Polishing composition, polishing method and production method of semiconductor substrate
The polishing composition with negative zeta potential abrasive grains and alkylamine compounds addresses the issue of selectivity and defects in polishing low-k materials and silicon nitride, achieving high polishing rates and reduced surface defects.
Patent Information
- Application Number
- JP2023127009
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2023-08-03
- Publication Date
- 2024-10-09
AI Technical Summary
Existing polishing compositions fail to achieve a suitable polishing rate selectivity and increase defects on the silicon oxide surface when polishing low-k materials like SiOC and silicon nitride, particularly in substrates containing both silicon oxide and silicon nitride.
A polishing composition containing abrasive grains with a negative zeta potential and an alkylamine compound with 2 to 15 carbon atoms, maintained at a pH of less than 7, enhances the polishing rate of low-k materials and silicon nitride while maintaining appropriate selectivity ratios and reducing surface defects.
The composition achieves high polishing rates for low-k materials and silicon nitride with selectivity ratios between 1.0 and 2.0, and reduces surface defects such as scratches on silicon oxide.
Smart Images

Figure 2024139651000001 
Figure 2024139651000002 
Figure 2024139651000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing composition, a polishing method, and a method for producing a semiconductor substrate. [Background technology]
[0002] In recent years, new microfabrication technologies have been developed to accompany the high integration and high performance of LSI (Large Scale Integration). Chemical mechanical polishing (CMP) is one of these technologies, and is frequently used in the LSI manufacturing process, especially in the multi-layer wiring formation process, for planarizing interlayer insulating films, forming metal plugs, and forming buried wiring (damascene wiring).
[0003] In order to suppress the capacitance between wiring, low-dielectric constant (Low-k) materials are being adopted as materials for the interlayer insulating film in the multi-layer wiring formation process. SiOC (carbon-containing silicon oxide, SiO2 doped with C) formed by the plasma CVD method is widely used as a low-dielectric constant (Low-k) material.
[0004] As a technique for polishing SiOC, Patent Document 1 discloses a polishing composition containing cerium-containing abrasive grains and hydroxyalkyl cellulose, and having a pH of 6.0 or more. According to Patent Document 1, such a composition is said to improve the polishing rate of SiOC. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-139349 A Summary of the Invention [Problem to be solved by the invention]
[0006] Recently, substrates containing both low-k material, typically SiOC, and silicon nitride (Si3N4) have come to be used. In such substrates, there is an increasing demand for polishing low-k material and silicon nitride at a high polishing rate while polishing at a moderate polishing rate selectivity (for example, polishing rate of low-k material / polishing rate of silicon nitride=1.0 or more and 2.0 or less). However, the polishing composition described in Patent Document 1 has a problem of not satisfying such requirements.
[0007] Substrates containing both silicon oxide and silicon nitride are also becoming used. For such substrates, there is an increasing demand to polish silicon oxide and silicon nitride at a high polishing rate while polishing with an appropriate polishing rate selectivity (e.g., polishing rate of silicon nitride / polishing rate of silicon oxide=1.5 to 2.5), and to reduce defects on the silicon oxide surface after polishing.
[0008] The present invention has been made in view of the above circumstances, and has an object to provide a means capable of polishing low-k materials and silicon nitride at a high polishing rate, and capable of achieving an appropriate selectivity ratio of the polishing rate for the low-k material to the polishing rate for silicon nitride.
[0009] Another object of the present invention is to provide a means for polishing silicon oxide and silicon nitride at a high polishing rate, while maintaining an appropriate selectivity ratio of the polishing rate of silicon nitride to that of silicon oxide, and reducing defects on the silicon oxide surface after polishing. [Means for solving the problem]
[0010] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that at least one of the above problems can be solved by a polishing composition that contains abrasive grains and an alkylamine compound having at least one linear or branched alkyl group having 2 to 15 carbon atoms, has a pH of less than 7, and has a negative zeta potential of the abrasive grains in the polishing composition, and have completed the present invention. Effect of the Invention
[0011] According to the present invention, a means can be provided that can polish low-k materials and silicon nitride at a high polishing rate and can achieve an appropriate selectivity ratio of the polishing rate of the low-k material to the polishing rate of silicon nitride.
[0012] Furthermore, the present invention can provide a means for polishing silicon oxide and silicon nitride at a high polishing rate while maintaining an appropriate selectivity ratio of the polishing rate of silicon nitride to the polishing rate of silicon oxide, and for reducing defects on the silicon oxide surface after polishing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] According to one embodiment of the present invention, there is provided a polishing composition comprising an abrasive grain and an alkylamine compound having at least one linear or branched alkyl group having 2 to 15 carbon atoms, and having a pH of less than 7, wherein the zeta potential of the abrasive grain in the polishing composition is negative. According to such a polishing composition of the present invention, low-k materials and silicon nitride can be polished at a high polishing rate, and the selectivity ratio of the polishing rate of the low-k material to the polishing rate of silicon nitride can be made moderate (e.g., polishing rate of low-k material / polishing rate of silicon nitride=1.0 to 2.0). Furthermore, according to the polishing composition of the present invention, while polishing silicon oxide and silicon nitride at a high polishing rate, the selectivity ratio of the polishing rate of silicon nitride to the polishing rate of silicon oxide can be made moderate (e.g., polishing rate of silicon nitride / polishing rate of silicon oxide=1.5 to 2.5), and defects (e.g., scratches) on the silicon oxide surface after polishing can be reduced.
[0014] The details of why the polishing composition of the present invention can achieve the above-mentioned effects are unclear. However, the effects on the polishing object containing low-k material and silicon nitride are considered to be due to the following mechanism. Note that this mechanism is based on speculation, and the technical scope of the present invention is not limited by this mechanism.
[0015] Although the surface of a low-k material is generally hydrophobic, an alkylamine compound is easily adsorbed to the low-k material. When an alkylamine compound is adsorbed to the surface of a low-k material, the chemical bonds of the low-k material are easily distorted and embrittled. This increases the polishing rate of the low-k material. In addition, the polishing composition according to the present invention has a pH of less than 7.0, and under such conditions, the zeta potential of the silicon nitride surface is positive. Due to electrostatic attraction, the abrasive grains having a negative zeta potential contained in the polishing composition are easily approached to the silicon nitride surface having a positive zeta potential, and the polishing rate of silicon nitride is also increased. As a result, the polishing rates of both the low-k material and silicon nitride are increased (for example, 300 Å / min or more), and the selectivity of the polishing rate of the low-k material to the polishing rate of silicon nitride can be made moderate (for example, the polishing rate of the low-k material / polishing rate of silicon nitride=1.0 or more and 2.0 or less). Furthermore, the polishing composition of the present invention can reduce defects (eg, scratches) on the surface of an object to be polished (particularly silicon nitride) after polishing.
[0016] The embodiments of the present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified in various ways within the scope of the claims. The embodiments described in this specification can be combined in any way to form other embodiments. In this specification, unless otherwise specified, operations and measurements of physical properties are performed under conditions of room temperature (20°C to 25°C) and relative humidity of 40% RH to 50% RH.
[0017] [Abrasive grain] The polishing composition according to the present invention contains abrasive grains. The abrasive grains have the function of mechanically polishing an object to be polished, and increase the polishing rate of the object to be polished by the polishing composition.
[0018] In the polishing composition of the present invention, the abrasive grains have a negative zeta potential. Here, the "zeta (ζ) potential" refers to the potential difference that occurs at the interface between a solid and a liquid that are in contact with each other when they undergo relative motion. When the zeta potential of the abrasive grains is 0 mV or more (0 mV or positive), the polishing speed of low-k materials, silicon nitride, and silicon oxide decreases.
[0019] In the polishing composition of the present invention, the zeta potential of the abrasive grains is preferably -60 mV or more and -10 mV or less, more preferably -50 mV or more and -10 mV or less, and even more preferably -45 mV or more and -15 mV or less. When the abrasive grains have a zeta potential in such a range, the polishing speed of the object to be polished can be further improved. In addition, the selectivity of the polishing speed of the low-k material to the polishing speed of silicon nitride can be made appropriate (for example, the polishing speed of the low-k material / polishing speed of silicon nitride=1.0 or more and 2.0 or less). In addition, the selectivity of the polishing speed of silicon nitride to the polishing speed of silicon oxide can be made appropriate (for example, the polishing speed of silicon nitride / polishing speed of silicon oxide=1.5 or more and 2.5 or less).
[0020] Here, the zeta potential of the abrasive grains in the polishing composition is a value measured by the method described in the Examples. The zeta potential of the abrasive grains can be adjusted by the amount of anionic groups (particularly organic acid groups) contained in the abrasive grains described below, the pH of the polishing composition, etc.
[0021] The type of abrasive grains is not particularly limited, and examples thereof include metal oxides such as silica, alumina, zirconia, and titania. The abrasive grains can be used alone or in combination of two or more kinds. The abrasive grains may be either commercially available products or synthetic products.
