Photosensitive resin composition

The photosensitive resin composition addresses discoloration and residue issues by using a carboxyl group-containing resin with an aromatic ring and rutile titanium oxide, ensuring enhanced adhesion, alkali developability, and light reflectance for printed wiring boards.

JP2024139566AInactive Publication Date: 2024-10-09TAMURA KK

Patent Information

Application Number
JP2023050566
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing photosensitive resin compositions used for printed wiring boards face issues with discoloration due to light or heat, leading to decreased light reflectance and poor alkali developability, and often result in residue formation during development.

Method used

A photosensitive resin composition containing a carboxyl group-containing photosensitive resin with an aromatic ring, rutile titanium oxide, a photopolymerization initiator, and a reactive diluent, with specific properties such as sulfuric acid-processed rutile titanium oxide and a wetting and dispersing agent, to enhance adhesion, alkali developability, and light reflectance.

Benefits of technology

The composition achieves improved adhesion to substrates, excellent alkali developability, and sustained light reflectance without impairing resolution, while minimizing residue formation during development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139566000001
    Figure 2024139566000001
  • Figure 2024139566000002
    Figure 2024139566000002
  • Figure 2024139566000003
    Figure 2024139566000003
Patent Text Reader

Abstract

To provide a photosensitive resin composition capable of producing an insulation coating that offers superior optical reflectance while ensuring excellent alkali developability, without impairing basic characteristics such as adhesion to substrates and resolution of cured coatings.SOLUTION: A photosensitive resin composition comprises (A) a carboxyl group-containing photosensitive resin with an aromatic ring, (B) a rutile titanium oxide, (C) a photopolymerization initiator, (D) a reactive diluent, and (E) an epoxy compound.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive resin composition that can be used as a covering material, for example, an insulating covering material for covering a conductor circuit pattern formed on a substrate such as a rigid printed wiring board or a flexible printed wiring board (hereinafter, sometimes simply referred to as a "printed wiring board"); a cured product obtained by curing the photosensitive resin composition; and a substrate such as a printed wiring board covered with the cured product. [Background technology]

[0002] A circuit pattern of a conductor (e.g., copper foil) is formed on the printed wiring board, electronic components are mounted on the soldering lands of the circuit pattern by soldering, and the circuit portion excluding the soldering lands is covered with an insulating film (e.g., solder resist film) as a protective film. As the insulating protective film for the circuit portion, a photocured film of a photosensitive resin composition containing a photosensitive resin and a photopolymerization initiator may be used.

[0003] Printed wiring boards are also used as substrates for mounting light-emitting diode elements (LEDs) and the like, and the insulating coating formed on the mounting surface is required to have the function of improving the reflectance of light from a light source. In such applications, photosensitive resin compositions containing a white coloring agent such as titanium oxide are mainly used as the photosensitive resin composition for forming the insulating coating.

[0004] However, in the case of photosensitive resin compositions containing white colorants such as titanium oxide, discoloration due to light or heat may occur, resulting in coloration and reduced light reflectance. Therefore, a solder resist composition capable of suppressing discoloration and reduced light reflectance has been proposed (Patent Document 1). Patent Document 1 claims that by using a carboxyl group-containing resin that does not have an aromatic ring and rutile-type titanium oxide as a white pigment, discoloration of the resin due to light caused by the aromatic rings of the photosensitive resin and the photoactivity of titanium oxide can be suppressed, and high reflectance can be maintained for a long period of time.

[0005] However, the carboxyl group-containing resin having no aromatic ring of Patent Document 1 still sometimes discolors due to heat, and there is room for improvement in improving light reflectance. Furthermore, when rutile-type titanium oxide is blended with the carboxyl group-containing resin having no aromatic ring of Patent Document 1, residues of the coating film of the photosensitive resin composition may remain on the substrate or conductor after alkaline development, and there is room for improvement in alkaline developability. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2007-322546 A Summary of the Invention [Problem to be solved by the invention]

[0007] In view of the above circumstances, an object of the present invention is to provide a photosensitive resin composition that can give an insulating coating film having excellent light reflectance while having excellent alkaline developability without impairing basic properties such as adhesion to a substrate and resolution of a cured coating film. [Means for solving the problem]

[0008] The gist of the configuration of the present invention is as follows. [1] A photosensitive resin composition comprising: (A) a carboxyl group-containing photosensitive resin having an aromatic ring; (B) rutile-type titanium oxide; (C) a photopolymerization initiator; (D) a reactive diluent; and (E) an epoxy compound. [2] The photosensitive resin composition according to [1], wherein the (B) rutile type titanium oxide is a titanium oxide produced by a sulfuric acid process. [3] The photosensitive resin composition according to [1] or [2], wherein the oil absorption of the (B) rutile-type titanium oxide is 30 g / 100 g or less. [4] The photosensitive resin composition according to [1] or [2], wherein the (B) rutile type titanium oxide is a titanium oxide produced by a sulfuric acid process having an oil absorption of 30 g / 100 g or less. [5] The photosensitive resin composition according to [1] or [2], further comprising (F) a wetting and dispersing agent. [6] The photosensitive resin composition according to [5], wherein the (F) wetting and dispersing agent has an acid value of 70 mgKOH / g or less. [7] The photosensitive resin composition according to [5], wherein the (B) rutile-type titanium oxide is a titanium oxide produced by a sulfuric acid process having an oil absorption of 30 g / 100 g or less, and the (F) wetting and dispersing agent has an acid value of 70 mg KOH / g or less. [8] The (A) carboxyl group-containing photosensitive resin having an aromatic ring, (A-1) General formula (I) [ka] (In the formula, R 1 represents a hydrogen atom or a methyl group), General formula (II) [ka] (In the formula, R 1 represents a hydrogen atom or a methyl group, and R 2 represents a phenyl group, an α-cumyl group, an alkoxy group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms in an alkyl group, a t-butyl group, an adamantyl group, or a trifluoromethyl group, and m is an integer of 0 or 1 to 3) and / or a compound represented by the general formula (III): [ka] (In the formula, R 1 represents a hydrogen atom or a methyl group, and R 2 represents a phenyl group, an α-cumyl group, an alkoxy group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms in an alkyl group, a t-butyl group, an adamantyl group, or a trifluoromethyl group; A 1 represents an alkylene group having 2 to 10 carbon atoms and containing a linear or cyclic skeleton, or a hydroxyalkylene group having 3 to 10 carbon atoms, m is an integer of 0 or 1 to 3, and p is an integer of 1 to 5), Or, (A-2) general formula (I) [ka] (In the formula, R 1 represents a hydrogen atom or a methyl group), General formula (II) [ka] (In the formula, R 1 represents a hydrogen atom or a methyl group, and R 2 represents a phenyl group, an α-cumyl group, an alkoxy group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms in an alkyl group, a t-butyl group, an adamantyl group, or a trifluoromethyl group, and m is an integer of 0 or 1 to 3) and / or a compound represented by the general formula (III): [ka] (In the formula, R 1 represents a hydrogen atom or a methyl group, and R 2 represents a phenyl group, an α-cumyl group, an alkoxy group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms in an alkyl group, a t-butyl group, an adamantyl group, or a trifluoromethyl group; A 1 represents an alkylene group having 2 to 10 carbon atoms and containing a straight-chain or cyclic skeleton, or a hydroxyalkylene group having 3 to 10 carbon atoms, m is an integer of 0 or 1 to 3, and p is an integer of 1 to 5), to which a compound having an oxirane ring and an ethylenically unsaturated bond is added to a part of the carboxyl groups of the copolymer obtained by reacting a compound represented by the following formula (I): [9] The compound having an oxirane ring and an ethylenically unsaturated bond is represented by the general formula (IV). [ka] (In the formula, R 1 represents a hydrogen atom or a methyl group, and A 2 represents an alkylene group having 2 to 10 carbon atoms, and q is an integer of 0 or 1 to 5.

