Polyimide resin composition and cured product thereof

A resin composition for printed wiring boards, combining polyimide resin with specific copolymers and thermosetting compounds, addresses adhesion and heat resistance issues, offering improved performance in high-frequency applications.

JP2024139792AInactive Publication Date: 2024-10-10NIPPON KAYAKU CO LTD

Patent Information

Application Number
JP2023050695
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing resin compositions for printed wiring boards have insufficient substrate adhesion and heat resistance, particularly in high-frequency applications, leading to issues such as swelling during multiple reflow processes.

Method used

A resin composition comprising a polyimide resin copolymerized with specific diamino compounds and tetrabasic acid dianhydride, combined with a copolymer resin containing structural units from aromatic vinyl compounds and oxazoline groups, along with optional thermosetting compounds and curing accelerators, to enhance adhesion and heat resistance.

Benefits of technology

The composition provides improved adhesiveness and heat resistance, suitable for high-frequency applications, with reduced swelling and enhanced dielectric properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139792000001
    Figure 2024139792000001
  • Figure 2024139792000002
    Figure 2024139792000002
  • Figure 2024139792000003
    Figure 2024139792000003
Patent Text Reader

Abstract

To provide a resin composition with superior substrate adhesion and heat resistance.SOLUTION: This invention has been completed based on the findings that: a resin composition comprising (A) a polyimide resin that is a copolymer of (a-1) at least one diamino compound with two amino groups in one molecule and (a-2) a tetrabasic acid dianhydride and (B) a copolymer resin comprising an aromatic vinyl compound-derived structural unit and an oxazoline group-derived structural unit can solve the foregoing problem.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition containing a polyimide resin and a cured product thereof. [Background technology]

[0002] Printed wiring boards are essential components for mobile communication devices such as smartphones and tablets, communication base station equipment, computers, car navigation systems, etc. Various resin materials with excellent properties such as adhesion to metal foil, heat resistance, and flexibility are used for printed wiring boards. Furthermore, in recent years, there has been progress in the development of printed wiring boards for next-generation high-speed, large-capacity radio frequency wireless applications, and in addition to the above-mentioned characteristics, the resin material is required to have low transmission loss, i.e., low dielectric constant and low dielectric dissipation factor.

[0003] Furthermore, adhesive films used as adhesives or coverlay films in multilayer printed wiring boards are required to exhibit excellent dielectric properties, as well as to have excellent adhesive strength to copper foil and substrates (polyimide film and PPE prepreg), and to have heat resistance that can withstand solder mounting.

[0004] Patent Document 1 describes that a cured product of a composition containing a polyimide resin having a dimer diamine skeleton and a crosslinking agent has excellent dielectric properties (low dielectric tangent). However, the composition described in the document has insufficient adhesion to a substrate. Patent Document 2 describes that a cured product of a resin composition containing a polyimide resin, a modified elastomer, and an epoxy resin has excellent dielectric properties, adhesion to a substrate, and solder heat resistance. However, the cured product of the resin composition described in the same document has insufficient heat resistance and blister occurs when the number of reflows is increased, so that a product with higher heat resistance is required. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-168369 A [Patent Document 2] WO2020 / 071154 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a resin composition which can be suitably used for printed wiring boards, and which provides a cured product having excellent substrate adhesion and heat resistance. [Means for solving the problem]

[0007] As a result of extensive investigations, the present inventors have found that a resin composition containing a polyimide resin and a copolymer having a specific structure can solve the above problems, and have completed the present invention. That is, the present invention relates to the following. [1] A resin composition comprising: a polyimide resin (A) which is a copolymer of one or more diamino compounds (a-1) having two amino groups in one molecule and a tetrabasic acid dianhydride (a-2); and a copolymer resin (B) which contains a structural unit derived from an aromatic vinyl compound and a structural unit derived from an oxazoline group, The structural unit derived from an aromatic vinyl compound of the component (B) is represented by the following formula (b-1):

[0008] [ka]

[0009] (In formula (b-1), R1 and R2 each independently represent a hydrogen atom, a methyl group, or an ethyl group, and x each independently represents an integer of 1 to 5.) In addition, the structural unit derived from an oxazoline group is represented by the following formula (b-2):

[0010] [ka]

[0011] (In formula (b-2), each R3 independently represents a hydrogen atom, a methyl group, or an ethyl group.) A resin composition comprising a structural unit represented by the formula: [2] The resin composition according to [1], wherein the diamino compound (a-1) includes an aliphatic diamino compound (a-3) having 6 to 36 carbon atoms. [3] At least one of the components (a-1) is represented by the following formula (1) or (2):

[0012] [ka]

[0013] (In formula (1), X represents C(CH3)2, C(CF3)2, SO2, CH2, CH(CH3), or CH(CF3).)

[0014] [ka]

[0015] or 9,9-bis(4-aminophenyl)fluorene. [4] The resin composition according to any one of [1] to [3], further comprising a thermosetting compound (C). [5] The thermosetting compound (C) is represented by the following formula (3) to (5):

[0016] [ka]

[0017] (In formula (3), R4 represents an alkyl group having 1 to 5 carbon atoms or a phenyl group, and when there are a plurality of R4's, they may be the same or different. Each k independently represents an integer of 0 to 3. 1 is the average number of repetitions and is a real number between 1 and 10.)

[0018] [ka]

[0019] (In formula (4), R5 represents an alkyl group having 1 to 5 carbon atoms or a phenyl group, and when there are a plurality of R5, they may be the same or different. Each 1 independently represents an integer of 0 to 3. n 2 is the average number of repetitions and is a real number between 1 and 10.)

[0020] [ka]

[0021] (In formula (5), R6 and R7 each independently represent a hydrogen atom, a methyl group, or an ethyl group.) The resin composition according to [4], comprising one or more compounds selected from the group consisting of compounds represented by the following formula: [6] The resin composition according to any one of [1] to [5], further comprising a curing accelerator (D). [7] A resin-coated copper foil having the resin composition according to any one of [1] to [6]. [8] A copper clad laminate obtained by curing a resin layer made of a resin composition contained in the resin-coated copper foil according to [7]. Effect of the Invention

[0022] By using the resin composition of the present invention, it is possible to provide a printed wiring board or the like having excellent adhesiveness and heat resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The resin composition of the present invention comprises The resin composition includes a polyimide resin (A) which is a copolymer of one or more diamino compounds (a-1) having two amino groups in one molecule and a tetrabasic acid dianhydride (a-2), and a copolymer resin (B) which contains a structural unit derived from an aromatic vinyl compound and a structural unit derived from an oxazoline group, and the structural unit derived from the aromatic vinyl compound of the component (B) is represented by the following formula (b-1):

[0024] [ka]

[0025] (In formula (b-1), R1 and R2 each independently represent a hydrogen atom, a methyl group, or an ethyl group, and x each independently represents an integer of 1 to 5.) In addition, the structural unit derived from an oxazoline group is represented by the following formula (b-2):

[0026] [ka]

