Laminate and method for manufacturing semiconductor device
A laminate with a laser-transparent substrate and resin film with defined viscoelastic properties addresses adhesive residue and debris issues in semiconductor transfer, ensuring precise and efficient placement of micro LEDs and other elements.
Patent Information
- Application Number
- JP2024045519
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-09
AI Technical Summary
Existing methods for transferring micro LEDs and other semiconductor elements face challenges such as adhesive residue and debris generation, leading to damage and poor positional accuracy during high-speed laser transfer processes.
A laminate structure comprising a laser-transparent substrate and a resin film with specific viscoelastic properties, including a loss tangent of 0.01 to 0.15 and a storage modulus of 300 MPa or more, allows for precise transfer of semiconductor elements by laser irradiation without generating debris.
The laminate enables fine and densely mounted semiconductor elements to be transferred with high positional accuracy and minimal adhesive residue, improving manufacturing efficiency and device quality.
Smart Images

Figure 2024139737000006 
Figure 2024139737000007 
Figure 2024139737000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate and a method for manufacturing a semiconductor device, more particularly to a laminate suitable for use when mounting a semiconductor element by laser transfer, and a method for manufacturing a semiconductor device using the same. [Background technology]
[0002] In general, elements to be incorporated in a semiconductor device are transferred and mounted on a circuit board by a pick-and-place method using a flip-chip bonder or the like. In recent years, semiconductor devices have become more sophisticated and smaller in size, and accordingly, elements to be incorporated in the semiconductor device have become smaller and thinner, and the number of elements mounted in the semiconductor device has increased. In recent years, displays in which light-emitting diodes (LEDs), a type of semiconductor element, are arranged in each pixel have attracted attention because of their high brightness, low power consumption, and high image quality. The LEDs mounted in each pixel are called micro LEDs, and small LEDs with sides of several hundred to several tens of μm are used. When manufacturing this micro LED display, the above mounting method takes too much time, so new methods are being considered.
[0003] As a method for mounting a large number of small semiconductor elements, a laser transfer technology has been proposed in which a laminate having an adhesive layer on a support substrate is prepared by mounting semiconductor elements on the surface of the adhesive layer opposite the support substrate side, and then a laser is irradiated from the support substrate side of the laminate to selectively transfer and mount the semiconductor elements to a counter substrate such as a circuit board located below the laminate at a certain distance from the laminate, so that the semiconductor elements are spaced apart at the desired interval. This method has the advantage that the semiconductor elements can be transferred quickly and over a wide area by irradiating the laser while moving the stage of the laminate and / or the counter substrate at high speed. Note that "transfer" refers to the transfer of the semiconductor elements from the original substrate to another substrate.
[0004] Examples of laminates used in the laser transfer technology include a laminate in which a thin adhesive layer is applied, and the adhesive layer present between the support substrate and the semiconductor element is entirely ablated and eliminated by laser irradiation, thereby enabling the transfer of the semiconductor element while also removing all adhesive layer residues on the semiconductor element (for example, Patent Document 1). Also included are laminates in which the resin film located at the interface between the support substrate and the resin film is ablated by laser irradiation, and the gas generated thereby accumulates at the interface between the adhesive layer and the support substrate to form voids (blisters), and the element peels off and separates due to the change in shape of the adhesive layer, thereby transferring the semiconductor element (for example, Patent Document 2). Furthermore, a technology is also included in which a semiconductor element is transferred without any adhesive layer residue by applying an adhesive layer with controlled absorbance and adhesive strength (for example, Patent Document 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2020-188037 [Patent Document 2] International Publication No. 2022 / 153745 [Patent Document 3] International Publication No. 2022 / 210155 Summary of the Invention [Problem to be solved by the invention]
[0006] In Patent Document 1, in order to avoid residues of the adhesive layer on the surface of the semiconductor element, it is necessary to irradiate excessive laser light and remove all of the adhesive layer by ablation, which poses issues such as contamination of the opposing substrate due to scattering of the adhesive layer and damage to the semiconductor element (hereinafter, the residue of the adhesive layer on the surface of the semiconductor element may be referred to as glue residue, and the scattered residue of the adhesive layer may be referred to as debris.) In Patent Documents 2 and 3, while it is possible to transfer semiconductor elements while suppressing the generation of residues and debris, it is insufficient for transferring semiconductor elements such as micro LEDs, which are finely and densely mounted, with high accuracy.
[0007] In view of the above circumstances, the present invention aims to provide a laminate capable of transferring fine, densely packed semiconductor elements without generating debris and with high positional accuracy, and a method for manufacturing semiconductor elements using the laminate. [Means for solving the problem]
[0008] In order to solve the above problems, the present invention includes the following aspects 1 to 10. 1. A laminate in which a first substrate having laser transparency and a resin film are laminated in this order, 25℃, 1.0×10 6 The resin film has a loss tangent of 0.01 to 0.15 as measured by dynamic viscoelasticity measurement at 100 Hz. 2.Further comprising a semiconductor element; 2. The laminate according to claim 1, wherein the first substrate, the resin film, and the semiconductor element are laminated in this order. 3.25℃, 1.0×10 6 3. The laminate according to claim 1 or 2, wherein the storage modulus of the resin film measured by dynamic viscoelasticity measurement at 100 Hz is 300 MPa or more. 4.25℃, 1.0×10 -2 4. The laminate according to any one of 1 to 3 above, wherein the loss tangent of the resin film measured by dynamic viscoelasticity measurement at 100 Hz is 0.4 or more. 5. The laminate according to any one of 1 to 4 above, wherein the resin film has a thickness of 0.7 μm or more and 30 μm or less. 6. The laminate according to any one of 1 to 5 above, wherein the resin film contains a light absorbing agent. 7. The laminate according to any one of 1 to 6 above, wherein the resin film has an absorbance of 0.4 or more and 5.0 or less in terms of a film thickness of 1.0 μm at any wavelength of 200 to 1100 nm. 8. A method for manufacturing a semiconductor device, comprising the steps of: (a) providing a semiconductor device having a first insulating layer; (a) A step of disposing a second substrate so as to face the surface of the laminate described in any one of 2 to 7 above, on which the semiconductor element is laminated. (b) A step of irradiating the laminate with laser light from the side of the first substrate to transfer the semiconductor element to the second substrate. 9. The method for manufacturing a semiconductor device according to claim 8, wherein an adhesive layer is laminated on the surface of the second substrate to which the semiconductor element is transferred. 10. The method for producing a semiconductor device according to claim 8 or 9, wherein the wavelength of the laser light is 355 nm. Effect of the Invention
[0009] According to the laminate of the present invention, semiconductor elements that are finely arranged and densely mounted can be transferred without generating debris and with high positional accuracy. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a diagram illustrating a method for producing the second laminate. [Diagram 2] FIG. 2 is a diagram illustrating a method for producing a second laminate using a temporary adhesive. [Diagram 3] FIG. 3 is a diagram illustrating a method for producing a second laminate using laser lift-off. [Figure 4] FIG. 4 is a diagram illustrating another method for producing the second stack using a semiconductor substrate. [Diagram 5] FIG. 5 is a diagram illustrating a step of opposing the semiconductor element surface of the second stack to a second substrate in the method for manufacturing a semiconductor device. [Figure 6] FIG. 6 is a diagram illustrating a step of transferring a semiconductor element to a second substrate by irradiating with laser light. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified in any manner without departing from the gist of the present invention. The laminate according to one embodiment of the present invention is a laminate in which a first substrate having laser transparency and a resin film are laminated in this order.6 The loss tangent of the resin film measured by dynamic viscoelasticity measurement at 200 Hz is 0.01 to 0.15. The laminate of this embodiment is hereinafter referred to as a first laminate. Moreover, a laminate according to one embodiment of the present invention includes the configuration of the first laminate and further includes a semiconductor element. That is, the laminate according to one embodiment of the present invention includes a first substrate having laser transparency, a resin film, and a semiconductor element stacked in this order. Hereinafter, the laminate of this aspect is referred to as a second laminate.
[0012] The first laminate according to an embodiment of the present invention and the second laminate according to an embodiment of the present invention may be collectively referred to simply as the laminate according to an embodiment of the present invention.
[0013] In the present invention, a semiconductor element refers to an element that includes a semiconductor and constitutes a semiconductor device. Specific examples of semiconductor elements include transistors, diodes, and light-emitting diodes including micro LED chips. A semiconductor device is a device in which a plurality of semiconductor elements are electrically connected and assembled, and includes, for example, an integrated circuit, a TFT substrate that drives a display, and a micro LED display in which micro LED chips are arranged.
[0014] Each of the components constituting the laminate according to the embodiment of the present invention will be described below. The first substrate having laser transparency refers to a substrate having an absorbance of 0.1 or less at least at any wavelength of 200 to 1100 nm. The absorbance being within a specific range at any wavelength of 200 to 1100 nm means, for example, that when the absorbance is measured at a wavelength range of 200 to 1100 nm, the absorbance at at least one value when the wavelength is an integer value is within a specific range. Examples of substrates having such absorbance include inorganic substrates such as quartz, sapphire, alkali glass, non-alkali glass, and borosilicate glass. The thickness of the substrate can be selected within a range that does not impair the absorbance, and is preferably, for example, 0.1 mm to 5.0 mm. That is, from the viewpoint of ease of handling of the substrate, the thickness of the substrate is more preferably 0.3 mm or more. On the other hand, from the viewpoints of availability and versatility, the thickness of the substrate is more preferably 2.0 mm or less.
[0015] For the first substrate having laser transparency, an organic substrate such as PET, aramid, polyester, polypropylene, or cycloolefin may be used. When an organic substrate is used, the thickness of the substrate can be selected within a range that does not impair the absorbance, and is preferably 0.05 mm to 3.0 mm, for example. From the viewpoint of ease of handling of the substrate, the thickness of the substrate is more preferably 0.1 mm or more. On the other hand, the thickness of the substrate is more preferably 1.0 mm or less, since light scattering during laser irradiation can be suppressed.
