Zinc secondary battery

The zinc secondary battery employs a dual LDH separator system with controlled conductivity to manage charge/discharge reactions, addressing dendrite-induced short circuits and maintaining electrode integrity for improved cycle life.

JP2024140385APending Publication Date: 2024-10-10NGK INSULATORS LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2023051505
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Zinc secondary batteries suffer from shortened cycle life due to zinc dendrites forming during charging, which penetrate the separator and cause short circuits, and the negative electrode material changes form leading to increased resistance and pore blockage.

Method used

A zinc secondary battery design incorporating a pair of LDH separators with controlled ionic conductivity ratios, where a low-conductivity separator is used on one side of the negative electrode plate and a high-conductivity separator on the other, to manage charge/discharge reactions and suppress dendrite formation.

Benefits of technology

This configuration improves cycle characteristics by maintaining the integrity of the negative electrode, reducing dendrite-induced short circuits, and enhancing the battery's durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140385000001_ABST
    Figure 2024140385000001_ABST
Patent Text Reader

Abstract

To provide a zinc secondary battery which can further improve battery cycle characteristics.SOLUTION: A zinc secondary battery includes: a negative electrode plate which contains a negative active substance containing at least one kind selected from the group consisting of zinc, zinc oxide, zinc alloy and a zinc compound, and has a first surface and a second surface: a pair of positive electrode plate which are provided so as to face the first surface and the second surface of the negative electrode plate, and contain a positive active substance; a pair of LDH separators which are interposed between the pair of positive electrode plates and the negative electrode plate, and contains a hydroxide ion conductive layered compound that is a layered double hydroxide (LDH) and / or an LDH-like compound; and an electrolyte, wherein the pair of LDH separators have a low conductivity separator provided on the first surface side of the negative electrode plate, and a high conductivity separator provided on the second surface side of the negative electrode plate, and a ratio CH / CL of ion conductivity CH of the high conductivity separator to ion conductivity CL of the low conductivity separator is 1.1 to 13.0.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a zinc secondary battery. [Background technology]

[0002] In zinc secondary batteries such as nickel-zinc secondary batteries and air-zinc secondary batteries, it is known that metallic zinc precipitates in the form of dendrites from the negative electrode during charging, penetrates the voids in the separator such as nonwoven fabric, and reaches the positive electrode, resulting in a short circuit. Such a short circuit caused by zinc dendrites shortens the repeated charge-discharge life.

[0003] In order to address the above problems, a battery has been proposed that includes a layered double hydroxide (LDH) separator that selectively allows hydroxide ions to pass through while preventing the penetration of zinc dendrites. For example, Patent Document 1 (WO 2013 / 118561) discloses that an LDH separator is provided between the positive and negative electrodes in a nickel-zinc secondary battery. In addition, Patent Document 2 (WO 2016 / 076047) discloses a separator structure that includes an LDH separator fitted or joined to a resin outer frame, and that the LDH separator has such high density that it is gas impermeable and / or water impermeable. This document also discloses that the LDH separator can be composited with a porous substrate. Furthermore, Patent Document 3 (WO 2016 / 067884) discloses various methods for obtaining a composite material by forming an LDH dense membrane on the surface of a porous substrate. This method includes a step of uniformly attaching an initiator substance capable of providing an initiator for the crystal growth of LDH to a porous substrate, and subjecting the porous substrate to hydrothermal treatment in a raw aqueous solution to form a dense LDH membrane on the surface of the porous substrate. An LDH separator has also been proposed that achieves further densification by roll pressing a composite material of LDH / porous substrate produced through hydrothermal treatment. For example, Patent Document 4 (International Publication No. 2019 / 124270) discloses an LDH separator that includes a polymeric porous substrate and an LDH filled in the porous substrate, and has a linear transmittance of 1% or more at a wavelength of 1000 nm.

[0004] In addition, although they cannot be called LDH, LDH-like compounds are known as hydroxides and / or oxides with a layered crystal structure similar to LDH, and exhibit hydroxide ion conductive properties similar to LDH, which can be collectively referred to as hydroxide ion conductive layered compounds together with LDH. For example, Patent Document 5 (WO 2020 / 255856) discloses an LDH separator comprising a porous substrate and a layered double hydroxide (LDH)-like compound that blocks the pores of the porous substrate, in which the LDH-like compound is a hydroxide and / or oxide of a layered crystal structure containing Mg and one or more elements including at least Ti selected from the group consisting of Ti, Y, and Al. In addition, Patent Document 6 (WO 2021 / 229916) discloses an LDH separator using an LDH-like compound containing (i) Ti, Y, and optionally Al and / or Mg, and (ii) an additive element M which is at least one selected from the group consisting of In, Bi, Ca, Sr, and Ba. Furthermore, Patent Document 7 (International Publication No. 2021 / 229917) discloses an LDH separator containing a mixture of an LDH-like compound and In(OH)3, in which the LDH-like compound is a hydroxide and / or oxide having a layered crystal structure containing Mg, Ti, Y, and optionally Al and / or In. The separators disclosed in Patent Documents 5 to 7 are said to have superior alkali resistance compared to conventional LDH separators, and to be able to more effectively suppress short circuits caused by zinc dendrites.

[0005] Meanwhile, another factor that shortens the life of zinc secondary batteries is the change in the morphology of zinc, which is the negative electrode active material. That is, as zinc dissolves and precipitates repeatedly due to repeated charging and discharging, the morphology of the negative electrode changes, causing high resistance due to blockage of pores, a decrease in the charge active material due to accumulation of isolated zinc, etc., resulting in a problem that charging and discharging becomes difficult. In order to address this problem, Patent Document 8 (WO 2020 / 049902) proposes using ZnO particles in combination with at least two selected from (i) metal Zn particles of a predetermined particle size, (ii) a predetermined metal element, and (iii) a binder resin having a hydroxyl group for use in the negative electrode. It is said that this negative electrode can suppress the deterioration of the negative electrode due to repeated charging and discharging in a zinc secondary battery, improve durability, and thereby extend the cycle life. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2013 / 118561 [Patent Document 2] International Publication No. 2016 / 076047 [Patent Document 3] International Publication No. 2016 / 067884 [Patent Document 4] International Publication No. 2019 / 124270 [Patent Document 5] International Publication No. 2020 / 255856 [Patent Document 6] International Publication No. 2021 / 229916 [Patent Document 7] International Publication No. 2021 / 229917 [Patent Document 8] International Publication No. 2020 / 049902 Summary of the Invention

[0007] When a zinc secondary battery such as a nickel-zinc battery is constructed using an LDH separator as disclosed in Patent Documents 1 to 7, short circuits caused by zinc dendrites can be prevented to some extent. However, further improvement in cycle characteristics is desired.

[0008] The present inventors have now discovered that in a zinc secondary battery including a pair of positive and negative electrode plates and a pair of LDH separators interposed therebetween, the cycle characteristics can be further improved by using, as the LDH separators, a low conductive separator and a high conductive separator whose ionic conductivity ratio is controlled within a predetermined range.

[0009] SUMMARY OF THE PRESENT DISCLOSURE ... It is therefore an object of the present invention to provide a zinc secondary battery having further improved cycle characteristics.

[0010] According to the present invention, the following aspects are provided. [Aspect 1] a negative electrode plate including a negative electrode active material including at least one selected from the group consisting of zinc, zinc oxide, a zinc alloy, and a zinc compound, the negative electrode plate having a first surface and a second surface; A pair of positive electrode plates including a positive electrode active material, the positive electrode plates being provided so as to face the first surface and the second surface of the negative electrode plate; a pair of LDH separators interposed between the pair of positive and negative electrode plates, the LDH separators comprising a hydroxide ion conducting layered compound that is a layered double hydroxide (LDH) and / or an LDH-like compound; An electrolyte; The pair of LDH separators includes a low conductive separator provided on a first surface side of the negative electrode plate and a high conductive separator provided on a second surface side of the negative electrode plate, and the ionic conductivity C L Ion conductivity C of the highly conductive separator H Ratio of C H / C L A zinc secondary battery, wherein the resistance is 1.1 to 13.0. [Aspect 2] Ion conductivity C of the low-conductivity separator L 0.8~2.5S / cm 22. The zinc secondary battery of embodiment 1, [Aspect 3] Ion conductivity C of the highly conductive separator H 2.5~10.0S / cm 2 3. The zinc secondary battery according to claim 1 or 2, [Aspect 4] The zinc secondary battery according to any one of aspects 1 to 3, wherein the negative electrode plate is covered or enveloped by the pair of LDH separators. [Aspect 5] The zinc secondary battery according to any one of aspects 1 to 4, wherein the LDH separator further comprises a porous substrate, the pores of the porous substrate being filled with the hydroxide ion-conducting layered compound, and / or at least one surface of the porous substrate is provided with a surface layer comprising the hydroxide ion-conducting layered compound. [Aspect 6] The zinc secondary battery of embodiment 5, wherein the porous substrate is made of a polymeric material. [Aspect 7] 7. The zinc secondary battery according to any one of aspects 1 to 6, wherein each of the low conductive separator and the high conductive separator has a He permeability per unit area of ​​10 cm / min·atm or less. [Aspect 8] The zinc secondary battery according to any one of aspects 1 to 7, wherein each of the low conductive separator and the high conductive separator is pressed in the thickness direction of the separator. [Aspect 9] The zinc secondary battery includes a stacked cell, the stacked cell comprising: A plurality of the positive electrode plates; A plurality of the negative electrode plates; A plurality of pairs of the LDH separators; The electrolyte; The zinc secondary battery according to any one of aspects 1 to 8, wherein the positive electrode plates and the negative electrode plates are alternately stacked with the LDH separator sandwiched therebetween, the low conductive separator is disposed on a first surface side of each of the plurality of negative electrode plates, and the high conductive separator is disposed on a second surface side of each of the plurality of negative electrode plates. [Aspect 10] The zinc secondary battery according to any one of aspects 1 to 9, wherein the positive electrode plate contains nickel hydroxide and / or nickel oxyhydroxide, thereby forming the zinc secondary battery into a nickel-zinc secondary battery. [Aspect 11] The zinc secondary battery according to any one of aspects 1 to 9, wherein the positive electrode plate is an air electrode, thereby making the zinc secondary battery an air-zinc secondary battery. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a zinc secondary battery according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing a cross section of the zinc secondary battery shown in FIG. 1 taken along line AA'. [Diagram 3] FIG. 2 is a perspective view showing a schematic diagram of a stacked cell of the zinc secondary battery shown in FIG. [Figure 4] FIG. 2 is a cross-sectional view showing a schematic diagram of a stacked cell of the zinc secondary battery shown in FIG. [Diagram 5] FIG. 5 is a cross-sectional view showing an example of the stacked cell shown in FIG. 4 after repeated charge-discharge cycles. [Figure 6] FIG. 1 is a diagram for explaining the change in shape of a negative electrode plate due to repeated charge-discharge cycles in a conventional zinc secondary battery. [Figure 7A] FIG. 1 is a conceptual diagram showing an example of a He permeability measurement system used in Examples A1 to B3. [Figure 7B] 7B is a schematic cross-sectional view of a sample holder and its surrounding structure used in the measurement system shown in FIG. 7A. [Figure 8] FIG. 2 is a schematic cross-sectional view showing an electrochemical measurement system used in Examples A1 to B3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Zinc secondary battery The zinc secondary battery of the present invention is not particularly limited as long as it is a secondary battery using zinc as the negative electrode and an alkaline electrolyte (typically an aqueous alkali metal hydroxide solution). Therefore, it can be a nickel-zinc secondary battery, a silver oxide zinc secondary battery, a manganese oxide zinc secondary battery, an air zinc secondary battery, or any other type of alkaline zinc secondary battery. For example, it is preferable that the positive electrode plate contains nickel hydroxide and / or nickel oxyhydroxide, thereby making the zinc secondary battery a nickel-zinc secondary battery. Alternatively, the positive electrode plate may be an air electrode, thereby making the zinc secondary battery an air zinc secondary battery.

