Cured product, curable resin composition, dry film, and printed wiring board
A curable resin composition with a carboxyl group-containing resin and hollow filler addresses the challenge of high dielectric loss in printed wiring boards, providing a cured product with low dielectric constant and loss tangent for improved signal transmission in high-frequency communication systems.
Patent Information
- Application Number
- JP2023050417
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Current photocurable thermosetting resin compositions for printed wiring boards face challenges in achieving low dielectric constant and dielectric loss tangent, leading to signal attenuation and heat generation due to high-frequency, high-density communication signals.
A curable resin composition containing a carboxyl group-containing resin, photopolymerization initiator, and hollow filler, with a porosity of 5-15% by volume, to form a cured product with a low dielectric constant and dielectric loss tangent.
The composition achieves a cured product with improved dielectric properties, reducing signal attenuation and heat generation, while maintaining sensitivity and adhesion, suitable for high-capacity communication systems.
Smart Images

Figure 2024139464000001 
Figure 2024139464000002 
Figure 2024139464000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a cured product that is soluble in a dilute alkaline aqueous solution, a curable resin composition capable of forming the cured product, a dry film thereof, and a printed wiring board having the cured product. [Background technology]
[0002] At present, for photocurable thermosetting resin compositions for solder resists in some consumer printed wiring boards and most industrial printed wiring boards, from the viewpoint of high precision and high density, liquid development type photocurable thermosetting resin compositions for solder resists are used, which are formed by irradiating with ultraviolet light, developing, and finish curing (main curing) by irradiating with heat and / or light. Among them, in consideration of environmental issues, alkaline development type photocurable thermosetting resin compositions for photo solder resists that use a dilute alkaline aqueous solution as a developer have become mainstream, and are used in large quantities in the actual production of printed wiring boards. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-539072 A Summary of the Invention [Problem to be solved by the invention]
[0004] One of the purposes of using solder resist is to protect printed wiring boards as an insulating material. However, in recent years, with the spread of high-capacity, high-speed communications such as the 5th generation communication system (5G), communication devices are required to have higher frequencies, higher density mounting, and larger currents. If the relative dielectric constant (Dk) and dielectric loss tangent (Df) are not low enough, the frequency will increase transmission loss due to dielectric loss, causing problems such as signal attenuation and heat generation. Therefore, it is required to form a cured material with a low dielectric constant and low dielectric loss tangent. To solve this problem, it is necessary to reduce the dielectric constant and dielectric loss tangent of solder resist.
[0005] An object of the present invention is to provide a cured product having a low dielectric constant and a low dielectric loss tangent, a curable resin composition capable of forming the cured product, a dry film, and a printed wiring board having the cured product. [Means for solving the problem]
[0006] The present inventors have conducted intensive research and have succeeded in providing a cured product having a low dielectric constant and a low dielectric loss tangent, and a resin composition capable of forming such a cured product, thereby completing the present invention.
[0007] That is, according to the present invention, the following inventions are provided. [1] A cured product of a curable resin composition, the cured product having a porosity of 5 volume % or more and 15 volume % or less. [2] A curable resin composition for use in the cured product according to [1], comprising a carboxyl group-containing resin, A curable resin composition comprising a photopolymerization initiator and a hollow filler. [3] The curable resin composition according to [2], wherein the hollow filler contains silica. [4] The curable resin composition according to either [2] or [3], wherein the hollow filler is mixed in an amount of 250 parts by mass or less per 100 parts by mass of the carboxyl group-containing resin. [5] The curable resin composition according to any one of [2] to [4], wherein the hollow filler has an average particle size D50 of 0.1 to 110 μm. [6] The curable resin composition according to any one of [2] to [5], wherein the hollow filler has a porosity of 30 to 50%. [7] The curable resin composition according to any one of [2] to [6], further comprising a photopolymerizable monomer. [8] A dry film obtained by applying the curable resin composition according to any one of [2] to [7] to a first film and drying it. [9] A cured product obtained by curing the dry film described in [8].
[10] A printed wiring board having the cured product described in [1] or [9]. Effect of the Invention
[0008] According to the present invention, it is possible to provide a cured product having a specific porosity, a low dielectric constant, and a low dielectric tangent, a curable resin composition containing a hollow filler for forming the cured product, a dry film, and a printed wiring board having the cured product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Preferred embodiments of the present invention will be described in detail below, however, the present invention is not limited to the following embodiments.
[0010] In this specification, "(meth)acrylate" is a term that collectively refers to "acrylate," "methacrylate," and mixtures thereof, and the same applies to other similar expressions.
[0011] [Cured product] The cured product according to the present invention is a cured product made of a curable resin composition, and has a porosity of 5% by volume or more and 15% by volume or less. The cured product of the present invention has excellent properties such as a low dielectric constant and a low dielectric tangent, and can be particularly suitably used as a solder resist for printed wiring boards. In the present invention, the cured state specifically means a state in which the curable resin composition is not attached to the surface of the cloth after placing a cloth containing isopropyl alcohol on the surface of the cured product, placing a 500 g weight on the cloth, and leaving it for 1 minute. The method for producing the cured product includes the method described in the description of the cured coating and the method described in the Examples below.
[0012] The porosity of the cured product is 5% by volume or more and 15% by volume or less. If the porosity of the cured product is within the above range, an excellent low dielectric constant and low dielectric loss tangent can be achieved. The porosity of the cured product is preferably from 5 vol. % to 13 vol. %, and more preferably from 6 vol. % to 12 vol. %. The porosity of the cured product can be calculated by a conventionally known method, for example, the method described in the Examples. The method for adjusting the porosity of the cured product is not particularly limited, and examples thereof include a method of adjusting the type and amount of a hollow filler blended in the curable resin composition of the present invention, and a method of adjusting the type and amount of a foaming agent blended in place of or in combination with the hollow filler.
[0013] [Curable resin composition] The curable resin composition of the present invention contains a carboxyl group-containing resin, a photopolymerization initiator, and a hollow filler. Since the curable resin composition of the present invention contains the above components, it is possible to obtain a cured product with high sensitivity, low dielectric constant and dielectric loss tangent, and excellent solder heat resistance. In the case of high sensitivity, the exposure time for obtaining a cured product can be shortened, which leads to a shortened tact time.
[0014] (Carboxyl group-containing resin) The carboxyl group-containing resin in the curable resin composition of the present embodiment is used to impart alkaline developability, and a known resin containing a carboxyl group in the molecule can be used. In particular, from the standpoint of photocurability and development resistance, a carboxyl group-containing resin having an ethylenically unsaturated double bond in the molecule is preferred. The unsaturated double bond is more preferably derived from acrylic acid or methacrylic acid or a derivative thereof. As the carboxyl group-containing resin, preferred are carboxyl group-containing resins made from an epoxy resin as a starting material, carboxyl group-containing urethane resins having a urethane skeleton, carboxyl group-containing copolymer resins having a copolymer structure of an unsaturated carboxylic acid, and carboxyl group-containing resins made from a phenol compound as a starting material. Specific examples of the carboxyl group-containing resin are given below.
