Multilayer structure

The multilayer structure addresses glass layer damage by optimizing adhesive peel force to minimize breakage risk, ensuring robustness and durability during peeling from adherends.

JP2024139426AInactive Publication Date: 2024-10-09NITTO DENKO CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023050362
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing multilayer structures face the risk of glass layer damage when peeled off from an adherend due to strong adhesive forces, which can occur during repair or rework.

Method used

A multilayer structure design with a support, glass layer, metal layer, and adhesive portion configured to minimize glass layer damage by setting the adhesive's peel force to ensure a 50% or less probability of breakage during peeling, using a hook-and-loop fastener or other adhesives with appropriate peeling characteristics.

Benefits of technology

The design reduces the likelihood of glass layer damage during peeling by optimizing the adhesive force, ensuring minimal breakage probability, thus enhancing structural integrity and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139426000001_ABST
    Figure 2024139426000001_ABST
Patent Text Reader

Abstract

To make a glass layer difficult to break when removing a multilayer structure from an adherend.SOLUTION: The multilayer structure includes: a support body; a glass layer laminated on an upper surface side of the support body; a metal layer laminated between the support body and the glass layer; and an adhesive part disposed on a lower surface side of the support body. The glass layer is 10 to 300 μm thick. In the adhesive part, a 45 degree peel force is set so that destruction probability by a glass layer destruction test is 50% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multi-layer structure. [Background technology]

[0002] A multilayer structure in which two or more layers are laminated is known. One example is a multilayer structure in which a silver reflective layer is laminated on a thin glass layer (glass film). The thickness of this multilayer structure is, for example, within the range of 10 to 200 μm. This multilayer structure is obtained, for example, from a glass roll formed by a down-draw method. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-231744 A Summary of the Invention [Problem to be solved by the invention]

[0004] Incidentally, it is also possible to use a resin support as the support of the multilayer structure, provide a metal layer on the resin support, and use it as a mirror. This multilayer structure is used, for example, by attaching the support to an adherend such as a wall via an adhesive layer or the like.

[0005] However, if the peel strength (separation strength) of the adhesive layer or the like is strong, there is a risk that the glass layer will be damaged when the multilayer structure is peeled off from the adherend for the purpose of repair or the like.

[0006] The present invention has been made in view of the above-mentioned points, and has an object to make it difficult for a glass layer to be damaged when a multilayer structure is peeled off from an adherend. [Means for solving the problem]

[0007] This multilayer structure comprises a support, a glass layer laminated on the upper surface of the support, a metal layer laminated between the support and the glass layer, and an adhesive portion provided on the lower surface of the support, wherein the thickness of the glass layer is 10 μm or more and 300 μm or less, and the 45 degree peel force of the adhesive portion is set so that the probability of failure in a glass layer failure test is 50% or less. Effect of the Invention

[0008] According to the disclosed technique, the glass layer can be made less susceptible to breakage when the multilayer structure is peeled off from an adherend. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a cross-sectional view illustrating a multilayer structure according to the present embodiment. [Diagram 2] FIG. 2 is a cross-sectional view illustrating a multilayer structure according to a first modified example of the present embodiment. [Diagram 3] FIG. 11 is a cross-sectional view illustrating a multilayer structure according to Modification 2 of the present embodiment. [Figure 4] FIG. 2 is a diagram illustrating a method for a glass layer destruction test. [Diagram 5] FIG. 13 is a diagram illustrating the results of a glass layer fracture test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the drawings, the same components are denoted by the same reference numerals, and duplicated explanations may be omitted.

[0011] Fig. 1 is a cross-sectional view illustrating a multilayer structure according to this embodiment. As shown in Fig. 1, the multilayer structure 1 has a support 10, a bonding layer 20, a thin glass mirror 30, and an adhesive portion 40. In the multilayer structure 1, the thin glass mirror 30 is laminated on the upper surface 10a of the support 10 via the bonding layer 20. The adhesive portion 40 is provided on the lower surface 10b of the support 10.

[0012] The thin glass mirror 30 has a resin layer 31, a metal layer 32, an adhesive layer 33, and a glass layer 34. However, the resin layer 31 and the adhesive layer 33 can be provided as necessary. For example, the thin glass mirror 30 may have a configuration in which the metal layer 32 is formed directly on the lower surface of the glass layer 34 without having the resin layer 31 and the adhesive layer 33.

