 50% by weight, less than 30% by weight, less than 15% by weight, less than 10% by weight, or less than 5% by weight of the monomer raw material B. The (meth)acrylic acid ester having an alicyclic hydrocarbon group may not be used.

[0083] In some preferred embodiments, the (meth)acrylic monomer, which is a component of the monomer raw material B, may contain a monomer M2 having a homopolymer Tg of 50° C. or more. In the polymer (B), the monomer S1 and the monomer M2 are copolymerized to suitably control the mobility and mobility of the polyorganosiloxane structure portion with increasing temperature, and it is easy to achieve both initial easy peelability (reworkability) and increased adhesive strength after heating. In some embodiments, the Tg of the homopolymer of the monomer M2 may be 60° C. or more, 70° C. or more, 80° C. or more, or 90° C. or more. In addition, the upper limit of the Tg of the homopolymer of the monomer M2 is not particularly limited, but from the viewpoint of ease of synthesis of the polymer (B), it is usually appropriate that it is 200° C. or less. In some embodiments, the Tg of the homopolymer of the monomer M2 may be, for example, 180° C. or less, 150° C. or less, or 120° C. or less.

[0084] As the monomer M2, for example, from among the (meth)acrylic monomers exemplified above, those that satisfy the conditions of Tg of the homopolymer can be used. For example, one or more monomers selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid esters having an alicyclic hydrocarbon group can be used. As the (meth)acrylic acid alkyl ester, a methacrylic acid alkyl ester having an alkyl group with a carbon number of 1 to 4 can be preferably used.

[0085] In an embodiment in which the monomer raw material B contains the monomer M2, the content of the monomer M2 may be, for example, 5% by weight or more, 10% by weight or more, 15% by weight or more, 20% by weight or more, 25% by weight or more, or 30% by weight or more of the monomer raw material B. In some embodiments, the content of the monomer M2 may be 35% by weight or more, 40% by weight or more, 45% by weight or more, 50% by weight or more, or 55% by weight or more of the monomer raw material B. In addition, the content of the monomer M2 may be, for example, 90% by weight or less, and is usually suitably 80% by weight or less, preferably 75% by weight or less, may be 70% by weight or less, or may be 65% by weight or less. In some preferred embodiments, the content of the monomer M2 is 60% by weight or less (for example, 50% by weight or less, typically 42% by weight or less). In polymer (B), the copolymerization ratio of monomer M2 having a Tg of 50° C. or higher is limited to a predetermined value or less, so that an increase in adhesive strength after heating can be preferably achieved based on the mobility of polymer (B) at around 50° C. From the same viewpoint, the content of monomer M2 in monomer raw material B may be 35% by weight or less, 25% by weight or less, or 15% by weight or less (e.g., 5% by weight or less).

[0086] The content of the monomer M2 can be preferably applied, for example, to an embodiment in which the monomer M2 is composed of one or more monomers selected from the group consisting of (meth)acrylic acid alkyl esters and the (meth)acrylic acid esters having an alicyclic hydrocarbon group, or an embodiment in which the monomer M2 is composed of one or more monomers selected from (meth)acrylic acid alkyl esters (e.g., methacrylic acid alkyl esters). One preferred example of such an embodiment is an embodiment in which the monomer M2 is composed of MMA.

[0087] In some embodiments, the (meth)acrylic monomer may contain a monomer M3 having a homopolymer Tg of less than 50° C. (typically, −20° C. or more and less than 50° C.). By using the monomer M3, it becomes easier to obtain a reinforcing film that has a good balance between adhesive strength and cohesive strength after the adhesive strength is increased. From the viewpoint of easily exerting such an effect, it is preferable to use the monomer M3 in combination with the monomer M2.

[0088] As the monomer M3, for example, from among the (meth)acrylic monomers exemplified above, those having a homopolymer Tg that satisfies the conditions can be used. For example, one or more monomers selected from the group consisting of (meth)acrylic acid alkyl esters can be used.

[0089] In an embodiment in which the monomer raw material B contains the monomer M3, the content of the monomer M3 may be, for example, 5% by weight or more, 10% by weight or more, 15% by weight or more, 20% by weight or more, 25% by weight or more, 30% by weight or more, or 35% by weight or more of the monomer raw material B. The content of the monomer M3 is usually suitably 70% by weight or less, 60% by weight or less, or 50% by weight or less of the monomer raw material B. The above content of the monomer M3 can be preferably applied, for example, to an embodiment in which the monomer M3 is composed of one or more monomers selected from (meth)acrylic acid alkyl esters (e.g., methacrylic acid alkyl esters).

[0090] In some embodiments of the reinforcing film disclosed herein, the monomer raw material B preferably contains 30% by weight or less of a monomer having a homopolymer Tg higher than 170°C. Here, unless otherwise specified, the monomer content of X% by weight or less in this specification is a concept including an embodiment in which the content of the monomer is 0% by weight, that is, an embodiment in which the monomer is not substantially contained. In addition, "substantially not contained" means that the monomer is not used at least intentionally. When the copolymerization ratio of a monomer having a homopolymer Tg higher than 170°C is high, the mobility of the polymer (B) tends to be insufficient, and it may be difficult to increase the adhesive strength by heating to a temperature range higher than 50°C.

[0091] In some embodiments, the monomer raw material B preferably contains at least MMA as a (meth)acrylic monomer. A polymer (B) in which MMA is copolymerized can easily produce a reinforcing film with high adhesive strength after heating. The proportion of MMA in the total amount of (meth)acrylic monomers contained in the monomer raw material B may be, for example, 5% by weight or more, 10% by weight or more, 20% by weight or more, 30% by weight or more, or 40% by weight or more. In addition, the proportion of MMA in the total amount of the monomer raw material B is usually appropriate to be 95% by weight or less, and in some preferred embodiments, the proportion of MMA in the total amount of the monomer raw material B may be 75% by weight or less, 65% by weight or less, 60% by weight or less, or 55% by weight or less (for example, 50% by weight or less) from the viewpoint of increasing adhesive strength after heating.

[0092] Other examples of monomers that may be included together with monomer S1 as a monomer unit constituting polymer (B) include the carboxyl group-containing monomers, acid anhydride group-containing monomers, hydroxyl group-containing monomers, epoxy group-containing monomers, cyano group-containing monomers, isocyanate group-containing monomers, amide group-containing monomers, monomers having a nitrogen atom-containing ring (N-vinyl cyclic amides, cyclic amides having a (meth)acryloyl group, monomers having a succinimide skeleton, maleimides, itaconimides, etc.), aminoalkyl (meth)acrylates, vinyl esters, vinyl ethers, olefins, (meth)acrylic acid esters having an aromatic hydrocarbon group, heterocyclic ring-containing (meth)acrylates, halogen atom-containing (meth)acrylates, and (meth)acrylic acid esters obtained from terpene compound derivative alcohols, etc.

[0093] Further examples of monomers that may be contained together with the monomer S1 as a monomer unit constituting the polymer (B) include oxyalkylene di(meth)acrylates such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, and tripropylene glycol di(meth)acrylate; monomers having a polyoxyalkylene skeleton, such as polyethylene glycol and polypropylene glycol, having a polymerizable functional group such as a (meth)acryloyl group, a vinyl group, or an allyl group at one end of the polyoxyalkylene chain and an ether structure (alkyl ether, aryl ether, aryl alkyl ether, or the like) at the other end; methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, and propoxyethyl (meth)acrylate. alkoxyalkyl (meth)acrylates such as butoxyethyl (meth)acrylate and ethoxypropyl (meth)acrylate; salts such as alkali metal (meth)acrylate; polyvalent (meth)acrylates such as trimethylolpropane tri(meth)acrylate; halogenated vinyl compounds such as vinylidene chloride and 2-chloroethyl (meth)acrylate; oxazoline group-containing monomers such as 2-vinyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline and 2-isopropenyl-2-oxazoline; aziridine group-containing monomers such as (meth)acryloylaziridine and 2-aziridinylethyl (meth)acrylate; hydroxyl group-containing vinyl monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate and adducts of lactones and 2-hydroxyethyl (meth)acrylate; fluorine-containing vinyl monomers such as fluorine-substituted (meth)acrylic acid alkyl esters; reactive halogen-containing vinyl monomers such as 2-chloroethyl vinyl ether and vinyl monochloroacetate;Examples of the vinyl monomer include organosilicon-containing vinyl monomers such as vinyltrimethoxysilane, γ-(meth)acryloxypropyltrimethoxysilane, allyltrimethoxysilane, trimethoxysilylpropylallylamine, and 2-methoxyethoxytrimethoxysilane; and macromonomers having a radical polymerizable vinyl group at the monomer end obtained by polymerizing a vinyl group. These may be copolymerized with monomer S1 either alone or in combination of two or more.

[0094] In some embodiments, the polymer (B) may preferably be one that does not have a functional group that undergoes a crosslinking reaction with the polymer (A). In other words, the polymer (B) is preferably included in the adhesive layer in a form that is not chemically bonded to the polymer (A). The adhesive layer containing the polymer (B) in such a form has good mobility of the polymer (B) when heated, and is suitable for improving the rate of increase in adhesive strength. The functional group that undergoes a crosslinking reaction with the polymer (A) may vary depending on the type of functional group possessed by the polymer (A), and may be, for example, an epoxy group, an isocyanate group, a carboxy group, an alkoxysilyl group, an amino group, etc.

[0095] The Mw of the polymer (B) is not particularly limited. The Mw of the polymer (B) may be, for example, 1000 or more, or 5000 or more. In some preferred embodiments, the Mw of the polymer (B) is 10,000 or more, more preferably 12,000 or more, 15,000 or more, 20,000 or more, 22,000 or more, or 25,000 or more, from the viewpoint of favorably exhibiting an increase in adhesive strength after heating. In some other embodiments, the Mw of the polymer (B) may be 30,000 or more, 50,000 or more, or 70,000 or more. The upper limit of the Mw of the polymer (B) is, for example, 500,000 or less, 350,000 or less, 200,000 or less, or 150,000 or less. From the viewpoint of adjusting the compatibility and mobility within the adhesive layer within an appropriate range and suitably exhibiting low adhesion at the initial stage of application, in some preferred embodiments, the Mw of the polymer (B) is 100,000 or less, more preferably 80,000 or less, even more preferably 60,000 or less, particularly preferably 40,000 or less (e.g., 30,000 or less), and may be 25,000 or less, or may even be 20,000 or less. By setting the Mw of the polymer (B) within an appropriate range, it is easy to obtain an adhesive that is excellent in both easy peelability and adhesive strength increase at the initial stage of application.

[0096] In some preferred embodiments, the Mw of the polymer (B) is preferably lower than the Mw of the polymer (A). This makes it easier to realize a reinforcing film that has both good reworkability at the initial stage of application and an increase in adhesive strength after heating. In some embodiments, the Mw of the polymer (B) may be, for example, 0.8 times or less, 0.75 times or less, 0.5 times or less, or 0.3 times or less of the Mw of the polymer (A). In some preferred embodiments, the Mw of the polymer (A) may be, for example, 0.8 times or less, 0.75 times or less, 0.5 times or less, or 0.3 times or less. A Mw of polymer (B) B Ratio (Mw B / Mw A ) is 0.3 or less, more preferably 0.2 or less, even more preferably 0.1 or less, and particularly preferably 0.06 or less (e.g., 0.05 or less). B / MwA ) is, for example, suitably 0.010 or more, preferably 0.020 or more, more preferably 0.03 or more, and even more preferably 0.04 or more. By setting the Mw of polymer (A) and the Mw of polymer (B) within an appropriate range, the effects of the technology disclosed herein can be better realized. In some other embodiments, the Mw of polymer (B) may be 0.03 times or less (e.g., 0.02 times or less) the Mw of polymer (A).