[0015] (1) Carboxyl group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, lower alkyl (meth)acrylate, or isobutylene. (2) Carboxylic acid-containing urethane resins obtained by the polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups. (3) Terminal carboxyl group-containing urethane resins obtained by reacting acid anhydrides with the terminals of urethane resins obtained by polyaddition reaction of diisocyanate compounds such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with diol compounds such as polycarbonate-based polyols, polyether-based polyols, polyester-based polyols, polyolefin-based polyols, acrylic polyols, bisphenol A-based alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups. (4) Carboxylic acid-containing photosensitive urethane resins obtained by the polyaddition reaction of diisocyanates with (meth)acrylates of bifunctional epoxy resins such as bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bixylenol type epoxy resins, and biphenol type epoxy resins, or their partial acid anhydride modified products, carboxyl group-containing dialcohol compounds, and diol compounds. (5) A carboxyl group-containing urethane resin obtained by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (2) or (4) described above, to thereby (meth)acrylate the terminals of the carboxyl group. (6) A carboxyl group-containing urethane resin having terminal (meth)acrylation obtained by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reactant of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (2) or (4) described above. (7) A carboxyl group-containing photosensitive resin obtained by reacting a bifunctional or more polyfunctional epoxy resin as described below with (meth)acrylic acid and adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the hydroxyl groups present in the side chains. Here, the epoxy resin is preferably solid. (8) A carboxyl group-containing photosensitive resin obtained by reacting a polyfunctional epoxy resin, in which the hydroxyl groups of a bifunctional epoxy resin as described below are further epoxidized with epichlorohydrin, with (meth)acrylic acid, and then adding a dibasic acid anhydride to the resulting hydroxyl groups. Here, the epoxy resin is preferably in a solid state. (9) A carboxyl group-containing photosensitive resin obtained by adding a cyclic ether such as ethylene oxide or a cyclic carbonate such as propylene carbonate to a polyfunctional phenol compound such as novolak, partially esterifying the resulting hydroxyl groups with (meth)acrylic acid, and reacting the remaining hydroxyl groups with a polybasic acid anhydride. (10) A carboxyl group-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in the molecule, such as glycidyl (meth)acrylate, α-methylglycidyl (meth)acrylate, to any of the resins (1) to (9).
[0016] The carboxyl group-containing resin is not limited to these, and may be used alone or in combination of two or more kinds. Incidentally, the term "(meth)acrylate" used herein is a general term for acrylate, methacrylate and mixtures thereof, and the same applies to other similar expressions hereinafter. Carboxylic acid-containing resins have many free carboxyl groups in the side chains of the backbone polymer, making them possible to develop with dilute alkaline aqueous solutions.
[0017] The acid value of the carboxyl group-containing resin is preferably 40 to 200 mgKOH / g. When the acid value of the carboxyl group-containing resin is 40 mgKOH / g to 200 mgKOH / g or less, the adhesion of the cured coating is obtained, alkaline development is facilitated, dissolution of the exposed area by the developer is suppressed, and the lines do not become thinner than necessary, making it easy to draw a normal resist pattern. The acid value is more preferably 45 to 120 mgKOH / g.
[0018] The weight average molecular weight of the carboxyl group-containing resin varies depending on the resin skeleton, but is generally preferably 2,000 to 150,000. When it is in the range of 2,000 to 150,000, the tack-free performance is good, the moisture resistance of the cured film after exposure is good, and film loss during development is unlikely to occur. Furthermore, when the weight average molecular weight is in the above range, the resolution is improved, the developability is good, and the storage stability is improved. It is more preferably 5,000 to 100,000.
[0019] The amount of the carboxyl group-containing resin in the curable resin composition is suitably 20 to 80% by mass. When the amount is 20 to 80% by mass, the film strength is good, the viscosity of the composition can be reduced, and the coating properties are excellent. The amount is more preferably 30 to 60% by mass.
[0020] (Photopolymerization initiator) As the photopolymerization initiator that can be suitably used in the curable resin composition of the present invention, one or more photopolymerization initiators selected from the group consisting of oxime ester-based photopolymerization initiators having an oxime ester group, alkylphenone-based photopolymerization initiators, α-aminoacetophenone-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, and titanocene-based photopolymerization initiators can be suitably used.
[0021] As the oxime ester photopolymerization initiator, commercially available products include CGI-325, Irgacure OXE01, Irgacure OXE02 manufactured by BASF Japan, and N-1919 and NCI-831 manufactured by ADEKA CORPORATION. In addition, photopolymerization initiators having two oxime ester groups in the molecule can also be suitably used. As the oxime ester photopolymerization initiator, an oxime ester compound having a carbazole structure is preferred.
[0022] Commercially available alkylphenone photopolymerization initiators include α-hydroxyalkylphenone types such as Irgacure 184, Darocure 1173, Irgacure 2959, and Irgacure 127, all manufactured by BASF Japan.
[0023] Specific examples of the α-aminoacetophenone-based photopolymerization initiator include 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropanone-1, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, and N,N-dimethylaminoacetophenone. Commercially available products include Irgacure 907, Irgacure 369, and Irgacure 379 manufactured by BASF Japan.
[0024] Specific examples of the acylphosphine oxide photopolymerization initiator include 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, etc. Commercially available products include Lucirin TPO manufactured by BASF and Irgacure 819 manufactured by BASF Japan. As the photopolymerization initiator, titanocene-based photopolymerization initiators such as Irgacure 389 and Irgacure 784 manufactured by BASF Japan can also be suitably used.
[0025] The amount of the photopolymerization initiator is preferably 0.1 to 25 parts by mass, more preferably 1 to 20 parts by mass, based on 100 parts by mass of the carboxyl group-containing resin. By using 0.1 to 25 parts by mass, a cured film having excellent photocurability and resolution, improved adhesion and PCT resistance, and excellent chemical resistance such as electroless gold plating resistance can be obtained. In particular, when the amount is 25 parts by mass or less, the effect of reducing outgassing can be obtained, and further, the decrease in deep curability due to intense light absorption on the surface of the cured film can be suppressed.
[0026] In addition to the photopolymerization initiator, the curable resin composition may contain a photoinitiator assistant and a sensitizer. Examples of the photopolymerization initiator, photoinitiator assistant and sensitizer that may be suitably used in the curable resin composition include a benzoin compound, an acetophenone compound, an anthraquinone compound, a thioxanthone compound, a ketal compound, a benzophenone compound, a tertiary amine compound and a xanthone compound.
[0027] These photopolymerization initiators, photoinitiator assistants, and sensitizers can be used alone or as a mixture of two or more kinds. The total amount of such photopolymerization initiators, photoinitiator assistants, and sensitizers is preferably 35 parts by mass or less per 100 parts by mass of the carboxyl group-containing resin. If it is 35 parts by mass or less, it is possible to suppress the deterioration of deep curing property due to light absorption by these.