[10] The photosensitive resin composition according to [1] or [2], comprising 100 parts by mass or more and 800 parts by mass or less of the rutile-type titanium oxide (B) relative to 100 parts by mass of the carboxyl group-containing photosensitive resin (A) having an aromatic ring.

[11] The photosensitive resin composition according to [5], further comprising 0.50 parts by mass or more and 15 parts by mass or less of the wetting and dispersing agent (F) relative to 100 parts by mass of the carboxyl group-containing photosensitive resin (A) having an aromatic ring.

[12] The photosensitive resin composition according to [5], comprising 0.15 parts by mass or more and 3.0 parts by mass or less of the wetting and dispersing agent (F) relative to 100 parts by mass of the rutile-type titanium oxide (B).

[13] A cured product of the photosensitive resin composition according to [1] or [2].

[14] A printed wiring board comprising the cured product according to

[13] . Effect of the Invention

[0009] According to an embodiment of the photosensitive resin composition of the present invention, by containing (A) a carboxyl group-containing photosensitive resin having an aromatic ring and (B) rutile-type titanium oxide, it is possible to obtain an insulating coating film having excellent light reflectance while having excellent alkaline developability without impairing basic properties such as adhesion to a substrate and resolution of a cured coating film.

[0010] According to an embodiment of the photosensitive resin composition of the present invention, the (B) rutile type titanium oxide is a titanium oxide prepared by a sulfate process, so that excellent alkaline developability can be reliably obtained.

[0011] According to an embodiment of the photosensitive resin composition of the present invention, the oil absorption of the rutile-type titanium oxide (B) is 30 g / 100 g or less, so that excellent alkaline developability can be reliably obtained.

[0012] According to an embodiment of the photosensitive resin composition of the present invention, the (B) rutile type titanium oxide is a titanium oxide produced by a sulfuric acid process having an oil absorption of 30 g / 100 g or less, thereby further improving the alkali developability.

[0013] According to an embodiment of the photosensitive resin composition of the present invention, the composition further contains a wetting and dispersing agent (F), which reliably improves the light reflectance and further improves the resolution.

[0014] According to an embodiment of the photosensitive resin composition of the present invention, the acid value of the (F) wetting and dispersing agent is 70 mgKOH / g or less, whereby the light reflectance is further reliably improved and the adhesion is further improved.

[0015] According to an embodiment of the photosensitive resin composition of the present invention, the (B) rutile-type titanium oxide is a sulfate-processed titanium oxide having an oil absorption of 30 g / 100 g or less, and the (F) wetting and dispersing agent has an acid value of 70 mgKOH / g or less, whereby the adhesion, resolution, alkali developability, and light reflectance are further improved.

[0016] According to an embodiment of the photosensitive resin composition of the present invention, the (A) carboxyl group-containing photosensitive resin having an aromatic ring is the (A-1) copolymer resin or the (A-2) copolymer resin, so that the carboxyl group is specified to a structure derived from (meth)acrylic acid, and as shown in general formula (II) or (III), after polymerization, a compound that does not have a hydrogen atom at the α-position of the side chain of the aromatic hydrocarbon skeleton is a constituent element of the copolymer resin, that is, a compound that does not have a hydrogen atom at the α-position of the side chain to the aromatic hydrocarbon skeleton or a compound in which a hydrogen atom at the α-position to the aromatic hydrocarbon skeleton is present in the main chain is a constituent element of the copolymer resin. Therefore, discoloration of the cured coating film, particularly discoloration of the cured coating film caused mainly by heat when forming the cured coating film on a conductor, can be suppressed, and excellent light reflectance can be reliably obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Next, the photosensitive resin composition of the present invention will be described in detail. The photosensitive resin composition of the present invention contains (A) a carboxyl group-containing photosensitive resin having an aromatic ring, (B) rutile-type titanium oxide, (C) a photopolymerization initiator, (D) a reactive diluent, and (E) an epoxy compound. The components (A) to (E) will be described in detail below.

[0018] (A) Aromatic ring-containing carboxyl group-containing photosensitive resin The incorporation of a carboxyl group-containing photosensitive resin having an aromatic ring as the carboxyl group-containing photosensitive resin contributes to obtaining an insulating coating (cured coating film) such as a solder resist film having excellent light reflectance. The carboxyl group-containing photosensitive resin having an aromatic ring is not particularly limited as long as it is a photosensitive resin having an aromatic ring and a carboxyl group, and may be, for example, (A-1) a photosensitive resin having the general formula (I): [ka] (In the formula, R 1 represents a hydrogen atom or a methyl group), General formula (II) [ka] (In the formula, R 1 represents a hydrogen atom or a methyl group, and R 2 represents a phenyl group, an α-cumyl group, an alkoxy group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms in an alkyl group, a t-butyl group, an adamantyl group, or a trifluoromethyl group, and m is an integer of 0 or 1 to 3) and / or a compound represented by the general formula (III): [ka] (In the formula, R 1 represents a hydrogen atom or a methyl group, and R 2 represents a phenyl group, an α-cumyl group, an alkoxy group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms in an alkyl group, a t-butyl group, an adamantyl group, or a trifluoromethyl group; A 1 represents an alkylene group having 2 to 10 carbon atoms containing a linear or cyclic skeleton or a hydroxyalkylene group having 3 to 10 carbon atoms, m is an integer of 0 or 1 to 3, and p is an integer of 1 to 5) (hereinafter, may be simply referred to as “A-1 copolymer resin”).

[0019] The (A) aromatic ring-containing carboxyl group-containing photosensitive resin may be, for example, (A-2) a photosensitive resin represented by general formula (I): [ka] (In the formula, R 1 represents a hydrogen atom or a methyl group), General formula (II) [ka] (In the formula, R 1 represents a hydrogen atom or a methyl group, and R 2 represents a phenyl group, an α-cumyl group, an alkoxy group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms in an alkyl group, a t-butyl group, an adamantyl group, or a trifluoromethyl group, and m is an integer of 0 or 1 to 3) and / or a compound represented by the general formula (III): [ka] (In the formula, R 1 represents a hydrogen atom or a methyl group, and R 2 represents a phenyl group, an α-cumyl group, an alkoxy group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms in an alkyl group, a t-butyl group, an adamantyl group, or a trifluoromethyl group; A 1 represents an alkylene group having 2 to 10 carbon atoms or a hydroxyalkylene group having 3 to 10 carbon atoms having a straight chain or cyclic skeleton, m is an integer of 0 or 1 to 3, and p is an integer of 1 to 5), to which a compound having an oxirane ring and an ethylenically unsaturated bond is added to a part of the carboxyl groups of the copolymer obtained by reacting the copolymer with a compound represented by the formula (I) (hereinafter, may be simply referred to as "A-2 copolymer resin").