[0022] The type of abrasive grain is preferably silica, more preferably colloidal silica.The method for producing colloidal silica includes sodium silicate method and sol-gel method, and the colloidal silica produced by any method can be suitably used as the abrasive grain of the present invention.However, from the viewpoint of reducing metal impurities, the colloidal silica produced by the sol-gel method is preferred because it can be produced with high purity.
[0023] Colloidal silica can be produced by the sol-gel method using a conventionally known method. Specifically, colloidal silica can be obtained by using a hydrolyzable silicon compound (e.g., alkoxysilane or a derivative thereof) as a raw material and carrying out a hydrolysis-condensation reaction.
[0024] In some embodiments of the present invention, the colloidal silica contained in the polishing composition is preferably anion-modified colloidal silica (anion-modified colloidal silica), more preferably colloidal silica with organic acid fixed on the surface. Colloidal silica with organic acid fixed on the surface tends to have a larger absolute value of zeta potential in the polishing composition than normal colloidal silica with no organic acid fixed on the surface. Therefore, the zeta potential of colloidal silica in the polishing composition is easily adjusted to be negative.
[0025] Preferred examples of colloidal silica having an organic acid fixed to its surface include colloidal silica having an organic acid group, such as a carboxylic acid group, a sulfonic acid group, a phosphonic acid group, or an aluminic acid group, fixed to its surface. Among these, from the viewpoint of ease of production, colloidal silica having a sulfonic acid or a carboxylic acid fixed to its surface is preferred, and colloidal silica having a sulfonic acid fixed to its surface is more preferred.
[0026] The immobilization of an organic acid on the surface of colloidal silica cannot be achieved by simply allowing colloidal silica and an organic acid to coexist. For example, if sulfonic acid, which is a type of organic acid, is to be immobilized on colloidal silica, it can be achieved by the method described in, for example, “Sulfonic acid-functionalized silica through quantitative oxidation of thiol groups”, Chem. Commun. 246-247 (2003). Specifically, a silane coupling agent having a thiol group, such as 3-mercaptopropyltrimethoxysilane, is coupled to colloidal silica, and then the thiol group is oxidized with hydrogen peroxide to obtain colloidal silica with sulfonic acid immobilized on the surface (sulfonic acid-modified colloidal silica, sulfonic acid-modified colloidal silica).
[0027] Alternatively, when a carboxylic acid, which is a type of organic acid, is immobilized on colloidal silica, it can be carried out by, for example, the method described in “Novel Silane Coupling Agents Containing a Photolabile 2-Nitrobenzyl Ester for Introduction of a Carboxy Group on the Surface of Silica Gel”, Chemistry Letters, 3, 228-229 (2000). Specifically, a silane coupling agent containing a photoreactive 2-nitrobenzyl ester is coupled to colloidal silica, followed by light irradiation, to obtain colloidal silica with a carboxylic acid immobilized on the surface (carboxylic acid-modified colloidal silica, carboxylic acid-modified colloidal silica).
[0028] The shape of the abrasive grains is not particularly limited, and may be spherical or non-spherical. Specific examples of non-spherical shapes include polygonal prisms such as triangular prisms and square prisms, cylinders, bales in which the center of a cylinder is bulged out more than the ends, donut shapes in which the center of a disk is penetrated, plates, so-called cocoon shapes with a constriction in the center, so-called association-type spheres in which multiple particles are integrated, so-called confetti shapes with multiple protrusions on the surface, and rugby ball shapes, and various other shapes are not particularly limited.
[0029] The size of the abrasive grains is not particularly limited. For example, the average primary particle diameter of the abrasive grains is preferably 5 nm or more, more preferably 8 nm or more, even more preferably 10 nm or more, and particularly preferably 12 nm or more. As the average primary particle diameter of the abrasive grains increases, the polishing speed of the object to be polished by the polishing composition increases. In addition, the average primary particle diameter of the abrasive grains is preferably 100 nm or less, more preferably 80 nm or less, and even more preferably 50 nm or less. As the average primary particle diameter of the abrasive grains decreases, it becomes easier to obtain a surface with fewer defects by polishing with the polishing composition. That is, the average primary particle diameter of the abrasive grains is preferably 5 nm or more and 100 nm or less, more preferably 8 nm or more and 80 nm or less, even more preferably 10 nm or more and 50 nm or less, and particularly preferably 12 nm or more and 50 nm or less. The average primary particle diameter of the abrasive grains can be calculated, for example, based on the specific surface area (SA) of the abrasive grains calculated by the BET method, assuming that the shape of the abrasive grains is a true sphere. In this specification, the average primary particle size of the abrasive grains is a value measured by the method described in the Examples.
[0030] In addition, the average secondary particle diameter of the abrasive grains is preferably 10 nm or more, more preferably 15 nm or more, even more preferably 20 nm or more, and particularly preferably 25 nm or more. As the average secondary particle diameter of the abrasive grains increases, the resistance during polishing decreases, and stable polishing becomes possible. In addition, the average secondary particle diameter of the abrasive grains is preferably 400 nm or less, more preferably 300 nm or less, even more preferably 200 nm or less, particularly preferably 100 nm or less, and most preferably 80 nm or less. As the average secondary particle diameter of the abrasive grains decreases, the surface area per unit mass of the abrasive grains increases, the contact frequency with the object to be polished increases, and the polishing speed increases. That is, the average secondary particle diameter of the abrasive grains is preferably 10 nm or more and 400 nm or less, more preferably 15 nm or more and 300 nm or less, even more preferably 20 nm or more and 200 nm or less, even more preferably 25 nm or more and 100 nm or less, and particularly preferably 25 nm or more and 80 nm or less. The average secondary particle size of the abrasive grains can be measured by, for example, a dynamic light scattering method such as a laser diffraction scattering method.
[0031] The average degree of association of the abrasive grains is preferably 5.0 or less, more preferably 4.0 or less, even more preferably 3.0 or less, and particularly preferably 2.5 or less. As the average degree of association of the abrasive grains decreases, defects can be reduced more. The average degree of association of the abrasive grains is also preferably 1.0 or more, more preferably 1.5 or more, and even more preferably 2.0 or more. This average degree of association is obtained by dividing the value of the average secondary particle diameter of the abrasive grains by the value of the average primary particle diameter. As the average degree of association of the abrasive grains increases, there is an advantageous effect that the polishing speed of the object to be polished by the polishing composition improves.
[0032] The upper limit of the aspect ratio of the abrasive grains in the polishing composition is not particularly limited, but is preferably less than 2.0, more preferably 1.8 or less, and even more preferably 1.5 or less. In such a range, defects on the surface of the object to be polished can be further reduced. The aspect ratio is the average of the values obtained by taking the smallest rectangle that circumscribes the image of the abrasive grains by a scanning electron microscope, and dividing the length of the long side of the rectangle by the length of the short side of the same rectangle, and can be determined using general image analysis software. The lower limit of the aspect ratio of the abrasive grains in the polishing composition is not particularly limited, but is preferably 1.0 or more, and more preferably 1.2 or more.
[0033] In the particle size distribution of abrasive grains obtained by laser diffraction scattering method, the lower limit of D90 / D10, which is the ratio of the particle diameter (D90) when the cumulative particle mass from the fine particle side reaches 90% of the total particle mass and the particle diameter (D10) when the cumulative particle mass from the fine particle side reaches 10% of the total particle mass of all particles, is not particularly limited, but is preferably 1.1 or more, more preferably 1.4 or more, even more preferably 1.7 or more, and most preferably 2.0 or more. In addition, in the particle size distribution of abrasive grains in a polishing composition obtained by laser diffraction scattering method, the upper limit of the ratio D90 / D10, which is the particle diameter (D90) when the cumulative particle mass from the fine particle side reaches 90% of the total particle mass and the particle diameter (D10) when the cumulative particle mass from the fine particle side reaches 10% of the total particle mass of all particles, is not particularly limited, but is preferably 3.0 or less, more preferably 2.5 or less. Within such a range, defects on the surface of the object to be polished can be reduced more.
[0034] The size of the abrasive grains (average primary particle size, average secondary particle size, aspect ratio, D90 / D10, etc.) can be appropriately controlled by selecting the manufacturing method of the abrasive grains, etc.
[0035] The concentration (content) of the abrasive grains is not particularly limited, but is preferably 0.5% by mass or more, more preferably 0.8% by mass or more, even more preferably 1% by mass or more, even more preferably more than 1% by mass, and particularly preferably 1.5% by mass or more, based on the total mass of the polishing composition. The upper limit of the concentration (content) of the abrasive grains is preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5% by mass or less, based on the total mass of the polishing composition. That is, the concentration (content) of the abrasive grains is preferably 0.5% by mass or more and 20% by mass or less, more preferably 0.8% by mass or more and 20% by mass or less, even more preferably 1% by mass or more and 15% by mass or less, even more preferably more than 1% by mass and 10% by mass or less, and particularly preferably 1.5% by mass or more and 5% by mass or less, based on the total mass of the polishing composition. Within such a range, the polishing speed can be improved while suppressing costs. When the polishing composition contains two or more types of abrasive grains, the concentration (content) of the abrasive grains means the total amount of these.