[0028] (Hollow filler) A hollow filler is a filler that is hollow inside. The degree of hollowness can be expressed by the porosity of the hollow filler, and the porosity of the hollow filler is preferably 30 to 50% by volume. When the porosity of the hollow filler is 30 to 50% by volume, a preferable porosity is obtained in the cured product. The hollow filler preferably has an average particle size D50 of 0.1 μm to 110 μm, more preferably 0.5 μm to 100 μm. When the average particle size D50 is 0.1 μm to 110 μm, a preferable porosity can be obtained in the cured product. The hollow filler may be any one having a hollow interior, but is preferably hollow silica. In addition to hollow silica, the hollow filler may be hollow glass. Specific examples of hollow silica include Sururia 1110 manufactured by JGC Catalysts and Chemicals Co., Ltd. Specific examples of hollow glass include Glass Bubbles K1, K15, K20, S22, K25, K37, S38, VS5500, S42XHS, K46, iM16K, S60J, S60HS, and iM30K manufactured by Sumitomo 3M Limited, and Sphericel 110P8, 60P18, 34P30, 25P45, Q-CEL 5020, 5020FPS, 7014, 7040S, Ceramic Multi Cellular CMC-20, CMC-15L, and Extendospheres SG manufactured by Potters-Barotini. The hollow fillers can be used alone or in combination of two or more kinds.
[0029] The amount of hollow filler is preferably 250 parts by mass or less, more preferably 20 to 150 parts by mass, and particularly preferably 30 to 130 parts by mass, relative to 100 parts by mass of the carboxyl group-containing resin. When the amount of hollow filler is 250 parts by mass or less, a cured product having a desired porosity can be obtained.
[0030] The curable resin composition of the present invention may contain a foaming agent instead of or in combination with the hollow filler in order to form the cured product of the present invention having the above-mentioned porosity. The foaming agent may be an inorganic foaming agent or an organic foaming agent, and examples of the inorganic foaming agent include sodium bicarbonate and ammonium carbonate. Examples of the organic foaming agent include organic azo compounds such as diazoamino derivatives, azonitrile derivatives, and azodicarboxylic acid derivatives. Examples of the organic azo compounds include azodicarboxylic acid amide and azobis-isobutyronitrile. Specific examples of the organic foaming agent include azodicarbonamide (ADCA), dinitrosopentamethylenetetramine (DPT), p,p-oxybisbenzenesulfonylhydrazide (OBSH), azobisisobutyronitrile (AIBN), and the like. The amount of the foaming agent is preferably 250 parts by mass or less based on 100 parts by mass of the carboxyl group-containing resin.
[0031] (Photopolymerizable monomer) The curable resin composition of the present invention may further contain a photopolymerizable monomer. As the photopolymerizable monomer, a compound having two or more ethylenically unsaturated groups in the molecule, a compound obtained by adding an α,β-unsaturated carboxylic acid to a polyhydric alcohol, a compound obtained by adding an α,β-unsaturated carboxylic acid to a glycidyl group-containing compound, etc. may be used.
[0032] Examples of compounds having two or more ethylenically unsaturated groups in the molecule include diacrylates of glycols such as ethylene glycol, methoxytetraethylene glycol, polyethylene glycol, and propylene glycol; polyhydric alcohols such as hexanediol, trimethylolpropane, pentaerythritol, dipentaerythritol, and tris-hydroxyethyl isocyanurate, and polyhydric acrylates such as ethylene oxide adducts or propylene oxide adducts of these alcohols; polyhydric acrylates such as phenoxy acrylate, bisphenol A diacrylate, and ethylene oxide adducts or propylene oxide adducts of these phenols; polyhydric acrylates of glycidyl ethers such as glycerin diglycidyl ether, glycerin triglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate; and melamine acrylate and / or methacrylates corresponding to the above acrylates.
[0033] Examples of compounds obtained by adding an α,β-unsaturated carboxylic acid to a polyhydric alcohol include ethylene glycol diacrylate, diethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, propylene glycol diacrylate, polypropylene glycol diacrylate, butylene glycol diacrylate, pentyl glycol diacrylate, 1,6-hexanediol diacrylate, trimethylolpropane diacrylate, trimethylolpropane triacrylate, tetramethylolmethane triacrylate, tetramethylolmethane tetraacrylate, glycerin diacrylate, pentaerythritol diacrylate, pentaerythritol triacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, and / or methacrylates corresponding to the above acrylates.
[0034] Examples of compounds obtained by adding an α,β-unsaturated carboxylic acid to a glycidyl group-containing compound include ethylene glycol diglycidyl ether diacrylate, diethylene glycol diglycidyl ether diacrylate, trimethylolpropane triglycidyl ether triacrylate, bisphenol A glycidyl ether diacrylate, phthalic acid diglycidyl ester diacrylate, glycerin polyglycidyl ether polyacrylate, and the like; and other compounds include 2,2-bis(4-acryloyloxydiethoxyphenyl)propane, 2,2-bis-(4-acryloyloxypolyethoxyphenyl)propane, 2-hydroxy-3-acryloyloxypropyl acrylate, and / or methacrylates corresponding to the above acrylates. These photopolymerizable monomers can be used alone or in combination.
[0035] The amount of the photopolymerizable monomer is preferably 5 to 100 parts by mass, more preferably 10 to 90 parts by mass, and even more preferably 15 to 85 parts by mass, relative to 100 parts by mass of the carboxyl group-containing resin. By setting the amount within the above range, the photocurability is improved, pattern formation becomes easy, and the strength of the cured film can also be improved.
[0036] The curable resin composition of the present invention may further contain a thermosetting component. As the thermosetting component, known and commonly used thermosetting resins such as blocked isocyanate compounds, amino resins, maleimide compounds, benzoxazine resins, carbodiimide resins, cyclocarbonate compounds, polyfunctional epoxy compounds, polyfunctional oxetane compounds, episulfide resins, and melamine derivatives can be used. Among these, preferred thermosetting components are those having two or more cyclic ether groups and / or cyclic thioether groups (hereinafter abbreviated as cyclic (thio)ether groups) in one molecule. There are many types of thermosetting components having these cyclic (thio)ether groups available on the market, and various properties can be imparted depending on their structures.
[0037] Such a thermosetting component having two or more cyclic (thio)ether groups in the molecule is a compound having two or more of either one or both of a 3-, 4-, or 5-membered cyclic ether group or a cyclic thioether group in the molecule, and examples thereof include a compound having at least two or more epoxy groups in the molecule, i.e., a polyfunctional epoxy compound, a compound having at least two or more oxetanyl groups in the molecule, i.e., a polyfunctional oxetane compound, and a compound having two or more thioether groups in the molecule, i.e., an episulfide resin.
