Pressure sensitive adhesive sheet

The adhesive sheet with a specific acrylic polymer and tackifier composition provides superior bending resistance and adhesiveness across a wide temperature range, addressing the limitations of conventional sheets in flexible displays.

JP2024140046APending Publication Date: 2024-10-10NITTO DENKO CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023051032
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Conventional pressure-sensitive adhesive sheets exhibit poor bending resistance at low temperatures and reduced adhesiveness at high temperatures, making them unsuitable for flexible displays used in various environments.

Method used

A pressure-sensitive adhesive sheet comprising an adhesive layer with an acrylic polymer containing specific (meth)acrylic acid alkyl esters and a tackifier, having an elastic modulus of 5.0 MPa or less at -30°C and a gel fraction of 50% or more, ensuring excellent bending resistance and adhesiveness across a wide temperature range.

Benefits of technology

The adhesive sheet maintains excellent bending resistance in low-temperature environments and adhesiveness in both normal and high-temperature conditions, preventing peeling and marking even with repeated bending.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140046000001_ABST
    Figure 2024140046000001_ABST
Patent Text Reader

Abstract

To provide a pressure sensitive adhesive sheet excellent in adhesiveness in a wide temperature range from room temperature to a high temperature environment, while having excellent flex residence under a low temperature environment.SOLUTION: A pressure sensitive adhesive sheet 1 includes an adhesive layer 2. The adhesive layer 2 includes: an acrylic polymer including, as a constitutional unit, a (meth)acrylic acid alkyl ester having a straight-chain or branched alkyl group having 10 or more carbon atoms; and a tackifier. The adhesive layer 2 has an elastic modulus of 5.0 MPa or less at -30°C, and a gel fraction of 50% or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive sheet. [Background technology]

[0002] Adhesive sheets used in image display devices and portable electronic devices such as mobile phones, smartphones, digital cameras, liquid crystal displays (LCDs), and organic electroluminescence (EL) displays are required to have a variety of performance characteristics, including high adhesive strength.

[0003] In recent years, organic electroluminescence (EL) panels using bendable substrates (flexible substrates) such as resin films have been put to practical use, and bendable flexible displays have been proposed. In flexible displays, in addition to the display panel such as an organic electroluminescence (EL) panel being bendable, the constituent members are also bendable, and these members are bonded together via an adhesive sheet. In foldable flexible displays (foldable displays), bending is performed repeatedly at the same location. At the bending point, compressive stress is applied to the inside and tensile stress is applied to the outside, causing distortion at the bending point and its surroundings, which raises concerns that the bending point may be bent or marked, or the adhesive layer may peel off.

[0004] For example, Patent Documents 1 to 7 disclose pressure-sensitive adhesive sheets that are intended to have bending resistance. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-111754 A [Patent Document 2] JP 2019-108498 A [Patent Document 3] JP 2020-111734 A [Patent Document 4] JP 2020-139034 A [Patent Document 5] JP 2020-164575 A [Patent Document 6] JP 2018-27996 A [Patent Document 7] JP 2019-218513 A Summary of the Invention [Problem to be solved by the invention]

[0006] Considering the possibility that flexible displays will be used all over the world, it is not enough for the flexible display to have excellent flex resistance only at room temperature in Japan, but it is required to have excellent flex resistance in various environments. However, even if a conventional pressure-sensitive adhesive sheet has flex resistance at room temperature, it may have poor flex resistance at low temperatures.

[0007] In order to improve the bending resistance at low temperature, it is considered to use a polymer with a low glass transition temperature as a base polymer in the adhesive layer that constitutes the adhesive sheet.However, in this case, the elastic modulus at high temperature is reduced as well as the elastic modulus at low temperature, and as a result, the cohesive force at high temperature is reduced, the adhesiveness is reduced, and the adhesive sheet is easily peeled off.For this reason, it is difficult to prepare an adhesive sheet that has excellent bending resistance at low temperature and excellent adhesiveness at high temperature.

[0008] The present invention was devised under these circumstances, and its object is to provide an adhesive sheet that has excellent bending resistance in low-temperature environments while having excellent adhesiveness over a wide temperature range from room temperature to high-temperature environments. [Means for solving the problem]

[0009] As a result of intensive research conducted by the present inventors to achieve the above object, they have found that a specific pressure-sensitive adhesive sheet has excellent flex resistance in a low-temperature environment, while also having excellent adhesiveness over a wide temperature range from room temperature to a high-temperature environment. The present invention has been completed based on these findings.

[0010] That is, the present invention provides an adhesive sheet having an adhesive layer, the adhesive layer comprising an acrylic polymer containing, as a constituent unit, a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms, and a tackifier, and the adhesive layer has an elastic modulus of 5.0 MPa or less at -30°C and a gel fraction of 50% or more.

[0011] The acrylic polymer preferably contains, as a constituent unit, an alkyl (meth)acrylate ester having a linear or branched alkyl group having 1 to 8 carbon atoms.

[0012] The tackifier preferably comprises an oligomer or a tackifying resin.

[0013] The pressure-sensitive adhesive sheet may be a double-sided pressure-sensitive adhesive sheet for fixing components together in an electric / electronic device.

[0014] The present invention also provides an electric / electronic device comprising the above-mentioned pressure-sensitive adhesive sheet, wherein both adhesive surfaces of the pressure-sensitive adhesive sheet fix components together. Effect of the Invention

[0015] The pressure-sensitive adhesive sheet of the present invention has excellent flex resistance in low-temperature environments and excellent adhesiveness in a wide temperature range from room temperature to high-temperature environments. Therefore, even when the sheet is used in a location where bending is repeatedly performed in a low-temperature environment, the sheet is unlikely to break or leave a mark at the bending location or peel off. [Brief description of the drawings]

[0016] [Figure 1] 1 is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] [Adhesive sheet] The pressure-sensitive adhesive sheet according to one embodiment of the present invention includes at least a pressure-sensitive adhesive layer that contains an acrylic polymer and a tackifier, and has an elastic modulus of 5.0 MPa or less and a gel fraction of 50% or more at −30° C. In this specification, the pressure-sensitive adhesive layer may be referred to as the “pressure-sensitive adhesive layer of the present invention.”

[0018] The pressure-sensitive adhesive sheet of the present invention may be a so-called "substrate-less type" pressure-sensitive adhesive sheet that does not have a substrate (substrate layer), or may be a type of pressure-sensitive adhesive sheet that has a substrate. In this specification, the "substrate-less type" pressure-sensitive adhesive sheet may be referred to as a "substrate-less pressure-sensitive adhesive sheet", and the type of pressure-sensitive adhesive sheet that has a substrate may be referred to as a "substrate-attached pressure-sensitive adhesive sheet". Examples of the substrate-less pressure-sensitive adhesive sheet include a double-sided pressure-sensitive adhesive sheet consisting of only the pressure-sensitive adhesive layer of the present invention, and a double-sided pressure-sensitive adhesive sheet consisting of the pressure-sensitive adhesive layer of the present invention and another pressure-sensitive adhesive layer (a pressure-sensitive adhesive layer other than the pressure-sensitive adhesive layer of the present invention). Examples of the substrate-attached pressure-sensitive adhesive sheet include a single-sided pressure-sensitive adhesive sheet having the pressure-sensitive adhesive layer of the present invention on one side of the substrate, a double-sided pressure-sensitive adhesive sheet having the pressure-sensitive adhesive layer of the present invention on both sides of the substrate, and a double-sided pressure-sensitive adhesive sheet having the pressure-sensitive adhesive layer of the present invention on one side of the substrate and another pressure-sensitive adhesive layer on the other side. The "substrate (substrate layer)" refers to a support, and is a part that is attached to the substrate together with the pressure-sensitive adhesive layer when the pressure-sensitive adhesive sheet of the present invention is used (attached) to the substrate. The release liner that is peeled off when the pressure-sensitive adhesive sheet is used (applied) is not included in the above-mentioned substrate.

[0019] Fig. 1 is a cross-sectional schematic diagram showing one embodiment of a pressure-sensitive adhesive sheet of the present invention. The pressure-sensitive adhesive sheet 1 shown in Fig. 1 is a substrate-less double-sided pressure-sensitive adhesive sheet consisting of a single pressure-sensitive adhesive layer 2 which is the pressure-sensitive adhesive layer of the present invention, and a release liner 3 and a release liner 4 are provided on both adhesive sides thereof, respectively.

[0020] (Pressure-sensitive adhesive layer of the present invention) The pressure-sensitive adhesive sheet of the present invention may have only one pressure-sensitive adhesive layer, or may have two or more layers. When two or more layers are included, at least one layer may be the pressure-sensitive adhesive layer of the present invention, and the other pressure-sensitive adhesive layers may be the pressure-sensitive adhesive layer of the present invention or other pressure-sensitive adhesive layers. When two or more pressure-sensitive adhesive layers of the present invention are included, the multiple pressure-sensitive adhesive layers of the present invention may be the same pressure-sensitive adhesive layer, or may be pressure-sensitive adhesive layers with different compositions, thicknesses, physical properties, etc. In addition, in the case of a pressure-sensitive adhesive sheet with a substrate, the pressure-sensitive adhesive layer provided on one side of the substrate may be a single layer, or may be a multilayer composed of layers that are the same or have different compositions, thicknesses, physical properties, etc.

[0021] The adhesive layer of the present invention has an elastic modulus of 5.0 MPa or less at -30°C, preferably 4.0 MPa or less, more preferably 3.0 MPa or less, even more preferably 2.0 MPa or less, and particularly preferably 1.0 MPa or less. By having the elastic modulus of 5.0 MPa or less, even when repeatedly bent at low temperatures, the bent portion is unlikely to be broken or marked, and the adhesive sheet is unlikely to peel off, and the layer has excellent bending resistance. The elastic modulus is, for example, 0.1 MPa or more, preferably 0.2 MPa or more.

[0022] In this specification, "elastic modulus" refers to dynamic shear storage modulus (G'), which can be measured, for example, using a viscoelasticity tester in shear mode while applying a shear strain at a frequency of 1 Hz in a temperature range of -50 to 150°C and at a heating rate of 5°C / min, and the peak G' at any temperature can be obtained as the elastic modulus.

