Thermally conductive particle and method for producing the same, mixture, article, resin composition, and thermally conductive thin film

Thermally conductive particles made from a mixture of aluminum, zinc, and additional compounds address the wear and moldability issues of alumina, offering high thermal conductivity and improved resin compatibility.

JP2024139424AActive Publication Date: 2024-10-09DAINICHISEIKA COLOR & CHEMICALS MFG CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023050358
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
2043-03-27

AI Technical Summary

Technical Problem

Alumina-based thermally conductive materials cause mechanical wear on processing equipment due to high hardness, leading to increased viscosity and poor moldability when mixed with resin compositions, while alternative materials like zinc oxide offer low thermal conductivity.

Method used

Thermally conductive particles composed of a mixture of aluminum and zinc raw materials, along with boron, titanium, tungsten, bismuth, and fluorine compounds, are produced by firing and pulverizing, resulting in a low-hardness material with high thermal conductivity, controlled shape, and improved resin compatibility.

Benefits of technology

The particles provide excellent thermal conductivity, chemical resistance, water resistance, and electrical insulation, reducing mechanical wear on processing equipment and enhancing moldability and fillability in resin compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139424000001
    Figure 2024139424000001
  • Figure 2024139424000002
    Figure 2024139424000002
  • Figure 2024139424000003
    Figure 2024139424000003
Patent Text Reader

Abstract

To provide low hardness thermally conductive particles which have low hardness in addition to thermal conductivity and reduces abrasion to a processing device, are excellent in chemical resistance, water resistance and electric insulation property, have good kneading property (filling property) to a resin, and enable manufacture of a material and an article of a resin composition excellent in moldability.SOLUTION: Thermally conductive particles contain at least an aluminum raw material, a zinc raw material, and a baked product obtained by baking other raw material other than the aluminum raw material and the zinc raw material, wherein a content of the zinc raw material with respect to 100 pts.mass of the aluminum raw material is more than 20 pts.mass and 70 pts.mass or less, the other raw material contains at least one selected from the group consisting of a boron compound, a tungsten compound, a titanium compound, a bismuth compound, and a fluorine compound, a content of the other raw material with respect to 100 pts.mass of the aluminum raw material is 0.05 pt.mass or more and 20 pts.mass or less, and the thermally conductive particles satisfy a prescribed condition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to thermally conductive particles having excellent mechanical wear reduction properties and a method for producing the same. [Background technology]

[0002] Currently, many materials are being considered as thermally conductive materials. With the increase in the integration density of semiconductor elements, the demand for heat dissipation is becoming stronger, making it essential to develop materials with much higher thermal conductivity and insulation than before. Composite materials (resin compositions) obtained by kneading thermally conductive fillers into resins are known as materials that meet these demands.

[0003] Alumina is used in many situations as a filler for composite materials because it has excellent water resistance, acid resistance, and insulation, good thermal conductivity, and is inexpensive. However, the alumina powder contained in the thermally conductive composition is a very hard material, which is one of the factors that promotes wear of equipment such as a device that processes the thermally conductive composite material into pellets or sheets. When applying a thermally conductive filler to a processed product, there is a strong demand for a thermally conductive filler that has high thermal conductivity and low wear properties. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-249226 A [Patent Document 2] International Publication No. 2015 / 137468 Summary of the Invention [Problem to be solved by the invention]

[0005] Alumina has a high Mohs hardness, which puts a load on the blade or shaft of the extruder, making it difficult to knead it into resin compositions, etc. Furthermore, worn parts may get mixed in and cause contamination. In addition, when applied to resin, the viscosity may increase, resulting in poor moldability and processability. To solve this problem, thermally conductive materials that have less mechanical wear than alumina and have a lower viscosity when kneaded into resin are being considered. However, although the spherical zinc oxide particles disclosed in Patent Document 1 have a coated surface, the thermal conductivity of zinc oxide itself is low, and therefore improvement is required. Patent Document 2 describes a fired product of an alumina compound and a compound of a metal other than aluminum, but the description concerns a fired product of only a combination of an aluminum raw material and a zinc raw material.

[0006] The present invention has been made in consideration of the problems associated with the conventional technology, and an object of the present invention is to provide low-hardness alumina-based thermally conductive particles (hereinafter sometimes referred to as "thermally conductive particles") that have excellent not only thermal conductivity but also chemical resistance, water resistance, and electrical insulation, and that can be used to produce materials and articles such as resin compositions that have low mechanical wear and excellent filling and moldability, and a method for producing the same. In order to solve the above problems, the present inventors have conducted intensive research and found that a mixture of aluminum raw material, zinc raw material, and other raw materials selected from the group consisting of at least boron compounds, titanium compounds, tungsten compounds, bismuth compounds, and fluorine compounds is fired at a predetermined temperature to react the raw materials with each other to generate a compound, and then pulverized to produce thermally conductive particles that can achieve both low mechanical wear and high thermal conductivity. Furthermore, it has been found that controlling the shape or surface properties of the particles is effective in improving thermal conductivity, resin kneadability, or paint suitability. It has been found that by using these thermally conductive particles, it is possible to impart high thermal conductivity to the matrix and simultaneously suppress wear of equipment such as equipment for processing and molding the thermally conductive composite material. [Means for solving the problem]

