Powder for lamination molding and lamination molded body
The use of amino group-containing coupling agent-coated particles in additive manufacturing powder facilitates faster and lower-temperature curing of epoxy resin, enhancing productivity and quality of laminate-molded bodies.
Patent Information
- Application Number
- JP2023051104
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
The existing powder for additive manufacturing using a binder containing epoxy resin requires high temperature and long time for binder solidification, leading to decreased productivity and potential deformation of the laminate-molded body.
A powder for additive manufacturing with shaping particles coated by a compound derived from a coupling agent having an amino group, which promotes faster curing of the epoxy resin at lower temperatures.
Enables the production of additively manufactured objects with high dimensional accuracy and increased mechanical strength by curing the epoxy resin at lower temperatures and in shorter times, reducing deformation and curing defects.
Smart Images

Figure 2024140106000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a powder for additive manufacturing and an additive manufactured product. [Background technology]
[0002] In recent years, additive manufacturing using metal powder has become popular as a technique for forming three-dimensional objects. This technique involves the steps of calculating the cross-sectional shape of the three-dimensional object when it is thinly sliced along a plane perpendicular to the lamination direction, forming powder layers by smoothing the metal powder into layers, and bonding parts of the powder layers based on the shape calculated. The three-dimensional object is formed by repeating the steps of forming the powder layers and bonding parts.
[0003] Known additive manufacturing methods include fused deposition modeling (FDM), selective laser sintering (SLS), binder jetting, and the like, depending on the bonding principle.
[0004] Patent Document 1 discloses a powder for additive manufacturing used to form an additive manufacturing body by a binder jetting method, the powder for additive manufacturing comprising a metal powder and a coating provided on the particle surface of the metal powder and containing a compound derived from a coupling agent having a functional group. Patent Document 1 also discloses that the average particle size of the powder for additive manufacturing is 3.0 μm or more and 30.0 μm or less, and that the functional group contains a cyclic structure-containing group, a fluoroalkyl group, or a fluoroaryl group.
[0005] Patent Document 1 also discloses that after forming a powder layer using the above-mentioned powder for additive manufacturing, a binder solution is supplied to a desired area, and then the powder layer is heated, thereby solidifying or curing the binder and bonding the particles in the desired area together. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2022-122503 Summary of the Invention [Problem to be solved by the invention]
[0007] However, the powder for additive manufacturing described in Patent Document 1 has a problem in that it takes a long time and high temperature to solidify or harden the binder. In particular, when the binder contains an epoxy resin, the hardening speed is slow. When it takes a long time to harden the binder, the productivity of the additive manufacturing object decreases. In addition, when a high temperature is required, the additive manufacturing object is easily deformed as it is heated.
[0008] Therefore, the challenge is to develop a powder for additive manufacturing that can produce additive objects at a lower temperature or in a shorter time, even when used in an additive manufacturing method that uses a binder containing an epoxy resin. [Means for solving the problem]
[0009] The powder for additive manufacturing according to the application example of the present invention is A powder for additive manufacturing used to manufacture an additive manufacturing body that becomes a metal sintered body by a binder jet method, Particles for shaping containing a metal material; a coating film provided on a surface of the particle for shaping, the coating film containing a compound derived from a coupling agent having an amino group; Equipped with.
[0010] The layered object according to the application example of the present invention is Powder for additive manufacturing according to an application example of the present invention; a binder that binds particles of the powder for additive manufacturing together and contains an epoxy resin; has. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a process diagram illustrating a method for manufacturing a layered object. [Diagram 2] FIG. 2 is a diagram for explaining a method for producing the layered object shown in FIG. [Diagram 3] FIG. 2 is a diagram for explaining a method for producing the layered object shown in FIG. [Figure 4] FIG. 2 is a diagram for explaining a method for producing the layered object shown in FIG. [Diagram 5] FIG. 2 is a diagram for explaining a method for producing the layered object shown in FIG. [Figure 6] FIG. 2 is a diagram for explaining a method for producing the layered object shown in FIG. [Figure 7] FIG. 2 is a diagram for explaining a method for producing the layered object shown in FIG. [Figure 8] FIG. 2 is a diagram for explaining a method for producing the layered object shown in FIG. [Figure 9] FIG. 2 is a diagram for explaining a method for producing the layered object shown in FIG. [Figure 10] FIG. 2 is a diagram for explaining a method for producing the layered object shown in FIG. [Figure 11] FIG. 1 is a cross-sectional view illustrating a powder for additive manufacturing according to an embodiment. [Figure 12] FIG. 12 is a process diagram showing an example of a method for producing the powder for layered manufacturing shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, preferred embodiments of the powder for layered manufacturing and the layered manufactured body of the present invention will be described in detail with reference to the accompanying drawings.
[0013] 1. Manufacturing method for additive manufacturing First, a method for manufacturing an additive manufacturing object using a powder for additive manufacturing will be described.
[0014] FIG. 1 is a process diagram for explaining a method for manufacturing a layered object. FIGS. 2 to 10 are diagrams for explaining a method for manufacturing the layered object shown in FIG. 1. In each diagram of the present application, an X-axis, a Y-axis, and a Z-axis are set as three mutually orthogonal axes. Each axis is represented by an arrow, with the tip side being the "plus side" and the base side being the "minus side". In the following description, the plus side of the Z-axis is particularly referred to as "up" and the minus side of the Z-axis is particularly referred to as "down". In addition, both directions parallel to the X-axis are referred to as X-axis directions, both directions parallel to the Y-axis are referred to as Y-axis directions, and both directions parallel to the Z-axis are referred to as Z-axis directions.
[0015] 1 to 10 is a method called the binder jet method, which is one type of additive manufacturing method, and includes a powder layer forming step S102, a binder solution supplying step S104, and a repeating step S106, as shown in Fig. 1. The binder jet method has the advantage that it is possible to produce additive objects with complex shapes because it does not require a support structure to support the object.
[0016] In the powder layer forming step S102, as shown in Fig. 3, powder 1 for additive manufacturing is spread to form a powder layer 31. In the binder solution supplying step S104, a binder solution 4 is supplied to a predetermined region of the powder layer 31 to bond the particles in the powder layer 31 together, thereby obtaining a bonded layer 41. In the repeating step S106, the powder layer forming step S102 and the binder solution supplying step S104 are repeated one or more times to obtain an additive manufacturing body 6 shown in Fig. 10. Each step will be described in order below.
[0017] The produced layered product 6 is subjected to a sintering process to become a metal sintered body. The shape of the layered product is reflected in the obtained metal sintered body, so that a metal sintered body having a complex shape can be efficiently produced.
[0018] 1.1.Additive manufacturing equipment First, prior to describing the powder layer forming step S102, the layered manufacturing apparatus 2 will be described.
[0019] The additive manufacturing device 2 comprises an apparatus main body 21 having a powder storage section 211 and a modeling section 212, a powder supply elevator 22 provided in the powder storage section 211, a modeling stage 23 provided in the modeling section 212, and a coater 24, a roller 25 and a liquid supply section 26 movably arranged on the apparatus main body 21.