[0020] In the A-1 copolymer resin and the A-2 copolymer resin, the carboxyl group is specified to have a structure derived from (meth)acrylic acid, and as shown in general formulas (II) and (III), after polymerization, a compound that does not have a hydrogen atom at the α-position of the side chain of the aromatic hydrocarbon skeleton is a constituent element of the copolymer resin; that is, a compound that does not have a hydrogen atom at the α-position of the side chain to the aromatic hydrocarbon skeleton or a compound in which a hydrogen atom at the α-position to the aromatic hydrocarbon skeleton is present in the main chain is a constituent element of the copolymer resin. This makes it possible to suppress discoloration of the cured coating film, in particular discoloration of the cured coating film caused mainly by heat when forming the cured coating film on a conductor, and reliably obtain excellent light reflectance.

[0021] A-1 copolymer resin The A-1 copolymer resin is obtained by copolymerizing acrylic acid or methacrylic acid represented by general formula (I) with an ethylenically unsaturated monomer having an aromatic ring represented by general formula (II) and / or a (meth)acrylate having an aromatic ring represented by general formula (III).

[0022] Examples of the ethylenically unsaturated monomer having an aromatic ring represented by general formula (II) include styrene, α-methylstyrene, p-methoxystyrene, mt-butoxystyrene, pt-butoxystyrene, p-(1-ethoxyethoxy)styrene, p-fluorostyrene, etc. These monomers may be used alone or in combination of two or more.

[0023] Examples of the (meth)acrylate having an aromatic ring represented by general formula (III) include phenoxy polyethylene glycol (meth)acrylates such as phenoxyethyl (meth)acrylate and 2-(2-phenoxyethoxy)ethyl (meth)acrylate, phenoxy polypropylene glycol (meth)acrylates such as phenoxypropyl (meth)acrylate and 2-phenoxypropyl (meth)acrylate, phenyl glycidyl ether (meth)acrylate, 4-α-cumylphenoxy polyethylene glycol (meth)acrylates such as 4-α-cumylphenoxyethyl (meth)acrylate, and 2-phenylphenoxy polyethylene glycol (meth)acrylates such as 2-phenylphenoxyethyl (meth)acrylate. These compounds may be used alone or in combination of two or more.

[0024] A-2 copolymer resin The A-2 copolymer resin is obtained by further adding a compound having an oxirane ring and an ethylenically unsaturated bond to a part of the carboxyl groups of the A-1 copolymer resin obtained by copolymerizing general formula (I) with general formula (II) and / or general formula (III).

[0025] The compound having an oxirane ring and an ethylenically unsaturated bond is not particularly limited, but may be, for example, a compound represented by the general formula (IV): [ka] (In the formula, R 1 represents a hydrogen atom or a methyl group, and A 2 represents an alkylene group having 2 to 10 carbon atoms, and q is an integer of 0 or 1 to 5).

[0026] Examples of the compound represented by the general formula (IV) include glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, hydroxyalkyl (meth)acrylate glycidyl ether, β-methylglycidyl (meth)acrylate, epoxycyclohexyl derivatives of (meth)acrylic acid such as (3,4-epoxycyclohexyl)methyl (meth)acrylate, alicyclic epoxy derivatives of (meth)acrylate, etc. These compounds may be used alone or in combination of two or more kinds.

[0027] To obtain the A-1 copolymer resin and the A-2 copolymer resin, either an ethylenically unsaturated monomer having an aromatic ring represented by general formula (II) or a (meth)acrylate having an aromatic ring represented by general formula (III) may be used, or both may be used in combination.

[0028] If necessary, an ethylenically unsaturated monomer having neither an aromatic ring nor a carboxyl group may be added to the ethylenically unsaturated monomer having an aromatic ring represented by general formula (II) and the (meth)acrylate having an aromatic ring represented by general formula (III), and copolymerized with the (meth)acrylic acid represented by general formula (I). Examples of the ethylenically unsaturated monomer having neither an aromatic ring nor a carboxyl group include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and the like. alkyl (meth)acrylates having a straight chain, branched or alicyclic skeleton, such as dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate and 2-ethyl-2-adamantyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, cyclohexanedimethanol mono(meth)acrylate, nonanediol mono(meth)acrylate, and other hydroxy mono(meth)acrylates, tetrahydrofurfuryl (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, alkoxylated tetrahydrofurfuryl (meth)acrylate, and other cyclic ether skeleton-containing (meth)acrylates, 2-hydroxyethyl (meth)acrylate-caprolactone adduct, 2-hydroxypropyl (meth)acrylate-caprolactone adduct, and other hydroxy mono(meth)acrylate-caprolactone adducts, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, poly(ethylene glycol-propylene glycol) mono(meth)acrylate,Examples of the polyalkylene glycol-modified hydroxy mono(meth)acrylates include poly(ethylene glycol·tetramethylene glycol) mono(meth)acrylate and poly(propylene glycol·tetramethylene glycol) mono(meth)acrylate; alkyl-terminated polyalkylene glycol mono(meth)acrylates such as methoxypolyethylene glycol mono(meth)acrylate, methoxypolypropylene glycol mono(meth)acrylate and ethoxypolyethylene glycol mono(meth)acrylate; fluorine-containing (meth)acrylates such as 2,2,2-trifluoromethyl(meth)acrylate, 2-(perfluorobutyl)ethyl(meth)acrylate, 3-(perfluorobutyl)-2-hydroxypropyl(meth)acrylate and 2-(perfluorohexyl)ethyl(meth)acrylate; imide group-containing (meth)acrylates such as N-(meth)acryloyloxyethylhexahydrophthalimide; and (meth)acrylic silicone compounds such as mono(meth)acrylates having a dimethylsiloxane skeleton. These compounds may be used alone or in combination of two or more.

[0029] The content of aromatic hydrocarbon skeleton in A-1 copolymer resin and A-2 copolymer resin is not particularly limited, but the lower limit is preferably 5 mass %, particularly preferably 10 mass %, from the viewpoint of imparting excellent heat resistance to the cured coating film, while the upper limit of the content of aromatic hydrocarbon skeleton in A-1 copolymer resin and A-2 copolymer resin is preferably 40 mass %, particularly preferably 30 mass %, from the viewpoint of imparting excellent flexibility to the cured coating film.