[0013] 1 to 4 show an embodiment of a zinc secondary battery and its internal structure according to the present invention. The zinc secondary battery 10 shown in these figures includes a negative electrode plate 12 having a first surface S1 and a second surface S2, a pair of positive electrode plates 14, a pair of LDH separators 16, and an electrolyte (not shown). The negative electrode plate 12 includes a negative electrode active material 12a and, if desired, a negative electrode current collector 12b. The negative electrode active material 12a includes at least one selected from the group consisting of zinc, zinc oxide, a zinc alloy, and a zinc compound. The pair of positive electrode plates 14 are provided so as to face the first surface S1 and the second surface S2 of the negative electrode plate 12. The positive electrode plate 14 includes a positive electrode active material 14a and, if desired, a positive electrode current collector 14b. The pair of LDH separators 16 are interposed between the pair of positive electrode plates 14 and negative electrode plates 12. The LDH separator 16 includes a hydroxide ion conductive layered compound that is a layered double hydroxide (LDH) and / or an LDH-like compound. In this specification, an "LDH separator" is defined as a separator that includes an LDH and / or an LDH-like compound and selectively passes hydroxide ions by utilizing the hydroxide ion conductivity of the LDH and / or the LDH-like compound. In this specification, an "LDH-like compound" is a hydroxide and / or oxide having a layered crystal structure that has hydroxide ion conductivity and can be said to be equivalent to LDH, although it may not be called LDH. However, in a broad sense, "LDH" can be interpreted as including not only LDH but also LDH-like compounds. The pair of LDH separators 16 includes a low conductive separator 16a and a high conductive separator 16b. The low conductive separator 16a is provided on the first surface S1 side of the negative electrode plate 12. The high conductive separator 16b is provided on the second surface S2 side of the negative electrode plate 12. And the ionic conductivity C of the low conductive separator 16a L Ion conductivity C of the highly conductive separator 16b H Ratio of C H / C L In this way, in the zinc secondary battery 10 including a pair of positive electrode plates 14, a pair of negative electrode plates 12, and a pair of LDH separators 16 interposed therebetween, the ionic conductivity ratio C H / C LBy using the low conductive separator 16a and the high conductive separator 16b whose resistance is controlled within a predetermined range, it is possible to further improve the cycle characteristics.

[0014] The mechanism by which the cycle characteristics of a zinc secondary battery are improved is not necessarily clear, but is believed to be as follows. That is, as described above, in conventional zinc secondary batteries, as zinc dissolves and precipitates repeatedly due to repeated charging and discharging, the negative electrode changes in shape, and ultimately charging and discharging becomes difficult. Here, an example of the change in shape of a negative plate due to repeated charging and discharging cycles in a conventional zinc secondary battery is shown in FIG. 6. The zinc secondary battery 110 shown in FIG. 6(i) has a stacked cell 111 including a negative plate 112 having a first surface S1 and a second surface S2, a pair of positive plates 114 provided so as to face the first surface S1 and the second surface S2 of the negative plate 112, a pair of LDH separators 116 interposed between the pair of positive plates 114 and the negative plate 112, and an electrolyte (not shown). The negative electrode plate 112 includes a negative electrode active material 112a and a negative electrode current collector 112b, and the positive electrode plate 114 includes a positive electrode active material 114a and a positive electrode current collector 114b. The LDH separator 116 provided on the first surface S1 side of the negative electrode plate 112 and the LDH separator 116 provided on the second surface S2 side have the same degree of ion conductivity. When the zinc secondary battery 110 is repeatedly charged and discharged, as shown in FIG. 6(ii), the negative electrode plate 112 is significantly deformed. That is, the negative electrode active material 112a disappears in the area where the charge and discharge reaction is likely to occur in the surface of the negative electrode plate 112, while the negative electrode active material 112a remains in the area where the charge and discharge reaction is unlikely to occur in the surface of the negative electrode plate 112. As a result, unevenness occurs in the surface of the negative electrode plate 112. In this regard, since the LDH separator 116 having the same degree of ion conductivity is provided on the first surface S1 side and the second surface S2 side of the negative electrode plate 112, the charge / discharge reaction proceeds to the same degree on both sides of the negative electrode plate 112, and the occurrence frequency of unevenness increases. As a result, the deformation of the negative electrode plate 112 becomes large, and the LDH separator 116 provided on the negative electrode plate 112 also deforms, making it easy for defects (e.g., voids, cracks, and peeling) to occur. It is considered that these defects are the starting point for penetration of the separator by dendrites, adversely affecting cycle characteristics.

[0015] In contrast, the zinc secondary battery 10 of the present invention uses a low-conductivity separator 16a with a relatively low ion conductivity on the first surface S1 side of the negative electrode plate 12, so that the charge / discharge reaction is suppressed on the first surface S1 side of the negative electrode plate 12, and the charge / discharge reaction proceeds mainly on the second surface S2 side of the negative electrode plate 12. As a result, even if the morphology of the negative electrode plate 12 changes due to repeated charge / discharge cycles, as shown in FIG. 5, the negative electrode active material 12a on the second surface S2 side of the negative electrode plate 12 disappears preferentially, and the negative electrode active material 12a on the first surface S1 side of the negative electrode plate 12 remains. In other words, when viewed as a whole negative electrode plate 12, the negative electrode active material 12a remains smoothly, and deformation of the negative electrode plate 12 is suppressed. Therefore, deformation of the LDH separator 16 on the negative electrode plate 12 is also effectively suppressed, and dendrite short circuit is less likely to occur, which is considered to improve cycle characteristics.

[0016] Therefore, the ionic conductivity C of the low-conductivity separator 16a in the zinc secondary battery 10 L Ion conductivity C of the highly conductive separator 16b H Ratio of C H / C L is 1.1 to 13.0, and preferably 2.0 to 10.0. Within these ranges, the smooth progress of the charge / discharge reaction is promoted, while the negative electrode plate 12 remains smooth, effectively suppressing deformation of the LDH separator 16, and improving cycle characteristics.

[0017] Ion conductivity C of low-conductivity separator 16a L 0.8~2.5S / cm 2 and more preferably 1.0 to 2.5 S / cm 2 Within these ranges, a good balance can be achieved between smooth progress of the charge / discharge reaction and suppression of deformation of the negative electrode plate 12, and the cycle characteristics can be further improved.

[0018] Ion conductivity C of highly conductive separator 16b H is 2.5~10.0S / cm 2 It is preferable that the resistance is 5.0 to 10.0 S / cm. 2Within these ranges, the negative electrode reaction proceeds more smoothly, and as a result, deterioration of the negative electrode plate 12 is effectively suppressed, leading to further improved cycle characteristics.