[0023] The gel fraction (mass ratio of solvent-insoluble components) of the pressure-sensitive adhesive layer of the present invention is 50% or more, preferably 60% or more, and more preferably 70% or more. When the gel fraction is 50% or more, the cohesive force of the pressure-sensitive adhesive layer is improved, and the adhesiveness to the adherend in a high-temperature environment is excellent. The gel fraction is, for example, 95% or less, preferably 90% or less. When the gel fraction is 95%, appropriate flexibility is obtained and adhesiveness is further improved. The gel fraction can be controlled, for example, by the monomer composition of the acrylic polymer, the weight average molecular weight, the amount of crosslinking agent used (addition amount), etc.

[0024] Specifically, the gel fraction is a value calculated by, for example, the "Method of Measuring Gel Fraction" described below. (Method of Measuring Gel Fraction) About 0.2 g of the adhesive layer is taken from the adhesive sheet, wrapped in a porous tetrafluoroethylene sheet (product name "NTF1122", manufactured by Nitto Denko Corporation) with an average pore size of 0.2 μm, and then tied with a string. The mass at this time is measured, and this mass is defined as the mass before immersion. The mass before immersion is the total mass of the mass (B) of the adhesive layer (the adhesive layer taken above), the mass of the tetrafluoroethylene sheet, and the mass of the string. The total mass of the tetrafluoroethylene sheet and the string is also measured, and this mass is defined as the wrapping mass (A). Next, the adhesive layer is wrapped in a tetrafluoroethylene sheet and tied with a kite string (referred to as a "sample"), which is placed in a 50 ml container filled with ethyl acetate and allowed to stand for 7 days at 23° C. Thereafter, the sample (after ethyl acetate treatment) is removed from the container, transferred to an aluminum cup, and dried in a dryer at 130° C. for 2 hours to remove the ethyl acetate, after which the mass is measured and this mass is defined as the post-immersion mass (C). Then, the gel fraction is calculated from the following formula. Gel fraction [mass%] = 100 × (CA) / B

[0025] The pressure-sensitive adhesive layer of the present invention preferably has a 180° peel adhesion strength against a SUS flat surface at room temperature of 5.0 N / 20 mm or more, more preferably 5.5 N / 20 mm or more, and more preferably 6.0 N / 20 mm or more. If the peel adhesion strength is 5.0 N / 20 mm or more, the pressure-sensitive adhesive sheet is unlikely to peel off even when repeatedly bent at around room temperature, and has excellent flex resistance. The higher the peel adhesion strength, the less likely peeling occurs, but for example, it is 20.0 N / 20 mm or less. The room temperature refers to an environment with a temperature of 23° C. and a relative humidity of 50% RH, for example.

[0026] The pressure-sensitive adhesive layer of the present invention is a pressure-sensitive adhesive layer containing an acrylic polymer. The pressure-sensitive adhesive layer of the present invention is preferably an acrylic pressure-sensitive adhesive layer containing an acrylic polymer as a base polymer that exhibits adhesiveness. In this specification, the base polymer refers to a main component among the polymer components in the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer, for example, a polymer component contained in an amount of more than 50 mass%. The content ratio of the base polymer in the pressure-sensitive adhesive layer is preferably 60 mass% or more, more preferably 70 mass% or more, relative to 100 mass% of the total amount of the pressure-sensitive adhesive layer.

[0027] The pressure-sensitive adhesive layer of the present invention contains at least an acrylic polymer containing, as a constituent unit, a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms, and a tackifier. The acrylic polymer may be referred to as the "acrylic polymer of the present invention." The pressure-sensitive adhesive layer of the present invention may contain only one type of the acrylic polymer of the present invention, or may contain two or more types.

[0028] The acrylic polymer of the present invention is a polymer containing an acrylic monomer (a monomer having a (meth)acryloyl group in the molecule) as a monomer component constituting the polymer. That is, the acrylic polymer contains a structural unit derived from an acrylic monomer. Only one type of acrylic polymer may be used, or two or more types may be used. Also, the acrylic polymer may contain only one type of acrylic monomer as a monomer component, or two or more types. In this specification, "(meth)acrylic" refers to "acrylic" and / or "methacrylic" (either one or both of "acrylic" and "methacrylic"), and the same applies to others.

[0029] The acrylic polymer of the present invention contains the above-mentioned (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms as a constituent unit. This allows the pressure-sensitive adhesive sheet of the present invention to have excellent flex resistance in a low-temperature environment without decreasing the adhesiveness in normal temperature and high-temperature environments. The above-mentioned (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms may be used alone or in combination of two or more.

[0030] Examples of the (meth)acrylic acid alkyl ester having a straight or branched alkyl group having 10 or more carbon atoms include decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (lauryl (meth)acrylate), tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0031] In the (meth)acrylic acid alkyl ester having a straight or branched alkyl group having 10 or more carbon atoms, the alkyl group preferably has 10-18 carbon atoms, and more preferably 12-16 carbon atoms.

[0032] The proportion of the (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms in all monomer components constituting the acrylic polymer of the present invention is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, based on the total amount (100% by mass) of all monomer components. In addition, from the viewpoint of copolymerizing other monomer components and obtaining the effects of the other monomer components, the proportion may be 70% by mass or less, 60% by mass or less, 50% by mass or less, 20% by mass or less, 16% by mass or less, or 10% by mass or less.

[0033] The acrylic polymer of the present invention preferably further contains, as a constituent unit, a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 8 carbon atoms. This provides the pressure-sensitive adhesive sheet of the present invention with superior adhesiveness at room temperature and at high temperatures. The (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 8 carbon atoms may be used alone or in combination of two or more.

[0034] Examples of the (meth)acrylic acid alkyl ester having a straight or branched alkyl group having 1 to 8 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isooctyl (meth)acrylate.

[0035] In the (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 8 or more carbon atoms, the alkyl group preferably has 2 to 8 carbon atoms, and more preferably has 4 to 8 carbon atoms.

[0036] The proportion of the (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 8 carbon atoms in all monomer components constituting the acrylic polymer of the present invention is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, still more preferably 60% by mass or more, and particularly preferably 70% by mass or more, based on the total amount (100% by mass) of all monomer components. In addition, the proportion may be 99% by mass or less, 96% by mass or less, or 93% by mass or less, from the viewpoint of copolymerizing other monomer components and obtaining the effects of the other monomer components.

[0037] The acrylic polymer of the present invention is preferably a polymer containing the most structural units derived from (meth)acrylic acid esters in terms of mass ratio. Examples of the (meth)acrylic acid esters include hydrocarbon group-containing (meth)acrylic acid esters. Examples of the hydrocarbon group-containing (meth)acrylic acid esters include (meth)acrylic acid alkyl esters having linear or branched aliphatic hydrocarbon groups, (meth)acrylic acid cycloalkyl esters having alicyclic hydrocarbon groups, and (meth)acrylic acid esters having aromatic hydrocarbon groups, such as (meth)acrylic acid aryl esters. The above hydrocarbon group-containing (meth)acrylic acid esters may be used alone or in combination of two or more.

[0038] Examples of the (meth)acrylic acid alkyl ester include those exemplified as the (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms, those exemplified as the (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 8 carbon atoms, nonyl (meth)acrylate, isononyl (meth)acrylate, etc.

[0039] Examples of the (meth)acrylic acid ester having an alicyclic hydrocarbon group include (meth)acrylic acid esters having a monocyclic aliphatic hydrocarbon ring, such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, and cyclooctyl (meth)acrylate; (meth)acrylic acid esters having a bicyclic aliphatic hydrocarbon ring, such as isobornyl (meth)acrylate; and (meth)acrylic acid esters having a tricyclic or higher aliphatic hydrocarbon ring, such as dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, tricyclopentanyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, and 2-ethyl-2-adamantyl (meth)acrylate.

[0040] Examples of the (meth)acrylic acid ester having an aromatic hydrocarbon group include (meth)acrylic acid phenyl ester and (meth)acrylic acid benzyl ester.

[0041] In order to adequately express the basic properties such as adhesion due to the above-mentioned hydrocarbon group-containing (meth)acrylic acid ester in the adhesive layer, the ratio of the above-mentioned hydrocarbon group-containing (meth)acrylic acid ester in all monomer components constituting the above-mentioned acrylic polymer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and may be 80% by mass or more, 90% by mass or more, or 95% by mass or more, based on the total amount (100% by mass) of the above-mentioned all monomer components. Moreover, the ratio may be 99.9% by mass or less, 98% by mass or less, 95% by mass or less, or 90% by mass or less, from the viewpoint of copolymerizing other monomer components and obtaining the effects of the other monomer components.

[0042] The acrylic polymer of the present invention may contain a structural unit derived from another monomer component copolymerizable with the above-mentioned hydrocarbon group-containing (meth)acrylic acid ester for the purpose of improving cohesive strength, introducing crosslinking points, and other modifications. Examples of the other monomer components include polar group-containing monomers such as carboxy group-containing monomers, acid anhydride monomers, hydroxy group-containing monomers, glycidyl group-containing monomers, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, and nitrogen atom-containing monomers. Only one type of the above-mentioned other monomer components may be used, or two or more types may be used.

[0043] Examples of the hydroxy group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate.

[0044] Examples of the nitrogen atom-containing monomer include amide group-containing monomer, amino group-containing monomer, cyano group-containing monomer, and monomer having a nitrogen atom-containing ring. Examples of the amide group-containing monomer include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylolpropane(meth)acrylamide, N-methoxymethyl(meth)acrylamide, and N-butoxymethyl(meth)acrylamide. Examples of the amino group-containing monomer include aminoethyl(meth)acrylate, N,N-dimethylaminoethyl(meth)acrylate, and t-butylaminoethyl(meth)acrylate. Examples of the cyano group-containing monomer include acrylonitrile and methacrylonitrile. Examples of the monomer having a nitrogen atom-containing ring include N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-vinylmorpholine, N-vinylcaprolactam, and N-(meth)acryloylmorpholine.

[0045] Examples of the carboxy group-containing monomer include acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, etc. Examples of the acid anhydride monomer include maleic anhydride, itaconic anhydride, etc.

[0046] Examples of the keto group-containing monomer include diacetone (meth)acrylamide, diacetone (meth)acrylate, vinyl methyl ketone, vinyl ethyl ketone, allyl acetoacetate, and vinyl acetoacetate.

[0047] Examples of the alkoxysilyl group-containing monomer include 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane.

[0048] Examples of the glycidyl group-containing monomer include glycidyl (meth)acrylate and methylglycidyl (meth)acrylate.