[0016] When the first substrate has laser transparency, the laser irradiated from the first substrate side of the laminate during laser transfer of the semiconductor element passes through the first substrate and reaches the resin film. In the case of the second laminate, the reaching laser is absorbed by the resin film, and the semiconductor element is transferred by the following method A or method B. Method A: The entire resin film in the area irradiated by the laser is decomposed, generating gas. The generated gas transfers the semiconductor element layered on the resin film. Method B: The surface of the resin film in the area irradiated by the laser that comes into contact with the first substrate and its vicinity decompose, generating gas at the interface between the first substrate and the resin film. The pressure of the generated gas causes the resin film to deform, and the semiconductor element layered on top of the resin film is transferred. Hereinafter, unless otherwise specified, the embodiment of the present invention will be further described taking as an example a case where a semiconductor element is transferred by method B.
[0017] <Resin film> The resin film is a film containing at least resin, and has a viscosity of 1.0×10 at 25°C. 6 The loss tangent measured by dynamic viscoelasticity measurement at 100 Hz (hereinafter also referred to simply as the loss tangent α of the resin film) is 0.01 to 0.15. The time from when the laser is irradiated until when the semiconductor element leaves the resin film is generally in the range of 0.1 to 10 μsec. Therefore, when this time range is converted into a frequency, it is 1.0×10 5 ~1.0×10 7 Hz. When the loss tangent α is greater than 0.15, the energy generated by the laser irradiation is easily consumed by the thermal motion of the resin film during the process from the irradiation of the laser to the transfer of the semiconductor element, and the deformation of the resin film is unlikely to occur. Therefore, the momentum of transferring the semiconductor element is weakened, and the positional accuracy of the transferred destination is reduced. On the other hand, a resin film having a loss tangent α of less than 0.01 is difficult to hold a semiconductor element, and there is a risk that the position of the semiconductor element stacked on the resin film may be shifted or dropped due to handling before the laser irradiation on the resin film. Therefore, when the loss tangent α of the resin film is within the above range, the laminate according to the embodiment of the present invention can appropriately hold the semiconductor element when it is made into the aspect of the second laminate, and further, the positional accuracy when the semiconductor element is transferred can be excellent. The loss tangent α is preferably 0.03 or more, more preferably 0.05 or more. Moreover, the loss tangent α is preferably 0.13 or less, more preferably 0.11 or less.
[0018] The resin film was also measured at 25°C and 1.0×10 6The storage modulus measured by dynamic viscoelasticity measurement at 1000 Hz (hereinafter also simply referred to as the storage modulus of the resin film) is preferably 300 MPa or more. If the storage modulus is 300 MPa or more, excessive deformation of the resin film can be suppressed, and the transfer accuracy can be better maintained. The storage modulus is more preferably 350 MPa or more, even more preferably 380 MPa or more, and particularly preferably 450 MPa or more.
[0019] The resin film was also measured at 25°C and 1.0×10 -2 It is preferable that the loss tangent measured by dynamic viscoelasticity measurement at 1000 Hz (hereinafter, simply referred to as the loss tangent β of the resin film) is 0.4 or more. In producing the second laminate, a mounting machine such as a flip chip bonder is used to laminate a semiconductor element on the resin film. At this time, as described later, pressure is applied while heating as necessary. The time is generally in the range of 10 to 1000 seconds. Therefore, when this time range is converted into a frequency, it is 1.0×10 -1 ~1.0×10 -3 Hz. If the loss tangent β is smaller than 0.4, the viscosity of the resin film is not easily expressed, and it is difficult to attach the semiconductor element to the resin film. Therefore, when the loss tangent β of the resin film is within the above range, the semiconductor element can be laminated on the resin film, and the second laminate can be produced. The loss tangent β is more preferably 0.45 or more, and even more preferably 0.5 or more.
[0020] In the laminate according to the embodiment of the present invention, the thickness of the resin film is preferably 0.7 μm or more and 30 μm or less. By making the thickness 0.7 μm or more, it is possible to reduce the transfer of heat generated when irradiated with laser light to the semiconductor element, suppress damage to the semiconductor element, and further prevent the resin film from breaking and becoming debris to contaminate the opposing substrate.
[0021] Furthermore, if the resin film has a thickness of 30 μm or less, the deformation caused by the ablation of the resin film by the irradiation of the laser light from the first substrate side having laser transparency is efficiently transmitted to the interface of the semiconductor element, and as a result, the semiconductor element can be transferred. The film thickness is more preferably 20 μm or less, which allows for better positional accuracy when transferring the semiconductor element to the opposing substrate.
[0022] The resin film preferably has an absorbance of 0.4 or more and 5.0 or less in terms of a film thickness of 1.0 μm at any wavelength of 200 to 1100 nm. The absorbance is more preferably 0.6 or more and 4.0 or less. If the absorbance is 0.4 or more, when a laser is irradiated from the first substrate side having laser transparency, the resin film completely absorbs the laser near the interface with the first substrate. Therefore, the laser does not penetrate into the resin film, and the semiconductor element can be transferred to the second laminate by the method B. In addition, it is possible to prevent the semiconductor element from being damaged by being irradiated with the laser. On the other hand, if the absorbance is 5.0 or less, the versatility of the resin that can be used is increased.
[0023] The wavelength that satisfies the above-mentioned absorbance is preferably any one or more of 248 nm, 266 nm, 308 nm, 355 nm, 532 nm, and 1064 nm. More preferably, it is any one or more of 248 nm, 266 nm, 308 nm, and 355 nm. Even more preferably, it is a wavelength of 335 nm. When the absorbance of the resin film satisfies the above-mentioned range at these wavelengths, the resin film can efficiently absorb laser energy.
[0024] The adhesive strength of the resin film on the surface opposite to the surface where the resin film contacts the first substrate is preferably 0.02 N / cm or more and 0.3 N / cm or less. The adhesive strength mentioned here refers to a value obtained from a 90° peel test of the surface of the resin film and Kapton film. A specific measurement method is to press a Kapton film cut to 1 cm x 9 cm onto the surface of the resin film under conditions of 0.6 MPa and 35°C using a vacuum laminator, and then to perform a peel test by pulling the pressed Kapton tape at a constant speed of 2 mm / sec in a direction perpendicular to the resin film using a tensile tester.
[0025] When the adhesive strength is 0.02 N / cm or more, the semiconductor element can be stably held when laminated on the resin film. When the adhesive strength is 0.3 N / cm or less, the semiconductor element can be transferred with a low laser light energy density during transfer. More preferably, the adhesive strength is 0.2 N / cm or less. By setting the adhesive strength within this range, glue residue on the semiconductor element can be suppressed when the semiconductor element is transferred by irradiating a laser from the first substrate side having laser transparency.
[0026] In order to set the adhesive strength of the resin film within the above range, it is preferable that the resin described below contains a flexible component or a bent component. By introducing a flexible component or a bent component, the glass transition temperature is lowered, and the adhesive strength can be increased. Examples of components that increase flexibility and bendability include a flexible structure derived from an aliphatic or silane such as an alkylene group, a siloxane, a flexible structure derived from an ether group such as an alkylene glycol or a biphenyl ether, an alicyclic structure, and a bent structure such as an olefin. By containing 20 mol % or more of monomer residues having such a structure that imparts flexibility relative to 100 mol % of all monomer residues constituting the resin contained in the resin film, the adhesive strength can be made 0.02 N / cm or more. In addition, by setting the content of the monomer residue to 70 mol % or less, the adhesive strength can be made 0.3 N / cm or less.
[0027] The resin contained in the resin film may be, but is not limited to, polyimide, polyamic acid, polybenzoxazole, polyhydroxyamide, polyurethane, polyurea, polyamide, polyester, polysiloxane, polyimidesiloxane, novolac resin, polyhydroxystyrene, acrylic resin, epoxy resin, etc. Specific examples of the resin are given below.
[0028] <Resin> In the embodiment of the present invention, the resin used in the resin film may be mainly composed of a repeating unit represented by chemical formula (1) or (2). Here, a resin mainly composed of a repeating unit represented by chemical formula (1) or (2) means that the repeating number of the repeating unit accounts for 50% or more of the total repeating number.
[0029] [ka]
[0030] In the chemical formulas (1) and (2), X represents a tetravalent tetracarboxylic acid residue having two or more carbon atoms, and Y represents a divalent diamine residue having two or more carbon atoms. 1 and R 2 each independently represents a hydrogen atom, a monovalent hydrocarbon group having 1 to 10 carbon atoms, an alkylsilyl group having 1 to 10 carbon atoms, an alkali metal ion, an ammonium ion, an imidazolium ion, or a pyridinium ion.
[0031] Chemical formula (1) shows the chemical structure of polyimide. Chemical formula (2) shows the chemical structure of polyamic acid. As described below, polyamic acid is obtained by reacting tetracarboxylic acid with a diamine compound. Furthermore, polyamic acid can be converted into polyimide, a heat-resistant resin, by heating or chemical treatment.
[0032] In chemical formulas (1) and (2), X is preferably a tetravalent organic group having 2 to 80 carbon atoms, which contains hydrogen atoms and carbon atoms as essential components and may contain one or more atoms selected from the group consisting of boron, oxygen, sulfur, nitrogen, phosphorus, silicon, and halogens, and more preferably a tetravalent hydrocarbon group having 2 to 80 carbon atoms. The number of each of the boron, oxygen, sulfur, nitrogen, phosphorus, silicon, and halogen atoms is preferably 20 or less, and more preferably 10 or less.
[0033] The tetracarboxylic acid that gives X is not particularly limited, and known tetracarboxylic acids can be used. Examples include pyromellitic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, 2,2',3,3'-biphenyltetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane, bis(3,4-dicarboxyphenyl)sulfone, bis(3,4-dicarboxyphenyl)ether, cyclobutanetetracarboxylic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, 1,2,4,5-cyclohexanetetracarboxylic acid, and tetracarboxylic acids described in International Publication No. 2017 / 099183.
[0034] These tetracarboxylic acids can be used as they are, or in the form of an acid anhydride, an activated ester, or an activated amide. Of these, the acid anhydrides are preferably used because they do not produce by-products during polymerization. Two or more of these may also be used.