[0097] The polymer (B) can be prepared, for example, by polymerizing the above-mentioned monomers by a known method such as solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, or photopolymerization.

[0098] In order to adjust the molecular weight of the polymer (B), a chain transfer agent can be used as necessary. Examples of the chain transfer agent to be used include compounds having a mercapto group such as octyl mercaptan, lauryl mercaptan, t-nonyl mercaptan, t-dodecyl mercaptan, mercaptoethanol, and α-thioglycerol; thioglycolic acid esters such as thioglycolic acid, methyl thioglycolate, ethyl thioglycolate, propyl thioglycolate, butyl thioglycolate, t-butyl thioglycolate, 2-ethylhexyl thioglycolate, octyl thioglycolate, isooctyl thioglycolate, decyl thioglycolate, dodecyl thioglycolate, thioglycolic acid ester of ethylene glycol, thioglycolic acid ester of neopentyl glycol, and thioglycolic acid ester of pentaerythritol; and α-methylstyrene dimer. The chain transfer agent can be used alone or in combination of two or more.

[0099] The amount of the chain transfer agent used is not particularly limited, but is usually 0.05 to 20 parts by weight, preferably 0.1 to 15 parts by weight, and more preferably 0.2 to 10 parts by weight, per 100 parts by weight of the monomer. By adjusting the amount of the chain transfer agent added in this manner, a polymer (B) having a suitable molecular weight can be obtained. In some preferred embodiments, the amount of the chain transfer agent used is 5 parts by weight or less, more preferably 3 parts by weight or less, and even more preferably 2 parts by weight or less, and may be 1.5 parts by weight or less, or 1 part by weight or less, per 100 parts by weight of the monomer.

[0100] As a means for adjusting the molecular weight of the polymer (B), various conventionally known means including the use of the chain transfer agent can be used alone or in appropriate combination. The same applies to the molecular weight of the polymer (A). Non-limiting examples of such means include selection of a polymerization method, selection of the type and amount of a polymerization initiator, selection of a polymerization temperature, selection of the type and amount of a polymerization solvent in a solution polymerization method, selection of light irradiation intensity in a photopolymerization method, etc. A person skilled in the art can understand how to obtain a polymer having a desired molecular weight based on the description of the present specification including the specific examples described below and the common general technical knowledge at the time of filing of the present application.

[0101] In the reinforcing film disclosed herein, the amount of polymer (B) used relative to 100 parts by weight of polymer (A) can be, for example, 0.1 parts by weight or more, and from the viewpoint of obtaining a higher effect (preferably, light peelability at the initial stage of application), it is preferably 0.2 parts by weight or more. In some embodiments, from the viewpoint of improving reworkability, the amount of polymer (B) used is appropriately 0.3 parts by weight or more, more preferably 0.5 parts by weight or more, and may be 0.8 parts by weight or more, 1.0 parts by weight or more, 1.5 parts by weight or more, 2.0 parts by weight or more, 3.0 parts by weight or more, 4.0 parts by weight or more, or 5.0 parts by weight or more. In addition, the amount of polymer (B) used relative to 100 parts by weight of polymer (A) may be, for example, 75 parts by weight or less, 30 parts by weight or less, or 20 parts by weight or less. It may be 15 parts by weight or less, or 10 parts by weight or less. From the viewpoint of facilitating the increase in adhesive strength after the increase in adhesive strength, in some embodiments, the amount of polymer (B) used relative to 100 parts by weight of polymer (A) is preferably 8.0 parts by weight or less, more preferably 5.0 parts by weight or less, and even more preferably 4.5 parts by weight or less, and may be 3.5 parts by weight or less, 3.0 parts by weight or less, or 2.5 parts by weight or less (for example, 2.0 parts by weight or less). By setting the amount of polymer (B) used within the above range, it is possible to better achieve both easy peeling property at the initial stage of application and increase in adhesive strength, and it is also easy to increase flexibility (particularly flexibility at low temperatures).

[0102] The pressure-sensitive adhesive layer may contain a polymer (optional polymer) other than the polymer (A) and the polymer (B) as necessary, within a range that does not significantly impair the performance of the reinforcing film disclosed herein. Non-limiting examples of such optional polymers include rubber-based polymers, polyester-based polymers, urethane-based polymers, polyether-based polymers, silicone-based polymers, polyamide-based polymers, fluorine-based polymers, etc., which are known in the field of pressure-sensitive adhesives, as well as acrylic polymers that do not fall under either polymer (A) or polymer (B). The amount of the optional polymer used is usually appropriate to be 20% by weight or less of the total polymer components contained in the pressure-sensitive adhesive layer, and may be 15% by weight or less, or may be 10% by weight or less. In some embodiments, the amount of the optional polymer used may be 5% by weight or less, 3% by weight or less, or 1% by weight or less of the total polymer components. The pressure-sensitive adhesive layer may be substantially free of polymers other than the polymer (A) and the polymer (B).

[0103] (Zirconium-containing compounds) The adhesive layer disclosed herein further contains a zirconium (Zr)-containing compound in addition to the above polymer (A) and polymer (B). By using the Zr-containing compound appropriately, it is possible to achieve good flexibility (particularly flexibility in a low temperature range), initial easy peelability, and high adhesive strength after the adhesive strength increases. The Zr-containing compound can be used alone or in combination of two or more. The Zr-containing compound is preferably an organic zirconium-containing compound, and for example, one or more selected from organometallic catalysts containing Zr (typically, organic compounds having Zr in the active center) can be used as the Zr-containing compound in the technology disclosed herein.

[0104] The Zr-containing compound (organic zirconium-containing compound) is not particularly limited, and examples thereof include zirconium tetraacetylacetonate, zirconium monoacetylacetonate, zirconium ethylacetoacetate, zirconium octylate compounds, etc. More specifically, zirconium alkoxides such as tetraethoxyzirconium, tetra-n-propoxyzirconium, tetra-i-propoxyzirconium, tetra-n-butoxyzirconium (normal butyl zirconate), tetra-i-butoxyzirconium, tetra-sec-butoxyzirconium, and tetra-t-butoxyzirconium; triethoxy mono(acetylacetonate)zirconium, tri-n-propoxy mono(acetylacetonate)zirconium, Tri-i-propoxy mono(acetylacetonate)zirconium, tri-n-butoxy mono(acetylacetonate)zirconium, tri-sec-butoxy mono(acetylacetonate)zirconium, tri-t-butoxy mono(acetylacetonate)zirconium, diethoxy bis(acetylacetonate)zirconium, di-n-propoxy bis(acetylacetonate)zirconium, di-i-propoxy bis(acetylacetonate)zirconium, di -n-Butoxy bis(acetylacetonate)zirconium, di-sec-butoxy bis(acetylacetonate)zirconium, di-t-butoxy bis(acetylacetonate)zirconium, monoethoxy tris(acetylacetonate)zirconium, mono-n-propoxy tris(acetylacetonate)zirconium, mono-i-propoxy tris(acetylacetonate)zirconium, mono-n-butoxy tris(acetylacetonate)zirconium , mono-sec-butoxy tris(acetylacetonate) zirconium, mono-t-butoxy tris(acetylacetonate) zirconium, tetrakis(acetylacetonate) zirconium, triethoxy mono(ethylacetoacetate) zirconium, tri-n-propoxy mono(ethylacetoacetate) zirconium, tri-i-propoxy mono(ethylacetoacetate) zirconium, tri-n-butoxy mono(ethylacetoacetate) zirconium,Tri-sec-butoxy mono(ethylacetoacetate)zirconium, tri-t-butoxy mono(ethylacetoacetate)zirconium, diethoxy bis(ethylacetoacetate)zirconium, di-n-propoxy bis(ethylacetoacetate)zirconium, di-i-propoxy bis(ethylacetoacetate)zirconium, di-n-butoxy bis(ethylacetoacetate)zirconium, di-sec-butoxy bis(ethylacetoacetate)zirconium, di-t-butoxy bis(ethylacetoacetate)zirconium, monoethoxy tris(ethylacetoacetate)zirconium , zirconium chelates such as mono-n-propoxy tris(ethylacetoacetate)zirconium, mono-i-propoxy tris(ethylacetoacetate)zirconium, mono-n-butoxy tris(ethylacetoacetate)zirconium, mono-sec-butoxy tris(ethylacetoacetate)zirconium, mono-t-butoxy tris(ethylacetoacetate)zirconium, tetrakis(ethylacetoacetate)zirconium, mono(acetylacetonato) tris(ethylacetoacetate)zirconium, bis(acetylacetonato) bis(ethylacetoacetate)zirconium, and tris(acetylacetonato) mono(ethylacetoacetate)zirconium; and the like. The above organic zirconium-containing compounds can be used alone or in combination of two or more.

[0105] The preferred amount of the Zr-containing compound to be used is the amount of the polymer (A) to be used and the amount W of the monomer units derived from the nitrogen-containing monomer contained in the polymer (A). N In some embodiments, the amount W of the Zr-containing compound relative to 100 parts by weight of the polymer (A) may be set based on the above. Zr [Parts by weight] is the amount W of monomer units derived from the nitrogen-containing monomer per 100 parts by weight of the polymer (A). N In relation to [parts by weight], the above W Zr [Parts by weight] N [Part by weight] ratio (W N / W Zr) is 4 or more. Zr [Parts by weight] N [Part by weight] ratio (W N / W Zr ) is 4 or more, so W N By limiting the ratio to 14 parts by weight or less, in a configuration suitable for improving flexibility (particularly flexibility in the low temperature range), it is possible to achieve both initial easy peelability and high adhesive strength after the adhesive strength increases. Without wishing to be bound by theory, the reason for obtaining such an effect is that in a pressure-sensitive adhesive containing a combination of polymer (A) containing a monomer unit derived from a nitrogen-containing monomer, polymer (B), and a Zr-containing compound, the Zr-containing compound has the effect of making the polymer (A) more easily attracted to the surface of an adherend (e.g., a polyimide film), and the above effect becomes apparent with the passage of time and / or by heating after application to the adherend, and the ratio (W N / W Zr ) in an appropriate range is believed to contribute to improving the adhesive strength after the adhesive strength has increased. However, the present invention is not limited to this reason alone.

[0106] In order to better exert the effect of increasing the adhesive strength after the adhesive strength increase (for example, the adhesive strength after heating N2), in some embodiments, the ratio (W N / W Zr ) is suitably 5 or more, advantageously 7 or more, and preferably 9 or more, for example 10 or more, 12 or more, 14 or more, or 16 or more. N / W Zr The upper limit of the ratio (W) is not particularly limited and may be appropriately set within a range in which the desired effect is obtained. N / W Zr ) may be, for example, 2000 or less, 1400 or less, 1000 or less, 700 or less, 500 or less, 300 or less, 250 or less, or 200 or less.

[0107] In some embodiments in which the polymer (A) contains a monomer unit derived from a monomer having a nitrogen atom-containing ring, the amount W of the monomer unit derived from the monomer having the nitrogen atom-containing ring contained in 100 parts by weight of the polymer (A) is RN [Parts by weight] of W Zr [parts by weight] (i.e., ratio (W RN / W Zr The lower limit of the ratio (W N / W Zr ) can be used. In some embodiments, the ratio (W RN / W Zr The upper limit of the above ratio (W N / W Zr ) or the lower limit thereof may be adopted.