[0049] Examples of the sulfonic acid group-containing monomer include styrenesulfonic acid, allylsulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidepropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid.

[0050] The above-mentioned phosphoric acid group-containing monomer includes, for example, 2-hydroxyethyl acryloyl phosphate.

[0051] The polar group-containing monomer constituting the acrylic polymer of the present invention preferably contains a hydroxyl group-containing monomer and / or a nitrogen atom-containing monomer. By using such a polar group-containing monomer, the cohesive strength and polarity of the adhesive can be adjusted, and the adhesiveness at room temperature and high temperature can be improved.

[0052] When the acrylic polymer of the present invention contains the above-mentioned hydroxyl group-containing monomer as a monomer component constituting the polymer, the ratio of the above-mentioned hydroxyl group-containing monomer in the above-mentioned total monomer components (100 mass%) is not particularly limited, but is preferably 0.01 mass% or more, more preferably 0.1 mass% or more, and even more preferably 0.5 mass% or more. In addition, from the viewpoint of improving the adhesion in a normal temperature environment and the flexibility in a low temperature environment, the ratio of the above-mentioned hydroxyl group-containing monomer is preferably 30 mass% or less, more preferably 10 mass% or less, even more preferably 5 mass% or less, and may be 3 mass% or less.

[0053] When the acrylic polymer of the present invention contains the nitrogen atom-containing monomer as a monomer component constituting the polymer, the ratio of the nitrogen atom-containing monomer in the total monomer components (100% by mass) is not particularly limited, but is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.5% by mass or more. In addition, from the viewpoint of improving the adhesion in a normal temperature environment and the flexibility in a low temperature environment, the ratio of the nitrogen atom-containing monomer is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less.

[0054] The total proportion of the polar group-containing monomers (particularly, the total of the nitrogen atom-containing monomers and the hydroxyl group-containing monomers) in the total monomer components (100% by mass) constituting the acrylic polymer of the present invention is not particularly limited, but from the viewpoint of better exerting the effect of using the polar group-containing monomers, it is preferably 0.1% by mass or more, more preferably 1% by mass or more. Also, from the viewpoint of obtaining a pressure-sensitive adhesive layer with appropriate flexibility, the total proportion is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 4% by mass or less, and particularly preferably 2% by mass or less.

[0055] The monomer components constituting the acrylic polymer of the present invention may further contain other monomers. Examples of the other monomers include vinyl ester monomers such as vinyl acetate, vinyl propionate, and vinyl laurate; aromatic vinyl compounds such as styrene, substituted styrene (α-methylstyrene, etc.), and vinyl toluene; olefin monomers such as ethylene, propylene, isoprene, butadiene, and isobutylene; chlorine-containing monomers such as vinyl chloride and vinylidene chloride; alkoxy group-containing monomers such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; and vinyl ether monomers such as methyl vinyl ether and ethyl vinyl ether. The other monomer components may each be used alone or in combination of two or more.

[0056] Examples of the alkoxy group-containing monomer include those in which one or more hydrogen atoms in the hydrocarbon group of the hydrocarbon group-containing (meth)acrylic ester are substituted with an alkoxy group, such as hydrocarbon group-containing (meth)acrylic esters having an alkoxy group, such as methoxymethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-methoxybutyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, and ethoxyethoxyethyl (meth)acrylate (ethyl carbitol (meth)acrylate).

[0057] The proportion of the other monomers in the total amount (100% by mass) of all monomer components constituting the acrylic polymer of the present invention may be, for example, 0.05% by mass or more, 0.5% by mass or more, 5% by mass or more, or 10% by mass or more. The proportion may be, for example, 20% by mass or less, 10% by mass or less, 5% by mass or less, or may be substantially absent.

[0058] The weight average molecular weight (Mw) of the acrylic polymer of the present invention is 10×10 4 More preferably, it is 60×10 or more. 4 More preferably, 100×10 4 The above Mw is 10×104 When the Mw is 500×10 or more, a pressure-sensitive adhesive exhibiting good cohesiveness is easily obtained. 4 It is preferable that the value is equal to or less than 400×10 4 Less than 300×10, more preferably 4 The above Mw is 500×10 4 If it is less than this, it is easy to form an adhesive that shows moderate fluidity (mobility of polymer chains), and therefore it has better flex resistance. The weight average molecular weight is measured by gel permeation chromatography (GPC) and calculated in terms of polystyrene.

[0059] The glass transition temperature (Tg) of the acrylic polymer of the present invention is preferably 0° C. or lower, more preferably -10° C. or lower, and more preferably -20° C. or lower. When the glass transition temperature is 0° C. or lower, even when repeatedly bent in a low-temperature environment, the bent portion is unlikely to be broken or marked, and the adhesive sheet is unlikely to peel off. The glass transition temperature is preferably -80° C. or higher, more preferably -70° C. or higher, and even more preferably -66° C. or higher.

[0060] The above glass transition temperature is a value calculated based on the following formula (X) (Fox formula). 1 / Tg=W1 / Tg1+W2 / Tg2+···+Wn / Tgn (X) [In formula (X), Tg is the glass transition temperature (unit: K) of the polymer, Tgi (i = 1, 2, ..., n) is the glass transition temperature (unit: K) when monomer i forms a homopolymer, and Wi (i = 1, 2, ..., n) is the mass fraction of monomer i in all monomer components.] The above formula (X) is a calculation formula when the polymer is composed of n types of monomer components, namely, monomer 1, monomer 2, . . . , monomer n.

[0061] In this specification, the term "glass transition temperature (Tg) when a homopolymer is formed" (sometimes simply referred to as "Tg of homopolymer") means "glass transition temperature (Tg) of a homopolymer of the monomer", and specifically, numerical values ​​are given in "Polymer Handbook" (3rd Edition, John Wiley & Sons, Inc., 1987). The Tg of a homopolymer of a monomer not described in the above literature refers to, for example, a value obtained by the following measurement method (see JP 2007-51271 A) except for a monomer having a polyorganosiloxane skeleton. That is, 100 parts by mass of a monomer, 0.2 parts by mass of 2,2'-azobisisobutyronitrile, and 200 parts by mass of ethyl acetate as a polymerization solvent are charged into a reactor equipped with a thermometer, a stirrer, a nitrogen inlet tube, and a reflux condenser tube, and stirred for 1 hour while introducing nitrogen gas. After removing oxygen from the polymerization system in this way, the temperature is raised to 63°C and reacted for 10 hours. Then, the mixture is cooled to room temperature to obtain a homopolymer solution with a solid content of 33% by mass. The homopolymer solution is then cast onto a release liner and dried to prepare a test sample (sheet-shaped homopolymer) with a thickness of about 2 mm. The test sample is then punched out into a disk shape with a diameter of 7.9 mm, sandwiched between parallel plates, and the viscoelasticity is measured in a shear mode at a temperature range of -70 to 150°C and a heating rate of 5°C / min using a viscoelasticity tester (product name "ARES", manufactured by Rheometrics Co., Ltd.) while applying a shear strain of 1 Hz. The peak top temperature of tan δ is taken as the Tg of the homopolymer.

[0062] The acrylic polymer of the present invention is obtained by polymerizing a composition containing at least an acrylic monomer. The polymerization method is not particularly limited, but includes, for example, a solution polymerization method, an emulsion polymerization method, a bulk polymerization method, a thermal polymerization method, and a polymerization method by irradiation with active energy rays (active energy ray polymerization method). Among them, the bulk polymerization method, the thermal polymerization method, and the active energy ray polymerization method are preferred from the viewpoints of the transparency of the adhesive layer, the cost, and the like. The obtained acrylic polymer may be any of a random copolymer, a block copolymer, a graft copolymer, and the like.

[0063] Various common solvents may be used when polymerizing the monomer components. Examples of the solvent include organic solvents such as esters such as ethyl acetate and n-butyl acetate, aromatic hydrocarbons such as toluene and benzene, aliphatic hydrocarbons such as n-hexane and n-heptane, alicyclic hydrocarbons such as cyclohexane and methylcyclohexane, and ketones such as methyl ethyl ketone and methyl isobutyl ketone. Only one of the above solvents may be used, or two or more of them may be used.

[0064] The polymerization initiator, chain transfer agent, emulsifier, etc. used in the radical polymerization of the monomer components are not particularly limited and can be appropriately selected and used. The weight average molecular weight of the polymer can be controlled by the amount of the polymerization initiator and chain transfer agent used and the reaction conditions, and the amount of each of these is appropriately adjusted depending on the type of the polymerization initiator and chain transfer agent used.

[0065] As the polymerization initiator used for the polymerization of the monomer components, a thermal polymerization initiator, a photopolymerization initiator (photoinitiator), etc. can be used depending on the type of polymerization reaction. The above polymerization initiators may be used alone or in combination of two or more.

[0066] The thermal polymerization initiator is not particularly limited, but examples thereof include azo polymerization initiators, peroxide polymerization initiators (e.g., persulfates such as dibenzoyl peroxide, tert-butyl permaleate, potassium persulfate, etc., benzoyl peroxide, hydrogen peroxide, etc.), substituted ethane initiators such as phenyl-substituted ethane, aromatic carbonyl compounds, redox polymerization initiators, etc. Among them, the azo polymerization initiators disclosed in JP-A-2002-69411 are preferred. Examples of the azo polymerization initiators include 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionate)dimethyl, and 4,4'-azobis-4-cyanovaleric acid. The amount of the thermal polymerization initiator used may be a normal amount, and may be selected, for example, from the range of 0.01 to 5 parts by mass, preferably 0.05 to 3 parts by mass, per 100 parts by mass of the monomer component.

