Polyamic acid, polyamic acid composition, polyimide, polyimide film, and printed circuit board
A polyamic acid composition with a fluorene and dimer diamine combination addresses the high dielectric and film-forming issues of existing polyimides, resulting in a polyimide with low dielectric properties and improved film-forming capabilities for high-speed communication applications.
Patent Information
- Application Number
- JP2023050565
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polyimides used in high-frequency printed wiring boards suffer from high dielectric properties, leading to signal delays and heat generation, and often have insufficient film-forming properties, limiting their performance in high-speed communication applications.
A polyamic acid composition is developed using a diamine with a fluorene skeleton and a dimer diamine, combined with tetracarboxylic dianhydride, to create a polyimide with low dielectric properties and improved film-forming capabilities.
The resulting polyimide exhibits low dielectric properties, high heat resistance, and good film-forming properties, enabling the production of polyimide films suitable for high-speed signal transmission and flexible printed wiring boards.
Smart Images

Figure 2024139565000001 
Figure 2024139565000002 
Figure 2024139565000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyamic acid capable of forming a polyimide exhibiting low dielectric properties and high heat resistance and having good film-formability, and to a polyamic acid composition, polyimide, polyimide film, and printed wiring board produced using the same. [Background technology]
[0002] High dielectric strength and heat resistance are required for insulating materials used in mobile communication devices such as smartphones and tablets, and electronic devices such as computers and car navigation systems. Polyimide is a polymer formed by imidizing polyamic acid, which is generally synthesized from acid dianhydride and aromatic diamine compound, and is widely used as such insulating material due to its excellent heat resistance, mechanical properties, and insulating properties.
[0003] In recent years, the development of high-speed, large-capacity printed wiring boards for next-generation high-frequency wireless has been underway, and the adoption of circuit boards with multilayer wiring structures has made high-speed signal transmission possible. Polyimide is used as an interlayer insulating film in multilayer wiring structures, but typical polyimide has high dielectric properties such as dielectric constant, which causes delays in signal transmission and hinders speed increases. Furthermore, a high dielectric constant increases the electrostatic capacitance, so when used for high-speed (high-frequency) communication, the wiring near the insulating film heats up, which can cause failure of the printed wiring board.
[0004] In order to meet such high frequencies, there is an increasing demand for polyimides that exhibit low dielectric properties. For example, Patent Document 1 discloses that a polyimide prepared using an aromatic diamine having a specific structure and a tetracarboxylic dianhydride exhibits a low dielectric constant and is also excellent in heat resistance.
[0005] Also, a method is known in which the imide group concentration is reduced by introducing a fluorene skeleton into a diamine component, the polarity of the entire molecule is reduced, and the dielectric constant of the polyimide is reduced. For example, Patent Document 2 discloses that a polyimide using trimellitic anhydride chloride as the acid anhydride and 9,9-bis(4-aminophenyl)fluorene as the diamine exhibits high heat resistance and low relative dielectric constant.
[0006] However, polyamic acid compositions having a fluorene skeleton generally tend to have insufficient film-forming properties, and may not be able to obtain polyimide films having good properties. Therefore, it is desired to provide a polyamic acid that can form polyamides having high heat resistance and low dielectric properties, as well as exhibit good film-forming properties. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 10-152559 [Patent Document 2] JP 2005-298625 A Summary of the Invention [Problem to be solved by the invention]
[0008] In view of the above circumstances, an object of the present invention is to provide a polyamic acid capable of forming a polyimide exhibiting low dielectric properties and high heat resistance and having good film-formability, as well as a polyamic acid composition, a polyimide, a polyimide film, and a printed wiring board produced using the same. [Means for solving the problem]
[0009] An embodiment of the present invention is a polyamic acid which is a polyaddition reaction product of (A) a tetracarboxylic dianhydride and (B) at least two diamines, the (B) at least two diamines including (B1) a diamine having a fluorene skeleton and (B2) a dimer diamine.