[0013] The planar shape of the multilayer structure 1 (the shape when viewed from the normal direction of the upper surface 10a of the support 10) is, for example, rectangular. However, this is not limited, and the planar shape of the multilayer structure 1 can be circular, elliptical, a combination of these, or any other appropriate shape. Furthermore, the planar shapes of the layers do not have to be the same. For example, the planar shape of the support 10 may be larger than the planar shape of the thin glass mirror 30. The multilayer structure 1 can be used, for example, as a mirror.

[0014] Here, the materials and the like of each part of the multi-layer structure 1 will be described.

[0015] [Support] The support 10 supports the thin glass mirror 30. The thickness of the support 10 can be, for example, 0.1 mm or more and 5 mm or less. The material of the support 10 can be resin, metal, glass, etc. Examples of resin include polycarbonate and polypropylene. Examples of metal include aluminum, stainless steel (SUS), copper, etc. When a resin support 10 is used, a flexible multilayer structure 1 can be realized. For example, the multilayer structure 1 can be attached along a curved surface.

[0016] [Joining layer] The bonding layer 20 is laminated on the support 10. As the bonding layer 20, any adhesive or adhesive can be used.

[0017] In this specification, the term "adhesive" refers to a layer that has adhesive properties at room temperature and adheres to an adherend with light pressure. Therefore, even when an adherend that has been stuck to the adhesive is peeled off, the adhesive retains practical adhesive strength. On the other hand, the term "adhesive" refers to a layer that can bond substances by being interposed between them. Therefore, when an adherend that has been stuck to the adhesive is peeled off, the adhesive no longer has practical adhesive strength.

[0018] When a pressure-sensitive adhesive is used for the bonding layer 20, a pressure-sensitive adhesive having, as a base polymer, for example, an acrylic polymer, a silicone polymer, polyester, polyurethane, polyamide, polyether, a fluorine-based polymer, a rubber-based polymer, or the like is used. When a pressure-sensitive adhesive is used for the bonding layer 20, an acrylic pressure-sensitive adhesive is preferably used. This is because an acrylic pressure-sensitive adhesive has excellent optical transparency, and exhibits adhesive properties such as appropriate wettability, cohesiveness, and adhesiveness, and can have excellent weather resistance, heat resistance, and the like. In particular, an acrylic pressure-sensitive adhesive made of an acrylic polymer having 4 to 12 carbon atoms is preferred.

[0019] When an adhesive is used for the bonding layer 20, for example, a polyester adhesive, a polyurethane adhesive, a polyvinyl alcohol adhesive, or an epoxy adhesive is used. When the adhesive is a thermosetting adhesive, it can exhibit peel resistance by heating and curing (solidifying). When the adhesive is a light-curing adhesive such as an ultraviolet-curing adhesive, it can exhibit peel resistance by curing by irradiating it with light such as ultraviolet light. When the adhesive is a moisture-curing adhesive, it can be cured by reacting with moisture in the air, and can therefore exhibit peel resistance by being left to stand.

[0020] [Resin layer] In the example of FIG. 1, a resin layer 31 is provided between a metal layer 32 and a glass layer 34. The resin layer 31 can be composed of, for example, one layer or multiple layers. When the resin layer 31 is composed of multiple layers, it is preferable to laminate the layers with an adhesive layer having an adhesive function interposed therebetween. The total thickness of the resin layer 31 may be 20 μm or more and 1000 μm or less from the viewpoint of flexibility, preferably 25 μm or more and 500 μm or less, more preferably 50 μm or more and 200 μm or less. When the resin layer 31 is composed of one layer, the thickness of the resin layer 31 can be, for example, 20 μm or more and 150 μm or less.

[0021] Examples of materials for the resin layer 31 include polyester-based resins such as polyethylene terephthalate-based resins and polyethylene naphthalate-based resins, cycloolefin-based resins such as norbornene-based resins, polyethersulfone-based resins, polycarbonate-based resins, acrylic-based resins, polyolefin-based resins, polyimide-based resins, polyamide-based resins, polyimideamide-based resins, polyarylate-based resins, polysulfone-based resins, polyetherimide-based resins, cellulose-based resins, and urethane-based resins.

