Coating composition and laminate

A coating composition with specific base agent and reaction regulator components addresses the wear and weather resistance issues of polycarbonate resin, offering improved scratch resistance and stability in cured films for laminates.

JP2024140285APending Publication Date: 2024-10-10MITSUBISHI CHEM CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023051353
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Polycarbonate resin molded products lack surface wear resistance and weather resistance, leading to issues such as scratches and yellowing due to exposure to sunlight, and existing urethane resin compositions have short pot life and storage stability issues.

Method used

A coating composition comprising at least two components: a base agent with specific hydroxyl value and acid value, a reaction regulator, and optionally including inorganic fine particles, ultraviolet absorbers, and hindered amine light stabilizers, which form a cured film with improved scratch resistance and weather resistance.

Benefits of technology

The coating composition provides enhanced storage stability, pot life, adhesion, and forms a cured film with excellent scratch resistance and weather resistance, suitable for laminates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140285000001
    Figure 2024140285000001
  • Figure 2024140285000002
    Figure 2024140285000002
  • Figure 2024140285000003
    Figure 2024140285000003
Patent Text Reader

Abstract

To provide: a coating composition having good storage stability and pot life and, further, capable of forming a coating film having excellent adhesion to a substrate, scratch resistance, and weather resistance; a cured product obtained by curing the coating composition; and a laminate formed by laminating the cured product.SOLUTION: A coating composition comprises at least two liquids including a base agent and a curing agent, where the base agent comprises a polyol (A) and a reaction modifier (B), the polyol (A) has a hydroxyl value of 50-300 mg KOH / g and an acid value of 1-100 mg KOH / g, the reaction modifier (B) is an isocyanate blocking agent, and the curing agent comprises a polyisocyanate (C).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to coating compositions and laminates. [Background technology]

[0002] Generally, polycarbonate resin, polymethyl methacrylate resin, polystyrene resin The molded products made of this material are not only lightweight and excellent in formability, but also have good transparency, making them comparable to glass products. It has superior impact resistance compared to other products. Therefore, it is used in Acrylate resin and polystyrene resin are used as glass substitutes for various lamp lenses and windows. They are used for materials such as glass and instrument covers. In particular, headlamp lenses are used in automobiles. Plastic materials are being used due to the diversification of automobile designs. Therefore, polycarbonate resin molded products with excellent impact resistance are used for window glass and sunroofs. is.

[0003] However, polycarbonate resin molded products lack surface abrasion resistance and weather resistance. Therefore, damage to the surface caused by contact with other hard objects, friction, scratches, etc., and damage caused by exposure to sunlight, etc. Yellowing due to exposure to ultraviolet light, which can cause the product to lose its commercial value.

[0004] To make up for these shortcomings of polycarbonate resin molded products, UV absorbers are added to the curing raw materials such as acrylic, melamine, urethane, and silicone. A method of applying the coating material composition containing the additive to the surface of a molded article and heating it to form a cured film, or It is cured by exposure to active energy rays such as ultraviolet rays and electron beams to form a weather-resistant cured film. Among them, the method of hardening thermosetting paint in a heat drying oven is suitable for various applications depending on the three-dimensional shape of the object to be coated. Since it is easy to apply uniform heating, the resulting cured film exhibits stable performance regardless of the part. It has the advantage of being easy to use.

[0005] As a method for forming a thermosetting cured film on the surface of a resin molded product, a melamine resin composition or It is known that coating with paint containing epoxy resin composition, urethane resin composition, etc. Among them, urethane resin compositions tend to react at lower temperatures than other resin compositions. This allows for a reduction in the amount of carbon dioxide emitted during the process from painting to curing. It excels in this respect.

[0006] However, in paints containing urethane resin compositions, the resin contains hydroxyl groups and isocyanate groups. The reaction begins as soon as the resin containing this compound is mixed, so the viscosity increases over time during the painting process. This can cause problems such as deterioration of the quality of the coating film and deterioration of its appearance. The time during which a resin containing ethylene can be used after it is mixed is called its usable time or pot life. The shortness of the adhesion time is an issue for paints made of urethane resin compositions.

[0007] Patent Document 1 describes a urethane coating composition using a blocked isocyanate compound. The isocyanate groups are blocked in advance to prevent reaction with hydroxyl groups. Patent Document 2 describes a method for producing a hydroxyl-containing resin-containing base material and a crosslinking agent. The curing agent containing the isocyanate group, which is the main component, is mixed just before painting, and the mixture ratio of the main component is A method for achieving a suitable pot life is described in Patent Document 3. There is a description of how to paint the material. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2020-132751 A [Patent Document 2] Japanese Patent Application Publication No. 5-239407 [Patent Document 3] Patent No. 4001220 Summary of the Invention [Problem to be solved by the invention]

[0009] A blocked isocyanate compound such as the resin composition described in Patent Document 1 is used. In this case, the pot life is significantly improved, but it takes time for the blocking agent to dissociate. However, the high reactivity, which is one of the advantages of urethane paint, is lost. The expected pot life extension effect is small based on the resin composition ratio alone. As stated in the literature, adding amine compounds or metal catalysts as curing accelerators improves weather resistance and This can impair storage stability and make it impossible to meet the current demand for high weather resistance.

[0010] The present invention has good storage stability and pot life, and further has good adhesion to substrates and scratch resistance. A coating composition capable of forming a coating film excellent in adhesion and weather resistance, and a coating composition cured by curing the coating composition and a laminate in which the cured product is laminated. [Means for solving the problem]

[0011] The present invention has the following aspects. That is, the above object of the present invention can be achieved by the following means [1] to

[10] . [1] A coating composition having at least two liquids, a base agent and a curing agent, the base agent being a polyol ( A reaction regulator (B) is included, and the polyol (A) has a hydroxyl value of 50 to 300 mgK. OH / g and the acid value is 1 to 100 mgKOH / g, and the reaction adjuster (B) is isocyanate. The coating composition according to claim 1, wherein the curing agent is a polyisocyanate (C). [2] The coating composition according to [1], which contains inorganic fine particles (D). [3] The inorganic fine particles (D) have an isocyanate group, an epoxy group, a mercapto group, or the like as a reactive group. The coating composition according to [1] or [2], further comprising at least one selected from the group consisting of aryl, aryl, aryl and aryl groups. [4] The reaction regulator (B) is a β-dicarbonyl compound, [1] to [3] any one of the above The coating composition according to claim 1 [5] The polyol (A) is at least one of an acrylic polyol and a polyester polyol. The coating composition according to any one of [1] to [4], [6] A polycarbonate polyol (E) different from the polyol (A), The coating composition according to any one of the items [1] to [5]. [7] The coating composition according to any one of [1] to [6], which contains an ultraviolet absorber (F). [8] The method according to any one of [1] to [7], further comprising the hindered amine light stabilizer (G). A coating composition. [9] A cured product of the coating composition described in any one of [1] to [8].

[10] A laminate having a coating film made of the cured product according to [9]. Effect of the Invention

[0012] According to the present invention, the composition has good storage stability and pot life, and further has excellent adhesion to a substrate, A coating composition capable of forming a coating film excellent in abrasion resistance and weather resistance, and a laminate in which the cured products are laminated. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The embodiment of the present invention will be described in detail below. The following description is based on the embodiment of the present invention. The following description is merely an example, and the present invention is not limited to the following description unless it exceeds the gist of the present invention. stomach. In this specification, when the expression "~" is used, the numerical values ​​or physical properties before and after it are The numerical ranges disclosed in this specification are intended to include the lower and upper limits. The values ​​can be arbitrarily combined to form a new numerical range. When the term "(meth)acrylic" is used, it can mean either "acrylic" or "methacrylic" or Both are meant. "(Meth)acrylate", "(meth)acryloyl", etc. The same is true for

[0014] <Paint composition> The coating composition of the present invention is a coating composition in which at least two liquids, a base agent and a curing agent, are mixed before application. The composition contains a polyol (A) and a reaction modifier (B) as a main component, and the polyol ( A) has a hydroxyl value of 50-300 mgKOH / g and an acid value of 1-100 mgKOH / g The reaction regulator (B) is an isocyanate blocking agent, and the curing agent is a polyisocyanate. The coating composition further comprises a carboxylate (C).

[0015] <Polyol (A)> The polyol (A) has a hydroxyl value in the range of 50 to 300 mgKOH / g and an acid value of 1 It is a compound with a pH of ~100mgKOH / g.

[0016] The pot life of the coating composition, compatibility with other components, and scratch resistance and durability of the coating film formed From the viewpoint of chemical resistance and adhesion, the hydroxyl value of polyol (A) is usually 50 to 300 mgKO H / g, preferably 70 to 280 mgKOH / g, more preferably 80 to 250 mgKOH / g. H / g, and more preferably in the range of 100 to 220 mgKOH / g. By doing so, the scratch resistance of the coating film is improved. If it is less than gKOH / g, the scratch resistance decreases, and if it is more than 300 mgKOH / g, The hydroxyl value is determined by, for example, dissolving polyol (A) in pyridine. It is measured by reacting it with excess acetic anhydride at 100°C and titrating the liberated acetic acid with potassium hydroxide. It is possible.

[0017] From the viewpoint of the pot life of the coating composition and the reactivity of the isocyanate group and the hydroxyl group, The acid value of the copolymer (A) is usually 1.0 to 100 mgKOH / g, preferably 5.5 to 85 mgKOH / g. OH / g, more preferably 7.0 to 47 mgKOH / g. This improves the reactivity of the coating film. If the value is less than H / g, the reactivity decreases, and the scratch resistance and water resistance become low. If the acid value of the thiol (A) is greater than 100 mg KOH / g, the pot life will be shortened. The acid value can be measured by the method shown in JIS K 0070-1992. do.

[0018] In addition, the solubility parameter (SP value) of polyol (A) is In order to ensure compatibility with other components such as inorganic fine particles (D) and ultraviolet absorbers (F), , 8.0 to 12.0, preferably 8.5 to 11.5, and more preferably 8.8 to 11.0 The most preferred range is 9.0 to 10.5. This ensures compatibility between polyol (A) and other components, improving scratch resistance and weather resistance. When the SP value of (D) is less than 8.0, it is incompatible with inorganic particles (D) and ultraviolet absorbers (F). The SP value of polyol (A) is less than 12.0, and the abrasion resistance and weather resistance are reduced. If the amount of the polyisocyanate (C) increases, the compatibility with the polyisocyanate (C) decreases, resulting in poor appearance and poor scratch resistance. This causes a decline.