[0038] Examples of the polyfunctional epoxy compound include jER828, jER834, jER1001, and jER1004 manufactured by Japan Epoxy Resins Co., Ltd.; Epicron 840, Epicron 850, Epicron 1050, and Epicron 2055 manufactured by Dainippon Ink and Chemicals Co., Ltd.; Epotohto YD-011, YD-013, YD-127, and YD-128 manufactured by Tohto Kasei Co., Ltd.; DER317, DER331, DER661, and DER664 manufactured by The Dow Chemical Company; and Araldite from Chiba Specialty Chemicals. Bisphenol A type epoxy resins such as 6071, Araldite 6084, Araldite DY250, Araldite DY260, Sumi-Epoxy ESA-011, ESA-014, ELA-115, ELA-128 manufactured by Sumitomo Chemical Co., Ltd., AER330, AER331, AER661, AER664 manufactured by Asahi Kasei Corporation (all trade names); jERYL903 manufactured by Japan Epoxy Resins Co., Ltd., Epicron 152, Epicron 165 manufactured by Dainippon Ink and Chemicals, Inc., and Epotohto YD manufactured by Tohto Kasei Co., Ltd. Brominated epoxy resins such as B-400, YDB-500, DER542 manufactured by Dow Chemical Company, Araldite 8011 manufactured by Chiba Specialty Chemicals, Sumi-Epoxy ESB-400, ESB-700 manufactured by Sumitomo Chemical Co., Ltd., AER711, AER714 manufactured by Asahi Kasei Corporation (all trade names); jER152, jER154 manufactured by Japan Epoxy Resins Co., Ltd., DEN431, DEN438 manufactured by Dow Chemical Company, Epicron N-730, Epicron N-7 manufactured by Dainippon Ink and Chemicals Co., Ltd. 70, Epicron N-865, Epotohto YDCN-701 and YDCN-704 manufactured by Tohto Kasei Co., Ltd., Araldite ECN1235, Araldite ECN1273, Araldite ECN1299, and Araldite XPY307 manufactured by Chiba Specialty Chemicals Co., Ltd., EPPN-201, EOCN-1025, EOCN-1020, EOCN-104S, and RE-306 manufactured by Nippon Kayaku Co., Ltd., Sumi-Epoxy ESCN-195X and ESCN-220 manufactured by Sumitomo Chemical Co., Ltd., and AER manufactured by Asahi Kasei Co., Ltd.Novolac type epoxy resins such as ECN-235 and ECN-299 (all trade names); bisphenol F type epoxy resins such as Epicron 830 manufactured by Dainippon Ink and Chemicals, jER807 manufactured by Japan Epoxy Resins, Epototo YDF-170, YDF-175, YDF-2004 manufactured by Tohto Kasei, and Araldite XPY306 manufactured by Chiba Specialty Chemicals (all trade names); hydrogenated bisphenol A type epoxy resins such as Epototo ST-2004, ST-2007, ST-3000 (trade names) manufactured by Tohto Kasei; jER604 manufactured by Japan Epoxy Resins, and Glycidylamine type epoxy resins such as Epotohto YH-434 manufactured by Daicel Chemical Co., Ltd., Araldite MY720 manufactured by Chiba Specialty Chemicals Co., Ltd., and Sumi-Epoxy ELM-120 manufactured by Sumitomo Chemical Co., Ltd. (all trade names); hydantoin type epoxy resins such as Araldite CY-350 manufactured by Chiba Specialty Chemicals Co., Ltd. (all trade names); alicyclic epoxy resins such as Celloxide 2021 manufactured by Daicel Chemical Industries, Ltd., Araldite CY175 and CY179 manufactured by Chiba Specialty Chemicals Co., Ltd. (all trade names); YL-933 manufactured by Japan Epoxy Resins Co., Ltd., and TEN manufactured by Dow Chemical Co., Ltd.trihydroxyphenylmethane type epoxy resins such as EPPN-501, EPPN-502 (all trade names); bixylenol type or biphenol type epoxy resins or mixtures thereof such as YL-6056, YX-4000, YL-6121 (all trade names) manufactured by Japan Epoxy Resins Co., Ltd.; bisphenols such as EBPS-200 manufactured by Nippon Kayaku Co., Ltd., EPX-30 manufactured by Asahi Denka Kogyo Co., Ltd., and EXA-1514 (trade name) manufactured by Dainippon Ink and Chemicals, Inc. S-type epoxy resins; bisphenol A novolac type epoxy resins such as jER157S (trade name) manufactured by Japan Epoxy Resins; tetraphenylolethane type epoxy resins such as jERYL-931 manufactured by Japan Epoxy Resins and Araldite 163 manufactured by Ciba Specialty Chemicals (all trade names); complex epoxy resins such as Araldite PT810 manufactured by Ciba Specialty Chemicals and TEPIC manufactured by Nissan Chemical Industries (all trade names) Cyclic epoxy resins; diglycidyl phthalate resins such as Blenmer DDT manufactured by Nippon Oil & Fats Co., Ltd.; tetraglycidyl xylenoylethane resins such as ZX-1063 manufactured by Tohto Kasei Co., Ltd.; naphthalene group-containing epoxy resins such as ESN-190 and ESN-360 manufactured by Nippon Steel Chemical Co., Ltd., HP-4032, EXA-4750, and EXA-4700 manufactured by Dainippon Ink & Chemicals Co., Ltd.; dicyclopentadiene skeleton epoxy resins such as HP-7200 and HP-7200H manufactured by Dainippon Ink & Chemicals Co., Ltd. glycidyl methacrylate copolymer epoxy resins such as CP-50S and CP-50M manufactured by Nippon Oil & Fats Co., Ltd.; furthermore, cyclohexylmaleimide and glycidyl methacrylate copolymer epoxy resins; epoxy-modified polybutadiene rubber derivatives (e.g., PB-3600 manufactured by Daicel Chemical Industries, Ltd.), CTBN-modified epoxy resins (e.g., YR-102 and YR-450 manufactured by Tohto Kasei Co., Ltd.), etc., but are not limited thereto. These epoxy resins can be used alone or in combination of two or more kinds. Among these, novolac-type epoxy resins, modified novolac-type epoxy resins, heterocyclic epoxy resins, bixylenol-type epoxy resins, or mixtures thereof are particularly preferred.
[0039] Examples of the polyfunctional oxetane compound include polyfunctional oxetanes such as bis[(3-methyl-3-oxetanylmethoxy)methyl]ether, bis[(3-ethyl-3-oxetanylmethoxy)methyl]ether, 1,4-bis[(3-methyl-3-oxetanylmethoxy)methyl]benzene, 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, (3-methyl-3-oxetanyl)methyl acrylate, (3-ethyl-3-oxetanyl)methyl acrylate, (3-methyl-3-oxetanyl)methyl methacrylate, (3-ethyl-3-oxetanyl)methyl methacrylate, and oligomers or copolymers thereof, as well as ethers of oxetane alcohols with novolac resins, poly(p-hydroxystyrene), cardo-type bisphenols, calixarenes, calixresorcinarenes, or resins having a hydroxyl group such as silsesquioxane. Other examples include copolymers of unsaturated monomers having an oxetane ring and alkyl (meth)acrylates.
[0040] Examples of the episulfide resin having two or more cyclic thioether groups in the molecule include YL7000 (bisphenol A type episulfide resin) manufactured by Japan Epoxy Resins Co., Ltd. and YSLV-120TE manufactured by Tohto Kasei Co., Ltd. In addition, episulfide resins in which the oxygen atoms of the epoxy groups of novolac type epoxy resins are replaced with sulfur atoms using a similar synthesis method can also be used.