[0007] That is, according to the present invention, there are provided the thermally conductive particles and the method for producing the same shown below. [1] Thermally conductive particles containing at least an aluminum raw material, a zinc raw material, and a calcined product obtained by calcining a raw material other than the aluminum raw material and the zinc raw material, The content of the zinc raw material relative to 100 parts by mass of the aluminum raw material is more than 20 parts by mass and not more than 70 parts by mass, the other raw materials contain at least one selected from the group consisting of a boron compound, a tungsten compound, a titanium compound, a bismuth compound, and a fluorine compound, and the content of the other raw materials is 0.05 parts by mass or more and 20 parts by mass or less with respect to 100 parts by mass of the aluminum raw material; Thermally conductive particles that meet the following conditions: (1) 50 g of the above thermally conductive particles and an epoxy equivalent of 200 g / eq or more and 1000 g / eq or less are mixed together using an E-type viscometer at a measurement temperature of 25°C, a cone rotor (3° x R9.7), and a rotation speed of 100 s -1 The resin composition for viscosity measurement obtained by the above method was measured using an E-type viscometer at a measurement temperature of 25°C, a cone rotor (3°×R9.7), and a rotation speed of 100 s. -1 The viscosity when measured under the above conditions is 3,000 mPa s or less. (2) 500 parts by mass of SUS304 steel balls with a diameter of 5 mm and 100 parts by mass of the thermally conductive particles are placed in a 250 mL wide-mouth cylindrical container, and rotated at 80 rpm for 3 hours around the central axis of the cylinder of the cylindrical container as the rotation axis. The steel balls and the thermally conductive particles are then separated using a sieve with 1 mm mesh to obtain thermally conductive particles after the abrasion test. 4 parts by mass of the thermally conductive particles before and after the abrasion test and 8 parts by mass of lithium borate are mixed and ground in a mortar for 5 minutes. The strength of the iron element is measured using an X-ray fluorescence analyzer, and the degree of abrasion calculated using the following formula for the X-ray fluorescence intensity (kcps) of the iron element before and after the abrasion test is 4 kcps or less. Abrasion degree = (fluorescent X-ray intensity of iron element after abrasion test) - (fluorescent X-ray intensity of iron element before abrasion test) (3) A resin composition obtained by kneading 30 parts of a mixture of an epoxy resin having an epoxy equivalent of 200 g / eq or more and 1,000 g / eq or less and an amine-based curing agent having an amine value of 100 mgKOH / g or more and 500 mgKOH / g or less in a ratio of 3:1 to 4:1 with 70 parts of thermally conductive particles is pressed into a mold into a circular sheet molded product with a diameter of 100 mm or more and a thickness of 4 mm or more, heat-cured at a set temperature of 120°C for 1 hour, and then cut into four equal parts so that the test piece is fan-shaped with a central angle of 90° after cooling. When the thermal conductivity is measured by the hot disk thermal property measurement method, the thermal conductivity of the test piece is 0.80 W / m·K or more. [2] The thermally conductive particles according to [1], wherein the other raw materials (excluding fluorine compounds) are at least one selected from the group consisting of oxides, oxoacid salts, hydroxides, carbonates, and basic carbonates. [3] The thermally conductive particles according to [1] or [2], which contain at least one element selected from the group consisting of iron, cobalt, copper, manganese, nickel, and chromium, and are colored. [4] A mixture obtained by mixing the thermally conductive particles according to any one of [1] to [3] with a thermally conductive filler. [5] The mixture described in [4], wherein the thermally conductive filler is at least one selected from the group consisting of barium sulfate, talc, boron nitride, and magnesium oxide. [6] A method for producing thermally conductive particles according to any one of [1] to [3], comprising firing a raw material mixture containing an aluminum raw material, a zinc raw material, and raw materials other than the aluminum raw material and the zinc raw material, the aluminum raw material is at least one selected from the group consisting of boehmite, aluminum hydroxide, and alumina, The method for producing thermally conductive particles, wherein the zinc raw material is at least one selected from the group consisting of zinc oxides and basic carbonates. [7] A method for producing thermally conductive particles, comprising firing the raw material mixture described in [6] at a temperature of 1,000°C or higher and 1,600°C or lower. [8] An article comprising the thermally conductive particles according to any one of [1] to [3]. [9] The article according to [8], which is any one of a gravure ink, a coating liquid, a resin composition, and an adhesive composition.

[10] A resin composition used to form a thermally conductive resin composition, A resin composition comprising the mixture according to [4] or [5] and a molding resin.

[11] The resin composition according to

[10] , wherein the content of the mixture relative to the total amount of the molding resin is 5% by mass or more and 95% by mass or less.

[12] A thermally conductive thin film formed by coating the article according to [9].

[13] The article according to [8], which is used as a heat dissipation member for any one of an electronic device part, an electronic device housing, an EV motor, and a lithium battery. Effect of the Invention

[0008] According to the present invention, it is possible to provide thermally conductive particles that are excellent not only in thermal conductivity but also in chemical resistance, water resistance, and electrical insulation, and that cause little wear on processing equipment, have good kneading properties (filling properties) in resin, and can be used to manufacture materials and articles such as colored resin compositions with excellent moldability by adding a coloring material, and a method for manufacturing the same. Furthermore, according to the present invention, it is possible to provide thermally conductive resin compositions and articles using the thermally conductive particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] <Thermal conductive particles> Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited to the following embodiment. The thermally conductive particles according to this embodiment are obtained by firing a raw material mixture containing an aluminum raw material, a zinc raw material, and other raw materials other than the aluminum raw material and the zinc raw material. The aluminum raw material is at least one selected from the group consisting of alumina, boehmite, and aluminum hydroxide. The zinc raw material is at least one selected from the group consisting of zinc oxide and basic carbonate. The raw material mixture further contains a zinc raw material and other raw materials selected from the group consisting of at least a boron compound, a titanium compound, a tungsten compound, a bismuth compound, and a fluorine compound. The content of the zinc raw material is more than 20 parts by mass and 70 parts by mass or less with respect to 100 parts by mass of the aluminum raw material. The content of the other raw materials is 0.05 parts by mass or more and 20 parts by mass or less with respect to 100 parts by mass of the aluminum raw material as a raw material. Hereinafter, the details of the thermally conductive particles according to this embodiment will be described.

[0010] The thermally conductive particles according to this embodiment are mainly composed of α-alumina and zinc aluminate having a spinel crystal structure. The volume average particle size of the thermally conductive particles is preferably 0.1 μm or more and 50 μm or less. By using a composition containing such thermally conductive particles as a filler, it is possible to impart high thermal conductivity to the composition, and at the same time, since the composition has a lower hardness than that of α-alumina alone, it is possible to suppress wear of equipment such as a device for molding or processing the composition. The average particle size can be measured using a laser diffraction particle size distribution measuring device or a transmission electron microscope photograph.

[0011] The content of the zinc raw material in the raw material mixture must be more than 20 parts by mass and not more than 70 parts by mass, and more preferably 25 parts by mass or more and not more than 65 parts by mass, relative to 100 parts by mass of the aluminum raw material. If the content of the zinc raw material is 20 parts by mass or less, the effect of improving hardness and thermal conductivity cannot be obtained. On the other hand, if the content of the zinc raw material is more than 70 parts by mass, the thermal conductivity is rather reduced. By setting the aluminum raw material and the zinc raw material in the above range, it is possible to obtain thermally conductive particles that are excellent in thermal conductivity, chemical resistance, water resistance, and low abrasion while maintaining various resistances, and have good kneadability (mixability) into resin, and can be used to manufacture materials and articles such as resin compositions with excellent moldability.

[0012] In addition to the zinc raw material, other raw materials other than the aluminum raw material and the zinc raw material are further mixed. These components are used for the purpose of supplementing the zinc component. The oxide raw material is added to solve problems such as when it is difficult to gelatinize the sintered ...

[0013] The content of the other raw materials in the raw material mixture is 0.05 parts by mass or more and 20 parts by mass or less, more preferably 0.1 parts by mass or more and 10 parts by mass or less, even more preferably 0.1 parts by mass or more and 8 parts by mass or less, and particularly preferably 0.5 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the aluminum raw material as the raw material. If the amount of the other raw materials relative to 100 parts by mass of the aluminum raw material as the raw material is less than 0.05 parts by mass, the particle size distribution is wide and the filling property is reduced. On the other hand, if the amount of the other raw materials relative to 100 parts by mass of the aluminum raw material as the raw material exceeds 20 parts by mass, the thermal conductivity is reduced rather. By setting the amount of the other raw materials relative to 100 parts by mass of the aluminum raw material as the raw material within the above range, the thermal conductive particles have excellent thermal conductivity, chemical resistance, water resistance, and electrical insulation, and can be used to manufacture materials or articles such as resin compositions that are low in wear and have excellent moldability.

[0014] The viscosity of the thermally conductive particles according to this embodiment when added to a resin was measured using the value when 50 parts by mass was added to 50 parts by mass of epoxy resin. The sample used for viscosity measurement was prepared by kneading for 1 minute at 1,000 rpm and degassing for 1 minute at 2,000 rpm using a planetary centrifugal mixer. The resin composition for viscosity measurement obtained by the above method was measured using an E-type viscometer at a measurement temperature of 25°C, a cone rotor (3°×R9.7), and a rotation speed of 100 s -1 The viscosity of the epoxy resin composition was measured under the following conditions. The viscosity of the epoxy resin composition must be 3,000 mPa·s or less, and is preferably 2,500 mPa·s or less. If the viscosity exceeds 3,000 mPa·s, the processability is poor. There is no particular lower limit, but if the viscosity is less than 10 mPa·s, it may be difficult to form a coating film. This makes it possible to produce a thermally conductive resin composition with excellent resin moldability or processability.