[0010] In one embodiment of the present invention, the (B1) diamine having a fluorene skeleton has a structure represented by the following formula (1). [ka] (In formula (1), R 1 ~R 4 each independently represents a hydrogen atom, a halogen atom, a C1-C8 alkyl group, or a C1-C8 halogenated alkyl group.
[0011] Another embodiment of the present invention is a polyamic acid composition containing the above polyamic acid and (C) an organic solvent.
[0012] Another embodiment of the present invention is a polyimide obtained by imidizing the above polyamic acid.
[0013] Another aspect of the present invention is a polyimide film comprising the above polyimide.
[0014] Another aspect of the present invention is a printed wiring board comprising the above-mentioned polyimide film. Effect of the Invention
[0015] According to the present invention, it is possible to provide a polyamic acid capable of forming a polyimide exhibiting low dielectric properties and high heat resistance and having good film-formability, as well as a polyamic acid composition, a polyimide, a polyimide film, and a printed wiring board produced using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present invention will be described in detail. The polyamic acid of the present invention is a polyaddition reaction product of (A) tetracarboxylic dianhydride and (B) at least two diamines, and the at least two diamines (B) include (B1) a diamine having a fluorene skeleton and (B2) a dimer diamine. That is, the polyamic acid of the present invention and the polyimide formed therefrom have a fluorene skeleton and a dimer skeleton. When only a diamine having a fluorene skeleton is included as a diamine component, the polyamic acid is not given sufficient film-forming properties, and on the other hand, when only a diamine having a dimer skeleton is included as a diamine component, although a polyimide exhibiting low dielectric properties can be formed, the polyimide is not given sufficient heat resistance and the mechanical properties are also inferior. In the present invention, since the polyamic acid has both a fluorene skeleton and a dimer skeleton, a polyamide exhibiting low dielectric properties and high heat resistance can be formed, and the insufficient film-forming properties of the polyamic acid derived from the fluorene skeleton are improved, and a polyamic acid exhibiting good film-forming properties can be realized.
[0017] (A) Tetracarboxylic acid dianhydride The polyamic acid of the present invention has a structural unit derived from a tetracarboxylic dianhydride in the molecule as an acid dianhydride component. The tetracarboxylic dianhydride may be any of an alicyclic tetracarboxylic dianhydride, an aromatic tetracarboxylic dianhydride, and an aliphatic tetracarboxylic dianhydride, and has two acid anhydride groups in one molecule. The tetracarboxylic dianhydride may be used alone or in combination of two or more kinds.
[0018] Examples of the alicyclic tetracarboxylic dianhydride include 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-cyclopentane tetracarboxylic dianhydride, 3-carboxymethylcyclopentane-1,2,4-tricarboxylic dianhydride, 1,2,3,4-cyclohexane tetracarboxylic dianhydride, 1,2,4,5-cyclohexane tetracarboxylic dianhydride, bicyclo[2.2.1]heptane tetracarboxylic dianhydride, bicyclo[2.2.1]heptane-5-carboxymethyl-2,3,6-tricarboxylic dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, bicyclo[2.2.2]octane-2,3,5,6-tetracarboxylic dianhydride, pentacyclo[8.2.1.1 4,7 .0 2,9 .0 3,8 ]tetradecane-5,6,11,12-tetracarboxylic dianhydride, 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, bicyclo[2.2.1]heptane-2-carboxymethyl-2,5,6-tricarboxylic dianhydride, bicyclo[2.2.2]octane-2-carboxyethyl-2,5,6-tricarboxylic dianhydride, 3,3',4,4'-dicyclohexyltetracarboxylic dianhydride, and derivatives thereof.
[0019] Examples of aromatic tetracarboxylic dianhydrides include 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, pyromellitic dianhydride, 2,2',3,3'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 2,2',3,3'-biphenyl tetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 2,2-bis(3,4-dicarboxyphenoxyphenyl)propane dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, and 1,2-bis(2,3-dicarboxyphenyl)ethane dianhydride. , 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,2-bis(3,4-dicarboxyphenyl)ethane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, 4,4'-(p-phenylenedioxy)diphthalic dianhydride, 4,4'-(m-phenylenedioxy)diphthalic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 1,2-ethylene bis(anhydrotrimellitate), 1,4-phenylene bis(anhydrotrimellitate), 1,3,3a,4,5,9b-hexahydro-5(tetrahydro-2,5-dioxo-3-furanyl)naphtho[1,2-c]furan-1,3-dione, and derivatives thereof.