[0027] (In formula (b-2), each R3 independently represents a hydrogen atom, a methyl group, or an ethyl group.) The resin composition contains a copolymer resin having a structural unit represented by the following formula:

[0028] The component (A) used in the resin composition of the present invention is not limited to either an aliphatic soluble polyimide resin or an aromatic soluble polyimide resin, as long as it is a soluble polyimide resin obtained by imidization reaction between one or more diamino compounds (a-1) having two amino groups in one molecule and a tetrabasic acid dianhydride component (a-2). In addition, soluble polyimide resins obtained by modifying the terminals or side chains of these soluble polyimide resins can also be used. The soluble polyimide resin may be a commercially available product or a synthesized product, and may be used alone or in combination of multiple types. In the present invention, the soluble polyimide is a polyimide resin that is soluble in an organic solvent, and soluble in this specification means that it is soluble in an amount of 1.0 mass % or more at 23° C. The organic solvents mentioned here are ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone, ether-based solvents such as 1,4-dioxane, tetrahydrofuran, and diglyme, glycol ether-based solvents such as methyl cellosolve, ethyl cellosolve, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, and diethylene glycol methyl ethyl ether, as well as benzyl alcohol, N-methylpyrrolidone, γ-butyrolactone, ethyl acetate, N,N-dimethylformamide, and anisole.

[0029] Specific examples of the one or more diamino compounds (a-1) having two amino groups in one molecule that can be used in the synthesis of the component (A) include 1,3-bis(3-aminophenoxy)benzene, 9,9-bis(4-aminophenyl)fluorene, m-phenylenediamine, p-phenylenediamine, m-tolylenediamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylthioether, 3,3'-dimethyl-4 ... phenylthioether, 3,3'-diethoxy-4,4'-diaminodiphenylthioether, 3,3'-diaminodiphenylthioether, 4,4'-diaminobenzophenone, 3,3'-dimethyl-4,4'-diaminobenzophenone, 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-dimethoxy-4,4'-diaminodiphenylthioether, 2,2'-bis(3-aminophenyl)propane, 2,2'-bis(4-aminophenyl)propane, 4,4'-diaminodiphenylthioether, Aminodiphenyl sulfoxide, 3,3'-diaminodiphenyl sulfone sulfone, 4,4'-diaminodiphenyl sulfone sulfone, benzidine, 3,3'-dimethylbenzidine, 3,3'-dimethoxybenzidine, 3,3'-diaminobiphenyl, p-xylylenediamine, m-xylylenediamine, o-xylylenediamine, 2,2'-bis(3-aminophenoxyphenyl)propane, 2,2'-bis(4-aminophenoxyphenyl)propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-biphenyl Bis(4-aminophenoxyphenyl)benzene, 1,3'-bis(3-aminophenoxyphenyl)propane, bis(4-amino-3-methylphenyl)methane, bis(4-amino-3,5-dimethylphenyl)methane, bis(4-amino-3-ethylphenyl)methane, bis(4-amino-3,5-diethylphenyl)methane, bis(4-amino-3-propylphenyl)methane and bis(4-amino-3,5-dipropylphenyl)methane, hexamethylenediamine, 1,3-bis(aminomethyl)cyclohexane, 3,3'-diamino-4,Examples of the dihydroxydiphenyl sulfone include 4'-dihydroxydiphenyl sulfone, 3,3'-diamino-4,4'-dihydroxydiphenyl ether, 3,3'-diamino-4,4'-dihydroxybiphenyl, 3,3'-diamino-4,4'-dihydroxybenzophenone, 2,2-bis(3-amino-4-hydroxyphenyl)methane, 2,2-bis(3-amino-4-hydroxyphenyl)ethane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 1,3-hexafluoro-2,2-bis(3-amino-4-hydroxyphenyl)propane, and 9,9'-bis(3-amino-4-hydroxyphenyl)fluorene, and diaminopolysiloxanes having 6 to 36 carbon atoms.

[0030] At least one of the diamino compounds (a-1) having two amino groups in one molecule is represented by the following formula (1) or (2):

[0031] [ka]

[0032] (In formula (1), X represents C(CH3)2, C(CF3)2, SO2, CH2, CH(CH3), or CH(CF3).)

[0033] [ka]

[0034] or 9,9-bis(4-aminophenyl)fluorene. In particular, from the viewpoint of adhesion, it is preferable to use 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-bis(3-aminophenoxy)benzene, or 9,9-bis(4-aminophenyl)fluorene. These diamine components may be used alone or in combination of two or more.

[0035] Specific examples of tetrabasic acid dianhydride components that can be used in the synthesis of component (A) include pyromellitic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenylsulfone tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 3,3',4,4'-biphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-dimethyldiphenylsilane tetracarboxylic dianhydride, 3,3',4,4'-tetraphenylsilane tetracarboxylic dianhydride, 1,2,3,4-furan tetracarboxylic dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride, 4,4'-biphenyl ether tetracarboxylic ... Examples of the dianhydride include bis(3,4-dicarboxyphenoxy)diphenylsulfone dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylpropane dianhydride, 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, bis(phthalic acid)phenylphosphine oxide dianhydride, p-phenylene-bis(triphenylphthalic acid) dianhydride, m-phenylene-bis(triphenylphthalic acid) dianhydride, bis(triphenylphthalic acid)-4,4'-diphenylether dianhydride, bis(triphenylphthalic acid)-4,4'-diphenylmethane dianhydride, and 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic dianhydride. Among these, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, or 3,3',4,4'-diphenylethertetracarboxylic dianhydride is preferred from the viewpoints of solvent solubility, adhesion to a substrate, and photosensitivity. These may be used alone or in combination of two or more.

[0036] The component (A) contained in the resin composition of the present invention preferably contains a soluble polyimide resin having an aliphatic chain having 6 to 36 carbon atoms introduced into the skeleton. When synthesizing the component (A), it is preferable to use an aliphatic diamino compound (a-3) having 6 to 36 carbon atoms. For example, by using 1,3-bisaminomethylcyclohexane, norbornanediamine, isophoronediamine, dimerdiamine, 2-methyl-1,5-diaminopentane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, 1,4-bis(aminomethyl)cyclohexane, 4,4'-methylenebiscyclohexylamine, Diamine H20 (manufactured by Okamura Oil Co., Ltd.), dimerdiamine, trimertriamine, or the like as a diamine component, it is possible to introduce an aliphatic chain derived from these diamine components into the skeleton of the soluble polyimide resin. In particular, from the viewpoint of improving the dielectric properties and the adhesion to the substrate, it is preferable that the component (A) contains a soluble polyimide resin having an aliphatic chain derived from Diamine H20 or dimer diamine introduced into the skeleton.

[0037] Dimer diamine is a compound in which two carboxyl groups of a dimer acid, which is a dimer of an unsaturated fatty acid such as oleic acid, are replaced with primary amino groups (see JP-A-9-12712, etc.). Specific examples of commercially available dimer diamines include PRIAMINE 1074 and PRIAMINE 1075 (both manufactured by Croda Japan Co., Ltd.), and Versamine 551 (manufactured by Cognis Japan Co., Ltd.). These may be used alone or in combination of two or more. Below, non-limiting general formulas of dimer diamines are shown (in each formula, m+n=6 to 17 is preferable, p+q=8 to 19 is preferable, and the dashed line represents a carbon-carbon single bond or a carbon-carbon double bond).