[0108] The amount of Zr-containing compound W relative to 100 parts by weight of polymer (A) Zr is not particularly limited, and may be, for example, in the range of about 0.0001 parts by weight to 3 parts by weight. In some embodiments, the amount W of the Zr-containing compound is Zr can be, for example, 0.001 parts by weight or more, 0.005 parts by weight or more, or 0.008 parts by weight or more. In an embodiment in which the Zr-containing compound can also function as a crosslinking catalyst (for example, an embodiment in which the pressure-sensitive adhesive layer contains an isocyanate-based crosslinking agent), the amount W of the Zr-containing compound Zr In some embodiments, the amount W of the Zr-containing compound is preferably 1 to 50. Zr may be 0.01 parts by weight or more, 0.03 parts by weight or more, 0.05 parts by weight or more, or 0.1 parts by weight or more. In addition, the amount W of the Zr-containing compound relative to 100 parts by weight of the polymer (A) may be Zr is preferably 2 parts by weight or less, more preferably 1.5 parts by weight or less (e.g., 1 part by weight or less, 0.7 parts by weight or less, or 0.5 parts by weight or less), and the ratio (W N / W Zr ) can be set to be 4 or more (for example, 5 or more, 7 or more, or 9 or more). ZrAppropriately limiting the adhesive strength can be advantageous in terms of adhesive strength and flexibility after the adhesive strength is increased.

[0109] The adhesive layer disclosed herein may contain one or more metal compounds (typically organometallic catalysts) other than the Zr-containing compound for the purpose of promoting crosslinking reaction. Examples of such metal compounds include tin (Sn)-containing compounds (tin-based catalysts), titanium (Ti)-containing compounds (titanium-based catalysts), hafnium (Hf)-containing compounds (hafnium-based catalysts), iron (Fe)-containing compounds (iron-based catalysts), aluminum (Al)-containing compounds (aluminum-based catalysts), zinc (Zn)-containing compounds (zinc-based catalysts), and bismuth (Bi)-containing compounds (bismuth-based catalysts). In some embodiments, the amount of the metal compound other than the Zr-containing compound is suitably less than the amount of the Zr-containing compound used (i.e., less than 1 times the amount of the Zr-containing compound used) on a weight basis, preferably less than 0.5 times, and more preferably less than 0.3 times or less than 0.1 times. Metal compounds other than the Zr-containing compound may not be used.

[0110] (Crosslinking agent) In the pressure-sensitive adhesive layer, a crosslinking agent may be used as necessary for the purpose of adjusting the cohesive force, etc. As the crosslinking agent, a crosslinking agent known in the field of pressure-sensitive adhesives may be used, and examples thereof include epoxy-based crosslinking agents, isocyanate-based crosslinking agents, silicone-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, silane-based crosslinking agents, and alkyl etherified melamine-based crosslinking agents. Isocyanate-based crosslinking agents and epoxy-based crosslinking agents can be preferably used. As a crosslinking agent suitable for achieving both increased adhesive strength and flexibility, an isocyanate-based crosslinking agent can be preferably used in some embodiments. The crosslinking agent can be used alone or in combination of two or more types.

[0111] As the isocyanate-based crosslinking agent, a polyfunctional isocyanate (which refers to a compound having an average of two or more isocyanate groups per molecule, including those having an isocyanurate structure) can be preferably used. The isocyanate-based crosslinking agent can be used alone or in combination of two or more kinds.

[0112] Examples of the polyfunctional isocyanate include aliphatic polyisocyanates, alicyclic polyisocyanates, and aromatic polyisocyanates. Specific examples of aliphatic polyisocyanates include 1,2-ethylene diisocyanate; tetramethylene diisocyanates such as 1,2-tetramethylene diisocyanate, 1,3-tetramethylene diisocyanate, and 1,4-tetramethylene diisocyanate; hexamethylene diisocyanates such as 1,2-hexamethylene diisocyanate, 1,3-hexamethylene diisocyanate, 1,4-hexamethylene diisocyanate, 1,5-hexamethylene diisocyanate, 1,6-hexamethylene diisocyanate, and 2,5-hexamethylene diisocyanate; 2-methyl-1,5-pentane diisocyanate, 3-methyl-1,5-pentane diisocyanate, and lysine diisocyanate.

[0113] Specific examples of alicyclic polyisocyanates include isophorone diisocyanate; cyclohexyl diisocyanates such as 1,2-cyclohexyl diisocyanate, 1,3-cyclohexyl diisocyanate, and 1,4-cyclohexyl diisocyanate; cyclopentyl diisocyanates such as 1,2-cyclopentyl diisocyanate and 1,3-cyclopentyl diisocyanate; hydrogenated xylylene diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated tetramethylxylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate.

[0114] Specific examples of aromatic polyisocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, 2-nitrodiphenyl-4,4'-diisocyanate, 2,2'-diphenylpropane-4,4'-diisocyanate, Examples of the diisocyanate include 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4'-diphenylpropane diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, naphthylene-1,4-diisocyanate, naphthylene-1,5-diisocyanate, 3,3'-dimethoxydiphenyl-4,4'-diisocyanate, xylylene-1,4-diisocyanate, and xylylene-1,3-diisocyanate.

[0115] A preferred example of the polyfunctional isocyanate is a polyfunctional isocyanate having an average of three or more isocyanate groups per molecule. Such a trifunctional or higher isocyanate may be a multimer (e.g., a dimer or trimer) of a bifunctional or trifunctional or higher isocyanate, a derivative (e.g., an addition reaction product of a polyhydric alcohol and two or more molecules of a polyfunctional isocyanate), a polymer, or the like. Examples of the isocyanate include a dimer or trimer of diphenylmethane diisocyanate, an isocyanurate of hexamethylene diisocyanate (a trimer adduct of an isocyanurate structure), a reaction product of trimethylolpropane and tolylene diisocyanate, a reaction product of trimethylolpropane and hexamethylene diisocyanate, a trimethylolpropane adduct of xylylene diisocyanate, a trimethylolpropane adduct of isophorone diisocyanate, a trimethylolpropane adduct of hexamethylene diisocyanate, polymethylene polyphenylisocyanate, polyether polyisocyanate, polyester polyisocyanate, and adducts of these with various polyols, and polyfunctional isocyanates such as polyisocyanates multifunctionalized with an isocyanurate bond, a biuret bond, an allophanate bond, or the like.

[0116] Commercially available products of the above-mentioned polyfunctional isocyanates include those manufactured by Asahi Kasei Chemicals Corporation under the trade name "Duranate TPA-100," those manufactured by Tosoh Corporation under the trade names "Coronate L," "Coronate HL," "Coronate HK," "Coronate HX," and "Coronate 2096," and those manufactured by Mitsui Chemicals, Inc. under the trade names "Takenate D110N," "Takenate D120N," "Takenate D140N," and "Takenate D160N."

[0117] Examples of epoxy crosslinking agents include bisphenol A, epichlorohydrin-type epoxy resins, ethylene glycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol glycidyl ether, trimethylolpropane triglycidyl ether, diglycidylaniline, diamine glycidylamine, N,N,N',N'-tetraglycidyl-m-xylylenediamine, and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, etc. These may be used alone or in combination of two or more.

[0118] The amount of the crosslinking agent used is not particularly limited, and may be, for example, more than 0 parts by weight relative to 100 parts by weight of the polymer (A). The amount of the crosslinking agent used may be, for example, 0.01 parts by weight or more relative to 100 parts by weight of the polymer (A), and is preferably 0.05 parts by weight or more. By increasing the amount of the crosslinking agent used, the adhesive strength at the initial stage of application is suppressed, and reworkability tends to be improved. In some embodiments, the amount of the crosslinking agent used relative to 100 parts by weight of the polymer (A) may be 0.07 parts by weight or more, may be 0.1 parts by weight or more, or may be 0.15 parts by weight or more. On the other hand, from the viewpoint of obtaining an increase in adhesive strength after heating by allowing the movement of the polymer (B) appropriately, the amount of the crosslinking agent used relative to 100 parts by weight of the polymer (A) is usually appropriate to be 15 parts by weight or less, may be 10 parts by weight or less, or may be 5 parts by weight or less.

[0119] The technology disclosed herein can be preferably implemented in an embodiment using at least an isocyanate-based crosslinking agent as a crosslinking agent. From the viewpoint of achieving both good reworkability at the initial stage of application and increased adhesive strength after heating, in some embodiments, the amount of the isocyanate-based crosslinking agent used relative to 100 parts by weight of the polymer (A) can be, for example, 0.01 parts by weight or more, preferably 0.05 parts by weight or more, more preferably 0.07 parts by weight or more, may be 0.10 parts by weight or more, or may be 0.15 parts by weight or more (for example, 0.20 parts by weight or more). By increasing the amount of the isocyanate-based crosslinking agent used, a moderate cohesive force is obtained, and the initial light peelability and processability also tend to be excellent. The amount of the isocyanate crosslinking agent used relative to 100 parts by weight of the polymer (A) can be, for example, 5 parts by weight or less, preferably less than 1.0 parts by weight, more preferably less than 0.5 parts by weight, and even more preferably less than 0.3 parts by weight, and may be 0.2 parts by weight or less (for example, less than 0.2 parts by weight or less), or may be 0.15 parts by weight or less (for example, less than 0.15 parts by weight). Appropriately limiting the amount of the isocyanate crosslinking agent used is advantageous from the viewpoint of improving the flexibility of the adhesive, and also makes it easier to obtain an increase in adhesive strength after heating.

[0120] (tackifier resin) The adhesive layer may contain a tackifier resin as necessary. The tackifier resin is not particularly limited, but may be, for example, a rosin-based tackifier resin, a terpene-based tackifier resin, a phenol-based tackifier resin, a hydrocarbon-based tackifier resin, a ketone-based tackifier resin, a polyamide-based tackifier resin, an epoxy-based tackifier resin, or an elastomer-based tackifier resin. The tackifier resin may be used alone or in combination of two or more.

[0121] The content of the tackifier resin is not particularly limited, and can be set so that appropriate adhesive performance is exhibited depending on the purpose and application. The content of the tackifier resin (when two or more kinds of tackifier resins are included, the total amount thereof) relative to 100 parts by weight of the polymer (A) can be, for example, about 0.5 to 200 parts by weight, and may be about 0.5 to 100 parts by weight or about 0.5 to 50 parts by weight. In addition, the technology disclosed herein can be preferably implemented in an embodiment in which the amount of the tackifier resin used is limited. For example, the content of the tackifier resin relative to 100 parts by weight of the polymer (A) can be less than 20 parts by weight, may be less than 10 parts by weight, may be less than 3 parts by weight, or may be less than 1 part by weight (0 parts by weight to less than 1 part by weight). In some embodiments, the pressure-sensitive adhesive layer does not substantially contain a tackifier resin.

[0122] In addition, the adhesive layer in the technology disclosed herein may contain, as necessary, known additives that can be used in adhesives, such as leveling agents, plasticizers, softeners, colorants (dyes, pigments, etc.), fillers, antistatic agents, antioxidants, UV absorbers, antioxidants, light stabilizers, and preservatives, provided that the effects of the present invention are not significantly impeded.

[0123] The adhesive layer constituting the reinforcing film disclosed herein may be a cured layer of an adhesive composition. That is, the adhesive layer may be formed by applying (for example, coating) an aqueous dispersion type, solvent type, photocurable type, hot melt type, or other adhesive composition to a suitable surface, and then appropriately carrying out a curing treatment. When two or more types of curing treatments (drying, crosslinking, polymerization, cooling, etc.) are performed, these can be performed simultaneously or in multiple stages. In an adhesive composition using a partial polymer (polymer syrup) of a monomer raw material, typically, a final copolymerization reaction is performed as the curing treatment. That is, the partial polymer is subjected to a further copolymerization reaction to form a complete polymer. For example, in the case of a photocurable adhesive composition, light irradiation is performed. If necessary, a curing treatment such as crosslinking or drying may be performed. For example, if a photocurable adhesive composition needs to be dried, it is recommended to perform photocuring after drying. In an adhesive composition using a complete polymer, typically, a treatment such as drying (heat drying) or crosslinking is performed as the curing treatment as necessary.