[0030] The A-1 copolymer resin and the A-2 copolymer resin can be synthesized by a known solution polymerization method. The solvent used is not particularly limited as long as it is inactive to radical polymerization. Examples of the solvent include ethylene glycol monoalkyl ether acetates such as ethyl acetate, isopropyl acetate, cellosolve acetate, and butyl cellosolve acetate; diethylene glycol monoalkyl ether acetates such as diethylene glycol monomethyl ether acetate, carbitol acetate, and butyl carbitol acetate; acetate esters such as propylene glycol monoalkyl ether acetates and dipropylene glycol monoalkyl ether acetates; diethylene glycol dialkyl ethers, methyl carbitol, ethyl carbitol, and butyl carbitol; Examples of the solvent include ethylene glycol dialkyl ethers, triethylene glycol dialkyl ethers, propylene glycol dialkyl ethers, dipropylene glycol dialkyl ethers, ethers such as 1,4-dioxane and tetrahydrofuran, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, hydrocarbons such as benzene, toluene, xylene, octane, and decane, petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha, lactic acid esters such as methyl lactate, ethyl lactate, and butyl lactate, dimethylformamide, and N-methylpyrrolidone. These solvents may be used alone or in combination of two or more. The amount of the solvent used is preferably 30 parts by mass or more and 1000 parts by mass or less, and particularly preferably 50 parts by mass or more and 800 parts by mass or less, based on 100 parts by mass of the A-1 copolymer resin and the A-2 copolymer resin.

[0031] The radical polymerization initiator used in the solution polymerization method is not particularly limited, and for example, an organic peroxide or an azo compound can be used. Specific examples include benzoyl peroxide, dicumyl peroxide, diisopropyl peroxide, di-t-butyl peroxide, t-butyl peroxybenzoate, t-hexyl peroxybenzoate, t-butyl peroxy-2-ethylhexanoate, t-hexyl peroxy-2-ethylhexanoate, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyl-3,3-isopropyl hydroperoxide, and t-butyl hydroperoxide. Examples of the radical polymerization initiator include 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-hexylperoxy)3,3,5-trimethylcyclohexane, azobisisobutyronitrile, and azobiscarbonamide. The radical polymerization initiator is appropriately selected from those having a suitable half-life depending on the polymerization temperature. The amount of the radical polymerization initiator used is preferably 0.5 parts by mass or more and 20 parts by mass or less, and particularly preferably 1 part by mass or more and 10 parts by mass or less, based on 100 parts by mass of the total of the radical polymerizable unsaturated compounds.

[0032] The polymerization method may be to drop the unsaturated monomer and the radical polymerization initiator into a heated solvent and then stir the mixture, or to dissolve the unsaturated monomer and the radical polymerization initiator in a solvent and heat the mixture while stirring to carry out the polymerization reaction. Alternatively, the radical polymerization initiator may be added to a solvent and the mixture may be heated and then the unsaturated monomer may be dropped into the solvent.

[0033] A-2 copolymer resin can be obtained by addition reaction of a compound having an oxirane ring and an ethylenically unsaturated bond with a part of the carboxyl group in the A-1 copolymer resin obtained by the above polymerization method. The lower limit of the amount of the compound having an oxirane ring and an ethylenically unsaturated bond added to one equivalent of the carboxyl group in the A-1 copolymer resin is preferably 0.1 equivalent, particularly preferably 0.2 equivalent, from the viewpoint of ensuring sufficient photosensitivity. On the other hand, the upper limit is preferably 0.8 equivalent, particularly preferably 0.6 equivalent, from the viewpoint of obtaining good alkaline developability.

[0034] Examples of catalysts used in the reaction between the carboxyl group in the A-1 copolymer resin and the compound having an oxirane ring and an ethylenically unsaturated bond include triphenylphosphine, lithium naphthenate, zirconium naphthenate, chromium naphthenate, chromium acetylacetonate, and chromium chloride. Examples of polymerization inhibitors include methoxyhydroquinone. The reaction can be carried out by a known method, and examples include a method in which the A-1 copolymer resin in the solvent obtained by the above polymerization reaction is set to a predetermined temperature, and then the compound having an oxirane ring and an ethylenically unsaturated bond, the catalyst, and the polymerization inhibitor are mixed and stirred. At this time, the amount of the catalyst used is preferably 0.01% by mass or more and 1% by mass or less based on the total of the A-1 copolymer resin and the compound having an oxirane ring and an ethylenically unsaturated bond. The amount of the polymerization inhibitor used is preferably 0.01% by mass or more and 1% by mass or less based on the total of the A-1 copolymer resin and the compound having an oxirane ring and an ethylenically unsaturated bond. The reaction temperature is preferably from 60° C. to 150° C., and the reaction time is preferably from 3 hours to 60 hours.

[0035] The lower limit of the weight average molecular weight of the A-1 copolymer resin is preferably 3000, particularly preferably 5000, from the viewpoint of the toughness and dryness to touch of the cured coating film. On the other hand, the upper limit of the weight average molecular weight of the A-1 copolymer resin is preferably 200000, particularly preferably 50000, from the viewpoint of obtaining good alkaline developability. Also, the lower limit of the weight average molecular weight of the A-2 copolymer resin is preferably 3000, particularly preferably 5000, from the viewpoint of the toughness and dryness to touch of the cured coating film. On the other hand, the upper limit of the weight average molecular weight of the A-2 copolymer resin is preferably 200000, particularly preferably 50000, from the viewpoint of obtaining good alkaline developability.

[0036] The acid values ​​of the A-1 copolymer resin and the A-2 copolymer resin are not particularly limited, but are preferably from 30 mgKOH / g to 150 mgKOH / g, respectively.

[0037] (B) Rutile titanium dioxide (rutile titanium dioxide) By containing the above-mentioned carboxyl group-containing photosensitive resin having an aromatic ring and rutile titanium oxide (rutile titanium dioxide), it is possible to obtain an insulating coating having excellent light reflectance while having excellent alkaline developability without impairing basic properties such as adhesion to the substrate and resolution of the cured coating film.

[0038] Examples of rutile titanium oxide include titanium oxide produced by the sulfuric acid process and titanium oxide produced by the hydrochloric acid process. Titanium oxide produced by the sulfuric acid process is slightly yellowish compared to titanium oxide produced by the hydrochloric acid process, and therefore can be visually confirmed. Among these, titanium oxide produced by the sulfuric acid process is preferred in that excellent alkaline developability can be reliably obtained.

[0039] The oil absorption of rutile titanium oxide is not particularly limited, but the upper limit is preferably 35g / 100g, more preferably 30g / 100g, even more preferably 25g / 100g, and particularly preferably 24g / 100g, from the viewpoint of reliably obtaining excellent alkaline developability. On the other hand, the lower limit of the oil absorption of rutile titanium oxide is preferably 5g / 100g, from the viewpoint of kneadability during preparation of the photosensitive resin composition. The oil absorption refers to the consumption volume of refined linseed oil per 100g of sample pigment in the test method of JIS K 5101-13-1.

[0040] Among these, from the viewpoint of further improving alkaline developability, the rutile titanium oxide is preferably a sulfate-processed titanium oxide having an oil absorption of 35 g / 100 g or less, more preferably a sulfate-processed titanium oxide having an oil absorption of 30 g / 100 g or less, and particularly preferably a sulfate-processed titanium oxide having an oil absorption of 25 g / 100 g or less.

[0041] The average particle size of rutile-type titanium oxide is not particularly limited, but is usually 0.01 μm or more and 1 μm or less. Examples of rutile-type titanium oxide include "TR-600", "TR-700", "TR-750", "TR-840" (all Fuji Titanium Industry Co., Ltd.), "R-550", "R-580", "R-630", "R-780", "R-820", "CR-50", "CR-60", "CR-80", "CR-90", "CR-93" (all Ishihara Sangyo Kaisha, Ltd.), "KR-270", "KR-310", "KR-380" (all Titanium Industry Co., Ltd.), "JR-1000" (Teika Corporation), and the like.