[0067] The photopolymerization initiator is not particularly limited, but examples thereof include benzoin ether-based photopolymerization initiators, acetophenone-based photopolymerization initiators, α-ketol-based photopolymerization initiators, aromatic sulfonyl chloride-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzyl-based photopolymerization initiators, benzophenone-based photopolymerization initiators, ketal-based photopolymerization initiators, and thioxanthone-based photopolymerization initiators. Other examples include acylphosphine oxide-based photopolymerization initiators and titanocene-based photopolymerization initiators. Examples of the benzoin ether-based photopolymerization initiators include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethane-1-one, and anisole methyl ether. Examples of the acetophenone-based photopolymerization initiator include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone. Examples of the α-ketol-based photopolymerization initiator include 2-methyl-2-hydroxypropiophenone and 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropan-1-one. Examples of the aromatic sulfonyl chloride-based photopolymerization initiator include 2-naphthalenesulfonyl chloride. Examples of the photoactive oxime-based photopolymerization initiator include 1-phenyl-1,1-propanedione-2-(O-ethoxycarbonyl)-oxime. Examples of the benzoin-based photopolymerization initiator include benzoin. Examples of the benzyl-based photopolymerization initiator include benzyl. Examples of the benzophenone-based photopolymerization initiator include benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, α-hydroxycyclohexylphenyl ketone, etc. Examples of the ketal-based photopolymerization initiator include benzyl dimethyl ketal, etc.Examples of the thioxanthone-based photopolymerization initiator include thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone. Examples of the acylphosphine oxide-based photopolymerization initiator include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. Examples of the titanocene-based photopolymerization initiator include bis(η5-2,4-cyclopentadiene-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium. The amount of the photopolymerization initiator used may be a normal amount, and can be selected, for example, from the range of 0.01 to 5 parts by mass, preferably 0.05 to 3 parts by mass, per 100 parts by mass of the monomer component.

[0068] The acrylic polymer of the present invention may contain a structural part derived from the crosslinking agent. That is, the acrylic polymer of the present invention may be crosslinked by the crosslinking agent. By using the crosslinking agent, a crosslinked structure is formed in the acrylic polymer in the acrylic pressure-sensitive adhesive layer, and the gel fraction can be controlled. The crosslinking agent may be used alone or in combination of two or more.

[0069] The crosslinking agent is not particularly limited, but examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, melamine-based crosslinking agents, peroxide-based crosslinking agents, urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, carbodiimide-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, amine-based crosslinking agents, hydrazine-based crosslinking agents, silicone-based crosslinking agents, and silane-based crosslinking agents (silane coupling agents).

[0070] The content of the crosslinking agent is not particularly limited, but is preferably 0.001 to 20 parts by mass, more preferably 0.01 to 15 parts by mass, even more preferably 0.15 to 5 parts by mass, still more preferably 0.1 to 3 parts by mass, and particularly preferably 0.2 to 2 parts by mass, relative to 100 parts by mass of the total amount of the monomer components constituting the acrylic polymer of the present invention.

[0071] The isocyanate crosslinking agent is a compound having an average of two or more isocyanate groups per molecule (a polyfunctional isocyanate compound). Examples of the isocyanate crosslinking agent include aliphatic polyisocyanates, alicyclic polyisocyanates, and aromatic polyisocyanates.

[0072] Examples of the aliphatic polyisocyanates include 1,2-ethylene diisocyanate; tetramethylene diisocyanates such as 1,2-tetramethylene diisocyanate, 1,3-tetramethylene diisocyanate, and 1,4-tetramethylene diisocyanate; hexamethylene diisocyanates such as 1,2-hexamethylene diisocyanate, 1,3-hexamethylene diisocyanate, 1,4-hexamethylene diisocyanate, 1,5-hexamethylene diisocyanate, 1,6-hexamethylene diisocyanate, and 2,5-hexamethylene diisocyanate; 2-methyl-1,5-pentane diisocyanate, 3-methyl-1,5-pentane diisocyanate, and lysine diisocyanate.

[0073] Examples of the alicyclic polyisocyanates include isophorone diisocyanate; cyclohexyl diisocyanates such as 1,2-cyclohexyl diisocyanate, 1,3-cyclohexyl diisocyanate, and 1,4-cyclohexyl diisocyanate; cyclopentyl diisocyanates such as 1,2-cyclopentyl diisocyanate and 1,3-cyclopentyl diisocyanate; hydrogenated xylylene diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated tetramethylxylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate.

[0074] Examples of the aromatic polyisocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, 2-nitrodiphenyl-4,4'-diisocyanate, 2,2'-diphenylpropane-4,4'-diisocyanate, Examples of the diisocyanate include 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4'-diphenylpropane diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, naphthylene-1,4-diisocyanate, naphthylene-1,5-diisocyanate, 3,3'-dimethoxydiphenyl-4,4'-diisocyanate, xylylene-1,4-diisocyanate, and xylylene-1,3-diisocyanate.

[0075] Examples of the isocyanate crosslinking agent include commercially available products such as trimethylolpropane / tolylene diisocyanate adduct (product name "Coronate L", manufactured by Tosoh Corporation), trimethylolpropane / hexamethylene diisocyanate adduct (product name "Coronate HL", manufactured by Tosoh Corporation), and trimethylolpropane / xylylene diisocyanate adduct (product name "Takenate D-110N", manufactured by Mitsui Chemicals, Inc.).

[0076] In addition, in the aqueous dispersion of the modified acrylic polymer prepared by emulsion polymerization, it is not necessary to use an isocyanate-based crosslinking agent. However, if necessary, a blocked isocyanate-based crosslinking agent can be used since it easily reacts with water.

[0077] When an isocyanate-based crosslinking agent is used as the crosslinking agent, the content of the isocyanate-based crosslinking agent is not particularly limited, but is preferably 0.01 parts by mass or more, more preferably 0.02 parts by mass or more, based on 100 parts by mass of the total amount of the monomer components constituting the acrylic polymer of the present invention. The content is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, even more preferably 0.3 parts by mass or less, even more preferably 0.2 parts by mass or less, and particularly preferably 0.1 parts by mass or less.

[0078] Examples of the epoxy crosslinking agent (polyfunctional epoxy compound) include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, sorbitol polyglycidyl ether, and ethylene glycol diglycidyl ether. Examples of the epoxy crosslinking agent include glycidyl ether, glycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether, sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl-tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. Examples of the epoxy crosslinking agent include commercially available products such as "Tetrad C" (manufactured by Mitsubishi Gas Chemical Co., Ltd.).

[0079] When an epoxy-based crosslinking agent is used as the crosslinking agent, the content of the epoxy-based crosslinking agent is not particularly limited, but is preferably more than 0 part by mass and not more than 1 part by mass, more preferably 0.001 to 0.5 parts by mass, still more preferably 0.002 to 0.2 parts by mass, still more preferably 0.005 to 0.1 parts by mass, still more preferably 0.008 to 0.1 parts by mass, and particularly preferably 0.009 to 0.05 parts by mass, relative to 100 parts by mass of the total amount of the monomer components constituting the acrylic polymer of the present invention.

[0080] As the peroxide-based crosslinking agent, any peroxide-based crosslinking agent that generates radical active species by heat and promotes crosslinking of the base polymer can be used as appropriate. Taking into consideration workability and stability, it is preferable to use a peroxide with a 1-minute half-life temperature of 80 to 160°C, and it is more preferable to use a peroxide with a 1-minute half-life temperature of 90 to 140°C.

[0081] Examples of the peroxide-based crosslinking agent include di(2-ethylhexyl)peroxydicarbonate (1-minute half-life temperature: 90.6° C.), di(4-t-butylcyclohexyl)peroxydicarbonate (1-minute half-life temperature: 92.1° C.), di-sec-butylperoxydicarbonate (1-minute half-life temperature: 92.4° C.), t-butylperoxyneodecanoate (1-minute half-life temperature: 103.5° C.), t-hexylperoxypivalate (1-minute half-life temperature: 109.1° C.), t-butylperoxypivalate (1-minute half-life temperature: 110.3° C.), dilauroylperoxy 1-minute half-life temperature: 116.4°C), di-n-octanoyl peroxide (1-minute half-life temperature: 117.4°C), 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate (1-minute half-life temperature: 124.3°C), di(4-methylbenzoyl)peroxide (1-minute half-life temperature: 128.2°C), dibenzoyl peroxide (1-minute half-life temperature: 130.0°C), t-butylperoxyisobutyrate (1-minute half-life temperature: 136.1°C), 1,1-di(t-hexylperoxy)cyclohexane (1-minute half-life temperature: 149.2°C), and the like.

[0082] The half-life of the peroxide-based crosslinking agent is an index showing the decomposition rate of the peroxide, and refers to the time until the remaining amount of the peroxide is reduced to half. The decomposition temperature for obtaining the half-life at any time and the half-life time at any temperature are described in the manufacturer's catalog, for example, NOF Corp.'s "Organic Peroxide Catalog 9th Edition (May 2003)". The amount of decomposed peroxide remaining after the reaction can be measured, for example, by HPLC (high performance liquid chromatography). More specifically, for example, about 0.2 g of the adhesive after the reaction is taken out, immersed in 10 ml of ethyl acetate, and shaken and extracted for 3 hours at 25°C and 120 rpm in a shaker, and then allowed to stand at room temperature for 3 days. Next, 10 ml of acetonitrile is added, shaken for 30 minutes at 25°C and 120 rpm, and filtered through a membrane filter (0.45 μm). About 10 μl of the extract obtained is injected into HPLC for analysis, and can be used as the amount of peroxide after the reaction.

[0083] When a peroxide-based crosslinking agent is used as the crosslinking agent, the content of the crosslinking agent is not particularly limited, but is preferably 2 parts by mass or less, more preferably 0.02 to 2 parts by mass, even more preferably 0.05 to 1.5 parts by mass, still more preferably 0.05 to 1 part by mass, and particularly preferably 0.1 to 1 part by mass, relative to 100 parts by mass of the total amount of the monomer components constituting the acrylic polymer of the present invention.

[0084] In addition, the crosslinking agent may be used in combination with an organic crosslinking agent or a polyfunctional metal chelate. The polyfunctional metal chelate is a compound in which a polyvalent metal is covalently or coordinately bonded to an organic compound. Examples of polyvalent metal atoms include Al, Cr, Zr, Co, Cu, Fe, Ni, V, Zn, In, Ca, Mg, Mn, Y, Ce, Sr, Ba, Mo, La, Sn, and Ti. Examples of atoms in the organic compound that are covalently or coordinately bonded include oxygen atoms, and examples of the organic compound include alkyl esters, alcohol compounds, carboxylic acid compounds, ether compounds, and ketone compounds.

[0085] The crosslinking agent preferably contains an isocyanate-based crosslinking agent. It is more preferable to contain another crosslinking agent together with the isocyanate-based crosslinking agent. The other crosslinking agent is preferably a peroxide-based crosslinking agent. By using such a crosslinking agent, the acrylic polymer of the present invention can provide a pressure-sensitive adhesive layer that is thin but has excellent adhesion.