[0036] [Alkylamine compounds] The polishing composition according to the present invention contains an alkylamine compound having at least one linear or branched alkyl group having 2 to 15 carbon atoms (hereinafter, also simply referred to as "alkylamine compound"). As described above, the alkylamine compound has the effect of distorting the chemical bonds of the low-k material, and can improve the polishing speed of the low-k material. In addition, the alkylamine compound can reduce defects (e.g., scratches) on the silicon oxide surface after polishing.
[0037] The alkylamine compound according to the present invention has at least one linear or branched alkyl group having a carbon number of 2 to 15. Any compound having such an alkyl group may be used, including monoalkylamine compounds (primary alkylamine compounds), dialkylamine compounds (secondary alkylamine compounds), and trialkylamine compounds (tertiary alkylamine compounds).
[0038] One of the factors that causes the increase in scratches is that the abrasive grains and organic residues (e.g., polishing pad debris) form a complex, which causes localized polishing. The alkylamine compound according to the present invention, which has at least one linear or branched alkyl group having 2 to 15 carbon atoms, is likely to adsorb to both the abrasive grains and organic residues (e.g., polishing pad debris). As a result, it is believed that a steric hindrance is brought about between the abrasive grains and the organic residues, which inhibits the formation of a complex between the abrasive grains and the organic residues, thereby inhibiting scratches.
[0039] In the case of an alkylamine compound having only an alkyl group with one carbon atom (methyl group), the effect of distorting the chemical bonds of the low-k material is reduced, and the polishing speed of the low-k material is reduced. In addition, it becomes difficult to adsorb to both abrasive grains and organic residues (e.g. polishing pad debris), making it difficult to suppress the formation of complexes due to the above-mentioned steric hindrance, and scratches tend to increase.
[0040] In the case of an alkylamine compound having only an alkyl group with more than 15 carbon atoms, it is easy to adsorb to the surface of silicon nitride, and acts like a protective film for silicon nitride, decreasing the polishing speed of silicon nitride. In addition, the abrasive grains are easy to aggregate, and scratches increase. In the case of a dialkylamine compound (secondary alkylamine compound) and a trialkylamine compound (tertiary alkylamine compound), as long as they have at least one alkyl group with 2 to 15 carbon atoms, the other alkyl group may be an alkyl group with 1 carbon atom (methyl group) or an alkyl group with more than 15 carbon atoms, but preferably they are compounds having only an alkyl group with 2 to 15 carbon atoms.
[0041] Examples of the linear or branched alkyl group having from 2 to 15 carbon atoms include, for example, an ethyl group, an n-propyl group, an isopropyl group, a 2-methylpropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an iso-amyl group, a tert-pentyl group, a neopentyl group, an n-hexyl group, a 3-methylpentan-2-yl group, a 3-methylpentan-3-yl group, a 4-methylpentyl group, a 4-methylpentan-2-yl group, a 1,3-dimethylbutyl group, a 3,3-dimethylbutyl group, a 3,3-dimethylbutan-2-yl group, a 2-methyl ... yl group, n-heptyl group, 1-methylhexyl group, 3-methylhexyl group, 4-methylhexyl group, 5-methylhexyl group, 1-ethylpentyl group, 1-(n-propyl)butyl group, 1,1-dimethylpentyl group, 1,4-dimethylpentyl group, 1,1-diethylpropyl group, 1,3,3-trimethylbutyl group, 1-ethyl-2,2-dimethylpropyl group, n-octyl group, 2-ethylhexyl group, 2-methylhexan-2-yl group, 2,4-dimethylpentan-3-yl group, 1,1-dimethylpentan-1-yl group, 2,2-dimethylhexane-3 -yl group, 2,3-dimethylhexane-2-yl group, 2,5-dimethylhexane-2-yl group, 2,5-dimethylhexane-3-yl group, 3,4-dimethylhexane-3-yl group, 3,5-dimethylhexane-3-yl group, 1-methylheptyl group, 2-methylheptyl group, 5-methylheptyl group, 2-methylheptan-2-yl group, 3-methylheptan-3-yl group, 4-methylheptan-3-yl group, 4-methylheptan-4-yl group, 1-ethylhexyl group, 2-ethylhexyl group, 1-propylpentyl group, 2-propylpentyl group, 1,1 -Dimethylhexyl group, 1,4-dimethylhexyl group, 1,5-dimethylhexyl group, 1-ethyl-1-methylpentyl group, 1-ethyl-4-methylpentyl group, 1,1,4-trimethylpentyl group, 2,4,4-trimethylpentyl group, 1-isopropyl-1,2-dimethylpropyl group, 1,1,3,3-tetramethylbutyl group, n-nonyl group, 1-methyloctyl group, 6-methyloctyl group, 1-ethylheptyl group, 1-(n-butyl)pentyl group, 4-methyl-1-(n-propyl)pentyl group, 1,5,5-trimethylhexyl group, 1,1,Examples of the alkyl groups include 5-trimethylhexyl, 2-methyloctane-3-yl, n-decyl, 1-methylnonyl, 1-ethyloctyl, 1-(n-butyl)hexyl, 1,1-dimethyloctyl, 3,7-dimethyloctyl, n-undecyl, 1-methyldecyl, 1-ethylnonyl, n-dodecyl, 1-methylundecyl, n-tridecyl, n-tetradecyl, 1-methyltridecyl, and n-pentadecyl. The two or more alkyl groups in the dialkylamine compound (secondary alkylamine compound) and the trialkylamine compound (tertiary alkylamine compound) may be the same or different.
[0042] More specific examples of the alkylamine compound include monoalkylamine compounds (primary alkylamine compounds) such as ethylamine, n-propylamine, isopropylamine, n-butylamine, isobutylamine, sec-butylamine, tert-butylamine, n-pentylamine, n-hexylamine, n-heptylamine, n-octylamine, n-nonylamine, n-decylamine, n-undecylamine, n-dodecylamine, n-tridecylamine, n-tetradecylamine, and n-pentadecylamine; Dialkylamine compounds (secondary alkylamine compounds) such as diethylamine, di-n-propylamine, diisopropylamine, di-n-butylamine, diisobutylamine, di-sec-butylamine, di-n-pentylamine, ethylmethylamine, methyl-n-propylamine, methyl-n-butylamine, methyl-n-pentylamine, methyl-n-octylamine, methyl-n-decylamine, methyl-n-dodecylamine, methyl-n-tetradecylamine, methyl-n-hexadecylamine, methyl-n-octadecylamine, ethylisopropylamine, ethyl-n-butylamine, ethyl-n-pentylamine, ethyl-n-octylamine, di-n-hexylamine, di-n-octylamine, and di-n-dodecylamine; Trialkylamine compounds (tertiary alkylamine compounds) such as triethylamine, tri-n-propylamine, tri-n-butylamine, tri-n-pentylamine, tri-n-hexylamine, tri-n-octylamine, tri-n-dodecylamine, dimethylethylamine, dimethyl-n-butylamine, dimethyl-n-hexylamine, dimethyl-n-octylamine, dimethyl-n-decylamine, diethyl-n-decylamine, dimethyl-n-dodecylamine, and dimethyl-n-tetradecylamine; These alkylamine compounds may be used alone or in combination of two or more. In addition, the alkylamine compounds may be commercially available products or synthetic products.
[0043] From the viewpoint of further improving the effect of the present invention, the alkylamine compound is preferably a monoalkylamine compound having only one linear or branched alkyl group having 2 to 15 carbon atoms. In addition, from the viewpoint of further reducing scratches on the surface of the object to be polished after polishing, the number of carbon atoms in the alkyl group of the alkylamine compound according to the present invention is more preferably 2 to 7, and even more preferably 2 to 6. When the number of carbon atoms in the alkyl group of the alkylamine compound is large, abrasive grains tend to aggregate more easily, and the number of scratches tends to increase.
[0044] In addition, from the viewpoints of availability and cost reduction, the alkyl group is preferably linear.
[0045] From the above, the alkylamine compound according to the present invention is more preferably at least one monoalkylamine compound selected from the group consisting of ethylamine, n-propylamine, n-butylamine, n-pentylamine, n-hexylamine, n-heptylamine, n-octylamine, n-nonylamine, n-decylamine, n-undecylamine, and n-dodecylamine.The alkylamine compound according to the present invention is more preferably at least one monoalkylamine compound selected from the group consisting of ethylamine, n-propylamine, n-butylamine, n-pentylamine, n-hexylamine, and n-heptylamine, and is particularly preferably at least one monoalkylamine compound selected from the group consisting of ethylamine, n-propylamine, n-butylamine, n-pentylamine, and n-hexylamine.
[0046] The lower limit of the concentration (content) of the alkylamine compound relative to the total mass of the polishing composition is preferably 0.001 mass% or more, more preferably 0.005 mass% or more, even more preferably 0.007 mass% or more, and particularly preferably 0.01 mass% or more. The upper limit of the concentration (content) of the alkylamine compound relative to the total mass of the polishing composition is preferably 3 mass% or less, more preferably 2 mass% or less, even more preferably 1 mass% or less, and particularly preferably 0.5 mass% or less. That is, the concentration (content) of the alkylamine compound relative to the total mass of the polishing composition is preferably 0.001 mass% or more and 3 mass% or less, more preferably 0.005 mass% or more and 2 mass% or less, even more preferably 0.007 mass% or more and 1 mass% or less, and particularly preferably 0.01 mass% or more and 0.5 mass% or less. By setting the concentration in such a range, it is possible to ensure stability while achieving the effect of reducing defects on the silicon oxide surface.