[0042] The amount of rutile-type titanium oxide is not particularly limited, but the lower limit is preferably 100 parts by mass, more preferably 200 parts by mass, and particularly preferably 300 parts by mass, relative to 100 parts by mass (solid content, the same applies below) of the carboxyl group-containing photosensitive resin having an aromatic ring, from the viewpoint of reliably obtaining excellent light reflectance. On the other hand, the upper limit of the amount of rutile-type titanium oxide is preferably 800 parts by mass, more preferably 600 parts by mass, and particularly preferably 500 parts by mass, from the viewpoint of reliably obtaining excellent alkaline developability and preventing a decrease in coatability.

[0043] (C) Photopolymerization initiator The photopolymerization initiator is not particularly limited, and examples thereof include 1,2-octanedione, 1-[4-(phenylthio)-2-(O-benzoyloxime)], ethanone 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime), 2-(acetyloxyiminomethyl)thioxanthen-9-one, 1,8-octanedione, 1,8-bis[9-ethyl-6-nitro-9H-carbazol-3-yl]-, 1,8-bis(O-acetyloxime), 1,8-octanedione, 1,8-bis[9-(2-ethylhexyl)-6-nitro-9H-carbazol-3-yl]-, 1,8-bis(O-acetyloxime), (Z) Examples of the photopolymerization initiator include oxime ester-based photopolymerization initiators such as -(9-ethyl-6-nitro-9H-carbazol-3-yl)(4-((1-methoxypropan-2-yl)oxy)-2-methylphenyl)methanone O-acetyloxime, and α-aminoalkylphenone-based photopolymerization initiators such as 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one.

[0044] Examples of photopolymerization initiators other than the oxime ester photopolymerization initiator and the α-aminoalkylphenone photopolymerization initiator include benzoin-based initiators such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, and benzoin isobutyl ether; acetophenone-based initiators such as acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, and 2,2-diethoxy-2-phenylacetophenone; benzophenone-based initiators such as benzophenone, p-phenylbenzophenone, 4,4′-diethylaminobenzophenone, and dichlorobenzophenone; anthraquinone-based initiators such as 2-methylanthraquinone, 2-ethylanthraquinone, 2-tertiary butylanthraquinone, and 2-aminoanthraquinone; 2-methylthioxanthone, 2- Examples of the photopolymerization initiator include thioxanthone such as ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, and 2,4-diethylthioxanthone; benzyl dimethyl ketal, acetophenone dimethyl ketal, p-dimethylaminobenzoic acid ethyl ester, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, and 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone. These photopolymerization initiators may be used alone or in combination of two or more.

[0045] The amount of the photopolymerization initiator is not particularly limited, but is preferably 0.50 parts by mass or more and 5.0 parts by mass or less, and particularly preferably 1.0 parts by mass or more and 3.0 parts by mass or less, per 100 parts by mass of the carboxyl group-containing photosensitive resin having an aromatic ring.

[0046] (D) Reactive diluent The reactive diluent is, for example, a photopolymerizable monomer, which is a compound having at least one polymerizable double bond per molecule, preferably two or more polymerizable double bonds per molecule. The reactive diluent reinforces the photocuring of the photosensitive resin composition, and can contribute to the formation of a photocured film having sufficient strength.

[0047] Examples of the reactive diluent include (meth)acrylate compounds such as monofunctional (meth)acrylate compounds and polyfunctional (meth)acrylate compounds. Examples of the (meth)acrylate compounds include monofunctional (meth)acrylate compounds such as hydroxyethyl (meth)acrylate, phenoxyethyl (meth)acrylate, diethylene glycol mono(meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and caprolactone-modified (meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, and ethylene oxide. Examples of the (meth)acrylate compound include bifunctional (meth)acrylate compounds such as modified phosphoric acid di(meth)acrylate, allylated cyclohexyl di(meth)acrylate, and isocyanurate di(meth)acrylate, trifunctional (meth)acrylate compounds such as trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, and tris(acryloxyethyl)isocyanurate, and tetrafunctional or higher (meth)acrylate compounds such as ditrimethylolpropane tetra(meth)acrylate, propionic acid modified dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. Examples of the (meth)acrylate compound include monofunctional or bifunctional or higher urethane (meth)acrylate compounds, and epoxy (meth)acrylate compounds. These (meth)acrylate compounds may be used alone or in combination of two or more kinds.

[0048] The amount of the reactive diluent is not particularly limited, but is preferably 50 parts by mass or more and 200 parts by mass or less, and particularly preferably 100 parts by mass or more and 150 parts by mass or less, per 100 parts by mass of the carboxyl group-containing photosensitive resin having an aromatic ring.

[0049] (E) Epoxy compounds The epoxy compound is a component for increasing the crosslink density of the photocured product to obtain a photocured film with sufficient strength. Examples of the epoxy compound include epoxy resins. Examples of the epoxy resin include rubber-modified epoxy resins such as biphenyl-type epoxy resins, naphthalene-type epoxy resins, dicyclopentadiene-type epoxy resins, and silicone-modified epoxy resins, ε-caprolactone-modified epoxy resins, phenol novolac-type epoxy resins such as bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, and bisphenol AD-type epoxy resins, cresol novolac-type epoxy resins such as o-cresol novolac-type epoxy resins, biphenyl novolac-type epoxy resins, bisphenol A novolac-type epoxy resins, cyclic aliphatic epoxy resins, glycidyl ester-type epoxy resins, glycidyl amine-type epoxy resins, heterocyclic epoxy resins, bisphenol-modified novolac-type epoxy resins, polyfunctionally modified novolac-type epoxy resins, and condensation-type epoxy resins of phenols and aromatic aldehydes having phenolic hydroxyl groups. These epoxy compounds may be used alone or in combination of two or more.

[0050] The amount of the epoxy compound is not particularly limited, but is preferably from 10 to 100 parts by mass, and particularly preferably from 20 to 50 parts by mass, per 100 parts by mass of the carboxyl group-containing photosensitive resin having an aromatic ring.

[0051] The photosensitive resin composition of the present invention may further contain a wetting dispersant (F) as required. By further containing the wetting dispersant (F) in the photosensitive resin composition of the present invention, the light reflectance is reliably improved and the resolution is further improved.

[0052] The wetting dispersant improves the dispersibility of the aromatic ring-containing carboxyl group-containing photosensitive resin and rutile-type titanium oxide in the photosensitive resin composition, thereby increasing the light reflectance of the cured coating film and contributing to suppressing the decrease in light reflectance due to heat treatment and light irradiation treatment. Examples of the wetting dispersant include various known organic or inorganic pigment dispersants. Examples of the wetting dispersant include copolymers having an acidic group, copolymers containing an acidic group, alkylol ammonium salts of copolymers having an acidic group, linear polymers having a pigment affinity group, and block copolymers having affinity to pigments.