[0124] The pressure-sensitive adhesive composition can be applied using a conventional coater such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a knife coater or a spray coater.

[0125] The thickness of the adhesive layer is not particularly limited, and can be, for example, 6 μm or more. In some embodiments, the thickness of the adhesive layer may be 8 μm or more, 10 μm or more, 15 μm or more, or 20 μm or more or more than 20 μm. The adhesive strength after heating tends to increase due to the increase in the thickness of the adhesive layer. In some embodiments, the thickness of the adhesive layer may be, for example, 300 μm or less, 200 μm or less, 150 μm or less, 100 μm or less, 70 μm or less, 50 μm or less, or 40 μm or less. It may be advantageous for the thickness of the adhesive layer not to be too large in terms of thinning the reinforcing film and preventing cohesive failure of the adhesive layer. A reinforcing film having an adhesive layer having a thickness within the above-mentioned range may be well-balanced between adhesive properties such as adhesive strength and flexibility. In addition, in the case of a reinforcing film having a first pressure-sensitive adhesive layer and a second pressure-sensitive adhesive layer on the first and second surfaces of a substrate, the thickness of the above-mentioned pressure-sensitive adhesive layer can be applied to at least the thickness of the first pressure-sensitive adhesive layer. The thickness of the second pressure-sensitive adhesive layer can also be selected from the same range. In addition, in the case of a reinforcing film without a substrate, the thickness of the reinforcing film is the same as the thickness of the pressure-sensitive adhesive layer.

[0126] (-20℃ storage modulus (G′ -20 )) In some embodiments of the technology disclosed herein, the storage modulus at −20° C. (hereinafter, “storage modulus (G′ -20 The storage modulus (G') may be, for example, 10,000 kPa, suitably 5,000 kPa or less, advantageously 3,000 kPa or less, and preferably 1,000 kPa or less. -20 By limiting the storage modulus (G') to a predetermined value or less, the pressure-sensitive adhesive exhibits good flexibility suitable for repeated folding and bending. From the viewpoint of further increasing the flexibility, in some embodiments, the storage modulus (G') of the pressure-sensitive adhesive is -20The storage modulus (G') of the pressure-sensitive adhesive is preferably 700 kPa or less, more preferably 500 kPa or less, and even more preferably 300 kPa or less, and may be 200 kPa or less, 150 kPa or less, 140 kPa or less, 130 kPa or less, 120 kPa or less, or 110 kPa or less. -20 The lower limit of the storage modulus (G') of the adhesive is not particularly limited, and may be, for example, 20 kPa or more or 30 kPa or more. In some embodiments, the storage modulus (G') of the adhesive is set to 100 kPa or more, taking into consideration the compatibility with other properties (e.g., one or more properties of a low initial adhesive strength N1, a high adhesive strength after heating, and a high rate of increase N2 / N1). -20 ) may be, for example, 50 kPa or more, 70 kPa or more, 80 kPa or more, 90 kPa or more, or 100 kPa or more.

[0127] (23℃ storage modulus (G′ 23 )) The storage modulus of the adhesive at 23°C (hereinafter referred to as "storage modulus (G' 23 The storage modulus (G') is not particularly limited and may be expressed as -20 In some embodiments, the storage modulus (G') of the PSA is preferably within a range not exceeding any of the upper limits mentioned above. 23 The storage modulus (G') should be 200 kPa or less. 23 Generally, adhesives having a storage modulus (G') of a certain value or less tend to have excellent strain relaxation properties at room temperature and are also prone to exhibiting increased adhesive strength. 23 In some preferred embodiments, the bulk elastic modulus G' is preferably 130 kPa or less, more preferably 80 kPa or less. 23 The pressure may be 50 kPa or less, or 40 kPa or less (eg, 35 kPa or less).

[0128] In some embodiments, the storage modulus (G' 23 The storage modulus (G') is preferably 10 kPa or more. 23By setting the storage modulus (G') to a predetermined value or more, the adhesive strength at the initial stage of application tends to be in a suitable range that provides excellent easy peelability. 23 ) is preferably 15 kPa or more, more preferably 20 kPa or more, may be 25 kPa or more, or may be 30 kPa or more.

[0129] (80℃ storage modulus (G′ 80 )) The storage modulus of the adhesive at 80°C (hereinafter referred to as "storage modulus (G' 80 The storage modulus (G') is not particularly limited and may be expressed as -20 In some embodiments, the storage modulus (G') of the pressure-sensitive adhesive layer is preferably within a range not exceeding any one of the upper limit values ​​mentioned above. 80 ) is suitably 100 kPa or less, preferably 70 kPa or less, more preferably 50 kPa or less, and may be 30 kPa or less, or may be 20 kPa or less.

[0130] In some embodiments, the storage modulus (G' 80 The storage modulus (G') is suitably 1 kPa or more, and preferably 2 kPa or more. 80 It may be advantageous from the viewpoint of heat resistance of the adhesive (e.g., adhesive properties in a high temperature range) that the storage modulus (G') is a predetermined value or more. 80 ) may be, for example, 3 kPa or more, 5 kPa or more, 7 kPa or more, 9 kPa or more, or 10 kPa or more.

[0131] The storage modulus of the pressure-sensitive adhesive layer at each temperature can be adjusted by the type and characteristics (molecular weight, glass transition temperature, molecular structure, etc.) of the polymer (A), the type (chemical structure, etc.) and characteristics (molecular weight, glass transition temperature, etc.) of the polymer (B), the amount used, the type and amount used of the crosslinking agent, etc. The storage modulus (G') of the pressure-sensitive adhesive layer at -20°C -20 The storage modulus at other temperatures can also be measured in a similar manner.

[0132] <Supporting base material> The reinforcing film according to some embodiments may be in the form of a substrate-attached adhesive sheet having an adhesive layer on one or both sides of the substrate. The material of the substrate is not particularly limited and can be appropriately selected according to the purpose and mode of use of the reinforcing film. Non-limiting examples of substrates that can be used include resin films such as plastic films; foam sheets made of foams such as polyurethane foam, polyethylene foam, and polychloroprene foam; woven and nonwoven fabrics made by single or mixed spinning of various fibrous materials (natural fibers such as hemp and cotton, synthetic fibers such as polyester and vinylon, semi-synthetic fibers such as acetate, etc.); papers such as Japanese paper, fine paper, craft paper, and crepe paper; metal foils such as aluminum foil and copper foil; and the like. The substrate may be a composite of these. Examples of such composite substrates include substrates having a structure in which metal foil and the above-mentioned plastic film are laminated, plastic substrates reinforced with inorganic fibers such as glass cloth, and the like.

[0133] As the substrate of the reinforcing film disclosed herein, various film substrates can be preferably used. The film substrate may be a porous substrate such as a foam film or a nonwoven sheet, or may be a nonporous substrate, or may be a substrate having a structure in which a porous layer and a nonporous layer are laminated. In some embodiments, the film substrate may preferably be one that includes a resin film that can independently maintain its shape (self-supporting or independent) as a base film. Here, the term "resin film" refers to a resin film that has a nonporous structure and typically does not substantially contain air bubbles (voidless). Therefore, the resin film is a concept that is distinguished from foam films and nonwoven fabrics. As the resin film, one that can independently maintain its shape (self-supporting or independent) can be preferably used. The resin film may be a single-layer structure, or may be a multi-layer structure of two or more layers (for example, a three-layer structure).

[0134] Examples of resin materials constituting the resin film include polyester, polyolefin, polyamide (PA) such as nylon 6, nylon 66, and partially aromatic polyamide, polyimide (PI), polyamideimide (PAI), polyetheretherketone (PEEK), polyethersulfone (PES), polyphenylene sulfide (PPS), polycarbonate (PC), polyurethane (PU), ethylene-vinyl acetate copolymer (EVA), fluororesin such as polytetrafluoroethylene (PTFE), acrylic resin, polyacrylate, polystyrene, polyvinyl chloride, and polyvinylidene chloride. The resin film may be formed using a resin material containing one of these resins alone, or may be formed using a resin material containing two or more of these resins blended together. The resin film may be unstretched or stretched (for example, uniaxially or biaxially stretched).

[0135] Suitable examples of resin materials constituting the resin film include polyimide-based resins, polyester-based resins, PPS resins, and polyolefin-based resins. Here, polyimide-based resins refer to resins containing more than 50% by weight of polyimide. Similarly, polyester-based resins refer to resins containing more than 50% by weight of polyester, PPS resins refer to resins containing more than 50% by weight of PPS, and polyolefin-based resins refer to resins containing more than 50% by weight of polyolefin.

[0136] Specific examples of polyester resins include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), and polybutylene naphthalate.

[0137] As the polyolefin resin, one type of polyolefin can be used alone, or two or more types of polyolefins can be used in combination. The polyolefin can be, for example, a homopolymer of an α-olefin, a copolymer of two or more types of α-olefins, or a copolymer of one or more types of α-olefins and other vinyl monomers. Specific examples include polyethylene (PE), polypropylene (PP), poly-1-butene, poly-4-methyl-1-pentene, ethylene-propylene copolymers such as ethylene-propylene rubber (EPR), ethylene-propylene-butene copolymers, ethylene-butene copolymers, ethylene-vinyl alcohol copolymers, and ethylene-ethyl acrylate copolymers. Both low density (LD) polyolefins and high density (HD) polyolefins can be used. Examples of polyolefin resin films include non-oriented polypropylene (CPP) film, biaxially oriented polypropylene (OPP) film, low-density polyethylene (LDPE) film, linear low-density polyethylene (LLDPE) film, medium-density polyethylene (MDPE) film, high-density polyethylene (HDPE) film, polyethylene (PE) film made by blending two or more types of polyethylene (PE), and PP / PE blend film made by blending polypropylene (PP) and polyethylene (PE).

[0138] Specific examples of resin films that can be preferably used as the base film of the reinforcing film disclosed herein include a PI film, a PET film, a PEN film, a PPS film, a PEEK film, a CPP film, and an OPP film.

[0139] The resin film may contain known additives such as light stabilizers, antioxidants, antistatic agents, colorants (dyes, pigments, etc.), fillers, slip agents, antiblocking agents, etc., as necessary, within the range that does not significantly impair the effects of the present invention. The amount of the additives to be added is not particularly limited, and can be appropriately set depending on the purpose, etc.

[0140] The method for producing the resin film is not particularly limited, and may be any of the conventionally known general resin film forming methods, such as extrusion molding, inflation molding, T-die casting, and calendar roll molding.

[0141] The substrate may be substantially composed of such a base film. Alternatively, the substrate may include an auxiliary layer in addition to the base film. Examples of the auxiliary layer include an optical property adjusting layer (e.g., a coloring layer, an anti-reflection layer), a printing layer or a lamination layer for imparting a desired appearance to the substrate, an antistatic layer, an undercoat layer, a peeling layer, and other surface treatment layers.

[0142] The thickness of the substrate is not particularly limited and may be selected according to the purpose and mode of use of the reinforcing film. The thickness of the substrate may be, for example, 1000 μm or less. In some embodiments, from the viewpoint of the handling and processability of the reinforcing film, the thickness of the substrate may be, for example, 500 μm or less, 300 μm or less, 250 μm or less, or 200 μm or less. In some embodiments, from the viewpoint of miniaturization and weight reduction of the product to which the reinforcing film is applied, the thickness of the substrate may be, for example, 160 μm or less, 130 μm or less, 100 μm or less, 90 μm or less, 80 μm or less, 60 μm or less, 50 μm or less, 25 μm or less, 10 μm or less, or 5 μm or less. When the thickness of the substrate is reduced, the flexibility of the reinforcing film and its ability to follow the surface shape of the adherend tend to be improved. In addition, from the viewpoint of handling and processability, the thickness of the substrate may be, for example, 2 μm or more, 5 μm or more, 10 μm or more, 20 μm or more, 25 μm or more, or more than 25 μm. In some embodiments, the thickness of the substrate may be, for example, 30 μm or more, 35 μm or more, 55 μm or more, 70 μm or more, 75 μm or more, 90 μm or more, or 120 μm or more. From the viewpoint of reinforcing performance, in some embodiments, a substrate having a thickness of 30 μm or more (for example, 45 μm or more, 55 μm or more, or 65 μm or more) may be preferably used.