[0020] Examples of the aliphatic tetracarboxylic dianhydride include 1,2,3,4-butanetetracarboxylic dianhydride, 1,2,3,4-pentanetetracarboxylic dianhydride, and derivatives thereof.
[0021] Of these tetracarboxylic dianhydrides, the acid dianhydride component is preferably an aromatic tetracarboxylic dianhydride, and among aromatic tetracarboxylic dianhydrides, pyromellitic dianhydride is preferred.
[0022] (B) Diamine The polyamic acid of the present invention has, as a diamine component, structural units derived from at least two diamines, one of which has a structural unit derived from a diamine having a fluorene skeleton (B1). Such a diamine having a fluorene skeleton preferably has a structure represented by the following formula (1). In formula (1), R 1 ~R 4 R each independently represents a hydrogen atom, a halogen atom, a C1-C8 alkyl group, or a C1-C8 halogenated alkyl group. 1 ~R 4 may be the same or different.
[0023] [ka]
[0024] The C1-C8 alkyl group is preferably a C1-C4 alkyl group, more preferably an ethyl group or a methyl group, and even more preferably a methyl group. The halogen atom is a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom, and is preferably a fluorine atom or a chlorine atom. Examples of the C1-C8 halogenated alkyl group include halogenated alkyl groups in which the hydrogen atom of the above C1-C8 alkyl group is substituted with the above halogen atom.
[0025] R 1 ~R 4 is preferably a hydrogen atom or a C1 to C8 alkyl group, and R 1 ~R 4 It is particularly preferable that all of are hydrogen atoms.
[0026] A preferred example of the diamine having a fluorene skeleton represented by formula (1) is a compound represented by the following formula (1-1), that is, 9,9-bis(4-aminophenyl)fluorene.
[0027] [ka]
[0028] The polyamic acid of the present invention has a structural unit derived from (B2) dimer diamine as another diamine component. Here, dimer diamine means an aliphatic diamine in which two terminal carboxylic acid groups (-COOH) of a cyclic or acyclic dimer acid obtained as a dimer of an unsaturated fatty acid are substituted with a primary aminomethyl group (-CH2-NH2) or an amino group (-NH2). The polyamic acid has a structural unit derived from dimer diamine, so that the obtained polyimide can be given low dielectric properties. The dimer diamine may be used alone or in combination of two or more kinds.
[0029] Dimer acid is a dibasic acid obtained by intermolecular polymerization of unsaturated fatty acids. Aliphatic diamines derived from dimer acids can be obtained by polymerizing unsaturated fatty acids such as oleic acid, linoleic acid, and linolenic acid to obtain dimer acids, reducing the dimer acids, and then aminating them. Such dimer diamines are preferably diamine compounds obtained by substituting the terminal carboxylic acid groups of dibasic acid compounds having carbon atoms in the range of 18 to 54, preferably 22 to 44, with primary aminomethyl groups or amino groups.
[0030] Commercially available dimer diamine products include "VERSAMINE (registered trademark) 551" and "VERSAMINE (registered trademark) 552" manufactured by Cognics Japan, and "PRIAMINE (registered trademark) 1073", "PRIAMINE (registered trademark) 1074", and "PRIAMINE (registered trademark) 1075" manufactured by Croda Japan.
[0031] In the polyamic acid of the present invention, the molar ratio of the diamine having a fluorene skeleton (B1) to the total diamine components is not particularly limited, but is preferably 0.25 or more, and more preferably 0.50 or more.