[0019] The SP value is a measure of solubility and is measured as follows. SUH,CLARKE [JPSA-1,5,1671-1681(1967)]. ·Measurement temperature 20℃ Weigh out 0.5 g of sample resin into a 100 ml beaker and add 10 ml of good solvent with a pipette. Add using a stir bar and dissolve using a magnetic stirrer. ·Solvent Good solvent: Acetone. Antisolvent: n-hexane, ion-exchanged water. Turbidity measurement: Drop the poor solvent using a 50ml burette, and measure the amount of the drop at which turbidity occurs. do. Calculation The SP value δ of a resin is given by the following formula:

number

[0020] In addition, the glass transition temperature (Tg) of the polyol (A) is set to 100° C. so as to achieve both indentation hardness and scratch resistance. Therefore, the temperature is usually -40 to 130°C, preferably 0 to 105°C, and more preferably 30 to 10 0°C, and most preferably 40 to 85°C. By using it in the corresponding range, good pressing It is possible to achieve both hardness and scratch resistance. When Tg is lower than -40°C, the indentation hardness If the temperature rises above 130°C, the scratch resistance will decrease and the appearance of the coating will become poor. Here, the Tg of the polyol is measured using a differential scanning calorimeter (DSC). Specific measurement conditions will be shown in the Examples section below.

[0021] Furthermore, the weight average molecular weight (Mw) of the polyol (A) is appropriately determined depending on the application of the resin composition. It should be appropriately selected, but it is preferably 1000 to 200,000, more preferably 1, 500 to 50,000, more preferably 1,800 to 20,000, and particularly preferably 2 By using it in this range, scratch resistance and indentation resistance are improved. It is possible to achieve both hardness and viscosity, and it is also easy to keep the viscosity of the composition in an appropriate range, which reduces the risk of damage when forming a coating film. The weight average molecular weight (Mw) is determined by the gel permeability. Using gel permeation chromatography (GPC), the values ​​were converted using polystyrene standards. The specific measurement conditions will be shown in the Examples below.

[0022] Examples of polyols that satisfy the above requirements include acrylic polyols, polyester polyols, and polyols. Among them, resins such as polyether polyols and the like can be used, and among them, From the viewpoint of being easy to adjust and to form a hard coat layer having good weather resistance, Polyols such as aryl polyols and polyester polyols are preferred. These polyols may be used alone or in combination of two or more kinds.

[0023] <Acrylic polyol> Acrylic polyol is, for example, an ethylenically unsaturated bond having one or more hydroxyl groups in one molecule. Monomer (a1) having an ethylenically unsaturated bond with one or more acid groups in one molecule and another ethylenically unsaturated monomer (a3) ​​copolymerizable therewith, It can be obtained by copolymerization.

[0024] A monomer (a1) having an ethylenically unsaturated bond having one or more hydroxyl groups in one molecule, Examples of 2-hydroxyethyl (meth)acrylate and 2-hydroxy (meth)acrylate are Propyl, 2-hydroxybutyl (meth)acrylate, 3-hydroxy(meth)acrylate (Meth)acrylic acid 4-hydroxypropyl, (meth)acrylic acid 3-hydroxybutyl xylbutyl, glycerol (meth)acrylate, cyclohexanedimethanol mono(meth)acrylate Acrylate, Plaxel F series (caprolactone-added monoacrylate manufactured by Daicel Corporation) Caprolactone addition monomers such as caprolactone esters (product name); "Blenmar PME-100" (manufactured by NOF Corp., methoxypolyethylene glycol methacrylate) Relate (ethylene glycol chains with 2 units), product name), "Blenmer PME -200" (NOF Corp., methoxypolyethylene glycol methacrylate (ethylene (Product name) "Blenmar PME-400" (NOF Corp. Methoxy polyethylene glycol methacrylate (ethylene glycol chain 9), "Blenmar AME-100" (manufactured by NOF Corp., product name), "Blenmar AME-200" (product name, manufactured by NOF Corp.) and "Blenmar 50AOEP -800B" (manufactured by NOF Corp., product name) and other glycol ester monomers containing hydroxyl groups (Meth)acrylic acid esters are included.

[0025] As the monomer (a1), (meth)acrylic acid 2 is used from the viewpoints of availability and scratch resistance. -Hydroxyethyl, (meth)acrylic acid 2-hydroxypropyl, (meth)acrylic acid 4-Hydroxybutyl, Plaxel FM1 (manufactured by Daicel Corporation, 2-hydroxymethacrylate 1 mol caprolactone addition monomer, trade name), Plaxel FM2 (Corporation Daicel, 2-hydroxyethyl methacrylate 1 mol caprolactone addition monomer, Product name), Plaxel FA1 (manufactured by Daicel Corporation, 2-hydroxyethyl acrylate 1m ol caprolactone addition monomer, product name), Plaxel FA2D (manufactured by Daicel Corporation, 2-Hydroxyethyl acrylate 1 mol caprolactone addition monomer (trade name) is preferred. Among them, 2-hydroxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate Dipropyl acrylate and 4-hydroxybutyl (meth)acrylate are particularly preferred.

[0026] The composition ratio of the monomer (a1) in the acrylic polyol is The amount is usually 5 to 70% by mass, preferably 10 to 65% by mass, based on 100% by mass of the structural unit. More preferably, it is 14 to 58% by mass, further preferably, it is 18 to 51% by mass, and most preferably, it is 2 The range of mass is 5 to 52. By using within this range, it is possible to obtain an acrylic acid having the desired hydroxyl value. Polyols can be obtained.

[0027] Monomer (a2) having an ethylenically unsaturated bond with one or more hydroxyl groups in one molecule is Examples of suitable compounds include, but are not limited to, the following compounds: (Meth)acrylic acid, itaconic acid, citraconic acid, maleic acid, monomethyl maleate , Monobutyl maleate, Monomethyl itaconate, Monobutyl itaconate, Vinyl benzoin Acid, Monohydroxyethyl (meth)acrylate, Monohydroxyethyl tetrahydrophthalate Hydroxyethyl (meth)acrylate, Monohydroxypropyl tetrahydrophthalate ( Meth)acrylate, 5-methyl-1,2-cyclohexanedicarboxylic acid monohydroxy Ethyl (meth)acrylate, Monohydroxyethyl (meth)acrylate phthalate, Phthalic acid Monohydroxypropyl talc (meth)acrylate, Monohydroxyethyl maleate (Meth)acrylate, Hydroxypropyl Maleate (Meth)acrylate, Tetrahydantoyl Monohydroxybutyl (meth)acrylate dorophthalate, etc. By including a monomer having an acid group, the curing of the coating composition can be accelerated.

[0028] The content ratio of the monomer (a2) having an acid group in the acrylic polyol is It is usually 0.1 to 15 mass%, preferably 0. 5 to 13 mass%, more preferably 0.7 to 10 mass%, and further preferably 1.0 to 7.0 % by mass, and most preferably in the range of 2.0 to 6.0 by mass. %, the reactivity is decreased and sufficient scratch resistance cannot be obtained. If the amount is more than 15% by mass, the reaction rate becomes too fast and a sufficient pot life cannot be obtained.

[0029] As the other copolymerizable ethylenically unsaturated monomer (a3), various ones can be used. Examples of the monomers include the following: Methyl (meth)acrylate, Ethyl (meth)acrylate, n-Propylene (meth)acrylate (meth)acrylate, isopropyl, n-butyl, (meth)acrylate isobutyl acrylate, t-butyl (meth)acrylate, isoamyl (meth)acrylate, (Meth)acrylic acid hexyl, (meth)acrylic acid 2-ethylhexyl, (meth)acrylic Octyl (meth)acrylate, Isooctyl (meth)acrylate, Nonyl (meth)acrylate, Isononyl acrylate, (meth) decyl acrylate, (meth) isodecyl acrylate, (meth) p) Lauryl acrylate, tridecyl (meth)acrylate, hexadeca (meth)acrylate (Meth)acrylate, Stearyl (Meth)acrylate, Isostearyl (Meth)acrylate, (Meth)acrylate Docosyl acrylate, Phenyl (meth)acrylate, Benzyl (meth)acrylate, (Meth)acrylate ) Cyclohexyl acrylate, (meth) tetrahydrofurfuryl acrylate, (meth) a Isobornyl acrylate, 3,5,5-trimethylcyclohexyl (meth)acrylate, ( Dicyclopentanyl (meth)acrylate, Dicyclopentenyl (meth)acrylate, (Meth ) Dicyclopentenyloxyethyl acrylate, terpene acrylate and its derivatives, water Additive rosin acrylate and its derivatives, hydrocarbon group-containing (meth)acrylic acid esters; (Meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diethyl N-isopropyl(meth)acrylamide, Nt-butyl(meth)acrylamide (Meth)acrylamide, Nt-octyl (meth)acrylamide, N-methylol ( (Meth)acrylamide, Hydroxyethyl (Meth)acrylamide, N-Methoxymethyl (Meth)acrylamide, N-butoxymethyl (meth)acrylamide, diacetone ( (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylamide, N,N -Dimethylaminopropyl (meth)acrylamide, N-vinylacetamide, maleic acid Amide bond-containing chain vinyl such as acid amide, N,N'-methylenebis(meth)acrylamide monomer, (meth)acryloylmorpholine, N-vinylpyrrolidone, N-vinyl-ε - Amide bond-containing cyclic vinyl monomers such as caprolactam and maleimide Vinyl monomers; Dimethyl maleate, dibutyl maleate, dimethyl fumarate, dibutyl fumarate, di Unsaturated dicarboxylic acids such as butyl itaconate and diperfluorocyclohexyl fumarate Diester monomers; (Meth)acrylate, glycidyl α-ethylacrylate, (meth)acrylate Epoxy group-containing vinyl monomers such as 3,4-epoxybutyl acetate; Dimethylaminoethyl (meth)acrylate, Diethylaminoethyl (meth)acrylate Amino group-containing (meth)acrylic acid ester monomers such as acrylate; Divinylbenzene, ethylene glycol di(meth)acrylate, 1,3-butylene glycol Ricohyl di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1 ,6-Hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol Di(meth)acrylate, polyethylene glycol di(meth)acrylate, triplyl Ethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate 1,9-Nonanediol di(meth)acrylate, 1,10-Decanediol di(meth)acrylate Trimethylolpropane tri(meth)acrylate, pentaerythritol Dipentaerythritol tetra(meth)acrylate, Dipentaerythritol hexa(meth)acrylate Allyl (meth)acrylate, triallyl cyanurate, diallyl maleate, poly Multifunctional vinyl monomers such as propylene glycol diallyl ether; Heterocyclic monomers such as vinylpyridine and vinylcarbazole; 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane Propylmethyldiethoxysilane, 3-(meth)acryloxypropyltriethoxysilane , 3-acryloxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyltrimethoxysilane Monomers containing silane coupling agents such as ethoxysilane; Trimethylsilyl (meth)acrylate, Triethylsilyl (meth)acrylate, Tri-n-propylsilyl (meth)acrylate, Tri-n-butylsilyl (meth)acrylate acrylate, tri-n-amylsilyl (meth)acrylate, tri-n-hexylsilyl (meth)acrylate (meth)acrylate, triphenylsilyl (meth)acrylate, tri-p-methylphenyl Tribenzylsilyl (meth)acrylate, Tribenzylsilyl (meth)acrylate, Triisopropylsilyl Triisobutylsilyl (meth)acrylate, Triisobutylsilyl (meth)acrylate, Triisobutylsilyl (meth)acrylate -s-Butylsilyl(meth)acrylate, Tri-2-methylisopropylsilyl(meth)acrylate ) acrylate, tri-t-butylsilyl (meth)acrylate, ethyldimethylsilyl (Meth)acrylate, n-butyldimethylsilyl (meth)acrylate, diisopropyl n-Butylsilyl (meth)acrylate, dicyclohexylphenylsilyl (meth)acrylate Acrylate, t-butyldiphenylsilyl (meth)acrylate, triisopropylsilyl methyl silyl maleate, triisopropylsilyl amyl maleate, tri-n-butylsilyl -n-Butyl maleate, t-butyldiphenylsilyl methyl maleate, t-butyldiphenyl Nylsilyl-n-butyl maleate, triisopropylsilyl methyl fumarate, triisopropylsilyl Propylsilyl amyl fumarate, tri-n-butylsilyl-n-butyl fumarate, t -Butyldiphenylsilyl methyl fumarate, t-butyldiphenylsilyl-n-butyl Fumarate, Silaplane FM-0711 (JNC Corporation, trade name), Silaplane FM-0721 (JNC Corporation, product name), Silaplane FM-0725 (JNC (manufactured by JNC Corporation, product name), Silaplane TM-0701 (manufactured by JNC Corporation, product name), Laplane TM-0701T (JNC Corporation, product name), X-22-174ASX (Fujitsu (manufactured by Etsu Chemical Co., Ltd., product name), X-22-174BX (manufactured by Shin-Etsu Chemical Co., Ltd., product name) ), KF-2012 (Shin-Etsu Chemical Co., Ltd., trade name), X-22-2426 (Shin-Etsu Chemical X-22-2404 (manufactured by Shin-Etsu Chemical Co., Ltd., product name), etc. an organosilyl group-containing monomer other than a silane coupling agent-containing monomer; Vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, chlorotrifluoro Halogenated olefins such as ethylene; Isocyanato group-containing monomers such as 2-isocyanatoethyl (meth)acrylate; 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3,3-penta Fluorophenyl (meth)acrylate, 2-(perfluorobutyl)ethyl (meth)acrylate Acrylate, 3-(perfluorobutyl)-2-hydroxypropyl (meth)acrylate 2-(perfluorohexyl)ethyl (meth)acrylate, 3-perfluorohexyl Sil-2-hydroxypropyl (meth)acrylate, 3-(perfluoro-3-methyl Butyl)-2-hydroxypropyl (meth)acrylate, 2,2,3,3-tetrafluoroethylene 1H,1H,5H-Octafluoropentyl (meth)acrylate ) acrylate, 1H,1H,5H-octafluoropentyl (meth) methacrylate, 1H,1H,2H,2H-Tridecafluorooctyl (meth)acrylate, 1H-1- (Trifluoromethyl)trifluoroethyl(meth)acrylate, 1H,1H,3H- Hexafluorobutyl (meth)acrylate, 1,2,2,2-tetrafluoro-1-( Fluorine-containing monomers such as (but not including) halogenated trifluoromethylethyl (meth)acrylate olefins excluded); 1-Butoxyethyl (meth)acrylate, 1-(cyclohexyloxy)ethyl meth acrylate), 2-tetrahydropyranyl (meth)acrylate, etc. One monomer; 4-Methacryloyloxybenzophenone, styrene, α-methylstyrene, vinyl thio Vinyl monomers such as olefins, (meth)acrylonitrile, vinyl acetate, and vinyl propionate etc. When these monomers are used, the monomers may be one type or two or more types. good.