[0047] When the polishing composition contains two or more kinds of alkylamine compounds, the concentration (content) of the alkylamine compounds means the total amount thereof.
[0048] [Electrical conductivity adjuster] The polishing composition according to one embodiment of the present invention preferably further contains an electrical conductivity adjuster. The electrical conductivity adjuster adjusts the electrical conductivity of the polishing composition to an appropriate range, thereby, for example, improving the removal rate of silicon oxide or improving the dispersion stability of the polishing composition.
[0049] The electrical conductivity adjuster is not particularly limited as long as it is a compound having an electrical conductivity adjustment function, and for example, a salt compound can be used. Examples of the salt compound include salts of acid compounds and salts of basic compounds. The salt of the acid compound may be an organic acid salt or an inorganic acid salt.
[0050] Specific examples of the electrical conductivity adjuster include sodium nitrate, potassium nitrate, ammonium nitrate, magnesium nitrate, calcium nitrate, sodium nitrite, potassium nitrite, lithium acetate, sodium acetate, potassium acetate, ammonium acetate, calcium acetate, calcium lactate, lithium benzoate, sodium benzoate, potassium benzoate, lithium carbonate, sodium carbonate, potassium carbonate, magnesium carbonate, calcium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, ammonium carbonate, sodium bicarbonate, sodium sulfate, potassium sulfate, ammonium sulfate, calcium sulfate, magnesium sulfate, sodium sulfite, potassium sulfite, calcium sulfite, magnesium sulfite, potassium thiosulfate, lithium sulfate, magnesium sulfate, Examples of the electric conductivity regulator include sodium thiosulfate, sodium hydrogen sulfite, sodium hydrogen sulfate, potassium hydrogen sulfate, disodium oxalate, dipotassium oxalate, ammonium oxalate, ammonium citrate, disodium glutarate, lithium fluoride, sodium fluoride, potassium fluoride, calcium fluoride, ammonium fluoride, potassium chloride, sodium chloride, ammonium chloride, calcium chloride, potassium bromide, sodium bromide, ammonium bromide, calcium bromide, sodium iodide, potassium iodide, potassium triiodide, calcium iodide, trilithium phosphate, tripotassium phosphate, trisodium phosphate, triammonium phosphate, sodium monohydrogen phosphate, potassium monohydrogen phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, ammonium dihydrogen phosphate, etc. These electric conductivity regulators may be used alone or in combination of two or more.
[0051] Among these electrical conductivity adjusters, ammonium sulfate, potassium hydrogen carbonate, ammonium carbonate, potassium acetate, potassium nitrate, ammonium nitrate, dipotassium oxalate, and ammonium oxalate are preferred.
[0052] The concentration (content) of the electrical conductivity adjuster may be appropriately selected so that the polishing composition has a preferred electrical conductivity value, which will be described later. According to some embodiments, the concentration (content) of the electrical conductivity adjuster is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, based on the total mass of the polishing composition being 100% by mass. The concentration (content) of the electrical conductivity adjuster is preferably 5.0% by mass or less, more preferably 3.0% by mass or less, and even more preferably 2.0% by mass or less, based on the total mass of the polishing composition being 100% by mass. That is, the concentration (content) of the electrical conductivity adjuster is preferably 0.01% by mass or more and 5.0% by mass or less, more preferably 0.05% by mass or more and 3.0% by mass or less, and even more preferably 0.1% by mass or more and 2.0% by mass or less, based on the total mass of the polishing composition being 100% by mass. With a concentration in such a range, it is possible to ensure stability while achieving an improvement in the polishing rate of silicon oxide.
[0053] When the polishing composition contains two or more kinds of electrical conductivity adjusters, the concentration (content) of the electrical conductivity adjusters means the total amount thereof.
[0054] [pH and pH adjusters] The pH of the polishing composition according to the present invention is less than 7.0. When the pH is 7.0 or more, the polishing rate of low-k material and silicon nitride decreases. The pH is preferably 1.0 or more, more preferably 1.5 or more, and even more preferably 2.0 or more. The pH is preferably 6.0 or less, more preferably 5.0 or less, and even more preferably 4.5 or less. That is, the pH of the polishing composition according to the present invention is preferably 1.0 or more and 6.0 or less, more preferably 1.5 or more and 5.0 or less, and even more preferably 2.0 or more and 4.5 or less.
[0055] The polishing composition of the present invention preferably contains a pH adjuster for adjusting pH.The pH adjuster may be either an acid or a base, and may be either an inorganic compound or an organic compound.The pH adjuster may be used alone or in combination of two or more kinds.
[0056] Specific examples of acids that can be used as a pH adjuster include inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid; and organic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, lactic acid, diglycolic acid, 2-furancarboxylic acid, 2,5-furandicarboxylic acid, 3-furancarboxylic acid, 2-tetrahydrofurancarboxylic acid, methoxyacetic acid, methoxyphenylacetic acid, and phenoxyacetic acid.
[0057] Examples of bases that can be used as pH adjusters include amines such as aliphatic amines and aromatic amines, organic bases such as quaternary ammonium hydroxides, hydroxides of alkali metals such as sodium hydroxide and potassium hydroxide, hydroxides of Group 2 elements, and ammonia.
[0058] The amount of pH adjuster to be added is not particularly limited, and can be appropriately adjusted so that the polishing composition has a desired pH. The pH of the polishing composition can be measured, for example, by a pH meter, and specifically, can be measured by the method described in Examples.
[0059] [Dispersion medium] The polishing composition according to the present invention preferably further contains a dispersion medium. Examples of the dispersion medium include water; alcohols such as methanol, ethanol, and ethylene glycol; ketones such as acetone, and mixtures thereof. Of these, water is preferable as the dispersion medium. That is, according to a more preferred embodiment of the present invention, the dispersion medium contains water. According to a more preferred embodiment of the present invention, the dispersion medium is substantially composed of water. Note that the above "substantially" means that a dispersion medium other than water may be included as long as the objective effect of the present invention can be achieved, and more specifically, the dispersion medium is preferably composed of 90% by mass or more and 100% by mass or less of water and 0% by mass or more and 10% by mass or less of a dispersion medium other than water, and more preferably composed of 99% by mass or more and 100% by mass or less of water and 0% by mass or more and 1% by mass or less of a dispersion medium other than water. Most preferably, the dispersion medium is water.
[0060] From the viewpoint of not inhibiting the action of the components contained in the polishing composition, it is preferable for the dispersion medium to be water that contains as few impurities as possible. Specifically, pure water or ultrapure water from which impurity ions have been removed with an ion exchange resin and then foreign matter has been removed through a filter, or distilled water is more preferable.
[0061] [Electrical Conductivity of Polishing Composition] The electrical conductivity (EC) of the polishing composition according to the present invention is not particularly limited, but is preferably 0.5 mS / cm or more, more preferably 1 mS / cm or more, and even more preferably 1.5 mS / cm or more. The electrical conductivity (EC) of the polishing composition according to the present invention is preferably 20 mS / cm or less, more preferably 15 mS / cm or less, and even more preferably 10 mS / cm or less. That is, the electrical conductivity (EC) of the polishing composition according to the present invention is preferably 0.5 mS / cm or more and 20 mS / cm or less, more preferably 1 mS / cm or more and 15 mS / cm or less, and even more preferably 1.5 mS / cm or more and 10 mS / cm or less. If the electrical conductivity (EC) of the polishing composition is in such a range, the polishing rate of the low-k material and silicon nitride can be maintained high, and the repulsion between the abrasive grains can be appropriately adjusted to ensure stability. The polishing rate of silicon oxide can be further improved. The electrical conductivity of the polishing composition can be adjusted by the type and amount of the electrical conductivity adjuster, the type and amount of the pH adjuster, etc. The electrical conductivity of the polishing composition can be measured by the method described in the Examples.