[0143] The first surface of the substrate may be subjected to a conventionally known surface treatment, such as a corona discharge treatment, a plasma treatment, an ultraviolet irradiation treatment, an acid treatment, an alkali treatment, or the formation of an undercoat layer by applying an undercoat agent (primer), if necessary. Such a surface treatment may be a treatment for improving the anchoring property of the pressure-sensitive adhesive layer to the substrate. For example, in a reinforcing film having a substrate containing a resin film as a base film, a substrate subjected to such an anchoring property improvement treatment may be preferably used. The above surface treatments may be applied alone or in combination. The composition of the primer used to form the undercoat layer is not particularly limited, and may be appropriately selected from known ones. The thickness of the undercoat layer is not particularly limited, but is usually appropriate to be about 0.01 μm to 1 μm, and preferably about 0.1 μm to 1 μm. Other treatments that may be applied to the first surface of the substrate as necessary include an antistatic layer forming treatment, a colored layer forming treatment, a printing treatment, and the like.

[0144] When the reinforcing film disclosed herein is in the form of a single-sided pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer only on the first surface of the substrate, the second surface of the substrate may be subjected to a conventionally known surface treatment such as a release treatment or an antistatic treatment, if necessary. For example, by surface treating the back surface of the substrate with a release treatment agent (typically by providing a release layer made of a release treatment agent), the unwinding force of the reinforcing film wound in a roll shape can be reduced. As the release treatment agent, a silicone-based release treatment agent, a long-chain alkyl-based release treatment agent, an olefin-based release treatment agent, a fluorine-based release treatment agent, a fatty acid amide-based release treatment agent, molybdenum sulfide, silica powder, etc. can be used. In addition, for the purpose of improving printability, reducing light reflectivity, improving overlapping adhesion, etc., the second surface of the substrate may be subjected to a corona discharge treatment, a plasma treatment, an ultraviolet irradiation treatment, an acid treatment, an alkali treatment, etc. In addition, in the case of a double-sided pressure-sensitive adhesive sheet, the second surface of the substrate may be subjected to a surface treatment similar to those exemplified above as the surface treatment that can be applied to the first surface of the substrate, if necessary. The surface treatment applied to the first surface of the substrate and the surface treatment applied to the second surface may be the same or different.

[0145] <Characteristics of the reinforcing film> The reinforcing film disclosed herein is preferably limited to a predetermined value or less in initial adhesive strength N1 measured after laminating to a polyimide film and holding at 23°C for 30 minutes. In some embodiments, the adhesive strength N1 is suitably less than 500gf / 25mm, advantageously less than 300gf / 25mm, preferably 200gf / 25mm or less or 180gf / 25mm or less, more preferably 150gf / 25mm or less or 130gf / 25mm or less, even more preferably 110gf / 25mm or less or 100gf / 25mm or less, and may be 90gf / 25mm or less, or may be 80gf / 25mm or less. A low adhesive strength N1 is preferable from the viewpoint of reworkability. The lower limit of the adhesive strength N1 is not particularly limited, and may be, for example, 1gf / 25mm or more. From the viewpoint of ease of application to an adherend and prevention of misalignment before the adhesive strength increases, the adhesive strength N1 is usually appropriate to be 10 gf / 25 mm or more. From the viewpoint of improving the adhesive strength after heating, in some embodiments, the adhesive strength N1 may be, for example, 20 gf / 25 mm or more, 30 gf / 25 mm or more, 50 gf / 25 mm or more, 60 gf / 25 mm or more, or 70 gf / 25 mm or more.

[0146] The adhesive strength N1 [gf / 25mm] is determined by pressing the polyimide film as the adherend, leaving it in an environment of 23°C and 50% RH for 30 minutes, and then measuring the 180° peel adhesive strength in the same environment (i.e., at 23°C) under the conditions of a peel angle of 180° and a tensile speed of 300mm / min. From the viewpoint of measurement workability, the polyimide film as the adherend can be used in the form of a measurement polyimide plate (a plate-shaped adherend having a surface made of the polyimide film) formed by fixing the polyimide film to a support plate (glass plate, stainless steel plate, etc.). In the measurement, if necessary, a suitable backing material (for example, a PET film with a thickness of about 25 μm) can be attached to the reinforcing film to be measured to reinforce it. More specifically, the adhesive strength N1 can be measured according to the measurement method of the initial adhesive strength described in the examples described later.

[0147] The reinforcing film disclosed herein has an adhesive strength that increases when heated. For example, the adhesive strength N2 measured after laminating the film to a polyimide film as an adherend, heating at 60° C. for 1 hour, and then holding at 23° C. for 30 minutes is suitably 800 gf / 25 mm or more, advantageously 950 gf / 25 mm or more, and preferably 1000 gf / 25 mm or more. The reinforcing film that satisfies this characteristic has an adhesive strength that increases to a predetermined value or more when heated after laminating the film to an adherend. According to the technology disclosed herein, it is possible to obtain a strong adhesive strength by heating. In some embodiments, the adhesive strength N2 is more preferably 1100 gf / 25 mm or more, more preferably 1200 gf / 25 mm or more, and may be 1300 gf / 25 mm or more, or may be 1400 gf / 25 mm or more. There is no particular upper limit to the adhesive strength N2. From the viewpoint of easily achieving both the flexibility of the adhesive layer (particularly flexibility in the low temperature range) and the initial easy peelability, in some embodiments, the adhesive strength N2 may be, for example, 4000 gf / 25 mm or less, 3500 gf / 25 mm or less, 3000 gf / 25 mm or less, 2000 gf / 25 mm or less, 1800 gf / 25 mm or less, or 1600 gf / 25 mm or less.

[0148] The adhesive strength N2 [gf / 25mm] is determined by pressing the film to a polyimide film as an adherend, keeping it in an environment of 60°C for 60 minutes, then leaving it in an environment of 23°C and 50%RH for 30 minutes, and then measuring the 180° peel adhesive strength in the same environment under the conditions of a peel angle of 180° and a tensile speed of 300mm / min. As with the adhesive strength N1, a polyimide film (which may be in the form of a polyimide plate for measurement as described above) is used as the adherend. In the measurement, if necessary, a suitable backing material (for example, a PET film with a thickness of about 25μm) can be attached to the reinforcing film to be measured to reinforce it. More specifically, the adhesive strength N2 can be measured according to the method for measuring adhesive strength after heating described in the examples described later.

[0149] The rate of increase of the adhesive strength N2 [gf / 25mm] after heating relative to the initial adhesive strength N1 [gf / 25mm], i.e., the adhesive strength increase rate N2 / N1 [%], is not particularly limited, and may be, for example, 160% or more, 250% or more, 500% or more, or 750% or more. In some embodiments, N2 / N1 is suitably 850% or more, preferably 900% or more, more preferably 950% or more, even more preferably 1000% or more, and may be 1200% or more, 1400% or more, 1500% or more, 1600% or more, 1700% or more, or 1800% or more. A reinforcing film with a large N2 / N1 exhibits good reworkability at the beginning of application, and can greatly increase the adhesive strength by subsequent heating or the like. The upper limit of N2 / N1 is not particularly limited, and may be, for example, 10000% or less, 7000% or less, or 5000% or less. From the viewpoint of facilitating compatibility with the flexibility of the adhesive (particularly flexibility in the low temperature range), in some embodiments, N2 / N1 may be, for example, 4000% or less, 3000% or less, 2500% or less, or 2000% or less.

[0150] The adhesive strength after heating of the reinforcing film disclosed herein represents one characteristic of the reinforcing film, and does not limit the use of the reinforcing film. In other words, the use of the reinforcing film disclosed herein is not limited to the use of the reinforcing film at 60°C for 60 minutes, and the reinforcing film can be used in a mode in which heating is not particularly performed to a temperature above room temperature (usually 20°C to 30°C, typically 23°C to 25°C). Even in such a use mode, the adhesive strength increases over the long term, and strong bonding can be achieved. In addition, the reinforcing film disclosed herein can be heated at a temperature above 30°C (for example, about 50 to 70°C) or higher than 60°C at any timing after attachment to promote an increase in adhesive strength. The heating temperature in such a heat treatment is not particularly limited, and can be set in consideration of workability, economy, heat resistance of the base material of the reinforcing film and the adherend, and the like. The heating temperature may be, for example, less than 150°C, 120°C or less, 100°C or less, 80°C or less, or 70°C or less. The heating temperature can be, for example, 40°C or higher, 45°C or higher, 50°C or higher, 55°C or higher, 60°C or higher, or 70°C or higher, and may be 80°C or higher, or 100°C or higher. The heating time is not particularly limited, and may be, for example, 3 hours or less, 1 hour or less, 30 minutes or less, or 10 minutes or less. The heating time may be, for example, 1 minute or more, 15 minutes or more, 30 minutes or more, or 1 hour or more. Alternatively, the heating treatment may be performed for a longer period of time as long as no significant thermal deterioration occurs in the reinforcing film or the adherend. The heating treatment may be performed all at once, or may be performed in multiple steps.

[0151] <Reinforcing film with substrate> When the reinforcing film disclosed herein is in the form of a pressure-sensitive adhesive sheet with a substrate, the thickness of the reinforcing film may be, for example, 1000 μm or less, 600 μm or less, 350 μm or less, or 250 μm or less. In view of the miniaturization, weight reduction, thinning, etc. of the product to which the reinforcing film is applied, in some embodiments, the thickness of the reinforcing film may be, for example, 200 μm or less, 175 μm or less, 160 μm or less, 140 μm or less, or 120 μm or less. The reinforcing film disclosed herein can also be implemented in an embodiment in which the thickness is 115 μm or less, 105 μm or less, 95 μm or less, or 85 μm or less. In addition, in view of the handleability, etc., the thickness of the reinforcing film may be, for example, 5 μm or more, 10 μm or more, 15 μm or more, 20 μm or more, 25 μm or more, or 30 μm or more. In some embodiments, the thickness of the reinforcing film may be, for example, 50 μm or more, 60 μm or more, 75 μm or more, 85 μm or more, 90 μm or more, 100 μm or more, or 120 μm or more. The upper limit of the thickness of the reinforcing film is not particularly limited. The thickness of the reinforcing film refers to the thickness of the portion attached to the adherend. For example, in the case of the reinforcing film 1 having the configuration shown in FIG. 1, the thickness refers to the thickness from the adhesive surface 21A of the reinforcing film 1 to the second surface 10B of the substrate 10, and does not include the thickness of the release liner 31.

[0152] The reinforcing film disclosed herein can be suitably implemented, for example, in an embodiment in which the thickness Ts of the support substrate is greater than the thickness Ta of the adhesive layer, that is, in an embodiment in which Ts / Ta is greater than 1. Although not particularly limited, Ts / Ta may be, for example, 1.1 or more, 1.2 or more, 1.5 or more, or 1.7 or more. For example, an increase in Ts / Ta tends to make it easier to exhibit good effects even when the reinforcing film is made thinner. In some embodiments, Ts / Ta may be 2 or more (e.g., greater than 2), 2.5 or more, or 2.8 or more. In addition, Ts / Ta may be, for example, 50 or less, or 20 or less. From the viewpoint of making it easier to exhibit high post-heat adhesive strength even when the reinforcing film is made thinner, Ts / Ta may be, for example, 10 or less, 8 or less, or 5 or less.

