Evaluation method of all-solid lithium ion battery
By uniformly sintering and assembling oxide-based all-solid-state batteries under controlled conditions, the method addresses variations in battery characteristic evaluations, enabling precise assessment of the battery's performance.
Patent Information
- Application Number
- JP2023050216
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
There are variations in the evaluation of battery characteristics of oxide-based all-solid-state batteries, making it difficult to accurately assess the positive electrode active material and solid electrolyte, which are crucial raw materials for these batteries.
A method involving the production of powder compacts of a solid electrolyte and positive electrode layer, followed by sintering under a uniform load, ensuring consistent application of pressure to form a fired body, and subsequent battery assembly and evaluation, utilizing specific compositional formulas for the solid electrolyte and positive electrode active material.
This method allows for accurate evaluation of battery characteristics by minimizing variations, thereby improving the reliability of assessing oxide-based all-solid-state batteries.
Smart Images

Figure 2024139328000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for evaluating an all-solid-state lithium-ion battery. [Background technology]
[0002] In recent years, with the rapid spread of information-related devices and communication devices such as personal computers, video cameras, and mobile phones, the development of batteries to be used as power sources for these devices has become important. Among these batteries, lithium ion batteries have attracted attention from the viewpoint of their high energy density. In addition, there is a demand for improvements in the energy density and battery characteristics of lithium secondary batteries for large-scale applications such as vehicle-mounted power sources and load leveling.
[0003] LISICON-type oxide-based solid electrolytes are expected to be the next-generation solid electrolyte for all-solid-state batteries as solid materials that conduct Li ions. In addition, it is possible to introduce Li deficiency or excess Li by replacing it with ions of different valence, and it has the advantage that materials can be prepared by combining various elements.
[0004] Non-Patent Document 1 describes a LISICON-type solid electrolyte, Li 3.5 Ge 0.5 V 0.5 They disclose that they combined O4 with NCM111 (a positive electrode active material containing Ni, Co and Mn in a 1:1:1 composition ratio), a Ni-Co-Mn ternary positive electrode active material, and co-sintered it using spark plasma sintering to create a cell, resulting in the production of a sintered body for a cell that exhibits stable charge / discharge behavior. [Prior art documents] [Non-patent literature]
[0005] [Non-Patent Document 1] Toyoki Okumura, Tomonari Takeuchi, and Hironori Kobayashi, All-Solid-State Batteries with LiCoO2-Type Electrodes: Realization of an Impurity-Free Interface by Utilizing a Cosinterable Li3.5Ge0.5V0.5O4 Electrolyte, ACS Appl. Energy Mater. (2021), 4, 1, 30-34. Summary of the Invention [Problem to be solved by the invention]
[0006] Oxide-based all-solid-state lithium-ion batteries, which use non-flammable oxide-based solid electrolytes, are attracting attention as next-generation batteries that are significantly safer and more reliable than conventional lithium-ion batteries.
[0007] The battery characteristics of oxide-based all-solid-state batteries have been evaluated from various viewpoints. It is necessary to accurately evaluate the battery characteristics of such oxide-based all-solid-state batteries, but there is a problem that the evaluation of the battery characteristics of oxide-based all-solid-state batteries produced using the same cathode active material and solid electrolyte as raw materials varies. If there is a variation in the evaluation of the battery characteristics, it becomes difficult to accurately evaluate the cathode active material and solid electrolyte that are the raw materials.