[0020] The powder storage section 211 is provided in the device body 21 and is a recess with an open top. The powder 1 for layered manufacturing is stored in the powder storage section 211. An appropriate amount of the powder 1 for layered manufacturing stored in the powder storage section 211 is supplied to the modeling section 212 by the coater 24.
[0021] A powder supply elevator 22 is disposed at the bottom of the powder storage section 211. The powder supply elevator 22 is capable of moving up and down with the powder 1 for additive manufacturing placed on it. By moving the powder supply elevator 22 upward, the powder 1 for additive manufacturing placed on the powder supply elevator 22 is pushed up and caused to overflow from the powder storage section 211. This allows the overflowing powder 1 for additive manufacturing to be moved toward the modeling section 212.
[0022] The modeling section 212 is provided in the device body 21, and is a recess with an open top. A modeling stage 23 is disposed inside the modeling section 212. The powder 1 for additive manufacturing is spread in layers on the modeling stage 23 by a coater 24. The modeling stage 23 is movable in the up and down direction with the powder 1 for additive manufacturing spread thereon. The amount of the powder 1 for additive manufacturing spread on the modeling stage 23 can be adjusted by appropriately setting the height of the modeling stage 23.
[0023] The coater 24 and roller 25 are movable in the X-axis direction from the powder storage section 211 to the modeling section 212. The coater 24 drags the powder 1 for additive manufacturing, thereby leveling the powder 1 for additive manufacturing and spreading it in layers. The roller 25 compresses the leveled powder 1 for additive manufacturing from above.
[0024] The liquid supply unit 26 is composed of, for example, an inkjet head or a dispenser, and is movable in the X-axis direction and the Y-axis direction in the modeling unit 212. The liquid supply unit 26 can supply a desired amount of the binder solution 4 to a desired position. The liquid supply unit 26 may have a single head equipped with a plurality of discharge nozzles. The binder solution 4 may be discharged from the plurality of discharge nozzles simultaneously or with a time lag.
[0025] 1.2. Powder layer formation process Next, the powder layer forming step S102 using the above-mentioned additive manufacturing apparatus 2 will be described. In the powder layer forming step S102, the additive manufacturing powder 1 is spread on the modeling stage 23 to form a powder layer 31. Specifically, as shown in Figs. 2 and 3, the additive manufacturing powder 1 stored in the powder storage section 211 is dragged onto the modeling stage 23 using a coater 24 and leveled to a uniform thickness. This results in the powder layer 31 shown in Fig. 4. At this time, the upper surface of the modeling stage 23 is lowered below the upper end of the modeling section 212, and the thickness of the powder layer 31 can be adjusted by adjusting the amount of lowering.
[0026] Next, while compressing the powder layer 31 in the thickness direction with the roller 25, the roller 25 is moved in the X-axis direction as shown in Fig. 4. This makes it possible to increase the filling rate of the powder 1 for layered manufacturing in the powder layer 31. Note that the compression with the roller 25 may be performed as necessary and may be omitted. Also, the powder layer 31 may be compressed by a means other than the roller 25, such as a pressing plate.
[0027] 1.3. Binder solution supply process In the binder solution supplying step S104, as shown in Fig. 5, the liquid supply unit 26 supplies the binder solution 4 to a formation region 60 of the powder layer 31 that corresponds to the layered model 6 to be formed. The binder solution 4 is a liquid containing a binder and a solvent or a dispersion medium. In the formation region 60 to which the binder solution 4 is supplied, a binding layer 41 shown in Fig. 6 is obtained. In the binding layer 41, the particles of the powder 1 for layered modeling are bound together by the binder, and the binding layer 41 has a shape retention that is sufficient to prevent it from breaking under its own weight.
[0028] The binder layer 41 may be heated simultaneously with or after the supply of the binder solution 4. This promotes the evaporation of the solvent or dispersion medium contained in the binder solution 4 and promotes the binding of particles together due to the hardening of the binder. When the binder contains a photocurable resin or an ultraviolet-curable resin, light irradiation or ultraviolet irradiation may be performed instead of or in addition to heating.
[0029] The heating temperature in the case of heating is not particularly limited, but is preferably from 50° C. to 250° C., and more preferably from 70° C. to 200° C. This allows a sufficient amount of heat to be applied to the binder layer 41, and can sufficiently promote the volatilization of the solvent or dispersion medium.
[0030] There is no particular limitation on the binder solution 4 as long as it is a liquid containing an epoxy resin. Examples of the solvent or dispersion medium contained in the binder solution 4 include water, alcohols, ketones, carboxylates, etc., and a mixed liquid containing at least one of these is used.
[0031] There are no particular limitations on the epoxy resin, and various types can be used as long as the epoxy resin is a compound containing one or more epoxy groups in the molecule.
[0032] Specific examples include bisphenol polyglycidyl ether type epoxy resins such as bisphenol A type epoxy resin, bisphenol B type epoxy resin, bisphenol C type epoxy resin, bisphenol E type epoxy resin, bisphenol F type epoxy resin, bisphenol AD type epoxy resin, and bisphenol S type epoxy resin; hydrogenated bisphenol type diglycidyl ethers obtained by hydrogenating the above bisphenol polyglycidyl ether type epoxy resins, glycidyl ester type epoxy resins, glycidylamine type epoxy resins, ethylene glycol diglycidyl ether, 1,3-propylene glycol diglycidyl ether, 1,2-propylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, 1,8-octanediol diglycidyl ether, 1,10-decanediol diglycidyl ether, 2,2-dimethyl-1,3-propanediol diglycidyl ether, diethylene glycol diglycidyl ether, triethylene glycol diglycidyl ether, tetraethylene glycol diglycidyl ether, and the like. diglycidyl ether, hexaethylene glycol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, 1,1,1-tri(glycidyloxymethyl)propane, 1,1,1-tri(glycidyloxymethyl)ethane, 1,1,1-tri(glycidyloxymethyl)methane, 1,1,1,1-tetra(glycidyloxymethyl)methane, glycerin triglycidyl ether, trimethylolpropane triglycidyl ether, sorbitol tetraglycidyl ether, dipentaerythritol hexaglycidyl ether, etc. glycidyl ethers of aliphatic polyhydric alcohols; polyglycidyl ethers of polyether polyols obtained by adding two or more alkylene oxides to polyhydric alcohols such as propylene glycol, trimethylolpropane, and glycerin; novolac type epoxy compounds such as phenol novolac type epoxy resins, alkyl novolac type epoxy resins, biphenyl novolac type epoxy compounds, cresol novolac type epoxy compounds, bisphenol A novolac type epoxy compounds, and dicyclopentadiene novolac type epoxy compounds;Naphthalene type epoxy resin, dicyclopentadiene type epoxy resin, biphenyl type epoxy resin, anthracene type epoxy resin, 3,4-epoxy-3-methylcyclohexylmethyl-3,4-epoxy-3-methylcyclohexane carboxylate, 3,4-epoxy-5-methylcyclohexylmethyl-3,4-epoxy-5-methylcyclohexane carboxylate, 3,4-epoxy-6-methylcyclohexylmethyl-3,4-epoxy-6-methylcyclohexane carboxylate, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexane carboxylate, 1-epoxyethyl-3,4-epoxycyclohexane, bis(3,4-epoxycyclohexylmethyl)adipate, methylene bis(3,4-epoxycyclohexane), isopropylidene bis(3,4-epoxycyclohexane), dicyclopentadiene diepoxide, ethylene bis(3 ,4-epoxycyclohexanecarboxylate), 1,2-epoxy-2-epoxyethylcyclohexane, and other alicyclic epoxy compounds; glycidyl esters of dibasic acids, such as diglycidyl ester of phthalic acid, diglycidyl ester of tetrahydrophthalic acid, and glycidyl ester of dimer acid; fluorinated epoxy resins, brominated epoxy resins, rubber-modified epoxy resins containing polybutadiene or NBR, flame-retardant epoxy resins, such as glycidyl ether of tetrabromobisphenol A, p-oxybenzoic acid glycidyl ether ester type epoxy resins, m-aminophenol type epoxy resins, diaminodiphenylmethane-based epoxy resins, urethane-modified epoxy resins having a urethane bond, various alicyclic epoxy resins, epoxidized products of unsaturated polymers, such as N,N-diglycidylaniline, N,N-diglycidyl-o-toluidine, hydantoin type epoxy resins, and petroleum resins;
[0033] The epoxy resin is not limited to these, and any commonly used epoxy resin may be used. These epoxy resins may be used alone or in combination of two or more.