[0022] The resin layer 31 is provided as necessary, but providing the resin layer 31 has the effect of improving the handleability of the multilayer structure 1.

[0023] [Metal layer] The metal layer 32 is laminated between the support 10 and the glass layer 34. In the example of FIG. 1, the metal layer 32 is laminated on the lower surface of the resin layer 31. In addition, in the example of FIG. 1, the side of the metal layer 32 opposite to the resin layer 31 is bonded to the support 10 via the bonding layer 20. The metal layer 32 is a layer that reflects visible light incident through the glass layer 34. That is, the upper surface 32a of the metal layer 32 (the surface in contact with the resin layer 31) is a reflective surface that reflects visible light incident through the glass layer 34. In addition, in the example of FIG. 1, visible light is incident on the upper surface 32a of the metal layer 32 through the glass layer 34, the adhesive layer 33, and the resin layer 31.

[0024] The metal layer 32 may be laminated between the support 10 and the glass layer 34, and is not limited to the example shown in FIG. 1. The metal layer 32 may be laminated on, for example, the resin layer 31. For example, as in the multilayer structure 1A shown in FIG. 2, a structure in which a bonding layer 20, a resin layer 31, a metal layer 32, an adhesive layer 33, and a glass layer 34 are laminated in this order on the upper surface 10a of the support 10 may be used. The metal layer 32 may be formed on the upper surface of the resin layer 31 by, for example, a sputtering method, a vapor deposition method, a plating method, or the like.

[0025] Alternatively, the metal layer 32 may be formed on the lower surface of the glass layer 34. For example, as in the multilayer structure 1B shown in Fig. 3, a structure in which a bonding layer 20, a resin layer 31, an adhesive layer 33, a metal layer 32, and a glass layer 34 are sequentially laminated on an upper surface 10a of a support 10 can be used. The metal layer 32 can be formed on the lower surface of the glass layer 34 by, for example, a sputtering method, a vapor deposition method, a plating method, or the like.

[0026] In the multilayer structure 1 shown in Fig. 1, the metal layer 32 is located below the resin layer 31, which makes it possible to reduce scratches that occur during the process. That is, when manufacturing a multilayer structure, if an adhesive that becomes the adhesive layer 33 is applied to the surface of the metal layer 32 and spread thinly, the surface of the metal layer 32 is easily scratched when spreading thinly. The structure in Fig. 1 does not require the process of applying and spreading an adhesive on the surface of the metal layer 32, so scratches on the surface of the metal layer 32 can be suppressed.

[0027] In the multilayer structure 1A shown in Fig. 2, the metal layer 32 is located above the resin layer 31, so that the reflected light is not affected by the light absorption of the resin layer 31, and it is possible to obtain clearer reflection characteristics. In the multilayer structure 1B shown in Fig. 3, the metal layer 32 is located directly below the glass layer 34, so that the reflected light is not affected by the light absorption of the resin layer 31 and the adhesive layer 33, and it is possible to obtain even clearer reflection characteristics.

[0028] The material of the metal layer 32 is preferably a material with high visible light reflectance, such as aluminum, silver, a silver alloy, etc. The visible light reflectance of the metal layer 32 alone is preferably 70% or more, more preferably 75% or more, and even more preferably 83% or more. The visible light reflectance of the metal layer 32 alone can be measured by a method in accordance with JIS R3220:2011.

[0029] The thickness of the metal layer 32 is not particularly limited, but is, for example, about 10 nm or more and 500 nm or less. The metal layer 32 can be formed directly on the lower surface of the resin layer 31 by, for example, a sputtering method, a vapor deposition method, a plating method, or the like. When the resin layer 31 is not provided, the metal layer 32 may be formed on the lower surface of the glass layer 34 by, for example, a sputtering method, a vapor deposition method, a plating method, or the like. The metal layer 32 may also be formed on the upper surface 10a of the support 10 by, for example, a sputtering method, a vapor deposition method, a plating method, or the like.