[0015] Regarding the wearability of the thermally conductive particles according to this embodiment, 500 parts by mass of SUS304 steel balls with a diameter of 5 mm and 100 parts by mass of the thermally conductive particles were placed in a cylindrical container of a wide-mouthed bottle of 250 mL, and the container was rotated at 80 rpm for 3 hours with the central axis of the cylinder as the rotation axis, and then the steel balls and the thermally conductive particles were separated using a sieve with a mesh size of 1 mm to obtain thermally conductive particles after the wear test. Each sample was prepared by mixing 4 parts by mass of the thermally conductive particles before and after the wear test with 8 parts by mass of lithium borate and pulverizing them in a mortar for 5 minutes, and the strength of the iron element was measured using a fluorescent X-ray analyzer. The fluorescent X-ray strength (kcps) of the iron element before and after the wear test was calculated using the following formula, and the wearability was evaluated according to the degree of wear of the steel balls. Abrasion degree = (fluorescent X-ray intensity of iron element after abrasion test) - (fluorescent X-ray intensity of iron element before abrasion test) The degree of abrasion must be 4 kcps or less. If the degree of abrasion exceeds 4 kcps, the thermally conductive particles are too hard and will wear down the devices when they are molded and processed into a resin composition, which is undesirable.

[0016] The thermal conductivity of the thermally conductive particles according to this embodiment was measured by adding 70 parts by mass to 30 parts by mass of a mixture of epoxy resin and amine-based curing agent. The sample used for the thermal conductivity measurement was pressed into a mold to form a circular sheet molded product with a diameter of 100 mm or more and a thickness of 4 mm or more, heated and cured at a set temperature of 120°C for 1 hour, and cut into four equal parts to form a fan shape with a central angle of 90° after cooling. The thermal conductivity was measured by hot disk method thermal property measurement, and the thermal conductivity of the epoxy resin composition at that time must be 0.80 W / m·K or more, and more preferably 0.90 W / m·K or more. If the thermal conductivity is less than 0.80 W / m·K, the thermal conductivity performance is insufficient. As a result, when used in electronic components, the thermal conductivity becomes high and the desired heat dissipation performance can be achieved.

[0017] The epoxy resin used for measuring thermal conductivity and viscosity must have an epoxy equivalent of 200 g / eq or more and 1000 g / eq or less, more preferably 300 g / eq or more and 800 g / eq or less, and even more preferably 350 g / eq or more and 700 g / eq or less. If the epoxy equivalent is less than 200 g / eq, the flexibility when cured is poor, and air bubbles cannot be removed, and molding becomes difficult, making various measurements difficult. On the other hand, if it exceeds 1000 g / eq, the viscosity decreases and the flexibility becomes too high, and the particles settle, making it difficult to prepare a uniform sample, and making various measurements difficult. In addition, the E-type viscometer was used at a measurement temperature of 25°C, a cone rotor (3° x R9.7), and a rotation speed of 100 s -1 The viscosity of the epoxy resin measured under the above conditions must be between 400mPa·s and 900mPa·s. When 50g of thermally conductive particles and 50g of epoxy resin are mixed, the viscosity is 3,000mPa·s or less, which is preferable as a viscosity with good moldability. If the viscosity of this epoxy is less than 400mPa·s, sedimentation occurs and measurement becomes difficult. If the viscosity of this epoxy is more than 900mPa·s, workability decreases, such as moldability deteriorates, and measurement becomes difficult, which is also undesirable.

[0018] The amine-based curing agent used in the thermal conductivity measurement must have an amine value of 100 mgKOH / g to 500 mgKOH / g, and more preferably 150 mgKOH / g to 450 mgKOH / g. If the amine value is less than 100 mgKOH / g, the viscosity is high, making it difficult to mix uniformly and difficult to handle, which is undesirable. If the amine value is more than 500 mgKOH / g, the resin after curing becomes too hard, making various measurements difficult, which is undesirable. The ratio of epoxy resin to amine-based hardener in the mixed solution is in the range of 3:1 to 4:1. If the mixing ratio is outside the above range, it is not preferable because the epoxy resin does not cure sufficiently. As the amine-based hardener, any common one can be used as long as it cures the epoxy resin. Examples of the amine-based hardener include amine, aliphatic amine, aromatic amine, and modified amine.

[0019] The thermally conductive particles according to the present embodiment have excellent thermal conductivity, low wear on processing equipment, and excellent chemical resistance, water resistance, and electrical insulation. Moreover, they have high wettability to resin and good kneadability (filling ability) into resin, so that they can be used to manufacture materials such as resin compositions with excellent moldability, and articles such as paints and adhesive compositions.

[0020] The thermally conductive particles according to this embodiment are obtained by firing a raw material mixture containing an aluminum raw material, a zinc raw material, and other raw materials, and are preferably composed mainly of α-alumina and zinc aluminate with a spinel crystal structure.

[0021] (Aluminum raw material) The aluminum raw material may be alumina, boehmite, aluminum hydroxide, or the like. The shape and particle size of the aluminum raw material are not particularly limited, but considering the dispersibility of the thermally conductive particles, it is preferable that the aluminum raw material be particles having an average particle size of 0.1 μm or more and 50 μm or less. More specific examples of the shape of the aluminum raw material include spherical and amorphous shapes.

[0022] (raw material mixture) The raw material mixture used together with the aluminum raw material contains, in addition to the zinc raw material, other raw materials. The other raw materials are at least one selected from the group consisting of boron compounds, titanium compounds, tungsten compounds, bismuth compounds, and fluorine compounds. These improve the dispersibility of thermally conductive particles, promote the gelatinization of alumina, or adjust the particle size distribution.

[0023] (Zinc raw material) As the zinc source, basic zinc carbonate, zinc hydroxide, zinc oxide, etc. can be used. The shape and particle size of the raw material are not particularly limited, but in consideration of the dispersibility of the thermally conductive particles, it is preferable that the particles have an average particle size of 0.1 μm or more and 50 μm or less.

[0024] (Other ingredients) Examples of other raw materials include boron compounds such as boric acid, sodium borate, ammonium borate, magnesium borate, and lithium borate. Examples of titanium compounds include rutile or anatase titanium oxide. Examples of tungsten compounds include tungsten oxide, ammonium tungstate, and sodium tungstate. Examples of bismuth compounds include bismuth oxide, basic bismuth carbonate, and sodium bismuthate. Examples of fluorine compounds include lithium fluoride, sodium fluoride, potassium fluoride, and aluminum fluoride. Among these, boric acid, sodium tungstate, titanium oxide, basic bismuth carbonate, sodium fluoride, or aluminum fluoride is preferred because it forms thermally conductive particles with a high filling rate. Moreover, the other raw materials (excluding the fluorine compound) are preferably at least one selected from the group consisting of oxides, oxoacid salts, hydroxides, carbonates, and basic carbonates.

[0025] (Coloring material) Furthermore, the thermally conductive particles according to this embodiment can be colored by containing at least one element selected from the group consisting of iron, cobalt, copper, manganese, and nickel, without the addition of a pigment or dye.