[0030] As the monomer (a3), a hydrocarbon-containing acrylic monomer is used because of the ease of designing the SP value and Tg. Acid esters are preferred, and among these, methyl (meth)acrylate and ethyl (meth)acrylate are preferred. , (meth)acrylate n-propyl, (meth)acrylate isopropyl, (meth)acrylate n-Butyl acrylate, isobutyl (meth)acrylate, cyclohexyl (meth)acrylate xyl, (meth)acrylate 2-ethylhexyl (meth)acrylate, (meth)acrylate lauryl Monomers having an alkyl group having 1 to 13 carbon atoms, such as stearyl acrylate, are preferred, and More preferred are monomers having an alkyl group having 1 to 8 carbon atoms.

[0031] From the viewpoint of weather resistance, among the monomers (a3), a monomer having an aromatic group, for example, styrene, The content of acrylic polyol structural units is 10% or more. It is preferably in the range of 0 to 30% by mass, and more preferably in the range of 0 to 20% by mass. It is more preferable that the monomer is in the range of 1 to 3, and further preferably that the monomer is free of aromatic monomers.

[0032] In the method for producing acrylic polyol, for example, a solution polymerization method, a suspension polymerization method, a bulk polymerization method, The polymerization method may be a known polymerization method such as a polymerization method using an acrylic acid to be produced, or an emulsion polymerization method. From the viewpoints of productivity of polyols and ease of use as coating compositions, a solvent that uses polymerization solvents was used. The liquid polymerization method is preferred. This polymerization method, for example, comprises supplying a polymerization solvent, a monomer, and a radical polymerization initiator into a polymerization vessel. and polymerizing it at a predetermined reaction temperature.

[0033] The radical polymerization initiator used in the radical polymerization is, for example, benzoyl peroxide. organic peroxides such as di-t-butyl peroxide; 2,2'-azobisbutyronitrile , 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4- Methoxy-2,4-dimethylvaleronitrile and other azo compounds are also included. These radical polymerization initiators may be used alone or in combination of two or more. The radical polymerization initiator may be used in an amount of 100% by mass of all the structural units of the acrylic polyol. It is preferable to use it in the range of 0.01 to 5 mass % based on the total mass of the material.

[0034] In addition, during radical polymerization, the weight average molecular weight of the (meth)acrylic resin is controlled. For this purpose, a chain transfer agent can be used. Examples of the chain transfer agent include butanethiol. thiol, octanethiol, decanethiol, dodecanethiol, hexadecanethiol, Octadecanethiol, cyclohexyl mercaptan, thiophenol, thioglycol Octyl mercaptopropionate, Octyl 2-mercaptopropionate, Octyl 3-mercaptopropionate mercaptopropionic acid 2-ethylhexyl ester, thioglycolic acid 2-ethyl Hexyl, butyl-3-mercaptopropionate, mercaptopropyl trimethoxysilane Ran, methyl-3-mercaptopropionate, 2,2-(ethylenedioxy)diethane Thiol, ethanethiol, 4-methylbenzenethiol, 2-mercaptoethyl octanoate ethyl ester, 1,8-dimercapto-3,6-dioxaoctane, decane trithiol , dodecyl mercaptan, diphenyl sulfoxide, dibenzyl sulfide, 2,3-di Methylcapto-1-propanol, mercaptoethanol, thiosalicylic acid, thioglyceryl mercaptoacetate, thioglycolic acid, 3-mercaptopropionic acid, thiomalic acid, mercaptoacetic acid Examples of thiol compounds include mercaptosuccinic acid, 2-mercaptoethanesulfonic acid, and other thiol compounds. These may be used alone or in combination of two or more.

[0035] The amount of the chain transfer agent used is 0.1% by mass based on 100% by mass of all the constituent units of the acrylic polyol. The content is preferably from 0.5 to 25% by mass, more preferably from 0.5 to 20% by mass, and even more preferably from 1.0 to 15% by mass. More preferred.

[0036] Examples of the polymerization solvent that can be used in the solution polymerization method include the following solvents. Aromatic solvents such as toluene, xylene, and other high boiling aromatic solvents; ethyl acetate, Butyl acetate, propylene glycol monomethyl ether acetate, and cellosolve acetate Ester solvents such as ethyl ketone, methyl isobutyl ketone, cyclopentane Ketone solvents such as cyclohexane, cycloheptanone, and cyclohexanone; methyl alcohol , ethyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol Alcohols such as propylene glycol monomethyl ether and diacetone alcohol Solvents based on alcohol: SS-100 (product name, manufactured by JXTG Nippon Oil & Energy Corporation), and cyclohexafluoropropane The polymerization solvent may be used alone or in combination of two or more. It may also be used in combination.

[0037] <Polyester polyol> Polyester polyol is a polymer that consists mainly of polycarboxylic acids and polyhydric alcohols. It is a polycondensation product of alcohol components.

[0038] The acid components include terephthalic acid, isophthalic acid, phthalic acid or its anhydride, 2,6- Naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, etc. Aromatic dicarboxylic acids and their anhydrides; succinic acid, adipic acid, azelaic acid, sebacic acid Aliphatic dicarboxylic acids such as dicarboxylic acid, dodecanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid In addition, lactones such as γ-butyrolactone and ε-caprolactone are also available. and the corresponding hydroxycarboxylic acids and aromatic compounds such as p-oxyethoxybenzoic acid. Oxymonocarboxylic acids; Trivalent or higher carboxylic acids such as trimellitic acid, trimesic acid, and pyromellitic acid The polycarboxylic acid may include a polyvalent carboxylic acid.

[0039] The alcohol components are ethylene glycol, 1,3-propanediol, 1,4- Butanediol, 1,5-pentanediol, 1,5-hexanediol Diethylene glycol, triethylene glycol, 1,4-cyclohexanediol 1,4-Cyclohexanedimethanol, Bisphenol A alkylene oxide adduct In addition to bisphenol S alkylene oxide adducts, 1,2-propanediol, Pentyl glycol, 1,2-butanediol, 1,3-butanediol, 1,2-pentyl glycol 2,3-pentanediol, 1,4-pentanediol, 1,4-hexanediol Sandiol, 2,5-Hexanediol, 3-Methyl-1,5-Pentanediol, 1 Aliphatic glycols with side chains such as 1,2-dodecanediol, 1,2-octadecanediol, etc. The alcohol component is also trimethylolpropane, glycerin, pentane, It may contain a polyhydric alcohol having three or more valences, such as rhythritol.

[0040] Polyester polyols are those that have trivalent or higher alcohol or carboxylic acid groups. Using monomers, we have developed hyperbranched polyols with random dendritic structures and The regular tree-like structure obtained by the stepwise condensation reaction using mers is shown in Fig. A dendrimer polyol having the above structure can be used. Boltorn (registered trademark) H20 (hydroxyl value 490 to 520 mg KOH / g) manufactured by Boltorn Corporation Molecular weight 2100 (catalog value)), Boltorn (registered trademark) H311 (hydroxyl value 2 30~260mgKOH / g, molecular weight 5300 (catalog value), Boltorn (registered Trademark) H2004 (Hydroxyl value 150-125mgKOH / g, molecular weight 3100 (catalog Boltorn (registered trademark) P500 (hydroxyl value 560-630 mg KOH / g, molecular weight 1800 (catalog value), Boltorn (registered trademark) P1000 (water Acid value 430~630mgKOH / g, molecular weight 1500 (catalog value), Boltor n(registered trademark) U3000 (hydroxyl value 15 mg KOH / g, molecular weight 6500 (catalog value), Boltorn (registered trademark) W3000 (hydroxyl value 15 mg KOH / g, molecular weight 10,000 (catalog value), Basonol® HPE manufactured by BASF 1170B (hydroxyl value 280 mg KOH / g, molecular weight 1800 (catalog value)), Bas Onol® HPE 021 (hydroxyl value 190 mg KOH / g, molecular weight 140 0 (catalog value)), Basonol (registered trademark) HPE 026 (hydroxyl value 180m gKOH / g, molecular weight 2600 (catalog value), Basonol® HPE 046 (hydroxyl value 250 mg KOH / g, molecular weight 4800 (catalog value)) can be.