[0019] The method for producing the LDH separator 16 is not particularly limited, and the LDH separator 16 can be produced by adopting the conditions of the already known methods for producing an LDH separator (or an LDH-containing functional layer and a composite material) (see, for example, Patent Documents 1 to 7) as they are, or by appropriately changing them. The ionic conductivity of the low-conductive separator 16a and the high-conductive separator 16b can be controlled by changing the thickness and / or density of the separator, applying a high-resistance layer (for example, a polymer layer), or the like. For example, the high-conductive separator 16b can be produced by pressing one LDH separator, while pressing two LDH separators in a stacked state to integrate these two LDH separators to produce the low-conductive separator 16a. In this way, the low-conductive separator 16a having a relatively low ionic conductivity compared to the high-conductive separator 16b can be produced. The pressing method may be, for example, roll pressing, uniaxial pressing, CIP (cold isostatic pressing), or the like, but is preferably roll pressing. By further densifying the LDH separator by pressing in this manner, it is possible to more effectively suppress short circuits caused by zinc dendrites while controlling the ion conductivity within a preferred range. Therefore, each of the low conductive separator 16a and the high conductive separator 16b (hereinafter, sometimes simply referred to as "LDH separator 16") is preferably pressed in the thickness direction of the separator. Also, as described above with reference to FIG. 5, the negative electrode active material 12a is likely to remain on the first surface S1 side of the negative electrode plate 12, and therefore it can be said that zinc dendrites are likely to extend toward the low conductive separator 16a provided on the first surface S1 side. In this regard, by forming the low conductive separator 16a by stacking two or more LDH separators, it is possible to increase the puncture strength, and as a result, it is possible to more effectively suppress short circuits caused by zinc dendrites.

[0020] Therefore, the thickness T of the low conductive separator 16a L is the thickness T of the highly conductive separator 16b H Specifically, the thickness T of the highly conductive separator 16b is preferably larger than H Thickness T of the low conductive separator 16a L Ratio of T L / T H is preferably 1.1 to 20, more preferably 1.5 to 12. The thickness of the low conductive separator 16a is preferably 20 to 100 μm, more preferably 20 to 60 μm. This makes it possible to more effectively suppress short circuits caused by zinc dendrites and further improve cycle characteristics. On the other hand, the thickness of the high conductive separator 16b is preferably 5 to 50 μm, more preferably 5 to 25 μm.

[0021] The LDH separator 16 is provided so as to separate the positive electrode plate 14 and the negative electrode plate 12 so as to be conductive to hydroxide ions. For example, the negative electrode plate 12 may be configured to be covered or wrapped with a pair of LDH separators 16. This makes it possible to manufacture a zinc secondary battery (particularly a stacked battery thereof) capable of preventing zinc dendrite extension extremely easily and with high productivity, without the need for a complicated sealing joint between the LDH separator 16 and the battery container. For example, the low conductive separator 16a and the high conductive separator 16b may be arranged so as to protrude from the first surface S1 and the second surface S2 of the negative electrode plate 12, respectively, and the excess parts of the low conductive separator 16a and the high conductive separator 16b protruding from the negative electrode plate 12 may be sealed by a method such as heat fusion. However, a simple configuration in which a pair of LDH separators 16 are arranged on both sides of the negative electrode plate 12 may also be used.

[0022] The denseness of the LDH separator 16 can be evaluated by the He permeability. That is, each of the low conductive separator 16a and the high conductive separator 16b has a He permeability per unit area of ​​preferably 10 cm / min·atm or less, more preferably 5.0 cm / min·atm or less, and further preferably 1.0 cm / min·atm or less. The LDH separator 16 having a He permeability within such a range can be said to have extremely high denseness. Therefore, a separator having a He permeability of 10 cm / min·atm or less can prevent the passage of substances other than hydroxide ions at a high level. For example, in the case of a zinc secondary battery, the permeation of Zn (typically the permeation of zinc ions or zincate ions) in the electrolyte can be extremely effectively suppressed. The He permeability is measured through a process of supplying He gas to one side of the separator to allow the He gas to permeate the separator, and a process of calculating the He permeability to evaluate the denseness of the LDH separator. The He permeability is calculated by the formula F / (P×S) using the amount of He gas permeated per unit time F, the pressure difference P applied to the separator when He gas permeates, and the membrane area S through which He gas permeates. By evaluating gas permeability using He gas in this way, it is possible to evaluate the presence or absence of denseness at an extremely high level, and as a result, it is possible to effectively evaluate a high level of denseness, such as not allowing substances other than hydroxide ions (especially Zn, which causes zinc dendrite growth) to permeate as much as possible (permeating only a very small amount). This is because He gas has the smallest structural unit among the wide variety of atoms or molecules that can constitute gas, and has extremely low reactivity. In other words, He does not form molecules, and He gas is composed of He atoms alone. In this regard, hydrogen gas is composed of H2 molecules, so that He atoms alone are smaller as a gas structural unit. In the first place, H2 gas is dangerous because it is a flammable gas. And by adopting the index of He gas permeability defined by the above formula, it is possible to easily and objectively evaluate denseness regardless of various sample sizes and differences in measurement conditions. In this way, it is possible to simply, safely and effectively evaluate whether a separator has a sufficiently high density suitable for use as a separator for a zinc secondary battery.The He permeability can be preferably measured according to the procedure shown in Evaluation 4 of the Examples described later.

[0023] The LDH separator 16 is preferably gas-impermeable and / or water-impermeable. In other words, the LDH separator 16 is preferably densified to the extent that it is gas-impermeable and / or water-impermeable. In this specification, "gas-impermeable" means that even if helium gas is brought into contact with one side of the object to be measured in water at a differential pressure of 0.5 atm, no bubbles due to helium gas are generated from the other side. In addition, in this specification, "water-impermeable" means that water that has come into contact with one side of the object to be measured does not permeate to the other side, as described in Patent Documents 2 and 3. In other words, the LDH separator 16 being gas-impermeable and / or water-impermeable means that the LDH separator 16 is highly dense enough to prevent gas or water from passing through, and is not a porous film or other porous material that is water-permeable or gas-permeable. In this way, the LDH separator 16 selectively passes only hydroxide ions due to its hydroxide ion conductivity, and can function as a battery separator. Therefore, it is extremely effective in preventing short circuits between the positive and negative electrodes by physically preventing zinc dendrites generated during charging from penetrating the separator. Since the LDH separator 16 has hydroxide ion conductivity, it is possible to efficiently move hydroxide ions between the positive and negative electrodes, thereby realizing charge and discharge reactions in the positive and negative electrodes.

[0024] The LDH separator 16 preferably further comprises a porous substrate. In this case, it is preferable that the pores of the porous substrate are filled with a hydroxide ion conductive layered compound and / or that at least one surface of the porous substrate is provided with a surface layer containing the hydroxide ion conductive layered compound. Since the surface layer can effectively prevent the extension of dendrites, the LDH separator 16 provided with such a surface layer is particularly excellent in resistance to dendrite short circuit. The surface layer may be provided only on one surface of the porous substrate, or on both surfaces of the porous substrate. It is particularly preferable that the hydroxide ion conductive layered compound is incorporated throughout the entire thickness of the porous substrate. However, the pores of the porous substrate do not need to be completely blocked, and a small amount of residual pores may be present.

[0025] The porous substrate is preferably made of a polymer material. The polymer porous substrate has the following advantages: 1) flexibility (so it is difficult to break even if it is thinned); 2) the porosity can be easily increased; 3) the conductivity can be easily increased (because the thickness can be reduced while increasing the porosity); and 4) it is easy to manufacture and handle. In addition, by utilizing the advantage derived from the flexibility of 1), 5) the LDH separator including the porous substrate made of a polymer material can be easily folded or sealed and joined. Preferable examples of the polymer material include polystyrene, polyethersulfone, polypropylene, epoxy resin, polyphenylene sulfide, fluororesin (tetrafluorinated resin: PTFE, etc.), cellulose, nylon, polyethylene, and any combination thereof. More preferably, from the viewpoint of a thermoplastic resin suitable for hot pressing, polystyrene, polyethersulfone, polypropylene, epoxy resin, polyphenylene sulfide, fluororesin (tetrafluorinated resin: PTFE, etc.), nylon, polyethylene, and any combination thereof can be mentioned. All of the above-mentioned various preferable materials have alkali resistance as resistance to the electrolyte of the battery. Particularly preferred polymeric materials are polyolefins such as polypropylene and polyethylene, which are excellent in hot water resistance, acid resistance and alkali resistance, and are low cost, and are most preferably polypropylene or polyethylene. It is particularly preferred that the hydroxide ion-conducting layered compound is incorporated throughout the entire thickness of the porous substrate (e.g., most or almost all of the pores inside the polymeric porous substrate are filled with the hydroxide ion-conducting layered compound). As such a polymeric porous substrate, a commercially available polymeric microporous membrane can be preferably used.

[0026] As described above, the hydroxide ion-conducting layered compound contained in the LDH separator 16 is an LDH and / or an LDH-like compound. Preferred embodiments of the LDH and LDH-like compound will be described below.

[0027] LDH is composed of a plurality of hydroxide base layers and intermediate layers interposed between the hydroxide base layers. The hydroxide base layers are mainly composed of metal elements (typically metal ions) and OH groups. The intermediate layers of LDH are composed of anions and HO. The anions are monovalent or higher anions, preferably monovalent or divalent ions. Preferably, the anions in LDH are OH - and / or CO3 2- In addition, LDH has excellent ionic conductivity due to its inherent properties. In general, LDH contains M 2+ 1-x M 3+ x (OH)2A n- x / n ·mH2O (in the formula, M 2+ is a divalent cation, M 3+ is a trivalent cation, and A n- is an anion with a valence of n, n is an integer of 1 or more, x is 0.1 to 0.4, and m is 0 or more. In the above basic formula, M 2+ can be any divalent cation, but preferred examples include Mg 2+ , Ca 2+ and Zn 2+ More preferably, Mg 2+ It is. 3+ can be any trivalent cation, but preferred examples include Al 3+ or Cr 3+ More preferably, Al 3+ A n- can be any anion, but preferred examples include OH - and CO3 2- Therefore, in the above basic composition formula, M 2+ Mg 2+ Including M 3+ Al 3+ Including A n- OH - and / or CO3 2-It is preferable that the formula contains the formula. n is an integer of 1 or more, preferably 1 or 2. x is 0.1 to 0.4, preferably 0.2 to 0.35. m is an arbitrary number representing the number of moles of water, and is a real number of 0 or more, typically exceeding 0 or 1 or more. However, the above basic composition formula is merely a formula of a "basic composition" typically exemplified for LDH, and the constituent ions can be appropriately replaced. For example, in the above basic composition formula, M 3+ Part or all of the cations are tetravalent or more (e.g., Ti 4+ In that case, the anion A in the above general formula may be replaced by n- The coefficient x / n may be changed as appropriate.