[0153] The pressure-sensitive adhesive layer is preferably fixed to the support substrate. Here, the term "fixed" refers to the fact that, in a reinforcing film whose adhesive strength has increased after being attached to an adherend, the pressure-sensitive adhesive layer exhibits sufficient anchoring properties to the support substrate to such an extent that peeling does not occur at the interface between the pressure-sensitive adhesive layer and the support substrate when the reinforcing film is peeled off from the adherend. A substrate-attached reinforcing film in which the pressure-sensitive adhesive layer is fixed to the support substrate can firmly integrate the adherend and the support substrate. A suitable example of a reinforcing film in which the pressure-sensitive adhesive layer is fixed to the substrate is a reinforcing film in which peeling (anchor failure) does not occur between the pressure-sensitive adhesive layer and the support substrate when the above-mentioned post-heating adhesive strength is measured. A reinforcing film in which anchor failure does not occur when the post-heating adhesive strength is measured is a suitable example of a reinforcing film in which the pressure-sensitive adhesive layer is fixed to the substrate.

[0154] The reinforcing film disclosed herein can be preferably produced by a method including, for example, contacting a liquid pressure-sensitive adhesive composition with a first surface of a substrate and curing the pressure-sensitive adhesive composition on the first surface to form a pressure-sensitive adhesive layer in this order. The curing of the pressure-sensitive adhesive composition may involve one or more of drying, crosslinking, polymerization, cooling, etc. of the pressure-sensitive adhesive composition. According to the method of curing a liquid pressure-sensitive adhesive composition on the first surface of a substrate to form a pressure-sensitive adhesive layer, the anchoring property of the pressure-sensitive adhesive layer to the substrate can be improved compared to the method of placing the pressure-sensitive adhesive layer on the first surface of the substrate by bonding the cured pressure-sensitive adhesive layer to the first surface of the substrate. By utilizing this, a reinforcing film in which the pressure-sensitive adhesive layer is fixed to the substrate can be preferably produced.

[0155] In some embodiments, the method of contacting the liquid pressure-sensitive adhesive composition with the first surface of the substrate can be a method of directly applying the pressure-sensitive adhesive composition to the first surface of the substrate. By contacting the first surface (adhesive surface) of the pressure-sensitive adhesive layer cured on the first surface of the substrate with the release surface, a reinforcing film can be obtained in which the second surface of the pressure-sensitive adhesive layer is fixed to the first surface of the substrate and the first surface of the pressure-sensitive adhesive layer is in contact with the release surface. The release surface can be the surface of a release liner, the back surface of a substrate that has been subjected to a release treatment, or the like.

[0156] In addition, for example, in the case of a photocurable pressure-sensitive adhesive composition using a partial polymer (polymer syrup) of a monomer raw material, the pressure-sensitive adhesive composition may be applied to a release surface, and then the applied pressure-sensitive adhesive composition may be covered with a first surface of a substrate to bring the uncured pressure-sensitive adhesive composition into contact with the first surface of the substrate, and in this state, the pressure-sensitive adhesive composition sandwiched between the first surface of the substrate and the release surface may be irradiated with light to cure it, thereby forming a pressure-sensitive adhesive layer.

[0157] The above-mentioned methods are not intended to limit the method for producing the reinforcing film disclosed herein. In producing the reinforcing film disclosed herein, any suitable method capable of adhering the adhesive layer to the first surface of the substrate can be used alone or in combination of two or more. Examples of such methods include the above-mentioned method of curing a liquid adhesive composition on the first surface of the substrate to form an adhesive layer, and the method of performing a surface treatment on the first surface of the substrate to enhance the anchoring property of the adhesive layer. For example, when the anchoring property of the adhesive layer to the substrate can be sufficiently improved by a method such as providing an undercoat layer on the first surface of the substrate, the reinforcing film may be produced by laminating the cured adhesive layer to the first surface of the substrate. In addition, the anchoring property of the adhesive layer to the substrate can be improved by selecting the material of the substrate or the composition of the adhesive. In addition, the anchoring property of the adhesive layer to the substrate can be improved by applying a temperature higher than room temperature to a reinforcing film having an adhesive layer on the first surface of the substrate. The temperature applied to enhance the anchoring property may be, for example, about 35°C to 80°C, about 40°C to 70°C, or about 45°C to 60°C.

[0158] When the reinforcing film disclosed herein is in the form of a pressure-sensitive adhesive sheet having a first pressure-sensitive adhesive layer provided on a first surface of a substrate and a second pressure-sensitive adhesive layer provided on a second surface of the substrate (i.e., a double-sided adhesive substrate-attached pressure-sensitive adhesive sheet), the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer may have the same configuration or different configurations. When the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer have different configurations, the difference may be, for example, a difference in composition or structure (thickness, surface roughness, formation range, formation pattern, etc.). For example, the second pressure-sensitive adhesive layer may be a pressure-sensitive adhesive layer that does not contain polymer (B). The surface (adhesive surface) of the second pressure-sensitive adhesive layer may have an initial adhesive strength to the above-mentioned polyimide film of 200 gf / 25 mm or less, or may be more than 200 gf / 25 mm, for example, 500 gf / 25 mm or more, 800 gf / 25 mm or more, or 1000 gf / 25 mm or more.

[0159] <Reinforcing film with release liner> The reinforcing film disclosed herein may take the form of an adhesive product in which the surface (adhesive surface) of the adhesive layer is in contact with the release surface of a release liner. Thus, this specification can provide a reinforcing film with a release liner, which includes any of the reinforcing films disclosed herein and a release liner having a release surface in contact with the adhesive surface of the reinforcing film. In this specification, the term "release liner" is also referred to as a "release liner," and is a concept that can include what are called release films and release sheets.

[0160] The thickness of the release liner is not particularly limited, but is usually about 5 μm to 200 μm. When the thickness of the release liner is within the above range, it is preferable because it is excellent in workability of laminating to the adhesive layer and workability of peeling from the adhesive layer. In some embodiments, the thickness of the release liner may be, for example, 10 μm or more, 20 μm or more, 30 μm or more, or 40 μm or more. In addition, from the viewpoint of facilitating peeling from the adhesive layer, the thickness of the release liner may be, for example, 100 μm or less, 80 μm or less, 60 μm or less, 50 μm or less, or 40 μm or less. The release liner may be subjected to a known antistatic treatment such as a coating type, a kneading type, or a deposition type, as necessary.

[0161] The release liner is not particularly limited, and examples thereof include a release liner having a release layer on the surface of a liner substrate such as a resin film or paper (which may be paper laminated with a resin such as polyethylene), and a release liner made of a resin film formed from a low-adhesion material such as a fluorine-based polymer (polytetrafluoroethylene, etc.) or a polyolefin resin (polyethylene, polypropylene, etc.). Since the surface smoothness is excellent, a release liner having a release layer on the surface of a resin film as a liner substrate, and a release liner made of a resin film formed from a low-adhesion material can be preferably used. The resin film is not particularly limited as long as it is a film that can protect the pressure-sensitive adhesive layer, and examples thereof include a polyethylene film, a polypropylene film, a polybutene film, a polybutadiene film, a polymethylpentene film, a polyvinyl chloride film, a vinyl chloride copolymer film, a polyester film (PET film, PBT film, etc.), a polyurethane film, and an ethylene-vinyl acetate copolymer film. The release layer can be formed using known release agents such as silicone-based release agents, long-chain alkyl-based release agents, olefin-based release agents, fluorine-based release agents, fatty acid amide-based release agents, molybdenum sulfide, silica powder, etc. The use of silicone-based release agents is particularly preferred.

[0162] The thickness of the release layer is not particularly limited, but is usually about 0.01 μm to 1 μm, and preferably about 0.1 μm to 1 μm. The method for forming the release layer is not particularly limited, and a known method can be appropriately adopted depending on the type of release treatment agent used, etc.

[0163] <Application> The reinforcing film provided by this specification can exhibit good reworkability, for example, in the initial stage after being attached to the adherend, and can contribute to suppressing a decrease in yield and improving the quality of products containing the reinforcing film. The adhesive strength of the reinforcing film can be greatly increased by aging or heating after being attached to the adherend. For example, by heating at an appropriate timing after being attached to the adherend, the reinforcing film can be firmly attached to the adherend. Taking advantage of such characteristics, the reinforcing film disclosed herein can be preferably used in various fields for the purpose of reinforcing members contained in various products.

[0164] The reinforcing film disclosed herein can be preferably used as a reinforcing film that is attached to an adherend and reinforces the adherend, for example, in the form of a substrate-attached pressure-sensitive adhesive sheet in which a pressure-sensitive adhesive layer is provided on at least the first surface of a film-like substrate having a first surface and a second surface. In such a reinforcing film, a film substrate containing a resin film as a base film can be preferably used. In addition, from the viewpoint of enhancing reinforcing performance, it is preferable that the pressure-sensitive adhesive layer is fixed to the first surface of the film-like substrate. For example, optical components used in optical products and electronic components used in electronic products are becoming highly integrated, smaller, lighter, and thinner, and multiple thin optical / electronic components with different linear expansion coefficients and thicknesses may be stacked. By attaching the above-mentioned reinforcing film to such components, it is possible to impart appropriate rigidity to the optical / electronic components. This makes it possible to suppress curling and curvature caused by stress that may occur between multiple components with different linear expansion coefficients and thicknesses during the manufacturing process and / or in the manufactured product. Furthermore, in the manufacturing process of optical products / electronic products, in the aspect of performing shaping processing such as cutting on thin optical / electronic components as described above, by attaching a reinforcing film to the components and processing the components, local stress concentration on the optical / electronic components accompanying processing can be alleviated, and the risk of cracks, breakage, peeling of laminated components, etc. Attaching the reinforcing film as a reinforcing member to the optical / electronic components and handling them can also be useful for alleviating local stress concentration during transportation, stacking, rotation, etc. of the components, and for suppressing bending or bending of the components due to their own weight. Furthermore, in the case of devices such as optical products and electronic products including the above-mentioned reinforcement film, when the devices are used by consumers in the market, even if the devices are subjected to unintentional stress such as when the devices are dropped, placed under a heavy object, or hit by a flying object, the inclusion of the reinforcement film in the devices can reduce stress on the devices. Therefore, the inclusion of the reinforcement film in the devices can improve the durability of the devices.

[0165] The reinforcing film disclosed herein may be preferably used in an embodiment in which it is attached to a member constituting various portable devices (portable devices). Here, "portable" does not mean that it is merely portable, but that it has a level of portability that allows an individual (average adult) to carry it relatively easily. Examples of portable devices herein include mobile phones, smartphones, tablet computers, notebook computers, various wearable devices, digital cameras, digital video cameras, audio devices (portable music players, IC recorders, etc.), calculators (calculators, etc.), portable game devices, electronic dictionaries, electronic organizers, electronic books, in-vehicle information devices, portable radios, portable televisions, portable printers, portable scanners, portable modems, and other portable electronic devices, as well as mechanical wristwatches, pocket watches, flashlights, hand mirrors, and the like. Examples of members constituting the above portable electronic devices may include optical films and display panels used in image display devices such as thin-layer displays such as liquid crystal displays and film-type displays. The reinforcing film disclosed herein may be preferably used in an embodiment in which it is attached to various members in automobiles, home appliances, and the like.