[0041] The content of the polyol (A) in the coating composition of the present invention is, based on the total solid content of the base material, The amount of the polyol (A) is preferably 10 to 90% by mass, and more preferably 20 to 80% by mass. If it is less than 10 mass%, the scratch resistance and chemical resistance of the cured product will decrease. If this occurs, the pot life of the coating composition will be shortened.

[0042] <Reaction adjuster (B)> The base material of the coating composition of the present invention contains a reaction modifier (B). The reaction modifier (B) acts as a hardener with the base material. After mixing the curing agent, the isocyanate groups of the polyisocyanate (C) or the polyol (A) This can act on the hydroxyl groups of the urethane-forming reaction, thereby providing a good It is possible to provide a coating composition having a long pot life. In particular, the nucleophilic reactivity is reduced due to solvation, and the nucleophilic reaction between the isocyanate group and the hydroxyl group of polyol (A) is also reduced. By having a functional group that inhibits the reaction, the urethanization reaction can be inhibited.

[0043] For this reason, it is recommended to use an isocyanate group blocking agent as the reaction regulator (B). Specifically, phenol, cresol, xylenol, and nitrophenol are suitable. , ethylphenol, hydroxydiphenyl, butylphenol, isopropylphenol Phenols such as phenyl, nonylphenol, octylphenol, and methyl hydroxybenzoate Series: ε-caprolactam, δ-valerolactam, γ-butyrolactam, β-propiolactam Lactams such as tam; methanol, ethanol, propyl alcohol, butyl alcohol , amyl alcohol, lauryl alcohol, diacetone alcohol, ethylene glycol ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether diethylene glycol monomethyl ether, diethylene glycol monobutyl ether ethyl ether, propylene glycol monomethyl ether, methoxybutanol, etc. Alcohol-based: benzyl alcohol, glycolic acid, methyl glycolate, glycolic acid Ethyl, butyl glycolate, lactic acid, methyl lactate, ethyl lactate, butyl lactate, methylol Urea, Methylolmelamine, 2-Hydroxyethyl acrylate, 2-Hydroxyethyl Other alcohol-based compounds such as methacrylates; formamide oxime, acetamide oxime oxime, acetoxime, methyl ethyl ketoxime, diacetyl monoxime, benzophenone Oximes such as non-oxime and cyclohexane oxime; dimethyl malonate, malonic acid Malonic acid esters such as diethyl esters, acetoacetates such as ethyl acetoacetate and methyl acetoacetate Acid esters, acetylacetone and other β-dicarbonyl compounds; butyl mercaptan, t- Butyl mercaptan, hexyl mercaptan, t-dodecyl mercaptan, 2-mercaptan Tribenzothiazole, thiophenol, methylthiophenol, ethylthiophenol, etc. Mercaptans: acetanilide, acetaniside, acetotoluide, acrylamide Acid amides such as amides, methacrylamides, acetate amides, stearic acid amides, and benzamides Imide-based compounds such as succinimide, phthalimide, and maleimide; Diphenylamine , phenylnaphthylamine, xylidine, N-phenylxylidine, carbazole, aniline Amines such as phosphorus, naphthylamine, butylamine, dibutylamine, and butylphenylamine imidazole, 2-ethylimidazole and other imidazoles; urea, thiourea, ethylenediamine Ureas such as ethyleneurea, ethylenethiourea, and diphenylurea; N-phenylcarbamic acid Carbamic acid esters such as phenyl; imine-based compounds such as ethyleneimine and propyleneimine Sulfite-based compounds such as sodium bisulfite and potassium bisulfite; azole-based compounds, etc. The azole compounds include pyrazole, 3,5-dimethylpyrazole, 3-methylpyrazole, 4-Benzyl-3,5-dimethylpyrazole, 4-nitro-3,5-dimethylpyrazole Tylpyrazole, 4-bromo-3,5-dimethylpyrazole, 3-methyl-5-phenyl Pyrazoles or pyrazole derivatives such as pyrazole; imidazole, benzimidazole, Imidazoles such as 2-methylimidazole, 2-ethylimidazole, and 2-phenylimidazole Imidazole or imidazole derivatives; 2-methylimidazoline, 2-phenylimidazoline and imidazoline derivatives such as phenylalanine.

[0044] The reaction regulator (B) is a substance that volatilizes together with the solvent during the curing process of the coating composition and is also isopropyl alcohol. Even if it reacts with the cyanate group and is incorporated into the coating, it does not impair scratch resistance or weather resistance. For this reason, alcohol-based, oxime-based, and β-dicarbonyl compound-based compounds are preferred. Alcohol-based and β-dicarbonyl compound-based solvents are preferred, and alcohol-based and β-dicarbonyl compound-based solvents are even more preferred. In the system, isopropyl alcohol, which is an alcohol having a secondary hydroxyl group, Butyl alcohol and propylene glycol monomethyl ether are particularly preferred. In the case of isocyanate compounds, due to their volatility and the stability of the products after reaction with isocyanate groups, Cetylacetone and malonic acid esters are particularly preferred.

[0045] The content of the reaction regulator (B) is determined based on the isocyanate content of the polyisocyanate (C) used as the curing agent. The amount is preferably 0.1 to 100 mol %, more preferably 1.0 to 70 mol %, based on the aryl group. It is preferable that the content is within the range of 10 to 40 mol %. This suppresses the reaction that occurs after mixing, and allows the viscosity and physical properties of the coating film to be maintained at a good level.

[0046] <Polyisocyanate (C)> The polyisocyanate (C) in the present invention reacts with the hydroxyl groups of the polyol (A). This forms a urethane bond, increasing the crosslink density of the cured film, improving weather resistance, chemical resistance and Improve the hardness of the material.

[0047] Polyisocyanate (C) includes hexamethylene diisocyanate, dicyclohexyl Silmethane diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanato) (trimethyl)cyclohexane, 4,4-dicyclohexyl diisocyanate, etc. Socyanate, biuret compound synthesized using the above difunctional isocyanate as starting material , trimethylolpropane adduct, isocyanurate, allophanate, etc. Examples of suitable isocyanates include those having a higher molecular weight than 10 ...

[0048] As an isocyanate with three or more functional groups, hexamethylene diisocyanate manufactured by Asahi Kasei Corporation is used. Duranate burette (trade name: Duranate (registered trademark; the same applies below) 24A-100 ), hexamethylene diisocyanate adduct (product name: Duranate P-301- 75E), hexamethylene diisocyanate isocyanurate (product name: Durane Polyfunctional isocyanate (product name: Duranate MHG-80B) , blocked isocyanate (product name: Duranate MF-K60X), manufactured by Mitsui Chemicals Trimethylolpropane adduct of 1,3-bis(isocyanatomethyl)cyclohexane (Takenate (registered trademark) D-120N), 1,3-bis(isopropyl alcohol) Isocyanurate of (cyanatomethyl)cyclohexane (product name: Takenate D-127 N), isophorone diisocyanate trimethylolpropane adduct (product name: Take Hexamethylene diisocyanate manufactured by Sumika Covestro Urethane Co., Ltd. Allophanate form (product name: Desmodur (registered trademark; the same applies below) XP2679) , EVONIK's isocyanurate derivative of isophorone diisocyanate (product name: Des Module T-1890 / 100) etc.

[0049] Polyisocyanate (C) increases the crosslink density of the cured film and improves weather resistance and stain resistance. In order to improve the hardness of the cured film, tri- or higher-functional isocyanates are preferred. The socyanate (C) may be used alone or in combination of two or more kinds.

[0050] The mixing ratio of polyisocyanate (C) and polyol (A) is N CO / OH [number of moles of isocyanate groups in polyisocyanate (C) / polyol] The mole number of hydroxyl groups in (A) is preferably 0.5 or more and 2.0 or less. Preferably, the ratio is 0.7 or more and 1.8 or less, more preferably, 0.8 or more and 1.5 or less. .

[0051] If the equivalent ratio of the isocyanate group of the polyisocyanate (C) is equal to or greater than the lower limit, By using such a composition, the curing rate of the resin composition can be increased, and the cured film of the resin composition can be formed more easily. The crosslink density of the cured film increases, and the hardness and water resistance of the cured film tend to improve. When the equivalent ratio of the isocyanate group of the above-mentioned copolymer is equal to or less than the upper limit, the curing of the resin composition is The drying properties and adhesion after the film is formed tend to be improved.

[0052] <Inorganic fine particles (D)> The inorganic fine particles (D) in the present invention have on the surface a hydroxyl group or an isocyanate group-reactive group. Has a functional group.

[0053] The inorganic fine particles (D) have on their surfaces functional groups capable of reacting with hydroxyl groups or isocyanate groups. As a result, the inorganic fine particles (D) are fixed in the resin component, improving the abrasion resistance of the cured film. .

[0054] Examples of functional groups that can react with hydroxyl groups include isocyanate groups, epoxy groups, and carboxyl groups. In addition, examples of functional groups that can react with an isocyanate group include mercapto groups, hydroxyl groups, and the like. Examples of such groups include an amino group, a carboxyl group, and an isocyanate group.

[0055] Since the reactivity with the hydroxyl group or isocyanate group of the inorganic fine particles (D) is high, Functional groups that can react with socyanate groups include mercapto groups, isocyanate groups, and amino groups. groups and epoxy groups are preferred.

[0056] The inorganic fine particles (D) have, for example, a functional group capable of reacting with a hydroxyl group or an isocyanate group on the surface. Silica particles that do not have a silane having a functional group capable of reacting with a hydroxyl group or an isocyanate group are This can be achieved by surface treatment with a coupling agent.

[0057] As silica particles having no functional group capable of reacting with a hydroxyl group or an isocyanate group on the surface thereof, For example, methanol-dispersed silica sol (MA-ST, MA-ST-M) manufactured by Nissan Chemical Co., Ltd. ), Isopropyl alcohol dispersed silica sol (IPA-ST, IPA-ST-L, IPA -ST-ZL, IPA-ST-UP), Ethylene glycol dispersed silica sol (EG-ST , EG-ST-L), dimethylacetamide dispersed silica sol (DMAC-ST, DMAC -ST-L), xylene / butanol dispersion silica sol (XBA-ST), methyl ethyl ketone Ton dispersion silica sol (MEK-ST, MEK-ST-L, MEK-ST-ZL, MEK- ST-UP), methyl isobutyl ketone dispersed silica sol (MIBK-ST), propylene Commercially available products such as glycol monomethyl ether acetate dispersed silica sol (PMA-ST) It can be used.