[0038] [ka]

[0039] The content of component (A) in the resin composition of the present invention is preferably 50 to 95% by mass based on the total of components (A) and (B). By setting the content of component (A) within this range, the dielectric properties (low dielectric properties) and substrate adhesion of the cured product of the resin composition are improved. The content of the component (A) is more preferably 70 to 95 mass % based on the total of the components (A) and (B).

[0040] The weight average molecular weight of component (A) is preferably 30,000 or more. By setting the weight average molecular weight within the above range, solder heat resistance is improved. From the above viewpoint, the number average molecular weight is more preferably 30,000 to 120,000. The number average molecular weight in the present invention is a value calculated in terms of polystyrene based on the measurement results of gel permeation chromatography (GPC).

[0041] The component (A) can be synthesized by a known method. For example, after dissolving the diamine and tetrabasic acid dianhydride used in the synthesis in a solvent, the mixture is heated and stirred at 10 to 140°C under an inert atmosphere such as nitrogen, whereby a copolymerization reaction between the diamine and the tetrabasic acid dianhydride occurs, and a polyamic acid resin solution is obtained. In addition, a dehydrating agent or catalyst is added to the polyamic acid resin solution obtained above as necessary, and the mixture is heated and stirred at 100 to 300°C, whereby an imidization reaction (a ring-closing reaction accompanied by dehydration) occurs, and the component (A) is obtained. As the dehydrating agent, toluene, xylene, etc. can be used, and as the catalyst, a tertiary amine and a dehydration catalyst can be used. As the tertiary amine, a heterocyclic tertiary amine is preferable, and examples thereof include pyridine, picoline, quinoline, and isoquinoline. As the dehydration catalyst, examples thereof include acetic anhydride, propionic anhydride, n-butyric anhydride, benzoic anhydride, and trifluoroacetic anhydride. The reaction time in synthesizing the polyamic acid resin and the polyimide resin is greatly affected by the reaction temperature, but it is preferable to carry out the reaction until the increase in viscosity accompanying the progress of the reaction reaches equilibrium and the maximum molecular weight is obtained, which is usually several minutes to 20 hours. The above example is a method for synthesizing a polyimide resin via a polyamic acid. Alternatively, the diamine and tetracarboxylic anhydride used in the synthesis may be dissolved in a solvent, and then a dehydrating agent and / or catalyst may be added, if necessary, and the mixture may be heated and stirred at 100 to 300° C. to carry out the copolymerization reaction and the imidization reaction in one go, thereby obtaining component (A).

[0042] Solvents that can be used in the synthesis of component (A) include methyl ethyl ketone, methyl propyl ketone, methyl isopropyl ketone, methyl butyl ketone, methyl isobutyl ketone, methyl n-hexyl ketone, diethyl ketone, diisopropyl ketone, diisobutyl ketone, cyclopentanone, cyclohexanone, methylcyclohexanone, acetylacetone, γ-butyrolactone, diacetone alcohol, cyclohexen-1-one, dipropyl ether, diisopropyl ether, dibutyl ether, tetrahydrofuran, tetrahydropyran, ethyl isoamyl ether, ethyl-t-butyl ether, ethyl benzyl ether, cresyl methyl ether, anisole, phenetole, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, Pyridine, butyl acetate, isobutyl acetate, amyl acetate, isoamyl acetate, 2-ethylhexyl acetate, cyclohexyl acetate, methylcyclohexyl acetate, benzyl acetate, methyl acetoacetate, ethyl acetoacetate, methyl propionate, ethyl propionate, butyl propionate, benzyl propionate, methyl butyrate, ethyl butyrate, isopropyl butyrate, butyl butyrate, isoamyl butyrate, methyl lactate, ethyl lactate, butyl lactate, ethyl isovalerate, isoamyl isovalerate, diethyl oxalate, dibutyl oxalate, methyl benzoate, ethyl benzoate, propyl benzoate, methyl salicylate, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, etc. may be mentioned, but are not limited thereto. These may be used alone or in a mixture of two or more. The amount of the solvent used should be appropriately adjusted depending on the viscosity and use of the resulting resin, but the solid content is preferably 60 to 10% by mass, more preferably 50 to 20% by mass.

[0043] In the synthesis of component (A), it is preferable to use a catalyst to promote the dehydration reaction, and the amount of the catalyst used is preferably 1 to 30% of twice the number of moles of component (A) (the number of moles of water generated by dehydration condensation), more preferably 5 to 15%. Specific examples of catalysts that can be used include known general basic catalysts such as triethylamine and pyridine. Among them, triethylamine is preferable because it has a low boiling point and is less likely to remain.

[0044] The copolymer resin (B) containing a structural unit derived from an aromatic vinyl compound and a structural unit derived from an oxazoline group in the composition of the present invention is a copolymer resin in which the structural unit derived from the aromatic vinyl compound is a structural unit represented by the above formula (b-1) and the structural unit derived from the oxazoline group is a structural unit represented by the above formula (b-2).

[0045] The component (B) can be obtained by polymerizing an α,β-unsaturated aromatic hydrocarbon compound such as styrene, α-methylstyrene, or α-ethylstyrene with an addition-polymerizable oxazoline such as 2-vinyl-2-oxazoline, 2-(propyl-1-en-2-yl)-2-oxazoline, 2-(butyl-1-en-2-yl)-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, or 2-ethyl-2-oxazoline. The polymerization method for the oxazoline group-containing polymer is not particularly limited, and various known polymerization methods can be used.

[0046] The weight average molecular weight of the component (B) is preferably from 10,000 to 250,000, more preferably from 30,000 to 250,000, and even more preferably from 50,000 to 230,000, from the viewpoints of heat resistance and flex resistance.

[0047] The weight average molecular weight of the component (B) can be measured under the following measurement conditions. <Gel Permeation Chromatography (GPC)> The weight average molecular weight (Mw) and number average molecular weight (Mn) are calculated in terms of polystyrene using a polystyrene standard solution. Equipment: LC-20AD, DGU-20A3R, SIL-20AHT, CTO-20A, CBM-20A, RID-20A (all manufactured by Shimadzu Corporation) Column: Shodex KF-601 x 1 + KF-602 x 1 + KF-602.5 x 1 + KF-603 x 1 Eluent: Tetrahydrofuran Flow rate: 1.5ml / min Column temperature: 40℃ Detection: RI (Differential Refractive Index Detector)

[0048] As the component (B), commercially available products may be used, and examples of commercially available products include Epocross RPS-1005 manufactured by Nippon Shokubai.

[0049] The content of component (B) in the resin composition of the present invention is preferably 1.0 to 50 mass% based on the total of components (A) and (B). By setting the content of component (A) within the above range, the substrate adhesion and heat resistance of the cured product of the resin composition are improved. The content of the component (B) is more preferably 5.0 to 30 mass % based on the total of the components (A) and (B).