[0008] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a method for accurately evaluating the battery characteristics of an oxide-based all-solid-state battery. [Means for solving the problem]
[0009] The present invention, which has been completed based on the above findings, is defined by the following (1) to (5). (1) A method for evaluating an all-solid-state lithium ion battery including a solid electrolyte layer including an oxide-based solid electrolyte, a positive electrode layer including a positive electrode active material, and a negative electrode layer, comprising: a sintered body producing step of producing a plurality of compacts of a solid electrolyte layer / anode layer by pressing the cathode composite material containing the cathode active material and the solid electrolyte, and producing a sintered body by sintering the plurality of compacts under a load; a battery production process in which a laminate produced by providing a negative electrode layer on a surface of the solid electrolyte layer of the fired body is placed in a sealed container and a predetermined confining pressure is applied to produce an all-solid-state lithium ion battery; A battery evaluation step of evaluating battery characteristics of the all-solid-state lithium ion battery; Including, In the sintered body preparation step, the plurality of green compacts are each formed into a columnar shape, and are provided on a plane at three vertices of an equilateral triangle, spaced apart from one another, and a pressure of 30 to 92 g / cm is applied from above the green compact. 2 This is a method for evaluating all-solid-state lithium-ion batteries in which the material is sintered under a load. (2) The method for evaluating an all-solid-state lithium ion battery according to (1), wherein in the sintered body preparation step, the plurality of compacts are provided on a flat surface, one at a time, at central positions of three sides of the equilateral triangle, spaced apart from each other. (3) The method for evaluating an all-solid-state lithium ion battery according to (1) or (2), wherein, in the sintered body preparation step, one more of the plurality of compacts is provided on a plane at a center of gravity of the equilateral triangle. (4) The method for evaluating an all-solid-state lithium ion battery according to any one of (1) to (3), wherein each of the plurality of powder compacts is formed into a cylindrical shape. (5) The oxide-based solid electrolyte has the composition formula 1: Li α A x M y O4 (In the composition formula 1, A is Ge, Si or Ti, M is V, P or As, 3.25≦α≦3.75, 0.30≦x≦0.75, and 0.25≦y≦0.70.) It is expressed as The positive electrode active material is represented by the formula 2: Li a Ni b Co c Mn dO2 (In the composition formula 2, 1.00≦a≦1.08, 0.33≦b≦0.90, and b+c+d=1.0.) The method for evaluating an all-solid-state lithium ion battery according to any one of (1) to (4), Effect of the Invention
[0010] According to the present invention, a method for accurately evaluating the battery characteristics of an oxide-based all-solid-state battery can be provided. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic view showing the appearance of a cylindrical green compact according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a schematic diagram showing an example of the arrangement of cylindrical powder compacts on a plane according to an embodiment of the present invention. [Diagram 3] 10A and 10B are schematic diagrams showing another example of the arrangement of cylindrical powder compacts on a plane according to an embodiment of the present invention. [Figure 4] FIG. 13 is a schematic diagram showing yet another example of arrangement of a cylindrical powder compact on a plane according to an embodiment of the present invention. [Diagram 5] FIG. 1 is a schematic diagram of an all-solid-state lithium-ion battery according to an embodiment of the present invention. [Figure 6] 1A is a schematic plan view of the arrangement of powder compacts according to Example 1, and FIG. 1B is a schematic side view of the arrangement of powder compacts according to Example 1. [Figure 7] FIG. 2 is a schematic plan view of the arrangement of a powder compact according to Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Next, the embodiments of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiments, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.
[0013] <Evaluation method for all-solid-state lithium-ion batteries> The method for evaluating an all-solid-state lithium-ion battery according to an embodiment of the present invention is a method for evaluating an all-solid-state lithium-ion battery including a solid electrolyte layer including an oxide-based solid electrolyte, a positive electrode layer including a positive electrode active material, and a negative electrode layer, and includes a sintered body preparation step, a battery preparation step, and a battery evaluation step.
[0014] <Sintered body production process> In the sintered body preparation process, a positive electrode composite material containing a positive electrode active material and a solid electrolyte are pressed to prepare multiple compacts of a solid electrolyte layer / positive electrode layer, and the multiple compacts are sintered under a load to prepare a sintered body.
[0015] The positive electrode mixture containing the positive electrode active material and the solid electrolyte may be pressed with a pressure of 300 to 400 g / cm using a known press, although this is not particularly limited. 2 The pressing can be performed by applying a pressure of 100 MPa. A plurality of pressed powder bodies of the solid electrolyte layer / positive electrode layer produced by pressing the positive electrode composite material containing the positive electrode active material and the solid electrolyte are each formed in a columnar shape. The pressed powder body may be a columnar shape (cylindrical shape) having a circular end face, a columnar shape (rectangular columnar shape) having a polygonal end face, or a columnar shape having an indeterminate end face. From the viewpoints of production efficiency and avoidance of stress concentration, the pressed powder body is preferably cylindrical.
[0016] As a specific example of a powder compact according to an embodiment of the present invention, a schematic external view of a cylindrical powder compact 10 is shown in Fig. 1. An embodiment of the present invention will be described using such a cylindrical powder compact 10 as an example, but as described above, the shape of the powder compact is not particularly limited as long as it is columnar, and the embodiment described below can be adopted.