[0030] [Adhesive layer] The adhesive layer 33 is formed from a material with high visible light transmittance. The thickness of the adhesive layer 33 is, for example, 0.1 μm or more and 25 μm or less. For example, an acrylic adhesive, a silicone adhesive, a rubber adhesive, an ultraviolet-curable acrylic adhesive, an ultraviolet-curable epoxy adhesive, a thermosetting epoxy adhesive, a thermosetting melamine adhesive, a thermosetting phenol adhesive, an ethylene vinyl acetate (EVA) intermediate film, a polyvinyl butyral (PVB) intermediate film, etc. can be used as the adhesive layer 33.

[0031] [Glass layer] The glass layer 34 is laminated on the upper surface 10a side of the support 10. In the example of FIG. 1, the glass layer 34 is laminated on the resin layer 31 via an adhesive layer 33. There is no particular limitation on the glass layer 34, and an appropriate one can be adopted depending on the purpose. The glass layer 34 can be classified according to its composition, for example, soda-lime glass, borate glass, aluminosilicate glass, quartz glass, etc. Also, according to the alkali component, it can be classified as non-alkali glass or low-alkali glass. The alkali metal component of the above glass (for example, Na 2OK 2 O, Li 2 The content of O) is preferably 15% by weight or less, and more preferably 10% by weight or less.

[0032] Considering the surface hardness, airtightness, and corrosion resistance of glass, the thickness of the glass layer 34 is preferably 10 μm or more. Since it is desirable for the glass layer 34 to have flexibility like a film, the thickness of the glass layer 34 is preferably 300 μm or less. The thickness of the glass layer 34 is more preferably 20 μm or more and 200 μm or less, and particularly preferably 30 μm or more and 150 μm or less.

[0033] The glass layer 34 preferably has a light transmittance of 85% or more at a wavelength of 550 nm. The glass layer 34 preferably has a refractive index of 1.4 to 1.65 at a wavelength of 550 nm. The glass layer 34 preferably has a density of 2.3 g / cm 3 ~3.0g / cm 3 and more preferably 2.3 g / cm 3 ~2.7g / cm 3 It is.

[0034] The method for forming the glass layer 34 is not particularly limited, and an appropriate method can be adopted depending on the purpose. Typically, the glass layer 34 can be produced by melting a mixture containing a main raw material such as silica or alumina, an antifoaming agent such as mirabilite or antimony oxide, and a reducing agent such as carbon at a temperature of about 1400°C to 1600°C, forming it into a thin plate, and then cooling it. Examples of the method for forming the glass layer 34 include a slot downdraw method, a fusion method, and a float method. The glass layer formed into a plate by these methods may be chemically polished with a solvent such as hydrofluoric acid as necessary to make it thinner or to increase the smoothness.

[0035] The upper surface of the glass layer 34 (the surface on which the adhesive layer 33 is not formed) may be provided with a functional layer such as an antifouling layer, an antireflection layer, a conductive layer, a reflective layer, or a decorative layer.

[0036] [Adhesive part 40] The adhesive part 40 is used to attach the multilayer structure 1 to the adherend. In consideration of rework, the adhesive part 40 is preferably one that can easily peel the multilayer structure 1 from the adherend. Here, rework refers to, for example, a case where a mistake in attachment occurs during construction and the multilayer structure is reattached. In such a case, if the peel force of the adhesive part 40 is too strong, the glass layer 34 of the thin glass mirror 30 may be damaged when the multilayer structure 1 is peeled off from the adherend. On the other hand, by appropriately setting the peel force of the adhesive part 40, the risk of damage to the glass layer 34 of the thin glass mirror 30 when the multilayer structure 1 is peeled off from the adherend can be reduced.

[0037] The adhesive portion 40 can be formed using any of the materials exemplified as the adhesive of the bonding layer 20, so long as it has an appropriate peel strength. Alternatively, the adhesive portion 40 may be a double-sided tape, a hook-and-loop fastener, or the like, so long as it has an appropriate peel strength. The thickness of the adhesive portion 40 is not particularly limited, but is, for example, about 5 μm or more and 2000 μm or less.

[0038] [Study of peel strength of adhesive part 40] The multilayer structure 1 is attached to an adherend via the adhesive portion 40. The adherend is typically a building material such as a wall containing calcium silicate. Alternatively, the adherend may be a material generally used in building materials, such as plasterboard, wallpaper, wood, metal, or glass.