[0035] In chemical formulas (1) and (2), Y is preferably a divalent organic group having 2 to 80 carbon atoms, which contains hydrogen atoms and carbon atoms as essential components and may contain one or more atoms selected from the group consisting of boron, oxygen, sulfur, nitrogen, phosphorus, silicon, and halogens, and more preferably a divalent hydrocarbon group having 2 to 80 carbon atoms. The number of each of the boron, oxygen, sulfur, nitrogen, phosphorus, silicon, and halogen atoms is preferably 20 or less, and more preferably 10 or less.
[0036] The diamine that gives Y is not particularly limited, and any known diamine can be used. Examples include m-phenylenediamine, p-phenylenediamine, 4,4'-diaminobenzanilide, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-di(trifluoromethyl)-4,4'-diaminobiphenyl, bis(4-aminophenoxyphenyl)sulfone, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, bis(3-amino-4-hydroxyphenyl)hexafluoropropane, ethylenediamine, propylenediamine, butanediamine, cyclohexanediamine, 4,4'-methylenebis(cyclohexylamine), 1,3-bis(3-aminopropyl)tetramethyldisiloxane, and diamines described in WO 2017 / 099183. These diamines can be used as they are or in the form of the corresponding trimethylsilylated diamines, and two or more of these can also be used.
[0037] Moreover, X or Y preferably has at least one structure selected from the group consisting of structures represented by chemical formulas (11) to (13).
[0038] [ka]
[0039] In chemical formula (11), R 11 and R 12 Each of R independently represents a monovalent hydrocarbon group having 1 to 10 carbon atoms. j represents an integer of 4 to 40. 13 and R 14 Each independently represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms. k represents an integer of 10 to 40. In chemical formula (13), R 15 and R 16each independently represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms, m represents an integer of 1 to 16, and n represents an integer of 4 to 40. When the resin film contains a resin having a structure represented by any one of chemical formulas (11) to (13), the adhesion between the first substrate and the interface or between the first substrate and the semiconductor element can be strengthened.
[0040] Diamines that provide Y having the structure represented by chemical formula (11) include α,ω-bis(3-aminopropyl)polydimethylsiloxane, α,ω-bis(3-aminopropyl)polydiethylsiloxane, α,ω-bis(3-aminopropyl)polydipropylsiloxane, α,ω-bis(3-aminopropyl)polydibutylsiloxane, α,ω-bis(3-aminopropyl)polydiphenoxysiloxane, α,ω-bis(2-aminoethyl)polydimethylsiloxane, α,ω- Examples of such compounds include bis(2-aminoethyl)polydiphenoxysiloxane, α,ω-bis(4-aminobutyl)polydimethylsiloxane, α,ω-bis(4-aminobutyl)polydiphenoxysiloxane, α,ω-bis(5-aminopentyl)polydimethylsiloxane, α,ω-bis(5-aminopentyl)polydiphenoxysiloxane, α,ω-bis(4-aminophenyl)polydimethylsiloxane, α,ω-bis(4-aminophenyl)polydiphenoxysiloxane, etc. Commercially available products include KF-8010, KF-8012, KF-8008, X22-161A, X-22-161B, X-22-1660B-3, and X-22-9409 (all trade names, manufactured by Shin-Etsu Chemical Co., Ltd.). Examples of tetracarboxylic acids that give X having the structure represented by chemical formula (11) include X-22-168AS, X-22-168A, X-22-168B, and X-22-168-P5-B (all trade names, manufactured by Shin-Etsu Chemical Co., Ltd.) etc. Examples of diamines that give Y having the structure represented by chemical formula (12) include 1,10-diaminodecane, 1,11-diaminoundecane, and 1,12-diaminododecane etc. Examples of diamines that provide Y having the structure represented by chemical formula (13) include Jeffamine KH-511, Jeffamine ED-600, Jeffamine ED-900, Jeffamine ED-2003, Jeffamine EDR-148, Jeffamine EDR-176, Jeffamine D-200, Jeffamine D-400, Jeffamine D-2000, Jeffamine D-4000 (all trade names, manufactured by HUNTSMAN), Elasmer 250P, Elasmer 650P, Elasmer 1000P, and Porea SL100A (all trade names, manufactured by Kumiai Chemical Industry Co., Ltd.). Two or more of these may be used.
[0041] When the terminal monomer is a diamine compound, a dicarboxylic acid anhydride, a monocarboxylic acid, a monocarboxylic acid chloride compound, a monocarboxylic acid active ester compound, a dialkyl dicarbonate ester, or the like can be used as an end-capping agent to cap the amino group. When the terminal monomer is an acid dianhydride, a monoamine, a monoalcohol, or the like can be used as an end-capping agent to cap the acid anhydride group.
[0042] The weight average molecular weight of the resin mainly composed of the repeating unit represented by chemical formula (1) or (2) is preferably 200,000 or less, more preferably 150,000 or less, and even more preferably 100,000 or less, as measured by gel permeation chromatography in terms of polystyrene. Within this range, the viscosity of the resin composition can be more effectively prevented from increasing, even in the case of a high-concentration resin composition. The weight average molecular weight is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 30,000 or more. If the weight average molecular weight is 30,000 or more, the viscosity of the resin composition is not too low, and better coating properties can be maintained. The number of repetitions of chemical formulas (1) and (2) may be within a range that satisfies the weight average molecular weight described above. It is preferably 5 or more, more preferably 10 or more. It is also preferably 1000 or less, more preferably 500 or less.
[0043] The resin used in the resin film in the embodiment of the present invention may contain, as a main component, a repeating unit represented by chemical formula (3).
[0044] [ka]
[0045] In chemical formula (3), U represents a divalent polyisocyanate residue having 2 or more carbon atoms, and V represents a divalent polyol residue having 2 or more carbon atoms.
[0046] The polyisocyanate which gives U is not particularly limited, and any known polyisocyanate can be used. Examples of the diisocyanates include aliphatic diisocyanates such as hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, and lysine diisocyanate; alicyclic diisocyanates such as dicyclohexylmethane diisocyanate, isophorone diisocyanate, 1,4-cyclohexane diisocyanate, hydrogenated xylylene diisocyanate, hydrogenated tolylene diisocyanate, and dicyclohexylmethane-4,4'-diisocyanate; and aromatic diisocyanates such as tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, naphthalene diisocyanate, xylylene diisocyanate, tolidine diisocyanate, p-phenylene diisocyanate, and naphthylene diisocyanate; as well as biuret forms, isocyanurate forms, and adducts with trimethylolpropane of these. Examples of commercially available products include Duranate (registered trademark) 24A-100, Duranate 22A-75P, Duranate TPA-100, Duranate TKA-100, Duranate P301-75E, Duranate 21S-75E, Duranate MFA-75B, Duranate MHG-80B, Duranate TUL-100, Duranate TLA-100, Duranate TSA-100, Duranate TSS-100, Duranate TSE100, Duranate E402-80B, Duranate E405-70B, Duranate AS700-100, Duranate D101, Duranate D201, and Duranate A201H (all trade names, manufactured by Asahi Kasei Corporation). Two or more of these may also be used.
[0047] The polyol that gives V is not particularly limited, and known polyols can be used. For example, low molecular weight polyols, polyether polyols, polyester polyols, polycarbonate polyols, etc. are preferably used. Examples of low molecular weight polyols include ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, 1,2-propanediol, 1,3-propanediol, dipropylene glycol, tripropylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 1,5-pentanediol, neopentyl glycol, 1,5-hexanediol, 1,6-hexanediol, 2,5-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,11-undecanediol. aliphatic polyols having a molecular weight of 50 to 300, such as 1,12-dodecanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 2-butyl-2-ethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2-ethyl-1,3-hexanediol, 2-methyl-1,8-octanediol, glycerin, trimethylolpropane, ditrimethylolpropane, trimethylolpropane, and pentaerythritol; polyols having an alicyclic structure, such as cyclohexanedimethanol and hydrogenated bisphenol A; and polyols having an aromatic structure, such as bisphenol A and bisphenol F. Two or more of these may be used.
[0048] Examples of polyether polyols include compounds obtained by addition polymerization of alkylene oxides using one or more compounds having two or more active hydrogen atoms as initiators. Examples of the compounds having two or more active hydrogen atoms include propylene glycol, trimethylene glycol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, glycerin, diglycerin, trimethylolethane, trimethylolpropane, water, hexanetriol, etc. Examples of the alkylene oxides include propylene oxide, butylene oxide, styrene oxide, epichlorohydrin, tetrahydrofuran, etc. Two or more of these may be used.
[0049] Examples of polyester polyols include polyester polyols obtained by reacting low molecular weight polyols with polycarboxylic acids; polyester polyols obtained by ring-opening polymerization of cyclic ester compounds such as ε-caprolactone; and polyester polyols obtained by copolymerizing these. The low molecular weight polyols used in the production of polyester polyols can be the same as the low molecular weight polyols. Examples of polycarboxylic acids include aliphatic polycarboxylic acids such as succinic acid, adipic acid, sebacic acid, and dodecanedicarboxylic acid; alicyclic polycarboxylic acids such as 1,4-cyclohexanedicarboxylic acid and cyclohexanetricarboxylic acid; aromatic polycarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, and naphthalenedicarboxylic acid; and anhydrides or esters thereof. Two or more of these may be used.
[0050] Examples of the polycarbonate polyol include an esterification reaction product of a carbonate ester and a polyhydric alcohol, a reaction product of a polyhydric alcohol and phosgene, etc. Examples of the carbonate ester include an aliphatic carbonate, an alicyclic carbonate, an aromatic carbonate, etc. Examples of the aliphatic carbonate include saturated aliphatic carbonates such as dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, di-n-butyl carbonate, diisobutyl carbonate, ethyl-n-butyl carbonate, and ethyl isobutyl carbonate; and unsaturated aliphatic carbonates such as ethylene carbonate, trimethylene carbonate, tetramethylene carbonate, 1,2-propylene carbonate, 1,2-butylene carbonate, 1,3-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 1,3-pentylene carbonate, 1,4-pentylene carbonate, 1,5-pentylene carbonate, 2,3-pentylene carbonate, and 2,4-pentylene carbonate. Examples of aromatic carbonates include diphenyl carbonate and dibenzyl carbonate. Two or more of these may be used. Examples of polyhydric alcohols include linear or branched diols such as ethylene glycol, propylene glycol, butanediol, pentanediol, 3-methyl-1,5-pentanediol, hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, polyethylene glycol, and polypropylene glycol; alicyclic diols such as 1,4-cyclohexanedimethanol and hydrogenated bisphenol A; and trifunctional or higher polyols such as trimethylolmethane, trimethylolpropane, ditrimethylolpropane, pentaerythritol, and dipentaerythritol. Two or more of these may be used.