[0034] In addition, the epoxy resin is preferably a compound containing two or more epoxy groups in the molecule. This makes it easier for the cured product of the epoxy resin to form a three-dimensional network. As a result, the mechanical strength of the layered product 6 containing the cured product can be further increased.
[0035] The binder solution 4 may contain a resin component other than the epoxy resin. Examples of such resin components include fatty acids, paraffin wax, microwax, polyethylene, polypropylene, polystyrene, acrylic resins, polyamide resins, polyesters, stearic acid, polyvinylpyrrolidone (PVP), polyvinyl alcohol (PVA), polyethylene glycol (PEG), urethane resins, vinyl resins, unsaturated polyester resins, and phenolic resins. The amount of these resin components added is preferably less than that of the epoxy resin in terms of mass ratio.
[0036] 1.4.Repetitive process In the repeating step S106, the powder layer forming step S102 and the binder solution supplying step S104 are repeated one or more times until the laminate formed by laminating a plurality of binder layers 41 has a predetermined shape. In other words, these steps are performed two or more times in total. In this way, a three-dimensional layered object 6 shown in FIG. 10 is obtained.
[0037] Specifically, first, a new powder layer 31 is formed on the binder layer 41 shown in Fig. 6, as shown in Fig. 7. Next, a binder solution 4 is supplied to a formation region 60 of the newly formed powder layer 31, as shown in Fig. 8. This results in the binder layer 41 shown in Fig. 9. By repeating these operations, a layered object 6 shown in Fig. 10 is obtained.
[0038] In addition, the powder 1 for layered manufacturing that does not form the binder layer 41 in the powder layer 31 is collected and reused as necessary, that is, it is provided again for manufacturing the layered object 6. The layered product 6 obtained in the above manner is subjected to a sintering process, which will be described later.
[0039] 1.5. Manufacturing method of metal sintered body A metal sintered body is obtained by subjecting the layered molded body 6 to a sintering treatment. In the sintering treatment, the layered molded body 6 is heated to cause a sintering reaction.
[0040] The sintering temperature varies depending on the constituent materials and particle size of the powder 1 for additive manufacturing, but is preferably 980° C. to 1330° C., and more preferably 1050° C. to 1260° C., for example. The sintering time is preferably 0.2 hours to 7 hours, and more preferably 1 hour to 6 hours.
[0041] The atmosphere for the sintering treatment may be, for example, a reducing atmosphere such as hydrogen, an inert atmosphere such as nitrogen or argon, or a reduced pressure atmosphere obtained by reducing the pressure of these atmospheres, etc. The pressure of the reduced pressure atmosphere is not particularly limited as long as it is less than normal pressure (100 kPa), but is preferably 10 kPa or less, and more preferably 1 kPa or less.
[0042] When the sintering process performed under the above conditions is referred to as "main sintering", the layered product 6 may be subjected to "pre-sintering" or "degreasing" as a pre-treatment for the main sintering, if necessary. This makes it possible to remove at least a part of the binder contained in the layered product 6, or to cause a sintering reaction in a part of it. This makes it possible to suppress unintended deformation, etc., when performing the main sintering.
[0043] The temperature of the preliminary sintering or degreasing is not particularly limited as long as it is a temperature that does not complete sintering of the metal powder, but is preferably 100° C. or more and 500° C. or less, and more preferably 150° C. or more and 300° C. or less. The time of the preliminary sintering or degreasing is preferably 5 minutes or more, more preferably 10 minutes or more and 120 minutes or less, and even more preferably 20 minutes or more and 60 minutes or less, within the above temperature range. The atmosphere for the preliminary sintering or degreasing may be, for example, an air atmosphere, an inert atmosphere such as nitrogen or argon, or a reduced pressure atmosphere obtained by reducing the pressure of these atmospheres.
[0044] The metal sintered body obtained as described above can be used as a material for constituting the whole or part of, for example, automobile parts, bicycle parts, railroad vehicle parts, ship parts, aircraft parts, and space transport parts, electronic device parts such as personal computer parts, mobile phone terminal parts, tablet terminal parts, and wearable terminal parts, electrical device parts such as refrigerators, washing machines, and air conditioners, machine parts such as machine tools and semiconductor manufacturing equipment, plant parts such as nuclear power plants, thermal power plants, hydroelectric power plants, refineries, and chemical complexes, watch parts, metal tableware, jewelry, and decorative items such as eyeglass frames.
[0045] 2. Powder for additive manufacturing Next, the powder for additive manufacturing according to the embodiment will be described. FIG. 11 is a cross-sectional view that illustrates a powder for additive manufacturing according to an embodiment.
[0046] The powder for additive manufacturing 1 according to this embodiment is a powder used in a binder jet method.
[0047] The powder for additive manufacturing 1 shown in Fig. 11 has a plurality of surface-coated particles 13 including a particle for manufacturing 11 containing a metal material and a coating 12 covering the surface of the particle for manufacturing 11. The coating 12 contains a compound derived from a coupling agent having an amino group. Note that the coating 12 preferably covers the entire surface of the particle for manufacturing 11, but may have some uncovered portions.
[0048] 2.1. Particles for modeling The metallic material contained in the shaping particles 11 is not particularly limited and may be any material that has sinterability. Examples include Fe, Ni, Co, Ti, and the like, or alloys and intermetallic compounds containing these as main components.
[0049] An Fe-based metal material is preferably used as the metal material contained in the shaping particles 11. An Fe-based metal material refers to a metal material having an Fe content of more than 50% in terms of atomic ratio. An Fe-based metal material is easy to obtain and can be used to produce a metal sintered body with excellent mechanical properties.
[0050] Examples of Fe-based metallic materials include stainless steels such as ferritic stainless steel, austenitic stainless steel, martensitic stainless steel, precipitation hardened stainless steel, and austenitic-ferritic (duplex) stainless steel, as well as low carbon steel, carbon steel, heat resistant steel, die steel, high speed tool steel, Fe-Ni alloys, and Fe-Ni-Co alloys.