[0028] For example, the hydroxide basic layer of the LDH preferably contains Mg, Al, and OH groups, and further contains Ti (i.e., contains Mg, Al, Ti, and OH groups), which is particularly preferred in terms of exhibiting excellent alkali resistance. In this case, the hydroxide basic layer may contain other elements or ions as long as it contains Mg, Al, and OH groups (and optionally Ti). For example, the LDH or hydroxide basic layer may contain Y and / or Zn. In addition, when the LDH or hydroxide basic layer contains Y and / or Zn, the LDH or hydroxide basic layer may not contain Al or Ti. However, the hydroxide basic layer preferably contains Mg, Al, Ti, and OH groups as main components. That is, the hydroxide basic layer is preferably mainly composed of Mg, Al, Ti, and OH groups. Therefore, the hydroxide basic layer is typically composed of Mg, Al, Ti, OH groups, and, in some cases, unavoidable impurities. The atomic ratio of Ti / Al in the LDH, as determined by energy dispersive X-ray analysis (EDS), is preferably 0.5 to 12, more preferably 1.0 to 12. Within the above range, the effect of suppressing short circuits caused by zinc dendrites (i.e., dendrite resistance) can be more effectively achieved without impairing ion conductivity. For the same reason, the atomic ratio of Ti / (Mg+Ti+Al) in the LDH, as determined by energy dispersive X-ray analysis (EDS), is preferably 0.1 to 0.7, more preferably 0.2 to 0.7. In addition, the atomic ratio of Al / (Mg+Ti+Al) in the LDH is preferably 0.05 to 0.4, more preferably 0.05 to 0.25. Furthermore, the atomic ratio of Mg / (Mg+Ti+Al) in the LDH is preferably 0.2 to 0.7, more preferably 0.2 to 0.6. The EDS analysis is preferably performed using an EDS analyzer (e.g., X-act, manufactured by Oxford Instruments) by 1) capturing an image at an accelerating voltage of 20 kV and a magnification of 5,000x, 2) performing three-point analysis in point analysis mode with an interval of about 5 μm, 3) repeating the above 1) and 2) once more, and 4) calculating the average value of the total six points.

[0029] Alternatively, the hydroxide basic layer of the LDH may contain Ni, Al, Ti, and OH groups. In this case, the hydroxide basic layer may contain other elements or ions as long as it contains Ni, Al, Ti, and OH groups. However, it is preferable that the hydroxide basic layer contains Ni, Al, Ti, and OH groups as main components. That is, it is preferable that the hydroxide basic layer mainly consists of Ni, Al, Ti, and OH groups. Therefore, the hydroxide basic layer is typically composed of Ni, Al, Ti, OH groups, and unavoidable impurities in some cases. The atomic ratio of Ti / (Ni+Ti+Al) in the LDH determined by energy dispersive X-ray analysis (EDS) is preferably 0.10 to 0.90, more preferably 0.20 to 0.80, even more preferably 0.25 to 0.70, and particularly preferably 0.30 to 0.61. Within the above ranges, both alkali resistance and ion conductivity can be improved. Therefore, the hydroxide ion conductive layered compound may contain a large amount of Ti so as to by-produce not only LDH but also titania. That is, the hydroxide ion conductive layered compound may further contain titania. The inclusion of titania is expected to increase hydrophilicity and improve wettability with the electrolyte (i.e., improve conductivity).

[0030] The LDH-like compound preferably contains (i) Mg and (ii) one or more elements including at least Ti selected from the group consisting of Ti, Y, and Al. In this way, by using an LDH-like compound that is a hydroxide and / or oxide having a layered crystal structure containing at least Mg and Ti as a hydroxide ion conductive material instead of a conventional LDH, it is possible to achieve excellent alkali resistance and more effectively suppress short circuits caused by zinc dendrites. Therefore, a preferred LDH-like compound is a hydroxide and / or oxide having a layered crystal structure containing (i) Mg and (ii) one or more elements including at least Ti selected from the group consisting of Ti, Y, and Al. Therefore, a typical LDH-like compound is a composite hydroxide and / or oxide of Mg, Ti, optionally Y, and optionally Al, and particularly preferably a composite hydroxide and / or oxide of Mg, Ti, Y, and Al. The above elements may be replaced with other elements or ions to the extent that the basic properties of the LDH-like compound are not impaired, but it is preferable that the LDH-like compound does not contain Ni.

[0031] The LDH-like compound can be identified by X-ray diffraction. Specifically, when X-ray diffraction is performed on the surface of the LDH separator 16, a peak derived from the LDH-like compound is typically detected in the range of 5°≦2θ≦10°, more typically in the range of 7°≦2θ≦10°. As described above, LDH is a substance having an alternating laminate structure in which exchangeable anions and H2O exist as intermediate layers between stacked hydroxide basic layers. In this regard, when LDH is measured by X-ray diffraction, a peak due to the crystal structure of LDH (i.e., the (003) peak of LDH) is essentially detected at a position of 2θ=11 to 12°. In contrast, when an LDH-like compound is measured by X-ray diffraction, a peak is typically detected in the above-mentioned range shifted to the lower angle side from the above-mentioned peak position of LDH. In addition, the interlayer distance of the layered crystal structure can be determined by the Bragg formula using 2θ corresponding to the peak derived from the LDH-like compound in X-ray diffraction. The interlayer distance of the layered crystal structure constituting the LDH-like compound thus determined is typically 0.883 to 1.8 nm, and more typically 0.883 to 1.3 nm.

[0032] The atomic ratio of Mg / (Mg+Ti+Y+Al) in the LDH-like compound determined by energy dispersive X-ray analysis (EDS) is preferably 0.03 to 0.25, more preferably 0.05 to 0.2. The atomic ratio of Ti / (Mg+Ti+Y+Al) in the LDH-like compound is preferably 0.40 to 0.97, more preferably 0.47 to 0.94. The atomic ratio of Y / (Mg+Ti+Y+Al) in the LDH-like compound is preferably 0 to 0.45, more preferably 0 to 0.37. The atomic ratio of Al / (Mg+Ti+Y+Al) in the LDH-like compound is preferably 0 to 0.05, more preferably 0 to 0.03. Within the above range, the alkali resistance is more excellent, and the effect of suppressing short circuits caused by zinc dendrites (i.e., dendrite resistance) can be more effectively realized. Regarding LDH separators, conventionally known LDHs have the general formula: M 2+ 1-x M 3+ x (OH)2A n- x / n ·mH2O (in the formula, M 2+ is a divalent cation, M 3+ is a trivalent cation, and A n- is an n-valent anion, n is an integer of 1 or more, x is 0.1 to 0.4, and m is 0 or more). In contrast, the above atomic ratio in the LDH-like compound generally deviates from the above general formula of LDH. For this reason, it can be said that the LDH-like compound generally has a composition ratio (atomic ratio) different from that of conventional LDH. It is preferable to perform the EDS analysis by using an EDS analyzer (e.g., X-act, manufactured by Oxford Instruments) by 1) capturing an image at an accelerating voltage of 20 kV and a magnification of 5,000 times, 2) performing three-point analysis with an interval of about 5 μm in the point analysis mode, 3) repeating the above 1) and 2) once more, and 4) calculating the average value of a total of six points.

[0033] According to another preferred embodiment of the present invention, the LDH-like compound may be a hydroxide and / or oxide having a layered crystal structure, comprising (i) Ti, Y, and optionally Al and / or Mg, and (ii) an additional element M. Thus, a typical LDH-like compound is a composite hydroxide and / or composite oxide of Ti, Y, the additional element M, optionally Al, and optionally Mg. The additional element M is In, Bi, Ca, Sr, Ba, or a combination thereof. The above elements may be replaced with other elements or ions to the extent that the basic properties of the LDH-like compound are not impaired, but it is preferred that the LDH-like compound does not contain Ni.

[0034] In the LDH separator according to the above embodiment, the atomic ratio of Ti / (Mg+Al+Ti+Y+M) in the LDH-like compound determined by energy dispersive X-ray analysis (EDS) is preferably 0.50 to 0.85, more preferably 0.56 to 0.81. The atomic ratio of Y / (Mg+Al+Ti+Y+M) in the LDH-like compound is preferably 0.03 to 0.20, more preferably 0.07 to 0.15. The atomic ratio of M / (Mg+Al+Ti+Y+M) in the LDH-like compound is preferably 0.03 to 0.35, more preferably 0.03 to 0.32. The atomic ratio of Mg / (Mg+Al+Ti+Y+M) in the LDH-like compound is preferably 0 to 0.10, more preferably 0 to 0.02. The atomic ratio of Al / (Mg+Al+Ti+Y+M) in the LDH-like compound is preferably 0 to 0.05, more preferably 0 to 0.04. Within the above range, the alkali resistance is more excellent, and the effect of suppressing short circuits caused by zinc dendrites (i.e., dendrite resistance) can be more effectively realized. Incidentally, LDHs conventionally known as LDH separators are represented by the general formula: M 2+ 1-x M 3+ x (OH)2A n- x / n ·mH2O (in the formula, M 2+ is a divalent cation, M 3+ is a trivalent cation, and A n-is an n-valent anion, n is an integer of 1 or more, x is 0.1 to 0.4, and m is 0 or more). In contrast, the above atomic ratio in the LDH-like compound generally deviates from the above general formula of LDH. For this reason, it can be said that the LDH-like compound in this embodiment generally has a composition ratio (atomic ratio) different from that of conventional LDH. It is preferable to perform the EDS analysis using an EDS analyzer (e.g., X-act, manufactured by Oxford Instruments) by 1) capturing an image at an accelerating voltage of 20 kV and a magnification of 5,000 times, 2) performing three-point analysis with an interval of about 5 μm in the point analysis mode, 3) repeating the above 1) and 2) once more, and 4) calculating the average value of a total of six points.