[0051] In the embodiment of the present invention, the resin used in the resin film may be obtained from an oligomer such as urethane acrylate, acrylic resin acrylate, or epoxy acrylate. These oligomers have polymerizable groups such as acrylic and methacrylic groups at the molecular chain end, so they can be cured with an electron beam or ultraviolet light to form a resin. Among them, urethane acrylate is preferred because it can hold a semiconductor element and can easily control adhesion and flexibility so that the resin film is appropriately deformed when the semiconductor element is transferred by a laser using method B. Urethane acrylate also contains a repeating unit represented by chemical formula (3), and its description is the same as that of the resin mainly composed of a repeating unit represented by chemical formula (3).
[0052] In the laminate according to the embodiment of the present invention, the loss tangent of the resin film is within a specific range, so that the positional accuracy when transferring the semiconductor element can be improved. Here, the method of adjusting the loss tangent of the resin film is not particularly limited, but for example, a method of controlling the thermal mobility of the resin by adjusting the structure, molecular weight, and degree of crosslinking of the resin can be mentioned. If the thermal mobility of the resin is low, the loss tangent can be designed to be small, and conversely, if the thermal mobility of the resin is high, the loss tangent can be designed to be large. Increasing the rigidity of the resin reduces the thermal mobility of the resin, and increasing the flexibility of the resin increases the thermal mobility of the resin. In order to increase the rigidity of the resin, it is effective to use a monomer having an aromatic group as a raw material. In addition, if a monomer having a functional group that brings about an intermolecular force such as hydrogen bonding is used, the intermolecular force between the resins is also increased, so that the thermal mobility of the resin decreases. Conversely, if these monomers are not used, the thermal mobility of the resin increases. On the other hand, in order to increase the flexibility of the resin, it is effective to use a monomer having a structure represented by the above chemical formulas (11) to (13) as a raw material in the case of polyimide, or a polyol having a molecular weight of 500 or more as a raw material in the case of polyurethane and urethane acrylate. The proportion of the monomers used to increase the flexibility in 100 parts by mass of the total monomers is preferably 50 parts by mass or more, more preferably 60 parts by mass or more. If it is 50 parts by mass or more, the thermal mobility of the resin is increased, and it is easy to design the loss tangent α to 0.01 or more and the loss tangent β to 0.4 or more. Therefore, the resin film is more likely to hold the semiconductor element, and the risk of the semiconductor element laminated on the resin film being displaced or falling can be reduced. On the other hand, if the thermal mobility is too high, the loss tangent α exceeds 0.15 and the transfer accuracy decreases, so that it is preferably 80 parts by mass or less, more preferably 70 parts by mass or less. If the molecular weight of the resin is increased, the entanglement of molecular chains increases, which acts as a crosslinking point to reduce the thermal mobility of the resin. By setting the molecular weight of the resin to a weight average molecular weight of preferably 5000 or more, more preferably 10000 or more, the thermal mobility of the resin can be sufficiently reduced. In addition, by coexisting a crosslinking agent described later, crosslinking points can be formed when the resin film is formed, and the thermal mobility of the resin can be reduced. In addition, increasing the rigidity of the resin or increasing the degree of crosslinking by using a crosslinking agent is also effective in increasing the storage modulus.
[0053] <Light absorber> The above absorbance can also be achieved by incorporating an ultraviolet absorbing agent or a light absorbing agent such as a dye, a coloring matter, or a pigment in the resin film. Examples of the light absorber contained in the resin film include ultraviolet absorbers such as Tinuvin PS, Tinuvin 99-2, Tinuvin 326, Tinuvin 328, Tinuvin 384-2, Tinuvin 400, Tinuvin 405, Tinuvin 460, Tinuvin 477, Tinuvin 479, Tinuvin 900, Tinuvin 928, Tinuvin 1130 (all trade names, manufactured by BASF), DAINSORB T-0, DAINSORB T-7, DAINSORB T-31, DAINSORB T-52, DAINSORB T-53, DAINSORB T-84, DAINSORB P-6, and DAINSORB P-7 (all trade names, manufactured by Daiwa Chemical Industry Co., Ltd.); Solvent Yellow 93, Solvent Yellow 33, Solvent Orange 60, Solvent Red 111, Solvent Red 135, Solvent Red 168, and Solvent Examples of dyes, dyes and pigments include Red 207, Solvent Red 52, Solvent Red 179, Solvent Blue 36, Solvent Blue 94, Solvent Blue 63, Solvent Blue 104, Solvent Blue 97, Solvent Green 20, Solvent Violet 13, Solvent Violet 36 (all trade names, manufactured by Tokyo Chemical Industry Co., Ltd.), carbon black, perylene black, cyanine black, and aniline black.
[0054] These may be contained alone or in combination in the resin film. The content of the light absorbent for bringing the absorbance into the above range is preferably 0.1 parts by mass or more relative to 100 parts by mass of the resin film, and is preferably 50 parts by mass or less from the viewpoint of stability in the varnish state before forming the laminate.
[0055] <Crosslinking agent> The resin film in the laminate according to the embodiment of the present invention preferably contains a crosslinking agent. By adding a crosslinking agent, a part of the structure is crosslinked to harden the surface of the resin film, and the adhesive strength can be adjusted. Furthermore, the surface of the resin film is crosslinked and strengthened, which enhances the effect of suppressing adhesive residue. As mentioned above, increasing the degree of crosslinking of the resin in the resin film can also contribute to making the loss tangent of the resin film relatively small.
[0056] Examples of the crosslinking agent include compounds having an alkoxymethyl group or a methylol group, such as DML-PC, DML-PEP, DML-OC, DML-OEP, DML-34X, DML-PTBP, DML-PCHP, DML-OCHP, DML-PFP, DML-PSBP, DML-POP, DML-MBOC, DML-MBPC, DML-MTrisPC, DML-BisOC-Z, DMLBisOCHP-Z, DML-BPC, DML-BisOC-P, DMOM-PC, DMOM-PTBP, Examples of such compounds include DMOM-MBPC, TriML-P, TriML-35XL, TML-HQ, TML-BP, TML-pp-BPF, TML-BPE, TML-BPA, TML-BPAF, TML-BPAP, TMOM-BP, TMOM-BPE, TMOM-BPA, TMOM-BPAF, TMOM-BPAP, HML-TPPHBA, HML-TPHAP, HMOM-TPPHBA, and HMOM-TPHAP (all trade names, manufactured by Honshu Chemical Industry Co., Ltd.), and "NIKALAC (registered trademark)" MX-290, NIKALAC MX-280, NIKALAC MX-270, NIKALAC MX-279, NIKALAC MW-100LM, and NIKALAC MX-750LM (all trade names, manufactured by Sanwa Chemical Co., Ltd.).
[0057] In addition, it is also preferable to include a compound having an epoxy group as a crosslinking agent. Examples of the compound having an epoxy group include, but are not limited to, bisphenol A type epoxy resin, bisphenol F type epoxy resin, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, epoxy group-containing silicone such as polymethyl(glycidyloxypropyl)siloxane, and dimer acid modified epoxy resin. Specifically, Epicron 850-S, Epicron HP-4032, Epicron HP-7200, Epicron HP-820, Epicron HP-4700, Epicron EXA-4710, Epicron HP-4770, Epicron EXA-859CRP, Epicron EXA-1514, Epicron EXA-4880, Epicron EXA-4850-150, Epicron EXA-4850-1000, Epicron EXA-4816, Epicron EXA-4822 (all trade names, manufactured by DIC Corporation), and Rikaresin Examples of such products include BEO-60E (hereinafter referred to as trade name, manufactured by New Japan Chemical Co., Ltd.), EP-4003S, EP-4000S (all trade names, manufactured by Adeka Corporation), JER871, JER872, YX-4000, YX-4000H (all trade names, manufactured by Mitsubishi Chemical Corporation), Celloxide 2021P (all trade names, manufactured by Daicel Corporation), Showfree PETG, Showfree CDMGB, Showfree BATG (all trade names, manufactured by Resonac Corporation), Denacol EX-201-IM (all trade names, manufactured by Nagase ChemteX Corporation), and TEPIC-VL (all trade names, manufactured by Nissan Chemical Co., Ltd.).
[0058] It is also preferable to have a crosslinking agent having an oxetanyl group, and specific examples include OXT-121, OXT-221, OX-SQ-H, OXT-191, PNOX-1009, RSOX (all trade names, manufactured by Toagosei Co., Ltd.), "Etanacol (registered trademark)" OXBP, and "Etanacol" OXTP (all trade names, manufactured by UBE Corporation).
[0059] The resin film may contain two or more kinds of crosslinking agents, and it is preferable that the crosslinking agent is contained in an amount of 1 part by mass or more in 100 parts by mass of the resin film. If the crosslinking agent is contained in an amount of 1 part by mass or more, the adhesive strength of the resin film can be reduced to reduce adhesive residue or to reduce the loss tangent. More preferably, the crosslinking agent is contained in an amount of 3 parts by mass or more in 100 parts by mass of the resin film. In addition, it is preferable that the crosslinking agent is contained in an amount of 25 parts by mass or less in 100 parts by mass of the resin film. If the crosslinking agent is contained in an amount of 25 parts by mass or less, an excessive decrease in the adhesive strength of the resin film can be prevented, and a semiconductor element can be stably held when stacked on the resin film. In addition, a curing accelerator may be contained for the purpose of promoting curing by a crosslinking agent. Examples of the curing accelerator include the curing accelerators described in WO 2022 / 210155.