[0017] The powder compact 10 is formed by pressing a cathode composite material containing a cathode active material and a solid electrolyte, and has a configuration in which a solid electrolyte layer 11 and a cathode layer 12 are laminated (solid electrolyte layer / cathode layer). It is most preferable that the end face of the powder compact 10 is a perfect circle, but it does not have to be a perfect circle and may be an ellipse. The central axis L of the cylindrical powder compact 10 passes through the center of gravity O of the circle at the end face of the powder compact 10. The powder compact 10 is placed on a flat surface so that the central axis L extends vertically.
[0018] 2, the powder compacts 10 are provided on a plane 13 at the three vertices of an equilateral triangle 14, spaced apart from one another. The powder compacts 10 are preferably provided such that the center of gravity O of the circle at the end face thereof overlaps with the three vertices of the equilateral triangle 14. The plane 13 is a flat surface on which the powder compact 10 can be stably placed, and the specific form thereof is not particularly limited to a pedestal, stage, or the like, but since the powder compact is placed in a firing furnace and heated for sintering, it is particularly preferable to use the surface of a ceramic setter, such as an MgO or ZrO2 setter, as the plane.
[0019] In the sintered body preparation process, a powder density of 30 to 92 g / cm is applied to the compacts 10 provided at the three vertices of the equilateral triangle 14, one at a time and spaced apart from each other. 2 According to this configuration, the three columnar green compacts 10 are provided at the three vertices of the equilateral triangle 14, spaced apart from each other, and a load of 30 to 92 g / cm is applied to the green compacts 10. 2 Since a load of 100 μm is applied to each of the powder compacts 10, sintering can be performed under a very stable and uniform load. Therefore, the powder compacts 10 have the same performance regardless of which one is used, and it is possible to suppress variations in the evaluation of the battery characteristics. As a result, the battery characteristics of the all-solid-state lithium-ion battery can be accurately evaluated.
[0020] 3, the powder compacts 10 are provided on a plane 13 at three vertices of an equilateral triangle 14, spaced apart from one another, and may also be provided at the centers of the three sides of the equilateral triangle 14, spaced apart from one another. With this configuration, a total of six powder compacts 10, one at each of the three vertices and the center of each side of the equilateral triangle 14, can be sintered at one time under a very stable and uniform load. This makes it possible to efficiently prevent variations in the evaluation of battery characteristics for a larger number of powder compacts.
[0021] 4, the powder compacts 10 are provided on a plane 13 at three vertices of an equilateral triangle 14, one at a time, spaced apart from one another, and one may be provided at the center A of the equilateral triangle 14. With this configuration, a total of four powder compacts 10, one at each of the three vertices of the equilateral triangle 14 and one at the center A of the equilateral triangle 14, can be sintered at one time under a very stable and uniform load. This makes it possible to efficiently prevent variations in the evaluation of battery characteristics for a larger number of powder compacts.
[0022] The area of the end face of the powder compact 10 is not particularly limited, but is preferably 0.5 to 1.0 cm 2 The height of the powder compact 10 is not particularly limited, and may be 0.03 to 0.06 cm. In the sintered body production process according to the embodiment of the present invention, a plurality of powder compacts 10 are placed on a flat surface 13 and a weight is applied from above, so that it is preferable that all of them have the same height in terms of applying an even load. In addition, from the viewpoints of applying an even load and facilitating control of the load per unit area, it is preferable that all of the plurality of powder compacts 10 have the same end face area.
[0023] In order to apply a load uniformly to the multiple powder compacts 10 at once, it is preferable to place a flat plate on the multiple powder compacts 10 and place a weight on the flat plate. The flat plate is not particularly limited, but is preferably a ceramic setter such as an MgO or ZrO2 setter, since it is placed in a firing furnace and heated for sintering. The setter may also be used as a weight. In this case, only a single flat setter is placed on the multiple powder compacts 10, in addition to the Au film described below, and serves as a weight.