[0051] Among these, stainless steel is preferably used as the Fe-based metal material. Stainless steel is a type of steel that is excellent in mechanical strength and corrosion resistance. Therefore, by using the powder 1 for additive manufacturing made of stainless steel, it is possible to efficiently manufacture a metal sintered body that is excellent in mechanical strength and corrosion resistance and has high shape accuracy.
[0052] Examples of austenitic stainless steels include SUS301, SUS301L, SUS301J1, SUS302B, SUS303, SUS304, SUS304Cu, SUS304L, SUS304N1, SUS304N2, SUS304LN, SUS304J1, SUS304J2, SUS305, SUS309S, SUS310S, SUS312L, SUS315J1, SUS315J2, SUS316, SUS316L, SUS316N, SUS316LN, SUS316Ti, SUS316J1, SUS316J1L, SUS317, SUS317L, SUS317LN, SUS317J1, SUS317J2, SUS836L, SUS890L, SUS321, SUS347, SUSXM7, and SUSXM15J1.
[0053] Examples of ferritic stainless steels include SUS405, SUS410L, SUS429, SUS430, SUS430LX, SUS430J1L, SUS434, SUS436L, SUS436J1L, SUS445J1, SUS445J2, SUS444, SUS447J1, and SUSXM27.
[0054] Examples of martensitic stainless steel include SUS403, SUS410, SUS410S, SUS420J1, SUS420J2, and SUS440A.
[0055] Examples of precipitation hardening stainless steel include SUS630 and SUS631.
[0056] Examples of austenitic-ferritic (duplex) stainless steels include SUS329J1, SUS329J3L, and SUS329J4L.
[0057] The above symbols are material symbols based on the JIS standard. In this specification, the types of stainless steel are distinguished by the above material symbols.
[0058] The additive manufacturing body 6 may be manufactured using powders for additive manufacturing 1 that contain different types of stainless steel. The additive manufacturing body 6 may be divided into two parts, with one part being manufactured using powder for additive manufacturing 1 that contains a first stainless steel, and the other part being manufactured using powder for additive manufacturing 1 that contains a second stainless steel.
[0059] 2.2.Coating The coating 12 is formed by reacting a coupling agent having an amino group with the surface of the shaping particles 11. Therefore, the coating 12 contains a compound derived from the coupling agent having an amino group, and exhibits properties derived from the amino group.
[0060] When the amino group derived from the coupling agent is applied to the coating 12, when the powder for additive manufacturing 1 and the epoxy resin come into contact with each other, the amino group acts as a curing agent that cures the epoxy resin. Therefore, when an uncured epoxy resin, that is, a binder for additive manufacturing containing a monomer containing an epoxy group, is supplied to the powder layer 31 composed of the powder for additive manufacturing 1, the curing of the epoxy resin is promoted. This allows the binder to be cured at a lower temperature or in a shorter time. As a result, the deformation of the additive manufacturing body 6 produced due to heat or the passage of time can be suppressed, and an additive manufacturing body 6 with high dimensional accuracy can be produced. In addition, since poor curing is less likely to occur, the mechanical strength of the additive manufacturing body 6 can also be increased.
[0061] Examples of the amino group include a functional group containing a primary amine, a functional group containing a secondary amine, a functional group containing a tertiary amine, etc. The coupling agent may have two or more kinds of these amino groups.
[0062] Of these, the amino group preferably contains a primary amine or a secondary amine, and more preferably contains a primary amine, which has high reactivity and allows the binder to be cured at an even lower temperature or in an even shorter time.
[0063] Furthermore, coupling agents having amino groups have a relatively low critical surface tension. The lower the critical surface tension, the higher the hydrophobicity. Therefore, the coating 12 containing a compound derived from a coupling agent having an amino group has a relatively high hydrophobicity. This provides the powder 1 for additive manufacturing with excellent fluidity even in a humid environment.
[0064] The average thickness of the coating 12 is not particularly limited, but is preferably 100 nm or less, more preferably 0.5 nm to 50 nm, and even more preferably 1 nm to 10 nm. This ensures a film thickness necessary to maintain the coating 12. The average thickness of the coating 12 is, for example, the average value of the film thickness of the coating 12 obtained from the observation image when the particle cross section of the powder for additive manufacturing 1 is observed with a transmission electron microscope, at five or more points.
[0065] The coating 12 may be a multilayer film in which molecules of the aforementioned compound are stacked in multiple layers, for example, 2 to 10 layers, but is preferably a monomolecular film of the aforementioned compound. The coating 12, which is a monomolecular film, can minimize its thickness. As a result, it is possible to obtain an additively molded body 6 in which the occupancy rate of the coating 12 is low and the occupancy rate of the particles 11 for molding is high. Such an additively molded body 6 is useful in that it is possible to obtain a metal sintered body with high dimensional accuracy because the shrinkage rate during sintering can be suppressed.
[0066] The monolayer is a film formed by self-organization of a coupling agent. That is, by using the coupling agent, molecules having affinity for the surface of the shape-forming particle 11 are densely arranged on the surface, so that a film having a thickness of one molecule can be efficiently formed.
[0067] Whether the coating 12 is a monolayer or not can be determined by, for example, qualitative and quantitative analysis in the depth direction using a combination of X-ray photoelectron spectroscopy and ion sputtering. Specifically, the concentration of the component derived from the coupling agent is examined in the depth direction. If the region where the concentration of the component derived from the coupling agent is high is equal to or smaller than the molecular size of the coupling agent, the coating 12 can be evaluated as a monolayer.
[0068] Coating 12 may contain any component other than the above-mentioned compound. In that case, from the viewpoint of reliably obtaining the above-mentioned effects, the mass ratio of the above-mentioned compound is preferably more than 50%, more preferably 70% or more, and even more preferably 90% or more.
[0069] 2.2.Various characteristics of powders for additive manufacturing Next, various characteristics of the powder 1 for layered manufacturing will be described.
[0070] 2.2.1.Particle size distribution When the particle size distribution of the powder for additive manufacturing 1 according to this embodiment is obtained on a volume basis by a laser diffraction particle size distribution measuring device, the particle size when the cumulative frequency is 10% from the small diameter side is defined as D10. Similarly, the particle sizes when the cumulative frequency is 50% and 90% from the small diameter side are defined as D50 and D90. Examples of the particle size distribution measuring device include Microtrac HRA9320-X100 manufactured by Nikkiso Co., Ltd.
[0071] The particle size D50 of the powder 1 for additive manufacturing is preferably 1.0 μm or more and 15.0 μm or less, more preferably 3.0 μm or more and 12.0 μm or less, and even more preferably 4.0 μm or more and 10.0 μm or less. This allows the powder 1 for additive manufacturing to have both good sinterability and good fluidity. As a result, an additive manufacturing body 6 that is dense and has high mechanical strength and molding accuracy can be obtained, and it can be used to finally manufacture a metal sintered body with high density and high surface accuracy.