[0026] (Surface treatment) The thermally conductive particles according to the present embodiment may be surface-treated. The surface-treated thermally conductive particles have improved affinity and dispersibility with respect to resin, and therefore can be used to manufacture articles such as resin compositions with excellent thermal conductivity. Examples of compounds (treatment agents) used for the surface treatment include fatty acids, fatty acid esters, fatty acid metal salts, phosphate esters, phosphate ester metal salts, silane coupling agents, surfactants, polymer flocculants, titanates, and silicones. These treatment agents can be used alone or in combination of two or more. The amount of the compound used for the surface treatment is preferably 0.01 parts by mass or more and 5 parts by mass or less with respect to 100 parts by mass of the thermally conductive particles. Examples of the treatment method include a method in which a treatment agent is added to a powder of thermally conductive particles and mixed to perform treatment, or a method in which a powder of thermally conductive particles is added to water to disperse the powder, and then a treatment agent is added, followed by filtration and drying.

[0027] (Use of thermally conductive particles) Among the preferable uses of the thermally conductive particles according to this embodiment, it is effective to add them to various plastics such as thermoplastic resins or thermosetting resins for the purpose of imparting thermal conductivity. Examples of the thermoplastic resin include polyethylene resin, polypropylene resin, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, acrylonitrile-ethylene-styrene copolymer, acrylonitrile-butadiene-styrene copolymer, acrylonitrile-styrene copolymer, polyvinyl chloride resin, polystyrene resin, polyacrylonitrile resin, polyamide resin, thermoplastic polyimide resin, thermoplastic urethane resin, polyaminobismaleimide resin, polyamideimide resin, polyetherimide resin, polymethylmethacrylate resin, polyvinyl acetate resin, polycarbonate resin, polyacetal resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polyphenylene oxide resin, polyphenylene sulfide resin, polysulfone resin, polyethersulfone resin, polyetheretherketone resin, polyarylsulfone resin, bismaleimide triazine resin, polymethylpentene resin, fluorinated resin, liquid crystal polymer, olefin-vinyl alcohol copolymer, ionomer resin, and polyarylate resin. These thermoplastic resins can be used alone or in combination of two or more. Examples of the thermosetting resin that can be used include phenol resin, urea resin, epoxy resin, melamine resin, silicone resin, polyurethane resin, unsaturated polyester resin, alkyd resin, polyimide resin, acrylic resin, and (modified) polyphenylene ether, etc. These thermosetting resins can be used alone or in combination of two or more.

[0028] <Method of manufacturing thermally conductive particles> Next, a method for producing thermally conductive particles according to the present embodiment will be described. The method for producing thermally conductive particles according to the present embodiment includes a step (step (1)) of mixing an aluminum raw material, a zinc raw material, and raw materials other than the aluminum raw material and the zinc raw material to obtain a raw material mixture, and a step (step (2)) of firing the obtained raw material mixture. According to this manufacturing method, particles having low hardness, low mechanical wear, and high thermal conductivity compared to conventional alumina can be easily obtained. The reason for this is not necessarily clear, but the present inventors speculate that it is as follows. That is, the thermally conductive particles contain at least α-alumina and spinel crystal structure zinc aluminate. In addition, the mixed crystals constituting the filler composition made of this particle material have a large number of α-alumina fine particles between spinel crystal structure zinc aluminate particles, which increases the contact area between the particles and reduces the interparticle thermal resistance (interface thermal resistance). Therefore, it shows higher thermal conductivity than pure spinel crystal structure zinc aluminate. On the other hand, although spinel crystal structure zinc aluminate particles have inferior thermal conductivity to α-alumina, they have excellent mechanical wear properties, so the manufactured thermally conductive particles have lower mechanical wear than alumina. The ratio of α-alumina to zinc aluminate with a spinel crystal structure in the thermally conductive particles (α-alumina: zinc aluminate with a spinel crystal structure) is preferably in the range of 8:2 to 1:9, and more preferably in the range of 6:4 to 4:6. In particular, when the ratio is 5:5, the balance between thermal conductivity and hardness is good.

[0029] In step (1), the aluminum raw material, zinc raw material, and other raw materials are mixed. The aluminum raw material, zinc raw material, and other raw materials are mixed using equipment such as a pot mill, Henschel mixer, air mix, conical blender, planetary ball mill, vibration mill, ribbon mixer, and vertical blender, and then the components are mixed and fired. When mixing the components, they should be mixed uniformly. The amount of each component in the raw material mixture is as described above.

[0030] In step (2), the raw material mixture obtained in step (1) is fired at 1,000° C. or more and 1,600° C. or less, and preferably at 1,200° C. or more and 1,500° C. or less. By firing, the aluminum raw material and the zinc raw material can be crystallized to produce α-alumina and zinc aluminate with a spinel crystal structure. If the firing temperature is less than 1,000°C, the crystalline structure of α-alumina and zinc aluminate with spinel crystal structure is difficult to form. In that case, the durability is reduced because the unreacted zinc raw material remains. In addition, since the thermal conductivity of transition alumina formed at low temperatures is lower than that of α-alumina, it is preferable to form α-alumina and zinc aluminate with spinel crystal structure by firing. On the other hand, even if the firing temperature exceeds 1,600°C, the properties of the obtained thermally conductive particles do not change significantly, and energy consumption is wasted. A method for confirming the presence of α-alumina and zinc aluminate with spinel crystal structure in the thermally conductive particles is a method of comparing the peaks obtained by powder X-ray diffraction measurement of standard substances of α-alumina and zinc aluminate with the peaks obtained by powder X-ray diffraction measurement of the produced thermally conductive particles. When α-alumina and zinc aluminate with spinel crystal structure are contained, the peaks are added together, and quantification can be performed by comparing the respective peak intensities. After the firing, the fired product can be crushed as necessary to obtain the thermally conductive particles according to the present embodiment. For crushing, a known method may be used, and various conventionally used machines such as a hammer mill, a roll mill, a ball mill, a jet mill, a bead mill, or a vibration mill may be used.

[0031] <Thermal conductive composition (mixture)> In the thermally conductive composition (mixture), in addition to the thermally conductive particles according to the present embodiment, it is also preferable to use other thermally conductive fillers such as alumina, boron nitride, graphite, zinc oxide, barium sulfate, talc, and magnesium oxide in combination. The details will be described below.

[0032] General fillers are added to materials such as resins, rubbers, and paints for the purpose of improving strength or functionality. When the amount of thermally conductive filler is increased, the melt flowability and mechanical strength of materials such as resins usually decrease. In addition, since carbon-based fillers have electrical conductivity, there is a problem that the insulating property, which is an inherent characteristic of resins, is easily impaired when they are added to resins. Furthermore, ceramic-based fillers have insulating properties, but have problems such as low thermal conductivity. Thermally conductive fillers include, for example, metal-based fillers such as silver, copper, aluminum, and iron; inorganic-based fillers such as alumina, magnesia, silica, boron nitride, aluminum nitride, silicon carbide, boron carbide, and titanium carbide; and carbon-based fillers such as diamond, graphite, and graphite. In electronic devices and the like that require high electrical insulation, fillers such as alumina, magnesium oxide, zinc oxide, silica, boron nitride, aluminum nitride, and diamond are considered to be preferable. However, these fillers have many issues in terms of water resistance, chemical resistance, hardness, and electrical insulation.