[0058] As a silane coupling agent having a functional group capable of reacting with a hydroxyl group or an isocyanate group For example, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3- Glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane Lan, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyl Silane compounds having a glycidyl group such as diethoxysilane, 1-mercaptomethyltrimethylsilane, Toxicsilane, 1-mercaptomethylmethyldimethoxysilane, 1-mercaptomethyl Diethoxysilane, 1-mercaptomethyl methyldiethoxysilane, 3-mercaptopropane Pyrtrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldimethoxysilane 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldiethoxysilane, etc. Silane compounds with mercapto groups, N-2-(aminoethyl)-3-aminopropyl mercapto groups Tyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane Lan, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane Silane compounds having amino groups such as 3-isocyanatepropyltriethoxysilane, etc. Examples include:

[0059] In addition, as a commercially available dispersion liquid of inorganic fine particles (D), for example, MEK manufactured by Nissan Chemical Industries, Ltd. -EC-2130Y, MEK-EC-6150P, MEK-EC-7150P, etc. can be. The inorganic fine particles (D) may be used alone or in combination of two or more kinds.

[0060] The content of the inorganic fine particles (D) in the coating composition of the present invention is, based on the total solid content of the base material, The content is preferably from 1.0 to 30% by mass, and more preferably from 5.0 to 20% by mass. If the amount is less than 1.0 mass%, the scratch resistance of the cured product decreases, and if it is 30 mass% or more, This will deteriorate the curing properties of the coating composition.

[0061] The average particle size of the inorganic fine particles (D) is preferably 2 nm or more and 300 nm or less, and more preferably 2 nm or more and 300 nm or less. More preferably, the thickness is 200 nm or less, and even more preferably, the thickness is 4 nm or more and 100 nm or less. A value of at most 50 nm is particularly preferred. When the average particle size of the inorganic fine particles (D) is equal to or more than the lower limit, the scratch resistance is likely to be improved. When the average particle size of the inorganic fine particles (D) is equal to or less than the upper limit, the cured film of the resin composition It is easier to maintain transparency.

[0062] The average particle size of the inorganic fine particles (D) is determined by the specific surface area measured by the BET adsorption method (JIS -Z8830) is used.

[0063] <Polycarbonate polyol (E)> The coating composition of the present invention contains, in addition to the polyol (A), a polycarbonate polyol (E). The polycarbonate polyol may contain a polycarbonate group in the molecule. It is acceptable as long as the terminal has two or more hydroxyl groups, but the terminal is either primary or secondary. In terms of weather resistance, the polycarbonate polyol (E ) is preferably an aliphatic polycarbonate polyol.

[0064] The aliphatic polycarbonate polyol is Kuraray Polyol (registered trademark) manufactured by Kuraray Co., Ltd. Registered trademark. The same applies below.) C-1090 (hydroxyl value 112 mg KOH / g, weight average molecular weight (Mw) 1000 (catalog value)), Kuraray Polyol C-2090 (hydroxyl value 56.1 mg·KOH / g, weight average molecular weight (Mw) 2000 (catalog value), Kuraray Polyol C-3090 (hydroxyl value 37 mg KOH / g, weight average molecular weight (Mw) 3000 ( (catalog value), Asahi Kasei Corporation's Duranol (registered trademark; the same applies below) T-5651 (hydroxyl group Value: 112mg KOH / g, weight average molecular weight (Mw): 1000 (catalog value), Durability: Nol T-5652 (hydroxyl value 56 mg KOH / g, weight average molecular weight (Mw) 2000) Catalog value), Duranol T-4691 (hydroxyl value 112mg KOH / g, weight average Average molecular weight (Mw) 1000 (catalog value), Duranol T-4692 (hydroxyl value 56 mg KOH / g, weight average molecular weight (Mw) 2000 (catalog value), Duranol T -4671 (Hydroxyl value 112 mg KOH / g, weight average molecular weight (Mw) 1000 (catalyst log value), Duranol G-4672 (hydroxyl value 56 mg KOH / g, weight average molecular weight weight (Mw) 2000 (catalog value), Duranol G-3450J (hydroxyl value 140m g·KOH / g, weight average molecular weight (Mw) 800 (catalog value), Duranol G-3 452 (hydroxyl value 56 mg KOH / g, weight average molecular weight (Mw) 2000 (catalog value )), Mitsubishi Chemical Corporation's Benebiol (registered trademark; the same applies below) NL1010DB (hydroxyl group Value: 112 mg KOH / g, weight average molecular weight (Mw): 1000 (catalog value), Beneb All NL2010DB (hydroxyl value 56 mg KOH / g, weight average molecular weight (Mw) 200 0 (catalog value)), Beneviol NL1000B (hydroxyl value 112 mg KOH / g, Weight average molecular weight (Mw) 1000 (catalog value), Beneviol NL2000B (hydroxyl Base value 56mg KOH / g, weight average molecular weight (Mw) 2000 (catalog value), Beneb All NL1050B (hydroxyl value 112 mg KOH / g, weight average molecular weight (Mw) 10 00 (catalog value)), Beneviol NL2050B (hydroxyl value 56 mg KOH / g, Weight average molecular weight (Mw) 2000 (catalog value)), Benebiol HS0840B (hydroxyl Base value 140mg KOH / g, weight average molecular weight (Mw) 800 (catalog value), Beneb All HS0850B (hydroxyl value 140 mg KOH / g, weight average molecular weight (Mw) 80 0 (catalog value), ETERNACOLL (registered trademark; the same applies below) UHC manufactured by Ube Industries 50-100 (hydroxyl value 112 mg KOH / g, weight average molecular weight (Mw) 1000 ( Catalog value), ETERNACOLL UHC50-200 (hydroxyl value 56 mg KOH / g, weight average molecular weight (Mw) 2000 (catalog value), ETERNACOLL UC -100 (hydroxyl value 112 mg KOH / g, weight average molecular weight (Mw) 1000 (catalog ETERNACOLL UM-90 (hydroxyl value 125 mg KOH / g, weight Examples include an average molecular weight (Mw) of 900 (catalog value).

[0065] The content of the polycarbonate polyol (E) in the coating composition of the present invention is the total amount of the base material. The content is preferably 5.0 to 50% by mass, more preferably 10 to 40% by mass, based on the solid content. The content is more preferably 5 to 35% by mass.

[0066] When the content of the polycarbonate polyol (E) is equal to or less than the upper limit, the abrasion resistance of the cured product is improved. When the content of the polycarbonate polyol (E) is equal to or more than the lower limit, If the coating is applied, the adhesion to the substrate is improved.

[0067] <Ultraviolet absorber (F)> In order to improve the weather resistance of the cured product, an ultraviolet absorber (F) is added to the main component of the coating composition. From the viewpoint of heat resistance, the molecular weight is preferably 500 or more. ) is a triazine-based, benzo-based, etc., from the viewpoint of good solubility in the composition and improvement of weather resistance. Triazoles, cyclic iminoesters, benzophenones, salicylic acid esters, or derived from a cyanoacrylate compound, and has a maximum absorption wavelength of 24 UV absorbents in the range of 0 to 380 nm are preferred.

[0068] The triazine-based ultraviolet absorber is not limited to the following, but may be, for example, 2- [4-([2-hydroxy-3-dodecyloxypropyl]oxy)-2-hydroxyphenyl phenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine and 2- [4-([2-hydroxy-3-tridecyloxypropyl]oxy)-2-hydroxy phenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine (T Inuvin (registered trademark) 400 (BASF), 2-[4,6-bis(2,4-dimethyl 3-(dodecyloxy)-1,3,5-triazin-2-yl -2-hydroxypropoxy]phenol), 2-(2,4-dihydroxyphenyl)- 4,6-bis-(2,4-dimethylphenyl)-1,3,5-triazine and (2-ethyl hexyl)-glycidic acid ester reaction product (Tinuvin® 405, B ASF), 2,4-bis "2-hydroxy-4-butoxyphenyl"-6-(2,4 -dibutoxyphenyl)-1,3-5-triazine (Tinuvin® 460 , manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazin-2-yl)- 5-[(Hexyl)oxy]-phenol (Tinuvin® 1577, BA SF Co., Ltd.), 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[ 2-(2-Ethylhexanoyloxy)ethoxy]-phenol (ADK STAB L A46, manufactured by ADEKA), 2-(2-hydroxy-4-[1-octyloxycarbonyl (ethoxy)phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triphenyl Examples of such antibacterial agents include Tinuvin (registered trademark) 479, manufactured by BASF.

[0069] Benzotriazole-based UV absorbers include, but are not limited to, the following: For example, 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(5-methyl 2-(2-hydroxy-5-tert-butyl-2-hydroxyphenyl)benzotriazole t-Butylphenyl)-5-chlorobenzotriazole, 2-(2-hydroxy-3,5 -Di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-5-t ert-butylphenyl)benzotriazole, 2-(2-hydroxy-4-octyloxy 2-[2'-hydroxy-5'-(methacryloyl)phenyl]benzotriazole 2-[2'-hydroxy-5'- (Methacryloyloxyethyl)phenyl]-2H-benzotriazole, 2-[2'- Hydroxy-5'-(methacryloyloxypropyl)phenyl]-2H-benzotriazole 2-[2'-hydroxy-5'-(methacryloyloxyhexyl)phenyl]zole -2H-benzotriazole, 2-[2'-hydroxy-3'-tert-butyl-5' -(methacryloyloxyethyl)phenyl]-2H-benzotriazole, 2-[2' -Hydroxy-5'-tert-butyl-3'-(methacryloyloxyethyl)phenyl 2-[2'-hydroxy-5'-(methacryloyl) 2-[2'-Hydroxyethyl)phenyl]-5-chloro-2H-benzotriazole [5'-(methacryloyloxyethyl)phenyl]-5-methoxy-2H-benzo Triazole, 2-[2'-hydroxy-5'-(methacryloyloxyethyl)phenyl 2-[2'-hydroxy-5'-(meth)- 5-tert-butyl-2H-benzotriazol-1,3-dimethyl-2H-phenyl-1H-acrylate 2-[2'-hydroxy-5'-(methacryloyloxyethyl)phenyl]-5- Nitro-2H-benzotriazole and other bisbenzotriazole-based UV absorbers Examples of such antibacterial agents include Dynesorb (registered trademark) T-33 (manufactured by Daiwa Kasei Co., Ltd.).