[0086] The pressure-sensitive adhesive layer of the present invention contains a tackifier. The pressure-sensitive adhesive layer of the present invention contains the acrylic polymer of the present invention and a tackifier, and therefore has excellent adhesion to the adherend, is not easily peeled off even when repeatedly bent in a low-temperature environment, and has excellent flex resistance. The above tackifier may be used alone or in combination of two or more.

[0087] The tackifier includes a tackifier resin and an oligomer. The oligomer may be present as an oligomer in the pressure-sensitive adhesive layer of the present invention, or may be present in the acrylic polymer of the present invention as a structural part derived from the oligomer. That is, the acrylic polymer of the present invention may have a structural part derived from the oligomer.

[0088] Examples of the tackifier resin include phenol-based tackifier resins, terpene-based tackifier resins, rosin-based tackifier resins, hydrocarbon-based tackifier resins, epoxy-based tackifier resins, polyamide-based tackifier resins, elastomer-based tackifier resins, ketone-based tackifier resins, etc. Only one type of the tackifier resins may be used, or two or more types may be used.

[0089] Examples of the phenol-based tackifier resin include terpene phenol resin, hydrogenated terpene phenol resin, alkyl phenol resin, and rosin phenol resin. The terpene phenol resin is a polymer containing a terpene residue and a phenol residue, and examples thereof include a copolymer of a terpene and a phenol compound (terpene-phenol copolymer resin), and a homopolymer or copolymer of a terpene modified with phenol (phenol modified terpene resin). Examples of the terpene phenol resin include monoterpenes such as α-pinene, β-pinene, and limonene (d-form, l-form, d / l-form (dipentene), etc.). The hydrogenated terpene phenol resin is a resin having a structure obtained by hydrogenating the terpene phenol resin. The alkyl phenol resin is a resin (oil-based phenol resin) obtained from an alkyl phenol and formaldehyde. Examples of the alkyl phenol resin include novolac type and resol type. The rosin phenol resin is a phenol modified product of rosins or various rosin derivatives described below. The rosin phenol resin can be obtained, for example, by adding phenol to rosins or various rosin derivatives described below in the presence of an acid catalyst and then thermally polymerizing the resulting mixture.

[0090] The terpene-based tackifying resin includes polymers of terpenes (typically monoterpenes) such as α-pinene, β-pinene, d-limonene, l-limonene, and dipentene. The terpene polymer may be a homopolymer of one type of terpene, or a copolymer of two or more types of terpenes. Examples of homopolymers of one type of terpene include α-pinene polymer, β-pinene polymer, and dipentene polymer. The modified terpene-based tackifying resin is a modified terpene resin (modified terpene resin). Examples of the modified terpene resin include styrene-modified terpene resin and hydrogenated terpene resin.

[0091] Examples of the rosin-based tackifier resin include rosins and rosin derivative resins. Examples of the rosins include unmodified rosins (raw rosins) such as gum rosin, wood rosin, and tall oil rosin; modified rosins (hydrogenated rosin, disproportionated rosin, polymerized rosin, and other chemically modified rosins) obtained by modifying these unmodified rosins through hydrogenation, disproportionation, polymerization, and the like. Examples of the rosin derivative resin include derivatives of the rosins. Examples of the rosin derivative resin include rosin esters such as unmodified rosin esters, which are esters of unmodified rosin and alcohols, and modified rosin esters, which are esters of modified rosin and alcohols; unsaturated fatty acid modified rosins obtained by modifying rosin with unsaturated fatty acids; unsaturated fatty acid modified rosin esters obtained by modifying rosin esters with unsaturated fatty acids; rosin alcohols obtained by reducing the carboxyl groups of rosins or the various rosin derivatives described above; and metal salts of rosins or the various rosin derivatives described above. Specific examples of the rosin esters include methyl esters, triethylene glycol esters, glycerin esters, and pentaerythritol esters of unmodified or modified rosin.

[0092] Examples of the hydrocarbon tackifier resin include aliphatic hydrocarbon resins, aromatic hydrocarbon resins, aliphatic cyclic hydrocarbon resins, aliphatic / aromatic petroleum resins (styrene-olefin copolymers, etc.), aliphatic / alicyclic petroleum resins, hydrogenated hydrocarbon resins, coumarone resins, and coumarone-indene resins.

[0093] The softening point of the tackifier resin is preferably 160° C. or lower, more preferably 150° C. or lower, and even more preferably 140° C. or lower. When the softening point is low, the elastic modulus can be maintained low even when a small amount is added, and the flex resistance is further improved in a low temperature environment. The softening point is, for example, 60° C. or higher, preferably 70° C. or higher.

[0094] The weight average molecular weight of the oligomer is preferably 2500 to 10000, and more preferably 3000 to 8000. The weight average molecular weight can be determined in terms of polystyrene by the GPC method. For example, it can be measured under the following conditions using a high-speed GPC device "HPLC-8120GPC" manufactured by Tosoh Corporation. Column: TSKgel SuperHZM-H / HZ4000 / HZ3000 / HZ2000 Solvent: Tetrahydrofuran Flow rate: 0.6ml / min

[0095] The oligomer is preferably an acrylic oligomer composed of an acrylic monomer as an essential monomer component. Examples of the acrylic monomer that is a monomer component that composes the acrylic oligomer include those exemplified and explained as monomer components that compose the acrylic polymer of the present invention. The acrylic oligomer preferably contains a (meth)acrylic acid ester having an alicyclic hydrocarbon group as a constituent unit. The acrylic monomer contained as the constituent unit may be one type or two or more types.

[0096] The proportion of the (meth)acrylic acid ester having an alicyclic hydrocarbon group in the total amount (100% by mass) of all monomer components constituting the acrylic oligomer is preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 55% by mass or more. The proportion is preferably 99% by mass or less, and may be 97% by mass or less.

[0097] In one embodiment, the acrylic oligomer preferably contains a (meth)acrylic acid alkyl ester as a constituent unit. The (meth)acrylic acid alkyl ester is preferably methyl methacrylate (MMA). The proportion of the (meth)acrylic acid alkyl ester in all monomer components constituting the acrylic oligomer is preferably 10% by mass or more, more preferably 20% by mass or more. The proportion is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 45% by mass or less. The acrylic oligomer may also contain the copolymerizable monomer as a constituent unit.

[0098] In one embodiment, the acrylic oligomer preferably contains a functional group-containing monomer as a constituent unit. The functional group-containing monomer is preferably a polar group-containing monomer, more preferably a carboxy group-containing monomer. The ratio of the functional group-containing monomer in the total monomer components constituting the acrylic oligomer is preferably 3% by mass or more, more preferably 4% by mass or more. The ratio is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 8% by mass or less. The acrylic oligomer may also contain the copolymerizable monomer as a constituent unit.

[0099] The oligomer is obtained by polymerizing a composition containing the monomer components constituting the oligomer. Examples of these polymerization methods include those exemplified and explained as the polymerization methods for the acrylic polymer described above. Among them, the bulk polymerization method, the thermal polymerization method, and the active energy ray polymerization method are preferable. Various general solvents may be used when polymerizing the monomer components. Examples of the solvent include those exemplified and explained as solvents that may be used in the polymerization of the acrylic polymer described above. Only one type of the solvent may be used, or two or more types may be used. The polymerization initiator, chain transfer agent, emulsifier, etc. used in the radical polymerization of the monomer components are not particularly limited and can be appropriately selected and used.

[0100] The content of the tackifier in the pressure-sensitive adhesive layer of the present invention is not particularly limited, but is, for example, 0.6 parts by mass or more, preferably 2 parts by mass or more, based on 100 parts by mass of the total amount of the acrylic polymer of the present invention. If the content is 0.6 parts by mass or more, peeling is unlikely to occur even when repeatedly bent in a low-temperature environment. From the viewpoint of unlikely peeling even when repeatedly bent at low temperatures, the content is preferably less than 30 parts by mass, more preferably 25 parts by mass or less.

[0101] The content of the tackifier in the pressure-sensitive adhesive layer of the present invention is not particularly limited, but is preferably more than 0% by mass and not more than 22% by mass, more preferably 1 to 16% by mass, relative to 100% by mass of the total amount of the pressure-sensitive adhesive layer of the present invention. When the content is within the above range, peeling is unlikely to occur even when repeatedly bent in a low-temperature environment.

[0102] The pressure-sensitive adhesive layer of the present invention may contain a colorant. The colorant may be a pigment or a dye. Examples of the colorant include black colorants, cyan colorants, magenta colorants, and yellow colorants. From the viewpoint of superior visibility and design, black colorants are preferred. The colorant may contain only one type, or may contain two or more types.

[0103] Examples of black colorants include carbon black, carbon nanotubes, graphite, copper oxide, manganese dioxide, azo pigments such as azomethine azo black, aniline black, perylene black, titanium black, cyanine black, activated carbon, ferrite, magnetite, chromium oxide, iron oxide, molybdenum disulfide, composite oxide black pigments, anthraquinone organic black dyes, azo organic black dyes, etc. Examples of carbon black include furnace black, channel black, acetylene black, thermal black, lamp black, etc. Examples of black colorants include CI Solvent Black 3, 7, 22, 27, 29, 34, 43, and 70; CI Direct Black 17, 19, 22, 32, 38, 51, and 71; CI Acid Black 1, 2, 24, 26, 31, 48, 52, 107, 109, 110, 119, and 154; CI Disperse Black 1, 3, 10, and 24; and CI Pigment Black 1 and 7.

[0104] Examples of cyan colorants include CI Solvent Blue 25, 36, 60, 70, 93, and 95; CI Acid Blue 6 and 45; CI Pigment Blue 1, 2, 3, 15, 15:1, 15:2, 15:3, 15:4, 15:5, 15:6, 16, 17, 17:1, 18, 22, 25, 56, 60, 63, 65, and 66; CI Bat Blue 4; CI Pigment Green 7; and the like.

[0105] Examples of magenta colorants include CI Solvent Red 1, 3, 8, 23, 24, 25, 27, 30, 49, 52, 58, 63, 81, 82, 83, 84, 100, 109, 111, 121, and 122; CI Disperse Red 9; CI Solvent Violet 8, 13, 14, 21, and 27; and CI Disperse Red 9. CI Basic Violet 1; CI Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39, 40; CI Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27, 28, etc. Examples of magenta colorants include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 39, 40, 41, 42, and 48:1. 48:2, 48:3, 48:4, 49, 49:1, 50, 51, 52, 52:2, 53:1, 54, 55, 56, 57:1, 58, 60, 60:1, 63, 63:1, 63:2, 64, 64:1, 67, 68, 81, 83, 87, 88, 89, 90, 92, 101 , 104, 105, 106, 108, 112, 114, 122, 123, 139, 144, 146, 147, 149, 150, 151, 163, 166, 168, 170, 171, 172, 175, 176, 177, 178, 179, 184, 185, 187, 190 , 193, 202, 206, 207, 209, 219, 222, 224, 238, 245; CI Pigment Violet 3, 9, 19, 23, 31, 32, 33, 36, 38, 43, 50; CI Bat Red 1, 2, 10, 13, 15, 23, 29, 35.