[0060] <Photopolymerization initiator> When a resin is obtained from an oligomer such as urethane acrylate, acrylic resin acrylate, or epoxy acrylate, a photopolymerization initiator can be added to promote polymerization of polymerizable groups such as acrylic and methacrylic groups at the molecular chain terminals. The photopolymerization initiator is not particularly limited, and a conventionally known photopolymerization initiator for UV curing can be used. Examples of the photopolymerization initiator include acetophenone-based polymerization initiators, phosphine oxide-based polymerization initiators, benzoyl formate-based polymerization initiators, thioxanthone-based polymerization initiators, oxime ester-based polymerization initiators, hydroxybenzoyl-based polymerization initiators, benzophenone-based polymerization initiators, and α-aminoalkylphenone-based polymerization initiators. Acetophenone-based polymerization initiators include acetophenone, 3-methylacetophenone, benzyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 2-methyl-1-[4-(methylthio)phenyl-2-morpholinopropan-1-one, and 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one. etc. Examples of the phosphine oxide polymerization initiator include phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide and diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide. Benzoyl formate-based polymerization initiators include methyl benzoyl formate and the like. An example of the thioxanthone-based polymerization initiator is isopropylthioxanthone. Examples of the oxime ester polymerization initiator include 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime), and the like. Examples of the hydroxybenzoyl-based polymerization initiator include 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, and benzoin alkyl ether. Benzophenone-based polymerization initiators include benzophenone, 4-chlorobenzophenone, and 4,4'-diaminobenzophenone. Examples of the α-aminoalkylphenone polymerization initiator include 2-methyl-1-(4-methylthiophenyl)-2-morpholinopro-butanone-1 and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone. The photopolymerization crosslinking agent may be contained in two or more kinds in the resin film, and is preferably contained in an amount of 0.1 parts by mass or more in 100 parts by mass of the resin film. If it is 0.1 parts by mass or more, it is possible to promote polymerization of the polymerizable group such as an acrylic group or a methacrylic group at the molecular chain terminal of the oligomer, and harden the resin film. Also, it is preferably 1 part by mass or less.
[0061] <Other additives> In addition, the resin film may further contain a silane compound as necessary. By containing a silane compound, the adhesion between the resin film and the first substrate having laser transparency can be adjusted. This makes it possible to prevent the resin film in the portion not irradiated with the laser light from peeling off from the first substrate having laser transparency. Specific examples of the silane compound include the silane compounds described in International Publication No. 2022 / 210155. Furthermore, the resin film may contain a surfactant, if necessary, for the purpose of improving the coatability with the first substrate having laser transparency during film formation and forming a resin film with a uniform thickness.
[0062] <Semiconductor element> Next, the semiconductor element in the second stack according to the embodiment of the present invention will be described. The semiconductor element in the present invention includes semiconductors such as GaN, AlN, InN, InP, GaAs, Si, and SiC that are made into an element. These semiconductor elements include those in which different types of semiconductors are further laminated, and those in which electrode materials, sapphire substrates, glass substrates, wiring, etc. are laminated. The size of the semiconductor element is preferably 5 μm or more and 5.0 mm or less on one side. More preferably, it is 3.0 mm or less. This allows the laser to be focused and irradiated with a small spot diameter, making it possible to transfer with high positional accuracy. The adhesive strength of the surface where the resin film contacts the semiconductor element is preferably 0.02 N / cm or more and 0.3 N / cm or less.
[0063] The number of semiconductor elements mounted on the second stack according to the embodiment of the present invention is 5 / cm per unit area. 2 More preferably, 50 / cm 2 By increasing the number of semiconductor elements to the above lower limit, the effect of improving throughput by using laser transfer is increased. In addition, since the laser can be accurately irradiated to each semiconductor element, the number of semiconductor elements mounted on the second laminate can be increased to 500,000 / cm. 2 Preferably less than 100,000 particles / cm, more preferably 100,000 particles / cm 2 The following is the result.
[0064] The stacking order of the second laminate of the present invention may be a laser-transmitting first substrate, a resin film, and a semiconductor element, with another layer being allowed in between. However, the semiconductor element is formed in contact with the resin film, and the laser-transmitting first substrate and the semiconductor element are located on the outermost surface of the second laminate. That is, the first substrate is located on one outermost surface of the second laminate, and the semiconductor element is located on the other outermost surface of the second laminate.
[0065] <Resin manufacturing method> The resin having as its main component the repeating unit represented by chemical formula (1) or (2) can be polymerized by a known method. For example, polyamic acid can be obtained by polymerizing tetracarboxylic acid or a corresponding acid dianhydride, active ester, active amide, etc. as an acid component and diamine or a corresponding trimethylsilylated diamine, etc. as a diamine component in a reaction solvent. The polyamic acid may be one in which the carboxyl group forms a salt with an alkali metal ion, ammonium ion, or imidazolium ion, or one esterified with a hydrocarbon group having 1 to 10 carbon atoms or an alkylsilyl group having 1 to 10 carbon atoms. On the other hand, polyimide can be obtained by imidizing polyamic acid by a method described later.
[0066] The reaction solvent is not particularly limited, and known ones can be used. For example, N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylisobutyramide, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, γ-butyrolactone, ethyl lactate, 1,3-dimethyl-2-imidazolidinone, N,N'-dimethylpropyleneurea, 1,1,3,3-tetramethylurea, dimethylsulfoxide, sulfolane, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, diethylene glycol ethyl methyl ether, diethylene glycol dimethyl ether, water, and the reaction solvents described in International Publication No. 2017 / 099183 can be used alone or in combination of two or more.
[0067] The amount of the reaction solvent used is preferably adjusted so that the total amount of the tetracarboxylic acid and the diamine compound is 0.1 to 50% by mass of the entire reaction solution. The reaction temperature is preferably -20°C to 150°C, more preferably 0 to 100°C. The reaction time is preferably 0.1 to 24 hours, more preferably 0.5 to 12 hours. The number of moles of the diamine compound and the number of moles of the tetracarboxylic acid used in the reaction are preferably equal. If they are equal, a resin film with high mechanical properties is easily obtained from the resin composition. The obtained polyamic acid solution may be used as it is as a raw material for a resin composition. In this case, the same solvent as that used for the resin composition may be used as the reaction solvent, or an additive or solvent may be added after the reaction is completed, so that the desired resin composition can be obtained without isolating the resin.
[0068] The polyamic acid obtained may further be imidized or esterified in part or all of the repeating units of the polyamic acid. In this case, the polyamic acid solution obtained by polymerization of the polyamic acid may be used in the next reaction as it is, or the polyamic acid may be isolated and then used in the next reaction. In the esterification and imidization reactions, the target resin composition can be obtained without isolating the resin by using as the reaction solvent the same as the solvent used for the resin composition, or by adding an additive or a solvent after completion of the reaction.
[0069] The imidization method is preferably a method of heating the polyamic acid, or a method of adding a dehydrating agent and an imidization catalyst and heating as necessary. In the latter method, a process of removing the reaction product of the dehydrating agent and the imidization catalyst is required, so the former method is more preferable. There are no particular limitations on the dehydrating agent and the imidization catalyst, and known ones can be used.
[0070] Examples of the reaction solvent used for the imidization include the reaction solvents exemplified for the polymerization reaction.
[0071] The reaction temperature of the imidization reaction is preferably 0 to 180° C., and more preferably 10 to 150° C. The reaction time is preferably 1.0 to 120 hours, and more preferably 2.0 to 30 hours. By appropriately adjusting the reaction temperature and reaction time within these ranges, a desired proportion of the polyamic acid can be imidized. The esterification method is preferably a method of reacting an esterifying agent or a method of reacting an alcohol in the presence of a dehydration condensation agent. There are no particular limitations on the materials and reaction conditions used for the esterification, and known materials can be used.
[0072] Moreover, a resin mainly composed of a repeating unit represented by chemical formula (3) can also be polymerized by a known method. For example, polyurethane can be obtained by polymerizing polyisocyanate and polyol. If necessary, a urethanization catalyst may be used. Examples of the urethanization catalyst include nitrogen-containing compounds such as triethylamine, tributylamine, benzyldibutylamine, triethylenediamine, and N-methylmorpholine; organic metal compounds such as titanium tetrabutoxide, dibutyltin oxide, dibutyltin dilaurate, tin 2-ethylcaproate, zinc naphthenate, cobalt naphthenate, zinc 2-ethylcaproate, molybdenum glycolate, potassium acetate, zinc stearate, tin octoate, dibutyltin dilaurate, and dioctyltin dineodecanoate; and inorganic compounds such as iron chloride and zinc chloride. Two or more of these may be used.
[0073] A reaction solvent may be used, and the same reaction solvent as that used in the polymerization of polyamic acid or polyimide can be used. The reaction temperature is preferably 0 to 100°C, more preferably 40 to 90°C. The reaction time is preferably 1.0 to 120 hours, more preferably 2.0 to 30 hours. In addition, it is preferable that the number of moles of isocyanate groups contained in the polyisocyanate used in the reaction is equal to the number of moles of hydroxyl groups contained in the polyol. If they are equal, a resin film having high mechanical properties can be easily obtained from the resin composition.
[0074] <Method of producing resin composition> As an example, the resin and, if necessary, additives such as a light absorber and a crosslinking agent are dissolved in a solvent to obtain a resin composition as a varnish, and the resin composition is formed into a film to obtain a resin film in a laminate. Methods for dissolving the resin when obtaining a resin composition (varnish) include stirring and heating, and stirring is usually performed at room temperature to 80°C. The order of dissolving each component is not particularly limited, and for example, there is a method in which compounds with low solubility are dissolved in order. The varnish obtained by these manufacturing methods is preferably filtered using a filter to remove foreign matter such as dust.