[0070] Examples of the cyclic imino ester-based ultraviolet absorbent include, but are not limited to, For example, 2-methyl-3,1-benzoxazin-4-one, 2-butyl-3,1-benzoxazin-4-one, Xazin-4-one, 2-phenyl-3,1-benzoxazin-4-one, 2-(1- or 2-naphthyl)-3,1-benzoxazin-4-one, 2-(4-biphenyl)- 3,1-Benzoxazin-4-one, 2-p-nitrophenyl-3,1-benzoxazin-4-one 2-m-nitrophenyl-3,1-benzoxazin-4-one, 2- p-Benzoylphenyl-3,1-benzoxazin-4-one, 2-p-methoxyphenyl 2-o-Methoxyphenyl-3,1-benzoxazin-4-one 2-cyclohexyl-3,1-benzoxazin-4-one, 2-p-(or m-)phthalimidophenyl-3,1-benzoxazin-4-one, N -phenyl-4-(3,1-benzoxazin-4-one-2-yl)phthalimide, N -Benzoyl-4-(3,1-benzoxazin-4-one-2-yl)aniline, N- Benzoyl-N-methyl-4-(3,1-benzoxazin-4-one-2-yl)aniline Phosphorus, 2-(p-(N-methylcarbonyl)phenyl)-3,1-benzoxazine-4 -one, 2,2'-bis(3,1-benzoxazin-4-one), 2,2'-ethylene Bis(3,1-benzoxazin-4-one), 2,2'-tetramethylenebis(3,1 -benzoxazin-4-one), 2,2'-decamethylenebis(3,1-benzoxazin-4-one) Zin-4-one, 2,2'-p-phenylenebis(3,1-benzoxazin-4-one) ), 2,2'-m-phenylenebis(3,1-benzoxazin-4-one), 2,2' -(4,4'-diphenylene)bis(3,1-benzoxazin-4-one), 2,2' -(2,6- or 1,5-naphthylene)bis(3,1-benzoxazin-4-one), 2,2'-(2-methyl-p-phenylene)bis(3,1-benzoxazin-4-one) ), 2,2'-(2-nitro-p-phenylene)bis(3,1-benzoxazine-4- 2,2'-(2-chloro-p-phenylene)bis(3,1-benzoxazine- 4-one), 2,2'-(1,4-cyclohexylene)bis(3,1-benzoxazine -4-one), 1,3,5-tri(3,1-benzoxazin-4-one-2-yl)be Benzene, 1,3,5-tri(3,1-benzoxazin-4-one-2-yl)naphthalene 2,4,6-tri(3,1-benzoxazin-4-one-2-yl)naphthalene, 2,8-Dimethyl-4H,6H-benzo(1,2-d;5,4-d')bis(1,3)- Oxazine-4,6-dione, 2,7-dimethyl-4H,9H-benzo(1,2-d;4 ,5-d') Bis(1,3)-oxazine-4,9-dione, 2,8-diphenyl-4H ,8H-benzo(1,2-d;5,4-d')bis(1,3)-oxazine-4,6-di , 2,7-diphenyl-4H,9H-benzo(1,2-d;4,5-d')bis(1 ,3)-Oxazine-4,6-dione, 6,6'-bis(2-methyl-4H,3,1-benzyl 6,6'-bis(2-ethyl-4H,3,1-benzoxazin-4-one), sazin-4-one), 6,6'-bis(2-phenyl-4H,3,1-benzoxazine -4-one), 6,6'-methylenebis(2-methyl-4H,3,1-benzoxazine -4-one), 6,6'-methylenebis(2-phenyl-4H,3,1-benzoxazine 6,6'-ethylenebis(2-methyl-4H,3,1-benzoxazine 6,6'-ethylenebis(2-phenyl-4H,3,1-benzoxa din-4-one), 6,6'-butylenebis(2-methyl-4H,3,1-benzoxa 6,6'-butylenebis(2-phenyl-4H,3,1-benzoxidine) sazin-4-one), 6,6'-oxybis(2-methyl-4H,3,1-benzoxa din-4-one), 6,6'-oxybis(2-phenyl-4H,3,1-benzoxa 6,6'-sulfonylbis(2-methyl-4H,3,1-benzoxidine-4-one) Sazin-4-one), 6,6'-sulfonylbis(2-phenyl-4H,3,1-benzo oxazin-4-one), 6,6'-carbonylbis(2-methyl-4H,3,1-benzoxazin-4-one) zooxazin-4-one), 6,6'-carbonylbis(2-phenyl-4H,3,1- Benzoxazin-4-one), 7,7'-methylenebis(2-methyl-4H,3,1- Benzoxazin-4-one), 7,7'-methylenebis(2-phenyl-4H,3,1 -benzoxazin-4-one), 7,7'-bis(2-methyl-4H,3,1-benzo oxazin-4-one), 7,7'-ethylenebis(2-methyl-4H,3,1-benzo oxazin-4-one), 7,7'-oxybis(2-methyl-4H,3,1-benzoxazin-4-one) Xazin-4-one), 7,7'-sulfonylbis(2-methyl-4H,3,1-benzoxazin-4-one) oxazin-4-one), 7,7'-carbonylbis(2-methyl-4H,3,1-benzoxazine 6,7'-bis(2-methyl-4H,3,1-benzoxazin-4-one), 6,7'-bis(2-phenyl-4H,3,1-benzoxazine- 4-one, 6,7'-methylenebis(2-methyl-4H,3,1-benzoxazine-4 -one), 6,7'-methylenebis(2-phenyl-4H,3,1-benzoxazine- 4-one).

[0071] Benzophenone-based UV absorbers (benzophenone-based compounds), oxybenzophenone-based Examples of ultraviolet absorbents (oxybenzophenone compounds) include 2,4-dihydroxybenzophenone. Dibenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4 -Methoxybenzophenone-5-sulfonic acid (anhydrous and trihydrate), 2-hydroxy-4- Octyloxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 4-benzyloxy-2-hydroxybenzophenone, 2,2'-dihydroxy-4-methyl Toxicbenzophenone (product name "KEMISORB111", manufactured by Chemipro Chemical Co., Ltd.) , 2,2',4,4'-tetrahydroxybenzophenone (product name "SEESORB10 6", manufactured by Shipro Chemical Co., Ltd.), 2,2'-dihydroxy-4,4-dimethoxybenzofuran Examples include phenone.

[0072] Examples of salicylic acid ester-based ultraviolet absorbents (salicylic acid ester-based compounds) include , phenyl-2-acryloyloxybenzoate, phenyl-2-acryloyloxy -3-methylbenzoate, phenyl-2-acryloyloxy-4-methylbenzoate , phenyl-2-acryloyloxy-5-methylbenzoate, phenyl-2-acryloyloxy-5-methylbenzoate aryloxy-3-methoxybenzoate, phenyl-2-hydroxybenzoate, Phenyl-2-hydroxy-3-methylbenzoate, Phenyl-2-hydroxy-4-methylbenzoate phenyl 2-hydroxy-5-methylbenzoate, phenyl 2- Hydroxy-3-methoxybenzoate, 2,4-di-tert-butylphenyl-3, 5-Di-tert-butyl-4-hydroxybenzoate (Tinuvin®) 120, manufactured by BASF).

[0073] Cyanoacrylate-based ultraviolet absorbers (cyanoacrylate-based compounds) include, for example: , alkyl-2-cyanoacrylate, cycloalkyl-2-cyanoacrylate, alkenyl Alkoxyalkyl-2-cyanoacrylate, alkenyl-2-cyanoacrylate, alkenyl quinyl-2-cyanoacrylate and the like. These compounds may be used alone or in combination of two or more.

[0074] Among these, it is said to have particularly high UV absorption and excellent appearance when cured into a film. From the viewpoint of the above, triazine-based and benzotriazole-based compounds are more preferable, and triazine-based compounds are more preferable. It is more preferable that the isocyanate group of the polyisocyanate (C) in the coating composition is reacted with the isocyanate group of the polyisocyanate (C). In order to prevent chipping from the coating film over a long period of time, non-phenolic hydroxyl groups are used. UV absorbers having a group are preferred, particularly 2-[4-([2-hydroxy-3-dodecyl Oxypropyl]oxy)-2-hydroxyphenyl]-4,6-bis(2,4-dimethyl 2-[4-([2-hydroxy-3-tridecylphenyl)-1,3,5-triazine and [2,4-dimethylaminopropyl]oxy)-2-hydroxyphenyl]-4,6-bis(2,4-dimethylaminopropyl) (ethylphenyl)-1,3,5-triazine (Tinuvin® 400 BAS F Company), 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine -2-yl]-5-[3-(dodecyloxy)-2-hydroxypropoxy]phenol ), 2-(2,4-dihydroxyphenyl)-4,6-bis-(2,4-dimethylphenyl) Reaction products of (2-ethylhexyl)-1,3,5-triazine and (2-ethylhexyl)-glycidic acid ester (Tinuvin® 405, manufactured by BASF), 3-[2-(2-hydroxypropyl) Polypropionate of (5-tert-butylphenyl)-benzotriazole-propionic acid Pyrene glycol ester (Tinuvin® 1130, manufactured by BASF), Insorb (registered trademark) T-33 (manufactured by Daiwa Kasei Co., Ltd.) is preferred.

[0075] The content of the ultraviolet absorber (F) in the coating composition is preferably 2% based on the non-volatile content. 0 mass% or less, more preferably 0.01 to 15 mass%, and even more preferably 0.1 to 10 mass%. %, particularly preferably 0.5 to 8 mass%, and most preferably 1 to 5 mass%. When the content of the ultraviolet ray absorber is equal to or more than the lower limit, the weather resistance of the cured film is likely to be improved. When the content of the absorbent is equal to or less than the upper limit, the curability of the coating composition, the toughness and heat resistance of the cured film are excellent. The adhesive strength and scratch resistance are likely to be improved.

[0076] <Light stabilizer (G)> In order to further improve the weather resistance of the cured product, a light stabilizer (G) is added to the coating composition. The light stabilizer (G) is not particularly limited as long as it is a hindered amine light stabilizer. Specific examples of the light stabilizer (G) include bis(2,2,6,6-tetramethyl-4-piperidinyl) Bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate Bis(1-methoxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate , bis(1-ethoxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate, bis(1-propoxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate, Bis(1-butoxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate, Bis(1-butoxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate bis(1-pentyloxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate, Bis(1-hexyloxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate , bis(1-heptyloxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate Bis(1-octoxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate Bis(1-nonyloxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate Bis(1-decyloxy-2,2,6,6-tetramethyl-4-piperidyl)sebake bis(1-dodecyloxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate Bis(1,2,2,6,6-pentamethyl-4-piperidyl)-2-(4-methanate) tetrakis(2,2,6,6-pentamethyl-4-pyridin)malonate Peridyl) 1,2,3,4-butanetetracarboxylate, Tetrakis(1,2,2, 6,6-Pentamethyl-4-piperidyl)1,2,3,4-butanetetracarboxylate Aminomethyl group-containing compounds such as 1,2,3,4-butanetetracarboxylic acid and 1,2, 2,6,6-Pentamethyl-4-piperidinol and β,β,β,β-Tetramethyl-3, 9-(2,4,8,10-tetraoxaspiro[5,5])undecane)diethanol and Condensation product of 1,2,3,4-butanetetracarboxylic acid and 2,2,6,6-pentamethyl- 4-Piperidinol and β,β,β,β-tetramethyl-3,9-(2,4,8,10-tetramethyl Traoxaspiro[5,5]undecane)diethanol condensation product, decanedicarbon Diesters of acids with 2,2,6,6-tetramethyl-1-octoxy-4-piperidinol Reaction products of 1,1-dimethylethyl hydroperoxide with octane (BA SF product, product name Tinuvin 123), bis(1,2,2,6,6-pentamethyl-4-piperidine Lysinyl)-[[3,5-bis(1,1,dimethylethyl)-4-hydroxyphenyl] Examples of compounds containing amino ether groups include methyl (BASF, product name Tinuvin 144) and the like. Among these, the amino ether group-containing compounds are preferred from the viewpoint of weather resistance of the cured product. , especially bis(1,2,2,6,6-pentamethyl-4-piperidinyl)-[[3,5-bi Particularly preferred is (1,1,dimethylethyl)-4-hydroxyphenylmethyl. These compounds may be used alone or in combination of two or more.