[0053] The wetting dispersant preferably has an acid value within a predetermined range. The upper limit of the acid value of the wetting dispersant is preferably 140 mgKOH / g, more preferably 100 mgKOH / g, from the viewpoint of reliably improving the light reflectance and improving the adhesion, and is more preferably 70 mgKOH / g, particularly preferably 50 mgKOH / g, from the viewpoint of more reliably improving the light reflectance and further improving the adhesion. The lower limit of the acid value of the wetting dispersant is preferably 20 mgKOH / g, from the viewpoint of contributing to the improvement of the alkaline developability.

[0054] Examples of wetting and dispersing agents available on the market include "DISPERBYK-102", "DISPERBYK-110", "DISPERBYK-111", "DISPERBYK-118", "DISPERBYK-162", "DISPERBYK-163", "DISPERBYK-164", and "DISPERBYK-180" (all from BYK).

[0055] In addition, the above-mentioned (B) rutile-type titanium oxide is a titanium oxide obtained by a sulfate process having an oil absorption of 30 g / 100 g or less, and the (F) wetting and dispersing agent has an acid value of 70 mgKOH / g or less, whereby the adhesion, resolution, alkali developability, and light reflectance are further improved.

[0056] The amount of the wetting dispersant (solid content) is not particularly limited, but the lower limit is preferably 0.50 parts by mass, more preferably 1.0 parts by mass, and particularly preferably 1.5 parts by mass, relative to 100 parts by mass of the carboxyl group-containing photosensitive resin having an aromatic ring, from the viewpoint of reliably improving the light reflectance and further improving the resolution. On the other hand, the upper limit of the amount of the wetting dispersant is preferably 15 parts by mass, more preferably 10 parts by mass, and particularly preferably 7.0 parts by mass, relative to 100 parts by mass of the carboxyl group-containing photosensitive resin having an aromatic ring, from the viewpoint of imparting excellent photosensitivity.

[0057] The mixing ratio of rutile titanium oxide to the wetting dispersant is not particularly limited, but from the viewpoint of reliably improving light reflectance, the amount of the wetting dispersant is preferably 0.15 parts by mass or more and 3.0 parts by mass or less, more preferably 0.30 parts by mass or more and 2.0 parts by mass or less, and particularly preferably 0.40 parts by mass or more and 1.5 parts by mass or less, per 100 parts by mass of rutile titanium oxide.

[0058] In addition to the above-described components (A) to (F), the photosensitive resin composition of the present invention may contain various other components, such as a flame retardant, a curing accelerator, an additive, a non-reactive diluent, etc., as necessary.

[0059] A light source or electronic components that generate a large amount of heat may be mounted on a printed wiring board. Therefore, by blending a flame retardant with the photosensitive resin composition, flame retardancy can be imparted to the cured film of the photosensitive resin composition. Examples of the flame retardant include phosphorus-based flame retardants such as organic phosphates.Examples of phosphorus-based flame retardants include halogen-containing phosphorus phosphates such as tris(chloroethyl)phosphate, tris(2,3-dichloropropyl)phosphate, tris(2-chloropropyl)phosphate, tris(2,3-bromopropyl)phosphate, tris(bromochloropropyl)phosphate, 2,3-dibromopropyl-2,3-chloropropyl phosphate, tris(tribromophenyl)phosphate, tris(dibromophenyl)phosphate, and tris(tribromoneopentyl)phosphate. Phosphate esters; non-halogenated aliphatic phosphate esters such as trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, and tributoxyethyl phosphate; triphenyl phosphate, cresyl diphenyl phosphate, dicresyl phenyl phosphate, tricresyl phosphate, trixylenyl phosphate, xylenyl diphenyl phosphate, tris(isopropylphenyl)phosphate, isopropylphenyl diphenyl phosphate, and diisopropyl phosphate. Examples of suitable phosphine oxide compounds include non-halogen-based aromatic phosphate esters such as propylphenylphenyl phosphate, tris(trimethylphenyl)phosphate, tris(t-butylphenyl)phosphate, hydroxyphenyldiphenylphosphate, and octyldiphenylphosphate; metal salts of phosphinic acid such as aluminum trisdiethylphosphinate, aluminum trismethylethylphosphinate, aluminum trisdiphenylphosphinate, zinc bisdiethylphosphinate, zinc bismethylethylphosphinate, zinc bisdiphenylphosphinate, titanyl bisdiethylphosphinate, titanium tetrakisdiethylphosphinate, titanyl bismethylethylphosphinate, titanium tetrakismethylethylphosphinate, titanyl bisdiphenylphosphinate, and titanium tetrakisdiphenylphosphinate; and phosphine oxide compounds such as diphenylvinylphosphine oxide, triphenylphosphine oxide, trialkylphosphine oxide, and tris(hydroxyalkyl)phosphine oxide.

[0060] Examples of the curing accelerator include dicyandiamide (DICY) and its derivatives, melamine and its derivatives, boron trifluoride-amine complex, organic acid hydrazide, diaminomaleonitrile (DAMN) and its derivatives, guanamine and its derivatives, aminimide, and polyamine.

[0061] The additive may include an acrylic polymer.

[0062] The non-reactive diluent is a component that is blended to appropriately adjust the viscosity, drying property, coatability, etc. of the photosensitive resin composition. Examples of the non-reactive diluent include organic solvents. Examples of the organic solvent include ketones such as methyl ethyl ketone, aromatic hydrocarbons such as benzene, toluene, and xylene, alcohols such as methanol, n-propanol, isopropanol, and cyclohexanol, alicyclic hydrocarbons such as cyclohexane and methylcyclohexane, cellosolves such as cellosolve and butyl cellosolve, carbitols such as carbitol and butyl carbitol, esters such as ethyl acetate, butyl acetate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, diethylene glycol monomethyl ether acetate, and ethyl diglycol acetate. These organic solvents may be used alone or in combination of two or more.

[0063] The method for producing the photosensitive resin composition of the present invention is not limited to a specific method, and the composition can be produced, for example, by blending the above-mentioned components in a predetermined ratio, and then kneading or mixing the mixture at room temperature (e.g., 25° C.) using a kneading means such as a triple roll mill, a ball mill, a sand mill, a bead mill, a kneader, or a stirring means such as a super mixer or a planetary mixer. Furthermore, prior to the kneading or mixing, pre-kneading or pre-mixing may be carried out as necessary.

[0064] Next, an example of a method for using the photosensitive resin composition of the present invention will be described. Here, a method for applying the photosensitive resin composition of the present invention as an insulating film (e.g., a solder resist film) onto a flexible printed wiring board having a circuit pattern formed by etching copper foil on a substrate will be described.

[0065] The photosensitive resin composition of the present invention is applied to a desired thickness on a flexible printed wiring board using a known coating method such as screen printing, a spray coater, a bar coater, an applicator, a blade coater, a knife coater, a roll coater, or a gravure coater. After application, when a non-reactive diluent is blended in the photosensitive resin composition, a pre-drying is performed by heating at a temperature of about 70 to 120°C for about 10 to 60 minutes in order to volatilize the non-reactive diluent in the photosensitive resin composition, thereby forming a tack-free coating film. Next, the photosensitive resin composition is directly irradiated with active energy rays (e.g., ultraviolet rays) according to a desired pattern using a direct imaging device, and the coating film is photocured in the pattern. Next, the non-exposed region is removed with a dilute alkaline aqueous solution, and the photocured coating film is developed. For example, a spray method, a shower method, or the like is used as the development method. For example, a 0.5 to 5 mass % aqueous sodium carbonate solution is used as the dilute alkaline aqueous solution. Next, a heat curing treatment (post cure) is performed for 20 to 80 minutes using a hot air circulation dryer or the like at 130 to 170°C to heat cure the developed photocured film, thereby forming a cured product of the photosensitive resin composition having a desired pattern on the flexible printed wiring board. EXAMPLES

[0066] Next, examples of the present invention will be described, but the present invention is not limited to these examples as long as they do not depart from the spirit of the present invention.