[0024] By placing a weight on the flat plate, each of the powder compacts 10 is pressed with a pressure of 30 to 92 g / cm. 2The mass of the weight is not particularly limited, and can be appropriately designed depending on the number of powder compacts 10 and the surface area of the upper end face of the powder compact 10. When an Au film and a setter, which will be described later, are placed on the powder compact 10, the mass of the setter is considered to be the load applied, and the mass of the setter is adjusted. Note that the Au film has a mass that is about 1 / 100 of the weight, and therefore can be ignored in the calculation of the load. The load applied to a plurality of powder compacts 10 is 45 to 65 g / cm. 2 It is more preferable that:
[0025] A precious metal film may be provided between the powder compact 10 and the flat surfaces of the setters, etc., provided above and below the powder compact 10, in order to prevent the diffusion of components of the setters, etc. The precious metal film is not particularly limited, but it is preferable to use an Au film, a Pt film, an Ir film, etc.
[0026] Sintering can be carried out using a known firing furnace or the like, and is preferably carried out at 700 to 800° C. for 2 to 12 hours.
[0027] <Battery manufacturing process> In the battery preparation process, a laminate prepared by providing an anode layer on the surface of the solid electrolyte layer of the fired body is placed in a sealed container, and a predetermined confining pressure is applied to prepare an all-solid-state lithium-ion battery. Here, the sealed container is a container for isolating the laminate from the atmosphere, and is not particularly limited as long as it is one that is generally used for all-solid-state lithium-ion batteries. The configuration of the anode layer will be described later. In addition, the material and shape of the sealed container in which the laminate is placed are not particularly limited, and can be appropriately designed according to the shape, size, etc. of the desired all-solid-state lithium-ion battery.
[0028] <Battery evaluation process> In the battery evaluation step, the all-solid-state lithium-ion battery produced as described above is evaluated for predetermined battery characteristics. Examples of the battery characteristics of the all-solid-state lithium-ion battery include discharge capacity and cycle characteristics. The all-solid-state lithium-ion batteries produced in the embodiment of the present invention are each produced from a plurality of compacts sintered as described above under a very stable and uniform load. This makes it possible to efficiently suppress variations in the evaluation of the battery characteristics of the all-solid-state lithium-ion battery. As a result, the battery characteristics of the all-solid-state lithium-ion battery can be accurately evaluated.
[0029] <All-solid-state lithium-ion battery> The all-solid-state lithium-ion battery to be evaluated in the evaluation method of the all-solid-state lithium-ion battery according to the embodiment of the present invention includes a solid electrolyte layer containing an oxide-based solid electrolyte, a positive electrode layer containing a positive electrode active material, and a negative electrode layer. The all-solid-state lithium-ion battery can have a configuration as shown in FIG.
[0030] (Solid electrolyte layer) The composition of the solid electrolyte layer of the present embodiment is not particularly limited, but may be, for example, a composition represented by the formula 1: Li α A x M y O4 (wherein A is Ge, Si or Ti, M is V, P or As, 3.25≦α≦3.75, 0.30≦x≦0.75, and 0.25≦y≦0.70). The oxide-based solid electrolyte of this embodiment is a LISICON-type solid electrolyte, Li α Ge x V y The composition is a base material of O4, or a base material substituted with Si, Ti, P, or As. With this composition, the number of elements constituting the oxide-based solid electrolyte is increased, and the activation energy is reduced, resulting in an oxide-based solid electrolyte with good ion conductivity. As a result, the capacity of the all-solid-state lithium-ion battery is increased. In the present invention, the oxide-based solid electrolyte refers to a solid electrolyte having, in its skeleton, an oxoacid ion in which an oxygen atom is coordinately bonded to a central element, as a counter anion to a lithium ion.
[0031] In the oxide-based solid electrolyte of the present embodiment, if α is less than 3.25 in the above composition formula 1, the carrier concentration is low, so that the ion conductivity may be reduced. If α is more than 3.75, the single-phase synthesis may be difficult. In the oxide-based solid electrolyte of the present embodiment, it is preferable that 3.40≦α≦3.70 in the above composition formula 1.
[0032] In the oxide-based solid electrolyte of this embodiment, if x is less than 0.30 in the above composition formula 1, a Li4GeO4 phase with low ionic conductivity may be generated. If x is more than 0.75, the crystal lattice becomes large, so the distance between Li sites becomes long, and the ionic conductivity may decrease. In the oxide-based solid electrolyte of this embodiment, it is preferable that 0.40≦x≦0.60 in the above composition formula 1.
[0033] In the oxide-based solid electrolyte of this embodiment, if y is less than 0.25 in the above composition formula 1, the effect of reducing activation energy by element substitution is weak, so the effect of improving ion conductivity may be small. Also, if y is more than 0.70, impurity phases such as Li4VO4 may be generated, and ion conductivity may decrease. In the oxide-based solid electrolyte of this embodiment, it is preferable that 0.30≦y≦0.60 in the above composition formula 1.