[0035] According to yet another preferred embodiment of the present invention, the LDH-like compound is a hydroxide and / or oxide having a layered crystal structure containing Mg, Ti, Y, and optionally Al and / or In, and the LDH-like compound may be present in the form of a mixture with In(OH)3. The LDH-like compound of this embodiment is a hydroxide and / or oxide having a layered crystal structure containing Mg, Ti, Y, and optionally Al and / or In. Thus, a typical LDH-like compound is a composite hydroxide and / or composite oxide of Mg, Ti, Y, optionally Al, and optionally In. The In that may be contained in the LDH-like compound may not only be that which is intentionally added to the LDH-like compound, but may also be that which is inevitably mixed into the LDH-like compound due to the formation of In(OH)3 or the like. The above elements may be replaced with other elements or ions to the extent that the basic properties of the LDH-like compound are not impaired, but it is preferable that the LDH-like compound does not contain Ni. Incidentally, LDHs conventionally known for LDH separators are represented by the general formula: M 2+ 1-x M 3+ x (OH)2A n- x / n ·mH2O (in the formula, M 2+ is a divalent cation, M 3+ is a trivalent cation, and A n-is an n-valent anion, n is an integer of 1 or more, x is 0.1 to 0.4, and m is 0 or more). In contrast, the atomic ratio in the LDH-like compound generally deviates from the above general formula of LDH. Therefore, it can be said that the LDH-like compound in this embodiment generally has a composition ratio (atomic ratio) different from that of conventional LDH.

[0036] The mixture according to the above embodiment contains not only the LDH-like compound but also In(OH)3 (typically composed of the LDH-like compound and In(OH)3). The inclusion of In(OH)3 can effectively improve the alkali resistance and dendrite resistance of the LDH separator. The content ratio of In(OH)3 in the mixture is preferably an amount that can improve the alkali resistance and dendrite resistance without substantially impairing the hydroxide ion conductivity of the LDH separator, and is not particularly limited. In(OH)3 may have a cubic crystal structure, and may have a structure in which In(OH)3 crystals are surrounded by the LDH-like compound. In(OH)3 can be identified by X-ray diffraction.

[0037] The zinc secondary battery 10 is preferably provided with a stacked cell 11 in, for example, a battery container 20. As shown in FIG. 3, the stacked cell 11 includes a plurality of negative electrode plates 12, a plurality of positive electrode plates 14, a plurality of pairs of LDH separators 16, and an electrolyte (not shown), and the negative electrode plates 12 and the positive electrode plates 14 are alternately stacked with the LDH separator 16 sandwiched therebetween. A low conductive separator 16a is disposed on the first surface S1 side of each of the plurality of negative electrode plates 12, and a high conductive separator 16b is disposed on the second surface S2 side of each of the plurality of negative electrode plates 12. That is, the zinc secondary battery 10 preferably has a plurality of unit cells including the negative electrode plates 12, the negative electrode current collector 13, the positive electrode plates 14, the positive electrode current collector 15, the LDH separator 16, and the electrolyte, and the plurality of unit cells form the stacked cell 11 as a whole. This is a so-called assembled battery or stacked battery configuration, and is advantageous in that it can provide high voltage and large current.

[0038] The negative electrode plate 12 includes a negative electrode active material 12a. The negative electrode active material 12a includes at least one selected from the group consisting of zinc, zinc oxide, zinc alloy, and zinc compound. Zinc may be included in any form of zinc metal, zinc compound, or zinc alloy, so long as it has electrochemical activity suitable for a negative electrode. Preferred examples of the negative electrode material include zinc oxide, zinc metal, calcium zincate, and the like, and a mixture of zinc metal and zinc oxide is more preferred. The negative electrode active material may be configured in a gel form, or may be mixed with an electrolyte to form a negative electrode mixture. For example, a gelled negative electrode can be easily obtained by adding an electrolyte and a thickener to the negative electrode active material. Examples of the thickener include polyvinyl alcohol, polyacrylate, CMC, alginic acid, and the like, and polyacrylic acid is preferred because of its excellent chemical resistance to strong alkali.

[0039] As the zinc alloy, a zinc alloy containing no mercury or lead, known as a mercury-free zinc alloy, can be used. For example, a zinc alloy containing 0.01 to 0.1 mass% indium, 0.005 to 0.02 mass% bismuth, and 0.0035 to 0.015 mass% aluminum is preferable because it has an effect of suppressing hydrogen gas generation. In particular, indium and bismuth are advantageous in terms of improving discharge performance. The use of a zinc alloy for the negative electrode can improve safety by suppressing hydrogen gas generation by slowing down the self-dissolution rate in an alkaline electrolyte.

[0040] The shape of the negative electrode material is not particularly limited, but it is preferably in powder form, which increases the surface area and allows for high-current discharge. The average particle size of the negative electrode material is preferably in the range of 3 to 100 μm in minor axis in the case of a zinc alloy, and within this range, the large surface area makes it suitable for high-current discharge, and it is easy to mix uniformly with the electrolyte and gelling agent, and is easy to handle when assembling a battery.

[0041] Typically, the negative electrode plate 12 further includes a negative electrode current collector 12b. The negative electrode current collector 12b is provided inside and / or on the surface of the negative electrode active material 12a, except for a portion extending as the negative electrode current collector 13. Preferably, the negative electrode active material 12a is provided on both sides of the negative electrode current collector 12b. It is preferable that a metallic negative electrode current collector 13 is further provided, which extends (for example, upward) from or connects to the negative electrode current collector 12b. It is preferable that the negative electrode current collector 13 is provided at a position where it does not overlap with the positive electrode current collector 15. The negative electrode current collector 13 may be made of the same material as the negative electrode current collector 12b, or may be made of a different material. In any case, the negative electrode current collector 13 may be extended by adding another current collector such as a tab lead to such a tab. Preferably, multiple negative current collecting members 13 are joined to one negative terminal 26 or to a further negative current collecting member 13 electrically connected thereto. The negative terminal 26 is typically connected to the negative current collecting member 13 and protrudes from the battery container 20.

[0042] From the viewpoint of active material adhesion, it is preferable to use a metal plate having a plurality (or a large number) of openings as the negative electrode current collector 12b. Preferred examples of such a negative electrode current collector 12b include expanded metal, punched metal, metal mesh, and combinations thereof, more preferably copper expanded metal, copper punched metal, and combinations thereof, and particularly preferably copper expanded metal. In this case, for example, a mixture containing zinc oxide powder and / or zinc powder, and optionally a binder (e.g., polytetrafluoroethylene particles) can be applied onto the copper expanded metal to preferably prepare a negative electrode plate consisting of a negative electrode / negative electrode current collector. In this case, it is also preferable to perform a press treatment on the negative electrode plate (i.e., a negative electrode / negative electrode current collector) after drying to prevent the electrode active material from falling off and improve the electrode density. The expanded metal is a mesh-shaped metal plate obtained by pressing and expanding a metal plate while making staggered cuts using an expander, and shaping the cuts into a diamond or tortoiseshell shape. Punching metal, also known as perforated metal, is a metal plate with holes punched into it. Metal mesh is a metal product with a wire mesh structure, and is different from expanded metal and punching metal.

[0043] The positive electrode plate 14 includes a positive electrode active material 14a. The positive electrode active material 14a may be appropriately selected from known positive electrode materials according to the type of zinc secondary battery, and is not particularly limited. For example, in the case of a nickel-zinc secondary battery, a positive electrode plate including nickel hydroxide and / or nickel oxyhydroxide may be used. Alternatively, in the case of an air-zinc secondary battery, an air electrode may be used as the positive electrode plate. Typically, the positive electrode plate 14 further includes a positive electrode collector 14b, and it is preferable that a metallic positive electrode collector member 15 extending (for example, upward) from or connected to the positive electrode collector is further provided. A preferable example of the positive electrode collector is a nickel porous substrate such as a foamed nickel plate. In this case, for example, a paste including an electrode active material such as nickel hydroxide is uniformly applied onto a nickel porous substrate and dried to preferably produce a positive electrode plate consisting of a positive electrode / positive electrode collector. At that time, it is also preferable to perform a press treatment on the dried positive electrode plate (i.e., positive electrode / positive electrode current collector) to prevent the electrode active material from falling off and improve the electrode density. The positive electrode current collector 15 may be made of the same material as the positive electrode current collector, or may be made of a different material. When the positive electrode current collector is a nickel porous substrate such as a foamed nickel plate, it can be processed into a tab shape by pressing it. In either case, the positive electrode current collector 15 may be extended by adding another current collector such as a tab lead to such a tab. In either case, it is preferable that a plurality of positive electrode current collectors 15 are joined to one positive electrode terminal 28 or to a further positive electrode current collector 15 electrically connected thereto. The positive electrode terminal 28 is typically connected to the positive electrode current collector 15 and protrudes from the battery container 20.