[0033] In contrast, the thermally conductive particles according to this embodiment have the above-mentioned various fillers' weaknesses improved and have excellent properties, so that they can be suitably used as an improved filler. Furthermore, it is also preferable to use them together with the above-mentioned various thermally conductive fillers to compensate for the weaknesses of existing thermally conductive fillers. That is, in the thermally conductive composition containing the above-mentioned various thermally conductive fillers, the use of the thermally conductive particles according to this embodiment is a preferred embodiment that is prepared according to the desired properties. The amount of the thermally conductive filler added is preferably 10 parts by mass or more and 150 parts by mass or less with respect to 100 parts by mass of the thermally conductive particles. If the amount of the thermally conductive filler added is less than 10 parts by mass, the effect of the thermally conductive filler may be difficult to obtain. If the amount of the thermally conductive filler added is more than 150 parts by mass, the effect of the thermally conductive particles may be difficult to obtain.

[0034] <Goods> The article according to the present embodiment is an article (thermally conductive article, thermally conductive material) containing the above-mentioned thermally conductive particles, such as a gravure ink, a coating liquid, a resin composition, and an adhesive composition. Note that the article according to the present embodiment preferably further contains the above-mentioned various thermally conductive fillers as necessary.

[0035] (gravure ink) The thermally conductive particles according to this embodiment can be added to gravure ink used as a topcoat agent for battery packaging materials. The content of the thermally conductive particles in the gravure ink is preferably 5% by mass or more and 80% by mass or less, more preferably 10% by mass or more and 50% by mass or less, based on the total amount of the gravure ink. By using such a gravure ink (topcoat agent for battery packaging materials), a battery packaging material having excellent chemical resistance such as acid resistance, high thermal conductivity, and high thermal emissivity can be produced.

[0036] (Coating fluid) The thermally conductive particles according to this embodiment can be used by adding them to a coating liquid such as a paint. The coating liquid can also be a coloring preparation obtained by mixing and dispersing, for example, a colorant, a resin for forming a coating or molded product, and an organic solvent in a vehicle together with the thermally conductive particles. The content of the thermally conductive particles in the coating liquid is preferably 5% by mass or more and 80% by mass or less, more preferably 10% by mass or more and 70% by mass or less, based on the total amount of the coating liquid. The coating film or coated molded product formed using the coating liquid thus prepared has excellent water resistance, chemical resistance, and insulation, retains strength, and is also excellent in thermal conductivity.

[0037] Specific examples of resins that can be contained in the coating liquid include thermoplastic resins such as polyolefins, polyesters, polystyrenes, acrylics, fluorine-based, polyamides, celluloses, polycarbonates, and polylactic acid; and thermosetting resins such as urethanes, phenols, and silicones. These resins may be in the form of emulsions.

[0038] Specific examples of the liquid medium that can be contained in the coating liquid include water, methanol, ethanol, butanol, acetone, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, butyl acetate, cyclohexane, etc. These liquid media may be used in combination of two or more kinds.

[0039] The coating liquid may contain "other components" selected appropriately according to the application, within the scope of not impairing the object of the present invention. Specific examples of "other components" include antioxidants, ultraviolet absorbers, light stabilizers, dispersants, antistatic agents, lubricants, and bactericides.

[0040] A conventionally known method can be used as a method for applying the coating liquid. Specifically, spray coating, brush coating, electrostatic coating, curtain coating, a method using a roll coater, or a method by immersion can be mentioned. Also, a conventionally known method can be used as a drying method for turning the applied coating liquid into a coating film. Specifically, a method such as natural drying or baking can be appropriately selected and used depending on the properties of the coating liquid.

[0041] By using the coating liquid, a coating film or a coating molded product can be produced by coating a substrate. The substrate can be selected from metal, glass, natural resin, synthetic resin, ceramics, wood, paper, fiber, nonwoven fabric, woven fabric, leather, etc., depending on the application. The coating film thus provided with functionality can be used in various industries such as industry, agriculture, mining, and fishing, in addition to household use. There is also no limitation on the coating shape, and it can be selected from sheet or film shapes depending on the application.

[0042] (Resin composition) The thermally conductive particles according to the present embodiment can be blended with a resin such as a polyamide resin or a polyolefin resin to obtain a resin composition. More specifically, the thermally conductive particles can be blended and mixed with the resin, if necessary, together with other additives, in accordance with a known method to obtain a resin composition. Furthermore, the obtained resin composition can be molded by being fed to an extrusion molding machine to produce a predetermined resin molded product. The content of the thermally conductive particles in the resin composition is preferably 5% by mass or more and 95% by mass or less with respect to the entire resin composition. By setting the content of the thermally conductive particles within the above range, a resin composition can be obtained that is more excellent in water resistance, chemical resistance, and insulation, further retains strength, and has better moldability. If the content of the thermally conductive particles is more than 95% by mass, the strength and moldability may decrease. On the other hand, if the content of the thermally conductive particles is less than 5% by mass, the thermal conductivity may be insufficient.

[0043] The method of adding the thermally conductive particles to the resin is not particularly limited, and a conventionally known method can be adopted. For example, in addition to a method of directly blending the thermally conductive particles with the resin and kneading and molding, there is a method of using a composition (master batch) in which the thermally conductive particles are previously dispersed in a resin, a lubricant, or the like at a high concentration. Other additives include antioxidants, ultraviolet absorbers, antistatic agents, antibacterial agents, stabilizers, crosslinking agents, plasticizers, lubricants, mold release agents, flame retardants, and inorganic fillers such as talc, alumina, clay, and silica. In addition, metal soaps and polyethylene waxes can be used as dispersion aids for the thermally conductive particles. Examples of metal soaps include lithium stearate, magnesium stearate, zinc stearate, calcium stearate, magnesium palmitate, calcium oleate, and cobalt oleate. Examples of the polyethylene wax include various polyethylene waxes such as general polymerization type, decomposition type, and modified type.

[0044] In addition, various organic pigments and inorganic pigments can also be blended as colorants in the above-mentioned coating liquid and resin composition. Examples of colorants include organic pigments such as phthalocyanine pigments, azo pigments, azomethine pigments, isoindolinone pigments, quinacridone pigments, anthraquinone pigments, dioxazine pigments, and perinone-perylene pigments; composite oxide pigments other than black; titanium oxide pigments such as titanium oxide white pigments, titanium oxide yellow pigments, and titanium oxide black pigments; and inorganic pigments such as carbon black, ultramarine, and red iron oxide. Examples of phthalocyanine pigments include brominated phthalocyanine blue pigments and phthalocyanine green pigments. Examples of azo pigments include polycondensed azo pigments and azomethine azo pigments.

[0045] Furthermore, a resin composition can also be obtained by melt-kneading a master batch compound in which thermally conductive particles, various pigments, and additives are blended with a resin for compounding using an extrusion molding machine or the like. More specifically, (i) a method in which thermally conductive particles and a dispersing aid are blended with a resin for compounding, and other additives are added as necessary, and mixed using a mixer such as a Henschel mixer; (ii) a method in which the master batch compound is kneaded using a kneader or a heated two-roll mill, cooled, and then pulverized with a pulverizer to form a coarse powder; or (iii) a method in which the master batch compound is fed to an extrusion molding machine and extruded to form into a bead-like or column-like shape, etc., to obtain a resin composition. The molding method is not particularly limited, and for example, an injection molding method, an extrusion molding method, a heat compression molding method, a blow molding method, an inflation molding method, or a vacuum molding method may be adopted.