[0041] The amount of the thermosetting component is preferably 10 to 100 parts by mass per 100 parts by mass of the carboxyl group-containing resin. In particular, the amount of the thermosetting component having two or more cyclic (thio)ether groups in the molecule is preferably in the range of 0.6 to 2.5 equivalents, more preferably 0.8 to 2.0 equivalents, of the cyclic (thio)ether groups relative to 1 equivalent of the carboxyl group of the carboxyl group-containing resin. When the amount of the thermosetting component is within the above range, the heat resistance, alkali resistance, electrical insulation, strength of the cured coating, etc. are good.
[0042] Furthermore, the curable resin composition of the present invention may contain a binder polymer for the purpose of improving dryness to the touch, improving handling, etc. For example, a polyester-based polymer, a polyurethane-based polymer, a polyester urethane-based polymer, a polyamide-based polymer, a polyester amide-based polymer, an acrylic polymer, a cellulose-based polymer, a polylactic acid-based polymer, a phenoxy-based polymer, etc. may be used. These binder polymers may be used alone or in a mixture of two or more kinds.
[0043] Further, the curable resin composition of the present invention may further contain other elastomers for the purpose of imparting flexibility and improving the brittleness of the cured product. For example, polyester-based elastomers, polyurethane-based elastomers, polyester urethane-based elastomers, polyamide-based elastomers, polyester amide-based elastomers, acrylic-based elastomers, and olefin-based elastomers may be used. In addition, resins in which some or all of the epoxy groups of epoxy resins having various skeletons are modified with both-end carboxylic acid-modified butadiene-acrylonitrile rubber may also be used. Furthermore, epoxy-containing polybutadiene-based elastomers, acrylic-containing polybutadiene-based elastomers, and the like may also be used. These elastomers may be used alone or as a mixture of two or more kinds.
[0044] Furthermore, in the curable resin composition of the present invention, an organic solvent can be used for the synthesis of the carboxyl group-containing resin, for adjusting the composition, or for adjusting the viscosity for application to a substrate or carrier film. Examples of such organic solvents include ketones, aromatic hydrocarbons, glycol ethers, glycol ether acetates, esters, alcohols, aliphatic hydrocarbons, and petroleum-based solvents. More specifically, the organic solvents include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, diethylene glycol ethyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, and propylene glycol butyl ether acetate; alcohols such as ethanol, propanol, ethylene glycol, and propylene glycol; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha. These organic solvents are used alone or as a mixture of two or more kinds.
[0045] Generally, in many polymer materials, once oxidation begins, oxidative degradation occurs in a chain reaction, resulting in a decrease in the functionality of the polymer material. Therefore, in order to prevent oxidation, an antioxidant such as (1) a radical scavenger that neutralizes the generated radicals and / or (2) a peroxide decomposer that decomposes the generated peroxides into harmless substances and prevents new radicals from being generated can be added to the curable resin composition of the present invention.
[0046] Specific examples of antioxidants that act as radical scavengers include hydroquinone, 4-t-butylcatechol, 2-t-butylhydroquinone, hydroquinone monomethyl ether, 2,6-di-t-butyl-p-cresol, 2,2-methylene-bis(4-methyl-6-t-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, and 1,3,5-trimethyl-2,4 Examples of suitable amine compounds include phenols such as 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene and 1,3,5-tris(3',5'-di-t-butyl-4-hydroxybenzyl)-S-triazine-2,4,6-(1H,3H,5H)trione, quinone compounds such as methoquinone and benzoquinone, and amine compounds such as bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate and phenothiazine.
[0047] The radical scavenger may be a commercially available product, for example, ADK STAB AO-30, ADK STAB AO-330, ADK STAB AO-20, ADK STAB LA-77, ADK STAB LA-57, ADK STAB LA-67, ADK STAB LA-68, ADK STAB LA-87 (all of which are trade names manufactured by Asahi Denka Co., Ltd.), IRGANOX1010, IRGANOX1035, IRGANOX1076, IRGANOX1135, TINUVIN 111FDL, TINUVIN 123, TINUVIN 144, TINUVIN 152, TINUV Examples include IN 292 and TINUVIN 5100 (both are product names manufactured by Chiba Specialty Chemicals).
[0048] Specific examples of antioxidants that act as peroxide decomposers include phosphorus compounds such as triphenyl phosphite, and sulfur compounds such as pentaerythritol tetralauryl thiopropionate, dilauryl thiodipropionate, and distearyl 3,3'-thiodipropionate.
[0049] The peroxide decomposer may be a commercially available product, such as Adeka STAB TPP (trade name, manufactured by Asahi Denka Co., Ltd.), Mark AO-412S (trade name, manufactured by Adeka Argus Chemical Co., Ltd.), or Sumilizer TPS (trade name, manufactured by Sumitomo Chemical Co., Ltd.). The above antioxidants can be used alone or in combination of two or more.
[0050] Generally, polymeric materials absorb light, which causes decomposition and deterioration. Therefore, in order to provide stabilization against ultraviolet light, an ultraviolet absorber can be used in the curable resin composition of the present invention in addition to the above-mentioned antioxidant.
[0051] Examples of ultraviolet absorbers include benzophenone derivatives, benzoate derivatives, benzotriazole derivatives, triazine derivatives, benzothiazole derivatives, cinnamate derivatives, anthranilate derivatives, and dibenzoylmethane derivatives.Specific examples of benzophenone derivatives include 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-n-octoxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, and 2,4-dihydroxybenzophenone.Specific examples of benzoate derivatives include 2-ethylhexyl salicylate, phenyl salicylate, pt-butylphenyl salicylate, 2,4-di-t-butylphenyl-3,5-di-t-butyl-4-hydroxybenzoate, and hexadecyl-3,5-di-t-butyl-4-hydroxybenzoate. Specific examples of the benzotriazole derivative include 2-(2'-hydroxy-5'-t-butylphenyl)benzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 2-(2'-hydroxy-3',5'-di-t-amylphenyl)benzotriazole, etc. Specific examples of the triazine derivative include hydroxyphenyltriazine, bisethylhexyloxyphenol methoxyphenyltriazine, etc.
[0052] The ultraviolet absorbing agent may be a commercially available product, for example, TINUVIN PS, TINUVIN 99-2, TINUVIN 109, TINUVIN 384-2, TINUVIN 900, TINUVIN 928, TINUVIN 1130, TINUVIN 400, TINUVIN 405, TINUVIN 460, TINUVIN 479( The above are product names manufactured by Chiba Specialty Chemicals. The above ultraviolet absorbents can be used alone or in combination of two or more. By using them in combination with the antioxidant, the molded product obtained from the curable resin composition of the present invention can be stabilized.
[0053] In the curable resin composition of the present invention, known and commonly used chain transfer agents such as N-phenylglycines, phenoxyacetic acids, thiophenoxyacetic acids, mercaptothiazoles, etc. may be used to improve sensitivity. Specific examples of the chain transfer agent include chain transfer agents having a carboxyl group, such as mercaptosuccinic acid, mercaptoacetic acid, mercaptopropionic acid, methionine, cysteine, thiosalicylic acid, and derivatives thereof; chain transfer agents having a hydroxyl group, such as mercaptoethanol, mercaptopropanol, mercaptobutanol, mercaptopropanediol, mercaptobutanediol, hydroxybenzenethiol, and derivatives thereof; 1-butanethiol, butyl-3-mercaptopropionate, methyl-3-mercaptopropionate, 2,2-(ethylenedioxy)diethanethiol, ethanethiol, 4-methylbenzenethiol, dodecyl mercaptan, propanethiol, butanethiol, pentanethiol, 1-octanethiol, cyclopentanethiol, cyclohexanethiol, thioglycerol, and 4,4-thiobisbenzenethiol.