[0034] The average particle size of the oxide-based solid electrolyte of this embodiment is not particularly limited, but may be 0.01 to 100 μm, 0.1 to 100 μm, or 0.1 to 50 μm.
[0035] The oxide-based solid electrolyte of this embodiment can be produced as follows. First, raw materials are weighed out to obtain a desired composition in a glove box with an inert gas atmosphere such as argon gas or nitrogen gas. Examples of the raw materials used here include LiOH·H2O, GeO2, V2O5, SiO2, TiO2, H3PO4, and H3AsO3.
[0036] Next, the mixture is mixed in a mortar or the like for 5 to 30 minutes to prepare a mixed powder. At this time, it is preferable to mix for such a time that the average particle size of the mixed powder becomes 5 to 40 μm.
[0037] Next, the mixed powder is placed in an alumina sagger and sintered at 600 to 1000°C for 1 to 20 hours to obtain a powder of the composition formula 1: Li α A x M y O4 (in composition formula 1, A is Ge, Si or Ti, M is V, P or As, 3.25≦α≦3.75, 0.30≦x≦0.75, and 0.25≦y≦0.70), it is possible to prepare an oxide-based solid electrolyte of the present embodiment.
[0038] The average thickness of the solid electrolyte layer of the lithium ion battery formed by the oxide-based solid electrolyte of this embodiment is not particularly limited and can be appropriately designed according to the purpose. The average thickness of the solid electrolyte layer of this embodiment may be, for example, 50 μm to 500 μm, or 50 μm to 100 μm.
[0039] (Positive electrode layer) The composition of the positive electrode active material contained in the positive electrode layer of the present embodiment is not particularly limited. For example, a Ni b Co c Mn dO2 (in composition formula 2, 1.00≦a≦1.08, 0.33≦b≦0.90, and b+c+d=1.0). More specifically, the positive electrode layer of this embodiment can be a layer of a positive electrode mixture obtained by mixing the positive electrode active material represented by composition formula 2 with the oxide-based solid electrolyte of this embodiment. The content of the positive electrode active material in the positive electrode layer is, for example, preferably 50% by mass or more and 99% by mass or less, and more preferably 55% by mass or more and 75% by mass or less.
[0040] The positive electrode active material of this embodiment preferably has a Ni ratio of 0.60≦b≦0.90. When a high-nickel NCM positive electrode active material having such a high Ni ratio is used, the capacity of the all-solid-state lithium-ion battery generally becomes high. From this viewpoint, it is more preferable that 0.80≦b≦0.90 in the above composition formula 2. The positive electrode active material of this embodiment is not particularly limited as long as it satisfies the above composition formula 2, and a known positive electrode active material can be used.
[0041] Previously, high-nickel NCM positive electrode active materials with a high Ni ratio of 0.60≦b≦0.90 would react with solid electrolytes to produce reactants that did not conduct Li ions, causing the battery to fail, but this type of high-nickel NCM positive electrode active material does not produce any reactants with the oxide-based solid electrolyte represented by the above composition formula 1. For this reason, an all-solid-state lithium-ion battery that has the oxide-based solid electrolyte represented by the above composition formula 1 in the solid electrolyte layer and the high-nickel NCM positive electrode active material represented by the above composition formula 2 in the positive electrode layer can provide an oxide-based all-solid-state battery that achieves high capacity.
[0042] The positive electrode mixture may further include a conductive assistant. As the conductive assistant, a carbon material, a metal material, or a mixture thereof may be used. The conductive assistant may include at least one element selected from the group consisting of, for example, carbon, nickel, copper, aluminum, indium, silver, cobalt, magnesium, lithium, chromium, gold, ruthenium, platinum, beryllium, iridium, molybdenum, niobium, osmium, rhodium, tungsten, and zinc. The conductive assistant is preferably a highly conductive carbon element, a metal element, a mixture, or a compound containing carbon, nickel, copper, silver, cobalt, magnesium, lithium, ruthenium, gold, platinum, niobium, osmium, or rhodium. As the carbon material, for example, carbon black such as Ketjen Black, acetylene black, denka black, thermal black, and channel black, graphite, carbon fiber, activated carbon, and the like may be used.