[0050] The resin composition may further contain a thermosetting compound (C) (hereinafter, also referred to as component (C)). Examples of the component (C) include a maleimide compound and a compound having an ethylenically unsaturated group.

[0051] The maleimide compound is not particularly limited as long as it has one or more maleimide groups in one molecule. Specific examples thereof include, for example, N-phenylmaleimide, N-hydroxyphenylmaleimide, bis(4-maleimidophenyl)methane, 4,4-diphenylmethane bismaleimide, bis(3,5-dimethyl-4-maleimidophenyl)methane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, bis(3,5-diethyl-4-maleimidophenyl)methane, phenylmethane maleimide, o-phenylene bismaleimide, m-phenylene bismaleimide, p-phenylene bismaleimide, p-phenylene biscitraconimide, 2,2-bis(4-(4-maleimidophenoxy)-phenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 1 ,6-bismaleimide-(2,2,4-trimethyl)hexane, 4,4-diphenylether bismaleimide, 4,4-diphenylsulfone bismaleimide, 1,3-bis(3-maleimidophenoxy)benzene, 1,3-bis(4-maleimidophenoxy)benzene, polyphenylmethane maleimide, novolak type maleimide compounds, biphenyl aralkyl type maleimide compounds, 2,2-bis(4-(4-maleimidophenoxy)phenyl)propane, 1,2-bis(maleimido)ethane, 1,4-bis(maleimido)butane, 1,6-bis(maleimido)hexane, N,N'-1,3-phenylene dimaleimide, N,N'-1,4-phenylene dimaleimide, N-phenylmaleimide, and maleimide compounds represented by formulas (1) to (5). The maleimide compound (C) can also be contained in the resin composition according to this embodiment in the form of a prepolymer obtained by polymerizing a maleimide compound, or a prepolymer obtained by polymerizing a maleimide compound with another compound such as an amine compound.Commercially available products can also be used. Specific examples include MIR-3000 (manufactured by Nippon Kayaku Co., Ltd.), MIR-5000 (manufactured by Nippon Kayaku Co., Ltd.), BMI-70 (manufactured by K.I. Kasei Co., Ltd.), BMI-80 (manufactured by K.I. Kasei Co., Ltd.), BMI-2300 (manufactured by Yamato Kasei Co., Ltd.), BMI-3000 (manufactured by Designer Molecules Inc.), BMI-5000 (manufactured by Designer Molecules Inc.), BMI-6000 (manufactured by Designer Molecules Inc.), BMI-689 (manufactured by Designer Molecules Inc.), BMI-1700 (manufactured by Designer Molecules Inc.), BMI-1500 (manufactured by Designer Molecules Inc.), and the like. Inc.), BMI-TMH (Yamato Chemical Industries, Ltd.), MAHD (Evonik), BMI-1000P (K.I. Chemical Industries, Ltd.), BMI-650P (K.I. Chemical Industries, Ltd.), BMI-250P (K.I. Chemical Industries, Ltd.), CUA-4 (K.I. Chemical Industries, Ltd.), etc. are examples. Maleimide resins having aromatic rings such as benzene rings, biphenyl rings, and naphthalene rings are preferred because the cured product of the resin composition has excellent properties such as mechanical strength and flame retardancy. The component (C) may be used alone or in combination of two or more types.

[0052] The compound having an ethylenically unsaturated group is not particularly limited as long as it has an ethylenically unsaturated group in one molecule.Specific examples of the compound having an ethylenically unsaturated group include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, lauryl (meth)acrylate, polyethylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate monomethyl ether, phenylethyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, nonanediol di(meth)acrylate, glycol di(meth)acrylate, diethylene di(meth)acrylate, polyethylene glycol di(meth)acrylate, tris(meth)acryloyloxyethyl isocyanurate, polypropylene glycol di(meth)acrylate , adipic acid epoxy di(meth)acrylate, bisphenol ethylene oxide di(meth)acrylate, hydrogenated bisphenol ethylene oxide (meth)acrylate, bisphenol di(meth)acrylate, ε-caprolactone modified hydroxypivalic acid neopen glycol di(meth)acrylate, ε-caprolactone modified dipentaerythritol hexa(meth)acrylate, ε-caprolactone modified dipentaerythritol poly(meth)acrylate, dipentaerythritol poly(meth)acrylate, trimethylolpropane tri(meth)acrylate, triethylolpropane tri(meth)acrylate, and ethylene oxide adducts thereof; pentaerythritol tri(meth)acrylate, and ethylene oxide adducts thereof; pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and ethylene oxide adducts thereof.

[0053] Other specific examples of the compound having an ethylenically unsaturated group include urethane (meth)acrylates having both a (meth)acryloyl group and a urethane bond in the same molecule; polyester (meth)acrylates having both a (meth)acryloyl group and an ester bond in the same molecule; epoxy (meth)acrylates derived from epoxy resins and having both a (meth)acryloyl group; and reactive oligomers in which these bonds are used in combination.

[0054] Examples of urethane (meth)acrylates include reaction products of hydroxyl group-containing (meth)acrylate with polyisocyanate and other alcohols used as necessary. Examples of urethane (meth)acrylates include hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate; glycerin (meth)acrylates such as glycerin mono(meth)acrylate and glycerin di(meth)acrylate; pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and the like. Examples of the polyisocyanate include urethane (meth)acrylates obtained by reacting sugar alcohol (meth)acrylates such as methacrylate with polyisocyanates such as toluene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, xylene diisocyanate, hydrogenated xylene diisocyanate, dicyclohexanemethylene diisocyanate, and their isocyanurates and biuret reaction products.

[0055] Examples of polyester (meth)acrylates include monofunctional (poly)ester (meth)acrylates such as caprolactone-modified 2-hydroxyethyl (meth)acrylate, ethylene oxide and / or propylene oxide-modified phthalic acid (meth)acrylate, ethylene oxide-modified succinic acid (meth)acrylate, and caprolactone-modified tetrahydrofurfuryl (meth)acrylate; di(poly)ester (meth)acrylates such as hydroxypivalic acid ester neopentyl glycol di(meth)acrylate, caprolactone-modified hydroxypivalic acid ester neopentyl glycol di(meth)acrylate, and epichlorohydrin-modified phthalic acid di(meth)acrylate; and mono-, di-, or tri(meth)acrylates of triols obtained by adding 1 mole or more of a cyclic lactone compound such as ε-caprolactone, γ-butyrolactone, or δ-valerolactone to 1 mole of trimethylolpropane or glycerin.

[0056] Further examples include mono-, di-, tri-, or tetra(meth)acrylates of triols obtained by adding 1 mole or more of a cyclic lactone compound such as ε-caprolactone, γ-butyrolactone, δ-valerolactone, etc. to 1 mole of pentaerythritol, dimethylolpropane, trimethylolpropane, or tetramethylolpropane; mono- or poly(meth)acrylates of triols obtained by adding 1 mole or more of a cyclic lactone compound such as ε-caprolactone, γ-butyrolactone, δ-valerolactone, etc. to 1 mole of dipentaerythritol, and mono(meth)acrylates or poly(meth)acrylates of polyhydric alcohols such as triols, tetraols, pentaols, or hexaols.