[0106] Examples of yellow colorants include CI Solvent Yellow 19, 44, 77, 79, 81, 82, 93, 98, 103, 104, 112, and 162; CI Pigment Orange 31 and 43; CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 24, 34, 35, 37, 42, 53, 55, 65, 73, and 74. , 75, 81, 83, 93, 94, 95, 97, 98, 100, 101, 104, 108, 109, 110, 113, 114, 116, 117, 120, 128, 129, 133, 138, 139, 147, 150, 151, 153, 154, 155, 156, 167, 172, 173, 180, 185, 195; CI Bat Yellow 1, 3, and 20.

[0107] The pressure-sensitive adhesive layer of the present invention may further contain additives such as crosslinking accelerators, antiaging agents, antioxidants, plasticizers, softeners, surfactants, antistatic agents, surface lubricants, leveling agents, light stabilizers, UV absorbers, polymerization inhibitors, foil-like materials, and rust inhibitors, as necessary, within the range that does not impair the effects of the present invention. Only one of the above additives may be used, or two or more of them may be used.

[0108] The rust inhibitor is a compound that prevents metal rust and corrosion. When the adherend is a metal, rust and corrosion can be suppressed when the pressure-sensitive adhesive sheet is attached. Examples of the rust inhibitor include amine compounds, benzotriazole compounds, and nitrites. Other examples include ammonium benzoate, ammonium phthalate, ammonium stearate, ammonium palmitate, ammonium oleate, ammonium carbonate, dicyclohexylamine benzoate, urea, urotropine, thiourea, phenyl carbamate, and cyclohexylammonium-N-cyclohexylcarbamate (CHC). The rust inhibitor may be used alone or in combination of two or more.

[0109] The content of the rust inhibitor is not particularly limited, but is preferably 0.02 to 15 parts by mass relative to 100 parts by mass of the base polymer. When the content is 0.02 parts by mass or more, good corrosion prevention performance is easily obtained. When the content is 15 parts by mass or less, transparency is easily ensured.

[0110] Among these, the rust inhibitor is preferably a benzotriazole-based compound, since it can provide a balanced and high level of compatibility with the base polymer, adhesion reliability, transparency, and corrosion prevention properties, and can provide excellent appearance.

[0111] The content of the benzotriazole compound is not particularly limited, but is preferably 0.02 to 3 parts by mass, more preferably 0.02 to 2.5 parts by mass, and even more preferably 0.02 to 2 parts by mass, relative to 100 parts by mass of the base polymer.

[0112] The thickness of the pressure-sensitive adhesive layer of the present invention is preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 30 μm or less. When the thickness is 50 μm or less, the difference between the inner and outer diameters when bent is small, and the stress applied when bent is easily alleviated. The thickness is not particularly limited, but from the viewpoint of excellent adhesion and less peeling when bent, it is preferably 6 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more.

[0113] When the pressure-sensitive adhesive sheet of the present invention is a double-sided pressure-sensitive adhesive sheet with a substrate, the total thickness of the pressure-sensitive adhesive layer on one side is not particularly limited, but is preferably 6 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more. When the thickness is 6 μm or more, the adhesiveness is excellent and peeling is unlikely to occur when the sheet is bent. The total thickness of the pressure-sensitive adhesive layer on one side is preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 30 μm or less. When the thickness is 50 μm or less, the difference between the inner and outer diameters when the sheet is bent is small, and the stress applied when the sheet is bent is easily alleviated. In addition, when the sheet is a double-sided pressure-sensitive adhesive sheet with a substrate, the thicknesses of the pressure-sensitive adhesive layers on both sides may be the same or different.

[0114] The pressure-sensitive adhesive layer constituting the pressure-sensitive adhesive sheet of the present invention may be in any form, for example, an emulsion type, a solvent type (solution type), an active energy ray curing type, a heat melting type (hot melt type), etc. Among these, a solvent type or an active energy ray curing type pressure-sensitive adhesive layer is preferred because it is easy to obtain a pressure-sensitive adhesive layer with excellent productivity.

[0115] Examples of the active energy rays include ionizing radiation such as α rays, β rays, γ rays, neutron rays, and electron beams, and ultraviolet rays, and ultraviolet rays are particularly preferred. That is, the active energy ray-curable pressure-sensitive adhesive layer is preferably an ultraviolet ray-curable pressure-sensitive adhesive layer.

[0116] The pressure-sensitive adhesive layer can be produced, for example, by applying (coating) a pressure-sensitive adhesive composition for forming the pressure-sensitive adhesive layer onto a release liner and drying and curing the resulting pressure-sensitive adhesive composition layer, or by applying (coating) the pressure-sensitive adhesive composition onto a release liner and irradiating the resulting pressure-sensitive adhesive composition layer with active energy rays to cure it. If necessary, the pressure-sensitive adhesive layer may be further dried by heating.

[0117] (base material) The substrate is an element that functions as a support in the pressure-sensitive adhesive sheet. The substrate may be a single layer or a laminate of substrates of the same or different types.

[0118] Examples of the substrate include a plastic substrate (e.g., a plastic film), a porous material such as paper, cloth, or nonwoven fabric, a net, or a foam sheet. The substrate is preferably a plastic substrate (particularly a plastic film). The substrate is preferably a non-foam sheet.

[0119] Examples of the resin constituting the plastic substrate include polyolefin resins such as low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, high-density polyethylene, very low-density polyethylene, random copolymer polypropylene, block copolymer polypropylene, homopolypropylene, polybutene, polymethylpentene, ethylene-vinyl acetate copolymer (EVA), ionomer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester (random, alternating) copolymer, ethylene-butene copolymer, ethylene-hexene copolymer, etc.; polyurethane resin; rubber resin (natural rubber, synthetic rubber, mixtures thereof, etc.): polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate, polybutylene terephthalate (PBT), etc.; polycarbonate; polyimide; polyether ether ketone; polyetherimide; polyamides such as aramid and fully aromatic polyamide; polyphenyl sulfide; fluororesin; polyvinyl chloride; polyvinylidene chloride; cellulose resin; silicone resin, etc. Only one of the above resins may be used, or two or more of them may be used.

[0120] The substrate may contain various additives such as fillers (inorganic fillers, organic fillers, etc.), colorants (pigments and dyes), dispersants (surfactants, etc.), antioxidants, antioxidants, UV absorbers, antistatic agents, lubricants, plasticizers, etc. The blending ratio of the various additives is about less than 30% by mass (e.g., less than 20% by mass, typically less than 10% by mass) relative to the total mass (100% by mass) of the substrate.

[0121] The substrate may include an auxiliary layer, such as a colored layer, a reflective layer, an undercoat layer, or an antistatic layer, provided on the surface of the substrate.

[0122] The surface of the substrate may be subjected to a surface treatment such as a physical treatment such as corona discharge treatment, plasma treatment, sand mat processing treatment, ozone exposure treatment, flame exposure treatment, high-voltage shock exposure treatment, ionizing radiation treatment, etc.; a chemical treatment such as chromate treatment; or an easy-adhesion treatment using a coating agent (primer), etc., for the purpose of improving adhesion and retention with the pressure-sensitive adhesive layer. The surface treatment for improving adhesion is preferably applied to the entire surface of the substrate.

[0123] (Adhesive sheet) The thickness of the pressure-sensitive adhesive sheet is preferably 6 to 100 μm, more preferably 100 to 80 μm, and even more preferably 20 to 70 μm. When the thickness is 6 μm or more, the adhesiveness is excellent and peeling is unlikely to occur when the sheet is bent. When the thickness is 100 μm or less, the difference between the inner and outer diameters when the sheet is bent is small, and it is easy to relieve the stress applied when the sheet is bent. The thickness of the pressure-sensitive adhesive sheet refers to the thickness from the surface of the substrate on which no pressure-sensitive adhesive layer is formed to the adhesive surface in the case of a single-sided pressure-sensitive adhesive sheet, and the thickness from one adhesive surface to the other adhesive surface in the case of a double-sided pressure-sensitive adhesive sheet, i.e., the thickness of the adhesive body, and does not include the release liner.

[0124] The pressure-sensitive adhesive sheet of the present invention may have a release liner attached to the surface (adhesive surface) of the pressure-sensitive adhesive layer until use. When the pressure-sensitive adhesive sheet is a double-sided pressure-sensitive adhesive sheet, each of the adhesive surfaces on both sides of the pressure-sensitive adhesive sheet may be protected by two release liners, or may be protected by a single release liner having release surfaces on both sides in a form wound into a roll (rolled body). The release liner is used as a protective material for the pressure-sensitive adhesive layer, and is peeled off when the sheet is attached to an adherend. The release liner is not necessarily provided.

[0125] The release liner can be a conventional release paper, and is not particularly limited. Examples of the release liner include a substrate having a release treatment layer, a low-adhesion substrate made of a fluoropolymer, and a low-adhesion substrate made of a non-polar polymer. Examples of the substrate having a release treatment layer include a plastic film or paper surface-treated with a release treatment agent such as a silicone-based, long-chain alkyl-based, fluorine-based, or molybdenum sulfide. Examples of the fluorine-based polymer in the low-adhesion substrate made of a fluoropolymer include polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, tetrafluoroethylene-hexafluoropropylene copolymer, and chlorofluoroethylene-vinylidene fluoride copolymer. Examples of the non-polar polymer include an olefin-based resin (e.g., polyethylene, polypropylene, etc.). The release liner can be formed by a known or conventional method. The thickness of the release liner is also not particularly limited.

[0126] The pressure-sensitive adhesive sheet is preferably used for attaching electric and electronic components to components included in electric and electronic devices. The pressure-sensitive adhesive sheet is particularly preferably used for attaching components included in electric and electronic devices to both adhesive surfaces of the double-sided pressure-sensitive adhesive sheet, that is, for fixing components in electric and electronic devices. The double-sided pressure-sensitive adhesive sheet may be used for either fixing the components or temporarily fixing them.