[0072] If the particle size D50 is below the lower limit, the particles of the powder 1 for additive manufacturing may easily aggregate. If aggregation occurs, the flowability of the powder 1 for additive manufacturing may decrease, and the density of the metal sintered body may decrease. On the other hand, if the particle size D50 is above the upper limit, the sinterability of the powder 1 for additive manufacturing may decrease, and the density of the metal sintered body may decrease.
[0073] The ratio (D90-D10) / D50 of the difference between the particle diameters D90 and D10 to the particle diameter D50 is preferably 0.8 to 2.7, more preferably 1.0 to 2.4, and even more preferably 1.2 to 2.2. This makes the particle diameter of the powder 1 for additive manufacturing relatively uniform, making it easier to increase the fluidity and ensuring the sinterability. If the ratio (D90-D10) / D50 is below the lower limit, the particle size distribution will be broadened, and the fluidity may decrease. On the other hand, if the ratio (D90-D10) / D50 is above the upper limit, the particle size distribution may be too narrow, making it difficult to increase the filling rate and decreasing the sinterability.
[0074] 2.2.2. Water contact angle The powder for additive manufacturing 1 in this embodiment is subjected to a heat treatment in which it is heated at 200°C for 72 hours in an air atmosphere, and then the water contact angle measured in a layered state is preferably 80° or more and 150° or less, more preferably 90° or more and 140° or less, and even more preferably 100° or more and 130° or less.
[0075] In the powder 1 for additive manufacturing showing such a water contact angle, the amino group is not inactivated even when it is subjected to repeated heat treatment, and the epoxy resin is hardened. Therefore, the powder 1 for additive manufacturing can harden the binder at a lower temperature or in a shorter time, even when it is reused multiple times. As a result, the deformation of the additive manufacturing body 6 produced due to heat or the passage of time can be suppressed, and a metal sintered body with high dimensional accuracy can be obtained.
[0076] Moreover, the powder 1 for additive manufacturing that exhibits the above-mentioned contact angle with water is a powder that is resistant to aggregation and has high fluidity. Therefore, even if the powder 1 for additive manufacturing is reused multiple times, it has excellent packing properties. As a result, even if the powder 1 for additive manufacturing that has been reused multiple times is used, an additive manufacturing body 6 that is dense and has high mechanical strength and dimensional accuracy can be obtained. Then, by subjecting such an additive manufacturing body 6 to a sintering process, an additive manufacturing body 6 that can be used to manufacture a metal sintered body that has excellent relative density, mechanical strength, and dimensional accuracy can be obtained.
[0077] Furthermore, the powder 1 for additive manufacturing having a water contact angle within the above range has excellent affinity with the binder solution 4. In other words, when the binder solution 4 contains an organic solvent that dissolves epoxy resin, the powder 1 for additive manufacturing has excellent affinity with the organic solvent. Therefore, when the powder layer 31 is formed by spreading the powder 1 for additive manufacturing and then the binder solution 4 is supplied, the binder solution 4 is more likely to permeate into the formation region 60 of the powder layer 31. This allows the binder solution 4 to permeate uniformly into the formation region 60, making it possible to manufacture an additive manufacturing object 6 with high dimensional accuracy.
[0078] If the contact angle of water is below the lower limit, the curing of the epoxy resin may not be sufficiently promoted. In addition, the powder 1 for additive manufacturing may absorb moisture and easily aggregate, resulting in a decrease in fluidity. On the other hand, the contact angle of water may be above the upper limit, but in that case, the hydrophobicity may be too high, and depending on the composition of the binder solution 4, the permeability of the binder solution 4 may decrease. This may result in a decrease in homogeneity of the additive manufacturing body 6.
[0079] The contact angle of water on the additive manufacturing powder 1 can be measured by the following procedure. First, the additive manufacturing powder 1 is subjected to a heat treatment in which it is heated at 200°C for 72 hours in an air atmosphere. Next, a double-sided tape is attached to a flat surface. Next, the additive manufacturing powder 1 that has been subjected to the heat treatment is spread on the double-sided tape. For example, a polyester adhesive tape No. 31B manufactured by Nitto Denko Corporation, with a total thickness of 0.080 mm, is used as the double-sided tape. Then, the spread additive manufacturing powder 1 is lightly pressed down by a plate-shaped member. Next, the excess additive manufacturing powder 1 is blown off with an air blower. This results in a test specimen for contact angle measurement. As an example of the air blower, a manual air blower used for cleaning cameras and the like can be used. Then, the tip of the air blower is fixed at a position 3 cm away from the test specimen, and blown three times.
[0080] Next, the contact angle of water on the test specimen is measured by the θ / 2 method using a contact angle measuring device, DropMaster500, manufactured by Kyowa Interface Science Co., Ltd. The measurement conditions are an air temperature of 25°C and a relative humidity of 50%±5%. The amount of water dropped is 3 μL, and the measurement is performed 5 seconds after the drop has landed.
[0081] 3. Manufacturing method of powder for additive manufacturing Next, an example of a method for producing the powder 1 for layered manufacturing will be described.
[0082] Fig. 12 is a process diagram showing an example of a method for producing the powder for layered manufacturing 1 shown in Fig. 11. In the following description, the method for producing the powder for layered manufacturing 1 described above will be described as an example.
[0083] The method for producing a powder for layered manufacturing shown in FIG. 12 includes a powder preparation step S202 for preparing particles for layered manufacturing 11, and a coating formation step S204 for forming a coating 12.
[0084] 3.1. Powder preparation process In the powder preparation step S202, metal powder to be used as the object particles 11 is prepared.
[0085] The metal powder may be produced by any method, for example, by the atomization method. In the atomization method, molten metal is made to flow down from a crucible and collide with a fluid such as a liquid or gas sprayed at high speed. The molten metal that collided with the fluid falls by inertia, and the droplets are made spherical at that time. As a result, it is possible to produce metal powder that has a relatively small diameter but a high degree of circularity and a relatively small specific surface area.
[0086] Atomization methods include water atomization, gas atomization, and rotary water flow atomization, depending on the type of coolant and the configuration of the device.
[0087] The flow rate of the molten metal varies depending on the size of the device, but is preferably more than 1.0 kg / min and not more than 20.0 kg / min, and more preferably 2.0 kg / min or more and not more than 10.0 kg / min. This allows the amount of molten metal flowing down in a certain period of time to be optimized, making it possible to efficiently produce metal powders with a narrow particle size distribution and sufficient spherical shape. As a result, it is possible to produce metal powders that are relatively small in diameter but have a high degree of circularity and a relatively small specific surface area.
[0088] The temperature of the molten metal in the crucible (casting temperature) is preferably set to Tm+100°C or more and Tm+350°C or less, more preferably Tm+180°C or more and Tm+320°C or less, and even more preferably Tm+250°C or more and Tm+300°C or less, relative to the melting point Tm [°C] of the constituent material of the powder for additive manufacturing. This allows the time during which the molten metal exists when it is refined by various atomization methods and solidifies to be longer than in the past. As a result, it is possible to produce metal powder with a high degree of circularity and a relatively small specific surface area even with a small diameter.