[0044] The positive electrode plate 14 may contain at least one additive selected from the group consisting of silver compounds, manganese compounds, and titanium compounds, which can promote a positive electrode reaction that absorbs hydrogen gas generated by a self-discharge reaction. The positive electrode plate 14 may further contain cobalt. Cobalt is preferably contained in the positive electrode plate 14 in the form of cobalt oxyhydroxide. In the positive electrode plate 14, cobalt functions as a conductive additive, thereby contributing to an improvement in charge / discharge capacity.

[0045] 1 and 2, it is preferable that the negative electrode plate 12, the negative electrode current collecting member 13, the positive electrode plate 14, the positive electrode current collecting member 15, and the LDH separator 16 are each arranged vertically, and the positive electrode terminal 28 and the negative electrode terminal 26 are provided on the upper cover 20a of the battery container 20. Therefore, in the case of a multi-layer cell, it is preferable that the cells are multi-layered in the horizontal direction. It is also preferable that the positive electrode current collecting member 15 and the negative electrode current collecting member 13 extend upward.

[0046] The zinc secondary battery 10 may further include a liquid-retaining member (not shown) in contact with the positive electrode plate 14 and / or the negative electrode plate 12. For example, it is preferable that not only the LDH separator 16 but also a liquid-retaining member is interposed between the positive electrode plate 14 and the negative electrode plate 12. It is preferable that the positive electrode plate 14 and / or the negative electrode plate 12 is covered or wrapped with the liquid-retaining member. However, a simple configuration in which the liquid-retaining member is disposed on one side of the positive electrode plate 14 or the negative electrode plate 12 may be used. In any case, by interposing the liquid-retaining member, the electrolyte can be evenly present between the positive electrode plate 14 and / or the negative electrode plate 12 and the LDH separator 16, and the hydroxide ions can be efficiently exchanged between the positive electrode plate 14 and / or the negative electrode plate 12 and the LDH separator 16. The liquid-retaining member is not particularly limited as long as it is a member capable of retaining the electrolyte, but is preferably a sheet-like member. Preferred examples of the liquid-retaining member include nonwoven fabric, water-absorbent resin, liquid-retaining resin, porous sheet, and various spacers, and particularly preferred is nonwoven fabric, which can produce a negative electrode structure with good performance at low cost. The liquid-retaining member or nonwoven fabric preferably has a thickness of 10 to 200 μm, more preferably 20 to 200 μm, even more preferably 20 to 150 μm, particularly preferably 20 to 100 μm, and most preferably 20 to 60 μm. If the thickness is within the above range, a sufficient amount of electrolyte can be retained in the liquid-retaining member while keeping the overall size of the positive electrode structure and / or negative electrode structure compact and without waste.

[0047] When the positive electrode plate 14 and / or the negative electrode plate 12 are covered or wrapped with the liquid retaining member and / or the LDH separator 16, it is preferable that the outer edge of the liquid retaining member and / or the LDH separator 16 is closed (except for the edge from which the positive electrode current collecting member 15 and the negative electrode current collecting member 13 extend). In this case, it is preferable that the closed edge of the outer edge of the liquid retaining member and / or the LDH separator 16 is realized by folding the liquid retaining member and / or the LDH separator 16, or by sealing the liquid retaining members and / or the LDH separators 16 together. Examples of preferable sealing methods include adhesives, heat welding, ultrasonic welding, adhesive tape, sealing tape, and combinations thereof. In particular, since an LDH separator including a porous base material made of a polymer material has an advantage of being flexible and therefore easy to bend, it is preferable to form the LDH separator into a long shape and fold it to form a state in which one side of the outer edge is closed. Thermal welding and ultrasonic welding may be performed using a commercially available heat sealer or the like, but in the case of sealing between LDH separators, it is preferable to perform thermal welding and ultrasonic welding by sandwiching the outer peripheral portion of the liquid-retaining member between the LDH separators constituting the outer peripheral portion, in order to perform more effective sealing. On the other hand, the adhesive, adhesive tape, and sealing tape may be commercially available products, but it is preferable to use those containing a resin having alkali resistance in order to prevent deterioration in an alkaline electrolyte. From this viewpoint, examples of preferable adhesives include epoxy resin adhesives, natural resin adhesives, modified olefin resin adhesives, and modified silicone resin adhesives, and among them, epoxy resin adhesives are more preferable because they are particularly excellent in alkali resistance. An example of a product of an epoxy resin adhesive is the epoxy adhesive Hysol (registered trademark) (manufactured by Henkel).

[0048] It is preferable that the outer edge of one side of the LDH separator 16, which is the upper end, is open. This open-top type configuration makes it possible to deal with problems that occur when a nickel-zinc battery or the like is overcharged. That is, when a nickel-zinc battery or the like is overcharged, oxygen (O2) may be generated at the positive electrode plate 14, but the LDH separator has such a high density that it allows only hydroxide ions to pass through, and therefore does not allow O2 to pass through. In this regard, according to the open-top type configuration, O2 can be released above the positive electrode plate 14 in the battery container 20 and sent to the negative electrode plate 12 side through the open-top part, whereby Zn, the negative electrode active material, can be oxidized by O2 and returned to ZnO. By going through such an oxygen reaction cycle, the open-top type stacked cell 11 can be used in a sealed zinc secondary battery to improve overcharge resistance. Note that even if the outer edge of one side of the LDH separator 16 or the liquid-retaining member, which is the upper end, is closed, the same effect as that of the open-top type configuration can be expected by providing a vent in a part of the closed outer edge. For example, the outer edge of one side that will be the upper end of the LDH separator may be sealed and then an air hole may be opened, or during sealing, part of the outer edge may be left unsealed so that an air hole will be formed.

[0049] The electrolyte preferably contains an aqueous solution of an alkali metal hydroxide. The electrolyte is not shown in Figs. 1 to 4 because it is distributed throughout the positive electrode plate 14 and the negative electrode plate 12. Examples of alkali metal hydroxides include potassium hydroxide, sodium hydroxide, lithium hydroxide, and ammonium hydroxide, with potassium hydroxide being more preferable. In order to suppress the self-dissolution of zinc and / or zinc oxide, a zinc compound such as zinc oxide or zinc hydroxide may be added to the electrolyte. As described above, the electrolyte may be mixed with the positive electrode active material and / or the negative electrode active material to be present in the form of a positive electrode mixture and / or a negative electrode mixture. In addition, the electrolyte may be gelled to prevent leakage of the electrolyte. As the gelling agent, it is preferable to use a polymer that absorbs the solvent of the electrolyte and swells, and polymers such as polyethylene oxide, polyvinyl alcohol, and polyacrylamide, and starch are used.

[0050] The battery container 20 is preferably made of resin. The resin constituting the battery container 20 is preferably a resin resistant to alkali metal hydroxides such as potassium hydroxide, more preferably a polyolefin resin, ABS resin, or modified polyphenylene ether, and even more preferably ABS resin or modified polyphenylene ether. The battery container 20 has an upper lid 20a. The battery container 20 (e.g., the upper lid 20a) may have a pressure relief valve for releasing gas. In addition, a group of containers in which two or more battery containers 20 are arranged may be housed in an outer frame to form a battery module. EXAMPLES

[0051] The present invention will be described more specifically with reference to the following examples. The LDH separators and zinc secondary batteries prepared in the following examples were evaluated as follows.

[0052] Rating 1 : Observation of microstructure The surface microstructure of the LDH separator was observed using a scanning electron microscope (SEM, JSM-6610LV, JEOL) at an accelerating voltage of 10 to 20 kV.

[0053] Rating 2 :Elemental analysis evaluation (EDS) A composition analysis was performed on the LDH separator surface using an EDS analyzer (instrument name: X-act, manufactured by Oxford Instruments), and it was confirmed that the specified elements were incorporated into the crystals. This analysis was performed by 1) capturing images at an accelerating voltage of 20 kV and a magnification of 5,000 times, 2) performing three-point analysis with an interval of about 5 μm in point analysis mode, and 3) repeating the above 1) and 2) once more.

[0054] Rating 3 : Identification of hydroxide ion conducting layered compounds The crystalline phase of the hydroxide ion conductive layered compound was measured using an X-ray diffractometer (Rigaku Corporation, RINT TTR III) under the measurement conditions of voltage: 50 kV, current value: 300 mA, and measurement range: 5 to 70° to obtain an XRD profile.

[0055] Rating 4 :He transmission measurement In order to evaluate the denseness of the LDH separator from the viewpoint of He permeability, a He permeability test was carried out as follows. First, a He permeability measurement system 310 shown in Figures 7A and 7B was constructed. The He permeability measurement system 310 was configured so that He gas from a gas cylinder filled with He gas was supplied to a sample holder 316 via a pressure gauge 312 and a flow meter 314 (digital flow meter), and the He gas was permeated from one side of an LDH separator 318 held by this sample holder 316 to the other side and discharged.

[0056] The sample holder 316 has a structure including a gas supply port 316a, a sealed space 316b, and a gas exhaust port 316c, and was assembled as follows. First, an adhesive 322 was applied along the outer periphery of the LDH separator 318, and the LDH separator 318 was attached to a jig 324 (made of ABS resin) having an opening in the center. Butyl rubber packings were arranged as sealing members 326a, 326b at the upper and lower ends of the jig 324, and the sealing members 326a, 326b were sandwiched from the outside by support members 328a, 328b (made of PTFE) having openings made of flanges. In this way, the LDH separator 318, the jig 324, the sealing member 326a, and the support member 328a defined a sealed space 316b. The support members 328a, 328b were tightly fastened together by a fastening means 330 using screws so that He gas would not leak from any part other than the gas exhaust port 316c. A gas supply pipe 334 was connected via a joint 332 to a gas supply port 316 a of the sample holder 316 thus assembled.