[0077] The content of the light stabilizer (G) in the coating composition is preferably 20 mass % based on the nonvolatile content. % by mass or less, more preferably 0.01 to 15% by mass, and even more preferably 0.1 to 10% by mass. The range is particularly preferably 0.5 to 8% by mass, and most preferably 1 to 5% by mass. By using it in such a range, a cured film can be formed effectively and the weather resistance of the cured film can be improved.

[0078] <Leveling agent> To improve the appearance of the cured product, a leveling agent may be added to the coating composition. Leveling agents include acrylic leveling agents, silicone leveling agents, and fluorine leveling agents. Among these, the abrasion resistance, which is one of the objectives of the present invention, is improved. From the viewpoint of being able to achieve a desired leveling effect, a silicone-based leveling agent is more preferred, and further The leveling agent also has the added benefit of preventing bleeding out after deterioration due to weathering. Therefore, silicone-based leveling agents having a hydroxyl group are particularly preferred. The adhesive agent imparts slip properties to the cured product, achieving high scratch resistance. The leveling agent is an isocyanate of the polyisocyanate (C) contained in the urethane resin composition. By reacting with anate groups, it is incorporated into the hardened material, providing long-term slip and scratch resistance. This is extremely useful as it allows one to achieve

[0079] The content of the leveling agent in the coating composition is preferably 20% by mass based on the non-volatile content. % or less, more preferably 0.01 to 10% by mass, even more preferably 0.1 to 5% by mass, The range is preferably 0.2 to 4 mass%, and most preferably 0.3 to 3 mass%. By using it in this range, not only can the appearance of the cured film be improved, but also the abrasion resistance can be improved. .

[0080] The coating composition may further contain, as necessary, an organic solvent, an antioxidant, an anti-yellowing agent, a blue-yellow agent, etc. Additives such as coloring agents, pigments, dyes, defoamers, thickeners, anti-settling agents, antistatic agents, and anti-fogging agents. Agents may also be included.

[0081] <Curing accelerating catalyst> The resin composition of the present invention can be cured at room temperature or by heating. The polymerization promoter may contain a polymerization promoter.

[0082] The curing-accelerating catalyst is not particularly limited, but examples thereof include triethylamine, N,N-diethylamine, Monoamines such as methylcyclohexylamine, diamines such as tetramethylethylenediamine Other amines, triamines, cyclic amines, and alcohol amines such as dimethylethanolamine amines such as ether amines, potassium acetate, potassium 2-ethylhexanoate, acetic acid Calcium, lead octylate, dibutyltin dilaurate, tin octylate, bismuth neodeca Bismuth 2-ethylhexanoate, octyl Commonly used metals such as zinc phosphate, zinc neodecanoate, phosphines, and phosphophosphates A catalyst may be used. These may be used alone or in combination of two or more kinds.

[0083] The content of the curing catalyst is based on the mass (100 mass%) of the polyisocyanate (C). The content is preferably 0.001% by mass or more and 10% by mass or less, and more preferably 0.01% by mass or more and 5% by mass or less. It is more preferable that the content be 0.1 mass % or more and 1 mass % or less.

[0084] <Organic solvent> The coating composition of the present invention is preferably a composition having a weight (100 mass % of the ink, the ink preferably contains an organic solvent in an amount of 1 mass % or more and 90 mass % or less. The content of the agent is preferably 20% by mass or more and 80% by mass or less, and more preferably 40% by mass or more and 70% by mass or less. % or less is even more preferable.

[0085] The organic solvent to be used is not particularly limited, but examples thereof include methanol, ethanol, and ethanol. isopropyl alcohol, n-butanol, diacetone alcohol, 2-methoxyethanol 2-ethoxyethanol (ethyl cellosolve), 2-butoxyethanol Alcohols such as ethanol (butyl cellosolve), tertiary amyl alcohol, vinegar Ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, Esters such as butyl acetate, methyl ethyl ketone, methyl isobutyl ketone, acetone, Ketones such as cyclohexanone, diisobutyl ketone, dimethylformamide, dimethyla Amides such as acetamide, diethyl ether, methoxytoluene, 1,2-dimethoxyethane ethane, 1,2-dibutoxyethane, 1,1-dimethoxymethane, 1,1-dimethoxyethane Ethers such as hexane, 1,4-dioxane, and tetrahydrofuran, pentane, Aliphatic hydrocarbons such as butane, cyclohexane, methylcyclohexane, toluene, xylose, Examples of the aromatic hydrocarbons include aromatic hydrocarbons such as benzene and benzene.

[0086] Among them, it has no reactivity with polyisocyanate (C) and does not deteriorate the physical properties of the cured film. In terms of the low concentration, it is preferable to use a solvent other than primary alcohols and secondary alcohols. They may be used alone or in combination of two or more kinds.

[0087] The organic solvent may be mixed in advance with the base agent and the hardener, or may be mixed with the base agent as a third liquid. It may be added after mixing the hardener.

[0088] The pot life of the coating composition is determined by the number of drops after 4 hours in the pot life test described below. The increase in the number of seconds is preferably 2.5 seconds or less, more preferably 2.0 seconds or less, and even more preferably Preferably, the time is 1.5 seconds or less, and more preferably, 1.0 seconds or less. During production, a cured product with good appearance can be obtained.

[0089] <Base material> The substrates are zinc-plated steel, zinc alloy-plated steel, stainless steel, and tin-plated steel. Metals such as polymethyl methacrylate resin, polycarbonate resin, polyester resin, Styrene resin, ABS resin, AS resin, polyamide resin, polyarylate resin, polymer Examples of the resin include tacrylimide resin and polyallyl diglycol carbonate resin.

[0090] Among these, polymethyl methacrylate resin, polycarbonate resin, polystyrene resin, etc. Resins and polymethacrylimide resins are preferred from the viewpoint of improving the abrasion resistance of the cured surface.

[0091] <Cured product> The coating composition of the present invention can be applied to a substrate by brush coating, bar coating, spray coating, direct coating, or the like. This can be done by a known method such as top coating, spin coating, curtain coating, etc.

[0092] The curing temperature when the coating composition of the present invention applied to a substrate is cured depends on the heat resistance and heat resistance of the substrate. The temperature may be appropriately set in consideration of deformation properties, etc., but it is preferable that the temperature is 20°C or higher and 200°C or lower, and 60°C or lower. The temperature is more preferably from 80°C to 120°C, and even more preferably from 80°C to 120°C.

[0093] The curing time for curing the coating composition of the present invention applied to a substrate is preferably 5 to 120 minutes. The curing time is preferably in the range of 8 to 30 minutes, and more preferably in the range of 10 to 20 minutes. The shorter the time, the shorter the manufacturing time, and the longer the curing time, the better the scratch resistance. .

[0094] <Laminate> In the laminate of the present invention, the thickness of the cured film of the coating composition of the present invention is 3 μm to 50 μm. The following is preferred:

[0095] When the thickness of the cured film in the laminate of the present invention is equal to or greater than the above lower limit, the scratch resistance and The hardness and weather resistance of the laminate of the present invention are good, and the appearance is easily maintained for a long period of time. If the thickness of the oxide film is equal to or less than the upper limit, cracks are easily suppressed.

[0096] The scratch resistance of the cured product is preferably measured as the amount of change in haze in the scratch test described below. 5.0% or less, more preferably 3.0% or less, even more preferably 2.6% or less, and particularly preferably The content is preferably 2.0% or less, and most preferably 1.9% or less, with the lower limit being 0.0%. By setting the thickness within this range, it is possible to prevent the laminate from being scratched.

[0097] The hardness of the cured product is preferably HB or higher in pencil hardness, and F or higher in the test described below. By setting the content within this range, damage to the laminate can be prevented.

[0098] <Application> The coating composition of the present invention is excellent in appearance, scratch resistance, weather resistance, hardness, etc., and is therefore suitable for use in automobiles, Plastic parts for various lamp lenses, grilles, side mirrors, pillars, bumpers, etc. It can be suitably used for applications such as exterior members and hard coats for glazing. EXAMPLES

[0099] The present invention will be described in more detail below with reference to examples, but the present invention does not exceed the gist of the invention. However, the present invention is not limited to the following examples. The values ​​of the conditions and evaluation results are meant as preferred upper or lower limits in the embodiments of the present invention. The preferred range is the upper or lower limit value described above and the value or actual value in the following examples. It may be a range defined by combining the values ​​of the examples. In addition, "parts" and "%" indicate "parts by mass" and "% by mass" respectively unless otherwise specified. . The measurement and evaluation methods used in the present invention are as follows.

[0100] [Measurement and evaluation methods] <Weight average molecular weight> Weight average molecular weight (Mw) is measured by gel permeation chromatography (GPC) method. The measurements were performed under the following conditions, and the values ​​were calculated using standard polystyrene equivalents. Equipment: Tosoh Corporation high-speed GPC equipment HLC-8320GPC type UV detector: Tosoh UV-8320 Flow rate: 0.35mL / min Inlet temperature: 40℃ Oven temperature: 40℃ RI temperature: 40℃ UV wavelength: 254nm Sample injection volume: 10 μL Columns: Three columns connected in the order of (1) to (3). (1) Tosoh TSKgel superHZM-M (4.6mm ID x 15cm L) ) (2) Tosoh TSKgel superHZM-M (4.6mm ID x 15cm L) ) (3) Tosoh TSKgel HZ2000 (4.6mm ID x 15cm L) Guard column: Tosoh TSKguardcolumn SuperHZ-L (4. 6mm ID x 3.5cm L) Solvent: THF (stabilized with BHT) Sample concentration: Resin content adjusted to 0.2% by mass

[0101] <Evaluation sample> Each coating composition shown in Table 2 was applied to a 3 mm thick polycarbonate resin plate (Mitsubishi Engineering Ring Plastics Co., Ltd., product name: "IUPILON ML-300") after hardening The coating was sprayed to a thickness of 10 μm. After that, it was left to set at room temperature for 1 minute. After that, the polycarbonate resin is dried by heating it in a dryer at 115℃ for 15 minutes. The coating film was formed on a grease plate and evaluated. The coating composition was placed in a container, sealed, and heated to 25 The coating composition was left for 4 hours in an atmosphere of 50% humidity and 20°C. The same procedure was followed for the coating composition after 4 hours. The coating was spray-coated onto a substrate and cured to obtain a cured product.