[0062] [Other ingredients] The polishing composition of the present invention may further contain known additives that can be used in polishing compositions, such as water-soluble polymers, complexing agents, metal corrosion inhibitors, preservatives, antifungal agents, oxidizing agents, reducing agents, and surfactants, as necessary. Among these, the polishing composition preferably contains an antifungal agent. The polishing composition of the present invention is acidic. For this reason, it is more preferable that the polishing composition contains an antifungal agent. That is, in one embodiment of the present invention, the polishing composition is substantially composed of an abrasive grain, an alkylamine compound having at least one linear or branched alkyl group having 2 to 15 carbon atoms, a dispersion medium, and at least one selected from the group consisting of an electrical conductivity adjuster, a pH adjuster, and an antifungal agent. Here, "the polishing composition is substantially composed of an abrasive grain, an alkylamine compound having at least one linear or branched alkyl group having 2 to 15 carbon atoms, a dispersion medium, and at least one selected from the group consisting of an electric conductivity adjuster, a pH adjuster, and an antifungal agent" means that the total content of the abrasive grain, the alkylamine compound having at least one linear or branched alkyl group having 2 to 15 carbon atoms, a dispersion medium, and at least one selected from the group consisting of an electric conductivity adjuster, a pH adjuster, and an antifungal agent is more than 99 mass% (upper limit: 100 mass%) with respect to the total mass of the polishing composition. According to a preferred embodiment, the polishing composition is composed of an abrasive grain, an alkylamine compound having at least one linear or branched alkyl group having 2 to 15 carbon atoms, a dispersion medium, a pH adjuster, and an antifungal agent (the total content=100 mass%). According to another preferred embodiment, the polishing composition is composed of an abrasive grain, an alkylamine compound having at least one linear or branched alkyl group having 2 to 15 carbon atoms, a dispersion medium, an electrical conductivity adjuster, a pH adjuster, and an antifungal agent (the total content is 100% by mass). According to another preferred embodiment, the polishing composition is composed of an abrasive grain, an alkylamine compound having at least one linear or branched alkyl group having 2 to 15 carbon atoms, a dispersion medium, and a pH adjuster (the total content is 100% by mass).According to another preferred embodiment, the polishing composition is composed of abrasive grains, an alkylamine compound having at least one linear or branched alkyl group having 2 to 15 carbon atoms, a dispersion medium, an electrical conductivity adjuster, and a pH adjuster (the above total content = 100 mass%).
[0063] The following describes the antifungal agent (preservative), which is a preferred other component, and the oxidizing agent.
[0064] (Anti-mold agent) Examples of the antifungal agent (preservative) that can be added to the polishing composition of the present invention include isothiazoline-based preservatives such as 2-methyl-4-isothiazolin-3-one and 5-chloro-2-methyl-4-isothiazolin-3-one, paraoxybenzoic acid esters, and phenoxyethanol, etc. These antifungal agents (preservatives) may be used alone or in combination of two or more.
[0065] (Oxidizing agent) The polishing composition according to the present invention preferably does not substantially contain an oxidizing agent. If an oxidizing agent is contained in the polishing composition, the surface of the object to be polished may be oxidized to generate an oxide film, which may result in a longer polishing time. Specific examples of the oxidizing agent include hydrogen peroxide (H2O2), sodium persulfate, ammonium persulfate, and sodium dichloroisocyanurate. The polishing composition substantially does not contain an oxidizing agent means that the oxidizing agent is not intentionally contained at least. Therefore, a polishing composition that inevitably contains a small amount of an oxidizing agent due to raw materials, manufacturing method, etc. is included in the concept of a polishing composition that does not substantially contain an oxidizing agent. For example, the concentration (content) of the oxidizing agent relative to the total mass of the polishing composition is preferably 0.01 mass% (100 mass ppm) or less, more preferably less than 0.01 mass% (100 mass ppm), and even more preferably 0.005 mass% (50 mass ppm) or less. The lower limit of the concentration (content) of the oxidizing agent is preferably 0% by mass or more, and more preferably 0.0005% by mass (5 ppm by mass) or more.
[0066] [Form of polishing composition] The polishing composition according to the present invention is typically supplied to an object to be polished in the form of a polishing liquid containing the polishing composition, and is used to polish the object to be polished. The polishing composition according to the present invention may be used as a polishing liquid after dilution (typically diluted with water), or may be used as a polishing liquid as it is. That is, the concept of the polishing composition according to the present invention includes both a polishing composition (working slurry) that is supplied to an object to be polished and used to polish the object to be polished, and a concentrated liquid (original working slurry liquid) that is diluted and used for polishing. The concentration ratio of the concentrated liquid can be, for example, about 2 to 100 times on a volume basis, and is usually about 3 to 50 times.
[0067] [Polished object] The object to be polished according to the present invention is not particularly limited, and examples thereof include single crystal silicon, polycrystalline silicon (polysilicon), polycrystalline silicon doped with n-type or p-type impurities, amorphous silicon, amorphous silicon doped with n-type or p-type impurities, silicon oxide, silicon nitride, silicon carbonitride (SiCN), metals, SiGe, carbon-containing materials, low dielectric constant materials (Low-k materials), and the like.
[0068] Examples of objects to be polished that contain silicon oxide include a TEOS-type silicon oxide film (hereinafter simply referred to as "TEOS" or "TEOS film") produced using tetraethyl orthosilicate as a precursor, a high density plasma (HDP) film, an undoped silicate glass (USG) film, a phosphorus silicate glass (PSG) film, a boron-phosphorus silicate glass (BPSG) film, and a rapid thermal oxidation (RTO) film.
[0069] Examples of metals include tungsten, copper, aluminum, cobalt, hafnium, nickel, gold, silver, platinum, palladium, rhodium, ruthenium, iridium, and osmium.
[0070] Examples of carbon-containing materials include amorphous carbon, spin-on carbon (SOC), diamond-like carbon (DLC), nanocrystalline diamond, graphene, and other materials other than low-k materials.
[0071] A low-dielectric constant material (Low-k material) is a material with a relative dielectric constant k lower than that of silicon oxide, and is preferably a material with a relative dielectric constant k of 3.0 or less. Specific examples include silicon carbide (SiC), carbon-containing silicon oxide (SiOC), silicon oxide containing a methyl group, benzocyclobutene (BCB), fluorinated silicon oxide (SiOF), HSQ (hydrogen silsesquioxane), MSQ (methyl silsesquioxane), HMSQ (hydride-methyl silsesquioxane), polyimide-based polymers, arylene ether-based polymers, cyclobutene-based polymers, and perfluorocyclobutene (PFCB).
[0072] The object to be polished may be a commercially available product or may be produced by a known method.
[0073] According to some embodiments, the polishing object preferably includes a low-k material and silicon nitride. Thus, according to a preferred embodiment of the present invention, the polishing composition is used to polish an object including a low-k material and silicon nitride. The low-k material is preferably silicon oxide containing carbon (SiOC).
[0074] According to some embodiments, the object to be polished preferably contains silicon oxide and silicon nitride. Thus, according to a preferred embodiment of the present invention, the polishing composition is used for polishing an object to be polished that contains silicon oxide and silicon nitride.
[0075] [Method of manufacturing the polishing composition] The method for producing the polishing composition according to this embodiment is not particularly limited, and can be obtained, for example, by stirring and mixing abrasive grains, an alkylamine compound having at least one linear or branched alkyl group having 2 to 15 carbon atoms, a dispersion medium, and other additives added as necessary. The details of each component are as described above.
[0076] The temperature at which the components are mixed is not particularly limited, but is preferably 10° C. to 40° C., and may be heated to increase the dissolution rate. The mixing time is also not particularly limited as long as the components can be mixed uniformly.
[0077] [Polishing method and semiconductor substrate manufacturing method] As described above, the polishing composition according to some embodiments of the present invention is particularly suitable for polishing an object having a low-k material and silicon nitride.Therefore, the present invention provides a polishing method for polishing an object containing a low-k material and silicon nitride with the polishing composition according to the present invention.The present invention also provides a method for producing a semiconductor substrate, comprising polishing a semiconductor substrate containing a low-k material and silicon nitride with the above-mentioned polishing method.
[0078] The polishing composition according to some embodiments of the present invention is particularly suitable for use in polishing an object having silicon oxide and silicon nitride. Thus, the present invention provides a polishing method for polishing an object containing silicon oxide and silicon nitride with the polishing composition according to the present invention. The present invention also provides a method for producing a semiconductor substrate, comprising polishing a semiconductor substrate containing silicon oxide and silicon nitride by the polishing method.
[0079] As a polishing device, a general polishing device can be used which is equipped with a holder for holding a substrate or the like having an object to be polished, a motor whose rotation speed can be changed, and a polishing platen onto which a polishing pad (polishing cloth) can be attached.
[0080] The polishing pad may be made of any material, including general nonwoven fabric, polyurethane, porous fluororesin, etc. It is preferable that the polishing pad has grooves formed thereon to allow the polishing liquid to accumulate.
[0081] Regarding the polishing conditions, for example, the rotation speed of the polishing table (platen) and the carrier (head) was 10 rpm (0.17 s -1 ) or more 500rpm (8.33s -1 The pressure (polishing pressure) applied to the substrate having the object to be polished is preferably 0.5 psi (3.45 kPa) or more and 10 psi (68.9 kPa) or less.
[0082] The method of supplying the polishing composition to the polishing pad is not particularly limited, and for example, a method of continuously supplying the composition using a pump, etc. is adopted. There is no limit to the amount of the composition supplied, but it is preferable that the surface of the polishing pad is always covered with the polishing composition according to the present invention.
[0083] The polishing composition according to the present embodiment may be a one-liquid type or a multi-liquid type such as a two-liquid type. The polishing composition according to the present invention may be prepared by diluting the stock solution of the polishing composition, for example, three times or more, with a diluent such as water.
[0084] [Polishing speed] As described above, the polishing composition of the present invention is capable of polishing low-k materials, silicon nitride, and silicon oxide at a high polishing rate.