[0043] The average thickness of the positive electrode layer of the all-solid-state lithium ion battery is not particularly limited and can be appropriately designed according to the purpose. The average thickness of the positive electrode layer of the all-solid-state lithium ion battery may be, for example, 1 μm to 100 μm, or 1 μm to 10 μm.
[0044] (Negative electrode layer) The negative electrode layer of the all-solid-state lithium ion battery is not particularly limited, and may be a layer of a known negative electrode active material for all-solid-state lithium ion batteries. The negative electrode layer may be a layer of a negative electrode mixture obtained by mixing a known negative electrode active material for all-solid-state lithium ion batteries with a solid electrolyte. The content of the negative electrode active material in the negative electrode layer is, for example, preferably 10% by mass or more and 99% by mass or less, and more preferably 20% by mass or more and 90% by mass or less.
[0045] The negative electrode layer may contain a conductive assistant, as in the positive electrode layer. The conductive assistant may be the same material as that described in the positive electrode layer. As the negative electrode active material, for example, a carbon material, specifically, artificial graphite, graphite carbon fiber, resin-calcined carbon, pyrolytic vapor-grown carbon, coke, mesocarbon microbeads (MCMB), furfuryl alcohol resin-calcined carbon, polyacene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, non-graphitizable carbon, or a mixture thereof may be used. As the negative electrode material, for example, a metal itself, such as metallic lithium, metallic indium, metallic aluminum, or metallic silicon, or an alloy in combination with other elements or compounds may be used.
[0046] The average thickness of the negative electrode layer of the all-solid-state lithium ion battery is not particularly limited and can be appropriately selected depending on the purpose. The average thickness of the negative electrode layer of the all-solid-state lithium ion battery may be, for example, 1 μm to 100 μm, or 1 μm to 10 μm.
[0047] The method for forming the negative electrode layer of the all-solid-state lithium ion battery is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method for forming the negative electrode layer of the all-solid-state lithium ion battery include a method of compressing and molding negative electrode active material particles, and a method of depositing a negative electrode active material.
[0048] Other members constituting the lithium ion battery are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include a positive electrode collector, a negative electrode collector, and a battery case.
[0049] The size and structure of the positive electrode current collector are not particularly limited and can be appropriately selected depending on the purpose. Examples of the material for the positive electrode current collector include die steel, stainless steel, aluminum, aluminum alloys, titanium alloys, copper, gold, and nickel. The positive electrode current collector may be in the form of, for example, a foil, a plate, or a mesh. The average thickness of the positive electrode current collector may be, for example, 10 μm to 500 μm, or 50 μm to 100 μm.
[0050] The size and structure of the negative electrode current collector are not particularly limited and can be appropriately selected depending on the purpose. Examples of the material for the negative electrode current collector include die steel, gold, indium, nickel, copper, and stainless steel. The negative electrode current collector may be in the form of, for example, a foil, a plate, or a mesh. The average thickness of the negative electrode current collector may be, for example, 10 μm to 500 μm, or 50 μm to 100 μm.
[0051] The battery case is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include known laminate films that can be used in conventional all-solid-state batteries, etc. Examples of the laminate film include a resin laminate film and a film in which a metal is vapor-deposited on a resin laminate film. The shape of the battery is not particularly limited and can be appropriately selected depending on the purpose. Examples of the shape of the battery include cylindrical, square, button, coin, and flat types. EXAMPLES
[0052] The following examples are provided to provide a better understanding of the present invention and its advantages, but the present invention is not limited to these examples.
[0053] <1. Preparation of oxide-based solid electrolyte and positive electrode active material> (Examples 1 to 3, Comparative Examples 1 to 2) Li 3.5 Ge 0.5 V 0.5 Oxide-based solid electrolyte with the composition of O4 and LiNi 0.6 Co 0.2 Mn 0.2 A positive electrode active material having a composition of O2 was prepared. The composition of the positive electrode active material was evaluated as follows. That is, 5 g of a sample (powder) of the positive electrode active material was weighed out and decomposed by the alkali fusion method, and then the composition was analyzed using an inductively coupled plasma optical emission spectrometer (ICP-OES) "PS7800" manufactured by Hitachi High-Tech Corporation. The oxygen content was obtained by subtracting the analysis values of Li and metal components, as well as the impurity concentration and residual alkali amount, from the total amount of the analyzed sample, and the z value of the oxygen composition (Oz) was calculated from the oxygen content. The composition of the oxide-based solid electrolyte was evaluated as follows: 0.5 g of a sample (powder) of the oxide-based solid electrolyte was weighed out and dissolved in various acids, and then the composition was analyzed using an inductively coupled plasma optical emission spectrometer (ICP-OES) "PS7800" manufactured by Hitachi High-Tech Corporation.