[0166] In addition, since the reinforcing film disclosed herein has an adhesive layer that exhibits good flexibility even in a low temperature range, it can be preferably used in an embodiment in which it is attached to a member constituting an apparatus having a bendable element (for example, a flexible device such as a flexible display. It may also be called a rollable device or a foldable device.) by taking advantage of this feature. Examples of such an apparatus include the above-mentioned various mobile devices (portable devices), and preferred examples include the above-mentioned various mobile electronic devices. Examples of members constituting the above-mentioned mobile electronic devices may include optical films and display panels used in image display devices such as liquid crystal displays and organic EL (electroluminescence) displays. The reinforcing film disclosed herein can be preferably used in such mobile electronic devices for reinforcing members constituting the apparatus (typically, image display devices called flexible devices, foldable devices, rollable devices, etc.).

[0167] The reinforcing film disclosed herein is suitable for use in reinforcing optical members during production, transportation, use, etc. of optical members used as components of liquid crystal display panels, plasma display panels (PDPs), organic EL displays, etc. The reinforcing film disclosed herein is useful as a reinforcing film applied to optical members such as polarizing plates (polarizing films), wave plates, retardation plates, optical compensation films, brightness enhancement films, light diffusion sheets, and reflective sheets for liquid crystal display panels.

[0168] The use of the reinforcing film disclosed herein is not particularly limited, and it can be used for various applications for the purpose of imparting rigidity and impact resistance. The reinforcing film disclosed herein can be preferably used not only for flexible device applications as described above, but also for other applications not including flexible devices. The fact that the reinforcing film has an adhesive with good flexibility (for example, flexibility in a low temperature range) means that there are few restrictions on the range of application of the reinforcing film, which has a great practical advantage.

[0169] The matters disclosed in this specification include the following. [1] A reinforcing film having a pressure-sensitive adhesive layer, The pressure-sensitive adhesive layer contains a polymer (A) and a polymer (B), The polymer (B) contains a monomer unit having a polyorganosiloxane skeleton and a (meth)acrylic monomer unit, The polymer (A) is an acrylic polymer containing a monomer unit derived from a nitrogen-containing monomer, The amount W of the monomer units derived from the nitrogen-containing monomer contained in 100 parts by weight of the polymer (A) N [Parts by weight] is 14 parts by weight or less, The pressure-sensitive adhesive layer is formed by mixing 100 parts by weight of the polymer (A) and 200 parts by weight of the polymer (A). Zr [parts by weight] of a zirconium-containing compound, Zr [Parts by weight] N [Part by weight] ratio (WN / W Zr ) is 4 or more. [2] The reinforcing film according to [1] above, wherein the pressure-sensitive adhesive layer contains a crosslinking agent. [3] The reinforcing film according to the above [1] or [2], wherein the content of the polymer (B) in the pressure-sensitive adhesive layer is 0.1 to 10 parts by weight per 100 parts by weight of the polymer (A). [4] The reinforcing film according to any one of [1] to [3], wherein the polymer (A) contains, as the monomer unit derived from the nitrogen-containing monomer, a monomer unit derived from a monomer having a nitrogen atom-containing ring. [5] The reinforcing film according to any one of the above [1] to [4], which has an adhesive strength N1 of 200 gf / 25 mm or less after being attached to a polyimide film at 23° C. for 30 minutes. [6] The reinforcing film according to any one of the above [1] to [5], which has an adhesive strength N2 of 1000 gf / 25 mm or more after being attached to a polyimide film and heated at 60°C for 1 hour and then at 23°C for 30 minutes. [7] The reinforcing film according to any one of the above [1] to [6], in which the rate of increase [%] in adhesive strength N2 [gf / 25 mm] after lamination to a polyimide film, heating at 60°C for 1 hour, and then at 23°C for 30 minutes, relative to adhesive strength N1 [gf / 25 mm] after lamination to a polyimide film and at 23°C for 30 minutes, is 900% or more. [8] The reinforcing film according to any one of the above [1] to [7], wherein the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer has a storage modulus at -20°C of 1000 kPa or less. [9] An optical member having the reinforcing film according to any one of [1] to [8] attached thereto.

[10] An electronic component having the reinforcing film according to any one of [1] to [8] attached thereto.

[11] A polymer (A) and a polymer (B), The polymer (B) contains a monomer unit having a polyorganosiloxane skeleton and a (meth)acrylic monomer unit, The polymer (A) is an acrylic polymer containing a monomer unit derived from a nitrogen-containing monomer, The amount W of the monomer units derived from the nitrogen-containing monomer contained in 100 parts by weight of the polymer (A) N [Parts by weight] is 14 parts by weight or less, W per 100 parts by weight of the above polymer (A) Zr [parts by weight] of a zirconium-containing compound, Zr [Parts by weight] N [Part by weight] ratio (W N / W Zr ) is 4 or more.

[12] A polymer (A) and a polymer (B), The polymer (B) contains a monomer unit having a polyorganosiloxane skeleton and a (meth)acrylic monomer unit, The polymer (A) is an acrylic polymer containing a monomer unit derived from a nitrogen-containing monomer, The amount W of the monomer units derived from the nitrogen-containing monomer contained in 100 parts by weight of the polymer (A) N [Parts by weight] is 14 parts by weight or less, W per 100 parts by weight of the above polymer (A) Zr [parts by weight] of a zirconium-containing compound, Zr [Parts by weight] N [Part by weight] ratio (W N / W Zr ) is 4 or more. EXAMPLES

[0170] Some examples of the present invention will be described below, but it is not intended that the present invention be limited to those specific examples. In the following description, "parts" and "%" are by weight unless otherwise specified.

[0171] <Synthesis of Polymer (A)> (Synthesis Example A1) In a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube and a condenser, 89.3 parts of 2-ethylhexyl acrylate (2EHA), 8.9 parts of 4-hydroxybutyl acrylate (4HBA), 1.8 parts of N-vinylpyrrolidone (NVP), 0.2 parts of 2,2'-azobisisobutyronitrile (AIBN) as a polymerization initiator, and ethyl acetate as a polymerization solvent were charged, and nitrogen gas was introduced while gently stirring. The liquid temperature in the flask was kept at around 65°C, and the polymerization reaction was carried out for 6 hours to prepare a polymer A1 solution with a polymer concentration of 35%. The weight average molecular weight (Mw) of polymer A1 was 540,000.

[0172] (Synthesis example A2) A solution of polymer A2 was obtained by carrying out solution polymerization in the same manner as in Synthesis Example A1, except that the monomer composition was changed to 2EHA / butyl acrylate (BA) / lauryl acrylate (LA) / 4HBA / NVP=70 parts / 20 parts / 8 parts / 1 part / 0.6 parts.

[0173] (Synthesis example A3) A solution of polymer A3 was obtained by carrying out solution polymerization in the same manner as in Synthesis Example A1, except that the monomer composition was changed to 2EHA / methyl methacrylate (MMA) / 2-hydroxyethyl acrylate (HEA) / NVP=63 parts / 9 parts / 13 parts / 15 parts.

[0174] <Synthesis of Polymer (B)> (Synthesis Example B1) 101.15 parts of ethyl acetate, 40 parts of MMA, 20 parts of n-butyl methacrylate (BMA), 20 parts of 2-ethylhexyl methacrylate (2EHMA), 8.7 parts of a polyorganosiloxane skeleton-containing methacrylate monomer having a functional group equivalent of 900 g / mol (trade name: X-22-174ASX, manufactured by Shin-Etsu Chemical Co., Ltd.), 11.3 parts of a polyorganosiloxane skeleton-containing methacrylate monomer having a functional group equivalent of 4600 g / mol (trade name: KF-2012, manufactured by Shin-Etsu Chemical Co., Ltd.), and 0.8 parts of thioglycerol as a chain transfer agent were charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas introduction tube, a cooler, and a dropping funnel. Then, after stirring for 30 minutes under a nitrogen atmosphere at 70 ° C, 0.2 parts of AIBN were charged as a thermal polymerization initiator and reacted at 70 ° C for 3 hours. After stirring at 80° C. for 30 minutes, 0.1 part of AIBN was further added and reacted at 80° C. for 2 hours. Then, 0.05 part of AIBN was further added and reacted at 80° C. for 2 hours to obtain polymer B1. Polymer B1 had an Mw of 20,000.

[0175] (Synthesis examples B2, B3) Polymers B2 and B3 were prepared in the same manner as in Synthesis Example B1, except that the amount of chain transfer agent (thioglycerol) used was changed to 0.6 parts (Synthesis Example B2) or 1.5 parts (Synthesis Example B3) per 100 parts of the monomer raw material. The Mw of Polymer B2 was 27,600, and the Mw of Polymer B3 was 12,600.

[0176] (Synthesis example B4) Polymer B4 was prepared in the same manner as in Synthesis Example B1, except that the monomer composition was changed to MMA / BMA / 2EHMA / X-22-174ASX / KF-2012=40 / 20 / 20 / 3.2 / 16.8. The Mw of Polymer B4 was 20,000.

[0177] The Mw of each of the above-mentioned polymers was measured under the following conditions using a GPC device (HLC-8220GPC, manufactured by Tosoh Corporation) and calculated in terms of polystyrene. [GPC conditions] Sample concentration: 0.2 wt% (tetrahydrofuran (THF) solution) Sample injection volume: 10μL ·Eluent: THF ·Flow rate: 0.6mL / min ·Measurement temperature: 40℃ ·column: Sample column: TSKguardcolumn SuperHZ-H (1 column) + TSKgel SuperHZM-H (2 columns) Reference column: TSKgel SuperH-RC (1 column) Detector: Differential refractometer (RI)

[0178] <Preparation of reinforcing film> (Example 1) To the polymer A1 solution, 2.0 parts of polymer B1, 0.1 part of isocyanate compound C1 (isocyanurate of hexamethylene diisocyanate, product name "Coronate HX", manufactured by Tosoh Corporation) as a crosslinking agent in terms of solid content, and 0.1 part of zirconium tetraacetylacetonate (product name "ZC150", manufactured by Matsumoto Fine Chemical Co., Ltd.) as a Zr-containing compound were added relative to 100 parts of polymer A1 contained in the solution, and the solution was diluted with ethyl acetate to a total solid content of 30%, thereby obtaining an acrylic adhesive solution according to this example. The adhesive solution obtained above was applied to a 75 μm-thick polyethylene terephthalate (PET) film (support substrate) having a first surface that was not surface-treated, and the solvent was removed by drying at 130° C. for 1 minute to form an adhesive layer having a thickness of 25 μm. The silicone-treated surface of a 25 μm-thick PET film (release liner) having one side that was silicone-treated was attached to the adhesive surface of this adhesive layer, and aging treatment was performed for 4 days at 25° C. In this way, a reinforcing film (reinforcing film) consisting of the support substrate and the adhesive layer laminated and fixed on the support substrate was obtained in the form of a reinforcing film with a release liner, in which a release liner was temporarily attached to the adhesive surface of the adhesive layer.

[0179] (Examples 2 to 7) Acrylic pressure-sensitive adhesive solutions according to each example were obtained in the same manner as in Example 1, except that the amounts of polymer B1, isocyanate compound C1, and Zr-containing compound used relative to 100 parts of polymer A1 were as shown in Table 1. Reinforcing films according to each example were prepared in the same manner as in Example 1, except that these acrylic pressure-sensitive adhesive solutions were used.

[0180] (Example 8) An acrylic adhesive solution according to each example was obtained in the same manner as in Example 1, except that an isocyanate compound C2 (a trimethylolpropane adduct of m-xylylene diisocyanate, product name "Takenate D110N", manufactured by Mitsui Chemicals, Inc.) was used instead of the isocyanate compound C1. A reinforcing film according to each example was produced in the same manner as in Example 1, except that each of these acrylic adhesive solutions was used.