[0067] Examples 1 to 9, Comparative Examples 1 to 4 The components shown in Table 1 below were mixed in the mixing ratios shown in Table 1 below and mixed and dispersed at room temperature using a three-roll mill to prepare photosensitive resin compositions used in Examples 1 to 9 and Comparative Examples 1 to 4. The amount of each component shown in Table 1 below means parts by mass unless otherwise specified.

[0068] Details of each component in Table 1 are as follows.

[0069] (A) Aromatic ring-containing carboxyl group-containing photosensitive resin ·Synthetic resin A A 500 mL four-neck flask equipped with a stirrer, thermometer, and reflux condenser was charged with 125 g of dipropylene glycol monomethyl ether (hereinafter referred to as "DPM") and heated to 120°C under a nitrogen atmosphere. A mixed solution of 34.4 g (0.4 mol) of methacrylic acid, 74.2 g (0.36 mol) of phenoxyethyl methacrylate (Sartomer Corporation, SR-340, PEMA), 5.5 g of dimethyl 2,2'-azobis(2-methylpropionate) (Wako Pure Chemical Industries, Ltd., V-601, DMAMP), and 10 g of DPM was added dropwise over approximately 1 hour, and the mixture was stirred at 120°C for 3 hours to obtain a copolymer having a carboxyl group. Next, after lowering the temperature in the flask to 100°C, a mixture of air and nitrogen (air volume to nitrogen volume ratio 1:2) was passed through the flask at 200mL / min, while 4-hydroxybutyl acrylate glycidyl ether (Nippon Kasei Co., Ltd., 4-HBAGE, 30.0g (0.15mol), 0.3g of triphenylphosphine (TPP) as a reaction catalyst, and 0.1g of methoxyhydroquinone (MEHQ) as a polymerization inhibitor were added, and the reaction was continued at 100°C for 5 hours, and then at 115°C until the decrease in acid value was completed, producing a DPM solution containing about 52% by mass of copolymer resin (A-2 copolymer resin), and obtaining a copolymer resin. The weight average molecular weight was about 16000 (polystyrene equivalent), and the solid acid value was 97mgKOH / g.

[0070] (B) Rutile titanium dioxide CR-80: Chlorine method rutile titanium dioxide, oil absorption 20g / 100g, Ishihara Sangyo Kaisha, Ltd. R-550: Sulfuric acid method rutile type titanium dioxide, oil absorption 23g / 100g, Ishihara Sangyo Kaisha, Ltd. R-780: Sulfuric acid method rutile type titanium dioxide, oil absorption 33g / 100g, Ishihara Sangyo Kaisha, Ltd.

[0071] (C) Photopolymerization initiator OXE-02: Ethanone 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(0-acetyloxime), ADEKA Corporation

[0072] (D) Reactive diluent EBECRYL8405: Urethane acrylate, Daicel Corporation

[0073] (E) Epoxy compounds EPICLON 850-S: Bisphenol A epoxy resin, DIC Corporation

[0074] (F) Wetting and dispersing agent ·DISPERBYK-111: Acid group-containing copolymer, acid value 129mgKOH / g, BYK company DISPERBYK-180: alkylol ammonium salt copolymer containing acid groups, acid value 94 mg KOH / g, BYK DISPERBYK-118: Linear polymer with pigment-compatible groups, acid value 36 mg KOH / g, BYK

[0075] Flame retardants · Exolit OP-935: Clariant Japan Curing Accelerator DICY-7: Mitsubishi Chemical Corporation Melamine: Nissan Chemical Industries, Ltd. Additives ·AC-303: Shin-Etsu Chemical Co., Ltd. Non-reactive diluents ·EDGAC: Sanyo Chemical Industries, Ltd.

[0076] Anatase type titanium dioxide A-100: Sulfuric acid method anatase type titanium dioxide, oil absorption 22g / 100g, Ishihara Sangyo Kaisha, Ltd.

[0077] Test specimen production process Substrate: Polyimide film (film thickness 25 μm, copper foil thickness 12 μm, Nippon Steel Sumikin Chemical Co., Ltd. "ESPANEX") Surface treatment: 5% sulfuric acid treatment Printing method: Screen printing Dry film thickness: 20μm Pre-drying: 80℃, 20 minutes Exposure: 200 mJ / cm on photosensitive resin composition 2 (Direct imaging exposure device "Nuvogo1000R" (light source: laser, main wavelength 375nm, 405nm), manufactured by Orbotech) Alkaline development: 1% by weight Na2CO3 aqueous solution, liquid temperature 30°C, spray pressure 0.2 MPa, development time 60 seconds Post-cure heat treatment: 150℃, 60 minutes

[0078] Evaluation items (1) Light reflectance The reflectance (initial reflectance) at 450 nm was measured for the test specimens on which the cured coating film had been formed after the main curing heat treatment using a spectrophotometer U-3414 (Hitachi, Ltd.: φ60 mm integrating sphere). In addition, after heat treatment in a reflow furnace under an N2 atmosphere at a reflow temperature of 260°C and a reflow time of 30 seconds, the reflectance at 450 nm was measured using a spectrophotometer U-3414 (Hitachi, Ltd.: φ60 mm integrating sphere) (reflectance after heating). The light reflectance was evaluated as follows, with a rating of △ or higher being considered a pass. ◎: Reflectance 85% or more both initially and after heating ○: Reflectance after heating is 80% or more and less than 85% △: Reflectance after heating is 75% or more but less than 80% ×: Reflectance after heating is less than 75%

[0079] (2) Adhesion In accordance with JIS K5600-5-6, 100 1 mm grids (10 x 10) were made on the test piece, and a peeling test (peel test) was conducted using cellophane tape. The peeled state of the grids was visually observed and rated according to the following criteria, with a rating of △ or higher being considered a pass. ◎: Peeling was not observed in 95 or more out of 100 pieces. ○: Peeling was not observed in 90 or more but less than 95 out of 100 pieces. △: Peeling was not observed in 50 to less than 90 pieces out of 100 pieces. ×: Less than 50 out of 100 pieces are peeled off

[0080] (3) Resolution The remaining lines in the exposed area formed through a specified photomask (line width 30 μm to 130 μm) were visually confirmed and rated according to the following criteria, with a rating of △ or higher being deemed a pass. ◎: Line 30~50μm, ○: Line 60~80μm, △: Line 90~110μm, ×: Line 120μm or more

[0081] (4) Alkaline developability After development, the presence or absence of residues on the copper body and polyimide was visually confirmed and rated according to the following criteria, with a rating of .DELTA. or higher being deemed a pass. ◎: Even after pre-drying at 80℃ for 60 minutes, no residue was left on either the copper or polyimide. ○: Even after pre-drying at 80°C for 40 minutes, no residue was left on either the copper or polyimide. △: Pre-drying at 80°C for 40 minutes left no residue on the copper body, but some residue remained on the polyimide. ×: Pre-drying at 80°C for 40 minutes left residue on both the copper body and the polyimide.