[0057] Further examples include polyfunctional (poly)ester (meth)acrylates such as (meth)acrylates of polyester polyols which are reaction products of diol components such as (poly)ethylene glycol, (poly)propylene glycol, (poly)tetramethylene glycol, (poly)butylene glycol, 3-methyl-1,5-pentanediol, and hexanediol with polybasic acids such as maleic acid, fumaric acid, succinic acid, adipic acid, phthalic acid, isophthalic acid, hexahydrophthalic acid, tetrahydrophthalic acid, dimer acid, sebacic acid, azelaic acid, and 5-sodium sulfoisophthalic acid, and their anhydrides; and (meth)acrylates of cyclic lactone-modified polyester diols consisting of diol components, polybasic acids, their anhydrides, and ε-caprolactone, γ-butyrolactone, δ-valerolactone, etc.

[0058] Epoxy (meth)acrylates are carboxylate compounds of a compound having an epoxy group and (meth)acrylic acid. For example, phenol novolac type epoxy (meth)acrylate, cresol novolac type epoxy (meth)acrylate, trishydroxyphenylmethane type epoxy (meth)acrylate, dicyclopentadiene phenol type epoxy (meth)acrylate, bisphenol A type epoxy (meth)acrylate, bisphenol F type epoxy (meth)acrylate, biphenol type epoxy (meth)acrylate, bisphenol A novolac type epoxy (meth)acrylate, naphthalene skeleton-containing epoxy (meth)acrylate, glyoxal type epoxy (meth)acrylate, heterocyclic epoxy (meth)acrylate, and the like, and the epoxy acrylates modified with acid anhydrides thereof, and the like can be mentioned.

[0059] Specific examples of the compound having an ethylenically unsaturated group include vinyl ethers such as ethyl vinyl ether, propyl vinyl ether, hydroxyethyl vinyl ether, and ethylene glycol divinyl ether; styrenes such as styrene, methylstyrene, ethylstyrene, and divinylbenzene; and compounds having a vinyl group such as triallyl isocyanurate, trimethallyl isocyanurate, and bisallylnadimide.

[0060] As the compound having an ethylenically unsaturated group, commercially available products can be used, such as KAYARAD ZCA (registered trademark)-601H (trade name, manufactured by Nippon Kayaku Co., Ltd.), propylene glycol monomethyl ether acetate of TrisP-PA epoxy acrylate compound (manufactured by Nippon Kayaku Co., Ltd., KAYARAD (registered trademark) ZCR-6007H (trade name), KAYARAD (registered trademark) ZCR-6001H (trade name), KAYARAD (registered trademark) ZCR-6002H (trade name), and KAYARAD (registered trademark) ZCR-6006H (trade name), and STR-2000-60T (manufactured by Nippon Kayaku Co., Ltd.). These compounds having an ethylenically unsaturated group can be used alone or in an appropriate mixture of two or more types.

[0061] Among these, from the viewpoint of compatibility, the thermosetting compounds represented by the following formulas (3) to (5) are more preferable.

[0062] [ka]

[0063] In formula (3), R4 represents an alkyl group having 1 to 5 carbon atoms or a phenyl group, and when there are a plurality of R4, they may be the same or different from each other. Examples of the alkyl group having 1 to 5 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a t-butyl group, an n-pentyl group, and a neopentyl group. The alkyl group having 1 to 5 carbon atoms represented by R4 in formula (3) is preferably a methyl group or an ethyl group. In formula (3), k's each independently represent an integer of 0 to 3, preferably an integer of 0 to 2, and more preferably 0. n 1 is the average number of repetitions and represents a real number between 1 and 10. When k is greater than 3 or when R4 is an alkyl group having 6 or more carbon atoms, the electrical characteristics may be degraded due to molecular vibration when the alkyl group is exposed to high frequency waves.

[0064] [ka]

[0065] In formula (4), R5 represents an alkyl group having 1 to 5 carbon atoms or a phenyl group, and when there are a plurality of R5, they may be the same or different from each other. Examples of the alkyl group having 1 to 5 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a t-butyl group, an n-pentyl group, and a neopentyl group. In formula (4), each 1 independently represents an integer of 0 to 3. In formula (4), n 2 is the average number of repetitions and represents a real number between 1 and 10.

[0066] [ka]

[0067] In formula (6), R6 and R7 each represent a hydrogen atom, a methyl group, or an ethyl group.

[0068] The content of component (C) in the resin composition of the present invention is preferably 5.0 to 40% by mass based on the total of components (A) to (C). By setting the content of component (C) within this range, the heat resistance, substrate adhesion, low water absorption, and dielectric properties of the cured product of the resin composition are improved. The content of the component (C) is more preferably 10 to 25 mass % based on the total of the components (A) to (C).

[0069] The resin composition of the present invention may further contain a curing accelerator (D) (hereinafter, also referred to as component (D)). By containing component (D), the curing speed of the resin composition can be adjusted, and appropriate moldability is imparted to the resin composition. The component (D) contained in the resin composition of the present invention is not particularly limited as long as it is a compound that can promote the curing of the component (C) and the optional thermosetting resin (described later). The component (D) can be used alone or in combination of two or more kinds.

[0070] The component (D) that can be used in the resin composition of the present invention is not particularly limited, and examples thereof include thermal radical polymerization initiators, imidazole compounds, and tertiary amines such as triethylamine and tributylamine, etc. Among these, thermal radical polymerization initiators are preferred because they provide a good curing rate. The thermal radical polymerization initiator is not particularly limited as long as it is a compound that releases an active substance (radical) by heating that can polymerize the maleimide group contained in the (C) component and the radically polymerizable functional group contained in the thermosetting resin described below, and any known thermal radical polymerization initiator can be used. The thermal radical polymerization initiator can be used alone or in combination of two or more kinds.

[0071] The 10-hour half-life temperature of the thermal radical polymerization initiator is preferably 100° C. or higher, and from the viewpoint of manufacturability, more preferably 110° C. or higher. By setting the 10-hour half-life temperature of the thermal radical polymerization initiator within the above-mentioned preferred range, the solvent removal step during production can be performed at a high temperature.