[0046] (Adhesive Composition) The thermally conductive particles according to the present embodiment can be added to an adhesive to be used as an adhesive composition. The type of resin contained in the adhesive is not limited, and may be a resin having adhesive properties such as a urethane-based, epoxy-based, vinyl acetate-based, or acrylic-based resin. The adhesive mechanism is also not limited, and may be any of a chemical reaction type, a solvent volatilization type, a thermal melting type, and a thermal pressure type. The content of the thermally conductive particles in the adhesive composition is preferably 5% by mass or more and 80% by mass or less, and more preferably 10% by mass or more and 50% by mass or less, based on the entire adhesive composition. By setting the content of the thermally conductive particles within the above range, an adhesive composition having superior thermal conductivity, adhesiveness, water resistance, chemical resistance, and insulation properties can be obtained. If the content of the thermally conductive particles is more than 80% by mass, the adhesive strength may be insufficient. On the other hand, if the content of the thermally conductive particles is less than 5% by mass, the thermal conductivity may be insufficient.

[0047] The thermally conductive particles according to this embodiment can be used as thermally conductive articles or materials such as the gravure ink, coating liquid, resin composition, and adhesive composition described above, and can be used as electronic devices having excellent chemical resistance, water resistance, and insulation properties as well as heat dissipation (thermal conductivity). More specifically, they can be used in metal circuit boards, circuit boards, metal laminates, metal-clad laminates with inner layer circuits, battery packaging materials, sealants, protective sheets, etc. Furthermore, they can be used as adhesive sheets, heat dissipation sheets, heat dissipation coating agents, semiconductor sealants, adhesives, heat dissipation spacers, greases, etc.

[0048] <Liquid composition (resin composition)> The liquid composition (resin composition) according to the present embodiment is a liquid composition used for forming a thermally conductive thin film, and contains a thermally conductive component (mixture) containing the above-mentioned thermally conductive particles, a forming resin, and a liquid medium as an optional component. It is preferable that the thermally conductive component further contains at least one selected from the group consisting of barium sulfate, talc, boron nitride, and magnesium oxide. The content of the thermally conductive particles in the liquid composition is preferably 5% by mass or more and 80% by mass or less, more preferably 10% by mass or more and 70% by mass or less, based on the entire liquid composition. The content of the thermally conductive component (mixture) relative to 100 parts by mass of the forming resin is preferably 20 parts by mass or more and 600 parts by mass or less, more preferably 20 parts by mass or more and 200 parts by mass or less. The thermally conductive thin film formed using the liquid composition prepared in this manner has excellent water resistance, chemical resistance, and insulation, retains strength, and is also excellent in thermal conductivity.

[0049] The forming resin is at least one solvent-soluble resin selected from the group consisting of acrylic resins, urethane resins, urea resins, epoxy resins, rubber resins, fluorine resins, polyamide resins, polyimide resins, silicone resins, cellulose resins, and thermoplastic elastomers. The liquid medium is the same as the liquid medium used in the coating liquid described above.

[0050] <Thermal conductive thin films and electronic device components> The thermally conductive thin film according to this embodiment is a thin film formed by applying the above-mentioned article or the above-mentioned liquid composition (resin composition). The thickness of the thermally conductive thin film is preferably 20 μm or more and 1000 μm or less, and more preferably 50 μm or more and 200 μm or less. The thermally conductive thin film according to this embodiment can also be used as an electronic device member. This electronic device member is a member including a metal member and the thermally conductive thin film described above disposed on the surface of the metal member. Examples of the metal member include a metal circuit board, a circuit board, a metal laminate, and a metal-clad laminate with an inner layer circuit.

[0051] The resin composition according to the present embodiment can be used for housings for electronic devices, motors (e.g., EV motors), lithium batteries, etc., to efficiently release internal heat to the outside and to reduce weight compared to conventional metal housings. The article according to the present embodiment can also be used for electronic device parts as a heat dissipation member. EXAMPLES

[0052] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples and comparative examples, "parts" and "%" are by mass unless otherwise specified.

[0053] <Aluminum raw materials> The following aluminum raw materials were used: A-1: Aluminum hydroxide (spherical, average particle size 6 μm) A-2: Aluminum hydroxide (spherical, average particle size 1 μm) A-3: Boehmite (spherical, average particle size 1 μm) A-4: Spherical alumina (spherical, average particle size 3μm) ·A-5: γ-Alumina (irregular shape, average particle size 0.1μm)

[0054] <Zinc raw material> The following zinc raw materials were used: B-1: Basic zinc carbonate (average particle size 10 μm) B-2: Zinc oxide (average particle size 1 μm) B-3: Zinc aluminate (average particle size 10 μm)

[0055] <Other ingredients> The following raw materials were used: C-1: Boric acid C-2: Sodium tungstate dihydrate C-3: Titanium oxide C-4: Basic bismuth carbonate C-5: Sodium fluoride C-6: Aluminum fluoride

[0056] <Thermal conductive filler> The following fillers were used: D-1: Barium sulfate (average particle size 0.9 μm) D-2: Talc (average particle size 4.3 μm) D-3: Boron nitride (average particle size 20 μm) D-4: Magnesium oxide (average particle size 20 μm)

[0057] <Production of Thermally Conductive Particles> Example 1 100 parts of aluminum hydroxide (A-1), 27.3 parts of basic zinc carbonate (B-1), 0.5 parts of boric acid (C-1), and 0.5 parts of sodium tungstate dihydrate (C-2) were put into a small mixer and stirred to obtain a raw material mixture. The obtained raw material mixture was fired in air at 1,250°C for 3 hours and then crushed to obtain powdered thermally conductive particles. Powder X-ray diffraction measurements confirmed the presence of α-alumina and zinc aluminate with a spinel crystal structure.

[0058] (Examples 2 to 22) Powdered thermally conductive particles were obtained in the same manner as in Example 1, except that the types and amounts of raw materials shown in Table 1 were used. For the thermally conductive fillers in Examples 18 to 22, the amounts shown in the table were added to 100 parts by mass of the fired thermally conductive particles, and then the mixture was stirred and mixed in a small mixer. The presence of α-alumina and zinc aluminate with a spinel crystal structure was confirmed by powder X-ray diffraction measurement.

[0059] (Comparative Examples 1 to 11 and 14) Powdered thermally conductive particles were obtained in the same manner as in Example 1, except that the types and amounts of raw materials shown in Table 1 were used. For the thermally conductive filler of Comparative Example 11, the amount shown in the table was added to 100 parts by mass of the fired thermally conductive particles, and then the mixture was stirred and mixed in a small mixer. The presence of α-alumina and zinc aluminate with a spinel crystal structure was confirmed by powder X-ray diffraction measurement.

[0060] (Comparative Examples 12, 13, and 15 to 17) The raw materials shown in Table 1 were used as the samples of Comparative Examples 12, 13, and 15 to 17, respectively.

[0061] (Comparative Example 18) Powdered thermally conductive particles were obtained in the same manner as in Example 1, except that the types and amounts of raw materials shown in Table 1 were used and the firing temperature was set to 900° C. Powder X-ray diffraction measurement was performed, but the presence of α-alumina could not be confirmed.