[0085] In the present invention, the polishing speed of the low-k material is preferably 300 Å / min or more, and may be 350 Å / min or more, 400 Å / min or more, 500 Å / min or more, 550 Å / min or more, or 600 Å / min or more. The polishing speed of silicon nitride is preferably 300 Å / min or more, and may be 350 Å / min or more, 370 Å / min or more, 400 Å / min or more, 450 Å / min or more, 500 Å / min or more, 550 Å / min or more, 600 Å / min or more, 650 Å / min or more, or 670 Å / min or more. Furthermore, the polishing speed of silicon oxide is preferably 250 Å / min or more, and may be 300 Å / min or more, 310 Å / min or more, 320 Å / min or more, 330 Å / min or more, 340 Å / min or more, 350 Å / min or more, or 360 Å / min or more.
[0086] [Selection ratio] As described above, the polishing composition of the present invention can control the ratio of the polishing rate of the low-k material to the polishing rate of silicon nitride (hereinafter also referred to as selectivity A) within an appropriate range. Also, as described above, the polishing composition of the present invention can control the ratio of the polishing rate of the silicon nitride to the polishing rate of silicon oxide (hereinafter also referred to as selectivity B) within an appropriate range.
[0087] In the present invention, the ratio of the polishing rate of the low-k material to the polishing rate of silicon nitride (selection ratio A, polishing rate of the low-k material / polishing rate of silicon nitride) is preferably 1.0 or more, more preferably 1.1 or more, even more preferably 1.2 or more, and particularly preferably 1.4 or more. In addition, the ratio of the polishing rate of the low-k material to the polishing rate of silicon nitride (selection ratio A, polishing rate of the low-k material / polishing rate of silicon nitride) is preferably 2.0 or less, more preferably 1.9 or less, even more preferably 1.8 or less, and particularly preferably 1.7 or less. That is, the selectivity A may be 1.0 or more and 2.0 or less, 1.0 or more and 1.9 or less, 1.0 or more and 1.8 or less, or 1.0 or more and 1.7 or less. The selectivity A may be 1.1 or more and 2.0 or less, 1.1 or more and 1.9 or less, 1.1 or more and 1.8 or less, or 1.1 or more and 1.7 or less. The selectivity A may be 1.2 or more and 2.0 or less, 1.2 or more and 1.9 or less, 1.2 or more and 1.8 or less, or 1.2 or more and 1.7 or less. The selectivity A may be 1.4 or more and 2.0 or less, 1.4 or more and 1.9 or less, 1.4 or more and 1.8 or less, or 1.4 or more and 1.7 or less. If the selectivity A is out of the above range, the surface condition of the object to be polished after the polishing may be poor.
[0088] In the present invention, the ratio of the polishing rate of silicon nitride to the polishing rate of silicon oxide (selection ratio B, polishing rate of silicon nitride / polishing rate of silicon oxide) is preferably 1.3 or more, more preferably 1.4 or more, even more preferably 1.5 or more, and particularly preferably 1.6 or more. The ratio of the polishing rate of silicon nitride to the polishing rate of silicon oxide (selection ratio B, polishing rate of silicon nitride / polishing rate of silicon oxide) is preferably 3.0 or less, more preferably 2.9 or less, even more preferably 2.8 or less, even more preferably 2.5 or less, and particularly preferably 2.4 or less. That is, the selectivity B may be 1.3 or more and 3.0 or less, 1.3 or more and 2.9 or less, 1.3 or more and 2.8 or less, 1.3 or more and 2.5 or less, or 1.3 or more and 2.4 or less. The selectivity B may be 1.4 or more and 3.0 or less, 1.4 or more and 2.9 or less, 1.4 or more and 2.8 or less, 1.4 or more and 2.5 or less, or 1.4 or more and 2.4 or less. The selectivity B may be 1.5 or more and 3.0 or less, 1.5 or more and 2.9 or less, 1.5 or more and 2.8 or less, 1.5 or more and 2.5 or less, or 1.5 or more and 2.4 or less. The selectivity B may be 1.6 or more and 3.0 or less, 1.6 or more and 2.9 or less, 1.6 or more and 2.8 or less, 1.6 or more and 2.5 or less, or 1.6 or more and 2.4 or less. If the selectivity B is out of the above range, the surface condition of the polished object obtained after polishing may be poor.
[0089] [scratch] As described above, the polishing composition of the present invention can reduce defects (eg, scratches) on the surface of an object to be polished (particularly silicon nitride and / or silicon oxide) after polishing.
[0090] In some embodiments of the present invention, the number of scratches on the surface of the object to be polished (particularly silicon nitride and / or silicon oxide) after polishing is preferably less than 30, more preferably less than 20, even more preferably less than 10, and particularly preferably less than 5. The lower limit of the number of scratches is 0. In this specification, a scratch refers to a flaw on the surface of the object to be polished that has a depth of 10 nm or more and less than 100 nm, a width of 5 nm or more and less than 500 nm, and a length of 100 nm or more. The number of scratches can be measured by the method described in the Examples.
[0091] Although the embodiments of the present invention have been described in detail, it is apparent that the same are illustrative and exemplary, not restrictive, and the scope of the present invention should be interpreted by the appended claims.
[0092] The present invention encompasses the following aspects and configurations. 1. A polishing composition comprising an abrasive grain and an alkylamine compound having at least one linear or branched alkyl group having 2 to 15 carbon atoms, and having a pH of less than 7, wherein the abrasive grain in the polishing composition has a negative zeta potential; 2. The polishing composition according to 1 above, wherein the alkylamine compound is a monoalkylamine compound having only one alkyl group; 3. The polishing composition according to 1 or 2 above, wherein the alkyl group has 2 or more and 7 or less carbon atoms; 4. The polishing composition according to any one of 1. to 3. above, wherein the alkylamine compound is at least one monoalkylamine compound selected from the group consisting of ethylamine, n-propylamine, n-butylamine, n-pentylamine, and n-hexylamine; 5. The polishing composition according to any one of 1. to 4. above, wherein the abrasive grains are anion-modified colloidal silica; 6. The polishing composition according to any one of 1. to 5. above, further comprising a pH adjuster; 7. The polishing composition according to any one of 1. to 6. above, further comprising an electrical conductivity adjuster; 8. The polishing composition according to any one of 1. to 7. above, further comprising a dispersion medium; 9. The polishing composition according to any one of 1. to 8. above, wherein the abrasive grains in the polishing composition have a zeta potential of -45 mV or more and -15 mV or less; 10. The polishing composition according to any one of 1. to 9. above, which is used for polishing an object to be polished, including a low-k material and silicon nitride; 11. The polishing composition according to claim 10, wherein the low-k material is SiOC; 12. The polishing composition according to 10 or 11 above, wherein the ratio of the polishing rate of the low-k material to the polishing rate of the silicon nitride (polishing rate of low-k material / polishing rate of silicon nitride) is 1.0 or more and 2.0 or less; 13. A polishing method, comprising a step of polishing an object containing a low-k material and silicon nitride with the polishing composition according to any one of 1. to 12. above; 14. A method for producing a semiconductor substrate, comprising a step of polishing a semiconductor substrate containing a low-k material and silicon nitride by the polishing method according to 13 above; 15. The polishing composition according to any one of 1. to 9. above, which is used for polishing an object to be polished containing silicon oxide and silicon nitride; 16. The polishing composition according to the above 15, wherein the ratio of the polishing rate of the silicon nitride to the polishing rate of the silicon oxide (polishing rate of silicon oxide / polishing rate of silicon nitride) is 1.5 or more and 2.5 or less; 17. A polishing method, comprising a step of polishing an object containing silicon oxide and silicon nitride with the polishing composition according to any one of 1. to 9. and 15. to 16. above; 18. A method for producing a semiconductor substrate, comprising the step of polishing a semiconductor substrate containing silicon oxide and silicon nitride by the polishing method described in 17 above. EXAMPLES
[0093] The present invention will be described in more detail using the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. Unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively. In the following examples, unless otherwise specified, the operations were performed under the conditions of room temperature (20°C to 25°C) / relative humidity 40% RH to 50% RH. Each physical property was measured as follows.
[0094] <Average secondary particle size of abrasive grains> The average secondary particle diameter of the abrasive grains was measured as the volume average particle diameter (arithmetic mean diameter based on volume; Mv) using a dynamic light scattering particle size / particle size distribution analyzer UPA-UT151 (manufactured by Nikkiso Co., Ltd.).
[0095] <Zeta potential of abrasive grains> The zeta potential of the abrasive grains in the polishing composition was measured using a zeta potential measuring device manufactured by Otsuka Electronics Co., Ltd. (device name "ELS-Z2").
[0096] <pH of polishing composition> The pH of the polishing composition was measured with a pH meter (manufactured by Horiba, Ltd., model number: LAQUA).
[0097] <Electrical Conductivity of Polishing Composition> The electrical conductivity (EC) of the polishing composition was measured with a tabletop electrical conductivity meter (manufactured by Horiba, Ltd., model number: DS-71 LAQUA (registered trademark)).