[0089] In addition, in various atomization methods, the outer diameter of the thin stream when the molten metal is allowed to flow is not particularly limited, but is preferably 3.0 mm or less, more preferably 0.3 mm to 2.0 mm, and even more preferably 0.5 mm to 1.5 mm. This makes it easier to apply the fluid to the molten metal uniformly, making it easier for droplets of appropriate size to scatter uniformly. As a result, metal powder with the average particle size as described above can be produced with a narrow particle size distribution.
[0090] The produced metal powder may be classified as necessary by a method such as dry classification, such as sieving classification, inertial classification, or centrifugal classification, or wet classification, such as sedimentation classification.
[0091] The produced metal powder may then be annealed (heat-treated). In the case where the particles 11 contain Si, this makes it easier for the concentration of Si to increase on the surface of the particles 11. As a result, the surface of the particles 11 serves as a base for increasing the adhesion of the coating 12.
[0092] The conditions of the annealing treatment are not particularly limited, but preferably, the heating temperature is 600° C. or more and 1000° C. or less, and the heating time is 10 minutes or more and 3 hours or less, and more preferably, the heating temperature is 700° C. or more and 900° C. or less, and the heating time is 30 minutes or more and 2 hours or less. This makes it possible to obtain the particles for molding 11 with the coating 12 having particularly improved adhesion. The heating atmosphere is, for example, air atmosphere.
[0093] On the other hand, a base film serving as a base for the coating 12 may be formed on the surface of the shaping particle 11 by various film formation methods. As the film formation method, a gas phase film formation method is preferably used, and an ALD (Atomic Layer Deposition) method is more preferably used. In the ALD method, raw materials can be deposited at the atomic layer level, so that a dense base film with a thin thickness can be formed. In addition, in the ALD method, raw materials, oxidizing agents, etc. can be easily introduced into recesses and shaded areas. Therefore, by using the ALD method, a base film with a high coverage can be formed. As a result, in the coating formation step S204 described later, the coverage of the coating 12 can also be increased.
[0094] In addition, the powder preparing step S202 does not have to be performed as described above if the shaping particles 11 are available.
[0095] 3.2. Film formation process In the coating formation step S204, the coating 12 is formed on the surface of the shaping particles 11. In this step, a coupling agent having an amino group is reacted with the shaping particles 11. As a result, the coupling agent is attached to the surface of the shaping particles 11.
[0096] Examples of this operation include the following three operations. The first operation includes a step of putting both the shaping particles 11 and the coupling agent into a chamber, and then heating the inside of the chamber.
[0097] The second operation includes a process of putting the shaping particles 11 into a chamber, and then spraying a coupling agent into the chamber while stirring the shaping particles 11.
[0098] The third operation includes adding water, a coupling agent, an alkaline solution such as ammonia or sodium hydroxide, and the moldable particles 11 to a primary alcohol such as methanol, ethanol, or isopropyl alcohol, stirring the mixture, filtering, and then drying.
[0099] Examples of the coupling agent include a silane coupling agent, a titanium coupling agent, and a zirconium coupling agent.
[0100] The following chemical formula is an example of the molecular structure of a silane coupling agent.
[0101] [ka]
[0102] In the above formula, X is a functional group, Y is a spacer, and OR is a hydrolyzable group, where X is an amino group and R is, for example, a methyl group or an ethyl group.
[0103] Examples of the spacer Y include an alkylene group, an arylene group, an aralkylene group, an alkylene ether group, etc. The spacer Y is a linking group provided between the hydrolyzable group OR and the functional group X.
[0104] Furthermore, when the spacer Y includes a linear structure, the number of carbon atoms in the linear structure is not particularly limited, but is preferably 10 or less, more preferably 1 to 8, and even more preferably 2 to 6. If the number of carbon atoms in the linear structure is within the above range, the length of the linear structure is optimized, improving the stability of the coating 12. As a result, even when the powder for additive manufacturing 1 is reused multiple times, it is possible to obtain a powder for additive manufacturing 1 that can harden the binder at a lower temperature or in a shorter time.
[0105] The number of carbon atoms in the straight-chain structure may be less than the lower limit, but in that case, the distance between the hydrolyzable group and the amino group may be too close, which may deteriorate the orientation of the amino group and make it difficult for the amino group to act on the epoxy resin. On the other hand, if the number of carbon atoms in the straight-chain structure exceeds the upper limit, the compound derived from the coupling agent may easily collapse, which may deteriorate the orientation of the amino group.
[0106] The term "straight-chain structure" refers to a series of carbon atoms bonded in series, and the number of carbon atoms in the straight-chain structure is the number of carbon atoms bonded in series in the straight-chain structure.
[0107] The hydrolyzable group is, for example, an alkoxy group, a halogen atom, a cyano group, an acetoxy group, an isocyanate group, etc., and among these, in the case of an alkoxy group, a silanol is generated by hydrolysis. This silanol reacts with a hydroxyl group generated on the surface of the shaping particle 11, and the coupling agent adheres to the surface of the shaping particle 11. If the aforementioned Si content is within the aforementioned range, the coupling agent is easily adhered uniformly without unevenness. As a result, a coating 12 with a high coverage rate close to a monolayer is obtained.
[0108] At least one such hydrolyzable group may be contained in one molecule of the coupling agent, but two or more are preferably contained, and three or more hydrolyzable groups are more preferably contained as in the above formula. For example, a coupling agent in which the hydrolyzable group is an alkoxy group preferably contains a dialkoxy group, and more preferably contains a trialkoxy group. A coupling agent containing a trialkoxy group reacts with three hydroxyl groups generated on the surface of the shaping particles 11. For this reason, it has good adhesion to the shaping particles 11. In addition, a coupling agent containing a trialkoxy group is also excellent in film-forming properties, so that a coating 12 with excellent continuity can be obtained. Such a coating 12 has particularly good adhesion and stability to the shaping particles 11, and contributes to further increasing the heat resistance and fluidity of the powder for layered manufacturing 1.
[0109] The upper limit of the number of hydrolyzable groups in one molecule does not have to be particularly set, but is preferably equal to or less than 6. This makes it easier to control the formation of the coating 12 and makes it easier to make the thickness of the coating 12 uniform.
[0110] Here, examples of coupling agents having an amino group will be given. Examples of coupling agents having an amino group include γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltriisopropoxysilane, γ-aminopropylmethyldimethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropylmethyldiethoxysilane, Examples of the silane include silane, γ-(2-aminoethyl)aminopropyltriisopropoxysilane, γ-(2-aminoethyl)aminooctyltrimethoxysilane, γ-ureidopropyltrimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-benzyl-γ-aminopropyltrimethoxysilane, N-vinylbenzyl-γ-aminopropyltriethoxysilane, 3-(6-aminohexylamino)propyl]trimethoxysilane, and N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine.
[0111] Specific examples of amino group-containing silane coupling agents include KBE-903, X-12-972F, XBM-6803, KBM-573, KBM-575, KBM-602, KBM-603, KBM-903, KBM-6103, and X-12-5263HP, all manufactured by Shin-Etsu Chemical Co., Ltd. Specific examples of amino group-containing silane coupling agents include Z-6610, Z-6611, OFS-6020, Z-6094, Z-6883, OFS-6032, Z-6269, and SZ-6032, all manufactured by Dow-Toray. Furthermore, specific examples of amino group-containing silane coupling agents include A0439, B2548, P1458, T2246, T3733, A0774, A0876, A2628, A3128, D1980, T3242, A1923, D4328, T1255, B6036, T2826, and T2796, all manufactured by Tokyo Chemical Industry Co., Ltd.