[0057] Next, He gas was supplied to the He permeability measurement system 310 via the gas supply pipe 334, and was allowed to permeate through the LDH separator 318 held in the sample holder 316. At this time, the gas supply pressure and flow rate were monitored by the pressure gauge 312 and the flow meter 314. After the He gas permeation was carried out for 1 to 30 minutes, the He permeability was calculated. The He permeability was calculated based on the amount of He gas permeated per unit time F (cm 3 / min), the pressure difference P (atm) applied to the LDH separator when He gas permeates, and the membrane area S (cm2 ) was used to calculate the amount of He gas permeation F (cm 3 / min) was read directly from the flow meter 314. The differential pressure P was the gauge pressure read from the pressure gauge 312. The He gas was supplied so that the differential pressure P was within the range of 0.05 to 0.90 atm. The He permeability was measured for each of the low conductivity separator and the high conductivity separator.

[0058] Rating 5 : Measurement of ionic conductivity The conductivity of the LDH separator in the electrolyte was measured using an electrochemical measurement system shown in FIG. 8 as follows. The LDH separator sample S was sandwiched between 1 mm thick silicone packings 440 on both sides and incorporated into a PTFE flange-type cell 442 with an inner diameter of 6 mm. As an electrode 446, a #100 mesh nickel wire mesh was incorporated into the cell 442 in the form of a cylinder with a diameter of 6 mm, and the distance between the electrodes was set to 2.2 mm. As the electrolyte 444, a 6 M KOH aqueous solution was filled into the cell 442. Using an electrochemical measurement system (potentio / galvanostat-frequency response analyzer, Solartron 1287A and 1255B models), measurements were performed under conditions of a frequency range of 1 MHz to 0.1 Hz and an applied voltage of 10 mV, and the intercept of the real axis was taken as the resistance of the LDH separator sample S. The same measurement as above was performed without the LDH separator sample S, and the blank resistance was also determined. The difference between the resistance of LDH separator sample S and the blank resistance was taken as the resistance of the LDH separator. The ionic conductivity was calculated using the obtained resistance of the LDH separator and the area of ​​LDH separator sample S. The above-mentioned ionic conductivity measurement was performed for each of the low conductivity separator and the high conductivity separator.

[0059] Rating 6 : Cycle test A cycle test of the zinc secondary battery was carried out as follows. First, the zinc secondary battery was formed by charging at 0.1C and discharging at 0.2C using a charge / discharge device (TOSCAT3100, manufactured by Toyo Systems Co., Ltd.). Then, a 1C charge / discharge cycle was carried out. While repeatedly carrying out charge / discharge cycles under the same conditions, the voltage between the positive and negative electrodes was monitored with a voltmeter, and the presence or absence of a sudden voltage drop (specifically, a voltage drop of 5mV or more from the voltage plotted immediately before) due to a short circuit caused by zinc dendrite between the positive and negative electrodes was examined, and the results were evaluated according to the following criteria. No short circuits: No sudden voltage drop was observed during charging even after 300 cycles. Short circuit: The above sudden voltage drop was observed during charging within 300 cycles.

[0060] Examples A1 to A4 An LDH separator containing an Mg-(Al,Ti,Y)-LDH-like compound and a zinc secondary battery including the same were produced and evaluated as follows.

[0061] (1) Preparation of polymeric porous substrate A commercially available polyethylene microporous membrane with a porosity of 50%, an average pore size of 0.1 μm, and a thickness of 20 μm was prepared as a polymeric porous substrate, and cut to a size of 16 cm×14 cm.

[0062] (2) Alumina-titania-yttria sol coating on polymeric porous substrate An amorphous alumina solution (Al-L7, manufactured by Taki Chemical Industry Co., Ltd.), a titania solution (AM-15, manufactured by Taki Chemical Industry Co., Ltd.), and yttria sol were applied by dip coating to the substrate prepared in (1) above. The dip solution was prepared by mixing the amorphous alumina solution, the titania solution, and the yttria sol so that Ti / (Y+Al) (molar ratio) = 2 and Y / Al (molar ratio) = 8. The dip coating was performed by immersing the substrate in 1 L of the sol solution and then pulling it up vertically. The dip-coated substrate was then dried at room temperature for 1 hour.

[0063] (3) Preparation of raw material aqueous solution As raw materials, magnesium nitrate hexahydrate (Mg(NO3)2·6H2O, manufactured by Kanto Chemical Co., Ltd.) and urea ((NH2)2CO, manufactured by Sigma-Aldrich) were prepared. Magnesium nitrate hexahydrate was 0.0075 mol / L, urea / NO3 - The raw materials were weighed out so that the molar ratio was 96 and placed in a beaker, and ion-exchanged water was added thereto to make the total volume 3 L. After that, the mixture was stirred to obtain a raw material aqueous solution.

[0064] (4) Film formation by hydrothermal treatment The raw material aqueous solution and the dip-coated substrate were both sealed in a Teflon (registered trademark) sealed container (autoclave container, capacity 5 L, outer stainless steel jacket). At this time, the substrate was fixed by floating it from the bottom of the Teflon (registered trademark) sealed container, and placed vertically so that the solution was in contact with both sides of the substrate. Thereafter, the substrate was subjected to hydrothermal treatment at a hydrothermal temperature of 120°C for 30 hours to form an LDH-like compound on the surface and inside of the substrate. After a predetermined time had passed, the substrate was removed from the sealed container, washed with ion-exchanged water, and dried overnight at room temperature to obtain an LDH separator in which an LDH-like compound was formed on both sides of the porous substrate and in the pores.

[0065] (5) Roll press processing For Examples A1 and A2, one LDH separator obtained in (4) above was roll-pressed to produce a more dense LDH separator. Meanwhile, for Examples A3 and A4, one LDH separator obtained in (4) above was roll-pressed to produce a more dense LDH separator as a high-conductivity separator. In addition, two LDH separators obtained in (4) above were roll-pressed in a stacked state to integrate the two separators into a low-conductivity separator. At this time, the temperature and load of the roll press were appropriately changed as shown in Table 1. In this way, a plurality of LDH separators with different ionic conductivities and thicknesses were produced.

[0066] (6) Preparation of zinc secondary battery The LDH separators (highly conductive separator and lowly conductive separator) obtained in (5) above, as well as a positive electrode plate, a positive electrode current collector, a negative electrode plate, a negative electrode current collector, a nonwoven fabric, a battery container, and an electrolyte solution shown below were prepared. Positive electrode plate: The pores of the nickel foam are filled with a positive electrode paste containing nickel hydroxide and a binder, and then dried (there is an uncoated area near one edge of the nickel foam where the positive electrode paste is not applied). Positive electrode current collecting material: The uncoated area of ​​the foamed nickel that makes up the positive electrode plate is compressed with a roll press to form a tab, and a tab lead (made of pure nickel, thickness: 100μm) is ultrasonically welded to this tab to extend it. Negative electrode plate: A negative electrode paste containing ZnO powder, metallic Zn powder, polytetrafluoroethylene (PTFE) and propylene glycol is pressed onto a current collector (copper expanded metal) (there is an uncoated area near one edge of the copper expanded metal where the negative electrode paste is not applied). Negative electrode current collecting material: A tab lead (made of copper, thickness: 100 μm) is ultrasonically welded to the uncoated part of the copper expanded metal. Non-woven fabric: Polypropylene, thickness 100μm Battery container: Box-shaped case made of modified polyphenylene ether resin (equipped with a pressure relief valve to release gas generated inside the case); Internal dimensions: length 190 mm, width 24 mm, height 165 mm; External dimensions: length 200 mm, width 30 mm, height 170 mm (not including the height of the positive and negative terminals) Electrolyte: 0.4M zinc oxide dissolved in 5.4M KOH solution

[0067] The positive electrode plate was wrapped in nonwoven fabric so as to cover both sides, so that the nonwoven fabric slightly protruded from the remaining three sides except for the side from which the positive electrode current collector member extended. The excess portion of the nonwoven fabric protruding from the three sides of the positive electrode plate was heat-sealed with a heat seal bar to obtain a positive electrode structure. The negative electrode plate was also wrapped in nonwoven fabric and LDH separator in order from both sides, so that the nonwoven fabric and LDH separator slightly protruded from the remaining three sides except for the side from which the negative electrode current collector member extended. At this time, a low conductive separator was arranged on the first surface side of the negative electrode plate, and a high conductive separator was arranged on the second surface side of the negative electrode plate. The excess portion of the nonwoven fabric and LDH separator protruding from the three sides of the negative electrode plate was heat-sealed with a heat seal bar to obtain a negative electrode structure. In this way, a plurality of positive electrode structures and a plurality of negative electrode structures were prepared.

[0068] An electrode laminate was produced by alternately stacking 12 positive electrode structures and 13 negative electrode structures. As in the configuration shown in FIG. 3, the multiple positive electrode current collectors 15 and the multiple negative electrode current collectors 13 are designed to extend from different positions from each other when viewed in a plan view, so that the multiple positive electrode current collectors 15 are stacked on top of each other, while the multiple negative electrode current collectors 13 are stacked on top of each other at a different position. As shown in FIGS. 1 and 2, the overlapping portions of the multiple positive electrode current collectors 15 were joined together to the positive electrode terminal 28 by laser welding. Similarly, the overlapping portions of the multiple negative electrode current collectors 13 were joined together to the negative electrode terminal 26 by laser welding. In this way, a stack of electrode structures including the positive electrode current collectors 15 and the negative electrode current collectors 13 was obtained as a laminated cell 11. The laminated cell 11 was placed in a box-shaped battery container 20, an electrolyte was injected to impregnate the laminated cell 11, and the upper lid 20a was closed and sealed. In this manner, a zinc secondary battery was produced.