[0082] The evaluation results are shown in Table 1 below.

[0083] [Table 1]

[0084] From the above Table 1, in Examples 1 to 9, which contain a carboxyl group-containing photosensitive resin having an aromatic ring and rutile titanium oxide (rutile titanium dioxide), a photocured film having excellent alkali developability and excellent light reflectance can be obtained, and the adhesion to the substrate and the resolution of the cured coating film are also excellent. In particular, in Examples 1 to 6, which contain a wetting dispersant, there is a tendency for the light reflectance to be further improved. Furthermore, Examples 4 to 6, which contain a sulfuric acid method rutile titanium oxide with an oil absorption of 23 g / 100 g, show a well-balanced improvement in light reflectance and alkali developability compared to Examples 1 to 3, which contain a chlorine method rutile titanium oxide with an oil absorption of 20 g / 100 g. Furthermore, Example 6, which contained a wetting dispersant with an acid value of 36 mgKOH / g, showed further improvements in light reflectance, adhesion, resolution, and alkaline developability compared to Example 4, which contained a wetting dispersant with an acid value of 129 mgKOH / g, and Example 5, which contained a wetting dispersant with an acid value of 94 mgKOH / g.

[0085] On the other hand, as can be seen from Table 1 above, in Comparative Examples 1 to 4 in which anatase type titanium oxide was blended, including Comparative Examples 2 to 4 in which a wetting dispersant was further blended, the light reflectance could not be obtained. [Industrial Applicability]

[0086] The photosensitive resin composition of the present invention has excellent alkaline developability and can provide an insulating coating film with excellent light reflectance, and is therefore highly useful, particularly in the field of substrates on which light sources such as light-emitting diode elements (LEDs) are mounted.

Claims

1. A photosensitive resin composition comprising: (A) a carboxyl group-containing photosensitive resin having an aromatic ring; (B) rutile-type titanium oxide; (C) a photopolymerization initiator; (D) a reactive diluent; and (E) an epoxy compound.

2. 2. The photosensitive resin composition according to claim 1, wherein the rutile type titanium oxide (B) is a titanium oxide produced by a sulfuric acid process.

3. 3. The photosensitive resin composition according to claim 1, wherein the rutile-type titanium oxide (B) has an oil absorption of 30 g / 100 g or less.

4. 3. The photosensitive resin composition according to claim 1, wherein the rutile type titanium oxide (B) is a titanium oxide produced by a sulfuric acid process having an oil absorption of 30 g / 100 g or less.

5. The photosensitive resin composition according to claim 1 or 2, further comprising (F) a wetting and dispersing agent.

6. 6. The photosensitive resin composition according to claim 5, wherein the wetting and dispersing agent (F) has an acid value of 70 mg KOH / g or less.

7. 6. The photosensitive resin composition according to claim 5, wherein the rutile titanium oxide (B) is a titanium oxide produced by a sulfuric acid process having an oil absorption of 30 g / 100 g or less, and the wetting and dispersing agent (F) has an acid value of 70 mg KOH / g or less.

8. The (A) carboxyl group-containing photosensitive resin having an aromatic ring is (A-1) General formula (I) 【Chemistry 1】 (In the formula, R 1 represents a hydrogen atom or a methyl group), General formula (II) 【Chemistry 2】 (In the formula, R 1 represents a hydrogen atom or a methyl group, R 2 represents a phenyl group, an α-cumyl group, an alkoxy group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms of an alkyl group, a t-butyl group, an adamantyl group, or a trifluoromethyl group, and m is an integer of 0 or 1 to 3) and / or a compound represented by the general formula (III): 【Chemistry 3】 (In the formula, R 1 represents a hydrogen atom or a methyl group, R 2 represents a phenyl group, an α-cumyl group, an alkoxy group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms of an alkyl group, a t-butyl group, an adamantyl group, or a trifluoromethyl group; A 1 represents an alkylene group having 2 to 10 carbon atoms and containing a linear or cyclic skeleton, or a hydroxyalkylene group having 3 to 10 carbon atoms, m is 0 or an integer of 1 to 3, and p is an integer of 1 to 5), Or, (A-2) general formula (I) 【Chemistry 4】 (In the formula, R 1 represents a hydrogen atom or a methyl group), General formula (II) 【Chemistry 5】 (In the formula, R 1 represents a hydrogen atom or a methyl group, R 2 represents a phenyl group, an α-cumyl group, an alkoxy group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms of an alkyl group, a t-butyl group, an adamantyl group, or a trifluoromethyl group, and m is an integer of 0 or 1 to 3) and / or a compound represented by the general formula (III): 【Chemistry 6】 (In the formula, R 1 represents a hydrogen atom or a methyl group, R 2 represents a phenyl group, an α-cumyl group, an alkoxy group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms of an alkyl group, a t-butyl group, an adamantyl group, or a trifluoromethyl group; 1 represents an alkylene group having 2 to 10 carbon atoms having a straight-chain or cyclic skeleton or a hydroxyalkylene group having 3 to 10 carbon atoms, m is an integer of 0 or 1 to 3, and p is an integer of 1 to 5), to which a compound having an oxirane ring and an ethylenically unsaturated bond is added to a part of the carboxyl groups of a copolymer obtained by reacting a compound represented by the following formula (I):

9. The compound having an oxirane ring and an ethylenically unsaturated bond is represented by the general formula (IV): 【Chemistry 7】 (In the formula, R 1 represents a hydrogen atom or a methyl group; A 2 represents an alkylene group having 2 to 10 carbon atoms, and q is 0 or an integer of 1 to 5.

10. 3. The photosensitive resin composition according to claim 1, further comprising 100 parts by mass or more and 800 parts by mass or less of the rutile-type titanium oxide (B) relative to 100 parts by mass of the carboxyl group-containing photosensitive resin (A) having an aromatic ring.

11. 6. The photosensitive resin composition according to claim 5, further comprising 0.50 parts by mass or more and 15 parts by mass or less of the wetting and dispersing agent (F) relative to 100 parts by mass of the carboxyl group-containing photosensitive resin (A) having an aromatic ring.

12. 6. The photosensitive resin composition according to claim 5, further comprising 0.15 parts by mass or more and 3.0 parts by mass or less of the wetting and dispersing agent (F) relative to 100 parts by mass of the rutile type titanium oxide (B).

13. A cured product of the photosensitive resin composition according to claim 1 or 2.

14. A printed wiring board comprising the cured product according to claim 13.

Citation Information

Patent Citations

  • Photocurable thermosetting resin composition, dry film, cured product, and printed wiring board

    JP2017529551A

  • Photosensitive composition and printed wiring board

    WO2011030580A1

  • Photosetting and thermosetting solder resist composition, and printed wiring board using the same

    JP2007322546A

Cited By

  • Curable resin composition and printed wiring board

    JP2026104203A