[0075] <Method of manufacturing laminate> Next, a method for producing a laminate according to an embodiment of the present invention will be described. The first laminate is obtained by forming a resin film on a first substrate having laser transparency. An example of a method for producing the first laminate will be described. The above-mentioned varnish is applied to a first substrate having laser transparency, and the resin film is produced by heating and curing. When the resin film is produced by a coating method, any coating method can be selected, and examples of the method include spin coating using a spinner, spray coating, roll coating, and slit die coating. The resin film after coating is preferably dried at a range of 50°C to 150°C for 1 minute to several tens of minutes using a hot plate, a drying oven, infrared rays, etc. Then, if necessary, the resin film is heated and cured at a range of 100°C to 500°C for several minutes to several hours. The thickness of the resin film at this time is preferably 0.7 μm to 30 μm. The thickness can be measured using a scanning electron microscope, an optical thickness gauge, a step gauge, etc.
[0076] Next, an example of a method for stacking semiconductor elements to produce a second stack will be described with reference to the drawings. 1 to 3 show an example of a method for producing the second laminate (120). When producing the second laminate by the method of FIG. 1, the semiconductor element (14) is directly arranged on the resin film (12) of the first laminate (110) in which the resin film (12) is laminated on the first substrate (11) having laser transparency, and laminated by pressing with a pressing device (41) such as a vacuum laminator, a wafer bonder, or a press machine. Alternatively, as shown in FIG. 2, a semiconductor element temporary bonding substrate (130) in which the semiconductor element (14) is temporarily bonded to another support (15) via a temporary adhesive (16) is prepared, and the semiconductor element (14) on the temporary adhesive (16) and the resin film (12) surface of the first laminate (110) are overlapped and pressed with the above-mentioned pressing device (41). Thereafter, the temporary adhesive (16) and the support (15) are removed from the semiconductor element (14), and the second laminate (120) can be produced. 3, a semiconductor element-mounted substrate (140) in which a semiconductor element (14) is directly fabricated on a crystal growth substrate (17) such as sapphire is stacked with the semiconductor element (14) surface facing the resin film (12) surface, and pressure-bonded by the above-mentioned device (41). Thereafter, a second stack (120) can be fabricated by a technique such as irradiating a laser beam (31) from the crystal growth substrate (17) side and laser lifting off the semiconductor element (14) from the crystal growth substrate (17) to the first stack (110) side.
[0077] The pressure when stacking the semiconductor elements can be selected at an optimum value depending on the adhesive strength of the resin film, and is selected, for example, in the range of 0.05 MPa to 5.0 MPa. In order to avoid damage to the semiconductor elements and to suppress embedding in the resin film, it is more preferable that the pressure be 2.0 MPa or less. In addition, when stacking the semiconductor elements, it is also possible to apply pressure while heating as necessary. Heating increases the flexibility of the resin film, and allows the semiconductor elements to be compressed at a lower pressure. Furthermore, by providing alignment marks on the laminate in advance, it becomes easier to adjust the transfer position in the subsequent operations.
[0078] Furthermore, another method for producing the second laminate will be described with reference to FIG. 4. The semiconductor substrate (18) before being singulated is attached to another support (15) via a temporary adhesive (16). Furthermore, varnish is applied onto the semiconductor substrate (18) before being singulated, and the varnish is heated and cured to form a resin film (12). In this state, the laser-transparent first substrate and the support with the resin film are bonded face to face. The support (15) and the temporary adhesive (16) adjacent to the support (15) are peeled off and removed, and then the semiconductor substrate (18) is singulated to form semiconductor elements (14), thereby producing the second laminate (120).
[0079] <Method of Manufacturing Semiconductor Device> Next, a method for manufacturing the semiconductor device will be described. A method for manufacturing a semiconductor device according to an embodiment of the present invention is a method for manufacturing a semiconductor device using the second stack, and includes the following steps (a) and (b). (a) A step of disposing a second substrate so as to face the surface of the second laminate on which the semiconductor elements are laminated. (b) A step of irradiating the second laminate with laser light from the side of the first substrate to transfer a semiconductor element to the second substrate.
[0080] The process of facing the semiconductor element surface of the second laminate to the second substrate will be described with reference to the drawings. Fig. 5 illustrates an example of a method for manufacturing a semiconductor device. The semiconductor element surface refers to the surface of the second stack (120) that has the semiconductor element (14) thereon (the surface on which the semiconductor element is stacked). With respect to the second laminate (120) and second substrate (21) produced by the above-mentioned method, the surface of the second laminate (120) on which the semiconductor element (14) is held is placed opposite the second substrate (21), and the substrate is fixed so that the second laminate (120) and the second substrate (21) are parallel to each other. In order to prevent misalignment due to the weight of the semiconductor element (14) during transfer, the second laminate (120) and the second substrate (21) are placed opposite each other with the second laminate (120) facing upward. The second laminate and the second substrate are placed with a certain distance between them. The distance between the semiconductor element surface and the second substrate can be selected depending on the size and thickness of the semiconductor element, and is selected, for example, in the range of several μm to several hundreds of μm.
[0081] The second substrate may be any substrate, such as a glass substrate, a resin substrate, a metal substrate, or a circuit substrate on which wiring has already been formed. The second substrate may have an adhesive layer to hold the semiconductor element after transfer. The adhesive layer may be made of a material having adhesive properties, such as polysiloxane resin, acrylic resin, polyester resin, ACF (Anisotropic Conductive Film) resin, conductive silver paste, or a resin film similar to the resin film in the laminate according to the embodiment of the present invention. The thickness of the adhesive layer is selected, for example, within the range of 0.5 μm to 100 μm, depending on the size of the semiconductor element and the distance between the semiconductor element and the second substrate. Furthermore, for the purpose of transfer alignment, there may be an alignment mark on the second substrate as well.
[0082] Next, the process of transferring the semiconductor element to the second substrate by irradiating the second laminate with laser light from the first substrate side having laser transparency will be described with reference to the drawings. An example of the transfer process is shown in (a) of FIG. 6. In the second laminate (120) and the second substrate (21) arranged by the above-mentioned method, the semiconductor element is irradiated with laser light (31) from the laser-transmissive first substrate (11) side of the second laminate (120) through the laser-transmissive first substrate (11). The type of laser light includes solid lasers such as YAG laser, YVO4 laser, fiber laser, and semiconductor laser, and gas lasers such as carbon dioxide laser, excimer laser, and argon laser, and can be selected according to the wavelength to be used. The beam shape of the irradiated laser light is not limited, and the laser spot size may be smaller than the size of the semiconductor element. However, the size must be such that the laser light does not hit the semiconductor element adjacent to the semiconductor element to be transferred.
[0083] In addition, when the spot size of the laser light is large enough to hit adjacent semiconductor elements, it is also possible to irradiate the laser light (31) through a photomask (51) as shown in FIG. 6(b). The laser light can be selected with any energy density. From the viewpoint of the stability of the energy density of the laser light, the energy density of the laser light is set to 1 mJ / cm. 2 The above is preferable, and from the viewpoint of preventing damage to the semiconductor element and shortening the processing time, 1000 mJ / cm 2 More preferably, the energy density of the laser beam is 10 mJ / cm or less. 2 More than 500mJ / cm 2 The following is the result.
[0084] By using the second laminate according to the embodiment of the present invention, transfer is possible even with low energy, and further, even when the energy density of the laser light is changed, the effects on positional accuracy, debris, and adhesive residue can be reduced. The energy density of the irradiated laser light may have output unevenness, and in order to reduce the effects of output unevenness on transferability, it is preferable that the second laminate has the same level of transferability regardless of the energy density of the laser light. The range of energy densities of laser light that has the same level of transferability is 30 mJ / cm. 2It is preferable to have a margin of at least 50 μm / cm. 2 The above is particularly preferred.
[0085] It is also possible to heat the second substrate when transferring the semiconductor element. In particular, when an adhesive layer is formed on the second substrate, heating the second substrate is preferable because it improves the retention of the transferred semiconductor element. When heating the second substrate, it is preferable that the heating temperature is 120° C. or less, since this prevents the second substrate from warping due to heat and allows for transfer with good positional accuracy.
[0086] The semiconductor elements are transferred while adjusting the position according to the actual mounting location of the semiconductor elements in the semiconductor device to be fabricated. For example, when fabricating an LED board, the LED elements are transferred while shifting the pitch according to the LED pixel size and the RGB arrangement. Next, the second board on which the LED elements have been transferred and the circuit board are placed face to face, and the circuit board is pressure-bonded to the circuit board to fabricate a circuit board on which the LED elements are mounted. When the transfer is performed using the laminate according to the embodiment of the present invention, the transfer can be performed with high positional accuracy, so that the semiconductor elements can be transferred without being misaligned from the circuit of the board to be finally mounted, and mounting defects caused by misalignment can be reduced.
[0087] The laser light preferably has a wavelength of 248 nm, 266 nm, 308 nm, 355 nm, 532 nm, or 1064 nm, and more preferably has a wavelength that has an absorbance of 0.4 or more in the resin film. By using such a laser light, damage to the semiconductor element can be reduced. In the method for manufacturing a semiconductor device according to the embodiment of the present invention, the laser light preferably has a wavelength of 248 nm, 266 nm, 308 nm, or 355 nm, and more preferably has a wavelength of 355 nm. This allows accurate transfer of even minute semiconductor elements such as μLEDs. As the laser light of 248 nm, 266 nm, 308 nm, or 355 nm, an excimer laser or a YAG laser is particularly preferred.
[0088] In addition, in the method for manufacturing a semiconductor device of the present invention, the second substrate is preferably a circuit substrate. If the second substrate is a circuit substrate, the substrate transferred by the above method can be directly fabricated into a semiconductor device. There is no concern about misalignment due to handling of the substrate after transfer, and the positional accuracy can be further improved. As the circuit substrate, a known one such as a TFT substrate or a printed wiring substrate can be used. EXAMPLES
[0089] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. First, the evaluation methods used in each example and comparative example will be described.