[0054] In addition, polyfunctional mercaptan compounds can be used, and examples thereof include, but are not limited to, aliphatic thiols such as hexane-1,6-dithiol, decane-1,10-dithiol, dimercaptodiethyl ether, and dimercaptodiethyl sulfide; aromatic thiols such as xylylene dimercaptan, 4,4'-dimercaptodiphenyl sulfide, and 1,4-benzenedithiol; ethylene glycol bis(mercaptoacetate), polyethylene glycol bis(mercaptoacetate), and polyolefins. poly(mercaptoacetates) of polyhydric alcohols such as ethylene glycol bis(mercaptoacetate), propylene glycol bis(mercaptoacetate), glycerin tris(mercaptoacetate), trimethylolethane tris(mercaptoacetate), trimethylolpropane tris(mercaptoacetate), pentaerythritol tetrakis(mercaptoacetate), and dipentaerythritol hexakis(mercaptoacetate); Ethylene glycol bis(3-mercaptopropionate), polyethylene glycol bis(3-mercaptopropionate), propylene glycol bis(3-mercaptopropionate), glycerin tris(3-mercaptopropionate), trimethylolethane tris(mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptopropionate), di Poly(3-mercaptopropionates) of polyhydric alcohols such as pentaerythritol hexakis(3-mercaptopropionate); poly(mercaptobutyrates) such as 1,4-bis(3-mercaptobutyryloxy)butane, 1,3,5-tris(3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, and pentaerythritol tetrakis(3-mercaptobutyrate) can be used. Examples of commercially available products of these include BMPA, MPM, EHMP, NOMP, MBMP, STMP, TMMP, PEMP, DPMP, and TEMPIC (all manufactured by Sakai Chemical Industry Co., Ltd.), Karenz MT-PE1, Karenz MT-BD1, and Karenz-NR1 (all manufactured by Showa Denko K.K.), and the like.
[0055] Further, examples of heterocyclic compounds having a mercapto group that act as a chain transfer agent include mercapto-4-butyrolactone (also known as 2-mercapto-4-butanolide), 2-mercapto-4-methyl-4-butyrolactone, 2-mercapto-4-ethyl-4-butyrolactone, 2-mercapto-4-butyrothiolactone, 2-mercapto-4-butyrolactam, N-methoxy-2-mercapto-4-butyrolactam, N-ethoxy-2-mercapto-4-butyrolactam, N-methyl-2-mercapto-4-butyrolactam, N-ethyl-2-mercapto-4-butyrolactam, N-(2-methoxy)ethyl-2-mercapto-4- Butyrolactam, N-(2-ethoxy)ethyl-2-mercapto-4-butyrolactam, 2-mercapto-5-valerolactone, 2-mercapto-5-valerolactam, N-methyl-2-mercapto-5-valerolactam, N-ethyl-2-mercapto-5-valerolactam, N-(2-methoxy)ethyl-2-mercapto-5-valerolactam, N-(2-ethoxy)ethyl-2-mercapto-5-valerolactam, 2-mercaptobenzothiazole, 2-mercapto-5-methylthio-thiadiazole, 2-mercapto-6-hexanolactam, 2,4,6-trimercapto-s-triazine (manufactured by Sankyo Kasei Co., Ltd.: trade name) Examples of the s-triazine include 2-dibutylamino-4,6-dimercapto-s-triazine (manufactured by Sankyo Kasei Co., Ltd.: trade name: Jisnet DB), 2-anilino-4,6-dimercapto-s-triazine (manufactured by Sankyo Kasei Co., Ltd.: trade name: Jisnet AF).
[0056] In particular, as a heterocyclic compound having a mercapto group, which is a chain transfer agent that does not impair the developability of the curable resin composition, mercaptobenzothiazole, 3-mercapto-4-methyl-4H-1,2,4-triazole, 5-methyl-1,3,4-thiadiazole-2-thiol, and 1-phenyl-5-mercapto-1H-tetrazole are preferred. These chain transfer agents can be used alone or in combination of two or more kinds.
[0057] In the curable resin composition of the present invention, an adhesion promoter can be used to improve the adhesion between layers or between a resin layer and a substrate.Specific examples include benzimidazole, benzoxazole, benzothiazole, 2-mercaptobenzimidazole, 2-mercaptobenzoxazole, 2-mercaptobenzothiazole (product name: Accel M manufactured by Kawaguchi Chemical Industry Co., Ltd.), 3-morpholinomethyl-1-phenyl-triazole-2-thione, 5-amino-3-morpholinomethyl-thiazole-2-thione, 2-mercapto-5-methylthio-thiadiazole, triazole, tetrazole, benzotriazole, carboxybenzotriazole, amino group-containing benzotriazole, and silane coupling agents.
[0058] When using a thermosetting component having two or more cyclic (thio) ether groups in the molecule, the curable resin composition of the present invention preferably contains a thermosetting catalyst. Examples of such a thermosetting catalyst include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and phosphorus compounds such as triphenylphosphine. In addition, examples of commercially available products include 2MZ-A, 2MZ-OK, 2PHZ, 2P4BHZ, and 2P4MHZ (all trade names of imidazole-based compounds) manufactured by Shikoku Chemical Industry Co., Ltd., and U-CAT (registered trademark) 3503N and U-CAT3502T (all trade names of dimethylamine blocked isocyanate compounds), DBU, DBN, U-CATSA102, and U-CAT5002 (all bicyclic amidine compounds and their salts) manufactured by San-Apro Co., Ltd. In particular, the present invention is not limited to these, and any heat curing catalyst for epoxy resins or oxetane compounds, or one that promotes the reaction of epoxy groups and / or oxetanyl groups with carboxyl groups may be used alone or in combination of two or more kinds. Also usable are S-triazine derivatives such as guanamine, acetoguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine·isocyanuric acid adduct, and 2,4-diamino-6-methacryloyloxyethyl-S-triazine·isocyanuric acid adduct. It is preferable to use such compounds that also function as adhesion-imparting agents in combination with the heat curing catalyst.
[0059] The amount of these thermosetting catalysts to be added is sufficient in a normal quantitative ratio, and is, for example, preferably 0.1 to 20 parts by mass, more preferably 0.5 to 15.0 parts by mass, relative to the carboxyl group-containing resin.
[0060] The curable resin composition of the present invention can be blended with fillers other than hollow silica within a range that does not adversely affect the properties. As such fillers, known and commonly used inorganic or organic fillers can be used, and barium sulfate, spherical silica, and talc are particularly preferred. Furthermore, in order to obtain a white appearance and flame retardancy, metal oxides such as titanium oxide and metal hydroxides such as aluminum hydroxide can also be used as extender pigment fillers.