[0032] The molar ratio of the diamine to the tetracarboxylic dianhydride [(B) / (A)] is not particularly limited, but is preferably 0.90 to 1.10, more preferably 0.95 to 1.05, even more preferably 0.97 to 1.03, and particularly preferably 0.98 to 1.02.
[0033] <Polyamic Acid and Polyamic Acid Composition> (C) Organic Solvent The polyamic acid of the present invention can be synthesized by a known general method. For example, a polyamic acid composition (polyamic acid solution) can be obtained by reacting a tetracarboxylic acid with a diamine in an organic solvent (C). The organic solvent used for the polymerization of the polyamic acid is not particularly limited as long as it can dissolve the tetracarboxylic dianhydride and diamine as monomer components and dissolve the polyamic acid produced by the polyaddition reaction. Examples of such organic solvents include urea-based solvents such as tetramethylurea and N,N-dimethylethylurea; sulfone-based solvents such as dimethylsulfoxide, diphenylsulfone, and tetramethylsulfone; amide-based solvents such as N,N-dimethylacetamide, N,N-dimethylformamide, N,N'-diethylacetamide, N-methyl-2-pyrrolidone, and hexamethylphosphoric acid triamide; ester-based solvents such as γ-butyrolactone; halogenated alkyl solvents such as chloroform and methylene chloride; aromatic hydrocarbon-based solvents such as benzene and toluene; phenol-based solvents such as phenol and cresol; ketone-based solvents such as cyclopentanone; and ether-based solvents such as tetrahydrofuran, 1,3-dioxolane, 1,4-dioxane, dimethyl ether, diethyl ether, and p-cresol methyl ether. These organic solvents may be used alone or in combination of two or more. From the viewpoint of increasing the solubility and reactivity of the polyamic acid, the organic solvent is preferably selected from the group consisting of amide solvents, ketone solvents, ester solvents, and ether solvents, and amide solvents such as N,N-dimethylacetamide, N,N-dimethylformamide, N,N'-diethylacetamide, and N-methyl-2-pyrrolidone are preferred.
[0034] The molecular weight of the polyamic acid can be adjusted by adjusting the molar ratio between the total number of moles of the tetracarboxylic dianhydride components and the total number of moles of the diamine components. The molecular weight (weight average molecular weight) of the polyamic acid is not particularly limited, but is preferably 10,000 or more and 100,000 or less from the viewpoint of solubility in organic solvents. The weight average molecular weight of the polyamic acid can be determined, for example, from a standard polystyrene-equivalent value measured by gel permeation chromatography (GPC).
[0035] The synthesis of polyamic acid by the polyaddition reaction of tetracarboxylic dianhydride and diamine is preferably carried out in an inert atmosphere such as argon or nitrogen. In an inert atmosphere, the polyaddition reaction proceeds by dissolving the tetracarboxylic dianhydride and the diamine in an organic solvent and mixing them. The order of addition of the tetracarboxylic dianhydride and the diamine is not particularly limited. For example, the diamine may be dissolved or dispersed in a slurry in an organic solvent to prepare a diamine solution, and the tetracarboxylic dianhydride may be added to the diamine solution. The tetracarboxylic dianhydride and the diamine may be added directly to the organic solvent in a solid state, or may be added in a state of being dissolved or dispersed in a slurry in an organic solvent separately.
[0036] The temperature conditions for the polyaddition reaction are not particularly limited, but from the viewpoint of suppressing a decrease in the molecular weight of the polyamic acid due to depolymerization, the reaction temperature is preferably 100° C. or less, and from the viewpoint of allowing the polyaddition reaction to proceed appropriately, the reaction temperature is more preferably 20 to 80° C. The reaction time may be set arbitrarily within the range of 1 to 72 hours, and may be allowed to stand overnight at room temperature as necessary.
[0037] The viscosity of the solution when preparing the polyamic acid composition of the present invention is preferably 500 mPa·s or more from the viewpoint of film-forming properties. The concentration of the polyamic acid in the polyamic acid composition of the present invention is preferably 15% by mass or more, more preferably 25% by mass or more. In particular, if the concentration of the polyamic acid is 25% by mass or more, the productivity when forming a polyimide coating film using the polyamic acid can be increased. The upper limit of the concentration of the polyamic acid is preferably 50% by mass or less, more preferably 30% by mass, from the viewpoint of sufficiently dissolving the polyamic acid in an organic solvent.