[0039] Conventionally, an adhesive with strong peel strength has been used for the adhesive portion 40. Therefore, the adhesive portion 40 adheres closely to the adherend, and a large force is required to peel it off, and there are cases where the glass layer 34 of the thin glass mirror 30 is damaged when the multilayer structure 1 is peeled off from the adherend.

[0040] Therefore, the inventors have investigated the peel strength of the adhesive portion 40 that can peel the multilayer structure 1 from the adherend without damaging the glass layer 34. Specifically, the following glass layer destruction test was carried out in an environment of room temperature (25°C).

[0041] 4 is a diagram for explaining the method of the glass layer destruction test. First, 10 pieces each of a hook-and-loop fastener, double-sided tape A, and double-sided tape B were prepared as the adhesive portion 40. Note that double-sided tapes A and B are double-sided tapes that have been used conventionally and have a relatively strong peel strength.

[0042] Next, 40 multilayer structures 1 shown in FIG. 4 were produced using 10 of each adhesive portion 40. The planar shape of the multilayer structure 1 was 20 mm×220 mm. A polycarbonate sheet having a thickness of 0.4 mm was used for the support 10. The metal layer 32 was an aluminum film having a thickness of 50 nm. The thickness of the glass layer 34 was 100 μm.

[0043] Next, an adherend 100 having a thickness of 1.3 mm was prepared, and the adhesive portion 40 of the multilayer structure 1 was attached to the flat upper surface 100a of the adherend 100. A plate glass was used as the adherend 100. An end of the adherend 100 was fixed to a fixing portion 120 via a string 110. The angle θ between the upper surface 100a of the adherend 100 and the upper surface 120a of the fixing portion 120 was 45 degrees.

[0044] Next, the adherend 100 was moved at 300 mm / min in a direction A perpendicular to the upper surface 100a, the adhesive portion 40 was peeled off from the upper surface 100a of the adherend 100, and the 45-degree peel force (N / 20 mm) was measured. After peeling, it was visually confirmed whether the glass layer 34 was damaged or not. Specifically, it was visually observed, and if even one crack penetrated the glass layer 34, it was determined that it was damaged.

[0045] The same test was performed on all 40 multilayer structures 1 to determine the 45-degree peel force and the probability of failure. The average 45-degree peel force and the probability of failure of the four types of adhesive portion 40 are summarized in Table 1. The probability of failure is the ratio of the number of multilayer structures in which the glass layer was broken to the number of multilayer structures tested. [Table 1]

[0046] As shown in Table 1, when the adhesive portion 40 was a hook-and-loop fastener, the 45-degree peel force was 7.5 (N / 20 mm) and the failure probability was 20%.

[0047] In contrast, when the adhesive portion 40 was double-sided tape A, the 45-degree peel force was 68.2 (N / 20 mm) and the failure probability was 100%. When the adhesive portion 40 was double-sided tape B, the 45-degree peel force was 38.5 (N / 20 mm) and the failure probability was 80%.

[0048] In this way, it was found that by using a hook-and-loop fastener as the adhesive portion 40, it was possible to reduce the 45-degree peel force compared to the double-sided tapes A and B that were conventionally used, and thus the probability of breakage could be significantly reduced.

[0049] Next, the results of Table 1 were summarized in Figure 5, and the approximate formula y = 1.4895x + 7.4351 was calculated. In Figure 5, the horizontal axis (x) is the 45 degree peel force (N / 20mm), and the vertical axis (y) is the failure probability (%). Since the failure probability of the conventionally used double-sided tapes A and B is 80% to 100%, it was determined that a failure probability of 50% or less (y = 50 or less) would be a sufficient improvement effect, and the condition where the failure probability is 50% or less was set as the pass line.

[0050] 5, from the viewpoint of further suppressing breakage of the thin glass mirror 30, it is preferable to satisfy the range of 0.03≦x≦28.57, where y=1.4895x+7.4351. Here, x=0.03 (N / 20 mm) is the minimum 45-degree peel force required when attaching the multilayer structure 1 to an adherend. Also, x=28.57 (N / 20 mm) is the 45-degree peel force for which y=50(%) in the above approximation formula.