[0054] <2. Preparation of powder compact> Example 1 The positive electrode active material, the oxide-based solid electrolyte, and the binder were mixed in this order in a mass ratio of 50:50:5, and anisole was added as a solvent so that the solid content of the slurry was approximately 55 mass%. The mixture was mixed in a Mazerustar for 400 seconds to form a positive electrode composite slurry. The solvent of the resulting slurry was dried at room temperature, and then the mixture was crushed in a mortar and pestle to obtain a positive electrode composite powder. Next, about 10 mg of the above-mentioned positive electrode composite powder was placed on the temporarily pressed oxide-based solid electrolyte, and pressed at 333 MPa to produce a cylindrical green compact of the solid electrolyte layer / positive electrode layer. 2 and the height was 0.03 cm. A total of three powder compacts having such a structure were produced and arranged as shown in Figures 6(A) and 6(B). Figure 6(A) is a schematic plan view of the arrangement of the powder compacts according to Example 1. Figure 6(B) is a schematic side view of the arrangement of the powder compacts according to Example 1. That is, first, an MgO setter 16 having a flat surface 13 was prepared, and an Au film 15 was provided on the flat surface 13 . Next, the powder compacts 10 were placed on the flat surface of the Au film 15, one at each of the three vertices of an equilateral triangle 14, spaced apart from one another. At this time, the length of each side of the equilateral triangle 14 was 2 cm. Next, with the Au film 15 inserted on top of the cylindrical powder compact 10, an MgO setter 17 (60 g) acting as a weight was placed on top of the compact, and the compact was placed in an electric furnace and sintered at 800° C. for 2 hours to produce a sintered body of the solid electrolyte layer / positive electrode layer.
[0055] Example 2 A sintered body of a solid electrolyte layer / positive electrode layer was produced under the same conditions as in Example 1, except that the mass of the MgO setter 17 placed on the upper surface was 120 g.
[0056] Example 3 A sintered body of a solid electrolyte layer / positive electrode layer was produced under the same conditions as in Example 1, except that the mass of the MgO setter 17 placed on the upper surface was 180 g.
[0057] Comparative Example 1 A total of five cylindrical powder compacts 20 having the same configuration as the powder compact 10 were produced by the same method as in Example 1, and were arranged as shown in Fig. 7. Fig. 7 is a schematic plan view of the arrangement of the powder compacts according to Comparative Example 1. Specifically, first, an MgO setter having a flat surface 23 was prepared, and an Au film was provided on the flat surface 23. Next, the powder compact 20 was placed on the flat surface of the Au film, one at each of the four vertices and the center of gravity of a regular rectangle 24, spaced apart from one another. At this time, the length of each side of the regular rectangle 24 was 3 cm. The powder compact 20 was placed so that the center of gravity O of the circle on its end face overlapped with the four vertices and the center of gravity of the regular rectangle 24, respectively. Next, with the Au film inserted on top of the cylindrical powder compact 20, an MgO setter (60 g) acting as a weight was placed on top, and the compact was placed in an electric furnace and sintered at 800°C for 2 hours to produce a sintered body of the solid electrolyte layer / positive electrode layer.
[0058] Comparative Example 2 A sintered body of a solid electrolyte layer / positive electrode layer was produced under the same conditions as in Example 1, except that the mass of the MgO setter placed on the upper surface was 230 g.
[0059] <3. Fabrication of all-solid-state lithium-ion batteries> (Examples 1 to 3, Comparative Examples 1 to 2) Next, a polymer solid electrolyte and metallic Li were pressed onto the negative electrode side of the solid electrolyte layer of the fired body to form the negative electrode layer. The laminate thus produced was placed in a sealed SUS304 battery test cell (sealed container) to block out the atmosphere, and a confining pressure of 0.4 N m was applied to produce an all-solid-state secondary battery. In this way, an all-solid-state lithium-ion battery was produced.