[0127] The term "electrical and electronic devices" refers to devices that fall into at least one of the categories of electrical devices and electronic devices. Examples of the electrical and electronic devices include image display devices such as liquid crystal displays, electroluminescence displays, and plasma displays, as well as portable electronic devices.

[0128] Examples of the portable electronic device include mobile phones, smartphones, tablet computers, notebook computers, various wearable devices (for example, wristwear devices worn on the wrist like a wristwatch, modular devices worn on a part of the body with a clip or strap, eyewear devices including glasses (monocular and binocular devices, including head-mounted devices), clothing devices attached to shirts, socks, hats, etc. in the form of accessories, and earwear devices attached to the ears like earphones), digital cameras, digital video cameras, audio devices (portable music players, IC recorders, etc.), calculators (calculators, etc.), portable game devices, electronic dictionaries, electronic organizers, electronic books, in-vehicle information devices, portable radios, portable televisions, portable printers, portable scanners, and portable modems. In this specification, the term "portable" does not mean that the device is merely portable, but rather that the device has a level of portability that allows an individual (average adult) to carry the device relatively easily. The double-sided pressure-sensitive adhesive sheet is used, for example, so that the pressure-sensitive adhesive layer adheres to the components of the portable electronic device.

[0129] The pressure-sensitive adhesive sheet of the present invention has excellent resistance to bending in a low-temperature environment. Therefore, even when used in a location where bending is repeatedly performed in a low-temperature environment, the bending location is unlikely to be broken or marked, and the pressure-sensitive adhesive sheet is unlikely to peel off. In addition, the pressure-sensitive adhesive sheet of the present invention has excellent adhesion to an adherend in a normal temperature and high-temperature environment. Therefore, the pressure-sensitive adhesive sheet of the present invention is preferably used in a location where the sheet is repeatedly folded for use. Therefore, the pressure-sensitive adhesive sheet of the present invention is preferably used for bonding members (particularly between members) in an electric / electronic device that is used while being folded, for example, an electric / electronic device having a foldable image display device (flexible display) (particularly, a foldable image display device (foldable display)). EXAMPLES

[0130] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these examples in any way.

[0131] Preparation Example 1 (Preparation of Acrylic Polymer A) In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, a reflux condenser, and a dropping funnel, 70 parts by mass of 2-ethylhexyl acrylate (2EHA), 20 parts by mass of n-butyl acrylate (BA), 8 parts by mass of lauryl acrylate (LA), 1 part by mass of 4-hydroxybutyl acrylate (4HBA), 0.6 parts by mass of N-vinyl-2-pyrrolidone (NVP), 0.1 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a thermal polymerization initiator, and a mixture containing ethyl acetate as a polymerization solvent (solid concentration 47% by mass) were stirred at 56°C for 6 hours under a nitrogen atmosphere (polymerization reaction). As a result, a polymer solution containing acrylic polymer A was obtained. The weight average molecular weight of the acrylic polymer A in this polymer solution was about 2 million, and the glass transition temperature was -63°C.

[0132] Preparation Example 2 (Preparation of Acrylic Polymer B) In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, a reflux condenser, and a dropping funnel, 95 parts by mass of 2EHA and 5 parts by mass of AA as monomer components and 199 parts by mass of ethyl acetate as a polymerization solvent were charged, and the mixture was stirred for 2 hours while introducing nitrogen gas. After removing oxygen from the polymerization system in this manner, 0.2 parts by mass of benzoyl peroxide was added as a polymerization initiator, and the mixture was solution polymerized at 60°C for 6 hours to obtain a solution of acrylic polymer B. The Mw of this acrylic polymer B was about 120×10 4 It was.

[0133] Preparation Example 3 (Preparation of Oligomer A) 60 parts by mass of dicyclopentanyl methacrylate and 40 parts by mass of methacrylic acid as monomer components, 3.5 parts by mass of α-thioglycerol as a chain transfer agent, and 100 parts by mass of toluene as a polymerization solvent were mixed and stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by mass of AIBN was added as a thermal polymerization initiator, and the mixture was reacted at 70°C for 2 hours, and then heated to 80°C and reacted for 2 hours. Thereafter, the reaction liquid was heated to 130°C, and toluene, the chain transfer agent, and unreacted monomers were dried and removed to obtain a solid acrylic oligomer (oligomer A). The weight average molecular weight of oligomer A was 5100.

[0134] Preparation Example 4 (Preparation of Oligomer B) 95 parts by mass of cyclohexyl methacrylate as monomer components, 5 parts by mass of AA, 10 parts by mass of α-methylstyrene dimer as a chain transfer agent, 10 parts by mass of AIBN as a polymerization initiator, and 120 parts by mass of toluene as a polymerization solvent were mixed and reacted at 85° C. for 5 hours under a nitrogen atmosphere to obtain a solution of Oligomer B with a solid content concentration of 50% by mass. The weight average molecular weight of Oligomer B was 4,300.

[0135] Example 1 (Preparation of Adhesive Composition) To the solution of acrylic polymer A prepared in Preparation Example 1, 3 parts by mass of oligomer A prepared in Preparation Example 3 as a tackifier, 0.26 parts by mass of dibenzoyl peroxide (product name "Niper BMT-40SV", manufactured by NOF Corporation) as crosslinking agent A, and 0.03 parts by mass of an isocyanate-based crosslinking agent (product name "Coronate L", manufactured by Tosoh Corporation) as crosslinking agent B were added per 100 parts by mass of acrylic polymer A, and the mixture was stirred to prepare a pressure-sensitive adhesive composition.

[0136] (Preparation of adhesive sheet) The above adhesive composition was applied onto a release treatment layer of a 75 μm thick polyethylene terephthalate film (product name "Diafoil MRF", manufactured by Mitsubishi Chemical Corporation) with one side having been release-treated with silicone, so that the adhesive layer was 25 μm thick, and dried at 150°C for 3 minutes to form an adhesive layer. A release treatment layer of a 38 μm thick polyethylene terephthalate film (product name "Diafoil MRF", manufactured by Mitsubishi Chemical Corporation) with one side having been release-treated with silicone was then superimposed on the above adhesive layer to produce the double-sided adhesive sheet of Example 1.

[0137] Example 2 (Preparation of Adhesive Composition) To a solution of the acrylic polymer A prepared in Preparation Example 1, 6 parts by mass of the oligomer A prepared in Preparation Example 3 as a tackifier, 0.52 parts by mass of dibenzoyl peroxide (product name "Niper BMT-40SV", manufactured by NOF Corporation) as crosslinking agent A, and 0.05 parts by mass of an isocyanate-based crosslinking agent (product name "Coronate L", manufactured by Tosoh Corporation) as crosslinking agent B were added per 100 parts by mass of the acrylic polymer A, and the mixture was stirred to prepare a pressure-sensitive adhesive composition.

[0138] (Preparation of adhesive sheet) A double-sided PSA sheet of Example 2 was produced in the same manner as in Example 1, except that the above PSA composition was used.

[0139] Example 3 A pressure-sensitive adhesive composition and a double-sided pressure-sensitive adhesive sheet were prepared in the same manner as in Example 2, except that 20 parts by mass of Oligomer B prepared in Preparation Example 4 was used as the tackifier.

[0140] Example 4 A pressure-sensitive adhesive composition and a double-sided pressure-sensitive adhesive sheet were prepared in the same manner as in Example 2, except that 6 parts by mass of Oligomer A and 6 parts by mass of Oligomer B were used as tackifiers.

[0141] Example 5 A pressure-sensitive adhesive composition and a double-sided pressure-sensitive adhesive sheet were prepared in the same manner as in Example 2, except that 6 parts by mass of Oligomer A and 15 parts by mass of Oligomer B were used as the tackifier.

[0142] Example 6 An adhesive composition and a double-sided adhesive sheet were prepared in the same manner as in Example 2, except that 20 parts by mass of tackifier resin B (product name "PENSEL D-125", rosin ester, manufactured by Arakawa Chemical Industries, Ltd., softening point approximately 125°C) was used as the tackifier.

[0143] Example 7 An adhesive composition and a double-sided adhesive sheet were prepared in the same manner as in Example 2, except that 10 parts by mass of oligomer A and 10 parts by mass of tackifier resin A (product name "YS Polystar S145", terpene phenol resin, manufactured by Yasuhara Chemical Co., Ltd., softening point approximately 145°C) were used as tackifiers.

[0144] Example 8 (Preparation of Adhesive Composition) To the solution of acrylic polymer A prepared in Preparation Example 1, 10 parts by mass of oligomer B as a tackifier and 0.2 parts by mass of an isocyanate-based crosslinking agent (product name "Coronate L", manufactured by Tosoh Corporation) as crosslinking agent B were added per 100 parts by mass of acrylic polymer A, and the mixture was stirred to prepare a pressure-sensitive adhesive composition.

[0145] (Preparation of adhesive sheet) A double-sided PSA sheet of Example 8 was produced in the same manner as in Example 1, except that the above PSA composition was used.

[0146] Comparative Example 1 A pressure-sensitive adhesive composition and a double-sided pressure-sensitive adhesive sheet were prepared in the same manner as in Example 1, except that no tackifier was added.

[0147] Comparative Example 2 (Preparation of Adhesive Composition) To the solution of acrylic polymer A prepared in Preparation Example 1, 30 parts by mass of tackifier resin B (product name "PENSEL D-125", rosin ester, manufactured by Arakawa Chemical Industries, Ltd., softening point approximately 125°C) as a tackifier, 0.78 parts by mass of dibenzoyl peroxide (product name "NIPER BMT-40SV", manufactured by NOF Corporation) as crosslinking agent A, and 0.1 part by mass of an isocyanate-based crosslinking agent (product name "CORONATE L", manufactured by Tosoh Corporation) as crosslinking agent B were added per 100 parts by mass of acrylic polymer A, and the mixture was stirred and mixed to prepare a pressure-sensitive adhesive composition.

[0148] (Preparation of adhesive sheet) A double-sided PSA sheet of Comparative Example 2 was produced in the same manner as in Example 1, except that the above PSA composition was used.