[0062] [Table 1]

[0063] (Measurement of thermal conductivity) A resin composition was obtained by kneading 30 parts of a mixture of epoxy resin (Mitsubishi Chemical, grade 871, epoxy equivalent 390-470g / eq, viscosity 400-900mPa·s) and amine-based hardener (ADEKA, EH-6024, amine value 370mgKOH / g) in a ratio of 3.5:1 with 70 parts of the obtained thermally conductive particles, and pressing it into a circular sheet molded product with a diameter of 100mm or more and a thickness of 4mm. The product was then heat-cured at a set temperature of 120°C for 1 hour, cooled, and then cut into four equal parts so as to form a sector shape with a central angle of 90° to prepare test pieces. The thermal conductivity of the prepared test pieces was measured using a hot disk method thermal property measuring device (product name "TPS-2500S", Kyoto Electronics Manufacturing Co., Ltd.). The results are shown in Table 2.

[0064] (Viscosity measurement) 50 g of the obtained thermally conductive particles were added to 50 g of epoxy resin (manufactured by Mitsubishi Chemical Corporation, grade 871, epoxy equivalent 390-470 g / eq, viscosity 400-900 mPa s) and mixed by hand. The mixed resin composition was kneaded by a planetary centrifugal mixer (kneading: 1000 rpm, 1 minute, degassing: 2000 rpm, 1 minute). The resin composition for viscosity measurement obtained by the above method was measured by an E-type viscometer (product name "TV-100EH / 200", manufactured by Toki Sangyo Co., Ltd.) at a measurement temperature of 25°C, a cone rotor (3°×R9.7), and a rotation speed of 100 s -1 The viscosity was measured at 100°C and evaluated according to the following criteria. The results are shown in Table 2. ○:3000mPa・s or less ×: More than 3000mPa·s

[0065] (Wear test) Approximately 500g of SUS304 steel balls (product name "1-9762-02", manufactured by Misumi Corporation) with a diameter of 5mm and approximately 100g of the obtained thermally conductive particles were placed in a cylindrical container of 250mL i-boy wide-mouth bottle (diameter 62mm, length 132mm, manufactured by AS ONE Corporation), and the container was rotated at 80 rpm for 3 hours with the central axis of the cylinder as the rotation axis, and the steel balls and the thermally conductive particles were separated using a sieve with a mesh size of 1mm to obtain thermally conductive particles after the abrasion test. The degree of abrasion was measured by mixing 4g of the thermally conductive particles after the abrasion test with 8g of lithium borate and pulverizing them in a mortar for 5 minutes. Similarly, the thermally conductive particles before the abrasion test were mixed and pulverized in a mortar, and the strength of the iron element was measured using a fluorescent X-ray analyzer (product name "ZSX PrimusII", manufactured by Rigaku Corporation). The difference in the fluorescent X-ray intensity (kcps) of the iron element before and after the abrasion test was calculated using the following formula. The results are shown in Table 2. Abrasion degree = (fluorescent X-ray intensity of iron element after abrasion test) - (fluorescent X-ray intensity of iron element before abrasion test) ○: Wear rate is 4kcps or less △: Wear level is over 4kcps and below 8kcps ×: Wear level exceeds 8 kcps

[0066] (acid resistance) The resin molded body for evaluation, which was made of the resin composition containing 70 parts by mass of the thermally conductive particles prepared above, was cut into a size of 20 mm x 20 mm x 60 mm, and the molded body obtained was immersed in a hydrochloric acid solution of pH 2.0 heated to 50°C for 3 hours. The withstand voltage was measured before and after immersion, and the acid resistance was evaluated according to the following criteria using the obtained measured values. The results are shown in Table 2. <Criteria for determining acid resistance> ○: The decrease in withstand voltage after immersion from the initial value before immersion is less than 10% △: The decrease in withstand voltage after immersion from the initial value before immersion is 10% or more but less than 50%. ×: The withstand voltage after immersion drops by 50% or more from the initial value before immersion

[0067] (water resistance) Five parts of the thermally conductive particles were immersed in 100 parts of pure water, placed in a container and boiled at 100°C for 5 minutes, then filtered, and the filtrate was used as a measurement sample. The measurement sample prepared as above was used to measure the electrical conductivity with an electrical conductivity meter, and was judged and evaluated according to the following criteria. The results are shown in Table 2. <Water resistance criteria> ○: The increase in electrical conductivity after immersion from the initial value before immersion is less than 300 μS / cm △: The increase in electrical conductivity after immersion from the initial value before immersion is 300 μS / cm or more and less than 1000 μS / cm. ×: The increase in electrical conductivity after immersion from the initial value before immersion is 1000 μS / cm or more

[0068] [Table 2]

[0069] Reference Example 1 When measuring the thermal conductivity, a test piece was prepared using 70 parts of the thermally conductive particles obtained in Example 1 for 70 parts of the thermally conductive particles. As a method for testing the thermal conductivity, a resin composition obtained by mixing 30 parts of polypropylene (manufactured by Prime Polymer Co., Ltd., MFR: 20 g / 10 min) and 70 parts of the thermally conductive particles was placed in a plastomill and melt-kneaded at a set temperature of 200°C. Then, a test piece was prepared by mold press molding at 175°C using a mold with a length of 20 mm, width of 20 mm, and height of 6 mm. The thermal conductivity of the prepared test piece was measured using a thermal property measuring device (product name "TPS-2500S", manufactured by Kyoto Electronics Manufacturing Co., Ltd.). The thermal conductivity at this time was 1.18 W / m·K.

[0070] (Reference Example 2) A test piece was prepared in the same manner as in Reference Example 1, except that 60 parts of the thermally conductive particles obtained in Example 1 and 10 parts of the thermally conductive rounded discoid particles described in Example 3 of Japanese Patent No. 7185798 were used to prepare the test piece. The thermal conductivity in this case was 1.19 W / m K, and even when particles of different shapes were mixed, the result was within the range of the examples, almost the same as when only thermally conductive particles were used.

[0071] (Reference Comparative Example 1) A test piece was prepared in the same manner as in Reference Example 1, except that 70 parts of the thermally conductive particles obtained in Comparative Example 7 were used to prepare the test piece. The thermal conductivity at this time was 0.92 W / m K.

[0072] (Reference Comparative Example 2) A test piece was prepared in the same manner as in Reference Example 1, except that 70 parts of the thermally conductive particles obtained in Comparative Example 14 were used to prepare the test piece. The thermal conductivity at this time was 1.07 W / m K.

[0073] <Preparation and evaluation of adhesive> (Application Example 1 and Comparative Application Example 1) 35 parts of the thermally conductive particles obtained in Example 1 and Comparative Example 13 were mixed with 65 parts of polyester polyol with a viscosity of 300 mPa·s, and dispersed using a disperser to prepare a dispersion. 98 parts of the prepared dispersion was mixed with 2 parts of polyisocyanate with a viscosity of 2,600 mPa·s, and stirred using a dissolver to obtain a urethane resin-based chemical reaction type adhesive. Each adhesive obtained was uniformly applied to release paper using a glass rod, and then placed in a 100°C oven for 2 minutes to volatilize the solvent. Furthermore, it was placed in a 40°C oven for 96 hours to form a cured film of the adhesive (Application Example 1 and Comparative Application Example 1). When the thermal conductivity of this cured film was measured, the thermal conductivity of the cured film of Comparative Application Example 1 formed using the α-alumina of Comparative Example 13 was 0.49 W / m·K. In contrast, the thermal conductivity of the cured coating of Application Example 1, which was formed using the thermally conductive particles of Example 1, was found to be high, at 0.56 W / m·K.