[0060] <4. Charge / discharge test> Each of the all-solid-state lithium ion batteries of Examples 1 to 3 and Comparative Examples 1 and 2 was initially charged and discharged at 60° C. and 0.05 C to evaluate the initial discharge capacity. Five all-solid-state lithium ion batteries were fabricated for each of Examples 1 to 3 and Comparative Examples 1 and 2, and the charge / discharge test was carried out for each of them. The standard deviation of the initial discharge capacity was divided by the average value of the initial discharge capacity to calculate the coefficient of variation in the initial discharge capacity. The above manufacturing conditions and test results are shown in Table 1.
[0061] [Table 1]
[0062] (Evaluation Results) In all of Examples 1 to 3, the coefficient of variation of the all-solid-state lithium ion battery was good, being 4.5% or less. Therefore, it was possible to efficiently suppress the occurrence of variations in the evaluation of the battery characteristics of the all-solid-state lithium ion battery. As a result, it was possible to accurately evaluate the battery characteristics of the all-solid-state lithium ion battery. In Comparative Examples 1 and 2, the coefficient of variation of the all-solid-state lithium ion batteries was poor, ranging from 6.1% to 7.1%, which resulted in variation in the evaluation of the battery characteristics of the all-solid-state lithium ion batteries, making it impossible to accurately evaluate the battery characteristics of the all-solid-state lithium ion batteries.
[0063] From the above, it was found that the evaluation method for an all-solid-state lithium ion battery according to the present invention can suppress the occurrence of variations in the evaluation of the battery characteristics of an oxide-based all-solid-state battery, and can accurately evaluate the battery characteristics. [Explanation of symbols]
[0064] 10 Powder Compacts 11 Solid electrolyte layer 12 Positive electrode layer 13 plane 14 equilateral triangle 15 Au film 16, 17 MgO setter 20 Powder Compacts 23 plane 24 square
Claims
1. A method for evaluating an all-solid-state lithium ion battery including a solid electrolyte layer including an oxide-based solid electrolyte, a positive electrode layer including a positive electrode active material, and a negative electrode layer, comprising: a sintered body preparation step of pressing the positive electrode composite material containing the positive electrode active material and the solid electrolyte to prepare a plurality of compacts of the solid electrolyte layer / positive electrode layer, and sintering the plurality of compacts in a state where a load is applied to the plurality of compacts to prepare a sintered body; a battery production process in which a laminate produced by providing a negative electrode layer on a surface of the solid electrolyte layer of the fired body is placed in a sealed container and a predetermined confining pressure is applied to produce an all-solid-state lithium ion battery; A battery evaluation step of evaluating battery characteristics of the all-solid-state lithium ion battery; Including, In the sintered body preparation step, the plurality of powder compacts are each formed into a columnar shape, and are provided on a plane at three vertices of an equilateral triangle, spaced apart from one another, and a pressure of 30 to 92 g / cm is applied from above the powder compact. 2 This is a method for evaluating all-solid-state lithium-ion batteries in which the material is sintered under a load.
2. 2. The method for evaluating an all-solid-state lithium ion battery according to claim 1, wherein in the sintered body preparation step, the plurality of compressed powder bodies are provided on a flat surface, one each at a center position of each of three sides of the equilateral triangle, spaced apart from each other.
3. 2. The method for evaluating an all-solid-state lithium ion battery according to claim 1, wherein in the sintered body preparation step, one more of the plurality of compacts is provided on a plane at a center of gravity of the equilateral triangle.
4. The method for evaluating an all-solid-state lithium ion battery according to claim 1 , wherein each of the plurality of powder compacts is formed into a cylindrical shape.
5. The oxide-based solid electrolyte has the composition formula 1: Li α A x M y O 4 (In the composition formula 1, A is Ge, Si or Ti, M is V, P or As, 3.25≦α≦3.75, 0.30≦x≦0.75, and 0.25≦y≦0.70.) It is expressed as The positive electrode active material has the composition formula 2: Li a Ni b Co c Mn d O 2 (In the composition formula 2, 1.00≦a≦1.08, 0.33≦b≦0.90, and b+c+d=1.0.) The method for evaluating the all-solid-state lithium ion battery according to any one of claims 1 to 4, wherein
Citation Information
Patent Citations
Method of dewaxing and burning ceramic formed body
JP1986205673A
Method of manufacturing cathode-solid electrolyte assembly
JP2013243111A