[0090] (1) Method for producing laminate A resin film varnish prepared by the method described below was applied using a spinner to a 4-inch quartz glass substrate with a thickness of 0.6 mm (manufactured by Taiko Seisakusho Co., Ltd., with an absorbance of 0.01 at wavelengths of 248 nm, 266 nm, 308 nm and 355 nm), pre-baked on a hot plate, and then cured to produce a resin film on the glass substrate, thereby producing a first laminate. The pre-bake conditions are as follows. Examples 1 to 6 and Comparative Examples 1 to 5: 120°C, 3 minutes Example 7, Comparative Examples 6 and 7: 80°C, 1 minute The curing conditions are as follows: Examples 1 to 5 and Comparative Examples 1 to 3: Using a gas oven "INH-21CD" (manufactured by Koyo Thermo Systems Co., Ltd.), the composition was heated from room temperature to 250°C in a nitrogen atmosphere (oxygen concentration 100 ppm or less), heated at 200°C for 30 minutes, and finally cooled to room temperature for heat curing. Example 6, Comparative Examples 4 and 5: Using a gas oven "INH-21CD" (manufactured by Koyo Thermo Systems Co., Ltd.), the composition was heated from room temperature to 250°C in a nitrogen atmosphere (oxygen concentration 100 ppm or less), heated at 250°C for 30 minutes, and finally cooled to room temperature to be heat-cured. Example 7, Comparative Examples 6 and 7: Using a mask aligner "PEM-6M" (manufactured by Union Optical Co., Ltd.), a mixed spectrum of ghi lines was irradiated at an exposure dose of 1000 mJ / cm without using a mask. 2 It was cured by irradiation. The thickness of the resin film was measured with an optical film thickness meter (Lambda Ace, manufactured by Dainippon Screen Co., Ltd., refractive index = 1.543). Separately, a 4-inch LED substrate (EPILEDS, with alignment marks) was prepared and cut into 20 mm squares using a dicer. The LEDs mounted on it are as follows. The size of the semiconductor element, the size of the protruding electrode part, and the distance between adjacent elements were measured using a scanning electron microscope (Hitachi High-Technologies Corporation, S-4800). Crystal growth substrate: Sapphire (thickness 0.8 mm) Semiconductor element type: GaN Size of semiconductor element: 20.2μm×30.3μm×9.4μm (including electrodes) Number of electrodes: 2 on each side Electrode size: 17.5μm×11.0μm×3.4μm Electrode type: Au Distance between adjacent elements: 10.0 μm
[0091] The resin film surface of the first laminate was placed in contact with the semiconductor element surface of the 4-inch LED substrate, and the two were bonded together by applying a pressure of 57.8 kN, 80°C, and 2 minutes using a flip chip bonder (Toray Engineering Co., Ltd., FC-3000WS). Then, a 266 nm wavelength laser device (HOYA Corporation, HSL-5500IIISUV, pulse width 5-7 nec, energy density 600 mJ / cm) was used from the first substrate side. 2 ) a laser was irradiated onto the entire surface of the LED substrate, and the crystal growth substrate was separated at the interface between the crystal growth substrate and the semiconductor element to produce a second laminate.
[0092] (2) Measurement of resin film absorbance For the first laminate prepared in (1), the transmittance from 200 nm to 1100 nm was continuously measured using an ultraviolet-visible spectrophotometer (U-2910, manufactured by Hitachi High-Tech Science Corporation). From the measured values, the values at 248 nm, 266 nm, and 355 nm were read, and the respective absorbances per 1.0 μm of film thickness were calculated using the following formula. In the measurement, a substrate similar to that used for the first laminate was measured in advance as a reference sample, and the absorbance of the resin film was obtained by subtracting the measured value of the reference sample from the measurement result of the first laminate. Absorbance per 1.0 μm of film thickness = (-log 10 (Transmittance)) / (Measured film thickness [μm]) For example, when the transmittance is 5% (=0.05) and the measured film thickness is 15 μm, Absorbance per 1.0 μm of film thickness = (-log 10 (0.05)) / 15 ≒ 0.087 It is required. For the second laminate produced by the method (1) described above, a dicing tape (UDC-1025MC) was attached to the semiconductor element surface and then peeled off to peel off the semiconductor element from the resin film. The transmittance was measured and the absorbance was calculated in the same manner as described above.
[0093] (3) Measurement of loss tangent and storage modulus The loss tangent α, loss tangent β and storage modulus were measured using a dynamic viscoelasticity measuring device (DVA-200, manufactured by IT Measurement & Control Co., Ltd.). First, the first laminate prepared in (1) was irradiated with a laser from the quartz glass substrate side using an excimer laser device (manufactured by Light Machinery, laser wavelength 308 nm) under the following conditions to separate the resin film and the quartz glass substrate. Energy density on the irradiated surface: 220mJ / cm 2 Repetition frequency: 30Hz Irradiation surface beam size: 2mm x 14mm Scan direction: Short axis direction Scan speed: 19.5mm / sec Longitudinal overlap: 2mm For the second laminate produced by the method (1) above, a dicing tape (UDC-1025MC) was attached to the semiconductor element surface, and the semiconductor element was peeled off from the resin film by peeling it off, and the resin film and the quartz glass substrate were separated in the same manner as above. Next, the resin film was cut into a size of 5 mm x 20 mm and used for measurement. [Measurement conditions] Measurement temperature: -130~25℃ Measurement frequency: 0.5 to 100 Hz Deformation mode: tension Initial grip length: 1cm Static / dynamic stress ratio: 1.7 Set distortion: 0.1% Heating rate: 2℃ / min Using the obtained data, a master curve was created with 25°C as the reference temperature. 6 The loss tangent (loss tangent α) and storage modulus in Hz were calculated. Also, from the same master curve, the loss tangent (α) and storage modulus in Hz were calculated. -2 The loss tangent (loss tangent β) in Hz was calculated.
[0094] (4) Evaluation of the adhesiveness of the resin film For the second laminate produced in (1), the yield of semiconductor elements transferred from the 4-inch LED substrate was calculated using the following formula. Yield = (any 1 mm of the second laminate 2 Number of semiconductor elements transferred from a 4-inch LED board) / (1mm of a 4-inch LED board) 2 (Number of chips per unit (1124)) The adhesiveness was evaluated based on the yield obtained. 98% or more was rated as "++++", 90% to less than 98% was rated as "+++", 70% to less than 90% was rated as "++", less than 70% was rated as "+", and 0% was rated as "0". For example, any 1 mm of the second laminate 2 When the number of semiconductor elements transferred is 1050, Yield = 1050 / 1124 = 93% Therefore, it is judged as "+++".
[0095] (5) Semiconductor element transfer test (5-1) Preparation of the opposing substrate Polydimethylsiloxane was diluted with toluene on a 4-inch alkali-free glass substrate (Corning Eagle XG) with a thickness of 0.5 mm, and the diluted solution was adjusted so that the mass ratio of polydimethylsiloxane to toluene was 1:3. The diluted solution was applied using a spinner and heated and cured on a hot plate at 120°C for 3 minutes to form an adhesive layer on the glass substrate. The thickness of the adhesive layer after thermal curing was measured with an optical film thickness meter (Dainippon Screen Co., Ltd., Lambda Ace, refractive index = 1.543), and a second substrate was prepared as an opposing substrate with an adhesive layer thickness of 5.0 μm.
[0096] (5-2) Transfer of semiconductor elements The laser light source, the second laminate produced by the above-mentioned method, and the second substrate were arranged in this order in the vertical direction. At this time, the surface of the second laminate on which the semiconductor element was held and the surface of the opposing second substrate on which the adhesive layer was formed were held facing each other so that the distance between the semiconductor element surface and the adhesive layer surface was 50 μm (about 6 times the height of the semiconductor element). The spot size of the laser light was a square shape of 18 μm × 36 μm, and the positions of the laser light source and the laminate were adjusted so that one semiconductor element was placed in the center of the laser light spot, and the laser light was not irradiated onto adjacent semiconductor elements. A YAG laser (HSL-5500IIIST, manufactured by HOYA Corporation) with a wavelength of 355 nm was used as the laser light source. A laser beam with a wavelength of 355 nm was irradiated to the semiconductor element placed at the laser light irradiation position at 250 to 400 mJ / cm. 2 Between 50mJ / cm 2 The irradiation was performed while changing the energy density step by step. For each energy density, a laser transfer test was performed on 20 semiconductor elements.
[0097] (5-3) Evaluation of transcription yield The opposing second substrate after irradiation with the laser beam (5-2) was observed, and the number of semiconductor elements that were transferred normally without being damaged or turned over was counted, and the transfer yield was calculated by the following formula. Transfer yield = number of semiconductor elements transferred normally / total number of semiconductor elements transferred by laser The transferability was evaluated based on the transfer yield obtained: 95% or more was rated as "A", 80% to less than 95% was rated as "B", 50% to less than 80% was rated as "C", and less than 50% was rated as "D". For example, if 20 semiconductor elements are laser-transferred and 15 of them are successfully transferred, Transcription yield = 15 / 20 = 75% Therefore, the answer is "B".
[0098] (5-4) Evaluation of position accuracy Except for the level judged as "D" in (5-3), the positional accuracy was evaluated by the following method. Using a CCD camera projected from a lens installed coaxially with the laser light source, an image of the semiconductor element on the second laminate before laser transfer and an image of the semiconductor element on the second substrate after laser transfer were acquired, and the amount of positional deviation of the center of the semiconductor element before and after transfer was calculated from the central coordinates of the semiconductor element in each acquired image. The amount of positional deviation was calculated only for semiconductor elements that were transferred normally, and the positional accuracy was evaluated based on the average value. An average value of 0 μm or more and less than 1.5 μm was judged as "a", 1.5 μm or more and less than 2 μm was judged as "b", 2 μm or more and less than 3 μm was judged as "c", and 3 μm or more was judged as "d".