[0181] (Examples 9-11) Except for using polymers B2 to B4 instead of polymer B1, acrylic pressure-sensitive adhesive solutions of each example were obtained in the same manner as in Example 1. Except for using these acrylic pressure-sensitive adhesive solutions, reinforcing films of each example were produced in the same manner as in the production of the reinforcing film of Example 1.

[0182] (Example 12) Except for using polymer A2 instead of polymer A1, an acrylic pressure-sensitive adhesive solution according to this example was obtained in the same manner as in Example 1. Except for using this acrylic pressure-sensitive adhesive solution, a reinforcing film according to this example was produced in the same manner as in the production of the reinforcing film according to Example 1.

[0183] (Example 13) An acrylic adhesive solution according to this example was obtained in the same manner as in Example 12, except that the amount of the Zr-containing compound used was as shown in Table 1. A reinforcing film according to this example was produced in the same manner as in Example 1, except that this acrylic adhesive solution was used.

[0184] (Examples 14-17) Instead of the Zr-containing compound used in Example 1, iron (III) acetylacetonate (trade name "Nacem Ferric", manufactured by Nippon Chemical Industry Co., Ltd.) was used in Example 14, aluminum tris acetylacetonate (trade name "AL3100", manufactured by Matsumoto Fine Chemical Co., Ltd.) was used in Example 15, titanium tetraacetylacetonate (trade name "TC401", manufactured by Matsumoto Fine Chemical Co., Ltd.) was used in Example 16, and dibutyltin (IV) dilaurate (trade name "OL-1", manufactured by Tokyo Fine Chemical Co., Ltd.) was used in Example 17. The acrylic adhesive solution according to each example was obtained in the same manner as in Example 1. The reinforcing film according to each example was produced in the same manner as in Example 1, except that these acrylic adhesive solutions were used.

[0185] (Example 18) An acrylic adhesive solution according to this example was obtained in the same manner as in Example 1, except that the amount of the Zr-containing compound used was as shown in Table 1. A reinforcing film according to this example was produced in the same manner as in Example 1, except that this acrylic adhesive solution was used.

[0186] (Example 19) Except for not using polymer B1, an acrylic pressure-sensitive adhesive solution according to this example was obtained in the same manner as in Example 1. Except for using this acrylic pressure-sensitive adhesive solution, a reinforcing film according to this example was produced in the same manner as in the production of the reinforcing film according to Example 1.

[0187] (Example 20) An acrylic pressure-sensitive adhesive solution according to this example was obtained in the same manner as in Example 8, except that polymer A3 was used instead of polymer A1 and the amount of isocyanate compound C2 used was as shown in Table 1. A reinforcing film according to this example was produced in the same manner as in the production of the reinforcing film according to Example 1, except that this acrylic pressure-sensitive adhesive solution was used.

[0188] <Evaluation> [-20℃ storage modulus (G′ -20 )] A release liner R1 (trade name "Diafoil MRF75", manufactured by Mitsubishi Chemical Corporation) made of polyester resin with a thickness of 75 μm and silicone-treated on one side was prepared, and the acrylic adhesive solution according to each example was applied to the silicone-treated surface, and dried at 130 ° C for 1 minute to form an adhesive layer with a thickness of 25 μm. Next, the surface of the obtained adhesive layer was covered with a release liner R2 (trade name "Diafoil MRE75", manufactured by Mitsubishi Chemical Corporation) made of polyester resin with a thickness of 75 μm and silicone-treated on one side, with the silicone-treated surface facing the adhesive layer, and aging was performed at 50 ° C for 1 day. Only the resulting adhesive layer was taken out and laminated to a thickness of about 1 mm, which was then punched out to a diameter of 8 mm to prepare a cylindrical pellet, which was used as a measurement sample. The above measurement sample was fixed to a φ8 mm parallel plate fixture and measured for the -20°C storage modulus (G′) under the following conditions using a dynamic viscoelasticity measuring device (TA Instruments, DHR-2). -20 ) [kPa] was measured. Measurement mode: Shear mode Temperature range: -30℃~100℃ Heating rate: 5℃ / min Frequency: 1Hz The storage modulus corresponds to the portion stored as elastic energy when a material is deformed, and is an index indicating the degree of hardness.

[0189] [Initial adhesive strength] The reinforcing film according to each example was cut together with the release liner to a width of 25 mm and a length of 140 mm to prepare a measurement sample. A 25 μm thick polyimide film (manufactured by Ube Industries, product name "Upilex 25S") was fixed to a glass plate via a double-sided adhesive tape (manufactured by Nitto Denko, product name "No. 531") to prepare a measurement polyimide plate. The release liner was peeled off from the measurement sample to expose the adhesive surface, and a 2 kg hand roller was rolled back and forth once to press the polyimide plate (adherend). The measurement sample thus pressed onto the adherend was left to stand for 30 minutes at an ambient temperature of 23°C, after which a tensile testing machine (Shimadzu Corporation, product name "Autograph AG-Xplus HS 6000mm / min high speed model (AG-50NX plus)") was used to measure the load when the reinforcing film was peeled off from the adherend at a peel angle of 180 degrees and a peel speed (tensile speed) of 300mm / min, and the average load during measurement was recorded as the initial adhesive strength [gf / 25mm]. In addition, since the reinforcing film of Example 19 had a high initial adhesive strength of 1000 gf / 25 mm or more, measurement of the adhesive strength after heating and calculation of the rate of increase were not performed.

[0190] [Adhesive strength after heating] For the reinforcing film according to each example, a measurement sample was prepared in the same manner as in the above initial adhesive strength measurement, and was pressed onto the polyimide substrate (adherend). The measurement sample pressed onto the adherend was heated for 60 minutes at an environmental temperature of 60°C. After that, it was left for 30 minutes at an environmental temperature of 23°C, and the load when the reinforcing film was peeled off from the adherend was measured using a tensile tester (manufactured by Shimadzu Corporation, product name "Autograph AG-Xplus HS 6000mm / min high-speed model (AG-50NX plus)") under the conditions of a peel angle of 180 degrees and a peel speed (tensile speed) of 300mm / min, and the average load during measurement was recorded as the adhesive strength after heating [gf / 25mm].

[0191] [Rise rate] Based on the initial adhesive strength [gf / 25 mm] and the adhesive strength after heating [gf / 25 mm] of the reinforcing film for each example, the rate of increase in adhesive strength was calculated using the following formula. Increase rate [%] = (Adhesive strength after heating [gf / 25mm] / Initial adhesive strength [gf / 25mm]) x 100

[0192] The evaluation results for the reinforcing film of each example are shown in Table 1. Table 1 also shows an outline of the composition of the pressure-sensitive adhesive layer of each example. N "[parts]" indicates the amount W of monomer units derived from nitrogen-containing monomers contained in 100 parts of the polymer (A) used in each example. N The amount of metal compounds in Table 1 is W Zr The "parts" in each example are the amount of metal compound used per 100 parts of polymer (A). For convenience, the "W" symbol is used even in examples where the metal species of the metal compound is not Zr. Zr " in Table 1. N / W Zr " is the amount of metal compound used in each example W Zr [parts] of polymer (A) N monomer content W N This is the ratio of [parts].

[0193] [Table 1]

[0194] As shown in Table 1, the pressure-sensitive adhesives according to Examples 1 to 13 contain a polymer (A), a polymer (B) and a Zr-containing compound. N is 14 parts or less, and the ratio (W N / W Zr ) was 4 or more. The reinforcing films according to these examples better achieved a balance between low initial adhesive strength and increased adhesive strength after heating compared to the reinforcing films according to Examples 14 to 19. Furthermore, the pressure-sensitive adhesives according to Examples 1 to 13 had a significantly lower -20°C storage modulus than the pressure-sensitive adhesive according to Example 20, and exhibited good flexibility in addition to achieving a balance between the above-mentioned low initial adhesive strength and increased adhesive strength after heating.

[0195] More specifically, a comparison between Example 1, in which a Zr-containing compound was used as the metal compound, and Examples 14 to 16, in which a Zr-free metal compound was used instead of the Zr-containing compound, shows that the use of a Zr-containing compound tends to improve the post-heat adhesive strength to polyimide. Example 17, in which a tin compound was used instead of the Zr-containing compound, showed higher post-heat adhesive strength than Examples 14 to 16, but the initial adhesive strength was also higher than Examples 14 to 16, resulting in a lower rate of increase in adhesive strength. Furthermore, a comparison between Examples 1 to 3 and Example 18, in which a Zr-containing compound was used, shows that the ratio (W N / W Zr When the W value fell below 4, the adhesive strength after heating dropped sharply. The reinforcing film of Example 19, which used an adhesive that did not contain polymer (B), had a high initial adhesive strength, and N The pressure-sensitive adhesive of Example 20, which used polymer (A) having a molecular weight of more than 14 parts, had a high storage modulus at -20°C.

[0196] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above. [Explanation of symbols]

[0197] 1,2,3 Reinforcement film 10 Supporting base material 10A front page 10B second side 21 Adhesive layer (first adhesive layer) 21A Adhesive surface (first adhesive surface) 21B Adhesive surface (second adhesive surface) 22 Adhesive layer (second adhesive layer) 22A Adhesive surface (second adhesive surface) 31,32 Release liner 100,200,300 Reinforcement film with release liner

Claims

1. A reinforcing film having a pressure-sensitive adhesive layer, The pressure-sensitive adhesive layer contains a polymer (A) and a polymer (B), The polymer (B) contains a monomer unit having a polyorganosiloxane skeleton and a (meth)acrylic monomer unit, The polymer (A) is an acrylic polymer containing a monomer unit derived from a nitrogen-containing monomer, The amount W of the monomer unit derived from the nitrogen-containing monomer contained in 100 parts by weight of the polymer (A) N [Parts by weight] is 14 parts by weight or less, The pressure-sensitive adhesive layer is formed by mixing 100 parts by weight of the polymer (A) and 200 parts by weight of the polymer (A). Zr [parts by weight] of a zirconium-containing compound, Zr [Parts by weight] N [weight parts] ratio (W N / W Zr ) is 4 or more.

2. The reinforcing film according to claim 1 , wherein the pressure-sensitive adhesive layer contains a crosslinking agent.

3. The reinforcing film according to claim 1 or 2, wherein the content of the polymer (B) in the pressure-sensitive adhesive layer is 0.1 to 10 parts by weight per 100 parts by weight of the polymer (A).

4. The reinforcing film according to claim 1 or 2, wherein the polymer (A) contains, as the monomer unit derived from the nitrogen-containing monomer, a monomer unit derived from a monomer having a nitrogen atom-containing ring.

5. 3. The reinforcing film according to claim 1, wherein the adhesive strength N1 after being attached to a polyimide film at 23° C. for 30 minutes is 200 gf / 25 mm or less.

6. The reinforcing film according to claim 5, which has an adhesive strength N2 of 1000 gf / 25 mm or more after being attached to a polyimide film and heated at 60° C. for 1 hour and then at 23° C. for 30 minutes.

7. The reinforcing film according to claim 6, wherein the rate of increase [%] of the adhesive strength N2 [gf / 25 mm] relative to the adhesive strength N1 [gf / 25 mm] is 900% or more.

8. The reinforcing film according to claim 1 or 2, wherein the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer has a storage modulus at -20°C of 1000 kPa or less.

9. An optical member having the reinforcing film according to claim 1 or 2 attached thereto.

10. An electronic component having the reinforcing film according to claim 1 or 2 attached thereto.

Citation Information

Patent Citations

  • JP1988066199A

  • Simple herpesvirus glycoprotein and production thereof

    JP1988066200A

  • Shared memory access device

    JP1988073458A

  • Alkailine zinc storage battery

    JP1988076271A

  • Adhesive for optical film, adhesive layer for optical film, optical member and image display device

    JP2016108555A