[0098] <Sulfonic acid modified colloidal silica> [Production Example 1] A sulfonic acid-modified colloidal silica was obtained as an abrasive grain according to the following procedure.
[0099] (Preparation process of raw colloidal silica dispersion (unmodified silica particles)) In a flask, 4080g of methanol, 610g of water, and 168g of 29% by mass aqueous ammonia solution were mixed, and the liquid temperature was kept at 20°C. A mixed liquid of 135g of methanol and 508g of tetramethoxysilane (TMOS) was added dropwise over a period of 25 minutes. After that, thermally concentrated water replacement was performed under conditions of pH 7 or higher, and 1000g of silica sol with a solid content concentration of 19.5% by mass was obtained (average secondary particle size: 34nm).
[0100] (Surface modification process) Next, 2.4 g (silane coupling agent concentration relative to the total mass of silica solids: 1.2 mass%) of 3-mercaptopropyltrimethoxysilane (MPS, silane coupling agent, product name: KBM-803, Shin-Etsu Chemical Co., Ltd.) mixed with 4.8 g of methanol was added dropwise at a flow rate of 1 mL / min to 1000 g of the silica sol obtained above (195 g in terms of silica solids). The mixture was then heated and stirred at 90°C for 1 hour.
[0101] Next, the reaction solution was left to cool overnight, and 0.0686 g of 30% by mass hydrogen peroxide solution (3 moles per mole of silane coupling agent) was added, and the mixture was heated again to 90° C. and stirred for 1 hour. After that, the mixture was cooled to room temperature (25° C.) to obtain sulfonic acid-modified colloidal silica.
[0102] Example 1 <Preparation of Polishing Composition> The sulfonic acid-modified colloidal silica (average secondary particle diameter: 34 nm) obtained in the above-mentioned Production Example 1 as the abrasive grains was added to water as a dispersion medium so that the final concentration was 2 mass%. Furthermore, n-hexylamine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to a final concentration of 0.1 mass%, and the mixture was stirred and mixed (stirring temperature: 25°C, stirring time: 20 minutes). The pH of the polishing composition was adjusted to 2.5 using nitric acid, and the polishing composition was completed.
[0103] Example 2 A polishing composition was prepared in the same manner as in Example 1, except that the pH of the polishing composition was adjusted to 4.0.
[0104] Example 3 A polishing composition was prepared in the same manner as in Example 1, except that ethylamine (manufactured by Tokyo Chemical Industry Co., Ltd.) was used instead of n-hexylamine.
[0105] Example 4 A polishing composition was prepared in the same manner as in Example 1, except that n-butylamine (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used instead of n-hexylamine.
[0106] Example 5 A polishing composition was prepared in the same manner as in Example 1, except that n-heptylamine (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used instead of n-hexylamine.
[0107] Example 6 A polishing composition was prepared in the same manner as in Example 1, except that n-octylamine (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used instead of n-hexylamine.
[0108] Example 7 A polishing composition was prepared in the same manner as in Example 1, except that n-dodecylamine (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used instead of n-hexylamine.
[0109] Comparative Example 1 A polishing composition was prepared in the same manner as in Example 1, except that n-hexylamine was not used.
[0110] Comparative Example 2 A polishing composition was prepared in the same manner as in Example 1, except that methylamine (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used instead of n-hexylamine.
[0111] Comparative Example 3 A polishing composition was prepared in the same manner as in Example 1, except that stearylamine (n-octadecylamine, manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used instead of n-hexylamine.
[0112] Comparative Example 4 A polishing composition was prepared in the same manner as in Example 1, except that the pH of the polishing composition was adjusted to 7.0.
[0113] [evaluation] (Evaluation of Polishing Rates of Polishing Compositions of Examples 1 to 7 and Comparative Examples 1 to 4) The surface of each object to be polished was polished under the following conditions using each of the polishing compositions of Examples 1 to 7 and Comparative Examples 1 to 4. The following objects to be polished (1) and (2) were prepared: (1) Silicon nitride film (Si3N4 film): A silicon wafer (200 mm, blanket wafer) with a 2000 Å thick silicon nitride film formed on its surface. (2) 200 mm wafer (SiOC film, manufactured by Advantec Corporation, product name: BD 5kA Blanket.
[0114] Using the polishing compositions of Examples 1 to 7 and Comparative Examples 1 to 4, the prepared substrates were polished under the following polishing conditions, and the removal rates were measured: (Polishing equipment and polishing conditions) Polishing equipment: Applied Materials 200mm CMP single-sided polishing equipment Mirra Polishing pad: Nitta DuPont hard polyurethane pad IC1010 Polishing pressure: 2.0psi (1psi=6894.76Pa) Polishing platen rotation speed: 87 rpm Head (carrier) rotation speed: 83 rpm Supply of polishing composition: free-flowing Polishing composition supply amount: 200mL / min Polishing time: 60 seconds.
[0115] (Calculation of polishing rate) The thickness of each polished object before and after polishing was measured using an optical film thickness measuring device (ASET-f5x: manufactured by KLA-Tencor Corporation). The film thickness was measured using an optical film thickness measuring device (ASET-f5x: manufactured by KLA-Tencor Corporation).
[0116]
number
[0117] (Selectivity A) The selectivity A was obtained by dividing the polishing speed of the SiOC film obtained above by the polishing speed of the silicon nitride film (Si3N4 film). The selectivity A is preferably 1.0 or more and 2.0 or less. The selectivity A shown in Table 1 below is a value rounded off to one decimal place.
[0118] (Scratch evaluation of polishing compositions of Examples 1 to 7 and Comparative Examples 1 to 4) The number of scratches on the surface of the object to be polished after polishing using the polishing compositions of Examples 1 to 7 and Comparative Examples 1 to 4 was evaluated. Specifically, the coordinates of the entire surface of the silicon nitride film (excluding the outer periphery of 10 mm) were measured using a wafer inspection device "Surfscan (registered trademark) SP2" manufactured by KLA-Tencor Corporation, and the number of scratches was measured by observing all the measured coordinates with a Review-SEM (RS-6000, manufactured by Hitachi High-Tech Corporation). Scratches on the polished surface of the object to be polished that were 10 nm or more and less than 100 nm in depth, 5 nm or more and less than 500 nm in width, and 100 nm or more in length were counted as scratches, and the number of scratches was evaluated according to the following evaluation criteria. The fewer the number of scratches, the better: <Evaluation criteria> 5: Less than 5 scratches 4: Scratch count is between 5 and 10 3: Scratch count is between 10 and 20 2: Scratch count is between 20 and 30 1: 30 or more scratches.
[0119] The compositions and evaluation results of the polishing compositions of Examples 1 to 7 and Comparative Examples 1 to 4 are shown in the following Table 1. In addition, "-" in Table 1 indicates that the corresponding agent was not used.
[0120] [Table 1]
[0121] As is clear from Table 1 above, when the polishing composition of the embodiment is used, the polishing speed of both SiOC and silicon nitride, which are low-k materials, is 300 Å / min or more, and it is found that a high polishing speed can be obtained. In addition, the ratio of the polishing speed of SiOC to the polishing speed of silicon nitride (selective ratio A) is 1.0 or more and 2.0 or less, and it is found that an appropriate selectivity can be obtained. On the other hand, when the polishing composition of the comparative example is used, the polishing speed of either SiOC or silicon nitride is low, and the selectivity is not appropriate (1.0 or more and 2.0 or less).
[0122] Furthermore, when the polishing composition of Example was used, scratches on the surface of the object to be polished after polishing were reduced, whereas when the polishing composition of Comparative Example 3 was used, scratches on the surface of the object to be polished after polishing were increased.
[0123] The results shown in Table 1 were obtained by polishing a low-k material (SiOC) and a silicon nitride separately. However, it is expected that the polishing speed, selectivity, and scratch results shown in Table 1 will be similar to those shown in Table 1 even when a low-k material and a silicon nitride are both polished.
[0124] Example 8 <Sulfonic acid modified colloidal silica> [Production Example 2] A sulfonic acid-modified colloidal silica was obtained as an abrasive grain according to the following procedure.
[0125] (Preparation process of raw colloidal silica dispersion (unmodified silica particles)) In a flask, 4080g of methanol, 610g of water, and 168g of 29% by mass aqueous ammonia solution were mixed, and the liquid temperature was kept at 20°C. A mixed liquid of 135g of methanol and 508g of tetramethoxysilane (TMOS) was added dropwise over a period of 25 minutes. After that, thermally concentrated water replacement was performed under conditions of pH 7 or higher, and 1000g of silica sol with a solid content of 19.5% by mass was obtained (average secondary particle size: 68nm).
[0126] (Surface modification process) Next, 2.4 g (silane coupling agent concentration relative to the total mass of silica solids: 1.2 mass%) of 3-mercaptopropyltrimethoxysilane (MPS, silane coupling agent, product name: KBM-803, Shin-Etsu Chemical Co., Ltd.) mixed with 4.8 g of methanol was added dropwise at a flow rate of 1 mL / min to 1000 g of the silica sol obtained above (195 g in terms of silica solids). The mixture was then heated and stirred at 90°C for 1 hour.