[0102] <Pot life> The pot life of the coating composition was measured by mixing the coating composition shown in Table 2 and then storing at 25°C and 50°C. After stirring for 15 minutes in an atmosphere of 50%, the falling speed was measured using a Ford cup #4. The viscosity of the coating composition was then measured after storing it in a closed container at 25°C for 4 hours. The drop rate was measured using a Ford cup #4, and the viscosity after 4 hours was calculated. The increased viscosity was calculated by subtracting the initial viscosity (seconds) from the viscosity (seconds). ○: Viscosity increase of less than 2 seconds ×: Viscosity increase for 2 seconds or more

[0103] <Appearance of coating film> The appearance of the coating film was evaluated visually based on the leveling property of the resulting cured product. ○: Good ×: Yuzu skin, bumps, pinholes, whitening

[0104] <Adhesion> The adhesion of the coating was evaluated using the following procedure: The surface of the coating was cut with a cutter at 1. 100 squares are created by cutting 11 holes at 5mm intervals into the base material, and cellophane is applied. Tape (25 mm wide, manufactured by Nichiban Co., Ltd.) is pressed against the squares and then peeled off rapidly upwards. The adhesion was evaluated based on the number of remaining squares / total number of squares (100) and visual observation according to the following criteria: It was determined. 〇: 100 / 100 (no peeling) ×: 0 / 100~99 / 100 (peeling occurs).

[0105] <Scratch resistance> The scratch resistance of the coating film was evaluated using a flat surface abrasion tester (KASAI scratch tester). Steel wool #000 was placed on the evaluation sample and subjected to a load of 250g / 1.1cm2 for 50 minutes. After reciprocating abrasion, the haze was measured using a haze meter (HM-65W, manufactured by Murakami Color Research Laboratory Co., Ltd.). The diffuse transmittance (haze value) was measured. ◎: Less than 2.0% ○: 2.0% or more and less than 3.0% ×: 3.0% or more

[0106] <Pencil hardness> The hardness of the coating was evaluated by pencil hardness in accordance with ISO / DIS 15184. After that, the highest hardness that did not cause any scratches was adopted as the pencil hardness of the coating film.

[0107] <Water resistance> The water resistance of the coating film was evaluated by immersing the resulting cured product in 80°C hot water for 8 hours and then examining the coating film appearance. The adhesion was evaluated according to the test methods described above.

[0108] <Production of polyol (A)> Production Example 1 (Polyol A-2) In a four-neck flask equipped with a stirrer, thermometer, condenser, and nitrogen gas inlet, Then, 55.7 parts of propylene glycol monomethyl ether acetate was added, and nitrogen gas was passed through the mixture. The mixture was heated under air until the internal temperature reached 140°C. After the internal temperature stabilized, 2-hydroxymethacrylate was added. 50 parts of diethyl methacrylate, 10 parts of methyl methacrylate, 30 parts of i-butyl methacrylate, acrylic 9.3 parts of 2-ethylhexyl acetate, 0.7 parts of acrylic acid, and perbutyl (registered trademark) as a polymerization initiator. O(tert-butylperoxy 2-ethylhexanoate), NOF Corporation A mixture of 6 parts of 100% ethanol (prepared by dripping) was dripped over a period of 4 hours. After the dripping was completed, the mixture was held for 1 hour. 0.3 parts of Perbutyl (registered trademark) O was mixed with propylene glycol monomethyl ether acetate. The mixture was dissolved in 15 parts of ethyl acetate and added to the mixture. After that, the mixture was held for 1 hour, and then cooled to room temperature. The weight average molecular weight (Mw) of the copolymer in polyol A-2 was The glass transition temperature (Tg), hydroxyl value (OHV), SP value, and acid value of the polyol are shown in Table 1. Shown in the physical characteristics column.

[0109] Production Examples 2 to 6 (Polyols A-3 to A-7) The same procedure as in Production Example 1 was repeated except that the monomers shown in Table 1 below were used. Polyols A-3 to A-7 with a shape content of 60% were obtained.

[0110] [Table 1]

[0111] <Production of inorganic fine particles (D)> Production Example 7 (Inorganic Particle Dispersion D-1) Flask A was filled with 1 mL of 3-mercaptopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.). Add 0.2g of tetrahydrofuran, 0.6g of distilled water, and 2.1g of tetrahydrofuran, and stir at 30°C for 3 hours. A silanol solution was obtained. Flask B was filled with methyl isobutyl ketone-dispersed silica sol (product name: "MI BK-ST", Solvent: Methyl isobutyl ketone, Solid content: 30% by mass, Average particle size: 100 g of 15 nm was added and the temperature was raised to 70°C. Add the silanol solution from flask A to flask B, and stir at 70°C for 1 hour after the addition. The solvent of the obtained inorganic fine particle dispersion was dried in an atmosphere of 100° C. for 2 hours, and the remaining 35 g Add 65 g of acetonitrile to the mixture and stir to obtain acetonitrile-containing inorganic particles with mercapto groups. A trinitrile dispersion D-1 (solid content 35%) was obtained.

[0112] [Example 1] Polyol A-1 was Basonol® HPE 1170B (solids content 7 0%, hydroxyl value 280mgKOH / g, acid value 85mgKOH / g, molecular weight 1800 (catalyst 56.6 parts (solid content 39.8 parts) of diethyl malonate as reaction retarder B-1 5.7 parts of ethanol, 48.6 parts of inorganic fine particles D-1 (solid content 17.1 parts), polycarbonate Polyol E-1 was Ethanacol UM-90 (3 / 1) (Mw : 900, hydroxyl value: 125 mgKOH / g) 28.4 parts, as ultraviolet absorber (F) 11.4 parts of Tinuvin 405 (BASF) and 11.4 parts of Tinuvin 152 ( 2.8 parts of BASF (manufactured by BASF) and 0.5 parts of BYK-370 (manufactured by BYK) as a leveling agent. 151.1 parts of cyclohexanone were used as a solvent, and these were mixed uniformly to form the base material. This base resin is used as a hardener, polyisocyanate B-1 Duranate MHG-80B (Asahi The resulting coating composition was evaluated as follows: The ratio of the hydroxyl group of the base resin to the isocyanate group of the curing agent is NCO / OH=1.0. The ratio of the reaction retarder B-1 to the isocyanate groups derived from the polyisocyanate (C) is The total amount is 18 mol%.

[0113] [Examples 2 to 11 and Comparative Examples 1 to 4] The same procedure as in Example 1 was repeated except that the paint composition in Example 1 was changed to the paint composition shown in Table 2. The evaluation results of the cured product are shown in Table 2 below.

[0114] [Table 2]

[0115] The ingredients in the table are as follows: A-1: Basonol HPE 1170B (BASF), a polymer with a hydroxyl group at the end Hyperbranched polyester polyol, solid content 70%, hydroxyl value: 280mg / KOH / g, acid value: 85mgKOH / g, weight average molecular weight (Mw): 1800. A-2: Polyol A-2 prepared in Production Example 1 A-3: Polyol A-3 prepared in Production Example 2 A-4: Polyol A-4 prepared in Production Example 3 A-5: Polyol A-5 prepared in Production Example 4 A-6: Polyol A-6 prepared in Production Example 5 A-7: Polyol A-7 prepared in Production Example 6 B-1: Diethyl malonate B-2: Acetylacetone B-3: Propylene glycol monomethyl ether B-4: Methyl ethyl ketoxime D-1: Dispersion liquid D-1 of inorganic particles prepared in Production Example 7 E-1: UM-90(3 / 1) (Ube Industries, Ltd.) polycarbonate diol, Solid content 100%, hydroxyl value: 127mgKOH / g, weight average molecular weight (Mw): 900. F-1: Tinuvin 405 (BASF) Hydroxyphenyl triazine UV absorber, hydroxyl value: 96.5mgKOH / g G-1: Tinuvin 152 (BASF) Hindered amine light stabilizer. C-1: Duranate MHG-80B (manufactured by Asahi Kasei Corporation), nurate type multifunctional isopropyl alcohol Cyanate, NCO value: 15.1%, solids content: 80%. C-2: Duranate TPA-100 (manufactured by Asahi Kasei Corporation), nurate type multifunctional isopropyl alcohol Cyanate, NCO number: 23.1%, solids: 100%. ·BYK-370: Silicone leveling agent (manufactured by BYK)

[0116] The coating compositions obtained in Examples 1 to 11 all had a good pot life. The cured product had good scratch resistance, hardness, and adhesion even after 4 hours.

[0117] In Comparative Example 1, when polyol A-6 having a hydroxyl group of less than 50 mgKOH / g was used, In this case, a sufficient crosslinked structure could not be formed, and the scratch resistance was low. In Comparative Example 2, when polyol A-7 having an acid value of 0 mgKOH / g was used, the reactivity The hardness was low, and the scratch resistance and water resistance of the obtained cured product were insufficient. In Comparative Examples 3 and 4, since the reaction retarder (B) was not included, the reaction did not proceed after the base agent and the hardener were mixed. The viscosity increased after 4 hours, and workability and the appearance of the coating film deteriorated.

Claims

1. A coating composition having at least two liquids, a base agent and a curing agent, the base agent being a polyol (A). , containing a reaction modifier (B), The polyol (A) has a hydroxyl value of 50 to 300 mgKOH / g and an acid value of 1 to 1 00 mg KOH / g, The reaction adjuster (B) is an isocyanate blocking agent, A coating composition in which the curing agent comprises a polyisocyanate (C).

2. The coating composition according to claim 1, further comprising inorganic fine particles (D).

3. The inorganic fine particles (D) have a reactive group such as an isocyanate group, an epoxy group, a mercapto group, The coating composition according to claim 1, comprising at least one selected from the group consisting of:

4. 2. The coating composition according to claim 1, wherein the reaction modifier (B) is a β-dicarbonyl compound.

5. The polyol (A) is at least one of an acrylic polyol and a polyester polyol. The coating composition according to claim 1, comprising any one of the following:

6. 2. The composition according to claim 1, further comprising a polycarbonate polyol (E) different from the polyol (A). The coating composition described herein.

7. The coating composition according to claim 1, further comprising an ultraviolet absorber (F).

8. 2. The coating composition according to claim 1, further comprising a hindered amine light stabilizer (G).

9. A cured product of the coating composition according to any one of claims 1 to 8.

10. A laminate having a coating film comprising the cured product according to claim 10.

Citation Information

Patent Citations

  • Coating or adhesive compositions and manufacture

    JP1984084951A

  • Coating agent composition having long pot life and short curing time

    JP1998338769A

  • Coating method and device for low-temperature curing two-liquid type polyurethane coating material

    JP2002316075A

  • Curing catalyst for polyurethane resin, polyurethane resin composition, and adhesive

    JP2006037028A

  • Coating composition

    JP2015196762A