[0149] Comparative Example 3 (Preparation of Adhesive Composition) To the solution of acrylic polymer B prepared in Preparation Example 2, 10 parts by mass of tackifier resin A (product name "YS Polystar S145", terpene phenol resin, manufactured by Yasuhara Chemical Co., Ltd., softening point approximately 145°C) as a tackifier, 3 parts by mass of an isocyanate-based crosslinking agent (product name "Coronate L", manufactured by Tosoh Corporation) as crosslinking agent B, and 0.03 parts by mass of an epoxy-based crosslinking agent (product name "TETRAD-C", manufactured by Mitsubishi Gas Chemical Co., Inc.) as crosslinking agent C were added per 100 parts by mass of acrylic polymer B, and the mixture was stirred to prepare a pressure-sensitive adhesive composition.

[0150] (Preparation of adhesive sheet) The above adhesive composition was applied onto a release treatment layer of a 75 μm thick polyethylene terephthalate film (product name "Diafoil MRF", manufactured by Mitsubishi Chemical Corporation) with one side having been release-treated with silicone, so that the adhesive layer was 25 μm thick, and dried at 100°C for 2 minutes to form an adhesive layer. A release treatment layer of a 38 μm thick polyethylene terephthalate film (product name "Diafoil MRF", manufactured by Mitsubishi Chemical Corporation) with one side having been release-treated with silicone was then superimposed on the above adhesive layer to produce the double-sided adhesive sheet of Example 1.

[0151] Comparative Example 4 (Preparation of Adhesive Composition) To the solution of acrylic polymer A prepared in Preparation Example 1, 20 parts by mass of tackifier resin B (product name "PENSEL D-125", rosin ester, manufactured by Arakawa Chemical Industries, Ltd., softening point approximately 125°C) as a tackifier, 0.26 parts by mass of dibenzoyl peroxide (product name "NIPER BMT-40SV", manufactured by NOF Corporation) as crosslinking agent A, and 0.05 parts by mass of an isocyanate-based crosslinking agent (product name "CORONATE L", manufactured by Tosoh Corporation) as crosslinking agent B were added per 100 parts by mass of acrylic polymer A, and the mixture was stirred and mixed to prepare a pressure-sensitive adhesive composition.

[0152] (Preparation of adhesive sheet) A double-sided PSA sheet of Comparative Example 4 was produced in the same manner as in Example 1, except that the above PSA composition was used.

[0153] <Evaluation> The pressure-sensitive adhesive sheets obtained in the Examples and Comparative Examples were subjected to the following evaluations, and the results are shown in the Table.

[0154] (1) Storage modulus G' (-30°C) The release liners on both sides were peeled off from the double-sided PSA sheets produced in the Examples and Comparative Examples, and the double-sided PSA sheets were laminated to produce test samples with a thickness of approximately 1 mm. These test samples were punched out into disks with a diameter of 7.9 mm, sandwiched between parallel plates, and viscoelasticity was measured in shear mode at a temperature range of -50 to 150°C and a heating rate of 5°C / min using a viscoelasticity tester (product name "ARES", manufactured by Rheometrics Co., Ltd.) while applying a shear strain of 1 Hz, and the peak top strength of G' (dynamic shear storage modulus) at -30°C was determined.

[0155] (2) Gel fraction About 0.2 g of adhesive was scraped off from the adhesive sheet, wrapped in a porous polytetrafluoroethylene membrane (trade name "NTF-1122", manufactured by Nitto Denko Corporation) with a pore diameter of 0.2 μm cut into a size of 100 mm × 100 mm, and the opening of the wrapping was tied with a string. The mass of the adhesive sample (B) was calculated by subtracting the total mass (A) of the porous polytetrafluoroethylene membrane and the string measured in advance from the mass of this sample. The adhesive sample wrapped in the porous polytetrafluoroethylene membrane was immersed in about 50 mL of ethyl acetate at 23 ° C. for 7 days, and the sol component of the adhesive was eluted outside the porous polytetrafluoroethylene membrane. After immersion, the adhesive wrapped in the porous polytetrafluoroethylene membrane was taken out, dried at 130 ° C. for 2 hours, and allowed to cool for about 20 minutes, and then the dry mass (C) was measured. The gel fraction of the adhesive was calculated by the following formula. Gel fraction (%) = 100 × (CA) / B

[0156] (3) 180° peel adhesion (RT) In a measurement environment of 23°C and 50% RH, the release liners on both sides were peeled off from the double-sided pressure-sensitive adhesive sheets prepared in the examples and comparative examples, and a PET film having a thickness of 25 μm was attached to one of the adhesive surfaces of the double-sided pressure-sensitive adhesive sheets to provide a backing, and the sheets were cut to a size of 20 mm wide and 100 mm long to prepare a measurement sample. In an environment of 23°C and 50% RH, the exposed adhesive surface of the measurement sample was pressed against the surface of a stainless steel plate (SUS304BA plate) by rolling a 2 kg roller back and forth once. After leaving the sample in the same environment for 24 hours, a universal tensile compression tester was used to measure the 180° peel strength (adhesive strength) [N / 20 mm] under the conditions of a tensile speed of 300 mm / min, a peel angle of 180°, a temperature of 23°C, and a relative humidity of 50% RH (room temperature). A universal tensile compression tester (product name "TG-1kN") manufactured by Minebea Co., Ltd. was used as the universal tensile compression tester. In the case of a single-sided pressure-sensitive adhesive sheet, the above-mentioned PET film backing is not necessary.

[0157] (4) Bending resistance test In an environment of -30°C / 50%RH, one release liner was peeled off from the double-sided pressure-sensitive adhesive sheet produced in the examples and comparative examples, and the exposed adhesive surface was attached to one side of a polyethylene terephthalate film (thickness: 50 μm, Young's modulus: 4.5 GPa). Next, the other release liner was peeled off, and the exposed adhesive surface was attached to one side of another polyethylene terephthalate film (thickness: 50 μm, Young's modulus: 4.5 GPa). Then, after pressurizing at 0.5 MPa and 50°C for 20 minutes in an autoclave manufactured by Kurihara Seisakusho Co., Ltd., the laminate was left for 24 hours under conditions of 23°C and 50%RH. The laminate consisting of [PET film / double-sided pressure-sensitive adhesive sheet / PET film] thus obtained was cut into a width of 20 mm and a length of 200 mm, which was used as a sample. The obtained sample was repeatedly bent under the following conditions using a durability tester (product name: Planar body unloaded U-shaped stretch environmental tester CL09-TypeD01-FSC90, manufactured by Yuasa System Devices Co., Ltd.) After the test at -30°C / 50% RH, the bent portion of the sample was visually checked for the presence or absence of creases (bending resistance (low temperature)), and the bending resistance was evaluated according to the following criteria. <Test conditions> Bending radius: 2mm, bending count: 200,000 times, bending speed: 60 times / min <Evaluation criteria> ◯: No creases or slight creases were observed but were at a level sufficient for practical use. △: Folds were visible when held up to light, but were still usable for practical purposes. ×: Breaking occurred to such an extent that practical use was not possible.

[0158] (5) High temperature holding power In a measurement environment of 23°C and 50% RH, the double-sided pressure-sensitive adhesive sheets prepared in the examples and comparative examples were cut into a size of 10 mm x 20 mm so that no glue would come out, and the release liner on the light release side (a 38 μm thick polyethylene terephthalate film with one side treated with silicone for release) was peeled off, and a 25 μm thick PET film was attached and backed. Then, the release liner on the heavy release side was peeled off and attached to a stainless steel plate (SUS304BA plate), and a 2 kg roller was moved back and forth at a speed of 5 mm / sec to press the sheet, and this was left in an 80°C atmosphere for 30 minutes. After that, the sheet was taken out of the measurement environment of 23°C and 50% RH, and the distance of the deviation that occurred between the PET film and the stainless steel plate (SUS304BA plate) from the starting point was measured. Then, the high temperature retention was evaluated according to the following evaluation criteria. <Evaluation criteria> 〇: No peeling ×: Peeled off

[0159] [Table 1]

[0160] Variations of the invention according to the present disclosure are described below. [Appendix 1] An adhesive sheet having an adhesive layer, The pressure-sensitive adhesive layer comprises an acrylic polymer including, as a constituent unit, a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms, and a tackifier; The pressure-sensitive adhesive sheet, wherein the pressure-sensitive adhesive layer has a modulus of elasticity of 5.0 MPa or less at -30°C and a gel fraction of 50% or more. [Appendix 2] The pressure-sensitive adhesive sheet according to appendix 1, wherein the acrylic polymer contains, as a constituent unit, a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 8 carbon atoms. [Appendix 3] The pressure-sensitive adhesive sheet according to appendix 1 or 2, wherein the tackifier comprises an oligomer or a tackifier resin. [Appendix 4] The pressure-sensitive adhesive sheet according to any one of Appendices 1 to 3, which is a double-sided pressure-sensitive adhesive sheet for fixing components together in an electric / electronic device. [Appendix 5] Equipped with the adhesive sheet according to Appendix 4, The adhesive sheet fixes components together using both adhesive surfaces of the adhesive sheet, in an electrical / electronic device. [Explanation of symbols]

[0161] 1 double-sided adhesive sheet 2 Adhesive layer 3,4 Release Liner

Claims

1. A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer, The pressure-sensitive adhesive layer comprises an acrylic polymer including, as a constituent unit, a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms, and a tackifier; The pressure-sensitive adhesive layer has an elastic modulus of 5.0 MPa or less at −30° C. and a gel fraction of 50% or more.

2. 2. The pressure-sensitive adhesive sheet according to claim 1, wherein the acrylic polymer contains, as a constituent unit, a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 8 carbon atoms.

3. The pressure-sensitive adhesive sheet according to claim 1 or 2, wherein the tackifier comprises an oligomer or a tackifier resin.

4. 3. The pressure-sensitive adhesive sheet according to claim 1, which is a double-sided pressure-sensitive adhesive sheet for fixing components together in an electric / electronic device.

5. The adhesive sheet according to claim 4, The adhesive sheet fixes components together using both adhesive surfaces of the adhesive sheet, in an electrical / electronic device.

Citation Information

Patent Citations

  • Adhesive agent layer for flexible image display device, laminate body for flexible image display device, and flexible image display device

    JP2019218513A

  • Low dielectric constant optically clear adhesives for flexible electronic displays

    JP2020513451A

  • Techniques for signaling multiple audio mixing gains for teleconferencing and telepresence for remote terminals

    JP2023525481A

  • Adhesive sheet roll and adhesive sheet

    JP2024093607A

  • Pressure-sensitive adhesive composition

    WO2022220498A1