[0061] The curable resin composition of the present invention may further contain, as necessary, a thixotropic agent such as fine silica, organic bentonite, montmorillonite, or hydrotalcite. As a thixotropic agent, organic bentonite and hydrotalcite are preferred in terms of stability over time, and hydrotalcite is particularly excellent in electrical properties. In addition, known and commonly used additives such as thermal polymerization inhibitors, silicone-based, fluorine-based, and polymer-based defoamers and / or leveling agents, imidazole-based, thiazole-based, and triazole-based silane coupling agents, colorants, rust inhibitors, and copper damage inhibitors such as bisphenol-based and triazinethiol-based agents may also be added.
[0062] The thermal polymerization inhibitor can be used to prevent the thermal polymerization or polymerization over time of the polymerizable compound. Examples of the thermal polymerization inhibitor include 4-methoxyphenol, hydroquinone, alkyl or aryl substituted hydroquinone, t-butylcatechol, pyrogallol, 2-hydroxybenzophenone, 4-methoxy-2-hydroxybenzophenone, cuprous chloride, phenothiazine, chloranil, naphthylamine, β-naphthol, 2,6-di-t-butyl-4-cresol, 2,2'-methylenebis(4-methyl-6-t-butylphenol), pyridine, nitrobenzene, dinitrobenzene, picric acid, 4-toluidine, methylene blue, a reaction product of copper and an organic chelating agent, methyl salicylate, and phenothiazine, a nitroso compound, and a chelate of a nitroso compound and Al.
[0063] [Cured film (cured product)] The curable resin composition of the present invention is adjusted to a viscosity suitable for the coating method using the organic solvent, and applied to a substrate by a method such as dip coating, flow coating, roll coating, bar coating, screen printing, or curtain coating, and the organic solvent contained in the composition is evaporated and dried (temporarily dried) at a temperature of about 60 to 100 ° C., thereby forming a tack-free dried coating film. Thereafter, the composition is selectively exposed to active energy rays through a photomask having a pattern formed thereon by a contact method (or a non-contact method), or directly exposed to a pattern by a laser direct exposure machine, and the unexposed area is developed with an alkaline aqueous solution (e.g., a 0.3 to 3% aqueous solution of sodium carbonate) to form a resist pattern. Furthermore, the thermosetting component is heated to a temperature of, for example, about 130 to 180 ° C. for thermal curing, whereby the carboxyl group-containing resin and the thermosetting component react to form a cured coating film having excellent properties such as heat resistance, chemical resistance, moisture absorption resistance, adhesion, and electrical properties.
[0064] Examples of the substrate that can be used include printed wiring boards and flexible printed wiring boards with pre-formed circuits, as well as paper-phenolic resin, paper-epoxy resin, glass cloth-epoxy resin, glass-polyimide, glass cloth / nonwoven cloth-epoxy resin, glass cloth / paper-epoxy resin, synthetic fiber-epoxy resin, copper-clad laminates of all grades (e.g., FR-4) made of composite materials such as fluororesin, polyethylene, PPO, cyanate, etc., polyimide films, PET films, glass substrates, ceramic substrates, wafer plates, etc.
[0065] The volatilization drying carried out after application of the curable resin composition of the present invention can be carried out using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, or the like (a method in which hot air in a dryer equipped with a heat source of an air heating method using steam is brought into countercurrent contact with the substrate, or a method in which hot air is blown onto the substrate from a nozzle).
[0066] The curable resin composition of the present invention is applied and volatilized and dried as described below, and then the resulting coating film is exposed (irradiated with active energy rays). The exposed portion (portion irradiated with active energy rays) of the coating film is cured. The exposure machine used for the above-mentioned active energy ray irradiation may be a direct imaging machine (e.g., a laser direct imaging machine that directly draws an image with a laser based on CAD data from a computer), an exposure machine equipped with a metal halide lamp, an exposure machine equipped with a (ultra) high pressure mercury lamp, an exposure machine equipped with a mercury short arc lamp, or a direct imaging machine using an ultraviolet lamp such as an (ultra) high pressure mercury lamp.
[0067] The developing method can be a dipping method, a shower method, a spray method, a brush method, or the like, and the developing solution can be an aqueous alkali solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines, or the like.
[0068] [Dry film] The curable resin composition of the present invention can be used in the form of a dry film having a resin layer formed by applying the curable resin composition to a film such as polyethylene terephthalate in advance and drying the composition, other than the method of directly applying the composition to a substrate in liquid form. The case where the curable resin composition of the present invention is used as a dry film is described below.
[0069] The dry film has a structure in which a first film, a resin layer, and a peelable second film used as needed are laminated in this order. The resin layer is a layer obtained by applying the curable resin composition of the present invention to the first film and drying it. After forming the resin layer on the first film, a second film is laminated thereon as needed to obtain a dry film.
[0070] As the first film, a thermoplastic film such as a polyester film having a thickness of 2 to 150 μm is used. The resin layer is formed by uniformly applying the curable resin composition to a carrier film or a cover film with a blade coater, lip coater, comma coater, film coater or the like to a thickness of 10 to 150 μm, and drying the applied composition. As the second film, a polyethylene film, a polypropylene film, or the like can be used, but it is preferable that the adhesive strength with the resin layer is smaller than that of the carrier film.
[0071] To prepare a cured coating on a printed wiring board using a dry film, the second film is peeled off, the resin layer and the substrate on which the circuit is formed are superimposed, and the substrate is laminated using a laminator or the like to form a resin layer on the substrate on which the circuit is formed. The formed resin layer is exposed to light, developed, and cured by heating in the same manner as described above to form a cured coating. The first film may be peeled off either before or after exposure.
[0072] [Printed wiring board] The curable resin composition of the present invention is used to form a cured coating on a printed wiring board. The cured coating is preferably a development-type permanent insulating coating, and is particularly preferably a development-type solder resist or coverlay. The curable resin composition of the present invention may be used as an interlayer insulating material, a hole filling material, or a material for forming a solder dam. EXAMPLES
[0073] The present invention will be specifically described below with reference to examples and comparative examples, but it goes without saying that the present invention is not limited to the following examples. In the following, "parts" and "%" are all based on mass unless otherwise specified.