[0051] Thus, in the multilayer structure 1, the adhesive portion 40 is preferably set at a 45-degree peel force so that the probability of failure in a glass layer failure test is 50% or less. It is more preferable that the adhesive portion 40 is set at a 45-degree peel force so that the probability of failure in a glass layer failure test is 20% or less. It is even more preferable that the adhesive portion 40 satisfies the range of 0.03≦x≦28.57, where x is the 45-degree peel force (N / 20 mm) and y is the probability of failure (%), where y=1.4895x+7.4351. This makes it possible to make the glass layer 34 of the thin glass mirror 30 less likely to break when the multilayer structure 1 is peeled off from the adherend.

[0052] In the above, a hook-and-loop fastener is exemplified as the adhesive portion 40 capable of setting the 45-degree peel force so that the probability of failure in the glass layer failure test is 50% or less. However, the present invention is not limited to this, and other materials and adhesives may be used as long as the 45-degree peel force can be set so that the probability of failure in the glass layer failure test is 50% or less.

[0053] Although the preferred embodiments have been described in detail above, the present invention is not limited to the above-described embodiments, and various modifications and substitutions can be made to the above-described embodiments without departing from the scope of the claims.

[0054] In addition to the above-described embodiments, the following supplementary notes are disclosed. (Appendix 1) A support; A glass layer laminated on the upper surface side of the support; a metal layer laminated between the support and the glass layer; An adhesive portion provided on the lower surface side of the support, The thickness of the glass layer is 10 μm or more and 300 μm or less, A multilayer structure, wherein the adhesive portion has a 45 degree peel force set so that the probability of breakage in a glass layer breakage test is 50% or less. (Appendix 2) 2. The multilayer structure according to claim 1, wherein the adhesive portion has a 45 degree peel force set so that the probability of breakage in a glass layer breakage test is 20% or less. (Appendix 3) When x is the 45 degree peel force (N / 20mm) and y is the probability of failure (%), 3. The multilayer structure according to claim 1 or 2, wherein y=1.4895x+7.4351 satisfies the range of 0.03≦x≦28.57. (Appendix 4) 4. The multilayer structure according to claim 1, wherein the adhesive portion is a hook-and-loop fastener. (Appendix 5) 5. The multilayer structure according to claim 1, further comprising a resin layer provided between the metal layer and the glass layer. (Appendix 6) the glass layer is laminated on an upper surface side of the resin layer via an adhesive layer, the metal layer is laminated on a lower surface of the resin layer, 6. The multilayer structure according to claim 5, wherein the metal layer is joined to the support via a joining layer on the opposite side to the resin layer. [Explanation of symbols]

[0055] 1,1A,1B Multi-layer structure 10 Support 10a Top 10b Bottom side 20 Bonding layer 30 Thin Glass Mirror 31 Resin layer 32 metal layer 33 Adhesive layer 34 Glass layer 40 Adhesive part

Claims

1. A support; A glass layer laminated on the upper surface side of the support; a metal layer laminated between the support and the glass layer; An adhesive portion provided on the lower surface side of the support, The thickness of the glass layer is 10 μm or more and 300 μm or less, A multilayer structure, wherein the adhesive portion has a 45 degree peel force set so that the probability of breakage in a glass layer breakage test is 50% or less.

2. The multilayer structure according to claim 1 , wherein the adhesive portion has a 45 degree peel force set so that a probability of breakage in a glass layer breakage test is 20% or less.

3. When x is the 45 degree peel force (N / 20 mm) and y is the failure probability (%), The multi-layer structure according to claim 1 , which satisfies the range of y=1.4895x+7.4351, where 0.03≦x≦28.

57.

4. The multi-layer structure according to claim 1 , wherein the adhesive portion is a hook-and-loop fastener.

5. The multilayer structure according to claim 1 , further comprising a resin layer provided between the metal layer and the glass layer.

6. the glass layer is laminated on an upper surface side of the resin layer via an adhesive layer; the metal layer is laminated on a lower surface of the resin layer, The multilayer structure according to claim 5 , wherein the metal layer is bonded to the support via a bonding layer on the side opposite to the resin layer.

Citation Information

Patent Citations

  • Film mirror, manufacturing method of the same, and sunlight reflecting mirror using the same

    JP2013231744A