[0038] In order to impart processing properties and various functionalities to the polyamic acid and the polyimide formed using the polyamic acid, various organic or inorganic low-molecular or high-molecular compounds may be blended into the polyamic acid composition. For example, the polyamic acid composition may contain a dye, a surfactant, a leveling agent, a plasticizer, fine particles, a sensitizer, a silane coupling agent, etc. The fine particles may be either organic fine particles or inorganic fine particles, and may have a porous or hollow structure.
[0039] <Polyimide> The method for converting polyamic acid to polyimide is not particularly limited, but polyimide can be produced by dehydrating and ring-closing (imidizing) the polyamic acid obtained as described above. The dehydrating and ring-closing (imidizing) method can be a known method such as thermal imidization, which involves dehydrating and ring-closing by heating, or chemical imidization, which involves chemical ring-closing using a known dehydrating and ring-closing catalyst.
[0040] In the case of thermal imidization, the heating temperature is preferably 120 to 350°C, more preferably 150 to 250°C. The heating time is preferably 0.5 to 3 hours, more preferably 1 to 2 hours. In the case of chemical imidization, for example, pyridine, triethylamine, acetic anhydride, etc. can be used as the dehydration ring-closing catalyst. In this case, the reaction temperature can be selected from any temperature between 20 and 250°C, and is preferably 100°C or less, and the reaction time is preferably 0.5 to 3 hours. The imidization may be performed in air, under reduced pressure, or in an inert gas such as nitrogen, but in order to obtain a polyimide film with high transparency, it is preferable to perform the imidization under reduced pressure or in an inert gas such as nitrogen.
[0041] The molecular weight (weight average molecular weight) of the polyimide is not particularly limited, but is preferably from 10,000 to 100,000 in terms of the low dielectric properties, film formability, and solubility in organic solvents of the resulting polyimide. The weight average molecular weight of the polyimide can be determined, for example, from a standard polystyrene-equivalent value measured by gel permeation chromatography (GPC).
[0042] <Polyimide film> The polyimide film of the present invention includes the polyimide obtained as described above. The method for producing such a polyimide film is not particularly limited, and for example, the above-mentioned polyamic acid composition is applied to a film on a substrate (e.g., plastic films such as polyethylene, polypropylene, urethane, polyester, polyethylene terephthalate (PET) or polycarbonate, glass plate, stainless steel plate, copper plate including ultra-thin copper foil, aluminum plate, etc.), and then dried and heated to remove the solvent and perform dehydration ring closure (imidization); or the polyimide obtained by converting the polyamic acid to polyimide is dissolved in an organic solvent, and the polyimide solution is applied to a film on a substrate and the solvent is dried and removed. The method for applying to the substrate is not particularly limited, and a conventionally known application method can be applied.
[0043] The thickness of the polyimide film is not particularly limited and can be appropriately selected depending on the application. The thickness of the polyimide film is preferably 10 to 100 μm, more preferably 20 to 30 μm. The thickness of the polyimide film can be easily controlled by appropriately adjusting the solid concentration and viscosity of each component in the polyamic acid composition.
[0044] <Printed wiring board> The polyimide film of the present invention is preferably used as a film for various components such as color filters, flexible displays, semiconductor parts, and optical components. Since the polyimide film exhibits insulating properties, it is preferably used as an insulating substrate for printed wiring boards. In addition, since the polyimide film is a thin and flexible film exhibiting insulating properties, it is also effectively used as a base film for flexible circuit boards called flexible printed wiring boards (FPCs). EXAMPLES
[0045] Next, examples of the present invention will be described, but the present invention is not limited to these examples as long as they do not depart from the spirit of the present invention.