[0074] Synthesis Example 1 Into an autoclave equipped with a thermometer, a nitrogen introduction device / alkylene oxide introduction device, and a stirrer, 119.4 g of novolac cresol resin (manufactured by Showa Polymer Co., Ltd., product name "Shonoru CRG951", OH equivalent: 119.4), 1.19 g of potassium hydroxide, and 119.4 g of toluene were charged, and the system was replaced with nitrogen while stirring, and heated to increase the temperature. Next, 63.8 g of propylene oxide was gradually added dropwise, and the temperature was adjusted to 125-132°C and 0-4.8 kg / cm. 2 The mixture was reacted at 40° C. for 16 hours. After that, it was cooled to room temperature, and 1.56 g of 89% phosphoric acid was added to the reaction solution to neutralize the potassium hydroxide, to obtain a propylene oxide reaction solution of novolac cresol resin with a non-volatile content of 62.1% and a hydroxyl value of 182.2 g / eq. This had an average of 1.08 moles of alkylene oxide added per equivalent of phenolic hydroxyl group. Next, 293.0g of the alkylene oxide reaction solution of the obtained novolac cresol resin, 43.2g of acrylic acid, 11.53g of methanesulfonic acid, 0.18g of methylhydroquinone, and 252.9g of toluene were charged into a reactor equipped with a stirrer, a thermometer, and an air inlet tube, and the mixture was reacted at 110°C for 12 hours while blowing air at a rate of 10ml / min and stirring. The water generated by the reaction was distilled as an azeotropic mixture with toluene, and 12.6g of water was distilled. After that, the mixture was cooled to room temperature, and the obtained reaction solution was neutralized with 35.35g of 15% aqueous sodium hydroxide solution, and then washed with water. After that, the toluene was distilled off while replacing it with 118.1g of diethylene glycol monoethyl ether acetate in an evaporator, and a novolac acrylate resin solution was obtained. Next, 332.5g of the obtained novolac type acrylate resin solution and 1.22g of triphenylphosphine were charged into a reactor equipped with a stirrer, a thermometer, and an air inlet tube, and 60.8g of tetrahydrophthalic anhydride was gradually added while blowing air at a rate of 10ml / min and stirring, and the reaction was carried out at 95 to 101°C for 6 hours. A resin solution of a carboxyl group-containing photosensitive resin with an acid value of 88mgKOH / g of solid matter and a non-volatile content of 71% was obtained. Hereinafter, this is referred to as a carboxyl group-containing resin.
[0075] The various components shown in Table 1 below were blended in the ratios (parts by mass) shown in Table 1, premixed with a stirrer, and then kneaded with a three-roll mill to prepare a curable resin composition. The average particle size D50 of the hollow filler was measured using a laser diffraction / scattering type particle size distribution measuring device ("Microtrac MT3200II" manufactured by Nikkiso Co., Ltd.
[0076] [Table 1]
[0077] In Table 1, the carboxyl group-containing resin was that of Synthesis Example 1 described above. The photoinitiator was IRGACURE 907 (2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one) manufactured by BASF. The hollow filler was hollow silica (average particle size D50 of 0.5 μm, porosity of 40%). The photopolymerizable monomer was NK Ester A-TMPT (trimethylolpropane triacrylate) manufactured by Shin-Nakamura Kogyo. The thermal curing catalyst was DICY (dicyandiamide). Thermosetting component 1 was N-660 (cresol novolac type epoxy resin, epoxy equivalent weight 202-212 g / eq) manufactured by DIC Corporation. Thermosetting component 2 was jER828 (bisphenol A type epoxy resin, epoxy equivalent 184-194 g / eq) manufactured by Japan Epoxy Resins. Colorant 1 was CI Pigment Blue 15:3. Colorant 2 was CI Pigment Yellow 147. The defoaming agent was FLOWLEN AC-902, a silicone-based defoaming agent manufactured by Kyoeisha Chemical Co., Ltd. The other filler was SFP-130MC manufactured by Denka.
[0078] <Preparation of evaluation board> Each of the curable resin compositions of the Examples and Comparative Examples in Table 1 was applied to a copper foil having a thickness of 0.018 μm, which had been buff-roll polished, washed with water, and dried, by screen printing twice on the entire surface with a 100 mesh to a film thickness of 50 to 65 μm, and then dried for 30 minutes in a hot air circulation drying oven at 80°C. After that, ultraviolet light with a wavelength of 365 nm was applied at 400 mJ / cm using an integrating light meter manufactured by Oak Seisakusho Co., Ltd. 2 The light was irradiated at a spray pressure of 2kg / cm 2 The resist was developed for 60 seconds in a developer (aqueous sodium carbonate solution) and then heat-cured for 60 minutes in a 150° C. hot air circulating drying oven to obtain a sample for measuring the dielectric constant Dk and dielectric tangent Df.
[0079] <Measurement of dielectric constant Dk and dielectric tangent Df> Using the evaluation substrate obtained in <Preparation of Evaluation Sample>, the dielectric constant Dk and dielectric loss tangent Df at 10 GHz were measured in accordance with JIS K6911: 1995. The measurement results are shown in Table 1.
[0080] <Calculation of void ratio in cured coating film> The copper foil was peeled off from the evaluation sample obtained in <Preparation of Evaluation Sample> to obtain the cured coating film (cured product) of the curable resin composition of Examples 1-2 and Comparative Examples 1-2. The cured coating film of the curable resin composition of Examples 1-2 and Comparative Examples 1-2 was cut into two pieces each measuring 5 cm x 8 cm. The thickness of the cut-out cured coating film of each curable resin composition was measured. The two pieces of the cut-out cured coating film of each curable resin composition were stacked so that the entire surfaces of the cut-out cured coating film were overlapped, and the density of the cured coating film was calculated from the weight and volume of the stacked cured coating films of each curable resin composition according to the following formula. TIFF2024139464000002.tif18160The true density of the hollow silica was measured separately by a gas displacement method. The porosity in the cured coating was calculated by the following formula based on the density of the cured coating film described above, the true density of the hollow silica, the weight ratio of the hollow silica in the cured coating film, and the porosity of the hollow silica (Examples 1-2: 40%, Comparative Examples 1-2: 0%). Note that in Comparative Examples 1-2, the porosity of the hollow silica was 0%, so the porosity in the cured coating film was set to 0%. The calculation results obtained are shown in Table 1. TIFF2024139464000003.tif26164
[0081] As is clear from Table 1, the curable resin compositions of Examples 1 and 2 had low dielectric constants and low dielectric tangents. In this example, an example was shown in which the porosity of the cured product was set to a range of 5 to 15 volume % by using a hollow filler. However, it was confirmed that the porosity of the cured product can also be set to a range of 5 to 15 volume % by using a foaming agent instead of a hollow filler.
Claims
1. A cured product of the curable resin composition, The porosity of the cured product is 5% by volume or more and 15% by volume or less. cured product.
2. A curable resin composition used for the cured product according to claim 1, Carboxyl group-containing resin, A photoinitiator, and Hollow filler, A curable resin composition comprising:
3. The curable resin composition of claim 2 , wherein the hollow filler comprises silica.
4. The amount of the hollow filler is 250 parts by mass or less per 100 parts by mass of the carboxyl group-containing resin; The curable resin composition according to claim 2.
5. The hollow filler has an average particle size D50 of 0.1 to 110 μm. The curable resin composition according to claim 2.
6. The curable resin composition according to claim 2, wherein the hollow filler has a porosity of 30 to 50 volume %.
7. The curable resin composition according to claim 2 , further comprising a photopolymerizable monomer.
8. A dry film obtained by applying the curable resin composition according to any one of claims 2 to 7 to a first film and drying the applied film.
9. A cured product obtained by curing the dry film according to claim 8 .
10. A printed wiring board comprising the cured product according to claim 1 or 9.
Citation Information
Patent Citations
Photosensitive resin composition, dry film solder resist, and circuit board
JP2013539072A
Cited By
Substrate processing method and substrate processing apparatus
EP4621834A2