[0127] Next, the reaction solution was left to cool overnight, and 0.0686 g of 30% by mass hydrogen peroxide solution (3 moles per mole of silane coupling agent) was added, and the mixture was heated again to 90° C. and stirred for 1 hour. After that, the mixture was cooled to room temperature (25° C.) to obtain sulfonic acid-modified colloidal silica.
[0128] <Preparation of Polishing Composition> The sulfonic acid-modified colloidal silica (average secondary particle diameter: 68 nm) obtained in the above-mentioned Production Example 2 as the abrasive grains was added to water as a dispersion medium so that the final concentration was 2 mass%. Furthermore, n-hexylamine (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was added to a final concentration of 0.01 mass%, and ammonium sulfate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was added to a final concentration of 6 mass%, and the mixture was stirred and mixed (stirring temperature: 25°C, stirring time: 20 minutes). The pH of the polishing composition was adjusted to 2.5 using nitric acid, and the polishing composition was completed.
[0129] Example 9 A polishing composition was prepared in the same manner as in Example 8, except that the pH of the polishing composition was adjusted to 4.0.
[0130] Example 10 A polishing composition was prepared in the same manner as in Example 8, except that ethylamine (manufactured by Tokyo Chemical Industry Co., Ltd.) was used instead of n-hexylamine.
[0131] Example 11 A polishing composition was prepared in the same manner as in Example 8, except that n-butylamine (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used instead of n-hexylamine.
[0132] Example 12 A polishing composition was prepared in the same manner as in Example 8, except that n-heptylamine (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used instead of n-hexylamine.
[0133] (Example 13) A polishing composition was prepared in the same manner as in Example 8, except that n-octylamine (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used instead of n-hexylamine.
[0134] Example 14 A polishing composition was prepared in the same manner as in Example 8, except that n-dodecylamine (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used instead of n-hexylamine.
[0135] Comparative Example 5 A polishing composition was prepared in the same manner as in Example 8, except that n-hexylamine and ammonium sulfate were not used.
[0136] Comparative Example 6 A polishing composition was prepared in the same manner as in Example 8, except that stearylamine (n-octadecylamine, manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used instead of n-hexylamine.
[0137] Comparative Example 7 A polishing composition was prepared in the same manner as in Example 8, except that the pH of the polishing composition was adjusted to 7.0.
[0138] (Evaluation of Polishing Rates of Polishing Compositions of Examples 8 to 14 and Comparative Examples 5 to 7) The surface of each object to be polished was polished under the following conditions using each of the polishing compositions of Examples 8 to 14 and Comparative Examples 5 to 7. The following objects to be polished (1) and (2) were prepared: (1) Silicon nitride film (Si3N4 film): A silicon wafer (200 mm, blanket wafer) with a 2000 Å thick silicon nitride film formed on its surface. (2) Silicon oxide film (SiO2 film): A silicon wafer (200 mm, blanket wafer) with a 10,000 Å-thick silicon oxide film (TEOS-type silicon oxide film produced using tetraethyl orthosilicate as a precursor) formed on its surface.
[0139] Using the polishing composition obtained above, the prepared substrate was polished under the following polishing conditions, and the removal rate was measured: (Polishing equipment and polishing conditions) Polishing equipment: Applied Materials 200mm CMP single-sided polishing equipment Mirra Polishing pad: Nitta DuPont hard polyurethane pad IC1010 Polishing pressure: 3.0 psi (1 psi = 6894.76 Pa) Polishing platen rotation speed: 87 rpm Head (carrier) rotation speed: 83 rpm Supply of polishing composition: free-flowing Polishing composition supply amount: 200mL / min Polishing time: 60 seconds.
[0140] The polishing rate was calculated in the same manner as in the case of the polishing compositions of Examples 1 to 7 and Comparative Examples 1 to 4 above.
[0141] (Selectivity B) The selectivity A was obtained by dividing the polishing speed of the silicon nitride film (Si3N4 film) obtained above by the polishing speed of the silicon oxide film (SiO2 film). The selectivity B is preferably 1.5 or more and 2.5 or less. The selectivity B shown in Table 2 below is a value rounded off to one decimal place.
[0142] (Scratch evaluation of polishing compositions of Examples 8 to 14 and Comparative Examples 5 to 7) The surface of the object to be polished after polishing using the polishing compositions of Examples 8 to 14 and Comparative Examples 5 to 7 was evaluated for scratches. Specifically, the coordinates of the entire surface of the silicon oxide film (excluding the outer periphery of 10 mm) were measured using a wafer inspection device "Surfscan (registered trademark) SP2" manufactured by KLA-Tencor Corporation, and the number of scratches was measured by observing all the measured coordinates with a Review-SEM (RS-6000, manufactured by Hitachi High-Tech Corporation). Scratches on the polished surface of the object to be polished that were 10 nm or more and less than 100 nm deep, 5 nm or more and less than 500 nm wide, and 100 nm or more long were counted as scratches, and the number of scratches was evaluated according to the following evaluation criteria. The fewer the number of scratches, the better: <Evaluation criteria> 5: Less than 5 scratches 4: Scratch count is between 5 and 10 3: Scratch count is between 10 and 20 2: Scratch count is between 20 and 30 1: 30 or more scratches.
[0143] The compositions and evaluation results of the polishing compositions of Examples 8 to 14 and Comparative Examples 5 to 7 are shown in the following Table 2. In addition, "-" in Table 2 indicates that the corresponding agent was not used.
[0144] [Table 2]
[0145] As is clear from Table 2 above, when the polishing compositions of Examples 8 to 13 were used, the polishing rates for silicon oxide and silicon nitride were both 300 Å / min or more, and it was found that a high polishing rate could be obtained. In addition, when the polishing compositions of Examples 8 to 14 were used, the ratio of the polishing rate for silicon nitride to the polishing rate for silicon oxide (selective ratio B) was 1.5 or more and 2.5 or less, and an appropriate selectivity was obtained, and it was found that scratches on the surface of the object to be polished after polishing were reduced. On the other hand, when the polishing compositions of Comparative Examples 5 to 6 were used, scratches on the surface of the object to be polished after polishing increased. In addition, when the polishing compositions of Comparative Examples 6 to 7 were used, the selectivity B did not reach an appropriate value (1.5 or more and 2.5 or less).
[0146] The results shown in Table 2 were obtained by polishing a silicon oxide-containing polishing object and a silicon nitride-containing polishing object separately. However, it is expected that the polishing speed, selectivity, and scratch results shown in Table 2 will be similar to those shown in Table 2 even when a polishing object containing both silicon oxide and silicon nitride is polished.
Claims
1. Abrasive grains and an alkylamine compound having at least one linear or branched alkyl group having from 2 to 15 carbon atoms; and having a pH of less than 7, A polishing composition, wherein the abrasive grains in the polishing composition have a negative zeta potential.
2. The polishing composition according to claim 1 , wherein the alkylamine compound is a monoalkylamine compound having only one alkyl group.
3. The polishing composition according to claim 1 , wherein the alkyl group has 2 or more and 7 or less carbon atoms.
4. 2. The polishing composition according to claim 1, wherein the alkylamine compound is at least one monoalkylamine compound selected from the group consisting of ethylamine, n-propylamine, n-butylamine, n-pentylamine, and n-hexylamine.
5. The polishing composition according to claim 1 , wherein the abrasive grains are anion-modified colloidal silica.
6. The polishing composition of claim 1 , further comprising a pH adjuster.
7. The polishing composition according to claim 1 , further comprising an electrical conductivity adjuster.
8. The polishing composition according to claim 1 , further comprising a dispersion medium.
9. 2. The polishing composition according to claim 1, wherein the abrasive grains in the polishing composition have a zeta potential of −45 mV or more and −15 mV or less.
10. 2. The polishing composition according to claim 1, which is used in polishing an object containing a low-k material and silicon nitride.
11. The polishing composition according to claim 10, wherein the low-k material is SiOC.
12. 11. The polishing composition according to claim 10, wherein the ratio of the polishing rate of the Low-k material to the polishing rate of the silicon nitride (polishing rate of the Low-k material / polishing rate of silicon nitride) is 1.0 or more and 2.0 or less.
13. 13. A polishing method comprising the step of polishing an object containing a low-k material and silicon nitride with the polishing composition according to claim 1.
14. A method for producing a semiconductor substrate, comprising a step of polishing a semiconductor substrate containing a low-k material and silicon nitride by the polishing method according to claim 13.
15. 2. The polishing composition according to claim 1, which is used for polishing an object containing silicon oxide and silicon nitride.
16. 16. The polishing composition according to claim 15, wherein the ratio of the polishing rate of said silicon nitride to the polishing rate of said silicon oxide (polishing rate of silicon nitride / polishing rate of silicon oxide) is 1.5 or more and 2.5 or less.
17. 17. A polishing method comprising a step of polishing an object containing silicon oxide and silicon nitride with the polishing composition according to claim 1.
18. A method for producing a semiconductor substrate, comprising a step of polishing a semiconductor substrate containing silicon oxide and silicon nitride by the polishing method according to claim 17.
Citation Information
Patent Citations