[0046] <Examples 1 to 2, Comparative Examples 1 to 3> The organic solvents in which the diamines shown in Table 1 below were dissolved were added to a separable flask in the blending ratios shown in Table 1 below, and then the tetracarboxylic acid dihydrates shown in Table 1 below were added in the order shown in Table 1 below in the blending ratios shown in Table 1 below. The resulting mixture was stirred at 50°C for 3.5 hours and then at room temperature for 24 hours to prepare polyamic acid compositions used in Examples 1-2 and Comparative Examples 1-3. The prepared polyamic acid compositions were applied to a substrate using a test piece preparation process described below to prepare test pieces. The prepared test pieces were used to evaluate the properties shown in Table 1 below. The evaluation results are shown in Table 1. The blending amounts of the components shown in Table 1 below are in parts by mass unless otherwise specified.
[0047] [Table 1]
[0048] Details of each component in Table 1 are as follows: (A) Tetracarboxylic acid dianhydride PMDA: Pyromellitic dianhydride (B1) Fluorene-based diamine BAF: 9,9-bis(4-aminophenyl)fluorene (B2) Dimer diamine PRIAMINE® 1075: Dimer diamine manufactured by Croda Japan (B3) Aromatic diamine 4,4-ODA: 4,4-oxydianiline (C) Organic Solvent NMP: N-methyl-2-pyrrolidone
[0049] <Test piece preparation process> A PET film substrate ("Micro-adhesive sheet for processing PET75" manufactured by Nichiei Kako Co., Ltd., thickness 75 μm) was surface-treated (degreased) with isopropyl alcohol, and then the polyamic acid compositions prepared in Examples 1-2 and Comparative Examples 1-3 were applied onto the substrate using a bar coater. The substrate was then heat-treated at 150°C for 1 hour and then at 180°C for 30 minutes to cause thermal curing, thereby forming a cured coating film (polyimide film) having a predetermined thickness on the substrate, and a test specimen was prepared.
[0050] <Evaluation> (1) Film formability In the test piece preparation process, test pieces were prepared so that the thickness of the cured coating film was 50 μm ± 10 μm. The formed cured coating film was visually inspected, and was evaluated as follows: "Good" if no aggregation or cracking was observed and the coating film had sufficient toughness, "△" if no aggregation or cracking was observed but the coating film had insufficient toughness, and "Poor" if aggregation or cracking was observed.
[0051] (2) Glass transition temperature Tg and thermal expansion coefficient CTE In the test piece preparation process, test pieces were prepared so that the thickness of the cured coating film was 50 μm ± 10 μm. Next, the formed cured coating film was peeled off from the substrate, and the sample was cut to a predetermined size. The glass transition temperature Tg [°C] and the thermal expansion coefficient CTEα1 (0°C-100°C) were measured for the sample using a thermomechanical analyzer (Hitachi High-Tech Science Corporation, "TMA / SS6000").
[0052] (3) Heat decomposition resistance In the test piece preparation process, the test pieces were prepared so that the thickness of the cured coating film was 30 μm ± 10 μm. The obtained test pieces were cut into small pieces, and the temperature at which the weight was reduced by 5% in an air atmosphere at a heating rate of 10°C / min was measured using a thermogravimetric analyzer (Hitachi High-Tech Science Corporation, thermogravimetric analyzer "STA 7200RV"), and evaluated as the thermal decomposition temperature (Td5) [°C].
[0053] (4) Dielectric constant and dielectric tangent In the test piece preparation process, test pieces were prepared so that the thickness of the cured coating film was 25 μm ± 10 μm. Next, the obtained test pieces were cut into samples with a length of 50 mm and a width of 1.75 mm by the cavity resonance method using a network analyzer and a cavity resonator manufactured by Key Sight Technologies, and the dielectric constant and dielectric loss tangent were measured under the conditions of a measurement temperature of 25°C, a measurement humidity of 50 RH%, and a frequency of 10 GHz.