[0072] Examples of the thermal radical polymerization initiator include ketone peroxides such as dicumyl peroxide, di(2-tert-butylperoxyisopropyl)benzene, 1,1,3,3-tetramethylbutyl hydroperoxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexyne-3, benzoyl peroxide, di-t-butyl peroxide, methyl ethyl ketone peroxide, and cyclohexanone peroxide; peroxyketals such as 1,1-di(t-butylperoxy)cyclohexane and 2,2-di(4,4-di(t-butylperoxy)cyclohexyl)propane; tert-butyl hydroperoxide, p-menthane hydroperoxide, diisopropylbenzene hydroperoxide, cumene hydroperoxide, and t-butyl hydroperoxide; di(2-t-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-di( Dialkyl peroxides such as t-butylperoxy)hexane, t-butylcumyl peroxide, di-t-hexyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, and di-t-butyl peroxide; diacyl peroxides such as dibenzoyl peroxide and di(4-methylbenzoyl) peroxide; peroxydica of di-n-propyl peroxydicarbonate and diisopropyl peroxydicarbonate. peroxyesters such as 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-hexylperoxybenzoate, t-butylperoxybenzoate, and t-butylperoxy-2-ethylhexanoate; and azo compounds such as 2,2'-azobisbutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile).In the composition of the present invention, organic peroxides are preferred in terms of obtaining a good curing rate, and peroxyesters, peroxyketals, dialkyl peroxides, and organic peroxides having a hydroperoxide skeleton are more preferred, and dicumyl peroxide, di(2-tert-butylperoxyisopropyl)benzene, 1,1,3,3-tetramethylbutyl hydroperoxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexyne-3, and tert-butyl hydroperoxide are even more preferred in terms of manufacturability.

[0073] The content of the (D) component in the resin composition of the present invention is preferably 0.05 to 10 parts by mass, and more preferably 0.05 to 8 parts by mass, per 100 parts by mass of the total of the (C) component and a thermosetting resin described later, in order to obtain a good curing rate.

[0074] The resin composition of the present invention may contain a thermosetting compound (E) (hereinafter also referred to as "component (E)") other than the component (C) in order to facilitate adjustment of the curing rate. Examples of the component (E) include epoxy resins, carbodiimide resins, benzoxazine compounds, etc. These resins or compounds can be used alone or in appropriate mixtures of two or more types depending on the physical properties and applications of the cured product of the resin composition.

[0075] The epoxy resin as component (E) is not particularly limited as long as it has one or more epoxy groups in one molecule, but because the cured product of the resin composition has excellent properties such as mechanical strength and flame retardancy, epoxy resins having an aromatic ring such as a benzene ring, a biphenyl ring, or a naphthalene ring are preferred, and specific examples thereof include jER828 (manufactured by Mitsubishi Chemical Corporation), NC-3000, and XD-1000 (all manufactured by Nippon Kayaku Co., Ltd.). When component (A) has an acid anhydride group, the epoxy resin can be reacted with this acid anhydride group, thereby increasing the crosslink density of the cured product, improving resistance to polar solvents, as well as improving adhesion to substrates and heat resistance. The curing temperature of the resin composition containing the epoxy resin is preferably 150 to 250° C. The curing time depends on the curing temperature, but is generally about several minutes to several hours.

[0076] In order to promote the curing reaction of the epoxy resin, a curing agent may be added to the resin composition of the present invention containing the epoxy resin, if necessary. Examples of the curing agent include imidazoles such as 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole, tertiary amines such as 2-(dimethylaminomethyl)phenol and 1,8-diaza-bicyclo(5,4,0)undecene-7, phosphines such as triphenylphosphine, and metal compounds such as tin octylate. The amount of the curing agent added to the resin composition of the present invention containing an epoxy resin is 0.1 to 10% by mass based on the epoxy resin.

[0077] The carbodiimide resin (compound) as component (E) is not particularly limited as long as it has one or more carbodiimide structures in one molecule. Specific examples of carbodiimide resins (compounds) include aliphatic biscarbodiimides such as tetramethylene-bis(t-butylcarbodiimide) and cyclohexane bis(methylene-t-butylcarbodiimide); aromatic biscarbodiimides such as phenylene-bis(xylylcarbodiimide); aliphatic polycarbodiimides such as polyhexamethylenecarbodiimide, polytrimethylhexamethylenecarbodiimide, polycyclohexylenecarbodiimide, poly(methylenebiscyclohexylenecarbodiimide), and poly(isophoronecarbodiimide); poly(phenylenecarbodiimide), Examples of polycarbodiimides include aromatic polycarbodiimides such as poly(naphthylenecarbodiimide), poly(tolylenecarbodiimide), poly(methyldiisopropylphenylenecarbodiimide), poly(triethylphenylenecarbodiimide), poly(diethylphenylenecarbodiimide), poly(triisopropylphenylenecarbodiimide), poly(diisopropylphenylenecarbodiimide), poly(xylylenecarbodiimide), poly(tetramethylxylylenecarbodiimide), poly(methylenediphenylenecarbodiimide), and poly[methylenebis(methylphenylene)carbodiimide]. These may be used in combination of two or more.

[0078] Commercially available carbodiimide resins (compounds) include, for example, "Carbodilite V-02B", "Carbodilite V-03", "Carbodilite V-04K", "Carbodilite V-07" and "Carbodilite V-09" manufactured by Nisshinbo Chemical Inc.; "Starbucksol P", "Starbucksol P400" and "Hi-Kasil 510" manufactured by Rhein Chemie.

[0079] The content of the carbodiimide resin (compound) in the resin composition of the present invention containing the carbodiimide resin (compound) is preferably 1.0 to 40 mass% based on the total of the components (A) to (C). By setting the content of the carbodiimide resin (compound) within the above range, the heat resistance, substrate adhesion, low water absorption, and dielectric properties of the cured product of the resin composition are improved. The content of the carbodiimide resin (compound) is more preferably 10 to 25% by mass based on the total of the components (A) to (C).

[0080] The benzoxazine resin (compound) as component (E) is not particularly limited as long as it has one or more benzoxazine structures in one molecule. Specific examples of the benzoxazine resin (compound) include bisphenol A type benzoxazine resin, bisphenol F type benzoxazine resin, diamine type benzoxazine resin, phenolphthalein type benzoxazine resin, dicyclopentadiene type benzoxazine resin, and bisphenolfluorene type benzoxazine resin. The benzoxazine resin may contain one or a mixture of two or more selected from the above, and is preferably bisphenol F type benzoxazine resin, diamine type benzoxazine resin, phenolphthalein type benzoxazine resin, and / or bisphenolfluorene type benzoxazine resin. These may be used in combination of two or more kinds, and include any one selected from these or a mixture of two or more kinds.

[0081] The content of the benzoxazine resin (compound) in the resin composition of the present invention containing the benzoxazine resin (compound) is preferably 1.0 to 40 mass% based on the total of the components (A) to (C). By setting the content of the benzoxazine resin (compound) within the above range, the heat resistance, substrate adhesion, low water absorption, and dielectric properties of the cured product of the resin composition are improved. The content of the benzoxazine resin (compound) is more preferably 10 to 25% by mass based on the total of the components (A) to (C).

[0082] The resin composition of the present invention can be made into a varnish-like composition (hereinafter simply referred to as varnish) by dissolving it in an organic solvent. Examples of the solvent that can be used include amide-based solvents such as γ-butyrolactones, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and N,N-dimethylimidazolidinone; sulfones such as tetramethylene sulfone; ether-based solvents such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether monoacetate, propylene glycol monobutyl ether, anisole, and tetrahydrofuran; ketone-based solvents such as methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone; and aromatic solvents such as toluene and xylene. The organic solvent is used in such a range that the solids concentration excluding the organic solvent in the varnish is preferably 10 to 80% by mass, more preferably 20 to 70% by mass.