[0069] (7) Various evaluations The obtained LDH separator and zinc secondary battery were subjected to evaluations 1 to 6. The results were as follows. - Rating 1: A large number of plate-like shapes characteristic of LDH were observed. - Evaluation 2: As a result of EDS elemental analysis, the constituent elements of LDH-like compounds, Mg, Al, Ti, and Y, were detected. In other words, it was confirmed that these elements were incorporated and crystallized as hydroxide ion conductive layered compounds. - Evaluation 3: In the XRD profile, a peak derived from an LDH-like compound was detected in the range of 5°≦2θ≦10°. Since the (003) peak position of LDH is usually observed at 2θ=11 to 12°, the above peak is considered to be the (003) peak of LDH shifted to the lower angle side. Therefore, although the above peak may not be called LDH, it suggests that it is a peak derived from a hydroxide and / or oxide of a layered crystal structure having hydroxide ion conductivity (i.e., an LDH-like compound). - Evaluation 4: In Examples A1 to A4, extremely high density was confirmed with a He permeability of 0 cm / min·atm. - Evaluation 5: Ionic conductivity of low-conductivity separator C L , ionic conductivity of high-conductivity separator C H , and ratio C H / C L was as shown in Table 1. - Evaluation 6: As shown in Table 1, in Examples A2 to A4, excellent cycle durability was confirmed, with no short circuit caused by zinc dendrites even after 300 cycles. On the other hand, in Example A1 (Comparative Example), a short circuit caused by zinc dendrites occurred in less than 300 cycles, and it was found to have poor cycle durability.

[0070] [Table 1]

[0071] Examples B1 to B3 An LDH separator containing Mg-(Al,Ti)-LDH and a zinc secondary battery including the same were produced and evaluated as follows.

[0072] (1) Preparation of polymeric porous substrate A commercially available polyethylene microporous membrane with a porosity of 50%, an average pore size of 0.1 μm, and a thickness of 20 μm was prepared as a polymeric porous substrate, and cut to a size of 16 cm×14 cm.

[0073] (2) Alumina-titania sol coating on polymeric porous substrate An amorphous alumina solution (Al-L7, manufactured by Taki Chemical Industry Co., Ltd.) and a titania sol solution (AM-15, manufactured by Taki Chemical Industry Co., Ltd.) were applied by dip coating to the substrate prepared in (1) above. The dip solution was prepared by mixing the amorphous alumina solution and the titania sol solution so that Ti / Al (molar ratio) = 2. The dip coating was performed by immersing the substrate in 1 L of the sol solution and then pulling it up vertically. The dip-coated substrate was then dried at room temperature for 1 hour.

[0074] (3) Preparation of raw material aqueous solution As raw materials, magnesium nitrate hexahydrate (Mg(NO3)2·6H2O, manufactured by Kanto Chemical Co., Ltd.) and urea ((NH2)2CO, manufactured by Sigma-Aldrich) were prepared. Magnesium nitrate hexahydrate was 0.015 mol / L, urea / NO3 - The raw materials were weighed out so that the molar ratio was 32 and placed in a beaker, and ion-exchanged water was added thereto to make the total volume 3 L. After that, the mixture was stirred to obtain a raw material aqueous solution.

[0075] (4) Film formation by hydrothermal treatment The raw material aqueous solution and the dip-coated substrate were both sealed in a Teflon (registered trademark) sealed container (autoclave container, capacity 5 L, outer stainless steel jacket). At this time, the substrate was fixed by floating it from the bottom of the Teflon (registered trademark) sealed container, and placed vertically so that the solution was in contact with both sides of the substrate. Thereafter, LDH was formed on the surface and inside of the substrate by performing hydrothermal treatment at a hydrothermal temperature of 90°C for 30 hours. After a predetermined time had passed, the substrate was removed from the sealed container, washed with ion-exchanged water, and dried overnight at room temperature to form LDH on the surface and in the pores of the porous substrate. In this way, an LDH separator was obtained.

[0076] (5) Roll press processing For Example B1, one LDH separator obtained in (4) above was roll-pressed to produce a more dense LDH separator. Meanwhile, for Examples B2 and B3, one LDH separator obtained in (4) above was roll-pressed to produce a more dense LDH separator as a high-conductivity separator. In addition, two LDH separators obtained in (4) above were roll-pressed in a stacked state to integrate the two separators into a low-conductivity separator. At this time, the temperature and load of the roll press were appropriately changed as shown in Table 2. In this way, a plurality of LDH separators with different ionic conductivities and thicknesses were produced.

[0077] (6) Preparation of zinc secondary battery Zinc secondary batteries were produced in the same manner as in Examples A1 to A4.

[0078] (7) Various evaluations The obtained LDH separator and zinc secondary battery were subjected to evaluations 1 to 6. The results were as follows. - Rating 1: A large number of plate-like crystals characteristic of LDH were observed. - Evaluation 2: As a result of EDS elemental analysis, Mg, Al, and Ti, which are the constituent elements of LDH, were detected. In other words, it was confirmed that these elements were incorporated and crystallized as hydroxide ion conductive layered compounds. - Evaluation 3: In the XRD profile, a peak was detected near 2θ = 11.5°, and it was identified as LDH (hydrotalcite-type compound). This identification was performed using the diffraction peak of LDH (hydrotalcite-type compound) described in JCPDS card No. 35-0964. - Evaluation 4: In Examples B1 to B3, extremely high density was confirmed with a He permeability of 0.0 cm / min·atm. - Evaluation 5: Ionic conductivity of low-conductivity separator C L , ionic conductivity of high-conductivity separator C H , and ratio C H / C L was as shown in Table 2. - Evaluation 6: As shown in Table 2, in Examples B2 and B3, excellent cycle durability was confirmed with no short circuit caused by zinc dendrite even after 300 cycles. On the other hand, in Example B1 (Comparative Example), a short circuit caused by zinc dendrite occurred in less than 300 cycles, and it was found to have poor cycle durability.

[0079] [Table 2] [Explanation of symbols]

[0080] 10,110 Zinc secondary battery 11,111 Stacked Cell 12,112 Negative plate 12a,112a Negative electrode active material 12b,112b Negative electrode current collector 13 Negative electrode current collector 14,114 Positive plate 14a,114a Cathode active material 14b,114b Positive electrode current collector 15 Positive electrode current collector 16,116 LDH separator 16a Low Conductive Separator 16b Highly conductive separator 20 Battery container 20a Top lid 26 Negative terminal 28 Positive terminal

Claims

1. a negative electrode plate including a negative electrode active material including at least one selected from the group consisting of zinc, zinc oxide, a zinc alloy, and a zinc compound, the negative electrode plate having a first surface and a second surface; A pair of positive electrode plates including a positive electrode active material, the positive electrode plates being provided so as to face the first surface and the second surface of the negative electrode plate; a pair of LDH separators interposed between the pair of positive and negative electrode plates, the LDH separators comprising a hydroxide ion conducting layered compound, which is a layered double hydroxide (LDH) and / or an LDH-like compound; An electrolyte; The pair of LDH separators includes a low-conductivity separator provided on a first surface side of the negative electrode plate and a high-conductivity separator provided on a second surface side of the negative electrode plate, and the ionic conductivity C L The ionic conductivity C of the highly conductive separator H Ratio C H / C L A zinc secondary battery, wherein the capacitance is 1.1 to 13.

0.

2. Ion conductivity C of the low-conductivity separator L is 0.8 to 2.5 S / cm 2 The zinc secondary battery according to claim 1 .

3. Ion conductivity C of the highly conductive separator H is 2.5 to 10.0 S / cm 2 The zinc secondary battery according to claim 1 or 2.

4. 3. The zinc secondary battery according to claim 1 or 2, wherein the negative electrode plate is covered or wrapped with the pair of LDH separators.

5. The zinc secondary battery according to claim 1 or 2, wherein the LDH separator further comprises a porous substrate, the pores of the porous substrate are filled with the hydroxide ion conductive layered compound, and / or at least one surface of the porous substrate is provided with a surface layer containing the hydroxide ion conductive layered compound.

6. The zinc secondary battery according to claim 5 , wherein the porous substrate is made of a polymeric material.

7. 6. The zinc secondary battery according to claim 5, wherein each of the low conductivity separator and the high conductivity separator has a He permeability per unit area of ​​10 cm / min·atm or less.

8. 6. The zinc secondary battery according to claim 5, wherein each of the low conductive separator and the high conductive separator is pressed in the thickness direction of the separator.

9. The zinc secondary battery includes a stacked cell, the stacked cell comprising: A plurality of the positive electrode plates; A plurality of the negative electrode plates; A plurality of pairs of the LDH separators; The electrolyte; The zinc secondary battery according to claim 1 or 2, wherein the positive electrode plate and the negative electrode plate are alternately stacked with the LDH separator sandwiched therebetween, the low conductive separator is arranged on a first surface side of each of the plurality of negative electrode plates, and the high conductive separator is arranged on a second surface side of each of the plurality of negative electrode plates.

10. 3. The zinc secondary battery according to claim 1 or 2, wherein the positive electrode plate contains nickel hydroxide and / or nickel oxyhydroxide, thereby making the zinc secondary battery a nickel-zinc secondary battery.

11. 3. The zinc secondary battery according to claim 1 or 2, wherein the positive electrode plate is an air electrode, thereby forming the zinc secondary battery into an air-zinc secondary battery.

Citation Information

Patent Citations

  • Structure for avoiding zinc dendrite short circuit, preparation and battery containing structure

    CN111463502A

  • LDH separator and zinc secondary battery

    JP2023038786A

  • Electrode / separator layered body and nickel zinc battery equipped therewith

    WO2018105178A1

  • LDH separator and zinc secondary battery

    WO2021229916A1

  • Zinc secondary battery

    WO2022113434A1