[0112] Moreover, the functional group X may have any organic group other than an amino group. For example, an aryl group such as a phenyl group can be used as the organic group. This can further increase the affinity between the epoxy resin containing an aromatic ring and the coating 12. As a result, the curing of the epoxy resin can be further promoted. In addition, the permeability of the binder solution 4 into the powder layer 31 can be further increased.
[0113] The amount of the coupling agent added is not particularly limited, but is preferably 0.01% by mass to 1.00% by mass, and more preferably 0.05% by mass to 0.50% by mass, based on the particles 11 for shaping.
[0114] The coupling agent is supplied by being left stationary in the chamber or by being sprayed into the chamber.
[0115] Thereafter, the particles 11 to which the coupling agent is attached are heated. As a result, a coating 12 is formed on the surface of the particles 11 to obtain the powder for layered manufacturing 1. In addition, the heating can remove any unreacted coupling agent.
[0116] The heating temperature of the particles for shaping 11 to which the coupling agent is attached is not particularly limited, but is preferably 50° C. to 300° C., and more preferably 100° C. to 250° C. The heating time is preferably 10 minutes to 24 hours, and more preferably 30 minutes to 10 hours. Examples of the atmosphere for the heat treatment include air and inert gas.
[0117] 4. Advantages of the above embodiment As described above, the powder for additive manufacturing 1 according to the embodiment is a powder for additive manufacturing used for manufacturing an additive manufacturing body 6 that becomes a metal sintered body by sintering by a binder jet method, and includes particles for molding 11 containing a metal material and a coating 12 provided on the surface of the particles for molding 11. The coating 12 contains a compound derived from a coupling agent having an amino group.
[0118] According to this configuration, when the powder 1 for additive manufacturing comes into contact with the epoxy resin, the amino group acts as a curing agent that cures the epoxy resin. Therefore, when the binder for additive manufacturing containing uncured epoxy resin is supplied to the powder layer 31 composed of the powder 1 for additive manufacturing, the curing of the epoxy resin is promoted. This allows the binder to be cured at a lower temperature or in a shorter time. As a result, in the additive manufacturing body 6 to be produced, deformation caused by heat or the passage of time can be suppressed, and an additive manufacturing body 6 with high dimensional accuracy can be produced. In addition, since poor curing is less likely to occur, the mechanical strength of the additive manufacturing body 6 can also be increased.
[0119] The coupling agent may also contain a linear structure, the number of carbon atoms of which is preferably 10 or less.
[0120] According to this configuration, the length of the linear chain structure is optimized, improving the stability of the coating 12. As a result, even when the powder 1 for additive manufacturing is reused multiple times, the powder 1 for additive manufacturing can harden the binder at a lower temperature or in a shorter time.
[0121] The amino group preferably includes a primary amine or a secondary amine. These are more reactive and therefore allow the binder to be cured at lower temperatures or in shorter times.
[0122] In addition, after being subjected to a heat treatment in which the material is heated at 200°C for 72 hours in an air atmosphere, it is preferable that the contact angle of water measured at 25°C by the θ / 2 method in a layered state is 80° or more and 150° or less.
[0123] According to this configuration, the powder 1 for additive manufacturing can be obtained in which the amino groups are not inactivated even when the powder is subjected to repeated heat treatments, and the curing of the epoxy resin is accelerated. The powder 1 for additive manufacturing can cure the binder at a lower temperature or in a shorter time, even when the powder is reused multiple times.
[0124] Furthermore, for the powder 1 for additive manufacturing according to the embodiment, when the particle size distribution on a volume basis is obtained using a laser diffraction particle size distribution measuring device, and the particle size when the cumulative frequency is 10% from the small diameter side is defined as D10, the particle size when the cumulative frequency is 50% from the small diameter side is defined as D50, and the particle size when the cumulative frequency is 90% from the small diameter side is defined as D90, it is preferable that the particle size D50 is 1.0 μm or more and 15.0 μm or less, and the ratio (D90-D10) / D50 is 0.8 or more and 2.7 or less.
[0125] This configuration makes it possible to achieve both sinterability and flowability of the layered manufacturing powder 1. As a result, it is possible to obtain a dense layered manufactured body 6 that has high mechanical strength and manufacturing accuracy.
[0126] The layered object 6 according to the embodiment includes the powder 1 for layered manufacturing, and a binder that bonds particles of the powder 1 for layered manufacturing together and contains an epoxy resin.
[0127] In such an additive manufacturing object 6, when the powder 1 for additive manufacturing comes into contact with the epoxy resin, the amino group acts as a curing agent that cures the epoxy resin. Therefore, when the binder for additive manufacturing containing uncured epoxy resin is supplied to the powder layer 31 composed of the powder 1 for additive manufacturing, the curing of the epoxy resin is promoted. This allows the binder to be cured at a lower temperature or in a shorter time. As a result, the additive manufacturing object 6 to be produced can be prevented from being deformed due to heat or the passage of time, and an additive manufacturing object 6 with high dimensional accuracy can be obtained. In addition, since poor curing is less likely to occur, the mechanical strength of the additive manufacturing object 6 can also be increased.
[0128] Moreover, the epoxy resin is preferably a compound having two or more epoxy groups in the molecule.
[0129] This makes it easier for the cured epoxy resin to form a three-dimensional network, which in turn increases the mechanical strength of the layered object 6 that contains the cured epoxy resin.
[0130] The powder for additive manufacturing and the additive manufacturing body of the present invention have been described above based on the illustrated embodiment, but the present invention is not limited to this. For example, the powder for additive manufacturing and the additive manufacturing body of the present invention may be the above embodiment to which any component has been added. EXAMPLES
[0131] Next, specific examples of the present invention will be described. 5. Production of powder for additive manufacturing Metal powders used for the additive manufacturing powders of Samples No. 1 to 22 were produced by water atomization. Next, a coating was formed on the obtained metal powders using a coupling agent. In this way, the additive manufacturing powders were obtained. The steel type of the metal powders, the representative particle size of the additive manufacturing powders, the composition of the coupling agent, and the contact angle of water after heat treatment are as shown in Tables 1 to 4.
[0132] [Table 1]
[0133] In addition, the chemical formula symbols shown in Tables 2 to 4 correspond to the following compounds. A-1: 3-aminopropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd., KBM-903) A-2: N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd., KBM-603) A-3: 3-(6-aminohexylamino)propyl]trimethoxysilane (Tokyo Chemical Industry Co., Ltd., A3128) A-4: N-2-(aminoethyl)-8-aminooctyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd., KBM-6803) A-5: N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine (Shin-Etsu Chemical Co., Ltd., X-12-5263HP) A-6: N-phenyl-3-aminopropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd., KBM-573)
[0134] In Tables 2 to 4, among the powders for additive manufacturing of each sample number, those that correspond to the present invention are designated as "Examples" and those that do not correspond to the present invention are designated as "Comparative Examples."