[0083] The resin composition of the present invention may be used in combination with known additives as necessary.Specific examples of additives that can be used in combination include polybutadiene or its modified product, modified acrylonitrile copolymer, polyphenylene ether, polystyrene, polyethylene, polyimide, fluororesin, cyanate ester compounds, silicone gel, silicone oil, and inorganic fillers such as silica, alumina, calcium carbonate, quartz powder, aluminum powder, graphite, talc, clay, iron oxide, titanium oxide, aluminum nitride, asbestos, mica, and glass powder, surface treatment agents for fillers such as silane coupling agents, release agents, colorants such as carbon black, phthalocyanine blue, and phthalocyanine green, thixotropy-imparting agents such as aerosil, silicone-based and fluorine-based leveling agents and defoamers, hydroquinone, hydroquinone monomethyl ether, phenol-based polymerization inhibitors, stabilizers, antioxidants, photopolymerization initiators, photobase generators, and photoacid generators. The amount of these additives is preferably 1,000 parts by mass or less, more preferably 700 parts by mass or less, based on 100 parts by mass of the resin composition. As the additive, a silane coupling agent having an acrylic group or a methacrylic group is particularly preferred from the viewpoint of heat resistance.

[0084] The curing temperature and curing time of the resin composition of the present invention are preferably 120 to 250° C., and the curing time is generally from several tens of minutes to several hours.

[0085] A prepreg can be obtained by heating and melting the resin composition of the present invention to reduce the viscosity and impregnating it into reinforcing fibers such as glass fibers, carbon fibers, polyester fibers, polyamide fibers, alumina fibers, etc. Alternatively, a prepreg can be obtained by impregnating reinforcing fibers with the varnish and drying them by heating. The above prepreg is cut into a desired shape and laminated with copper foil or the like as necessary. The resin composition is then heated and cured while applying pressure to the laminate by press molding, autoclave molding, sheet winding molding or the like, to obtain a substrate (article) comprising the cured product of the present invention, such as an electrical and electronic laminate (printed wiring board) or a carbon fiber reinforced material.

[0086] Alternatively, a substrate having the cured product of the present invention can be obtained by coating the varnish on a copper foil, drying the solvent, laminating a polyimide film or LCP (liquid crystal polymer), hot pressing, and then heat curing. In some cases, a substrate having the cured product of the present invention can be obtained by coating the polyimide film or LCP side and laminating it with a copper foil. Alternatively, a substrate having the cured product of the present invention can be obtained by coating a copper foil with a varnish, drying the solvent, laminating a prepreg in which reinforcing fibers such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, or alumina fiber are impregnated with a resin, hot pressing, and then heat curing. A substrate provided with a thin film made of the above-mentioned resin composition can be used for a copper clad laminate (CCL), or a printed wiring board or multilayer wiring board having a circuit pattern on the copper foil of the CCL. EXAMPLES

[0087] The present invention will be described in more detail below with reference to examples and comparative examples. Note that the present invention is not limited to these examples. In the examples, "parts" means parts by mass, and "%" means % by mass. The GPC measurement conditions in the examples are as follows. Model: TOSOH ECOSEC Elite HLC-8420GPC Column: TSKgel Super AWM-H Eluent: NMP (N-methylpyrrolidone); 0.5 ml / min, 40°C Detector: UV (differential refractometer) Molecular weight standards: polystyrene

[0088] Synthesis Example 1 (Synthesis of Soluble Polyimide A-1) A 300 ml reactor equipped with a thermometer, a reflux condenser, a Dean-Stark apparatus, a raw material inlet, a nitrogen inlet and a stirrer was charged with 7.96 parts of BAPP (2,2-bis[4-(4-aminophenoxy)phenyl]propane, manufactured by Wakayama Seika Kogyo Co., Ltd., molecular weight 410.52 g / mol), 11.01 parts of PRIAMINE1075 (C36 dimer diamine, manufactured by Croda Japan Co., Ltd., molecular weight 534.38 g / mol), 13.03 parts of ODPA (oxydiphthalic anhydride, manufactured by Manac Co., Ltd., molecular weight 310.22 g / mol), 86.98 parts of anisole, 0.85 parts of triethylamine and 20.11 parts of toluene, and heated to 120 ° C. to dissolve the raw materials. The reaction was carried out at 135 ° C. for 4 hours while removing water generated by ring closure of the amic acid by azeotropic distillation with toluene. Next, 0.26 parts of IPDI (isophorone diisocyanate, reagent, molecular weight 222.29 g / mol) and 5.36 parts of anisole were added and heated at 130° C. for 3 hours to obtain a soluble polyimide resin (A-1) (molecular weight 82,400) solution.

[0089] Synthesis Example 2 (Synthesis of Soluble Polyimide A-2) A 300 ml reactor equipped with a thermometer, reflux condenser, Dean-Stark apparatus, raw material inlet, nitrogen inlet and stirrer was charged with 6.20 parts of APB-N (1,3-bis(3-aminophenoxy)benzene, Mitsui Chemicals Fine Co., Ltd., molecular weight 292.33 g / mol), 13.14 parts of PRIAMINE1075 (C36 dimer diamine, Croda Japan Co., Ltd., molecular weight 534.38 g / mol), 13.03 parts of ODPA (oxydiphthalic anhydride, Manac Co., Ltd., molecular weight 310.22 g / mol), 83.09 parts of anisole, 0.85 parts of triethylamine and 20.11 parts of toluene, and heated to 120 ° C. to dissolve the raw materials. The reaction was carried out at 135 ° C. for 4 hours while removing water generated by ring closure of amic acid by azeotropic distillation with toluene. Next, 0.26 parts of IPDI (isophorone diisocyanate, reagent, molecular weight 222.29 g / mol) and 5.15 parts of anisole were added and heated at 130° C. for 3 hours to obtain a soluble polyimide resin (A-2) (molecular weight 65,300) solution.

[0090] Synthesis Example 3 (Synthesis of Soluble Polyimide A-3) A 300 ml reactor equipped with a thermometer, a reflux condenser, a Dean-Stark apparatus, a raw material inlet, a nitrogen inlet and a stirrer was charged with 7.95 parts of BAFL (9,9-bis(4-aminophenyl)fluorene, manufactured by JFE Chemical Corporation, molecular weight 348.45 g / mol), 11.86 parts of PRIAMINE1075 (C36 dimer diamine, manufactured by Croda Japan Co., Ltd., molecular weight 534.38 g / mol), 14.66 parts of ODPA (oxydiphthalic anhydride, manufactured by Manac Co., Ltd., molecular weight 310.22 g / mol), 93.48 parts of anisole, 0.96 parts of triethylamine and 21.37 parts of toluene, and heated to 120 ° C. to dissolve the raw materials. The reaction was carried out at 135 ° C. for 4 hours while removing water generated by ring closure of the amic acid by azeotropic distillation with toluene. Next, 0.29 parts of IPDI (isophorone diisocyanate, reagent, molecular weight 222.29 g / mol) and 5.79 parts of anisole were added and heated at 130° C. for 3 hours to obtain a soluble polyimide resin (A-3) (molecular weight 62,500) solution.