[0054] (5) Elastic modulus In the test piece preparation process, test pieces were prepared so that the thickness of the cured coating film was 50 μm ± 10 μm. Next, the formed cured coating film was peeled off from the substrate, and the specimen was cut to a predetermined size. The elastic modulus of the specimen was measured at a pulling speed of 5 mm / min using an autograph manufactured by Shimazu Corporation.
[0055] As shown in Table 1, in Examples 1 and 2 using polyamic acid obtained by polyaddition reaction of tetracarboxylic dianhydride with diamine having both fluorene skeleton and diamine containing dimer diamine, the film formability was evaluated as "△" or better, and therefore polyamic acid exhibiting good film formability could be produced. In addition, polyimide exhibiting low dielectric properties and high heat resistance could be produced because it exhibited high glass transition temperature Tg and low thermal expansion coefficient CTE, and furthermore, low dielectric constant and dielectric loss tangent were also low.
[0056] On the other hand, in Comparative Example 1, which did not contain any diamine having a fluorene skeleton or dimer diamine as the diamine component and used a general aromatic diamine, the film-forming property was excellent, but the dielectric constant and dielectric loss tangent were both higher than those of Examples 1 and 2, and it was not possible to prepare a polyimide exhibiting the desired low dielectric properties. Note that, since Comparative Example 1 exhibited high dielectric properties, other properties were not measured / evaluated.
[0057] In addition, in Comparative Example 2, which did not contain a diamine having a fluorene skeleton and used only dimer diamine as the diamine component, the film-forming property was excellent and both the dielectric constant and the dielectric tangent were low. However, the glass transition temperature Tg was lower than in Examples 1 and 2, and the thermal expansion coefficient CTE was also higher, so that it was not possible to prepare a polyimide exhibiting the desired high heat resistance.
[0058] In Comparative Example 3, in which the diamine component did not contain dimer diamine and only a diamine having a fluorene skeleton was used, aggregation and cracking of the coating film were observed, and a polyamic acid exhibiting good film-forming properties could not be produced. Since aggregation and cracking of the coating film were observed in Comparative Example 3, a polyimide could not be produced, and other characteristics were not measured / evaluated. [Industrial Applicability]
[0059] The polyamic acid of the present invention not only exhibits good film-forming properties but also exhibits low dielectric properties and high heat resistance, and can form polyimides that exhibit good mechanical strength. Therefore, a polyimide film prepared using such a polyimide is highly useful, for example, as an insulating substrate for a printed wiring board, in particular as a base film for a flexible printed wiring board.
Claims
1. A polyamic acid which is a polyaddition reaction product of (A) a tetracarboxylic dianhydride and (B) at least two diamines, The polyamic acid (B) is characterized in that the at least two diamines (B1) include a diamine having a fluorene skeleton and (B2) a dimer diamine.
2. The polyamic acid according to claim 1 , wherein the diamine having a fluorene skeleton (B1) has a structure represented by the following formula (1): 【Chemistry 1】 (In formula (1), R 1 ~R 4 are each independently a hydrogen atom, a halogen atom, or C 1 ~C 8 Alkyl group or C 1 ~C 8 represents a halogenated alkyl group.
3. A polyamic acid composition comprising the polyamic acid according to claim 1 or 2 and (C) an organic solvent.
4. A polyimide obtained by imidizing the polyamic acid according to claim 1 or 2.
5. A polyimide film comprising the polyimide according to claim 4.
6. A printed wiring board comprising the polyimide film according to claim 5 .
Citation Information
Patent Citations
Thermosetting ink composition and application of the same
JP2013032501A
Solvent-soluble polyimide resin
JP2015180750A
Polyimide, adhesive, film-like adhesive, adhesion layer, adhesive sheet, copper foil with resin, copper-clad laminate, printed wiring board, and multilayer wiring board and method for producing the same
JP2018168370A
Polyimide, crosslinked polyimide, adhesive film, laminate, coverlay film, copper foil with resin, metal-clad laminate, circuit board and multilayer circuit board
JP2021147610A
Benzocyclobutene-containing polyimide resin and its composition, manufacturing method, redistribution layer, polyimide film, and use
JP2021176961A