[0099] (6) Method for measuring the solid content of a resin solution Approximately 1 g of the resin solution produced by the method described below was weighed out into an aluminum cup, placed on a hot plate at 120°C and heated for 3 minutes, then heated to 250°C, and heated for 30 minutes after reaching 250°C. The mass of the resin remaining after heating was measured, and the solid content was calculated using the following formula. Solid content (mass%) = mass of resin after heating [g] / mass of resin solution before heating [g] For example, when 1.10 g of resin solution is heated and the mass of the remaining resin is 0.60 g, Solid content = 0.60 / 1.10 ≒ 0.55 (i.e., 55% by mass) It is required. The abbreviations for the raw materials, additives, and solvents used in the synthesis examples and preparation examples are as follows. MDI: Diphenylmethane diisocyanate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) PTMG: Polytetramethylene oxide (average molecular weight: 1000, Fujifilm Wako Pure Chemical Industries, Ltd.) BPDA: 3,3',4,4'-biphenyltetracarboxylic anhydride (manufactured by Mitsubishi Chemical Corporation) BTDA: 3,3',4,4'-benzophenonetetracarboxylic anhydride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) BAHF: 4,4'-dihydroxy-3,3'-diaminophenylhexafluoropropane (Merck) APPS1: α,ω-bis(3-aminopropyl)polydimethylsiloxane (average molecular weight: 860, q=9 (average value)) (manufactured by Shin-Etsu Chemical Co., Ltd.) APPS2: α,ω-bis(3-aminopropyl)polydimethylsiloxane (average molecular weight: 1600, q=19 (average value)) (manufactured by Shin-Etsu Chemical Co., Ltd.) PA: Phthalic anhydride (Tokyo Chemical Industry Co., Ltd.) UN-333: Urethane acrylate (manufactured by Negami Chemical Industries, Ltd.) UN-6306: Urethane acrylate (manufactured by Negami Chemical Industries, Ltd.) UN-2601: Urethane acrylate (manufactured by Negami Chemical Industries, Ltd.) DMAC: N,N-dimethylacetamide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) CHN: Cyclohexanone (manufactured by Toyo Gosei Co., Ltd.) MEK: Methyl ethyl ketone (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) Tinuvin 477: Hydroxyphenyltriazine UV absorber (manufactured by BASF) Omnirad819: Photopolymerization initiator phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (manufactured by IGM Resins BV) TG-129: A crosslinking agent having an alkoxymethyl group represented by the following formula (21) (manufactured by Sanwa Chemical Co., Ltd.)
[0100] [ka]
[0101] Synthesis Example 1: Synthesis of Resin P-1 A thermometer and a stirring rod with stirring blades were set in a 500 mL four-neck flask. Next, DMAC (110 g) and MDI (24.78 g (99.00 mmol)) were added under a dry nitrogen gas flow and stirred at 40 ° C. PTMG (50.00 g (50.00 mmol)) was added while stirring and washed in with DMAC (20 g). After stirring at 80 ° C for 3 hours, 1,4-butanediol ((4.506 g (50.00 mmol)) was added and washed in with DMAC (20 g). After stirring at 80 ° C for 5 hours, a solution of resin P-1 was obtained. The solid content was 41 mass %.
[0102] Synthesis Example 2: Synthesis of Resin P-2 A thermometer and a stirring rod with stirring blades were set in a 500 mL four-neck flask. Next, DMAC (110 g) and MDI (24.78 g (99.00 mmol)) were added under a dry nitrogen gas flow and stirred at 40 ° C. PTMG (60.00 g (40.00 mmol)) was added while stirring and washed in with DMAC (20 g). After stirring at 80 ° C for 3 hours, 1,4-butanediol ((3.605 g (60.00 mmol)) was added and washed in with DMAC (20 g). After stirring at 80 ° C for 5 hours, a solution of resin P-2 was obtained. The solid content was 42 mass %.
[0103] Synthesis Example 3: Synthesis of Resin P-3 A thermometer and a stirring rod with stirring blades were set in a 500 mL four-neck flask. Next, DMAC (110 g) and MDI (24.78 g (99.00 mmol)) were added under a dry nitrogen gas flow and stirred at 40 ° C. PTMG (75.00 g (75.00 mmol)) was added while stirring and washed in with DMAC (20 g). After stirring at 80 ° C for 3 hours, 1,4-butanediol ((2.253 g (25.00 mmol)) was added and washed in with DMAC (20 g). After stirring at 80 ° C for 5 hours, a solution of resin P-3 was obtained. The solid content was 45 mass %.
[0104] Synthesis Example 4: Synthesis of Resin P-4 A thermometer and a stirring rod with stirring blades were set in a 500 mL four-neck flask. Next, under a dry nitrogen stream, CHN (110 g), APPS1 (63.64 g (74.00 mmol)), APPS2 (8.000 g (5.000 mmol)), and BAHF (7.325 g (20.00 mmol)) were added and stirred at 50 ° C. While stirring, BTDA (16.11 g (50.00 mmol)) and BPDA (14.71 g (50.00 mmol)) were added and washed in with CHN (40 g). After stirring at 95 ° C for 1 hour and further stirring at 150 ° C for 5 hours, a solution of resin P-4 was obtained. The solid content was 52 mass%.
[0105] Synthesis Example 5: Synthesis of Resin P-5 A thermometer and a stirring rod with stirring blades were set in a 500 mL four-neck flask. Next, under a dry nitrogen stream, CHN (110 g), APPS1 (68.80 g (80.00 mmol)), APPS2 (8.000 g (5.000 mmol)), and BAHF (5.494 g (15.00 mmol)) were added and stirred at 50 ° C. PA (2.962 g (20.00 mmol)) was added while stirring, washed with CHN (20 g), and stirred at 60 ° C. for 15 minutes. Next, PMDA (19.63 g (90.00 mmol)) was added while stirring, and washed with CHN (20 g). After stirring at 60 ° C. for 1 hour and further stirring at 145 ° C. for 4 hours, a solution of resin P-5 was obtained. The solid content was 49 mass%.
[0106] Preparation Example 1: 18 parts by mass of Tinuvin 477 (based on 100 parts by mass of the solid content of the solution of Resin P-1) and 5 parts by mass of TG-129 (same) were added and stirred to the solution of Resin P-1 obtained in Synthesis Example 1. After stirring, the mixture was filtered using a high-density polyethylene filter with a pore size of 0.2 μm to prepare a varnish.
[0107] Preparation Examples 2-11: Using the resins and additives shown in Table 1, varnishes were prepared in the same manner as in Preparation Example 1.
[0108] Preparation 12: 20 parts by mass of Tinuvin 477 (resin is taken as 100 parts by mass), 3 parts by mass of Omnirad 127 (same as above), and 20 parts by mass of MEK (same as above) were added to 20 g of UN-333 and stirred. After stirring, the mixture was filtered using a high-density polyethylene filter with a pore size of 0.2 μm to prepare a varnish.
[0109] Preparation 13: A varnish was prepared in the same manner as in Preparation Example 12, except that UN-6306 was used in place of UN-333.
[0110] Preparation 14: A varnish was prepared in the same manner as in Preparation Example 12, except that UN-2601 was used in place of UN-333.
[0111] The first laminate and the second laminate were produced by the above-mentioned method using the varnishes obtained in Preparation Examples 1 to 14 (Examples 1 to 7, Comparative Examples 1 to 7). The evaluation results of the produced laminates are summarized in Table 1.
[0112] [Table 1]
[0113] From the results of Table 1, in the laminates of Examples 1 to 7, the semiconductor elements could be transferred with excellent positional accuracy. On the other hand, in Comparative Examples 1 and 3 to 7, the number of semiconductor elements that could be transferred normally was small, or the positional accuracy was poor. This is considered to be because the loss tangent α of the resin film was too large, so that the energy generated by the laser irradiation was consumed in large amounts by the thermal motion of the resin film, and the energy for transferring the semiconductor elements was not sufficiently transmitted. In Comparative Example 2, the loss tangent β of the resin film was too small, so that the adhesiveness was reduced, and the semiconductor elements could not be transferred onto the resin film, resulting in the failure to produce the second laminate. [Explanation of symbols]
[0114] 11 First substrate having laser transparency 12 Resin film 14 Semiconductor elements 15 Support 16 Temporary adhesive 17 Crystal growth substrate 18 Semiconductor Substrate 21 Second board 31 Laser Light 41 Crimping device 51 Photomask 110 First laminate 120 Second laminate 130 Semiconductor element temporary adhesive substrate 140 Substrate with semiconductor element
Claims
1. A laminate in which a first substrate having laser transparency and a resin film are laminated in this order, 25°C, 1.0 x 10 6 The resin film has a loss tangent of 0.01 to 0.15 as measured by dynamic viscoelasticity measurement at 100 Hz.
2. Further, the semiconductor device includes The laminate according to claim 1 , wherein the first substrate, the resin film, and the semiconductor element are laminated in this order.
3. 25°C, 1.0 x 10 6 3. The laminate according to claim 1, wherein the resin film has a storage modulus of 300 MPa or more as measured by dynamic viscoelasticity measurement at 100 Hz.
4. 25°C, 1.0 x 10 -2 3. The laminate according to claim 1, wherein the resin film has a loss tangent of 0.4 or more as measured by dynamic viscoelasticity measurement at 100 Hz.
5. 3. The laminate according to claim 1, wherein the resin film has a thickness of 0.7 μm or more and 30 μm or less.
6. The laminate according to claim 1 , wherein the resin film contains a light absorbing agent.
7. 3. The laminate according to claim 1, wherein the resin film has an absorbance of 0.4 or more and 5.0 or less in terms of a film thickness of 1.0 μm at any wavelength of 200 to 1100 nm.
8. A method for manufacturing a semiconductor device, comprising the steps of: (a) a step of disposing a second substrate in opposition to a surface of the laminate according to claim 2 on which the semiconductor element is laminated. (b) A step of irradiating the laminate with laser light from the side of the first substrate to transfer the semiconductor element to the second substrate.
9. The method for manufacturing a semiconductor device according to claim 8 , wherein an adhesive layer is laminated on a surface of the second substrate onto which the semiconductor element is transferred.
10. 10. The method for manufacturing a semiconductor device according to claim 8, wherein the wavelength of the laser light is 355 nm.
Citation Information
Patent Citations
Manufacturing method of display device and source substrate structure
JP2020188037A
Workpiece handling sheet and device manufacturing method
WO2022153745A1
Laminate, resin composition, and method for manufacturing semiconductor device
WO2022210155A1
Cited By
Composition, laminate, and method for manufacturing semiconductor device
WO2026105609A1