[0091] Examples 1 to 7 (Preparation of Resin Compositions of the Present Invention) The components were mixed in the amounts shown in Table 1 (the unit is "parts", and the parts of the polyimide resin and the maleimide resin are parts converted into solid content not including the solvent), and then anisole was added as a solvent in an amount such that the solid content concentration became 25 mass %, and the mixture was mixed uniformly to prepare each of the resin compositions of the present invention.

[0092] The components in Table 1 are as follows: <Component (A)> (A-1) to (A-3): Soluble polyimide resins (A-1) to (A-3) obtained in Synthesis Examples 1 to 3 <(B) component> RPS-1005: Oxazoline group-containing reactive polystyrene, manufactured by Nippon Shokubai Co., Ltd. (weight average molecular weight: 203,068) <(C) component> (C-1); MIR-3000-70MT; maleimide resin, manufactured by Nippon Kayaku Co., Ltd. (maleimide resin (C) represented by the above formula (4)) (C-2); MIR-5000-60T; maleimide resin, manufactured by Nippon Kayaku Co., Ltd. (maleimide resin (C) represented by the above formula (3)) (C-3): BMI-70; maleimide resin, manufactured by K.I. Chemicals Co., Ltd. (maleimide resin (C) represented by the above formula (5)) <Curing accelerator> DCP: Dicumyl peroxide, manufactured by Nouryon Chemical Co., Ltd.

[0093] Using each of the resin compositions obtained in Examples 1 to 7, the compatibility of the resin compositions, the adhesive strength of the cured product to copper foil, the thermal properties, and Tg were evaluated by the following methods.

[0094] (Evaluation of adhesive strength) Ultra-low roughness non-roughening treated electrolytic copper foil CF-T49A-SV (hereinafter referred to as The resin composition is applied to the rough surface of the Each was coated and dried at 120°C for 10 minutes. The thickness of the coating after drying was 20μm. The coating film on the copper foil obtained above was overlaid with CF-T9FZ-THE-35, and vacuum pressed at 200°C for 60 minutes under 3 MPa. The obtained test pieces were cut into 10 mm wide pieces, and the 90° peel strength (peel speed: 50 mm / min) was measured using an autograph AGS-X-500N (Shimadzu Corporation) to evaluate the adhesive strength of the T49A copper foil. The results are shown in Table 1.

[0095] (Evaluation of thermal properties) The test pieces were prepared in the same manner as in the "Evaluation of Adhesive Strength" above, and then used a POT-200C (Taiyo Electric) The time it takes for a blister to appear after floating the solder in a solder bath heated to 288°C (manufactured by Sangyo Co., Ltd.) The thermal properties were evaluated by the following method. The results are shown in Table 1. (Evaluation Criteria) ○ No swelling for more than 600 seconds △ Less than 600 seconds No swelling for 60 seconds or more × Blisters appear in less than 60 seconds

[0096] (Measurement of Tg) The resin compositions were applied to UBE polyimide film Upilex using an automatic applicator, and then dried by heating at 120°C for 10 minutes. The thickness of the coating film after drying was 20 μm. Upilex was placed on the coating film obtained above, and vacuum pressed at 200°C for 60 minutes at 3 MPa. The obtained test pieces were cut into 5 mm wide and 40 mm long, and Tg was measured using DMA (EXSTAR DMS6100, Hitachi High-Tech Corporation). The results are shown in Table 1.

[0097] [Table 1]

[0098] From the results in Table 1, it is clear that the resin composition of the present invention is excellent in adhesive strength and heat resistance. [Industrial Applicability]

[0099] By using the polyimide resin composition of the present invention, it is possible to provide a printed wiring board or the like having excellent adhesiveness and heat resistance.

Claims

1. The resin composition includes: a polyimide resin (A) that is a copolymer of one or more diamino compounds (a-1) having two amino groups in one molecule and a tetrabasic acid dianhydride (a-2); and a copolymer resin (B) that contains a structural unit derived from an aromatic vinyl compound and a structural unit derived from an oxazoline group, The structural unit derived from the aromatic vinyl compound of the component (B) is represented by the following formula (b-1): 【Chemical 1】 (In formula (b-1), R 1 , R 2 each independently represents a hydrogen atom, a methyl group, or an ethyl group, and each x independently represents an integer of 1 to 5. In addition, the structural unit derived from an oxazoline group is represented by the following formula (b-2): 【Chemistry 2】 (In formula (b-2), R 3 each independently represents a hydrogen atom, a methyl group, or an ethyl group. A resin composition, wherein the structural unit is represented by the following formula:

2. 2. The resin composition according to claim 1, wherein the diamino compound (a-1) comprises an aliphatic diamino compound (a-3) having 6 to 36 carbon atoms.

3. At least one of the components (a-1) is represented by the following formula (1) or (2): 【Chemistry 3】 (In formula (1), X is C(CH 3 ) 2 , C(CF 3 ) 2 , S.O. 2 , C.H. 2 , CH(CH 3 ), CH(CF 3 ) indicates 【Chemistry 4】 The resin composition according to claim 1 or 2, wherein the compound is a compound represented by the formula:

4. The resin composition according to claim 1 , further comprising a thermosetting compound (C).

5. The thermosetting compound (C) is represented by the following formulas (3) to (5): 【Chemistry 5】 (In formula (3), R 4 represents an alkyl group having 1 to 5 carbon atoms or a phenyl group, R 4 When a plurality of n are present, they may be the same or different. Each k independently represents an integer of 0 to 3. 1 is the average number of repetitions and represents a real number between 1 and 10.) 【Chemistry 6】 (In formula (4), R 5 represents an alkyl group having 1 to 5 carbon atoms or a phenyl group, R 5 When a plurality of 1's are present, they may be the same or different. Each 1' independently represents an integer of 0 to 3. 2 is the average number of repetitions and represents a real number between 1 and 10.) 【Chemistry 7】 (In formula (5), R 6 and R 7 each independently represents a hydrogen atom, a methyl group, or an ethyl group. The resin composition according to claim 4, comprising one or more compounds selected from the group consisting of compounds represented by the following formula:

6. The resin composition according to claim 4, further comprising a curing accelerator (D).

7. A resin-coated copper foil comprising the resin composition according to claim 1.

8. A copper clad laminate obtained by curing a resin layer made of the resin composition contained in the resin-coated copper foil according to claim 7.

Citation Information

Patent Citations

  • Polyimide, adhesive, film-like adhesive, adhesion layer, adhesive sheet, copper foil with resin, copper-clad laminate, printed wiring board, and multilayer wiring board and method for producing the same

    JP2018168369A

  • Resin composition, film, layered sheet, and semiconductor device

    WO2020071154A1

Cited By

  • Polyimide resin-containing composition and cured product thereof

    WO2025063274A1

  • Resin composition, cured product, laminate, method for manufacturing cured product, method for manufacturing laminate, method for manufacturing semiconductor device, and semiconductor device

    WO2026172949A1