[0135] 6. Evaluation of Powders for Additive Manufacturing 6.1.Curing properties of epoxy resin For each powder for additive manufacturing, the curing property of the epoxy resin was evaluated according to the following procedure.
[0136] First, 0.1 of each additive manufacturing powder was weighed and packed into a resin tube with a diameter of 0.5 inches. Three resin tubes filled with the same additive manufacturing powder were prepared. Next, 1 mL of epoxy resin emulsion was diluted with 1 mL of pure water to prepare a binder solution. ADEKA's EM-058 epoxy resin emulsion was used. 1 mL of the prepared binder solution was dropped into each resin tube, and a curing process was performed by heating it in a constant temperature bath at 60°C.
[0137] 30 minutes, 60 minutes, and 90 minutes after the start of the curing process, one resin tube was removed from the thermostatic chamber. Next, the powder for additive manufacturing was extruded from the removed resin tube. The state of the extruded powder for additive manufacturing was then visually observed, and the observation results were evaluated according to the following evaluation criteria. The evaluation results are shown in Tables 2 to 4.
[0138] A: More than 90% of the volume of the powder for additive manufacturing is bound by epoxy resin. B: More than 50% but less than 90% of the volume of the powder for additive manufacturing is bound by epoxy resin C: More than 30% but less than 50% of the volume of the powder for additive manufacturing is bound by epoxy resin D: Less than 30% of the volume of the powder for additive manufacturing is bound by epoxy resin Tables 2 to 4 show the functionality (the number of epoxy groups in the molecule) of the epoxy resins used.
[0139] 6.2. Dimensional Accuracy of the Laminated Object Each powder for additive manufacturing was used to fabricate an additive manufacturing object having a rectangular parallelepiped shape by the binder jet method. The binder solution used was the same as that in 6.1. The amount of binder used in the binder jet method (mass ratio of solid content) was 70 mass% of the powder for additive manufacturing. Next, the dimensions of the resulting additive manufacturing object were measured. Next, the deviation from the target value of the dimension was calculated, and the absolute value of the ratio of the deviation to the target value was taken as the dimensional accuracy of the additive manufacturing object. The calculated dimensional accuracy was then evaluated against the following evaluation criteria. The evaluation results are shown in Tables 2 to 4.
[0140] A: Dimensional accuracy is less than 1% B: Dimensional accuracy is 1% or more but less than 2% C: Dimensional accuracy is 2% or more but less than 3% D: Dimensional accuracy is 3% or more Tables 2 to 4 show the functionality (the number of epoxy groups in the molecule) of the epoxy resins used.
[0141] 6.3. Mechanical Strength of the Laminated Object Using each powder for additive manufacturing, an additive manufacturing object having a rectangular parallelepiped shape was produced by the binder jet method. The binder solution used was the same as in 6.1. The amount of binder used in the binder jet method (mass ratio of solid content) was 70 mass% of the powder for additive manufacturing. The size of the additive manufacturing object produced was 40 mm in length, 20 mm in width, and 5 mm in thickness.
[0142] Next, the bending load of the produced layered object was measured using a three-point bending test jig, and the bending stress σ of the layered object was calculated using the following formula.
[0143]
number
[0144] In the above formula, F is the bending load, L is the distance between the supports of the three-point bending test jig, b is the width of the layered object, and h is the thickness of the layered object. The calculation results were evaluated against the following evaluation criteria. The evaluation results are shown in Tables 2 to 4.
[0145] A: The mechanical strength of the laminated body is high (bending stress σ is 25 N / cm 2 That's all.) B: The mechanical strength of the laminated object is somewhat high (bending stress σ is 20 N / cm 2 More than 25N / cm 2 is less than C: The mechanical strength of the laminated object is somewhat low (bending stress σ is 15 N / cm 2 More than 20N / cm 2 is less than D: The mechanical strength of the additive manufacturing body is low (bending stress σ is 15 N / cm 2 is less than Tables 2 to 4 show the functionality (the number of epoxy groups in the molecule) of the epoxy resins used.
[0146] [Table 2]
[0147] [Table 3]
[0148] [Table 4]
[0149] 6.4. Considerations of the evaluation results As shown in Tables 2 to 4, it was confirmed that the powder for additive manufacturing of each Example can cure the epoxy resin in a shorter time when a binder solution containing an epoxy resin is used. In addition, since the curing temperature is sufficiently low, it was confirmed that the powder for additive manufacturing of each Example can produce an additive manufacturing object at a lower temperature or in a shorter time. It was also confirmed that the dimensional accuracy of the manufactured additive manufacturing object can be improved by using the powder for additive manufacturing of each Example, and that the mechanical strength of the obtained additive manufacturing object is sufficiently high. [Explanation of symbols]
[0150] 1... Powder for additive manufacturing, 2... Additive manufacturing apparatus, 4... Binder solution, 6... Additive manufacturing body, 11... Particles for molding, 12... Coating, 13... Surface-coated particles, 21... Apparatus body, 22... Powder supply elevator, 23... Molding stage, 24... Coater, 25... Roller, 26... Liquid supply section, 31... Powder layer, 41... Bonding layer, 60... Formation area, 211... Powder storage section, 212... Molding section, S102... Powder layer formation process, S104... Binder solution supply process, S106... Repeating process, S202... Powder preparation process, S204... Coating formation process
Claims
1. A powder for additive manufacturing used to manufacture an additive manufacturing body that becomes a metal sintered body by a binder jet method, Particles for shaping containing a metal material; a coating film provided on a surface of the particle for shaping, the coating film containing a compound derived from a coupling agent having an amino group; A powder for additive manufacturing comprising:
2. The coupling agent comprises a linear structure, The powder for additive manufacturing according to claim 1 , wherein the number of carbon atoms in the linear structure is 10 or less.
3. The powder for additive manufacturing according to claim 1 or 2, wherein the amino group includes a primary amine or a secondary amine.
4. The powder for additive manufacturing according to claim 3, which, after being subjected to a heat treatment in which it is heated at 200° C. for 72 hours in an air atmosphere, has a water contact angle of 80° or more and 150° or less when measured at 25° C. by the θ / 2 method in a layered state.
5. A particle size distribution on a volume basis is obtained using a laser diffraction particle size distribution measuring device, and the particle size when the cumulative frequency is 10% from the small diameter side is defined as D10, the particle size when the cumulative frequency is 50% from the small diameter side is defined as D50, and the particle size when the cumulative frequency is 90% from the small diameter side is defined as D90. The particle size D50 is 1.0 μm or more and 15.0 μm or less, The powder for layered manufacturing according to claim 1 or 2, wherein the ratio (D90-D10) / D50 is 0.8 or more and 2.7 or less.
6. The powder for layered manufacturing according to claim 1 or 2, a binder that binds particles of the powder for additive manufacturing together and contains an epoxy resin; An additive manufacturing object comprising:
7. The layered object according to claim 6 , wherein the epoxy resin is a compound having two or more epoxy groups in the molecule.
Citation Information
Patent Citations
Laminated molding powder, production method of laminated molding powder, laminated molding and sintered metal
JP2022122503A