[0074] <Evaluation of thermally conductive particles> (Measurement of thermal conductivity (block)) A resin composition obtained by mixing 50 parts of polypropylene (manufactured by Prime Polymer Co., Ltd., MFR: 20 g / 10 min) and 50 parts of each thermally conductive component was placed in a plastomill and melt-kneaded at a set temperature of 200 ° C. Next, a mold having a length of 20 mm, a width of 20 mm, and a height of 6 mm was used to perform mold press molding at a condition of 175 ° C. to obtain a test piece. The thermal conductivity of the obtained test piece was measured using the "Standard Isotropic Measurement Module" of a thermal property measuring device (product name "TPS-2500S", manufactured by Kyoto Electronics Manufacturing Co., Ltd.). The thermal conductivity of the test piece formed using α-alumina in Comparative Example 13 was 0.43 W / m·K. In contrast, the thermal conductivity of the test piece formed using the thermally conductive particles in Example 4 was found to be high at 0.59 W / m·K.

[0075] (Dielectric breakdown strength) A resin composition obtained by mixing 30 parts of polypropylene (manufactured by Prime Polymer Co., Ltd., MFR 20g / 10min) and 70 parts of thermally conductive particles was placed in a plastomill and melt-kneaded at a set temperature of 200°C. Then, mold press molding was performed at 175°C to prepare a molded body for evaluation. The obtained molded body for evaluation was cut into a size of 100mm x 100mm x thickness 1mm to obtain a test piece. The obtained test piece was immersed in oil, and the dielectric breakdown voltage was measured in accordance with JIS K6911 and C2110-1 under conditions of AC 10mA and voltage rise rate 2kV / sec. The dielectric breakdown strength (kV / mm) obtained by dividing the measured dielectric breakdown voltage value by the thickness (mm) of the test piece is shown in Table 3.

[0076] [Table 3]

Claims

1. A thermally conductive particle comprising at least an aluminum raw material, a zinc raw material, and a fired material obtained by firing a raw material other than the aluminum raw material and the zinc raw material, The content of the zinc raw material relative to 100 parts by mass of the aluminum raw material is more than 20 parts by mass and not more than 70 parts by mass, the other raw materials contain at least one selected from the group consisting of a boron compound, a tungsten compound, a titanium compound, a bismuth compound, and a fluorine compound, and the content of the other raw materials is 0.05 parts by mass or more and 20 parts by mass or less with respect to 100 parts by mass of the aluminum raw material, Thermally conductive particles that meet the following conditions: (1) 50 g of the thermally conductive particles and an epoxy equivalent of 200 g / eq or more and 1000 g / eq or less are mixed together using an E-type viscometer at a measurement temperature of 25° C., a cone rotor (3°×R9.7), and a rotation speed of 100 s -1 The resin composition for viscosity measurement obtained by the above method was kneaded for 1 minute at 1,000 rpm and 1 minute at 2,000 rpm using an E-type viscometer at a measurement temperature of 25° C., a cone rotor (3°×R9.7), and a rotation speed of 100 s. -1 The viscosity measured under the above conditions is 3,000 mPa·s or less. (2) 500 parts by mass of SUS304 steel balls with a diameter of 5 mm and 100 parts by mass of the thermally conductive particles are placed in a 250 mL wide-mouth cylindrical container, and rotated for 3 hours at 80 rpm with the central axis of the cylinder of the cylindrical container as the rotation axis. The steel balls and the thermally conductive particles are then separated using a sieve with 1 mm mesh to obtain thermally conductive particles after the abrasion test. 4 parts by mass of the thermally conductive particles before and after the abrasion test and 8 parts by mass of lithium borate are mixed and ground in a mortar for 5 minutes. The strength of the iron element is measured using a fluorescent X-ray analyzer, and the degree of abrasion calculated using the following formula for the fluorescent X-ray strength (kcps) of the iron element before and after the abrasion test is 4 kcps or less. Abrasion degree = (fluorescent X-ray intensity of iron element after abrasion test) - (fluorescent X-ray intensity of iron element before abrasion test) (3) A resin composition obtained by kneading 30 parts of a mixed liquid obtained by mixing an epoxy resin having an epoxy equivalent of 200 g / eq or more and 1,000 g / eq or less and an amine-based curing agent having an amine value of 100 mgKOH / g or more and 500 mgKOH / g or less in a ratio of 3:1 to 4:1 with 70 parts of thermally conductive particles is pressed into a mold into a circular sheet molded product having a diameter of 100 mm or more and a thickness of 4 mm or more, heat-cured at a set temperature of 120°C for 1 hour, and cut into four equal parts so as to form a sector shape with a central angle of 90° after cooling. When the thermal conductivity of the test piece is measured by a hot disk thermal property measurement, the thermal conductivity is 0.80 W / m·K or more.

2. 2. The thermally conductive particle according to claim 1, wherein the other raw materials (excluding fluorine compounds) are at least one selected from the group consisting of oxides, oxoacid salts, hydroxides, carbonates, and basic carbonates.

3. It contains at least one element selected from the group consisting of iron, cobalt, copper, manganese, nickel, and chromium, and is colored by this. The thermally conductive particle of claim 1 .

4. A mixture obtained by mixing the thermally conductive particles according to any one of claims 1 to 3 with a thermally conductive filler.

5. 5. The mixture of claim 4, wherein the thermally conductive filler is at least one selected from the group consisting of barium sulfate, talc, boron nitride, and magnesium oxide.

6. The method for producing the thermally conductive particles according to any one of claims 1 to 3, comprising calcining a raw material mixture containing an aluminum raw material, a zinc raw material, and raw materials other than the aluminum raw material and the zinc raw material, the aluminum raw material is at least one selected from the group consisting of boehmite, aluminum hydroxide, and alumina, The method for producing thermally conductive particles, wherein the zinc raw material is at least one selected from the group consisting of zinc oxides and basic carbonates.

7. A method for producing thermally conductive particles, comprising firing the raw material mixture according to claim 6 at 1,000°C or more and 1,600°C or less.

8. An article comprising the thermally conductive particles according to any one of claims 1 to 3.

9. The article according to claim 8 , which is any one of a gravure ink, a coating liquid, a resin composition, and an adhesive composition.

10. A resin composition used to form a thermally conductive resin composition, A resin composition comprising the mixture according to claim 4 and a molding resin.

11. The resin composition according to claim 10, wherein the content of the mixture relative to the entire molding resin is 5% by mass or more and 95% by mass or less.

12. A thermally conductive thin film formed by coating the article according to claim 9 .

13. The article according to claim 8, which is used as a heat dissipation member in any one of an electronic device part, an electronic device housing, an EV motor, and a lithium battery.

Citation Information

Patent Citations

  • Package for accommodating semiconductor device

    JP2003100932A

  • Microcapsule for latent heat storage material, method for producing the same, powder containing microcapsule for latent heat storage material, and heat storage device comprising powder

    JP2022127429A

  • Thermally conductive complex oxide, production method therefor, thermally conductive complex oxide-containing composition, and use therefor

    WO2015137468A1

  • Alumina-based thermally conductive oxide and method for producing same

    WO2018159608A1

  • Spherical zinc oxide particle powder and high thermal conductivity composition

    JP2009249226A